Varistor and manufacturing method thereof

The varistor design with optimized ineffective layer thicknesses and manufacturing process addresses surge resistance and heat dissipation challenges, enhancing protection against high-energy surges and thermal damage.

JP7565484B2Active Publication Date: 2024-10-11PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2021501585
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-02-22
Filing Date
2019-12-02
Publication Date
2024-10-11
Estimated Expiration
2039-12-02

AI Technical Summary

Technical Problem

Conventional varistors face challenges in providing effective surge resistance and heat dissipation, especially in applications requiring high-energy surge protection, leading to potential thermal damage and deformation.

Method used

A varistor design with a thinner ineffective layer facing the mounting surface and a thicker ineffective layer on the opposite side, enhancing heat dissipation and surge resistance by optimizing the thickness ratio of these layers, along with a manufacturing process that includes specific material composition and alignment techniques.

Benefits of technology

The varistor achieves improved surge resistance and heat dissipation, allowing for effective protection against high-energy surges while minimizing thermal runaway and deformation, suitable for in-vehicle applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000007_0000
    Figure 00000007_0000
  • Figure 00000008_0000
    Figure 00000008_0000
  • Figure 00000008_0001
    Figure 00000008_0001
Patent Text Reader

Abstract

A varistor comprises: an effective layer having a first surface and a second surface on opposite sides from one another; a first inactive layer laminated on the first surface of the effective layer; a second inactive layer laminated on the second surface of the effective layer; and an external electrode. The effective layer comprises: a ceramic layer having a polycrystalline structure constituted of a plurality of crystal particles which exhibit voltage nonlinearity; and a plurality of internal electrodes laminated alternately with the ceramic layers. The thickness of the second inactive layer falls within the range of 1.1x to 6x the thickness of the first inactive layer, inclusive. This varistor is compact and has suitable surge-resistance.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a varistor that protects semiconductor elements and the like from surges and static electricity. [Background technology]

[0002] When abnormal voltages such as surges or static electricity are applied to, for example, a semiconductor IC in the circuit of an electronic device, the electronic device may malfunction or be destroyed. Varistors are an example of electronic components that protect electronic devices from such abnormal voltages. Conventional varistors are disclosed in Patent Documents 1 and 2. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2008-218749 A [Patent Document 2] Japanese Patent Application Publication No. 4-325413 Summary of the Invention

[0004] The varistor comprises an effective layer having first and second surfaces opposite to each other, a first ineffective layer laminated on the first surface of the effective layer, a second ineffective layer laminated on the second surface of the effective layer, and an external electrode. The effective layer has a ceramic layer having a polycrystalline structure composed of a plurality of crystal grains exhibiting voltage nonlinearity characteristics, and a plurality of internal electrodes laminated alternately with the ceramic layer. The thickness of the second ineffective layer is 1.1 times or more and 6 times or less the thickness of the first ineffective layer.

[0005] This varistor is small and has good surge resistance. [Brief description of the drawings]

[0006] [Figure 1A] FIG. 1A is a cross-sectional view of a varistor according to an embodiment. [Figure 1B] FIG. 1B is a perspective view of a varistor according to an embodiment. [Diagram 2] FIG. 2 is an enlarged cross-sectional view of the varistor according to the embodiment. [Diagram 3] FIG. 3 is a graph showing the relationship between the thickness of the ineffective layer and the withstand current of the varistor according to the embodiment. [Figure 4] FIG. 4 is a graph showing the relationship between the thickness of another ineffective layer of the varistor according to the embodiment and the withstand current. [Diagram 5] FIG. 5 is a graph showing the relationship between the ratio of the thicknesses of the two ineffective layers of the varistor and the withstand current in the embodiment. [Figure 6] FIG. 6 is a flow diagram showing a method for manufacturing a varistor in accordance with an embodiment. [Figure 7] FIG. 7 is a cross-sectional view of a varistor manufacturing apparatus according to the embodiment. [Figure 8] FIG. 8 is a schematic diagram of a varistor manufacturing apparatus according to the embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0007] The embodiments described below each show a specific example. The numerical values, shapes, materials, components, the arrangement positions and connection forms of the components shown in the following embodiments are examples and are not intended to limit the present invention. Furthermore, among the components in the following embodiments, components that are not described in the independent claims showing the highest concept are described as optional components. In the following, the same or corresponding components are given the same reference numerals throughout all the figures, and duplicate descriptions thereof are omitted.

