Manufacturing method for Ta alloy member
By employing specific Ta alloy compositions and heat treatment processes, the method addresses the property discrepancies in additive-manufactured Ta alloys, resulting in Ta alloy members with enhanced mechanical properties for space applications.
Patent Information
- Application Number
- JP2024055306
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2024-03-29
- Publication Date
- 2024-10-10
- Estimated Expiration
- 2044-03-29
AI Technical Summary
The challenge lies in manufacturing Ta alloy members suitable for space applications using additive manufacturing, as existing methods result in materials with different properties from cast or forged materials, and there is a lack of effective heat treatment methods to enhance mechanical strength at high temperatures.
A method involving the use of Ta alloy powder with specific compositions, such as Ta-2.5W or Ta-4W-1Re-0.7Hf-0.025C, combined with additive manufacturing and heat treatment processes including residual stress removal and stabilization at controlled temperatures, to produce Ta alloy members suitable for space applications.
The method enables the production of Ta alloy members with improved mechanical properties, including sufficient strength and ductility, making them suitable for thruster nozzles and other space components.
Smart Images

Figure 00000011_0000 
Figure 00000011_0001 
Figure 00000011_0002
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing refractory Ta alloy components applicable for space applications by additive manufacturing and heat treatment. [Background technology]
[0002] Ta has excellent corrosion resistance and heat resistance, so its pure metal and alloys are used for various purposes such as capacitors, chemical plants, medical materials, etc. In addition, due to its high heat resistance, refractory Ta alloys are expected to be used in space applications, especially in thruster (engine) nozzles.
[0003] In rocket and satellite thrusters, Nb alloy parts are used in parts exposed to high temperatures. If these could be replaced with Ta alloy parts, the fuel could be burned at a higher temperature, and the thrust of the thruster could be increased. Non-Patent Document 2 describes an oxidation resistance test of an oxidation-resistant coating of Ta-10W alloy for aerospace applications, conducted at 1800°C.
[0004] Nb alloy members in practical use are generally shaped by cutting cast ingots or forged bars, but in many cases, more than 90% of the material is cut off from the material to the final product, which poses a cost problem. In response to this, research and development has been actively conducted on the manufacture of fire-resistant Nb alloy members using additive manufacturing methods that can mold complex shapes from powder materials. For example, Patent Document 1 discloses a method for manufacturing fire-resistant Nb alloy members by additive manufacturing and heat treatment. Ta, which is a rare resource, is even more expensive than Nb, so there is an even stronger demand for the use of additive manufacturing methods, rather than casting or forging, in the manufacture of Ta alloy members. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Patent No. 7412867 [Non-patent literature]
[0006] [Non-Patent Document 1] Katsuhiro Nose, "Metal Sketches Series No. 19 Tantalum", Material, Japan Institute of Metals, 2021, Vol. 60, No. 11, p. 685 [Non-Patent Document 2] Z. Cai et al., "Microstructure and oxidation resistance of a YSZ modified silicide coating for Ta-W alloy at 1800C", Corrosion Science, Elsevier BV, 2018, vol.143, pp.116-128 Summary of the Invention [Problem to be solved by the invention]
[0007] Because additive manufacturing uses powdered raw materials and involves rapid heating and cooling, the properties of objects made from the same alloy are different from those of cast or forged materials, and the composition of a Ta alloy suitable for the manufacture of space components by additive manufacturing was unknown. In addition, because it is not easy to carry out tests to measure mechanical strength at high temperatures, the heat treatment method for making Ta alloys applicable to space applications was also unknown.
[0008] The present invention has been made in consideration of the above, and aims to provide a method for producing a Ta alloy part applicable to space applications using additive manufacturing. [Means for solving the problem]
[0009] The method for producing a Ta alloy part of the present invention includes the steps of: preparing an alloy powder of a Ta alloy containing 2.0 to 4.5 mass% W with the remainder being Ta and unavoidable impurities; an additive manufacturing step of stacking the alloy powder by an additive manufacturing technique to form a shaped object; and a stabilization step of heat treating the shaped object at a temperature of 1400°C or higher and 2000°C or lower.
