Luminous marker particles

By optimizing the surface group ratio in luminescent marker nanoparticles, stability and biomolecule-binding are enhanced, addressing aggregation issues and improving assay sensitivity.

JP7565914B2Active Publication Date: 2024-10-11SUMITOMO CHEM CO LTD
View PDF 18 Cites 0 Cited by

Patent Information

Application Number
JP2021515076
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-08-08
Filing Date
2019-09-09
Publication Date
2024-10-11
Estimated Expiration
2039-09-09

AI Technical Summary

Technical Problem

Existing luminescent marker particles face challenges in maintaining stability and preventing aggregation, particularly in aqueous solutions commonly used in biological assays, which affects their performance in applications such as flow cytometry.

Method used

The development of luminescent marker nanoparticles with a specific ratio of polar and biomolecule-binding surface groups, where the molar ratio of inert polar groups to biomolecule-binding groups is greater than 90:10, ensures the formation of stable colloids that maintain the ability to bind biomolecules effectively.

Benefits of technology

This configuration enhances the stability and biomolecule-binding capacity of the nanoparticles, leading to improved performance in assays like flow cytometry with reduced aggregation and increased sensitivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007565914000021
    Figure 0007565914000021
  • Figure 0007565914000022
    Figure 0007565914000022
  • Figure 0007565914000023
    Figure 0007565914000023
Patent Text Reader

Abstract

A luminescent marker particle has a luminescent particle core containing a luminescent material and first and second surface groups attached to the luminescent particle core. The first surface group contains a polar group and is an inert group that does not bind to biomolecules. The second surface group contains a biomolecule-binding group. [Selected Figure] Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Background technology]

[0001] In some embodiments, the present disclosure provides luminescent marker particles, optionally luminescent marker nanoparticles, for use as markers in biosensor applications.

[0002] Nanoparticles of silica and luminescent materials have been disclosed as labels or detection reagents.

[0003] WO 2018 / 060722 discloses composite particles comprising a mixture of silica and a light-emitting polymer having polar groups.

[0004] Estevez, MC. et al. 'Highly Fluorescent Dye-Doped Silica Nanoparticles Increase Flow Cytometry Sensitivity for Cancer Cell Monitoring' Nano. Res. 2009, 2, 448-461 discloses dye-doped silica nanoparticles functionalized with polyethylene glycol.

[0005] US 2010 / 209946 discloses silica nanoparticles functionalized with water-dispersing groups, shielding groups and biomolecule binding groups.

[0006] In Nanoscale, 2013, vol. 5, pp 8593-8601, Geng et al. describe silica-conjugated polymer (CP) nanoparticles in which the LEPs have pendant non-polar alkyl side chains and the nanoparticles have a “SiO2@CP@SiO2” structure.

[0007] Behrendt et al. J. Mater. Chem., 2013, vol. 1, pp 3297-3304, describe silica-LEP nanoparticles in which LEP is covalently bonded to silica. The light-emitting polymer has alkoxysilane groups pendant from the polymer backbone that react with silica monomers during the formation of the nanoparticles.

[0008] Nanoscale Res. Lett., 2011, vol. 6, p 328, discloses the entrapment of small molecules in silica matrices.

[0009] Langmuir, 1992, vol. 8, pp 2921-2931, discloses the coupling of dyes to silane coupling agents which are incorporated into silica spheres.

[0010] Chem. Mater., 2014, vol. 26, pp1874-1880, Geng et al. disclose poly(9,9-dihexylfluorene-alt-2,1,3-benzothiadiazole) (PFBT)-loaded nanoparticles. [Prior art documents] [Patent documents]

[0011] [Patent Document 1] International Publication No. 2018 / 060722 [Patent Document 2] US Patent No. 2010 / 209946 [Non-patent literature]

[0012] [Non-Patent Document 1] Estevez,MC.et al.'Highly Fluorescent Dye-Doped Silica Nanoparticles Increase Flow Cytometry Sensitivity for Cancer Cell Monitoring' Nano.Res.2009,2,448-461 [Non-Patent Document 2] Nanoscale,2013,vol.5,pp8593-8601,Geng et al. [Non-Patent Document 3] Behrendt et al.J.Mater.Chem.,2013,vol.1,pp3297-3304 [Non-Patent Document 4] Nanoscale Res.Lett.,2011,vol.6,p 328 [Non-Patent Document 5] Langmuir,1992,vol.8,pp2921-2931 [Non-Patent Document 6] Chem.Mater.,2014,vol.26,pp1874-1880,Geng et al. Summary of the Invention

[0013] A summary of the aspects of the specific embodiments disclosed herein is set forth below. It should be understood that these aspects are merely presented to provide the reader with a brief summary of these specific embodiments, and are not intended to limit the scope of the present disclosure. In fact, the present disclosure may encompass various aspects and / or combinations of aspects that may not be described.

[0014] Luminescent particles configured to bind to biomolecules to form colloids that are stable, and in particular do not aggregate during use and / or storage, are desirable. The inventors have found that maintaining the stability of such colloids is particularly troublesome in aqueous solutions, such as aqueous buffers, commonly used in biological assays.

[0015] The inventors have found that stable colloids containing luminescent marker nanoparticles can be formed from particles having polar surface groups with biomolecule binding groups and surface groups without biomolecule binding groups, while maintaining the ability of the luminescent marker particles to bind biomolecules.

[0016] Thus, in some embodiments, a luminescent marker particle is provided having a luminescent particle core containing a luminescent material and first and second surface groups attached to the luminescent particle core. The first surface group contains a polar group and is inert. The second surface group contains a biomolecule binding group.

[0017] In some embodiments, the molar ratio of first surface groups:second surface groups is greater than 90:10.

[0018] The aforementioned aggregation problem can be exacerbated in luminescent particles in which the luminescent material is a polymer. However, the inventors have found that good stability can be achieved using surface groups as described herein for luminescent cores containing luminescent polymers. Thus, in some embodiments, the luminescent material is a luminescent polymer.

[0019] In some embodiments, the nanoparticle core contains an inorganic matrix, which can be an inorganic oxide, optionally silica.

[0020] The inventors have found that marker particles having surface groups with and without biomolecule binding groups can be formed such that the ratio of biomolecule binding groups to non-biomolecule binding groups can be controlled, and this ratio can be selected to balance the colloidal stability of the particle with the biomolecule binding capacity of the particle.

[0021] Thus, in some embodiments, a method is provided for forming a luminescent marker particle, in which a luminescent particle core having a plurality of first reactive groups attached to its surface is reacted with first and second reactive compounds to form the first and second surface groups, respectively, or to form precursors to first and second surface groups that may undergo one or more additional reactions to form the first and second surface groups.

[0022] The particles may, for example, be dispersed in a liquid for use in an assay.

[0023] Thus, in some embodiments, a colloidal suspension is provided that includes particles suspended in a liquid.

[0024] The particles can be used to mark biomolecules, for example to track or detect the biomolecules. Thus, in some embodiments, a method of marking a biomolecule is provided that includes binding the biomolecule to a particle.

[0025] In some embodiments, a method of assaying a target analyte is provided that includes contacting a sample with a luminescent marker particle described herein and determining any binding of the target analyte to the luminescent marker.

[0026] The sample contacted with the luminescent marker particles may be analyzed by flow cytometry.

[0027] The amount of target analyte bound to the light-emitting marker particles may be determined.

[0028] The sample may contain a mixture of cells, and one or more different types of target cells bound to a luminescent marker may be identified and / or quantified.

