Conductive leather or conductive fiber, and method for producing conductive leather or conductive fiber
Conductive leather or fiber is achieved using carbon nanotubes, graphene, and nanoparticles with a water-repellent layer, addressing color variation and friction issues, ensuring high conductivity and abrasion resistance while maintaining texture.
Patent Information
- Application Number
- JP2021561100
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2019-11-29
- Publication Date
- 2024-10-10
- Estimated Expiration
- 2039-11-29
AI Technical Summary
Existing conductive materials for touch-sensitive products, such as smartphone gloves, often cause color variation, allergic reactions, and reduced conductivity due to friction, and there is a lack of conductive natural leather products that maintain texture and provide water repellency.
A conductive leather or fiber configuration using single-wall carbon nanotubes, graphene nanoparticles, silica and tin oxide nanoparticles, with a first layer of these nanoparticles and a second layer containing a water repellent and conductive material, applied in specific proportions to maintain conductivity and abrasion resistance.
The solution provides conductive leather or fiber with excellent abrasion resistance and conductivity without altering the texture, achieving a surface resistance comparable to human skin and maintaining transparency.
Abstract
Description
[Technical field]
[0001] The present invention relates to conductive leather or conductive fiber, and a method for producing conductive leather or conductive fiber. [Background technology]
[0002] Nowadays, with the spread of smartphones and other devices, touch panel operations are commonplace. Products that allow users to use these touch panels while wearing gloves or other winter gear are on sale.
[0003] However, these products generally use conductive threads, and when metallic conductive threads are used, the color of the product differs only in the parts where the conductive threads are used, which not only mars the product's appearance but also may cause allergic reactions depending on the type of metal.In addition, conductive threads are generally relatively weak against friction, and therefore their conductivity often decreases due to friction.
[0004] Processing for imparting electrical conductivity is used for synthetic fibers and the like. On the other hand, it seems that there are few products that use electrical conductivity processing for natural fibers or natural leather. In particular, since many natural leather products are high-end products, products that do not change the texture, such as color, are required from the viewpoint of design. In addition, among the characteristics required for products such as gloves for smartphones, there is a demand for the surface of the product to be water-repellent. However, surface treatment agents that impart water repellency make the surface of the product insulating, thereby hindering the conductivity of the product surface, so products that are used on the entire surface of the product are not widespread. As a result, in the case of gloves for smartphones, it is common to make only a part of the fingertips conductive (for example, Patent Document 1). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2017-160582 A Summary of the Invention [Problem to be solved by the invention]
[0006] An object of the present invention is to provide leather or fiber that is imparted with electrical conductivity without changing the texture of the base and has excellent abrasion resistance. [Means for solving the problem]
[0007] The present invention relates to conductive leather or conductive fiber that has solved the above problems by having the following configuration, and a method for producing conductive leather or conductive fiber. [1] (A) A nanoparticle comprising a single-walled carbon nanotube, a graphene nanoparticle, a single silica nanoparticle, and a single tin oxide nanoparticle; A first layer including 40 to 60 parts by mass of silica single nanoparticles having a size of 5 nm or less as measured by a transmission electron microscope, and 60 to 40 parts by mass of tin oxide particles having a size of 2 nm or less as measured by a transmission electron microscope, per 100 parts by mass of the total of the silica single nanoparticles and the tin oxide single nanoparticles; (B) a second layer including a water repellent and a conductive material; A conductive leather or a conductive fiber, comprising the above in this order from the surface. [2] The surface sheet resistance is 9.9×10 6 The conductive leather or conductive fiber according to the above [1], having a resistance of Ω / □ or less. [3] A process for the surface of leather or textiles, comprising: (A) a single-walled carbon nanotube, a graphene nanoparticle, a single silica nanoparticle, a single tin oxide nanoparticle, and water; a step of forming a first layer by applying or immersing a surface in a first layer forming dispersion liquid containing 40 to 60 parts by mass of single silica nanoparticles of 5 nm or less as measured by a transmission electron microscope and 60 to 40 parts by mass of single tin oxide nanoparticles of 2 nm or less as measured by a transmission electron microscope, per 100 parts by mass of the total of single silica nanoparticles and single tin oxide nanoparticles; (B) A process of applying to or immersing a surface in an aqueous solution for forming a second layer, the aqueous solution containing a water repellent, a conductive material, and water, to form a second layer. A method for producing conductive leather or conductive fiber, comprising the steps of: [4] A method for producing conductive leather or conductive fiber according to the above [3], wherein in step (A), the dispersion for forming a transparent conductive thin film is applied to or immersed in a surface, and then the surface is rolled. Effect of the Invention
[0008] According to the present invention [1], it is possible to provide leather or fiber that is imparted with electrical conductivity without changing the texture of the base and has excellent abrasion resistance.
