Method for producing composite cathode for lithium-ion cell
The composite cathode manufacturing method enhances lithium ion cell performance by improving peel strength and capacity retention through controlled mixing and calendering, addressing the challenges of existing cathode materials in lithium ion cells.
Patent Information
- Application Number
- JP2021553775
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-03-14
- Filing Date
- 2020-03-10
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2040-03-10
AI Technical Summary
Existing lithium ion cell cathode materials face challenges in achieving high specific capacity, good cycling performance, and safety, particularly in applications requiring predictable discharge curves.
A manufacturing method involving mixing an active material, conductive diluent, and binder in a planetary mixer, applying the slurry onto an aluminum foil substrate, and calendering at controlled temperatures to produce a composite cathode with improved peel strength and capacity retention.
The method results in lithium ion cells with excellent cathode properties, including capacity retention of over 80% at 2000 cycles and high specific capacity, suitable for applications in electric vehicles, launch vehicles, artificial satellites, submarines, and aircraft.
Smart Images

Figure 0007565939000001 
Figure 0007565939000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a composite cathode for a lithium ion cell, and more particularly to a method for producing a composite cathode for a lithium ion cell having excellent peel strength, specific capacity, and retention capacity. [Background technology]
[0002] In recent years, lithium ion cells have attracted considerable attention as power sources for a variety of devices, such as mobile phones, cameras, and notebook computers, as well as for high-tech devices, such as military products, aircraft, space equipment, and electric vehicles.
[0003] Generally, a lithium-ion cell includes a cathode, an anode, and an electrolyte as its main components. The performance of a lithium-ion cell depends on the characteristics of the electrodes used, which in turn depend on the type of material used, the composition of the electrodes, and the manufacturing technique of the electrodes.
[0004] Many lithiated metal oxides and phosphates have been used as active materials for the cathode of lithium-ion cells. The cathode materials of lithium-ion cells are required to have high specific capacity, good cycling performance, rate capability, and safety. In addition, some applications, such as satellites, require the discharge curve to be sloped rather than flat, so that the state of charge at any time can be predicted by checking the cell voltage.
[0005] Much research and development has been done on cathode materials, electrode compositions, and processes for lithium-ion cells with specific capacities.
[0006] U.S. Pat. No. 5,672,446 discloses a cathode made of lithium cobalt oxide, lithium manganese oxide, lithium nickel oxide, Li x Ni 1-y Co yThe present invention discloses an electrochemical cell comprising O2 (x is preferably about 1, and y is preferably 0.1 to 0.9), LiNiVO4, or LiCoVO4.
[0007] It would be useful to provide an effective method for producing a composite cathode having excellent cathode properties such as loading level, thickness, water content, and peel strength to achieve good specific capacity and capacity retention, as well as a system for such production. Summary of the Invention
[0008] An object of the present invention is to provide a method for producing a composite cathode for a lithium-ion cell, for a lithium-ion cell having excellent cathode properties applicable to various applications such as electric vehicles, launch vehicles, artificial satellites, submarines, aircraft, etc., the method including the steps of (i) mixing an active material, a conductive diluent, and a binder in a planetary mixer to prepare a cathode slurry; (ii) coating the slurry on an aluminum foil substrate at a speed of 0.2 to 0.8 m / min in a coating device; and (iii) calendering the cathode at a temperature of 50 to 150° C. in a calendering device. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] For purposes of the following detailed description, unless expressly specified to the contrary, the present invention should be understood to include various alternative variations and sequences of steps. Furthermore, except in the operational examples or where otherwise indicated, all numbers used in the specification, such as amounts of materials, should be understood to be modified in all cases by the word "about." Furthermore, unless otherwise specified, all percentages described in this specification and the appended claims refer to amounts by weight of the total composition.
[0010] Thus, before describing the present invention in detail, it is to be understood that this invention is not limited to the parameters of the illustrated systems and methods, as such may, of course, vary. It is also to be understood that the terminology used herein is for the purpose of describing particular embodiments of the invention only, and is not intended to limit the scope of the present invention in any way.
