Luminescent Composition

Incorporating a polymer with a high Tg into the emissive layer of OLEDs stabilizes the layer and slows down brightness decay, addressing the rapid decay issue in solvent-based deposition methods.

JP7565923B2Active Publication Date: 2024-10-11SUMITOMO CHEM CO LTD
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2021537039
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-01-31
Filing Date
2020-01-31
Publication Date
2024-10-11
Estimated Expiration
2040-01-31

AI Technical Summary

Technical Problem

The rapid decay of brightness in organic light-emitting diodes (OLEDs) is a challenge when using a solvent-based deposition method for the emissive layer, particularly when low glass transition temperature (Tg) host materials are used, leading to inefficient performance.

Method used

Incorporating a polymer with a high Tg into the emissive layer of OLEDs, along with a semiconductor host material having a Tg below 80°C, to stabilize the layer and slow down brightness decay.

Benefits of technology

The presence of a polymer in the emissive layer significantly prolongs the lifetime of OLEDs by maintaining brightness, as demonstrated by reduced decay rates in comparative tests.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007565923000019
    Figure 0007565923000019
  • Figure 0007565923000020
    Figure 0007565923000020
  • Figure 0007565923000021
    Figure 0007565923000021
Patent Text Reader

Abstract

A composition comprising a first semiconducting host compound having a glass transition temperature (Tg) of less than 80°C, a first light-emitting material, and a polymer. The polymer may be an inert polymer, such as polystyrene. The composition may be used in an emissive layer of an organic light-emitting device.
Need to check novelty before this filing date? Find Prior Art

Description

[Background technology]

[0001] SUMMARY OF THE DISCLOSURE Embodiments of the present disclosure relate to light-emitting compositions, particularly for organic light-emitting diodes.

[0002] Electronic devices containing active organic materials are known for use in devices such as organic light emitting diodes (OLEDs), organic photoresponsive devices (particularly organic solar cell devices and organic photosensors), organic transistors, and memory array devices. Devices containing active organic materials offer advantages such as low weight, low power consumption, and flexibility. Furthermore, the use of soluble organic materials allows the use of solution processing, e.g., inkjet printing or spin coating, in device fabrication.

[0003] An OLED may include a substrate carrying an anode, a cathode, and one or more organic light-emitting layers between the anode and the cathode.

[0004] Holes are injected into the device through the anode and electrons are injected through the cathode during operation of the device. A hole in the highest occupied molecular orbital (HOMO) and an electron in the lowest unoccupied molecular orbital (LUMO) of the light-emitting material combine to form an exciton, which releases its energy as light.

[0005] Light-emitting materials include small molecule materials, polymeric materials, and dendritic materials. Light-emitting polymers include poly(arylene vinylenes), such as poly(p-phenylene vinylene), and polymers containing arylene repeat units, such as fluorene repeat units.

[0006] The light-emitting layer may include a host material and a light-emitting dopant, in which energy is transferred from the host material to the light-emitting dopant. For example, J. Appl. Phys. 65, 3610, 1989 discloses a host material doped with a fluorescent light-emitting dopant (i.e., a light-emitting material that emits light via the decay of singlet excitons).

[0007] Phosphorescent emissive dopants (ie, emissive dopants that emit light via the decay of triplet excitons) are also known.

[0008] US2016 / 197275 discloses mixed hosts for use in the emissive layer of an OLED. Summary of the Invention

[0009] The following is a summary of the aspects of certain embodiments disclosed herein. It should be understood that these aspects are presented only to provide the reader with a concise summary of these specific embodiments, and these aspects are not intended to limit the scope of the present disclosure. In fact, the present disclosure may encompass various aspects and / or combinations of aspects that may not be described.

[0010] When the light-emitting layer of an OLED is formed by depositing the components of the layer using a solution deposition method, it is desirable to heat the layer to remove the solvent. The inventors have found that heating a light-emitting layer containing a host material having a low glass transition temperature (Tg), for example a Tg less than about 80° C., can result in a rapid decay of luminance from the resulting OLED.

[0011] The present inventors have found that the presence of a polymer in the light-emitting layer of an OLED can slow the rate at which the luminance of the OLED decays.

[0012] Thus, in some embodiments, a composition is provided that includes a semiconducting host material having a Tg less than 80° C., a light-emitting material, and a polymer.

[0013] In some embodiments, a formulation is provided that includes a composition described herein dissolved or dispersed in one or more solvents.

[0014] In some embodiments, an organic light emitting device is provided that includes an anode, a cathode, and an emissive layer between the anode and the cathode, where the emissive layer includes a composition described herein.

[0015] In some embodiments, a method of forming an organic light-emitting device is provided that includes forming an emissive layer over one of an anode and a cathode, and forming the other of the anode and cathode over the emissive layer, where forming the emissive layer includes depositing a formulation as described herein and evaporating one or more solvents. [Brief description of the drawings]

[0016] The present disclosure is described in conjunction with the accompanying drawings. It is emphasized that, according to standard practice in the industry, various features are not drawn to scale. In fact, dimensions of various features may be arbitrarily increased or decreased for clarity of discussion. In the accompanying drawings, similar components and / or features may have the same reference label. Additionally, various components of the same type may be distinguished by following the reference label with a dash and a second label that distinguishes between the similar components. In this specification, if only a first reference label is used, the description is applicable to any one of the similar components having the same first reference label, regardless of the second reference label. [Figure 1] 1 illustrates an OLED according to some embodiments of the present disclosure. [Diagram 2] 1 is a graph of luminance versus time for OLEDs according to some embodiments of the present disclosure and a comparative OLED in which the emissive layer does not contain a polymer. [Diagram 3] 1 is a graph of luminance versus time for OLEDs according to some embodiments of the present disclosure and a comparative OLED in which the emissive layer does not contain a polymer. [Figure 4] 1 is a graph of luminance versus time for a comparative OLED in which the light-emitting layer does not contain a semiconductor host material. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] 1 shows an OLED 100 according to one embodiment, including an anode 101, a cathode 105, and an emissive layer 103 between the anode and the cathode. The device 100 is supported on a substrate 107, for example a glass or plastic substrate.

