Composite plating material and its manufacturing method

By forming a composite plating film with controlled carbon particle distribution and surface treatments, the composite plating material achieves improved wear resistance and reduced carbon shedding, addressing the issues of high friction and detachment in conventional materials.

JP7564687B2Active Publication Date: 2024-10-09DOWA METALTECH CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020186993
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-11-10
Publication Date
2024-10-09
Estimated Expiration
2040-11-10

AI Technical Summary

Technical Problem

Conventional composite plating materials for sliding contact parts like switches and connectors suffer from high friction coefficients and inadequate wear resistance, leading to carbon particle detachment that can cause short circuits in electronic equipment.

Method used

A composite plating film containing carbon particles in a silver layer is formed on a material, with a silver plating film added on top, ensuring the carbon particle proportion on the surface is 20% or less, and carbon particles are partially removed through treatments like ultrasonic cleaning to minimize detachment.

Benefits of technology

The method produces a composite plating material with reduced carbon particle shedding, enhancing wear resistance and reducing the risk of short circuits, while maintaining low friction coefficients.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007564687000001
    Figure 0007564687000001
  • Figure 0007564687000002
    Figure 0007564687000002
  • Figure 0007564687000003
    Figure 0007564687000003
Patent Text Reader

Abstract

To provide a composite plated material comprising a composite plated film composed of a composite material containing carbon particles in a silver layer and formed on a material, allowing a few carbon particles to fall off therefrom, and a method of producing the same.SOLUTION: The composite plated material comprising a composite plated film composed of a composite material containing carbon particles in a silver layer and formed on a material, with a silver plating film formed on the composite plated film, is characterized in that the ratio of carbon particles on the surface of the surface layer consisting of the silver plating film and the composite plated film is 20 area% or less, and the ratio of carbon particles sticking to an adhesive tape is 10 area% or less relative to the area of the adhesive surface of the adhesive tape, when the adhesive tape with adhesion strength of 4.02 N / 10 mm is stuck to the surface of the surface layer and thereafter peeled off therefrom.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a composite plated product and a manufacturing method thereof, and more particularly to a composite plated product used as a material for sliding contact parts such as switches and connectors, and a manufacturing method thereof. [Background technology]

[0002] Conventionally, silver-plated materials have been used as materials for sliding contact parts such as switches and connectors in order to prevent oxidation of conductive materials such as copper and copper alloys due to heating during the sliding process.

[0003] However, silver plating is soft and easily worn, and generally has a high coefficient of friction, so that it is prone to peeling off due to sliding. To solve this problem, a method has been proposed in which a composite film in which graphite particles, such as carbon particles such as graphite and carbon black, which have excellent heat resistance, wear resistance, and lubricity, are dispersed in a silver matrix is ​​formed on a conductor material by electroplating to improve wear resistance (see, for example, Patent Document 1). In addition, a method has been proposed in which a plating bath containing a wetting agent suitable for dispersing graphite particles is used to produce a silver plating film containing graphite particles (see, for example, Patent Document 2). In addition, a method has been proposed in which carbon particles are coated with metal oxides or the like by a sol-gel method to increase the dispersibility of carbon particles in a composite plating solution of silver and carbon particles, and the amount of carbon particles to be composited in the plating film is increased (see, for example, Patent Document 3).

[0004] However, the composite plated materials produced by the methods of Patent Documents 1 to 3 have a problem in that they have a relatively high friction coefficient and are unable to accommodate the need to extend the life of contacts and terminals. It is therefore desirable to provide a composite plated material with even better wear resistance by increasing the carbon particle content and the proportion of carbon particles on the surface compared to the composite plated materials produced by the methods of Patent Documents 1 to 3.

[0005] As methods for producing such composite plated products, there have been proposed a method in which electroplating is performed using a cyanide-based silver plating solution to which carbon particles that have been subjected to an oxidation treatment have been added, thereby forming a film made of a composite material containing carbon particles in a silver layer on a base material (see, for example, Patent Document 4), and a method in which electroplating is performed using a silver plating solution to which carbon particles that have been subjected to an oxidation treatment have been added, thereby forming a composite plating film made of a composite material containing carbon particles in a silver layer on a base material, and then silver plating is performed to form a silver plating film on the composite plating film (see, for example, Patent Document 5). [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Japanese Patent Application Publication No. 9-7445 (paragraph number 0005-0007) [Patent Document 2] Special Publication No. 5-505853 (pages 1-2) [Patent Document 3] JP-A-3-253598 (page 2) [Patent Document 4] JP 2006-37225 A (paragraph number 0009) [Patent Document 5] JP 2007-254876 A (paragraph number 0009) Summary of the Invention [Problem to be solved by the invention]

[0007] However, if the composite plated product produced by the method of Patent Document 4 is used as a material for sliding contact parts such as switches and connectors, carbon particles from the surface layer will fall off when the composite plated product is pressed, and these fallen carbon particles may cause a short circuit in electronic devices (using those sliding contact parts, etc.).

[0008] Furthermore, even if the composite plated product produced by the method of Patent Document 5 is used as a material for sliding contact parts such as switches and connectors, the carbon particles in the surface layer cannot be sufficiently prevented from falling off when the composite plated product is pressed, and these fallen carbon particles may cause a short circuit in electronic devices (using those sliding contact parts, etc.).

[0009] In view of the above-mentioned problems in the prior art, the present invention aims to provide a composite plated material in which a composite plating film made of a composite material containing carbon particles in a silver layer is formed on a base material, and in which the carbon particles are less likely to fall off, and a method for producing the same. [Means for solving the problem]

[0010] As a result of intensive research into solving the above-mentioned problems, the inventors have found that a composite plating film made of a composite material containing carbon particles in a silver layer can be formed on a material, and a composite plated material with little carbon particle dropout can be produced by forming a composite plating film made of a composite material containing carbon particles in a silver layer on a material, forming a silver plating film on the composite plating film, and setting the proportion of carbon particles on the surface of a surface layer made of this silver plating film and composite plating film to 20 area % or less, and when an adhesive tape with an adhesive strength of 4.02 N / 10 mm is attached to the surface of the surface layer and then peeled off, the proportion of carbon particles adhering to the adhesive tape is 10 area % or less relative to the area of ​​the attached surface of the adhesive tape, and thus completing the present invention.

[0011] That is, the composite plated product according to the present invention is characterized in that a composite plating film made of a composite material containing carbon particles in a silver layer is formed on a base material, a silver plating film is formed on the composite plating film, the proportion of carbon particles on the surface of a surface layer made of this silver plating film and the composite plating film is 20 area % or less, and when an adhesive tape with an adhesive strength of 4.02 N / 10 mm is attached to the surface of the surface layer and then peeled off, the proportion of carbon particles adhered to the adhesive tape is 10 area % or less relative to the area of ​​the attached surface of the adhesive tape.

[0012] In this composite plated product, the thickness of the composite plating film is preferably 0.8 to 25 μm, and the thickness of the silver plating film is preferably 0.1 to 5 μm. The carbon content in the surface layer consisting of the silver plating film and the composite plating film is preferably 0.3 to 10 mass %, and the friction coefficient of the composite plated product is preferably 0.9 or less. Furthermore, the base material is preferably made of copper or a copper alloy, and a nickel plating film is preferably formed between the composite plating film and the base material.

