Trivalent chromium plating solution and trivalent chromium plating method

A trivalent chromium plating solution with specific components and a plating method improves film hardness, wear resistance, and current efficiency, addressing environmental concerns and enhancing the performance of trivalent chromium plating.

JP7566250B2Active Publication Date: 2024-10-15OKUNO CHEM IND CO LTD +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020118275
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-07-12
Filing Date
2020-07-09
Publication Date
2024-10-15
Estimated Expiration
2040-07-09

AI Technical Summary

Technical Problem

Existing trivalent chromium plating solutions lack sufficient hardness, wear resistance, and current efficiency, and do not adequately address environmental concerns associated with hexavalent chromium plating.

Method used

A trivalent chromium plating solution containing trivalent chromium ions, metal halides, boron compounds, and dispersants, with a metal halide concentration of 2 mol/L or more, and a plating method using a soluble anode to form a trivalent chromium plating film with improved appearance, hardness, and wear resistance.

Benefits of technology

The solution achieves a trivalent chromium plating film with excellent appearance, hardness, and wear resistance, while maintaining high current efficiency and reducing environmental impact by minimizing impurity contamination and hydrogen generation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007566250000011
    Figure 0007566250000011
  • Figure 0007566250000012
    Figure 0007566250000012
  • Figure 0007566250000013
    Figure 0007566250000013
Patent Text Reader

Abstract

To provide a trivalent chromium plating solution that can form a trivalent chromium plating film having excellent plating film appearance and having excellent hardness and wear resistance, and that is excellent in current efficiency.SOLUTION: Provided is a trivalent chromium plating solution characterized by containing (A) trivalent chromium ion, (B) at least one metal halide selected from the group consisting of alkali metal halide and alkaline earth metal halide, (C) a boron compound and (D) at least one dispersant selected from the group consisting of glycol, water-soluble polymer, anionic surfactant, amphoteric surfactant and fluorine-based surfactant, and in which the contained amount of the metal halide is 2 mol / L or more.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a trivalent chromium plating solution and a trivalent chromium plating method. [Background technology]

[0002] Chrome plating, which has high hardness and excellent corrosion resistance, wear resistance, etc., is widely used for automobile parts, molding dies, rolling rolls, printing rolls, etc. In particular, chrome plating called hard chrome plating is used for applications such as molding dies and rolls. Chrome plating used for the above applications is required to have excellent appearance of the plating film.

[0003] Conventionally, a hexavalent chromium plating solution containing hexavalent chromium has been used as a chromium plating solution for carrying out chromium plating.

[0004] However, in recent years, there have been concerns about the environmental impact of using harmful hexavalent chromium plating solutions, and alternative technologies to hexavalent chromium plating solutions are being considered.

[0005] For this reason, the use of a trivalent chromium plating bath containing trivalent chromium, which has a lower environmental impact than hexavalent chromium, has been considered (see, for example, Patent Document 1).

[0006] However, the hardness and abrasion resistance of the plating film formed are not fully discussed in Patent Document 1. The trivalent chromium plating film formed using a trivalent chromium plating solution tends to have inferior abrasion resistance to the hexavalent chromium plating film formed using a hexavalent chromium plating solution, and there is a demand for improvement in abrasion resistance.

[0007] Furthermore, Patent Document 1 does not consider the current efficiency of the trivalent chromium plating solution. Depending on the application, thick plating may be required for trivalent chromium plating, and a high deposition rate is required. For this reason, it is desirable for the trivalent chromium plating solution to exhibit high current efficiency.

[0008] Therefore, there is a need for the development of a trivalent chromium plating solution that is excellent in current efficiency and that can form a trivalent chromium plating film that has excellent appearance, hardness, and abrasion resistance, and a trivalent chromium plating method that uses the trivalent chromium plating solution. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] International Publication No. 2015 / 037391 Summary of the Invention [Problem to be solved by the invention]

[0010] The present invention aims to provide a trivalent chromium plating solution capable of forming a trivalent chromium plating film having excellent appearance, hardness and abrasion resistance, and having excellent current efficiency. The present invention also aims to provide a trivalent chromium plating method capable of forming a trivalent chromium plating film having excellent appearance, hardness and abrasion resistance, and having excellent current efficiency. [Means for solving the problem]

[0011] As a result of extensive research, the present inventors have found that the above object can be achieved by a trivalent chromium plating solution containing the above components (A) to (D) and having a content of the metal halide as component (B) of 2 mol / L or more. The present inventors have also found that the above object can be achieved by a trivalent chromium plating method using the above trivalent chromium plating solution, the method including a step of immersing an object to be plated as a cathode in the trivalent chromium plating solution and an anode in the same to perform electrolytic plating, and have completed the present invention.

