Medical device and its manufacturing method
A medical device with a hydrophilic copolymer and hyaluronic acid-based surface lubricating layer addresses high friction in narrow body lumens, ensuring durable lubricity and smooth operation.
Patent Information
- Application Number
- JP2021540985
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-08-21
- Filing Date
- 2020-08-21
- Publication Date
- 2024-10-09
- Estimated Expiration
- 2040-08-21
AI Technical Summary
Existing medical devices, particularly catheters, face high frictional resistance due to reduced diameters for navigating narrow body lumens, necessitating improved lubricity and durability in surface coatings to enhance operability in tight spaces.
A medical device with a surface lubricating layer comprising a hydrophilic copolymer containing specific constitutional units and a water-retaining material like hyaluronic acid, combined with a photoreactive group, to form a durable adhesive layer that maintains lubricity under high load conditions.
The device exhibits excellent lubricity and durability, allowing for smooth operation in narrow body lumens by retaining hydration through the surface lubricating layer, even under high load conditions, thereby improving operability and maintaining lubrication over time.
Smart Images

Figure 0007564807000020 
Figure 0007564807000021 
Figure 0007564807000022
Abstract
Description
[Technical field]
[0001] The present invention relates to a medical device and a method for producing the same, and in particular to a medical device having a surface lubricating layer that exhibits excellent lubricity and a method for producing the same. [Background technology]
[0002] In recent years, catheters have been used for the diagnosis and treatment of various lesions by reducing the outer diameter to improve the ease of insertion into peripheral blood vessels. Therefore, in diagnosis or treatment using a catheter, the clearance between the catheter and the inner surface of the body lumen becomes extremely small, which may cause high friction resistance on the catheter surface. Therefore, catheters are required to have a coating that gives the catheter surface lubricity and durability (lubrication maintenance).
[0003] For example, International Publication No. 2018 / 038063 (corresponding to US 2019 / 0185776 A1) discloses the use of a hydrophilic copolymer in a surface lubricating layer, the hydrophilic copolymer including a constituent unit derived from a polymerizable monomer (A) having a sulfobetaine structure, a constituent unit derived from a polymerizable monomer (B) having a group such as a sulfonic acid group, and a constituent unit derived from a polymerizable monomer (C) having a photoreactive group. Summary of the Invention
[0004] The surface lubricating layer disclosed in International Publication No. 2018 / 038063 (corresponding to US 2019 / 0185776 A1) certainly exhibits excellent lubricity and durability (lubrication maintenance). On the other hand, medical procedures in which medical tools approach more flexible and narrower lesion sites in vivo are becoming more widespread, and the demand for operability to reach the lesion site of the medical tool has been increasing in recent years. For this reason, there is a demand for technology to further improve lubricity in order to operate the medical tool well even in a narrower lesion site.
[0005] Therefore, an object of the present invention is to provide a means for improving lubrication.
[0006] The present inventors have carried out intensive research to solve the above-mentioned problems.As a result, they have found that the above-mentioned problems can be solved by providing a substrate layer with an adhesive layer that contains the hydrophilic copolymer having specific structural units and a surface lubricating layer that contains the hydrophilic copolymer having specific structural units and a specific water-retaining material such as hyaluronic acid (salt), and have completed the present invention.
[0007] That is, the above object is to provide a substrate layer, a polymerizable monomer (A) having a sulfobetaine structure and a sulfonic acid group (-SO 3 H), sulfate group (-OSO 3 H) and sulfite groups (-OSO 2 and an adhesive layer comprising a hydrophilic copolymer (1) containing a structural unit derived from a polymerizable monomer (B) having at least one group selected from the group consisting of groups consisting of groups of hyaluronic acid or a salt thereof, and a structural unit derived from a polymerizable monomer (C) having a photoreactive group; and a hydrophilic copolymer (2) formed in at least a part of the adhesive layer, the hydrophilic copolymer (2) containing a structural unit derived from a polymerizable monomer (B) having at least one group selected from the group consisting of groups consisting of groups of hyaluronic acid or a salt thereof, and a structural unit derived from a polymerizable monomer (A') having a sulfobetaine structure, and a sulfonic acid group (-SO 3 H), sulfate group (-OSO 3 H) and sulfite groups (-OSO 2 This can be achieved by a medical device having a surface lubricating layer comprising a hydrophilic copolymer (2) containing a structural unit derived from a polymerizable monomer (B') having at least one group selected from the group consisting of groups consisting of groups of polymerizable monomers (H) and salts thereof, and a structural unit derived from a polymerizable monomer (C') having a photoreactive group.
[0008] The above object is also achieved by providing a substrate layer, a polymerizable monomer (A) having a sulfobetaine structure and a sulfonic acid group (-SO 3 H), sulfate group (-OSO 3 H) and sulfite groups (-OSO 2an adhesive layer comprising a hydrophilic copolymer (1) containing a structural unit derived from a polymerizable monomer (B) having at least one group selected from the group consisting of a ... 3 H), sulfate group (-OSO 3 H) and sulfite groups (-OSO 2 This can also be achieved by a medical device having a surface lubricating layer containing a hydrophilic copolymer (2) that contains a structural unit derived from a polymerizable monomer (B') having at least one group selected from the group consisting of groups consisting of groups of polymerizable monomers (H) and salts thereof, and a structural unit derived from a polymerizable monomer (C') having a photoreactive group. [Brief description of the drawings]
[0009] [Figure 1] FIG. 1 is a partial cross-sectional view showing a schematic representation of a layered structure on a surface of a representative embodiment of a medical device according to the present invention. [Diagram 2] FIG. 2 is a partial cross-sectional view showing a schematic example of a configuration having a different surface layer structure as an application example of the embodiment in FIG. [Diagram 3] FIG. 2 is a schematic diagram of a lubricity and durability test device (friction tester) used in the examples and comparative examples. [Figure 4] 1 is a diagram showing the results of lubricity and durability tests in Example 1 and Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, the embodiment for carrying out the present invention will be described in detail. Note that the present invention is not limited to only the following embodiment. In addition, in this specification, "X to Y" indicating a range includes X and Y and means "X or more and Y or less". In this specification, "X and / or Y" means including at least one of X and Y, and includes "X alone", "Y alone" and "combination of X and Y". In addition, unless otherwise specified, the operation and measurement of physical properties are performed under the conditions of room temperature (20 to 25°C) / relative humidity 40 to 60% RH.
[0011] As used herein, the term "(meth)acrylic" includes both acrylic and methacrylic. Thus, for example, the term "(meth)acrylic acid" includes both acrylic acid and methacrylic acid. Similarly, the term "(meth)acryloyl" includes both acryloyl and methacryloyl. Thus, for example, the term "(meth)acryloyl group" includes both acryloyl and methacryloyl groups.
[0012] In addition, in this specification, unless otherwise defined, "substituted" refers to being substituted with a C1-C30 alkyl group, a C2-C30 alkenyl group, a C2-C30 alkynyl group, a C1-C30 alkoxy group, an alkoxycarbonyl group (-COOR, R is a C1-C30 alkyl group), a halogen atom (F, Cl, Br or I atom), a C6-C30 aryl group, a C6-C30 aryloxy group, an amino group, a C1-C30 alkylamino group, a cyano group, a nitro group, a thiol group, a C1-C30 alkylthio group or a hydroxyl group. Note that when a group is substituted, the form of substitution that is included in the definition before the substituted structure is further substituted is excluded. For example, when the substituent is an alkyl group, this alkyl group as a substituent is not further substituted with an alkyl group.
[0013] In this specification, the "polymerizable monomer (A) having a sulfobetaine structure" is also simply referred to as the "polymerizable monomer (A)" or the "polymerizable monomer (A) according to the present invention." Similarly, the "structural unit derived from the polymerizable monomer (A) having a sulfobetaine structure" is also simply referred to as the "structural unit (A)" or the "structural unit (A) according to the present invention." Similarly, in this specification, the "polymerizable monomer (A') having a sulfobetaine structure" is also simply referred to as the "polymerizable monomer (A')" or the "polymerizable monomer (A') according to the present invention." Similarly, the "structural unit derived from the polymerizable monomer (A') having a sulfobetaine structure" is also simply referred to as the "structural unit (A')" or the "structural unit (A') according to the present invention."
[0014] In this specification, "sulfonic acid group (-SO 3 H), sulfate group (-OSO 3 H) and sulfite groups (-OSO 2 The polymerizable monomer (B) having at least one group selected from the group consisting of a sulfonic acid group (-SO 3 H), sulfate group (-OSO 3 H) and sulfite groups (-OSO 2 A "structural unit derived from a polymerizable monomer (B) having at least one group selected from the group consisting of a sulfonic acid group (-SO 3 H), sulfate group (-OSO 3 H) and sulfite groups (-OSO 2 The polymerizable monomer (B') having at least one group selected from the group consisting of a sulfonic acid group (-SO 3 H), sulfate group (-OSO 3 H) and sulfite groups (-OSO 2The "structural unit derived from polymerizable monomer (B') having at least one group selected from the group consisting of groups consisting of groups of a salt thereof and a group of a salt thereof" is also referred to simply as "structural unit (B')" or "structural unit (B') according to the present invention."
[0015] In this specification, the "polymerizable monomer (C) having a photoreactive group" is also simply referred to as the "polymerizable monomer (C)" or the "polymerizable monomer (C) according to the present invention". Similarly, the "structural unit derived from the polymerizable monomer (C) having a photoreactive group" is also simply referred to as the "structural unit (C)" or the "structural unit (C) according to the present invention". Similarly, in this specification, the "polymerizable monomer (C') having a photoreactive group" is also simply referred to as the "polymerizable monomer (C')" or the "polymerizable monomer (C') according to the present invention". Similarly, the "structural unit derived from the polymerizable monomer (C') having a photoreactive group" is also simply referred to as the "structural unit (C')" or the "structural unit (C') according to the present invention".
[0016] In this specification, "hydrophilic copolymer (1) containing structural unit (A), structural unit (B), and structural unit (C)" is also referred to simply as "hydrophilic copolymer (1)" or "hydrophilic copolymer (1) of the present invention." Similarly, in this specification, "hydrophilic copolymer (2) containing structural unit (A'), structural unit (B'), and structural unit (C')" is also referred to simply as "hydrophilic copolymer (2)" or "hydrophilic copolymer (2) of the present invention."
[0017] In this specification, the "polymerizable monomer" may also be simply referred to as "monomer".
[0018] In this specification, "hyaluronic acid or a salt thereof" is also referred to simply as "hyaluronic acid (salt)".
[0019] In this specification, when a certain structural unit is said to be "derived from" a certain monomer, it means that the structural unit is a divalent structural unit resulting from the conversion of a polymerizable unsaturated double bond (C=C) present in the monomer corresponding to that structural unit to a single bond (-CC-).
[0020] In a first aspect of the present invention, there is provided a polymerizable composition comprising a base material layer, a polymerizable monomer (A) having a sulfobetaine structure, a sulfonic acid group (-SO 3 H), sulfate group (-OSO 3 H) and sulfite groups (-OSO 2 and an adhesive layer comprising a hydrophilic copolymer (1) containing a structural unit derived from a polymerizable monomer (B) having at least one group selected from the group consisting of groups consisting of groups of hyaluronic acid or a salt thereof, and a structural unit derived from a polymerizable monomer (C) having a photoreactive group; and a hydrophilic copolymer (2) formed in at least a part of the adhesive layer, the hydrophilic copolymer (2) containing a structural unit derived from a polymerizable monomer (B) having at least one group selected from the group consisting of groups consisting of groups of hyaluronic acid or a salt thereof, and a structural unit derived from a polymerizable monomer (A') having a sulfobetaine structure, and a sulfonic acid group (-SO 3 H), sulfate group (-OSO 3 H) and sulfite groups (-OSO 2 and a surface lubricating layer comprising a hydrophilic copolymer (2) containing a structural unit derived from a polymerizable monomer (B') having at least one group selected from the group consisting of groups consisting of groups of a polymerizable monomer (H) and salts thereof, and a structural unit derived from a polymerizable monomer (C') having a photoreactive group.
[0021] In a second aspect of the present invention, there is provided a polymerizable composition comprising a base layer, a polymerizable monomer (A) having a sulfobetaine structure, a sulfonic acid group (-SO 3 H), sulfate group (-OSO 3 H) and sulfite groups (-OSO 2 an adhesive layer comprising a hydrophilic copolymer (1) containing a structural unit derived from a polymerizable monomer (B) having at least one group selected from the group consisting of a ... 3 H), sulfate group (-OSO 3 H) and sulfite groups (-OSO 2and a surface lubricating layer comprising a hydrophilic copolymer (2) containing a structural unit derived from a polymerizable monomer (B') having at least one group selected from the group consisting of groups consisting of groups of a polymerizable monomer (H) and salts thereof, and a structural unit derived from a polymerizable monomer (C') having a photoreactive group.
[0022] The medical device having the configuration described in the first and second aspects above can exhibit excellent lubricity.
[0023] In recent years, medical tools have become smaller and thinner, and medical procedures in which medical tools approach more flexible and narrower lesions in vivo are becoming more widespread. There is a demand for devices that can maintain good operability even in areas where the clearance between such medical tools and the inner surface of the living lumen is small. The present inventors have conducted intensive studies to meet such demands. As a result, it has been found that by using the surface lubricating layer described in the above International Publication No. 2018 / 038063 (corresponding to US 2019 / 0185776 A1) as an adhesive layer and providing a surface lubricating layer containing a hydrophilic copolymer and a specific water-retaining material (hyaluronic acid (salt), polyelectrolyte, polysaccharide, nonionic polymer) on the adhesive layer, high lubricity can be exhibited even under high load conditions (i.e., even in areas where the clearance between the medical tool and the inner surface of the living lumen is small). The mechanism by which such an effect is achieved is not clear, but the following mechanism is presumed. Note that the following mechanism is presumed, and the present invention is not limited by the following presumption. In detail, the hydrophilic copolymer (hydrophilic copolymer (2)) contained in the surface lubricating layer exhibits lubricity when wet (for example, when contacting with aqueous liquids such as body fluids or physiological saline). According to the present invention, the surface lubricating layer contains a water-retaining material (in the first embodiment, hyaluronic acid (salt); in the second embodiment, at least one of a polymer electrolyte, a polysaccharide, and a nonionic polymer; the same applies below) in addition to this hydrophilic copolymer (hydrophilic copolymer (2)). In addition to the water-absorbing effect of the water-retaining material itself, such a surface lubricating layer has a moderately low crosslink density due to the presence of the water-retaining material. Therefore, aqueous liquids easily enter the surface lubricating layer (hydrophilic copolymer (2) easily exhibits lubricity (surface gel hydration lubrication) in contact with aqueous liquids). In addition, under high load conditions, the surface lubricating layer of the present invention can maintain a sufficient hydration layer on the medical device surface due to the aqueous liquid held by the surface lubricating layer. For this reason, it is considered that the hydrophilic copolymer (2) can exhibit sufficient lubricity even under high load conditions.
[0024] In addition, the hydrophilic copolymer (1) in the adhesive layer and the hydrophilic copolymer (2) in the surface lubricating layer have photoreactive groups. When the adhesive layer or the surface lubricating layer is irradiated with active energy rays, the photoreactive groups generate reactive species, and the hydrophilic copolymer (1) in the adhesive layer reacts with the base layer (resin) to form a covalent bond between the base layer and the adhesive layer. In addition, due to the generation of these reactive species, the hydrophilic copolymer (1) in the adhesive layer reacts with the hydrophilic copolymer (2) in the surface lubricating layer and the water-retaining material (particularly hyaluronic acid (salt)) to form a covalent bond between the adhesive layer and the surface lubricating layer. Therefore, in the present invention, by providing an adhesive layer between the base layer and the surface lubricating layer, the surface lubricating layer can be firmly fixed to the base layer via the adhesive layer. Therefore, the medical device of the present invention can maintain its initial lubricity for a longer period of time and further improve its durability (lubrication maintenance).
[0025] Therefore, the medical device of the present invention can exhibit excellent lubricity even under conditions where the clearance between the medical device and the inner surface of a biological lumen is smaller (high load).Furthermore, the medical device of the present invention can exhibit excellent durability (lubrication maintenance).
[0026] Hereinafter, preferred embodiments of the medical device according to the present invention will be described with reference to the accompanying drawings.
[0027] Fig. 1 is a partial cross-sectional view showing a typical surface layer structure of a typical embodiment of a medical device according to the present invention (hereinafter, also simply referred to as "medical device"). Fig. 2 is a partial cross-sectional view showing a typical example of a different surface layer structure as an application example of this embodiment. In Figs. 1 and 2, 1 represents a base layer, 1a represents a base layer core, 1b represents a base surface layer, 2 represents an adhesive layer, 3 represents a surface lubricating layer, and 10 represents a medical device.
[0028] As shown in Fig. 1 and Fig. 2, the medical device 10 of this embodiment includes a base layer 1, an adhesive layer 2 including a hydrophilic copolymer (1) fixed (disposed) so as to cover at least a part of the surface of the base layer 1 (the figure shows an example of fixing (disposed) on the entire (whole) surface of the base layer 1 in the drawing), and a surface lubricating layer 3 including a hydrophilic copolymer (2) fixed (disposed) so as to cover at least a part of the surface of the adhesive layer 2 (the figure shows an example of fixing (disposed) on the entire (whole) surface of the adhesive layer 2 in the drawing) and a water-retaining material (in the first embodiment, hyaluronic acid (salt); in the second embodiment, at least one of a polyelectrolyte, a polysaccharide, and a nonionic polymer). The adhesive layer 2 is bonded to the hydrophilic copolymer (2) and the water-retaining material (particularly hyaluronic acid (salt)) in the base layer 1 and the surface lubricating layer 3 via the photoreactive group of the hydrophilic copolymer (1).
[0029] Each component of the medical device of this embodiment will be described below.
[0030] <First aspect> The first aspect of the present invention is a polymerizable composition comprising a base layer, a polymerizable monomer (A) having a sulfobetaine structure, a sulfonic acid group (-SO 3 H), sulfate group (-OSO 3 H) and sulfite groups (-OSO 2 and an adhesive layer comprising a hydrophilic copolymer (1) containing a structural unit derived from a polymerizable monomer (B) having at least one group selected from the group consisting of groups consisting of groups of hyaluronic acid or a salt thereof, and a structural unit derived from a polymerizable monomer (C) having a photoreactive group; and a hydrophilic copolymer (2) formed in at least a part of the adhesive layer, the hydrophilic copolymer (2) containing a structural unit derived from a polymerizable monomer (B) having at least one group selected from the group consisting of groups consisting of groups of hyaluronic acid or a salt thereof, and a structural unit derived from a polymerizable monomer (A') having a sulfobetaine structure, and a sulfonic acid group (-SO 3 H), sulfate group (-OSO 3 H) and sulfite groups (-OSO 2 and a surface lubricating layer comprising a hydrophilic copolymer (2) containing a structural unit derived from a polymerizable monomer (B') having at least one group selected from the group consisting of groups consisting of groups of a polymerizable monomer (H) and salts thereof, and a structural unit derived from a polymerizable monomer (C') having a photoreactive group.