[0018] One or more additional layers, such as a hole transporting layer, an electron transporting layer, a hole blocking layer, and an electron blocking layer, may be provided between the anode 101 and the cathode 105. The device may contain two or more light-emitting layers.

[0019] Exemplary device structures include, but are not limited to, the following: Anode / hole injection layer / light emitting layer / cathode Anode / hole transport layer / light emitting layer / cathode Anode / hole injection layer / hole transport layer / light emitting layer / cathode Anode / hole injection layer / hole transport layer / light emitting layer / electron transport layer / cathode.

[0020] Preferably, at least one of a hole transport layer and a hole injection layer is present. Preferably, both a hole injection layer and a hole transport layer are present.

[0021] The light emitting materials include red, green, and blue light emitting materials.

[0022] The blue light-emitting material may have a photoluminescent spectrum with a peak in the range of 400 to 490 nm, optionally 420 to 490 nm.

[0023] The green emitting material may have a photoluminescent spectrum with a peak in the range from greater than 490 nm to 580 nm, optionally greater than 490 nm to 540 nm.

[0024] The red emitting material may optionally have a peak in its photoluminescent spectrum between greater than 580 nm and 630 nm, optionally between 585 and 625 nm.

[0025] The photoluminescence spectrum of the compounds of formula (I) may be measured by casting 5% by weight of the material in a polystyrene film onto a quartz substrate and measuring in a nitrogen environment using an instrument C9920-02 supplied by Hamamatsu.

[0026] Light-emitting layer 103 contains a composition that includes a first semiconducting host compound doped with a first light-emitting material, the first semiconducting host compound having a Tg less than 80° C. The light-emitting layer further contains a polymer.

[0027] Light-emitting layer 103 may consist essentially of these materials, or it may contain one or more additional materials, such as one or more additional semiconducting host materials and / or one or more additional light-emitting materials.

[0028] In some embodiments, the semiconducting host compound comprises from 40 to 95 weight percent, optionally from 40 to 75 weight percent, and optionally from 40 to 60 weight percent of the mass of the composition.

[0029] In some embodiments, the first emissive material comprises from 0.5 to 45 weight percent, optionally from 5 to 45 weight percent, optionally from 10 to 30 weight percent of the mass of the composition.

[0030] In some embodiments, the polymer comprises from 10 to 40% by weight, optionally from 15 to 30% by weight, optionally from 20 to 25% by weight of the mass of the composition.

[0031] The first and any further emissive materials may be selected from fluorescent and phosphorescent emissive materials.

[0032] In the case of fluorescent materials, the lowest excited state singlet (S 1 ) is preferably 0.1 eV or less lower than that of the fluorescent light-emitting material, and more preferably is about the same as or higher than that of the fluorescent light-emitting material.

[0033] In the case of a phosphorescent light-emitting material, the lowest excited state triplet (T1) energy level of the or each host material is preferably no more than 0.1 eV below that of the phosphorescent light-emitting material, and more preferably about the same as or higher than that of the phosphorescent light-emitting material.

[0034] When the light-emitting layer includes a phosphorescent light-emitting dopant, the or each host compound preferably has a T1 greater than 2.8 eV, preferably greater than 3.0 eV.

[0035] The triplet energy levels of the host compound and the phosphorescent compound can be determined from the energy onset of the phosphorescent emission spectrum measured by low-temperature phosphorescence emission spectroscopy (YV Romaovskii et al, Physical Review Letters, 2000, 85(5), p1027, A. van Dijken et al, Journal of the American Chemical Society, 2004, 126, p7718).

[0036] The first host compound preferably has a HOMO level at least 5.8 eV above the vacuum level, preferably at least 5.9 eV above the vacuum level.

[0037] The first host compound preferably has a LUMO level no greater than 2.5 eV from the vacuum level, optionally no greater than 2.0 eV from the vacuum level.

[0038] The HOMO and LUMO levels given herein are measured by square wave voltammetry.

[0039] First Host Compound The first host compound has a Tg of less than 80°C, optionally no greater than 75°C, 70°C, or 65°C.

[0040] The first host compound has the formula (I): [ka] (In the formula, Ar 1 is an arylene or heteroarylene group that is unsubstituted or substituted with one or more substituents; each Y is independently O or S; R 3 is independently, at each occurrence, a substituent; each x is independently 0, 1, 2, or 3.

[0041] Ar 1 may be a monocyclic or fused arylene or heteroarylene group. Ar 1 Optionally, C 6-20 arylene and 5- to 20-membered heteroarylene. 1 is phenylene.

[0042] Ar 1 may be unsubstituted or may contain one or more groups R 4 and R 4 is, independently at each occurrence, a substituent. When present, the substituent R 4 is optionally branched, linear, or cyclic C 1-20 alkyl (wherein one or more non-adjacent C atoms are optionally replaced by O, S, CO, or COO).

[0043] Optionally, one or both of the dibenzofuran or dibenzofuran groups of formula (I) may be linked through their 2-position to Ar 1 is combined with

[0044] Preferably, each x is 0 or 1, more preferably 0.

[0045] Optionally, the compound of formula (I) has formula (Ia): [ka] wherein a is 0, 1, 2, or 3, preferably 0 or 1.

[0046] Optionally, the first host compound has Formula (II): [ka] (In the formula, Ar 1 , Y, R 3 and x is as described for formula (I), R 1 is a substituent, R 2 is a substituent and each b is independently 0, 1, 2, or 3.

