Ruthenium compound, raw material for forming thin film and method for producing thin film

A ruthenium compound with specific ligand structures addresses the limitations of conventional compounds by providing low melting points, high vapor pressures, and thermal stability, enhancing the quality and productivity of thin films in CVD and ALD methods.

JP7565270B2Active Publication Date: 2024-10-10ADEKA CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2021528132
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-06-21
Filing Date
2020-06-10
Publication Date
2024-10-10
Estimated Expiration
2040-06-10

AI Technical Summary

Technical Problem

Conventional ruthenium compounds used in thin film formation methods have low melting points, high vapor pressures, and are not thermally stable, leading to low-quality thin films with poor productivity.

Method used

A ruthenium compound with a specific ligand structure, represented by general formulas (1) and (2), offering low melting points, high vapor pressures, and high thermal stability, suitable for CVD and ALD methods.

Benefits of technology

The new ruthenium compound enables the production of high-quality thin films with improved productivity and stability, particularly in ALD methods, resulting in superior thin film properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000021_0000
    Figure 00000021_0000
  • Figure 00000021_0001
    Figure 00000021_0001
  • Figure 00000021_0002
    Figure 00000021_0002
Patent Text Reader

Abstract

The present invention provides a ruthenium compound represented by general formula (1) or (2), a raw material for thin film formation containing the same, and a method for producing a thin film using the raw material for thin film formation. Formula (1) (In the formula, R1-R12 each independently represent a hydrogen atom, a C1-5 alkyl group, or a fluorine atom, and n represents an integer of 0-2. However, at least one of R1-R12 is a fluorine atom-containing group.) Formula (2) (In the formula, R13-R17 each independently represent a hydrogen atom or a C1-5 alkyl group, and the total number of carbon atoms in R13-R17 is 3 or more.)
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a novel ruthenium compound, a thin film-forming material containing said compound, and a method for producing a thin film using said thin film-forming material. [Background technology]

[0002] Thin film forming materials containing ruthenium exhibit unique electrical properties and are used in a wide variety of technologies, such as in electrode materials for memory elements such as DRAM elements, resistive films, diamagnetic films used in the recording layers of hard disks, and catalyst materials for polymer electrolyte fuel cells.

[0003] Examples of methods for manufacturing the above-mentioned thin films include sputtering, ion plating, MOD methods such as coating pyrolysis and sol-gel methods, chemical vapor deposition, etc. Among these, chemical vapor deposition (hereinafter sometimes simply referred to as "CVD") methods including ALD (Atomic Layer Deposition) are the most suitable manufacturing process because they have many advantages such as excellent composition controllability and step coverage, suitability for mass production, and the possibility of hybrid integration.

[0004] A large number of different raw materials have been reported as ruthenium atom sources used in chemical vapor deposition. For example, Patent Document 1 discloses bis(1-ethylpentadienyl)ruthenium as a material that can be suitably used as a raw material for forming a thin film. Patent Document 2 discloses bis(2,4-dimethyl-1,3-pentadienyl)ruthenium, and Patent Document 3 discloses a ruthenium compound in which a cyclohexadienyl group and a pentadienyl group are coordinated. Patent Document 4 discloses bis(fluorocyclopentadienyl)ruthenium and bis(trifluoromethylcyclopentadienyl)ruthenium as ruthenium compounds containing fluorine atoms. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2008-069453 A [Patent Document 2] Special Publication No. 2011-521983 [Patent Document 3] JP 2016-074929 A [Patent Document 4] JP 2005-060814 A Summary of the Invention [Problem to be solved by the invention]

[0006] In a method for forming a thin film by vaporizing a compound, such as a CVD method, the compound (precursor) used as a raw material is required to have a low melting point so that it can be transported in a liquid state, a high vapor pressure so that it can be easily vaporized, high thermal stability, and high productivity for forming a high-quality thin film. However, there has been no conventional ruthenium compound that is fully satisfactory in these respects.

[0007] Therefore, an object of the present invention is to provide a novel ruthenium compound which has a low melting point, a high vapor pressure, and high thermal stability and which enables the production of high quality thin films with higher productivity than conventional ruthenium compounds; a thin film-forming raw material containing the compound; and a thin film manufacturing method for forming a thin film containing ruthenium atoms using the raw material. [Means for solving the problem]

[0008] As a result of extensive investigations, the present inventors discovered that a ruthenium compound having a ligand with a specific structure can solve the above problems, and thus arrived at the present invention.

[0009] That is, the present invention provides a ruthenium compound represented by the following general formula (1) or (2) and a thin film-forming material containing the same.

[0010] [ka]

[0011] (In the formula, R 1 ~R 12 each independently represents a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, or a fluorine atom-containing group, and n represents an integer of 0 to 2. 1 ~R 12 At least one of the groups is a fluorine atom-containing group.

[0012] [ka]

[0013] (In the formula, R 13 ~R 17 each independently represents a hydrogen atom or an alkyl group having 1 to 5 carbon atoms; R 13 ~R 17 The total number of carbon atoms is 3 or more.)

[0014] The present invention also provides a method for producing a thin film, comprising the steps of: vaporizing a thin film-forming raw material containing a ruthenium compound represented by the above general formula (1) or (2); introducing the vapor containing the ruthenium compound obtained in the above step into a film-forming chamber in which a substrate is placed; and decomposing and / or chemically reacting the ruthenium compound to form a thin film containing ruthenium atoms on the surface of the substrate. Effect of the Invention

[0015] The present invention provides a ruthenium compound having a low melting point, a high vapor pressure, and high thermal stability, which is suitable as a thin film forming material for the CVD method, and in particular, has an ALD window and can be suitably used as a thin film forming material for the ALD method. [Brief description of the drawings]

[0016] [Figure 1]FIG. 1 is a schematic diagram showing an example of a chemical vapor deposition apparatus used in the thin film manufacturing method according to the present invention. [Diagram 2] FIG. 2 is a schematic diagram showing another example of a chemical vapor deposition apparatus used in the thin film manufacturing method according to the present invention. [Diagram 3] FIG. 3 is a schematic diagram showing yet another example of a chemical vapor deposition apparatus used in the thin film manufacturing method according to the present invention. [Figure 4] FIG. 4 is a schematic diagram showing yet another example of a chemical vapor deposition apparatus used in the thin film manufacturing method according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] The ruthenium compound of the present invention is represented by the above general formula (1) or (2) and is suitable as a thin film forming raw material used in a thin film production method having a vaporization step such as a CVD method, and can also form a thin film using an ALD method.