[0031] [Base material layer (base material)] The substrate layer used in this embodiment may be made of any material as long as it can react with the photoreactive group contained in the hydrophilic copolymer (1) described later to form a chemical bond. Specifically, the material constituting (forming) the substrate layer 1 may be a metal material, a polymer material, a ceramic, or the like. Here, the substrate layer 1 may have a structure in which the entire substrate layer 1 is made of any of the above materials as shown in FIG. 1, or the surface of the substrate layer core portion 1a made of any of the above materials is coated with any of the other materials by an appropriate method to form a substrate surface layer 1b as shown in FIG. 2. Examples of the latter case include a substrate surface layer 1b formed by coating the surface of a substrate core portion 1a made of a resin material or the like with a metal material by an appropriate method (conventionally known methods such as plating, metal deposition, sputtering, etc.); a substrate surface layer 1b formed by coating the surface of a substrate core portion 1a made of a hard reinforcing material such as a metal material or a ceramic material with a polymer material that is softer than the reinforcing material such as a metal material by an appropriate method (conventionally known methods such as dipping, spraying, coating, printing, etc.), or a substrate surface layer 1b formed by compounding (appropriate reaction treatment) the reinforcing material of the substrate core portion 1a and the polymer material of the substrate surface layer 1b. Thus, the substrate core portion 1a may be a multilayer structure formed by laminating different materials in multiple layers, or a structure (composite) in which members formed of different materials are joined for each part of the medical device. In addition, another middle layer (not shown) may be formed between the substrate core portion 1a and the substrate surface layer 1b. Furthermore, the substrate surface layer 1b may also be a multi-layer structure in which different materials are laminated in multiple layers, or a structure (composite) in which members made of different materials are joined together for each portion of the medical device.
[0032] Among the materials constituting (forming) the base layer 1, the metal material is not particularly limited, and metal materials generally used for medical devices such as catheters, stents, and guidewires are used. Specifically, various stainless steels (SUS) such as SUS304, SUS316, SUS316L, SUS420J2, and SUS630, gold, platinum, silver, copper, nickel, cobalt, titanium, iron, aluminum, tin, and various alloys such as nickel-titanium (Ni-Ti) alloy, nickel-cobalt (Ni-Co) alloy, cobalt-chromium (Co-Cr) alloy, and zinc-tungsten (Zn-W) alloy can be mentioned. These may be used alone or in combination of two or more. The metal material may be appropriately selected from the metal materials most suitable for the base layer of the catheter, stent, guidewire, etc., which is the intended use.
[0033] Among the materials constituting (forming) the base layer 1, the polymeric material is not particularly limited, and polymeric materials generally used for medical devices such as catheters, stents, and guidewires can be used. Specifically, polyamide resin, polyethylene such as linear low density polyethylene (LLDPE), low density polyethylene (LDPE), high density polyethylene (HDPE), modified polyethylene, polyolefin resin such as polypropylene, polyester resin such as polyethylene terephthalate, styrene resin such as polystyrene, cyclic polyolefin resin, modified polyolefin resin, epoxy resin, urethane resin, diallyl phthalate resin (allyl resin), polycarbonate resin, fluorine resin, amino resin (urea resin, melamine resin, benzoguanamine resin), acrylic resin, polyacetal resin, vinyl acetate resin, phenol resin, vinyl chloride resin, silicone resin (silicon resin), polyether resin such as polyether ether ketone (PEEK), polyimide resin, etc. are mentioned, and from the viewpoint of adhesion with the adhesive layer described later, high density polyethylene (HDPE), polyethylene such as modified polyethylene, polyether resin such as polyether ether ketone (PEEK), polyamide resin are preferable. These may be used alone or in combination of two or more. The polymer material may be appropriately selected from those suitable for the substrate layer of the intended use, such as catheters, stents, guidewires, and the like.
[0034] The shape of the substrate layer is not particularly limited, and may be appropriately selected depending on the mode of use, such as a sheet, a linear (wire), or a tubular shape.
[0035] [Adhesive layer (hydrophilic copolymer (1))] The adhesive layer is formed on at least a portion of the base layer, and is composed of a structural unit (structural unit (A)) derived from a polymerizable monomer (A) having a sulfobetaine structure and a sulfonic acid group (-SO 3 H), sulfate group (-OSO 3 H) and sulfite groups (-OSO 2The hydrophilic copolymer (1) includes a structural unit (structural unit (B)) derived from a polymerizable monomer (B) having at least one group selected from the group consisting of groups of H) and salts thereof, and a structural unit (structural unit (C)) derived from a polymerizable monomer (C) having a photoreactive group. Here, the adhesive layer does not necessarily have to be formed on the entire surface of the base layer. For example, the adhesive layer may be formed on the surface portion (part) of the base layer that comes into contact with body fluids.
[0036] The hydrophilic copolymer (1) contained in the adhesive layer according to the present invention is a copolymer having a sulfobetaine structure, a structural unit (structural unit (A)) derived from a polymerizable monomer (A) (hereinafter also referred to as "monomer A"), and a sulfonic acid group (-SO 3 H), sulfate group (-OSO 3 H) and sulfite groups (-OSO 2 The hydrophilic copolymer (1) has a structural unit (structural unit (B)) derived from a polymerizable monomer (B) (hereinafter also referred to as "monomer B") having at least one group selected from the group consisting of groups of H) and salts thereof, and a structural unit (structural unit (C)) derived from a polymerizable monomer (C) (hereinafter also referred to as "monomer C") having a photoreactive group. The hydrophilic copolymer (1) (hence the adhesive layer) can exhibit sufficient lubricity and durability (lubrication maintenance). In addition, the hydrophilic copolymer (1) has good binding (adhesiveness) with the hydrophilic copolymer (2) and water-retaining material (especially hyaluronic acid (salt)) in the base layer and the surface lubricating layer described below. The mechanism by which such an effect is exerted is not completely clear, but the following mechanism is presumed. The photoreactive group contained in the structural unit derived from monomer C generates reactive species by irradiation with active energy rays, and reacts with the hydrophilic copolymer (2) and water retention material (especially hyaluronic acid (salt)) in the surface of the base layer and the surface lubricating layer described below to form a chemical bond. Therefore, the adhesive layer containing the hydrophilic copolymer (1) according to the present invention is firmly fixed on the base layer and firmly fixes the surface lubricating layer, so that it has excellent durability (lubrication maintenance). Note that the above mechanism is an assumption, and the present invention is not limited by the above assumption.
[0037] In the present invention, other layers may be present between the adhesive layer and the base layer as long as they do not affect the effects of the present invention, but the adhesive layer is preferably located directly on the base layer.
[0038] The thickness of the adhesive layer is not particularly limited. From the viewpoints of adhesion to the base layer, adhesion to the surface lubricating layer, lubricity, etc., the thickness of the adhesive layer (dry film thickness) is preferably 0.1 to 100 μm, more preferably 0.2 to 50 μm.
[0039] Hereinafter, each polymerizable monomer constituting the hydrophilic copolymer (1) contained in the adhesive layer according to the present invention will be described.
[0040] (Polymerizable monomer (A)) The hydrophilic copolymer (1) has a constituent unit (constituent unit (A)) derived from a polymerizable monomer (A) having a sulfobetaine structure. Here, the constituent unit (A) constituting the hydrophilic copolymer (1) may be a single type, or a combination of two or more types. That is, the constituent unit (A) may be composed of only one type of constituent unit (A), or may be composed of two or more types of constituent units (A). Note that the multiple constituent units (A) may be present in a block form or a random form.
[0041] The polymerizable monomer (A) (monomer A) is a polymerizable monomer having a sulfobetaine structure. The sulfobetaine structure contained in the constituent unit derived from monomer A has excellent lubricity-imparting effect. Therefore, it is considered that the hydrophilic copolymer (1) having the constituent unit derived from monomer A has excellent lubricity. In addition, the homopolymer of monomer A is soluble in an aqueous NaCl solution, but is insoluble or difficult to dissolve in water or lower alcohol. Therefore, it is suggested that the sulfobetaine structure may have strong electrostatic interaction. For this reason, a strong cohesive force acts inside the adhesive layer containing the hydrophilic copolymer (1) according to the present invention. It is considered that the adhesive layer has high strength (excellent durability). Note that the above is an assumption, and the present invention is not limited by the above assumption.
[0042] Here, the term "sulfobetaine structure" refers to a structure in which a positive charge and a negative charge containing a sulfur element are not adjacent to each other, no dissociable hydrogen atom is bonded to the positively charged atom, and the sum of the charges is zero.
[0043] Examples of the monomer A include, but are not limited to, compounds represented by the following general formula:
[0044] [ka]
[0045] In the above general formula, R a and R d R may each independently be an optionally substituted alkylene group having 1 to 30 carbon atoms or an optionally substituted arylene group having 6 to 30 carbon atoms. b and R c may each independently be an optionally substituted alkyl group having 1 to 30 carbon atoms or an optionally substituted aryl group having 6 to 30 carbon atoms. Y is an acryloyl group (CH 2 =CH-C(=O)-), methacryloyl group (CH 2 =C(CH 3 )-C(=O)-), vinyl group (CH 2 It may also be a group having an ethylenically unsaturated group such as =CH-), provided that in the above general formula, the sum of the positive charge and the negative charge is zero.
[0046] Examples of the alkylene group having 1 to 30 carbon atoms include a methylene group, an ethylene group, a trimethylene group, a propylene group, an isopropylene group, a butylene group, an isobutylene group, a sec-butylene group, a tert-butylene group, and a pentylene group.
[0047] Examples of the arylene group having 6 to 30 carbon atoms include a phenylene group, a naphthylene group, an anthracenylene group, a phenanthrenylene group, a pyrenylene group, a perylenylene group, a fluorenylene group, and a biphenylene group.
[0048] Examples of alkyl groups having 1 to 30 carbon atoms include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, an n-pentyl group, an iso-amyl group, a tert-pentyl group, a neopentyl group, and an n-hexyl group.
[0049] Examples of the aryl group having 6 to 30 carbon atoms include a phenyl group, a biphenyl group, a terphenyl group, a pentalenyl group, an indenyl group, a naphthyl group, an azulenyl group, a heptalenyl group, and a biphenylenyl group.
[0050] Among them, from the viewpoint of further improving lubricity and durability (lubrication maintenance), the monomer A is preferably a compound represented by the following formula (1): That is, in a preferred embodiment of the present invention, the polymerizable monomer (A) is represented by the following formula (1).
[0051] [ka]
[0052] In the above formula (1), R 11 is a hydrogen atom or a methyl group. 1 is an oxygen atom (-O-) or -NH-, and is preferably an oxygen atom (-O-).
[0053] In addition, in the above formula (1), R 12 and R 15From the viewpoint of further improving lubricity and durability (lubrication maintenance), each of R is independently a straight-chain or branched-chain alkylene group having 1 to 20 carbon atoms, preferably a straight-chain or branched-chain alkylene group having 1 to 12 carbon atoms, more preferably a straight-chain or branched-chain alkylene group having 1 to 8 carbon atoms, even more preferably a straight-chain or branched-chain alkylene group having 1 to 6 carbon atoms, still more preferably a straight-chain alkylene group having 1 to 4 carbon atoms (methylene group, ethylene group, trimethylene group, or tetramethylene group), and particularly preferably a straight-chain alkylene group having 1 to 3 carbon atoms (methylene group, ethylene group, or trimethylene group). 12 and R 15 From the viewpoint of further improving lubricity and durability (lubrication maintenance), the combination of R is preferably 12 is an ethylene group and R 15 is a trimethylene group; or R 12 is a trimethylene group and R 15 is a tetramethylene group.
[0054] In the above formula (1), R 13 and R 14 From the viewpoint of further improving lubricity and durability (lubrication maintenance), each independently represents a linear or branched chain alkyl group having 1 to 20 carbon atoms, preferably a linear or branched chain alkyl group having 1 to 12 carbon atoms, more preferably a linear or branched chain alkyl group having 1 to 8 carbon atoms, even more preferably a linear or branched chain alkyl group having 1 to 4 carbon atoms, and particularly preferably a methyl group.
[0055] Examples of the compound represented by the above formula (1) include {2-[(meth)acryloyloxy]ethyl}dimethyl-(3-sulfopropyl)ammonium hydroxide, {2-[(meth)acryloyloxy]ethyl}dimethyl-(2-sulfoethyl)ammonium hydroxide, {2-[(meth)acryloyloxy]ethyl}dimethyl-(2-sulfobutyl)ammonium hydroxide, {2-[(meth)acryloyloxy]ethyl}diethyl-(2-sulfoethyl)ammonium hydroxide, {2-[(meth)acryloyloxy]ethyl}diethyl-(3-sulfopropyl)ammonium hydroxide, {2-[(meth)acryloyloxy]ethyl}diethyl-(2-sulfobutyl)ammonium hydroxide. ammonium hydroxide, {3-[(meth)acryloyloxy]propyl}dimethyl-(2-sulfoethyl)ammonium hydroxide, {3-[(meth)acryloyloxy]propyl}dimethyl-(3-sulfopropyl)ammonium hydroxide, {3-[(meth)acryloylamino)propyl}dimethyl(3-sulfobutyl)ammonium hydroxide, {3-[(meth)acryloyloxy]propyl}diethyl-(2-sulfoethyl)ammonium hydroxide, {3-[(meth)acryloyloxy]propyl}diethyl-(3-sulfopropyl)ammonium hydroxide, {3-[(meth)acryloyloxy]propyl}diethyl-(3-sulfobutyl)ammonium hydroxide, and the like. Among these, {2-[(meth)acryloyloxy]ethyl}dimethyl-(3-sulfopropyl)ammonium hydroxide and {3-[(meth)acryloyloxy)propyl]dimethyl(3-sulfobutyl)ammonium hydroxide are preferred, {2-[methacryloyloxy]ethyl}dimethyl-(3-sulfopropyl)ammonium hydroxide (MSPB) and [3-(methacryloylamino)propyl]dimethyl(3-sulfobutyl)ammonium hydroxide (MSBB) are more preferred, and {2-[methacryloyloxy]ethyl}dimethyl-(3-sulfopropyl)ammonium hydroxide (MSPB) is even more preferred. The above compounds may be used alone or in combination of two or more.
[0056] The monomer A may be either a synthetic product or a commercially available product. Commercially available products are available from Sigma-Aldrich Corporation, Fujifilm Wako Pure Chemical Industries, Ltd., etc. In addition, when synthesizing the monomer A, A. Laschewsky, Polymers, 6, 1544-1601 (2014), etc. can be referred to.
[0057] Furthermore, the monomer A is not limited to the compound represented by the above general formula, but may be a compound having a positive charge at the terminal.
[0058] In the hydrophilic copolymer (1), the content of the monomer A-derived structural unit is preferably 0.1 to 99 mol%, more preferably 1 to 99 mol%, even more preferably 5 to 99 mol%, and particularly preferably 10 to 99 mol%, when the total of all monomer-derived structural units is taken as 100 mol%. Within such a range, the balance between lubricity and solvent solubility is good. When the structural unit (A) is composed of two or more types of structural units (A), the composition of the structural unit (A) is the ratio (molar ratio (mol%)) of the total of the structural units (A) derived from all monomers to the total (100 mol%). The mol% is substantially equivalent to the ratio of the amount (mol) of monomer A to the total amount (mol) of all monomers to be charged when producing a polymer.
[0059] (Polymerizable monomer (B)) The hydrophilic copolymer (1) contains sulfonic acid groups (-SO 3 H), sulfate group (-OSO 3 H) and sulfite groups (-OSO 2 The hydrophilic copolymer (1) has a structural unit (structural unit (B)) derived from a polymerizable monomer (B) having at least one group selected from the group consisting of H) and salt groups thereof. Here, the structural unit (B) constituting the hydrophilic copolymer (1) may be a single type, or a combination of two or more types. That is, the structural unit (B) may be composed of only one type of structural unit (B), or may be composed of two or more types of structural units (B). The multiple structural units (B) may be present in a block form or a random form.
[0060] The polymerizable monomer (B) (monomer B) has a sulfonic acid group (-SO 3 H), sulfate group (-OSO 3 H) and sulfite groups (-OSO 2 H) and salts thereof. By introducing such a group, the hydrophilic copolymers are anionized in an aqueous solvent, and electrostatic repulsion occurs between the hydrophilic copolymers. As a result, the electrostatic interaction between the sulfobetaine structures between the hydrophilic copolymers and the hydrophobic interaction between the photoreactive groups between the hydrophilic copolymers are reduced. Therefore, the solvent solubility of the copolymer (particularly the solubility in water, lower alcohol, or a mixed solvent of water and lower alcohol) is improved. This improvement effect is particularly remarkable when the photoreactive group of the monomer C is a benzophenone group. Since the benzophenone group has multiple aromatic rings, it is easy to associate through π-π interactions, and as a result, the polymer containing the benzophenone group is easily aggregated and insoluble. Therefore, by introducing a structural unit derived from the monomer B, electrostatic repulsion occurs as described above, and the association between the benzophenone groups is suppressed, so that the solubility or dispersibility of the polymer is thought to be dramatically improved. Note that the above mechanism is an assumption, and the present invention is not limited by the above assumption. Alternatively, the above-mentioned improving effect can be obtained well even when the monomer C contains an ester group. In addition, the monomer B preferably has an ethylenically unsaturated group such as a (meth)acryloyl group, a vinyl group, or an allyl group in addition to the above groups.
[0061] Among them, from the viewpoint of further improving the solvent solubility, the monomer B is preferably a compound represented by the following formula (2), (3) or (4), and more preferably a compound represented by the following formula (2). That is, in a preferred embodiment of the present invention, the polymerizable monomer (B) is represented by the following formula (2), (3) or (4). In a more preferred embodiment of the present invention, the polymerizable monomer (B) is represented by the following formula (2).
[0062] [ka]
[0063] In the above formula (2), R 21 is a hydrogen atom or a methyl group. 2 is an oxygen atom (-O-) or -NH-, preferably -NH-.
