Method for manufacturing a positive electrode mixture for flat lithium primary battery, and flat lithium primary battery

By using fluorocarbon resin particles in the positive electrode mixture, the battery maintains electrical connection and performance at high temperatures, addressing the issue of case expansion and resistance increase.

JP7565528B2Active Publication Date: 2024-10-11PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023506869
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-03-17
Filing Date
2022-02-10
Publication Date
2024-10-11
Estimated Expiration
2042-02-10

AI Technical Summary

Technical Problem

Flat lithium primary batteries experience deterioration in electrical connection and characteristics at high temperatures due to case expansion from internal gas generation, leading to increased resistance and reduced performance.

Method used

Incorporating fluorocarbon resin particles with swelling properties into the positive electrode mixture, maintaining electrical connection by absorbing electrolyte and expanding uniformly with the case, while ensuring a particle size range of 10 to 200 μm and content of 0.2 to 6 parts by mass relative to the positive electrode active material.

Benefits of technology

The battery maintains high characteristics and electrical connectivity even at high temperatures, suppressing deterioration and ensuring prolonged discharge times.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007565528000002
    Figure 0007565528000002
  • Figure 0007565528000001
    Figure 0007565528000001
Patent Text Reader

Abstract

The disclosed flat lithium primary battery includes: a case; and, a positive electrode, a negative electrode, a separator, and a non-aqueous electrolytic solution disposed within the case. The positive electrode includes a positive-electrode active material and a fluorocarbon resin having swelling properties with respect to the non-aqueous electrolytic solution. In the positive electrode, the fluorocarbon resin exists in a particulate state. When the flat lithium primary battery placed in a 25°C environment was subjected to a high-temperature storage test involving storage in a 125°C environment for 100 hours, the ratio d2 / d1 of the particle diameter d2 of the fluorocarbon resin after the high-temperature storage test to the particle diameter d1 of the fluorocarbon resin before the high-temperature storage test is 1.5 to 3.1, inclusive.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a positive electrode mixture for a flat lithium primary battery, and to a flat lithium primary battery. [Background technology]

[0002] Flat lithium primary batteries are characterized by their high energy density and high voltage, and therefore have been used as power sources for a variety of electronic devices.

[0003] Various flat lithium primary batteries have been proposed. For example, Patent Document 1 discloses a lithium battery using lithium as the negative electrode active material, in which manganese dioxide is used as the positive electrode active material and a mixture of carbon black and graphite is used as a conductive assistant. The positive electrode of the lithium battery is produced by, for example, forming the positive electrode mixture into a sheet by pressure molding, which is prepared by adding a conductive assistant to manganese dioxide, which is the positive electrode active material, and further adding and mixing a binder (polytetrafluoroethylene, polyvinylidene fluoride, etc.) as necessary. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Publication No. 8-106903 Summary of the Invention

[0005] In recent years, non-aqueous electrolyte batteries are used in high-temperature environments. For example, lithium primary batteries are used as power sources for sensors in tire pressure monitoring systems (TPMS). In such cases, the temperature of the battery may reach 100° C. or higher (e.g., 125° C. or higher). When a non-aqueous electrolyte battery is used at such high temperatures, the battery case may expand due to gas generated inside the battery case. Similarly, when a non-aqueous electrolyte battery is stored at high temperatures, the battery case may expand.

[0006] When the battery case expands as described above, the electrical connection between the components constituting the battery becomes insufficient, and the battery characteristics may deteriorate. For example, the resistance between the positive electrode and the positive electrode case (or the current collector) may increase, and the battery characteristics may deteriorate.

[0007] As a result of intensive research, the present inventors have newly discovered that a flat lithium primary battery capable of maintaining high characteristics even at high temperatures can be obtained by adding a specific polymer to the positive electrode. The present invention is based on this new discovery.

[0008] In view of the above, one aspect of the present invention relates to a method for producing a positive electrode mixture for a flat lithium primary battery, the method comprising: obtaining a positive electrode mixture by mixing a material including particles of a fluorocarbon resin having a property of swelling in an electrolytic solution and particles of a positive electrode active material, the average particle size of the fluorocarbon resin being in the range of 10 to 200 μm, a content of the fluorocarbon resin in the material being in the range of 0.2 to 6 parts by mass per 100 parts by mass of the positive electrode active material, and the fluorocarbon resin being present in a particulate state in the positive electrode mixture.

[0009] Another aspect of the present invention relates to a flat lithium primary battery including a case, and a positive electrode, a negative electrode, a separator, and a non-aqueous electrolyte solution disposed within the case, wherein the positive electrode includes a positive electrode active material and a fluorocarbon resin having a property of swelling with the non-aqueous electrolyte solution, the fluorocarbon resin is present in a particulate state within the positive electrode, and when the flat lithium primary battery is placed in an environment of 25° C. and subjected to a high-temperature storage test in which the battery is stored in an environment of 125° C. for 100 hours, a ratio d2 / d1 of a particle size d2 of the fluorocarbon resin after the high-temperature storage test to a particle size d1 of the fluorocarbon resin before the high-temperature storage test is in the range of 1.5 or more and 3.1 or less.

[0010] According to the present invention, a flat lithium primary battery capable of maintaining high characteristics even at high temperatures can be obtained. [Brief description of the drawings]

[0011] [Figure 1] 1 is a schematic cross-sectional view of a configuration of an example of a lithium primary battery according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Hereinafter, an embodiment of the present invention will be described. In the following description, an embodiment of the present invention will be described by way of example, but the present invention is not limited to the example described below. In the following description, specific numerical values ​​and materials may be exemplified, but other numerical values ​​and materials may be applied as long as the effects of the present invention can be obtained.

