Zinc carbonate manufacturing method
The method improves zinc carbonate production efficiency by converting by-products into reusable alkali hydroxide and reducing impurities, addressing inefficiencies in existing zinc carbonate production methods.
Patent Information
- Application Number
- JP2020202011
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-12-04
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2040-12-04
AI Technical Summary
Existing methods for producing zinc carbonate from electric furnace dust and secondary dust inefficiently recycle alkaline components, leading to suboptimal use of alkaline agents and potential by-products like alkali carbonate or hydrogen carbonate.
A method involving zinc extraction, carbonate separation, and alkali regeneration steps, utilizing alkali hydroxide solutions and calcium hydroxide to convert by-products into reusable alkali hydroxide, while reducing metal impurities through substitution and deironization processes.
Enhances the efficiency of zinc carbonate production by recycling alkaline agents and effectively utilizing raw materials, resulting in stable, high-yield production with reduced impurities.
Smart Images

Figure 0007565585000004 
Figure 0007565585000005 
Figure 0007565585000006
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing zinc carbonate, and in particular to a method for producing zinc carbonate using so-called secondary dust as a raw material, such as electric furnace dust generated during the melting and smelting of scrap in the electric furnace process, which is one of the iron-making processes, secondary dust (crude zinc oxide) generated in a reduction furnace when part of the electric furnace dust is recycled as a zinc raw material, and secondary dust (crude zinc oxide) generated in the blast furnace process, which is one of the iron-making processes, and recovered as a zinc-containing oxide in a rotary hearth furnace. [Background technology]
[0002] In the electric furnace process, which is one of the steelmaking processes, electric furnace dust is generated as industrial waste containing zinc oxide and accounts for approximately 1.5% to 2.0% of the steel produced during the melting and smelting of scrap. It is said that 8 million tons of electric furnace dust is generated worldwide, and 400,000 tons is generated in Japan.
[0003] Most of the iron scrap is from abandoned buildings, discarded home appliances, or scrapped automobiles. The paint base of abandoned buildings, discarded home appliances, or scrapped automobiles is zinc-plated. The scrap also contains paint, plastic, oil, and the like. Therefore, electric furnace dust contains heavy metals such as zinc and lead, as well as harmful organic matter such as chlorides and dioxins. On the other hand, electric furnace dust contains about 20-30% iron and 20-30% zinc. Furthermore, crude zinc oxide contains about 10% iron and about 60% zinc. Therefore, electric furnace dust and secondary dust (crude zinc oxide) are very useful resources.
[0004] Under such circumstances, Patent Document 1 discloses a method for producing zinc ingot, which includes the steps of: producing a zinc-containing aqueous solution containing a zinc component using electric furnace dust or secondary dust generated when electric furnace dust is reduced in a reduction furnace as a raw material; converting the zinc component in the zinc-containing aqueous solution into a zinc-containing compound in at least one form of carbonate, hydroxide, and oxide, and chlorinating the zinc component of the zinc-containing compound to produce purified zinc chloride containing purified zinc chloride; dehydrating the purified zinc chloride to produce anhydrous molten purified zinc chloride containing dehydrated molten purified zinc chloride; and electrolyzing the anhydrous molten purified zinc chloride to produce zinc ingot as an electrolysis product. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2019-119895 A Summary of the Invention [Problem to be solved by the invention]
[0006] However, according to the investigations of the present inventors, in the configuration disclosed in Patent Document 1, the filtrate remaining after separation of zinc-containing compounds in at least one form of carbonate, hydroxide, and oxide is repeatedly used as an alkaline agent for selectively extracting zinc components from electric furnace dust or secondary dust. However, since this only circulates the alkaline components remaining in the filtrate, there is room for improvement in terms of efficiently sending alkaline components in a more appropriate form to the zinc extraction process.
[0007] In particular, according to the investigations of the present inventors, when electric furnace dust or secondary dust generated when electric furnace dust is reduced in a reduction furnace is used as a raw material, the zinc component in the raw material is selectively extracted using an aqueous alkali hydroxide solution as an extraction solvent, and the extracted zinc component is converted into a zinc-containing compound in the form of carbonate to produce zinc carbonate. In this case, however, alkali carbonate components or alkali hydrogen carbonate components may be by-produced. However, if such by-products can be converted into alkali components that can extract the zinc component in the aqueous zinc-containing solution, it will be possible to efficiently use an alkali agent in a more appropriate form.