[0018] In the above general formula (1) of the present invention, R 1 ~R 12 each independently represents a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, or a fluorine atom-containing group, and n represents an integer of 0 to 2. 1 ~R 12 At least one of the groups is a fluorine atom-containing group. n is preferably 0 or 2, and more preferably 2.

[0019] Above R 1 ~R 12 Examples of the alkyl group having 1 to 5 carbon atoms represented by the formula (I) include a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, a pentyl group, an isopentyl group, and a neopentyl group.

[0020] Examples of the fluorine atom-containing group include a fluoro group, a monofluoromethyl group, a difluoromethyl group, a trifluoromethyl group, and a trifluoroethyl group. Furthermore, when the fluorine atom-containing group contains a carbon atom, it is preferably a fluoroalkyl group having 1 to 3 carbon atoms, more preferably a fluoroalkyl group having 1 to 2 carbon atoms, and even more preferably a fluoroalkyl group having 1 carbon atom.

[0021] In the above general formula (1), R 1 ~R 12 is appropriately selected depending on the thin film manufacturing method to be applied. When used in a thin film manufacturing method having a step of vaporizing a compound, R is selected so as to obtain a compound with a high vapor pressure, a low melting point, and high thermal stability. 1 ~R 12 It is preferable to select

[0022] Specifically, the vapor pressure of the compound increases, so R 1 ~R 12 are each preferably independently selected from a hydrogen atom, an alkyl group having 1 to 3 carbon atoms, or a fluorine atom-containing group. As the alkyl group having 1 to 3 carbon atoms, a methyl group or an ethyl group is preferred, and a methyl group is more preferred. As the fluorine atom-containing group, a fluorine atom, a monofluoromethyl group, a difluoromethyl group, or a trifluoromethyl group is preferred, and a trifluoromethyl group is more preferred. Similarly, since the vapor pressure of the compound increases, R 1 ~R 12 On the other hand, from the viewpoint of thermal stability, R 1 ~R 12 It is preferable that R contains at least one alkyl group having 1 to 5 carbon atoms. 1 ~R 12 It is more preferable that the alkyl group contains 1 to 3 alkyl groups having 1 to 5 carbon atoms. In addition, in the case of the thin film manufacturing method using the MOD method, which does not involve a vaporization process, R 1 ~R 12 can be arbitrarily selected depending on the solubility in the solvent used, the thin film forming reaction, and the like.

[0023] Also, when n is 2, R 1 ~R 5Preferably, contains one or two methyl or ethyl groups, and more preferably contains one or two methyl groups. Also, when n is 2, R 1 ~R 5 It is preferable that the alkyl group contains one or two fluorine atom-containing groups, and it is more preferable that the alkyl group contains one or two trifluoromethyl groups.

[0024] More specifically, when n is 2, R 1 ~R 5 Preferably, R contains one methyl or ethyl group, one trifluoromethyl group, and three hydrogen atoms, and more preferably contains one methyl group, one trifluoromethyl group, and three hydrogen atoms. In this case, R 1 or R 2 is a methyl group, R 4 or R 5 is preferably a trifluoromethyl group, and R 2 is a methyl group, and R 4 is a trifluoromethyl group, and R 1 , R 3 and R 5 It is more preferable that is a hydrogen atom.

[0025] Preferable specific examples of the ruthenium compound represented by the general formula (1) include the following compounds No. 1 to No. 96. In the following compounds No. 1 to No. 96, "Me" represents a methyl group, "Et" represents an ethyl group, "iPr" represents an isopropyl group, and "tBu" represents a tert-butyl group.

[0026] [ka]

[0027] [ka]

[0028] [ka]

[0029] [ka]

[0030] The method for producing the compound represented by the above general formula (1) is not particularly limited, and the compound is produced by applying a well-known reaction. For example, the production method includes reacting dichlorodi-μ-chlorobis[(1,2,3,6,7,8-η-2,7-alkyl-2,6-octadiene] with dichlorodi-μ-chlorobis[(1,2,3,6,7,8-η-2,7-alkyl-2,6-octadiene] in an alcohol solvent. ) [-1,8-diyl]diruthenium(IV), lithium carbonate, acetonitrile, and a fluorine-based diene compound of the corresponding structure are reacted, and the solvent is removed to obtain an intermediate. Dichloromethane is added to the obtained intermediate, and the mixture is filtered. The solvent is removed from the filtrate, and then the mixture is purified by distillation to obtain the product.

[0031] Examples of the fluorine-based diene compound include 1-fluoropenta-1,3-diene, 2-fluoropenta-1,3-diene, 3-fluoropenta-1,3-diene, 2,4-difluoropenta-1,3-diene, 1,5-difluoropenta-1,3-diene, 1,2-difluoropenta-1,3-diene, 1,2,4,5-tetrafluoropenta-1,3-diene, 1,2,3,4,5-pentafluoropenta-1,3-diene, 1-fluorohexa-2 ,4-diene, 1-fluorohepta-2,4-diene, 4-fluoro-2-methylpenta-1,3-diene, 2-fluoro-4-methylenehexa-2-ene, 1,5-difluoro-2,4-dimethylpenta-1,3-diene, 3,5-difluorohepta-2,4-diene, 6,6,6-trifluorohexa-1,3-diene, 5,5,5-trifluoro-4-methylpenta-1,3-diene, 3-(trifluoromethyl)penta-1,3-diene, 5,5,5-trifluoro-4-methyl-2-(trifluoromethyl)penta-1,3-diene, 1,1,1,7,7,7-hexafluoropenta-2,4-diene, 6,6,6-trifluoro-4-(trifluoromethyl)hexa-1,3-diene, 1,1,1,7,7,7-hexafluoro-3,5-bis(trifluoromethyl)hepta-2,4-diene, 1,1,1,7,7,7-hexafluoro-3,4,5-tris(trifluoromethyl) )hepta-2,4-diene, 7,7,7-trifluorohepta-2,4-diene, 1,1,1-trifluoroocta-3,5-diene, 4-methyl-2-(trifluoromethyl)penta-1,3-diene, 1,1,1-trifluoro-2-methyl-4-methylhexa-2-ene, 1,1,1,7,7,7-hexafluoro-3,5-dimethylhepta-2,4-diene, 3,5-bis(trifluoromethyl)hepta-2,4-diene, etc. Also, dichlorodi-μ-chlorobis[(1,2,3,6,7,8-η-2,7-alkyl-2,6-octadiene] ) The fluorine-based diene compound is added in an amount of 5 to 10 moles per mole of [-1,8-diyl]diruthenium (IV).