[0013] The flat lithium primary battery according to the present invention is realized, for example, by using a positive electrode mixture for a flat lithium primary battery produced by the method described below. Hereinafter, the "positive electrode mixture for a flat lithium primary battery" may be simply referred to as a "positive electrode mixture." Furthermore, the "flat lithium primary battery" may be simply referred to as a "lithium primary battery."

[0014] (Method of manufacturing positive electrode mixture for flat lithium primary batteries) A method for producing a positive electrode mixture for a flat lithium primary battery according to one embodiment of the present invention includes a step of obtaining a positive electrode mixture by mixing a material including particles of a fluorocarbon resin having a swelling property in an electrolyte and particles of a positive electrode active material. In the step of obtaining the positive electrode mixture, the average particle size of the fluorocarbon resin is in the range of 10 to 200 μm, and the content of the fluorocarbon resin relative to 100 parts by mass of the positive electrode active material is in the range of 0.2 to 6 parts by mass. In the step of obtaining the positive electrode mixture, the fluorocarbon resin is allowed to remain in a particulate state in the positive electrode mixture.

[0015] In the positive electrode mixture obtained by such a manufacturing method, the fluorocarbon resin is dispersed in a particulate state. By obtaining a flat lithium primary battery positive electrode (hereinafter, sometimes simply referred to as a "positive electrode") using such a positive electrode mixture, a lithium primary battery capable of maintaining high characteristics even at high temperatures can be realized.

[0016] Fluorocarbon resins are generally used as binders (binding agents) that maintain the binding between particles of the positive electrode active material in the positive electrode. However, in this embodiment, the property of fluorocarbon resins that swells in an electrolyte solution is utilized. A fluorocarbon resin that swells in an electrolyte solution may also function as a binder, and may not function as a binder. Here, "fluorocarbon resins swell in an electrolyte solution" means that the particle size increases when particles of the fluorocarbon resin are immersed in an electrolyte solution for a certain period of time. In particular, a specific fluorocarbon resin has a large swelling property in an electrolyte solution at high temperatures (e.g., 60°C or higher), and an extremely large swelling property in an electrolyte solution at even higher temperatures (e.g., 100°C or higher). In addition, a fluorocarbon resin that has swelled once in a high-temperature environment maintains the swollen state (state in which the particle size is large) even when it is returned to room temperature.

[0017] When using a fluorocarbon resin as a binder, the fluorocarbon resin particles and the positive electrode active material particles are usually mixed in a liquid to form a positive electrode mixture into a disk-shaped pellet, and then the pellet is dried to remove the liquid to manufacture a positive electrode. A solvent that dissolves the fluorocarbon resin, such as N-methyl-2-pyrrolidone (NMP), is used as the liquid. Alternatively, a fluorocarbon resin having an average particle size sufficiently smaller (for example, 1 μm or less) than the average particle size of the positive electrode active material is used. In these cases, the fluorocarbon resin adheres or precipitates in the positive electrode so as to cover the surface of the particles of the positive electrode active material. In contrast, in this embodiment, the fluorocarbon resin is dispersed in the positive electrode in the form of particles having an average particle size of 10 μm or more.

[0018] In the following description, unless otherwise specified, the fluorocarbon resin refers to a fluorocarbon resin that has swelling properties in an electrolyte solution, and when referring to a fluorocarbon resin that does not have swelling properties, this will be clearly stated.

[0019] The fluorocarbon resin contained in the positive electrode using the positive electrode mixture produced by the method of this embodiment is particulate and is in contact with the surface of the positive electrode active material particles at points. At high temperatures, when the battery case expands due to generated gas, the fluorocarbon resin absorbs the electrolyte and swells, increasing the particle size. As a result, the positive electrode expands following the expansion of the case, and the adhesion between the case and the positive electrode is maintained. On the other hand, since the particles of the positive electrode active material have a large surface area and fine irregularities, when the positive electrode expands, the particles of the fluorocarbon resin increase in particle size while engaging with the irregularities of the positive electrode active material. The fluorocarbon resin expands while maintaining the state of engaging with the irregularities of the positive electrode active material, so that the entire positive electrode expands uniformly, and the positive electrode expands while maintaining the conductive path between the positive electrode active materials. As a result, even when the case expands at high temperatures, the electrical connection between the case and the positive electrode is maintained, and high characteristics are maintained.

[0020] In the process of obtaining a positive electrode mixture, the average particle size of the fluorocarbon resin particles mixed with the positive electrode active material particles is in the range of 10 to 200 μm. When the average particle size of the fluorocarbon resin particles is 10 μm or more, the fluorocarbon resin particles swell at high temperatures, thereby maintaining the electrical connection between the case and the positive electrode, and the effect of maintaining high battery characteristics is exhibited. On the other hand, the larger the particle size of the fluorocarbon resin, the fewer the contact points (engagement points) between the fluorocarbon resin and the positive electrode active material, and the fluorocarbon resin is more likely to expand uniquely by itself, and the conductive path between the positive electrode active materials is more likely to be cut. However, when the average particle size of the fluorocarbon resin particles is 200 μm or less, the positive electrode is more likely to expand while maintaining the conductive path between the positive electrode active materials as the fluorocarbon resin particles swell.

[0021] In order to enhance the effect of maintaining the electrical connection between the case and the positive electrode by expanding the positive electrode while maintaining the conductive path between the positive electrode active materials, the average particle size of the fluorocarbon resin particles in the step of obtaining the positive electrode mixture is preferably 30 μm or more, and more preferably 70 μm or more. In order to easily maintain the conductive path between the positive electrode active materials when the positive electrode expands, the average particle size of the fluorocarbon resin particles in the step of obtaining the positive electrode mixture is preferably 140 μm or less.

[0022] The average particle size of the fluorocarbon resin particles in the step of obtaining the positive electrode mixture is preferably in the range of 30 to 200 μm, and more preferably in the range of 70 to 200 μm or 70 to 140 μm.

