Polymer Coated Paper and Board

A dual-layer polyethylene coating structure with specific blends of high and low-density polyethylenes addresses adhesion and stability issues in extrusion coating, achieving reduced basis weights and improved performance for paper and paperboard products.

JP7565915B2Active Publication Date: 2024-10-11STORA ENSO OYJ
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2021517763
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-10-03
Filing Date
2019-10-01
Publication Date
2024-10-11
Estimated Expiration
2039-10-01

AI Technical Summary

Technical Problem

Existing extrusion coating processes for paper and paperboard face challenges in achieving sufficient adhesion and stability of polyethylene coatings at reduced basis weights, often leading to pinhole formation and defects.

Method used

A dual-layer polyethylene coating structure comprising a blend of high-density, medium-density, or linear low-density polyethylene as the first layer and low-density polyethylene as the second layer, applied via extrusion coating, reduces the total basis weight to less than 12 g/m² while maintaining adhesion and stability.

Benefits of technology

The dual-layer coating significantly improves adhesion and reduces pinhole formation, enabling the production of coated paper and paperboard with enhanced mechanical properties at lower coating weights, suitable for applications like waterproof paper cups.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007565915000001
    Figure 0007565915000001
  • Figure 0007565915000002
    Figure 0007565915000002
  • Figure 0007565915000003
    Figure 0007565915000003
Patent Text Reader

Abstract

The present invention relates to a paper or paperboard comprising: 1. Paper or paperboard comprising a polymeric coating, said polymeric coating comprising: A first coating layer applied to a surface of paper or paperboard, said first coating layer comprising a blend of: High density polyethylene (HDPE), medium density polyethylene (MDPE) or linear low density polyethylene (LLDPE), or a mixture thereof; and Low density polyethylene (LDPE); and a second coating layer attached to the first coating layer, said second coating layer consisting essentially of low density polyethylene (LDPE); Here, the first coating layer and the second coating layer have a thickness of 12 g / m 2 having a total basis weight of less than The present invention relates to a method for producing a polyethylene (PE) coated paper or paperboard substrate.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] Technical Field The present disclosure relates to coated papers and paperboards that include a polyethylene coating. [Background technology]

[0002] background Coating paper and paperboard with plastics is often used to combine the mechanical properties of paperboard with the barrier and sealing properties of plastic films. Paperboard with a relatively small amount of the appropriate plastic material can provide the properties necessary to make the paperboard suitable for many demanding applications.

[0003] Paper or paperboard itself is generally suitable for packaging dry products. However, untreated paperboard is of limited use in direct contact with wet or greasy products because moisture affects the mechanical properties of the packaging and absorbed grease causes staining of the paper. These effects impair the protective function and the appearance of the packaging. Polyethylene (PE) coatings on paper and paperboard are often suitable for packaging applications where moisture barrier properties are important. Examples include the packaging of fresh and frozen foods such as vegetables, meat, fish and ice cream. One important use of PE-coated paperboard is in the production of waterproof paper cups.

[0004] Extrusion coating is the process of applying molten plastic material to a substrate such as paper or paperboard to form a very thin, smooth, uniform layer. The coating can be formed by the extruded plastic itself, or the molten plastic can be used as an adhesive to laminate a solid plastic film onto the substrate. Common plastic resins used in extrusion coating include polyethylene (PE), polypropylene (PP), and polyethylene terephthalate (PET).

[0005] Extrusion coating may be used, for example, to achieve moisture protection, barrier properties against water vapor, oxygen, fragrances, etc., stain or grease resistance, heat sealability, and / or to impart a desired finish or texture to a substrate surface.

[0006] Extrusion coating greatly expands the range of applications for paper and paperboard. The thin plastic layer provides resistance to grease and moisture and in some cases also heat resistance. Plastic coatings can also be used for heat sealing. Depending on the application, the paper or paperboard can be extrusion coated on one or both sides.

[0007] For environmental and economic reasons, it is generally desirable to keep plastic coatings as thin as possible, as long as the barrier and protective properties are maintained at acceptable levels. However, in many cases, further reduction in thickness (or basis weight) of plastic coatings is limited by impaired adhesion and stability of film formation in the extrusion process, as well as the formation of pinholes. For example, PE is typically rated at 15-25 g / m 2 PE resins traditionally used in paper cup manufacturing can be extrusion coated to a basis weight of 12 g / m2 onto paper or paperboard without loss of adhesion, loss of heat sealability, or increased pinhole formation. 2 It is not possible to extrusion coat below this basis weight or defects will result in the coated product.