[0013] In addition, the method for producing a composite plated product according to the present invention is characterized in that a composite plating film made of a composite material containing carbon particles in a silver layer is formed on a base material by electroplating using a silver plating solution to which carbon particles have been added, followed by a treatment to remove some of the carbon particles on the surface, and then a silver plating film is formed on the composite plating film after this treatment.

[0014] In this method for producing a composite plated product, the treatment for removing a portion of the carbon particles is preferably a treatment for ultrasonically cleaning the surface of the composite plated film. In this case, the ultrasonic cleaning is preferably carried out at 20 to 100 kHz for 1 to 300 seconds. Alternatively, the treatment for removing a portion of the carbon particles may be a treatment for electrolytically cleaning the surface of the composite plated film. In this case, the electrolytic cleaning is preferably carried out at 1 to 30 A / dm 2 It is preferable that the treatment is carried out at a temperature of 10 to 300 seconds. It is also preferable that the removal rate of the carbon particles by the treatment for removing a part of the carbon particles on the surface is 35 to 85%. It is also preferable that the carbon particles are graphite particles having an average particle size of 0.5 to 15 μm, and it is preferable that a nickel plating film is formed on the base material before forming a film made of a composite material.

[0015] A terminal according to the present invention is characterized in that it uses the above composite plating material as its material.

[0016] Furthermore, a method for manufacturing a terminal according to the present invention is characterized in that the above-mentioned composite plated product is bent into the shape of a terminal.

[0017] In this specification, the term "average particle size" refers to the cumulative 50% particle size (D) on a volume basis measured by a laser diffraction / scattering particle size distribution analyzer. 50 ) Effect of the Invention

[0018] According to the present invention, a composite plating film made of a composite material containing carbon particles in a silver layer is formed on a base material, and a composite plated product with little carbon particle shedding can be produced. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] In an embodiment of the composite plated product according to the present invention, a composite plating film made of a composite material containing carbon particles in a silver layer is formed on a base material, a silver plating film is formed on the composite plating film, the proportion of carbon particles on the surface of the surface layer made of this silver plating film and the composite plating film is 20 area % or less (preferably 0.1 to 20 area %, more preferably 0.2 to 18 area %), and when an adhesive tape with an adhesive strength of 4.02 N / 10 mm is attached to the surface of the surface layer and then peeled off, the proportion of carbon particles attached to the adhesive tape is 10 area % or less relative to the area of ​​the adhesive tape attachment surface (assuming that 0 area % is when no carbon particles are attached to the adhesive tape and 100 area % is when carbon particles are attached to the entire surface of the adhesive tape without gaps). If the proportion of carbon particles on the surface of the surface layer exceeds 20 area %, many carbon particles fall off from the composite plated product.

[0020] The thickness of the composite plating film is preferably 0.8 to 25 μm, and more preferably 1 to 20 μm. If the thickness of the composite plating film is less than 0.8 μm, the wear resistance of the composite plating material may be insufficient, and if it exceeds 25 μm, the amount of silver increases, and the manufacturing cost of the composite plating material increases. The thickness of the silver plating film is preferably 0.1 to 5 μm, and more preferably 0.15 to 4 μm. If the thickness of the silver plating film is less than 0.1 μm, the effect of suppressing the falling off of carbon particles is insufficient, and if it exceeds 5 μm, the amount of silver increases, and the manufacturing cost of the composite plating material increases. In order to improve the heat resistance of the composite plating material, a nickel plating film (preferably having a thickness of 0.3 to 5 μm) may be formed between the composite plating film and the material. In addition, the carbon content in the surface layer consisting of the silver plating film and the composite plating film is preferably 0.3 to 10 mass %, and more preferably 0.4 to 5 mass %, from the viewpoint of wear resistance.

[0021] The material of the composite plating material is preferably made of copper or a copper alloy. From the viewpoint of electrical conductivity and wear resistance, it is preferable to use an alloy containing at least one selected from the group consisting of Si (silicon), Fe (iron), Mg (magnesium), P (phosphorus), Ni (nickel), Sn (tin), Co (cobalt), Zn (zinc), Be (beryllium), Pb (lead), Te (tellurium), Ag (silver), Zr (zirconium), Cr (chromium), Al (aluminum) and Ti (titanium), with the remainder being Cu and unavoidable impurities. The content of Cu in this copper alloy is preferably 85% by mass or more, more preferably 92% by mass or more, most preferably 95% by mass or more, and preferably 99.95% by mass or less.

[0022] A test piece cut from an embodiment of the composite plated material according to the present invention was used as a flat test piece (evaluation sample), and a 40 mm x 10 mm x 0.2 mm Cu-Ni-Sn-P alloy plate (copper alloy plate containing 1.0 mass% Ni, 0.9 mass% Sn, 0.05 mass% P, and the remainder Cu) was indented to form a hemispherical shape with an inner radius of 1.0 mm, on which a 20 μm thick AgSb plating film containing 2 mass% Sb was formed. The AgSb plated material (Vickers hardness HV 180) thus prepared is used as an indented test piece (indenter), and a sliding wear tester is used to press the indented test piece against a flat test piece with a constant load of 2N while continuing a reciprocating sliding motion (sliding distance 10mm, sliding speed 3mm / s) to check the wear state of the flat test piece. When the wear resistance is evaluated by this, it is preferable that the material is not exposed after 3,000 reciprocating sliding motions. In addition, the force applied in the horizontal direction during the reciprocating sliding motion is measured, the average value F is calculated, and the dynamic friction coefficient (μ) between the flat test piece and the indented test piece is calculated from μ=F / N. The dynamic friction coefficient is preferably 0.9 or less, more preferably 0.01 to 0.8.

[0023] In addition, in an embodiment of the method for manufacturing a composite plated product according to the present invention, electroplating is performed using a silver plating solution containing added carbon particles, thereby forming a composite plating film made of a composite material containing carbon particles in a silver layer on a base material (preferably made of copper or a copper alloy), and then a process is performed to remove some of the carbon particles on the surface, and a silver plating film is formed on the composite plating film after this process.

[0024] In the method for producing a composite plated product, the treatment for removing a portion of the carbon particles on the surface of the composite plating film can be ultrasonic cleaning, electrolytic cleaning, high-pressure cleaning, buffing, or other treatments. It is preferable to perform ultrasonic cleaning or electrolytic cleaning of the surface of the composite plating film. In the case of ultrasonic cleaning, it is preferably performed at 20 to 100 kHz for 1 to 300 seconds, and more preferably at 25 to 50 kHz for 2 to 270 seconds. In the case of electrolytic cleaning, it is preferably performed at 1 to 30 A / dm 2It is preferable to perform the heating at 2 to 25 A / dm for 10 to 300 seconds. 2 It is more preferable that the treatment is carried out at 0.8 to 25 μm for 20 to 270 seconds. From the viewpoint of preventing the carbon particles from falling off from the composite plated product, the removal rate of the carbon particles by the treatment for removing a portion of the surface carbon particles is preferably 35 to 85%, and more preferably 40 to 80%. The thickness of the composite plating film is preferably 0.8 to 25 μm, and more preferably 1.0 to 20 μm. The thickness of the silver plating film is preferably 0.1 to 5 μm, and more preferably 0.15 to 4 μm.