[0008] The present invention has been made through the above-mentioned studies, and an object of the present invention is to provide a method for producing zinc carbonate, which comprises selectively extracting, using an aqueous alkali hydroxide solution as an extraction solvent, a zinc component in a zinc-containing aqueous solution produced from electric furnace dust or secondary dust generated when electric furnace dust is reduced in a reduction furnace as a raw material, and converting the extracted zinc component into a zinc-containing compound in the form of carbonate to produce zinc carbonate, thereby converting a by-produced alkali carbonate component or alkali hydrogen carbonate component into an alkali component that can extract the zinc component in the zinc-containing aqueous solution. [Means for solving the problem]
[0009] In order to achieve the above object, a method for producing zinc carbonate in a first aspect of the present invention includes a zinc-containing aqueous solution production step of selectively extracting a zinc component from electric furnace dust or secondary dust generated when the electric furnace dust is reduced in a reduction furnace to produce a zinc-containing aqueous solution containing the zinc component, and a zinc carbonate separation step of separating the zinc component from the zinc-containing aqueous solution as zinc carbonate to obtain the zinc carbonate as a product, the method further including an alkali regeneration step of using an aqueous alkali hydroxide solution as an extraction solvent for selectively extracting the zinc component in the aqueous zinc-containing solution production step, converting a by-product alkali component produced in the zinc carbonate separation step into an alkali hydroxide component, and sending the alkali hydroxide component to the aqueous alkali hydroxide solution in the aqueous zinc-containing solution production step. In the zinc carbonate separation step, carbon dioxide is brought into contact with the zinc-containing aqueous solution to separate the zinc carbonate, and an alkali carbonate or an alkali hydrogen carbonate is generated as the by-product alkali component. In the alkali regeneration step, calcium hydroxide is brought into contact with the alkali carbonate or alkali hydrogen carbonate by-produced in the zinc carbonate separation step to generate the alkali hydroxide. The calcium hydroxide brought into contact with the alkali carbonate or alkali hydrogen carbonate in the alkali regeneration step is obtained by using a calcium component in the residue obtained in the zinc-containing aqueous solution generation step. do.
[0012] The present invention also relates to the first 1 In addition to the above-mentioned aspect, the present invention further includes a substitution step of contacting the zinc-containing aqueous solution produced in the zinc-containing aqueous solution production step with metallic zinc to reduce and precipitate metal impurity components more noble than zinc in the zinc-containing aqueous solution, and the zinc carbonate separation step is intended to separate the zinc component in the zinc-containing aqueous solution that has been subjected to the substitution step as zinc carbonate. 2 The situation is as follows.
[0013] The present invention also relates to the first Or second In addition to the above-mentioned aspect, the present invention further comprises a deironization / demanganization step of contacting an oxidizing agent with the zinc-containing aqueous solution produced in the zinc-containing aqueous solution production step to separate iron and manganese components in the zinc-containing aqueous solution, and a substitution step of contacting metallic zinc with the zinc-containing aqueous solution that has been subjected to the deironization / demanganization step to reduce and precipitate metal impurity components that are more noble than zinc in the zinc-containing aqueous solution, and the zinc carbonate separation step is intended to separate the zinc component in the zinc-containing aqueous solution that has been subjected to the substitution step as zinc carbonate. 3 The situation is as follows. Effect of the Invention
[0014] According to the method for producing zinc carbonate in the first aspect of the present invention, an aqueous alkali hydroxide solution is used as an extraction solvent for selectively extracting the zinc component in the zinc-containing aqueous solution production step, and the method further includes an alkali regeneration step of converting the by-produced alkali component produced in the zinc carbonate separation step into an alkali hydroxide component and sending the alkali hydroxide component into the aqueous alkali hydroxide solution in the zinc-containing aqueous solution production step. Therefore, the by-produced alkali component can be converted into an alkali component that can extract the zinc component in the zinc-containing aqueous solution, and zinc carbonate can be produced more efficiently by efficiently using an alkali agent in a more appropriate form.
[0015] In addition, the present invention 1According to the method for producing zinc carbonate in the above aspect, in the zinc carbonate separation step, zinc carbonate is separated by contacting the zinc-containing aqueous solution with carbon dioxide, and an alkali carbonate or alkali hydrogen carbonate is produced as a by-product alkali component. In the alkali regeneration step, an alkali hydroxide is produced by contacting the alkali carbonate or alkali hydrogen carbonate produced as a by-product in the zinc carbonate separation step with calcium hydroxide. Therefore, the by-product alkali components such as sodium carbonate and sodium hydrogen carbonate are converted into an alkali component such as sodium hydroxide, and can be reused as an extraction solvent that can extract the zinc component in the zinc-containing aqueous solution. Therefore, the extraction solvent can be recycled without being discarded, and zinc carbonate can be produced more efficiently.
[0016] In addition, the present invention 1 According to the method for producing zinc carbonate in the above aspect, the calcium hydroxide that is brought into contact with the alkali carbonate or alkali hydrogencarbonate in the alkali regeneration step is obtained using the calcium component in the residue obtained in the zinc-containing aqueous solution production step, so that the calcium component in the raw material for the zinc-containing aqueous solution can be effectively utilized, and zinc carbonate can be produced more efficiently.
[0017] In addition, the present invention 2 According to the aspect of the method for producing zinc carbonate, the method further includes a substitution step of contacting the zinc-containing aqueous solution produced in the zinc-containing aqueous solution production step with metallic zinc to reduce and precipitate metal impurity components that are more noble than zinc in the zinc-containing aqueous solution, and a zinc carbonate separation step of separating the zinc components in the zinc-containing aqueous solution that has been subjected to the substitution step as zinc carbonate, thereby making it possible to stably mass-produce zinc carbonate with reduced metal impurity components with good yield.