[0008] 1A and 1B are respectively a cross-sectional view and a perspective view of a varistor 100 according to an embodiment. FIG. 1A shows a cross-section of the varistor 100 shown in FIG. 1B along line 1A-1A. The varistor 100 includes an effective layer 10c having mutually opposite faces 110c and 210c, an ineffective layer 10a laminated on the face 110c of the effective layer 10c in a lamination direction D100, an ineffective layer 10b laminated on the face 210c of the effective layer 10c in a direction D101 opposite to the lamination direction D100, and external electrodes 13 and 14. The effective layer 10c includes a ceramic layer 10d, an internal electrode 11 abutting against the ceramic layer 10d, and an internal electrode 12 abutting against the ceramic layer 10d and facing the internal electrode 11 via the ceramic layer 10d. The ceramic layer 10d and the internal electrodes 11 and 12 are alternately stacked to form the effective layer 10c. The ineffective layer 10a is made of the same material as the ceramic layer 10d and abuts the internal electrode 11. The ineffective layer 10b is made of the same material as the ceramic layer 10d and abuts the internal electrode 12. The ceramic layer 10d, the ineffective layer 10b, and the ineffective layer 10a are integrally formed to form the element body 10. The internal electrode 11 is embedded in the element body 10 and has one end exposed at an end face 110 of the element body 10 and electrically connected to the external electrode 13. The internal electrode 12 is embedded in the element body 10 facing the internal electrode 11 and has one end exposed at an end face 210 of the element body 10 opposite the end face 110 and electrically connected to the external electrode 14. The element body 10 and the internal electrodes 11 and 12 form a sintered body 25.

[0009] 1A, the varistor 100 is configured to be mounted on a mounting surface 200 such that the surface 1100, i.e., the reactive layer 10a, faces the mounting surface 200 of the substrate 201. When the varistor 100 is mounted on the mounting surface 200 of the substrate 201, the reactive layer 10b is located on the opposite side of the mounting surface 200 with respect to the reactive layer 10a.

[0010] The varistor 100 in the embodiment is used in applications requiring improved resistance to high-energy surges, such as in-vehicle applications. Destruction due to high-energy surges is caused by thermal damage, and improving heat dissipation is necessary to improve resistance. An example of the varistor 100 in the embodiment will be described below. The element of this example has a thin ineffective layer 10a facing the mounting surface, improving heat dissipation from the effective layer 10c, which generates heat when an abnormal voltage is applied, to the substrate 201. In addition, the ineffective layer 10b on the opposite side to the mounting surface 200 is thickened to function as a heat sink, further improving heat dissipation.

[0011] Table 1 shows the thickness Ta of the ineffective layer 10a, the thickness Tb of the ineffective layer 10b, the ratio Tb / Ta of the thickness Tb to the thickness Ta, and the withstand current of the samples. In Table 1, samples marked with "*" are comparative examples that are different from the examples. In this disclosure, the nonlinearity of the varistor 100 is expressed as the voltage value V between the external electrodes 13 and 14 when a current of 1 mA is applied to the voltage nonlinear resistor composition. 1mA In this example, protection of ICs for automotive applications is assumed, and V 1mA =22V element was used.

