Coating composition, coating film and article, optical device, lighting device
A coating composition with silica and metal oxide fine particles, along with a high-boiling-point solvent, addresses the inefficiency of conventional fogging removal methods by forming a porous film that quickly eliminates fogging and maintains transparency and uniformity on substrates.
Patent Information
- Application Number
- JP2023527170
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-06-07
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2041-06-07
AI Technical Summary
Conventional methods for suppressing fogging on substrates, such as glass and plastics, are inefficient in completely removing organic substances that cause clouding, leading to reduced transparency over time.
A coating composition comprising silica fine particles with an average size of 3-25 nm, metal oxide fine particles with a refractive index of 1.6 or more, and a high-boiling-point solvent, which forms a porous and hydrophilic coating film that quickly eliminates fogging by allowing organic substances to penetrate and spread, maintaining transparency and uniformity.
The coating composition effectively and rapidly eliminates fogging, maintaining high transparency and uniformity by allowing organic substances to penetrate into the porous film, reducing light scattering and adhesion, while also providing antifouling properties.
Smart Images

Figure 0007566150000001 
Figure 0007566150000002 
Figure 0007566150000003
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a coating composition, a coating film and an article, an optical device, and a lighting device, each of which includes silica fine particles. [Background technology]
[0002] It is known that organic substances such as plasticizers and additives contained in rubber products and plastics themselves, which are components other than the glass of vehicles and buildings, and transparent plastic covers of headlights, volatilize on the surfaces of substrates, etc., and the volatilized organic substances adhere to the surfaces of the substrates, causing a fogging phenomenon, which reduces the transparency of the substrates. Various techniques have been proposed to suppress the fogging of the substrates. For example, Patent Document 1 discloses a method of forming a thin film of a metal oxide exhibiting photocatalytic activity with a thickness of 10 to 200 nm on the surface of glass, as a technique for decomposing and removing the organic substances that cause the fogging. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Japanese Patent Application Publication No. 9-235140 Summary of the Invention [Problem to be solved by the invention]
[0004] However, in the technology described in Patent Document 1, the photocatalyst is excited by receiving light energy and decomposes the organic matter attached to the thin film, so there is a problem in that it takes time to completely remove the organic matter attached to the thin film.
[0005] The present disclosure has been made in view of the above, and has an object to provide a coating composition, a coating film, and an article, an optical device, and a lighting device that can quickly eliminate clouding of a substrate due to the fogging phenomenon and maintain high transparency of the coating film compared to conventional techniques. [Means for solving the problem]
[0006] In order to solve the above problems and achieve the object, the coating composition of the present disclosure includes silica fine particles having an average particle size of 3 nm to 25 nm, metal oxide fine particles, a solvent having a boiling point of 150° C. to 300° C., and water. The content of the silica fine particles is 0.1% by mass to 5% by mass. The content of the solvent is 20% by mass to 70% by mass. The content of the metal oxide fine particles is 2% by mass or more and 80% by mass or less based on the silica fine particles. The average particle size of the metal oxide fine particles is 1 nm or more and 25 nm or less. Effect of the Invention
[0007] According to the present disclosure, it is possible to more quickly eliminate clouding of a substrate due to the fogging phenomenon and to maintain high transparency of a coating film, as compared with the conventional techniques. [Brief description of the drawings]
[0008] [Figure 1] FIG. 1 is a cross-sectional view showing a schematic example of a structure of a coating film using a coating composition according to a first embodiment. [Diagram 2] FIG. 2 is a diagram for explaining the effect of a coating film using the coating composition according to the first embodiment. [Diagram 3] FIG. 2 is a cross-sectional view that illustrates a schematic example of a method for producing a coating film using the coating composition according to the first embodiment. [Figure 4] 1A to 1C are cross-sectional views that diagrammatically show an example of a procedure for producing a coating film using the coating composition according to the first embodiment. [Diagram 5] 1A to 1C are cross-sectional views that diagrammatically show an example of a procedure for producing a coating film using the coating composition according to the first embodiment. [Figure 6] 1A to 1C are cross-sectional views that diagrammatically show an example of a procedure for producing a coating film using the coating composition according to the first embodiment. [Figure 7] FIG. 11 is a front view showing an example of an optical device having a coating film according to a second embodiment. [Figure 8]8 is a cross-sectional view taken along line AA in FIG. 7. [Figure 9] FIG. 11 is a front view showing an example of an optical device having a coating film according to a second embodiment. [Figure 10] 10 is a cross-sectional view of FIG. 9 taken along line B-B. [Figure 11] FIG. 11 is a front view showing an example of an optical device having a coating film according to a second embodiment. [Figure 12] 12 is a cross-sectional view taken along CC in FIG. 11 . [Figure 13] FIG. 11 is a front view showing an example of an optical device having a coating film according to a second embodiment. [Figure 14] FIG. 14 is a cross-sectional view taken along line DD of FIG. [Figure 15] FIG. 11 is a front view showing an example of a lighting device having a coating film according to a third embodiment. [Figure 16] 16 is a cross-sectional view of FIG. 15 taken along line E-E. [Figure 17] FIG. 1 is a diagram summarizing the evaluation results of examples and comparative examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Hereinafter, a coating composition, a coating film, an article, an optical device, and a lighting device according to embodiments of the present disclosure will be described in detail with reference to the drawings.
[0010] Embodiment 1 <Coating Composition> The coating composition according to the first embodiment includes silica fine particles, metal oxide fine particles, a high boiling point solvent, and water. The coating composition according to the first embodiment may further include fluororesin particles and a non-volatile hydrophilic organic substance. The components included in the coating composition are described below.
[0011] <Silica fine particles> The silica fine particles contained in the coating composition according to the first embodiment are the base component of the coating film. By blending silica fine particles and metal oxide fine particles in the coating composition, a highly transparent hydrophilic surface can be formed and maintained in the coating film formed by the coating composition. The coating film formed by the coating composition according to the first embodiment is formed by agglomeration of silica fine particles and metal oxide fine particles, and is therefore porous on the nanometer order. Since the surface of the coating film is hydrophilic, it is possible to improve the ability to suppress adhesion of hydrophobic dirt, and also to make the attached water easier to spread and easier to flow off. Furthermore, since the spread of the attached water is improved, water gets between the film surface and the dirt, making it easier for the dirt to flow off.
[0012] Furthermore, the coating film formed by the coating composition of the present embodiment 1 based on silica fine particles is porous and low density, so that the interaction between the coating film surface and dust and other adherents is small, making it difficult for dirt to adhere. If an organic substance that causes clouding due to the fogging phenomenon adheres to the coating film formed by the coating composition of the present embodiment 1, the organic substance penetrates the silica fine particles, so that the clouding is quickly eliminated and transparency can be maintained. Here, the clouding due to the fogging phenomenon is a white cloud that appears due to light scattering caused by the unevenness of organic substances such as plasticizers and solvents that adhere to the surface of the coating film. In addition, since metal oxide fine particles are included, even if the absorption of the organic substance 18 becomes uneven, visibility is not affected, and high transparency and uniformity are maintained.
[0013] Silica fine particles have a lower refractive index than other inorganic particles, and have a value close to the refractive index of transparent resins such as plastics and glass that are commonly used as substrates. If the substrate and the coating film have similar refractive indices, the coating film is prevented from appearing white due to light reflection at the interface and surface between them, and the color tone of the substrate is not easily impaired.
[0014] The average particle size of the silica microparticles is preferably 3 nm or more and 25 nm or less, and particularly preferably 4 nm or more and 10 nm or less. Here, the average particle size means the average particle size value of the primary particles measured by a laser light scattering type or dynamic scattering type particle size distribution meter. In addition, the primary particle is the smallest unit of the particle, and is a particle that is not further divided. An aggregate of primary particles in which a plurality of primary particles are agglomerated is called a secondary particle. If the average particle size of the silica microparticles is less than 3 nm, the coating film becomes too dense, and the intermolecular force acting between the film surface and the dirt becomes large, and the desired antifouling properties may not be obtained. If the average particle size of the silica microparticles is larger than 25 nm, the surface unevenness of the coating film becomes too large, and cloudiness is easily generated. In addition, the average particle size of the silica microparticles is 3 nm or more and 25 nm or less, and the coating film contains metal oxide fine particles. This results in a coating film with appropriate density, which allows organic matter that causes clouding due to the fogging phenomenon to easily penetrate the surface of the coating film, and since the organic matter penetrates into the porous film made of silica fine particles, the clouding is quickly eliminated and high transparency can be maintained. In addition, the contact area between the surface of the coating film and dirt such as dust is reduced, so sufficient anti-fouling properties can be obtained. Here, anti-fouling properties refer to the property of making it difficult for dirt to adhere to the surface or the property of making it easy to remove adhered dirt.