[0008] In the extrusion coating and lamination of paper and paperboard with plastics, it is very important to obtain sufficient adhesion of the plastic to the substrate. The adhesion of the plastic depends primarily on the surface properties of the substrate and the heat capacity of the plastic melt when applied to the paperboard. Poor adhesion between the plastic coating and the paper or paperboard is a common and consistent problem.

[0009] Pinholes are tiny holes that may form in plastic films during the coating process. The main reasons for pinholes include irregularities in the substrate surface (high surface roughness, loose fibers, etc.), uneven distribution of the coating, and too low basis weight of the coating. Summary of the Invention [Problem to be solved by the invention]

[0010] Although adhesion can be improved by surface treatment of the substrate, for example with corona discharge or ozone, there remains a need for improved solutions to reduce the basis weight of the plastic coating in extrusion coating of PE while maintaining good adhesion, heat sealability, and film formation stability during the extrusion process. [Means for solving the problem]

[0011] Description of the invention An objective of the present disclosure is to reduce the minimum basis weight of PE resin required to achieve sufficient adhesion, heat sealability, and / or stability of film formation in extrusion coating.

[0012] A further object of the present disclosure is to provide a method for producing a PE resin having a viscosity of 12 g / m while maintaining good adhesion of the PE resin to the paper or paperboard and while avoiding the formation of pinholes. 2 The object of the present invention is to provide a PE resin-coated paper or paperboard which enables the total basis weight of the PE resin to be reduced, such as a basis weight of less than 100 g / m2.

[0013] It is a further object of the present disclosure to provide a method for producing PE resin coated paper or paperboard, which can achieve a coating strength of 12 g / m while maintaining good stability of film formation in the extrusion process. 2 This allows for a reduced basis weight of the PE resin, such as a basis weight of less than 100 g / m2.

[0014] A further object of the present disclosure is to provide a method for producing paper or paperboard coated with PE resin, which allows for improved stability of film formation in the extrusion process at low basis weights of the PE resin.

[0015] The above objectives, as well as other objectives which will be realized by one skilled in the art in light of the present disclosure, are accomplished by various aspects of the present disclosure.

[0016] According to a first aspect presented herein, there is provided a paper or paperboard comprising: 1. A paper or paperboard comprising a polymeric coating, the polymeric coating comprising: A first coating layer applied to a surface of a paper or paperboard, said first coating layer comprising a blend of: High density polyethylene (HDPE), medium density polyethylene (MDPE) or linear low density polyethylene (LLDPE), or a mixture thereof; and Low density polyethylene (LDPE); and a second coating layer attached to the first coating layer, said second coating layer consisting essentially of low density polyethylene (LDPE); Here, the first coating layer and the second coating layer have a thickness of 12 g / m 2 has a total basis weight of less than In relation to the present invention, the following is further disclosed: [1] 1. A paper or paperboard comprising a polymeric coating, the polymeric coating comprising: A first coating layer applied to a surface of a paper or paperboard, said first coating layer comprising a blend of: High density polyethylene (HDPE), medium density polyethylene (MDPE) or linear low density polyethylene (LLDPE), or a mixture thereof; and Low density polyethylene (LDPE); and a second coating layer attached to the first coating layer, said second coating layer consisting essentially of low density polyethylene (LDPE); Here, the first coating layer and the second coating layer have a thickness of 12 g / m 2 has a total basis weight of less than [2] The paper or paperboard of [1], wherein the first coating layer consists essentially of a blend of: 1 to 49% by weight of high density polyethylene (HDPE), medium density polyethylene (MDPE), linear low density polyethylene (LLDPE), or mixtures thereof; and 51-99% by weight low density polyethylene (LDPE). [3] The paper or paperboard according to any one of [1] to [2], wherein the first coating layer is formed by extrusion coating onto a surface of the paper or paperboard. [4] The paper or paperboard according to any one of [1] to [3], wherein the second coating layer is formed by extrusion coating onto the first coating layer. [5] The first coating layer and the second coating layer have a thickness of 10 g / m 2 Less than 8g / m 2 1. The paper or paperboard according to any of [1] to [4], having a total basis weight of less than [6] The first coating layer is 5 g / m 2 Less than 4 g / m 2 less than 3 g / m 2 1. The paper or paperboard according to any one of [1] to [5], having a basis weight of less than [7] The second coating layer has a thickness of 10 g / m 2 Less than 8g / m 2 less than 6 g / m 2 1. The paper or paperboard according to any one of [1] to [6], having a basis weight of less than [8] HDPE is 0.930~0.970g / cm 3 and MDPE has a density in the range of 0.926 to 0.940 g / cm 3 and LLDPE has a density in the range of 0.918 to 0.940 g / cm 3 and / or LDPE has a density in the range of 0.910 to 0.940 g / cm 3 8. The paper or paperboard according to any one of [1] to [7], having a density in the range of [9] The paper or paperboard according to any of [1] to [8], wherein the first coating layer comprises a blend of MDPE and LDPE.

