Method for manufacturing power transmission cable using halogen-free flame-retardant resin composition

A non-halogen flame-retardant resin composition for power transmission cables, using magnesium hydroxide, aluminum hydroxide, or silica, addresses the challenge of maintaining heat aging characteristics during steam crosslinking, ensuring efficient production and improved mechanical properties.

JP7565696B2Active Publication Date: 2024-10-11PROTERIAL LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020042060
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-03-11
Publication Date
2024-10-11
Estimated Expiration
2040-03-11

AI Technical Summary

Technical Problem

Existing methods for manufacturing power transmission cables using non-halogen flame-retardant resin compositions face challenges in maintaining good heat aging characteristics when crosslinking is done through direct steam contact, leading to undesirable products that reduce heat aging elongation retention below predetermined standards.

Method used

A method involving a non-halogen flame-retardant resin composition for the sheath layer, comprising a base polymer and flame retardants like magnesium hydroxide, aluminum hydroxide, or silica, with specific ratios, is used for crosslinking by direct steam contact, avoiding the need for protective layers and reducing the formation of undesirable products.

Benefits of technology

This method ensures the production of power transmission cables with excellent heat aging characteristics and improved mechanical properties, maintaining flexibility over time without the need for protective layers, thus enhancing production efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007565696000002
    Figure 0007565696000002
  • Figure 0007565696000003
    Figure 0007565696000003
  • Figure 0007565696000001
    Figure 0007565696000001
Patent Text Reader

Abstract

To provide a method for producing a power transmission cable using a non-halogen flame-retardant resin composition which shows good thermal aging characteristics even when steam crosslinking is performed.SOLUTION: Provided is a method for producing a power transmission cable in which a sheath layer is crosslinked by making it contact with steam, where the sheath layer 9 is formed of a non-halogen flame-retardant resin composition comprising a base polymer and a flame retardant, where the flame retardant is one of magnesium hydroxide alone, aluminum hydroxide alone, silica alone, co-use of magnesium hydroxide and aluminum hydroxide, co-use of aluminum hydroxide and silica, and a content thereof is 50 pts.mass or more relative to 100 pts.mass of the base polymer. With such a sheath layer, even when steam crosslinking is performed by a steam pipe 240, magnesium silicate is not generated and lowering of a residual elongation rate after a thermal aging can be suppressed. Further, a power transmission cable can be produced efficiently without using a protective layer for suppressing generation of magnesium silicate.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a power transmission cable using a halogen-free flame-retardant resin composition. [Background technology]

[0002] Cables used in railroad vehicles and other vehicles are required to have properties such as flame retardancy and low smoke emission to minimize damage in the event of a fire. To achieve high flame retardancy, materials are used in which halogen-based flame retardants such as chlorine-based or bromine-based ones are added to polyolefin. However, substances that contain large amounts of these halogen-based flame retardants generate large amounts of toxic and harmful gases when burned, and depending on the incineration conditions, they can generate highly toxic dioxins. For this reason, cables that use non-halogen materials (halogen-free materials) as coating materials that do not contain halogen substances are becoming more common, from the perspective of fire safety and reducing environmental impact.

[0003] For example, Patent Document 1 discloses a power transmission cable that uses, as a sheath layer, a base polymer containing an ethylene-vinyl acetate copolymer with a vinyl acetate content of 50% by weight or more, and a non-halogen flame-retardant resin composition that contains 100 to 180 parts by mass of metal hydrate and silica in total per 100 parts by mass of the base polymer, in order to achieve high flame retardancy and low smoke generation. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2016-100140 A Summary of the Invention [Problem to be solved by the invention]

[0005] The present inventors are engaged in the research and development of covering materials for power transmission cables, and are investigating a resin composition as a covering material that is halogen-free and has good properties.