[0015] The content of silica fine particles in the coating composition is preferably 0.1% by mass or more and 5% by mass or less, and preferably 0.5% by mass or more and 2% by mass or less. When the content of silica fine particles in the coating composition is less than 0.1% by mass, the formed coating film may be too thin and the desired antifouling properties may not be obtained. On the other hand, when the content of silica fine particles in the coating composition is more than 5% by mass, the coating film may be too thick, cracks and unevenness may occur, and the film may easily become cloudy. From the above, the content of silica fine particles in the coating composition is preferably 0.1% by mass or more and 5% by mass or less. In particular, when the content of silica fine particles in the coating composition is 0.5% by mass or more and 2% by mass or less, a uniform coating film having a suitable thickness can be formed, and sufficient antifouling properties can be obtained.
[0016] The silica microparticles having the above characteristics can be prepared according to a known method. For example, colloidal silica prepared from an aqueous solution of sodium silicate or prepared by a sol-gel method can be used as the silica microparticles. The silica microparticles may be spherical or irregularly shaped, such as hollow, scaly, or rod-like. When scaly silica microparticles are used, the film strength obtained tends to be high. Therefore, for applications requiring abrasion resistance, the use of scaly silica microparticles can provide favorable results. It is also possible to achieve both strength of the transparent coating film by mixing scaly silica and spherical silica. In addition, silica microparticles linked in a beaded shape may be used.
[0017] <Metal oxide fine particles> The metal oxide fine particles contained in the coating composition of the present embodiment 1 preferably exhibit a high refractive index and, when formed into a coating film, exhibit transparency. By including metal oxide fine particles with a high refractive index, there is an effect of making unevenness less noticeable when organic matter that causes cloudiness due to the fogging phenomenon penetrates into the coating film, and contributes to the transparency and uniformity of the coating film. Since a coating film based on silica fine particles is porous, the refractive index of the coating film is one that takes into account air. When metal oxide fine particles with a high refractive index are included, the refractive index of the coating film is higher than that of a silica fine particle layer consisting only of silica fine particles. Therefore, the difference between the refractive index of the film containing metal oxide fine particles and the refractive index of the organic matter becomes smaller, and unevenness when organic matter penetrates into the coating film becomes less noticeable, and the transparency and uniformity of the coating film can be realized.
[0018] The refractive index of the metal oxide fine particles is preferably 1.6 or more. When the refractive index of the metal oxide is 1.6 or more, when a coating film is formed using the coating composition of the present embodiment 1, unevenness caused by the penetration of an organic substance into the coating film is reduced.
[0019] Metal oxides that exhibit high photocatalytic properties can also be used. By including fine particles of metal oxides with photocatalytic properties in the coating film, organic matter that penetrates the coating film is decomposed under sunlight or artificial light irradiation. Furthermore, because it exhibits hydrophilicity, it has self-cleaning properties that wash away dirt that adheres to the surface.
[0020] The metal oxide may be an oxide of a single metal, a solid solution of two or more oxides, or a composite oxide. For example, the single metal oxide includes aluminum oxide, titanium oxide, zirconium oxide, indium oxide, zinc oxide, tin oxide, lanthanum oxide, yttrium oxide, cerium oxide, and magnesium oxide. The solid solution of two or more oxides includes indium tin oxide. The composite oxide includes, for example, barium titanate, perovskite, and spinel. When the coating film formed of the coating composition of the first embodiment containing a metal oxide having a photocatalytic effect is applied to the surface of a substrate formed of a resin, for example, apatite-coated titanium oxide does not decompose the resin.
[0021] The average particle size of the metal oxide particles is preferably 1 nm or more and 25 nm or less, and particularly preferably 2 nm or more and 10 nm or less. Here, the average particle size means the average particle size of the primary particles measured by a laser light scattering type or dynamic scattering type particle size distribution meter. If the particle size is larger than 25 nm, the light scattering on the coating film surface may increase, and the haze may increase. If the average particle size of the metal oxide particles is 1 nm or less, the coating film may become too dense, and the organic matter that causes the clouding due to the fogging phenomenon may not penetrate easily. In particular, if the average particle size of the metal oxide particles is 2 nm or more and 10 nm or less, the coating film has a moderate density, and the organic matter that causes the clouding due to the fogging phenomenon may penetrate more easily.
[0022] The content of the metal oxide particles in the coating composition is preferably 80% by mass or less and 2% by mass or more relative to the silica particles, and particularly preferably 50% by mass or less and 5% by mass or more. If the content is 80% by mass or less and 2% by mass or more relative to the silica particles, the refractive index can be appropriately adjusted, and the effect of suppressing unevenness caused by the penetration of organic matter that causes cloudiness due to the fogging phenomenon into the coating film can be easily obtained.
[0023] Examples of the shape of the metal oxide fine particles include spherical, granular, hollow, elliptical, cubic, rectangular, needle-like, columnar, rod-like, cylindrical, and scaly shapes. Considering the formation of a porous coating film, the shape is preferably spherical, elliptical, columnar, or the like.
[0024] <High boiling point solvent> The high boiling point solvent contained in the coating composition according to the first embodiment is a solvent having a boiling point higher than room temperature, and is a solvent having a boiling point of 150°C or more and 300°C or less, as described below. The high boiling point solvent can control the drying speed of the coating composition in the process of forming the coating film. This allows the liquid film to be formed while maintaining the initial concentration of silica fine particles in the coating composition, and can prevent the aggregation of silica fine particles during application. Furthermore, by changing the content of the high boiling point solvent so that the drying time becomes longer, the liquid film after application can be leveled. These effects allow a uniform coating film to be obtained.
[0025] The boiling point of the high-boiling solvent is preferably 150°C or more and 300°C or less. If the boiling point of the high-boiling solvent is less than 150°C, the drying speed becomes too fast, and the effect of preventing the aggregation of silica fine particles and leveling the liquid film after application cannot be obtained. On the other hand, if the boiling point of the high-boiling solvent exceeds 300°C, the solvent tends to remain in the coating film, and a coating film having the desired properties cannot be obtained. For the above reasons, the boiling point of the high-boiling solvent is preferably 150°C or more and 300°C or less.
[0026] The solubility of the high boiling point solvent in water is not particularly limited, but is preferably 70% by mass or more, because if the solubility in water is less than 70% by mass, the solvent will be easily separated from water.
[0027] Examples of high boiling point solvents include ethylene glycol, propylene glycol, propylene glycol propylene glycol monomethyl ether, ethylene glycol monomethyl ether, ethylene glycol monomethyl ether acetate, ethyl lactate, diethylene glycol dimethyl ether, dipropylene glycol dimethyl ether, dipropylene glycol dimethyl ether, diethylene glycol ethyl methyl ether, diethylene glycol isopropyl methyl ether, dipropylene glycol monomethyl ether, diethylene glycol diethyl ether, diethylene glycol monomethyl ether, diethylene glycol butyl methyl ether, tripropylene glycol dimethyl ether, triethylene glycol dimethyl ether, diethylene glycol monobutyl ether, ethylene glycol monophenyl ether, triethylene glycol monomethyl ether, diethylene glycol dibutyl ether, triethylene glycol butyl methyl ether, polyethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, polyethylene glycol monomethyl ether, and N-methyl-2-pyrrolidone. These may be used alone or in combination as the high boiling point solvent.