[10] 10. The paper or paperboard according to any of [1] to [9], wherein the second coating layer has a lower density than the first coating layer.

[11] 11. The paper or paperboard according to any of [1] to

[10] , wherein the second coating layer is a top layer of a polymeric coating.

[12] 12. The paper or paperboard according to any of [1] to

[11] , wherein the polymeric coating has better adhesion to the surface of the paper or paperboard than an LDPE coating of the same total basis weight.

[13] A heat-sealed paper or paperboard product comprising the paper or paperboard described in any one of [1] to

[12] .

[14] 13. The heat-sealed paper or paperboard product according to claim 12, wherein the product is a paper cup.

[15] 1. A method for producing a polyethylene (PE) coated paper or paperboard substrate, comprising: a) providing a paper or paperboard substrate; b) applying at least one layer of a molten first polymer resin to a surface of the substrate by extrusion coating to form a first polymer coating layer, the first polymer resin comprising a blend of: High density polyethylene (HDPE), medium density polyethylene (MDPE) or linear low density polyethylene (LLDPE), or a mixture thereof; and Low density polyethylene (LDPE), c) applying at least one layer of a molten second polymeric resin to a surface of the first polymeric coating layer by extrusion coating to form a second polymeric coating layer, the second polymeric resin consisting essentially of low density polyethylene (LDPE); d) cooling and solidifying the first and second coating layers; and e) Recovering the PE coated paper or paperboard substrate.

[16] The method according to

[15] , wherein the first coating layer and the second coating layer are further defined as described in any one of [2 to 12].

[17] The method according to any one of

[15] to

[16] , wherein the first coating layer and the second coating layer are simultaneously formed by coextrusion coating.

[0017] Paper generally refers to a material manufactured in thin sheets from wood pulp or other fibrous substances containing cellulose fibers and used for writing, drawing, or printing, or used as a packaging material.

[0018] Paperboard generally refers to a strong, thick paper or corrugated board containing cellulose fibers used for boxes and other types of packaging. Paperboard can be produced in a variety of thicknesses, either bleached or unbleached, coated or uncoated, depending on the end-use requirements.

[0019] The term coating as used herein refers to an operation in which the surface of a substrate is covered with a composition to impart a desired property, finish or texture to the substrate. The coating may be a multi-layer coating in which the PE coating resin may be used in one or more layers. The coating may be applied to one or both sides of the paper or paperboard.

[0020] The problems of poor adhesion and pinhole formation in low basis weight PE coatings are particularly evident in paper and paperboard coatings, where the fiber-based substrate and its natural voids and surface roughness may play a key role. Current waterproof paper cups have a basis weight of 0.910-0.940 g / cm 3The coating basis weight is typically 12 g / m. 2 That's it. This conventional LDPE can be applied at up to 12 g / m without losing adhesion and film-forming stability that can lead to defects in the coated product. 2 It is not possible to extrusion coat onto paper or paperboard to a coating basis weight less than this.

[0021] The inventors have demonstrated that by using a specific combination of different PE types, specifically a first coating layer comprising a blend or mixture of high density polyethylene (HDPE), medium density polyethylene (MDPE) or linear low density polyethylene (LLDPE), and low density polyethylene (LDPE), the minimum basis weight of PE required to achieve sufficient adhesion and stability of film formation in extrusion coating of paper and paperboard can be significantly reduced. Proper adhesion is important in many converting operations such as printing and heat sealing.

[0022] The inventors have surprisingly found that the coating structure of the present invention having a first coating layer comprising a blend or mixture of high density polyethylene (HDPE), medium density polyethylene (MDPE) or linear low density polyethylene (LLDPE) and a second coating layer consisting essentially of low density polyethylene (LDPE) as an adhesive layer and a top layer, allows the total basis weight of the coating to be reduced further than would be possible with a coating structure comprising only the blend and also further than would be possible with a similar structure in which the layer order is reversed, i.e., the blend as the top layer and LDPE as the adhesive layer. This shows that not only the blend composition but also the order of the layers influences the coating process and the resulting coating.

[0023] The first coating layer comprises a blend or mixture of high density polyethylene (HDPE), medium density polyethylene (MDPE) or linear low density polyethylene (LLDPE), and low density polyethylene (LDPE).