[0047] Optionally, R 1 teeth, Alkyl, optionally C 1-20 alkyl (wherein one or more non-adjacent, non-terminal C atoms may be replaced by a group selected from O, S, C═O, or —COO), and Formula -(Ar 2 ) n Group (Ar 2 is, in each occurrence, independently unsubstituted or substituted with one or more substituents; 6-20 aryl or a 5-20 membered heteroaryl group, where n is at least 1, and optionally 1, 2, or 3.

[0048] As used herein, a "non-terminal C atom" of an alkyl group means an atom of the alkyl chain other than the terminal methyl group of an n-alkyl chain or the terminal methyl group of a branched alkyl chain.

[0049] Optionally, Ar 2 is phenyl.

[0050] Ar 2 The substituents, if present, are C 1-12alkyl (one or more non-adjacent, non-terminal C atoms may be replaced by a group selected from O, S, C=O, or -COO, and one or more H atoms of the alkyl may be replaced by F).

[0051] If present, R 2 may, at each occurrence, independently 1-20 alkyl (wherein one or more non-adjacent, non-terminal carbon atoms of the alkyl are optionally replaced with O, S, C=O, or COO, and one or more H atoms of the alkyl are optionally replaced with F).

[0052] Preferably, b is 0 or 1, and more preferably 0.

[0053] The compound of formula (II) has the formula (IIa): [ka] may have the following structure:

[0054] Exemplary compounds of formula (I) are: [ka]

[0055] Exemplary compounds of formula (II) are: [ka]

[0056] polymer The polymer may be an inactive polymer, ie, a polymer that does not contribute to hole or electron transport in the light-emitting layer of the OLED.

[0057] The inert polymer preferably has a non-conjugated backbone, e.g., sp 3-hybridized carbon atoms. Monocyclic aromatic rings may be pendant from the polymer backbone, for example, as in polystyrene.

[0058] The inert polymer may have a HOMO that is at least 1 eV deeper (further away from the vacuum level) than the first emissive material. The inert polymer may have a LUMO that is shallower (closer to vacuum) than any other material of the composition.

[0059] The lowest triplet excited state (T1) of the inert polymer is preferably higher than that of any other material in the light-emitting layer. Optionally, the T1 of the polymer is at least 3.0 eV, optionally at least 3.5 eV.

[0060] Optionally, the weight average molecular weight of the polymer is at least 10,000, optionally at least 100,000, optionally at least 250,000. Optionally, the Mw of the polymer may be up to about 2,000,000.

[0061] Luminescent Compounds Light-emitting materials for the light-emitting layers, including the first and additional light-emitting materials described herein, include polymeric and non-polymeric light-emitting materials, each of which may be fluorescent or phosphorescent.

[0062] Preferably, the first light-emitting material is a non-polymeric light-emitting material.

[0063] An exemplary phosphorescent emitting compound has formula (IX): ML 1 q L 2 r L 3 s (III) (Wherein, M is a metal and L 1 , L 2 , and L 3each independently represents a coordinating group which may be unsubstituted or substituted with one or more substituents, q is a positive integer, r and s are each independently 0 or a positive integer, the sum of (aq)+(br)+(cs) is equal to the number of coordination sites available on M, and a is a value equal to the number of coordination sites available on L 1 is the number of coordination points on L 2 is the number of coordination points on L 3 (where θ is the number of coordination points on the

[0064] a, b, and c are preferably each independently 1, 2, or 3. 1 , L 2 , and L 3 are each bidentate ligand (a, b, and c are each 2). In one embodiment, q is 3 and r and s are 0. In another embodiment, q is 1 or 2, r is 1, and s is 0 or 1, preferably 0.

[0065] Heavy elements M induce strong spin-orbit coupling, allowing rapid intersystem crossing and emission from triplet or higher states. Suitable heavy metals M include the d-block metals, especially the second and third row elements, i.e., elements 39-48 and 72-80, especially ruthenium, rhodium, palladium, rhenium, osmium, iridium, platinum, and gold. Iridium is particularly preferred.

[0066] Exemplary Ligands L 1 , L 2 , and L 3 is represented by formula (IV): [ka] (In the formula, Ar 5 and Ar 6 may be the same or different and are independently selected from substituted or unsubstituted aryl or heteroaryl; X 1 and Y 1may be the same or different and may be independently selected from carbon or nitrogen; Ar 5 and Ar 6 X includes a carbon or nitrogen donor such as a porphyrin or a bidentate ligand, which may be condensed together. 1 is carbon and Y 1 Ligands in which Ar is nitrogen are preferred, especially those in which Ar 5 is a monocyclic or fused heteroaromatic ring of only N and C atoms, e.g., pyridyl or isoquinoline, and Ar 6 Preferred are ligands in which is a monocyclic or fused aromatic ring, for example phenyl or naphthyl.

[0067] Ar 5 and Ar 6 Each of may carry one or more substituents. Two or more of these substituents may be linked to form a ring, for example an aromatic ring. Preferred substituents are D, F, C, 1-20 an alkyl group (wherein one or more non-adjacent C atoms are optionally replaced by O, S, CO or COO and one or more H atoms are optionally replaced by F), a phenyl or biphenyl which may be unsubstituted or substituted by one or more substituents, optionally containing one or more C 1- 10 Alkyl or C 1-12 The alkoxy group is selected from a dendron.

[0068] To achieve red emission, Ar 5 may be selected from phenyl, fluorene, naphthyl; Ar 6 is selected from quinoline, isoquinoline, thiophene, and benzothiophene. To achieve green emission, Ar 5 may be selected from phenyl or fluorene; Ar 6 may be pyridine.

[0069] To achieve blue emission, Ar 5 may be selected from phenyl, Ar 6may be selected from imidazole, pyrazole, triazole, and tetrazole.