[0064] In the above formula (2), R 22 From the viewpoint of further improving the solvent solubility, is a straight-chain or branched-chain alkylene group having 1 to 20 carbon atoms, preferably a straight-chain or branched-chain alkylene group having 1 to 12 carbon atoms, more preferably a straight-chain or branched-chain alkylene group having 1 to 8 carbon atoms, still more preferably a straight-chain or branched-chain alkylene group having 1 to 6 carbon atoms, and particularly preferably a branched-chain alkylene group having 3 to 5 carbon atoms. The branched-chain alkylene group having 3 to 5 carbon atoms is represented by -CH(CH 3 )-CH 2 -, -C(CH 3 ) 2 -CH 2 -, -CH(CH 3 )-CH(CH 3 )-, -C(CH 3 ) 2 -CH 2 -CH 2 -, -CH(CH 3 )-CH(CH 3 )-CH 2 -, -CH(CH 3 )-CH 2 -CH(CH 3 )-, -CH 2 -C(CH 3 ) 2 -CH 2 -, -C(CH 3 ) 2 -CH(CH 3 )-, etc. (however, the order of linking the above groups in the above formula (2) is not particularly limited), and among these, 3 ) 2 -CH 2 A group represented by - is particularly preferred.
[0065] In the above formula (2), X is a sulfonic acid group (-SO3 H), sulfate group (-OSO 3 H) and sulfite groups (-OSO 2 H) and salts thereof, preferably from the viewpoint of the degree of dissociation of the acid (i.e., ease of anionization) and hence the solvent solubility of the copolymer, it is a group selected from the group consisting of a sulfonic acid group, a sulfuric acid group and salts thereof, and more preferably from the viewpoint of the ease of availability of the monomer, it is a sulfonic acid group or a salt thereof. Here, the salt is not particularly limited, and examples thereof include alkali metal salts (sodium salt, potassium salt, etc.) of the above groups.
[0066] Examples of the compound represented by the above formula (2) include 2-(meth)acrylamido-2-methyl-1-propanesulfonic acid, 1-[(meth)acryloyloxymethyl]-1-propanesulfonic acid, 2-[(meth)acryloyloxy]-2-propanesulfonic acid, 3-[(meth)acryloyloxy]-1-methyl-1-propanesulfonic acid, 2-sulfoethyl(meth)acrylate, 3-sulfopropyl(meth)acrylate, and their salts (preferably sodium salt, potassium salt), etc. Among these, 2-(meth)acrylamido-2-methyl-1-propanesulfonic acid or its salts (particularly alkali metal salts) are preferred, and 2-acrylamido-2-methyl-1-propanesulfonic acid or its salts (particularly sodium salts) are more preferred. These compounds may be used alone or in combination of two or more.
[0067] The compound represented by the above formula (2) may be either a synthetic product or a commercially available product, and commercially available products are available from Tokyo Chemical Industry Co., Ltd., Sigma-Aldrich Corporation, and the like.
[0068] [ka]
[0069] In the above formula (3), R 31 is a hydrogen atom or a methyl group.
[0070] In the above formula (3), R 32 is a single bond or a linear or branched alkylene group having 1 to 20 carbon atoms, preferably a single bond or a linear or branched alkylene group having 1 to 12 carbon atoms, more preferably a single bond or a linear or branched alkylene group having 1 to 8 carbon atoms, even more preferably a single bond or a linear or branched alkylene group having 1 to 4 carbon atoms, and particularly preferably a single bond. Specific examples of the alkylene group are the same as those in the above formula (2), and therefore will not be described here.
[0071] In the above formula (3), X is a sulfonic acid group (-SO 3 H), sulfate group (-OSO 3 H) and sulfite groups (-OSO 2 From the viewpoint of the degree of dissociation of the acid (i.e., the ease of anionization) and thus the solvent solubility of the copolymer, it is preferably a group selected from the group consisting of a sulfonic acid group, a sulfuric acid group, and a salt group thereof, and from the viewpoint of ease of availability of the monomer, it is more preferably a sulfonic acid group or a salt group thereof.
[0072] Examples of the compound represented by the above formula (3) include vinyl sulfonic acid, allyl sulfonic acid, methallyl sulfonic acid, 2-propene-1-sulfonic acid, 2-methyl-2-propene-1-sulfonic acid, and salts thereof. These compounds may be used alone or in combination of two or more.
[0073] The compound represented by the above formula (3) may be either a synthetic product or a commercially available product. Commercially available products include those available from Asahi Kasei Finechem Corporation, Tokyo Chemical Industry Co., Ltd. (e.g., 2-methyl-2-propene-1-sulfonic acid sodium salt), and the like.
[0074] [ka]
[0075] In the above formula (4), R 41 is a hydrogen atom or a methyl group.
[0076] In the above formula (4), R 42 is a straight or branched chain alkylene group having 1 to 20 carbon atoms, preferably a straight or branched chain alkylene group having 1 to 12 carbon atoms, more preferably a straight or branched chain alkylene group having 1 to 8 carbon atoms, and even more preferably a straight or branched chain alkylene group having 1 to 6 carbon atoms. Specific examples of the alkylene group are the same as those in the above formula (2), and therefore will not be described here.
[0077] In the above formula (4), X is a sulfonic acid group (-SO 3 H), sulfate group (-OSO 3 H) and sulfite groups (-OSO 2 From the viewpoint of the degree of dissociation of the acid (i.e., the ease of anionization) and thus the solvent solubility of the copolymer, it is preferably a group selected from the group consisting of a sulfonic acid group, a sulfuric acid group, and a salt group thereof, and from the viewpoint of ease of availability of the monomer, it is more preferably a sulfonic acid group or a salt group thereof.
[0078] Examples of the compound represented by the above formula (4) include 2-sulfoxyethyl vinyl ether, 3-sulfoxy-n-propyl vinyl ether, and salts thereof. These compounds may be used alone or in combination of two or more.
[0079] The compound represented by the above formula (4) may be either a synthetic product or a commercially available product.
[0080] In the hydrophilic copolymer (1), the content of the monomer B-derived structural unit is preferably 0.1 to 99 mol%, more preferably 0.2 to 99 mol%, even more preferably 0.5 to 99 mol%, and particularly preferably 1 to 99 mol%, when the total of the structural units derived from all monomers is taken as 100 mol%. Within such a range, the balance between lubricity and solvent solubility is good. When the structural unit (B) is composed of two or more types of structural units (B), the composition of the structural unit (B) is the ratio (molar ratio (mol%)) of the total of the structural units derived from all monomers to the total (100 mol%) of the structural units derived from all monomers. Moreover, the mol% is substantially equivalent to the ratio of the amount (mol) of the monomer B to the total amount (mol) of all monomers to be charged when producing a polymer.
[0081] (Polymerizable monomer (C)) The hydrophilic copolymer (1) has a structural unit (structural unit (C)) derived from a polymerizable monomer (C) having a photoreactive group. Here, the structural unit (C) constituting the hydrophilic copolymer (1) may be a single type, or a combination of two or more types. That is, the structural unit (C) may be composed of only one type of structural unit (C), or may be composed of two or more types of structural units (C). Note that the multiple structural units (C) may be present in a block form or a random form.
[0082] The polymerizable monomer (C) (monomer C) is a polymerizable monomer having a photoreactive group. Here, the "photoreactive group" refers to a group that generates reactive species such as radicals, nitrenes, and carbenes by irradiation with active energy rays, and reacts with the base layer (resin) and the surface lubricating layer (hydrophilic copolymer (2) and water-retaining material, especially hyaluronic acid (salt)) to form a chemical bond. As a result, the adhesive layer containing the hydrophilic copolymer (1) can firmly fix the surface of the base layer and the surface lubricating layer. Therefore, by disposing the adhesive layer between the base layer and the surface lubricating layer, the medical device can exhibit sufficient durability (lubrication maintenance). In addition, it is preferable that the monomer C has an ethylenically unsaturated group such as a (meth)acryloyl group, a vinyl group, or an allyl group in addition to the above-mentioned photoreactive group.
[0083] Examples of the photoreactive group include an azide group, a diazo group, a diazirine group, a ketone group, and a quinone group.
[0084] Examples of the azide group include aryl azide groups such as phenyl azide and 4-fluoro-3-nitrophenyl azide; acyl azide groups such as benzoyl azide and p-methylbenzoyl azide; azidoformate groups such as ethyl azidoformate and phenyl azidoformate; sulfonyl azide groups such as benzenesulfonyl azide; and phosphoryl azide groups such as diphenylphosphoryl azide and diethylphosphoryl azide.
[0085] Examples of the diazo group include groups derived from diazoalkanes such as diazomethane and diphenyldiazomethane; diazoketones such as diazoacetophenone and 1-trifluoromethyl-1-diazo-2-pentanone; diazoacetates such as t-butyl diazoacetate and phenyl diazoacetate; and α-diazoacetoacetates such as t-butyl-α-diazoacetoacetate.
[0086] Examples of the diazirine group include groups derived from 3-trifluoromethyl-3-phenyldiazirine, and the like.
[0087] Examples of the ketone group include groups having an acetophenone, benzophenone, anthrone, xanthine, thioxanthone structure, and the like.
[0088] The quinone group includes, for example, groups derived from anthraquinone and the like.
[0089] These photoreactive groups are appropriately selected depending on the type of the base layer of the medical device. For example, when the base layer is formed of a polyolefin resin such as a polyethylene resin, a polyamide resin, a polyurethane resin, a polyester resin, or the like, a ketone group or a phenylazide group is preferable, and a group having a benzophenone structure (benzophenone group) is more preferable in terms of easy availability of the monomer. That is, in a preferred embodiment of the present invention, the polymerizable monomer (C) has a group having a benzophenone structure.
[0090] Examples of monomer C include 2-azidoethyl (meth)acrylate, 2-azidopropyl (meth)acrylate, 3-azidopropyl (meth)acrylate, 4-azidobutyl (meth)acrylate, 4-(meth)acryloyloxybenzophenone (MBP), 4-(meth)acryloyloxyethoxybenzophenone, 4-(meth)acryloyloxy-4'-methoxybenzophenone, 4-(meth)acryloyloxyethoxy-4'-methoxybenzophenone, 4-(meth)acryloyloxy-4'-bromobenzophenone, 4-(meth)acryloyloxyethoxy-4'-bromobenzophenone, 4-styrylmethoxybenzophenone, 4-(meth)acryloyloxythioxanthone, 2-(meth) a Examples thereof include acryloyloxyethyl-4-azidobenzoate.
[0091] Monomer C may be either a synthetic product or a commercially available product, and commercially available products can be obtained from MCC Unitech Co., Ltd., etc.
[0092] In the hydrophilic copolymer (1), the content of the constituent units derived from the monomer C is preferably 0.1 to 40 mol%, more preferably 0.1 to 30 mol%, even more preferably 0.1 to 25 mol%, and particularly preferably 0.1 to 20 mol%, when the total of the constituent units derived from all monomers is taken as 100 mol%. Within such a range, the hydrophilic copolymer (1) can be sufficiently bonded to the base layer (resin) and the surface lubricating layer (hydrophilic copolymer (2) and the water-retaining material, particularly hyaluronic acid (salt)). Therefore, the adhesive layer containing the hydrophilic copolymer (1) can more firmly fix the base layer and the surface lubricating layer. In addition, within such a range, since other monomers (monomers A and B) can be present in sufficient amounts, the hydrophilic copolymer (1) can more effectively improve sufficient lubricity and durability due to the monomer A, and solvent solubility due to the monomer B. When the structural unit (C) is composed of two or more kinds of structural units (C), the composition of the structural unit (C) is the ratio (molar ratio (mol%)) of the total of the structural units (C) to the total of the structural units derived from all monomers (100 mol%). The mol% is substantially the same as the ratio of the amount (mol) of monomer C charged to the total amount (mol) of all monomers charged when producing a polymer.
[0093] The hydrophilic copolymer (1) may contain a structural unit derived from a polymerizable monomer other than the above-mentioned monomer A, monomer B, and monomer C (hereinafter also referred to as "other monomers") within a range that does not impair the effects of the present invention. In the hydrophilic copolymer (1) of the present invention, the content of the structural unit derived from the other monomer is preferably less than 10 mol%, more preferably less than 5 mol%, and even more preferably less than 1 mol% relative to the total amount of the structural units derived from all monomers (100 mol%) (lower limit: more than 0 mol%). In addition, when the structural unit derived from the other monomer is composed of two or more kinds of structural units, the composition of the structural unit derived from the other monomer is the ratio (molar ratio (mol%)) of the total structural units derived from the other monomers to the total of the structural units derived from all monomers (100 mol%). Preferably, the hydrophilic copolymer (1) of the present invention is composed only of monomer A, monomer B, and monomer C (composition of other monomers = 0 mol%). The mole percent is substantially equal to the ratio of the amount (mol) of the other monomer to the total amount (mol) of all monomers charged when producing a polymer.
[0094] The terminal of the hydrophilic copolymer (1) is not particularly limited and is appropriately determined depending on the type of raw material used, but is usually a hydrogen atom. The structure of the copolymer is also not particularly limited and may be any of a random copolymer, an alternating copolymer, a periodic copolymer, and a block copolymer.
[0095] The weight average molecular weight (Mw) of the hydrophilic copolymer (1) is preferably several thousand to several million, more preferably 1,000 to 1,000,000, and particularly preferably 5,000 to 500,000. In the present invention, the "weight average molecular weight" is a value measured by gel permeation chromatography (GPC) using polyethylene glycol as a standard substance.
[0096] [Method for producing hydrophilic copolymer (1)] The method for producing the hydrophilic copolymer (1) is not particularly limited, and any known polymerization method such as radical polymerization, anionic polymerization, or cationic polymerization can be used. Radical polymerization is preferably used because it is easy to produce.
[0097] The polymerization method generally employed is a method in which the above-mentioned monomer A, monomer B, monomer C, and, if necessary, other monomers are copolymerized by stirring and heating together with a polymerization initiator in a polymerization solvent.
[0098] The polymerization temperature is not particularly limited, but is preferably 25 to 100° C., and more preferably 30 to 80° C. The polymerization time is also not particularly limited, but is preferably 30 minutes to 24 hours, and more preferably 1 to 8 hours.
[0099] The polymerization solvent is preferably an aqueous solvent such as water or alcohols such as methanol, ethanol, propanol, n-butanol, 2,2,2-trifluoroethanol, etc. From the viewpoint of dissolving the raw materials used in the polymerization, these may be used alone or in combination of two or more.
[0100] The concentration of the polymerizable monomers is not particularly limited, but is preferably 0.05 to 1 g / mL, more preferably 0.1 to 0.5 g / mL, as the total solid content (g) of each polymerizable monomer relative to the polymerization solvent (mL). The preferred ratio of the amount (mol) of each monomer to the total amount (mol) of all monomers is as described above.
[0101] The reaction solution containing the polymerizable monomer may be degassed before the polymerization initiator is added. The degassing may be performed, for example, by bubbling the reaction solution with an inert gas such as nitrogen gas or argon gas for about 0.5 to 5 hours. During the degassing, the reaction solution may be heated to about 30 to 100°C.
[0102] For producing the polymer, a conventionally known polymerization initiator can be used, and is not particularly limited. For example, azo-based polymerization initiators such as 2,2'-azobisisobutyronitrile, 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile), 4,4'-azobis(4-cyanovaleric acid), 2,2'-azobis(2,4-dimethylvaleronitrile) and the like; and redox-based polymerization initiators in which an oxidizing agent such as persulfates, e.g. potassium persulfate (KPS), sodium persulfate, ammonium persulfate, etc., and peroxides, e.g. hydrogen peroxide, t-butyl peroxide, methyl ethyl ketone peroxide, etc., are combined with a reducing agent such as sodium sulfite, sodium hydrogen sulfite, ascorbic acid, etc. can be used.
[0103] The amount of the polymerization initiator to be added is preferably 0.001 to 10 mol %, more preferably 0.01 to 5 mol %, based on the total amount (mol) of polymerizable monomers.
[0104] Furthermore, if necessary, chain transfer agents, polymerization rate regulators, surfactants, and other additives may be appropriately used during the polymerization.
[0105] The atmosphere in which the polymerization reaction is carried out is not particularly limited, and the reaction can be carried out in an air atmosphere or an inert gas atmosphere such as nitrogen gas or argon gas, etc. During the polymerization reaction, the reaction liquid may be stirred.
[0106] The copolymer may precipitate during the polymerization reaction. After polymerization, the copolymer can be purified by a common purification method such as reprecipitation, dialysis, ultrafiltration, extraction, or the like.
[0107] The purified copolymer can be dried by any method such as freeze-drying, vacuum drying, spray drying, or heat drying. From the viewpoint of having little effect on the physical properties of the polymer, freeze-drying or vacuum drying is preferred.
[0108] The amount of unreacted monomer contained in the obtained copolymer is preferably 0.01% by weight or less based on the total weight of the copolymer. The less the amount of unreacted monomer, the more preferable (lower limit: 0% by weight). The amount of residual monomer can be measured by a known method such as high performance liquid chromatography.
[0109] In addition, the presence and ratio of the structural units derived from each polymerizable monomer in the hydrophilic copolymer (1) in the adhesive layer can be confirmed by analyzing the peak intensity of the group contained in each structural unit using known means such as IR, NMR, pyrolysis GC / MS, etc. In this specification, the presence and ratio of the structural units derived from each polymerizable monomer in the hydrophilic copolymer (1) in the adhesive layer are measured according to the following method.
[0110] (Method of detecting and measuring the presence and proportion of structural units derived from each polymerizable monomer in hydrophilic copolymer (1) in adhesive layer) With the surface of the medical device swollen with heavy water or the like, the medical device is precisely cut obliquely to prepare an inclined cross section of the medical device. The adhesive layer portion located near the substrate of the medical device is cut from the cross section, and the material of the adhesive layer portion is collected. Next, the material of the adhesive layer portion is packed tightly into a sample tube for solid-state NMR to prepare a sample, and NMR is measured. Here, peaks specific to the site specific to the structural unit (A) (e.g., sulfobetaine structure); the site specific to the structural unit (B) (e.g., salt of sulfonic acid group); and the site specific to the structural unit (C) (e.g., benzophenone group) are confirmed, and if these peaks are confirmed, it is determined that the corresponding structural unit is present in the sample. In addition, the concentration (concentration (a)) of the site specific to the structural unit (A) (e.g., sulfobetaine structure); the concentration (concentration (b)) of the site specific to the structural unit (B) (e.g., salt of sulfonic acid group); and the concentration (concentration (c)) of the site specific to the structural unit (C) (e.g., benzophenone group) are measured, respectively. The ratio of these concentrations (a), (b), and (c) is regarded as the abundance ratio of the structural units derived from each polymerizable monomer in the hydrophilic copolymer (1). The analytical device and measurement conditions used in the above measurement are as follows.
[0111] Analytical equipment: JEOL Ltd., NM080006 Measurement conditions: Heavy water, or a mixture of heavy water and a heavy solvent such as a lower alcohol.