[0012] That is, the present invention relates to the following trivalent chromium plating solution and trivalent chromium plating method. 1. (A) Trivalent chromium ion, (B) at least one metal halide selected from the group consisting of alkali metal halides and alkaline earth metal halides; (C) a boron compound, and (D) At least one dispersant selected from the group consisting of glycols, water-soluble polymers, anionic surfactants, amphoteric surfactants, and fluorosurfactants. Including, The content of the metal halide is 2 mol / L or more; 1. A trivalent chromium plating solution comprising: 2. The trivalent chromium plating solution according to item 1, wherein the content of the metal halide is 4 mol / L or more. 3. The trivalent chromium plating solution according to item 1 or 2, wherein the metal halide is at least one selected from the group consisting of calcium chloride and lithium chloride. 4. The trivalent chromium plating solution according to any one of items 1 to 3, wherein the boron compound is at least one selected from the group consisting of boric acid, a borate salt, and boron oxide. 5. The trivalent chromium plating solution according to any one of Items 1 to 4, wherein the content of the boron compound is 5 to 100 g / L. 6. The trivalent chromium plating solution according to any one of items 1 to 5, wherein the dispersant is a water-soluble polymer. 7. The trivalent chromium plating solution according to any one of items 1 to 6, wherein the content of the dispersant is 0.01 to 100 g / L. 8. (A) Trivalent chromium ion, (B) at least one metal halide selected from the group consisting of alkali metal halides and alkaline earth metal halides; (C) a boron compound, and (D) At least one dispersant selected from the group consisting of glycols, water-soluble polymers, anionic surfactants, amphoteric surfactants, and fluorosurfactants. The method includes a step of immersing an object to be plated as a cathode in a trivalent chromium plating solution containing the above-mentioned, and also immersing an anode in the solution to perform electrolytic plating, The content of the metal halide in the trivalent chromium plating solution is 2 mol / L or more. A trivalent chromium plating method comprising the steps of: 9. The trivalent chromium plating method according to item 8, wherein the anode is a soluble anode containing metallic chromium. Effect of the Invention

[0013] The trivalent chromium plating solution of the present invention can form a trivalent chromium plating film having excellent appearance, hardness and abrasion resistance, and can exhibit excellent current efficiency. The trivalent chromium plating method of the present invention uses the above-mentioned trivalent chromium plating solution, can form a trivalent chromium plating film having excellent appearance, hardness and abrasion resistance, and exhibits excellent current efficiency. [Brief description of the drawings]

[0014] [Figure 1] FIG. 2 is a cross-sectional photograph of the trivalent chromium plating film of Example 1. [Diagram 2] FIG. 2 is a cross-sectional photograph of the hexavalent chromium plating film of Comparative Example 1. [Diagram 3] FIG. 2 is a cross-sectional photograph of the trivalent chromium plating film of Comparative Example 2. [Figure 4] FIG. 1 is a cross-sectional photograph of a trivalent chromium plating film of Comparative Example 3. [Diagram 5] FIG. 1 is a cross-sectional photograph of a trivalent chromium plating film of Comparative Example 4. [Figure 6] FIG. 2 is a schematic diagram showing an example of a trivalent chromium plating method using the trivalent chromium plating solution of Example 21. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] 1. Trivalent chromium plating solution The trivalent chromium plating solution of the present invention contains (A) trivalent chromium ions, (B) at least one metal halide selected from the group consisting of alkali metal halides and alkaline earth metal halides, (C) a boron compound, and (D) at least one dispersant selected from the group consisting of glycols, water-soluble polymers, anionic surfactants, amphoteric surfactants, and fluorosurfactants, and the content of the metal halide is 2 mol / L or more.

[0016] In conventional plating solutions, complexing agents have been added to obtain sufficient solubility of metals in the plating solution, but the addition of complexing agents causes contamination with nitrogen, carbon, sulfur, etc., resulting in reduced productivity and reduced quality of plated products, and making it difficult to manage the plating solution.

[0017] In addition, when plating is performed using conventional plating solutions, side reactions such as hydrogen generation may occur. As a result, the amount of electricity (current efficiency) used in the main reaction of producing the plated product decreases, resulting in a decrease in productivity of the plated product. In particular, in chromium plating, the absorbed hydrogen is a direct cause of cracking, which affects the quality of the plating film of the plated product obtained.

