Fregocement made from a new earth-inspired clinker

By using igneous rocks to produce hydraulic clinker, cement production achieves a 70% reduction in carbon emissions and creates a durable, resilient cement with improved mechanical properties, addressing the limitations of existing carbon reduction methods.

JP7565357B2Active Publication Date: 2024-10-10THE BOARD OF TRUSTEES OF THE LELAND STANFORD JUNIOR UNIV
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2022533362
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-12-06
Filing Date
2020-12-04
Publication Date
2024-10-10
Estimated Expiration
2040-12-04

AI Technical Summary

Technical Problem

Cement production is a significant source of greenhouse gas emissions, and existing methods to reduce these emissions, such as carbon upcycling and carbon capture and storage, are costly, inefficient, and limited by the formation of unstable carbonate minerals and high operational costs.

Method used

The use of igneous rocks as an alternative raw material for cement production, which eliminates carbon dioxide emissions by replacing lime with calcium oxide and forming hydraulic clinker that produces calcium-sulfo-aluminate hydrate fibers and geopolymers, resulting in a cross-braided mortar structure with enhanced mechanical and chemical properties.

Benefits of technology

This approach reduces carbon emissions by approximately 70%, enhances durability and physicochemical resilience, and improves compressive strength and thermal stability, making it suitable for harsh environments and applications requiring strain energy absorption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000006_0000
    Figure 00000006_0000
  • Figure 00000006_0001
    Figure 00000006_0001
  • Figure 00000006_0002
    Figure 00000006_0002
Patent Text Reader

Abstract

The present disclosure provides an improved cement for concrete that achieves a reduced carbon footprint and improved mechanical properties. A limestone-free clinker production process reduces the carbon footprint by 70% compared to traditional Portland cement production. Curing the resulting cement at temperatures ranging from 80 to 100°C advantageously promotes the growth of fibrous minerals in the concrete.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing cement with a reduced carbon footprint. [Background technology]

[0002] High energy and chemical processes are the main contributors to greenhouse gas emissions, and in the case of concrete, this is cement production. Cement production accounts for 8% of global CO2 emissions, both directly from the pyrolysis of calcined limestone and clay rocks required for Portland cement clinker (about 70% of emissions) and indirectly from energy use, especially the combustion of fossil fuels (about 30% of emissions). Each year, about 1,300 Mt / year of CO2 is emitted worldwide as a result of the calcination reactions and the energy used to do so. Considering that a typical car emits about 4.6 tons of carbon dioxide per year, a reduction of about 70% of carbon dioxide emissions by using the clinker of the present invention is equivalent to removing 75% of the cars in the United States from the road.

[0003] Importantly, focusing only on CO2 emissions is insufficient for sustainable development. The above calculations do not include the lifespan of concrete. Modern concrete starts to deteriorate after around 10 years, with a total lifespan set at 50-100 years. Research literature highlights the importance of including key factors, namely strength, performance, and durability, when assessing the life cycle impacts of concrete. It is therefore crucial to minimize the carbon footprint of material technologies while pushing the boundaries of material performance under harsh conditions of temperature, stress, stress changes, chemical environments, and their complex interactions. Summary of the Invention [Means for solving the problem]

[0004] The focus of this invention is to achieve low or near zero greenhouse gas emissions of cement clinker by using alternative raw materials with zero carbon footprint instead of lime. The final output is the design and testing of crossbred mortar structures from nano-scale to macro-scale components that show the best properties of two worlds: Roman marine concrete (Figure 1A) and concrete-like rock created by nature (Figure 1B). These properties include improved durability, physicochemical resilience, and serviceability in harsh environments, i.e. temperature, stress changes, and acidic fluids. Most importantly, the use of alternative raw materials according to this invention allows a 70% reduction in CO2 emissions (Figure 3).

[0005] The novel lime-producing rocks, which are alternative raw materials according to the present invention, are igneous rocks rather than carbonate rocks, i.e. sedimentary rocks, which belong to the rock category to which limestone and dolomite belong. Like carbonate rocks, igneous rocks contain calcium oxide (CaO, quicklime) as part of their mineral composition. However, such compositions lack the carbonate ion (CO3 - ) is missing.

[0006] The advantages and improvements of the alternative raw materials according to the present invention over conventional clinker are manifold.

[0007] First, the alternative raw material, the novel igneous rock-derived "lime", according to the present invention, is itself hydraulic.