[0023] The average particle size of the fluorocarbon resin particles in the production of the positive electrode mixture means the median diameter D50 on a volume basis, and can be measured by a laser diffraction type particle size distribution measuring device.

[0024] The fluorocarbon resin may be a polymer containing vinylidene fluoride units. High effects can be obtained by including a polymer containing vinylidene fluoride units in a particulate state in the positive electrode mixture. Examples of polymers containing vinylidene fluoride units include copolymers of vinylidene fluoride and other monomers. Examples of other monomers include hexafluoropropylene (HFP) and tetrafluoroethylene (TFE). The proportion of vinylidene fluoride units in all monomer units is preferably in the range of 50 to 100 mol%, and more preferably in the range of 75 to 100 mol%.

[0025] Examples of fluorocarbon resins containing vinylidene fluoride units include polyvinylidene fluoride (PVDF) and its modified products, vinylidene fluoride-hexafluoropropylene copolymers, vinylidene fluoride-chlorotrifluoroethylene copolymers, and vinylidene fluoride-pentafluoropropylene copolymers.

[0026] The most preferable fluorocarbon resin is polyvinylidene fluoride (PVDF). Polyvinylidene fluoride (PVDF) has high swelling properties, and by adding fluorocarbon resin particles to the positive electrode active material particles, a particularly high effect can be obtained.

[0027] The swelling property of the fluorocarbon resin in the electrolyte solution is evaluated, for example, by the following method.

[0028] First, a fluorocarbon resin was used to create a film with a thickness of 1.5 mm (density 1.78 g / cm 3) is formed, and the film is immersed in an electrolyte at 60°C for 24 hours or more. The swelling property can be evaluated by comparing the mass W1 of the film before immersion with the mass W2 of the film after immersion. The swelling ratio is expressed as swelling ratio (%) = 100 x (W2 - W1) / W1. The fluorocarbon resin preferably has a swelling ratio of 20% or more (in the range of 30 to 50%).

[0029] The content of the swellable fluorocarbon resin in the positive electrode mixture is in the range of 0.2 to 6 parts by mass per 100 parts by mass of the positive electrode active material, and may be in the range of 0.4 to 4 parts by mass (for example, 1 to 4 parts by mass or 2 to 3 parts by mass) per 100 parts by mass of the positive electrode active material.

[0030] The weight average molecular weight (mass average molecular weight) of the fluorocarbon resin may be, for example, in the range of 100,000 to 1.5 million. The weight average molecular weight of the fluorocarbon resin can be measured, for example, by gel permeation chromatography (GPC). The weight average molecular weight may be in the range of 400,000 to 1.5 million (for example, in the range of 500,000 to 1.5 million, the range of 800,000 to 1.2 million, or the range of 1 million to 1.2 million).

[0031] The mixture of the fluorocarbon resin particles and the positive electrode active material particles is molded into a disk-shaped pellet by, for example, press molding, to obtain a flat lithium primary battery positive electrode (hereinafter, sometimes simply referred to as a "positive electrode"). To facilitate molding, the positive electrode mixture may be obtained by mixing the fluorocarbon resin particles, the positive electrode active material particles, and a liquid. That is, the material of the positive electrode mixture may contain a liquid. After molding, at least a part of the liquid may be evaporated as necessary to obtain a positive electrode. The liquid used is one that does not dissolve the fluorocarbon resin (the fluorocarbon resin has low swelling property in the liquid). The liquid is, for example, water.

[0032] The positive electrode active material typically consists of only manganese dioxide, and therefore, in a typical example, in this specification, the "positive electrode active material" can be read as "manganese dioxide."

[0033] The positive electrode active material has a BET specific surface area A (m 2 The ratio A / B of the BET specific surface area A (m 2 / g) is measured by the BET method. Nitrogen gas is used as the gas used in the BET method. The average particle size B (μm) means the median diameter D50 on a volume basis, and is measured by a laser diffraction type particle size distribution measuring device. When the ratio A / B is within the above range, the specific surface area of ​​the positive electrode active material is appropriately large, and the surface has appropriate unevenness. Therefore, the positive electrode is likely to expand while maintaining a conductive path between the positive electrode active material, and even when the case expands at high temperatures, the electrical connection between the case and the positive electrode can be maintained, making it easy to maintain high battery characteristics.

[0034] In another aspect, the present invention provides a positive electrode mixture and a positive electrode using the same. The positive electrode mixture and the positive electrode using the same each contain particles of a fluorocarbon resin having swelling properties in an electrolyte and particles of a positive electrode active material, the average particle size of the fluorocarbon resin being in the range of 10 to 200 μm, and the content of the fluorocarbon resin relative to 100 parts by mass of the positive electrode active material being in the range of 0.2 to 6 parts by mass. The positive electrode mixture can be manufactured by the manufacturing method of the present embodiment described above, and therefore the matters described in the manufacturing method of the present embodiment can be applied to the positive electrode mixture and the positive electrode. Therefore, overlapping descriptions will be omitted.

[0035] In another aspect, the present invention provides a method for manufacturing a positive electrode. The method for manufacturing a positive electrode according to one embodiment of the present invention includes a step of obtaining a positive electrode mixture and a step of forming a positive electrode using the obtained positive electrode mixture. The step of obtaining a positive electrode mixture has been described above, so a duplicated description will be omitted. There is no particular limitation on the step of forming a positive electrode, and a known method may be used. For example, the positive electrode may be formed by forming the positive electrode mixture into a disk-shaped pellet and then drying the pellet as necessary.