[0011] The applications given as examples herein, such as examples of specific items discussed in this application, are exemplary only and are not intended to limit the scope and meaning of the invention, nor any of the exemplary terms.Similarly, the invention is not limited to the various embodiments herein.
[0012] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. In case of conflict, the present document, including definitions, will control.
[0013] It is to be noted that, as used in this specification and the appended claims, the singular forms "a," "an," and "the" may refer to plural objects unless the context clearly dictates. For example, reference to a "polymer" includes two or more polymers.
[0014] The terms "preffered" and "prefferable" may refer to embodiments of the invention that provide certain advantages in particular situations. However, other embodiments may also be preferred, under the same or different situations. Furthermore, the recitation of one or more preferred embodiments does not imply that other embodiments are not useful, and is not intended to exclude other embodiments from the scope of the invention.
[0015] Moreover, the terms "comprising," "including," "containing," "involving," and the like, should be understood to be open-ended, i.e., meaning including, and not limited.
[0016] In one aspect, the present application provides a method for making a composite cathode for a lithium-ion cell, the method comprising the steps of: (i) mixing an active material, a conductive diluent, and a binder in a planetary mixer to prepare a cathode slurry; (ii) applying the slurry onto an aluminum foil substrate with a coating device at a speed of 0.2 to 0.8 m / min; and (iii) calendering the cathode in a calendering apparatus at a temperature of 50-150°C.
[0017] In one embodiment, the cathode slurry is prepared by mixing the active material, conductive diluent, and binder in the presence of a solvent in a planetary mixer.
[0018] In one embodiment, the active material is LiCoO2, LiNi x Co y Al z O2, LiNi x Co y Mn z O2, etc. In a preferred embodiment, the active material is LiNi x Co y Al z It's O2.
[0019] In one embodiment, the conductive diluent is selected from acetylene black, graphite, carbon nanotubes, and the like, or combinations thereof. In a preferred embodiment, a mixture of acetylene black and graphite is used as the conductive diluent.
[0020] Acetylene black alone is widely used as a conductive diluent for the cathode of lithium-ion cells. Acetylene black is a high-volume particle with an average particle size of tens to hundreds of nanometers. Therefore, the contact between acetylene black and the active material is likely to be a point contact rather than a surface contact. As a result, the contact resistance between the active material and the conductive assistant is high. In addition, if the amount of the conductive assistant is increased to increase the contact points between the active material and the conductive assistant, the proportion of the active material in the cathode is reduced, resulting in a decrease in the discharge performance of the battery. In order to avoid the drawbacks in the prior art, in the present disclosure, a mixture of acetylene black and graphite is used as a conductive diluent. This achieves favorable cathode properties based on uniform distribution of the components and an increase in the specific capacity of the cathode.
[0021] In one embodiment, the binder is selected from polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymers, and the like. In a specific embodiment, the binder is polyvinylidene fluoride. The binder not only provides good adhesion between the components in the electrode, but also binds the components onto the substrate. The binder must be compatible with the materials used in the cell and must be electrochemically stable in the operating voltage window of the cell.
[0022] In one embodiment, the solvent is selected from 1-methyl-2-pyrrolidone (NMP), dimethylacetamide (DMAC), dimethylformamide (DMF), etc. In a preferred embodiment, 1-methyl-2-pyrrolidone is used as the solvent.
[0023] The above method includes a step of drying the materials before mixing in a planetary mixer. The moisture content of the cathode is an important factor that affects the efficiency, reversible capacity, and cycle life of a lithium-ion cell. The moisture content of the cathode is a key factor that affects the efficiency, reversible capacity, and cycle life of a lithium-ion cell. x Co y Al z This is extremely important for materials that are moisture sensitive, such as O2, so the materials used in preparing the cathode slurry are dried before mixing to remove any moisture.
[0024] Powder materials, except PVDF, are dried at 150-230°C for 20-36 hours under a vacuum of 600-700mmHg. PVDF is dried at 50-80°C for 2-7 hours under a vacuum of 600-700mmHg.