[0010] Another method for producing a Ta alloy member of the present invention includes the steps of preparing an alloy powder of a Ta alloy containing 2.0-4.5 mass% W, 0.5-1.2 mass% Re, 0.5-1.0 mass% Hf, 0.005-0.045 mass% C, with the balance being Ta and unavoidable impurities, an additive manufacturing step of layering the alloy powder by an additive manufacturing technique to form a shaped object, and a stabilization step of heat treating the shaped object at 1400° C. or more and 2000° C. or less. Preferably, oxides of Hf and carbides of Ta are precipitated in the stabilization step.
[0011] Preferably, any of the above-mentioned methods for producing a Ta alloy part further includes a residual stress relief step of heat treating the shaped article at 1100°C or higher and 1300°C or lower after the additive manufacturing step. Effect of the Invention
[0012] According to the method for producing a Ta alloy part of the present invention, additive manufacturing can be used to obtain a Ta alloy part applicable to space applications such as thruster nozzles. [Brief description of the drawings]
[0013] [Figure 1] FIG. 1 is a process flow diagram of a method for producing a Ta alloy member according to one embodiment. [Diagram 2] These are the results of room temperature tensile tests on the as-formed material. [Diagram 3] A to C: Results of tensile tests at room temperature for the as-formed and heat-treated materials. [Figure 4] FIG. 2 is an EBSD diagram showing grain boundaries of a Ta pure metal component. [Diagram 5] FIG. 2 is an EBSD diagram showing grain boundaries of the Ta alloy members of the comparative example and the example. [Figure 6] FIG. 2 is an EBSD diagram showing grain boundaries of the Ta alloy members of the comparative example and the example. [Figure 7] FIG. 2 is an EBSD diagram showing grain boundaries of the Ta alloy members of the comparative example and the example. [Figure 8]FIG. 2 is an EBSD diagram showing grain boundaries of a Ta alloy member of a comparative example. [Figure 9] A to D: SEM images showing precipitates in some samples. [Figure 10] A and B are the results of tensile tests on heat-treated materials at 500 to 1000°C. [Figure 11] These are the results of tensile tests on heat-treated materials at 1400 to 1600°C. [Figure 12] Room temperature tensile test results of samples using different additive manufacturing techniques. [Figure 13] FIG. 1 is a diagram showing the shape of a test piece for a tensile test at 1400 to 1600° C. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] One embodiment of the method for producing a Ta alloy member according to the present invention will be described with reference to the process flow shown in FIG.
[0015] The Ta alloy powder used in this embodiment contains Ta as a main component and a small amount of W. W improves the strength of the Ta alloy by solid solution strengthening.
[0016] An example of such a Ta alloy is an alloy whose representative composition by mass is represented as "Ta-2.5W", containing 2.0-3.5 mass% W, with the balance being Ta and unavoidable impurities. In this specification, the number before the alloying element in the representative composition indicates the content by mass%. R05252, the uniform numbering system (UNS) for alloys by the American Society for Testing and Materials (ASTM) and the Society of Automotive Engineers (SAE), specifies an alloy whose representative composition is Ta-2.5W, containing 2.0-3.5 mass% W, with the balance being Ta and unavoidable impurities. In this standard, the maximum values of impurities are, by mass, Nb: 0.50%, Fe: 0.010%, Ti: 0.010%, Mo: 0.020%, Si: 0.005%, Ni: 0.010%, C: 0.010%, O: 0.015%, N: 0.010%, and H: 0.0015%. The Ta alloy powder used in this embodiment contains the elements listed here as representative unavoidable impurities. In the powder raw material used in additive manufacturing, the surface area is large, so the content of non-metallic impurities may exceed the maximum value of the standard, and in particular, oxygen (O) inevitably exceeds the maximum value of the standard in most cases.
[0017] Another example of a Ta alloy has a representative composition by mass of "Ta-4W-1Re-0.7Hf-0.025C", which contains 2.0-4.5% W, 0.5-1.2% Re, 0.5-1.0% Hf, 0.005-0.045% C, and the remainder is Ta and unavoidable impurities. This alloy was designed based on ASTAR-811C (representative composition: Ta-8W-1Re-0.7Hf-0.025C) developed for casting in the United States in the 1960s, taking into consideration the effect of residual stress in additive manufacturing materials. Additive manufacturing materials have a larger residual stress than cast materials, and in the experimental results described below, Ta-13W alloy material cracked after long-term polishing. Therefore, it was considered necessary to reduce the W content for additive manufacturing, and the W content of ASTAR-811C was reduced to 4% by mass. As with Ta-2.5W, the powder raw material used for additive manufacturing contains a higher amount of nonmetallic impurities than the cast product. The carbon (C) in this alloy is not an impurity but an alloying element added with the intention of precipitation hardening by forming carbides, but the powder used in the examples described below contains about 0.04% C, which is higher than that of ASTAR-811C. Note that 0.05 to 0.15 mass% Zr may be added to this alloy for precipitation hardening by forming oxides.