[0009] According to the present invention [3], electrical conductivity is imparted without changing the texture of the base, and leather or fiber having excellent abrasion resistance can be easily produced. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] [Conductive leather or conductive fabric] The conductive leather or conductive fiber of the present invention (hereinafter referred to as conductive leather, etc.) comprises (A) single-walled carbon nanotubes, graphene nanoparticles, single silica nanoparticles, and single tin oxide nanoparticles, A first layer including 40 to 60 parts by mass of silica single nanoparticles having a size of 5 nm or less as measured by a transmission electron microscope, and 60 to 40 parts by mass of tin oxide single nanoparticles having a size of 2 nm or less as measured by a transmission electron microscope, per 100 parts by mass of the total of silica single nanoparticles and tin oxide single nanoparticles; (B) a second layer comprising a water repellent and a transparent conductive material; The first layer and the second layer can be formed from a dispersion liquid described later.
[0011] With this configuration, the present invention can provide leather or fiber that is imparted with electrical conductivity without changing the texture of the base and has excellent abrasion resistance.
[0012] The present invention forms a transparent conductive film on leather or fiber (hereinafter referred to as leather, etc.). The transparent conductive film uses single-walled carbon nanotubes and graphene, and has a surface resistance of 10 times that of a human hand without compromising transparency. 6 The first layer is made to have a resistance of Ω / □ or less, and the second layer is made to have a water repellent agent on top of it to maintain the conductivity of the first layer, and a conductive material such as tin oxide. This reduces the sheet resistance to 10 7 It is possible to form a transparent conductive film that is a water-repellent coating without lowering the conductivity to the Ω / □ range. The present invention can achieve water-repellent conductivity without changing the texture of leather or the like with this transparent conductive film, and unlike synthetic fibers and synthetic leathers that have conductive agents kneaded into them, it can contribute to the multi-functionalization of natural fibers and natural leathers.
[0013] The leather is not particularly limited, but examples include natural leather, artificial leather, etc. An example of the thickness of the leather is 0.5 to 2 mm, and in particular, the thickness of the leather for gloves is about 0.5 mm.
[0014] The fibers are not particularly limited, but include natural fibers (cotton, linen, silk, etc.), synthetic fibers, etc.
[0015] Although the single-walled carbon nanotube is not particularly limited, it is preferable that the single-walled carbon nanotube has a fiber diameter of 0.5 nm or less, an aspect ratio of 5 or more, and a length of 10 nm or less. Among the single-walled carbon nanotubes, the single-walled carbon nanotube is more preferable. The single-walled carbon nanotubes having the above fiber diameter and aspect ratio can be uniformly dispersed in a solvent and can form sufficient contact points with each other.
[0016] The fiber diameter of single-walled carbon nanotubes is the mass average particle diameter obtained by observing a transmission electron microscope photograph (magnification: 100,000 times) (n=50). Also, the aspect ratio of single-walled carbon nanotubes is obtained by observing a transmission electron microscope photograph (magnification: 100,000 times) and calculating (length / fiber diameter) (n=50).
[0017] In addition, it is preferable that the single-walled carbon nanotubes are dispersible in a solvent without using a dispersant. Treatment with a strong acid such as sulfuric acid is an example of a treatment for dispersing the single-walled carbon nanotubes in a solvent. Single-walled carbon nanotube dispersions that do not use a dispersant are also commercially available.
[0018] Graphene nanoparticles include graphene having an average thickness (c-axis direction) of 50 nm or less and a diameter in the radial direction (a-axis direction) of 2 μm or less, which is monodispersed in water. Powder of graphene nanoparticles having an average thickness of 5 nm or less imparts antistatic properties and abrasion resistance to a thin film formed from a coating agent. An example of the length of graphene is 5 nm to 3 μm. From the viewpoint of flame retardancy and film formation of a uniform thickness, the average thickness of graphene is preferably 1 to 5 nm. Here, the average thickness and length of graphene are the mass average particle diameters obtained by observing transmission electron microscope photographs (magnification 100,000 times) (n=50).
[0019] Single nanoparticles refer to those whose particle diameter (n=50) measured by a transmission electron microscope is less than 10 nm. For 100 parts by mass of single nanoparticles, it is preferable that the amount of single silica nanoparticles of 5 nm or less is 40 to 60 parts by mass, and that of single silica nanoparticles of 2 nm or less is 30 to 40 parts by mass. Here, if silica nanoparticles of 10 nm or more are used, the increase in the transmittance of the substrate with a transparent conductive thin film is low, and the abrasion resistance of the transparent conductive thin film is reduced. In addition, the conductivity is likely to decrease. If the amount of single silica nanoparticles of 2 nm or less exceeds 40 parts by mass, the dispersion for forming a transparent conductive thin film is likely to gel. From the viewpoints of handling and availability, it is preferable that the single silica nanoparticles of 2 nm or less are 0.5 nm or more.
