Method for aligning laminated components and method for manufacturing laminated ceramic electronic components

The method aligns laminated ceramic components using a non-magnetic support and magnetic field to address alignment challenges, facilitating efficient and rapid processing of small components.

JP7566127B2Active Publication Date: 2024-10-11KYOCERA CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2023503857
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-03-02
Filing Date
2022-03-01
Publication Date
2024-10-11
Estimated Expiration
2042-03-01

AI Technical Summary

Technical Problem

Existing methods for aligning small laminated ceramic components, such as multilayer ceramic capacitors, face challenges in accurately orienting and processing surfaces as components become smaller, leading to increased operational complexity.

Method used

A method involving a non-magnetic support member with a flat surface and application of a magnetic field intersecting with the support surface to align laminated components, followed by processing and firing, utilizing a non-magnetic material and a magnetic field to orient ferromagnetic layers.

Benefits of technology

Enables efficient and rapid alignment of laminated components, allowing for simplified and quicker processing of multiple parts under uniform conditions, reducing operational complexity and enhancing manufacturing efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007566127000001
    Figure 0007566127000001
  • Figure 0007566127000002
    Figure 0007566127000002
  • Figure 0007566127000003
    Figure 0007566127000003
Patent Text Reader

Abstract

The direction of a plurality of elemental components is aligned by applying a magnetic field in which magnetic flux lines intersect a support surface to the plurality of elemental components, wherein the plurality of elemental components are arranged in a gap between: the support member composed of a non-magnetic material and having a flat support surface parallel to a horizontal direction; and an upper member composed of a non-magnetic material, and being provided at a position above the support member and separated from the support surface by a predetermined distance.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a method for aligning laminated components and a method for manufacturing a laminated ceramic electronic component. [Background technology]

[0002] An example of the prior art is described in Patent Document 1. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2003-7574 A Summary of the Invention

[0004] The method for aligning laminated components disclosed herein includes applying a magnetic field in which magnetic flux lines cross the support surface to a rectangular parallelepiped laminated component in which ceramic green sheets and ferromagnetic layers are alternately laminated, the laminated components being arranged in a gap between a support member including a non-magnetic material and having a flat support surface parallel to the horizontal direction, and an upper member including a non-magnetic material and located above the support member at a predetermined distance from the support surface, thereby aligning the orientation of the laminated components. The application of the magnetic field is stopped in a state where the plurality of laminated components having the same orientation are sandwiched between the support member and the upper member. .

[0005] The method of manufacturing a laminated ceramic component according to the present disclosure includes the above-described method of aligning laminated components, and after processing the surfaces of the laminated components whose orientation is aligned, the laminated components are fired. [Brief description of the drawings]

[0006] The objects, features and advantages of the present disclosure will become more apparent from the following detailed description and drawings.

[0007] [Figure 1] FIG. 1 is a perspective view of an example of a multilayer ceramic capacitor. [Diagram 2] FIG. 2 is a diagram showing an element part before firing. [Diagram 3]FIG. 2 is a perspective view showing a precursor of an element part. [Figure 4] FIG. 2 is an enlarged cross-sectional view showing a schematic diagram of an element precursor. [Figure 5A] 1 shows a state in which an element part is placed on a support member. [Figure 5B] 1 shows a state in which an element part is placed on a support member. [Figure 5C] 3A to 3C are schematic diagrams illustrating an alignment method according to the present embodiment. [Figure 5D] 3A to 3C are schematic diagrams illustrating an alignment method according to the present embodiment. [Figure 6] 13A to 13C are schematic diagrams illustrating an alignment method according to another embodiment. [Figure 7] FIG. 13 is a schematic diagram showing a process of forming a part assembly. [Figure 8] FIG. 11 is a schematic diagram showing how an element part is fixed. [Figure 9] FIG. 4 is a schematic diagram showing a method for producing a laminate component. [Figure 10] FIG. 4 is a schematic diagram showing a method for producing a laminate component. [Figure 11] FIG. 4 is a schematic diagram showing a method for producing a laminate component. [Figure 12] FIG. 4 is a schematic diagram showing a method for producing a laminate component. [Figure 13A] FIG. 13 is a schematic diagram showing a method for aligning stacked components. [Figure 13B] FIG. 13 is a schematic diagram showing a method for aligning stacked components. [Figure 13C] FIG. 13 is a schematic diagram showing a method for aligning stacked components. [Figure 13D] FIG. 13 is a schematic diagram showing a method for aligning stacked components. [Figure 14] FIG. 4 is a schematic diagram showing a method for producing a laminate component. [Figure 15] FIG. 4 is a schematic diagram showing a method for producing a laminate component. [Figure 16] FIG. 4 is a schematic diagram showing a method for producing a laminate component. [Figure 17] 10A to 10C are schematic diagrams showing another method for producing a laminate component. [Figure 18] 10A to 10C are schematic diagrams showing another method for producing a laminate component. [Figure 19] 10A to 10C are schematic diagrams showing another method for producing a laminate component. [Figure 20A] FIG. 13 is a schematic diagram showing another method of aligning stacked components. [Figure 20B] FIG. 13 is a schematic diagram showing another method of aligning stacked components. [Figure 21] 10A to 10C are schematic diagrams showing another method for producing a laminate component. [Figure 22] 10A to 10C are schematic diagrams showing another method for producing a laminate component. [Figure 23] FIG. 11 is a perspective view showing another example of the upper member. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] In recent years, as electronic devices become smaller and more functional, there is a demand for smaller electronic components to be installed in them. One example of such an electronic component is the multilayer ceramic capacitor. Multilayer ceramic capacitors with a side length of 1 mm or less are becoming mainstream.