[0112] [Surface lubricant layer] The surface lubricating layer in the present invention is formed on at least a part of the adhesive layer, and is composed of (i) hyaluronic acid or a salt thereof, and (ii) a constitutional unit derived from a polymerizable monomer (A') having a sulfobetaine structure and a sulfonic acid group (-SO 3 H), sulfate group (-OSO 3 H) and sulfite groups (-OSO 2 The hydrophilic copolymer (2) includes a structural unit derived from a polymerizable monomer (B') having at least one group selected from the group consisting of groups of H) and salts thereof, and a structural unit derived from a polymerizable monomer (C') having a photoreactive group. Here, the surface lubricating layer does not need to be formed on the entire surface of the adhesive layer. The surface lubricating layer may be formed on the surface portion (part) of the contact layer that comes into contact with body fluids, but it is preferable that the surface of the adhesive layer is formed.
[0113] The surface lubricating layer contains (i) hyaluronic acid (salt) and (ii) hydrophilic copolymer (2). Of these, (ii) hydrophilic copolymer (2) exhibits lubricity when wet (for example, when in contact with aqueous liquids such as body fluids or physiological saline). (i) hyaluronic acid (salt) acts to retain aqueous liquid. In addition, the presence of hyaluronic acid (salt) moderately reduces the crosslink density of the surface lubricating layer. Therefore, aqueous liquids easily enter the surface lubricating layer, and the hydrophilic copolymer (2) easily exhibits lubricity (gel hydration lubrication). In addition, under high load conditions, the surface lubricating layer forms a hydration layer between the inner surface of the biological lumen and the medical device due to the aqueous liquid retained by the surface lubricating layer. Therefore, it is considered that the hydrophilic copolymer (2) can exhibit lubricity by contacting a sufficient amount of aqueous liquid even under high load conditions. Note that the above mechanism is an assumption, and the present invention is not limited by the above assumption.
[0114] In the present invention, as long as it does not affect the effect of the present invention, it is acceptable to have another layer between the surface lubricating layer and the adhesive layer, but preferably, the surface lubricating layer is located directly above the adhesive layer.In addition, as long as it does not affect the effect of the present invention, it is acceptable to have another layer on the surface lubricating layer, but preferably, no other layer is disposed on the surface lubricating layer (the surface lubricating layer is the outermost layer).This form allows the effect (lubricity) of the present invention to be effectively exhibited.
[0115] The thickness of the surface lubricating layer is not particularly limited. From the viewpoints of lubricity, durability (lubrication maintenance), adhesion to the adhesive layer, etc., the thickness (dry film thickness) of the surface lubricating layer is preferably 0.1 to 100 μm, more preferably 0.2 to 50 μm.
[0116] The components contained in the surface lubricating layer according to the present invention (hyaluronic acid (salt), hydrophilic copolymer (2), etc.) will be described below.
[0117] (Hyaluronic acid (salt)) The surface lubricating layer contains hyaluronic acid (salt). Here, hyaluronic acid is composed of a basic structure (repeating unit) of GlcUA-GlcNAc, which is formed by binding glucuronic acid (GlcUA) and N-acetylglucosamine (GlcNAc). In addition, the salt of hyaluronic acid is not particularly limited as long as it is in the form of a medicamentarily or pharmacologically acceptable salt. For example, alkali metal salts such as sodium salt and potassium salt, alkaline earth metal salts such as calcium salt and magnesium salt, metal salts such as ammonium salt and aluminum salt; and salts with organic amines such as methylamine, triethylamine, triethanolamine, morpholine, piperazine, pyrrolidine, tripyridine, picoline, etc. Among these, from the viewpoint of water retention and biocompatibility, inorganic salts are preferred, alkali metal salts are preferred, and sodium salts are particularly preferred.
[0118] The weight-average molecular weight of hyaluronic acid (salt) is preferably 1,000 to 4,000,000, more preferably 10,000 to 3,500,000, particularly preferably 50,000 to 3,000,000, and most preferably 80,000 to 2,500,000. With such a weight-average molecular weight, hyaluronic acid (salt) can exhibit a higher water-retaining effect (water-retaining capacity) (hence, lubricity and further durability (lubrication maintenance) can be further improved).
[0119] The hyaluronic acid (salt) may be any of natural products, synthetic products, and commercially available products, such as those available from Sigma-Aldrich Co.
[0120] (Hydrophilic copolymer (2)) The surface lubricating layer contains, in addition to hyaluronic acid (salt), a hydrophilic copolymer (2). The hydrophilic copolymer (2) is a structural unit derived from a polymerizable monomer (A') having a sulfobetaine structure and a sulfonic acid group (-SO 3 H), sulfate group (-OSO 3 H) and sulfite groups (-OSO 2H) and a structural unit derived from a polymerizable monomer (B') having at least one group selected from the group consisting of salt groups thereof, and a structural unit derived from a polymerizable monomer (C') having a photoreactive group. The hydrophilic copolymer (2) contained in the surface lubricating layer may have the same structure as the hydrophilic copolymer (1) contained in the adhesive layer, or may have a different structure. From the viewpoint of the fixation strength (and therefore durability) between the adhesive layer and the surface lubricating layer, it is preferable that the hydrophilic copolymer (1) and the hydrophilic copolymer (2) have the same structure. In addition, in the above-mentioned form, only one process for producing the hydrophilic copolymer is required, and the amount of the hydrophilic copolymer used increases, which is particularly preferable from the viewpoint of the number of manufacturing steps during mass production, the cost of the product, and the like. Here, "hydrophilic copolymer (1) and hydrophilic copolymer (2) have the same structure" means that the types of the structural units (A), (B) and (C) constituting hydrophilic copolymer (1) and the structural units derived from other monomers, if any, are all the same (hydrophilic copolymers (1) and (2) are composed of the same structural units). From the viewpoint of the effect of improving the fixation strength (and therefore durability) between the adhesive layer and the surface lubricating layer, productivity, etc., it is preferable that the types and compositions (content ratios (molar ratios)) of the structural units constituting hydrophilic copolymers (1) and (2) are all the same (hydrophilic copolymers (1) and (2) are composed of the same structural units and the same composition).
[0121] In the surface lubricating layer, the ratio (mixing ratio) of hyaluronic acid (salt) and hydrophilic copolymer (2) is not particularly limited.In the surface lubricating layer, the ratio (mixing ratio) of hyaluronic acid (salt) and hydrophilic copolymer (2) is preferably 5 parts by weight or more and 1000 parts by weight or less, more preferably more than 5 parts by weight and less than 500 parts by weight, more preferably more than 5 parts by weight and 450 parts by weight or less, more preferably more than 5 parts by weight and 350 parts by weight or less, more preferably 10 to 250 parts by weight, particularly preferably 10 to 200 parts by weight, and most preferably 50 to 200 parts by weight. That is, in a preferred embodiment of the present invention, the hydrophilic copolymer (2) is contained in the surface lubricating layer at a ratio of 5 parts by weight or more and 1000 parts by weight or less (more preferably more than 5 parts by weight and less than 500 parts by weight, more preferably more than 5 parts by weight and 450 parts by weight, even more preferably 5 to 350 parts by weight, even more preferably 10 to 250 parts by weight, particularly preferably 10 to 200 parts by weight, and most preferably 50 to 200 parts by weight) per part by weight of hyaluronic acid or its salt. With such an existence ratio (mixing ratio), the water retention effect of hyaluronic acid (salt) and the lubricity of hydrophilic copolymer (2) can be exhibited in a better balance. In addition, when the surface lubricating layer contains two or more kinds of hyaluronic acid (salt), the above "1 part by weight" means that the total amount of these hyaluronic acids (salts) is 1 part by weight. Similarly, when the surface lubricating layer contains two or more kinds of hydrophilic copolymers (2), the amount (parts by weight) of the hydrophilic copolymer (2) means the total amount of these hydrophilic copolymers (2). Furthermore, the above-mentioned existence ratio (mixing ratio) is substantially equivalent to the ratio of the total amount (weight) of hydrophilic copolymer (2) to the total amount (weight) of hyaluronic acid (salt) when forming a surface lubricating layer.
[0122] Here, the presence and ratio (composition) of the constituent units derived from each polymerizable monomer in the hydrophilic copolymer (2) in the surface lubricating layer and the presence of hyaluronic acid (salt) can be confirmed by analyzing the peak intensity of the group contained in each constituent unit using known means such as IR, NMR, pyrolysis GC / MS. In this specification, the presence and ratio (composition) of the constituent units derived from each polymerizable monomer in the hydrophilic copolymer (2) in the surface lubricating layer can be detected and measured by the same method as described above (detection and measurement method of the presence and ratio of the constituent units derived from each polymerizable monomer in the hydrophilic copolymer (1) in the adhesive layer). In addition, hyaluronic acid (salt) in the surface lubricating layer can also be confirmed in the same manner as described above (detection and measurement method of the presence and ratio of the constituent units derived from each polymerizable monomer in the hydrophilic copolymer (1) in the adhesive layer). That is, in the above method, peaks specific to the site specific to hyaluronic acid (salt) (e.g., carboxyl group or its salt) are confirmed, and if these peaks are confirmed, it is determined that hyaluronic acid (salt) is present in the sample.
[0123] In addition, the ratio (mixing ratio) of hyaluronic acid (salt) and hydrophilic copolymer (2) in surface lubrication layer can also be measured by using the same known means as above.In this specification, the ratio (mixing ratio) of hyaluronic acid (salt) and hydrophilic copolymer (2) in surface lubrication layer is measured according to the following method.
[0124] (Method for measuring the ratio (mixture ratio) of hyaluronic acid (salt) and hydrophilic copolymer (2) in the surface lubricating layer) With the surface of the medical device swollen with heavy water or the like, the medical device is precisely cut obliquely to prepare an inclined cross section of the medical device. The surface lubricant layer portion located near the surface of the medical device is cut from the cross section, and the material of the surface lubricant layer portion is collected. Next, the material of the surface lubricant layer portion is packed tightly into a sample tube for solid-state NMR, a sample is prepared, and NMR is measured. Here, the concentration (concentration (c')) of the portion (e.g., benzophenone group) specific to the structural unit (C') is measured. Based on this concentration (c') and the composition of the hydrophilic copolymer (2), the copolymer concentration is calculated (concentration (c")). This concentration (c") is regarded as the amount of hydrophilic copolymer (2) in the surface lubricant layer. Separately, in the same manner, the concentration of the portion (e.g., carboxyl group or its salt) specific to hyaluronic acid (salt) is measured (concentration (h)). This concentration (h) is regarded as the amount of hyaluronic acid (salt) in the surface lubricant layer. The value obtained by dividing the concentration (c") by the concentration (h) (concentration (c") / concentration (h)) is the abundance ratio (mixing ratio) of hyaluronic acid (salt) and hydrophilic copolymer (2) in the surface lubricating layer. The analytical equipment and measurement conditions used in the above measurement are as follows.
[0125] Analytical equipment: JEOL Ltd., NM080006 Measurement conditions: Heavy water, or a mixture of heavy water and a heavy solvent such as a lower alcohol.
[0126] Hereinafter, each polymerizable monomer constituting the hydrophilic copolymer (2) contained in the surface lubricating layer according to the present invention will be described.
[0127] (Polymerizable monomer (A')) The hydrophilic copolymer (2) has a structural unit (structural unit (A')) derived from a polymerizable monomer (A') having a sulfobetaine structure. Here, the structural unit (A') constituting the hydrophilic copolymer (2) may be a single type, or a combination of two or more types. That is, the structural unit (A') may be composed of only one type of structural unit (A'), or may be composed of two or more types of structural units (A'). The multiple structural units (A') may be present in a block form or a random form.
[0128] The polymerizable monomer (A') (monomer A') is a polymerizable monomer having a sulfobetaine structure. The sulfobetaine structure contained in the constituent unit derived from the monomer A' has excellent lubricity-imparting effect. Therefore, it is considered that the hydrophilic copolymer (2) having the constituent unit derived from the monomer A' has excellent lubricity. In addition, the homopolymer of the monomer A' is soluble in an aqueous NaCl solution, but is insoluble or difficult to dissolve in water or lower alcohol. Therefore, it is suggested that the sulfobetaine structure may have strong electrostatic interaction. For this reason, a strong cohesive force acts inside the surface lubricating layer containing the hydrophilic copolymer according to the present invention. It is considered that the surface lubricating layer has high strength (excellent durability). Note that the above is an assumption, and the present invention is not limited by the above assumption.
[0129] Specific definitions and examples of the polymerizable monomer (A') are the same as those of the polymerizable monomer (A) in the adhesive layer, and therefore, description thereof will be omitted here.
[0130] From the viewpoint of further improving lubricity and durability (lubrication maintenance), the monomer A' is preferably a compound represented by the above formula (1). That is, in a preferred embodiment of the present invention, the polymerizable monomer (A') is represented by the above formula (1).
[0131] (Polymerizable monomer (B')) The hydrophilic copolymer (2) contains sulfonic acid groups (-SO 3 H), sulfate group (-OSO 3 H) and sulfite groups (-OSO 2 H), and salt groups thereof. The structural unit (B') constituting the hydrophilic copolymer (2) may be a single type, or a combination of two or more types. That is, the structural unit (B') may be composed of only one type of structural unit (B'), or may be composed of two or more types of structural units (B'). The multiple structural units (B') may be present in a block form or a random form.
[0132] The polymerizable monomer (B') (monomer B') has a sulfonic acid group (-SO 3 H), sulfate group (-OSO 3 H) and sulfite groups (-OSO 2 H) and salts thereof. By introducing such a group, the hydrophilic copolymers are anionized in an aqueous solvent, and electrostatic repulsion occurs between the hydrophilic copolymers. As a result, the electrostatic interaction between the sulfobetaine structures between the hydrophilic copolymers and the hydrophobic interaction between the photoreactive groups between the hydrophilic copolymers are reduced. Therefore, the solvent solubility of the copolymer (particularly the solubility in water, lower alcohol, or a mixed solvent of water and lower alcohol) is improved. This improvement effect is particularly remarkable when the photoreactive group of the monomer C' is a benzophenone group. Since the benzophenone group has multiple aromatic rings, it is easy to associate through π-π interactions, and as a result, the polymer containing the benzophenone group is easily aggregated and insoluble. Therefore, it is considered that by introducing a structural unit derived from the polymerizable monomer (B'), electrostatic repulsion occurs as described above, and the association between the benzophenone groups is suppressed, so that the solubility or dispersibility of the polymer is dramatically improved. Note that the above mechanism is an assumption, and the present invention is not limited by the above assumption. Alternatively, even when the monomer C' contains an ester group, the above-mentioned improving effect can be satisfactorily obtained.
[0133] Specific definitions and examples of the polymerizable monomer (B') are the same as those of the polymerizable monomer (B) in the adhesive layer, and therefore will not be described here.
[0134] Among them, from the viewpoint of further improving the solvent solubility, the polymerizable monomer (B') is preferably a compound represented by the following formula (2), (3) or (4), and more preferably a compound represented by the following formula (2). That is, in a preferred embodiment of the present invention, the polymerizable monomer (B') is represented by the following formula (2), (3) or (4). In a more preferred embodiment of the present invention, the polymerizable monomer (B') is represented by the following formula (2). The definitions of the following formulas (2) to (4) are the same as those in the above (polymerizable monomer (B)), and therefore explanations will be omitted here.
[0135] [ka]
[0136] In the above formula (2), R 21 is a hydrogen atom or a methyl group, Z 2 is an oxygen atom or -NH-, R 22 is a linear or branched alkylene group having 1 to 20 carbon atoms, X is a sulfonic acid group (-SO 3 H), sulfate group (-OSO 3 H) and sulfite groups (-OSO 2 H) and salts thereof;
[0137] [ka]
[0138] In the above formula (3), R 31 is a hydrogen atom or a methyl group, R 32 is a single bond or a linear or branched alkylene group having 1 to 20 carbon atoms, X is a sulfonic acid group (-SO 3 H), sulfate group (-OSO 3 H) and sulfite groups (-OSO 2 H) and salts thereof;
[0139] [ka]
[0140] In the above formula (4), R 41 is a hydrogen atom or a methyl group, R 42is a linear or branched alkylene group having 1 to 20 carbon atoms, X is a sulfonic acid group (-SO 3 H), sulfate group (-OSO 3 H) and sulfite groups (-OSO 2 H) and salts thereof.
[0141] (Polymerizable monomer (C')) The hydrophilic copolymer (2) has a structural unit (structural unit (C')) derived from a polymerizable monomer (C') having a photoreactive group. Here, the structural unit (C') constituting the hydrophilic copolymer (2) may be a single type, or a combination of two or more types. That is, the structural unit (C') may be composed of only one type of structural unit (C'), or may be composed of two or more types of structural units (C'). The multiple structural units (C') may be present in a block form or a random form.
[0142] The polymerizable monomer (C') (monomer C') is a polymerizable monomer having a photoreactive group. The polymer monomer C' allows the surface lubricating layer containing the hydrophilic copolymer (2) to be firmly fixed to the base layer via the adhesive layer. Therefore, the medical device can exhibit sufficient durability (lubrication retention).
[0143] Specific definitions and examples of the polymerizable monomer (C') are the same as those of the polymerizable monomer (C) in the adhesive layer, and therefore will not be described here.
[0144] From the viewpoint of forming a covalent bond with the adhesive layer and firmly fixing it to the base layer, the photoreactive group of the polymerizable monomer (C') is preferably the same as the photoreactive group of the polymerizable monomer (C) of the hydrophilic copolymer (1) contained in the adhesive layer. That is, in a preferred embodiment of the present invention, the polymerizable monomer (C') has a group having a benzophenone structure.
[0145] The hydrophilic copolymer (2) may contain structural units derived from polymerizable monomers other than the above-mentioned monomer A', monomer B', and monomer C' (hereinafter also referred to as "other monomers") within a range that does not impair the effects of the present invention. In the hydrophilic copolymer (2) of the present invention, the content of structural units derived from other monomers is preferably less than 10 mol%, more preferably less than 5 mol%, and even more preferably less than 1 mol% relative to the total amount of structural units derived from all monomers (100 mol%) (lower limit: more than 0 mol%). In addition, when the structural units derived from other monomers are composed of two or more types of structural units, the composition of the structural units derived from the above-mentioned other monomers is the ratio (molar ratio (mol%)) of the total structural units derived from other monomers to the total of structural units derived from all monomers (100 mol%). Preferably, the hydrophilic copolymer (2) of the present invention is composed only of monomer A', monomer B', and monomer C' (composition of other monomers = 0 mol%). The mole percent is substantially equal to the ratio of the amount (mol) of the other monomer to the total amount (mol) of all monomers charged when producing a polymer.
[0146] The terminal of the hydrophilic copolymer (2) is not particularly limited and is appropriately determined depending on the type of raw material used, but is usually a hydrogen atom. The structure of the copolymer is also not particularly limited and may be any of a random copolymer, an alternating copolymer, a periodic copolymer, and a block copolymer.