[0020] The single silica nanoparticles of 2 nm or less preferably contain amorphous silica, the amorphous nature of which is confirmed by X-ray diffraction.
[0021] From the viewpoints of the conductivity, transmittance, and abrasion resistance of the first layer, the amount of single nanoparticles of tin oxide of 2 nm or less is 60 to 40 parts by mass, preferably 50 parts by mass or more, per 100 parts by mass of single nanoparticles. Tin oxide powder with an average primary particle size of 10 nm or more is unlikely to cause secondary aggregation by itself, but is prone to secondary aggregation when mixed with other materials, which is not preferred.
[0022] The first layer preferably has a thickness of 50 to 300 nm from the viewpoints of electrical conductivity, transparency, and abrasion resistance, and more preferably has a thickness of 50 to 80 nm from the viewpoint of the effect on the color of leather, etc. If the thickness of the first layer is less than 50 nm, the sheet resistance of the surface of leather, etc., may be less than 10 6 If the resistance exceeds 300 nm, the film will crack and peel off easily. 7 When the resistance is in the Ω / □ range, it becomes difficult to use, so the surface sheet resistance is 9.9×10 6 It is preferable that the resistance is Ω / □ or less.
[0023] The second layer contains a water repellent agent to maintain the electrical conductivity of the first layer, and a transparent conductive material with antistatic properties.
[0024] Examples of the water repellent include fluorine resins and silicone resins, which may be used alone or in combination. As the fluorine resin, Asahi Guard series AG-E600 from AGC Corporation, and as the silicone resin, water-based emulsion POLON-SR CONIC from Shin-Etsu Silicone, etc. are preferred as water repellents that can be used in combination with antistatic substances such as ionic surfactants.
[0025] Examples of the conductive material include tin oxide powder and ionic surfactants, and tin oxide alone and a combination of tin oxide powder and an ionic surfactant are preferred. The tin oxide powder is as described above, and examples of the ionic surfactant include quaternary ammonium salts. The ionic surfactant is preferably an amphoteric surfactant having both cationic and anionic polarities.
[0026] Examples of quaternary ammonium salts include alkyltrimethylammonium salts and dialkyldimethylammonium salts, and examples of commercially available products include the 1SX series from Taisei Fine Chemical Co., Ltd.
[0027] As the second layer forming dispersion for forming the second layer, a dispersion made by Japan Nano Coat (product name: AS-WR) can be used easily because the components are premixed.
[0028] From the viewpoints of water repellency and electrical conductivity, the second layer preferably has a thickness of 20 to 100 nm. If the thickness is less than 20 nm, the water repellency is likely to be insufficient, and if the thickness is more than 100 nm, the electrical conductivity is likely to decrease.
[0029] The second layer is 1×10 10 As long as the resistivity is Ω / □ or less and the transparency does not decrease (no change in color tone is observed visually), the effects of the present invention can be achieved.
[0030] [Method of producing conductive leather or conductive fiber] The method for producing the conductive leather or conductive fiber of the present invention comprises the steps of: A process for leather or textile surfaces, comprising the steps of: (A) a single-walled carbon nanotube, a graphene nanoparticle, a single silica nanoparticle, a single tin oxide nanoparticle, and water; a step of forming a first layer by applying or immersing a surface in a first layer forming dispersion liquid containing 40 to 60 parts by mass of single silica nanoparticles of 5 nm or less as measured by a transmission electron microscope and 60 to 40 parts by mass of single tin oxide nanoparticles of 2 nm or less as measured by a transmission electron microscope, per 100 parts by mass of the total of single silica nanoparticles and single tin oxide nanoparticles; (B) A process of applying to or immersing a surface in an aqueous solution for forming a second layer, the aqueous solution containing a water repellent, a conductive material, and water, to form a second layer. in that order.
[0031] [(A) Process] (A) step includes a single-walled carbon nanotube, a graphene nanoparticle, a single silica nanoparticle, a single tin oxide nanoparticle, and water; A first layer is formed by applying to or immersing the surface in a dispersion for forming a first layer, which contains 40 to 60 parts by mass of single silica nanoparticles of 5 nm or less as measured by a transmission electron microscope, and 60 to 40 parts by mass of single tin oxide nanoparticles of 2 nm or less as measured by a transmission electron microscope, per 100 parts by mass of the total of single silica nanoparticles and single tin oxide nanoparticles.