[0029] The present disclosure will be described in conjunction with the accompanying figures. It is emphasized that, according to standard industry practice, various features are not drawn to scale. In fact, dimensions of various features may be arbitrarily increased or decreased for clarity of illustration.

[0030] In the accompanying figures, similar components and / or features may have the same reference label. Furthermore, various components of the same type may be distinguished by following the reference label with a dash and a second label that distinguishes the similar components. When only a first reference label is used in this specification, the description may apply to any one of the similar components having the same first reference label, regardless of the second reference label.

[0031] The invention will now be described in more detail with reference to the following drawings, in which: [Brief description of the drawings]

[0032] [Figure 1] 1 is a schematic diagram of a nanoparticle according to some embodiments. [Diagram 2] 1 is a schematic diagram of a method of forming nanoparticles, according to some embodiments. [Diagram 3] 1 is a graph of the signal-to-noise ratio for luminescent nanoparticles in which 0.1.1 and 10 mol % of the nanoparticle surface groups contain biotin binding groups. [Figure 4] 1 is a graph of the rate of change of Z-average diameter versus time for nanoparticles having methoxy-terminated surface groups dispersed in a buffer solution. [Diagram 5] 1 is a graph of the rate of change of Z-average diameter versus time for nanoparticles with carboxy-terminated surface groups dispersed in a buffer solution. [Figure 6] 1 is a staining index chart of Cyto-Trol cells stained with a biotinylated dissolved luminescent polymer marker according to an embodiment of the present disclosure conjugated to an anti-human CD4 antibody via streptavidin, and a comparative luminescent nanoparticle conjugated to the same antibody. [Figure 7] FIG. 7 is a staining index chart of Cyto-Trol cells stained with streptavidin-conjugated nanoparticles, isotype-conjugated luminescent nanoparticles, and non-streptavidin-conjugated luminescent nanoparticles of FIG. 6. [Figure 8] 1 is a staining index chart of Cyto-Trol cells stained with biotinylated nanoparticles according to an embodiment of the present disclosure conjugated to anti-human CD4 antibody via neutravidin and a comparative dissolved luminescent polymer marker conjugated to the same antibody. [Figure 9] FIG. 9 is a staining index chart of Cyto-Trol cells stained with neutravidin-conjugated nanoparticles of FIG. 8, luminescent nanoparticles conjugated to isotypes, and luminescent nanoparticles not conjugated to neutravidin. [Figure 10]1 is a staining index chart of Cyto-Trol cells stained with biotinylated nanoparticles with different amounts of biotin according to an embodiment of the present disclosure conjugated to an anti-human CD4 antibody via streptavidin, and a comparative dissolved luminescent polymer marker conjugated to the same antibody. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0033] Unless the context clearly dictates otherwise, throughout the specification and claims, words such as "comprise," "comprising," and the like, are to be construed in an inclusive sense, i.e., "including, but not limited to," as opposed to an exclusive or exhaustive sense. As used herein, the terms "connected," "coupled," or any variation thereof, refer to any direct or indirect connection or coupling between two or more elements. Additionally, the words "herein," "above," "below," and words of similar import, when used in this application, refer to this application as a whole and not to any particular portions of this application. Also, where the context permits, words using a singular number or a plural number in the Detailed Description may include the plural number or singular number, respectively. The word "or," referring to a list of two or more items, encompasses all of the following interpretations of the word, namely, any of the items in the list, every item in the list, and any combination of the items in the list.

[0034] The teachings of the technology provided herein may be applied to other systems, not necessarily the system described below. Elements and acts of the various examples described below may be combined to provide further implementations of the technology. Some alternative implementations of the technology may include additional elements to the implementations described below, as well as fewer elements.

[0035] These and other changes can be made to the technology in light of the detailed description below. The description describes a particular example of the technology and describes the best mode contemplated, but no matter how detailed the description appears, the technology can be implemented in many ways. The details of the system are encompassed in the technology disclosed herein, but may vary considerably in its particular implementation. As stated above, a particular term used in describing a particular feature or aspect of the technology should not be interpreted as meaning that the term is redefined herein to be limited to any particular characteristic, feature or aspect of the technology with which the term is associated. In general, the terms used in the appended claims should not be interpreted as limiting the technology to the particular examples disclosed herein, unless the "Description of the Invention" section explicitly defines such terms. Thus, the actual scope of the technology encompasses not only the disclosed examples, but also any equivalent ways of implementing or practicing the technology based on the claims.

[0036] Although certain aspects of the technology are presented below in certain claim forms in order to reduce the number of claims, applicants contemplate various aspects of the technology in any number of claim forms.

[0037] In the following description, for purposes of explanation, numerous specific details are set forth in order to provide a thorough understanding of the implementation of the disclosed technology. However, it will be apparent to one skilled in the art that embodiments of the disclosed technology may be practiced without some of these specific details.

[0038] FIG. 1 illustrates a particle 100 according to some embodiments of the present disclosure.

[0039] Luminescent particle 100 has a core 101 that includes or consists of a luminescent material. Core 101 may include a matrix material, optionally an inorganic matrix material, optionally an inorganic oxide, optionally silica.

[0040] When a matrix material is present, in some embodiments the luminescent material may be directly or indirectly covalently bonded to the matrix material. In some embodiments the luminescent material may be mixed (i.e. not covalently bonded) with the matrix material. The core 101 may include a silica shell partially or completely covering an inner core that includes or consists of a luminescent material, preferably a luminescent polymer.

[0041] The core 101 may contain one or more light-emitting polymer chains mixed with and penetrating a matrix material. The one or more light-emitting polymer chains may protrude beyond the surface of the core defined by the matrix material.

[0042] Preferably, the particles have a number average diameter of 5000 nm or less, more preferably 2500 nm or less, 1000 nm or less, 900 nm or less, 800 nm or less, 700 nm or less, 600 nm or less, 500 nm or less or 400 nm or less, as measured by dynamic light scattering (DLS) using a Malvern Zetasizer Nano ZS. Preferably, the particles have a number average diameter of 5 to 5000 nm, optionally 10 to 1000 nm, preferably 10 to 500 nm, most preferably 10 to 100 nm, as measured by a Malvern Zetasizer Nano ZS.

[0043] In some embodiments, the emissive material is inorganic. The inorganic emissive material may be a quantum dot.

[0044] In some embodiments, the light emitting material is organic. In some embodiments, the organic light emitting material is non-polymeric. In some embodiments, the organic light emitting material is a light emitting polymer.

[0045] A first surface group 103 and a second surface group 105 are attached to the luminescent particle core.

[0046] In some embodiments, the first surface group 103 and / or the second surface group 105 may be covalently attached to the matrix material of the luminescent particle core. The second surface group 105 comprises a biomolecule binding group 107. The first surface group 103 is inert, i.e., does not comprise a biomolecule binding group.

[0047] The first surface group 103 comprises a first polar group PG1. The polar group may be a heteroatom capable of forming a van der Waals bond with water, optionally in which one or more C atoms of the alkylene chain are O or NR 6 (In the formula, R 6 is C 1~12 A hydrocarbyl group, optionally C 1~12 Alkyl group or C 1~4 The alkyl group may include a straight or branched alkylene chain substituted with a radical (which is an alkyl group).

[0048] PG1 can be a linear or branched polar group.

[0049] Preferably, PG1 is a polyether chain. As used herein, "polyether chain" refers to a divalent chain comprising multiple ether groups.