[0024] Low density polyethylene (LDPE) has rheological properties that make it suitable for the production of films by extrusion. LDPE has several long branches and many short branches. Typically, there may be three long branches and 30 short branches per molecule. The molecular weight is relatively low and the molecular weight distribution is broad. The melt strength and shear thinning properties of LDPE enhance processing. LDPE films have relatively low tensile strength but good impact strength. LDPE films exhibit excellent clarity and gloss. The good clarity and gloss are due to the relatively low crystallinity. LDPE is obtained by a high pressure radical polymerization process, usually in an autoclave or tubular reactor. Autoclaves generally result in more branching and a broader molecular weight distribution. LDPE has a wide melting range, with a peak melting temperature of 110°C. The density of LDPE is typically 0.910-0.940 g / cm. 3 The range is.

[0025] High density polyethylene (HDPE) has a linear structure and little or no branching. HDPE is usually produced by the Ziegler-Natta, Phillips, or Unipol processes. These processes are relatively low pressure and are catalyzed by organometallic complexes with transition metals. Polymerization is usually carried out in the gas phase with a catalyst in a slurry with a liquid such as heptane, or in a fluidized bed configuration. The density of HDPE is usually 0.930 to 0.970 g / cm 3 The range is.

[0026] Medium density polyethylene (MDPE) is a variation of HDPE in which some short branches are introduced by copolymerization with 1-alkenes such as 1-butene, 1-hexene, and 1-octene. The density of MDPE is typically 0.926 to 0.940 g / cm. 3 The range is.

[0027] HDPE and MDPE exhibit a more Newtonian rheology than LDPE, making them less suitable for extrusion processing. HDPE and MDPE are more crystalline than LDPE, which gives them higher tensile strength, but may lack the impact strength for many applications.

[0028] Linear low density polyethylene (LLDPE) is a copolymer of ethylene and an 1-alkene, typically 1-butene, 1-hexene, or 1-octene, although branched alkenes such as 4-methyl-1-pentene are also used. These polymers have a density of 0.918 to 0.940 g / cm 3 They have densities ranging from 0.1 to 1.0, and contain 2-7% by weight of 1-alkenes. Like HDPE, they are polymerized using multisite catalysts such as Ziegler-Natta in either gas phase or slurry processes. The comonomer composition usually has a wide distribution, so that some molecules have little branching and others have a lot of branching. This distribution is reflected in the wide melting temperature range of LLDPE. The properties of LLDPE tend to be between those of LDPE and HDPE. They have short branching but no long branching, which improves the mechanical properties that depend on crystallization, but the processing rheological properties are inferior to those of LDPE.

[0029] Those skilled in the art would expect LDPE to show the lowest pinhole sensitivity due to its strain hardening behavior during the extrusion coating process. This behavior is expected to protect the coating from pinhole formation due to film defects as well as from non-uniformities in fiber-based substrates. Surprisingly, the inventors have discovered that by introducing HDPE, MDPE or LLDPE into LDPE, pinhole formation can be significantly reduced, and therefore the minimum coating weight required for the first extrusion coating layer of paper or paperboard can be reduced.

[0030] In some embodiments, the polymer coating does not include any additional coating layers other than the first and second coating layers, i.e., the polymer coating consists of the first and second coating layers. In some embodiments, the polymer coating includes one or more additional coating layers in addition to the first and second coating layers.

[0031] In some embodiments, the first coating layer consists essentially of a blend of the following: 1 to 49% by weight of high density polyethylene (HDPE), medium density polyethylene (MDPE) or linear low density polyethylene (LLDPE), or a mixture thereof; and 51-99% by weight low density polyethylene (LDPE).

[0032] In some embodiments, the first coating layer consists essentially of a blend of the following: 1 to 39% by weight, for example 1 to 29% by weight, for example 1 to 19% by weight, of high density polyethylene (HDPE), medium density polyethylene (MDPE), or linear low density polyethylene (LLDPE), or a mixture thereof; and 61-99% by weight, such as 71-99% by weight, for example 81-99% by weight, of low density polyethylene (LDPE).

[0033] As used herein, the term "consisting essentially of" means that the coating layer consists of at least 95% by weight, preferably at least 98% by weight, of the component in question. The remainder may be other polymers or additives.

[0034] Coating resin formulations can vary widely depending on the intended use of the coating and the coated paper or paperboard. Coating compositions can contain a wide range of ingredients in varying amounts to improve the final performance of the product or the processing of the coating. In some embodiments, the PE coating contains at least one additional ingredient selected from the group consisting of polymers other than PE, pigments (e.g., TiO2 or carbon black), dyes, and fillers (e.g., CaCO3, talc).