[0032] The first layer forming dispersion liquid contains (A) single-walled carbon nanotubes, graphene nanoparticles, single silica nanoparticles, single tin oxide nanoparticles, and water; The composition contains 40 to 60 parts by mass of silica single nanoparticles having a size of 5 nm or less as measured by a transmission electron microscope, and 60 to 40 parts by mass of tin oxide single nanoparticles having a size of 2 nm or less as measured by a transmission electron microscope, relative to a total of 100 parts by mass of silica single nanoparticles and tin oxide single nanoparticles.
[0033] The single-walled carbon nanotubes, graphene nanoparticles, and single silica nanoparticles are as described above.
[0034] The single-walled carbon nanotubes are preferably 0.01 to 0.1 parts by mass, more preferably 0.03 to 0.06 parts by mass, relative to 100 parts by mass of the first layer forming dispersion. If the amount is 0.2 parts by mass or more, the viscosity increases, the carbon nanotubes are easily aggregated, and the transmittance decreases.
[0035] The graphene nanoparticles are preferably contained in an amount of 0.001 to 0.1 parts by mass, and more preferably 0.005 to 0.01% by mass, relative to 100 parts by mass of the dispersion for forming the first layer.
[0036] The single nanoparticles are preferably 18 to 99.5 parts by mass relative to 100 parts by mass of the single nanoparticles, single-walled carbon nanotubes, and graphene nanoparticles in total. If the single nanoparticles are less than 18 parts by mass, the adhesion of the transparent conductive thin film is likely to decrease, and if the single nanoparticles are more than 99.5 parts by mass, the conductivity and heat dissipation of the transparent conductive thin film are likely to decrease. In addition, it is more preferable that the silica single nanoparticles are 40 to 60 parts by mass relative to 100 parts by mass of the silica single nanoparticles, single-walled carbon nanotubes, graphene nanoparticles, and tin oxide single nanoparticles in total, since the first layer has high conductivity and high transparency.
[0037] The amount of water is preferably 99.0 to 99.5 parts by mass relative to 100 parts by mass of the dispersion for forming the first layer. Although organic solvents other than water can be used as the solvent, water is used from the viewpoint of suppressing environmental pollution due to solvent volatilization.
[0038] The dispersion for forming the first layer can be obtained, for example, by stirring, melting, mixing, and dispersing various nanopowders, solvents, and other additives, simultaneously or separately, while adding heat treatment as necessary. The device for mixing, stirring, dispersing, etc. is not particularly limited, but a mortar and pestle machine, a ball mill, a planetary mixer, a bead mill, etc. can be used. These devices may also be used in appropriate combination. The dispersion for forming the second layer, which will be described later, can be obtained in the same manner.
[0039] The first layer forming dispersion may further contain additives and the like as necessary within the scope of the invention.
[0040] An example of a commercially available dispersion for forming the first layer is AS-SCNT manufactured by Japan Nano Coat.
[0041] The method for applying the first layer forming dispersion to the surface of leather or the like or immersing the surface in the dispersion is not particularly limited, but examples thereof include brush coating, spray coating, dipping, and the like.
[0042] As described above, the thickness of the first layer is preferably 50 to 300 nm. In the case of leather (thickness 0.5 to 2 mm, particularly 0.5 mm for gloves), the pick-up rate (mass of the first layer relative to 100 mass% of leather) is preferably 60%. In the case of cloth, the pick-up rate is preferably 200 to 300% after coating and immersion, and 60 to 120% after rolling, and more preferably 100%.
[0043] In step (A), when the dispersion for forming a transparent conductive thin film is applied to the surface or the surface is immersed in the dispersion liquid, and then the surface is rolled, the single-walled carbon nanotubes and graphene tend to be oriented horizontally to the surface of the leather or the like, which is preferable from the viewpoint of improving the conductivity and the transparency.
[0044] [(B) Process] In the step (B), a second layer is formed by applying to or immersing the surface in an aqueous solution for forming a second layer, the aqueous solution containing a water repellent, a conductive material, and water.
[0045] The second layer forming aqueous solution contains a water repellent, a conductive material, and water.
[0046] The water repellent and the conductive material are as described above. Although organic solvents other than water can be used as the solvent, water is used from the viewpoint of suppressing environmental pollution caused by the evaporation of the solvent.
[0047] The content of the water repellent agent is preferably 0.05 to 0.5 parts by mass with respect to 100 parts by mass of the second layer forming dispersion liquid.
[0048] The transparent conductive material is preferably 0.01 to 0.1 parts by mass with respect to 100 parts by mass of the second layer forming dispersion.
[0049] The amount of water is preferably 99.4 to 99.94 parts by mass with respect to 100 parts by mass of the second layer forming dispersion.