[0050] Preferably, PG1 comprises or consists of a repeat unit of formula (I) -((CR 14 R 15 ) b O) c - (I) In the formula, R 14 and R 15 are each independently H or C 1~6 alkyl, b is at least 1, optionally 1-5, preferably 2, and c is at least 2, optionally 2-1,000, preferably 10-500, 10-200, or 10-100.

[0051] Most preferably, PG1 comprises a polyethylene glycol chain.

[0052] The first polar group is attached directly or indirectly to the particle core at one end. A linking group may be provided between the polar group and the particle core to attach the polar group to the particle core.

[0053] The binding groups may include siloxane groups attached to silica at the surface of the particle core and binding groups BG attached to the polar groups.

[0054] The linking group BG may comprise or consist of a group selected from an ester, an amide, a urea, a thiourea, a Schiff base, a primary amine (CN) bond, a maleimide-thiol adduct, or a triazole formed by the cycloaddition of an azide and an alkyne.

[0055] The first polar group PG1 is substituted at the other end (in the case of a divalent chain) or at each of the other ends (in the case of a branched, trivalent or higher chain) by an end group EG. The end group may be an acid group or a salt or ester thereof, optionally a carboxylic acid group, a sulfonic acid group or a phosphonic acid group, or a salt or ester thereof.

[0056] The first surface group is inert, meaning that the first surface group does not bind to a biomolecule when contacted with the biomolecule in water at 25°C.

[0057] Suitably, the first surface group does not bind to proteins (particularly amine groups of proteins), such as antibodies or other proteins.

[0058] The first polar group may be polydisperse. The first polar group may have a Mn of at least 500, and optionally at least 2000.

[0059] The first surface groups may have a multimodal weight distribution, and optionally a bimodal weight distribution.

[0060] The second surface group comprises a biomolecule binding group 107 capable of binding to a biomolecule. Biomolecule binding groups include, but are not limited to, DNA, RNA, peptides, carbohydrates, antibodies, antigens, enzymes, proteins and hormones. A preferred biomolecule binding group is biotin.

[0061] In some embodiments, the biotin biomolecule binding group binds directly to the target analyte.

[0062] In some embodiments, the biotin biomolecule binding group is bound to a protein having multiple biotin binding sites, preferably streptavidin, neutravidin, avidin or recombinant mutants or derivatives thereof.Preferably, the protein is not luminescent.The biotinylated biomolecule having the second biotin group is bound to the same protein.The biotinylated biomolecule can be selected according to the target analyte.The biotinylated biomolecule can include an antigen-binding fragment, for example, an antibody, which can be selected according to the target antigen.

[0063] The biomolecule binding group 107 may be attached to the particle core by group 105. Group 105 may be a second polar group PG2. The second polar group may be the same or different from the first polar group PG1 of the first surface group. Group 105 may be directly attached to the surface of the particle core or may be attached to a binding group BG, which may be the same or different, preferably the same, as the binding group BG of the first surface group.

[0064] In some embodiments, the first surface group has a weight average molecular weight in the range of 750 to 7,500 daltons, optionally in the range of 1,000 to 3,000 daltons.

[0065] Figure 1 shows a particle having two different surface groups, in some embodiments, the particle may have three, four, or more different surface groups.

[0066] Formation of surface groups FIG. 2 illustrates a process for forming luminescent marker particles according to some embodiments of the present disclosure.

[0067] According to some embodiments, a luminescent marker particle having first and second surface groups may be formed from a luminescent particle core 101 carrying a plurality of first reactive groups RG1.

[0068] The first reactive group RG1 may be selected from: Amine group, optionally -NR 8 2 (wherein, R 8 is, at each occurrence, independently H or a substituent, preferably H or C 1~5 alkyl, more preferably H); -COOH; -OH, -SH; alkenes; alkynes; and azides.

[0069] The first reactive group RG1 can be attached directly or indirectly to the particle core by reacting a compound that includes the reactive group RG1 with the particle core.

[0070] The particle core may comprise silica and the compound comprising the reactive group RG1 may have the formula (I): (R 7 O)3Si-(Sp 1 ) x -RG1 (I) In the formula, R 7 is H or a substituent, preferably C 1~10 is an alkyl group, Sp 1 is a spacer group, x is 0 or 1, RG1 is the first reactive group.

[0071] Preferably, the silane formed by reaction of the compound of formula (I) forms a monolayer on the silica at the surface of the particle core.

[0072] Sp 1 means that one or more non-adjacent C atoms are O, S, C(=O), C(=O)O, C(=O)NR 12or NR 12 (In the formula, R 12 Each occurrence independently denotes H and C 1~12 Hydrocarbyl, optionally C 1~12 The alkyl group may be selected from linear or branched divalent alkylene chains optionally substituted with alkyl groups.

[0073] An exemplary compound of formula (I) is 3-aminopropyltriethoxysilane.

[0074] The particles are mixed with a first and a second reactive compound: some of the RG1 groups on the surface react with the first reactive compound 103' and some of the RG1 groups react with the second reactive compound 105' to form first and second surface groups, or precursors thereof, respectively.

[0075] Each of the first and second reactive compounds includes a second reactive group RG2 that can react with the reactive group RG1 to form a binding group BG, as described above, which covalently bonds the first and second surface groups 103 and 105 to the particle core 101.

[0076] The molar ratio of the first and second reactive compounds can be selected according to the desired molar ratio of first surface groups:second surface groups. The second reactive groups RG2 can be the same or different for the first and second reactive compounds.

[0077] Compound 103' may be a polydisperse compound. Compound 103' may have a multimodal weight distribution, possibly a bimodal weight distribution. Multimodal weight distribution may be achieved by mixing polydisperse materials with different average molecular weights.

[0078] In some embodiments, compound 103' is formed by converting a precursor compound to form one or more second reactive groups RG2, such as by reacting poly(ethylene glycol) to form at least one carboxylic acid group or ester thereof. Compound 103' having a multimodal weight distribution may be formed by mixing materials of different average molecular weights before or after formation of the one or more reactive groups RG2.

[0079] In some embodiments, compound 103' comprises a plurality of second reactive groups RG2. According to these embodiments, compound 103' can have formula (IIa): RG2-PG1-RG2 (IIa) In some embodiments, each RG2 group of formula (IIa) reacts with a reactive group RG1 to form a first surface group extending between two binding groups BG.

[0080] In some embodiments, only one RG2 group of formula (IIa) reacts with reactive group RG1 to form a first surface group having reactive group RG2 as a terminal group. It will be understood that reactive group RG2 is selected for its reactivity with reactive group RG1. Reactive group RG2 can be selected from groups that do not bind to target biomolecules.

[0081] RG1 and RG2 may be selected from: Amines, preferably -N(R 8 )2(wherein, R 8 is, at each occurrence, H or a substituent, preferably H or C 1~5 alkyl, more preferably H); Hydroxyl; Thiol; and A carboxylic acid or a derivative thereof, such as an anhydride, acid chloride, or ester, that forms a carboxylic acid group or a salt thereof upon reaction of RG1 with RG2.

[0082] Preferably, one of RG1 and RG2 is a carboxylic acid or a derivative thereof, such as an ester, preferably an NHS ester, an acid chloride group or an acid anhydride group, and the other of RG1 and RG2 is a protic group, such as a hydroxyl group, a thiol group or an amino group, preferably an amino group, and RG1 and RG2 can react to form an ester linking group BG or an amide linking group BG. One of RG1 and RG2 can be converted to an activated form prior to reaction with RG2, for example prior to activation of the carboxylic acid group using a carbodiimide, such as EDC.