[0018] In addition, the present invention 3According to the aspect of the method for producing zinc carbonate, the method further includes a deironization / demanganization step of contacting an oxidizing agent with the zinc-containing aqueous solution produced in the zinc-containing aqueous solution production step to separate iron and manganese components in the zinc-containing aqueous solution, and a substitution step of contacting metallic zinc with the zinc-containing aqueous solution that has been subjected to the deironization / demanganization step to reduce and precipitate metal impurity components that are more noble than zinc in the zinc-containing aqueous solution. Since the zinc carbonate separation step separates the zinc components in the zinc-containing aqueous solution that has been subjected to the substitution step as zinc carbonate, zinc carbonate in which iron and manganese components are reduced can be mass-produced stably with good yield. [Brief description of the drawings]
[0019] [Figure 1] FIG. 1(a) is a process diagram of a method for producing zinc carbonate in a first embodiment of the present invention, and FIG. 1(b) is a process diagram for producing secondary dust that can be used as a raw material in the method for producing zinc carbonate in this embodiment. [Diagram 2] FIG. 2 is a process diagram showing a method for producing zinc carbonate in a second embodiment of the present invention. [Diagram 3] FIG. 3 is a process diagram of a method for producing zinc carbonate in a third embodiment of the present invention. [Figure 4] FIG. 4 is Table 1 showing the results of an experimental example of the first embodiment of the present invention. [Diagram 5] FIG. 5 is Table 2 showing the results of an experimental example of the second embodiment of the present invention. [Figure 6] FIG. 6 is Table 3 showing the results of an experimental example of the third embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] Hereinafter, the method for producing zinc carbonate in each embodiment of the present invention will be described in detail with reference to the drawings as appropriate.
[0021] (First embodiment) First, with reference to FIG. 1, a method for producing zinc carbonate in a first embodiment of the present invention will be described in detail.
[0022] FIG. 1(a) is a diagram showing steps of a method for producing zinc carbonate in this embodiment, and FIG. 1(b) is a diagram showing a process for producing secondary dust that can be used as a raw material in the method for producing zinc carbonate in this embodiment.
[0023] As shown in Fig. 1(a), in this embodiment, a zinc extraction step 101 and a zinc carbonate separation step 102 are carried out in this order, and an alkali regeneration step 103 is also carried out. The zinc extraction step 101 corresponds to a zinc-containing aqueous solution production step. This is based on a production concept in which priority is given to producing an aqueous solution in which zinc components are extracted from electric furnace dust or secondary dust as a raw material, and zinc carbonate is produced as a zinc-containing compound in the form of carbonate produced from the zinc components in the aqueous solution.
[0024] Specifically, first, in the zinc extraction process 101, electric furnace dust 1 as a raw material containing zinc-containing compounds such as zinc oxide and iron compounds such as iron oxide is directly contacted with an aqueous solution of an alkaline agent 3 as an extraction solvent for zinc, and the zinc component is selectively extracted from the zinc-containing compounds to produce a zinc extract solution containing the zinc component, a zinc-containing aqueous alkaline agent solution 5, and the solid content that does not dissolve in the aqueous solution of the alkaline agent 3 is left as a residue 4.
[0025] Typically, the chemical formula for obtaining a zinc-containing aqueous alkaline agent solution 5, which is a zinc-containing aqueous solution obtained by selectively extracting zinc components from zinc oxide in electric furnace dust 1 using sodium hydroxide as an alkaline agent 3, is shown below in Chemical Formula 1. [ka]
[0026] As the raw material used in the zinc extraction step 101, a secondary dust 2 obtained by reducing the electric furnace dust 1 in a reduction furnace may be used instead of the electric furnace dust 1. In addition, as the raw material used in the zinc extraction step 101, when the calcination step 104 shown in FIG. 1(b) is adopted, Secondary dust 2 obtained by mixing and calcining electric furnace dust 1 with calcium carbonate 10 may also be used. By such calcination, the zinc component contained in the zinc ferrite component of the electric furnace dust 1 is converted into alkali. In this way, when the secondary dust 2 obtained by calcining the calcium carbonate 10 is used as a raw material, the zinc extraction process The calcium content in the residue 4 obtained in 101 can be increased. The carbon dioxide 6 obtained in step 102 can be used in the next zinc carbonate separation step 102. Furthermore, as the raw material used in the zinc extraction step 101, secondary dust such as crude zinc hydroxide obtained from the electric furnace dust 1 may be used.
[0027] Next, in the zinc carbonate separation step 102, the zinc-containing aqueous alkaline agent solution 5 containing the zinc component extracted in the zinc extraction step 101 is directly contacted with carbon dioxide (carbon dioxide gas) 6 to precipitate zinc carbonate 7 from the zinc-containing aqueous alkaline agent solution 5 containing the zinc component extracted in the zinc extraction step 101, which is then recovered as a solid by solid-liquid separation, and used as the product as is.