[0032] In the above general formula (2) of the present invention, R 13 ~R17 each independently represents a hydrogen atom or an alkyl group having 1 to 5 carbon atoms; R 13 ~R 17 The total number of carbon atoms in R is 3 or more. 13 ~R 17 The total number of carbon atoms is preferably 10 or less, more preferably 6 or less, and even more preferably 4 or less.

[0033] Above R 13 ~R 17 Examples of the alkyl group having 1 to 5 carbon atoms represented by the formula (I) include a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, a pentyl group, an isopentyl group, and a neopentyl group.

[0034] In the above general formula (2), R 13 ~R 17 is appropriately selected depending on the thin film manufacturing method to be applied. When used in a thin film manufacturing method having a step of vaporizing a compound, R is selected so as to obtain a compound with a high vapor pressure, a low melting point, and high thermal stability. 13 ~R 17 It is preferable to select

[0035] Specifically, the vapor pressure of the compound increases, so R 13 ~R 17 are each independently selected from a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, and R 13 ~R 17 is more preferably selected from a hydrogen atom, a methyl group, or an ethyl group, and even more preferably a methyl group. In addition, since the vapor pressure of the compound increases, R 13 ~R 17 The total number of carbon atoms in R is preferably 3 to 10. 13 ~R 17 More preferably, the total number of carbon atoms in R is 3 to 6. 13 ~R 17 More preferably, the total number of carbon atoms in R is 3 to 4. 13 ~R 17It is even more preferable that the total number of carbon atoms in R is 3. Since the melting point of the compound is lowered, 13 and R 17 are different groups and / or R 14 and R 16 are preferably different groups. On the other hand, from the viewpoint of the thermal stability of the compound, R 13 ~R 17 It is preferable that the alkyl group contains three or more alkyl groups having 1 to 5 carbon atoms. In addition, in the case of the thin film manufacturing method using the MOD method, which does not involve a vaporization process, R 13 ~R 17 can be arbitrarily selected depending on the solubility in the solvent used, the thin film forming reaction, and the like.

[0036] As an embodiment of the ruthenium compound represented by the general formula (2), R 13 ~R 17 If the total number of carbon atoms in is 3, R 13 ~R 17 Preferably, R contains three methyl groups. 14 , R 16 and R 17 is preferably a methyl group.

[0037] Preferable specific examples of the ruthenium compound represented by the general formula (2) include the following compounds No. 97 to No. 117. In the following compounds No. 97 to No. 117, "Me" represents a methyl group, "Et" represents an ethyl group, "iPr" represents an isopropyl group, and "tBu" represents a tert-butyl group.

[0038] [ka]

[0039] The method for producing the compound represented by the above general formula (2) is not particularly limited, and the compound is produced by applying a well-known reaction. For example, the production method includes reacting dichlorodi-μ-chlorobis[(1,2,3,6,7,8-η-2,7-alkyl-2,6-octadiene] with dichlorodi-μ-chlorobis[(1,2,3,6,7,8-η-2,7-alkyl-2,6-octadiene] in an alcohol solvent.) [-1,8-diyl]diruthenium(IV), lithium carbonate, acetonitrile, and a diene compound of the corresponding structure are reacted, and the solvent is removed to obtain an intermediate. Dichloromethane is added to the resulting intermediate, and the mixture is filtered. The solvent is removed from the filtrate, and then the mixture is purified by distillation to obtain the product.

[0040] Examples of the diene compound include 2-methyl-4-methylenehex-2-ene and 2,4-dimethylhexa-1,3-diene. Also, dichlorodi-μ-chlorobis[(1,2,3,6,7,8-η-2,7-alkyl-2,6-octadiene] ) The fluorine-based diene compound is added in an amount of 5 to 10 moles per mole of [-1,8-diyl]diruthenium (IV).

[0041] Next, the thin film forming raw material of the present invention contains the ruthenium compound of the present invention described above as a precursor of the thin film. The form of the thin film forming raw material varies depending on the manufacturing process to which the thin film forming raw material is applied. For example, when manufacturing a thin film containing only ruthenium as a metal, the thin film forming raw material of the present invention does not contain metal compounds and metalloid compounds other than the ruthenium compound of the present invention. On the other hand, when manufacturing a thin film containing two or more types of metals and / or metalloids, the thin film forming raw material of the present invention can also contain a compound containing a desired metal and / or a compound containing a metalloid (hereinafter, sometimes referred to as "other precursors") in addition to the ruthenium compound of the present invention. The thin film forming raw material of the present invention may further contain an organic solvent and / or a nucleophilic reagent, as described below. As described above, the thin film forming raw material of the present invention is particularly useful as a raw material for chemical vapor deposition (hereinafter, sometimes referred to as "raw material for CVD"), since the physical properties of the ruthenium compound of the present invention, which is a precursor, are suitable for the CVD method and the ALD method.

[0042] When the thin film forming material of the present invention is a material for chemical vapor deposition, its form is appropriately selected depending on the method of transportation and supply in the CVD method to be used.