[0028] The content of the high boiling point solvent in the coating composition is 20% by mass or more and 70% by mass or less, preferably 30% by mass or more and 50% by mass or less. If the content of the high boiling point solvent is less than 20% by mass, the effect of preventing aggregation of silica fine particles and the effect of leveling the liquid film after application are not sufficiently obtained. In addition, if the content of the high boiling point solvent is more than 70% by mass, the solubility of the silica fine particles and the fluororesin particles that can be optionally contained in the coating composition decreases, and they tend to aggregate. From the above, the content of the high boiling point solvent in the coating composition is preferably 20% by mass or more and 70% by mass or less. In particular, if the content of the high boiling point solvent in the coating composition is 30% by mass or more and 50% by mass or less, the dispersion state of the silica fine particles and the fluororesin particles in the liquid film by the coating composition can be maintained while the leveling effect of the liquid film can be obtained, so that a uniform and highly transparent coating film can be formed.
[0029] <Water> The water contained in the coating composition according to the first embodiment is not particularly limited, and tap water, pure water, RO (Reverse Osmosis) water, deionized water, etc. can be used. RO water is water obtained by removing impurities from tap water using a reverse osmosis membrane. From the viewpoint of improving the dispersion stability of silica fine particles in the coating composition, it is preferable that the water contains fewer ionic impurities such as calcium ions or magnesium ions. Specifically, the amount of divalent or higher ionic impurities contained in the water is preferably 200 ppm or less, more preferably 50 ppm or less. If the amount of divalent or higher ionic impurities is more than 200 ppm, aggregation of silica fine particles may occur, which may cause a decrease in the fluidity of the coating composition, resulting in a decrease in the applicability and a decrease in the transparency of the coating film.
[0030] The water content in the coating composition is not particularly limited, but is preferably 25% by mass or more and 80% by mass or less, and more preferably 50% by mass or more and 70% by mass or less. If the water content is less than 25% by mass, the solubility of the silica fine particles and the fluororesin particles that can be optionally contained in the coating composition may decrease, and they may be easily aggregated. If the water content is less than 25% by mass, the coating film may become thick and defects such as cracks may easily occur. On the other hand, if the water content exceeds 80% by mass, the amount of solids in the composition may become too small, and it may be difficult to efficiently form the coating film. From the above, the water content in the coating composition is preferably 25% by mass or more and 80% by mass or less. In particular, if the water content in the coating composition is 50% by mass or more and 70% by mass or less, the dispersion state of the silica fine particles and the fluororesin particles in the liquid film of the coating composition can be maintained, and a coating film with a suitable thickness, uniformity, and high transparency can be formed.
[0031] <Fluororesin particles> The coating composition according to the first embodiment may also contain fluororesin particles. By blending the fluororesin particles, a partially hydrophobic surface can be formed on the coating film to be formed. This can improve the ability to prevent dirt from adhering. In addition, the surface of the coating film formed by the fluororesin particles can be given lubricity. This can improve the abrasion resistance of the coating film.
[0032] The fluororesin particles are not particularly limited, but examples include particles formed from PTFE (polytetrafluoroethylene), FEP (tetrafluoroethylene-hexafluoropropylene copolymer), PFA (tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer), ETFE (ethylene-tetrafluoroethylene copolymer), ECTFE (ethylene-chlorotrifluoroethylene copolymer), PVDF (polyvinylidene fluoride), PCTFE (polychlorotrifluoroethylene), PVF (polyvinyl fluoride), fluoroethylene-vinyl ether copolymer, fluoroethylene-vinyl ester copolymer, copolymers and mixtures of these, and mixtures of these fluororesins with other resins.
[0033] The average particle size of the fluororesin particles is preferably 80 nm or more and 550 nm or less, more preferably 100 nm or more and 500 nm or less. If the average particle size of the fluororesin particles is less than 80 nm, the hydrophobic portion may not be formed sufficiently on the surface of the coating film. On the other hand, if the particle size of the fluororesin particles exceeds 550 nm, the surface of the coating film becomes uneven and dirt is easily caught, so that the desired antifouling property may not be obtained. In addition, the unevenness of the surface of the coating film may cause light scattering, causing the coating film to become cloudy. From the above, the average particle size of the fluororesin particles is preferably 80 nm or more and 550 nm or less. In particular, if the average particle size of the fluororesin particles is 100 nm or more and 500 nm or less, the coating film has a hydrophobic surface due to the fluororesin particles and moderate unevenness, so that sufficient antifouling property can be obtained.
[0034] In addition, by minimizing the surface irregularities of the coating film formed using rod-like or scaly fluororesin particles, the transparency of the coating film can be improved.Furthermore, by using a dispersion of fluororesin particles that contains low molecular weight components or solvents, has flexibility when applied, and solidifies after application as these components volatilize, it is also possible to improve the smoothness and transparency of the resulting film.
[0035] The fluororesin particles can be prepared according to a known method. Commercially available fluororesin particles dispersed in water can be used as a raw material for the coating composition.
[0036] The content of the fluororesin particles in the coating composition is preferably 5% by mass or more and 50% by mass or less relative to the content of the silica fine particles, and particularly preferably 10% by mass or more and 30% by mass or less. If the content of the fluororesin particles relative to the content of the silica fine particles in the coating composition is less than 5% by mass, the ratio of the hydrophobic surface on the surface of the coating film is low, and the desired antifouling properties may not be obtained. On the other hand, if the content of the fluororesin particles relative to the content of the silica fine particles is more than 50% by mass, dust tends to easily adhere to the coating film, which is not preferable. From the above, the content of the fluororesin particles relative to the content of the silica fine particles in the coating composition is preferably 5% by mass or more and 50% by mass or less. In particular, when the content of the fluororesin particles relative to the content of the silica fine particles in the coating composition is 10% by mass or more and 30% by mass or less, the coating film has a hydrophilic surface and a hydrophobic surface at an appropriate ratio, and sufficient antifouling properties can be obtained.
[0037] <Non-volatile hydrophilic organic substances> The coating composition according to the first embodiment may also contain a non-volatile hydrophilic organic substance, which is a non-volatile and hydrophilic organic substance. By blending the non-volatile hydrophilic organic substance, it is possible to fill voids in the formed coating film, reduce scattering inside the coating film, and improve the transparency of the coating film. In addition, it is possible to improve the applicability of the coating composition.
[0038] The non-volatile hydrophilic organic substance is not particularly limited, and various organic substances that are not deliquescent and are non-volatile can be used. Examples of non-volatile hydrophilic organic substances are polyethylene glycol, polypropylene glycol, polytetramethylene glycol, dimethicone copolyol, and mixtures thereof.
[0039] A surfactant can also be used as the non-volatile hydrophilic organic substance. There are no particular limitations on the surfactant, but nonionic surfactants that are less likely to cause aggregation of silica fine particles are preferred. However, anionic surfactants and cationic surfactants can also be used if attention is paid to the amount added, the pH of the solvent, etc.
[0040] Examples of the nonionic surfactant include polyoxyethylene alkyl ethers, polyoxyethylene alkylphenol ethers, polyoxyethylene alkyl esters, polyoxyethylene alkylamines, polyoxyethylene alkylamides, sorbitan alkyl esters, and polyoxyethylene sorbitan alkyl esters.
[0041] Examples of anionic surfactants include higher alcohol sulfates (sodium salts or amine salts), alkyl allyl sulfonates (sodium salts or amine salts), alkyl naphthalene sulfonates (sodium salts or amine salts), alkyl naphthalene sulfonate condensates, alkyl phosphates, dialkyl sulfosuccinates, rosin soaps, and fatty acid salts (sodium salts or amine salts).
[0042] Examples of the cationic surfactant include octadecylamine acetate, imidazoline derivative acetate, polyalkylenepolyamine derivatives or salts thereof, octadecyltrimethylammonium chloride, triethylaminoethyl alkylamido halogenides, alkylpyridinium sulfates, and alkyltrimethylammonium halogenides.