[0147] The weight average molecular weight (Mw) of the hydrophilic copolymer (2) is preferably several thousand to several million, more preferably 1,000 to 1,000,000, and particularly preferably 5,000 to 500,000. In the present invention, the "weight average molecular weight" is a value measured by gel permeation chromatography (GPC) using polyethylene glycol as a standard substance.
[0148] [Method for producing hydrophilic copolymer (2)] The method for producing the hydrophilic copolymer (2) is not particularly limited, and the specific description is the same as that of the [Method for producing the hydrophilic copolymer (1)] for the adhesive layer described above, so that the description is omitted here.
[0149] [Manufacturing method of medical devices] The method for producing a medical device according to the present invention is not particularly limited except that an adhesive layer is formed using the hydrophilic copolymer (1) and a surface lubricating layer is formed using the hydrophilic copolymer (2) and hyaluronic acid (salt), and a known method can be applied in the same manner or with appropriate modification. For example, a method is preferred in which the hydrophilic copolymer (1) is dissolved in a solvent to prepare a coating liquid, the coating liquid is coated on the base layer of the medical device to form an adhesive layer, and then the hydrophilic copolymer (2) and hyaluronic acid (salt) are dissolved in a solvent to prepare a coating liquid, and the coating liquid is coated on the adhesive layer to form a surface lubricating layer. That is, the present invention also provides a method for producing a medical device according to the present invention, which comprises applying a coating liquid (1) containing the hydrophilic copolymer (1) to the base layer to form an adhesive layer, and applying a coating liquid (2) containing the hyaluronic acid or its salt and the hydrophilic copolymer (2) to the adhesive layer to form a surface lubricating layer. By such a method, lubricity and durability (lubrication maintenance) can be imparted to the surface of the medical device.
[0150] (Adhesive layer application process) In the above method, the solvent used to dissolve the hydrophilic copolymer (1) is preferably water, a lower alcohol, or a mixed solvent of water and a lower alcohol from the viewpoints of work safety (low toxicity) and solubility. Here, the lower alcohol refers to a primary alcohol having 1 to 3 carbon atoms, that is, methanol, ethanol, n-propanol, or isopropanol. The above lower alcohols may be used alone or in combination of two or more kinds.
[0151] In addition, the concentration of the hydrophilic copolymer (1) in the coating liquid (1) is not particularly limited, but is preferably 0.01 to 50% by weight, more preferably 0.05 to 40% by weight, and even more preferably 0.1 to 30% by weight. Within such a range, the coating property of the coating liquid (1) is good, and the resulting adhesive layer has sufficient lubricity and durability (lubrication maintenance). In addition, a uniform adhesive layer of a desired thickness can be easily obtained by one coating. Therefore, the hydrophilic copolymer (1) can form a strong and uniform chemical bond with the base layer by the subsequent irradiation with active energy rays (adhesive layer fixing step). In addition, it is preferable in terms of production efficiency. Note that, if the concentration of the hydrophilic copolymer (1) is less than 0.01% by weight, a sufficient amount of the hydrophilic copolymer (1) may not be fixed to the surface of the base layer. Also, if the concentration of the hydrophilic copolymer (1) is more than 50% by weight, the viscosity of the coating liquid (1) becomes too high, and an adhesive layer of a uniform thickness may not be obtained. However, even if it is outside the above range, it can be used sufficiently as long as it does not affect the effects of the present invention.
[0152] The amount of coating liquid (1) to be applied is not particularly limited, but is preferably an amount that results in the above-mentioned thickness of the adhesive layer.
[0153] Before applying the coating liquid (1), the surface of the substrate layer may be pretreated by ultraviolet irradiation treatment, plasma treatment, corona discharge treatment, flame treatment, oxidation treatment, silane coupling treatment, phosphoric acid coupling treatment, or the like. When the solvent of the coating liquid (1) is only water, it is difficult to apply it to the hydrophobic substrate layer surface, but the substrate layer surface is made hydrophilic by subjecting the substrate layer surface to plasma treatment. This improves the wettability of the coating liquid (1) to the substrate layer surface, and a uniform adhesive layer can be formed. In addition, by subjecting the substrate layer surface, which does not have a C-H bond, such as a metal or a fluororesin, to the above treatment, it becomes possible to form a covalent bond with the photoreactive group of the hydrophilic copolymer (1).
[0154] The method for applying the coating liquid (1) to the surface of the base layer is not particularly limited, and any conventionally known method can be applied, such as a coating / printing method, a dipping method (dipping method, dip coating method), a spraying method (spray method), a mixed solution impregnated sponge coating method, etc. Among these, the dipping method (dipping method, dip coating method) is preferred.
[0155] (Adhesive layer drying process) As described above, after the coating liquid (1) containing the hydrophilic copolymer (1) of the present invention is applied to the surface of the substrate layer, it is preferable to remove the substrate layer from the coating liquid (1) and dry the coating. The drying conditions are not particularly limited as long as the solvent can be removed from the coating, and hot air treatment using a dryer or the like may be performed, or natural drying may be performed. The pressure conditions during drying are also not particularly limited, and drying may be performed under normal pressure (atmospheric pressure), or under pressure or reduced pressure. For example, an oven, a reduced pressure dryer, etc. can be used as the drying means (device), but in the case of natural drying, no particular drying means (device) is required.
[0156] (Adhesive layer fixing process) The coating film after the drying step is irradiated with active energy rays. This activates the photoreactive group in the coating film (monomer C of hydrophilic copolymer (1)), and a chemical bond is formed between the photoreactive group and the alkyl group (hydrocarbon group) contained in the base layer. More specifically, a combination of a photoreactive group having a benzophenone structure and a resin (material having a hydrocarbon group) constituting the base layer will be described. When the hydrophilic copolymer (1) contains a photoreactive group having a benzophenone structure, two radicals are generated in the photoreactive group by irradiation with ultraviolet light. One of these radicals extracts a hydrogen atom from the alkyl group (hydrocarbon group) in the resin, and instead, one radical is generated in the material. After that, the remaining radical in the photoreactive group and the radical generated in the material combine to form a covalent bond between the photoreactive group of the hydrophilic copolymer (1) in the adhesive layer and the material (resin) in the base layer. By such chemical bonds, the adhesive layer containing the hydrophilic copolymer (1) is firmly fixed to the base layer. Therefore, the adhesive layer can exhibit sufficient durability (lubrication retention).
[0157] Examples of active energy rays include ultraviolet rays (UV), electron beams, gamma rays, etc., but ultraviolet rays or electron beams are preferred, and ultraviolet rays are more preferred in consideration of their effects on the human body. When the active energy rays are ultraviolet rays, the wavelength of irradiation can be appropriately selected from wavelengths that can activate photoreactive groups. Specifically, the wavelength range of ultraviolet rays is preferably 200 to 400 nm, and more preferably 220 to 390 nm. Moreover, ultraviolet irradiation is preferably carried out under temperature conditions of 10 to 100°C, more preferably 20 to 80°C. The irradiation intensity of ultraviolet rays is not particularly limited, but is preferably 1 to 5000 mW / cm. 2 , more preferably 10 to 1000 mW / cm 2 , and more preferably 50 to 500 mW / cm 2 The integrated amount of ultraviolet light (integrated amount of ultraviolet light on the adhesive layer before the surface lubricating layer is applied) is not particularly limited, but is preferably 100 to 100,000 mJ / cm. 2 and more preferably 500 to 50,000 mJ / cm 2Examples of the device for irradiating ultraviolet rays include a high pressure mercury lamp, a low pressure mercury lamp, a metal halide lamp, a xenon lamp, a halogen lamp, etc. The method of irradiating active energy rays is not particularly limited, and may be performed from one direction, from multiple directions, while rotating the irradiation source, or while rotating the irradiated object (a substrate layer having a coating of an adhesive layer formed thereon).
[0158] After the above-mentioned irradiation with active energy rays, the coating film may be washed with a solvent (for example, the solvent used in preparing the coating liquid (1)) to remove unreacted hydrophilic copolymer (1).
[0159] The fixation of the coating (adhesive layer) to the substrate layer can be confirmed by using known analytical means such as FT-IR, XPS, TOF-SIMS, etc. For example, it can be confirmed by performing FT-IR measurement before and after irradiation with active energy rays, and comparing the ratio of the peak of the bond formed by irradiation with active energy rays to the peak of the bond that remains unchanged.
[0160] By the above method, in the medical device according to the present invention, an adhesive layer containing the hydrophilic copolymer (1) is formed on the surface of the base layer.
[0161] (Surface lubricant layer application process) Here, the hydrophilic copolymer (2) and hyaluronic acid (salt) are dissolved in a solvent to prepare a coating liquid (2), and the coating liquid (2) is applied onto the adhesive layer formed above. In the above method, the solvent used to dissolve the hydrophilic copolymer (2) and hyaluronic acid (salt) is preferably water, a lower alcohol, or a mixed solvent of water and a lower alcohol from the viewpoints of work safety (low toxicity) and solubility. Here, the lower alcohol refers to a primary alcohol having 1 to 3 carbon atoms, that is, methanol, ethanol, n-propanol, or isopropanol. The above lower alcohol may be used alone or in combination of two or more kinds. Here, the hydrophilic copolymer (2) and hyaluronic acid (salt) may be added to a solvent together, or may be added to the same solvent in sequence (hydrophilic copolymer (2) followed by hyaluronic acid (salt) or hyaluronic acid (salt) followed by hydrophilic copolymer (2)), or may be dissolved in a different solvent and then mixed. When the hydrophilic copolymer (2) and the hyaluronic acid (salt) are used in different solvents, the solvents may be the same or different, but in consideration of ease of operation, it is preferable that they are the same.
[0162] The concentration of the hydrophilic copolymer (2) in the coating liquid (2) is not particularly limited, but is preferably more than 0.05% by weight and less than 5% by weight, more preferably 0.1 to 4.5% by weight, even more preferably 0.1 to 3.5% by weight, even more preferably 0.2 to 3.5% by weight, and particularly preferably 0.5 to 1.0% by weight. Within such a range, the coating property of the coating liquid (2) is good, and a strong and uniform chemical bond can be formed with the adhesive layer (hydrophilic copolymer (1)) and hyaluronic acid (salt) by the subsequent irradiation of active energy rays (fixing process of the surface lubricating layer) (hence the surface lubricating layer has excellent lubricity and durability (lubrication maintenance)). In addition, it is preferable in terms of production efficiency. In addition, the concentration of the hyaluronic acid (salt) in the coating liquid (2) is not particularly limited, but is preferably more than 0.001% by weight and less than 1% by weight, more preferably 0.005 to 0.7% by weight, and even more preferably 0.01 to 0.5% by weight. Within this range, the coating liquid (2) has good applicability, and the surface lubricating layer obtained can exhibit sufficient water retention (therefore, the surface lubricating layer can exhibit excellent lubrication even under high load conditions). Here, the mixing ratio of the hydrophilic copolymer (2) and hyaluronic acid (salt) in the coating liquid (2) is not particularly limited, but it is preferably the same mixing ratio as described in the above-mentioned surface lubricating layer section.
[0163] The amount of coating liquid (2) to be applied is not particularly limited, but it is preferably an amount that results in the above-mentioned thickness of the surface lubricating layer.
[0164] The method for applying the coating liquid (2) to the adhesive layer surface is not particularly limited, and any conventionally known method can be applied, such as a coating / printing method, a dipping method (dipping method, dip coating method), a spraying method (spray method), a mixed solution impregnated sponge coating method, etc. Among these, the dipping method (dipping method, dip coating method) is preferred.
[0165] (Drying process of the surface lubricant layer) As described above, it is preferable to immerse the substrate layer on which the adhesive layer has been formed in advance in the coating liquid (2), and then remove the substrate layer from the coating liquid (2) and dry the coating. The drying conditions are not particularly limited as long as the solvent can be removed from the coating, and hot air treatment using a dryer or the like may be performed, or natural drying may be performed. The pressure conditions during drying are also not particularly limited, and drying may be performed under normal pressure (atmospheric pressure), or under pressure or reduced pressure. For example, an oven, a reduced pressure dryer, or the like may be used as the drying means (device), but in the case of natural drying, no particular drying means (device) is required.
[0166] (Surface lubricant layer fixing process) The coating film after the drying step is irradiated with active energy rays. This activates the photoreactive group of the hydrophilic copolymer (1) (monomer C) in the adhesive layer and the photoreactive group of the hydrophilic copolymer (2) (monomer C') in the surface lubricating layer, and a chemical bond is formed between the photoreactive group of the hydrophilic copolymer (1), the photoreactive group of the hydrophilic copolymer (2), and hyaluronic acid (salt). As an example, a combination of a photoreactive group having a benzophenone structure of the hydrophilic copolymer (1) in the adhesive layer, a photoreactive group having a benzophenone structure of the hydrophilic copolymer (2) in the surface lubricating layer, and hyaluronic acid (salt) will be described. When the hydrophilic copolymers (1) and (2) contain photoreactive groups having a benzophenone structure, two radicals are generated in the photoreactive group of each hydrophilic copolymer by irradiating them with ultraviolet light. One of these radicals extracts a hydrogen atom from an alkyl group (hydrocarbon group) in the hyaluronic acid (salt), and one radical is generated in the hyaluronic acid (salt) instead. After that, the remaining radicals in the photoreactive group and the radicals generated in the hyaluronic acid (salt) combine to form a covalent bond between the photoreactive group of the hydrophilic copolymer (1) in the adhesive layer and the hyaluronic acid (salt) in the surface lubricating layer, or between the photoreactive group of the hydrophilic copolymer (2) in the surface lubricating layer and the hyaluronic acid (salt). By such chemical bonding between the hyaluronic acid (salt) and the hydrophilic copolymer in the adhesive layer or surface lubricating layer, the surface lubricating layer is firmly fixed to the adhesive layer, and at the same time, the hyaluronic acid (salt) is firmly fixed in the surface lubricating layer. In addition, one of the two radicals in the hydrophilic copolymer (1) generated by ultraviolet irradiation pulls out a hydrogen atom from the alkyl group (hydrocarbon group) in the hydrophilic copolymer (2), and instead one radical is generated in the hydrophilic copolymer (2). Then, the remaining radical in the photoreactive group of the hydrophilic copolymer (1) and the radical generated in the hydrophilic copolymer (2) combine to form a covalent bond between the photoreactive group of the hydrophilic copolymer (1) in the adhesive layer and the hydrophilic copolymer (2) in the surface lubrication layer. Similarly, one of the two radicals in the hydrophilic copolymer (2) generated by ultraviolet irradiation abstracts a hydrogen atom from the alkyl group (hydrocarbon group) in the hydrophilic copolymer (1), and one radical is generated in the hydrophilic copolymer (1) in return.Thereafter, the remaining radicals in the photoreactive group of the hydrophilic copolymer (2) and the radicals generated in the hydrophilic copolymer (1) are bonded to each other, forming a covalent bond between the photoreactive group of the hydrophilic copolymer (1) in the adhesive layer and the hydrophilic copolymer (2) in the surface lubricating layer. The surface lubricating layer is also firmly fixed to the adhesive layer by such chemical bonding between the hydrophilic copolymer (1) in the adhesive layer and the hydrophilic copolymer (2) in the surface lubricating layer. Therefore, the surface lubricating layer can effectively exert the water-retaining effect of hyaluronic acid (salt) and can exhibit excellent lubricity. In addition, the water-retaining effect of the hyaluronic acid (salt) can be maintained for a long period of time, and excellent durability (lubrication maintenance) can be exhibited.
[0167] Examples of active energy rays include ultraviolet rays (UV), electron beams, gamma rays, etc., but ultraviolet rays or electron beams are preferred, and ultraviolet rays are more preferred in consideration of their effects on the human body. When the active energy rays are ultraviolet rays, the wavelength of irradiation can be appropriately selected from wavelengths that can activate photoreactive groups. Specifically, the wavelength range of ultraviolet rays is preferably 200 to 400 nm, and more preferably 220 to 390 nm. Moreover, ultraviolet irradiation is preferably carried out under temperature conditions of 10 to 100°C, more preferably 20 to 80°C. The irradiation intensity of ultraviolet rays is not particularly limited, but is preferably 1 to 5000 mW / cm. 2 , more preferably 10 to 1000 mW / cm 2 , and more preferably 50 to 500 mW / cm 2 The integrated amount of ultraviolet light (integrated amount of ultraviolet light on the surface lubricating layer) is not particularly limited, but is preferably 100 to 100,000 mJ / cm. 2 and more preferably 500 to 50,000 mJ / cm 2 Examples of the device for irradiating ultraviolet rays include a high pressure mercury lamp, a low pressure mercury lamp, a metal halide lamp, a xenon lamp, a halogen lamp, etc. The method of irradiating active energy rays is not particularly limited, and may be performed from one direction, from multiple directions, while rotating the irradiation source, or while rotating the irradiated object (a substrate layer having a coating of an adhesive layer formed thereon).
[0168] After the above-mentioned irradiation with active energy rays, the coating film may be washed with a solvent (for example, the solvent used in preparing the coating liquid (2)) to remove unreacted hydrophilic copolymer (2).
[0169] The fixation of the coating (surface lubricating layer) to the adhesive layer can be confirmed by using known analytical means such as FT-IR, XPS, TOF-SIMS, etc. For example, it can be confirmed by performing FT-IR measurement before and after irradiation with active energy rays, and comparing the ratio of the peak of the bond formed by irradiation with active energy rays to the peak of the bond that remains unchanged.
[0170] By the above method, in the medical device according to the present invention, a surface lubricating layer containing the hydrophilic copolymer (2) and hyaluronic acid (salt) is formed on the surface of the adhesive layer.
[0171] <Second aspect> A second aspect of the present invention is a polymerizable composition comprising a base layer, a polymerizable monomer (A) having a sulfobetaine structure, a sulfonic acid group (-SO 3 H), sulfate group (-OSO 3 H) and sulfite groups (-OSO 2 an adhesive layer comprising a hydrophilic copolymer (1) containing a structural unit derived from a polymerizable monomer (B) having at least one group selected from the group consisting of a ... 3 H), sulfate group (-OSO 3 H) and sulfite groups (-OSO 2 and a surface lubricating layer comprising a hydrophilic copolymer (2) containing a structural unit derived from a polymerizable monomer (B') having at least one group selected from the group consisting of groups consisting of groups of a polymerizable monomer (H) and salts thereof, and a structural unit derived from a polymerizable monomer (C') having a photoreactive group.
[0172] [Base material layer (base material)] The substrate layer used in this embodiment is the same as the [Substrate Layer (Substrate)] in the above <First embodiment>, and therefore a description thereof will be omitted here.