[0009] The manufacturing process of multilayer ceramic capacitors includes a processing step in which the end faces or sides of element components are polished or a protective layer is applied, and prior to this processing step, a step is required in which multiple element components are rotated to align the processed surfaces. For example, roughly rectangular chip components, in which the lead electrodes of the internal electrodes are exposed at the widthwise ends, are placed in pockets of a pallet shaped like a recess, and a magnet is moved along the bottom surface outside the pallet to attract and roll the chip components inside the pocket, aligning the orientation of the chip components (see Patent Document 1).

[0010] The smaller the element components are, the more difficult it becomes to align the processed surfaces. For example, the alignment method described in Patent Document 1 requires an operation to place the chip components in pockets, and the smaller the element components are, the more complicated this operation becomes.

[0011] Hereinafter, an embodiment of the method for aligning a laminated component and the method for manufacturing a laminated ceramic component according to the present disclosure will be described with reference to the drawings. Note that, although a laminated ceramic capacitor will be described below as an example of a laminated ceramic electronic component, the laminated ceramic component to which the present disclosure is directed is not limited to a laminated ceramic capacitor, and can also be applied to various other laminated ceramic components such as a laminated piezoelectric element, a laminated thermistor element, a laminated chip coil, and a ceramic multilayer substrate.

[0012] First, a multilayer ceramic capacitor, which is an example of a multilayer ceramic electronic component, will be described. FIG. 1 is a perspective view of an example of a multilayer ceramic capacitor. FIG. 2 is a perspective view that typically shows an element component of the multilayer ceramic capacitor of FIG. 1. FIG. 2 is a view showing the element component before firing. Note that although the element component after firing shrinks due to firing, it has the same structure as the element component before firing, so FIG. 2 can also be said to be a view showing the element component after firing. FIG. 3 is a perspective view showing a precursor of the element component of FIG. 2. Hereinafter, the precursor of the element component may be referred to as an element precursor.

[0013] The multilayer ceramic capacitor 1 has an element component 2 and an external electrode 3. As shown in FIG. 2, the element component 2 has a substantially rectangular parallelepiped shape. The element component 2 is made of dielectric ceramics 4 and has a plurality of internal electrode layers 5 connected to the external electrode 3. The external electrodes 3 are disposed on a pair of end faces of the element component 2 and extend around to other adjacent faces. The multiple internal electrode layers 5 extend inward from a pair of end faces of the element component 2 and are alternately stacked without contacting each other. The internal electrode layers 5 are, for example, ferromagnetic layers containing a ferromagnetic metal material.

[0014] The external electrode 3 is configured to have an undercoat layer that connects to the element component 2, and a plated outer layer that facilitates solder mounting of external wiring to the external electrode 3. The undercoat layer may be applied and baked onto the element component 2 after sintering. The undercoat layer may be disposed on the element component 2 before sintering, and may be fired simultaneously with the element component 2. The undercoat layer and plated outer layer may be multiple layers according to the required function. The external electrode 3 may not have a plated outer layer, and may be configured to have an undercoat layer and a conductive resin layer.

[0015] As shown in Figures 2 and 3, the element part 2 has an element precursor 13 and a protective layer 6. As shown in Figure 3, the element precursor 13 has a substantially rectangular parallelepiped shape. The element precursor 13 has opposing faces 7, opposing end faces 8, and opposing side faces 9. In the element part 2, if the long side dimension of the face 7 is a, the width dimension is b, and the dimension in the stacking direction which is the thickness is c, then, for example, there is a relationship a>b≧c.

[0016] The internal electrode layer 5 is exposed on the end face 8 and the side face 9 of the element precursor 13. The protective layer 6 is disposed on the side face 9 of the element precursor 13. The protective layer 6 suppresses electrical short-circuiting between the internal electrode layer 5 exposed on the first end face 8A and the internal electrode layer 5 exposed on the second end face 8B. The protective layer 6 also physically protects the part of the internal electrode layer 5 exposed on the side face 9 of the element precursor 13. The protective layer 6 is attached last in the production of the element part 2. The protective layer 6 protects the internal electrode layer 5 exposed on the side face 9 of the element precursor 13. The protective layer 6 may be made of a ceramic material. In this case, the protective layer 6 can be made to have insulating properties and high mechanical strength. The ceramic material to become the protective layer 6 is usually disposed on the element precursor 13 before firing. In FIG. 2, the boundary between element precursor 13 and protective layer 6 is indicated by a two-dot chain line, but in reality the boundary is not clearly visible.