[0043] The non-volatile hydrophilic organic substance is not particularly limited, but one having an average molecular weight of 400 or more and 500,000 or less can be used, and one having an average molecular weight of 700 or more and 100,000 or less is preferable. If the average molecular weight is lower than 400, it is not preferable because dust adhesion may increase when a large amount of non-volatile hydrophilic organic substance is added. In addition, if the average molecular weight exceeds 500,000, the fluidity of the coating liquid may decrease, making it difficult to achieve a uniform coating. For the above reasons, it is desirable that the average molecular weight of the non-volatile hydrophilic organic substance is 400 or more and 500,000 or less. In particular, if the average molecular weight of the non-volatile hydrophilic organic substance is 700 or more and 100,000 or less, it has a moderate fluidity, so that a highly transparent coating film can be obtained by filling the voids in the coating film.
[0044] The content of the non-volatile hydrophilic organic matter in the coating composition is preferably 10% by mass or more and 40% by mass or less relative to the content of the silica fine particles, and particularly preferably 10% by mass or more and 30% by mass or less. If the content of the non-volatile hydrophilic organic matter relative to the content of the silica fine particles in the coating composition is less than 10% by mass, the voids inside the coating film to be formed may not be sufficiently filled, or the spreadability of the coating composition may be reduced, and the transparency of the coating film may be insufficient. On the other hand, if the content of the non-volatile hydrophilic organic matter relative to the content of the silica fine particles is more than 40% by mass, the coating film may become too soft and the durability may be insufficient. From the above, it is preferable that the content of the non-volatile hydrophilic organic matter relative to the content of the silica fine particles in the coating composition is 10% by mass or more and 40% by mass or less. In particular, when the content of the non-volatile hydrophilic organic matter in the coating composition is 10% by mass or more and 30% by mass or less, the effect of sufficiently filling the voids in the coating film can be obtained, so that a coating film with high transparency can be formed.
[0045] <Other> The coating composition according to the first embodiment may contain components known in the art from the viewpoint of imparting various properties to the coating composition, within a range that does not impair the effects of the present disclosure. Examples of such components include coupling agents and silane compounds. The amounts of these components are not particularly limited as long as they do not impair the effects of the present disclosure, and may be appropriately adjusted depending on the types of components used.
[0046] The method for producing the coating composition according to the first embodiment containing the above-mentioned components is not particularly limited and can be carried out according to a method known in the art. Specifically, the coating composition can be prepared by blending and mixing the above-mentioned components.
[0047] Next, a coating film prepared using the above coating composition will be described.
[0048] <Coating film> The coating composition according to the first embodiment is applied onto a substrate and dried to form a coating film.
[0049] 1 is a cross-sectional view showing a schematic example of a structure of a coating film using the coating composition according to embodiment 1. In this example, the coating composition contains silica fine particles, metal oxide fine particles, a high boiling point solvent, water, fluororesin particles, and a non-volatile hydrophilic organic substance.
[0050] The coating film 10 is disposed on a substrate 20, and has a silica fine particle layer 11 formed by aggregation of silica fine particles 15 (shown in FIG. 6 described later, etc.) and metal oxide fine particles 17. Some of the fluororesin particles 12 are exposed on the surface of the coating film 10, i.e., the surface of the silica fine particle layer 11, and some are not exposed. In other words, the fluororesin particles 12 are disposed in a state where they are partially exposed on the surface of the coating film 10 and dispersed in the silica fine particle layer 11.
[0051] FIG. 1 shows a schematic diagram of a crack 13, which is an example of a defect formed by aggregation of silica fine particles 15 when the applied liquid film of the coating composition dries. In reality, small voids are often formed instead of clear cracks 13. Conventionally, these defects scatter light and cause the film to become cloudy. However, in the coating film 10 using the coating composition according to the first embodiment, the inside of these defects is filled with a non-volatile hydrophilic organic substance 14. This suppresses light scattering, and increases the transparency of the coating film 10. In addition, the addition of the non-volatile hydrophilic organic substance 14 also has the effect of suppressing the occurrence of these defects themselves.
[0052] As shown in FIG. 1, the surface of a coating film 10 formed using the coating composition according to the first embodiment has both a hydrophilic portion due to the silica fine particles 15 and a hydrophobic portion due to the fluororesin particles 12.
[0053] As described later, the coating composition according to the first embodiment contains a high boiling point solvent, so that the time from when the coating composition is applied to the substrate 20 to form a liquid film to when the coating film 10 is formed by drying is longer than in the past. Therefore, the liquid film after application is leveled, and the coating film 10 is formed in that state. As a result, a coating film 10 with smoothed surface irregularities is obtained, and the transparency can be increased compared to the past.
[0054] The thickness of the coating film 10 is preferably 20 nm or more and 250 nm or less. If the thickness is less than 20 nm, the coating film is too thin and the desired antifouling properties cannot be obtained. If the thickness is more than 250 nm, the surface of the coating film 10 may become uneven and cloudy. For the above reasons, the thickness of the coating film 10 is preferably 20 nm or more and 250 nm or less. If the thickness of the coating film 10 is 80 nm or more and 150 nm or less, particularly if it is around 100 nm, the coating film 10 can be given an antireflection function and the transmittance of the substrate 20 to which the coating film 10 is applied can be improved.
[0055] Fig. 2 is a diagram for explaining the effect of a coating film using the coating composition according to the embodiment 1. Here, Fig. 2a shows a state in which an organic substance that causes clouding due to the fogging phenomenon is directly attached to a substrate such as glass without applying a coating film. Organic substance 18 that causes clouding due to the fogging phenomenon is attached to the surface of substrate 20 as minute droplets, which scatter light and cause the substrate to become cloudy.
[0056] FIG. 2b shows an example of a coating film using a conventional coating composition, in which a film consisting of only silica fine particles is formed on a substrate, and organic matter 18, which causes clouding due to the fogging phenomenon, is attached to the film. Since the organic matter 18 is absorbed by the silica fine particle layer 11, as explained in FIG. 2a, droplets are not generated on the substrate, and therefore no significant light scattering occurs. However, the difference in refractive index between the portion 21b in FIG. 2b that absorbs the organic matter 18, i.e., the portion close to the outermost surface of the film, and the portion 22b that does not absorb the organic matter 18, i.e., the portion close to the substrate, becomes large, which causes unevenness in transmittance, loss of transparency, and glare. Since a film consisting of only silica fine particles is a porous film, the refractive index of the film is a value that takes into account the refractive index of air. The portion 21b in FIG. 2b that absorbs the organic matter 18 is a value that takes into account the refractive index of the organic matter. Therefore, the difference in refractive index between the portion 21b in FIG. 2b that absorbs the organic matter 18 and the portion 22b that does not absorb the organic matter 18 becomes large. Furthermore, if there are areas where the amount of organic matter 18 absorbed differs due to differences in exposure conditions to the organic matter, such as air currents, or the temperature of the substrate, there is a problem that the transmittance of the coating film also differs.
[0057] FIG. 2c shows the state where organic matter 18, which causes clouding due to the fogging phenomenon, is attached to the coating film using the coating composition according to the first embodiment. Since the coating film using the coating composition according to the first embodiment contains metal oxide fine particles with a high refractive index, the refractive index of the film is higher than that of the conventional coating film made of only silica fine particles described in FIG. 2b, that is, close to the refractive index of the organic matter. Therefore, the difference in refractive index between the part 21c in FIG. 2c that absorbs the organic matter 18, i.e., the part close to the outermost surface of the film, and the part 22c that does not absorb the organic matter 18, i.e., the part close to the substrate, is smaller than that of the film made of only silica fine particles described in FIG. 2b. Therefore, even if the absorption of the organic matter 18 is uneven, visibility is not affected, and high transparency and uniformity are maintained.
