Manufacturing method of polarizing film

By differentially cleaning polyvinyl alcohol resin films through controlled temperature and flow rate adjustments in a multi-stage process, the method addresses width-direction variations in polarizing films, achieving enhanced optical uniformity and performance.

JP7564629B2Active Publication Date: 2024-10-09SUMITOMO CHEM CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2020034837
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-03-02
Publication Date
2024-10-09
Estimated Expiration
2040-03-02

AI Technical Summary

Technical Problem

Existing methods for manufacturing polarizing films fail to adequately address variations in optical properties along the width direction, leading to inconsistencies in the polarizing film's performance.

Method used

A method involving differential cleaning of polyvinyl alcohol resin films by adjusting cleaning temperatures and liquid flow rates across different sections of the film width, ensuring greater cleaning at the ends than the center, using a multi-stage cleaning process with controlled discharge ports and temperatures to uniformize the film's optical properties.

Benefits of technology

The method effectively reduces variations in optical properties along the width of the polarizing film, enhancing its uniformity and performance consistency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007564629000001
    Figure 0007564629000001
  • Figure 0007564629000002
    Figure 0007564629000002
  • Figure 0007564629000003
    Figure 0007564629000003
Patent Text Reader

Abstract

To reduce variations in optical characteristics in a width direction of a polarizing film.SOLUTION: A method for producing a polarizing film for producing a polarizing film from a polyvinyl alcohol-based resin film includes: a treatment step of bringing a treatment liquid into contact with the polyvinyl alcohol-based resin film, and treating the polyvinyl alcohol-based resin film; and a cleaning step of bringing a cleaning liquid into contact with the polyvinyl alcohol-based resin film, and cleaning the polyvinyl alcohol-based resin film, in this order. The cleaning step is a step of dividing the polyvinyl alcohol-based resin film into one end including one end in a width direction of the polyvinyl alcohol-based resin film, the other end including the other end in the width direction, and a central part in an inner side in the width direction with respect to the one end and the other end, with the width of the polyvinyl alcohol-based resin film as a reference, and cleaning the polyvinyl alcohol-based resin film so that a degree of cleaning of the one end is larger than a degree of cleaning of the other end and the degree of cleaning of the other end is larger than a degree of cleaning of the central part.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a polarizing film from a polyvinyl alcohol-based resin film. [Background technology]

[0002] Conventionally, a polarizing film in which a dichroic dye is adsorbed and aligned on a polyvinyl alcohol-based resin film has been known. The polarizing film is used, for example, as a material for a polarizing plate. A polarizing plate is usually produced by laminating a protective film such as triacetyl cellulose to at least one side, preferably both sides, of a polarizing film via an adhesive made of an aqueous solution of a polyvinyl alcohol-based resin. The polarizing plate is used, for example, as a display screen in liquid crystal display devices (LCDs) such as liquid crystal televisions, personal computer monitors, and mobile phones.

[0003] In the manufacturing process of polarizing films, there have been efforts to suppress the variation in the optical properties of the polarizing film in the width direction. For example, JP 2013-140345 A (Patent Document 1) and Taiwan Patent Publication No. 201142375 A (Patent Document 2) propose that when a polyvinyl alcohol resin film is subjected to various treatments such as dyeing and then washed with water to produce a polarizing film, the water washing temperature of both ends in the width direction of the polarizing film is made different from the water washing temperature of the center part in the width direction of the polarizing film to suppress the variation in the optical properties. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2013-140345 A [Patent Document 2] Taiwan Publication Patent No. 201142375 Summary of the Invention [Problem to be solved by the invention]

[0005] An object of the present invention is to provide a method for producing a polarizing film that can reduce variation in optical properties in the width direction of the polarizing film. [Means for solving the problem]

[0006] The present invention provides the following method for producing a polarizing film. [1] A method for producing a polarizing film from a polyvinyl alcohol-based resin film, comprising the steps of: a treatment step of treating the polyvinyl alcohol-based resin film by contacting the film with a treatment liquid; a cleaning step of contacting the polyvinyl alcohol-based resin film with a cleaning liquid to clean the film, the cleaning step is a step of dividing the polyvinyl alcohol-based resin film based on a width of the polyvinyl alcohol-based resin film into one end portion including one end in a width direction of the polyvinyl alcohol-based resin film, another end portion including the other end in the width direction, and a central portion that is more inward in the width direction than the one end portion and the other end portion, and cleaning the polyvinyl alcohol-based resin film by making the degree of cleaning of the one end portion greater than the degree of cleaning of the other end portion and by making the degree of cleaning of the other end portion greater than the degree of cleaning of the central portion. [2] The method for producing a polarizing film according to [1], wherein the washing step is carried out so as to satisfy the following i): i) If the temperature of the cleaning liquid in contact with the one end portion is T1 [°C], the temperature of the cleaning liquid in contact with the other end portion is T2 [°C], and the temperature of the cleaning liquid in contact with the central portion is T3 [°C], T1, T2, and T3 satisfy the relationship T1>T2>T3. [3] The method for producing a polarizing film according to [2], wherein the washing step is carried out so as to satisfy the above i) and at least one of the following a1) and b1): a1) 1≦T1-T2≦15 b1) 2≦T2-T3≦30 [4] The method for producing a polarizing film according to [2] or [3], wherein the washing step is carried out so as to satisfy the above i) and the following c1): c1) 3≦T3≦25 [5] The method for producing a polarized film according to any one of [1] to [4], wherein the washing step is carried out so as to satisfy the following ii): ii) If the unit width and the amount of the cleaning liquid per unit time in contact with the one end portion are M1 [L / m / min], the unit width and the amount of the cleaning liquid per unit time in contact with the other end portion are M2 [L / m / min], and the unit width and the amount of the cleaning liquid per unit time in contact with the central portion are M3 [L / m / min], then M1, M2 and M3 satisfy the relationship M1>M2>M3. [6] The method for producing a polarized film according to any one of [1] to [5], wherein the cleaning step includes an operation of continuously discharging the cleaning liquid from a cleaning device having a plurality of outlets for discharging the cleaning liquid toward the polyvinyl alcohol-based resin film from the outlets. [7] The method for producing a polarized film according to [6], wherein, in the operation of continuously discharging the cleaning liquid, the polyvinyl alcohol-based resin film is transported vertically upward, and a height position of the discharge port that discharges the cleaning liquid toward the central portion is lower than a height position of the discharge port that discharges the cleaning liquid toward the one end portion and a height position of the discharge port that discharges the cleaning liquid toward the other end portion. Effect of the Invention

[0007] According to the present invention, it is possible to provide a method for producing a polarizing film that can reduce variations in the optical properties of the polarizing film in the width direction. [Brief description of the drawings]

[0008] [Figure 1] FIG. 2 is a partially sectional perspective view illustrating a cleaning device having a plurality of outlets for discharging a cleaning liquid used in a two-stage cleaning process in a first embodiment. [Diagram 2]FIG. 1(a) is a schematic cross-sectional side view showing the cleaning device to explain an example of a two-stage cleaning process in a first embodiment, and FIG. 1(b) and (c) are schematic top views showing multiple outlets for discharging cleaning liquid in the cleaning device. [Diagram 3] FIG. 11 is a partially sectional perspective view illustrating a cleaning device having a plurality of outlets for discharging a cleaning liquid used in a three-stage cleaning process in a second embodiment, for explaining the example of the three-stage cleaning process. [Figure 4] FIG. 1(a) is a schematic cross-sectional side view showing the cleaning device to explain an example of a three-stage cleaning process in the second embodiment, and FIG. 1(b), (c) and (d) are schematic top views showing multiple outlets for discharging cleaning liquid in the cleaning device. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Hereinafter, a method for producing a polarizing film according to one aspect of the present invention (hereinafter also referred to as "the production method according to the present embodiment") will be described with reference to the drawings.