[0070] X 1 is carbon and Y 1 Examples of bidentate ligands of formula (X) where is nitrogen are [ka] (In the formula, R 14 is a substituent and each C atom may independently be unsubstituted or be a substituent R 15 (which may be substituted with).

[0071] Substituent R 14 and R 15 is preferably C 1-40 Hydrocarbyl groups, preferably linear, branched or cyclic C 1-20 Alkyl groups, which may be unsubstituted or have one or more C 1-12 It is selected from phenyl or biphenyl, which may be substituted with an alkyl group, and dendrons.

[0072] Other suitable ligands for use with the d-block elements include O,O-bidentate ligands, optionally diketonates, O,N-bidentate ligands, and N,N-bidentate ligands, particularly acetylacetonate (acac), tetrakis-(pyrazol-1-yl)borate, 2-carboxypyridyl, triarylphosphines, and pyridine.

[0073] L 1 , L 2 , and L 3 One or more of may contain a carbene group.

[0074] In some embodiments, the compositions described herein have formula (III): (q is 2 or 3, and each L 1 is represented by formula (IV); r is 0 or 1, and L 2is, if present, a C,N-bidentate ligand or an O,O-, N,N- or O,N-bidentate ligand of formula (IV); s is 0, M is iridium.

[0075] The dendrons described herein include a branch point attached to a ligand of a metal complex and two or more dendritic branches. Preferably, the dendrons are at least partially conjugated, and at least one of the branch points and dendritic branches includes an aryl or heteroaryl group, e.g., a phenyl group. In one arrangement, the branch point group and the branching groups are all phenyl, and each phenyl independently includes one or more substituents, e.g., C 1-20 It may be substituted with alkyl or alkoxy.

[0076] The dendron may optionally be represented by a substituted formula (V): [ka] where BP represents the branch point of attachment to the core and G1 represents a first generation branching group.

[0077] The dendron may be a first, second, third or higher generation dendron. G1 is optionally a substituted group of formula (Va): [ka] where u is 0 or 1, v can be 0 when u is 0, or 0 or 1 when u is 1, BP represents the branch points for attachment to the core, and G1, G2, and G3 represent the first, second, and third generation dendron branching groups, and may be substituted with two or more second generation branching groups G2, etc., such as: n is phenyl, and each phenyl B, G, G...G n-1 is a 3,5-linked phenyl.

[0078] Preferred dendrons have the formula (Vb): [ka] where * represents the point of attachment of the dendron to the ligand.

[0079] BP and / or any group G may be one or more substituents, e.g., one or more C 1-20 It may be substituted with an alkyl group or an alkoxy group.

[0080] The light-emitting layer may include a first light-emitting material and one or more additional light-emitting materials, for example a mixture of light-emitting materials that together provide white light emission.

[0081] A white-emitting OLED may contain a single white-light-emitting layer containing the light-emitting composition described herein, or it may contain two or more layers that emit different colors that combine to produce white light, at least one of the light-emitting layers comprising the composition described herein.

[0082] Light emitted from a white-emitting OLED may have CIEx coordinates equivalent to that emitted by a black body at a temperature in the range of 2500-9000 K, and CIEy coordinates within 0.05 or 0.025 of the CIEy coordinates of the light emitted by a black body, optionally CIEx coordinates equivalent to that emitted by a black body at a temperature in the range of 2700-6000 K.

[0083] Charge Transport and Charge Blocking Layers The OLEDs described herein may have one or more layers selected from charge transport and charge blocking layers.

[0084] A hole transport layer may be provided between the anode and the light emitting layer(s) of the OLED. An electron transport layer may be provided between the cathode and the light emitting layer(s).

[0085] An electron blocking layer may be provided between the anode and the light-emitting layer(s), and a hole blocking layer may be provided between the cathode and the light-emitting layer(s). Charge transport layers and charge blocking layers may be used in combination. Depending on the HOMO and LUMO levels of the material(s) in the layer, a single layer may transport one of holes and electrons and block the other of holes and electrons.

[0086] If present, a hole transport layer located between the anode and the light-emitting layer(s) preferably has a material with a HOMO level of 5.5 eV or less, more preferably about 4.8-5.5 eV or 4.9-5.3 eV, as measured by square wave voltammetry. The HOMO level of the material in the hole transport layer may be selected to be within 0.2 eV, optionally within 0.1 eV, of the light-emitting material of the light-emitting layer. The inert polymer of the light-emitting layer may have a HOMO level at least 1 eV deeper than any material in the hole transport layer.

[0087] The hole transport layer may contain a polymeric or non-polymeric charge transport material. The hole transport polymer may be as described in WO99 / 54385, WO2004 / 060970, WO2005 / 049546, or WO2013 / 108023, the contents of which are incorporated herein by reference.

[0088] The charge transport layer or the charge blocking layer may be crosslinked, especially when the layer above the charge transport layer or the charge blocking layer is deposited from a solution. The crosslinkable group used for this crosslinking may be a crosslinkable group that includes such reactive double bonds and vinyl or acrylate groups, or benzocyclobutane groups. The crosslinkable group may be provided as a substituent of the charge transport material or the charge blocking material used to form the charge transport layer or the charge blocking layer, or may be mixed therewith. The crosslinkable group may be provided as a substituent of the repeat unit of the hole transport polymer, for example, as described in WO2016 / 005749, the contents of which are incorporated herein by reference.

[0089] A charge transport layer adjacent to an emissive layer containing a phosphorescent emissive material preferably contains a charge transport material having a lowest triplet excited state (T1) excited state of 0.1 eV or less lower than, and preferably the same as or higher than, the T1 excited state energy level of the phosphorescent emissive material(s) to avoid quenching of triplet excitons.