[0043] The above-mentioned transport supply method includes a gas transport method in which the CVD raw material is heated and / or depressurized in a container (hereinafter sometimes referred to as a "raw material container") in which the raw material is stored, thereby vaporizing the raw material into a vapor, and the vapor is introduced into a film formation chamber (hereinafter sometimes referred to as a "deposition reaction section") in which a substrate is placed together with a carrier gas such as argon, nitrogen, or helium used as necessary; and a liquid transport method in which the CVD raw material is transported in a liquid or solution state to a vaporization chamber, heated and / or depressurized in the vaporization chamber to vaporize the raw material into a vapor, and the vapor is introduced into a film formation chamber. In the case of the gas transport method, the ruthenium compound represented by the above general formula (1) or (2) itself can be used as the CVD raw material. In the case of the liquid transport method, the ruthenium compound represented by the above general formula (1) or (2) itself or a solution in which the compound is dissolved in an organic solvent can be used as the CVD raw material. These CVD raw materials may further contain other precursors, nucleophilic reagents, etc.

[0044] In addition, in the multi-component CVD method, there are a method in which each component of the CVD raw material is vaporized and supplied independently (hereinafter, sometimes referred to as the "single source method"), and a method in which a mixed raw material in which multi-component raw materials are mixed in advance with a desired composition is vaporized and supplied (hereinafter, sometimes referred to as the "cocktail source method"). In the case of the cocktail source method, a mixture of the ruthenium compound of the present invention and other precursors, or a mixed solution in which the mixture is dissolved in an organic solvent, can be used as the CVD raw material. This mixture or mixed solution may further contain a nucleophilic reagent, etc.

[0045] The organic solvent is not particularly limited, and any well-known organic solvent can be used. Examples of the organic solvent include acetates such as ethyl acetate, butyl acetate, and methoxyethyl acetate; ethers such as tetrahydrofuran, tetrahydropyran, ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, dibutyl ether, and dioxane; ketones such as methyl butyl ketone, methyl isobutyl ketone, ethyl butyl ketone, dipropyl ketone, diisobutyl ketone, methyl amyl ketone, cyclohexanone, and methylcyclohexanone; hexane, cyclohexane, methylcyclohexanone, and methylcyclohexanone; and methylcyclohexanone. Examples of suitable solvents include hydrocarbons such as hexane, dimethylcyclohexane, ethylcyclohexane, heptane, octane, toluene, and xylene; hydrocarbons having a cyano group such as 1-cyanopropane, 1-cyanobutane, 1-cyanohexane, cyanocyclohexane, cyanobenzene, 1,3-dicyanopropane, 1,4-dicyanobutane, 1,6-dicyanohexane, 1,4-dicyanocyclohexane, and 1,4-dicyanobenzene; and pyridine and lutidine. These are used alone or as a mixture of two or more solvents depending on the solubility of the solute, the relationship between the use temperature and the boiling point and the flash point, etc. The CVD raw material (solution state) obtained by dissolving the precursor in the above organic solvent usually contains the entire precursor in an amount of 0.01 to 2.0 mol / L, and preferably contains the entire precursor in an amount of 0.05 to 1.0 mol / L. The total amount of precursors means the amount of the ruthenium compound of the present invention when the thin film forming raw material of the present invention does not contain any metal compound or metalloid compound other than the ruthenium compound of the present invention, and means the total amount of the ruthenium compound of the present invention and other precursors when the thin film forming raw material of the present invention contains, in addition to the ruthenium compound, a compound containing another metal and / or a compound containing a metalloid.

[0046] In the case of a multi-component CVD method, other precursors used together with the ruthenium compound of the present invention are not particularly limited, and any well-known precursors used as CVD materials can be used.

[0047] Examples of the other precursors include compounds of silicon or metal with one or more selected from the group consisting of compounds used as organic ligands such as alcohol compounds, glycol compounds, β-diketone compounds, cyclopentadiene compounds, and organic amine compounds. Examples of the metal species of the precursor include lithium, sodium, potassium, magnesium, calcium, strontium, barium, titanium, zirconium, hafnium, vanadium, tantalum, chromium, molybdenum, tungsten, manganese, iron, cobalt, rhodium, iridium, nickel, palladium, platinum, copper, silver, gold, zinc, aluminum, gallium, indium, germanium, tin, lead, antimony, bismuth, yttrium, lanthanum, cerium, praseodymium, neodymium, promethium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium, and lutetium.

[0048] Examples of the alcohol compounds that can be used as organic ligands for the other precursors include alkyl alcohols such as methanol, ethanol, propanol, isopropyl alcohol, butanol, sec-butyl alcohol, isobutyl alcohol, tert-butyl alcohol, pentyl alcohol, isopentyl alcohol, and tert-pentyl alcohol; 2-methoxyethanol, 2-ethoxyethanol, 2-butoxyethanol, 2-(2-methoxyethoxy)ethanol, 2-methoxy-1-methylethanol, 2-methoxy-1,1-dimethylethanol, 2-ethoxy-1,1-dimethylethanol, 2-isopropoxy-1,1-dimethylethanol, 2-butoxyethanol, and 2-isopropoxy-1,1-dimethylethanol. ether alcohols such as 2-(2-methoxyethoxy)-1,1-dimethylethanol, 2-propoxy-1,1-diethylethanol, 2-s-butoxy-1,1-diethylethanol, and 3-methoxy-1,1-dimethylpropanol; and dialkylamino alcohols such as dimethylaminoethanol, ethylmethylaminoethanol, diethylaminoethanol, dimethylamino-2-pentanol, ethylmethylamino-2-pentanol, dimethylamino-2-methyl-2-pentanol, ethylmethylamino-2-methyl-2-pentanol, and diethylamino-2-methyl-2-pentanol.

[0049] Examples of glycol compounds that can be used as organic ligands for the other precursors include 1,2-ethanediol, 1,2-propanediol, 1,3-propanediol, 2,4-hexanediol, 2,2-dimethyl-1,3-propanediol, 2,2-diethyl-1,3-propanediol, 1,3-butanediol, 2,4-butanediol, 2,2-diethyl-1,3-butanediol, 2-ethyl-2-butyl-1,3-propanediol, 2,4-pentanediol, 2-methyl-1,3-propanediol, 2-methyl-2,4-pentanediol, 2,4-hexanediol, and 2,4-dimethyl-2,4-pentanediol.