[0083] In some embodiments, PG1 is a repeat unit of formula (I) that is directly bonded to one or two reactive groups RG2, as described below.

[0084] In some embodiments, PG1 is a repeat unit of formula (I) and PG1 further comprises a linking group linking the repeat unit of formula (I) to the or each reactive group RG2. The linking group may comprise or consist of an amide group.

[0085] The compound of formula (IIa) may have the formula: [ka]

[0086] In the formula, RG2, R 14 , R 15 , b and c are as defined above; each y is independently 0, 1, 2, 3, 4 or 5; each z is independently 0 or 1; each R 16 are independently H or C 1~6 It is an alkyl group.

[0087] The second surface group 105 may include a polar group PG2 which may be selected from the polar groups PG1 described above and which may be the same as or different from the polar group PG1 of the first surface group.

[0088] Biomolecule binding group 107 is preferably selected such that under reaction conditions for reacting with RG1 and RG2, it does not react with RG1, or such that RG2 reacts preferentially with RG1.

[0089] Preferably, the number of first surface groups 103 is greater than the number of second surface groups 105. The number of moles of first surface groups may be at least twice, preferably three times, and more preferably at least five times the number of moles of second surface groups. Most preferably, the number of second surface groups is less than 10 mol %, and optionally up to 5 mol %, of the total number of moles of first and second surface groups.

[0090] Preferably, the number of second surface groups is greater than 0.1 mol %, optionally at least 0.5 mol %, of the total number of moles of first and second surface groups.

[0091] Nanoparticle Core The particle core may consist of one or more luminescent materials.

[0092] The particle core may comprise or consist of one or more luminescent materials and a matrix material, including but not limited to an inorganic matrix material, optionally an inorganic oxide, optionally silica.

[0093] In some embodiments, the silica particles are formed by the Stober process, for example, as described in WO 2018 / 060722, the contents of which are incorporated herein by reference.

[0094] In some embodiments, the particle core may be formed by polymerization of silica monomers in the presence of an emissive material, for example as described in WO 2018 / 060722, the contents of which are incorporated herein by reference.

[0095] At least 0.1 wt% of the total weight of the particle core may consist of one or more luminescent materials.Preferably at least 1, 10, 25 wt% of the total weight of the particle core consists of one or more luminescent materials.

[0096] At least 50% by weight of the total weight of the particle core may consist of silica. Preferably, at least 60, 70, 80, 90, 95, 98, 99, 99.5, 99.9% by weight of the total weight of the particle core consists of silica.

[0097] The particle cores described herein are cores that have no surface-attached or surface groups thereon.

[0098] In one embodiment of the present disclosure, at least 70% by weight of the total weight of the particle core is composed of one or more luminescent materials and silica.Preferably, at least 80, 90, 95, 98, 99, 99.5, 99.9% by weight of the total weight of the particle core is composed of one or more luminescent materials and silica.More preferably, the particle core is essentially composed of one or more luminescent materials and silica.

[0099] Luminescent materials The luminescent material of the particle core may emit fluorescence, phosphorescence or a combination thereof.

[0100] The light emitting material can be a non-polymeric or a polymeric light emitting material, with polymeric light emitting materials being preferred.

[0101] The light emitting polymer may be a homopolymer or may be a copolymer containing two or more different repeat units.

[0102] Light emitting polymers may include light emitting groups in the polymer backbone, pendant from the polymer backbone, or as end groups of the polymer backbone. In the case of phosphorescent polymers, phosphorescent metal complexes, preferably phosphorescent iridium complexes, may be provided in the polymer backbone, pendant from the polymer backbone, or as end groups of the polymer backbone.

[0103] Light-emitting polymers can have a non-conjugated backbone or can be conjugated polymers. "Conjugated polymer" means a polymer that includes repeat units in the polymer backbone that are directly conjugated to adjacent repeat units. Conjugated light-emitting polymers include, but are not limited to, polymers that include one or more of arylene, heteroarylene, and vinylene groups that are conjugated to each other along the polymer backbone.

[0104] Light emitting polymers can have linear, branched or crosslinked backbones.

[0105] A light emitting polymer may include one or more repeat units substituted on the polymer backbone with one or more substituents selected from non-polar and polar substituents.

[0106] Preferably, the light-emitting polymer comprises at least one polar substituent. The one or more polar substituents may be the only substituents of the repeat unit, or the repeat unit may also contain one or more non-polar substituents, optionally one or more C 1~40 The repeat unit or units substituted with one or more polar substituents may be the only repeat units of the polymer, or the polymer may include one or more additional co-repeat units, where the or each co-repeat unit is unsubstituted or may include a non-polar substituent, optionally one or more C 1~40 It is substituted by a hydrocarbyl substituent.

[0107] C as described herein 1~40 Hydrocarbyl substituents include, but are not limited to, C 1~20 Alkyl, unsubstituted phenyl, and one or more C 1~20 It includes phenyl substituted with an alkyl group.

[0108] As used herein, a "polar substituent" is a compound that, alone or in combination with one or more additional polar substituents, has a concentration of at least 0.01 mg / ml in an alcohol solvent, preferably at least 0.1The alcohol solvent may refer to a substituent that results in a light-emitting polymer having a solubility of 1, 5 or 10 mg / ml. The solubility may be in the range of 0.01 to 10 mg / ml. The solubility is measured at 25° C. Preferably, the alcohol solvent is 1~10 An alcohol, more preferably methanol.

[0109] Polar substituents are preferably those capable of forming hydrogen bonds or ionic groups.

[0110] In some embodiments, the light emitting polymer has the formula -O(R 3 O) t -R 4 wherein R 3 At each occurrence, C 1~10 An alkylene group, optionally C 1~5 is an alkylene group, one or more non-adjacent, non-terminal C atoms of which may be replaced by O; R 4 is H or C 1~5 alkyl, and t is at least 1, optionally from 1 to 10. Preferably, t is at least 2. More preferably, t is from 2 to 5. The value of t is a group represented by the formula -O(R 3 O) t -R 4 The value of t may be the same for all polar groups of the same polymer. The value of t may vary between polar groups of the same polymer.

[0111] R 3 As used herein with respect to 1~5 An "alkylene group" is a group of the formula -(CH2) f - group, where f is 1-5.

[0112] Preferably, the light emitting polymer has the formula -O(CH2CH2O) t -R 4 where t is at least 1, and optionally 1 to 10; R 4 is C 1~5It is an alkyl group, preferably methyl. Preferably, t is at least 2. More preferably, t is 2 to 5, and most preferably, q is 3.

[0113] In some embodiments, the light emitting polymer has the formula -N(R 5 )2 polar substituents, wherein R 5 is H or C 1~12 Preferably, each R 5 is C 1~12 It is a hydrocarbyl.

[0114] In some embodiments, the light-emitting polymer comprises a polar substituent that is an ionizable group, which can be anionic, cationic, or zwitterionic. Preferably, the ionizable group is an anionic group.

[0115] Exemplary anionic groups include the sulfonic acid group, -COO - ; hydroxide; sulfate; phosphate; phosphinate; or phosphonate.

[0116] Exemplary cationic groups include -N(R 5 )3 + where R 5 Each occurrence is H or C 1~12 Preferably, each R 5 is C 1~12 It is a hydrocarbyl.

[0117] Light emitting polymers that contain cationic or anionic groups contain counterions to balance the charge of these ionic groups.