[0058] <Base material> The substrate is a member on which the coating film is to be formed. In one example, the substrate is a member that constitutes an article. The substrate can be transparent glass or transparent plastic. When a coating film is formed on a transparent substrate, the transparency of the substrate is not deteriorated, and an anti-reflection effect can be obtained by appropriately designing the thickness of the coating film, and the light transmittance can be improved. When a coating film is formed on a non-transparent substrate, there is an advantage that the color tone of the substrate can be treated without changing. In the case of a glossy surface, the above-mentioned anti-reflection effect can also be used to improve the depth or vividness of the color. Since fogging phenomenon is easily noticeable on a surface with high gloss, when a coating film using the coating composition according to the first embodiment is formed on a substrate surface with a 60° specular gloss of 50 or more, the effect of suppressing the fogging phenomenon of the substrate is particularly likely to be obtained. When a coating film using the coating composition according to the first embodiment is formed on a substrate surface with a color such as black, regardless of the gloss, the effect of suppressing the fogging phenomenon is particularly likely to be obtained. On a transparent or white substrate with a low gloss, fogging due to the fogging phenomenon is not particularly noticeable even if it occurs.
[0059] <Manufacturing method> 3 is a cross-sectional view showing a schematic example of a method for producing a coating film using the coating composition according to the first embodiment. A fabric-like material 31 impregnated with the coating composition is fixed to a block 30, which is a coater, and the surface to which the fabric-like material 31 is fixed is brought into close contact with the substrate 20 and slid thereon, thereby applying the coating composition onto the substrate 20. As a result, a liquid film made of the coating composition is formed on the substrate 20. By combining the fabric-like material 31 with the block 30, a small amount of the coating composition can be applied onto the substrate 20 while applying a uniform pressure to the fabric-like material 31, and a uniform coating film can be formed.
[0060] The thickness of the cloth-like material 31 is preferably 5 mm or less. If the thickness is greater than 5 mm, the amount of the coating composition impregnated becomes too large, which may prevent the coating from being applied uniformly. Here, the cloth-like material 31 refers to an accumulation of fibers, such as woven fabric, nonwoven fabric, or paper. The material of the cloth-like material 31 is not particularly limited as long as it can be impregnated with the coating composition. An example of the cloth-like material 31 is a rayon cloth. It is preferable that the cloth-like material contain as few short fibers as possible, since fiber waste will cause defects in the coating.
[0061] The shape of the block 30 is not particularly limited, but it is preferable that the block 30 can be slid along the surface of the substrate 20. In other words, it is preferable to use a block 30 having a surface shaped to fit the surface of the substrate 20.
[0062] The material of the block 30 is not particularly limited. In one example, the material of the block 30 is polycarbonate. Also, the material of the block 30 can be impregnated with the coating composition. Sponges of various materials having communicating holes can be used as the block 30, but the hole diameter of the sponge is preferably 0.05 mm or more and 2 mm or less, and more preferably 0.1 mm or more and 1.5 mm or less. If the hole diameter is less than 0.05 mm, it is difficult to apply a sufficient amount of the coating composition. Also, if the hole diameter exceeds 2 mm, the amount of the coating composition applied becomes too large, which is not preferable because unevenness is likely to occur in the liquid film. From the above, the hole diameter of the sponge is preferably 0.05 mm or more and 2 mm or less.
[0063] The coating method described above is a method for stably applying the coating to a wide area, but other coating methods can also be used, such as a dipping method, a coating method using a brush, a spray coating method, a coating method using various coaters, etc. Also, the coating composition can be applied by pouring it onto the substrate 20.
[0064] 4 to 6 are cross-sectional views showing an example of a procedure of a method for producing a coating film using the coating composition according to the first embodiment. First, a liquid film forming step is performed in which a coating composition is applied onto a substrate 20 to form a liquid film. FIG. 4 shows an initial state of a liquid film 10A immediately after the coating composition is applied onto the substrate 20. As shown in FIG. 4, in the initial state, the thickness of the liquid film 10A due to the applied coating composition is uneven. In addition, in the liquid film 10A, silica fine particles 15 and metal oxide fine particles 17 are in a state of being dispersed in the solvent 16 without being aggregated. Next, a drying step is performed in which the liquid film 10A is dried in this state.
[0065] Since the coating composition according to the first embodiment contains a high-boiling point solvent, the solvent 16 in the coating composition does not volatilize immediately after application, but volatilizes over a period of time according to the content of the high-boiling point solvent. During this period, as shown in Fig. 5, the liquid film 10A is gradually leveled, so that the upper surface of the liquid film 10A becomes flat. At this time, the silica fine particles 15 and the metal oxide fine particles 17 do not aggregate in the liquid film 10A, but remain dispersed.
[0066] Then, when the solvent 16 is finally dried, the silica fine particles 15 and the metal oxide fine particles 17 are aggregated to form the coating film 10 having the silica fine particle layer 11 as shown in FIG.
[0067] As a method for drying the coating composition, it is important not to cause temperature unevenness on the surface of the coated liquid film 10A. After application, it is preferable to allow the coating composition to dry naturally. When accelerating the drying with an airflow, it is preferable not to use an airflow that is 15°C or more higher than the temperature of the substrate 20. When an airflow that is 15°C or more higher than the temperature of the substrate 20 is used, temperature unevenness occurs on the surface of the coated liquid film 10A, and unevenness also occurs in the coating film 10 obtained after drying. The speed of the airflow is not particularly limited, but is preferably 25 m / sec or less. If the speed of the airflow exceeds 25 m / sec, the liquid film 10A before drying may be disturbed, and a uniform coating film 10 may not be obtained.
[0068] In the first embodiment, the coating composition contains silica fine particles, metal oxide fine particles, a high boiling point solvent, and water. The average particle size of the silica fine particles is 3 nm or more and 25 nm or less, and the content of the silica fine particles in the coating composition is 0.1 mass % or more and 5 mass % or less. The boiling point of the high boiling point solvent is 150° C. or more and 300° C. or less, and the content of the high boiling point solvent in the coating composition is 20 mass % or more and 70 mass % or less. As a result, when an organic matter that causes clouding due to the fogging phenomenon adheres to the coating film formed by the coating composition of the first embodiment, the organic matter penetrates the silica fine particles, so that the clouding is quickly eliminated and transparency can be maintained. In addition, since the metal oxide fine particles are contained, even if the absorption of the organic matter 18 is uneven, visibility is not affected and high transparency is maintained.
[0069] Embodiment 2 In the second embodiment, a case where a coating film is formed on an optical device, which is an article, using the coating composition described in the first embodiment, is described. Figs. 7 to 14 are diagrams showing an example of an optical device having a coating film according to the second embodiment. Among these, Figs. 7 to 12 show headlights 40, 50, and 60 as examples of optical devices. Also, Figs. 13 and 14 show a camera 100 as an example of an optical device. Fig. 7 is a front view of a headlight 40 having a reflector, which shows an example of an optical device having a coating film according to the second embodiment, and Fig. 8 is a cross-sectional view taken along line AA in Fig. 7. Also, Fig. 9 is a front view of a headlight 50 having a lens and an outer, which shows an example of an optical device having a coating film according to the second embodiment, and Fig. 10 is a cross-sectional view taken along line BB in Fig. 9. Also, Fig. 11 is a front view of a headlight 60, which shows an example of an optical device having a coating film according to the second embodiment, and Fig. 12 is a cross-sectional view taken along line CC in Fig. 11. Also, FIG. 13 is a front view of a camera 100 showing an example of an optical device having a coating film according to the second embodiment, and FIG. 14 is a DD cross-sectional view of FIG.
[0070] As shown in Figs. 7 to 14, the headlight has light sources 43, 53, and 63. Other configurations include a headlight 40 having a reflector 41 inside an outer 42 that covers the light source, a headlight 50 in which a lens 54 is covered by an outer 52, and a headlight 60 in which a lens 64 is exposed without an outer 52. Since the headlight is sealed and heated to high temperatures, organic matter may volatilize from the components inside the headlight, causing fogging due to the fogging phenomenon in which the inside of the outer 52 and the lens surface become cloudy. Therefore, by forming a coating film 10 on the inside of the outer 52 and the lens surface that constitute the headlight, transparency can be maintained without causing fogging due to the fogging phenomenon.
[0071] Moreover, by forming the coating film 10 on the outside of the outer layer or on the surface of the exposed lens, a hydrophilic effect can be obtained. When water droplets adhere to the surface, the water droplets act as lenses, which may change the light distribution value. If the surface is hydrophilic, the water spreads and does not form droplets, so the light distribution value can be maintained. Furthermore, by forming a coating film on the outside of the outer layer or on the surface of the exposed lens, an anti-soiling effect can be obtained, and changes in the light distribution value due to dirt can be prevented. Furthermore, by adjusting the thickness of the coating film so that it has an anti-reflection function, the transmittance of the member to which the coating film is applied can also be improved.