[0050] In addition, examples of β-diketone compounds include acetylacetone, hexane-2,4-dione, 5-methylhexane-2,4-dione, heptane-2,4-dione, 2-methylheptane-3,5-dione, 5-methylheptane-2,4-dione, 6-methylheptane-2,4-dione, 2,2-dimethylheptane-3,5-dione, 2,6-dimethylheptane-3,5-dione, 2,2,6-trimethylheptane-3,5-dione, 2,2,6,6-tetramethylheptane-3,5-dione, octane-2,4-dione, 2,2,6-trimethyloctane-3,5-dione, 2,6-dimethyloctane-3,5-dione, 2,9-dimethylnonane-4,6-dione, and 2-methyl-6-ethyldecane-3,5-dione. 1,1,1-trifluoropentane-2,4-dione, 1,1,1-trifluoro-5,5-dimethylhexane-2,4-dione, 1,1,1,5,5,5-hexafluoropentane-2,4-dione, 1,3-diperfluorohexylpropane-1,3-dione, and other fluorine-substituted alkyl β-diketones; 1,1,5,5-tetramethyl-1-methoxyhexane-2,4-dione, 2,2,6,6-tetramethyl-1-methoxyheptane-3,5-dione, 2,2,6,6-tetramethyl-1-(2-methoxyethoxy)heptane-3,5-dione, and other ether-substituted β-diketones.

[0051] Examples of the cyclopentadiene compound include cyclopentadiene, methylcyclopentadiene, ethylcyclopentadiene, propylcyclopentadiene, isopropylcyclopentadiene, butylcyclopentadiene, sec-butylcyclopentadiene, isobutylcyclopentadiene, tert-butylcyclopentadiene, dimethylcyclopentadiene, and tetramethylcyclopentadiene. Examples of the organic amine compound used as the organic ligand include methylamine, ethylamine, propylamine, isopropylamine, butylamine, sec-butylamine, tert-butylamine, isobutylamine, dimethylamine, diethylamine, dipropylamine, diisopropylamine, ethylmethylamine, propylmethylamine, and isopropylmethylamine.

[0052] The above other precursors are known in the art, and their manufacturing methods are also known. As an example of the manufacturing method, when an alcohol compound is used as the organic ligand, the precursor can be manufactured by reacting the inorganic salt of the metal or its hydrate described above with an alkali metal alkoxide of the alcohol compound. Here, examples of the inorganic salt of the metal or its hydrate include metal halides and nitrates, and examples of the alkali metal alkoxide include sodium alkoxide, lithium alkoxide, potassium alkoxide, and the like.

[0053] As the other precursor, in the case of the single source method, it is preferable to use a compound whose thermal decomposition and / or oxidative decomposition behavior is similar to that of the ruthenium compound of the present invention, and in the case of the cocktail source method, it is preferable to use a compound that not only has similar thermal decomposition and / or oxidative decomposition behavior, but also does not undergo changes that impair the desired properties as a precursor due to chemical reactions, etc. during mixing.

[0054] Furthermore, the thin film forming material of the present invention may contain a nucleophilic reagent, if necessary, to provide stability to the ruthenium compound of the present invention and other precursors. Examples of the nucleophilic reagent include ethylene glycol ethers such as glyme, diglyme, triglyme, and tetraglyme, crown ethers such as 18-crown-6, dicyclohexyl-18-crown-6, 24-crown-8, dicyclohexyl-24-crown-8, and dibenzo-24-crown-8, polyamines such as ethylenediamine, N,N'-tetramethylethylenediamine, diethylenetriamine, triethylenetetramine, tetraethylenepentamine, pentaethylenehexamine, 1,1,4,7,7-pentamethyldiethylenetriamine, 1,1,4,7,10,10-hexamethyltriethylenetetramine, and triethoxytriethyleneamine, cyclam, cyclen, etc. heterocyclic compounds such as pyridine, pyrrolidine, piperidine, morpholine, N-methylpyrrolidine, N-methylpiperidine, N-methylmorpholine, tetrahydrofuran, tetrahydropyran, 1,4-dioxane, oxazole, thiazole, and oxathiolane; β-ketoesters such as methyl acetoacetate, ethyl acetoacetate, and 2-methoxyethyl acetoacetate; and β-diketones such as acetylacetone, 2,4-hexanedione, 2,4-heptanedione, 3,5-heptanedione, and dipivaloylmethane. The amount of these nucleophilic reagents used is preferably 0.1 mol to 10 mol, and more preferably 1 to 4 mol, relative to 1 mol of the total amount of the precursor.

[0055] The thin film forming material of the present invention is made to contain as little impurity metal elements, impurity halogens such as impurity chlorine, and impurity organic matter as possible, other than the components constituting the thin film. The impurity metal elements are preferably 100 ppb or less per element, more preferably 10 ppb or less, and the total amount is preferably 1 ppm or less, more preferably 100 ppb or less. In particular, when used as a gate insulating film, gate film, or barrier layer of an LSI, it is necessary to reduce the content of alkali metal elements and alkaline earth metal elements that affect the electrical properties of the resulting thin film. The impurity halogens are preferably 100 ppm or less, more preferably 10 ppm or less, and most preferably 1 ppm or less. The impurity organic matter is preferably 500 ppm or less in total, more preferably 50 ppm or less, and most preferably 10 ppm or less. In addition, moisture is a cause of particle generation in the chemical vapor deposition material and particle generation during thin film formation, so it is preferable to remove moisture as much as possible from the precursor, organic solvent, and nucleophilic reagent before use. The moisture content of each of the precursor, the organic solvent and the nucleophilic reagent is preferably 10 ppm or less, and more preferably 1 ppm or less.

[0056] In addition, the thin film forming material of the present invention is preferably free of particles as much as possible in order to reduce or prevent particle contamination of the thin film to be formed. Specifically, in particle measurement in the liquid phase using a light scattering type liquid-borne particle detector, the number of particles larger than 0.3 μm is preferably 100 or less per 1 mL of liquid phase, more preferably the number of particles larger than 0.2 μm is 1000 or less per 1 mL of liquid phase, and most preferably the number of particles larger than 0.2 μm is 100 or less per 1 mL of liquid phase.