[0017] In the above, in addition to the element part 2, its precursor, the element precursor 13, has also been described; however, in this disclosure, the “laminate component” includes both the element part 2 and the element precursor 13.

[0018] 4 is an enlarged cross-sectional view showing a schematic diagram of the element precursor. Ceramic green sheets 10 and internal electrode layers 5 are alternately laminated. Before the ceramic powder and metal powder are sintered by firing, the ceramic green sheets 10 are in a state in which dielectric ceramic particles 35 are dispersed in an organic binder, and the internal electrode layers 5 are in a state in which nickel particles 36 are dispersed in an organic binder.

[0019] In the method for aligning a laminated component according to the present embodiment described below, it is necessary to increase the magnetic susceptibility of the internal electrode layers 5 in order to apply a magnetic field to the internal electrode layers 5. The nickel particles 36 of the internal electrode layers 5 are surrounded by an organic binder, and therefore are mostly not in contact with each other. In order to increase the magnetic susceptibility of the internal electrode layers 5, the content of the organic binder may be set to 1.5 times or less by volume of the nickel particles, which are ferromagnetic metal materials.

[0020] 5A and 5B show the state of element parts 2 placed on a support member 16. As shown in Fig. 5A, even when element parts 2 are placed on support member 16 without intentionally aligning the orientation of element parts 2, most element parts 2 are oriented such that surface 7, which is the widest surface, is parallel to support surface 16a of support member 16.

[0021] As shown in FIG. 5B, when a magnetic field in which the magnetic flux lines 18 intersect with the support surface 16a is applied to the element component 2 in the state of FIG. 5A, the element component 2 rotates so that the extension direction (plane direction) of the internal electrode layer 5 of the element component 2 becomes parallel to the magnetic flux lines 18. In other words, the element component 2 rotates so that the thickness direction of the internal electrode layer 5 is perpendicular to the magnetic flux lines 18. As a result, the element component 2 becomes either a state in which the side surface 9 is parallel to the support surface 16a (first state) or a state in which the end surface 8 is parallel to the support surface 16a (second state). Here, the element component 2 is often subjected to processing such as forming a protective layer 6 on the side surface 9, and it is necessary to align the orientation of all the element components 2 so that they are in the first state. However, as described above, the element components 2 are in two states, and it is difficult to align the orientation of the element components 2. Furthermore, element components 2 in the first state may overlap each other in the vertical direction.

[0022] 5C and 5D are schematic diagrams illustrating the alignment method of this embodiment. As shown in Fig. 5C, in this embodiment, a magnetic field in which magnetic flux lines 18 intersect with support surface 16a is applied to a plurality of element components 2 arranged in a gap between support member 16 made of a non-magnetic material and having flat support surface 16a parallel to the horizontal direction, and upper member 19 made of a non-magnetic material and provided above support member 16 at a predetermined distance from support surface 16a, to align the orientations of element components 2.

[0023] Furthermore, as shown in FIG. 5D, in this embodiment, a magnetic field in which magnetic flux lines 18 intersect with the support surface 16a is applied to multiple element body precursors 13 arranged in the gap between the support member 16 and the upper member 19, thereby aligning the orientation of the element body precursors 13.

[0024] The material constituting the support member 16 and the upper member 19 may be any non-magnetic material, such as a resin material, hard paper, a ceramic material, or a non-magnetic metal material such as aluminum. The support member 16 and the upper member 19 may be made of any non-magnetic material having a thickness sufficient to provide rigidity without bending.

[0025] The distance between the support member 16 and the upper member 19 is a distance that allows the base component 2 or the base precursor 13 to rotate with the longitudinal direction, that is, the direction orthogonal to the end face 8, as the axial direction, and is a distance that inhibits the base components 2 (base precursors 13) in the first state from overlapping in the vertical direction and the base component 2 (base precursor 13) from entering the second state.

[0026] The longitudinal and lateral dimensions of the end face 8 of the base component 2 are b and c, and the diagonal dimension of the end face 8 is b1. When aligning the orientation of the base component 2, if the distance between the support member 16 and the upper member 19 is s, then the distance s may be set such that b1 < s < (the smaller of 2×b or a). By setting b1 < s, rotation of the base component 2 is allowed. By setting s < (the smaller of 2×b or a), overlap of the base components 2 in the first state and entering the second state can be inhibited.

[0027] If the width of the internal electrode layer 5 is b2, then the longitudinal and lateral dimensions of the end face 8 of the base precursor 13 are b2 and c, and the diagonal dimension of the end face 8 is b3. When aligning the orientation of the base precursor 13, if the distance between the support member 16 and the upper member 19 is s and the diagonal dimension of the end face 8 is b3, then the distance s may be set such that b3 < s < (the smaller of 2×b2 or a). By setting b3 < s, rotation of the base precursor 13 is allowed. By setting s < (the smaller of 2×b2 or a), overlap of the base precursors 13 in the first state and entering the second state can be inhibited. Note that for the base component 2, by setting 0.75b < b2 < b for the width b2 of the internal electrode layer 5 , even if it has the protective layer 6, a sufficient rotational moment can be obtained by the action of the magnetic field.