[0008] Secondly, it contributes to reducing the CO2 emissions in cement production. The key idea behind the use of alternative raw materials in accordance with the present invention is to directly reduce carbon emissions from the "upstream" of the cement production process, rather than relying on carbon upcycling for cement production. The use of alternative raw materials in accordance with the present invention results in zero carbon footprint from pyrolysis reactions in the firing process, which in turn reduces the CO2 emissions from the conventional firing process by approximately 70%. Conventional technologies aimed at reducing CO2 emissions in cement production rely heavily on carbon upcycling, i.e. carbon capture and storage (CCS), i.e. capturing carbon dioxide emitted by industrial activities and turning it into cement to produce potentially carbon-neutral concrete. However, CO2 mineral storage through carbon curing reactions has three drawbacks: (1) alkaline wastewater is generated, which needs to be treated; and (2) carbonate minerals are formed in the hardened concrete, which are unstable and subject to chemical weathering. This raises questions about the long-term stability and performance of CO2-hardened concrete. (3) The utilization of this technology is hindered by the high cost of building new cement plants.

[0009] Third, the hydraulic clinker produces calcium-sulfo-aluminate hydrate fibers that, when slaked and dispersed in the pozzolanic ash, form fiber clusters that constitute the functional and structural units of cement.

[0010] Fourth, hydraulic clinker produces geopolymers. When hydraulic clinker is slaked, the alkali metal oxides (Na2O, K2O), CaO, and Al2O3 contained in the hydraulic clinker form geopolymers, which serve to strengthen the interfacial bond between the fibers and the matrix. Geopolymers exhibit superior mechanical and physical properties, such as improved compressive strength, thermal stability, and acid fluid resistance.

[0011] In summary, slaking the clinker according to the present invention promotes a cross-braided structure created by the natural growth of fibrous minerals of CSAH and geopolymers due to the natural blend composition of the clinker. When this clinker is mixed with naturally occurring ash such as volcanic ash or fly ash or industrial by-products, CASH is formed. By embedding fiber clusters in the cross-braided mortar, a naturally reinforced mortar is formed. This cross-braided nature of the mortar, both fibrous and polymeric, has good potential to provide superior physicochemical properties such as improved compressive strength, thermal stability, and acidic fluid resistance. Also, the absence of free and amorphous silica in the raw materials is expected to minimize alkali-silica reaction (ASR). [Brief description of the drawings]

[0012] [Figure 1A] FIG. 1A is a SEM image showing an exemplary conventional cementitious microstructure. [Figure 1B] FIG. 1B is a SEM image showing an exemplary conventional cementitious microstructure. [Diagram 2] FIG. 2 is a table showing exemplary compositions according to the present invention. [Diagram 3] FIG. 3 is a graph illustrating the reduction in carbon emissions according to the principles of the present invention. [Figure 4A] FIG. 4A is an SEM image showing an exemplary growth of fibrous minerals produced by hydrothermal synthesis. [Figure 4B] FIG. 4B is an SEM image showing an exemplary growth of fibrous minerals produced by hydrothermal synthesis. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] (A) Decarbonization of cement production

[0014] Decarbonizing cement production is not an easy task. The carbon-emitting moieties in Portland cement (i.e., CaO from limestone) are also involved in the formation of Portland cement's adhesive (calcium silicate hydrate: CSH). Therefore, decarbonizing cement production requires replacing these carbon-emitting moieties with others that promote the formation of cementitious phases. Eco-friendly adhesives must also ensure durability and serviceability.

[0015] Prior art has focused on alternative processes and / or materials, such as capturing the CO2 generated from firing for use in concrete hardening techniques, producing alternative cementitious mixtures, and using alternative raw materials to promote the formation of cementitious phases.

[0016] Hardening carbonation relies on carbon upcycling, an accelerated hardening process that captures waste carbon dioxide produced during firing and injects supercritical (temperature = 31°C, pressure = 72.8 atm) CO2 into fresh concrete, trapping the CO2 within the concrete by mineralizing it into calcite (CaCO3). This conventional technology, which potentially leads to carbon-neutral concrete cementation, is limited to precast concrete products and suffers from the drawback of the formation of carbonate minerals within the concrete, which are brittle and prone to chemical weathering. Furthermore, the high costs of adapting cement plants to the above needs also hinder the adoption of this technology.