[0025] The preparation of the cathode slurry is carried out in a planetary mixer by mixing the active material, conductive diluent, and binder. The cathode materials are fed into the planetary mixer through an inlet. The planetary mixer includes a planetary blade and a high speed disperser. Mixing the materials with the planetary mixer ensures uniform mixing of the materials and inhibits grinding of the active material, helping to form a cathode with superior performance characteristics.
[0026] In one embodiment, the planetary blade speed is between 40 and 160 rpm.
[0027] In one embodiment, the disperser speed is in the range of 450-600 rpm.
[0028] The order of mixing the materials is very important to determine the electrochemical properties of the cathode. In this disclosure, the cathode slurry preparation process is carried out in a planetary mixer with a high-speed disperser. As the first step of cathode slurry preparation, the powdered materials are dry mixed at a lower speed, followed by adding the required amount of PVDF solution. Then, while continuing mixing, NMP is added at different intervals until the viscosity of the cathode slurry is reduced to the desired state.
[0029] The preparation of the slurry is carried out in a humidity-controlled environment with a relative humidity of 2 to 15%.
[0030] In a specific embodiment, the viscosity of the slurry is 2000-15000 cps at a speed of 100 rpm (measured on a Brookfield Viscometer RVDV-1 Prime, spindle S-06). The viscosity of the slurry plays an important role in determining the properties of the electrode. It determines the controllability of the loading level, the peel strength, and therefore the performance of the electrode during cycling.
[0031] In one embodiment, the amount of active material is 47 to 53% by weight based on the total weight of the cathode slurry.
[0032] In one embodiment, the amount of the conductive diluent is 2-6% by weight based on the total weight of the cathode slurry.
[0033] In one embodiment, the amount of the binder is 2 to 7% by weight based on the total weight of the cathode slurry.
[0034] In one embodiment, the amount of the solvent is 38 to 44% by weight based on the total weight of the cathode slurry.
[0035] The composition of the electrode is very important in determining its electrochemical properties. The concentration of active material in the electrode determines the capacity delivered by the electrode. Conductive diluents are required to improve the conductivity of the electrode. Binders bond the components in the electrode to each other as well as to the substrate. Higher concentrations of active material result in higher specific capacity. However, optimal concentrations of conductive diluents and binders are required for good cycling and rate capabilities of the cell.
[0036] The manufacturing method further includes a step of applying the cathode slurry onto an aluminum foil substrate using a coating device. In one embodiment, the aluminum foil substrate has a thickness of 15 to 25 μm.
[0037] The cathode slurry is applied onto the aluminum foil substrate in a coating device. The cathode slurry prepared in the planetary mixer is transferred to the coating device. The coating device is driven by a cone-reverse system. The distance between the cone-reverse blade and the applicator is adjusted according to the desired loading level of the active material onto the aluminum foil substrate. In one embodiment, the set value of the gap is 150 to 300 μm.
[0038] The cathode slurry application process in this disclosure includes: a) feeding the slurry into a slurry dam to initiate application; b) moving the slurry onto the foil based on the gap between the cone reverse blade and the applicator; c) passing the foil coated with the slurry through two heating zones; and d) flipping the foil with the coating on one side to coat the other side.
[0039] The coating apparatus includes multiple heating zones. The foil coated with the slurry is passed through the heating zones. After coating is completed on one side of the foil, the foil is turned over to coat the other side. Coating speed and temperature are set based on the drying of the cathode after passing through two heating zones.
[0040] In one embodiment, the cathode is dried at 50-150° C. in a heating zone of a coater.
[0041] The dried cathode is finally wound into a roll. In one embodiment, the coating speed is 0.2 to 0.8 m / min.
[0042] The environment during the cathode coating process is important in determining the cathode's characteristics, especially for LiNi, which is sensitive to humidity. x Co y Al z This is important with materials like O2. If the proper humidity conditions are not maintained, the slurry will thicken during application and it will be difficult for the slurry to spread evenly over the substrate.