[0036] (Flat lithium primary battery) A flat lithium primary battery according to one embodiment of the present invention includes a case, a positive electrode, a negative electrode, a separator, and a non-aqueous electrolyte, which are disposed in the case. The positive electrode and the negative electrode face each other with the separator interposed therebetween. The positive electrode includes a positive electrode active material and a fluorocarbon resin having swelling properties with respect to the non-aqueous electrolyte. In the positive electrode, the fluorocarbon resin exists in a particulate state. The positive electrode may be formed using the positive electrode mixture of this embodiment. Therefore, the matters described regarding the positive electrode mixture may be applied to the positive electrode of the battery of this embodiment. For example, the average particle size of the fluorocarbon resin particles and the ratio of the positive electrode active material to the fluorocarbon resin may be within the above-mentioned range. However, they may change depending on the change over time or the temperature of the surrounding environment. For example, the average particle size of the fluorocarbon resin particles may increase depending on the change over time or the temperature of the surrounding environment.

[0037] When a flat lithium primary battery is subjected to a high-temperature storage test in which the flat lithium primary battery is placed in a 25°C environment and stored in a 125°C environment for 100 hours, the ratio d2 / d1 of the particle size d2 of the fluorocarbon resin after the high-temperature storage test to the particle size d1 of the fluorocarbon resin before the high-temperature storage test is 1.5 to 3.1. A lithium primary battery that satisfies these conditions can maintain high characteristics even at high temperatures.

[0038] The high-temperature storage test can be performed under the following conditions. First, the battery to be measured is placed in the state it was in before the high-temperature storage test. Specifically, the battery is placed in a 25°C environment for 2 hours. Next, the high-temperature storage test is started. Specifically, the battery is moved to a 125°C environment (for example, an air atmosphere in a thermostatic chamber set at 125°C) and left in that environment for 100 hours. In this manner, the high-temperature storage test can be performed.

[0039] In a lithium primary battery, the particle size of the fluorocarbon resin in the positive electrode before the high-temperature storage test is defined as d1. It is assumed that a lithium primary battery has not been intentionally exposed to a high-temperature environment unless its case is expanded. Therefore, the particle size d1 at that time can be regarded as the particle size before the high-temperature storage test.

[0040] When a lithium primary battery is placed in a high-temperature environment, as described above, the fluorocarbon resin absorbs the electrolyte, swells, and the particle size increases. The particle size of the fluorocarbon resin after the high-temperature storage test is d2 (d2>d1). When the ratio d2 / d1 is 1.5 or more and 3.1 or less, the fluorocarbon resin particles swell appropriately in a high-temperature environment, suppressing the deterioration of battery characteristics at high temperatures.

[0041] In addition, when the flat lithium primary battery according to one embodiment of the present invention is placed in a high-temperature (e.g., 125°C or higher) atmosphere for a long time, the particles of the fluorocarbon resin in the positive electrode swell. The particle size of the fluorocarbon resin particles once swollen does not return to the initial particle size even if the temperature of the battery drops. Therefore, even if the battery uses the positive electrode mixture of this embodiment, when the battery is placed in a high-temperature (e.g., 125°C or higher) environment for a long time and then subjected to the above-mentioned high-temperature storage test (storage at 125°C for 100 hours), the ratio d2 / d1 may not be 1.5 or more and 3.1 or less. That is, even if the ratio d2 / d1 is out of the range of 1.5 or more and 3.1 or less, it does not necessarily mean that the positive electrode mixture of this embodiment is not used. However, if the ratio d2 / d1 is 1.5 or more and 3.1 or less, it can be said that the flat lithium primary battery according to one embodiment of the present invention is a flat lithium primary battery. For example, if the battery using the positive electrode mixture of this embodiment is not intentionally heated from the time of manufacture to the high-temperature storage test, the ratio d2 / d1 is generally considered to be 1.5 to 3.1. For example, if the temperature of the battery using the positive electrode mixture of this embodiment is kept at 35° C. or less from the time of manufacture to the high-temperature storage test, and the high-temperature storage test is performed within 12 months from the time of manufacture of the battery, the ratio d2 / d1 is generally considered to be 1.5 to 3.1.

[0042] The ratio d2 / d1 is preferably 1.5 or more and 2.4 or less, more preferably 1.7 or more and 2.0 or less. When the ratio d2 / d1 is in this range, the effect of suppressing the deterioration of the battery characteristics at high temperatures is remarkable. The fluorocarbon resin may be the one described above in the manufacturing method of the positive electrode mixture.

[0043] The positive electrode includes a positive electrode active material. The positive electrode active material has a BET specific surface area A (m 2 The ratio A / B of the particle diameter (A / g) to the average particle diameter B (μm) may be 0.25 to 1.5.

[0044] The average particle size of the positive electrode active material and the particle sizes d1 and d2 of the fluorocarbon resin are determined by analyzing the cross section of the positive electrode or the powder of the positive electrode mixture with an electron probe microanalyzer (EPMA) or micro-Raman spectroscopy. The area occupied by the particle in the cross section from the grain boundaries of the particles of the positive electrode active material and the particles of the fluorocarbon resin is determined, and the diameter of a circle (equivalent circle) having an area equal to that area is defined as the particle size of the particle. The particle sizes of multiple particles (e.g., 10 or more) are determined, and the average value is defined as the average particle size of the positive electrode active material and the particle sizes d1 and d2 of the fluorocarbon resin.

[0045] The non-aqueous electrolyte may contain dimethoxyethane (DME) as a solvent. In this case, the content ratio of the dimethoxyethane in the solvent of the non-aqueous electrolyte may be 50% by volume or more. Since dimethoxyethane has a small specific gravity, the volume occupied by the electrolyte increases when the weight is the same. This allows the amount of electrolyte swelling in the fluorocarbon resin to be increased, which contributes to suppressing the deterioration of battery characteristics at high temperatures.

[0046] The shape of the case of the lithium primary battery (i.e., the shape of the battery) is generally flat. The case may be, for example, a flat rectangular shape or a coin shape (including a button shape). When the lithium primary battery of the present embodiment is a coin-shaped lithium primary battery using a coin-shaped case, typically, the positive electrode and the negative electrode are each disk-shaped.