[0010] [Method for producing polarizing film] A method for producing a polarizing film according to one aspect of the present invention (a method for producing a polarizing film according to the present embodiment) is a method for producing a polarizing film from a polyvinyl alcohol-based resin film. The method for producing a polarizing film includes, in this order, a treatment step of contacting the polyvinyl alcohol-based resin film with a treatment liquid and a cleaning step of contacting the polyvinyl alcohol-based resin film with a cleaning liquid. The cleaning step is a step of dividing the polyvinyl alcohol-based resin film into one end including one end in the width direction of the polyvinyl alcohol-based resin film, the other end including the other end in the width direction, and a central portion that is inside the one end and the other end in the width direction, based on the width of the polyvinyl alcohol-based resin film, and cleaning the polyvinyl alcohol-based resin film by making the degree of cleaning of the one end greater than the degree of cleaning of the other end and making the degree of cleaning of the other end greater than the degree of cleaning of the central portion.

[0011] <Polyvinyl alcohol resin film> The polarizing film can be obtained, for example, by adsorbing and orienting a dichroic dye (iodine, dichroic dye, etc.) on a uniaxially stretched polyvinyl alcohol resin film. The polyvinyl alcohol resin film means a film made of a polyvinyl alcohol resin, and examples thereof include saponified polyvinyl acetate resins. Examples of polyvinyl acetate resins include polyvinyl acetate, which is a homopolymer of vinyl acetate, as well as copolymers of vinyl acetate and other monomers copolymerizable therewith (e.g., ethylene-vinyl acetate copolymers). Examples of other copolymerizable monomers include unsaturated carboxylic acids, olefins, vinyl ethers, and unsaturated sulfonic acids. The degree of polymerization of the polyvinyl alcohol resin is usually about 1000 to 10000, preferably about 1500 to 5000. The degree of saponification is usually 85 mol% or more, preferably 90 mol% or more, and more preferably 99 to 100 mol%. These polyvinyl alcohol resins may be modified, and for example, polyvinyl formal, polyvinyl acetal, polyvinyl butyral, etc. modified with aldehydes can be used.

[0012] In the manufacturing method according to the present embodiment, the starting material for the polyvinyl alcohol-based resin film may be an unstretched polyvinyl alcohol-based resin film (raw film) having a thickness of 65 μm or less (for example, 60 μm or less), preferably 50 μm or less, more preferably 35 μm or less, and even more preferably 30 μm or less. This makes it possible to obtain a thin polarizing film, which is increasingly in demand in the market. The width of the raw film is not particularly limited, and is, for example, 400 mm or more and 8000 mm or less, preferably 2000 mm or more and 5500 mm or less. When the width of the raw film is 2000 mm or more, the optical properties such as hue tend to vary in the width direction of the polarizing film, but the manufacturing method according to the present embodiment can reduce the variation. The thickness of the unstretched polyvinyl alcohol-based resin film is preferably 20 μm or more. The raw film is prepared, for example, as a roll (raw roll) of a long unstretched polyvinyl alcohol-based resin film. The unstretched polyvinyl alcohol-based resin film (raw film) is usually supplied as a rolled film.

[0013] The polyvinyl alcohol-based resin film may be laminated on a substrate film that supports the polyvinyl alcohol-based resin film. That is, the polyvinyl alcohol-based resin film may be prepared as a laminate film of a substrate film and a polyvinyl alcohol-based resin film laminated thereon. In this case, the polyvinyl alcohol-based resin film can be produced, for example, by applying a coating liquid containing a polyvinyl alcohol-based resin to at least one surface of the substrate film and then drying the coating liquid.

[0014] The substrate film may be, for example, a film made of a thermoplastic resin. Specific examples of the film may include a film made of a thermoplastic resin having light transmission, preferably an optically transparent thermoplastic resin, such as a polyolefin resin such as a chain polyolefin resin (polypropylene resin, etc.) or a cyclic polyolefin resin (norbornene resin, etc.); a cellulose resin such as triacetyl cellulose or diacetyl cellulose; a polyester resin such as polyethylene terephthalate or polybutylene terephthalate; a polycarbonate resin; a (meth)acrylic resin such as a methyl methacrylate resin; a polystyrene resin; a polyvinyl chloride resin; an acrylonitrile-butadiene-styrene resin; an acrylonitrile-styrene resin; a polyvinyl acetate resin; a polyvinylidene chloride resin; a polyamide resin; a polyacetal resin; a modified polyphenylene ether resin; a polysulfone resin; a polyethersulfone resin; a polyarylate resin; a polyamideimide resin; a polyimide resin, etc.

[0015] <Treatment process> The manufacturing method according to the present embodiment includes, in this order, a treatment step of contacting the polyvinyl alcohol-based resin film with a treatment liquid and a cleaning step of contacting the polyvinyl alcohol-based resin film with a cleaning liquid to clean the film. The treatment step is a step of performing various treatments, such as swelling treatment, dyeing treatment, and crosslinking treatment (boric acid treatment), on the raw film.

[0016] Specifically, the above-mentioned treatment process can include a swelling process in which a swelling liquid is brought into contact with the raw film to perform a swelling process, a dyeing process in which a dyeing liquid is brought into contact with the polyvinyl alcohol-based resin film (hereinafter also referred to as a "swollen film") after the swelling process to perform a dyeing process, a crosslinking process in which a crosslinking liquid is brought into contact with the polyvinyl alcohol-based resin film (hereinafter also referred to as a "dyed film") after the dyeing process to perform a crosslinking process, and a complementary color process in which a complementary color liquid is brought into contact with the polyvinyl alcohol-based resin film (hereinafter also referred to as a "crosslinked film") after the crosslinking process to perform a color adjustment process. In this specification, the polyvinyl alcohol-based resin film after the color adjustment process is also referred to as a "color correction film".

[0017] In the above-mentioned processing step, it is preferable to include an operation of uniaxially stretching the film before or during any of the steps such as the swelling step described above. For example, the above-mentioned processing step can be exemplified by performing a swelling step, a dyeing step, a crosslinking step, and a color complementing step in this order after uniaxially stretching (dry stretching) an unstretched raw film in air or an inert gas. In addition, it can be exemplified by performing a swelling step, a dyeing step, a crosslinking step, and a color complementing step in this order using an unstretched raw film, and uniaxially stretching the film in a wet manner before or during the crosslinking step. Furthermore, the above-mentioned processing step can include other steps as long as the effects of the present invention are achieved.

[0018] In the above-mentioned treatment step, for example, the raw film described above is unwound from the raw film roll and continuously transported along the film transport path of a conventionally known polarizing film manufacturing apparatus, so that the raw film can be immersed in each treatment liquid (hereinafter also referred to as "treatment bath") contained in each treatment tank for performing the above-mentioned swelling step, dyeing step, crosslinking step, color complementation step, etc. Furthermore, after the raw film is pulled out from the treatment tank, the method for manufacturing the polarizing film described above can proceed to a cleaning step described below. The above-mentioned treatment step is not limited to the above-mentioned method of immersing the raw film in the treatment bath, as long as it is a method of contacting the raw film with the treatment liquid and treating it, and may be any other method of contacting the treatment liquid with the raw film surface. As another method of contacting the treatment liquid with the raw film surface, a method of contacting the treatment liquid with the raw film surface by a shower of the treatment liquid is suitable. Here, the "shower" of the treatment liquid means a flow of the treatment liquid discharged from a plurality of discharge ports, and in the above flow, the treatment liquid may be any of granular, misty, and liquid flow. To contact the treatment liquid with the raw film surface by the shower, a shower device is usually used. The shower device has a plurality of outlets, and can create a liquid flow by releasing the treatment liquid from the outlets. On the other hand, when the treatment step is performed by immersing the raw film in a treatment bath, the treatment bath for one treatment (e.g., crosslinking treatment) is not limited to one, and the raw film can be immersed in two or more treatment baths in sequence.