[0035] In some embodiments, the first coating layer is formed by extrusion coating onto the surface of the paper or paperboard. The extrusion coated PE blend coating layer may help promote adhesion of a subsequently applied or coextruded polymeric coating layer. The extrusion coated PE blend layer may help promote adhesion of a subsequently applied or coextruded second coating layer, for example, consisting essentially of low density polyethylene (LDPE).

[0036] In some embodiments, the second coating layer is formed by extrusion coating onto the first coating layer. Preferably, the first coating layer and the second coating layer are formed simultaneously by co-extrusion coating.

[0037] The PE blend used in the first coating layer of the present invention has improved stability in film formation and has a coating strength of 12 g / m 2 This enables the production of coated paper or paperboard with adhesion of the PE coating to the paper or paperboard at low total basis weights of PE, such as basis weights of less than 100 g / m2.

[0038] The first coating layer and the second coating layer have a thickness of 12 g / m 2 Preferably, the first coating layer and the second coating layer have a total basis weight of 5 to 12 g / m 2 In some embodiments, the first coating layer and the second coating layer have a total basis weight in the range of 10 g / m 2Less than 5-10g / m 2 in the range of 8 g / m 2 Less than 5-8g / m 2 The total basis weight ranges from 1.0 to 1.0 grammage.

[0039] In some embodiments, the first coating layer has a thickness of 5 g / m 2 Less than 1-5g / m 2 in the range of 4 g / m 2 Less than 1-4g / m 2 More preferably, in the range of 3 g / m 2 Less than 1-3g / m 2 The composition has a basis weight in the range of 1000 to 2000 g.

[0040] In some embodiments, the second coating layer has a thickness of 10 g / m 2 Less than 4-10g / m 2 in the range of 8 g / m 2 Less than 4-8g / m 2 More preferably, in the range of 6 g / m 2 Less than 4-6g / m 2 The composition has a basis weight in the range of 1000 to 2000 g.

[0041] The first coating layer comprises a blend or mixture of high density polyethylene (HDPE), medium density polyethylene (MDPE) or linear low density polyethylene (LLDPE), and low density polyethylene (LDPE). HDPE has a density of 0.930 to 0.940 g / cm. 3 , and the density of MDPE is 0.926~0.940g / cm 3 The density of LLDPE is 0.918~0.940g / cm 3 The density of LDPE is in the range of 0.910 to 0.940 g / cm 3 The range is.

[0042] In some embodiments, the first coating layer comprises a blend of MDPE and LDPE. The MDPE preferably contains higher alpha olefin branching, preferably octene.

[0043] In some embodiments, the second coating layer has a lower density than the first coating layer.

[0044] In some embodiments, the second coating layer is the top layer of the polymeric coating.

[0045] In some embodiments, the polymeric coating has better adhesion to the surface of the paper or paperboard than an LDPE coating having the same total basis weight.

[0046] The paper or paperboard of the present invention is particularly useful in the manufacture of sealed paper or paperboard products, such as waterproof paper cups. According to a second aspect shown herein, there is provided a sealed paper or paperboard product comprising the paper or paperboard according to the first aspect described herein. In a preferred embodiment, the product is a paper cup.

[0047] According to a third aspect presented herein, there is provided a method comprising: 1. A method for producing a polyethylene (PE) coated paper or paperboard substrate, comprising: a) providing a paper or paperboard substrate; b) applying at least one layer of a molten first polymer resin to a surface of the substrate by extrusion coating to form a first polymer coating layer, the first polymer resin comprising a blend of: High density polyethylene (HDPE), medium density polyethylene (MDPE) or linear low density polyethylene (LLDPE), or a mixture thereof; and Low density polyethylene (LDPE), c) applying at least one layer of a molten second polymeric resin to a surface of the first polymeric coating layer by extrusion coating to form a second polymeric coating layer, the second polymeric resin consisting essentially of low density polyethylene (LDPE); d) cooling and solidifying the first and second coating layers; and e) Recovering the PE coated paper or paperboard substrate.

[0048] The first and second coating layers of the third embodiment may be further defined as above with reference to the first embodiment.

[0049] In some embodiments, the first coating layer and the second coating layer are formed simultaneously by coextrusion coating.

[0050] In some embodiments, the method does not include applying an additional coating layer other than the first and second coating layers, i.e., the polymer coating, the formed PE coated substrate consists of the first and second coating layers. In other embodiments, the method includes applying one or more additional coating layers in addition to the first and second coating layers.