[0050] The second layer forming dispersion may further contain additives and the like as necessary within the scope of the invention.
[0051] An example of a commercially available dispersion for forming the second layer is a dispersion made by Japan Nano Coat (product name: AS-WR). It is preferable to dilute this dispersion made by Japan Nano Coat (product name: AS-WR) by about 20 times before use from the viewpoint of thickness control, etc.
[0052] The method for applying the dispersion for forming the second layer to the surface of leather or the like or immersing the surface in the dispersion for forming the first layer is not particularly limited, and is the same as the method for applying the dispersion for forming the first layer to the surface of leather or the like or immersing the surface in the dispersion for forming the first layer.
[0053] As described above, the thickness of the second layer is preferably 20 to 100 nm. In the case of leather (thickness 0.5 to 2 mm, particularly 0.5 mm for gloves), the pick-up rate (mass of the first layer relative to 100 mass% of leather) is preferably 60%. In the case of cloth, the pick-up rate is preferably 200 to 300% after coating and immersion, and 60 to 120% after rolling, and more preferably 100%. EXAMPLES
[0054] The present invention will be described with reference to examples, but the present invention is not limited thereto. In the following examples, parts and % indicate parts by mass and % by mass, unless otherwise specified.
[0055] The dispersion for forming the first layer in Example 1 was a water-based antistatic coating agent (product name: AS-SCNT) manufactured by Japan Nano Coat. This AS-SCNT was composed of 0.21% silica nanoparticles, 0.24% tin oxide nanoparticles, 0.04% single carbon nanotubes, 0.01% graphene, and the remainder: water. In Comparative Example 4, silica nanoparticles with an average particle size of 6 nm (manufactured by Fuso Chemical Co., Ltd., product name: PL-06L) were used. In Comparative Example 5, a mixture of 20 parts by mass of silica nanoparticles with an average particle size of 15 nm (manufactured by Fuso Chemical Co., Ltd., product name: PL-1) and 80 parts by mass of water was used.
[0056] The second layer forming dispersion was a 20-fold diluted dispersion made by Japan Nano Coat (product name: AS-WR, fluororesin: 5 mass %, silicone resin: 5 mass %, tin oxide: 0.1 mass %, balance: water).
[0057] Surface resistance was measured using Hozan Corporation (model number: F-109). Transparency was measured by measuring the transmittance of a transparent conductive thin film formed on a glass substrate (float glass) using a glass transmittance meter (model number: MJ-TM110) manufactured by Sato Shoji Co., Ltd. A transmittance drop of less than 1% from the float glass transmittance was deemed to have passed. Abrasion resistance testing was performed using a rubbing tester manufactured by Imoto Manufacturing Co., Ltd., and a cotton cloth was placed on the coated surface with a load of 1 kg, and after 20,000 revolutions, a product was deemed to have passed if the surface resistance did not drop to the 107 power.
[0058] Example 1 An aqueous solution for forming a first layer in Example 1 was prepared by mixing Japan Nano Coat's silica binder (product name: B-30 (3% solid content), Japan Nano Coat's tin oxide dispersion (product name: 4% tin oxide dispersion), and water to prepare a 3% solid content liquid (silica solid content: 1.4%, tin oxide solid content: 1.6%). 20 parts by mass of Japan Nano Coat's CNF 0.2% aqueous dispersion (product name: SCNT 0.2% aqueous dispersion) and 10 parts by mass of Japan Nano Coat's graphene liquid 0.1% aqueous dispersion (product name: graphene 0.1% aqueous dispersion) were added to the resulting solution, with the remainder being 55 parts by mass of water.
[0059] Glass substrate (float glass, transmittance: 91.6%, refractive index: 1.51, surface resistance: 10) with width: 50 mm, length: 100 mm, thickness: 3 mm 13 The first layer forming aqueous solution of Example 1 at 20°C to 25°C was added to the 3 The glass substrate was placed in a beaker and immersed for 20 seconds, after which the glass substrate was stood vertically and the aqueous solution for forming the first layer was poured over it, and coating was performed under conditions of an atmospheric temperature of 20 to 25° C. and a humidity of 50 to 55%. After coating, the glass substrate was dried at a temperature of 20° C. for 10 minutes to obtain a glass substrate with a first layer having a center thickness of approximately 60 nm.
[0060] The obtained glass substrate with the first layer had a transmittance of 91.5% and a surface resistance of 3.21×10 6 It was Omega.
[0061] Next, AS-WR was diluted 20 times with water to form the second layer dispersion, and the result was a transmittance of 91.0% and a surface resistance of 5.46×10 6 The transmittance after the abrasion resistance test was 91.0%, and the surface resistance was 7.32×10 6 It was Omega.