[0018] The grain size of the alloy powder is preferably 10 to 100 μm, more preferably 20 to 60 μm, in terms of the volume-based median value (d50) of the grain size measured by a laser diffraction / scattering method. In addition, it is preferable that the raw material powder for additive manufacturing has a relatively wide grain size distribution so that the filling rate can be increased when forming a thin layer. As a guideline for the grain size distribution width, (d90-d10) is preferably 0.5 to 1.5 times d50. Note that d10, d50, and d90 represent the grain sizes at the points where the cumulative curve is 10%, 50%, and 90%, respectively, when the total volume is 100%.
[0019] Using the alloy powder, a component is formed by additive manufacturing technology. The additive manufacturing method preferably uses selective laser melting (SLM). The SLM method is a type of powder bed fusion method, in which the raw alloy powder is spread on a modeling stage to form a uniform thin layer, and a laser beam is scanned and irradiated to a predetermined position of the thin layer to melt and solidify the alloy powder, thereby stacking the alloy layers and forming a desired shape.
[0020] Due to the molding method, objects molded by the SLM method contain many columnar crystals extending in the lamination direction of the alloy. Therefore, mechanical properties such as tensile strength differ between the lamination direction and the direction perpendicular to it. In the following, the lamination direction during molding is called the Z direction, and the direction perpendicular to the lamination direction is called the XY direction. In the SLM method, in order to suppress the influence of bias in the scanning direction of the laser light, lamination is performed by rotating the scanning direction by a predetermined angle for each layer, so that the structure of the molded object is isotropic in a plane perpendicular to the Z direction. In this specification, the XY direction only means perpendicular to the Z direction, and does not mean a specific direction in a plane perpendicular to the Z direction.
[0021] Next, the object obtained by additive manufacturing is heat-treated to remove residual stress. In additive manufacturing of high-melting-point metals such as Ta alloys, the molten powder solidifies rapidly, so the residual stress after molding is particularly large. By removing the residual stress, it is possible to prevent the object from cracking during heat treatment to stabilize the structure, which will be described later, or during processing to finish the product.
[0022] The residual stress relief treatment is preferably carried out at a temperature of 1100°C or higher and 1300°C or lower. If the treatment temperature is too low, the residual stress is not sufficiently relieved. On the other hand, if the treatment temperature is too high, the molded object may crack while being heated to the treatment temperature. The time for which the molded object is held at the treatment temperature is preferably 30 minutes or more and 5 hours or less. If the holding time is too short, the internal temperature may not rise to the set temperature depending on the shape of the molded object. On the other hand, a longer holding time has no particular effect and reduces productivity.
[0023] In order to distinguish between heat treatment for residual stress relief and heat treatment for stabilizing the structure, which will be described below, the former will be referred to as "residual stress relief treatment" and the latter as "stabilization treatment" or simply "heat treatment."
[0024] The molded product from which the residual stress has been removed is further heat-treated at a high temperature to stabilize the structure, etc. The purpose of this heat treatment is to give the molded product ductility and stabilize the structure. This stabilization treatment reduces the dislocation density, thereby improving the ductility of the molded product. The stabilization treatment temperature is 1400°C or higher, preferably 1600°C or higher. This provides sufficient ductility and stabilizes the structure. Furthermore, the higher the temperature, the faster the stabilization of the structure progresses. On the other hand, the stabilization treatment temperature is 2000°C or lower, more preferably 1800°C or lower. Increasing the treatment temperature beyond this level does not have any particular effect, and increases the treatment cost.
[0025] The stabilization treatment uniformly dissolves the solute atoms, but the stabilization treatment in this embodiment is different from the solution treatment for precipitation hardened alloys. In the case of precipitation hardened alloys, solution treatment is performed to dissolve the solute atoms uniformly, and then aging treatment is performed to precipitate the precipitates. In the solution treatment, cooling is performed by water cooling or air cooling to a degree of rapid cooling in order to maintain the state of the solution structure. In contrast, Ta-2.5W is a solid solution strengthened alloy by W, so solution treatment is not required. It is said that the effect of precipitation hardening due to the precipitation of carbides is also manifested in ASTAR-811C, and aging treatment may be performed in the Ta-4W-1Re-0.7Hf-0.025C alloy, but aging treatment after heat treatment is not performed in this embodiment. Rapid cooling is not required in the stabilization treatment in this embodiment.