[0028] 6 is a schematic diagram for explaining an alignment method according to another embodiment. As shown in the figure, the element component 2 placed in the gap between the support member 16 and the upper member 19 is moved relatively along the horizontal direction in a magnetic field that has been generated in advance. The word "relative" here means that the position of the magnetic field may be fixed and the element component 2 placed in the gap may be moved together with the support member 16 and the upper member 19, or the element component 2 placed in the gap may be moved by fixing the positions of the support member 16 and the upper member 19 and moving the magnetic field that has been generated in advance. When a magnetic field acts on the element component 2 on the support member 16, the element component 2 spontaneously rotates so that the extension direction of the internal electrode layer 5 and the direction of the magnetic flux lines 18 become parallel, and the orientation of the element component 2 can be aligned.

[0029] When the element parts 2 placed in the gap are moved horizontally into the magnetic field, they start to rotate in the order beginning with the element parts 2 that are acted upon by the magnetic field. The rotation direction of the element parts 2 can also be made constant depending on the direction of the magnetic flux lines 18. For example, when the element parts 2 are moved from the left side into a magnetic field in which the magnetic flux lines 18 are either upward or downward, the element parts 2 placed at the right end of the gap will all rotate clockwise until they are aligned in the same direction. In this way, the rotation direction of the element parts 2 can be controlled.

[0030] Furthermore, vibration may be applied to the element parts 2 placed in the gap between the support member 16 and the upper member 19. In this embodiment, for example, vertical vibration as indicated by arrow 22 is applied. Also, in this embodiment, vibration is applied to the support member 16. If the horizontal distance between the element parts 2 in the gap between the support member 16 and the upper member 19 is narrow, rotation may be hindered by adjacent element parts 2 even if a magnetic field is applied. By applying vibration, the distance between the element parts 2 can be widened, making it easier for the element parts 2 to rotate. Note that the upper member 19 may also be vibrated in the same manner as the support member 16. Furthermore, the vibration direction is not limited to the vertical direction, but may be the horizontal direction, or these may be combined.

[0031] The magnetic field applied to the element component 2 may be generated, for example, by a magnet (first magnet) 17 located below the support member 16 and a magnet (second magnet) 17 located above the upper member 19. The opposing sides of the two magnets 17 may have opposite polarities such that magnetic flux lines 18 of the generated magnetic field intersect with the support surface 16a. The magnet 17 may be a permanent magnet or an electromagnet. The size of the magnet 17 may be such that it has an area larger than the area of ​​the support surface 16a of the support member 16 on which the element component 2 is placed.

[0032] Furthermore, the magnetic field may be applied to element parts 2 continuously, or an intermittent magnetic field may be used in which periods when the magnetic field is applied and periods when the magnetic field is not applied are repeated. By using an intermittent magnetic field, the distance between element parts 2 can be increased, as in the case of applying vibration described above. When magnet 17 is a permanent magnet, the period during which magnet 17 is brought close to support member 16 and upper member 19 can be set as the application period, and the period during which magnet 17 is moved away from support member 16 and upper member 19 can be set as the non-application period. When magnet 17 is an electromagnet, the period during which current is supplied can be set as the application period, and the period during which current supply is stopped can be set as the non-application period.

[0033] As for the magnet 17, for example, only the magnet (first magnet) 17 located below the support member 16 may be used, or only the magnet (second magnet) 17 located above the upper member 19 may be used, but by using two magnets 17, one above the other, a uniform magnetic field can be generated over a wide range. This makes it possible to rotate the element part 2 and align its orientation regardless of the position on the support surface 16a.

[0034] Furthermore, the magnetic field may be one in which the direction of the magnetic flux lines 18 (the direction of the magnetic field) is repeatedly reversed. The internal electrode layers 5 of the element component 2 are ferromagnetic, and when a magnetic field is applied to them, the internal electrode layers 5 may be magnetized and may take on residual magnetism. This residual magnetism may make it difficult to handle the element component 2 in a later process. By repeatedly reversing the direction of the magnetic flux lines 18, the internal electrode layers 5 can be repeatedly magnetized and demagnetized, thereby reducing the residual magnetism of the internal electrode layers 5.

[0035] FIG. 7 is a schematic diagram showing how a parts assembly is formed. As described above, after the element parts 2 are aligned in the gap between the support member 16 and the upper member 19, a magnetic field is applied and multiple aligned element parts 2 are assembled to form a parts assembly. For example, a jig 25 is moved horizontally from the outside left and right of the gap toward the center. The element parts 2 sandwiched between the jig 25 from both sides gather in the center to form an assembly. The part assembly can be handled as a whole in subsequent processing steps, allowing multiple element parts 2 to be processed collectively. This allows for faster processing than processing the element parts 2 individually. Furthermore, multiple element parts 2 can be processed in a single process. The body part 2 can be processed under the same conditions.