[0173] [Adhesive layer (hydrophilic copolymer (1))] The adhesive layer used in this embodiment is the same as the [adhesive layer (hydrophilic copolymer (1))] in the above <First embodiment>, so a description thereof will be omitted here.
[0174] [Surface lubricant layer] The main difference between the surface lubricating layer used in this embodiment is that the water-retaining material is not hyaluronic acid (salt), but polyelectrolyte and / or polysaccharide and / or nonionic polymer (at least one of polyelectrolyte, polysaccharide and nonionic polymer). Therefore, only the matters different from the [surface lubricating layer] in the above <First embodiment> will be described below. Therefore, the matters not described below are considered to be the same as the [surface lubricating layer] in the above <First embodiment>.
[0175] (polymer electrolyte) The polymer electrolyte is not particularly limited. Specific examples of the polymer electrolyte include acrylic acid, methacrylic acid, vinyl sulfonic acid, vinyl sulfate, vinyl phosphonic acid, vinyl phosphoric acid, vinyl boronic acid, citraconic acid, maleic acid, fumaric acid, crotonic acid, itaconic acid, methacryloxyethyl phosphate, methacryloxyethyl sulfate, styrene sulfonic acid, methacryloxyethyl sulfonic acid, and 2-acrylamidomethylpropanesulfonic acid (AMPS), 2-methyl-2-propenoic acid ethyl-2-phosphate ester (HEMA phosphate), methacryloyloxy PPG-7 phosphate, and the like. Examples of the polymer electrolyte include polymeric substances of anionic or anionizable ethylenically unsaturated monomers or their salts, such as phosphate, β-carboxyethyl acrylate, 3-acrylamido-3-methylbutanoic acid, and AMBA polyacrylic acid, and polymeric substances of amphoteric ethylenically unsaturated monomers, such as carboxybetaine (meth)acrylate, carboxybetaine (meth)acrylamide, sulfobetaine (meth)acrylate, sulfobetaine (meth)acrylamide, and phosphobetaine methacrylate (MPC). The polymer electrolyte may also be a polypeptide. Specific examples include polyglutamic acid, polyaspartic acid, and their salts. Here, the form of the salt is not particularly limited, and examples thereof include alkali metal salts (sodium salt, potassium salt, etc.) of the above monomers. The above polymer electrolyte may be used alone or in combination of two or more kinds. The above polymer electrolyte contains the above unsaturated monomer-derived constitutional unit at a ratio of more than 50 mol% (upper limit: 100 mol%) with respect to the total amount of all constitutional units constituting the polymer electrolyte, 100 mol%. When the polymer electrolyte is composed of two or more kinds of unsaturated monomer-derived constituent units, the composition of the constituent units is the ratio (molar ratio (mol%)) of the total of the unsaturated monomer-derived constituent units to the total of the constituent units derived from all monomers (100 mol%). The mol% is substantially the same as the ratio of the amount (mol) of the unsaturated monomer charged to the total amount (mol) of all monomers charged when producing a polymer. Among these, at least one (co)polymer selected from the group consisting of acrylic acid, styrenesulfonic acid, and salts thereof (particularly alkali metal salts) is preferred.In addition, when the polymer electrolyte falls under the category of hydrophilic copolymer (2), the polymer electrolyte is classified as hydrophilic copolymer (2).
[0176] The weight-average molecular weight of the polymer electrolyte is preferably 1,000 to 4,000,000, more preferably 10,000 to 3,500,000, particularly preferably 50,000 to 3,000,000, and most preferably 80,000 to 2,500,000. With such a weight-average molecular weight, the polymer electrolyte can exhibit a higher water retention effect (water retention ability) (hence, the lubricity and further durability (lubrication maintenance ability) can be further improved).
[0177] The polymer electrolyte may be either a synthetic product or a commercially available product.
[0178] (polysaccharide) The polysaccharide is not particularly limited. Specific examples include alginic acid, pectin, carrageenan, xanthan, chondroitin sulfate, gum arabic, guar gum, karaya gum, tragacanth gum, arabinoxylan, heparan sulfate, starch, gum, cellulose derivatives, carboxymethyl starch, starch phosphate, hydroxypropyl starch phosphate, starch sulfate, starch-2-hydroxypropyl citrate, carboxymethyl guar, carboxymethyl hydroxypropyl guar, other anionic galactomannan derivatives, carboxymethyl cellulose, polyanionic cellulose, cellulose sulfate, cellulose phosphate, and carboxyethyl cellulose, dextran, dextran sulfate, and dextrin. These polysaccharides may be in the form of a salt. Here, the form of the salt is not particularly limited, and examples thereof include alkali metal salts (sodium salt, potassium salt, etc.) of the above polysaccharides. The above polysaccharides may be used alone or in combination of two or more. Among these, chondroitin sulfate, carboxymethylcellulose and their salts (particularly alkali metal salts) are preferred, and chondroitin sulfate and carboxymethylcellulose are more preferred. When a polysaccharide falls under the category of hydrophilic copolymer (2), the polysaccharide is classified as hydrophilic copolymer (2).
[0179] The weight-average molecular weight of the polysaccharide is preferably 1,000 to 7,000,000, more preferably 10,000 to 5,000,000, particularly preferably 50,000 to 3,000,000, and most preferably 80,000 to 3,000,000. With such a weight-average molecular weight, the polysaccharide can exhibit a higher water retention effect (water retention capacity) (hence, the lubricity and further durability (lubrication maintenance ability) can be further improved).
[0180] The polysaccharides used may be either synthetic or commercially available.
[0181] (Non-ionic polymer) The nonionic polymer is not particularly limited. Specific examples include homopolymers or copolymers containing structural units derived from nonionic monomers such as vinylpyrrolidone, N,N-dimethylacrylamide, and N-isopropylacrylamide. The nonionic polymer may be used alone or in combination of two or more. The nonionic polymer contains the structural units derived from the nonionic monomer at a ratio of more than 50 mol% (upper limit: 100 mol%) relative to the total amount of all structural units constituting the nonionic polymer, which is 100 mol%. When the nonionic polymer is composed of structural units derived from two or more nonionic monomers, the composition of the structural units is the ratio (molar ratio (mol%)) of the total structural units derived from the nonionic monomer to the total amount (100 mol%) of the structural units derived from all monomers. The mol% is substantially equivalent to the ratio of the amount (mol) of the nonionic monomer to the total amount (mol) of the monomers when producing a polymer. In addition, when a nonionic polymer falls under the category of hydrophilic copolymer (2), the nonionic polymer is classified as hydrophilic copolymer (2).
[0182] The weight-average molecular weight of the nonionic polymer is preferably 1,000 to 3,000,000, more preferably 10,000 to 2,500,000, particularly preferably 50,000 to 2,000,000, and most preferably 80,000 to 2,000,000. With such a weight-average molecular weight, the nonionic polymer can exhibit a higher water retention effect (water retention capacity) (hence, the lubricity and further durability (lubrication maintenance ability) can be further improved).
[0183] The nonionic polymer may be either a synthetic product or a commercially available product.
[0184] Of the above water-retaining materials (hyaluronic acid (salts), polymer electrolytes, polysaccharides, nonionic polymers), from the viewpoint of water-retaining effect (water-retaining capacity), ionic hyaluronic acid (salts), polymer electrolytes, and polysaccharides are preferred, and hyaluronic acid (salts) and polysaccharides having hydroxyl groups in the main skeleton are more preferred.
[0185] The surface lubricating layer contains at least one of a polyelectrolyte, a polysaccharide, and a nonionic polymer in addition to the hydrophilic copolymer (2). That is, the present invention according to the second aspect includes the forms in which the surface lubricating layer contains a hydrophilic copolymer (2) and a polyelectrolyte; contains a hydrophilic copolymer (2) and a polysaccharide; contains a hydrophilic copolymer (2) and a nonionic polymer; contains a hydrophilic copolymer (2), a polyelectrolyte, and a polysaccharide; contains a hydrophilic copolymer (2), a polyelectrolyte, and a nonionic polymer; contains a hydrophilic copolymer (2), a polysaccharide, and a nonionic polymer; contains a hydrophilic copolymer (2), a polyelectrolyte, a polysaccharide, and a nonionic polymer.
[0186] In the surface lubricating layer, the ratio (mixing ratio) of at least one of the polymer electrolyte, polysaccharide and nonionic polymer to the hydrophilic copolymer (2) is not particularly limited.The ratio (mixing ratio) of at least one of the polymer electrolyte, polysaccharide and nonionic polymer to the hydrophilic copolymer (2) is preferably more than 0.1 parts by weight, more preferably 0.2 parts by weight or more, even more preferably 0.5 parts by weight or more, even more preferably 1 part by weight or more, even more preferably 5 parts by weight or more, even more preferably more than 5 parts by weight, even more preferably 10 parts by weight or more, particularly preferably 50 parts by weight or more, per 1 part by weight of at least one of the polymer electrolyte, polysaccharide and nonionic polymer in the surface lubricating layer. In addition, the presence ratio (mixing ratio) of at least one of the polymer electrolyte, polysaccharide, and nonionic polymer to the hydrophilic copolymer (2) in the surface lubrication layer is preferably less than 1,000 parts by weight, more preferably 750 parts by weight or less, even more preferably 500 parts by weight or less, even more preferably less than 500 parts by weight, even more preferably 450 parts by weight or less, even more preferably 350 parts by weight or less, even more preferably 250 parts by weight or less, even more preferably 200 parts by weight or less, and particularly preferably 100 parts by weight or less, per 1 part by weight of at least one of the polymer electrolyte, polysaccharide, and nonionic polymer. That is, in a preferred embodiment of the present invention, the hydrophilic copolymer (2) is contained in the surface lubricating layer at a ratio of more than 5 parts by weight and less than 500 parts by weight (more preferably more than 5 parts by weight and 450 parts by weight, even more preferably more than 5 parts by weight and 350 parts by weight, even more preferably 10 to 250 parts by weight, particularly preferably 10 to 200 parts by weight, and most preferably 50 to 100 parts by weight) per part by weight of at least one of the polymer electrolyte, polysaccharide, and nonionic polymer. With such an existence ratio (mixing ratio), the water retention effect of at least one of the polymer electrolyte, polysaccharide, and nonionic polymer and the lubricity of the hydrophilic copolymer (2) can be exhibited in a better balance. In addition, when the surface lubricating layer contains two or more polymer electrolytes, the above "1 part by weight" means that the total amount of these polymer electrolytes is 1 part by weight. Similarly, when the surface lubricating layer contains two or more polysaccharides, the above "1 part by weight" means that the total amount of these polysaccharides is 1 part by weight.Similarly, when the surface lubricating layer contains two or more nonionic polymers, the above "1 part by weight" means that the total amount of these nonionic polymers is 1 part by weight. Similarly, when the surface lubricating layer contains two or more of any of a polymer electrolyte, a polysaccharide, and a nonionic polymer, the above "1 part by weight" means that the total amount of the polymer electrolyte, the polysaccharide, and the nonionic polymer contained therein is 1 part by weight. Similarly, when the surface lubricating layer contains two or more hydrophilic copolymers (2), the amount of the hydrophilic copolymer (2) means the total amount (parts by weight) of these hydrophilic copolymers (2).
[0187] Here, the presence and ratio of the constitutional units derived from each polymerizable monomer in the hydrophilic copolymer (2) in the surface lubricating layer, as well as the presence of the polyelectrolyte, polysaccharide and nonionic polymer, can be confirmed by the same method as described in the above <First embodiment>. For example, in the case of sodium polyacrylate, the sodium carboxylate group (-COONa); in the case of polystyrene sulfonic acid, the sulfonic acid group; in the case of chondroitin sulfate, the sulfate group; or in the case of N,N-dimethylacrylamide polymer, the proton (hydrogen atom) of the methyl group adjacent to the amide group ( 1 1H-NMR), or the carbon atom adjacent to the amide group ( 13 C-NMR) or in the case of vinylpyrrolidone polymers, the carbon atom adjacent to the nitrogen atom ( 13 C-NMR) or the proton (hydrogen atom) bonded to that carbon atom ( 1 H-NMR), or the carbon atom adjacent to the carbonyl group ( 13 C-NMR) or the proton (hydrogen atom) bonded to that carbon atom ( 1 1H-NMR) or in the case of polymers of N-isopropylacrylamide, the carbon atom adjacent to the amide group ( 13 C-NMR) or the proton hydrogen atom bonded to that carbon) ( 1 In the case of H-NMR, the same method as described in the above <First embodiment> can be applied, except that a unique peak is confirmed for each.
[0188] In addition, the presence ratio (mixing ratio) of at least one of the polymer electrolyte, polysaccharide and nonionic polymer in the surface lubricating layer to the hydrophilic copolymer (2) is also measured by the same method as described in the above <First embodiment>.
[0189] [Medical device uses] The medical device according to the present invention is used in contact with body fluids, blood, etc., and has a surface that is lubricated in body fluids, physiological saline, and other aqueous liquids, thereby improving operability and reducing damage to tissue mucosa. Specific examples include catheters, stents, guidewires, etc. that are used in blood vessels. That is, the medical device according to one embodiment of the present invention is a catheter, stent, or guidewire. Other examples of the medical device include the following:
[0190] (a) Catheters that are inserted or left in the digestive tract via the mouth or nose, such as gastric catheters, nutritional catheters, and tube feeding tubes.
[0191] (b) Catheters that are inserted or placed in the airway or trachea via the mouth or nose, such as oxygen catheters, oxygen cannulas, endotracheal tubes and cuffs, tracheostomy tubes and cuffs, and endotracheal suction catheters.
[0192] (c) Catheters that are inserted or left in the urethra or ureter, such as urethral catheters, urinary catheters, and urethral balloon catheters.
[0193] (d) Catheters that are inserted or left in various body cavities, organs, or tissues, such as suction catheters, drainage catheters, and rectal catheters.
[0194] (e) Catheters that are inserted or left in blood vessels, such as indwelling needles, IVH catheters, thermodilution catheters, angiography catheters, vasodilator catheters, and dilators or introducers, as well as guide wires and stylets for these catheters.
[0195] (f) Artificial trachea, artificial bronchi, etc.
[0196] (g) Medical devices for extracorporeal circulation therapy (artificial lungs, artificial hearts, artificial kidneys, etc.) and their circuits. EXAMPLES
[0197] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. In each example, parts and percentages are all by weight. In the following examples, the room temperature storage conditions are all 23°C / 55% RH unless otherwise specified.
[0198] Production Example 1: Production of hydrophilic copolymer (A) A reaction solution was prepared by dissolving 1.82 g (6.5 mmol) of [2-(methacryloyloxy)ethyl]dimethyl-(3-sulfopropyl)ammonium hydroxide (MSPB) manufactured by Sigma-Aldrich, 1.46 g (3.2 mmol) of 50 wt% aqueous solution of 2-acrylamido-2-methyl-1-propanesulfonic acid sodium salt (AMPS(Na)) manufactured by Sigma-Aldrich, and 0.080 g (0.3 mmol) of 4-methacryloyloxybenzophenone (MBP) manufactured by MCC Unitech Co., Ltd. in 10 mL of a 2,2,2-trifluoroethanol / water (9 / 1 v / v) mixed solvent. Next, this reaction solution was placed in a 30 mL eggplant-shaped flask, oxygen was removed by sufficient nitrogen bubbling, and 2.8 mg (0.010 mmol) of the polymerization initiator 4,4'-azobis(4-cyanovaleric acid) was added, and the flask was quickly sealed and polymerized in a water bath at 75 °C for 3 hours. Next, reprecipitation was performed in acetone, and the supernatant was removed by decantation to obtain a copolymer (A).
[0199] The composition of the obtained copolymer (A) was MSPB:AMPS(Na):MBP=65:32:3 in mol%. Here, the obtained copolymer (A) corresponds to the hydrophilic copolymer (1) contained in the adhesive layer according to the present invention and the hydrophilic copolymer (2) contained in the surface lubricating layer according to the present invention. In addition, the weight average molecular weight (Mw) of the obtained copolymer was measured by GPC and was 180,000 in terms of polyethylene glycol.
[0200] Production Example 2: Production of hydrophilic copolymer (B) A reaction solution was prepared by dissolving 1.99g (6.5mmol) of [3-(methacryloylamino)propyl]dimethyl(3-sulfobutyl)ammonium hydroxide inner salt (MSBB) manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., 1.46g (3.2mmol) of 50% by weight aqueous solution of 2-acrylamido-2-methyl-1-propanesulfonic acid sodium salt (AMPS(Na)) manufactured by Sigma-Aldrich Co., Ltd., and 0.080g (0.3mmol) of 4-methacryloyloxybenzophenone (MBP) manufactured by MCC Unitech Co., Ltd. in 10mL of a 2,2,2-trifluoroethanol / water (9 / 1 v / v) mixed solvent. Next, this reaction solution was placed in a 30mL eggplant-shaped flask, oxygen was removed by sufficient nitrogen bubbling, and 2.8mg (0.010mmol) of the polymerization initiator 4,4'-azobis(4-cyanovaleric acid) was added, and the flask was quickly sealed and polymerized in a water bath at 75°C for 3 hours. Next, the mixture was reprecipitated in acetone, and the supernatant was removed by decantation to obtain a copolymer (B).
[0201] The composition of the obtained copolymer (B) was MSBB:AMPS(Na):MBP=65:32:3 in mol%. Here, the obtained copolymer (B) corresponds to the hydrophilic copolymer (1) contained in the adhesive layer according to the present invention and the hydrophilic copolymer (2) contained in the surface lubricating layer according to the present invention. In addition, the weight average molecular weight (Mw) of the obtained copolymer (B) was measured by GPC and found to be 190,000 in terms of polyethylene glycol.
[0202] [Example 1] The copolymer (A) obtained in Production Example 1 (corresponding to the hydrophilic copolymer (1) according to the present invention) was dissolved in ethanol / water (3 / 7 w / w) to a concentration of 10% by weight to prepare a coating liquid (1-A). Next, a polyamide tube (outer diameter 2.4 mm x length 70 mm) was dipped into the above coating liquid (1-A) and pulled up at a speed of 1 mm / sec. Next, the polyamide tube was dried at room temperature for 60 seconds to remove the solvent. Next, the polyamide tube was irradiated with a 365 nm wavelength and 105 mW / cm irradiation output. 2 The adhesive layer was formed on the polyamide tube (Polyamide Tube (1-A)) by irradiating the tube with ultraviolet (UV) rays at an irradiation distance of 250 mm and a sample rotation speed of 3 mm / sec for 3 minutes. The UV irradiation device used was Dymax's ECE2000 (high pressure mercury lamp).