[0025] From the viewpoint of wear resistance of the composite plating material, the carbon particles are preferably graphite particles, and the average particle size of the graphite particles is preferably 0.5 to 15 μm, and more preferably 1 to 10 μm. In addition, it is preferable to remove lipophilic organic substances adsorbed on the surface of the carbon particles by oxidizing the carbon particles. Examples of such lipophilic organic substances include aliphatic hydrocarbons such as alkanes and alkenes, and aromatic hydrocarbons such as alkylbenzenes. As the oxidation treatment of the carbon particles, in addition to wet oxidation treatment, dry oxidation treatment using O2 gas or the like can be used, but from the viewpoint of mass production, wet oxidation treatment is preferably used, and carbon particles with a large surface area can be uniformly treated by wet oxidation treatment. As a method of wet oxidation treatment, a method of adding an appropriate amount of oxidizing agent after suspending carbon particles in water can be used. As the oxidizing agent, nitric acid, hydrogen peroxide, potassium permanganate, potassium persulfate, sodium perchlorate, or the like can be used. It is believed that the lipophilic organic matter attached to the carbon particles is oxidized by the added oxidizing agent to a form that is easily soluble in water, and is appropriately removed from the surface of the carbon particles. In addition, by filtering and washing the carbon particles with water after the wet oxidation treatment, the effect of removing the lipophilic organic matter from the surface of the carbon particles can be further enhanced. The oxidation treatment of the carbon particles can remove lipophilic organic matter such as aliphatic hydrocarbons and aromatic hydrocarbons from the surface of the carbon particles, and according to an analysis of the 300°C heated gas, the gas generated by heating the carbon particles after the oxidation treatment at 300°C contains almost no lipophilic aliphatic hydrocarbons such as alkanes and alkenes, or lipophilic aromatic hydrocarbons such as alkylbenzenes. Even if the carbon particles after oxidation treatment contain small amounts of aliphatic or aromatic hydrocarbons, the carbon particles can be dispersed in the silver plating solution. However, it is preferable that the carbon particles do not contain any hydrocarbons with a molecular weight of 160 or more, and that the intensity of the gas evolved from the hydrocarbons in the carbon particles with a molecular weight of less than 160 when heated at 300°C (purge-and-trap gas chromatograph mass spectrometry intensity) is 5,000,000 or less.

[0026] It is preferable to use a sulfonic acid-based silver plating solution as the silver plating solution (used when forming the composite plating film and when forming the silver plating film), and this sulfonic acid-based silver plating solution contains silver ions and sulfonic acid ions in a solvent, and may contain additives such as a brightener. As the solvent for this sulfonic acid-based silver plating solution, it is preferable to use a solvent consisting of water (or mainly water), taking into consideration the solubility of (complexed) silver ions, the solubility of other components in this silver plating solution, and reducing the burden on the environment, and a mixed solvent of water and alcohol may also be used. The Ag concentration in this silver plating solution is preferably 5 to 150 g / L, more preferably 10 to 120 g / L, and most preferably 20 to 100 g / L. If the Ag concentration in the silver plating solution is less than 5 g / L, the current efficiency may be poor, and a composite plating film of the desired thickness may not be obtained. On the other hand, even if the Ag concentration in the silver plating solution is higher than 150 g / L, the plating efficiency is saturated and the cost of the silver plating solution increases. The concentration of sulfonic acid in the silver plating solution is preferably 30 to 90 g / L, more preferably 40 to 80 g / L. If the concentration of sulfonic acid in the silver plating solution is less than 30 g / L, Ag from the Ag electrode plate used as the anode during silver plating is difficult to dissolve, and the Ag concentration in the silver plating solution may decrease, resulting in a decrease in plating efficiency. On the other hand, even if the concentration of sulfonic acid in the silver plating solution is higher than 90 g / L, the plating efficiency is saturated and the cost of the silver plating solution becomes high. As the silver sulfonate contained in this sulfonic acid-based silver plating solution, silver methanesulfonate, silver alkanolsulfonate, silver phenolsulfonate, etc. can be used.

[0027] Furthermore, the amount of carbon particles added to the silver plating solution (to form a composite plating film) is preferably 10 to 100 g / L, more preferably 15 to 95 g / L, and most preferably 20 to 90 g / L. If the amount of carbon particles in the silver plating solution is less than 10 g / L, the carbon particle content in the composite plating film may not be sufficiently high, and even if the amount is more than 100 g / L, the carbon particle content in the composite plating film cannot be increased.

[0028] In addition, when forming composite plating films or silver plating films, the electric plating is performed at a current density of 0.5 to 10 A / dm 2 It is preferable to use a current of 1 to 8 A / dm 2 It is more preferable to operate at 2 to 7 A / dm 2 If the current density is too low, the formation of the composite plating film or silver plating film may be slow and inefficient, whereas if the current density is too high, the appearance of the composite plating film or silver plating film may become uneven.

[0029] The material used in the embodiment of the method for producing a composite plated material according to the present invention is preferably made of copper or a copper alloy. From the viewpoint of electrical conductivity and wear resistance, it is preferable to use an alloy containing at least one selected from the group consisting of Si (silicon), Fe (iron), Mg (magnesium), P (phosphorus), Ni (nickel), Sn (tin), Co (cobalt), Zn (zinc), Be (beryllium), Pb (lead), Te (tellurium), Ag (silver), Zr (zirconium), Cr (chromium), Al (aluminum) and Ti (titanium), with the balance being Cu and unavoidable impurities. The content of Cu in this copper alloy is preferably 85% by mass or more, more preferably 92% by mass or more, most preferably 95% by mass or more, and preferably 99.95% by mass or less.

[0030] As in the embodiment of the method for producing a composite plated product according to the present invention, by performing electroplating using a silver plating solution containing carbon particles, a film made of a composite material in which carbon particles are dispersed in a silver layer is formed on a material, and a composite plated product with a large proportion of carbon particles on the surface and excellent wear resistance can be produced. In addition, by performing a process to remove some of the carbon particles (carbon particles that are easily shed) on the surface of the film made of a composite material (preferably a process to ultrasonically clean or electrolytically clean the surface of the composite plating film) (to reduce the carbon particles that are easily shed), and then forming a silver plating film (to prevent the carbon particles from falling off), a composite plating film made of a composite material containing carbon particles in a silver layer is formed on the material, and a composite plated product with very little carbon particle falling off (when an adhesive tape with an adhesive strength of 4.02 N / 10 mm is attached to the surface of the surface layer and then peeled off, the proportion of carbon particles attached to the adhesive tape is 10 area % or less of the area of ​​the adhesive tape) can be produced.