[0018] The trivalent chromium plating solution of the present invention contains components (A), (B), (C) and (D), and therefore can contain at least one metal halide selected from the group consisting of alkali metal halides and alkaline earth metal halides, which is component (B), at a high concentration of 2 mol / L or more, and can be used as a plating solution without using a complexing agent. The trivalent chromium plating solution of the present invention does not need to contain a complexing agent, so that the inclusion of impurities such as nitrogen, carbon and sulfur is suppressed, and therefore the plating film has an excellent appearance, and a trivalent chromium plating film having excellent hardness and abrasion resistance can be formed, and excellent current efficiency can be exhibited.

[0019] The trivalent chromium plating solution of the present invention contains at least one metal halide selected from the group consisting of alkali metal halides and alkaline earth metal halides, which is the component (B), at a high concentration of 2 mol / L or more. This allows the solvent molecules to coordinate with the metal ions and stabilize them, thereby suppressing side reactions such as hydrogen generation during the formation of a plating film, thereby improving the productivity of the plating film and reducing the impact on the quality of the plating film.

[0020] The trivalent chromium plating solution of the present invention further contains the components (C) and (D), thereby making it possible to improve the appearance of a trivalent chromium plating film and form a trivalent chromium plating film having excellent hardness and abrasion resistance.

[0021] The trivalent chromium plating solution of the present invention will be specifically described below.

[0022] 1. Trivalent chromium plating solution Component (A) The trivalent chromium plating solution of the present invention contains trivalent chromium ions as component (A). The trivalent chromium ions are present in the trivalent chromium plating solution by dissolving a trivalent chromium compound in a solvent contained in the trivalent chromium plating solution.

[0023] The trivalent chromium compound may be any trivalent chromium compound that is soluble in a solvent, such as chromium chloride, chromium sulfate, basic chromium sulfate, etc. Among these, chromium chloride is preferred because it is less likely to produce an insoluble salt. The trivalent chromium compound may be used alone or in combination of two or more.

[0024] The concentration of trivalent chromium ions is not particularly limited, but is preferably, for example, 2 to 100 g / L, and more preferably 5 to 70 g / L.

[0025] (B) Component The trivalent chromium plating solution of the present invention contains, as component (B), at least one metal halide selected from the group consisting of alkali metal halides and alkaline earth metal halides.

[0026] The alkali metal halide is not particularly limited, and examples thereof include chlorides and bromides of alkali metals. As the alkali metal halide, lithium chloride and lithium bromide are preferred, and lithium chloride is more preferred.

[0027] The alkaline earth metal halide is not particularly limited, and examples thereof include chlorides and bromides of alkaline earth metals. Examples of alkaline earth metal halides include calcium chloride. 、 Calcium bromide is preferred, and calcium chloride is more preferred.

[0028] As the metal halide, calcium chloride and lithium chloride can be preferably used, and calcium chloride can be more preferably used.

[0029] The above metal halides may be used alone or in combination of two or more.

[0030] The content of the metal halide in the trivalent chromium plating solution is 2 mol / L or more. If the content of the metal halide is less than 2 mol / L, the appearance of the plating film is poor, and the hardness and wear resistance are reduced. The content of the metal halide is preferably 4 mol / L or more, more preferably 4.2 mol / L or more. The content of the metal halide is preferably 18 mol / L or less, more preferably 15 mol / L or less, even more preferably 10 mol / L or less, and particularly preferably 7 mol / L or less. By setting the upper limit of the content of the metal halide within the above range, the generation of halogen gas such as chlorine gas during the formation of the trivalent chromium plating film can be further suppressed.

[0031] (C) Component The trivalent chromium plating solution of the present invention contains a boron compound as component (C).

[0032] The boron compound is not particularly limited, and examples thereof include boric acid, borates such as sodium borate and potassium borate, and boron oxide. Among these, boric acid and boron oxide are preferred because they are less likely to form insoluble salts. The boron compound may be used alone or in combination of two or more.

[0033] The concentration of the boron compound is not particularly limited, but is preferably 5 to 100 g / L, more preferably 10 to 90 g / L, even more preferably 10 to 80 g / L, and particularly preferably 20 to 80 g / L. When the content of the boron compound is within the above range, the appearance of the trivalent chromium plating film formed using the trivalent chromium plating solution is further improved, and the hardness and abrasion resistance are further improved.