[0051] Although the present invention has been described with reference to various exemplary embodiments, those skilled in the art will recognize that various changes can be made and equivalents can be substituted for elements thereof without departing from the scope of the invention. In addition, many modifications can be made to adapt a particular situation or material to the teachings of the invention without departing from its essential scope. Therefore, it is not intended that the invention be limited to the particular embodiment disclosed as the best mode contemplated for carrying out this invention, but the invention is intended to include all embodiments falling within the scope of the appended claims. [Brief description of the drawings]

[0052] Brief description of the drawings [Figure 1] FIG. 1 is an optical micrograph showing the coating layer thickness of Coating Structure 1 at the pinhole limit of about 11 g / m2. The magnification of the optical micrograph is 400x. [Diagram 2]FIG. 2 shows the adhesion properties of coating structure 1 as a function of decreasing coating weight. [Diagram 3] FIG. 3 shows the pinhole performance of Coating Structure 1 as a function of decreasing coating weight. [Figure 4] FIG. 4 is an optical micrograph (400x) showing the coating layer thickness of Coating Structure 2 at the pinhole limit with a coating weight of about 10 g / m2. [Diagram 5] FIG. 5 shows the adhesion properties of coating structure 2 as a function of decreasing coating weight. [Figure 6] FIG. 6 shows the pinhole performance of coating structure 2 as a function of decreasing coating weight. [Figure 7] FIG. 7 is an optical micrograph (400x) showing the coating layer thickness of Coating Structure 3 at the pinhole limit with a coating weight of about 5.5 g / m2. [Figure 8] FIG. 8 shows the adhesion properties of coating structure 3 as a function of decreasing coating weight. [Figure 9] FIG. 9 shows the pinhole performance of coating structure 3 as a function of decreasing coating weight. [Figure 10] FIG. 10 is an optical micrograph (400x) showing the coating layer thickness of Coating Structure 4 at the pinhole limit with a coating weight of about 9 g / m2. [Figure 11] FIG. 11 shows the adhesion properties of coating structure 4 as a function of decreasing coating weight. [Figure 12] FIG. 12 shows the pinhole performance of coating structure 4 as a function of decreasing coating weight. [Figure 13] FIG. 13 is an optical micrograph (400x) showing the coating layer thickness of Coating Structure 5 at the pinhole limit with a coating weight of about 12 g / m2. [Figure 14]FIG. 14 shows the adhesion properties of coating structure 5 as a function of decreasing coating weight. [Figure 15] FIG. 15 shows the pinhole characteristics of coating structure 5 as a function of decreasing coating weight.

[0053] example The invention is now illustrated using five different low density polyethylene (LDPE) based coating structures extrusion coated on the same type of paperboard (Cupforma Natura 195 gsm, Stora Enso Oy) using the same extrusion coating equipment and the same optimized processing parameter settings. 3 ) was added to the branched LDPE grade (Borealis CA7230, density 923 kg / m 3 The effect of PE on the coating properties was investigated by mixing experiments. The drawdown properties of PE-based coating structures were evaluated by extrusion coating at increasing line speeds until the polymer curtain collapsed. The coating properties were measured as a function of layer thickness (coating weight, i.e. basis weight).

[0054] For the extrusion coating procedures in Examples 1-5 below, a pilot line configuration was used with two single screw extruders (1 and 2) and a typical chill and nip roll arrangement. A conventional wide tapered land die with lip heater, inner deckle, and encapsulation system was used. The coating weight (basis weight) of the extrusion coated structures was measured according to standard EN ISO536. Five parallel measurements were made at each line speed. The actual film thickness on the coated paperboard samples was measured with an Axioskop 40 polarizing microscope (Carl Zeiss Light Microscopy, Germany).

[0055] The adhesion of the coated polymer layer to the paperboard substrate was evaluated using a manual coating peel evaluation method. An X is cut in the coated film layer on the substrate, and then the coating film is peeled in the machine and cross directions. If the fibers are torn from the substrate, the adhesion can be evaluated by determining the amount of torn fibers. The size of the coating surface area of ​​the release film covered with the torn fibers is a visual measure of the adhesion value. If there are no fibers attached on the peeled coating, the coating is not adhered to the substrate, i.e., the adhesion value is 1. If there are few substrate fibers covering the peeled coating surface, the adhesion value is 2. If less than 50% of the peeled coating area is covered with torn substrate fibers, the adhesion value is 3. If more than 50% of the peeled coating area is covered with torn substrate fibers, the adhesion value is 4. If the peeled coating is completely (100%) covered with torn fibers, the adhesion is 5. If all of the coating is not attached to the substrate, i.e., the coating is loose, the adhesion value is zero (0).