[0031] In addition, when a terminal such as a sliding contact part (such as a switch or a connector) is manufactured using a plated material having a plating film formed on the material, there are a method of manufacturing a terminal by forming a plating film after bending the material into the shape of the terminal (manufacturing method by post-plating) and a method of manufacturing a terminal by forming a plating film on the material and bending it into the shape of the terminal (manufacturing method by pre-plating). In terms of productivity of the terminal, the manufacturing method of a terminal by pre-plating is preferable. In the manufacturing method of a terminal by pre-plating, when a terminal is manufactured while conveying a strip-shaped composite plated material by a conveying roll, carbon particles in the composite plating film adhere to the surface of the conveying roll, and the carbon particles adhered to the conveying roll may be transferred to the composite plated material, or the composite plated material may be crushed by being pressed down by a mass of carbon particles adhered to the conveying roll. However, when a terminal such as a sliding contact part is manufactured while conveying the composite plated material of the above-mentioned embodiment, it is extremely difficult for carbon particles to adhere to the surface of the roll that continuously conveys the composite plated material, and the possibility of the composite plated material being crushed by being pressed down by a mass of carbon particles is extremely small. In addition, when a terminal such as a sliding contact part manufactured from the composite plating material of the above-mentioned embodiment is used, the silver plating film on the surface of the composite plating material is worn away by sliding, but the composite plating film formed underneath it can exhibit excellent wear resistance. Furthermore, in the terminal such as a sliding contact part manufactured from the composite plating material of the above-mentioned embodiment, even if the silver plating film is worn away by sliding, few carbon particles fall off from the surface of the composite plating material, so the possibility of carbon particles falling off when inserting and removing the terminal during connection and causing a short circuit in the electronic device is extremely small. EXAMPLES

[0032] EXAMPLES Hereinafter, examples of the composite plated product and the manufacturing method thereof according to the present invention will be described in detail.

[0033] [Example 1] First, artificial graphite particles with an average particle size of 5 μm (PAG-3000 manufactured by Nippon Graphite Industries Co., Ltd.) were prepared as carbon particles. The average particle size of the carbon particles was measured using a laser diffraction / scattering particle size distribution analyzer (MT3000II manufactured by Microtrack Bell Co., Ltd.). 100 g of the carbon particles were added to 1.6 L of pure water, and the mixed solution was heated to 50° C. while being stirred. 25 mL of an aqueous solution containing 3.3 g of potassium hydroxide was added to the mixed solution, and the solution was stirred for 5 minutes. Next, 0.6 L of an aqueous solution containing 34 g of potassium persulfate as an oxidizing agent was gradually added to the mixed solution, and the solution was stirred for 2 hours to perform an oxidation treatment, after which the solution was filtered through filter paper and washed with water. Hydrophobic substances such as hydrocarbons attached to the carbon particles were removed by such an oxidation treatment.

[0034] In addition, a 0.2 mm thick plate material made of a Cu-Ni-Sn-P alloy (a copper alloy plate material containing 1.0 mass% Ni, 0.9 mass% Sn, 0.05 mass% P, with the remainder being Cu) (NB109EH manufactured by DOWA Metaltech Co., Ltd.) was prepared as a material. This material was used as the cathode and the Ni electrode plate was used as the anode in a nickel plating bath consisting of an aqueous solution containing nickel sulfamate and 45 g / L of boric acid (nickel concentration 80 g / L) while stirring at 450 rpm with a magnetic stirrer (REXIM RS-1DN manufactured by AS ONE Corporation, a cross stirrer with a width of 38.1 mm and a height of 15.8 mm) at a liquid temperature of 55°C and a current density of 6 A / dm 2 Electroplating (Ni plating) was performed at 4000 K for 43 seconds to form a Ni plating film as a base layer on the material. The thickness of this Ni plating film was measured with a fluorescent X-ray thickness meter (FT110A manufactured by Hitachi High-Tech Science Corporation) and found to be 0.5 μm.

[0035] Next, the material with the Ni plating film formed was used as the cathode, and the titanium platinum mesh electrode plate (a titanium mesh material plated with platinum) was used as the anode. The material was placed in a sulfonic acid-based (non-cyanide) Ag strike plating solution (Dynasilver GPE-ST manufactured by Daiwa Kasei Co., Ltd.) containing sulfonic acid as a complexing agent, and the solution temperature was set at 25°C, with a current density of 5A / dm2, while stirring at 450 rpm. 2Electroplating (Ag strike plating) was carried out at 400° C. for 60 seconds.

[0036] In addition, the carbon particles that had been subjected to the above-mentioned oxidation treatment were added to a sulfonic acid-based (non-cyanide) silver plating solution (Dynesilver GPE-PL, manufactured by Daiwa Kasei Co., Ltd.) containing sulfonic acid as a complexing agent and having an Ag concentration of 30 g / L, and the mixture was stirred to disperse (suspend) the particles, thereby preparing a sulfonic acid-based silver plating solution containing 50 g / L of carbon particles and 30 g / L of Ag.

[0037] Next, the Ag strike-plated material was used as the cathode and the Ag electrode plate was used as the anode, and the plating was performed at a temperature of 25°C, a current density of 3 A / dm in the sulfonic acid-based silver plating solution containing the carbon particles, while stirring at 450 rpm. 2 Electroplating was performed for 115 seconds at 1000 K for 115 seconds to form a composite plating film (Ag-C plating film) containing carbon particles in the silver plating layer on the material. The thickness of this composite plating film (within a 0.2 mm diameter area at the center) was measured with a fluorescent X-ray thickness gauge (FT110A manufactured by Hitachi High-Tech Science Corporation) and found to be 2.3 μm. Note that it is difficult to detect the C atoms of the carbon particles with a fluorescent X-ray thickness gauge, so the thickness of the film was determined by detecting Ag atoms, and this thickness is referred to as the thickness of the composite plating film (Ag-C plating film) in this specification.

[0038] Next, this composite plating film was ultrasonically cleaned in pure water at 28 kHz for 240 seconds using an ultrasonic cleaner (USK-5 manufactured by AS ONE Corporation) to remove some of the carbon particles on the surface, and then washed with pure water and dried with an air blower to produce a composite plating film-forming material. Note that by observing the surface of this composite plating film-forming material, the proportion of the area occupied by carbon particles on the surface of this composite plating film (from which some of the carbon particles on the surface had been removed) (area ratio (area%)) was calculated. The area ratio of carbon particles on the surface of this composite plating film (with some of the carbon particles on the surface removed) was calculated as the ratio Y / X, where Y is the number of pixels in the carbon particle part to X is the number of pixels in the entire image, by binarizing the backscattered electron composition (BSE) image (1000x magnification) obtained from the backscattered electron detector by irradiating the surface of the test piece with an electron beam at an accelerating voltage of 5kV using a tabletop electron microscope (TM4000Plus, Hitachi High-Technologies Corporation) (given the highest brightness of all pixels as 255 and the lowest brightness as 0, so that pixels with a brightness of 127 or less are black and pixels with a brightness of more than 127 are white) using an image analysis application (image editing and processing software GIMP2.10.12), and separating the image into silver parts (white parts) and carbon particle parts (black parts). As a result, the ratio (area ratio) of the area occupied by carbon particles on the surface of the composite plating film (with some of the carbon particles on the surface removed) was 12.1% by area. In addition, when the proportion of the area occupied by carbon particles on the surface of the composite plating film was calculated using the same method for the composite plating film forming material before the treatment to remove a portion of the surface carbon particles, it was 48.3 area%, and the change in the area ratio due to the treatment to remove a portion of the surface carbon particles was 36.2 area % (= 48.3 area % - 12.1 area %), and the rate of change in the area ratio (carbon particle removal rate due to the treatment to remove a portion of the surface carbon particles) was 74.9% (= (48.3 - 12.1) area % × 100 / 48.3 area %).