[0057] The method for producing a thin film of the present invention using the thin film-forming raw material of the present invention is a CVD method in which the vapor obtained by vaporizing the thin film-forming raw material of the present invention and a reactive gas used as necessary are introduced into a film-forming chamber (treatment atmosphere) in which a substrate is placed, and then the precursor is decomposed and / or chemically reacted on the substrate to grow and deposit a thin film containing a metal on the substrate surface. There are no particular limitations on the method for transporting and supplying the raw material, the deposition method, the production conditions, the production equipment, etc., and well-known general conditions and methods can be used.

[0058] Examples of the reactive gases used as necessary as above include oxygen, ozone, nitrogen dioxide, nitrogen monoxide, water vapor, hydrogen peroxide, formic acid, acetic acid, acetic anhydride, etc. as oxidizing gases, and hydrocarbon compounds such as methane and ethane, hydrogen, carbon monoxide, organometallic compounds, etc. as reducing gases, and examples of the gases for producing nitrides include organic amine compounds such as monoalkylamines, dialkylamines, trialkylamines, and alkylenediamines, hydrazine, ammonia, etc., and these can be used alone or in combination. Among these, the thin film forming material of the present invention has good reactivity with reducing gases, and is particularly good in reactivity with hydrogen. Therefore, when one type is used as the reactive gas, it is preferable to use hydrogen, and when a mixed gas of two or more types is used as the reactive gas, it is preferable to include at least hydrogen.

[0059] The above-mentioned transport supply method may include the gas transport method, liquid transport method, single source method, cocktail source method, etc.

[0060] In addition, examples of the above deposition method include thermal CVD, which deposits a thin film by reacting a source gas or a source gas and a reactive gas using only heat, plasma CVD, which uses heat and plasma, photo-CVD, which uses heat and light, photo-plasma CVD, which uses heat, light, and plasma, and ALD, which divides the CVD deposition reaction into elementary processes and deposits in stages at the molecular level.

[0061] Examples of the material of the substrate include silicon, ceramics such as silicon nitride, titanium nitride, tantalum nitride, titanium oxide, titanium nitride, ruthenium oxide, zirconium oxide, hafnium oxide, and lanthanum oxide, glass, and metals such as metal cobalt. Examples of the shape of the substrate include plate-like, spherical, fibrous, and scaly shapes. The surface of the substrate may be flat or may have a three-dimensional structure such as a trench structure.

[0062] The above-mentioned production conditions include reaction temperature (substrate temperature), reaction pressure, deposition rate, etc. The reaction temperature is preferably 100° C. or higher, at which the compound of the present invention reacts sufficiently, more preferably 150° C. to 400° C., and particularly preferably 200° C. to 350° C. The reaction pressure is preferably 10 Pa to atmospheric pressure in the case of thermal CVD or photo-CVD, and is preferably 10 Pa to 2000 Pa in the case of using plasma. The deposition rate can be controlled by the supply conditions of the raw material (vaporization temperature, vaporization pressure), the reaction temperature, and the reaction pressure. If the deposition rate is high, the properties of the obtained thin film may deteriorate, and if it is low, problems may occur in productivity, so that the deposition rate is preferably 0.01 nm / min to 100 nm / min, and more preferably 1 nm / min to 50 nm / min. In the case of the ALD method, the deposition rate is controlled by the number of cycles so as to obtain a desired film thickness.

[0063] Further examples of the above manufacturing conditions include the temperature and pressure when the thin film forming raw material is vaporized to form vapor. The step of vaporizing the thin film forming raw material to form vapor may be performed in a raw material container or in a vaporization chamber. In either case, the thin film forming raw material of the present invention is preferably evaporated at 0°C to 150°C. In addition, when the thin film forming raw material is vaporized to form vapor in a raw material container or in a vaporization chamber, the pressure in the raw material container and the pressure in the vaporization chamber are both preferably 1 Pa to 10,000 Pa.

[0064] The method for producing a thin film of the present invention employs an ALD method, and may include a raw material introduction step of vaporizing a thin film-forming raw material to form vapor by the above-mentioned transport and supply method and introducing the vapor into a film formation chamber, as well as a precursor thin film formation step of forming a precursor thin film on the surface of the substrate using the above-mentioned compound in the vapor, an exhaust step of exhausting unreacted compound gas, and a metal-containing thin film formation step of chemically reacting the precursor thin film with a reactive gas to form a thin film containing a metal on the surface of the substrate.

[0065] Each step of the ALD method is described below in detail using the case of forming a metal thin film as an example. First, the above-mentioned raw material introduction step is performed. The preferred temperature and pressure when the raw material for forming the thin film is vaporized are the same as those described in the thin film manufacturing method by the CVD method. Next, the vapor introduced into the film formation chamber comes into contact with the surface of the substrate to form a precursor thin film on the substrate surface (precursor thin film formation step). At this time, the substrate or the film formation chamber may be heated to apply heat. The precursor thin film formed in this step is a thin film formed from the compound of the present invention, or a thin film formed by decomposition and / or reaction of a part of the compound of the present invention, and has a different composition from the target metal nitride thin film. The substrate temperature when this step is performed is preferably room temperature to 500°C, more preferably 150°C to 350°C. The pressure of the system (inside the film formation chamber) when this step is performed is preferably 1 Pa to 10,000 Pa, more preferably 10 Pa to 1000 Pa.

[0066] Next, unreacted compound gases and by-produced gases are exhausted from the deposition chamber (exhaust process). Ideally, unreacted compound gases and by-produced gases are completely exhausted from the deposition chamber, but it is not necessary to exhaust them completely. Exhaust methods include a method of purging the system with an inert gas such as nitrogen, helium, or argon, a method of exhausting by reducing the pressure inside the system, and a combination of these methods. When reducing the pressure, the degree of reduction is preferably 0.01 Pa to 300 Pa, and more preferably 0.01 Pa to 100 Pa.

[0067] Next, a reducing gas is introduced into the film-forming chamber as a reactive gas, and a metal thin film is formed from the precursor thin film obtained in the previous precursor thin film forming step by the action of the reducing gas or the action of the reducing gas and heat (metal-containing thin film forming step). The temperature when applying heat in this step is preferably room temperature to 500°C, more preferably 150 to 350°C. The pressure of the system (inside the film-forming chamber) when this step is performed is preferably 1 Pa to 10,000 Pa, more preferably 10 Pa to 1,000 Pa. The compound of the present invention has good reactivity with a reducing gas, so that a high-quality metal thin film with a low residual carbon content can be obtained.