[0034] (D) Component The trivalent chromium plating solution of the present invention contains at least one dispersant selected from the group consisting of glycols, water-soluble polymers, anionic surfactants, amphoteric surfactants, and fluorosurfactants as component (D). The dispersants may be used alone or in combination of two or more.

[0035] The glycols are not particularly limited, and examples thereof include alkyl glycols and derivatives thereof, such as ethylene glycol, propylene glycol, and diethylene glycol.

[0036] The trivalent chromium plating solution of the present invention preferably contains a water-soluble polymer as component (D). By containing a water-soluble polymer in the trivalent chromium plating solution of the present invention, the occurrence of pitting corrosion in the formed trivalent chromium plating film is suppressed, the appearance of the trivalent chromium plating film is further improved, and the hardness and wear resistance are further improved. Although not intended to be limited in interpretation, it is believed that one of the reasons why the water-soluble polymer exerts a pitting corrosion suppression effect is that it captures halide ions such as chloride ions that cause pitting corrosion.

[0037] The water-soluble polymer is not particularly limited as long as it can exhibit the above-mentioned functions. Examples of the water-soluble polymer include synthetic polymers such as polyalkylene glycol (e.g., polyethylene glycol, polypropylene glycol, polybutylene glycol), polyvinyl alcohol, polyethylene oxide, polyvinylpyrrolidone, polyamide, polyimide, polyoxyethylene alkyl ether, polyoxyethylene glycol-glyceryl ether, polyoxypropylene glycol-glyceryl ether, polyethylene glycol-polypropylene glycol block ether, polyoxyalkylene alkyl ether, polyoxyethylene alkyl glycol, polyoxypropylene alkyl glycol, polyoxyethylene oxypropylene glycol, polyoxyethylene nonylphenyl ether, polyacrylic acid, polymethacrylic acid, polyacrylamide, poly(2-hydroxy-2-oxo-1,3,2-dioxaphospholane) (PHP), and polymethacryloyloxyethyl phosphorylcholine; natural or semi-synthetic polymers such as proteins and polysaccharides (dextran, starch, cellulose, cellulose derivatives, etc.). Among these, synthetic polymers are preferable, polyalkylene glycol, polyoxyalkylene alkyl ether, polyvinyl alcohol, etc. are more preferable, polyalkylene glycol is further preferable, and polyethylene glycol and polypropylene glycol are further preferable.

[0038] The water-soluble polymer may be a copolymer formed of two or more types of constitutional units, such as a random copolymer, a block copolymer, or a graft copolymer.

[0039] The average molecular weight of the water-soluble polymer is preferably 200 to 20,000, more preferably 200 to 5,000, and even more preferably 200 to 2,000. The average molecular weight here may be either a number average molecular weight or a weight average molecular weight, and these average molecular weights can be measured by gel permeation chromatography (GPC) or the like.

[0040] The anionic surfactant is not particularly limited, and examples thereof include sodium alkyl sulfate, sodium polyoxyethylene alkyl ether sulfate, and dialkyl sulfosuccinic acid.

[0041] The amphoteric surfactant is not particularly limited, and examples thereof include alkyl dimethylamine oxide and alkyl carboxybetaine.

[0042] The fluorine-based surfactant is not particularly limited, and may be an anionic fluorine-based surfactant. As the fluorine-based surfactant, a commercially available product may be used. As a commercially available fluorine-based surfactant, for example, Futergent 110 (a fluorine-based anionic surfactant manufactured by Neos Co., Ltd.) may be used.

[0043] As the dispersant, glycols, polyethylene glycol, polypropylene glycol, polybutylene glycol, polyoxyethylene glycol-glyceryl ether, polyoxypropylene glycol-glyceryl ether, polyethylene glycol-polypropylene glycol block ether, polyoxyethylene alkyl ether, and polyoxyethylene alkyl ether sulfate sodium salt are preferred, and polyethylene glycol and polypropylene glycol are more preferred.

[0044] The concentration of the dispersant is not particularly limited, but is preferably 0.01 to 100 g / L, more preferably 0.1 to 50 g / L, even more preferably 0.1 to 30 g / L, and particularly preferably 0.1 to 20 g / L. When the content of the dispersant is within the above range, the appearance of the trivalent chromium plating film formed using the trivalent chromium plating solution is further improved, and the hardness and abrasion resistance are further improved.

[0045] (Other additives) The trivalent chromium plating solution of the present invention may contain additives other than the above-mentioned components (A) to (D), such as complexing agents, fluorides, conductive salts, chlorine generation inhibitors, precipitation accelerators, mist inhibitors, and pit inhibitors, which are used in ordinary trivalent chromium plating solutions.