[0036] FIG. 8 is a schematic diagram showing how element parts are fixed. After the element parts 2 are aligned in the gap between the support member 16 and the upper member 19 as described above, the distance between the support member 16 and the upper member 19 is reduced while the magnetic field is applied, and the application of the magnetic field is stopped while the gap between the support member 16 and the upper member 19 is maintained. If the application of the magnetic field is stopped while the gap between the support member 16 and the upper member 19 is maintained, the element parts 2 may rotate due to disturbance in the magnetic field when the magnetic field is stopped or due to subsequent handling, causing the element parts 2 to lose their alignment. By clamping the element parts 2 between the support member 16 and the upper member 19, By fixing the body part 2 and then terminating the application of the magnetic field, it is possible to prevent the body part 2 from rotating when stopped.

[0037] When the element part 2 is sandwiched between the support member 16 and the upper member 19, the element part 2 comes into contact with the support member 16 and the upper member 19. At this time, a configuration may be used in which a portion of the upper member 19 facing the support surface 16a contains an elastic material so that the element part 2 is not damaged even if an impact is applied to the element part 2. For example, an elastic sheet 20 may be attached to the upper member 19. Similarly, an elastic sheet 20 may be attached to the support member 16. The material of the elastic sheet 20 is preferably one that has excellent durability and abrasion resistance, and for example, silicone rubber or urethane rubber may be used.

[0038] The following describes a method for manufacturing the element component 2 and the multilayer ceramic capacitor 1 shown in Fig. 2. This manufacturing method includes the above-mentioned alignment method.

[0039] First, a ceramic powder mixture of BaTiO3, a ceramic dielectric material, and additives is wet-milled and mixed in a bead mill. A polyvinyl butyral binder, a plasticizer, and an organic solvent are added to the milled and mixed slurry to produce a ceramic slurry.

[0040] Next, a ceramic green sheet 10 is formed on the carrier film using a die coater. The thickness of the ceramic green sheet 10 may be, for example, about 1 to 10 μm. The thinner the ceramic green sheet 10, the higher the capacitance of the multilayer ceramic capacitor can be. The forming of the ceramic green sheet 10 is not limited to the die coater, and may be performed using, for example, a doctor blade coater or a gravure coater.

[0041] Next, as shown in FIG. 9, a conductive paste containing nickel (Ni), which is a ferromagnetic metal material that will become the internal electrode layer 5, is printed in a predetermined pattern on the ceramic green sheet 10 prepared above by using a screen printing method. The printing of the conductive paste is not limited to the screen printing method, and may be performed by using, for example, a gravure printing method or the like. The conductive paste may contain, for example, metals such as Pd, Cu, Ag, etc., or alloys thereof, other than Ni. In the figure, an example is shown in which the pattern of the internal electrode layer 5 is a strip-shaped pattern of multiple rows, but the pattern of the internal electrode layer 5 may be, for example, an individual electrode pattern or the like.

[0042] After printing, the conductive paste is dried. Since the solvent is mainly evaporated by drying, the internal electrode layer 5 after drying is in a state where nickel particles are dispersed in the organic binder. As long as the characteristics as a capacitor are secured, the thinner the thickness of the internal electrode layer 5, the more the internal defects caused by internal stress can be prevented. In the case of a capacitor with a high number of layers, the thickness of the internal electrode layer 5 may be, for example, 2.0 μm or less.

[0043] Next, as shown in Fig. 10, a predetermined number of ceramic green sheets 10 with internal electrode layers 5 printed thereon are laminated on top of the predetermined number of laminated ceramic green sheets 10, and a predetermined number of ceramic green sheets 10 are further laminated. A predetermined number of ceramic green sheets 10 with internal electrode layers 5 printed thereon are laminated while shifting the patterns of the internal electrode layers 5. Although omitted in Fig. 10, the ceramic green sheets 10 are laminated on a support sheet. The support sheet may be an adhesive release sheet that can be adhered and released, such as a weak adhesive sheet or a foam release sheet.

[0044] Next, the laminate formed by stacking a plurality of ceramic green sheets 10 is pressed in the stacking direction to obtain an integrated base laminate 11 as shown in FIG. 11. The laminate can be pressed using, for example, a hydrostatic press. Inside the base laminate 11, the internal electrode layers 5 are embedded in layers with the ceramic green sheets 10 sandwiched therebetween. When the base laminate 11 is cut lengthwise and crosswise, it becomes the element precursor 13 shown in FIG. 3. The faces, end faces, and side faces of the base laminate 11 correspond to the faces 7, end faces 8, and side faces 9 of the element precursor 13, respectively, and therefore will be denoted by the same reference numerals below. Although omitted in FIG. 6, a support sheet used when stacking the ceramic green sheets 10 is located below the base laminate 11.