[0039] Next, the composite plating film forming material (with some of the carbon particles on the surface removed) was used as the cathode and the Ag electrode plate was used as the anode. The plating was performed in a sulfonic acid-based (non-cyanide-based) silver plating solution (Dynesilver GPE-PL manufactured by Daiwa Kasei Co., Ltd.) containing sulfonic acid as a complexing agent and having an Ag concentration of 30 g / L, with stirring at 450 rpm at a temperature of 25°C and a current density of 3 A / dm. 2 Electroplating was performed for 95 seconds at 1000 K for 95 seconds, and a silver plating film was formed on the composite plating film (from which some of the carbon particles on the surface had been removed) to produce a composite plating material. The total thickness of the composite plating film (from which some of the carbon particles on the surface had been removed) and the silver plating film (within a 0.2 mm diameter range at the center) of this composite plating material was measured using a fluorescent X-ray thickness meter (FT110A manufactured by Hitachi High-Tech Science Co., Ltd.), and the thickness of the silver plating film was calculated by subtracting the thickness of the composite plating film (from which some of the carbon particles on the surface had been removed), resulting in a thickness of 1.9 μm. The area ratio of the carbon particles on the surface of this composite plating material was determined by the same method as above, and was found to be 0.9 area %.

[0040] Samples (5mm x 5mm, weighing about 5g) cut out from the composite plating material (including the base material) thus obtained were prepared for the analysis of Ag and C, and one sample was dissolved to determine the silver content (X% by mass) in the sample using an inductively coupled plasma optical emission spectrometer (ICP-OES) (SPS5100, Hitachi High-Tech Science Co., Ltd.), while the carbon content (Y% by mass) in the other sample was determined by infrared absorption using a trace carbon / sulfur analyzer (EMIA-810W, Horiba, Ltd.), and the carbon content in the surface layer consisting of the silver plating film and the composite plating film was calculated as Y / (X+Y), which was 0.6% by mass. Note that the plate material made of Cu-Ni-Sn-P alloy did not contain Ag and C or contained only trace amounts of them, so the carbon content in the surface layer was calculated on the assumption that they did not contain Ag and C.

[0041] In addition, a 40 mm × 10 mm × 0.2 mm Cu-Ni-Sn-P alloy plate (copper alloy plate containing 1.0 mass% Ni, 0.9 mass% Sn, 0.05 mass% P, with the remainder being Cu) (NB109EH manufactured by DOWA Metaltech Co., Ltd.) was indented to form a hemispherical shape with an inner radius of 1.0 mm to prepare a material. This material was then plated in an AgSb plating solution (a solution containing 60 g / L silver and 100 g / L sodium cyanide with Nissin Bright N (manufactured by Nisshin Seiki Co., Ltd.) at a solution temperature of 15°C and a current density of 1.5 A / dm 2 For 1,800 seconds, electroplating (Ag-Sb plating) was performed at 400° C. for 1,800 seconds to produce an AgSb-plated material having a 20 μm-thick Ag-Sb plating film containing 2 mass % Sb (Vickers hardness HV of 180).

[0042] A test piece cut from the above composite plated material was used as a flat test piece (evaluation sample), and the above AgSb plated material was used as an indented test piece (indenter). Using a sliding wear tester (CRS-G2050-DWA manufactured by Yamazaki Seiki Kenkyusho Co., Ltd.), the indented test piece was pressed against the flat test piece with a constant load of 2N (i.e., the normal force was kept at 2N) while performing a reciprocating sliding motion (sliding distance 10mm, sliding speed 3mm / s) 3,000 times to check the wear state of the flat test piece, and wear resistance was evaluated. As a result, after 3,000 reciprocating sliding motions, there was no exposure of the material, indicating that the material has excellent wear resistance. In addition, the horizontal force F applied at the center of each of the 3,000 reciprocating sliding movements was measured, and the dynamic friction coefficient (μ) between the flat test piece and the indented test piece was calculated from μ = F / N (N is the normal force), and the average value was 0.7.

[0043] In addition, the average contact resistance measured by the four-terminal method when the contact had traveled half the forward sliding distance during the 3,000 reciprocating sliding operations was found to be low at 1.4 mΩ.

[0044] In addition, an adhesive tape (Cellotape (registered trademark) CT-18 (adhesive strength 4.02 N / 10 mm) manufactured by Nichiban Co., Ltd.) was attached to the surface of the obtained composite plated product, and the adhesive tape was then peeled off. The carbon particles attached to the adhesive tape were observed at 1000 times (field of view 143 μm × 110 μm) using a laser microscope (VK-X100 manufactured by Keyence Co., Ltd.). The image was binarized using an image analysis application (image editing and processing software GIMP 2.10.12) (where the highest brightness of all pixels is 255 and the lowest brightness is 0, so that pixels with a brightness of 160 or less are black and pixels with a brightness of more than 160 are white), and the adhesive tape part (white part) and the carbon particle part (black part) were separated, and the ratio Y / X of the number of pixels Y of the carbon particle part to the number of pixels X of the entire image was calculated as the area ratio occupied by carbon in the field of view (carbon deposition rate). As a result, the carbon deposition rate was 0.9 area %.

[0045] [Example 2] A composite plated material was obtained in the same manner as in Example 1, except that no nickel plating film was formed as a base layer, artificial graphite particles with an average particle size of 3 μm (PAG-4500 manufactured by Nippon Graphite Industries Co., Ltd.) were used as the carbon particles, the electroplating time when forming the composite plating film was 275 seconds, and the electroplating time when forming the silver plating film was 25 seconds.

[0046] For the obtained composite plated material, the thicknesses of the composite plating film (Ag-C plating film) and the silver plating film were measured using the same method as in Example 1. The thickness of the composite plating film was 5.5 μm, and the thickness of the silver plating film was 0.5 μm.

[0047] The area ratio (area ratio) of the carbon particles on the surface of the composite plating film was calculated for the obtained composite plating material by the same method as in Example 1. As a result, the area ratio was 23.0 area%, the area ratio (area ratio) of the carbon particles on the surface of the composite plating film before the treatment to remove a portion of the carbon particles on the surface was 61.9 area%, the change in the area ratio due to the treatment to remove a portion of the carbon particles on the surface was 38.9 area% (=61.9 area%-23.0 area%), and the change rate of the area ratio (carbon particle removal rate due to the treatment to remove a portion of the carbon particles on the surface) was 62.8% (=(61.9-23.0) area% x 100 / 61.9 area%). The area ratio of the carbon particles on the surface of the surface layer of this composite plating material was calculated by the same method as in Example 1 and was 12.0 area%.

[0048] Furthermore, for the obtained composite plated product, the carbon content in the surface layer consisting of the silver plating film and the composite plating film was calculated by the same method as in Example 1, and was found to be 1.8 mass %.

[0049] The abrasion resistance of the obtained composite plated material was evaluated by the same method as in Example 1, and the average dynamic friction coefficient was calculated, and the average contact resistance was obtained. As a result, there was no exposure of the material after 3,000 reciprocating sliding operations, and it was found that the abrasion resistance was excellent. The average dynamic friction coefficient was 0.3, and the average contact resistance was low at 1.0 mΩ.

[0050] Furthermore, for the resulting composite plated product, the carbon deposition rate was calculated in the same manner as in Example 1, and was found to be 0.1% by area.