[0028] Typically, carbon dioxide 6 is blown into the zinc component in a zinc-containing aqueous alkaline agent solution 5 shown in chemical formula (Chemical Formula 1) to precipitate zinc carbonate 7, as shown in the following chemical formula (Chemical Formula 2). The precipitated zinc carbonate 7 is then filtered to obtain zinc carbonate 7 as a solid content. [ka]
[0029] In the zinc carbonate separation step 102, a liquid containing carbonate ions may be used instead of carbon dioxide 6 to be contacted with the zinc-containing alkaline agent aqueous solution 5. As is clear from the chemical formula (Chemical formula 2), in order for zinc hydroxide to dissolve in the alkaline aqueous solution, excess hydroxide ions are required. Therefore, in the zinc carbonate separation step 102, zinc hydroxide may be precipitated instead of zinc carbonate 7 or together with zinc carbonate. Since zinc carbonate and zinc hydroxide have the property of becoming zinc oxide when heated, a part of the zinc carbonate may be zinc oxide as well as zinc hydroxide. In addition, by repeatedly precipitating and redissolving zinc carbonate and zinc hydroxide by techniques such as heating, cooling and pH adjustment of the zinc-containing alkaline agent aqueous solution 5 containing the zinc component, a purification effect can be actively utilized to obtain a product of even higher purity.
[0030] Here, in the alkali regeneration step 103, since the filtrate 8 obtained after solid-liquid separation of the zinc carbonate 7 in the zinc carbonate separation step 102 contains alkali carbonate components and alkali hydrogen carbonate components as by-products, these alkali carbonate components and alkali hydrogen carbonate components are converted into alkali hydroxide components, and the alkaline agent 3 consisting of the converted alkali hydroxide components is returned to the aqueous solution of the alkaline agent 3 in the zinc extraction step 101.
[0031] Typically, calcium hydroxide 9 is added to the filtrate 8 after solid-liquid separation of zinc carbonate 7 in the zinc carbonate separation step 102 to convert sodium carbonate and sodium hydrogen carbonate into sodium hydroxide, and the sodium hydroxide thus converted is returned as the alkaline agent 3 to the aqueous solution of the alkaline agent 3 in the zinc extraction step 101. The chemical formula for obtaining sodium hydroxide from sodium carbonate and calcium hydroxide is shown in the following (Chemical Formula 3). [ka]
[0032] In the alkali regeneration step 103, calcium hydroxide 9 containing a calcium component contained in the residue 4 obtained when the zinc-containing alkaline agent aqueous solution 5 is produced in the zinc extraction step 101 may be used as the calcium hydroxide 9 to be added to the filtrate 8 after solid-liquid separation of zinc carbonate 7 in the zinc carbonate separation step 102. When calcium components are contained in the electric furnace dust 1 or the secondary dust 2, they can be used as the calcium components in the residue 4. Alternatively, when a calcination step 104 is adopted in which calcium carbonate 10 is mixed with the electric furnace dust 1 and calcined, It is also possible to use a calcium component derived from the calcium carbonate 10. In addition, the calcium hydroxide 9 may be not only one derived from such a calcium component, but also commercially available slaked lime.
[0033] In the zinc carbonate production method of this embodiment described above, an aqueous alkali hydroxide solution is used as an extraction solvent for selectively extracting the zinc component in the zinc-containing aqueous solution production step 101, and the method further includes an alkali regeneration step 103 for converting the by-produced alkali component produced in the zinc carbonate separation step 102 into an alkali hydroxide component and sending the alkali hydroxide component to the aqueous alkali hydroxide solution in the zinc-containing aqueous solution production step. Therefore, the by-produced alkali component can be converted into an alkali component that can extract the zinc component in the zinc-containing aqueous solution, and zinc carbonate can be produced more efficiently by efficiently using an alkali agent in a more appropriate form.
[0034] In addition, in the zinc carbonate production method of this embodiment, zinc carbonate is separated by contacting the zinc-containing aqueous solution with carbon dioxide in the zinc carbonate separation step 102, and an alkali carbonate or alkali hydrogen carbonate is generated as a by-product alkali component. The alkali carbonate or alkali hydrogen carbonate by-produced in the zinc carbonate separation step 102 is contacted with calcium hydroxide in the alkali regeneration step 103 to generate an alkali hydroxide component. Therefore, the by-produced alkali components such as sodium carbonate and sodium hydrogen carbonate are converted into alkali components such as sodium hydroxide, and can be reused as an extraction solvent that can extract the zinc component in the zinc-containing aqueous solution. The extraction solvent can be recycled without being discarded, and zinc carbonate can be produced more efficiently.
[0035] Furthermore, in the method for producing zinc carbonate of this embodiment, the calcium hydroxide that is brought into contact with the alkali carbonate or alkali hydrogencarbonate in the alkali regeneration step 103 is obtained using the calcium component in the residue obtained in the zinc-containing aqueous solution production step, so that the calcium in the raw material for the zinc-containing aqueous solution can be effectively utilized, and zinc carbonate can be produced more efficiently.
[0036] Second embodiment Next, a method for producing zinc carbonate according to a second embodiment of the present invention will be described in detail with reference to FIG.
[0037] FIG. 2 is a diagram showing steps of a method for producing zinc carbonate in this embodiment.
[0038] 2, the zinc carbonate production method according to this embodiment is mainly different from the zinc carbonate production method according to the first embodiment in that the zinc carbonate production method according to this embodiment has a substitution step (cementation step) 105 between a zinc extraction step 101 and a zinc carbonate separation step 102. In this embodiment, the description will be given focusing on such a difference, and the same components are denoted by the same reference numerals, and the description thereof will be omitted or simplified.