[0012] [Table 1]

[0013] Fig. 2 is an enlarged cross-sectional view showing the element body 10 of the varistor 100 shown in Fig. 1A. The element body 10 is composed of a plurality of zinc oxide particles 10e and an oxide layer 10f as main components. The oxide layer 10f contains the elements bismuth, cobalt, manganese, antimony, nickel, and germanium. The plurality of zinc oxide particles 10e have a hexagonal crystal structure. The oxide layer 10f is interposed between the plurality of zinc oxide particles 10e.

[0014] The element 10 is a voltage nonlinear resistor composition comprising a plurality of zinc oxide particles 10e and an oxide layer 10f interposed between the plurality of zinc oxide particles 10e.

[0015] The voltage non-linearity of the varistor 100 will now be described. The resistance value of a varistor drops sharply at a certain applied voltage value. This causes the varistor to have a non-linear relationship between voltage and current. In other words, it is preferable that the varistor 100 exhibits a higher resistance value in the region where the applied voltage is low, and a lower resistance value in the region where the applied voltage is high.

[0016] The resistance of the varistor 100 of the present disclosure will now be described in detail.

[0017] The influence of the thickness Ta of the ineffective layer 10a facing the mounting surface 200 on the heat dissipation to the substrate 201 was examined. FIG. 3 shows the withstand current when the thickness Ta of the ineffective layer 10a is 150 to 750 μm in an element (see FIG. 1B) with length L×width W×thickness T=3.2×2.5×1.6. The values ​​shown in FIG. 3 are test results of the samples with sample numbers 1 to 7 listed in Table 1. The thickness Tb of the ineffective layer 10b on the opposite side of the mounting surface 200 is fixed at 500 μm. It can be seen that the withstand current increases and improves with the decrease in thickness Ta. This is because the ineffective layer 10a facing the mounting surface 200 becomes thinner, which shortens the distance from the heat-generating effective layer 10c to the surface 1100 facing the mounting surface 200, making it easier to conduct heat to the substrate 201. When the thickness Ta of the ineffective layer 10a is reduced from 750 μm to 500 μm and the ratio Tb / Ta of the thickness Tb of the ineffective layer 10b to the thickness Ta of the ineffective layer 10a is increased from 0.67 to 1.00, the withstand current increases by 12.5% ​​from 0.16 A to 0.18 A. When the thickness Ta of the ineffective layer 10a is reduced from 500 μm to 400 μm and the ratio Tb / Ta is increased from 1.00 to 1.25, the withstand current increases by 55.6% from 0.18 A to 0.28 A, which shows that the resistance to surges is greatly improved.

[0018] In addition, as the element body 10 becomes larger, the heat dissipation from inside the element body 10 decreases, making the varistor more susceptible to thermal runaway. Further improvement in resistance can be expected by improving the heat dissipation from the upper part of the element body 10. Since the element body 10 of the varistor 100 of this embodiment has a high thermal conductivity of 38 W / (m·K) among ceramics, the ineffective layer 10b can be made to function as a heat sink by increasing the thickness Tb of the ineffective layer 10b on the opposite side of the mounting surface 200. FIG. 4 shows the relationship between the thickness Tb (100 to 900 μm) of the ineffective layer 10b on the opposite side of the mounting surface 200 of the element body 10 of the same size and the withstand current. The thickness Ta of the ineffective layer 10a facing the mounting surface 200 was fixed at 500 μm. Contrary to the ineffective layer 10a, the withstand current increases as the thickness Tb of the ineffective layer 10b increases. This is due to the ineffective layer 10b functioning as a heat sink, drawing out and dissipating the heat generated in the internal effective layer 10c. When the thickness Tb of the ineffective layer 10b increases from 300 μm to 500 μm and the ratio Tb / Ta of the thickness Tb of the ineffective layer 10b to the thickness Ta of the ineffective layer 10a increases from 0.6 to 1.00, the withstand current increases by 20.0% from 0.15 A to 0.18 A. When the thickness Tb of the ineffective layer 10b increases from 500 μm to 550 μm and the ratio Tb / Ta increases from 1.00 to 1.10, the withstand current increases by 44.4% from 0.18 A to 0.26 A, and it can be seen that the resistance to surges is greatly improved. Together with the results of FIG. 3, a significant improvement in resistance is observed when the ratio Tb / Ta is 1.1 or more.