[0019] Here, in this specification, the term "treatment tank" refers to a general term including a swelling tank, a dyeing tank, a crosslinking tank, and a complementary color tank. Furthermore, the term "treatment liquid" refers to a general term including a swelling liquid, a dyeing liquid, a crosslinking liquid, and a complementary color liquid, and the term "treatment bath" refers to a general term including a swelling bath, a dyeing bath, a crosslinking bath, and a complementary color bath. Hereinafter, as an example of the treatment process in the manufacturing method according to this embodiment, a method in which the above-mentioned conventionally known polarizing film manufacturing device is used to continuously transport the raw film along the film transport path, and the swelling process, the dyeing process, the crosslinking process, and the complementary color process are performed in this order will be described.

[0020] (Swelling process) The swelling process is carried out for the purposes of removing foreign matter from the surface of the raw film, removing plasticizers in the raw film, imparting ease of dyeing, plasticizing the raw film, etc. The treatment conditions are determined within a range in which the above purposes can be achieved and defects such as extreme dissolution and devitrification of the raw film do not occur.

[0021] In the swelling step, the raw film is continuously unwound from the raw film roll, transported along a film transport path constructed by a guide roll and a nip roll, and then immersed in a swelling bath (swelling liquid contained in a swelling tank) for a predetermined time, and then the raw film is pulled out as a swollen film, thereby performing the swelling treatment. As the swelling liquid used in the swelling bath, in addition to pure water, it is possible to use an aqueous solution containing boric acid (JP Patent Publication No. 10-153709), chloride (JP Patent Publication No. 06-281816), inorganic acid, inorganic salt, water-soluble organic solvent, alcohol, etc., added in a range of about 0.01 to 10 mass %.

[0022] The temperature of the swelling bath is, for example, about 10 to 50° C., preferably about 10 to 40° C., and more preferably about 15 to 30° C. The immersion time of the raw film is preferably about 10 to 300 seconds, and more preferably about 20 to 200 seconds. When the raw film is a polyvinyl alcohol-based resin film that has been stretched in advance in a gas, the temperature of the swelling bath is, for example, about 20 to 70° C., and preferably about 30 to 60° C. The immersion time of the raw film is preferably about 30 to 300 seconds, and more preferably about 60 to 240 seconds.

[0023] In the swelling treatment, the original film swells in the width direction, which tends to cause a problem of wrinkles in the swollen film. As one means for transporting the swollen film while removing the wrinkles, a known roll having a width-expanding function such as a width-expanding roll (expander roll), a spiral roll, or a crown roll can be used as a guide roll, or a known width-expanding device such as a cross guider, a bend bar, or a tenter clip can be used. Another means for suppressing the occurrence of wrinkles is to perform a stretching treatment. For example, the original film in the swelling bath can be uniaxially stretched by utilizing the difference in peripheral speed between each nip roll provided in the film transport path.

[0024] In the swelling treatment, the film also swells and expands in the film transport direction, so when the raw film is not actively stretched, it is preferable to take measures such as controlling the speed of nip rolls placed before and after the swelling bath in order to eliminate slack in the film in the transport direction. In addition, for the purpose of stabilizing the film transport in the swelling bath, it is also useful to control the water flow in the swelling bath with a shower device or to use an EPC device (Edge Position Control device: a device that detects the edge of the film and prevents the film from meandering).

[0025] After the swelling treatment, the swollen film is pulled out of the swelling bath and introduced along a film transport path into a dye bath used in the dyeing step described below.

[0026] (dying process) The dyeing process is carried out for the purpose of adsorbing a dichroic dye such as iodine to the polyvinyl alcohol resin film after the swelling process and orienting the dye. The processing conditions are determined within a range in which the above-mentioned purpose can be achieved and defects such as extreme dissolution and devitrification of the film do not occur. The dyeing process can be carried out by immersing the swollen film transported along a film transport path constructed by a guide roll and a nip roll in a dye bath (a dyeing solution contained in a dyeing tank) for a predetermined time and then drawing out the film as a dyed film. In order to improve the dyeability of the dichroic dye, it is preferable that the swollen film to be subjected to the dyeing process is a film that has been subjected to at least a certain degree of uniaxial stretching, and it is preferable to carry out a uniaxial stretching process during the dyeing process instead of or in addition to the uniaxial stretching process before the dyeing process.

[0027] It is preferable to use iodine as the dichroic dye, and the dyeing solution used in the dye bath can be, for example, an aqueous solution having a mass ratio of iodine / potassium iodide / water=about 0.003-0.3 / about 0.1-10 / 100. Instead of potassium iodide, other iodides such as zinc iodide may be used, or potassium iodide may be used in combination with other iodides. In addition, compounds other than iodides, such as boric acid, zinc chloride, cobalt chloride, etc., may be allowed to coexist. When boric acid is added, it is distinguished from the crosslinking solution described below in that it contains a dichroic dye. In this specification, when the aqueous solution contains about 0.003 parts by mass or more of a dichroic dye per 100 parts by mass of water, the aqueous solution can be considered as a dyeing solution. The temperature of the dye bath when the swollen film is immersed is usually about 10 to 45°C, preferably 10 to 40°C, and more preferably 20 to 35°C, and the immersion time of the swollen film is usually about 30 to 600 seconds, and preferably 60 to 300 seconds.

[0028] A dichroic dye may be used instead of iodine as the dichroic pigment, and the dyeing solution used in the dye bath may be, for example, an aqueous solution having a mass ratio of dichroic dye / water of about 0.001 to 0.1 / 100. This dyeing solution may contain dyeing auxiliaries, such as inorganic salts such as sodium sulfate, surfactants, etc. One type of dichroic dye may be used alone, or two or more types of dichroic dyes may be used in combination.

[0029] As described above, in the dyeing step, the swollen film can be uniaxially stretched in the dye bath by creating a difference in peripheral speed between nip rolls disposed before and after the dye bath.

[0030] In the dyeing process, in order to transport the polyvinyl alcohol-based resin film while removing wrinkles, as in the swelling process, known rolls having a width-widening function such as the above-mentioned expander roll, spiral roll, and crown roll, or known width-widening devices such as cross guiders, bend bars, and tenter clips can be used. Another means for suppressing the occurrence of wrinkles is to perform a stretching process, as in the swelling process.

[0031] After the dyeing treatment, the dyed film is pulled out of the dye bath and introduced along a film transport path into a crosslinking bath used in the crosslinking step described below. In this case, the dyed film is preferably roughly washed by passing through a shower device before being introduced into the crosslinking bath, so that excess dye solution adhering to the dyed film is washed away.

[0032] (Crosslinking process) The crosslinking step is carried out for the purpose of imparting water resistance to the dyed film. The crosslinking step may be carried out once or multiple times. In the crosslinking step, the dyed film transported along a film transport path constructed by a guide roll and a nip roll is immersed in a crosslinking bath (a crosslinking liquid contained in a crosslinking tank) for a predetermined time, and then the film is pulled out as a crosslinked film, thereby carrying out a crosslinking treatment.

[0033] The crosslinking liquid may be a solution in which a crosslinking agent is dissolved in a solvent. Examples of the crosslinking agent include boric acid, boron compounds such as borax, glyoxal, and glutaraldehyde. These may be used alone or in combination of two or more. The solvent may be, for example, water, and may further contain an organic solvent compatible with water. The concentration of the crosslinking agent in the crosslinking liquid is not limited thereto, but is preferably in the range of 1 to 20% by mass, and more preferably 4 to 15% by mass.

[0034] The crosslinking liquid may be, for example, an aqueous solution containing about 1 to 10 parts by mass of boric acid per 100 parts by mass of water. When the dichroic dye used in the dyeing process is iodine, the crosslinking liquid preferably contains an iodide in addition to boric acid, and the amount of the iodide may be, for example, 1 to 30 parts by mass per 100 parts by mass of water. Examples of the iodide include potassium iodide and zinc iodide. In addition, compounds other than iodide, such as zinc chloride, cobalt chloride, zirconium chloride, sodium thiosulfate, potassium sulfite, and sodium sulfate, may be allowed to coexist.