[0045] Next, as shown in FIG. 12, the base laminate 11 is cut into a predetermined size using a press-cutting device to obtain a plurality of first rod-shaped bodies 12. The cut surface of the first rod-shaped body 12 corresponds to the side surface 9 of the element precursor 13, and the internal electrode layer 5 is exposed on the cut surface of the first rod-shaped body 12. The method of cutting the base laminate 11 is not limited to the method using the press-cutting device, and for example, a dicing saw device may be used. In the longitudinal direction of the first rod-shaped body 12, each internal electrode layer 5 has discontinuous parts that are divided at multiple points. In such a case, in a magnetic field, the apparent magnetic susceptibility of the internal electrode layer 5 in the longitudinal direction is not high, so that the first rod-shaped body 12 easily rotates around the longitudinal axis. The discontinuous parts of the internal electrode layer 5 are, for example, 40 μm or more.

[0046] A method of aligning the first rod-shaped bodies 12 as stacked components will be described. First, as shown in FIG. 13A, a plurality of first rod-shaped bodies 12 obtained by cutting are arranged on the support surface 16a of the support member 16, and then the upper member 19 is installed. The first rod-shaped bodies 12 are arranged so that their longitudinal directions are parallel to each other. The distance s between the support member 16 and the upper member 19 is, for example, 1.1 times the diagonal dimension b3 of the end face 8 of the first rod-shaped body 12. Next, as shown in FIG. 13B, the support member 16 and the upper member 19 are moved to approach the magnet 17 so that the magnet 17, which has been previously provided, is below the support member 16. An electromagnet is used as the magnet 17. When a permanent magnet with N and S poles on opposing planes is used, the magnetic force is adjusted by the distance from the magnet surface. The first rod-shaped body 12 to which the magnetic field from the magnet 17 is applied rotates around an axis extending in the longitudinal direction through the center of the end face 8. When a magnetic field acts on all of the first rod-shaped bodies 12, all of the first rod-shaped bodies 12 are aligned so that the extension direction of the internal electrode layers 5 is parallel to the magnetic flux lines 18. Thereafter, the first rod-shaped bodies 12 with the aligned orientation are clamped and fixed between the upper member 19 and the support member 16.

[0047] The magnetic field applied to the first rod-shaped body 12, which is a laminated component, can be controlled by the type of magnet used, the distance between the laminated component and the magnet, etc. For example, in the case of a laminated component having 400 internal electrode layers 5 with a thickness c in the lamination direction of 0.63 mm and a width b2 of the end face of 1.33 mm, respectively, the type of magnet and the distance from the magnet may be set so that the magnetic flux density is 50 Gauss or more.

[0048] The magnetic field acting on the first rod-shaped body 12 is stopped in a state where the first rod-shaped body 12 is sandwiched and fixed between the upper member 19 and the support member 16. For example, the current supply to the magnet 17, which is an electromagnet, may be stopped. Also, as shown in FIG. 13C, after the orientations of the first rod-shaped body 12 are aligned, the upper member 19 with the support sheet 21 may be brought into contact with the first rod-shaped body 12 aligned in the direction from above while the magnetic field is acting, by either attaching an adhesive support sheet 21 to the upper member 19 or by replacing the upper member 19 with another upper member 19 to which an adhesive support sheet 21 has been attached in advance. As shown in FIG. 13D, the magnetic field acting on the first rod-shaped body 12 may be stopped by moving the first rod-shaped body 12 away from the magnet 17 while the first rod-shaped body 12 is sandwiched between the upper member 19 and the support member 16. The first rod-shaped body 12 fixed to the support sheet 21 can be moved in a state where the orientations of the first rod-shaped body 12 are aligned.

[0049] As shown in FIG. 14, when the upper member 19 is turned upside down, the side surfaces 9 of the first rod-shaped bodies 12 face upward, and in a later process, the upwardly facing side surfaces 9 can be processed all at once.

[0050] FIG. 15 is a perspective view of the first rod-shaped body that has been subjected to processing. The processing is, for example, a process for forming a protective layer 6. With the side surfaces 9 of the first rod-shaped bodies 12 aligned in the same direction, the ceramic slurry can be applied to the side surfaces 9 at once. After drying, the side surfaces 9 to which the ceramic slurry has been applied are fixed with another support sheet 21, and the original support sheet 21 is peeled off. The ceramic slurry is also applied to the side surfaces 9 newly exposed by peeling off the original support sheet 21. By applying the ceramic slurry to the side surfaces 9 in this way, the protective layer 6 can be formed. The ceramic slurry to be applied can be one having the same composition as the ceramic green sheets 10 that constitute the base laminate 11. After forming the protective layer 6, as shown in FIG. 16, the first rod-shaped bodies 12 are cut to obtain the element parts 2. The element parts 2 thus obtained are fired, and then the external electrodes 3 are formed, and the multilayer ceramic capacitor 1 can be manufactured. The firing temperature can be appropriately set according to the dielectric ceramic material and the metal material contained in the conductive paste that becomes the internal electrode layer 5. The firing temperature may be, for example, 1100 to 1250°C.