[0062] Natural leather (thickness: 0.5 mm) was treated in the same process. The color of the treated natural leather did not change, and the surface resistance was 3.64×10 6 Ω, and the surface resistance after the abrasion test was 5.21×10 6 There was no significant drop in the pick-up rate of the first layer, Ω. The pick-up rate of the second layer was 160%.
[0063] Example 2 An aqueous solution for forming a first layer in Example 2 was prepared by mixing Japan Nano Coat silica binder (product name: B-30 (solid content 3%)), Japan Nano Coat tin oxide dispersion (product name: tin oxide 4% dispersion), and water to prepare a 3% solid content liquid (silica solid content 1.2%, tin oxide solid content 1.8%), adding 20 parts by mass of Japan Nano Coat CNF 0.2% aqueous dispersion (product name: SCNT 0.2% aqueous dispersion), adding 10 parts by mass of Japan Nano Coat graphene liquid 0.1% aqueous dispersion (product name: graphene 0.1% aqueous dispersion), and the remainder being 55 parts by mass of water.
[0064] The glass substrate with the first layer obtained in the same manner as in Example 1 had a transmittance of 91.0% and a surface resistance of 8.35×10 5 It was Omega.
[0065] Next, dip-apply AS-WR diluted 20 times with water onto the first layer. Transmittance: 90.5%, Surface resistance: 3.34×10 6 The transmittance after the abrasion test was 90.5%, and the surface resistance was 5.77×10 6 It was Omega.
[0066] Example 3 An aqueous solution for forming a first layer of Example 3 was prepared by mixing Japan Nano Coat's silica binder (product name: B-30 (3% solid content), Japan Nano Coat's tin oxide dispersion (product name: 4% tin oxide dispersion), and water to prepare a 3% solid content liquid (1.8% silica solid content, 1.2% tin oxide solid content). 20 parts by mass of Japan Nano Coat's CNF 0.2% aqueous dispersion (product name: 0.2% SCNT aqueous dispersion) was added to the 15 parts by mass of the 3% solid content liquid (1.8% silica solid content, 1.2% tin oxide solid content) and 10 parts by mass of Japan Nano Coat's graphene liquid 0.1% aqueous dispersion (product name: 0.1% graphene aqueous dispersion), with the remainder being 55 parts by mass of water.
[0067] The glass substrate with the first layer obtained in the same manner as in Example 1 had a transmittance of 91.5% and a surface resistance of 6.46×10 6 It was Omega. Next, dip-apply AS-WR diluted 20 times with water onto the first layer. Transmittance 90.9%, surface resistance 6.77×10 6 After the abrasion test, the transmittance was 90.8%, and the surface resistance was 8.77×10 6 It was Omega.
[0068] Comparative Example 1 To 15 parts by mass of Japan Nano Coat's silica binder (product name: B-30 (solid content 3%)), 20 parts by mass of Japan Nano Coat's CNF 0.2% aqueous dispersion (product name: SCNT 0.2% aqueous dispersion) and 10 parts by mass of Japan Nano Coat's graphene liquid 0.1% aqueous dispersion (product name: graphene 0.1% aqueous dispersion) were added, with the remainder being 55 parts by mass of water, to prepare an aqueous solution for forming a first layer in Comparative Example 1.
[0069] The glass substrate with the first layer obtained in the same manner as in Example 1 had a transmittance of 91.2% and a surface resistance of 6.37×10 7 Ω, and the conductivity was low.
[0070] Comparative Example 2 An aqueous solution for forming the first layer of Comparative Example 2 was prepared by mixing Japan Nano Coat's silica binder (product name: B-30 (3% solid content), Japan Nano Coat's tin oxide dispersion (product name: 4% tin oxide dispersion), and water to prepare a 3% solid content liquid (2% silica solid content, 1% tin oxide solid content). 20 parts by mass of Japan Nano Coat's CNF 0.2% aqueous dispersion (product name: 0.2% SCNT aqueous dispersion) was added to this, and 10 parts by mass of Japan Nano Coat's graphene liquid 0.1% aqueous dispersion (product name: 0.1% graphene aqueous dispersion) was added, with the remainder being 55 parts by mass of water.
[0071] The glass substrate with the first layer obtained in the same manner as in Example 1 had a transmittance of 91.5% and a surface resistance of 8.76×10 6 It was Omega.
[0072] Next, dip-apply AS-WR diluted 20 times with water onto the first layer. Transmittance: 91.2%, Surface resistance: 3.21×10 7The conductivity of the substrate after the second layer was formed was low.