[0035] In the crosslinking treatment, the concentration of boric acid and iodide, and the temperature of the crosslinking bath can be appropriately changed depending on the purpose. For example, the concentration can be an aqueous solution with a mass ratio of boric acid / iodide / water = 3 to 10 / 1 to 20 / 100. If necessary, other crosslinking agents may be used instead of boric acid, or boric acid may be used in combination with other crosslinking agents. The temperature of the crosslinking bath when the dyed film is immersed is usually about 50 to 70 ° C, preferably 53 to 65 ° C, and the immersion time of the dyed film is usually about 10 to 600 seconds, preferably 20 to 300 seconds, more preferably 20 to 200 seconds. In addition, when the dyeing treatment and the crosslinking treatment are performed in this order on a polyvinyl alcohol-based resin film that has been stretched before the swelling treatment, the temperature of the crosslinking bath is usually about 50 to 85 ° C, preferably 55 to 80 ° C.

[0036] The crosslinking treatment may be carried out multiple times, usually 2 to 5 times. In this case, the composition and temperature of each crosslinking bath used may be the same or different as long as they are within the above range. In addition, uniaxial stretching treatment can be carried out in the crosslinking bath by utilizing the difference in peripheral speed of each nip roll.

[0037] In the crosslinking treatment, in order to transport the polyvinyl alcohol-based resin film while removing wrinkles, as in the swelling treatment, known rolls having a width-widening function such as the above-mentioned expander roll, spiral roll, and crown roll, or known width-widening devices such as cross guiders, bend bars, and tenter clips can be used. Another means for suppressing the occurrence of wrinkles is to perform a stretching treatment, as in the swelling treatment.

[0038] After the above crosslinking treatment, the crosslinked film is pulled out from the crosslinking bath and introduced along a film transport path into a complementary color bath used in the complementary color step described next.

[0039] (complementary color process) The complementary color process is carried out for the purpose of adjusting the hue of the crosslinked film. In the complementary color process, the crosslinked film conveyed along the film conveying path constructed by the guide roll and the nip roll is immersed in a complementary color bath (complementary color liquid contained in a complementary color tank) for a predetermined time, and then drawn out as a color correction film, thereby performing complementary color processing. For example, when the dichroic dye contained in the dyeing solution is iodine, the complementary color liquid can be an aqueous solution having a concentration of boric acid / iodide / water=1-5 / 3-30 / 100 by mass ratio. The temperature of the complementary color bath when the crosslinked film is immersed is usually about 20-65° C., and the immersion time of the crosslinked film is usually about 1-300 seconds, preferably 2-100 seconds.

[0040] The color correction film is then introduced into a washing bath along the film transport path to be used in the washing step described below.

[0041] (Stretching process) As described above, the polyvinyl alcohol-based resin film is preferably uniaxially stretched in a wet or dry manner during a series of treatment steps and a washing step described later (i.e., before and after any one or more treatment steps and washing steps and / or during any one or more treatment steps and washing steps). Specific methods of uniaxial stretching include, for example, inter-roll stretching, which performs longitudinal uniaxial stretching by applying a peripheral speed difference between two nip rolls (e.g., two nip rolls arranged before and after a treatment bath) constituting a film transport path, hot roll stretching as described in Japanese Patent No. 2731813, tenter stretching, etc., and preferably inter-roll stretching. The uniaxial stretching step can be performed multiple times from the raw film of the polyvinyl alcohol-based resin film, which is the starting material, to obtaining a polarizing film. The stretching process is also effective in suppressing the occurrence of wrinkles in the film.

[0042] The final cumulative stretch ratio of the polarizing film based on the above-mentioned raw film is usually about 4.5 to 7 times, and preferably 5 to 6.5 times. The stretching step may be performed in any processing step, and even when the stretching treatment is performed in two or more processing steps, the stretching treatment may be performed in any processing step.

[0043] <Cleaning process> The manufacturing method according to the present embodiment includes, in this order, a treatment step of bringing the polyvinyl alcohol-based resin film (hereinafter also simply referred to as "film") into contact with a treatment liquid for treatment, and a cleaning step of bringing the polyvinyl alcohol-based resin film into contact with a cleaning liquid for cleaning, as described above. Of these, the cleaning step is performed after the treatment step described above, for example, after the color complementing step described above. In the cleaning step, a cleaning treatment is performed to remove excess boric acid, iodine, and other chemicals attached to the film in the crosslinking step, color complementing step, and the like. The cleaning treatment can be performed, for example, by immersing the color complementing-treated film in a cleaning bath and bringing the cleaning liquid into contact with the film. The cleaning treatment can be performed by contacting the film with the cleaning liquid by releasing the cleaning liquid from a shower device instead of immersing the film in the cleaning bath, or by combining immersion in the cleaning bath with the release of the cleaning liquid from a shower device.

[0044] In the washing process, for the purpose of conveying the polyvinyl alcohol-based resin film while removing wrinkles, known rolls having a width-widening function such as the above-mentioned expander roll, spiral roll, and crown roll can be used, or known widening devices such as cross guiders, bend bars, and tenter clips can be used. In addition, a stretching process may be performed in order to suppress the occurrence of wrinkles in the washing process. As the washing liquid used in the washing step, water and any of the conventionally known washing liquids used for washing this type of polyvinyl alcohol-based resin film can be used. Note that, as a liquid-removing means for removing the washing liquid from the surface of the polyvinyl alcohol-based resin film after the washing step, for example, a nip roll can be used, and in addition to the nip roll, a means for blowing air onto the film to remove the liquid, a scraper that comes into contact with the film to remove the liquid, and the like can be used.

[0045] In the manufacturing method according to the present embodiment, specifically, the cleaning step is a step of dividing the polyvinyl alcohol-based resin film into one end including one end in the width direction of the polyvinyl alcohol-based resin film, the other end including the other end in the width direction, and a central portion that is inside the one end and the other end in the width direction, based on the width of the polyvinyl alcohol-based resin film, and cleaning the polyvinyl alcohol-based resin film by making the degree of cleaning of the one end greater than the degree of cleaning of the other end and making the degree of cleaning of the other end greater than the degree of cleaning of the central portion. Even if the degree of cleaning is gradually increased from the center to one end and the other end in the width direction of the film, the cleaning step does not deviate from the scope of the present embodiment as long as the relationship between the degree of cleaning at one end, the other end, and the central portion satisfies the above-mentioned condition.

[0046] The cause of the variation in optical properties in the width direction of the polarizing film is not clear in detail, but the following cause is presumed. That is, in the above-mentioned treatment process, the treatment liquid is more likely to penetrate from the end face than from the surface of the polyvinyl alcohol-based resin film, and the amount of the treatment liquid that penetrates the end and center of the film is different. This causes a difference in the degree of treatment between the end and center of the film, which is presumed to cause the optical properties to vary in the width direction of the polarizing film. Alternatively, the above-mentioned uniaxial stretching process or the like causes a variation in the thickness in the width direction of the film, and the degree of treatment also varies according to this variation in thickness, which is presumed to cause the optical properties to vary in the width direction of the polarizing film. Based on the above-presumed causes, the present inventors have conceived a method of equalizing the difference in the degree of treatment between the end and center of the film by dividing the polyvinyl alcohol-based resin film into "one end / center / other end" based on its width and washing it, and have completed the present invention.

[0047] Here, in this specification, the "one end" and the "other end" of the polyvinyl alcohol-based resin film in the width direction can be determined arbitrarily. For example, the "one end" and the "other end" of the long polyvinyl alcohol-based resin film that has been subjected to the above-mentioned treatment process may be fixed or moved in the washing process. In this case, the "one end" of the polyvinyl alcohol-based resin film in the width direction is preferably the side that has been treated to a greater extent by the treatment liquid, and the "other end" of the film in the width direction is preferably the side that has been treated to a lesser extent by the treatment liquid than the "one end". The degree of treatment by the treatment liquid can be determined, for example, based on the orthogonal hue b value.