[0047] The case may include a positive electrode case that functions as a positive electrode terminal, a sealing plate that functions as a negative electrode terminal, and a gasket disposed between the positive electrode case and the sealing plate. The gasket may contain polyphenylene sulfide (e.g., the polyphenylene sulfide content is 50 mass% or more) or may be made of polyphenylene sulfide.

[0048] There is no particular limitation on the material of the gasket, and materials generally used for gaskets can be used. Examples of gasket materials include resins such as polypropylene (PP), polyphenylene sulfide (PPS), perfluoroalkoxyalkane (PFA), and polyetheretherketone (PEEK). Among these, PPS is characterized by high heat resistance and rigidity. Therefore, PPS is preferable as a gasket material when a lithium primary battery is used at high temperatures. On the other hand, when a gasket containing PPS is used, the internal pressure of the case may easily increase when the lithium primary battery is used at high temperatures. Therefore, by using a gasket containing PPS and the positive electrode of this embodiment, a lithium primary battery with particularly small deterioration in characteristics at high temperatures can be obtained.

[0049] In order to prevent the expansion of the case due to use of the battery at high temperatures, it is possible to make the case thicker. However, there is a problem in that a thick case is difficult to mold. Therefore, it is difficult to prevent the case from expanding to a certain extent. According to this embodiment, high characteristics can be maintained even in the case where the case expands.

[0050] The lithium primary battery of this embodiment is unlikely to deteriorate in characteristics even in a high-temperature environment, and therefore can be preferably used in applications where use in a high-temperature environment is expected. The lithium primary battery may be a coin battery mounted in a tire. As a system for monitoring tire air pressure and the like in a vehicle, a tire pressure monitoring system (TPMS) or a tire monitoring system (TMS) is known. In one example of a TPMS, a sensor for detecting tire air pressure and the like is attached inside a tire or a tire wheel, and information such as air pressure is transmitted to the vehicle body side in a timely manner. The lithium primary battery of this embodiment can be preferably used as a power source for operating the sensor and / or transmitting sensor information.

[0051] The configuration of the lithium primary battery according to one embodiment of the present invention will be described more specifically below.

[0052] (positive electrode) The positive electrode includes a positive electrode active material and the above-mentioned fluorocarbon resin. The fluorocarbon resin is added to the positive electrode to suppress deterioration of battery characteristics at high temperatures. The positive electrode may further include other substances (such as known substances used in the positive electrodes of general lithium primary batteries). The positive electrode usually includes a binder and a conductive agent. The binder may include a non-swellable fluorocarbon resin, or a swellable fluorocarbon resin may also serve as the binder.

[0053] Examples of binders include fluorocarbon resins such as polytetrafluoroethylene (PTFE), perfluoroalkoxyalkane (PFA), perfluoroethylenepropene copolymer (FEP), and ethylene-tetrafluoroethylene copolymer (ETFE). These are substantially not swollen by the non-aqueous electrolyte used in lithium primary batteries, but the strength of the positive electrode (positive electrode pellet) can be increased by using these binders. Other binders include rubber particles, acrylic resins, and the like. Examples of conductive agents include carbon-based materials such as graphite and carbon black (e.g., Ketjen black).

[0054] The mass of the binder contained in the positive electrode may be in the range of 1.2 to 6% (for example, in the range of 1.5 to 3%) of the mass of the positive electrode active material contained in the positive electrode. By containing a binder in this range, the formation of the positive electrode becomes easier, and in particular mass productivity is improved. In the positive electrode, the mass ratio of the binder to the fluorocarbon resin having swelling properties in the electrolyte may be in the range of 1:0.1 to 3 (for example, in the range of 1:0.2 to 2).

[0055] The positive electrode active material contained in the positive electrode includes manganese dioxide. A positive electrode containing manganese dioxide exhibits a relatively high voltage and has excellent pulse discharge characteristics. The manganese dioxide may be in a mixed crystal state including a plurality of crystal states. The positive electrode may contain manganese oxide other than manganese dioxide. Examples of manganese oxide other than manganese dioxide include MnO, Mn3O4, Mn2O3, and Mn2O7. It is preferable that the main component of the manganese oxide contained in the positive electrode is manganese dioxide.

[0056] A part of the manganese dioxide contained in the positive electrode may be doped with lithium. If the amount of lithium doped is small, a high capacity can be ensured. Manganese dioxide and manganese dioxide doped with a small amount of lithium are Li x MnO2 (0≦x≦0.05). The average composition of the manganese oxide in the positive electrode is Li x MnO2 (0≦x≦0.05). The Li ratio x generally increases as the discharge of a lithium primary battery progresses. The Li ratio x should be 0.05 or less in the initial discharge state of the lithium primary battery.

[0057] The positive electrode may contain other positive electrode active materials used in lithium primary batteries. Examples of other positive electrode active materials include graphite fluoride. The percentage of Li in the total positive electrode active material is x The proportion of MnO2 may be 90 mass % or more.

[0058] As the manganese dioxide, electrolytic manganese dioxide is preferably used. If necessary, electrolytic manganese dioxide that has been subjected to at least one of neutralization, washing, and calcination may be used. Electrolytic manganese dioxide is generally obtained by electrolysis of an aqueous manganese sulfate solution.

[0059] By adjusting the conditions during electrolytic synthesis, the crystallinity of manganese dioxide can be increased and the specific surface area of ​​electrolytic manganese dioxide can be reduced. x The BET specific surface area of ​​MnO2 is 10m 2 / g or more 50m 2 / g or less, 2 / g or more 30m 2 / g or less. x The BET specific surface area of ​​MnO2 may be measured by a known method, for example, based on the BET method using a specific surface area measuring device (for example, manufactured by Mountec Co., Ltd.). For example, LixMnO2 separated from the positive electrode taken out of the battery may be used as a measurement sample.