[0043] In one embodiment, the coating step is carried out at a relative humidity of 2 to 15%. The cathode after coating is dried for 3 to 10 hours at a temperature of 60 to 100° C. under a vacuum of 600 to 700 mmHg. In one embodiment, the thickness of the cathode after double-sided coating is 150 to 300 μm.
[0044] The next step of the manufacturing process involves calendering the cathode in a calendering machine. In one embodiment, the calendering of the cathode is carried out at a speed of 3-5 m / min. In one embodiment, the calendering of the cathode is carried out in the calendering machine at a temperature of 50-150° C.
[0045] The calendering device includes a preheating zone and two heated rolls for pressing the cathode. The rolled cathode manufactured according to the present disclosure is passed through the preheating zone and pressed to a thickness of 140 to 200 μm by the rollers of the calendering device at a speed of 3 to 5 m / min.
[0046] In one embodiment, the temperature of the preheating zone is 80-150° C. In one embodiment, the temperature of the calender rolls is 50-100° C.
[0047] The cathode thus prepared according to the present disclosure is mated with a graphite anode and assembled into a lithium ion cell. The lithium ion cells prepared according to the present disclosure exhibit excellent cell performance. A lithium ion battery having a cathode according to the present disclosure and a graphite anode exhibited a capacity retention of over 80% at 100% depth of discharge at C / 2-1C charge / discharge rates for 2000 cycles.
[0048] In one embodiment, the peel strength of the cathode is 200 to 500 g f / cm.
[0049] In one embodiment, the cathode has a specific capacity of 160-165 mAh / g at 4.1 V at a C / 10 rate.
[0050] The composite cathode for a lithium-ion cell according to the present disclosure comprises: (i) 70 to 93% LiNi x Co y Al z O2 (x=0.8, y=0.15, and z=0.05), (ii) 2-15% acetylene black, (iii) 2-15% graphite, and (iv) 2-15% polyvinylidene fluoride. In some embodiments, the active material in the composite cathode can be lithium cobalt oxide, lithium nickel oxide, lithium nickel cobalt manganese oxide, lithium iron phosphate, or the like.
[0051] The following examples are provided to better illustrate the claimed invention and should not be construed as limiting the scope of the invention in any way. All specific materials and methods described below are within the scope of the invention. These specific compositions, materials, and methods are not intended to limit the invention, but are merely intended to illustrate specific embodiments within the scope of the invention. Those skilled in the art can make modifications to equivalent materials and methods without departing from the scope of the invention without exerting inventive ability. It is the inventors' intention that such modifications are also included within the scope of the invention. EXAMPLES
[0052] The preparation of a composite cathode for a lithium ion cell with excellent cell performance is described in the following examples.
[0053] [Example 1] LiNi x Co y Al z The electrode manufacturing method for the O2-based cathode is shown below.
[0054] The cathode contains LiNi as the active material. x Co y Al z The electrode composition contains LiNiO2, a mixture of acetylene black and graphite as a conductive diluent, and polyvinylidene fluoride (PVDF) as a binder. xCo y Al z O2: 85-90%, acetylene black: 3-6%, graphite: 4-7%, PVDF: 3-8%. 1-Methyl-2-pyrrolidone (NMP) is used as a solvent in the preparation of electrode slurry. The active material, the conductive diluent, and the PVDF are dried under vacuum before mixing. The electrode fabrication includes slurry preparation, electrode coating, and calendaring.
[0055] The slurry is prepared in a planetary mixer equipped with a high-speed disperser. x Co y Al z Dry mix O2 and conductive diluent with planetary mixer at planetary blade speed of 50-80 rpm and disperser speed of 450-500 rpm, then add polyvinylidene fluoride solution while continuing mixing at planetary blade speed of 50-150 rpm, and further add NMP at different time intervals from polyvinylidene fluoride solution to prepare slurry. The volume of NMP is adjusted so that the solid content of the slurry is 60-62%.