[0118] The anionic or cationic group and the counterion may have the same valence, and the counterion balances the charge of each anionic or cationic group.

[0119] The anionic or cationic groups can be monovalent or polyvalent. Preferably, the anionic and cationic groups are monovalent.

[0120] The light-emitting polymer may include multiple anionic or cationic polar substituents, where the charges of two or more anionic or cationic groups are balanced by a single counterion. The polar substituents may include anionic or cationic groups with divalent or trivalent counterions.

[0121] The counterion is optionally a cation, optionally a metal cation, optionally Li + , Na + , K + , Cs + , preferably Cs + or an organic cation, optionally ammonium, for example tetraalkylammonium, ethylmethylimidazolium or pyridinium.

[0122] The counterion is optionally an anion, optionally a halide; a sulfonate group, optionally a mesylate or tosylate; a hydroxide; a carboxylate; a sulfate; a phosphate; a phosphinate; a phosphonate; or a borate.

[0123] In some embodiments, the light emitting polymer has the formula -O(R 3 O) t -R 4 a group of the formula -N(R 5 )2 groups of the formula OR 4 and / or ionic groups. Preferably, the light emitting polymer comprises a group of formula -O(CH2CH2O) t R 4 a group of the formula -N(R 5 )2 groups and / or groups of the formula -COO - Preferably, the polar substituent is an anionic group of the formula -O(R 3 O) t -R 4 a group of the formula -N(R 5 Preferably, the polar substituent is selected from the group consisting of a group of the formula -O(CH2CH2O) t R 4 a polyethylene glycol (PEG) group of the formula -N(R5 )2 groups and / or groups of the formula -COO - R 3 , R 4 , R 5 and t is as above.

[0124] The backbone of the light-emitting polymer may be a conjugated polymer. The backbone of the conjugated light-emitting polymer may comprise a repeat unit of formula (III): [ka]

[0125] In the formula, Ar 1 is an arylene group or a heteroarylene group; Sp is a spacer group; m is 0 or 1; R 1 is independently at each occurrence a polar substituent; when m is 0, n is 1, and when m is 1, n is at least 1, and optionally 1, 2, 3, or 4; R 2 is independently at each occurrence a non-polar substituent; p is 0 or a positive integer, optionally 1, 2, 3 or 4; q is 0 or a positive integer, optionally 1, 2, 3 or 4; Sp, R 1 and R 2 may be independently the same or different at each occurrence.

[0126] Preferably, m is 1, and n is 2 to 4, more preferably 4. Preferably, p is 0.

[0127] Ar in formula (III) 1 is C 6~20 Ar may be an arylene group or a 5- to 20-membered heteroarylene group. 1 is preferably C 6~20 The arylene group is optionally phenylene, fluorene, benzofluorene, phenanthrene, naphthalene or anthracene, more preferably fluorene or phenylene, most preferably fluorene.

[0128] Sp-(R 1 )n may be a polar group, optionally a branched group substituted with -NH2 or -OH groups, such as polyethyleneimine, optionally a dendritic group.

[0129] Preferably, Sp is selected from: C, in which one or more non-adjacent C atoms may be replaced by O, S, N or C=O 1~20 Alkylene or phenylene-C 1~20 Alkylene; one or more substituents R 1 In addition to the above, it may be unsubstituted or may have one or more non-polar substituents, optionally one or more C 1~20 C optionally substituted with an alkyl group 6~20 Arylene or 5- to 20-membered heteroarylene, more preferably phenylene.

[0130] As used herein, "alkylene" means a branched or straight-chained divalent alkyl chain.

[0131] As used herein, a "non-terminal C atom" of an alkyl group means a C atom other than the terminal methyl group of an n-alkyl group or the terminal methyl group of a branched alkyl chain.

[0132] More preferably, Sp is selected from: C, in which one or more non-adjacent C atoms may be replaced by O, S or CO 1~20 alkylene; and C, which may be unsubstituted or substituted by one or more non-polar substituents 6~20 Arylene or 5- to 20-membered heteroarylene, more preferably phenylene.

[0133] R 1 may be a polar substituent as described anywhere herein. Preferably, R 1 is: Formula -O(CH2CH2O) t R 4wherein t is at least 1, and optionally 1 to 10; R 4 is C 1~5 a polyethylene glycol (PEG) group, the alkyl group being preferably methyl; ·Formula-N(R 5 )2(wherein, R 5 is H or C 1~12 hydrocarbyl; or ·Formula-COO - Anionic groups.

[0134] When n is at least 2, each R 1 may be independently the same or different at each occurrence. Preferably, each R attached to a given Sp group 1 is different.

[0135] When p is a positive integer, optionally 1, 2, 3 or 4, the group R 2 may be selected from: Alkyl, optionally C 1~20 Alkyl; and Aryl and heteroaryl groups, which may be unsubstituted or substituted by one or more substituents, preferably one or more C 1~20 Phenyl substituted by an alkyl group; an aryl or heteroaryl group, each of which may be independently substituted, such as a group of the formula -(Ar 3 ) s (In the formula, each Ar 3 is independently an aryl or heteroaryl group, and s is at least 2), each of which may be unsubstituted or may be substituted with one or more C 1~20 Branched or straight chain phenyl groups optionally substituted by alkyl groups; and Crosslinkable groups, such as groups containing double bonds, and vinyl or acrylate groups, or benzocyclobutene groups.

[0136] Preferably, each R 2 If present, C 1~40hydrocarbyl, more preferably C 1~20 Alkyl; unsubstituted phenyl; one or more C 1~20 phenyl substituted by alkyl groups; and straight or branched chain phenyl groups, each phenyl being unsubstituted or substituted by one or more substituents.

[0137] The polymers described herein may comprise or consist of only one form of repeat unit of formula (III), or may comprise or consist of two or more different repeat units of formula (III).

[0138] A polymer comprising one or more repeat units of formula (III) may be a copolymer comprising one or more co-repeat units.

[0139] When co-repeat units are present, the repeat units of formula (III) may form 0.1-99 mol %, possibly 50-99 mol % or 80-99 mol % of the repeat units of the polymer. Preferably, the repeat units of formula (I) form at least 50 mol %, more preferably at least 60, 70, 80, 90, 95, 98 or 99 mol % of the repeat units of the polymer. Most preferably, the repeat units of the polymer consist of one or more repeat units of formula (I).

[0140] The or each repeat unit of the polymer may be selected to produce a desired emission color of the polymer.

[0141] The luminescent material may emit light having a peak wavelength in the range of 350 to 1000 nm.

[0142] Blue light-emitting materials, such as the blue light-emitting polymers of the composite particles described herein, may have a photoluminescence spectrum with a peak below 500 nm, preferably in the range of 400 to 500 nm, and optionally 400 to 490 nm.

[0143] Green light-emitting materials, such as the green light-emitting polymers of the composite particles described herein, can have a photoluminescence spectrum with a peak from greater than 500 nm up to 580 nm, and optionally from greater than 500 nm up to 540 nm.

[0144] Red light-emitting materials, such as the red light-emitting polymers of the composite particles described herein, can have a photoluminescence spectrum with a peak from greater than 580 nm up to 630 nm, and optionally from 585 nm up to 625 nm.

[0145] The luminescent material may have an absorption spectrum with a maximum in the range of 300 to 900 nm.

[0146] The luminescent material may have a Stokes shift in the range of 10 to 850 nm.

[0147] The photoluminescence spectra of the light-emitting polymers described herein can be measured in solution using a Hamamatsu C9920-02 instrument.