[0060] Positive electrode active material Li x The average particle size (median size D50) of MnO2 may be, for example, 20 to 40 μm. x Li relative to the average particle size of MnO2 (μm) x BET specific surface area of ​​MnO2 (m 2 / g) may be 0.25 to 1.5 in order to suppress deterioration of characteristics at high temperatures.

[0061] There is no particular limitation on the components other than the positive electrode (negative electrode, separator, non-aqueous electrolyte, case, etc.), and the battery may include components other than the above components (for example, a current collector). The components other than the positive electrode may be known components used in general lithium primary batteries. Examples of the components other than the positive electrode are described below.

[0062] (Negative electrode) The negative electrode contains at least one selected from the group consisting of metallic lithium and a lithium alloy as a negative electrode active material. The negative electrode may contain metallic lithium or a lithium alloy, or may contain both metallic lithium and a lithium alloy. For example, a composite containing metallic lithium and a lithium alloy may be used for the negative electrode.

[0063] The lithium alloy is not particularly limited, and an alloy used as a negative electrode active material of a lithium primary battery can be used. Examples of the lithium alloy include Li-Al alloy, Li-Sn alloy, Li-Ni-Si alloy, and Li-Pb alloy. The content of metal elements other than lithium contained in the lithium alloy is preferably 0.05 to 15 mass % from the viewpoint of ensuring discharge capacity and stabilizing internal resistance.

[0064] (Separator) A lithium primary battery usually includes a separator interposed between a positive electrode and a negative electrode. As the separator, a porous sheet formed of an insulating material having resistance to the internal environment of a lithium primary battery may be used. Specifically, a synthetic resin nonwoven fabric, a synthetic resin microporous film, or a laminate thereof may be used.

[0065] Examples of synthetic resins used for nonwoven fabrics include polypropylene, polyphenylene sulfide, polybutylene terephthalate, etc. Examples of synthetic resins used for microporous membranes include polyolefin resins such as polyethylene, polypropylene, and ethylene-propylene copolymers, etc. The microporous membrane may contain inorganic particles as necessary.

[0066] (electrolyte) The electrolyte is not particularly limited, and a non-aqueous electrolyte commonly used in lithium primary batteries may be used. For example, the electrolyte may be a non-aqueous electrolyte in which a lithium salt or lithium ions are dissolved in a non-aqueous solvent.

[0067] The non-aqueous solvent may be an organic solvent that can be generally used in non-aqueous electrolytes for lithium primary batteries. The non-aqueous solvent may be an ether, an ester, a carbonate ester, or the like. The non-aqueous solvent may be dimethyl ether, γ-butyl lactone, propylene carbonate, ethylene carbonate, 1,2-dimethoxyethane, or the like. The non-aqueous electrolyte may contain one type of non-aqueous solvent, or may contain two or more types of non-aqueous solvents.

[0068] From the viewpoint of improving the discharge characteristics of the lithium primary battery, the non-aqueous solvent preferably contains a cyclic carbonate having a high boiling point and a chain ether having a low viscosity even at low temperatures. The cyclic carbonate preferably contains at least one selected from the group consisting of propylene carbonate (PC) and ethylene carbonate (EC), and PC is particularly preferred. The chain ether preferably has a viscosity of 1 mPa·s or less at 25°C, and particularly preferably contains dimethoxyethane (DME). The viscosity of the non-aqueous solvent is measured at 25°C and a shear rate of 10,000 (1 / s) using a microsample viscometer m-VROC manufactured by Rheosens.

[0069] The non-aqueous electrolyte may contain a lithium salt other than the cyclic imide component. Examples of the lithium salt include lithium salts used as solutes in lithium primary batteries. Examples of such lithium salts include LiCF3SO3, LiN(CF3SO2)2, LiClO4, LiBF4, LiPF6, LiR a SO3(R a is a fluoroalkyl group having 1 to 4 carbon atoms), LiFSO3, LiN(SO2R b )(SO2R c )(R b and R c are each independently a fluoroalkyl group having 1 to 4 carbon atoms), LiN(FSO2)2, LiPO2F 2、 LiB(C2O4)2, LiBF2(C2O4). The non-aqueous electrolyte may contain one or more of these lithium salts.

[0070] The concentration of lithium ions contained in the electrolyte (total concentration of lithium salts) is, for example, 0.2 to 2.0 mol / L, and may be 0.3 to 1.5 mol / L.

[0071] The electrolyte may contain additives as necessary. Examples of such additives include propane sultone, vinylene carbonate, etc. The total concentration of such additives contained in the non-aqueous electrolyte is, for example, 0.003 to 5 mol / L.

[0072] The positive electrode case can be made of, for example, electrically conductive stainless steel.

[0073] The cross-sectional view of Fig. 1 shows an example of the configuration of a lithium primary battery (coin type or button type) of this embodiment. The lithium primary battery 10 of Fig. 1 includes a positive electrode 11, a separator 12, a negative electrode 13, and a case 20. The case 20 includes a positive electrode case 21 that functions as a positive electrode terminal, a sealing plate 22 that functions as a negative electrode terminal, and a gasket 23 disposed between the positive electrode case 21 and the sealing plate 22. The positive electrode 11 and the negative electrode 13 face each other with the separator 12 interposed therebetween. The positive electrode 11 includes a positive electrode active material and a fluorocarbon resin (not shown), and the fluorocarbon resin is present in a particulate state within the positive electrode.

[0074] A positive electrode 11, a separator 12, a negative electrode 13, a gasket 23, and a non-aqueous electrolyte (not shown) are arranged between the positive electrode case 21 and a sealing plate 22, and the positive electrode case 21 is sealed by bending the upper part of the positive electrode case 21 inward and crimping it. EXAMPLES

[0075] The lithium primary battery of this embodiment will be described in more detail with reference to the following examples, although the present invention is not limited to the following examples.