[0056] A coating device driven by the Kondo-reverse method is used for electrode coating. Aluminum foil with a thickness of 15 μm is used for the coating. The gap between the Kondo-reverse blade and the applicator is adjusted to 180-230 μm. The slurry is filled into a slurry dam and applied. The application is performed at a speed of 0.4-0.7 m / min. The temperature of the heating zone is kept at 70-130°C. The electrode after drying is wound up in a roll from the device. The electrode is then dried under vacuum at 60-100°C for 5-7 hours. The thickness of the electrode after double-sided coating is 180-220 μm.
[0057] The calendering of the electrode is carried out in a calendering device having a preheating zone and a calender roll. The preheating temperature is 100 to 120°C, and the calender roll temperature is 50 to 80°C. To make the final electrode thickness 140 to 170 μm, the rolled electrode is passed through the preheating roll and the calender roll at a speed of 4 to 5 m / min.
[0058] [Example 2] LiNi x Co y Mn z The electrode fabrication method for the O2-based cathode is described below.
[0059] The cathode contains LiNi as the active material. x Co y Mn z O2, acetylene black and graphite as conductive diluents, and polyvinylidene fluoride (PVDF) as a binder. The electrode composition is LiNi x Co y Mn z O2: 86-93%, acetylene black: 2-5%, graphite: 3-7%, PVDF: 2-6%. NMP is used as the solvent. The active material, the conductive diluent, and the PVDF are dried under vacuum before mixing. The electrode fabrication includes slurry preparation, electrode coating, and calendaring.
[0060] The slurry is prepared using a planetary mixer with a high-speed disperser. A 5-10% (by mass) PVDF solution is prepared in NMP. LiNi x Co y Mn z O2 and conductive diluent are dry mixed in a planetary mixer with planetary blade speed of 50-100 rpm and disperser speed of 450-550 rpm. Polyvinylidene fluoride solution is then added, followed by NMP at different time intervals while continuing mixing with planetary blade speed of 60-150 rpm. The volume of NMP is adjusted so that the solids concentration of the slurry is 58-62%.
[0061] A coating device for the Kondo-reverse method is used for electrode coating. A 20 μm thick aluminum foil is used for the coating. The gap between the Kondo-reverse blade and the applicator is adjusted to 230-250 μm. The slurry is filled into a slurry dam and applied. The coating is performed at a speed of 0.3-0.7 m / min. The temperature of the heating zone is kept at 80-130°C. The dried electrode is wound up from the device into a roll. The electrode is then dried under vacuum at 80-100°C for 5-7 hours. The thickness of the electrode after double-sided coating is 200-240 μm.
[0062] The calendering of the electrode is carried out in a calendering device equipped with a preheating zone and a calender roll. The preheating temperature is 100 to 120° C., and the calender roll temperature is 60 to 90° C. In order to make the final electrode thickness 160 to 190 μm, the rolled electrode is passed through the preheating roll and the calender roll at a speed of 4 to 5 m / min.
[0063] [Example 3] The method for manufacturing the LiCoO2-based cathode electrode is shown below.
[0064] The cathode contains LiCoO2 as an active material, a mixture of acetylene black and graphite as a conductive diluent, and polyvinylidene fluoride (PVDF) as a binder. The electrode composition is LiCoO2: 87-93%, acetylene black: 2-5%, graphite: 2-4%, and PVDF: 3-5%. 1-methyl-2-pyrrolidone (NMP) is used as a solvent for preparing the electrode slurry. The active material, conductive diluent, and PVDF are dried under vacuum. The electrode fabrication includes slurry preparation, electrode coating, and calendaring.
[0065] The slurry is prepared in a planetary mixer with a high-speed disperser. LiCoO2 and conductive diluent are dry mixed in the mixer at a planetary blade speed of 40-90 rpm and a disperser speed of 450-550 rpm, then the polyvinylidene fluoride solution is added while continuing mixing at a planetary blade speed of 50-150 rpm, and NMP is added at different time intervals from the polyvinylidene fluoride to prepare the slurry. The volume of NMP is adjusted so that the solid content of the slurry is 57-60%.