[0051] Another manufacturing method will be described. The procedure for producing the base laminate 11 is the same as the above-mentioned method, so the description will be omitted. As shown in FIG. 17, the base laminate 11 is cut to a predetermined size to obtain a plurality of second rod-shaped bodies 12A. The cutting direction is different by 90° from that of the first rod-shaped body 12 described above, and the cut surface of the second rod-shaped body 12A corresponds to the end surface 8 of the element precursor 13. As shown in FIG. 18, the thermoplastic resin 15 is embedded in the gaps between the second rod-shaped bodies 12A obtained by cutting, and the surface (face) is covered with the thermoplastic resin 15 to obtain a flat block 23. The flat block 23 is further cut to obtain a third rod-shaped body 24 as shown in FIG. 19. The cutting direction is different by 90° from that of the second rod-shaped body 12A, and is the same as the cutting direction of the first rod-shaped body 12. The cut surface of the third rod-shaped body 24 corresponds to the side surface 9 of the element precursor 13. The third rod-shaped body 24 has a structure in which the element precursors 13 are connected by the thermoplastic resin 15. The internal electrode layer 5 has discontinuous portions in the longitudinal direction of the third rod-shaped body 24, which are divided by the thermoplastic resin 15 at multiple locations. In such a case, the apparent magnetic susceptibility of the internal electrode layer 5 in the longitudinal direction does not increase in a magnetic field, so that the third rod-shaped body 24 easily rotates around the longitudinal axis. The discontinuous portions of the internal electrode layer 5 are, for example, 40 μm or more.

[0052] A method of aligning the third rod-shaped bodies 24 as laminated components will be described. First, a plurality of the third rod-shaped bodies 24 obtained by cutting are arranged on the support surface 16a of the support member 16, and then the upper member 19 is installed. The first rod-shaped bodies 12 are arranged so that their longitudinal directions are parallel to each other. The support member 16 and the upper member 19 are both provided with an elastic sheet 20 attached thereto. As shown in FIG. 20A, two magnets 17 are arranged in advance, and the element component 2 placed in the gap between the support member 16 and the upper member 19 is moved in a direction of 90° to the longitudinal direction of the first rod-shaped bodies 12 along the horizontal direction in a magnetic field generated in advance so that the element component 2 is positioned between the two magnets 17. The third rod-shaped body 24 spontaneously rotates so that the extension direction of the internal electrode layer 5 and the direction of the magnetic flux lines 18 are parallel to each other, and the orientation of the third rod-shaped body 24 can be aligned.

[0053] As shown in Fig. 20B, after the third rod-shaped bodies 24 are aligned, a plurality of aligned third rod-shaped bodies 24 are assembled in a magnetic field to form a part assembly 27. For example, a jig 25 is moved horizontally from the outer left-right direction of the gap toward the center. As shown in the perspective view of Fig. 21, the jig 25 is an L-shaped formwork, and the two jigs 25 position the plurality of third rod-shaped bodies 24 in the longitudinal direction and in a direction perpendicular to the longitudinal direction, respectively, to form a plate-shaped part assembly 27.

[0054] After forming part assembly 27, part assembly 27 and jig 25 are fixed by support sheet 21 provided on upper member 19. On the side of part assembly 27 opposite to the side fixed by support sheet 21, side surface 9 of element precursor 13 is exposed.

[0055] FIG. 22 is a schematic diagram showing a state in which a processing process is performed on a part assembly. The processing process is, for example, a process of polishing the side surface 9. The exposed side surface 9 of the part assembly 27 fixed by the support sheet 21 can be polished using a polishing disk 28. The polishing is performed using multiple grindstones and abrasive powder, progressing from coarse to fine. In the final polishing, abrasive grains with an average grain size of 1 μm or less may be used, or abrasive grains with an average grain size of 0.5 μm or less may be used. The abrasive grain material may be diamond abrasive grains, which have excellent polishing properties and are unlikely to react with the dielectric material and the electrode material during firing.

[0056] After the exposed side surface 9 of the component assembly 27 is polished, the polished side surface 9 is fixed with another support sheet 21, and the original support sheet 21 is peeled off. The side surface 9 of the component assembly 27 that is newly exposed by peeling off the original support sheet 21 can also be polished.

[0057] FIG. 23 is a perspective view showing another example of the upper member. In the above, a plate-like member similar to the support member 16 is used as the upper member 19. As described above, the upper member 19 may be, for example, a mesh-like member or a vertical lattice-like member, as long as it can be specified so that a plurality of stacked components are not oriented vertically or two components are not overlapped. The upper member 19A in the example shown in the figure is a vertical lattice-like member. When it is a vertical lattice-like member, the upper member 19A may be arranged so that the vertical lattice is not parallel to the longitudinal direction of the stacked components.

[0058] The present disclosure may have the following embodiments.