[0039] Specifically, in the substitution step 105 following the zinc extraction step 101, a zinc-containing aqueous alkaline agent solution 5 serving as a zinc extract containing the zinc component extracted in the zinc extraction step 101 is directly contacted with metallic zinc 11 such as zinc fine particles, whereby metal impurity components 12 such as copper, lead, cadmium, etc., which are more noble than zinc in the zinc-containing aqueous alkaline agent solution 5, are reduced and precipitated, thereby reducing the concentration of impurity components in the zinc-containing aqueous alkaline agent solution 5.
[0040] Next, in the zinc carbonate separation step 102, the zinc-containing aqueous alkaline agent solution 13, the concentration of impurity components of which has been reduced in the substitution step 105, is contacted with carbon dioxide 6 to precipitate zinc carbonate 7 from the zinc-containing aqueous alkaline agent solution 13, which is then subjected to solid-liquid separation to be recovered as a solid matter.
[0041] According to the method for producing zinc carbonate of the present embodiment, in addition to the configuration of the first embodiment, the method further includes a substitution step 105 in which metallic zinc is brought into contact with the zinc-containing aqueous solution produced in the zinc-containing aqueous solution production step 101 to reduce and precipitate metal impurity components that are more noble than zinc in the zinc-containing aqueous solution, so that zinc carbonate with reduced metal impurity components can be mass-produced stably with good yield.
[0042] (Third embodiment) Next, a method for producing zinc carbonate according to a third embodiment of the present invention will be described in detail with reference to FIG.
[0043] FIG. 3 is a diagram showing steps of a method for producing zinc carbonate in this embodiment.
[0044] As shown in Fig. 3, the zinc carbonate production method according to this embodiment is mainly different from the zinc carbonate production method according to the second embodiment in that it has a deironization / demanganization step 106 between a zinc extraction step 101 and a substitution step 105. This embodiment will be described focusing on such a difference, and the same components are denoted by the same reference numerals, and the description thereof will be omitted or simplified.
[0045] In this embodiment, the provision of the deironization / demanganese step 106 is particularly effective when the iron or manganese components contained in the electric furnace dust or the like are alkali-soluble Fe(II) and Mn(II), and is also effective even when the iron or manganese components are alkali-insoluble, because when, for example, an aqueous zinc-containing solution in which alkali-insoluble Fe(III) and Mn(IV) are suspended is treated in the substitution step, they are reduced to alkali-soluble Fe(II) and dissolved in the aqueous zinc-containing solution. In addition, since an alkali-soluble iron or manganese component may be generated in the substitution step 105, not only the substitution step may be provided after the deironization / demanganese step, but also the substitution step may be provided before the deironization / demanganese step. Specific methods for the deironization / demanganese step 106 include aeration and oxidation by addition of permanganate, and when the soluble manganese component is Mn(VII), a method of contacting with activated carbon may be used.
[0046] Specifically, in the deironization / demanganization step 106 following the zinc extraction step 101, in order to remove the iron and soluble manganese contained in the zinc-containing alkaline agent aqueous solution 5 as the zinc extract containing the zinc component extracted in the zinc extraction step 101, the iron or soluble manganese contained in the zinc-containing alkaline agent aqueous solution 5 is oxidized, and the iron and manganese components in the zinc-containing alkaline agent aqueous solution 5 are separated and removed as insoluble precipitate sludge 17. Specifically, the iron (I) component in the zinc-containing alkaline agent aqueous solution 5 is oxidized to an iron (II) component by blowing in an oxygen-containing gas (for example, blowing in air, i.e., aeration) into the zinc-containing alkaline agent aqueous solution 5, or adding an oxidizing agent 15 such as permanganate, chlorate, or chlorine dioxide, and the like, and the soluble manganese is oxidized and converted to an insoluble manganese compound, which is separated and removed as sludge 17. The iron component in the zinc-containing alkaline agent aqueous solution 5 can also be converted to a magnetic iron oxide such as maghemite containing both ferrous and ferric components by controlling the temperature, alkali concentration, and oxidation-reduction potential (ORP) value.
[0047] When permanganate is used as the oxidizing agent 15, the end point of demanganization can be determined by supplying permanganate until an excess of permanganic acid remains in the zinc-containing aqueous alkaline agent solution 5, and the remaining permanganate is directly brought into contact with activated carbon and converted into insoluble manganese dioxide, which is then removed.
[0048] Next, in the substitution step 105, the zinc-containing alkaline agent aqueous solution 16, the concentration of which has been reduced in the iron and manganese removal step 106, is contacted with metallic zinc 11 such as zinc fine particles to reduce and precipitate metal impurity components 12, such as copper, lead, and cadmium, which are more noble than zinc in the zinc-containing alkaline agent aqueous solution 16, thereby further reducing the concentration of impurity components in the zinc-containing alkaline agent aqueous solution 16.