[0019] Next, the relationship between the ratio Tb / Ta of the thickness Tb of the ineffective layer 10b on the opposite side of the mounting surface 200 to the thickness Ta of the ineffective layer 10a facing the mounting surface 200 and the withstand current will be described. FIG. 5 shows the relationship between the ratio Tb / Ta and the withstand current. Table 1 also shows combinations of the thickness Ta of the ineffective layer 10a and the thickness Tb of the ineffective layer 10b, and the withstand current for each combination. It can be seen that the withstand current increases with an increase in the ratio Tb / Ta. That is, it is shown that a high withstand current is achieved when the thickness Ta of the ineffective layer 10a facing the mounting surface 200 is small and the thickness Tb of the ineffective layer 10b on the opposite side is large. Also, when the thickness Tb of the ineffective layer 10b is more than six times the thickness Ta of the ineffective layer 10a, the effective layer 10c is excessively close to the ineffective layer 10a, and the shrinkage during firing of the element 10 becomes locally large in the ineffective layer 10a, which is undesirable because it makes the element 10 more likely to deform or crack. In order to prevent a short circuit on the surface 2100 of the varistor 100, the thickness Ta of the ineffective layer 10a is preferably larger than the thickness Td (see FIG. 1A) of the ceramic layer 10d sandwiched between adjacent internal electrodes 11, 12 among the multiple internal electrodes. If the thickness Tb of the ineffective layer 10b is made twice or more the thickness Ta of the ineffective layer 10a, the position of the effective layer 10c is biased from the center to the ineffective layer 10a. Since the density of the internal electrodes 11, 12 is larger than that of the element body 10, this bias causes the center of gravity 100g of the varistor 100 to be closer to the surface 1100. In other words, the distance from the center of gravity 100g to the surface 1100 is smaller than the distance from the center of gravity 100g to the surface 2100. This makes it easier to align the directions of the ineffective layers 10a and 10b in the manufacturing process, which is more preferable.

[0020] Next, a method for manufacturing the varistor 100 will be described.

[0021] FIG. 6 is a manufacturing flow diagram showing the manufacturing process of the varistor 100.

[0022] First, as starting materials for the element 10, zinc oxide powder, bismuth oxide powder, cobalt oxide powder, manganese oxide powder, antimony oxide powder, nickel oxide powder, and germanium oxide powder are prepared.

[0023] The mixing ratio of the starting materials is 96.54 mol% zinc oxide powder, 1.00 mol% bismuth oxide powder, 1.06 mol% cobalt oxide powder, 0.30 mol% manganese oxide powder, 0.50 mol% antimony oxide powder, 0.50 mol% nickel oxide powder, and 0.10 mol% germanium oxide powder. A slurry containing these powders and an organic binder is prepared (step S1).

[0024] Next, the steps of obtaining a plurality of green sheets will be described in detail.

[0025] FIG. 7 is a cross-sectional view of an apparatus showing a schematic step of obtaining a plurality of green sheets.

[0026] The above-mentioned slurry 20 is applied onto a film 21 made of polyethylene terephthalate (PET) through a gap having a width LA of 180 μm, and then dried to obtain a plurality of green sheets (step S2).

[0027] Next, an electrode paste containing silver-palladium alloy powder is printed in a predetermined shape on a predetermined number of green sheets, and a predetermined number of these green sheets are stacked in a stacking direction D100 (see FIG. 1A) perpendicular to the surface direction of the green sheets to obtain a laminate (step S3). At this time, the thickness Tb of the ineffective layer 10b and the thickness Ta of the ineffective layer 10a are adjusted to predetermined values ​​depending on the number of green sheets stacked that are not printed with the electrode paste.