[0046] The complexing agent is not particularly limited as long as it is a compound that has a complexing ability with trivalent chromium. As the complexing agent, a complexing agent that does not form an insoluble salt with calcium, such as a water-soluble carboxylic acid compound, is preferable. Examples of such complexing agents include formic acid, acetic acid, malonic acid, succinic acid, citric acid, glycine, and salts thereof.

[0047] As the fluoride, sodium fluoride, potassium fluoride, ammonium fluoride, boron fluoride, calcium fluoride, aluminum fluoride, etc. can be used.

[0048] As the conductive salt, a chloride salt such as sodium chloride, potassium chloride, ammonium chloride, aluminum chloride, magnesium chloride, barium chloride, etc. can be used.

[0049] As the chlorine generation inhibitor, bromides such as sodium bromide, potassium bromide, and ammonium bromide can be used.

[0050] As the deposition accelerator, sulfur compounds such as sodium saccharin, sodium dithionate, sodium thiosulfate, and sodium thiocyanate can be used.

[0051] Trivalent chromium plating solution The trivalent chromium plating solution of the present invention is prepared by dissolving the above-mentioned components (A) to (D) and, if necessary, other additives in a solvent, and the order in which each component is dissolved is arbitrary.

[0052] The solvent used in the trivalent chromium plating solution is not particularly limited as long as it can dissolve the above components (A) to (D), and for example, water can be used.

[0053] The pH of the trivalent chromium plating solution of the present invention is not particularly limited, but is preferably -2 to 4, and more preferably -1 to 2.

[0054] 2. Trivalent chromium plating method The trivalent chromium plating method of the present invention comprises the steps of: (A) trivalent chromium ion, (B) at least one metal halide selected from the group consisting of alkali metal halides and alkaline earth metal halides; (C) a boron compound, and (D) At least one dispersant selected from the group consisting of glycols, water-soluble polymers, anionic surfactants, amphoteric surfactants, and fluorosurfactants. The method includes a step of immersing an object to be plated as a cathode in a trivalent chromium plating solution containing the above-mentioned, and also immersing an anode in the solution to perform electrolytic plating, The method for trivalent chromium plating, wherein the content of the metal halide in the trivalent chromium plating solution is 2 mol / L or more.

[0055] In the trivalent chromium plating method of the present invention, by using the above-mentioned trivalent chromium plating solution of the present invention, it is possible to form a trivalent chromium plating film having excellent appearance, hardness and abrasion resistance, and exhibiting excellent current efficiency.

[0056] (Process) The trivalent chromium plating method of the present invention includes a step of immersing an object to be plated as a cathode in the above-mentioned trivalent chromium plating solution of the present invention, and also immersing an anode in the same, to perform electrolytic plating.

[0057] The anode is not particularly limited, and various insoluble or soluble anodes can be used.

[0058] Examples of insoluble anodes include carbon, Ti / Pt (Ti with a platinum-based coating), Ti / Ir oxide (Ti with an Ir oxide coating), Ti / Ru oxide (Ti with a Ru oxide coating), Ti / Ir oxide-Ru oxide (Ti with a mixed Ir oxide and Ru oxide coating), Ti / Ir oxide-Ta oxide (Ti with a mixed Ir oxide and Ta oxide coating), Ti / Pt / Ir oxide-Ru oxide (Ti / Pt with Ir oxide and Ta oxide coating), Examples of the electrode include a coating of Ti / Pt / Ir oxide-Ta oxide (Ti / Pt coated with Ir oxide and Ta oxide), stainless steel, aluminum, lead alloys (Pb-Sn alloy, Pb-Ag alloy, Pb-Sb alloy), lead oxide (lead monoxide, lead dioxide, lead trioxide, trilead tetroxide), lead, tin oxide, carbon, diamond electrodes (a substrate of silicon or niobium coated with diamond containing nitrogen or boron), and ITO electrodes (indium tin electrodes). Among these, carbon electrodes are preferred because of their excellent durability.

[0059] The soluble anode is not particularly limited, and it is preferable to use a soluble anode containing metallic chromium. In the trivalent chromium plating method of the present invention, a trivalent chromium plating solution containing 2 mol / L or more of metal halide is used as the trivalent chromium plating solution, which may easily generate halogen gas such as chlorine gas at the anode. However, when a soluble anode containing metallic chromium is used, metallic chromium (Cr 0 ) is trivalent chromium ion (Cr 3+ ), which makes it possible to further suppress the generation of halogen gas.