[0026] The Ta alloy part of the present embodiment is obtained by the above-mentioned additive manufacturing, residual stress relief, and stabilization treatment. The obtained Ta alloy part is then subjected to processes such as cutting, polishing, cleaning, drying, and protective coating for oxidation suppression as necessary to become a final product. EXAMPLES
[0027] The method for producing the Ta alloy member of this embodiment will be described in further detail based on experimental results.
[0028] Four types of Ta alloy powders with different compositions and pure Ta powder were used, and additive manufacturing was performed by the SLM method to produce Ta alloy parts and Ta pure metal parts in the examples and comparative examples by changing the presence or absence and conditions of residual stress relief treatment and stabilization treatment.
[0029] Additive manufacturing was performed using a powder deposition modeling system (EOS GmbH, M100) equipped with a Yb-fiber laser (power 200 W, beam diameter 40 μm). Some alloy compositions were also fabricated with a larger powder deposition modeling system (EOS GmbH, M290, Yb-fiber laser power 400 W, beam diameter 80 μm).
[0030] The residual stress relief treatment was performed by placing the molded object in an electric furnace and heating it at 900 to 1200°C for 1 to 4 hours. The stabilization treatment was performed by further increasing the temperature of the electric furnace after the residual stress relief treatment, and heating it at 1400 to 1600°C for 1 to 4 hours, and then cooling it at 200°C / h to 1200°C, and 10°C / min from 1200°C to 400°C, and then furnace cooling. It is also possible to cool the molded object after the residual stress relief treatment and then heat it again to perform the stabilization treatment, rather than performing the residual stress relief treatment and the stabilization treatment consecutively.
[0031] The microstructure of the components was observed by optical microscopy, scanning electron microscopy (SEM) and energy dispersive X-ray spectroscopy (EDS) of the cross-sections of the samples, and the grain size and crystal orientation were measured by electron backscatter diffraction (EBSD).
[0032] The mechanical properties of the components were evaluated by tensile tests, and were evaluated by 0.2% yield strength, tensile strength, and elongation at break. Tensile tests at room temperature in air were performed in accordance with the ASTM E8-21 standard. The test speed was a stress increase rate of 9MPa / s up to 0.2% yield strength, and a strain rate of 20% / min thereafter. Tensile tests at 500-1600°C in an Ar atmosphere were performed using an MTS808 material testing machine in accordance with the ASTM E21-20 standard. The test pieces were heated at a rate of 50°C / min, and the test temperature was maintained for 30 minutes before the test was started. The test speed was a strain rate of 0.5% / min up to 0.2% yield strength, and a strain rate of 5% / min thereafter. Tensile tests at -170°C in air were performed using an MTS810 material testing machine in accordance with the ASTM E8-21 standard. The test piece was cooled to -170℃, and after reaching the test temperature, it was held for 30 minutes before the test was started. The test speed was a stress increase rate of 9MPa / s up to 0.2% yield strength, and thereafter the strain rate was 20% / min. In the following, 0.2% yield strength and tensile strength are collectively referred to as "strength", and breaking elongation is simply referred to as "elongation".
[0033] For the tensile tests at room temperature and 500 to 1000 ° C, round test pieces with a straight part diameter of 3 mm and a length of 15 mm were used. The tensile test pieces in the stacking direction (Z direction) were made by layering a 6 × 6 × 46 mm rectangular parallelepiped in the long side direction and cutting. The tensile test pieces in the direction perpendicular to the stacking direction (XY direction) were made by layering the same rectangular parallelepiped in the short side direction and cutting. On the other hand, for the tensile tests at 1400 to 1600 ° C, flat test pieces shown in Figure 13 were used. The tensile test pieces in the Z direction were made by layering a 3 mm thick rectangular plate in the long side direction and cutting. The tensile test pieces in the XY direction were made by layering a 3 mm thick rectangular plate in the short side direction and cutting. All test pieces were polished with abrasive paper so that the arithmetic mean roughness Ra of the surface was 0.8 μm. In addition, for the tensile tests at 1400°C to 1600°C, a chuck made by additive manufacturing of a Ta-3W alloy was used.