[0048] The width of one end and the other end of the polyvinyl alcohol-based resin film is 5 to 30%, preferably 5 to 25%, based on the width of the polyvinyl alcohol-based resin film. When the ratio of the one end and the other end where the degree of cleaning is greater than that of the center is within the above-mentioned numerical range with respect to the width of the film, the effect of the present invention of making the optical characteristics such as hue uniform in the width direction can be sufficiently obtained. It is preferable that the width of one end and the other end of the polyvinyl alcohol-based resin film are the same length.

[0049] A more specific cleaning method in the cleaning step includes a method in which the polyvinyl alcohol-based resin film is immersed in a cleaning bath and a cleaning liquid is discharged from a shower device toward the film, thereby contacting the film with the cleaning liquid. In particular, in this embodiment, since the degree of cleaning is made different at one end, the other end, and the center of the film, a method is preferably adopted in which the cleaning liquid is discharged from a shower device at multiple locations along the transport direction of the film, thereby contacting the film with the cleaning liquid. In this case, the cleaning method is preferably, first, on the upstream side of the transport direction of the film, the degree of cleaning of the center of the film is made greater than that of the one end and the other end, or the degree of cleaning is made uniform over the entire width direction of the film. Furthermore, on the downstream side of the transport direction of the film, the degree of cleaning of one end of the film is made greater than that of the other end, and the degree of cleaning of the other end is made greater than that of the center. By such a cleaning method, it is possible to suppress the variation in optical properties in the width direction of the film in which the cleaning liquid has been contacted.

[0050] (First Form) As a first embodiment for making one end of a polyvinyl alcohol-based resin film cleaned to a greater extent than the other end of the film, and making the other end of the film cleaned to a greater extent than the central portion of the film, the following embodiment can be exemplified. That is, in the production method according to this embodiment, the cleaning step is preferably carried out so as to satisfy the following i).

[0051] i) If the temperature of the cleaning liquid in contact with the one end is T1 [°C], the temperature of the cleaning liquid in contact with the other end is T2 [°C], and the temperature of the cleaning liquid in contact with the center is T3 [°C], T1, T2, and T3 satisfy the relationship T1>T2>T3. That is, the relationship shown in i) above means that the higher the temperature of the cleaning liquid in contact with the polyvinyl alcohol-based resin film, the greater the degree of cleaning of the film.

[0052] The washing step is preferably carried out so as to satisfy the above i) and at least one of the following a1) and b1). It is more preferable that the washing step is carried out so as to satisfy both the following a1) and b1). a1) 1≦T1-T2≦15 b1) 2≦T2-T3≦30.

[0053] It is also preferable that the washing step is carried out so as to satisfy the above i) and the following c1). c1) 3≦T3≦25.

[0054] The temperature of the cleaning solution brought into contact with the polyvinyl alcohol-based resin film is preferably 65° C. or less. If the temperature of the cleaning solution exceeds 65° C., the optical performance of the polarizing film obtained by the manufacturing method according to the present embodiment and the polarizing plate using the same is likely to deteriorate. Furthermore, if the temperature of the cleaning solution brought into contact with the polyvinyl alcohol-based resin film is less than 3° C., the cleaning is not sufficient, and there is a risk that the variation in the optical properties in the width direction of the polarizing film obtained by the manufacturing method according to the present embodiment will not be sufficiently suppressed.

[0055] When the first embodiment is adopted, the temperature T3 of the cleaning liquid brought into contact with the central portion of the polyvinyl alcohol-based resin film preferably satisfies the above c1), i.e., 3 to 25° C. More preferably, the temperature T3 of the cleaning liquid brought into contact with the central portion of the polyvinyl alcohol-based resin film satisfies the following c2). c2) 5≦T3≦20.

[0056] When the first embodiment is adopted, the temperature T2 of the cleaning liquid brought into contact with the other end of the polyvinyl alcohol-based resin film can be a temperature that satisfies the above b1) in relation to the above T3, that is, 2≦T2−T3≦30. Specifically, in consideration of the above c1), the temperature T2 is preferably 5 to 55° C. More preferably, the temperature T2 of the cleaning liquid brought into contact with the other end of the polyvinyl alcohol-based resin film satisfies the following b2) in relation to the above T3. b2) 2≦T2-T3≦20.

[0057] When the first embodiment is adopted, the temperature T1 of the cleaning liquid brought into contact with one end of the polyvinyl alcohol-based resin film can be a temperature that satisfies the above a1) in relation to the above T2, that is, 1≦T1-T2≦15. Specifically, in consideration of the above c1) and b1), the temperature T1 is preferably 6 to 65° C. More preferably, the temperature T1 of the cleaning liquid brought into contact with one end of the polyvinyl alcohol-based resin film satisfies the following b2) in relation to the above T2. a2) 3≦T1-T2≦10.

[0058] When T1, T2, and T3 satisfy the relationship T1>T2>T3 and also satisfy the above-mentioned relationships [a1), b1), and c1)], the difference in the degree of treatment between the end and center of the film in the treatment step is made more uniform in the cleaning step, which is preferable because it allows the hue adjustment effect in the cleaning step to be fully exerted and reduces the variation in the optical properties of the polarizing film in the width direction.

[0059] In the first embodiment, the cleaning step preferably includes an operation of continuously discharging the cleaning liquid from a cleaning device having a plurality of discharge ports for discharging the cleaning liquid toward the polyvinyl alcohol-based resin film. Specifically, in the first embodiment, a two-stage cleaning step is performed in which the degree of cleaning of the central portion of the film is made greater than that of one end and the other end on the upstream side of the transport direction of the polyvinyl alcohol-based resin film, and the degree of cleaning of the one end of the film is made greater than that of the other end on the downstream side of the transport direction of the film, and the degree of cleaning of the other end is made greater than that of the central portion.

[0060] The cleaning step in the first embodiment will be described below with reference to Figures 1 and 2. Figure 1 is a partially sectional perspective view showing a cleaning device having a plurality of outlets for discharging a cleaning liquid used in the cleaning step, for explaining an example of a two-stage cleaning step in the first embodiment. Figure 2(a) is a schematic sectional side view showing the cleaning device for explaining an example of the two-stage cleaning step in the first embodiment, and Figures 2(b) and 2(c) are schematic top views showing a plurality of outlets for discharging a cleaning liquid in the cleaning device.

[0061] As shown in FIG. 1 and FIG. 2(a), a polyvinyl alcohol-based resin film 1 (hereinafter, simply referred to as "film 1") is transported in the direction of the arrow in the figure by a transport guide roll 2. As a result, the film 1 is immersed in a cleaning liquid 32 in a cleaning bath 31, and then passes through a first-stage shower device 41 and a second-stage shower device 42 in that order. Each of the shower devices 41, 42 has a plurality of shower nozzles 411, 421 arranged in the width direction of the film 1. After passing through the shower devices 41, 42, the film 1 is sent to a drain roll 5, where moisture adhering to the surface is removed. Here, it is preferable that the cleaning liquid 32 in the cleaning bath 31 and the cleaning liquid 32 discharged from the shower devices 41, 42 have the same or similar composition.

[0062] The shower devices 41, 42 are configured to adjust and release the temperature and amount of cleaning liquid according to the widthwise position of the film 1. In the above cleaning step, a cleaning treatment with cleaning liquid 32 in cleaning bath 31 and a cleaning treatment with shower devices 41, 42 are performed, so that the difference in the degree of treatment that occurs between the ends and center in the widthwise direction of the film 1 that has been brought into contact with the cleaning liquid is made uniform, thereby reducing variation in the optical properties of the polarizing film. In the first embodiment, the order of the cleaning treatment of immersion treatment with cleaning liquid 32 in cleaning bath 31 and the cleaning treatment with shower devices 41, 42 is not particularly limited.