[0148] The UV / vis absorption spectra of the luminescent materials described herein may be those measured in solution or suspension using a Cary 5000 UV-vis-IR spectrometer.

[0149] The arylene repeat units of the polymer include, but are not limited to, fluorene, preferably 2,7-linked fluorene; phenylene, preferably 1,4-linked phenylene; naphthalene, anthracene, indenofluorene, phenanthrene and dihydrophenanthrene repeat units.

[0150] The light-emitting polymers or silica polymers described herein have a polystyrene equivalent number average molecular weight (Mn) measured by gel permeation chromatography of about 1×10 3 ~1x10 8 , preferably 1x10 4 ~5x10 6The polystyrene equivalent weight average molecular weight (Mw) of the polymers described herein can range from 1x10 3 ~1x10 8 , preferably 1x10 4 ~1x10 7 It could be.

[0151] The polymers described herein are preferably amorphous polymers.

[0152] colloid The particles may be provided as a colloidal suspension, comprising the particles suspended in a liquid. Preferably, the liquid is water, C 1~10 Preferably, the particles form a homogenous (non-aggregated) colloid in the liquid.

[0153] The liquid may be a solution, optionally a buffer, with a salt dissolved therein. The buffer may have a pH ranging from 1 to 14, preferably from 5 to 8. The buffer may contain, but is not limited to, phosphates, such as sodium phosphate, tris(hydroxymethyl)aminomethane (Tris), acetates, such as sodium acetate, borate, and / or 2-(N-morpholino)ethanesulfonic acid (MES).

[0154] The salt concentration of the buffer may range from about 1 mmol / L to 200 mmol / L.

[0155] The concentration of the particles in the colloidal suspension is preferably in the range of 0.1 to 20 mg / mL, optionally 5 to 20 mg / mL.

[0156] In some embodiments, the particles may be stored as a colloidal suspension, optionally having a particle concentration of 0.1 mg / mL, preferably at least 0.5 mg / mL or greater than 1 mg / mL.

[0157] In some embodiments, the particles may be stored in a lyophilized or frozen form.

[0158] Purpose The particles of the present disclosure may be fluorescent or phosphorescent. Preferably, the particles are fluorescent. Preferably, the particles are for use as fluorescent probes for detecting or labeling biomolecules. In some embodiments, the particles may be used as fluorescent probes in immunoassays, such as lateral flow immunoassays or solid-state immunoassays. The particles may be for use in fluorescence microscopy, flow cytometry, next generation sequencing, in vivo imaging, or any other application in which a luminescent marker configured to bind to a target analyte is contacted with a sample to be analyzed. These applications may be for medical, veterinary, agricultural, or environmental applications, whether involving a patient (if applicable) or for research purposes.

[0159] In use, the biomolecule binding groups of the particles can bind to target biomolecules, including but not limited to DNA, RNA, peptides, carbohydrates, antibodies, antigens, enzymes, proteins and hormones. It will be understood that the biomolecule binding groups can be selected according to the target biomolecule.

[0160] The sample to be analyzed may be contacted with the particles, for example, the particles in a colloidal suspension.

[0161] In some embodiments, the sample after contacting with the particles is analyzed by flow cytometry. In flow cytometry, the particles are illuminated with at least one wavelength of light, and optionally with one or more wavelengths including at least one of two or more different wavelengths, for example, 355, 405, 488, 562 and 640 nm. The light emitted by the particles can be collected by one or more detectors. The detector can be selected from, but not limited to, a photomultiplier tube and a photodiode. Measurements of the particles mixed with cells that do not bind to the particles can be performed to provide a background signal for calculating the staining index.

[0162] In some embodiments, for example plate assays, the target biomolecule may be immobilized on a surface that is contacted with the particles.

[0163] [Example 1] Formation of biotinylated nanoparticles Formation of luminescent nanoparticle cores with reactive amine groups Nanoparticles having a silica core and a luminescent polymer were formed by the Stober method, and the nanoparticle cores were reacted with (3-aminopropyl)triethoxysilane as described in the Examples of WO 2018 / 060722, the contents of which are incorporated herein by reference, to yield nanoparticles with a number average diameter of 80 nm by dynamic light scattering and amine reactive groups on the surface of the core.

[0164] Attachment of surface groups to amino-modified luminescent nanoparticles A 1 mL suspension of amino-modified nanoparticle cores in methanol, as formed in the above examples, was centrifuged at 14,000 rpm for 2 min to separate the nanoparticles by decantation of the supernatant. The nanoparticle pellet was redispersed by gentle sonication using 1 mL of a methanolic solution of α,ω-bis{2-[(3-carboxy-1-oxopropyl)amino]ethyl}polyethylene glycol (SAA-PEG-SAA, shown below, MW=2000 g / mol), biotin-PEG-COOH (MW=2000 g / mol), N-(3-aminopropyl)-N-ethylcarbodiimide (2.1 mg) and N-hydroxysuccinimide (2.5 mg), and the resulting suspension was stirred for 1 h at room temperature. The relative amounts of SAA-PEG-SAA and biotin-PEG-COOH are shown in Table 1. The resulting silica-LEP nanoparticles were separated from the supernatant, which contained excess unreacted PEGylation reagent, by centrifugation of the suspension at 14,000 rpm for 2 min. The supernatant was removed by decantation, and the isolated pellet of nanoparticles was redispersed in 1 mL of fresh methanol using gentle sonication. The washing cycle consisting of centrifugation, decantation, and redispersion in methanol (1 mL) was repeated two more times. Before the final centrifugation and decantation, the suspension was aliquoted into four 250 μL portions, and the resulting pellet was stored at -20 °C before use. [ka] [ka] [Table 1]

[0165] [Example 2] Conjugation of biotinylated nanoparticles to streptavidin One of the isolated PEGylated nanoparticle pellets from Example 1 was resuspended in 1 mL of phosphate buffered saline (pH 7.4, containing 1 wt% bovine serum albumin) by gentle sonication, followed by immediate addition of 50 μL of streptavidin solution in the same buffer (1 mg / mL). After stirring the suspension for 1 h at room temperature, the sample was centrifuged at 14000 rpm for 3 min to collect and separate the protein-conjugated nanoparticles from the supernatant and unconjugated proteins. The pellet was resuspended in 100 μL of phosphate buffered saline by gentle sonication and stored.

[0166] [Example 3] Nanoparticle stability Colloids of nanoparticles bearing the inert PEG surface groups and biotin-substituted PEG surface groups described in Example 1 were formed using phosphate buffered saline (PBS, pH 7.4), and the Z-average diameter of the nanoparticles was measured periodically using dynamic light scattering to determine nanoparticle aggregation.

[0167] Referring to Table 1, there is a surprising reduction in aggregation with increasing nanoparticle concentration, especially at concentrations above 0.1 mg / mL.

[0168] The stability of the nanoparticles described in Examples 1 and 2, with 1 mol % or 10 mol % biotin-substituted PEG groups, in PBS (ie, with and without streptavidin) was tested.

[0169] Referring to Table 2, 1 mol% and 10 mol% biotin-substituted PEG groups without streptavidin are much more stable in lower concentrations of PBS. Attaching streptavidin with higher concentrations of biotin-substituted PEG groups significantly reduces stability. However, both of these nanoparticles were found to be much more stable than nanoparticles with 100% of the surface groups bearing biotin-substituted PEG groups. The nanoparticles were found to aggregate within minutes of being dispersed in PBS. [Table 2]

[0170] The stability times in Table 2 are the times required for the Z-average diameter of the particles, as determined by dynamic light scattering, to exceed 10% of the starting diameter when stored at 5° C. without agitation between measurements.