[0051] [Example 3] The amount of carbon particles added to the silver plating solution used to form the composite plating film was 80g / L, the electroplating time for forming the composite plating film was 245 seconds, and the electroplating time for forming the silver plating film was 70 seconds. Instead of ultrasonic cleaning, an anode plate made of SUS304 was used in an electrolyte solution in which 10% by mass of a degreasing cleaner (BONDERITE C-AK PZ manufactured by Henkel Japan Co., Ltd.) was dissolved in pure water. The material on which the composite plating film was formed was used as the cathode plate, and the plating was conducted at 5A / dm 2 A composite plated product was produced in the same manner as in Example 1, except that the product was subjected to electrolytic cleaning at 0.5 V for 30 seconds to remove some of the carbon particles on the surface.

[0052] For the obtained composite plated material, the thicknesses of the composite plating film (Ag-C plating film) and the silver plating film were measured using the same method as in Example 1. The thickness of the composite plating film was 4.9 μm, and the thickness of the silver plating film was 1.4 μm.

[0053] The area ratio (area ratio) of the carbon particles on the surface of the composite plating film was calculated for the obtained composite plating material by the same method as in Example 1. As a result, the area ratio was 26.1 area%, the area ratio (area ratio) of the carbon particles on the surface of the composite plating film before the treatment to remove a portion of the carbon particles on the surface was 60.0 area%, the change in the area ratio due to the treatment to remove a portion of the carbon particles on the surface was 33.9 area% (=60.0 area%-26.1 area%), and the change rate of the area ratio (carbon particle removal rate due to the treatment to remove a portion of the carbon particles on the surface) was 56.5% (=(60.0-26.1) area% x 100 / 60.0 area%). The area ratio of the carbon particles on the surface of the surface layer of this composite plating material was calculated by the same method as in Example 1 and was 2.0 area%.

[0054] Furthermore, for the obtained composite plated product, the carbon content in the surface layer consisting of the silver plating film and the composite plating film was calculated by the same method as in Example 1, and was found to be 1.5 mass %.

[0055] The abrasion resistance of the obtained composite plated material was evaluated in the same manner as in Example 1, and the average dynamic friction coefficient was calculated, and the average contact resistance was obtained. As a result, after 3,000 reciprocating sliding operations, there was no exposure of the material, and it was found that the abrasion resistance was excellent. The average dynamic friction coefficient was 0.3, and the average contact resistance was low at 1.3 mΩ.

[0056] Furthermore, the carbon deposition rate of the obtained composite plated product was calculated by the same method as in Example 1, and was found to be 0 area %.

[0057] [Example 4] The nickel plating film was not formed as a base layer, and the electroplating time for forming the composite plating film was set to 245 seconds. The current density for forming the silver plating film was set to 6A / dm 2 A composite plated material was obtained in the same manner as in Example 1, except that the electroplating time was 90 seconds.

[0058] For the obtained composite plated material, the thicknesses of the composite plating film (Ag-C plating film) and the silver plating film were measured using the same method as in Example 1. The thickness of the composite plating film was 4.9 μm, and the thickness of the silver plating film was 3.5 μm.

[0059] The area ratio (area ratio) of the carbon particles on the surface of the composite plating film was calculated for the obtained composite plating material by the same method as in Example 1. As a result, the area ratio was 30.1 area%, the area ratio (area ratio) of the carbon particles on the surface of the composite plating film before the treatment to remove a portion of the carbon particles on the surface was 63.4 area%, the change in the area ratio due to the treatment to remove a portion of the carbon particles on the surface was 33.3 area% (=63.4 area%-30.1 area%), and the change rate of the area ratio (carbon particle removal rate due to the treatment to remove a portion of the carbon particles on the surface) was 52.5% (=(63.4-30.1) area% x 100 / 63.4 area%). The area ratio of the carbon particles on the surface of the surface layer of this composite plating material was calculated by the same method as in Example 1 and was 0.4 area%.

[0060] Furthermore, for the obtained composite plated product, the carbon content in the surface layer consisting of the silver plating film and the composite plating film was calculated by the same method as in Example 1, and was found to be 1.2 mass %.

[0061] The abrasion resistance of the obtained composite plated material was evaluated in the same manner as in Example 1, and the average dynamic friction coefficient was calculated, and the average contact resistance was determined. As a result, there was no exposure of the material after 3,000 reciprocating sliding operations, and it was found that the abrasion resistance was excellent. The average dynamic friction coefficient was 0.3, and the average contact resistance was low at 1.2 mΩ.

[0062] Furthermore, for the resulting composite plated product, the carbon deposition rate was calculated in the same manner as in Example 1, and was found to be 0.1% by area.

[0063] [Example 5] The amount of Ag in the silver plating solution (with carbon particles added) used to form the composite plating film without forming a nickel plating film as a base layer was set to 80 g / L, and the current density when forming the composite plating film was set to 6 A / dm 2 A composite plated material was obtained in the same manner as in Example 1, except that the electroplating time was 260 seconds.

[0064] For the obtained composite plated material, the thicknesses of the composite plating film (Ag-C plating film) and the silver plating film were measured using the same method as in Example 1. The thickness of the composite plating film was 10.6 μm, and the thickness of the silver plating film was 1.9 μm.

[0065] The area ratio (area ratio) of the carbon particles on the surface of the composite plating film was calculated for the obtained composite plating material by the same method as in Example 1. As a result, the area ratio was 29.0 area%, the area ratio (area ratio) of the carbon particles on the surface of the composite plating film before the treatment to remove a portion of the carbon particles on the surface was 67.9 area%, the change in the area ratio due to the treatment to remove a portion of the carbon particles on the surface was 38.9 area% (=67.9 area%-29.0 area%), and the change rate of the area ratio (carbon particle removal rate due to the treatment to remove a portion of the carbon particles on the surface) was 57.3% (=(67.9-29.0) area% x 100 / 67.9 area%). The area ratio of the carbon particles on the surface of the surface layer of this composite plating material was calculated by the same method as in Example 1 and was 2.2 area%.

[0066] Furthermore, for the obtained composite plated product, the carbon content in the surface layer consisting of the silver plating film and the composite plating film was calculated by the same method as in Example 1, and was found to be 1.5 mass %.

[0067] The composite plated material was evaluated for wear resistance by the same method as in Example 1, and the average dynamic friction coefficient was calculated, and the average contact resistance was determined. As a result, there was no exposure of the material after 3,000 reciprocating sliding operations, and it was found to have excellent wear resistance. The average dynamic friction coefficient was 0.4, and the average contact resistance was low at 1.0 mΩ.

[0068] Furthermore, the carbon deposition rate of the obtained composite plated product was calculated in the same manner as in Example 1, and was found to be 1.1% by area.

[0069] [Example 6] A composite plated material was obtained in the same manner as in Example 1, except that a nickel plating film was not formed as a base layer, the amount of carbon particles added to the silver plating solution used to form the composite plating film was 30 g / L, the electroplating time to form the composite plating film was 900 seconds, and the electroplating time to form the silver plating film was 45 seconds.

[0070] For the obtained composite plated material, the thicknesses of the composite plating film (Ag-C plating film) and the silver plating film were measured using the same method as in Example 1. The thickness of the composite plating film was 18.0 μm, and the thickness of the silver plating film was 0.9 μm.

[0071] The area ratio (area ratio) of the carbon particles on the surface of the composite plating film was calculated for the obtained composite plating material by the same method as in Example 1. As a result, the area ratio was 27.1 area%, the area ratio (area ratio) of the carbon particles on the surface of the composite plating film before the treatment to remove a portion of the carbon particles on the surface was 72.6 area%, the change in the area ratio due to the treatment to remove a portion of the carbon particles on the surface was 45.5 area% (=72.6 area%-27.1 area%), and the change rate of the area ratio (carbon particle removal rate due to the treatment to remove a portion of the carbon particles on the surface) was 62.7% (=(72.6-27.1) area% x 100 / 72.6 area%). The area ratio of the carbon particles on the surface of the surface layer of this composite plating material was calculated by the same method as in Example 1 and was 4.4 area%.