[0090] The charge transport layer described herein may be non-emissive or may contain a light-emitting material so that the layer is a charge transport light-emitting layer. When the charge transport layer is a polymer, the light-emitting dopant may be provided as a side group of the polymer, a repeat unit in the backbone of the polymer, or an end group of the polymer. Optionally, the hole transport polymer described herein includes a phosphorescent light-emitting polymer in a side group of the polymer, a repeat unit in the backbone of the polymer, or an end group of the polymer.

[0091] Hole injection layer A conductive hole injection layer, which may be formed from a conductive organic or inorganic material, may be provided between the anode 101 and the light-emitting layer 103 of the OLED, as shown in Figure 1, to assist hole injection from the anode into the layer(s) of semiconducting polymer. Examples of doped organic hole injection materials include optionally substituted doped poly(ethylenedioxythiophene) (PEDOT), in particular PEDOT doped with charge-balancing polyacids such as polystyrene sulfonate (PSS) as disclosed in EP0901176 and EP0947123, polyacrylic acid or fluorinated sulfonic acid, e.g. Nafion®, polyaniline as disclosed in US5723873 and US5798170, and optionally substituted polythiophenes or poly(thienothiophenes). Examples of conductive inorganic materials include transition metal oxides, such as VOx, MoOx, and RuOx, as disclosed in Journal of Physics D: Applied Physics (1996), 29(11), 2750-2753.

[0092] Cathode The cathode 105 is selected from materials having a work function that allows injection of electrons into the light-emitting layer of the OLED. Other factors, such as the possibility of adverse interactions between the cathode and the light-emitting material, influence the choice of the cathode. The cathode may consist of a single material, such as a layer of aluminum. Alternatively, the cathode may comprise a bilayer of multiple conductive materials, such as metals, e.g., a low work function material and a high work function material, e.g., calcium and aluminum, as disclosed, for example, in WO 98 / 10621. The cathode may comprise elemental barium, as disclosed, for example, in WO 98 / 57381, Appl. Phys. Lett. 2002, 81(4), 634, and WO 02 / 84759. The cathode may comprise a thin layer of a metal compound (e.g., 1-5 nm), particularly an alkali or alkaline earth metal oxide or fluoride, between the organic layer of the device and one or more conductive cathode layers to aid in electron injection, for example, lithium fluoride as disclosed in WO00 / 48258, barium fluoride as disclosed in Appl. Phys. Lett. 2001, 79(5), 2001, and barium oxide. To provide efficient injection of electrons into the device, the cathode preferably has a work function of less than 3.5 eV, more preferably less than 3.2 eV, and most preferably less than 3 eV. Work functions of metals can be found, for example, in Michaelson, J. Appl. Phys. 48(11), 4729, 1977.

[0093] The cathode may be opaque or transparent. Transparent cathodes are particularly advantageous for active matrix devices, since light emission through the transparent anode in such devices is at least partially blocked by drive circuitry located below the emitting pixels. Transparent cathodes include a layer of electron injection material that is thin enough to be transparent. Typically, the lateral conductivity of this layer is low as a result of its thinness. In this case, the layer of electron injection material is used in combination with a thicker layer of a transparent conductive material, such as indium tin oxide.

[0094] It will be appreciated that a transparent cathode device does not need to have a transparent anode (unless, of course, a completely transparent device is desired) and therefore a transparent anode used for a bottom-emitting device may be replaced or supplemented with a layer of reflective material, for example aluminium. Examples of transparent cathode devices are disclosed, for example, in GB 2348316.

[0095] Enclosure Organic-based optoelectronic devices tend to be sensitive to moisture and oxygen. Therefore, the substrate preferably has good barrier properties to prevent the ingress of moisture and oxygen into the device. The substrate is typically glass, but alternative substrates can be used, especially when device flexibility is desired. For example, the substrate may include one or more plastic layers, such as alternative plastic and dielectric barrier layers, or a substrate of a laminate of thin glass and plastic.

[0096] The device can be encapsulated with an encapsulant to prevent the ingress of moisture and oxygen. Suitable encapsulants include glass plates, films with suitable barrier properties, such as silicon dioxide, silicon monoxide, silicon nitride, or alternating stacks of polymers and dielectrics, or airtight containers. In the case of transparent cathode devices, the transparent encapsulant layer, such as silicon monoxide or silicon dioxide, may be deposited to micron-level thicknesses, but in one preferred embodiment, the thickness of such a layer is in the range of 20-300 nm. A getter material for absorbing any atmospheric moisture and / or oxygen that may permeate through the substrate or encapsulant may be disposed between the substrate and the encapsulant.

[0097] Processing of the formulation Formulations suitable for forming the light-emitting layer of an OLED may be formed by dissolving or dispersing the components of the compositions described herein in one or more solvents.

[0098] The formulation may be a solution of the composition or may be a dispersion in which one or more components of the composition are not dissolved. Preferably, the formulation is a solution.

[0099] Exemplary solvents include one or more of C 1-10 Alkyl or C 1-10 Alkoxy substituted benzenes include, but are not limited to, toluene, xylene, and methylanisole.

[0100] The formulation may contain at least one solvent having a boiling point of at least 100°C, optionally 110°C or 120°C.

[0101] Particularly preferred solution deposition techniques include printing and coating techniques such as spin coating, ink jet printing and slot die coating.

[0102] Spin-coating is particularly suitable for devices in which patterning of the light-emitting layer is not required, for example for lighting applications or simple monochrome split displays.

[0103] Inkjet printing is particularly suitable for displaying large amounts of information content, especially full color displays. The device may be inkjet printed by providing a patterned layer above the first electrode and defining wells for printing one color (for a monochromatic device) or multiple colors (for a multicolor, especially full color device). The patterned layer is typically a layer of photoresist that is patterned to define wells, for example as described in EP0880303.