[0049] Regarding the order of carrying out the iron removal / demanganese step 106 and the replacement step 105, the iron removal / demanganese step 106 may be carried out after the replacement step 105. For example, when the raw material is a material that has been subjected to an iron reduction step, such as secondary dust, the raw material may contain a large amount of divalent iron (Fe(II): ferrous component), and it is therefore more reasonable to carry out the replacement step 105 first when treating such raw material. This also applies to an embodiment in which the iron removal / demanganese step 106 is separated into a deironization step and a demanganese step, each of which is carried out separately.
[0050] According to the method for producing zinc carbonate of the present embodiment, in addition to the configuration of the second embodiment, the method further includes a deironization / demanganese step 106 in which an oxidizing agent is brought into contact with the zinc-containing aqueous solution produced in the zinc-containing aqueous solution production step 101 to separate iron and manganese components in the zinc-containing aqueous solution, so that zinc carbonate with reduced iron and manganese components can be mass-produced stably with good yield.
[0051] Finally, in contrast to the present embodiment described above, experimental examples representatively corresponding to the first to third embodiments will be described in detail with reference to FIGS. 4 to 6. FIG.
[0052] Fig. 4 is Table 1 showing the results of Experimental Example 1 of the first embodiment of the present invention, Fig. 5 is Table 2 showing the results of Experimental Example 2 of the second embodiment of the present invention, and Fig. 6 is Table 3 showing the results of Experimental Example 2 of the third embodiment of the present invention. Note that ND in the tables indicates not detected. Also, blank spaces in the tables indicate that electric furnace dust, secondary dust, and residue were below the detection limit or not detected, and that items other than electric furnace dust, secondary dust, and residue were not included in the analysis.
[0053] (Experimental Example 1) This experimental example corresponds to the first embodiment of the present invention, and the results are shown in Table 1 of FIG.
[0054] First, in the zinc extraction process 101, calcium carbonate weighing 441 g was extracted in a calcination process 104. The secondary dust of 870g was obtained by mixing and calcining the aluminum and the electric furnace dust of 762.8g. A secondary dust 2 weighing 60.5 g was separated from the dust, and the separated secondary dust 2 was contacted with a 16.5% NaOH aqueous solution as an aqueous solution of an alkaline agent 3, and the solid matter that was not dissolved in the aqueous solution of the alkaline agent 3 was separated by filtration to obtain a zinc extract (zinc-containing aqueous alkaline agent solution) 5 with a volume of 395 ml as the remaining liquid. The solid matter that was not dissolved in the aqueous solution of the alkaline agent 3 was filtered, washed with pure water, and then dried to obtain a residue 4 weighing 43.3 g. The extraction conditions in the zinc extraction step 101 were a temperature of 95° C. and normal pressure, and the contact time between the aqueous solution of the alkaline agent 3 and the secondary dust 2 was 8 hours. The filtrate from which the residue 4 was separated (the filtrate from which extractable components were extracted from the insoluble solid matter) was repeatedly used as the alkaline agent 3 for dissolving the secondary dust 2, and the washing water after washing the residue 4 with pure water was repeatedly used as dilution water in the purification step.
[0055] Next, in the zinc carbonate separation process 102, carbon dioxide 6 is blown into the zinc-containing alkaline agent aqueous solution 5 to precipitate zinc carbonate 7, and the zinc carbonate 7 is separated by suction and filtration using GF (glass fiber) / C filter paper. The zinc carbonate 7 is used as a product as it is. It is generated by the decomposition of calcium carbonate 10 during the calcination of electric furnace dust 1 in the calcination process 104. The composition of zinc carbonate 7 is shown in Table 1, and for the zinc carbonate 7, the value is the analytical value of the zinc oxide converted by heating and drying for convenience.
[0056] In the alkali regeneration step 103, the filtrate 8 from which the zinc carbonate 7 has been separated is brought into contact with slaked lime 9, and Na2CO3 and NaHCO3, which are by-produced when carbon dioxide 6 is blown into the zinc-containing aqueous alkaline agent solution 5 in the zinc carbonate separation step 102, are converted into NaOH, and this NaOH is sent to the zinc extraction step 101 as the alkaline agent 3 and used repeatedly for zinc extraction. The slaked lime 9 is calcium carbonate derived from calcium carbonate 10 used in calcining the electric furnace dust 1 in the calcination step 104. The zinc component used was obtained by utilizing the calcium component contained in the residue 4 from the zinc extraction process 101.
[0057] (Experimental Example 2) This experimental example corresponds to the second embodiment of the present invention, and the results are shown in Table 2 of FIG.
[0058] First, in the zinc extraction step 101, the secondary dust (crude zinc hydroxide sample) 2 with a weight of 100 g derived from the electric furnace dust 1 was contacted with a 16.5% NaOH aqueous solution as an aqueous solution of an alkaline agent 3, and the whole amount was filtered after stirring. Next, the solid matter that did not dissolve in the aqueous solution of the alkaline agent 3 was contacted with a new aqueous solution of an NaOH solution with a concentration of 16.5% as an aqueous solution of an alkaline agent 3, and the whole amount was filtered after stirring. The solid matter that did not dissolve in each aqueous solution of the alkaline agent 3 was separated by filtration to obtain a residue 4, and the remaining liquids from which the residue 4 was separated were used to obtain a zinc extract solution (zinc-containing aqueous alkaline agent solution) 5 with a zinc concentration of 45800 ppm. Note that the conditions such as temperature in the zinc extraction step 101 of this experimental example were the same as those of experimental example 1.