[0076] 《Batteries A1~A6, B1~B5》 (1) Preparation of the positive electrode A positive electrode mixture was prepared by mixing electrolytic manganese dioxide, graphite (conductive agent), PVDF (carbon fluoride resin), and PTFE (average particle size 0.25 μm) in a mass ratio of manganese dioxide:graphite:PVDF:PTFE=100:5:2:2. That is, the ratio of PVDF contained in the positive electrode mixture (positive electrode) was 2 parts by mass per 100 parts by mass of manganese dioxide (positive electrode active material).

[0077] The PVDF used was powdered PVDF manufactured by SOLVAY. The weight average molecular weight of the PVDF was 1 million. The weight average molecular weight value was measured by GPC. The PVDF used had an average particle size (median diameter D50 on a volume basis) shown in Table 1.

[0078] The positive electrode mixture was molded to obtain a disk-shaped pellet (positive electrode) having a diameter of 15 mm and a thickness of 2.0 mm. In this way, a disk-shaped positive electrode was formed.

[0079] (2) Preparation of the negative electrode A disk-shaped negative electrode having a diameter of 16 mm and a thickness of 1.0 mm was obtained by punching out a plate of metallic lithium.

[0080] (3) Preparation of non-aqueous electrolyte Propylene carbonate (PC) and 1,2-dimethoxyethane (DME) were mixed in a volume ratio of 1:1 to obtain a non-aqueous solvent. Lithium perchlorate (LiClO4) was dissolved in this non-aqueous solvent to a concentration of 0.5 mol / L to prepare a non-aqueous electrolyte.

[0081] (4) Assembly of lithium primary batteries A polyphenylene sulfide nonwoven fabric (thickness: 0.5 mm) was prepared as a separator. A polyphenylene sulfide gasket was prepared. A positive electrode case formed by pressing conductive stainless steel with a thickness of 0.25 mm was prepared. A sealing plate formed by pressing conductive stainless steel with a thickness of 0.20 mm was prepared. Using these positive electrode, negative electrode, electrolyte, separator, positive electrode case, gasket, and sealing plate, a flat lithium primary battery (diameter: 20 mm, thickness: 3 mm) having the structure shown in Figure 1 was assembled.

[0082] In preparing the positive electrode mixture, the average particle size of the PVDF fluorocarbon resin was changed, and several types of lithium primary batteries A1 to A6 and B1 to B5 were fabricated, and each was evaluated as described below.

[0083] (5) Evaluation [Measurement of discharge characteristics after high-temperature storage test] The manufactured lithium primary battery was placed in an environment at 125° C. Thereafter, discharge was performed under specified conditions at 125° C., and the discharge time until the battery discharge voltage reached 2.0 V was measured. Discharge was performed by repeating a cycle consisting of 100 ms discharge at 8 mA and 10 s no discharge.

[0084] [Measurement of particle size of fluorocarbon resin] Two of the manufactured lithium primary batteries were prepared and each was placed in an environment at 25°C for two hours. After that, the following measurements were performed on one battery, and the other battery was placed in an environment at 125°C for 100 hours (high temperature storage test).

[0085] A positive electrode was taken out from one of the lithium primary batteries that had not been subjected to the high-temperature storage test. Microscopic Raman spectroscopy was performed on the cross section of the positive electrode, and the grain boundaries of the PVDF particles were identified from the area where the scattering peak derived from PVDF was detected. Ten PVDF particles were randomly selected, and the area of ​​the area occupied by PVDF in the cross section of each PVDF particle was calculated, and the diameter of a circle (equivalent circle) having an area equal to that area was calculated as the particle size of the particle. The average value of the calculated particle sizes of the PVDF particles was calculated, and this average value was used as the particle size d1 of the fluorocarbon resin before the high-temperature storage test.

[0086] The positive electrode was taken out from the other lithium primary battery that had been subjected to the high-temperature storage test. Microscopic Raman spectroscopy was performed on the cross section of the positive electrode, and the average particle size of the PVDF particles was calculated in the same manner as for the other lithium primary battery. The average value was taken as the particle size d2 of the fluorocarbon resin after the high-temperature storage test.

[0087] 《Battery A7》 In preparing the positive electrode mixture, the content ratio of PVDF contained in the positive electrode mixture (positive electrode) was 0.2 parts by mass per 100 parts by mass of manganese dioxide (positive electrode active material). Except for this, a lithium primary battery A7 was produced in the same manner as Battery A4 and evaluated in the same manner.

[0088] 《Battery A8》 In preparing the positive electrode mixture, the content ratio of PVDF contained in the positive electrode mixture (positive electrode) was 6 parts by mass per 100 parts by mass of manganese dioxide (positive electrode active material). Except for this, a lithium primary battery A8 was produced in the same manner as Battery A4 and evaluated in the same manner.

[0089] The evaluation results are shown in Table 1. Table 1 shows the particle size d1 of the fluorocarbon resin before the high-temperature storage test, the particle size d2 of the fluorocarbon resin after the high-temperature storage test, the ratio d2 / d1, the moldability of the positive electrode mixture, and the discharge time at 125° C. Table 1 also shows the average particle size of the fluorocarbon resin mixed in the positive electrode mixture and its content ratio (parts by mass relative to 100 parts by mass of the positive electrode active material).

[0090] In Table 1, "good" moldability means that the pellets could be molded without any problems, and "bad" moldability means that the pellets collapsed during molding.

[0091] In Table 1, lithium primary batteries A1 to A8 are examples, and lithium primary batteries B1 to B5 are comparative examples.