[0072] Furthermore, for the obtained composite plated product, the carbon content in the surface layer consisting of the silver plating film and the composite plating film was calculated by the same method as in Example 1, and was found to be 2.4 mass %.

[0073] The composite plated material was evaluated for wear resistance by the same method as in Example 1, and the average dynamic friction coefficient was calculated, and the average contact resistance was determined. As a result, there was no exposure of the material after 3,000 reciprocating sliding operations, and it was found to have excellent wear resistance. The average dynamic friction coefficient was 0.3, and the average contact resistance was low at 1.1 mΩ.

[0074] Furthermore, the carbon deposition rate of the obtained composite plated product was calculated in the same manner as in Example 1, and was found to be 0.8 area %.

[0075] [Example 7] A composite plated material was obtained in the same manner as in Example 1, except that a nickel plating film was not formed as a base layer, the electroplating time for forming the composite plating film was 260 seconds, and the electroplating time for forming the silver plating film was 10 seconds.

[0076] The thicknesses of the composite plating film (Ag-C plating film) and the silver plating film of the obtained composite plated material were determined using the same method as in Example 1, and the thickness of the composite plating film was 5.2 μm and the thickness of the silver plating film was 0.2 μm.

[0077] The area ratio (area ratio) of the carbon particles on the surface of the composite plating film was calculated for the obtained composite plating material by the same method as in Example 1. As a result, the area ratio was 26.3 area%, the area ratio (area ratio) of the carbon particles on the surface of the composite plating film before the treatment to remove a portion of the carbon particles on the surface was 63.1 area%, the change in the area ratio due to the treatment to remove a portion of the carbon particles on the surface was 36.8 area% (=63.1 area%-26.3 area%), and the change rate of the area ratio (carbon particle removal rate due to the treatment to remove a portion of the carbon particles on the surface) was 58.3% (=(63.1-26.3) area% x 100 / 63.1 area%). The area ratio of the carbon particles on the surface of the surface layer of this composite plating material was calculated by the same method as in Example 1 and was 17.2 area%.

[0078] Furthermore, for the obtained composite plated product, the carbon content in the surface layer consisting of the silver plating film and the composite plating film was calculated by the same method as in Example 1, and was found to be 1.9 mass %.

[0079] The abrasion resistance of the obtained composite plated material was evaluated in the same manner as in Example 1, and the average dynamic friction coefficient was calculated, and the average contact resistance was obtained. As a result, after 3,000 reciprocating sliding operations, there was no exposure of the material, and it was found that the abrasion resistance was excellent. The average dynamic friction coefficient was 0.3, and the average contact resistance was low at 1.3 mΩ.

[0080] Furthermore, for the resulting composite plated product, the carbon deposition rate was calculated in the same manner as in Example 1, and was found to be 3.6 area %.

[0081] [Example 8] A composite plated material was obtained in the same manner as in Example 1, except that no nickel plating film was formed as a base layer, flake graphite particles (UTC-1 manufactured by Nippon Graphite Industries Co., Ltd.) having an average particle size of 2.3 μm were used as the carbon particles, the electroplating time when forming the composite plating film was 75 seconds, and the electroplating time when forming the silver plating film was 25 seconds.

[0082] For the obtained composite plated material, the thicknesses of the composite plating film (Ag-C plating film) and the silver plating film were measured using the same method as in Example 1. The thickness of the composite plating film was 1.5 μm, and the thickness of the silver plating film was 0.5 μm.

[0083] The area ratio (area ratio) of the carbon particles on the surface of the composite plating film was calculated for the obtained composite plating material by the same method as in Example 1. As a result, the area ratio was 18.1 area%, the area ratio (area ratio) of the carbon particles on the surface of the composite plating film before the treatment to remove a portion of the carbon particles on the surface was 52.4 area%, the change in the area ratio due to the treatment to remove a portion of the carbon particles on the surface was 34.3 area% (=52.4 area%-18.1 area%), and the change rate of the area ratio (carbon particle removal rate due to the treatment to remove a portion of the carbon particles on the surface) was 65.5% (=(52.4-18.1) area% x 100 / 52.4 area%). The area ratio of the carbon particles on the surface of the surface layer of this composite plating material was calculated by the same method as in Example 1 and was 7.5 area%.

[0084] Furthermore, for the obtained composite plated product, the carbon content in the surface layer consisting of the silver plating film and the composite plating film was calculated by the same method as in Example 1, and was found to be 0.5 mass %.

[0085] The abrasion resistance of the obtained composite plated material was evaluated by the same method as in Example 1, and the average dynamic friction coefficient was calculated and the average contact resistance was obtained. As a result, there was no exposure of the material after 3,000 reciprocating sliding operations, and it was found that the abrasion resistance was excellent. The average dynamic friction coefficient was 0.3, and the average contact resistance was low at 0.8 mΩ.

[0086] Furthermore, the carbon deposition rate of the obtained composite plated product was calculated in the same manner as in Example 1, and was found to be 0.3 area %.

[0087] [Comparative Example 1] A composite plated material was produced in the same manner as in Example 1, except that a nickel plating film was not formed as a base layer, the electroplating time for forming the composite plating film was 260 seconds, the electroplating time for forming the silver plating film was 80 seconds, and ultrasonic cleaning was not performed.

[0088] For the obtained composite plated material, the thicknesses of the composite plating film (Ag-C plating film) and the silver plating film were measured using the same method as in Example 1. The thickness of the composite plating film was 5.2 μm, and the thickness of the silver plating film was 1.6 μm.

[0089] The proportion of the area occupied by the carbon particles on the surface of the composite plating film of the obtained composite plated product (area ratio) was calculated using the same method as in Example 1. As a result, the area ratio of the composite plated product (wherein the treatment to remove a portion of the carbon particles on the surface was not performed) was 60.3 area %. The area ratio of the carbon particles on the surface of the surface layer of this composite plated product was also determined using the same method as in Example 1 and was 31.0 area %.

[0090] Furthermore, for the obtained composite plated product, the carbon content in the surface layer consisting of the silver plating film and the composite plating film was calculated by the same method as in Example 1, and was found to be 1.7 mass %.

[0091] The composite plated material was evaluated for wear resistance by the same method as in Example 1, and the average dynamic friction coefficient was calculated, and the average contact resistance was determined. As a result, there was no exposure of the material after 3,000 reciprocating sliding operations, and it was found to have excellent wear resistance. The average dynamic friction coefficient was 0.4, and the average contact resistance was low at 0.8 mΩ.

[0092] Furthermore, the carbon deposition rate of the obtained composite plated product was calculated in the same manner as in Example 1, and was found to be 20 area %.

[0093] [Comparative Example 2] A silver-plated material was produced in the same manner as in Example 1, except that a nickel plating film as a base layer and a composite plating film (Ag-C plating film) were not formed, the electroplating time for forming the silver plating film was 1100 seconds, and ultrasonic cleaning was not performed.