[0063] In the cleaning process using the above shower devices 41 and 42, as shown in Figure 2(c), in the first-stage shower device 41, cleaning liquid 32 is discharged from shower nozzle 411b of the shower nozzles 411 that corresponds to the center of the film 1. Furthermore, as shown in Figure 2(b), in the second-stage shower device 42, cleaning liquid 32 is discharged from shower nozzle 421a of the shower nozzles 421 that corresponds to one end of the film 1 and from shower nozzle 421c that corresponds to the other end of the film 1, but cleaning liquid 32 is not discharged from shower nozzle 421b that corresponds to the center of the film 1.

[0064] In the cleaning process using the shower devices 41 and 42, the temperature T3 of the cleaning liquid discharged from the shower nozzle 411b to the center of the film 1 in the first-stage shower device 41 and brought into contact with the center of the film 1 can be selected from, for example, 3 to 25°C as a temperature that satisfies the above c1). Furthermore, the temperature T2 of the cleaning liquid discharged from the shower nozzle 421c to the other end of the film 1 in the second-stage shower device 42 can be selected from, for example, a temperature that satisfies the above b1) in relation to T3, that is, a temperature that satisfies 2≦T2−T3≦30, for example, from 5 to 55°C. Furthermore, the temperature T1 of the cleaning liquid discharged from the shower nozzle 421a to one end of the film 1 and brought into contact with one end of the film 1 can be selected from, for example, a temperature that satisfies the above a1) in relation to T2, that is, a temperature that satisfies 1≦T1−T2≦15, for example, from 6 to 65°C. By carrying out such a cleaning process, the occurrence of cleaning unevenness in the width direction of the film 1 contacted with the cleaning liquid is suppressed.

[0065] Here, the first embodiment is not limited to the above-mentioned embodiment, and may include an embodiment in which the cleaning liquid 32 is discharged from all shower nozzles of the first-stage shower device 41 or the second-stage shower device 42 to the film 1 while satisfying the relationship T1>T2>T3. It may also include an embodiment in which the cleaning liquid is discharged only to one end and the other end of the film 1 from the shower nozzles 411a and 411c of the first-stage shower device 41 and the shower nozzles 421a and 421c of the second-stage shower device 42. In the latter case, it is preferable to perform a cleaning process of the film 1 with the cleaning liquid 32 in the cleaning bath 31 before the cleaning process with the shower devices 41 and 42. This is because it is preferable to clean the center of the film 1 to some extent in order to adjust the optical properties of the polarizing film. Furthermore, the above cleaning process does not deviate from the first embodiment even if the temperature of the cleaning liquid discharged from the shower nozzle and contacted with the film is gradually increased from the center to one end and the other end of the film in the width direction.

[0066] (Second Form) As a second embodiment for making one end of the polyvinyl alcohol-based resin film cleaned to a greater extent than the other end of the film, and making the other end of the film cleaned to a greater extent than the central portion of the film, the following embodiment can be exemplified. That is, in the production method according to this embodiment, the cleaning step is preferably carried out so as to satisfy the following ii).

[0067] ii) If the amount of the cleaning liquid per unit width and unit time in contact with the one end is M1 [L / m / min], the amount of the cleaning liquid per unit width and unit time in contact with the other end is M2 [L / m / min], and the amount of the cleaning liquid per unit width and unit time in contact with the central portion is M3 [L / m / min], the above M1, M2, and M3 satisfy the relationship M1>M2>M3. That is, the relationship shown in ii) above means that the greater the amount of the cleaning liquid per unit width and unit time in contact with the polyvinyl alcohol-based resin film, the greater the degree of cleaning of the film.

[0068] The values ​​of M1, M2, and M3 as the amounts of the cleaning liquid per unit width and unit time (min) are not particularly limited as long as they satisfy the relationship M1>M2>M3. However, from the viewpoint of the production efficiency of the polarizing film, it is preferable to select M1 from 1 to 20 L / m / min, M2 from 1 to 17 L / m / min, and M3 from 1 to 15 L / m / min as the amounts of the cleaning liquid per unit width and unit time of the film, respectively, so as to satisfy the relationship M1>M2>M3.

[0069] Here, in the second embodiment, the cleaning step preferably includes an operation of continuously discharging the cleaning liquid from the discharge ports toward the polyvinyl alcohol-based resin film using a cleaning device having a plurality of discharge ports for discharging the cleaning liquid. In particular, in the second embodiment, in the operation of continuously discharging the cleaning liquid, the polyvinyl alcohol-based resin film is transported vertically upward, and the height position of the discharge port for discharging the cleaning liquid toward the central portion is preferably lower than the height position of the discharge port for discharging the cleaning liquid toward the one end portion and the height position of the discharge port for discharging the cleaning liquid toward the other end portion. More specifically, the operation of continuously discharging the cleaning liquid is preferably performed in a three-stage cleaning step in which the height position of the discharge port for discharging the cleaning liquid toward the central portion is lower than the height positions of the discharge ports for discharging the cleaning liquid toward the other end portion and the one end portion, and the height position of the discharge port for discharging the cleaning liquid toward the other end portion is lower than the height position of the discharge port for discharging the cleaning liquid toward the one end portion. This makes it possible to easily satisfy the relationship shown in ii) above in the cleaning step carried out using the above cleaning device.

[0070] The cleaning process in the second embodiment will be described below with reference to Figures 3 and 4. Figure 3 is a partially sectional perspective view showing a cleaning device having a plurality of outlets for discharging the cleaning liquid used in the cleaning process, for explaining an example of a three-stage cleaning process in the second embodiment. Figure 4(a) is a schematic sectional side view showing the cleaning device for explaining an example of the three-stage cleaning process in the second embodiment, and Figures 4(b), 4(c), and 4(d) are schematic top views showing a plurality of outlets for discharging the cleaning liquid in the cleaning device.

[0071] As shown in FIG. 3 and FIG. 4(a), the film 1 (polyvinyl alcohol-based resin film 1) is transported in the direction of the arrow in the figure by a transport guide roll 2. As a result, the film 1 is immersed in a cleaning liquid 32 in a cleaning bath 31, and then passes through a first-stage shower device 41, a second-stage shower device 42, and a third-stage shower device 43 in this order. Each of the shower devices 41, 42, and 43 has a plurality of shower nozzles 411, 421, and 431 arranged in the width direction of the film 1. After passing through the shower devices 41, 42, and 43, the film 1 is sent to a drain roll 5, and moisture attached to the surface is removed. Here, in the second embodiment, as in the first embodiment, the cleaning liquid 32 in the cleaning bath 31 and the cleaning liquid 32 discharged from the shower devices 41 and 42 preferably have the same or similar composition.

[0072] Furthermore, similarly to the first embodiment, the shower devices 41, 42, and 43 are configured to adjust and release the temperature and amount of the cleaning liquid according to the position in the width direction of the film 1. In the cleaning step, a cleaning treatment with the cleaning liquid 32 in the cleaning bath 31 and a cleaning treatment with the shower devices 41, 42, and 43 are performed, so that the difference in the degree of treatment that occurs between the ends and the center in the width direction of the film 1 that has been brought into contact with the cleaning liquid is made uniform, thereby reducing the variation in the optical properties of the polarizing film. Note that, also in the second embodiment, the order of the cleaning treatment of immersion treatment with the cleaning liquid 32 in the cleaning bath 31 and the cleaning treatment with the shower devices 41, 42, and 43 is not particularly limited.

[0073] In the cleaning process using the above shower devices 41, 42, and 43, as shown in Fig. 4(d), in the first-stage shower device 41, the cleaning liquid 32 is discharged from shower nozzle 411b in the portion of shower nozzle 411 that corresponds to the center of film 1, and the cleaning liquid 32 is not discharged from shower nozzles 411a and 411c in the portions that correspond to one end and the other end of film 1. Next, as shown in Fig. 4(c), in the second-stage shower device 42, the cleaning liquid 32 is discharged from shower nozzle 421c in the portion that corresponds to the other end of film 1, and the cleaning liquid 32 is not discharged from shower nozzles 421a and 421b in the portions that correspond to one end and the center of film 1. Furthermore, as shown in Fig. 4(b), in the third-stage shower device 43, the cleaning liquid 32 is discharged from shower nozzle 431a in the portion of shower nozzle 431 that corresponds to one end of film 1, and the cleaning liquid 32 is not discharged from shower nozzles 431b and 431c in the portions that correspond to one end and the center of film 1.