[0006] In particular, power transmission cables are required to maintain good flexibility for a long period of time. To evaluate the flexibility life of power transmission cables, they are required to have heat aging properties that satisfy a certain standard in the "heat aging elongation retention rate" based on a heat aging test.

[0007] In addition, when crosslinking the sheath layer, which is the outermost covering material of a power cable, by heat, the heat of steam may be used. In such a crosslinking method using the heat of steam, a protective layer with good thermal conductivity may be provided on the outside of the power cable to prevent deterioration due to direct contact with steam, and then crosslinking is performed. In such a crosslinking method, a step of providing a protective layer on the outside of the sheath layer and a step of peeling off the protective layer on the outside of the sheath layer are required before and after crosslinking, respectively.

[0008] Therefore, if steam can be brought into direct contact with the sheath layer to perform crosslinking, the steps of providing a protective layer on the outside of the sheath layer and peeling off the protective layer on the outside of the sheath layer will be unnecessary, improving production efficiency.

[0009] However, when crosslinking is performed by directly contacting the sheath layer with steam, there is a problem that the direct contact with steam causes deterioration, resulting in undesirable products that deteriorate the heat aging properties, i.e., the "heat aging elongation retention rate" cannot meet a predetermined standard.

[0010] Therefore, an object of the present invention is to provide a method for producing a power transmission cable using a halogen-free flame-retardant resin composition that has good heat aging properties even when a crosslinking method involving direct contact with steam is used. [Means for solving the problem]

[0011] [1] A method for producing a power transmission cable using a halogen-free flame-retardant resin composition according to one embodiment of the present invention includes the steps of (a) coating a core having a conductor and an insulating layer formed around the conductor with a halogen-free flame-retardant resin composition to form a sheath layer, and (b) cross-linking the sheath layer by contacting it with water vapor. The sheath layer is made of a halogen-free flame-retardant resin composition containing a base polymer and a flame retardant, and the flame retardant is any one of magnesium hydroxide alone, aluminum hydroxide alone, silica alone, a combination of magnesium hydroxide and aluminum hydroxide, and a combination of aluminum hydroxide and silica, and the content of the flame retardant is 50 parts by mass or more per 100 parts by mass of the base polymer.

[0012] [2] In the composition according to [1], the base polymer comprises an ethylene vinyl acetate copolymer.

[0013] [3] In the composition according to [1], the content of the flame retardant is 100 parts by mass or more and 150 parts by mass or less per 100 parts by mass of the base polymer.

[0014] [4] [1] In the above-mentioned sheath layer, the tensile elongation retention rate after a heat aging test at 120°C for 168 hours is 75% or more.

[0015] [5] A method for manufacturing a power transmission cable using a halogen-free flame-retardant resin composition according to one embodiment of the present invention includes the steps of: forming an internal semiconductive layer, an insulating layer, and an external semiconductive layer around the outer periphery of a conductor, in that order from the inside; forming a shielding layer by winding a wire around the outer periphery of the external semiconductive layer; forming a pressure tape layer by winding a pressure tape around the outer periphery of the shielding layer; and forming a sheath layer around the outer periphery of the pressure tape layer, wherein the step of forming the sheath layer includes: (a) coating the outer periphery of the pressure tape layer with a halogen-free flame-retardant resin composition that will become the sheath layer; and (b) cross-linking the sheath layer by contacting it with water vapor, wherein the sheath layer is made of a halogen-free flame-retardant resin composition containing a base polymer and a flame retardant, and the flame retardant is any one of magnesium hydroxide alone, aluminum hydroxide alone, silica alone, a combination of magnesium hydroxide and aluminum hydroxide, or a combination of aluminum hydroxide and silica, and the content of the flame retardant is 50 parts by mass or more per 100 parts by mass of the base polymer. Effect of the Invention

[0016] According to the method for producing a power transmission cable using the halogen-free flame-retardant resin composition of one embodiment of the present invention, a power transmission cable with good heat aging properties can be produced even when a crosslinking method involving direct contact with steam is used. [Brief description of the drawings]

[0017] [Figure 1] FIG. 2 is a cross-sectional view showing a configuration of a power transmission cable. [Diagram 2] FIG. 1 is a schematic diagram showing a power transmission cable manufacturing apparatus. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] (Embodiment) A method for producing a power transmission cable according to the present embodiment will be described below. Fig. 1 is a cross-sectional view showing a configuration of a power transmission cable. In the present embodiment, the method for producing the power transmission cable shown in Fig. 1 will be described as an example.