[0028] Next, this laminate is pressurized at 55 MPa along the lamination direction D100 and the direction D101 (step S4). The pressure is preferably in the range of 30 MPa to 100 MPa. Pressurizing the laminate with a pressure of 30 MPa or more increases the adhesion of the green sheets, and an element without structural defects is obtained. Pressurizing the laminate with a pressure of 100 MPa or less allows the shape of the electrode paste inside the laminate to be maintained. In addition, when the material of the ineffective layer 10a and the ineffective layer 10b is different from that of the effective layer 10c, it is more preferable to press isotropically by warm isostatic pressing, which has the effect of preventing structural defects such as cracks and deformation of the element. Then, the obtained laminate was cut into each element size to produce a chip laminate 25a (see FIG. 1A).

[0029] Next, the laminate 25a chip is fired at 850°C to obtain a sintered body 25 (see Fig. 1A) consisting of the element 10 (voltage nonlinear resistor composition) and the internal electrodes 11 and 12 (step S5). This firing process turns the multiple zinc oxide powder starting material into multiple zinc oxide particles 10e as shown in Fig. 2, and a voltage nonlinear resistor in which oxide layers 10f are interposed between the multiple zinc oxide particles 10e can be obtained.

[0030] Next, an electrode paste containing an alloy powder of silver and palladium is applied to the end faces 210, 220 of the element body 10 and heat-treated at 800° C. to form the external electrodes 13, 14. The external electrodes 13 and 14 may be formed by a plating method. The external electrodes 13 and 14 may also be a combination of an external electrode formed by firing an electrode paste and an external electrode formed by a plating method.

[0031] In this example, the V of the sample of varistor 100 1mA The thickness of element 10 was designed so that the input voltage was 22 V (±2 V), and the firing conditions were determined so that the material constants after firing would be the same. The resistance was evaluated by mounting a sample of varistor 100 on substrate 201 with solder and measuring the withstand current when a DC voltage was applied, that is, the current at which thermal runaway begins.

[0032] In order to mount the varistor 100 so that the ineffective layer 10a faces the mounting surface 200, it is necessary to align the vertical positional relationship of the ineffective layers 10a and 10b in advance. For example, by making the stacking direction D100 the vertical direction, which is the predetermined direction Dv, when the varistor 100 is placed in a carrier tape to be attached to a mounting machine, the positional relationship of the ineffective layers 10a and 10b can be set to a predetermined relationship without the need for a process of aligning the orientation of the varistor 100. Since the ineffective layer 10a is thinner than the ineffective layer 10b, the center of gravity 100g of the varistor 100 is biased toward the ineffective layer 10a. In other words, the center of gravity 100g is closer to the surface 1100 than to the surface 2100.

[0033] FIG. 8 is a schematic diagram of a manufacturing apparatus 300 for the varistor 100. The manufacturing apparatus 300 includes a storage tank 301 that contains a liquid 302. As described above, when plating the external electrodes 13, 14, the varistor 100 is placed in the plating liquid 302. Even if the ineffective layers 10a, 10b are not aligned vertically at this time, the surface 1100 closest to the center of gravity 100g, i.e., the ineffective layer 10a, is positioned downward in the liquid 302 due to its own weight, so that the ineffective layers 10a, 10b can be aligned vertically in a predetermined relationship, i.e., the stacking direction D100 can be aligned with the predetermined direction Dv. This configuration is suitable for a mass production line. In the embodiment, the predetermined direction Dv is the vertical direction. The step of aligning the stacking direction D100 with the predetermined direction Dv may be performed after the plating step.