[0074] In the cleaning treatment using the above shower devices 41, 42, and 43, for example, the amount of cleaning liquid 32 discharged per unit width and unit time from shower nozzle 411b toward the center of film 1 in first-stage shower device 41, the amount of cleaning liquid 32 discharged per unit width and unit time from shower nozzle 421c toward the other end of film 1 in second-stage shower device 42, and the amount of cleaning liquid 32 discharged per unit width and unit time from shower nozzle 431a toward one end of film 1 in third-stage shower device 43 can be the same, for example, 1 to 20 L / m / min. The amount of cleaning liquid 32 discharged per unit width and unit time toward one end, the other end, and the center of film 1 is more preferably 3 to 10 L / m / min.

[0075] By carrying out such cleaning, the amount M1 ([L / m / min]) of cleaning liquid 32 per unit width and unit time in contact with one end of film 1 can be made larger than the amount M2 ([L / m / min]) of cleaning liquid 32 per unit width and unit time in contact with the other end of film 1, and the amount M2 can be made larger than the amount M3 ([L / m / min]) of cleaning liquid 32 per unit width and unit time in contact with the central portion of film 1, thereby satisfying the relationship M1>M2>M3. Thus, the degree of cleaning of one end of polyvinyl alcohol-based resin film 1 can be made larger than the degree of cleaning of the other end, and the degree of cleaning of the other end can be made larger than the degree of cleaning of the central portion.

[0076] This is because in the second embodiment, the film 1 is first transported vertically upward. In this transport state, the height position of the shower nozzle that discharges the cleaning liquid 32 toward the center of the film 1 is lower than the height position of the shower nozzle that discharges the cleaning liquid 32 toward the other end of the film 1, and the height position of the shower nozzle that discharges the cleaning liquid 32 toward the other end of the film 1 is lower than the height position of the shower nozzle that discharges the cleaning liquid 32 toward one end of the film 1. In this case, the distance that the cleaning liquid 32 drips on the film 1 is the longest at one end, the next longest at the other end, and the shortest at the center. As a result, the higher the height position of the shower nozzle (discharge port) that discharges the cleaning liquid 32 toward the film 1, the longer the distance that the cleaning liquid 32 drips on the film 1, and as a result, the amount of cleaning liquid 32 that comes into contact with the film 1 per unit width and per unit time can be increased. In addition, the amounts of cleaning liquid 32 per unit width and unit time (M1, M2, and M3) that come into contact with one end, the other end, and the center of the film 1 can also be controlled by adjusting the amount of cleaning liquid 32 released from the shower devices 41, 42, and 43 and adjusting the transport speed of the film 1, etc.

[0077] In the second embodiment, in order to further enhance the effect of uniforming the optical properties in the width direction of the polyvinyl alcohol-based resin film, it is preferable to increase the temperature of the cleaning liquid discharged from the shower device in the order of the third stage, the second stage, and the first stage, or to increase the amount of the cleaning liquid discharged from the shower device per unit width and unit time in the order of the third stage, the second stage, and the first stage. However, even if the temperatures and amounts of the cleaning liquid discharged from the first, second, and third stages are the same, in the second embodiment, the first stage shower device discharges the cleaning liquid to the center, the second stage shower device discharges the cleaning liquid to the other end, and the third stage shower device discharges the cleaning liquid to one end, so that the degree of cleaning of one end of the polyvinyl alcohol-based resin film can be made greater than the degree of cleaning of the other end, and the degree of cleaning of the other end can be made greater than the degree of cleaning of the central portion.

[0078] (Selection of the first and second forms) In the cleaning step, as described above, the means for providing a difference in the degree of cleaning at one end, the other end, and the center of the polyvinyl alcohol-based resin film can include a temperature difference in the cleaning liquid brought into contact with the film and a difference in the amount of the cleaning liquid brought into contact with the film per unit width and unit time. In this case, the temperature difference is generally given priority over the amount of the liquid as a means for providing a difference in the degree of cleaning. This is because providing a temperature difference in the cleaning liquid brought into contact with one end, the other end, and the center of the film makes it easier to achieve a difference in the degree of cleaning, and makes it easier to achieve uniform optical properties in the width direction of the resulting polarizing film.

[0079] Therefore, in the manufacturing method according to the present embodiment, the first form is the first option for the cleaning step, and if the cleaning step cannot be performed by the first form, the second form is recommended as a preferred management form for performing the cleaning step. Of course, it is more preferable to perform the first form as the cleaning step and provide a difference in the amount of cleaning liquid per unit width and per unit time at one end, the other end, and the center of the film by the first-stage shower device and / or the second-stage shower device, respectively, in order to further enhance the effect of uniforming the optical properties in the width direction of the polyvinyl alcohol-based resin film. It is also more preferable to perform the second form as the cleaning step and provide a difference in the temperature of the cleaning liquid that is contacted at one end, the other end, and the center of the film between the first-stage, second-stage, and third-stage shower devices, in order to further enhance the effect of uniforming the optical properties in the width direction of the polyvinyl alcohol-based resin film.

[0080] As described above, in the manufacturing method according to the present embodiment, in the cleaning step after the treatment steps (swelling step, dyeing step, crosslinking step, color complementation step, etc.), the degree of cleaning of one end of the polyvinyl alcohol-based resin film is made greater than the degree of cleaning of the other end, and the degree of cleaning of the other end is made greater than the degree of cleaning of the central portion. This makes it possible to equalize the degree of treatment between the end and central portion in the width direction of the polyvinyl alcohol-based resin film in the treatment steps, thereby reducing the variation in the optical properties in the width direction of the polarizing film.

[0081] <Other processes> The manufacturing method according to the present embodiment may include steps other than the above-mentioned treatment step and cleaning step. Examples of steps and treatments that may be added include immersion treatment in an aqueous solution that does not contain a boron compound and contains zinc chloride or the like (zinc treatment step). The zinc treatment is preferably performed after the crosslinking step.

[0082] (drying process) As another step, a drying step may be included in which the polyvinyl alcohol-based resin film is dried after the washing step. The drying method in the drying step is not particularly limited, but for example, hot air drying may be performed using a drying oven. In this case, the drying temperature is, for example, about 30 to 100°C, and the drying time is, for example, about 30 to 600 seconds. The treatment for drying the polyvinyl alcohol-based resin film may also be performed using a far-infrared heater. In this manner, a polarizing film can be produced. The thickness of the polarizing film is, for example, about 5 to 50 μm.

[0083] <Method for evaluating uniformity of optical properties in the width direction of polarizing film> Regarding the polarizing film obtained by the manufacturing method according to the present embodiment, whether or not the variation in the optical properties in the width direction has been reduced (evaluation of the uniformity of the optical properties in the width direction) can be evaluated, for example, by using the following method. First, at any position in the conveying direction of the polarizing film, the orthogonal hue b value is obtained at five points in the width direction of the position (one end, the other end, the center, the midpoint between the one end and the center, and the midpoint between the other end and the center). Next, regarding the orthogonal hue b values ​​of the above five points, the difference Δ(MAX-MIN) between the maximum value (MAX) and the minimum value (MIN) is used as an index of the uniformity of the optical properties. If the ratio (difference Δ(MAX-MIN) / maximum value (MAX)×100%) of this difference Δ(MAX-MIN) to the above maximum value (MAX) is within 40%, it is evaluated that the variation in the optical properties has been reduced, and if the ratio exceeds 40%, it is evaluated that the reduction in the variation in the optical properties is insufficient.