[0019] The power transmission cable shown in Figure 1 has a conductor 2 made of twisted wire, an internal semiconductive layer 3 formed on the outer periphery of the conductor 2, an insulating layer 4 formed on the outer periphery of the internal semiconductive layer 3, an external semiconductive layer 5 formed on the outer periphery of the insulating layer 4, a semiconductive tape layer 6 formed on the outer periphery of the external semiconductive layer 5, a shielding layer 7 formed on the outer periphery of the semiconductive tape layer 6, a pressure tape layer 8 formed on the outer periphery of the shielding layer 7, and a sheath layer 9 formed on the outer periphery of the pressure tape layer 8.

[0020] First, the inner semiconductive layer 3, the insulating layer 4, and the outer semiconductive layer 5 are simultaneously extruded around the conductor 2. Alternatively, the inner semiconductive layer 3, the insulating layer 4, and the outer semiconductive layer 5 may be extruded in sequence.

[0021] The conductor 2 is formed by twisting together a plurality of metal wires. The wires may be metal-plated, and may be made of, for example, tin-plated soft copper wire. The conductor 2 transmits a high voltage of, for example, 7000V or more.

[0022] The inner semiconductive layer 3 and the outer semiconductive layer 5 are made of a material that is made conductive by dispersing conductive powder such as carbon in rubber such as ethylene propylene rubber or butyl rubber. The inner semiconductive layer 3 and the outer semiconductive layer 5 are provided to reduce the concentration of the electric field between the insulating layer 4 and the conductor 2 and between the insulating layer 4 and the shielding layer 7.

[0023] The insulating layer 4 is made of a material such as ethylene propylene rubber, vinyl chloride, cross-linked polyethylene, silicone rubber, or a fluorine-based material.

[0024] Next, a semiconductive tape is spirally wound around the outer periphery of the external semiconductive layer 5 along the cable axial direction to form a semiconductive tape layer 6. As the semiconductive tape, for example, one formed by impregnating a base fabric or nonwoven fabric in which warp and weft threads made of nylon, rayon, PET, or the like are woven with rubber such as ethylene propylene rubber or butyl rubber in which conductive powder such as carbon is dispersed, can be used. As the semiconductive tape, for example, one having a thickness of 0.1 mm to 0.4 mm and a width of 30 mm to 70 mm can be used. The semiconductive tape may be wound in an overlapping manner, for example, by overlapping 1 / 4 to 1 / 2 of the tape width.

[0025] Next, a wire is wound helically around the outer circumference of the semiconductive tape layer 6 along the cable axial direction to form the shielding layer 7. The wire is made of a conductive material such as tin-plated soft copper, and may be a wire rod with a diameter of 0.4 mm to 0.6 mm. This shielding layer 7 is connected to the ground when in use.

[0026] Next, a pressure tape is spirally wound around the outer periphery of the shielding layer 7 in the axial direction of the cable to form a pressure tape layer 8. As the pressure tape, for example, a tape made of plastic or rayon having a thickness of 0.03 mm to 0.2 mm and a width of 50 mm to 90 mm can be used.

[0027] The laminate from the conductor 2 to the holding tape layer 8 is referred to as a core portion C.

[0028] Next, a halogen-free flame-retardant resin composition is extrusion molded onto the outer periphery of the core portion C (pressing tape layer 8) to form the sheath layer 9. Thereafter, the sheath layer 9 is crosslinked.