[0072] Camera 100 includes camera body 111 and lens 112 in housing 110. When camera 100 is used indoors or outdoors, dirt may adhere to the surface of lens 112. By forming coating film 10 described in the first embodiment on the surface of lens 112, it is possible to prevent dirt from adhering for a long period of time without affecting the image captured by camera 100.
[0073] In the second embodiment, a coating film 10 is formed on the lens 112 of the camera 100. The coating film 10 has higher transparency than conventional coating films, so that the light collecting performance of the lens 112 can be expected to be equivalent to that before the coating film 10 is applied. In addition, by adjusting the film thickness of the coating film 10 so that it has an anti-reflection function, the transmittance of the lens 112 to which the coating film 10 is applied can also be improved.
[0074] Embodiment 3 In the third embodiment, a coating film is formed on a lighting device, which is an article, using the coating composition described in the first embodiment. Fig. 15 is a front view showing an example of a lighting device having a coating film according to the third embodiment, and Fig. 16 is an E-E cross-sectional view of Fig. 15. In the third embodiment, the lighting device 200 includes a main body 210 that emits light, and a lighting cover 211 that covers the main body 210.
[0075] In the lighting device 200, pyrolysis products and compounds from the components may volatilize and adhere to the inside of the lighting cover 211, causing clouding due to the fogging phenomenon. In addition, volatile organic substances in the environment may adhere to the outside of the lighting cover 211, causing clouding due to the fogging phenomenon. By forming a coating film made of the coating composition described in the first embodiment on the inside and outside of the lighting cover 211, the occurrence of clouding can be suppressed and transparency can be maintained for a long period of time. In addition, by forming a coating film made of the coating composition described in the first embodiment on the outside of the lighting cover 211, an anti-fouling effect against dust and the like from the outside can also be obtained. EXAMPLES
[0076] The present disclosure will be described in detail below with reference to examples and comparative examples, but the present disclosure is not limited thereto.
[0077] <Method for preparing coating composition and method for forming coating film> [Example 1] A coating composition is prepared by blending colloidal silica containing silica particles with an average particle size of 12 nm (Nissan Chemical Industries, Ltd., NH4+ stable alkaline sol, ST-N), tin oxide sol containing tin oxide particles, which are metal oxide particles with an average particle size of 2 nm (Taki Chemical Industry Co., Ltd., Ceramace S-8), diethylene glycol monobutyl ether with a boiling point of 230°C as a high boiling point solvent, and deionized water as water, and mixing and stirring the mixture. In this coating composition, the content of silica particles is 1 mass%, the content of tin oxide particles is 0.2 mass%, the content of diethylene glycol monobutyl ether is 50 mass%, and the content of deionized water is the remainder.
[0078] The obtained coating composition is impregnated into a nonwoven fabric (manufactured by Kuraray Kuraflex Co., Ltd., product name: Kuraclean (registered trademark) Wiper, fiber used: rayon) and fixed to a polycarbonate block. The nonwoven fabric surface is brought into close contact with a glass substrate (50 mm x 50 mm x 1 mm) and slid thereon, and then dried at 25°C for 24 hours to form a coating film.
[0079] [Example 2] A coating composition is prepared in the same manner as in Example 1, except that the content of the high boiling point solvent, diethylene glycol monobutyl ether, is changed to 20 mass %. A coating film is formed on a glass substrate in the same manner as in Example 1.
[0080] [Example 3] A coating composition is prepared in the same manner as in Example 1, except that the content of the high boiling point solvent, diethylene glycol monobutyl ether, is changed to 21 mass %. A coating film is formed on a glass substrate in the same manner as in Example 1.
[0081] [Example 4] The content of the high boiling point solvent diethylene glycol monobutyl ether 55 Except for changing the mass %, a coating composition is prepared in the same manner as in Example 1. Also, a coating film is formed on a glass substrate in the same manner as in Example 1.
[0082] [Example 5] A coating composition is prepared in the same manner as in Example 1, except that the content of the high boiling point solvent, diethylene glycol monobutyl ether, is changed to 69 mass %. A coating film is formed on a glass substrate in the same manner as in Example 1.
[0083] [Example 6] A coating composition is prepared in the same manner as in Example 1, except that the content of the high boiling point solvent, diethylene glycol monobutyl ether, is changed to 70 mass %. A coating film is formed on a glass substrate in the same manner as in Example 1.
[0084] [Example 7] A coating composition is prepared in the same manner as in Example 1, except that dipropylene glycol dimethyl ether having a boiling point of 171° C. is used instead of the high boiling point solvent diethylene glycol monobutyl ether. A coating film is formed on a glass substrate in the same manner as in Example 1.
[0085] [Example 8] A coating composition is prepared in the same manner as in Example 1, except that the content of the silica fine particles is changed to 0.2 mass %. A coating film is formed on a glass substrate in the same manner as in Example 1.
[0086] [Example 9] Except for changing the content of silica fine particles to 4 mass %, a coating composition is prepared in the same manner as in Example 1. Also, a coating film is formed on a glass substrate in the same manner as in Example 1.
[0087] [Example 10] Except for changing the average particle size of the silica fine particles to 5 nm, a coating composition is prepared in the same manner as in Example 1. A coating film is formed on a glass substrate in the same manner as in Example 1.
[0088] [Example 11] A coating composition is prepared in the same manner as in Example 1, except that the average particle size of the silica fine particles is changed to 20 nm. A coating film is formed on a glass substrate in the same manner as in Example 1.
[0089] [Example 12] A coating composition is prepared in the same manner as in Example 1, except that the content of the tin oxide fine particles is changed to 0.7 mass %. A coating film is formed on a glass substrate in the same manner as in Example 1.
[0090] [Example 13] A coating composition is prepared in the same manner as in Example 1, except that the tin oxide sol is changed to a zirconium oxide dispersion liquid (Sakai Chemical Industry Co., Ltd., SZR-GCW) containing zirconium oxide with an average particle size of 10 nm. A coating film is formed on a glass substrate in the same manner as in Example 1.
[0091] [Example 14] A coating composition is prepared in the same manner as in Example 1, except that the tin oxide sol is replaced with a cerium oxide sol having an average particle size of 8 nm (Taki Chemical Industry Co., Ltd., B-10). A coating film is formed on a glass substrate in the same manner as in Example 1.
[0092] [Example 15] A coating composition is prepared in the same manner as in Example 1, except that PTFE particles (manufactured by Mitsui DuPont Fluorochemicals Co., Ltd., product name: 31JR) are added as fluororesin particles in an amount of 10 mass% relative to the silica fine particles. The average particle size of the PTFE particles is 0.25 μm. A coating film is formed on a glass substrate in the same manner as in Example 1.
[0093] [Example 16] A coating composition is prepared in the same manner as in Example 1, except that PTFE particles (manufactured by DuPont-Mitsui Fluorochemicals Co., Ltd., product name: 31JR) are added as fluororesin particles in an amount of 40 mass% relative to the silica fine particles. The average particle size of the PTFE particles is 0.25 μm. A coating film is formed on a glass substrate in the same manner as in Example 1.
[0094] [Example 17] A coating composition is prepared in the same manner as in Example 1, except that polyethylene glycol (manufactured by Tokyo Chemical Industry Co., Ltd., product name: Polyethylene Glycol 400) is added as a non-volatile hydrophilic organic substance in an amount of 15 mass% relative to the silica fine particles. The average molecular weight of the polyethylene glycol is 380 or more and 420 or less. A coating film is formed on a glass substrate in the same manner as in Example 1.
[0095] [Example 18] A coating composition is prepared in the same manner as in Example 1, except that polyethylene glycol (manufactured by Tokyo Chemical Industry Co., Ltd., product name: polyethylene glycol 400) is added as a non-volatile hydrophilic organic substance in an amount of 35 mass% relative to the silica fine particles. The average molecular weight of the polyethylene glycol is 380 or more and 420 or less. A coating film is formed on a glass substrate in the same manner as in Example 1.