[0171] Streptavidin-containing particles formed using the process of Example 2, along with a large excess of streptavidin, were used to explore the possibility that streptavidin could cause aggregation by binding to the biotin molecules of the various nanoparticles by reducing or eliminating the occurrence of nanoparticles with free biotin groups. Similar aggregation was observed, indicating that streptavidin was not promoting aggregation by binding to the various nanoparticles.

[0172] [Example 4] The effect of aggregation on bioassay sensitivity. Preparation of biotin-BSA modified glass slides for bioassays A glass microscope slide functionalized with a self-assembled monolayer of (3-aminopropyl)silane was immersed in a solution of acetonitrile (50 mL) containing succinic anhydride (1 g) and trimethylamine (1.3 mL) for 16 h, followed by washing three times with fresh acetonitrile (50 mL). After drying, the surface of the resulting carboxy-functionalized glass slide was affixed with Grace-Biolabs Secure Seal imaging spacers to isolate four circular areas (diameter = 9 mm) for use in the subsequent binding assay. Within each isolated area of ​​the slide, 80 μL of a 1 mL solution containing N-(3-aminopropyl)-N-ethylcarbodiimide (77.0 mg) and N-hydroxylsulfosuccinimide (33.0 mg) was added. After standing at room temperature for 30 min, the solution was removed and the isolated areas were washed three times with water (80 μL). After removing the last wash, 80 μL of a solution of biotinylated bovine serum albumin (50 μg / mL) in phosphate-buffered saline (pH 7.4) was added to two regions, and 80 μL of a blocking buffer containing bovine serum albumin (3 wt%) in phosphate-buffered saline (pH 7.4) containing 0.01 wt% Tween-20 was added to the remaining two regions. After 1 h at room temperature, the solution was removed from the two regions containing the biotinylated bovine serum albumin solution and 80 μL of the blocking buffer described above was added instead. After another hour at room temperature, the solution was removed from all four regions and each was washed three times with phosphate-buffered saline (pH 7.4) containing 0.01 wt% Tween-20.

[0173] Biotin-binding assay using streptavidin-modified nanoparticles Colloids (0.1 mg / mL in phosphate-buffered saline containing 1% bovine serum albumin) containing 0.1 mol%, 1 mol% and 10 mol% of streptavidin-modified biotinylated nanoparticles as described in Example 2 were applied to glass slides. After standing at room temperature for 30 min, the solution was removed and washed three times with 80 μL of phosphate-buffered saline (pH 7.4). After drying in air, the fluorescence intensity of each of the four assay regions was measured using a microscope-based spectrometer using a mercury lamp as the excitation source (λex=365 nm) and a fiber optic spectrometer for detection. The signal-to-noise was determined by dividing the average integrated intensity from the regions functionalized with biotin by the average intensity of the regions blocked with BSA only (no biotin).

[0174] The strongest signal-to-noise ratio was observed for 1 mol% biotinylated nanoparticles, as shown in Figure 3. Without wishing to be bound by any theory, this is attributed to a higher percentage of biotinylated groups compared to 0.1 mol% biotinylated nanoparticles and less aggregation (which may result in less accessible binding groups) compared to 10 mol% biotinylated nanoparticles.

[0175] [Example 5] Effect of molecular weight of surface groups Nanoparticles were prepared as described in Example 1, except that the amino groups were reacted with only SAA-PEG-SAA (Mw 550, 100, 2000 or 5000 Da) or only mPEG-SAA (MW 550, 100, 2000 and 5000 Da, as shown below), i.e., the resulting surface groups did not contain groups bearing biomolecule binding groups. [ka]

[0176] All particles formed dispersions in methanol and were found to be stable for over a month.

[0177] To determine the stability of the particles in buffer, a 1 mg / mL dispersion of PEG-coated particles in methanol was measured by DLS to determine the Z-average diameter of the particles.

[0178] 1 mg of nanoparticles were then separated from the methanol dispersion by centrifugation and decantation of the supernatant and redispersed in 1 mL of phosphate buffered saline (PBS, pH 7.4) by sonication in an ultrasonic bath for 5 min.

[0179] DLS measurements of the dispersions in PBS were taken after 5, 60, 300 and 1440 minutes (or until they aggregated), leaving the samples at room temperature in sealed sample tubes between measurements.

[0180] Referring to FIG. 4, all nanoparticles having methoxy PEG terminal surface groups formed by reaction of the core with mPEG-SAA were found to aggregate within 5 minutes of dispersion in PBS.

[0181] Referring to FIG. 5, nanoparticles with carboxy-terminated surface groups formed by reaction of the core with SAA-PEG-SAA were stable for up to 24 hours depending on the Mw of the surface group.

[0182] [Example 6] Conjugation to biotinylated antibodies To 1 mg of streptavidin-functionalized nanoparticles as described in Example 2, 250 μL of 0.5 mg / mL biotinylated goat anti-mouse antibody (clone Poly4053, purchased from Biolegend) was added and the mixture was stirred for 1 h at room temperature. This step was repeated four times. In the final step, the pellet was resuspended in 500 μL of BSA / PBS to obtain a final particle concentration of 2 mg / mL.

[0183] [Example 7] Flow cytometry assay Flow cytometric analysis was performed using a Propel Labs YETI analyzer.

[0184] BV421-anti-human CD4 (clone SK3) [BV421-hCD4] and BV421-mouse IgG1, kappa isotype (clone MOPC-21) [BV421-isotype] were purchased from Biolegend.

[0185] CYTO-TROL cells were supplied by Beckman Coulter.

[0186] 1. CYTO-TROL cells were brought to room temperature and resuspended in the buffer provided by the manufacturer prior to use.

[0187] 2. The antibody tag was diluted to the required concentration in BSA / PBS in a microcentrifuge tube.

[0188] 3. To each of the antibody-NP dilutions, 100 μL of prepared Cyto-Trol was added. The preparation was mixed thoroughly, left to stand, and incubated at 4° C. for 30 minutes away from direct light.

[0189] 4. After incubation, the cells were washed twice with cell staining buffer, centrifuged at 2000 rpm for 3 minutes at 4° C., and the supernatant was discarded.

[0190] 5. Resuspend cells in 200 μL of cell staining buffer ready for analysis.

[0191] 6. A flow rate of 0.5 μL / sec was used for analysis. Data was gated on single cells and 10,000 events were acquired in this gate for each measurement.

[0192] A series of different exemplary nanoparticle NP(x)-hCD4 (where NP is the nanoparticle described in Example 6, x=s for streptavidin; x=n for neutravidin; hCD4=anti-human CD4 antibody) dilutions were screened to determine the optimal working concentration for maximum staining index of each dye.

[0193] Conjugation of antibodies using neutravidin was as described above for streptavidin, except that 50 μL of a 1 mg / mL solution of neutravidin in PBS was used in place of streptavidin.

[0194] The staining index [SI] is as follows:

number

[0195] where MFI1 is the median fluorescence intensity of the positive population, MFI2 is the median fluorescence intensity of the negative population, and SD is the standard deviation of the negative signals.

[0196] The same was done for the comparative marker BV421-hCD4, where BV421 is a soluble fluorescent polymer Brilliant Violet 421™ available from BioLegend.