[0029] The halogen-free flame-retardant resin composition constituting the sheath layer 9 contains a base polymer (resin component) and a flame retardant (metal hydroxide, silica).

[0030] The base polymer contains, for example, an ethylene-vinyl acetate copolymer (EVA) and an ethylene-α-olefin copolymer modified with maleic anhydride (hereinafter, also simply referred to as a "maleic acid modified ethylene copolymer").

[0031] The ethylene vinyl acetate copolymer (EVA) in the base polymer may have a vinyl acetate content of 40% by mass or more. By making the vinyl acetate content 40% by mass or more, the cinders become stronger, and good flame retardancy and low smoke generation can be obtained.

[0032] In the ethylene-α-olefin copolymer modified with maleic anhydride in the base polymer, an α-olefin having 3 to 8 carbon atoms can be used as the α-olefin, taking into consideration the flexibility of the cable. Examples of such α-olefins include propylene, 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, etc., and isomers can also be used. In addition, the α-olefins may be used alone or in combination of two or more kinds.

[0033] As the base polymer, styrene-butadiene rubber may be added to ethylene-vinyl acetate copolymer (EVA) and ethylene-α-olefin copolymer modified with maleic anhydride.

[0034] The flame retardant may be a metal hydroxide or silica.

[0035] As the metal hydroxide, magnesium hydroxide or aluminum hydroxide can be used. As such a metal hydroxide, one that has been surface-treated with silane can be used. For example, magnesium hydroxide that has been surface-treated with a silane coupling agent or aluminum hydroxide that has been surface-treated with a silane coupling agent can be used. By using a surface-treated product that uses a silane coupling agent, mechanical properties (tensile strength, elongation) become good.

[0036] Either amorphous silica or crystalline silica may be used. This silica is used to solidify the cinders during combustion and to improve mechanical properties. The silica is spherical in shape and has an average particle size of 0.05 μm or more and 1.0 μm or less. A more preferable average particle size is 0.15 μm or more and 0.3 μm or less. By using such silica in combination with a metal hydroxide, it is possible to balance flame retardancy, low smoke generation, and mechanical properties. In particular, by making the silica spherical, the silica penetrates between the metal hydroxides, improving the dispersibility of the metal hydroxide. In addition, by making the average particle size of the silica 0.05 μm or more and 1.0 μm or less, the interaction with the polymer becomes appropriate, and the mechanical properties are improved. The average particle size of the silica can be the value of the particle size D50 median size (μm) at which the cumulative frequency is exactly 50%. The shape of the silica (whether it is spherical or not) can be confirmed by an electron microscope.

[0037] In this embodiment, the flame retardant used is any one of (a1) magnesium hydroxide alone, (a2) aluminum hydroxide alone, (a3) ​​silica alone, (a4) magnesium hydroxide and aluminum hydroxide in combination, and (a5) aluminum hydroxide and silica in combination. The amount of the flame retardant added is 50 parts by mass or more, more preferably 100 parts by mass or more and 150 parts by mass or less, per 100 parts by mass of the base polymer.

[0038] In this way, by selecting the flame retardant from the above (a1) to (a5) and avoiding the combined use of magnesium hydroxide and silica, it is possible to suppress the decrease in heat aging elongation retention even when steam crosslinking, which will be described later, is performed. In other words, it is possible to suppress the decrease in mechanical properties after a heat aging test. A heat aging test can be considered as a type of accelerated test, and good properties after a heat aging test are an indicator that mechanical properties (e.g., flexibility) can be maintained for a long period of time.