[0203] Next, 0.01% by weight of sodium hyaluronate (derived from Streptococcus pyogenes) (weight average molecular weight = 15,000,000 to 18,000,000) from Sigma-Aldrich and 1% by weight of copolymer (A) obtained in Production Example 1 (corresponding to hydrophilic copolymer (2) according to the present invention) were dissolved in water to prepare a coating liquid (1'). The mixing ratio (weight ratio) of sodium hyaluronate to hydrophilic copolymer (2) in the coating liquid (1') was 1:100. Next, the polyamide tube (1-A) prepared above was dipped into the coating liquid (1') and pulled up at a speed of 5 mm / sec. Next, the polyamide tube (1-A) was dried at room temperature for 60 seconds to remove the solvent. Next, the polyamide tube (1-A) was irradiated with a 365 nm wavelength and 105 mW / cm irradiation output. 2 A surface lubricating layer was formed on the adhesive layer of the polyamide tube (1-A) by irradiating it with ultraviolet (UV) rays for 3 minutes at an irradiation distance of 250 mm and a sample rotation speed of 3 mm / sec (polyamide tube (1')). The UV irradiation device used was a Dymax ECE2000 (high pressure mercury lamp). The mixture ratio (weight ratio) of sodium hyaluronate and hydrophilic copolymer (2) in the surface lubricating layer of the polyamide tube (1') was 1:100.
[0204] Next, the lubricity and durability (lubrication maintenance) of the obtained polyamide tube (1') were evaluated according to the following method using a friction tester (Handy Tribomaster TL201, manufactured by Trinity Labs) 20 shown in Figure 3. The results are shown in Figure 4.
[0205] That is, a core material 18 was inserted into the above sample (polyamide tube (1')) to prepare a sample 16. The sample 16 was fixed in a petri dish 12 lying in the length direction and immersed in physiological saline 17 at a height that completely immersed the sample 16. The petri dish 12 was placed on a moving table 15 of a friction measuring device 20 shown in FIG. 3. A silicon terminal (φ10 mm) 13 was brought into contact with the sample, and a load 14 of 450 g was applied to the terminal. The sliding resistance value (gf) was measured when the moving table 15 was moved horizontally back and forth 10 times with a sliding distance of 25 mm and a sliding speed of 16.7 mm / sec. The sliding resistance values during the outward path from the first to the tenth reciprocation were averaged for each reciprocation and plotted on a graph as a test force to evaluate the change in the sliding resistance value for 10 repeated slidings.
[0206] [Comparative Example 1] The copolymer (A) obtained in Production Example 1 (corresponding to the hydrophilic copolymer (1) according to the present invention) was dissolved in ethanol / water (3 / 7 w / w) to a concentration of 10% by weight to prepare a coating liquid (1-A). Next, a polyamide tube (outer diameter 2.4 mm x length 70 mm) was dipped into the above coating liquid (1-A) and pulled up at a speed of 1 mm / sec. Next, the polyamide tube was dried at room temperature for 60 seconds to remove the solvent. Next, the polyamide tube was irradiated with a 365 nm wavelength and 105 mW / cm irradiation output. 2 The polyamide tube was irradiated with UV for 3 minutes at an irradiation distance of 250 mm and a sample rotation speed of 3 mm / sec to form a copolymer layer on the polyamide tube (Comparative polyamide tube (1)). The UV irradiation device used was ECE2000 (high pressure mercury lamp) manufactured by Dymax. The comparative polyamide tube (1) has the same structure as the polyamide tube (1') of Example 1, except that there is no surface lubricating layer.
[0207] Next, the obtained comparative polyamide tube (1) was evaluated for lubricity and durability (lubrication maintenance ability) in the same manner as in Example 1. The results are shown in FIG.
[0208] From FIG. 4, the polyamide tube (1') of the present invention has a low sliding resistance value (excellent lubricity) at the initial stage (first reciprocation), and the sliding resistance value hardly changes until the tenth reciprocation (excellent durability (lubrication retention)). In contrast, the comparative polyamide tube (1) has excellent durability (lubrication retention), but the initial sliding resistance value is higher than that of the polyamide tube (1') of the present invention. This evaluation method is a method assuming a high load condition where the clearance between the catheter and the inner surface of the biological lumen is small. That is, the sliding resistance value is measured using a tube as a sample. The contact area between the terminal of the tube-shaped sample is smaller than that of the sheet-shaped sample. Therefore, the force per unit area applied from the terminal to the tube-shaped sample is larger than that of the sheet-shaped sample (heavy load). Therefore, it is considered that the medical device of the present invention can exhibit excellent lubricity and durability (lubrication retention) even under a high load condition where the clearance between the catheter and the inner surface of the biological lumen is small. In addition, the comparative polyamide tube (1) of Comparative Example 1 also has higher sliding resistance values at the initial stage (first reciprocation) and up to the tenth reciprocation compared to the polyamide tube (1') of the present invention, but is considered to exhibit sufficient lubricity and durability (lubrication maintenance) under normal conditions.
[0209] [Examples 2 to 6] Sigma-Aldrich's sodium hyaluronate (derived from Streptococcus pyogenes) (weight average molecular weight = 15,000,000 to 18,000,000) was dissolved in water at 0.01% by weight, and the copolymer (A) obtained in Production Example 1 (corresponding to the hydrophilic copolymer (2) of the present invention) was dissolved in water at 5% by weight (coating liquid (2')), 2.5% by weight (coating liquid (3')), 0.5% by weight (coating liquid (4')), 0.1% by weight (coating liquid (5')), and 0.05% by weight (coating liquid (6')), to prepare coating liquids (2') to (6'). The mixing ratios (weight ratios) of sodium hyaluronate and hydrophilic copolymer (2) in coating liquids (2') to (6') are 1:500, 1:250, 1:50, 1:10, and 1:5, respectively.
[0210] Polyamide tubes (2') to (6') were produced in the same manner as in Example 1, except that the coating liquid (1') was replaced with the coating liquids (2') to (6') prepared above. Here, the mixing ratios (weight ratio) of sodium hyaluronate and hydrophilic copolymer (2) in the surface lubricating layers of the polyamide tubes (2') to (6') were 1:500, 1:250, 1:50, 1:10, and 1:5, respectively.
[0211] Next, the obtained polyamide tubes (2') to (6') and the polyamide tube (1') produced in the same manner as in Example 1 were evaluated for lubricity (first sliding resistance value) in the same manner as in Example 1. The results are shown in Table 1 below. The results of Comparative Example 1 are also shown in Table 1 below. The evaluation criteria in Table 1 below are as follows. The lubricity (first sliding resistance value) in Table 1 shows the results for two samples (n=2). If both samples were rated as ◎, the lubricity (first sliding resistance value) is shown as "◎", and if one sample was rated as ◎ and the other sample was ◯, the lubricity (first sliding resistance value) is shown as "◯ to ◎".
[0212] (Evaluation Criteria) ◎: The sliding resistance value for the first time is less than 40% of that of Comparative Example 1. ◯: The sliding resistance value for the first time is 40% or more and less than 60% of that of Comparative Example 1. △: The sliding resistance value for the first time is 60% or more and less than 90% of that of Comparative Example 1. ×: The sliding resistance value for the first time is 90% or more of that for Comparative Example 1.
[0213] [Table 1]
[0214] [Examples 7 to 9] The copolymer (A) obtained in Production Example 1 (corresponding to the hydrophilic copolymer (2) according to the present invention) was dissolved in water at 1% by weight, and sodium hyaluronate (derived from Streptococcus pyogenes) (weight average molecular weight = 15,000,000 to 18,000,000) from Sigma-Aldrich was dissolved in water at 0.01% by weight (coating solution (7')), 0.005% by weight (coating solution (8')), and 0.001% by weight (coating solution (9')), to prepare coating solutions (7') to (9'). The mixing ratios (weight ratio) of sodium hyaluronate and hydrophilic copolymer (2) in coating solutions (7') to (9') are 1:100, 1:200, and 1:1000, respectively.
[0215] Polyamide tubes (7') to (9') were produced in the same manner as in Example 1, except that the coating liquid (1') in Example 1 was replaced with the coating liquids (7') to (9') prepared above. Here, the mixing ratios (weight ratio) of sodium hyaluronate and hydrophilic copolymer (2) in the surface lubricating layers of the polyamide tubes (7') to (9') were 1:100, 1:200, and 1:1000, respectively.
[0216] Next, the obtained polyamide tubes (7') to (9') and the polyamide tube (1') produced in the same manner as in Example 1 were evaluated for lubricity (first sliding resistance value) in the same manner as in Example 1. The results are shown in Table 2 below. In addition, the results of Comparative Example 1 are also shown in Table 2 below. The evaluation criteria in Table 2 below are the same as those in Table 1 above.
[0217] [Table 2]
[0218] [Example 10] Sigma-Aldrich sodium polystyrene sulfonate (weight average molecular weight = about 1,000,000) was dissolved in water at 0.02 wt % and copolymer (A) obtained in Production Example 1 (corresponding to hydrophilic copolymer (2) according to the present invention) was dissolved in water at 1 wt %, respectively, to prepare a coating liquid (10'). The mixing ratio (weight ratio) of sodium polystyrene sulfonate to hydrophilic copolymer (2) in the coating liquid (10') was 1:50.
[0219] A polyamide tube (10') was produced in the same manner as in Example 1, except that the coating liquid (10') prepared above was used instead of the coating liquid (1') in Example 1. Here, the mixing ratio (weight ratio) of sodium polystyrene sulfonate and hydrophilic copolymer (2) in the surface lubricating layer of the polyamide tube (10') was 1:50.
[0220] Next, the lubricity (first sliding resistance value) of the obtained polyamide tube (10') was evaluated in the same manner as in Example 1 and based on the same evaluation criteria, resulting in a rating of "A".
[0221] [Example 11] Polyvinylpyrrolidone (Polyvinylpyrrolidone K90 manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was dissolved in water to a concentration of 0.04% by weight, and copolymer (A) obtained in Production Example 1 (corresponding to hydrophilic copolymer (2) according to the present invention) was dissolved in water to a concentration of 1% by weight, to prepare a coating liquid (11'). The mixing ratio (weight ratio) of polyvinylpyrrolidone to hydrophilic copolymer (2) in the coating liquid (11') was 1:25.
[0222] A polyamide tube (11') was produced in the same manner as in Example 1, except that the coating liquid (11') prepared above was used instead of the coating liquid (1') in Example 1. Here, the mixing ratio (weight ratio) of polyvinylpyrrolidone to hydrophilic copolymer (2) in the surface lubricating layer of the polyamide tube (11') was 1:25.
[0223] Next, the lubricity (first sliding resistance value) of the obtained polyamide tube (11') was evaluated in the same manner as in Example 1 and based on the same evaluation criteria, resulting in a result of "good."
[0224] [Example 12] A coating liquid (12') was prepared by dissolving 0.01% by weight of carboxymethylcellulose sodium salt (product name: Carboxymethylcellulose sodium salt Medium viscosity) manufactured by Sigma-Aldrich Corporation and 1% by weight of the copolymer obtained in Production Example 1 (corresponding to the hydrophilic copolymer (2) according to the present invention) in water. The mixing ratio (weight ratio) of carboxymethylcellulose sodium salt to hydrophilic copolymer (2) in the coating liquid (12') was 1:100.
[0225] A polyamide tube (12') was produced in the same manner as in Example 1, except that the coating liquid (12') prepared above was used instead of the coating liquid (1') in Example 1. Here, the mixing ratio (weight ratio) of carboxymethyl cellulose sodium salt and hydrophilic copolymer (2) in the surface lubricating layer of the polyamide tube (12') was 1:100.
[0226] Next, the lubricity (first sliding resistance value) of the obtained polyamide tube (12') was evaluated in the same manner as in Example 1 and based on the same evaluation criteria, resulting in a rating of "A".
[0227] [Example 13] The copolymer (B) obtained in Production Example 2 (corresponding to the hydrophilic copolymer (1) according to the present invention) was dissolved in ethanol / water (3 / 7 w / w) to a concentration of 10% by weight to prepare a coating liquid (1-B). Next, a polyamide tube (outer diameter 2.4 mm x length 70 mm) was dipped into the above coating liquid (1-B) and pulled up at a speed of 1 mm / sec. Next, the polyamide tube was dried at room temperature for 60 seconds to remove the solvent. Next, the polyamide tube was irradiated with a 365 nm wavelength and 105 mW / cm irradiation output. 2 The adhesive layer was formed on the polyamide tube (Polyamide tube (1-B)) by irradiating the tube with ultraviolet (UV) rays at an irradiation distance of 250 mm and a sample rotation speed of 3 mm / sec for 3 minutes. The UV irradiation device used was Dymax's ECE2000 (high pressure mercury lamp).
[0228] Next, 0.01% by weight of sodium hyaluronate (derived from Streptococcus pyogenes) (weight average molecular weight = 15,000,000 to 18,000,000) from Sigma-Aldrich and 1% by weight of copolymer (B) obtained in Production Example 2 (corresponding to hydrophilic copolymer (2) according to the present invention) were dissolved in water to prepare a coating liquid (13'). The mixing ratio (weight ratio) of sodium hyaluronate to hydrophilic copolymer (2) in the coating liquid (13') was 1:100. Next, the polyamide tube (1-B) prepared above was dipped into the coating liquid (13') and pulled up at a speed of 5 mm / sec. Next, the polyamide tube (1-B) was dried at room temperature for 60 seconds to remove the solvent. Next, the polyamide tube (1-B) was irradiated with a 365 nm wavelength and 105 mW / cm irradiation output. 2 A surface lubricating layer was formed on the adhesive layer of the polyamide tube (1-B) by irradiating it with ultraviolet (UV) rays for 3 minutes at an irradiation distance of 250 mm and a sample rotation speed of 3 mm / sec (polyamide tube (13')). The UV irradiation device used was a Dymax ECE2000 (high pressure mercury lamp). The mixture ratio (weight ratio) of sodium hyaluronate and hydrophilic copolymer (2) in the surface lubricating layer of the polyamide tube (13') was 1:100.
[0229] Next, the lubricity (first sliding resistance value) of the obtained polyamide tube (13') was evaluated in the same manner as in Example 1 and based on the same evaluation criteria, resulting in a rating of "A".
[0230] [Example 14] Sigma-Aldrich's sodium hyaluronate (derived from Streptococcus pyogenes) (weight average molecular weight = 15,000,000 to 18,000,000) was dissolved in water at 0.01% by weight, and the copolymer (B) obtained in Production Example 2 (corresponding to the hydrophilic copolymer (2) of the present invention) was dissolved in water at 1% by weight to prepare a coating liquid (14'). The mixing ratio (weight ratio) of sodium hyaluronate to hydrophilic copolymer (2) in the coating liquid (14') was 1:100.
[0231] A polyamide tube (14') was prepared in the same manner as in Example 1, except that the coating liquid (14') prepared above was used instead of the coating liquid (1') in Example 1. Here, the mixing ratio (weight ratio) of sodium hyaluronate and hydrophilic copolymer (2) in the surface lubricating layer of the polyamide tube (14') was 1:100.
[0232] Next, the lubricity (first sliding resistance value) of the obtained polyamide tube (14') was evaluated in the same manner as in Example 1 and based on the same evaluation criteria, resulting in a rating of "A".
[0233] [Example 15] Sigma-Aldrich's sodium hyaluronate (derived from Streptococcus pyogenes) (weight average molecular weight = 15,000,000 to 18,000,000) was dissolved in water at 0.01% by weight, and the copolymer (A) obtained in Production Example 1 (corresponding to the hydrophilic copolymer (2) of the present invention) was dissolved in water at 1% by weight to prepare a coating liquid (15'). The mixing ratio (weight ratio) of sodium hyaluronate to hydrophilic copolymer (2) in the coating liquid (15') was 1:100.
[0234] In Example 13, except for using the coating liquid (15') prepared above instead of the coating liquid (13'), a polyamide tube (15') was prepared in the same manner as in Example 13. Here, the mixing ratio (weight ratio) of sodium hyaluronate and hydrophilic copolymer (2) in the surface lubricating layer of the polyamide tube (15') is 1:100.
[0235] Next, the lubricity (first sliding resistance value) of the obtained polyamide tube (15') was evaluated in the same manner as in Example 1 and based on the same evaluation criteria, resulting in a rating of "A".
[0236] [Example 16] The copolymer (A) obtained in Production Example 1 (corresponding to the hydrophilic copolymer (1) according to the present invention) was dissolved in ethanol / water (3 / 7 w / w) to a concentration of 7% by weight to prepare a coating liquid (1-C). Next, a polyamide tube (outer diameter 2.4 mm x length 70 mm) was dipped into the above coating liquid (1-C) and pulled up at a speed of 1 mm / sec. Next, the polyamide tube was dried at room temperature for 60 seconds to remove the solvent. Next, the polyamide tube was irradiated with a 365 nm wavelength and 105 mW / cm irradiation output. 2 The adhesive layer was formed on the polyamide tube by irradiating it with ultraviolet (UV) rays at an irradiation distance of 250 mm and a sample rotation speed of 3 mm / sec for 3 minutes (Polyamide Tube (1-C)). The UV irradiation device used was a Dymax ECE2000 (high pressure mercury lamp).
[0237] Next, 0.01% by weight of sodium hyaluronate (derived from Streptococcus pyogenes) (weight average molecular weight = 15,000,000 to 18,000,000) from Sigma-Aldrich and 1% by weight of copolymer (A) obtained in Production Example 1 (corresponding to hydrophilic copolymer (2) according to the present invention) were dissolved in water to prepare a coating liquid (16'). The mixing ratio (weight ratio) of sodium hyaluronate to hydrophilic copolymer (2) in the coating liquid (16') was 1:100. Next, the polyamide tube (1-C) prepared above was dipped into the coating liquid (16') and pulled up at a speed of 5 mm / sec. Next, the polyamide tube (1-C) was dried at room temperature for 60 seconds to remove the solvent. Next, the polyamide tube (1-C) was irradiated with a 365 nm wavelength and 105 mW / cm irradiation output. 2 A surface lubricating layer was formed on the adhesive layer of the polyamide tube (1-C) by irradiating it with ultraviolet (UV) rays for 3 minutes at an irradiation distance of 250 mm and a sample rotation speed of 3 mm / sec (polyamide tube (16')). The UV irradiation device used was a Dymax ECE2000 (high pressure mercury lamp). The mixture ratio (weight ratio) of sodium hyaluronate and hydrophilic copolymer (2) in the surface lubricating layer of the polyamide tube (16') was 1:100.
[0238] Next, the lubricity (first sliding resistance value) of the obtained polyamide tube (16') was evaluated in the same manner as in Example 1 and based on the same evaluation criteria, resulting in a rating of "A".