[0068] In the thin film manufacturing method of the present invention, when the ALD method is adopted as described above, thin film deposition by a series of operations consisting of the raw material introduction step, precursor thin film formation step, exhaust step, and metal-containing thin film formation step is regarded as one cycle, and this cycle may be repeated several times until a thin film of a required thickness is obtained. In this case, after one cycle, it is preferable to exhaust unreacted compound gas, reactive gas, and by-product gas from the deposition reaction section in the same manner as in the exhaust step, and then perform the next cycle.

[0069] In addition, in forming a metal thin film by the ALD method, energy such as plasma, light, voltage, etc. may be applied, and a catalyst may be used. The timing of applying the energy and the timing of using the catalyst are not particularly limited, and may be, for example, when introducing a compound gas in the raw material introduction step, when heating in the precursor thin film formation step or the metal-containing thin film formation step, when exhausting the system in the exhaust step, when introducing a reducing gas in the metal-containing thin film formation step, or between the above steps.

[0070] In the method for producing a thin film of the present invention, after deposition of the thin film, an annealing treatment may be performed in an inert atmosphere, an oxidizing atmosphere, or a reducing atmosphere in order to obtain better electrical properties, and a reflow step may be performed if step filling is required. The temperature in this case is 200°C to 1000°C, and preferably 250°C to 500°C.

[0071] The apparatus for manufacturing a thin film using the thin film forming material of the present invention may be a well-known chemical vapor deposition apparatus. Specific examples of the apparatus include an apparatus capable of bubbling and supplying a precursor as shown in Fig. 1, and an apparatus having a vaporization chamber as shown in Fig. 2. In addition, an apparatus capable of performing plasma treatment on a reactive gas as shown in Figs. 3 and 4 may be used. Note that the apparatus is not limited to the single-wafer type apparatus as shown in Figs. 1 to 4, and an apparatus capable of simultaneously processing multiple wafers using a batch furnace may also be used.

[0072] The thin film produced by using the thin film forming material of the present invention can be a desired type of thin film such as metal, oxide ceramics, nitride ceramics, glass, etc., by appropriately selecting other precursors, reactive gases, and production conditions. The thin film is known to exhibit electrical properties and optical properties, and is used in various applications. For example, metal ruthenium thin film, ruthenium oxide thin film, ruthenium nitride thin film, ruthenium alloy, and ruthenium-containing complex oxide thin film can be mentioned. Ruthenium alloy can be Ru-Pd alloy or Ru-Pt alloy. These thin films are widely used, for example, in the manufacture of electrode materials for memory elements such as DRAM elements, resistive films, diamagnetic films used in the recording layers of hard disks, and catalyst materials for solid polymer fuel cells. EXAMPLES

[0073] The present invention will be described in more detail below with reference to Production Examples, Evaluation Examples, Examples and Comparative Examples, but the present invention is not limited to the following Examples.

[0074] [Production Example 1] Synthesis of Compound No. 37 In a 1 L four-neck flask, dichlorodi-μ-chlorobis[(1,2,3,6,7,8-η-2,7-dimethyl-2,6-octadiene )10 g of -1,8-diyl]diruthenium (IV) and 19 g of lithium carbonate were added, and 405 ml of ethanol, 19 g of 4-methyl-2-(trifluoromethyl)penta-1,3-diene, and 0.7 g of acetonitrile were added thereto. This reaction solution was heated and stirred at 90°C for 5 hours. After heating and stirring, the solvent was distilled off from the reaction solution under reduced pressure at an oil bath of 90°C, and 200 ml of dichloromethane was added to the resulting residue, followed by filtration. After filtration, the solvent was distilled off from the filtrate at an oil bath of 55°C under normal pressure. After removing the solvent, distillation was performed at an oil bath of 105°C and 15 Pa to obtain pale yellow crystalline compound No. 37 (yield 2.44 g, yield 18.8%).

[0075] (Analysis value) (1) Ambient Pressure TG-DTA Mass reduction by 50% Temperature: 180℃ (760Torr, Ar flow rate: 100ml / min, temperature increase 10℃ / min) (2) Low-pressure TG-DTA Mass reduction by 50% Temperature: 105℃ (10Torr, Ar flow rate: 50ml / min, temperature increase 10℃ / min) (3) 1H-NMR (heavy benzene) 0.138ppm(1H,multiplet), 0.415-0.443ppm(1H,multiplet), 1.418-1.437ppm(3H,doublet), 1.595-1.624ppm(6H,multiplet), 2.5 23-2.862ppm(2H,multiplet), 3.928-4.144ppm(1H,multiplet), 4.461-4.813ppm(1H,multiplet), 5.574-5.640ppm(1H,multiplet) (4) Elemental analysis (theoretical value) Ru:25.5%(25.3%), C:42.0%(42.1%), H:4.3%(4.1%), F:28.2%(28.5%)

[0076] [Production Example 2] Production of Compound No. 106 In a 1 L four-necked reaction flask, dichlorodi-μ-chlorobis[(1,2,3,6,7,8-η-2,7-dimethyl-2,6-octadiene )10 g of [-1,8-diyl]diruthenium (IV) and 19 g of lithium carbonate were added, and 405 ml of ethanol, 13.9 g of 2.4-dimethylhexa-1,3-diene, and 0.7 g of acetonitrile were added thereto. This reaction solution was heated and stirred at 90°C for 5 hours. After heating and stirring, the solvent was distilled off from the reaction solution under reduced pressure at an oil bath of 90°C, and 200 ml of dichloromethane was added to the resulting residue, followed by filtration. After filtration, the solvent was distilled off from the filtrate at an oil bath of 55°C under normal pressure. After removing the solvent, distillation was performed at an oil bath of 130°C and 15 Pa to obtain compound No. 106 as a pale yellow liquid (yield 2.80 g, yield 44.2%).