[0017] Alternative cementitious mixtures replace part of the Portland cement (a source of CaO) with a source of Si and Al, i.e., aluminosilicate materials. The aluminosilicate materials can be industrial by-products, such as cheap fly ash and slag from coal-fired power plants and steel mills, or natural origin raw materials, such as volcanic ash and metakaolin. The CaO content in Portland clinker significantly affects the compressive strength, so cementation is induced by adding an alkaline solution (e.g., sodium alumino-silicate hydrate, NASH) to promote the activation of the different cementitious phases. There are various challenges, ranging from cost to operational safety concerns related to the corrosiveness of the chemical additives. In addition, fly ash and slag are not as abundant as they used to be, as coal-fired power plants are closing and steel production is declining.

[0018] The alternative raw materials presented herein are solid and naturally contain both alkaline earth oxides (CaO, MgO) and alkali metal oxides (Na2O, K2O).

[0019] (B) Examples of conventional cementitious microstructures

[0020] Figures 1A and 1B are scanning electron microscope (SEM) images of Roman marine concrete (MacFarlane et al., 2020) and concrete-like rock from the caldera (Vanorio and Kanitpanyacharoen, 2015). Both of the cementitious microstructures show fine fibrous structure.

[0021] (C) Examples of clinker compositions of the present invention

[0022] Exemplary compositions of the compositions of the present invention are shown in the table of Figure 2. The Leucitophyre column is the composition of the input rock (an igneous rock replacing limestone and clay), the Raw Materials column is the composition of the input materials for the clinker calcination process, and the Pozzolanic Ash column is the composition of the ash that is mixed with the clinker and slaked to produce phlego cement.

[0023] The overall process flow is: (1) crushing an input rock to generate a raw material; (2) calcining the raw materials to form clinker (e.g., using a calcination temperature in the range of 900-1200°C and a residence time of 60 minutes, similar to the process used to calcinate conventional raw materials to produce conventional clinker); (3) slaking the clinker; (4) mixing the slaked clinker with pozzolanic ash and allowing it to harden to form a mortar having the desired properties as described above.

[0024] The raw materials contain minerals that lack carbonic acid or carbonate ions. Therefore, the clinker burning process is carbon neutral. The raw materials can contain both oxides of alkaline earth metals (magnesium, calcium, strontium, barium) and oxides of alkali metals (sodium, potassium). When mixed with pozzolanic ash, the clinker produces Fregocement, a hybrid CASH-geopolymer cement that is expected to have excellent mechanical properties and performance.

[0025] Moreover, these types of rocks exhibit naturally mixed compositions, (1) Ettringite (CSAH, calcium sulfo-aluminate hydrate) natural mineral fiber; (2) CASH phase (calcium-alumino-silicate hydrate) present in Al-rich pozzolanic cements; (3) Geopolymer; It is possible to produce a clinker having the ability to form a cross-blended mortar consisting of: The cement clinker according to the invention ensures the presence of several of these phases by the addition of additives.

[0026] The igneous rock is called leucite-tephrite or tephrite-basanite (or foid-monzodiolite / monzogabbro). These terms refer to rocks that have the same elemental composition. The only difference is the type of microstructure and crystallinity of the rock. This type of igneous rock is ubiquitous in nature, found during activity above subduction boundaries and in ancient ultrapotassic or calc-alkaline magmatism.

[0027] The composition of the novel raw material of the present invention is (a) silica (40 to 60% by weight); (b) aluminum oxide (10 to 25% by weight); (c) sulfur oxides (0.5-2 wt%) (sulfur oxides have the ability to form fibrous ettringite (CSAH, calcium-sulfo-aluminate hydrate) in the presence of CaO and Al2O3. Sulfur oxides also produce natural fiber reinforced mortar); (d) calcium oxide (5–15 wt%) (which forms Al-tobermorite (CASH, calcium-alumino-silicate hydrate) when mixed with pozzolanic ash in the presence of Al2O3); (e) Alkali metal oxides (Na2O, K2O, 5 to 15% by weight).

[0028] Alkali is important because it serves two purposes: (1) to speed up the hydration process of CASH, and (2) to promote chemical cross-linking that results in the formation of polymeric phases. In the clinker of the present invention, the presence of alkali is ensured by high temperature treatment of the clayey stone added to the raw materials. The presence of alkali metal oxides in the naturally mixed mixture of CaO and Al2O3 ensures the formation of geopolymers when the clinker is slaked under alkaline conditions at temperatures as low as 80°C. The inclusion of almost the same amount of alkali metal oxides (Na2O, K2O) as CaO and the presence of Al2O3 give the mixture the ability to produce a clinker with hydraulic properties.