[0034] Table 1 shows the composition and particle size of the powder used. Table 2 shows the manufacturing conditions for the components. In Tables 1 and 2, "CPTa" is commercially pure Ta. "Ta2.5W" and "Ta3W" are both alloys with the representative composition Ta-2.5W. "Ta4W+" is an alloy with the representative composition Ta-4W-1Re-0.7Hf-0.025C. The Ta4W+ alloy powder was manufactured with a target C content of 0.025 mass%, but analysis showed that the C content was approximately 0.04 mass%. "Ta13W" is a Ta-13W alloy.
[0035] [Table 1]
[0036] [Table 2]
[0037] When the cross section perpendicular to the lamination direction was examined with an optical microscope, numerous cracks were found at the grain boundaries of Ta13W in both the as-printed material and the sample that had been subjected to residual stress relief treatment and stabilization treatment at 1600℃ for 1h. These cracks are believed to have been generated during polishing for cross-sectional observation. This indicates that the residual stress of the additively manufactured material is extremely high in Ta13W, and that recrystallization did not occur even after stabilization treatment at 1600℃. No such cracks were observed in samples other than Ta13W.
[0038] Table 3 shows the results of the tensile tests at room temperature.
[0039] [Table 3]
[0040] Figure 2 shows the results of tensile tests at room temperature on the as-printed materials. For Ta2.5W, data is shown for materials printed using the same equipment (M100) as the other compositions. The effects of differences in equipment will be discussed later. From the results in Table 3 and Figure 2, it was confirmed that for samples from CPTa to Ta4W+, there was a tendency for strength to increase and elongation to decrease as the W content increased. Ta4W+ showed very high strength, but poor ductility and low elongation. Ta13W had low strength and elongation, and it is thought that the test specimen probably contained microcracks.
[0041] Figure 3 shows the results of tensile tests at room temperature for the as-printed material (AS) and heat-treated material. For Ta2.5W, data is shown for material printed using the same equipment (M100) as for the other compositions. The results in Table 3 and Figure 3 show that for CPTa, residual stress relief treatment and stabilization treatment caused a slight decrease in strength and an increase in elongation. For Ta2.5W and Ta3W, there was a tendency for stabilization treatment to increase both strength and elongation. For Ta4W+, stabilization treatment caused a decrease in strength and an increase in elongation. For Ta13W, sufficient elongation was not obtained even with stabilization treatment. Since cracks due to residual stress in Ta13W are not improved by heat treatment, it is thought that ductility was not obtained.
[0042] For space applications, strength at room temperature is not a particular issue, but a certain degree of elongation is required to withstand the vibrations that occur during launch, and an elongation of approximately 5% or more is preferable. In this regard, CPTa, Ta2.5W, and Ta3W showed sufficient elongation even in the as-formed state. For Ta4W+, the elongation was small in the as-formed state, but the elongation exceeded 5% after heat treatment at 1500°C, and the elongation was similarly good in both the Z and XY directions after heat treatment at 1600°C. This shows that the heat treatment temperature for Ta4W+ is preferably 1500°C or higher, and more preferably 1600°C or higher.
[0043] The changes in the structure due to heat treatment were investigated using EBSD. Figures 4 to 8 show the grain boundaries obtained by EBSD. The figures show an area of 700 x 1750 μm in a cross section parallel to the stacking direction, and the areas where the crystal orientation is misaligned by 15 degrees or more are regarded as grain boundaries. Figures 4 to 8 show that for all compositions, the size of the grains does not appear to change significantly due to heat treatment.
[0044] Table 4 shows the average and standard deviation of the distance between two parallel lines sandwiching a crystal grain in Figures 4 to 8. In Table 4, H is the value in the horizontal direction in Figures 4 to 8, and V is the value in the vertical direction (stacking direction Z) in Figures 4 to 8. In what follows, this distance is referred to as the "grain size in the cross section." Because the cut surface does not pass through the part where the grain size of each crystal grain is at its maximum, the grain size in the cross section is smaller than the actual grain size and there is a large variation, but it does provide a quantitative index of the size of the crystal grains. From Table 4, it appears that the grain size in the cross section increases somewhat due to heat treatment, but the change is not significant, and since the structure does not recrystallize, it is considered to be within the margin of error.