[0039] (a4) When magnesium hydroxide and aluminum hydroxide are used in combination, the mass ratio of aluminum hydroxide:magnesium hydroxide is preferably 40:60 to 60:40. This is because a stepwise dehydration method is more effective for suppressing temperature rise and solidifying the cinders during combustion of a halogen-free flame-retardant resin composition. Since the dehydration start temperature of aluminum hydroxide is around 210°C and that of magnesium hydroxide is around 280°C, stepwise dehydration occurs in the order of aluminum hydroxide and magnesium hydroxide, effectively suppressing temperature rise in the sheath layer and solidifying the cinders.

[0040] Of the above flame retardants, magnesium hydroxide, aluminum hydroxide and silica all contribute to flame retardancy and low smoke generation, with magnesium hydroxide and aluminum hydroxide contributing more to flame retardancy and silica contributing more to low smoke generation due to solidification of the cinders.

[0041] The halogen-free flame-retardant resin composition used in the power transmission cable may also contain other polymers (other EVAs, other polyolefins modified with maleic acid or the like, unmodified polyolefins, etc.), crosslinking agents, crosslinking assistants, colorants, lubricants, antioxidants, etc., as necessary.

[0042] For example, a peroxide may be used as a crosslinking agent. Carbon may be used as a coloring agent. A stearate compound may be used as a lubricant. By adding a lubricant, the processability during extrusion can be improved.

[0043] FIG. 2 is a schematic diagram showing a manufacturing apparatus for a power cable. The single-screw extruder 200 shown in FIG. 2 includes a screw 220 disposed in a cylinder and a material inlet 221. The above-mentioned halogen-free flame-retardant resin composition is charged from the material inlet (hopper) 221 as a material for the sheath layer 9. The above-mentioned halogen-free flame-retardant resin composition is melted, extruded from the extruder 200, passes through the extrusion head 230, and is coated on the core part C sent out from the sending machine. Next, the core part C and the sheath layer 9 around it are crosslinked while passing through a steam pipe (crosslinking pipe) 240. Using such a continuous crosslinking device, the sheath layer 9 is directly brought into contact with water vapor to perform crosslinking (crosslinking is performed by passing through water vapor). For example, crosslinking is performed for 5 minutes to 60 minutes in a water vapor atmosphere at 150° C. to 180° C. In this manner, the power cable 1 can be manufactured.

[0044] As described above, according to the manufacturing method of the power transmission cable 1 of the present embodiment, a composite of magnesium hydroxide and silica is not used as a flame retardant, but a flame retardant is selected from the above (a1) to (a5). This makes it possible to avoid the production of magnesium silicate, which is an undesirable reaction product of magnesium hydroxide and silica that occurs during vapor crosslinking, and suppresses the decrease in the elongation retention rate (%) after thermal aging.

[0045] As described above, the power cable manufacturing method of the present embodiment can manufacture a power cable using a halogen-free flame-retardant resin composition having excellent thermal aging properties. Also, the power cable manufacturing method of the present embodiment can manufacture a power cable efficiently without using a protective layer for suppressing the generation of undesired reactants.

[0046] Here, in the power transmission cable according to the present embodiment, the outer diameter (diameter) is, for example, not less than 30 mm and not more than 60 mm, and the thickness of the sheath layer is, for example, not less than 2 mm and not more than 4 mm.

[0047] Furthermore, the power transmission cable according to the present embodiment can be used, for example, as an extra-high voltage cable arranged in a railway vehicle (hereinafter referred to as an extra-high voltage cable for railway vehicles). The extra-high voltage cable for railway vehicles is arranged along the roof or walls so as to connect, for example, a pantograph arranged on the roof of the railway vehicle and a multi-voltage device arranged under the floor. Here, the extra-high voltage refers to a voltage of 7000V or more.