[0029] An important aspect of this feedstock is that it does not contain any carbon-containing species, and preferably contains less than 1% by weight of carbon-containing species, and preferably close to 0% by weight.

[0030] To produce Fregocement, a portion of the clinker of the present invention is mixed with pozzolanic ash of natural origin or industrial by-product (e.g. volcanic ash or fly ash) in a ratio of 1:2. Each clinker lump dispersed in the pozzolan constitutes a functional and structural unit of cement. Upon slaking, each clinker lump forms fibrous ettringite (CSAH, calcium-sulfo-aluminate hydrate) and forms clusters of intertwined fibers that disperse in the pozzolanic ash and spread to the surrounding area. This forms a natural fiber reinforced material. Due to the presence of alkali metal oxides (Na2O, KO) and CaO in both the clinker and the pozzolan ash, the fibrous ettringite becomes embedded in a cross-blended mortar matrix made of geopolymer and CASH (calcium-alumino-silicate hydrate).

[0031] In addition to the environmental benefits of reduced CO2 emissions, the cement also improves durability, physicochemical resilience, and serviceability, most notably in applications requiring strain energy absorption and / or stability in harsh environments, such as: (1) concrete used in areas subject to earthquake ground vibrations, (2) cement sheaths between well casings exposed to CO2 injection, fracking acid fluids, or reinjection of fracking wastewater, which pose a risk to water resources, (3) industrial waste encapsulation, and (4) planetary shelters and future habitats.

[0032] (D) Reducing carbon emissions

[0033] Figure 3 shows the mass loss when both limestone and the novel binder precursor are heated (calcined) at 900 °C. The mass loss of limestone (squares) is stoichiometric (43.9%, slope of the fitting trend) and corresponds to the mass of CO2 released upon calcination of CaCO3. The novel binder precursor (circles) is carbon-free compared to limestone, suggesting a significant reduction in CO2 emissions during pyrolysis.

[0034] (E) Example of fiber growth by hydrothermal synthesis

[0035] Figures 4A and 4B are images showing an example of fiber growth by hydrothermal synthesis (Head et al., 2018). The use of an alkali-calcium clinker composition (as described above) in conjunction with a synthesis mimicking natural hydrothermal systems (approximately 80-100 °C) allows the growth of fiber minerals to be promoted inside the binder. This results in the unique advantages of (a) eliminating the problem of increased cement viscosity due to the addition of fibers to the material, and (b) being able to chemically and mechanically blend the fibers in the mortar. The former avoids problems with the workability of the slurry, while the latter promotes the bonding process at the matrix-fiber interface.

Claims

1. 1. A method for producing clinker for use in cement production, comprising: providing a feedstock comprising silica, aluminum oxide, alkali metal oxide, calcium oxide, and sulfur oxide; and calcining the raw materials to produce clinker; The weight fraction of silica in the raw material is in the range of 40 to 60%; The weight fraction of aluminum oxide in the raw material is in the range of 10 to 25%; The weight fraction of the alkali metal oxide in the raw material is in the range of 5 to 15%; The weight fraction of calcium oxide in the raw material is in the range of 5 to 15%; The weight fraction of sulfur oxide in the feedstock is in the range of 0.5 to 2%; and The method of claim 1, wherein the weight fraction of carbon-containing species in said feedstock is less than 1%.

2. 2. The method of claim 1 , The method of claim 1, wherein said step of calcining said raw materials to form clinker is carried out at a temperature range of 900-1200°C.

3. 1. A method of forming concrete comprising the steps of: carrying out the method of claim 1 to produce clinker; slaking the clinker to form a slurry; and curing the slurry at a temperature in the range of 80-100°C to promote the growth of fibrous minerals.

Citation Information

Patent Citations

  • Simultaneous production of steam power and cement clinker in the same equipment, its product, equipment and method of use

    JP1999511107A

  • Dimensionally stable geopolymer composition and method

    JP2015518462A

  • Geopolymer cured body with high bending performance and method for producing the same

    JP2019147719A

  • Quality control method for cement clinker

    JP2019151526A

  • Rapid hardening, ultra-high early strength Portland-type cement compositions, novel clinkers and methods for their manufacture which reduce harmful gaseous emissions

    US6113684A