[0045] [Table 4]
[0046] In addition, although not shown in the figure, EBSD showed that the crystal orientation of each crystal grain was varied in the samples of Figures 4 to 8, and no change in this tendency was observed even after heat treatment. As will be described later, in the Ta2.5W fabricated by M290, the crystal orientation was body-centered cubic in the Z direction. <001> Although the direction was consistent, there was no difference between the as-formed material and the heat-treated material.
[0047] From the above results, it is believed that the heat treatment causes almost no change in the size of the crystal grains, but increases ductility by reducing the dislocation density within the crystal grains, and the structure becomes stable thereafter. However, there were internal cracks in Ta13W, which were not improved by heat treatment.
[0048] Furthermore, the effects of oxygen (O) and carbon (C) were investigated using SEM and EDS. Figure 9 shows SEM images of the as-printed and heat-treated Ta4W+ materials, and the heat-treated Ta2.5W material. The length of the bar at the bottom of Figure 9 is 1 μm. No precipitates were observed in the as-printed Ta4W+ material (Figure 9A). In contrast, precipitates were observed at the grain boundaries in the Ta4W+ materials heat-treated at 1500°C (Figure 9B) and 1600°C (Figure 9C). There was no significant difference between Figures 9B and 9C. Additionally, no precipitates were observed in the heat-treated Ta2.5W material that did not contain Re or Hf (Figure 9D).
[0049] The elemental distribution by EDS (not shown) confirmed that the relatively large precipitates in the heat-treated Ta4W+ material were carbides and the smaller precipitates were oxides. It was further confirmed that the oxides were oxides of Hf. The oxides were probably HfO 2 It was also confirmed that the carbide was Ta. According to the Ta-C binary phase diagram, the carbide was Ta. 2 In the heat-treated Ta2.5W material (Fig. 9D), oxides did not precipitate because it did not contain Hf, and carbides did not precipitate because the C content was low.
[0050] From the above results, it is believed that Ta4W+ has poor ductility due to impurities such as O, C, and the metallic elements W, Re, and Hf being supersaturated in the Ta matrix phase when rapidly cooled after additive manufacturing, and that ductility is restored by stabilization treatment, with O precipitating at the grain boundaries as Hf oxides and C as Ta carbides. In addition, the oxides and carbides that form are stable, and therefore it is presumed that the structure after high-temperature stabilization treatment is stable and does not change depending on the cooling rate.
[0051] The results of tensile tests at high and low temperatures for the heat-treated materials are shown in Table 5. Figure 10 shows the test results at 500-1000°C, and Figure 11 shows the test results at 1400-1600°C.
[0052] [Table 5]
[0053] Comparing the results of the tensile tests at room temperature (Table 3 and Figure 3) in Table 5 and Figures 10 and 11, the strength of all samples decreased, and the strength gradually decreased as the test temperature increased. In addition, the elongation of CPTa also clearly decreased as the test temperature increased.
[0054] From Table 5 and Figure 11, the samples stabilized at 1500°C or 1600°C of Ta2.5W had sufficient strength even at 1600°C, which is higher than the heat resistance temperature of Nb alloys. Furthermore, the sample heat-treated at 1600°C of Ta4W+ showed an extremely large tensile strength of 208MPa in the XY directions at 1600°C. There are no tensile test results at 1600°C for the Z direction of the same sample, but since the strength and elongation were similar in both the Z direction and the XY direction in the tensile test at room temperature (Table 3 and Figure 3), it is believed that the strength and elongation in the Z direction at 1600°C will also be similar to those in the XY direction. Ta13W also showed small elongation in the tensile test at 1600°C.
[0055] As mentioned in the explanation of the tensile test results at room temperature, the as-formed Ta4W+ material has poor ductility because impurities such as O, C, and the metallic elements W, Re, and Hf are supersaturated in the Ta matrix phase due to rapid cooling after additive manufacturing, and it is believed that the ductility was restored by the stabilization treatment causing O to precipitate as oxides and C to precipitate as carbides at the grain boundaries. Furthermore, it is believed that the oxides and carbides precipitated at the grain boundaries suppressed recrystallization, stabilizing the structure and contributing to improving the tensile strength at high temperatures.
[0056] In space applications, both strength and elongation at high temperatures are important. In this regard, Ta2.5W and Ta4W+ showed sufficient strength and elongation in tensile tests at 1600℃, making them suitable for space applications.