[0048] [Example] The halogen-free flame-retardant resin composition used in the power transmission cable of the present embodiment will be described more specifically below with reference to examples. (Material name) 1) EVA: LANXESS "Revaprene 600HV" (VA content: 60% by mass) 2) Acid-modified polyolefin: Acid-modified ethylene-α-olefin copolymer, "Tafmer MH5040" manufactured by Mitsui Chemicals 3) Magnesium hydroxide: Huber's "Magnifin H10A" (vinyl silane 0.8-1.1 μm) 4) Aluminum hydroxide: Nippon Light Metal Co., Ltd. "BF013STV" (silane 1.0 μm) 5) Silica: Elkem's "Sidistar T120U" (spherical, average particle size 0.15 μm) 6) t-Butylperoxy 2-ethylhexyl carbonate: Nouryon "Trigonox 117" 7) Triallyl isocyanate: "TAIC" manufactured by Nippon Kasei 8) Zinc oxide: "Zinc Oxide No. 3" manufactured by Sakai Chemical Industry 9) Blended antioxidant: Adeka AO-18 (AO20 / 412S=6 / 4) 10) Carbon: "FT Carbon" manufactured by Asahi Carbon Co., Ltd. 11) Lithium hydroxstearate: "LS-6" manufactured by Nitto Kasei Kogyo Co., Ltd. 12) Zinc stearate: "EZ-101" manufactured by Nitto Kasei Kogyo Co., Ltd. (Examples 1 to 5) A halogen-free flame-retardant resin composition was prepared according to the component composition shown in Table 1, kneaded using a roll, and then molded into a sheet shape with a thickness of 1 mm. The molded sheet was subjected to steam crosslinking using a crosslinking tube. Specifically, the sheet (kneaded halogen-free flame-retardant resin composition) was directly contacted with steam (water vapor) having a saturated water vapor pressure of 1 MPa, and crosslinking was performed at 180°C for 10 minutes to obtain a steam-crosslinked sheet.

[0049] (Comparative Examples 1 to 3) The component composition was changed as shown in Table 1, and steam-crosslinked sheets were obtained in the same manner as in Examples 1 to 5.

[0050] The amount of each component shown in Table 1 is shown in parts by mass relative to 100 parts by mass of the total base polymer.

[0051] [Table 1]

[0052] The mechanical properties of the obtained sheet before and after the heat aging test were evaluated by tensile tests in accordance with the ICE 60811-1-1 and ICE 60811-1-2 standards as described below.

[0053] The obtained sheet was punched out using a No. 6 dumbbell to prepare a test piece with a gauge length of 20 mm. This test piece was pulled at a tensile speed of 200 mm / min, and the gauge length after break was measured. The gauge length after break was determined by butting the test piece after break to determine the gauge length. The elongation (%) before heat aging was calculated using the following formula.

[0054] Elongation before heat aging (%) = 100 × gauge length after break (mm) / 20 (mm) The obtained sheet was exposed to an oven at 120°C for 168 hours, and then punched out using a No. 6 dumbbell to prepare a test piece with a gauge length of 20 mm. The test piece was subjected to a tensile test at a tensile speed of 200 mm / min to measure the elongation at the breaking point. The elongation (%) after heat aging was calculated using the following formula.

[0055] Elongation after heat aging (%) = 100 x gauge length after break (mm) / 20 (mm) Furthermore, the elongation retention (%) after heat aging was calculated using the following formula.

[0056] Elongation retention after heat aging (%) = 100 × elongation after heat aging (%) / elongation before heat aging (%) Table 1 shows the elongation (%) before heat aging and the elongation retention (%) after heat aging.

[0057] A specimen with a residual elongation rate (%) of 75% or more after heat aging was rated as "passed", and a specimen with a residual elongation rate of less than 75% was rated as "failed".

[0058] As shown in Table 1, all of the sheets of Examples 1 to 5 had a post-heat aging elongation retention (%) of 75% or more, and thus had good heat aging properties.

[0059] Specifically, in Example 1, (a5) a composite of aluminum hydroxide and silica was used as the flame retardant, and the elongation retention (%) after heat aging was 75% or more, and the heat aging properties were good.