[0239] The results of the above examples and comparative examples are summarized in Table 3 below. In Table 3 below, the mixing ratio indicates the weight ratio of hydrophilic copolymer: water retention material in the surface lubrication layer. For example, in Example 1, the mixing ratio indicates the "mixing weight ratio of hydrophilic copolymer (A): sodium hyaluronate", and in Example 10, the mixing ratio indicates the "mixing weight ratio of hydrophilic copolymer (A): sodium polystyrene sulfonate". In addition, the columns for each hydrophilic copolymer and each water retention material indicate the concentration of each hydrophilic copolymer and each water retention material in the coating liquid, and lubricity means lubricity (first sliding resistance value).
[0240] [Table 3]
[0241] This application is based on Japanese Patent Application No. 2019-151581, filed on August 21, 2019, the disclosure of which is hereby incorporated by reference in its entirety. [Explanation of symbols]
[0242] 1 base material layer, 1a: base material layer core portion; 1b base material surface layer, 2 adhesive layer, 3 surface lubricant layer, 10 Medical equipment, 12 Petri dishes, 13 Silicon terminal, 14 Load, 15 Moving table, 16 samples, 17 Saline, 18 Core material, 20 Friction measuring machine.
Claims
1. A base layer; A polymerizable monomer (A) having a sulfobetaine structure and a sulfonic acid group (—SO 3 H), sulfate group (-OSO 3 H) and sulfite group (-OSO 2 an adhesive layer comprising a hydrophilic copolymer (1) containing a structural unit derived from a polymerizable monomer (B) having at least one group selected from the group consisting of groups consisting of groups of H) and salts thereof, and a structural unit derived from a polymerizable monomer (C) having a photoreactive group; The adhesive layer is formed in at least a part thereof, and the adhesive layer is formed of a polymerizable monomer (A′) having a sulfobetaine structure, a sulfonic acid group (—SO 3 H), sulfate group (-OSO 3 H) and sulfite group (-OSO 2 and a surface lubricating layer containing a hydrophilic copolymer (2) including a structural unit derived from a polymerizable monomer (B') having at least one group selected from the group consisting of groups of the polymerizable monomers (H) and salts thereof, and a structural unit derived from a polymerizable monomer (C') having a photoreactive group, The polymerizable monomers (A) and (A′) are each independently represented by the following formula (1): 【Chemistry 1】 In the above formula (1), R 11 is a hydrogen atom or a methyl group; Z 1 is an oxygen atom or -NH-; R 12 and R 15 each independently represent a linear or branched alkylene group having 1 to 20 carbon atoms; R 13 and R 14 each independently represent a linear or branched alkyl group having 1 to 20 carbon atoms; The polymerizable monomers (B) and (B') are each independently represented by the following formula (2), (3) or (4): 【Chemistry 2】 In the above formula (2), R 21 is a hydrogen atom or a methyl group; Z 2 is an oxygen atom or -NH-; R 22 is a linear or branched alkylene group having 1 to 20 carbon atoms; X is a group selected from the group consisting of a sulfonic acid group (-SO 3 H), a sulfate group (-OSO 3 H) and a sulfite group (-OSO 2 H) and salt groups thereof; 【Chemistry 3】 In the above formula (3), R 31 is a hydrogen atom or a methyl group; R 32 is a single bond or a linear or branched alkylene group having 1 to 20 carbon atoms; X is a group selected from the group consisting of a sulfonic acid group (-SO 3 H), a sulfate group (-OSO 3 H) and a sulfite group (-OSO 2 H) and salt groups thereof; 【Chemistry 4】 In the above formula (4), R 41 is a hydrogen atom or a methyl group; R 42 is a linear or branched alkylene group having 1 to 20 carbon atoms; X is a group selected from the group consisting of a sulfonic acid group (-SO 3 H), a sulfate group (-OSO 3 H) and a sulfite group (-OSO 2 H) and salt groups thereof; the polymerizable monomers (C) and (C') each independently have an ethylenically unsaturated group selected from the group consisting of a (meth)acryloyl group, a vinyl group, and an allyl group, and a photoreactive group selected from the group consisting of an azide group, a diazo group, a diazirine group, a ketone group, and a quinone group; the content of the structural units derived from the polymerizable monomers (A) and (A') is each independently 1 to 99 mol % when the total of the structural units derived from all monomers is 100 mol %, the content of the structural units derived from the polymerizable monomers (B) and (B') is each independently 0.2 to 99 mol % when the total of the structural units derived from all monomers is 100 mol %, the content of the structural units derived from the polymerizable monomers (C) and (C') is each independently 0.1 to 30 mol % when the total of the structural units derived from all monomers is 100 mol %, the total content of the structural units derived from the polymerizable monomer (A), the total content of the structural units derived from the polymerizable monomer (B), and the total content of the structural units derived from the polymerizable monomer (C) is more than 95 mol % and 100 mol % or less, relative to 100 mol %, which is the total amount of the structural units derived from all monomers; A medical device, wherein the total content of the structural units derived from the polymerizable monomer (A'), the content of the structural units derived from the polymerizable monomer (B') and the content of the structural units derived from the polymerizable monomer (C') is more than 95 mol % and not more than 100 mol %, relative to 100 mol %, the total amount of the structural units derived from all monomers.
2. The medical device according to claim 1 , wherein the hydrophilic copolymer (2) is contained in the surface lubricating layer in a ratio of more than 5 parts by weight and less than 500 parts by weight per 1 part by weight of the hyaluronic acid or its salt.
3. The polymerizable monomers (A) and (A') are each independently selected from the group consisting of {2-[(meth)acryloyloxy]ethyl}dimethyl-(3-sulfopropyl)ammonium hydroxide, {2-[(meth)acryloyloxy]ethyl}dimethyl-(2-sulfoethyl)ammonium hydroxide, {2-[(meth)acryloyloxy]ethyl}dimethyl-(2-sulfobutyl)ammonium hydroxide, {2-[(meth)acryloyloxy]ethyl}diethyl-(2-sulfoethyl)ammonium hydroxide, {2-[(meth)acryloyloxy]ethyl}diethyl-(3-sulfopropyl)ammonium hydroxide, {2-[(meth)acryloyloxy]ethyl}diethyl-(2-sulfobutyl)ammonium hydroxide, at least one selected from the group consisting of {3-[(meth)acryloyloxy]propyl}dimethyl-(2-sulfoethyl)ammonium hydroxide, {3-[(meth)acryloyloxy]propyl}dimethyl-(3-sulfopropyl)ammonium hydroxide, {3-[(meth)acryloylamino)propyl}dimethyl(3-sulfobutyl)ammonium hydroxide, {3-[(meth)acryloyloxy]propyl}diethyl-(2-sulfoethyl)ammonium hydroxide, {3-[(meth)acryloyloxy]propyl}diethyl-(3-sulfopropyl)ammonium hydroxide, and {3-[(meth)acryloyloxy]propyl}diethyl-(3-sulfobutyl)ammonium hydroxide, The polymerizable monomers (B) and (B') are each independently at least one selected from the group consisting of 2-(meth)acrylamido-2-methyl-1-propanesulfonic acid, 1-[(meth)acryloyloxymethyl]-1-propanesulfonic acid, 2-[(meth)acryloyloxy]-2-propanesulfonic acid, 3-[(meth)acryloyloxy]-1-methyl-1-propanesulfonic acid, 2-sulfoethyl (meth)acrylate, and 3-sulfopropyl (meth)acrylate, and salts thereof; The polymerizable monomers (C) and (C') are each independently at least one selected from the group consisting of 2-azidoethyl (meth)acrylate, 2-azidopropyl (meth)acrylate, 3-azidopropyl (meth)acrylate, 4-azidobutyl (meth)acrylate, 4-(meth)acryloyloxybenzophenone (MBP), 4-(meth)acryloyloxyethoxybenzophenone, 4-(meth)acryloyloxy-4'-methoxybenzophenone, 4-(meth)acryloyloxyethoxy-4'-methoxybenzophenone, 4-(meth)acryloyloxy-4'-bromobenzophenone, 4-(meth)acryloyloxyethoxy-4'-bromobenzophenone, 4-styrylmethoxybenzophenone, 4-(meth)acryloyloxythioxanthone, and 2-(meth)acryloyloxyethyl-4-azidobenzoate; the content of the structural units derived from the polymerizable monomers (A) and (A') is independently 5 to 99 mol % when the total of the structural units derived from all monomers is 100 mol %, the content of the structural units derived from the polymerizable monomers (B) and (B') is independently 0.5 to 99 mol % when the total of the structural units derived from all monomers is 100 mol %, the content of the structural units derived from the polymerizable monomers (C) and (C') is each independently 0.1 to 25 mol % when the total of the structural units derived from all monomers is 100 mol %, the total content of the structural units derived from the polymerizable monomer (A), the total content of the structural units derived from the polymerizable monomer (B), and the total content of the structural units derived from the polymerizable monomer (C) is more than 99 mol % and 100 mol % or less, relative to 100 mol %, which is the total amount of the structural units derived from all monomers; 3. The medical device according to claim 1 or 2, wherein the total content of the structural units derived from the polymerizable monomer (A'), the content of the structural units derived from the polymerizable monomer (B') and the content of the structural units derived from the polymerizable monomer (C') is more than 99 mol% and not more than 100 mol%, relative to 100 mol% as a total amount of structural units derived from all monomers.
4. The medical device according to any one of claims 1 to 3, wherein the polymerizable monomer (C) and / or (C') has a group having a benzophenone structure.
5. The medical device according to any one of claims 1 to 4, wherein the hydrophilic copolymer (1) and the hydrophilic copolymer (2) have the same structure.
6. The medical device according to any one of claims 1 to 5, which is a catheter, a stent or a guidewire.
7. A method for producing the medical device according to any one of claims 1 to 6, A coating liquid (1) containing the hydrophilic copolymer (1) is applied to the base layer to form an adhesive layer; A coating liquid (2) containing the hyaluronic acid or a salt thereof and the hydrophilic copolymer (2) is applied to the adhesive layer to form a surface lubricating layer. The method comprises:
8. The method according to claim 7, wherein the concentration of the hydrophilic copolymer (2) in the coating liquid (2) is 0.1 to 4.5% by weight.
9. A base layer; A polymerizable monomer (A) having a sulfobetaine structure and a sulfonic acid group (—SO 3 H), sulfate group (-OSO 3 H) and sulfite group (-OSO 2 an adhesive layer comprising a hydrophilic copolymer (1) containing a structural unit derived from a polymerizable monomer (B) having at least one group selected from the group consisting of groups consisting of groups of H) and salts thereof, and a structural unit derived from a polymerizable monomer (C) having a photoreactive group; The adhesive layer is formed in at least a part thereof, and the adhesive layer is formed of at least one selected from the group consisting of a polymer electrolyte, a polysaccharide, and a nonionic polymer, and a polymerizable monomer (A′) having a sulfobetaine structure, and a sulfonic acid group (—SO 3 H), sulfate group (-OSO 3 H) and sulfite group (-OSO 2 and a surface lubricating layer containing a hydrophilic copolymer (2) including a structural unit derived from a polymerizable monomer (B') having at least one group selected from the group consisting of groups of the polymerizable monomers (H) and salts thereof, and a structural unit derived from a polymerizable monomer (C') having a photoreactive group, The polymerizable monomers (A) and (A′) are each independently represented by the following formula (1): 【Chemistry 5】 In the above formula (1), R 11 is a hydrogen atom or a methyl group; Z 1 is an oxygen atom or -NH-; R 12 and R 15 each independently represent a linear or branched alkylene group having 1 to 20 carbon atoms; R 13 and R 14 each independently represent a linear or branched alkyl group having 1 to 20 carbon atoms; The polymerizable monomers (B) and (B') are each independently represented by the following formula (2), (3) or (4): 【Chemistry 6】 In the above formula (2), R 21 is a hydrogen atom or a methyl group; Z 2 is an oxygen atom or -NH-; R 22 is a linear or branched alkylene group having 1 to 20 carbon atoms; X is a group selected from the group consisting of a sulfonic acid group (-SO 3 H), a sulfate group (-OSO 3 H) and a sulfite group (-OSO 2 H) and salt groups thereof; 【Chemistry 7】 In the above formula (3), R 31 is a hydrogen atom or a methyl group; R 32 is a single bond or a linear or branched alkylene group having 1 to 20 carbon atoms; X is a group selected from the group consisting of a sulfonic acid group (-SO 3 H), a sulfate group (-OSO 3 H) and a sulfite group (-OSO 2 H) and salt groups thereof; 【Chemistry 8】 In the above formula (4), R 41 is a hydrogen atom or a methyl group; R 42 is a linear or branched alkylene group having 1 to 20 carbon atoms; X is a group selected from the group consisting of a sulfonic acid group (-SO 3 H), a sulfate group (-OSO 3 H) and a sulfite group (-OSO 2 H) and salt groups thereof; the polymerizable monomers (C) and (C') each independently have an ethylenically unsaturated group selected from the group consisting of a (meth)acryloyl group, a vinyl group, and an allyl group, and a photoreactive group selected from the group consisting of an azide group, a diazo group, a diazirine group, a ketone group, and a quinone group; the content of the structural units derived from the polymerizable monomers (A) and (A') is each independently 1 to 99 mol % when the total of the structural units derived from all monomers is 100 mol %, the content of the structural units derived from the polymerizable monomers (B) and (B') is each independently 0.2 to 99 mol % when the total of the structural units derived from all monomers is 100 mol %, the content of the structural units derived from the polymerizable monomers (C) and (C') is each independently 0.1 to 30 mol % when the total of the structural units derived from all monomers is 100 mol %, the total content of the structural units derived from the polymerizable monomer (A), the total content of the structural units derived from the polymerizable monomer (B), and the total content of the structural units derived from the polymerizable monomer (C) is more than 95 mol % and 100 mol % or less, relative to 100 mol %, which is the total amount of the structural units derived from all monomers; the total content of the structural units derived from the polymerizable monomer (A'), the total content of the structural units derived from the polymerizable monomer (B') and the total content of the structural units derived from the polymerizable monomer (C') is more than 95 mol % and 100 mol % or less, relative to 100 mol %, the total amount of the structural units derived from all monomers; the polymer electrolyte is at least one (co)polymer selected from the group consisting of acrylic acid, styrenesulfonic acid, and salts thereof; The polysaccharide is at least one selected from the group consisting of chondroitin sulfate, carboxymethylcellulose, and salts thereof; The medical device, wherein the nonionic polymer is a homopolymer or copolymer containing constitutional units derived from a nonionic monomer selected from the group consisting of vinylpyrrolidone, N,N-dimethylacrylamide and N-isopropylacrylamide.
10. The polymerizable monomers (A) and (A') are each independently selected from the group consisting of {2-[(meth)acryloyloxy]ethyl}dimethyl-(3-sulfopropyl)ammonium hydroxide, {2-[(meth)acryloyloxy]ethyl}dimethyl-(2-sulfoethyl)ammonium hydroxide, {2-[(meth)acryloyloxy]ethyl}dimethyl-(2-sulfobutyl)ammonium hydroxide, {2-[(meth)acryloyloxy]ethyl}diethyl-(2-sulfoethyl)ammonium hydroxide, {2-[(meth)acryloyloxy]ethyl}diethyl-(3-sulfopropyl)ammonium hydroxide, {2-[(meth)acryloyloxy]ethyl}diethyl-(2-sulfobutyl)ammonium hydroxide, at least one selected from the group consisting of {3-[(meth)acryloyloxy]propyl}dimethyl-(2-sulfoethyl)ammonium hydroxide, {3-[(meth)acryloyloxy]propyl}dimethyl-(3-sulfopropyl)ammonium hydroxide, {3-[(meth)acryloylamino)propyl}dimethyl(3-sulfobutyl)ammonium hydroxide, {3-[(meth)acryloyloxy]propyl}diethyl-(2-sulfoethyl)ammonium hydroxide, {3-[(meth)acryloyloxy]propyl}diethyl-(3-sulfopropyl)ammonium hydroxide, and {3-[(meth)acryloyloxy]propyl}diethyl-(3-sulfobutyl)ammonium hydroxide, The polymerizable monomers (B) and (B') are each independently at least one selected from the group consisting of 2-(meth)acrylamido-2-methyl-1-propanesulfonic acid, 1-[(meth)acryloyloxymethyl]-1-propanesulfonic acid, 2-[(meth)acryloyloxy]-2-propanesulfonic acid, 3-[(meth)acryloyloxy]-1-methyl-1-propanesulfonic acid, 2-sulfoethyl (meth)acrylate, and 3-sulfopropyl (meth)acrylate, and salts thereof; The polymerizable monomers (C) and (C') are each independently at least one selected from the group consisting of 2-azidoethyl (meth)acrylate, 2-azidopropyl (meth)acrylate, 3-azidopropyl (meth)acrylate, 4-azidobutyl (meth)acrylate, 4-(meth)acryloyloxybenzophenone (MBP), 4-(meth)acryloyloxyethoxybenzophenone, 4-(meth)acryloyloxy-4'-methoxybenzophenone, 4-(meth)acryloyloxyethoxy-4'-methoxybenzophenone, 4-(meth)acryloyloxy-4'-bromobenzophenone, 4-(meth)acryloyloxyethoxy-4'-bromobenzophenone, 4-styrylmethoxybenzophenone, 4-(meth)acryloyloxythioxanthone, and 2-(meth)acryloyloxyethyl-4-azidobenzoate; the content of the structural units derived from the polymerizable monomers (A) and (A') is independently 5 to 99 mol % when the total of the structural units derived from all monomers is 100 mol %, the content of the structural units derived from the polymerizable monomers (B) and (B') is independently 0.5 to 99 mol % when the total of the structural units derived from all monomers is 100 mol %, the content of the structural units derived from the polymerizable monomers (C) and (C') is each independently 0.1 to 25 mol % when the total of the structural units derived from all monomers is 100 mol %, the total content of the structural units derived from the polymerizable monomer (A), the total content of the structural units derived from the polymerizable monomer (B), and the total content of the structural units derived from the polymerizable monomer (C) is more than 99 mol % and 100 mol % or less, relative to 100 mol %, which is the total amount of the structural units derived from all monomers; the total content of the structural units derived from the polymerizable monomer (A'), the total content of the structural units derived from the polymerizable monomer (B') and the total content of the structural units derived from the polymerizable monomer (C') is more than 99 mol% and 100 mol% or less, relative to 100 mol% in the total amount of the structural units derived from all monomers; the polymer electrolyte is at least one (co)polymer selected from the group consisting of styrenesulfonic acid and its sodium salt and potassium salt, The polysaccharide is at least one selected from the group consisting of carboxymethylcellulose and its sodium and potassium salts, The medical device according to claim 9 , wherein the non-ionic polymer is polyvinylpyrrolidone.
Citation Information
Patent Citations
Compliant hydrophilic coatings for medical devices
US20190092961A1
Hydrophilic copolymer and medical device
WO2018038063A1
Medical instrument and method for manufacturing same
WO2021033765A1
Medical instrument and method for manufacturing same