[0092] [Table 1]

[0093] As shown in Table 1, in the lithium primary batteries A1 to A8 using positive electrodes in which a fluorocarbon resin having an average particle size (D50) of 10 to 200 μm was mixed with a positive electrode active material in a positive electrode mixture, and the content ratio of the fluorocarbon resin was in the range of 0.2 to 6 parts by mass per 100 parts by mass of the positive electrode active material, the deterioration of battery characteristics at high temperatures was suppressed and a long discharge time of 500 hours or more was maintained. In addition, the lithium primary batteries A2 to A8 using a fluorocarbon resin having an average particle size (D50) of 30 to 200 μm were able to maintain a long discharge time of 600 hours or more, and the lithium primary batteries A3 to A8 using a fluorocarbon resin having an average particle size (D50) of 70 to 200 μm were able to maintain a long discharge time of 800 hours or more.

[0094] Also, from Table 1, it can be seen that the larger the average particle size (D50) of the fluorocarbon resin in the positive electrode mixture, the smaller the ratio d2 / d1 tends to be. When d2 / d1 is in the range of 1.5 to 3.1, the deterioration of battery characteristics at high temperatures can be suppressed.

[0095] In the lithium primary batteries B1 to B3, in which the average particle size (D50) of the fluorocarbon resin in the positive electrode mixture is 1 μm or less, the discharge characteristics at high temperatures are significantly degraded. In the lithium primary batteries B1 and B2, the grain boundaries of the fluorocarbon resin could not be identified in the cross section of the positive electrode, and d1 and d2 could not be calculated. However, since the detection limit of the Raman microscope is about 1 μm, it is estimated that d1 and d2 in the batteries B1 and B2 are both 1 μm or less.

[0096] In the lithium primary battery B5 in which the average particle size (D50) of the fluorocarbon resin in the positive electrode mixture was set to 300 μm, the positive electrode could not be formed into a pellet, and the battery did not function. [Industrial Applicability]

[0097] The present invention can be used in flat lithium primary batteries. [Explanation of symbols]

[0098] 10 Flat lithium primary battery 11 Positive electrode 12 Separator 13 Negative electrode 20 cases 21 Positive electrode case 22 Sealing plate 23 Gasket

Claims

1. The method includes a step of obtaining a positive electrode mixture by mixing a material including particles of a fluorocarbon resin having a swelling property in an electrolytic solution and particles of a positive electrode active material, The average particle size of the fluorocarbon resin is in the range of 10 to 200 μm, In the material, the content of the fluorocarbon resin is in the range of 0.2 to 6 parts by mass relative to 100 parts by mass of the positive electrode active material, The method for producing a positive electrode mixture for a flat lithium primary battery, wherein the fluorocarbon resin is present in the positive electrode mixture in a particulate state.

2. The method for producing a positive electrode mixture for a flat lithium primary battery according to claim 1 , wherein the fluorocarbon resin contains polyvinylidene fluoride.

3. 3. The method for producing a positive electrode mixture for a flat lithium primary battery according to claim 1, wherein the material includes particles of the fluorocarbon resin, particles of the positive electrode active material, and a liquid.

4. The method for producing a positive electrode mixture for a flat lithium primary battery according to claim 3 , wherein the liquid is water.

5. The method for producing a positive electrode mixture for a flat lithium primary battery according to any one of claims 1 to 4, wherein the average particle size of the carbon fluoride resin is in the range of 30 to 200 µm.

6. The method for producing a positive electrode mixture for a flat lithium primary battery according to claim 5, wherein the average particle size of the fluorocarbon resin is in the range of 70 to 200 μm.

7. The BET specific surface area A (m 2 7. The method for producing a flat lithium primary battery positive electrode mixture according to claim 1, wherein the ratio A / B of the average particle diameter B (μm) of the positive electrode active material (A / g) is in the range of 0.25 to 1.

5.

8. The method for producing a positive electrode mixture for a flat lithium primary battery according to any one of claims 1 to 7, wherein the positive electrode active material contains manganese dioxide.

9. A flat lithium primary battery including a case, and a positive electrode, a negative electrode, a separator, and a non-aqueous electrolyte disposed in the case, the positive electrode includes a positive electrode active material and a fluorocarbon resin having a swelling property in the nonaqueous electrolyte solution, In the positive electrode, the fluorocarbon resin is present in a particulate state, a ratio d2 / d1 of a particle diameter d2 of the fluorocarbon resin after a high-temperature storage test to a particle diameter d1 of the fluorocarbon resin before the high-temperature storage test is 1.5 or more and 3.1 or less when a high-temperature storage test is performed in which the flat lithium primary battery is placed in an environment of 25°C and stored in an environment of 125°C for 100 hours.

10. 10. The flat lithium primary battery according to claim 9, wherein the fluorocarbon resin is polyvinylidene fluoride.

11. The BET specific surface area A (m 2 11. The flat lithium primary battery according to claim 9, wherein the ratio A / B of the average particle size (μm) of the positive electrode active material (A / g) to the average particle size (μm) of the positive electrode active material is in the range of 0.25 to 1.

5.

12. the case includes a positive electrode case that functions as a positive electrode terminal, a sealing plate that functions as a negative electrode terminal, and a gasket disposed between the positive electrode case and the sealing plate, 12. The flat lithium primary battery according to claim 9, wherein the gasket comprises polyphenylene sulfide.

13. The non-aqueous electrolyte contains dimethoxyethane as a solvent, 13. The flat lithium primary battery according to claim 9, wherein the ratio of the dimethoxyethane to the solvent of the nonaqueous electrolyte is 50% by volume or more.

14. The flat lithium primary battery according to any one of claims 9 to 13, which is a coin battery to be mounted on a tire.

Citation Information

Patent Citations

  • Lithium battery

    JP1996106903A

  • Nonaqueous electrolyte secondary battery

    JP2000285923A

  • Electrode for secondary battery and secondary battery using the same

    JP2003109581A

  • Alkaline primary battery and method for manufacturing alkaline primary battery

    JP2010040334A

  • All-solid battery and manufacturing method thereof

    JP2020194706A