[0104] As an alternative to wells, the ink may be printed into channels defined in the patterned layer. In particular, the photoresist may be patterned to form channels which, unlike wells, extend over multiple pixels and which may be closed or open at the channel ends.

[0105] Other solution deposition techniques include dip coating, roll printing, and screen printing.

[0106] After deposition of the formulation, the formulation may be heated at atmospheric pressure or in vacuum to evaporate the solvent(s). Optionally, the formulation is heated to a temperature above the Tg of the first host. Optionally, the formulation is heated to a temperature in the range of 80-180°C, optionally 100-150°C. EXAMPLES

[0107] material Host 2 was prepared according to the following reaction scheme: [ka]

[0108] Step 1 - Synthesis of intermediate 3 In a 10 L, 3-neck round bottom flask equipped with a mechanical overhead stirrer, nitrogen inlet and exhaust, 1,3-dibromobenzene (288 g, 1.220 mol) was taken up in tetrahydrofuran (2 L) and cooled to -78°C.

[0109] 2.5M n-Butyllithium in hexane (443mL, 1.109mol) was added slowly and stirred at the same temperature for 2h. 9-Fluorenone (200g, 1.109mol) in THF (500mL) was added slowly at the same temperature. The reaction mixture was allowed to reach room temperature and stirred for 18h, after which it was quenched with saturated NH4Cl solution (200mL) and extracted with EtOAc (3x1L).

[0110] The combined organic phase was washed with water (1000 mL), brine (500 mL), dried over sodium sulfate and concentrated.

[0111] The residue represented about 60% intermediate 3, which was used without further purification.

[0112] Step 2 - Synthesis of intermediate 4 Intermediate 3 (approximately 60% purity, 420 g, 0.771 mol) and triethylsilane (186 mL, 1.156 mol) were taken up in dry dichloromethane (3 L) in a 10 L, 3-neck round bottom flask equipped with a mechanical overhead stirrer, nitrogen inlet and exhaust.

[0113] The reaction mixture was cooled to -10°C and stirred for 0.5 h. Trifluoroacetic acid (175 mL, 2.313 mol) was added slowly and the reaction mixture was stirred at room temperature for 2 h. Crude GCMS analysis showed complete conversion of starting material. The reaction mixture was quenched with water (300 mL) and the organic phase was washed with water (500 mL), brine (500 mL), dried over sodium sulfate and concentrated to give 326 g of crude product.

[0114] The crude product was purified by silica column chromatography using 3-4% ethyl acetate in hexane as eluent and the product was triturated with methanol to give 216 g of intermediate 4 with 92.9% HPLC purity. The compound was crystallized using hot acetonitrile to give 195 g of intermediate 4 with 97.02% purity.

[0115] Step 3 - Synthesis of intermediate 5 Intermediate 4 (195 g, 0.607 mol) was dissolved in dry tetrahydrofuran (1800 mL) and degassed with N for 1 h in a 10 L, 3-neck round bottom flask equipped with a mechanical overhead stirrer, nitrogen inlet and exhaust, then cooled to -20 °C.

[0116] To degassed THF (1200 mL) was added potassium tert-butoxide (68.1 g, 0.607 mol) and purged with nitrogen for 1 h. Methyl iodide (37.9 mL, 0.607 mol) and degassed potassium tert-butoxide solution were added dropwise to intermediate 4.

[0117] The reaction mixture was slowly warmed to room temperature and stirred for 18 h. The reaction mixture was then quenched with NH4Cl solution (500 mL) and extracted with ethyl acetate (3 x 1 L). The combined organic phases were washed with water (1 L), brine (500 mL), dried over sodium sulfate, and concentrated (210 g). The crude product (210 g) was purified by silica column chromatography using 5-6% ethyl acetate in hexane as eluent. The pure fractions were purified twice by hot methanol crystallization to give 155 g of intermediate 5 with 99.19% HPLC purity.

[0118] Step 4 - Synthesizing Host 2 A mixture of intermediate 5 (18 g, 0.053 mol) and dibenzothiophene-4 boronic acid (18.3 g, 0.053 mol) in toluene (360 mL) was purged with N2 gas for 1 h. In a separate vessel, a solution of 25% tetraethylammonium hydroxide (124 mL, 0.212 mol) was degassed with N2 for 1 h.

[0119] The reaction mixture was heated to 60° C. S-phos (0.43 g, 0.0011 mol) and Pd2(dba)3 (0.41 g, 0.00053 mol) were added at 60° C. Degassed tetraethylammonium hydroxide was added and refluxed at 110° C. for 18 h. The reaction mixture was filtered and washed with toluene. The organic phase was washed with water (400 mL), brine (300 mL), dried over sodium sulfate and concentrated (28 g). The crude product was purified by silica column chromatography using 5% ethyl acetate in hexane as eluent to give 24 g of host 2 with 91.6% HPLC purity.

[0120] The product was recrystallized twice with hot toluene / acetonitrile to give 16 g with 99.70% purity, then dissolved in toluene, washed with concentrated sulfuric acid, and concentrated to give 15.5 g of M849 with 99.91% HPLC purity.

[0121] HOMO and LUMO measurements Equipment: CHI660D Electrochemical workstation with software (IJ Cambria Scientific Ltd) CHI 104 3mm Glassy Carbon Disk Working Electrode(IJ Cambria Scientific Ltd)) Platinum wire auxiliary electrode Reference electrode (Ag / AgCl) (Harvard Apparatus Ltd)

[0122] chemicals Acetonitrile (Hi-dry anhydrous grade - ROMIL) (cell solution solvent) Toluene (Hi-dry anhydrous grade) (sample preparation solvent) Ferrocene-FLUKA (reference standard) Tetrabutylammonium Hexafluorophosphate - FLUKA (Cell Solution Salt)

[0123] Sample preparation The HOMO and LUMO values ​​of the semiconducting host compounds were measured from dilute solutions (0.3 wt %) in toluene.