[0066] A coating device driven by the Kondo-reverse method is used for electrode coating. Aluminum foil with a thickness of 15 to 20 μm is used for the coating. The gap between the Kondo-reverse blade and the applicator is adjusted to 230 to 250 μm. The slurry is filled into a slurry dam and applied. The application is performed at a speed of 0.4 to 0.6 m / min. The temperature of the heating zone is maintained at 75 to 135°C. The electrode after drying is wound up in a roll from the device. The electrode is then dried under vacuum at 70 to 100°C for 5 to 7 hours. The thickness of the electrode after coating is 260 to 300 μm.
[0067] The electrode is calendered in a calendering device having a preheating zone and calender rolls. The preheating temperature is 100-120°C, and the calender roll temperature is 50-80°C. To make the final electrode thickness 170-200μm, the rolled electrode is passed through the preheating rolls and calender rolls at a speed of 4-5m / min.
[0068] [Table 1]
[0069] [Table 2]
Claims
1. (i) mixing an active material, a conductive diluent, a solvent, and a binder in a planetary mixer to prepare a cathode slurry; (ii) coating the cathode slurry onto an aluminum foil substrate in a coating zone at a speed of 0.2-0.8 m / min; and (iii) calendering the cathode in a calendering apparatus at a temperature of 50-150° C.; Including, the active material is selected from the group consisting of LiCoO2, LiNi x Co y Al z O2, and LiNi x Co y Mn z O2; the conductive diluent is selected from the group consisting of acetylene book, graphite, carbon nanotubes, and mixtures thereof; the solvent is selected from the group consisting of 1-methyl-2-pyrrolidone, dimethylacetamide, and dimethylformamide; the binder is selected from the group consisting of polyvinylidene fluoride and vinylidene fluoride-hexafluoropropylene copolymer; the amount of the active material is 47 to 53% by weight based on the total weight of the cathode slurry; the amount of the conductive diluent is 2 to 6 wt. %, based on the total weight of the cathode slurry; the amount of the solvent is 38 to 44% by weight based on the total weight of the cathode slurry; The amount of the binder is 2 to 7% by weight based on the total weight of the cathode slurry; A method for making a composite cathode for a lithium-ion cell.
2. further comprising the step of drying the materials prior to mixing in the planetary mixer. A method for producing the composite cathode for a lithium ion cell according to claim 1.
3. The conductive diluent is selected from acetylene black and graphite. A method for producing the composite cathode for a lithium ion cell according to claim 1.
4. The conductive diluent is a combination of acetylene black and graphite; A method for producing the composite cathode for a lithium ion cell according to claim 1.
5. dry-mixing the active material and the conductive diluent, and adding the binder solution and the solvent at different times while continuing the mixing; A method for producing the composite cathode for a lithium ion cell according to claim 1.
6. The thickness of the aluminum foil substrate is 15 to 25 μm. A method for producing the composite cathode for a lithium ion cell according to claim 1.
7. The thickness of the cathode after coating is 150 to 300 μm; A method for producing the composite cathode for a lithium ion cell according to claim 1.
8. The final thickness of the cathode after the calendaring is 140 to 200 μm; A method for producing the composite cathode for a lithium ion cell according to claim 1.
9. The relative humidity in the room where the electrode coating is performed is 2-15%; A method for producing the composite cathode for a lithium ion cell according to claim 1.
10. After the coating, the method further comprises drying the cathode at a temperature of 50 to 150° C. in a drying zone of a coating apparatus. A method for producing the composite cathode for a lithium ion cell according to claim 1.
11. The calendering of the cathode is carried out at a speed of 3 to 5 m / min and a temperature of 50 to 150° C.; A method for producing the composite cathode for a lithium ion cell according to claim 1.
Citation Information
Patent Citations
flexible cathode
JP2006505914A
battery
JP2009545859A
Electrode for nonaqueous battery and method for manufacturing the same
JP2014203572A
Manufacturing method of cathode for nonaqueous secondary battery, and cathode for nonaqueous secondary battery
JP2015201283A
Method of evaluating stability of positive electrode material slurry for lithium ion secondary battery