[0059] Next, in the substitution step 105, 5 g of powdered zinc particles 11 with an average particle size of about 6 μm was added to the zinc-containing alkaline agent aqueous solution 5, followed by heating and stirring, and the stirred matter was aspirated and filtered through a membrane filter with a filtration accuracy of 0.1 μm to obtain a filtrate of a zinc-containing alkaline agent aqueous solution 13. The solid matter separated from the membrane filter was a mixture of metal powder 12 that was reduced and precipitated as the zinc particles 11 were dissolved, and the powdered zinc that remained undissolved.
[0060] Next, the zinc carbonate separation step 102 following the substitution step 105 was carried out in the same manner as in Experimental Example 1 using a zinc-containing alkaline agent aqueous solution 13, and the separated zinc carbonate 7 was used as a product as is. The composition of the zinc carbonate 7 obtained in this Experimental Example is as shown in Table 2, and compared to that in Experimental Example 1, the amount of metal impurities such as copper, lead, and cadmium was reduced. For convenience, the value of zinc carbonate 7 is the analytical value of zinc oxide converted by heating and drying.
[0061] In the alkali regeneration step 103, calcium hydroxide 9 is brought into contact with the filtrate 8 remaining after separation of the zinc carbonate 7, and Na2CO3 and NaHCO3 produced as by-products when carbon dioxide 6 is blown into the zinc-containing aqueous alkaline agent solution 5 in the zinc carbonate separation step 102 are converted to NaOH, and this NaOH is sent to the zinc extraction step 101 as the alkaline agent 3 and repeatedly used for zinc extraction. The calcium hydroxide 9 is a calcium component derived from the secondary dust 2 used in the zinc extraction step 101, and was obtained by utilizing the calcium component contained in the residue 4 of the zinc extraction step 101.
[0062] (Experimental Example 3) This experimental example corresponds to the third embodiment of the present invention, and the results are shown in Table 3 of FIG.
[0063] First, in the zinc extraction step 101, the secondary dust (crude zinc hydroxide sample) 2 with a weight of 300 g derived from the electric furnace dust 1 was contacted with a 16.5% NaOH aqueous solution as an aqueous solution of the alkaline agent 3, stirred, and the entire amount was filtered to obtain a zinc extract solution (zinc-containing aqueous alkaline agent solution) 5 with a volume of 1800 ml as the remaining liquid after separating the solid matter that does not dissolve in the aqueous solution of the alkaline agent 3. Next, the solid matter that does not dissolve in the aqueous solution of the alkaline agent 3 was contacted with a 16.5% NaOH aqueous solution as a new aqueous solution of the alkaline agent 3, stirred, and the entire amount was filtered to separate the solid matter that does not dissolve in the aqueous solution of the alkaline agent 3 by filtration to obtain a residue 2 with a weight of 161 g. The conditions in the zinc extraction step 101 in this experimental example were the same as those in the experimental example 1.
[0064] Next, in the deironization / demanganization process 106 following the zinc extraction process 101, air was blown into the zinc-containing alkaline agent aqueous solution 5 as an oxidizing agent 11 under heating to precipitate a brown precipitate, which was then aspirated and filtered through a membrane filter with a filtration accuracy of 0.1 μm to obtain a filtrate (deironized and demanganized zinc-containing alkaline agent aqueous solution 16). As the solid content on the filter paper, deironized and demanganized sludge 17 weighing 263 mg was obtained.
[0065] Next, the substitution step 103 following the iron removal / manganese removal step 106 was carried out using a zinc-containing aqueous alkaline agent solution 16 in the same manner as in Experimental Example 2, and the zinc carbonate separation step 102 and the alkali regeneration step 103 were carried out in the same manner as in Experimental Example 2, with the zinc carbonate 7 separated in the zinc carbonate separation step 102 being used as a product as is. The composition of the zinc carbonate 7 obtained in this experiment is as shown in Table 3, and compared to that in Experimental Example 2, the amount of metal impurities such as iron and manganese was reduced. For convenience, the value of zinc carbonate 7 is the analytical value of zinc oxide converted during heating and drying.