[0034] The manufacturing apparatus 300 may further include a magnet 303 provided in the storage tank 301. When the internal electrodes 11, 12 contain a magnetic metal such as Ni, the thin ineffective layer 10a configured to face the mounting surface 200 is attracted to the magnet 303 as the magnet 303 approaches the varistor 100. It is therefore possible to set the upper and lower relationship of the ineffective layers 10a, 10b to a predetermined relationship. In addition to the magnet 303, it is also possible to add a step of applying a magnetic field M3 to the varistor 100 in the liquid 302. This step can be easily introduced into a mass production process, so the varistor 100 of this embodiment is suitable for mass production.

[0035] The liquid 302 is not limited to a plating liquid, and the above process can be carried out with other liquids, so the above process can also be applied to varistors 100 that have not been plated.

[0036] Moreover, the magnetic field M3 can be applied not only in the liquid 302 but also in a gaseous state while applying vibrations, thereby making it possible to set the upper and lower relationship of the ineffective layers 10a, 10b to a predetermined relationship.

[0037] By making the thickness Tb of the ineffective layer 10b at least twice the thickness Ta of the ineffective layer 10a, the position of the effective layer 10c is biased from the center toward the ineffective layer 10a, and the position of the center of gravity 100g is also biased, which makes it easier to align the stacking direction D100 in the manufacturing process, and is therefore more preferable.

[0038] Zinc oxide varistors are ceramic polycrystalline bodies made by adding additives such as bismuth and praseodymium to zinc oxide and sintering them. When aiming to protect against surges with a large amount of energy, the expected effect could not be obtained by making the element larger and expanding the area of ​​the internal electrodes. It is difficult to achieve good surge resistance in the large current range with conventional varistors.

[0039] As described above, the varistor 100 in the embodiment is small and has good surge resistance. [Explanation of symbols]

[0040] 10 Base 10a Ineffective layer (first ineffective layer) 10b Ineffective layer (second ineffective layer) 10c Effective layer 10d Ceramic layer 11 Internal electrode 12 Internal electrode 13 External electrode 14 External electrode 100 Barista 302 liquid 303 Magnet M3 magnetic field

Claims

1. one or more ceramic layers; a plurality of internal electrodes, each of which includes a magnetic metal and is laminated alternately with the one or more ceramic layers; an active layer having opposed first and second surfaces, a first ineffective layer laminated in a lamination direction on the first surface of the effective layer; obtaining a sintered body comprising a second ineffective layer laminated on the second surface of the effective layer in a direction opposite to the lamination direction, the second ineffective layer having a thickness of 1.1 times or more and 6 times or less than the thickness of the first ineffective layer; forming an external electrode provided on an end surface of the sintered body and electrically connected to one of the plurality of internal electrodes; positioning the sintered body so that the lamination direction is a predetermined direction; plating the external electrodes in a plating solution; Including, A method for manufacturing a varistor, wherein the step of positioning the sintered body includes a step of applying a magnetic field to the sintered body while the sintered body is immersed in the plating solution, thereby aligning the stacking direction to the predetermined direction.

2. The method for manufacturing a varistor according to claim 1 , wherein the step of setting the lamination direction to the predetermined direction is performed after the step of plating.

3. The step of obtaining the sintered body includes: Obtaining a ceramic raw material powder having a polycrystalline structure; preparing a slurry containing the raw material powder and an organic solvent; applying the slurry onto a film to obtain a plurality of green sheets; A step of laminating the plurality of green sheets and a plurality of electrode pastes each including an electrode paste that becomes the plurality of internal electrodes to obtain a laminate; sintering the laminate to obtain the sintered body; A method for producing the varistor according to claim 1, comprising:

4. The step of forming the external electrodes includes: applying a metal paste to the sintered body; subjecting the applied metal paste to a heat treatment; A method for producing the varistor according to claim 1, comprising:

Citation Information

Patent Citations

  • JP1987124835U

  • Manufacture of pin head diode

    JP1988222451A

  • Oriented zinc oxide powder and its manufacture

    JP1992325413A

  • Chip type varistor and its manufacture

    JP1998172809A

  • Transport arrangement device of electronic component and transport arrangement method of electronic component

    JP2018098413A