[0060] In Example 2, (a4) a complex of magnesium hydroxide and aluminum hydroxide was used as the flame retardant, and the elongation retention (%) after heat aging was 75% or more, and the heat aging properties were good.

[0061] In Example 3, (a3) ​​silica was used alone as the flame retardant, and the elongation retention (%) after heat aging was 75% or more, indicating good heat aging properties.

[0062] In Example 4, (a1) magnesium hydroxide was used alone as the flame retardant, and the elongation retention (%) after heat aging was 75% or more, indicating good heat aging properties.

[0063] In Example 5, (a2) aluminum hydroxide was used alone as the flame retardant, and the elongation retention (%) after heat aging was 75% or more, indicating good heat aging properties.

[0064] Furthermore, in the above Examples 1 to 5, the amount of flame retardant added was 50 parts by mass or more per 100 parts by mass of the base polymer. In Examples 1, 2, 4, and 5, in which the amount of flame retardant added was large, i.e., 100 parts by mass or more per 100 parts by mass of the base polymer, the elongation retention (%) after heat aging was 90% or more, and the heat aging properties were better.

[0065] In contrast, in Comparative Examples 1 to 3, a composite of magnesium hydroxide and silica was used as the flame retardant, and all of them had low elongation retention (%) after heat aging of less than 75%, indicating poor heat aging properties. In these Comparative Examples, the amount of flame retardant added was 100 parts by mass or more relative to 100 parts by mass of the base polymer, but the elongation retention (%) after heat aging was low.

[0066] Such a decrease in the elongation retention (%) after heat aging is due to the formation of magnesium silicate, which is an undesirable reaction product of magnesium hydroxide and silica during steam crosslinking.

[0067] Therefore, as shown in the above (a1) to (a5), by avoiding the combined use of magnesium hydroxide and silica and blending a flame retardant, the elongation retention (%) after heat aging can be improved and the heat aging properties can be improved.

[0068] Here, when performing the above-mentioned vapor crosslinking, in order to suppress the generation of undesirable reaction products due to vapor, it is also possible to deal with this by covering the sheath layer with a protective layer as described above, performing vapor crosslinking, and then peeling off the protective layer; however, in this case, a process of forming and peeling off the protective layer is required, which reduces production efficiency.

[0069] In contrast, according to the present embodiment, by adjusting the combination of flame retardants as described above, even if vapor crosslinking is performed, undesired reactants (magnesium silicate) are not generated, and the production efficiency can be improved while suppressing the decrease in heat aging elongation retention.

[0070] The test pieces used in the present examples correspond to, for example, power transmission cables whose sheath layers have been stripped off and punched out with the dumbbell.

[0071] (Application example) In the above embodiment, the power transmission cable is formed of a plurality of laminates as shown in Fig. 1, but the power transmission cable may have an insulated electric wire having a conductor 2 and an insulating layer 4 provided around the conductor 2 as a core layer, and a sheath layer 9 provided around the core layer. Also, a plurality of insulated electric wires may be used as the core layer. As the sheath layer of the power transmission cable having such a configuration, the above-mentioned halogen-free flame-retardant resin composition may be used, and a sheath layer may be formed around the core layer in the same manner as in the above embodiment.

[0072] The present invention is not limited to the above-described embodiment and examples, and various modifications can be made without departing from the spirit and scope of the present invention. [Explanation of symbols]

[0073] 1. Power Cables 2 Conductors 3. Inner semiconducting layer 4. Insulation Layer 5. Outer semiconducting layer 6 Semiconductive Tape Layers 7 Shielding layer 8. Holding Tape Layer 9 Sheath layer 200 Extruder 220 Screw 221 Material inlet (hopper) 230 Extrusion Head 240 Steam pipe (bridge pipe) C Core

Claims

1. (a) a step of coating a core portion having a conductor and an insulating layer formed on the outer periphery of the conductor with a halogen-free flame-retardant resin composition to form a sheath layer; (b) crosslinking the sheath layer by contacting it with water vapor; having the sheath layer is made of a halogen-free flame-retardant resin composition containing a base polymer and a flame retardant; The flame retardant is A combination of aluminum hydroxide and silica (excluding combination with magnesium hydroxide and silica), The content of the flame retardant is 150 parts by mass relative to 100 parts by mass of the base polymer, The method for producing a power transmission cable using the halogen-free flame-retardant resin composition, wherein the sheath layer has a tensile elongation retention of 75% or more after a heat aging test at 120°C for 168 hours.