[0124] Electrochemical Cell The measurement cell contains an electrolyte, a glassy carbon working electrode, a platinum counter electrode, and a Ag / AgCl reference glass electrode. Ferrocene is added to the cell at the end of the experiment as a reference material (LUMO(ferrocene)=-4.8 eV).

[0125] Tg measurement The Tg values ​​given herein were determined by differential scanning calorimetry using a PerkinElmer DSC8500 according to the following method. The apparatus is purged with nitrogen gas at 20 ml / min.

[0126] Weigh out 5-10 mg of sample into a sample pan and crimp the lid onto the sample pan to close it.

[0127] The reference pan (empty sample pan and lid) is placed in the reference furnace and the sample is loaded into the sample furnace.

[0128] Heating and cooling are carried out according to the following temperature program: 1) Hold at -50.00°C for 1.0 minute. Switch gas to helium at 20.0 ml / min at the start of the step. 2) Heat from -50.00°C to 300.00°C at 300.00°C / min. 3) Hold at 300.00°C for 1.0 minute. 4) Cool from 300.00°C to 50.00°C at 300.00°C / min. 5) Hold at -50.00°C for 1.0 minute. 6) Heat from -50.00°C to 300.00°C at 20.00°C / min. 7) Hold at 300.00°C for 1.0 minute. 8) Cool from 300.00°C to -50.00°C at 20.00°C / min. 9) Hold at -50.00°C for 1.0 minute. 10) Heat from -50.00°C to 300.00°C at 100.00°C / min. 11) Hold at 300.00°C for 1.0 minute. 12) Cool from 300.00°C to -50.00°C at 100.00°C / min. 13) Hold at -50.00°C for 1.0 minute and switch gas to nitrogen at 20.0 ml / min at the end of the step.

[0129] After analysis, the sample Tg is determined from an increasing temperature ramp of 20° C. / min (i.e., step 6 above). A decreasing temperature ramp of 100° C. / min is used to confirm the Tg event.

[0130] Formulation Example 1 A formulation of host 1 (50 wt%), blue phosphorescent emitter 1 (25 wt%), and polystyrene (25 wt%) was dissolved in mixed xylenes. [ka] Host 1 has a Tg of 54° C. and a LUMO of 1.78 eV.

[0131] Comparative formulation 1 For comparative purposes, a formulation was prepared as described for Formulation Example 1, except that the polystyrene was omitted and the weight ratio of Host 1 to Blue Phosphorescent Emitter 1 was 75:25.

[0132] Formulation Example 2 A formulation of host 2 (55 wt%), blue phosphorescent emitter 2 (25 wt%), and polystyrene (20 wt%) was dissolved in mixed xylenes. [ka] Host 2 has a Tg of 62° C. and a LUMO of 1.93 eV.

[0133] Comparative formulation 2 For comparative purposes, a formulation was prepared as described for Formulation Example 2, except that the polystyrene was omitted and the weight ratio of host 2 to blue phosphorescent emitter 2 was 75:25.

[0134] Device Example 1 An organic light-emitting device was fabricated having the following structure: ITO / HIL / HTL / LEL / ETL / Cathode In the formula, ITO is an indium-tin-oxide anode, HIL is a hole-injection layer comprising a hole-injection material, HTL is a hole-transport layer, LEL is an emissive layer, and ETL is an electron-transport layer.

[0135] A substrate bearing ITO (45 nm) was cleaned using UV / ozone. A hole injection layer was formed to a thickness of about 35 nm by spin-coating a formulation of hole injection material available from Nissan Chemical Industries. A hole transport layer was formed to a thickness of about 20 nm by spin-coating a cross-linkable hole transport polymer containing cross-linkable fluorene repeat units, amine repeat units, and red phosphorescent repeat units, and cross-linking the polymer by heating at 180° C. A light-emitting layer was formed to a thickness of about 90 nm by spin-coating formulation Example 1, followed by heating at 130° C. for 10 minutes. An electron transport layer was formed by spin-coating a polymer containing the cesium salt of electron transport unit 1 described in WO2012 / 133229 to a thickness of 10 nm. A cathode was formed on the electron transport layer of a first layer of sodium fluoride about 10 nm thick, a layer of aluminum about 100 nm thick, and a layer of silver about 100 nm thick. [ka]

[0136] Device Example 2 Device Example 2 was prepared as described for Device Example 1, except that Formulation Example 2 was used instead of Formulation Example 1.

[0137] Compare Device 1 and 2 Comparative Devices 1 and 2 were prepared as described for Device Examples 1 and 2, respectively, except that Comparative Formulations 1 and 2 were used in place of Formulation Examples 1 and 2, respectively.

[0138] Referring to FIG. 2, T 70 (the time it takes for the luminance to drop to 70% of its initial value at constant current) is much longer for Device Example 1 than for Comparative Device 1.

[0139] Referring to FIG. 3, T 70is much longer for Device Example 2 than for Comparative Device 2.

[0140] Comparison Device 3 Comparative Device 3 was prepared as described for Device Example 1, except that the emissive layer was formed from a formulation containing polystyrene (50 wt %) and phosphorescent blue emitter 3 (50 wt %). [ka]

[0141] Comparison Device 4 Comparative Device 4 was prepared as described for Comparative Device 3, except that the weight ratio of polystyrene:phosphorescent blue emitter 3 was 40:60.

[0142] Referring to FIG. 4, a very rapid decay in luminance was observed, demonstrating that the improved lifetime observed in device examples 1 and 2 is not solely due to the presence of polystyrene.