[0056] The amount of pinholes in the coating structure was measured using a colored turpentine solution penetration method as follows: -Ingredients of pinhole solution: 1) turpentine (L-turpentine) as a solvent, 2) Sudan III (Sudan G) as a red colorant (1%), 3) anhydrous calcium chloride (5%). -The colored turpentine solution was applied with a brush onto a polymer-coated cardboard. -The solution was kept on the surface for 10 minutes and allowed to dry, penetrating possible pinholes in the coating. - 100cm surface area on the opposite side of the coated structure 2 The number of pinholes on the top was calculated and marked as the result. -Three parallel measurements were made, all of which had to show the absence of pinholes at the grammage in question in order to prove the absence of pinholes.

[0057] Example 1 - LDPE as top layer and adhesive layer (Comparative Example) A coating structure 1 consisting of a low density polyethylene (LDPE, Borealis CA7230) as the first coating layer (1) and the same low density polyethylene (LDPE) as the second coating layer (2) was coextrusion coated onto paperboard (Cupforma Natura 195 gsm, Stora Enso Oy) using fixed process parameter settings. The second coating layer (2) was the top layer of the coating structure.

[0058] The minimum coating weight achievable with coating structure 1 is 7 g / m 2 (See Figure 2).

[0059] Adhesion strength is at a minimum coating weight of 7g / m 2 It was complete (value 5).

[0060] Coating weight is approximately 11g / m 2 Below this, pinholes began to appear in coating structure 1 (see Figure 3). In that case, the thicknesses of the first and second coating layers were 6.2 and 4.1 μm, respectively (see Figure 1). The draw-down ratio (DDR) at the pinhole limit was 54.

[0061] Example 2 - MDPE / LDPE blend as top layer and LDPE as adhesive layer Coating structure 2, consisting of a low density polyethylene (LDPE, Borealis CA7230) as the first coating layer (1) and a blend of the same low density polyethylene (LDPE) and medium density polyethylene (MDPE, DOWLEX 2062GC) as the second coating layer (2), was coextrusion coated onto paperboard (Cupforma Natura 195 gsm, Stora Enso Oy) using fixed process parameter settings. The blend consisted of 80 wt% LDPE and 20 wt% MDPE. The second coating layer (2) was the top layer of the coating structure.

[0062] The minimum coating weight achievable with coating structure 2 is 6.5 g / m2 (See Figure 5).

[0063] Adhesion strength is at a minimum coating weight of 6.5g / m 2 It was complete (value 5).

[0064] Coating weight is approximately 10g / m 2 Below this, pinholes began to appear in coating structure 2 (see Figure 6). In that case, the thicknesses of the first and second coating layers were 6.0 and 4.3 μm, respectively (see Figure 4). The draw-down ratio (DDR) at the pinhole limit was 57.

[0065] Example 3 - LDPE as top layer and MDPE / LDPE blend as adhesive layer A coating structure 3 consisting of a blend of medium density polyethylene (MDPE, DOWLEX 2062GC) and low density polyethylene (LDPE, Borealis CA7230) as the first coating layer (1) and the same low density polyethylene (LDPE) as the second coating layer (2) was coextrusion coated onto paperboard (Cupforma Natura 195 gsm, Stora Enso Oy) using fixed process parameter settings. The blend consisted of 80 wt% LDPE and 20 wt% MDPE. The second coating layer (2) was the top layer in the coating structure.

[0066] The minimum coating weight achievable with coating structure 2 is 3.8 g / m 2 (See Figure 8).

[0067] Adhesion strength is at a minimum coating weight of 3.8g / m 2 It was complete (value 5).

[0068] Coating weight is approximately 5.5g / m 2Below this thickness, pinholes began to appear in coating structure 3 (see FIG. 9). In that case, the thicknesses of the first and second coating layers were 3.4 and 2.8 μm, respectively (see FIG. 7). The drawdown ratio (DDR) at the pinhole limit was 103.

[0069] Example 4 - MDPE / LDPE blend as top layer and adhesive layer Coating structure 4, consisting of a blend of medium density polyethylene (MDPE, DOWLEX 2062GC) and low density polyethylene (LDPE, Borealis CA7230) as the first coating layer (1) and the same blend of medium density polyethylene (MDPE) and low density polyethylene (LDPE) as the second coating layer (2), was coextrusion coated onto paperboard (Cupforma Natura 195 gsm, Stora Enso Oy) using fixed process parameter settings. The blend consisted of 80 wt% LDPE and 20 wt% MDPE. The second coating layer (2) was the top layer of the coating structure.

[0070] The minimum coating weight achievable with coating structure 2 is 4.8 g / m 2 (See Figure 11).

[0071] Adhesion strength is at a minimum coating weight of 4.8g / m 2 It was complete (value 5).