[0073] Comparative Example 3 A first layer-forming aqueous solution for Comparative Example 3 was prepared by mixing Japan Nano Coat's silica binder (product name: B-30 (3% solid content), Japan Nano Coat's tin oxide dispersion (product name: 4% tin oxide dispersion), and water to prepare a 3% solid content liquid (silica solid content: 1%, tin oxide solid content: 2%), to which 20 parts by mass of Japan Nano Coat's CNF 0.2% aqueous dispersion (product name: SCNT 0.2% aqueous dispersion) and 10 parts by mass of Japan Nano Coat's graphene liquid 0.1% aqueous dispersion (product name: graphene 0.1% aqueous dispersion), with the remainder being 55 parts by mass of water.
[0074] The glass substrate with the first layer obtained in the same manner as in Example 1 had a transmittance of 90.3% and a surface resistance of 7.86×10 5 It was Omega.
[0075] Next, dip-apply AS-WR diluted 20 times with water onto the first layer. Transmittance: 90.1%, Surface resistance: 1.56×10 6 In this comparative example, the transmittance was low. After the abrasion resistance test, the transmittance was 90.3% and the surface resistance was 3.36×10 7 Ω and the wear resistance was also low.
[0076] Comparative Example 4 A first layer-forming aqueous solution for Comparative Example 4 was prepared by mixing Fuso Chemical's silica binder (product name: PL-06L (solid content 6%), Japan Nano Coat's tin oxide dispersion (product name: tin oxide 4% dispersion), and water to prepare a 3% solid content liquid (silica solid content: 1.8%, tin oxide solid content: 1.2%). 20 parts by mass of Japan Nano Coat's CNF 0.2% aqueous dispersion (product name: SCNT 0.2% aqueous dispersion) and 10 parts by mass of Japan Nano Coat's graphene liquid 0.1% aqueous dispersion (product name: graphene 0.1% aqueous dispersion) were added to the 15 parts by mass of the resulting liquid, with the remainder being 55 parts by mass of water.
[0077] The glass substrate with the first layer obtained in the same manner as in Example 1 had a transmittance of 89.5% and a surface resistance of 7.46×10 7 Ω, and the transmittance and conductivity were low.
[0078] Comparative Example 5 A first layer-forming aqueous solution for Comparative Example 4 was prepared by mixing Fuso Chemical's silica binder (product name: PL-1 (12% solids)), Japan Nano Coat's tin oxide dispersion (product name: 4% tin oxide dispersion), and water to prepare a 3% solids solution (1.8% silica solids, 1.2% tin oxide solids). 20 parts by mass of Japan Nano Coat's CNF 0.2% aqueous dispersion (product name: 0.2% SCNT aqueous dispersion) and 10 parts by mass of Japan Nano Coat's graphene liquid 0.1% aqueous dispersion (product name: 0.1% graphene aqueous dispersion) were added to the 15 parts by mass of the resulting solution, with the remainder being 55 parts by mass of water.
[0079] The glass substrate with the first layer obtained in the same manner as in Example 1 had a transmittance of 90.7% and a surface resistance of 7.76×10 6 It was Omega.
[0080] Next, dip-apply AS-WR diluted 20 times with water onto the first layer. Transmittance 90.3%, surface resistance 1.31×10 7 A substrate with a resistance of Ω was obtained. The conductivity and transmittance after the second layer was formed were low.
[0081] Comparative Example 6 A first layer-forming aqueous solution for Comparative Example 6 was prepared by mixing 15 parts by mass of a 3% solids liquid (1% silica solids, 2% tin oxide solids) made by mixing Japan Nano Coat's silica binder (product name: B-30 (3% solids), a 10 nm tin oxide dispersion (4% solids) prepared by dispersing 10 nm tin oxide powder in water, and water, to which 20 parts by mass of Japan Nano Coat's CNF 0.2% aqueous dispersion (product name: SCNT 0.2% aqueous dispersion) and 10 parts by mass of Japan Nano Coat's graphene liquid 0.1% aqueous dispersion (product name: graphene 0.1% aqueous dispersion) were added, with the remainder being 55 parts by mass of water.
[0082] The glass substrate with the first layer obtained in the same manner as in Example 1 had a transmittance of 89.3% and a surface resistance of 1.86×10 7 Ω, and the transmittance and conductivity were low.
[0083] Comparative Example 7 A first layer-forming aqueous solution for Comparative Example 6 was prepared by mixing Japan Nano Coat's silica binder (product name: B-30 (3% solids)), Japan Nano Coat's tin oxide dispersion (product name: 4% tin oxide dispersion), and water to prepare a 3% solids solution (1.4% silica solids, 1.6% tin oxide solids). 20 parts by mass of Japan Nano Coat's CNF 0.2% aqueous dispersion (product name: SCNT 0.2% aqueous dispersion) was added to the mixture, with the remainder being 65 parts by mass of water.