[0059] The method for aligning laminated components disclosed herein involves applying a magnetic field in which magnetic flux lines intersect with the support surface to rectangular laminated components, the laminated components being formed by alternating stacking of ceramic green sheets and ferromagnetic electrode layers, and arranged in a space defined by a support member made of a non-magnetic material and having a flat support surface that is parallel to the horizontal direction, and an upper member made of a non-magnetic material and located above the support member at a predetermined distance from the support surface, thereby aligning the orientation of the laminated components.

[0060] The method of manufacturing a laminated ceramic component according to the present disclosure includes the above-described method of aligning laminated components, and after processing the surfaces of the laminated components whose orientation is aligned, the laminated components are fired.

[0061] According to the method for aligning stacked components disclosed herein, the orientation of stacked components can be easily and quickly aligned by simply placing a plurality of stacked components on a flat support surface.

[0062] According to the method for producing a multilayer ceramic component of the present disclosure, a multilayer ceramic component can be produced easily and quickly.

[0063] The methods, devices, materials, etc. used in each embodiment are not limited to the embodiment, and may be used in combination. For example, the ceramic green sheet or the flat plate assembly to which the ceramic slurry is applied as the protective layer may be cut before firing, or the flat plate assembly may be polished and then washed. Changing the processing conditions of each embodiment or adding a new process to each embodiment does not affect the gist of the present disclosure. [Explanation of symbols]

[0064] 1. Multilayer ceramic capacitors 2. Base parts 3 External electrode 4. Dielectric ceramics 5 Internal electrode layer 6 Protective layer 7 sides 8 End face 8A First End Face 8B Second end face 9. Side 10 Ceramic green sheet 11 Mother laminate 12 First rod-shaped body 12A Second rod-shaped body 13. Primer 15 Thermoplastic resin 16 Support member 16a Support surface 17 Magnet 18 Magnetic flux lines 19, 19A Upper member 20 Elastic sheet 21 Support Sheet 22 Arrow 23 Flat block 24 Third rod-shaped body 25 Jig 27 Parts Assembly 28 Polishing machine 35 Dielectric ceramic particles 36 Nickel particles

Claims

1. A method for aligning laminated components, comprising: applying a magnetic field whose magnetic flux lines intersect with the support surface to rectangular parallelepiped laminated components, the rectangular parallelepiped laminated components being formed by alternating stacking of ceramic green sheets and ferromagnetic layers, the rectangular parallelepiped laminated components being arranged in a gap between a support member which contains a non-magnetic material and has a flat support surface which is parallel to the horizontal direction, and an upper member which contains a non-magnetic material and is located above the support member at a predetermined distance from the support surface, to align the orientation of the laminated components, and then stopping the application of the magnetic field when the multiple laminated components with the aligned orientation are sandwiched between the support member and the upper member.

2. The method for aligning laminated components according to claim 1 , further comprising the step of applying vibration to the laminated components disposed in the gap.

3. The method for aligning laminated components according to claim 1 or 2, wherein the magnetic field is an intermittent magnetic field.

4. 4. The method for aligning laminated components according to claim 1, wherein the magnetic field is a magnetic field in which the direction of magnetic flux lines repeatedly reverses.

5. 5. The method for aligning stacked components according to claim 1, wherein the magnetic field is generated by a first magnet positioned below the support member and a second magnet positioned above the upper member.

6. 6. The method for aligning laminated components according to claim 1, further comprising the step of moving the laminated components placed in the gap into a magnetic field that has been generated in advance.

7. 7. The method for aligning stacked components according to claim 1, further comprising the step of: assembling a plurality of stacked components with the same orientation in the gap to form a component assembly while a magnetic field is applied to the stacked components.

8. The method for aligning laminated components according to any one of claims 1 to 7, wherein a portion of the upper member facing the support surface comprises an elastic material.

9. The method for aligning stacked components according to any one of claims 1 to 8, wherein the upper member is a mesh-like member or a vertical lattice-like member.

10. 10. The method for aligning laminated components according to claim 1, wherein the ferromagnetic layer contains a ferromagnetic metal material and an organic binder, and the content of the organic binder is 1.5 times or less, in terms of volume ratio, that of the ferromagnetic metal material.

11. 11. The method for aligning laminated components according to claim 1, wherein the ferromagnetic layers have discontinuous portions in the longitudinal direction of the laminated components.

12. The method for aligning stacked components according to any one of claims 1 to 11, A method for manufacturing multilayer ceramic components in which the surfaces of aligned laminated components are processed and then fired.

Citation Information

Patent Citations

  • Alignment equipment and alignment method of electronic components

    JP1998284355A

  • Method and device for aligning electronic parts, and method of manufacturing electronic parts

    JP2001150249A

  • Alignment method of orientation of chip component

    JP2003007574A

  • Circuit board mount structure and method for multilayer ceramic capacitor, land pattern of circuit board, and package and alignment method for multilayer ceramic capacitor

    JP2012134498A

  • Manufacturing method and manufacturing apparatus for capacitor element

    JP2015084406A