[0077] (Analysis value) (1) Ambient Pressure TG-DTA 50% mass reduction Temperature: 220℃ (760Torr, Ar flow rate: 100ml / min, temperature increase 10℃ / min) (2) Low-pressure TG-DTA 50% mass reduction Temperature: 130℃ (10Torr, Ar flow rate: 50ml / min, temperature increase 10℃ / min) (3) 1H-NMR (heavy benzene) 0.696-1.031ppm(4H,multiplet), 1.113-1.172ppm(6H,quartet), 1.613-1.868ppm(10H,multiplet), 2.434-2.988ppm(4H,multiplet), 4.638ppm(2H,singlet) (4) Elemental analysis (theoretical value) Ru:31.9%(31.7%), C:60.4%(60.2%), H:7.7%(8.1%)

[0078] [Evaluation Examples 1-2 and Comparative Evaluation Example 1] Evaluation of the physical properties of ruthenium compounds The state of the compounds No. 37 and No. 106 of the present invention obtained in Production Examples 1 and 2, and the comparative compound 1 described below, at 25°C was visually observed. For those that were solid at 25°C, the melting points were measured. In addition, the thermal decomposition onset temperature was measured using a DSC measurement device. These results and the 50% mass loss temperature (TG) measured by reduced pressure TG-DTA were also used. 50) are shown in Table 1. In addition, in the chemical formula of the following comparative compound 1, "Me" represents a methyl group.

[0079] [ka]

[0080] [Table 1]

[0081] As shown in Table 1 above, compound No. 106 was liquid at 25°C. Compound No. 37 was solid at 25°C, but had a relatively low melting point of 55°C. On the other hand, comparative compound 1 had a melting point of 90°C or higher, which was much higher than the present invention. Compounds No. 37 and No. 106 had thermal decomposition onset temperatures 15°C or higher than comparative compound 1, and compound No. 37 in particular had a thermal decomposition onset temperature 30°C higher than comparative compound 1.

[0082] Also, T.G. 50 It was found that the values ​​of compounds No. 37 and No. 106 were lower than those of comparative compound 1, and in particular the value of compound No. 37 was 30°C lower than that of comparative compound 1. From these results, it was found that compounds No. 37 and No. 106 have lower melting points, higher thermal stability, and higher vapor pressures than comparative compound 1, and therefore are excellent as chemical vapor deposition raw materials, with compound No. 37 being particularly excellent.

[0083] [Examples 1-2 and Comparative Example 1] Evaluation of thin films by ALD method Compounds No. 37 and No. 106, and Comparative Compound 1 were used as chemical vapor deposition raw materials, and a ruthenium nitride thin film was produced on a silicon substrate by the ALD method under the following conditions using the ALD apparatus shown in Figure 1. The film thickness of the obtained thin film was measured by X-ray reflectivity method, the compounds in the thin film were identified by X-ray diffraction method, and the carbon content in the thin film was measured by X-ray photoelectron spectroscopy. The results are shown in Table 2.

[0084] (conditions) Reaction temperature (substrate temperature): 200°C, reactive gas: ammonia (Process) A series of steps consisting of the following steps (1) to (4) was defined as one cycle, and 150 cycles were repeated. (1) The vapor of the chemical vapor deposition source material vaporized under the conditions of a source container heating temperature of 100° C. and a source container internal pressure of 100 Pa is introduced and deposited at a system pressure of 100 Pa for 30 seconds. (2) Unreacted materials are removed by purging with argon for 10 seconds. (3) A reactive gas is introduced and reacted at a system pressure of 100 Pa for 30 seconds. (4) Unreacted materials are removed by purging with argon for 10 seconds.

[0085] [Table 2] *1:The detection limit is 0.1atm%.

[0086] The carbon content in the thin film obtained by the ALD method was 10 atm% or more in Comparative Example 1, whereas it was below the detection limit of 0.1 atm% in Examples 1 and 2. In other words, it was shown that a high-quality thin film can be obtained by using the ruthenium compound of the present invention. In addition, the thickness of the thin film obtained was 2.5 nm in Comparative Example 1, whereas it was 5.5 nm or more in Examples 1 and 2, and the thin film was obtained with high productivity by using the ruthenium compound of the present invention. In particular, when Compound No. 37 was used as a chemical vapor deposition material, a thin film could be obtained with high productivity, indicating that it is excellent as a chemical vapor deposition material.

Claims

1. A ruthenium compound represented by the following general formula (1): 【Chemistry 1】 (In the formula, R 1 ~R 12 each independently represents a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, or a fluorine atom-containing group, the fluorine atom-containing group being a fluoro group, a monofluoromethyl group, a difluoromethyl group, or a trifluoromethyl group, and n represents an integer of 2. 1 ~R 12 At least one of the groups is a fluorine atom-containing group.

2. A raw material for forming a thin film containing the ruthenium compound described in claim 1.

3. A raw material for forming a thin film by an ALD method, comprising a ruthenium compound represented by the following general formula (2): 【Chemistry 2】 (In the formula, R 13 and R 15 represents a hydrogen atom, and R 14 , R 16 and R 17 represent a methyl group.

4. A step of vaporizing the thin film forming material according to claim 2; A step of introducing the vapor containing the ruthenium compound obtained in the above step into a deposition chamber in which a substrate is placed; and The method for producing a thin film containing ruthenium atoms on the surface of a substrate includes a step of decomposing and / or chemically reacting the ruthenium compound to form a thin film containing ruthenium atoms on the surface of the substrate.

5. A method for producing a thin film containing ruthenium atoms on a surface of a substrate by an ALD method, comprising the steps of: A step of vaporizing the thin film forming material according to claim 3; A step of introducing the vapor containing the ruthenium compound obtained in the above step into a deposition chamber in which a substrate is placed; and The method for producing a thin film containing ruthenium atoms on the surface of a substrate by an ALD method includes a step of decomposing and / or chemically reacting the ruthenium compound to form a thin film containing ruthenium atoms on the surface of the substrate.

Citation Information

Patent Citations

  • Ruthenium compound, and method of forming metallic ruthenium film

    JP2005060814A

  • Precursor having open ligand for ruthenium-containing film deposition

    JP2008069453A

  • Method and apparatus for optical excitation of chemicals for atomic layer deposition of dielectric films

    JP2009536267A

  • Method for producing dienyl-ruthenium complexes

    JP2011521983A

  • Organic light-emitting element

    JP2015153993A