[0197] The voltage was adjusted to ensure that both the negative and positive signals were on scale. For NP(n)-hCD4, no voltage could be found where the negative and positive were completely on scale, so the voltage where the negative was completely on scale was used for analysis. [Table 3]

[0198] The optimal concentration of each tag was determined as follows: BV421-hCD4: 250μg / mL NP(s)-hCD4: 31.3 μg / mL NP(n)-hCD4: 15.6 μg / mL The optimal voltages for BV421-hCD4, NP(s)-hCD4 and NP(n)-hCD4 for each channel were the same and are summarized in Table 2: [Table 4]

[0199] Each of the following tags in Table 3 was measured in triplicate at the optimized concentrations and voltages above. [Table 5]

[0200] The same was done with the biotinylated nanoparticles of Example 1 (ie, without streptavidin or neutravidin) and unstained cells.

[0201] These particles, not conjugated to streptavidin or neutravidin, were dispensed into microcentrifuge tubes. The suspension was centrifuged at 14,000 rpm for 4 min. The solvent was decanted and the pellet was resuspended in 100 μL of BSA / PBS by sonication to give a final particle concentration of 10 mg / mL.

[0202] Result: NP(s)-hCD4 Figure 6 and Table 4 compare the staining of Cyto-Trol cells by NP(s)-hCD4 with BV421-hCD4. Similar to BV421-hCD4, NP(s)-hCD4 shows negligible staining of negative cells. However, the positive signal of NP(s)-hCD4 is significantly shifted to a relatively higher extinction coefficient with only a small increase in the standard deviation of the positive signal compared to BV421-hCD4. This increase in MFI1 translates into an approximately 2.5-fold increase in the staining index of NP(s)-hCD4 compared to BV421. [Table 6]

[0203] The low negative staining of NP(s)-derived particles is further shown in Figure 7 and Table 5. Neither non-functionalized NP(s)-isotype nor NP(s)-hCD4 showed significant negative staining, indicating low non-specific uptake into cells for the fluorescent nanoparticles described herein and their streptavidin- and antibody-conjugated derivatives. [Table 7]

[0204] Result: NP(n)-hCD4 Figure 8 and Table 6 compare the staining of Cyto-Trol cells by NP(n)-hCD4 with BV421-hCD4 with respect to NP(s)-hCD4. Similar to NP(s)-hCD4, NP(n)-hCD4 shows negligible negative staining. The relatively bright positive signal of NP(n)-hCD4 shows a staining index of 5.4 times higher than BV421-hCD4. [Table 8]

[0205] The low negative staining of NP(n)-derived particles is further shown in Figure 9 and Table 7. Neither the non-functionalized NP(n) isotype nor NP(n)-hCD4 showed significant negative staining, indicating low non-specific uptake into cells for the fluorescent NPs and their neutravidin- and antibody-conjugated derivatives. [Table 9]

[0206] Effect of first biotin group density Biotin-PEG-COOH+SAA-PEG-SAA The effect of the first biotin group density (and therefore the number of protein binding sites on the surface of the precursor nanoparticles) was tested using the nanoparticles described in Example 1, except that the biotin-PEG-COOH as a percentage of the total weight of SAA was varied from 0.5 wt%, 1 wt%, 5 wt% and 10 wt%.

[0207] The volumes of reagents used for various weight percentages of the first and second surface groups are shown in Table 8. [Table 10]

[0208] Nanoparticles conjugated to anti-human CD4 [NP(x)-hCD4] were formed using a biotin mouse anti-human CD4 antibody (clone SK3) supplied by Biolegend.

[0209] For isotype control particles [NP(x)-isotype], biotin mouse IgG1, kappa isotype (clone MOPC-21) supplied by Biolegend was used.

[0210] A series of different NP(s)-x%hCD4 (where x = 0.5, 1, 5, or 10 represents the percentage of PEG-biotin used to functionalize the NPs) and BV421-hCD4 dilutions were screened to determine the optimal working concentration for maximum staining index of each dye.

[0211] The voltage was adjusted to ensure that both the negative and positive signals were on scale. [Table 11]

[0212] The optimal concentration of each tag was determined as follows: BV421-hCD4: 250μg / mL NP(s)-0.5%hCD4: 62.5μg / mL NP(s)-1%hCD4: 250μg / mL NP(s)-5%hCD4: 125μg / mL NP(s)-10%hCD4: 62.5μg / mL The optimal voltages for BV421-hCD4 and NP(s)-x%hCD4 for each channel are the same and are summarized in Table 10: [Table 12]

[0213] The tags in Table 11 were measured in triplicate at the above optimized concentrations and optimized voltages. [Table 13]

[0214] Unstained cells were also measured.

[0215] The effect of varying the percentage of surface biotin groups on the staining of Cyto-Trol cells is shown in Figure 10 and Table 12. For all biotin concentrations, except for 1% biotin, which is due to a very high optimal staining concentration (250 μg / mL) compared to the other tags, the negative population showed negligible background staining compared to unstained cells. The effect of this high staining concentration is evident from the NP(s)-1% hCD4 used in the streptavidin / neutravidin comparison experiment above, where a much lower optimal staining concentration of 31.3 μg / mL shows negligible staining for the negative population.

[0216] Therefore, it can be concluded that variations in surface biotin concentration from 0.5 to 10% do not increase the nonspecific binding of the obtained tags to Cyto-Trol cells. [Table 14]

[0217] These data show that the more surface biotin, the higher the staining index of the resulting antibody conjugate, with the 10% (wt) biotin tag exhibiting a staining index 1.9-fold higher than the 0.5% (wt) biotin tag. Even at 0.5% (wt) biotin, the staining index exceeds that of BV421-hCD4.

Claims

1. A method for marking a biomolecule, comprising the steps of binding the biomolecule to a luminescent marker particle comprising a luminescent particle core comprising a silica matrix, a first surface group covalently bonded to the silica of the luminescent particle core, and a second surface group covalently bonded to the silica of the luminescent particle core, wherein the luminescent particle core comprises the silica matrix and a luminescent polymer, the first surface group comprises a polar group, the first surface group is an inert surface group that does not bind to the biomolecule when contacted with the biomolecule in water at 25° C., the second surface group comprises a biomolecule binding group, the number of moles of the second surface group is less than 10% of the total number of moles of the first surface group and the second surface group, and the first surface group does not comprise a zwitterion, The method of claim 1, wherein the light emitting polymer has a solubility in methanol of at least 0.1 mg / ml.

2. The method of claim 1 , wherein the polar group comprises a polyether chain.

3. the polar group is a group of formula (I), -((CR 14 R 15 ) b O) c - (I) In the formula, R 14 and R 15 are each independently H or C 1~6 is alkyl, The method of claim 2 , wherein b is at least 1 and c is at least 2.

4. 4. The method according to claim 1, wherein the biomolecule is selected from the group consisting of DNA, RNA, peptides, carbohydrates, antibodies, antigens, enzymes, proteins and hormones.

5. The method of claim 1 , wherein the second surface group comprises a polar group between the luminescent particle core and the biomolecule binding group.

6. 6. The method of claim 1, wherein the number of moles of the second surface groups is 5% or less of the total number of moles of the first surface groups and the second surface groups.

Citation Information

Patent Citations

  • Structure with bonding functional group on substrate for use in bonding acquisition molecule for acquiring target substance

    JP2007127630A

  • Preparation method of mixed sam

    JP2009216483A

  • Nonspecific adsorption constraint material

    JP2009236848A

  • Fluorescent magnetic nanoparticles, method for producing the same, and use thereof

    JP2009508105A

  • Surface and method for independent detection of labels

    JP2011516885A