[0143] The above description provides only preferred exemplary embodiment(s) and is not intended to limit the scope, applicability, or configuration of the present invention. Rather, the following description of the preferred exemplary embodiment(s) will provide those skilled in the art with an effective description for implementing the preferred exemplary embodiments of the present invention. It should be understood that various changes may be made in the function and arrangement of elements, including combinations of features of different embodiments, without departing from the scope of the present invention.

[0144] Unless the context clearly requires otherwise, throughout the description and claims, the words "comprise," "comprising," and the like, should be interpreted in an inclusive sense, as opposed to an exclusive or exhaustive sense. That is, they should be interpreted in the sense of "including, but not limited to." As used herein, the terms "connected," "coupled," or any variation thereof, mean any connection or coupling, either direct or indirect, between two or more elements, and the coupling or coupling between the elements may be physical, logical, electromagnetic, or combinations thereof. Additionally, the words "herein," "above," "below," and words of similar meaning, when used in this application, refer to this application as a whole and not to any particular portion of this application. Where the context permits, words in the "Detailed Description" using singular or plural numbers may also include the plural or singular, respectively. The word "or" in reference to a list of two or more items covers all of the following interpretations of the word, namely, any of the items in the list, all of the items in the list, and any combination of the items in the list.

[0145] The teachings of the technology provided herein are applicable to other systems, not necessarily the system described below. Elements and operations of the various embodiments described below can be combined to provide further implementations of the technology. Some alternative implementations of the technology may include fewer elements as well as additional elements to those implementations described below.

[0146] These and other changes can be made to the technology in light of the detailed description below. Although the description describes a particular example of the technology and describes the best mode contemplated, no matter how detailed the description may appear, the technology can be practiced in many ways. The details of the system may vary considerably in its specific implementation, but are still encompassed by the technology disclosed herein. As mentioned above, a particular term used in describing a particular feature or aspect of the technology should not be taken to imply that the term is redefined herein to be limited to any particular characteristic, feature, or aspect of the technology to which it relates. In general, the terms used in the following claims should not be construed to limit the technology to the particular examples disclosed herein, unless the "Description of the Invention" section expressly defines such terms. Thus, the actual scope of the technology encompasses not only the disclosed embodiments, but also all equivalent ways of practicing or implementing the technology based on the claims.

[0147] In order to reduce the number of claims, certain aspects of the technology are presented below in certain claim forms, but the applicant contemplates various aspects of the technology in any claim form. For example, some aspects of the technology may be recited as computer-readable medium claims, but other aspects may also be embodied in other forms, such as computer-readable medium claims or means-plus-function claims.

[0148] In the above description, for purposes of explanation, numerous specific details are set forth in order to provide a thorough understanding of the implementation of the disclosed technology. However, it will be apparent to one skilled in the art that embodiments of the disclosed technology can be practiced without some of these specific details.

Claims

1. A composition comprising a first semiconducting host compound having a glass transition temperature (Tg) of less than 80° C., a first light-emitting material, and a polymer, The first semiconductor host compound has Formula (I) or Formula (II): 【Chemistry 1】 【Chemistry 2】 (In the formula, Ar 1 is an arylene or heteroarylene group that is unsubstituted or substituted with one or more substituents; each Y is independently O or S; R 1 , R 2 , and R 3 are independently, at each occurrence, a substituent; each x is independently 0, 1, 2, or 3; each b is independently 0, 1, 2, or 3; The composition having the formula:

2. 2. The composition of claim 1, wherein the Tg of the first semiconducting host compound is less than 70°C.

3. 3. The composition of claim 2, wherein the Tg of the first semiconducting host compound is less than 65°C.

4. The composition according to any one of claims 1 to 3, wherein the polymer is an inert polymer.

5. The composition of claim 4 , wherein the polymer has a non-conjugated backbone.

6. The composition according to any one of claims 1 to 5, wherein the polymer is polystyrene.

7. The composition of any one of claims 1 to 6, wherein the first semiconducting host compound comprises 40 to 95 weight percent of the mass of the composition.

8. The composition of any one of claims 1 to 7, wherein the first emissive material comprises 0.5 to 45% by weight of the mass of the composition.

9. The composition according to any one of claims 1 to 8, wherein the polymer constitutes 10 to 40% by weight of the mass of the composition.

10. The composition of any one of claims 1 to 9, wherein the first light-emitting material is a phosphorescent light-emitting material.

11. The composition of any one of claims 1 to 10, wherein the first light-emitting material is a blue light-emitting material.

12. The composition according to any one of claims 1 to 11, wherein the first semiconducting host compound has a LUMO of 2.5 eV or less from the vacuum level.

13. A formulation comprising the composition of any one of claims 1 to 12 and one or more solvents.

14. 13. An organic light emitting device comprising an anode, a cathode, and an emissive layer between the anode and the cathode, the emissive layer comprising the composition of any one of claims 1 to 12.

15. 15. A method of forming an organic light-emitting device according to claim 14, comprising forming the light-emitting layer over one of the anode and cathode, and forming the other of the anode and cathode over the light-emitting layer, wherein forming the light-emitting layer comprises depositing the formulation of claim 13 and evaporating the one or more solvents.

16. 16. The method of claim 15, wherein evaporating the one or more solvents comprises heating the deposited formulation at a temperature above the glass transition temperature of the first semiconductor host material.

17. The method of claim 16, wherein the heating temperature is in the range of 80 to 180°C.

Citation Information

Patent Citations

  • Electron transport material

    JP1996259939A

  • Organic el element

    JP2006172762A

  • Bis(aminobiphenyl ethynyl)-based compound, blue fluorescent dye, and organic el element

    JP2012077069A

  • Organic electrophosphorescence device

    JP2012191234A

  • Composition and light emitting element prepared therewith

    JP2018083941A