[0084] Here, the orthogonal hue b value can be obtained by measuring the UV-visible transmission spectrum when linearly polarized light is incident on the polarizing film set in a UV-visible spectrophotometer V-7100 manufactured by JASCO Corporation, both in the case where linearly polarized light is incident on the polarizing film in the transmission axis direction and in the case where linearly polarized light is incident on the polarizing film in the absorption axis direction. The orthogonal hue b value is calculated by software built into the UV-visible spectrophotometer V-7100 based on the UV-visible transmission spectrum value. The "b value" of the orthogonal hue b value means the b value in the Hunter Lab color system. In other words, the orthogonal hue b value corresponds to the b value of the hue of the light transmitted to the opposite surface when natural light is incident on one surface of two polarizing films stacked so that the absorption axes are perpendicular to each other.

[0085] <Polarizing film> The manufacturing method according to the present embodiment makes it possible to obtain a polarizing film in which variations in optical properties in the width direction are suppressed. The luminosity-corrected single transmittance Ty of the polarizing film is preferably 40 to 47%, more preferably 41 to 45%, in consideration of the balance with the luminosity-corrected polarization degree Py. The luminosity-corrected polarization degree Py is preferably 99.9% or more, more preferably 99.95% or more at any position in the width direction. The difference between the maximum and minimum values ​​of the luminosity-corrected polarization degree Py in the width direction is preferably 0.0015% or less, and the smaller the difference, the more preferable.

[0086] The luminosity-corrected single transmittance (Ty) and the luminosity-corrected polarization degree (Py) can be determined by the following measurement method. First, the MD transmittance and TD transmittance of the polarizing film are measured in the wavelength range of 380 to 780 nm using a spectrophotometer equipped with an integrating sphere ("V7100" manufactured by JASCO Corporation), and the luminosity-corrected single transmittance and the luminosity-corrected polarization degree (Py) are calculated using the following formula: Single layer transmittance (%) = (MD + TD) / 2 Degree of polarization (%)={(MD-TD) / (MD+TD)}×100 The single transmittance and the degree of polarization at each wavelength are calculated based on the above.

[0087] Here, "MD transmittance" refers to the transmittance when the direction of polarized light exiting the Glan-Thompson prism is parallel to the transmission axis of the polarizing film sample, and is represented as "MD" in the above formula. "TD transmittance" refers to the transmittance when the direction of polarized light exiting the Glan-Thompson prism is perpendicular to the transmission axis of the polarizing film sample, and is represented as "TD" in the above formula. Next, the above single transmittance and polarization degree are described in JIS Z 8701:1999 "Method of displaying color - XYZ color system and XYZ color system" 10 Y 10 Z 10 By performing visibility correction based on the 2-degree visual field (C light source) of the "Color Space Specification System," it is possible to obtain the visibility-corrected single transmittance (Ty) and visibility-corrected degree of polarization (Py).

[0088] The width of the polarizing film is, for example, 50 mm to 5000 mm, preferably 500 mm to 4000 mm. The obtained polarizing film may be wound up on a winding roll to form a roll, or may be directly subjected to a step of producing a polarizing plate (a step of laminating a protective film or the like on one or both sides of the polarizing film) without being wound up.

[0089] <Polarizing plate> A polarizing plate can be obtained by bonding a protective film to at least one side of the polarizing film produced as described above via an adhesive. Examples of the protective film include films made of acetylcellulose-based resins such as triacetylcellulose and diacetylcellulose; films made of polyester-based resins such as polyethylene terephthalate, polyethylene naphthalate, and polybutylene terephthalate; polycarbonate-based resin films, cycloolefin-based resin films; acrylic-based resin films; and films made of linear olefin-based resins such as polypropylene-based resins.

[0090] In order to improve the adhesion between the polarizing film and the protective film, the bonding surface of the polarizing film and / or the protective film may be subjected to a surface treatment such as a corona treatment, a flame treatment, a plasma treatment, ultraviolet irradiation, a primer coating treatment, or a saponification treatment. Examples of adhesives used for bonding the polarizing film and the protective film include active energy ray curable adhesives such as ultraviolet curable adhesives, aqueous solutions of polyvinyl alcohol resins or aqueous solutions containing crosslinking agents, and water-based adhesives such as urethane emulsion adhesives. The ultraviolet curable adhesive may be a mixture of an acrylic compound and a photoradical polymerization initiator, or a mixture of an epoxy compound and a photocationic polymerization initiator. It is also possible to use a cationic polymerizable epoxy compound in combination with a radical polymerizable acrylic compound, and use a photocationic polymerization initiator and a photoradical polymerization initiator in combination as initiators.

[0091] As described above, the manufacturing method according to the present embodiment can provide a polarizing film with reduced variations in optical properties in the width direction. A polarizing plate to which such a polarizing film is applied is useful for various display devices such as liquid crystal display devices. [Explanation of symbols]

[0092] 1 polyvinyl alcohol resin film, 2 conveying guide roll, 31 cleaning bath, 32 cleaning solution, 41, 42, 43 shower device, 411, 411a, 411b, 411c, 421, 421a, 421b, 421c, 431, 431a, 431b, 431c shower nozzle, 5 drain roll.

Claims

1. A method for producing a polarizing film from a polyvinyl alcohol-based resin film, comprising the steps of: a treatment step of treating the polyvinyl alcohol-based resin film by contacting the film with a treatment liquid; a cleaning step of contacting the polyvinyl alcohol-based resin film with a cleaning liquid to clean the film; in that order, the cleaning step is a step of dividing the polyvinyl alcohol-based resin film into one end portion including one end in the width direction of the polyvinyl alcohol-based resin film, the other end portion including the other end in the width direction, and a central portion that is more inward in the width direction than the one end portion and the other end portion, based on the width of the polyvinyl alcohol-based resin film, and cleaning the polyvinyl alcohol-based resin film by making the degree of cleaning of the one end portion greater than the degree of cleaning of the other end portion and by making the degree of cleaning of the other end portion greater than the degree of cleaning of the central portion; The washing step is carried out so as to satisfy the following i) and at least one of the following a1) and b1), The cleaning step includes providing a plurality of outlets for discharging the cleaning liquid, The cleaning liquid is continuously discharged from the discharge port toward the polyvinyl alcohol-based resin film, the cleaning step includes conveying the polyvinyl alcohol-based resin film vertically upward, and setting a height position of the outlet for releasing the cleaning liquid toward the central portion lower than height positions of the outlet for releasing the cleaning liquid toward the other end portion and the outlet for releasing the cleaning liquid toward the one end portion, and setting a height position of the outlet for releasing the cleaning liquid toward the other end portion lower than a height position of the outlet for releasing the cleaning liquid toward the one end portion, The polyvinyl alcohol-based resin film has a thickness that varies in the width direction. i) When the temperature of the cleaning liquid in contact with the one end portion is T1 [°C], the temperature of the cleaning liquid in contact with the other end portion is T2 [°C], and the temperature of the cleaning liquid in contact with the central portion is T3 [°C], T1, T2, and T3 satisfy the relationship T1>T2>T3. a1) 1≦T1-T2≦15 b1) 2≦T2-T3≦30

2. The method for producing a polarizing film according to claim 1 , wherein the cleaning step is carried out so as to satisfy the following c1): c1) 3≦T3≦25

3. The method for producing a polarizing film according to claim 1 or 2, wherein the cleaning step is carried out so as to satisfy the following ii): ii) When the unit width and the amount of the cleaning liquid per unit time in contact with the one end portion are M1 [L / m / min], the unit width and the amount of the cleaning liquid per unit time in contact with the other end portion are M2 [L / m / min], and the unit width and the amount of the cleaning liquid per unit time in contact with the central portion are M3 [L / m / min], M1, M2 and M3 satisfy the relationship M1>M2>M3.

Citation Information

Patent Citations

  • Method for producing polarizing film

    JP2013140345A

  • Method for making a polarizing film and polarizing plate

    TW201142375A