[0072] Coating weight is approximately 9.0g / m 2 Below this thickness, pinholes began to appear in coating structure 4 (see FIG. 12). In that case, the thicknesses of the first and second coating layers were 5.2 and 4.7 μm, respectively (see FIG. 10). The drawdown ratio (DDR) at the pinhole limit was 65.

[0073] Example 5 - LDPE single layer (comparison) Coating structure 5, consisting of only low density polyethylene (LDPE, Borealis CA7230) as a single coating layer, was extrusion coated onto paperboard (Cupforma Natura 195 gsm, Stora Enso Oy) using fixed process parameter settings.

[0074] The minimum coating weight achievable with coating structure 1 is 3.6 g / m 2 (See Figure 14).

[0075] Adhesion strength is at a minimum coating weight of 3.6g / m 2 It was complete (value 5).

[0076] Coating weight is approximately 12g / m 2 Below this thickness, pinholes began to appear in coating structure 1 (see FIG. 15). In that case, the thickness of the first and second coating layers was 11.9 μm (see FIG. 13). The drawdown ratio (DDR) at the pinhole limit was 49.

Claims

1. 1. A paper or paperboard comprising a polymeric coating, the polymeric coating comprising: A first coating layer attached to a surface of a paper or paperboard, said first coating layer comprising a blend of: High density polyethylene (HDPE), medium density polyethylene (MDPE) or linear low density polyethylene (LLDPE), or a mixture thereof; and Low density polyethylene (LDPE); and a second coating layer attached to the first coating layer, said second coating layer consisting essentially of low density polyethylene (LDPE); Here, the first coating layer and the second coating layer have a thickness of 12 g / m 2 and the first coating layer and the second coating layer have a total basis weight of less than 5.5 g / m 2 or more. Moreover, the first coating layer consists essentially of a blend of: 1-49% by weight of high density polyethylene (HDPE), medium density polyethylene (MDPE), linear low density polyethylene (LLDPE), or mixtures thereof; and 51-99% by weight of low density polyethylene (LDPE), Moreover, HDPE is 0.930 to 0.970 g / cm 3 and MDPE has a density in the range of 0.926 to 0.940 g / cm 3 and LLDPE has a density in the range of 0.918 to 0.940 g / cm 3 and / or the LDPE has a density in the range of 0.910 to 0.940 g / cm 3 having a density in the range Moreover, the density of HDPE is higher than each of the densities of MDPE, LLDPE and LDPE, and the density of MDPE is higher than each of the densities of LLDPE and LDPE. Moreover, LDPE is a homopolyethylene with some long branches and many short branches. HDPE is a homopolyethylene with a linear structure with little or no branching. The MDPE has some short branches introduced by copolymerization with 1-alkenes selected from 1-butene, 1-hexene and 1-octene, and LLDPE is a copolymer of ethylene and a 1-alkene selected from 1-butene, 1-hexene, 1-octene and 4-methyl-1-pentene, containing 2 to 7% by weight of the 1-alkene. The paper or paperboard as described above.

2. The paper or paperboard of claim 1 , wherein the first coating layer is formed by extrusion coating onto a surface of the paper or paperboard.

3. 3. The paper or paperboard according to any one of claims 1 to 2, wherein the second coating layer is formed by extrusion coating onto the first coating layer.

4. The first coating layer and the second coating layer have a thickness of 10 g / m 2 4. The paper or paperboard of claim 1 having a total basis weight of less than

5. The first coating layer is 5 g / m 2 5. The paper or paperboard of claim 1 having a basis weight of less than 100 g / m.

6. The second coating layer has a thickness of 10 g / m 2 6. The paper or paperboard of claim 1 having a basis weight of less than 100 g / m.

7. The paper or paperboard of any one of the preceding claims, wherein the first coating layer comprises a blend of MDPE and LDPE.

8. 8. The paper or paperboard according to any one of the preceding claims, wherein the second coating layer has a lower density than the first coating layer.

9. 9. The paper or paperboard according to any one of the preceding claims, wherein the second coating layer is a top layer of a polymeric coating.

10. 10. The paper or paperboard of any one of the preceding claims, wherein the polymeric coating has better adhesion to the surface of the paper or paperboard than a LDPE coating of the same total basis weight.

11. 11. A heat sealed paper or paperboard product comprising the paper or paperboard of any one of claims 1 to 10.

12. 12. The heat sealed paper or paperboard product of claim 11, wherein the product is a paper cup.

Citation Information

Patent Citations

  • Extrusion coating polyethylene

    EP1836232A1

  • For the release paper substrates

    JP1984149944U

  • Laminated paper

    JP1993138829A

  • Resin coated paper

    JP1994190983A

  • Easily tearable composite film and easily tearable paper container

    JP1998337829A