[0094] For the obtained silver-plated product, the thickness of the silver plating film was measured in the same manner as in Example 1, and was found to be 22.0 μm.

[0095] The wear resistance of the obtained silver-plated material was evaluated by the same method as in Example 1, and the average dynamic friction coefficient was calculated and the average contact resistance was obtained. As a result, after 3,000 reciprocating sliding operations, the material was exposed, and it was found that the wear resistance was poor. The average dynamic friction coefficient was 1.3, and the average contact resistance was low at 1.1 mΩ.

[0096] Furthermore, the carbon deposition rate of the obtained silver-plated product was calculated by the same method as in Example 1, and was found to be 0 area %.

[0097] [Comparative Example 3] A composite plated material was prepared in the same manner as in Example 1, except that no nickel plating film or silver plating film was formed as a base layer, the electroplating time for forming the composite plating film (Ag-C plating film) was set to 270 seconds, and ultrasonic cleaning was not performed.

[0098] For the obtained composite plated product, the thickness of the composite plating film (Ag-C plating film) was measured by the same method as in Example 1, and was found to be 5.4 μm.

[0099] Furthermore, for the obtained composite plated product, the proportion of the area occupied by the carbon particles on the surface of the composite plating film (area ratio) was calculated by the same method as in Example 1. As a result, the area ratio of the composite plated product (wherein the treatment to remove a portion of the carbon particles on the surface was not performed) was 62.0 area %.

[0100] Furthermore, for the obtained composite plated product, the carbon content in the surface layer consisting of the composite plating film was calculated by the same method as in Example 1, and was found to be 2.4 mass %.

[0101] The composite plated material was evaluated for wear resistance by the same method as in Example 1, and the average dynamic friction coefficient was calculated, and the average contact resistance was determined. As a result, there was no exposure of the material after 3,000 reciprocating sliding operations, and it was found to have excellent wear resistance. The average dynamic friction coefficient was 0.3, and the average contact resistance was low at 1.4 mΩ.

[0102] Furthermore, for the resulting composite plated product, the carbon deposition rate was calculated in the same manner as in Example 1, and was found to be 82 area %.

[0103] [Comparative Example 4] A composite plated material was prepared in the same manner as in Example 1, except that no nickel plating film or silver plating film was formed as a base layer, and the electroplating time for forming the composite plating film (Ag-C plating film) was set to 235 seconds.

[0104] For the obtained composite plated product, the thickness of the composite plating film (Ag-C plating film) was measured by the same method as in Example 1, and was found to be 4.7 μm.

[0105] Furthermore, for the obtained composite plated material, the proportion of the area occupied by the carbon particles on the surface of the composite plating film (area ratio) was calculated by the same method as in Example 1. As a result, the area ratio was 36.4 area%, the proportion of the area occupied by the carbon particles on the surface of the composite plating film (area ratio) before the treatment to remove a portion of the carbon particles on the surface was 68.7 area%, the change in the area ratio due to the treatment to remove a portion of the carbon particles on the surface was 32.3 area % (= 68.7 area % - 36.4 area %), and the rate of change in the area ratio (carbon particle removal rate due to the treatment to remove a portion of the carbon particles on the surface) was 47.0% (= (68.7 - 36.4) area % × 100 / 68.7 area %).

[0106] Furthermore, for the obtained composite plated product, the carbon content in the surface layer consisting of the composite plating film was calculated by the same method as in Example 1, and was found to be 2.0 mass %.

[0107] The abrasion resistance of the obtained composite plated material was evaluated by the same method as in Example 1, and the average dynamic friction coefficient was calculated and the average contact resistance was obtained. As a result, there was no exposure of the material after 3,000 reciprocating sliding operations, and it was found that the abrasion resistance was excellent. The average dynamic friction coefficient was 0.3, and the average contact resistance was low at 0.8 mΩ.

[0108] Furthermore, the carbon deposition rate of the obtained composite plated product was calculated by the same method as in Example 1, and was found to be 13% area.

[0109] Tables 1 to 3 show the manufacturing conditions and properties of the plated materials of these examples and comparative examples.

[0110] [Table 1]

[0111] [Table 2]

[0112]

Table 3

Claims

1. A composite plating material comprising: a composite plating film made of a composite material containing carbon particles in a silver layer formed on a base material; a silver plating film having a thickness of 0.1 to 1.9 μm formed on the composite plating film; a surface layer made of the silver plating film and the composite plating film having a proportion of carbon particles on the surface of the surface layer consisting of the silver plating film and the composite plating film of 17.2 area % or less; and when an adhesive tape having an adhesive strength of 4.02 N / 10 mm is attached to the surface of the surface layer and then peeled off, the proportion of carbon particles attached to the adhesive tape is 10 area % or less relative to the area of ​​the attached surface of the adhesive tape.

2. 2. The composite plated product according to claim 1, wherein the thickness of the composite plated film is 0.8 to 25 μm.

3. 3. The composite plated material according to claim 1, wherein a carbon content in a surface layer consisting of said composite plating film and said silver plating film is 0.3 to 10 mass %.

4. 4. The composite plated product according to claim 1, wherein the composite plated product has a friction coefficient of 0.9 or less.

5. 5. The composite plated product according to claim 1, wherein the base material is made of copper or a copper alloy.

6. 6. The composite plated product according to claim 1, further comprising a nickel plating film formed between said composite plating film and said base material.

7. A method for producing a composite plated product, comprising the steps of: performing electroplating using a silver plating solution containing added carbon particles to form a composite plating film on a base material, the composite plating film being made of a composite material containing carbon particles in a silver layer; performing a treatment to remove some of the carbon particles on the surface; and forming a silver plating film on the composite plating film after this treatment.

8. 8. The method for producing a composite plated product according to claim 7, wherein the treatment for removing a portion of the carbon particles is a treatment for ultrasonically cleaning the surface of the composite plating film.

9. 9. The method for producing a composite plated product according to claim 8, wherein the ultrasonic cleaning is carried out at 20 to 100 kHz for 1 to 300 seconds.

10. 8. The method for producing a composite plated product according to claim 7, wherein the treatment for removing a portion of the carbon particles is a treatment for electrolytically cleaning the surface of the composite plating film.

11. The electrolytic cleaning is performed at 1 to 30 A / dm 2 The method for producing a composite plated product according to claim 10, wherein the plating is performed at a temperature of from 10 to 300 seconds.

12. 12. The method for producing a composite plated product according to claim 7, wherein a removal rate of carbon particles by the treatment for removing a portion of the surface carbon particles is 35 to 85%.

13. 13. The method for producing a composite plated product according to claim 7, wherein the carbon particles are graphite particles having an average particle size of 0.5 to 15 μm.

14. The method for producing a composite plated product according to any one of claims 7 to 13, further comprising forming a nickel plating film on the base material before forming the film made of the composite material.

15. A terminal, characterized in that the composite plating material according to any one of claims 1 to 6 is used as a material.

16. A method for manufacturing a terminal, comprising bending the composite plated product according to any one of claims 1 to 6 into a shape of a terminal.

Citation Information

Patent Citations

  • Dispersion plating method

    JP1991253598A

  • Method for forming silver-graphite dispersion coating

    JP1993505853A

  • Sliding contact of electric equipment

    JP1997007445A

  • Composite plated material and method for producing same

    JP2006037225A

  • Composite plating material and method of manufacturing the same

    JP2007254876A