[0084] The glass substrate with the first layer obtained in the same manner as in Example 1 had a transmittance of 90.3% and a surface resistance of 1.36×10 7 Ω, and the transmittance and conductivity were low.
[0085] Comparative Example 8 A 3% solids solution (1.4% silica solids, 1.6% tin oxide solids) made by mixing Japan Nano Coat's silica binder (product name: B-30 (3% solids), Japan Nano Coat's tin oxide dispersion (product name: 4% tin oxide dispersion), and water was prepared, to which 15 parts by mass of Japan Nano Coat's 0.1% aqueous graphene dispersion (product name: 0.1% aqueous graphene dispersion) was added, with the remainder being 75 parts by mass of water, to prepare an aqueous solution for forming a first layer of Comparative Example 7.
[0086] The glass substrate with the first layer obtained in the same manner as in Example 1 had a transmittance of 91.5% and a surface resistance of 3.21×10 8 Ω, and the conductivity was low.
[0087] Comparative Example 9 Japan Nano Coat's silica binder product name: B-30 (solid content 3%), Japan Nano Coat's tin oxide dispersion (product name: tin oxide 4% dispersion) and water were mixed to prepare a 3% solid content liquid (silica solid content 1.4%, tin oxide solid content 1.6%) 15 parts by mass of Japan Nano Coat's multi-CNF (multi-wall carbon nanofiber) 3% aqueous dispersion (product name: CNT 3% aqueous dispersion) was added, and 10 parts by mass of Japan Nano Coat's graphene liquid 0.1% aqueous dispersion (product name graphene 0.1% aqueous dispersion) was added, with the remaining part being 65 parts by mass of water to prepare a first layer forming aqueous solution of Comparative Example 9.
[0088] The glass substrate with the first layer obtained in the same manner as in Example 1 had a central film thickness of about 100 nm, a transmittance of 79.3%, and a surface resistance of 2.86×10 5 Ω, and the transmittance was low.
[0089] Next, AS-WR diluted 20 times with water was applied by dip coating on the first layer, resulting in a transmittance of 78.1% and a surface resistance of 1.56×10 9 A substrate with a resistance of Ω was obtained. Not only was the transmittance low, but the surface resistance increased significantly by applying a water-repellent coating to the surface in the same manner as in Example 1. This shows that the single nano carbon nanotube has excellent conductivity even when it is thin, and is therefore superior in terms of the conductivity of the substrate.
Claims
1. (A) a single-walled carbon nanotube, a graphene nanoparticle, a single silica nanoparticle, and a single tin oxide nanoparticle; a first layer including 40 to 60 parts by mass of silica single nanoparticles having a size of 5 nm or less as measured by a transmission electron microscope, and 60 to 40 parts by mass of tin oxide single nanoparticles having a size of 2 nm or less as measured by a transmission electron microscope, relative to a total of 100 parts by mass of silica single nanoparticles and tin oxide single nanoparticles; (B) a second layer including a water repellent and a conductive material; A conductive leather or a conductive fiber, characterized in that a first layer and a second layer are provided in this order from the surface of the conductive leather or the conductive fiber.
2. The surface sheet resistance is 9.9×10 6 The conductive leather or conductive fiber according to claim 1, having a resistance of Ω / □ or less.
3. A process for leather or textile surfaces, comprising the steps of: (A) a single-walled carbon nanotube, a graphene nanoparticle, a single silica nanoparticle, a single tin oxide nanoparticle, and water; a step of forming a first layer by applying or immersing a surface in a first layer forming dispersion liquid containing 40 to 60 parts by mass of single silica nanoparticles of 5 nm or less as measured by a transmission electron microscope and 60 to 40 parts by mass of single tin oxide nanoparticles of 2 nm or less as measured by a transmission electron microscope, relative to a total of 100 parts by mass of single silica nanoparticles and single tin oxide nanoparticles; (B) A step of applying an aqueous solution for forming a second layer, which contains a water repellent, a conductive material, and water, to the surface or immersing the surface in the aqueous solution to form a second layer. A method for producing conductive leather or conductive fiber, comprising the steps of:
4. 4. The method for producing conductive leather or conductive fiber according to claim 3, wherein in step (A), the surface is coated or immersed in the dispersion for forming a transparent conductive thin film, and then the surface is rolled.
Citation Information
Patent Citations
Coating composition and textile material
JP1992255767A
Materials used with capacitive touchscreens
JP2012529127A
Glove
JP2017160582A
Antistatic antibacterial film material
JP2019064078A
Dispersion liquid for formation of transparent conductive thin film and substrate equipped with transparent conductive thin film
WO2014115792A1