[0066] In addition, the shape, arrangement, number, etc. of the components of the present invention are not limited to the above-described embodiment, and such components can be appropriately modified within the scope of the gist of the invention, such as by appropriately replacing such components with those that achieve equivalent functions and effects. [Industrial Applicability]
[0067] As described above, the present invention provides a method for producing zinc carbonate in which a zinc component in a zinc-containing aqueous solution produced using electric furnace dust or secondary dust generated when electric furnace dust is reduced in a reducing furnace as a raw material is selectively extracted using an aqueous alkali hydroxide solution as an extraction solvent, and the extracted zinc component is converted into a zinc-containing compound in the form of a carbonate to produce zinc carbonate. Therefore, due to its versatile and universal nature, it is expected that the present invention can be widely applied to a method for producing zinc carbonate using electric furnace dust generated during the melting and smelting of scrap in the electric furnace process, which is one of the iron-making processes, or secondary dust generated in a reducing furnace when part of the electric furnace dust is recycled as an iron-making raw material. [Explanation of symbols]
[0068] 1. Electric furnace dust 2...Secondary dust 3. Alkaline agent 4...Residue 5. Zinc-containing alkaline solution 6. Carbon dioxide 7. Zinc carbonate 8. Filtrate 9. Calcium hydroxide 10...Calcium carbonate 11...Zinc particles 12...Metal impurities 13. Zinc-containing alkaline solution 15...Oxidizer 16...Zinc-containing alkaline solution 17. Sludge 101...Zinc-containing aqueous solution generation process 101...Zinc extraction process 102...Zinc carbonate separation process 103...Alkaline regeneration process 104...Caking process 105...Replacement process 106…Iron removal and manganese removal process
Claims
1. a zinc-containing aqueous solution producing step of selectively extracting zinc components from electric furnace dust or secondary dust generated when the electric furnace dust is reduced in a reducing furnace as a raw material to produce a zinc-containing aqueous solution containing the zinc components; a zinc carbonate separation step of separating the zinc component from the zinc-containing aqueous solution as zinc carbonate to obtain the zinc carbonate as a product; A method for producing zinc carbonate comprising: an alkali hydroxide aqueous solution is used as an extraction solvent for selectively extracting the zinc component in the zinc-containing aqueous solution producing step; The method further comprises an alkali regeneration step of converting a by-product alkali component produced in the zinc carbonate separation step into an alkali hydroxide component, and feeding the alkali hydroxide component into the alkali hydroxide aqueous solution in the zinc-containing aqueous solution production step, In the zinc carbonate separation step, carbon dioxide is brought into contact with the zinc-containing aqueous solution to separate the zinc carbonate and generate an alkali carbonate or an alkali hydrogen carbonate as the by-product alkali component, the alkali carbonate or the alkali hydrogencarbonate by-produced in the zinc carbonate separation step is brought into contact with calcium hydroxide in the alkali regeneration step to produce the alkali hydroxide; The calcium hydroxide to be brought into contact with the alkali carbonate or the alkali hydrogencarbonate in the alkali regeneration step is obtained using the calcium component in the residue obtained in the zinc-containing aqueous solution production step.
2. The method further comprises a substitution step of contacting metallic zinc with the zinc-containing aqueous solution produced in the zinc-containing aqueous solution production step to reduce and precipitate metal impurity components nobler than zinc in the zinc-containing aqueous solution, 2. The method for producing zinc carbonate according to claim 1, wherein the zinc carbonate separation step separates the zinc component in the zinc-containing aqueous solution that has been subjected to the substitution step as the zinc carbonate.
3. a deironization / demanganization step of contacting the zinc-containing aqueous solution produced in the zinc-containing aqueous solution production step with an oxidizing agent to separate iron components and manganese components in the zinc-containing aqueous solution; a substitution step of bringing metallic zinc into contact with the zinc-containing aqueous solution that has been subjected to the iron removal and manganese removal step, thereby reducing and precipitating metal impurity components that are more noble than zinc in the zinc-containing aqueous solution; and 3. The method for producing zinc carbonate according to claim 1, wherein the zinc carbonate separation step separates the zinc component in the zinc-containing aqueous solution that has been subjected to the substitution step as the zinc carbonate.
4. A method for producing zinc carbonate described in any of claims 1 to 3, wherein the raw material in the zinc-containing aqueous solution production process is calcined dust obtained in a calcination process in which calcium carbonate is mixed with the electric furnace dust and calcined.
5. A method for producing zinc carbonate as described in claim 4, wherein in the zinc carbonate separation step, the zinc-containing aqueous solution is contacted with carbon dioxide obtained in the calcination step to separate the zinc carbonate.
6. A method for producing zinc carbonate as described in claim 4 or 5, wherein the calcium hydroxide that is brought into contact with the alkali carbonate component or the alkali bicarbonate component in the alkali regeneration process is obtained using a calcium component derived from the calcium carbonate used in the calcination process.
7. A method for producing zinc carbonate described in any of claims 1 to 6, wherein in the zinc-containing aqueous solution production process, the raw material is brought into contact with the aqueous alkali hydroxide solution, filtered, and the zinc-containing aqueous solution is obtained by separating solid components that are not dissolved in the aqueous alkali hydroxide solution from the aqueous alkali hydroxide solution.
8. A method for producing zinc carbonate described in any of claims 1 to 7, wherein in the zinc-containing aqueous solution production process, the raw material is contacted with the alkaline hydroxide aqueous solution and filtered, and the filtrate obtained is repeatedly used as the extraction solvent for selectively extracting the zinc component.
Citation Information
Patent Citations
Method for recovering zn from zn containing material
JP1986261446A
Treatment process of heavy metal in waste
JP2002011429A
Selective leaching and recovery of zinc from complex sulfide deposits, tailings, crushed ore, or mine sludge.
JP2013542321A
Method for fixing arsenic
JP2017115196A
Manufacturing method of zinc bullion
JP2019119895A