2. (a) a step of coating a core portion having a conductor and an insulating layer formed on the outer periphery of the conductor with a halogen-free flame-retardant resin composition to form a sheath layer; (b) crosslinking the sheath layer by contacting it with water vapor; having the sheath layer is made of a halogen-free flame-retardant resin composition containing a base polymer and a flame retardant; The flame retardant is Silica alone, The content of the flame retardant is 50 parts by mass relative to 100 parts by mass of the base polymer, The method for producing a power transmission cable using the halogen-free flame-retardant resin composition, wherein the sheath layer has a tensile elongation retention of 75% or more after a heat aging test at 120°C for 168 hours.

3. A method for producing a power transmission cable using the halogen-free flame-retardant resin composition according to claim 1 or 2, The method for producing a power transmission cable uses a halogen-free flame-retardant resin composition, wherein the base polymer contains an ethylene-vinyl acetate copolymer.

4. forming an inner semiconductive layer, an insulating layer and an outer semiconductive layer on the outer periphery of the conductor in this order from the inside; forming a shielding layer by winding a wire around the outer semiconducting layer; forming a pressure tape layer by winding a pressure tape around an outer periphery of the shielding layer; forming a sheath layer on the outer periphery of the pressing tape layer; The step of forming the sheath layer includes: (a) a step of coating an outer periphery of the pressing tape layer with a halogen-free flame-retardant resin composition which will become the sheath layer; (b) crosslinking the sheath layer by contacting it with water vapor; Including, the sheath layer is made of a halogen-free flame-retardant resin composition containing a base polymer and a flame retardant; The flame retardant is A combination of aluminum hydroxide and silica (excluding combination with magnesium hydroxide and silica), The content of the flame retardant is 150 parts by mass relative to 100 parts by mass of the base polymer, The method for producing a power transmission cable using the halogen-free flame-retardant resin composition, wherein the sheath layer has a tensile elongation retention of 75% or more after a heat aging test at 120°C for 168 hours.

5. forming an inner semiconductive layer, an insulating layer and an outer semiconductive layer on the outer periphery of the conductor in this order from the inside; forming a shielding layer by winding a wire around the outer semiconducting layer; forming a pressure tape layer by winding a pressure tape around an outer periphery of the shielding layer; forming a sheath layer on the outer periphery of the pressing tape layer; The step of forming the sheath layer includes: (a) a step of coating an outer periphery of the pressing tape layer with a halogen-free flame-retardant resin composition which will become the sheath layer; (b) crosslinking the sheath layer by contacting it with water vapor; Including, the sheath layer is made of a halogen-free flame-retardant resin composition containing a base polymer and a flame retardant; The flame retardant is Silica alone, The content of the flame retardant is 50 parts by mass relative to 100 parts by mass of the base polymer, The sheath layer has a tensile elongation retention of 75% or more after a heat aging test at 120°C for 168 hours. A method for producing a power transmission cable using a halogen-free flame-retardant resin composition.

Citation Information

Patent Citations

  • Insulated wire

    JP2002042574A

  • Insulated wire and method for production the same

    JP2012087238A

  • Insulated electric wire for vehicle and cable for vehicle

    JP2014011140A

  • Power transmission cable using non-halogen flame-retardant resin composition

    JP2016100140A

  • Non-halogen flame retardant insulation wire and non-halogen flame retardant cable

    JP2017004798A