[0096] [Example 19] A coating film is formed in the same manner as in Example 1, except that the coating composition of Example 1 is applied to an acrylic substrate (ABS (Acrylonitrile Butadiene Styrene), 50 mm×50 mm×2 mm).
[0097] [Example 20] The coating composition of Example 1 is spray-coated onto a glass substrate (50 mm×50 mm×1 mm) and then dried at 25° C. for 24 hours to form a coating film.
[0098] [Comparative Example 1] A coating composition is prepared in the same manner as in Example 1, except that the content of the high boiling point solvent, diethylene glycol monobutyl ether, is changed to 15 mass %. A coating film is formed on a glass substrate in the same manner as in Example 1.
[0099] [Comparative Example 2] A coating composition is prepared in the same manner as in Example 1, except that the content of the high boiling point solvent, diethylene glycol monobutyl ether, is changed to 19 mass %. A coating film is formed on a glass substrate in the same manner as in Example 1.
[0100] [Comparative Example 3] A coating composition is prepared in the same manner as in Example 1, except that the content of the high boiling point solvent, diethylene glycol monobutyl ether, is changed to 71 mass %. A coating film is formed on a glass substrate in the same manner as in Example 1.
[0101] [Comparative Example 4] A coating composition is prepared in the same manner as in Example 1, except that the content of the high boiling point solvent, diethylene glycol monobutyl ether, is changed to 75 mass %. A coating film is formed on a glass substrate in the same manner as in Example 1.
[0102] [Comparative Example 5] A coating composition is prepared in the same manner as in Example 1, except that ethanol having a boiling point of 87° C. is used instead of the high boiling point solvent diethylene glycol monobutyl ether. A coating film is formed on a glass substrate in the same manner as in Example 1.
[0103] [Comparative Example 6] A coating composition is prepared in the same manner as in Example 1, except that lithium silicate (manufactured by Nissan Chemical Industries, Ltd., product name: Lithium Silicate 45) is used instead of silica fine particles. A coating film is formed on a glass substrate in the same manner as in Example 1.
[0104] [Comparative Example 7] A coating composition is prepared in the same manner as in Example 1, except that the average particle diameter of the silica fine particles is changed to 30 nm. A coating film is formed on a glass substrate in the same manner as in Example 1.
[0105] [Comparative Example 8] Except for changing the content of the silica fine particles to 0.05% by mass, a coating composition is prepared in the same manner as in Example 1. A coating film is formed on a glass substrate in the same manner as in Example 1.
[0106] [Comparative Example 9] A coating composition is prepared in the same manner as in Example 1, except that the content of the silica fine particles is changed to 7 mass %. A coating film is formed on a glass substrate in the same manner as in Example 1.
[0107] [Comparative Example 10] A coating composition is prepared in the same manner as in Example 1, except that tin oxide fine particles are not added. A coating film is formed on a glass substrate in the same manner as in Example 1.
[0108] [Comparative Example 11] A coating composition is prepared in the same manner as in Example 1, except that PTFE particles (manufactured by DuPont-Mitsui Fluorochemicals Co., Ltd., product name: 31JR) are added as fluororesin particles in an amount of 60 mass% relative to the silica fine particles. The average particle size of the PTFE particles is 0.25 μm. A coating film is formed on a glass substrate in the same manner as in Example 1.
[0109] [Comparative Example 12] A coating composition is prepared in the same manner as in Example 1, except that polyethylene glycol (manufactured by Tokyo Chemical Industry Co., Ltd., product name: Polyethylene Glycol 400), which is a non-volatile hydrophilic organic substance, is added in an amount of 50 mass% relative to the silica fine particles. The average molecular weight of the polyethylene glycol is 380 or more and 420 or less. A coating film is formed on a glass substrate in the same manner as in Example 1.
[0110] <Coating film evaluation method> The coating films formed with the coating compositions of Examples 1 to 20 and Comparative Examples 1 to 12 were measured for thickness, and the transparency, fogging resistance, and appearance after a fogging test were evaluated, as well as the transparency and antifouling properties.
[0111] - Film thickness measurement A portion of the coating film formed on the substrate is scraped off, and a 3D measuring laser microscope (Olympus Corporation) is used to measure the height difference between the coating film and the substrate, thereby measuring the film thickness. The measurement results of the coating film thickness are classified according to the following criteria. 1: Film thickness less than 20 nm 2: Film thickness is 20 nm or more and 250 nm or less 3: Film thickness exceeds 250 nm
[0112] Transparency rating The clarity of the coating film is measured using Hazeguard i (manufactured by BYK). The clarity measurement results of the coating film are evaluated according to the following criteria, and a clarity of 90% or more is considered to be highly transparent. 1: Clarity of 95% or more 2: Clarity is less than 95% and more than 90% 3: Clarity less than 90%
[0113] -Fogging resistance evaluation 1 mL of bis(2-ethylhexyl) phthalate was placed in a glass bottle with a diameter of 9 cm and a height of 19 cm, and the mouth of the glass bottle was covered with the coated sample plate. After heating the bottom of the glass bottle in a water bath at 80°C for 30 minutes, the haze of the sample plate was measured using Haze Guard i (manufactured by BYK) and compared with the initial value before the fogging test. A difference in haze value ΔHaze of less than 4 is considered to have high fogging resistance. 1: ΔHaze is less than 2 2: ΔHaze is 3 or more and less than 7 3: ΔHaze is 7 or more
[0114] Appearance evaluation after fogging test Using Hazeguard i (manufactured by BYK), measure the clarity of the coating film after the fogging test. The measurement results of the clarity of the coating film are evaluated according to the following criteria, and a clarity of 90% or more is considered to be highly transparent. 1: Clarity of 95% or more 2: Clarity is less than 95% and more than 90% 3: Clarity is less than 90% or more
[0115] ·Evaluation of stain resistance The antifouling performance is evaluated by the adhesion of sand dust, which is a hydrophilic fouling substance, to the coating film. Specifically, Kanto loam dust, a JIS (Japanese Industrial Standards) test powder with a median particle size in the range of 1 μm to 3 μm, is blown onto the coating film with air under conditions of a temperature of 25°C and humidity of 50%. The Kanto loam dust blown onto the coating film is then transferred to a mending tape (manufactured by Sumitomo 3M Limited). The absorbance at a wavelength of 550 nm is measured using a spectrophotometer (manufactured by Shimadzu Corporation, product name: UV-3100PC) for another transparent substrate to which the tape with the transferred dust has been attached. The absorbance is evaluated according to the following criteria, and an absorbance of less than 0.3 is considered to have high antifouling properties. 1: Absorbance less than 0.2 2: Absorbance is 0.2 or more and less than 0.3 3: Absorbance of 0.3 or more
[0116] FIG. 17 is a diagram summarizing the evaluation results of Examples 1 to 20 and Comparative Examples 1 to 12. As shown in FIG. 17, in the coating compositions of Examples 1 to 14, the average particle size of the silica fine particles is in the range of 3 nm to 25 nm, and the content of the silica fine particles in the coating composition is in the range of 0.1 mass % to 5 mass %. In addition, the coating compositions of Examples 1 to 14 contain metal oxide fine particles. In addition, in the coating compositions of Examples 1 to 14, the boiling point of the high boiling point solvent is in the range of 150° C. to 300° C., and the content of the high boiling point solvent in the coating composition is in the range of 20 mass % to 70 mass %. Therefore, the coating films formed using these coating compositions have good transparency, fogging resistance, transparency after fogging test, and antifouling properties.
[0117] In addition, the coating compositions of Examples 15 and 16 contain fluororesin particles in a range of 5% by mass to 50% by mass relative to the silica fine particles, and therefore have good transparency, fogging resistance, appearance evaluation after fogging test, and antifouling properties.Similarly, the coating compositions of Examples 17 and 18 contain non-volatile hydrophilic organic substances in a range of 10% by mass to 40% by mass relative to the silica fine particles, and therefore have good transparency, fogging resistance, transparency after fogging test, and antifouling properties.