[0057] From Table 5, it was confirmed that the sample in which the residual stress of Ta3W was relieved at 1200°C and stabilized at 1500°C did not show low-temperature brittleness even in the tensile test at -170°C.
[0058] Next, we will discuss the effects of differences in the equipment. The M100, which was mainly used in the additive manufacturing of this example, is a small equipment used for research and development and the production of small parts, while the M290 is a large equipment used for the production of larger parts.
[0059] Table 6 and Figure 12 show the results of tensile tests on samples printed using M100 and M290 for Ta2.5W. Table 6 and Figure 12 show that in tensile tests at room temperature, the sample printed using M100 had a higher tensile strength. This is thought to be because the crystal grains in the printing material for M100 were smaller than those in M290, as shown in Table 4, resulting in higher strength. It is known that the crystal grain size depends on the laser beam diameter and output. On the other hand, there is no significant difference between the two in terms of elongation. Measurement of crystal orientation using EBSD showed that the crystal orientation was random in the material printed using M100, while the material printed using M290 had a body-centered cubic orientation in the Z direction. <001> The crystal orientation was consistent. This difference in crystal orientation is thought to be due to the difference in the characteristics of the additive manufacturing equipment, and probably due to the difference in the direction of the heat flow during solidification. Thus, although there are some differences in the structure and properties of the molded parts between M100 and M290, the strength and elongation of the tensile test were comparable, and the findings obtained with M100 are thought to be valid when using M290.
[0060] [Table 6]
[0061] Conventionally, Ta alloys with a high W content, such as Ta-10W and ASTAR-811C, have often been considered for space applications. However, the above-mentioned comparative example, Ta13W, did not achieve sufficient elongation even after heat treatment. From this, it was found that Ta alloys with a relatively low W content are suitable for the production of space components using additive manufacturing.
[0062] From the results of the tensile test at 1600°C, it was found that sufficient strength and elongation can be obtained for Ta2.5W and Ta4W+ by stabilization at 1500°C or higher. It was confirmed that the additively manufactured stabilized Ta2.5W material can be applied to space applications, not to mention other applications such as chemical plants. Furthermore, the stabilized Ta4W+ material showed very high strength at 1600°C, and was the most suitable alloy for space applications among the present examples. Since there was almost no difference in the tensile test results at room temperature between Ta2.5W and Ta3W, it is considered that almost the same results were obtained if the W content of Ta4W+ was in the range of 4.0±0.5 mass%.
[0063] The present invention is not limited to the above-described embodiment and examples, and various modifications are possible within the scope of the technical concept thereof.
Claims
1. preparing an alloy powder of a Ta alloy containing 2.0 to 4.5 mass% W with the remainder being Ta and unavoidable impurities; an additive manufacturing step of depositing the alloy powder by additive manufacturing techniques to form a shaped object; A stabilization step of heat treating the shaped object at a temperature of 1400° C. or more and 2000° C. or less, The additive manufacturing process is carried out using selective laser melting. A method for manufacturing a Ta alloy part.
2. preparing an alloy powder of Ta alloy containing 2.0 to 4.5 mass% W, 0.5 to 1.2 mass% Re, 0.5 to 1.0 mass% Hf, 0.005 to 0.045 mass% C, with the balance being Ta and unavoidable impurities; an additive manufacturing step of depositing the alloy powder by additive manufacturing techniques to form a shaped object; a stabilization step of heat treating the shaped object at 1400° C. or more and 2000° C. or less; A method for producing a Ta alloy member having the above structure.
3. The stabilization step causes oxides of Hf and carbides of Ta to precipitate. The method for producing a Ta alloy part according to claim 2.
4. The method further includes a residual stress relief step of heat treating the shaped object at 1100° C. or more and 1300° C. or less after the additive manufacturing step. The method for producing a Ta alloy part according to any one of claims 1 to 3.
Citation Information
Patent Citations
Method for Producing Parts with Tantalum and Tantalum Alloy
CN106334793A
Method and apparatus for producing metal powder material
JP2018522136A
Manufacturing methods for electronic components using 3D printing
JP2019529709A
Spherical tantalum powder, products containing same, and methods for producing same
JP2021515105A
Manufacturing method for Nb alloy components
JP7412867B1
Cited By
Dynamic self-enhancement dislocation configuration regulation and control method for refractory alloy in additive manufacturing and application of dynamic self-enhancement dislocation configuration regulation and control method
CN119368763A