[0118] Furthermore, the coating film formed on the acrylic substrate in Example 19 and the coating film formed by spray application in Example 20 also have good transparency, fogging resistance, appearance evaluation after fogging test, and antifouling properties. That is, the coating film has good transparency, fogging resistance, transparency after fogging test, and antifouling properties whether the substrate is glass or acrylic. The transparency, fogging resistance, transparency after fogging test, and antifouling properties are good whether the coating film is formed by application using a nonwoven fabric or by spray application.
[0119] In contrast, in Comparative Examples 1 and 2, the evaluations of transparency, transparency after the fogging test, and antifouling property are low. This is believed to be because the amount of high-boiling point solvent added is insufficient, and therefore the effect of forming a uniform film is not sufficiently obtained. In Comparative Examples 3 and 4, the evaluations of transparency, transparency after the fogging test, and antifouling property are low. This is believed to be because the amount of high-boiling point solvent added is excessive, which reduces the dispersibility of silica fine particles and metal oxide, and increases the unevenness of the surface of the coating film.
[0120] In Comparative Example 5, the evaluations of transparency, fogging resistance, transparency after fogging test, and antifouling are low. This is thought to be because the boiling point of ethanol used as a solvent is 87°C, which is lower than the boiling points of other high boiling point solvents. In Comparative Example 6, a dense film is formed, so the evaluations of transparency, fogging resistance, transparency after fogging test, and antifouling are low. In Comparative Example 7, the particle size of the silica fine particles is too large, so the evaluations of transparency, transparency after fogging test, and antifouling are low. In Comparative Example 8, the addition amount of silica fine particles is small, so a thin film is formed, so the evaluations of fogging resistance, transparency after fogging test, and antifouling are low. In Comparative Example 9, the addition amount of silica fine particles is large, so a thick film is formed, so the evaluations of transparency, transparency after fogging test, and antifouling are low. In Comparative Example 10, the evaluation of transparency after fogging test is low. This is because the coating film does not contain metal oxide, and unevenness is noticeable when organic matter causing fogging penetrates. In Comparative Example 11, the evaluations of transparency and transparency after fogging test are low. This is believed to be because the amount of fluororesin particles added is excessive, which causes the unevenness to increase and the surface to become cloudy. In Comparative Example 12, the evaluations of fogging resistance, transparency after the fogging test, and antifouling properties are low. This is because the amount of non-volatile hydrophilic organic matter added is excessive, which reduces the penetration effect of the organic matter that causes fogging, and makes it easier for dirt to adhere.
[0121] <Examples of applying a coating composition to an article> [Example 21] The coating composition of Example 1 was impregnated into a nonwoven fabric (manufactured by Kuraray Kuraflex Co., Ltd., product name: Kuraclean Wiper, fiber used: rayon), and applied by sliding it against the inside of the outer casing of a headlight, and then allowed to dry naturally at 25°C for 24 hours to form a coating film.
[0122] [Example 22] The coating composition of Example 1 is sprayed onto the inside of a glass lighting cover and allowed to dry naturally at 25° C. for 24 hours.
[0123] In Examples 21 and 22, the coating films were formed on the respective substrates, but there was no change in the appearance of the substrates. That is, the coating films formed in Examples 21 and 22 have high transparency.
[0124] 1 mL of bis(2-ethylhexyl) phthalate is placed in a glass bottle with a diameter of 9 cm and a height of 19 cm, the cut substrate is fixed to the top of the glass bottle, and the glass bottle is sealed. The bottom of the glass bottle is heated in a water bath at 80°C for 30 minutes, and then the haze of the substrate is measured. When the haze was measured using Haze Guard i (manufactured by Big Gardner Co., Ltd.), it was found to be 5% or less, indicating high fogging resistance. In addition, under conditions of a temperature of 25°C and a humidity of 50%, Kanto loam dust, which is a JIS test powder with a median particle size in the range of 1 μm to 3 μm, is blown onto each of the articles with the coating films of Examples 21 and 22 with air, and then each article is lightly vibrated. As a result, dust falls from each of the articles with the coating films of Examples 21 and 22 formed thereon, indicating that the coating films formed in Examples 21 and 22 have high antifouling properties.
[0125] The configurations shown in the above embodiments are merely examples, and may be combined with other known technologies, or the embodiments may be combined with each other. Also, parts of the configurations may be omitted or modified without departing from the spirit of the invention. [Explanation of symbols]
[0126] 10 coating film, 10A liquid film, 11 silica fine particle layer, 12 fluororesin particles, 13 cracks, 14 non-volatile hydrophilic organic matter, 15 silica fine particles, 16 solvent, 17 metal oxide fine particles, 18 organic matter causing fogging, 20 substrate, 21b part of film made of silica fine particles only that has absorbed organic matter, 21c part of coating film that has absorbed organic matter, 22b part of film made of silica fine particles only that has not absorbed organic matter, 22c part of coating film that has not absorbed organic matter, 30 block, 31 cloth-like material, 40 headlight having reflector, 41 reflector, 42, 52 outer, 43, 53, 63 light source, 50 headlight having lens and outer, 54, 64 lens, 60 headlight having lens, 100 camera, 110, 310 housing, 111 camera body, 112 lens, 200 Lighting equipment, 210 main body, 211 lighting cover.
Claims
1. Silica fine particles having an average particle size of 3 nm or more and 25 nm or less; Metal oxide fine particles, A solvent having a boiling point of 150° C. or more and 300° C. or less; Water, Including, The content of the silica fine particles is 0.1% by mass or more and 5% by mass or less, The content of the solvent is 20% by mass or more and 70% by mass or less, The content of the metal oxide fine particles is 2% by mass or more and 80% by mass or less based on the silica fine particles, The average particle size of the metal oxide particles is 1 nm or more and 25 nm or less. A coating composition comprising:
2. 2. The coating composition according to claim 1, further comprising fluororesin particles in an amount of 5% by mass to 50% by mass based on the silica fine particles.
3. 3. The coating composition according to claim 1, further comprising a non-volatile hydrophilic organic substance, the content of which is 10% by mass or more and 40% by mass or less relative to the silica fine particles.
4. A coating film formed on a substrate by the coating composition according to claim 1, A coating film comprising a silica fine particle layer disposed on the substrate and formed by agglomeration of the silica fine particles and the metal oxide fine particles.
5. A coating film formed on a substrate by the coating composition according to claim 2, a silica fine particle layer disposed on the substrate and formed by agglomerating the silica fine particles and the metal oxide fine particles; The coating film is characterized in that the fluororesin particles are partially exposed on the surface of the coating film and are disposed in a dispersed state in the silica fine particle layer.
6. A coating film formed on a substrate by the coating composition according to claim 3, a silica fine particle layer disposed on the substrate and formed by agglomerating the silica fine particles and the metal oxide fine particles; A coating film, characterized in that the non-volatile hydrophilic organic material is filled into defects in the silica fine particle layer.
7. 7. The coating film according to claim 4, wherein the thickness of the coating film is from 20 nm to 250 nm.
8. 7. The coating film according to claim 4, wherein the surface of the substrate has a 60° specular gloss of 50 or more.
9. An article comprising the coating film according to any one of claims 4 to 8.
10. 9. An optical device comprising an outer layer, the optical device comprising the coating film according to claim 4 on one or both of the outer and inner surfaces of the outer layer.
11. 9. An optical device comprising a lens, the optical device comprising the coating film according to claim 4 on a surface of the lens.
12. A lighting device comprising a lighting cover, the lighting device being provided with the coating film according to any one of claims 4 to 8 on one or both of an outer surface and an inner surface of the lighting cover.
Citation Information
Patent Citations
Formula of antifog pad pasting for automobile glass and preparation process thereof
CN108329856A
Glass
JP1997235140A
Hydrophilic stain-proof coating composition, method for forming coating film using the same and use using the same
JP2006265462A
Coating composition imparting antifouling properties, coated article using the coating composition, and method of manufacturing the coated article
JP2011246603A
Coating composition and production method therefor, and antifouling porous article and production method therefor
JP2013032421A