[0060] Metallic chromium used as a soluble anode is usually used as a metallic chromium electrode, and metallic chromium (Cr 0 ) is dissolved and trivalent chromium ions (Cr 3+The soluble anode is not particularly limited as long as it can produce the reaction: (1) Cr+Cr+H ...

[0061] In the trivalent chromium plating method of the present invention, the object to be plated is immersed as a cathode in the above-mentioned trivalent chromium plating solution. The object to be plated is not particularly limited, and examples thereof include metal materials such as iron, stainless steel, brass, and zinc die-casting used in the manufacture of dies, rolling rolls, printing rolls, etc.; and other metal materials such as nickel, aluminum, titanium, zirconium, and molybdenum. For such objects to be plated, thick plating of about 50 μm or more may be performed to form a trivalent chromium plating film.

[0062] The temperature of the trivalent chromium plating solution in the above step is preferably 20 to 70° C., and more preferably 30 to 60° C. When the lower limit of the temperature of the trivalent chromium plating solution is within the above range, the appearance, hardness, and abrasion resistance of the trivalent chromium plating film are further improved. Also, when the upper limit of the temperature of the trivalent chromium plating solution is within the above range, the throwing power of the trivalent chromium plating film is further improved.

[0063] The voltage applied during electrolytic plating may be appropriately set depending on the size of the object to be plated, and is preferably 1 to 50 V, more preferably 3 to 20 V. By setting the lower limit of the applied voltage within the above range, the appearance, hardness, and abrasion resistance of the trivalent chromium plating film are further improved, and the current efficiency is further improved. Also, by setting the upper limit of the applied voltage within the above range, the generation of halogen gas is further suppressed.

[0064] The applied current during electrolytic plating is preferably 0.1 to 5000 A, more preferably 1 to 1000 A. By setting the lower limit of the applied current value within the above range, the appearance, hardness, and abrasion resistance of the trivalent chromium plating film are further improved, and the current efficiency is further improved. Also, by setting the upper limit of the applied current within the above range, the generation of halogen gas is further suppressed.

[0065] The current density during electrolytic plating is not particularly limited and may be appropriately determined depending on the type of object to be plated. For example, it may be 1 to 20 A / dm 2 An appropriate current density range can be appropriately determined from the current density ranges.

[0066] The plating time in the above steps may be appropriately determined depending on the thickness of the desired trivalent chromium plating film, and is, for example, preferably 1 to 600 minutes, more preferably 2 to 300 minutes. When the lower limit of the voltage application time is within the above range, the trivalent chromium plating film is more sufficiently formed on the surface of the plated object, and the adhesion between the trivalent chromium plating film and the plated object is further improved. Also, when the upper limit of the voltage application time is within the above range, the plating appearance is further improved.

[0067] The anode / cathode area ratio in the above steps is not particularly limited and may be appropriately determined depending on the type of object to be plated. For example, an appropriate anode / cathode area ratio may be appropriately determined within the anode / cathode area ratio range of 0.5 to 3.

[0068] In the above process, the trivalent chromium plating solution may be stirred during electrolytic plating. The stirring method is not particularly limited, and examples thereof include bubbling stirring with air or nitrogen, circulating stirring with a pump, and stirring by rocking the object to be plated in the plating solution.

[0069] Through the steps described above, trivalent chromium plating is applied to the object to be plated, and an article having a trivalent chromium plating film formed thereon can be obtained.

[0070] The trivalent chromium plating method of the present invention may further include a washing step of washing the article on which the trivalent chromium plating film is formed with an alkaline solution. In the article on which the trivalent chromium plating film is formed, cracks may occur in the trivalent chromium plating film, or trivalent chromium plating solution may remain at the interface between the plated object and the trivalent chromium plating film, which may promote corrosion of the trivalent chromium plating film or the plated object. By including the washing step in the trivalent chromium plating method of the present invention, the remaining trivalent chromium plating solution can be removed, and the above-mentioned corrosion can be suppressed.

[0071] The alkaline compound contained in the alkaline solution used in the washing step is not particularly limited, and examples thereof include sodium hydroxide, potassium hydroxide, lithium hydroxide, calcium hydroxide, magnesium hydroxide, sodium carbonate, potassium carbonate, ammonium carbonate, sodium hydrogen carbonate, potassium hydrogen carbonate, ammonium hydrogen carbonate, and ammonia.

[0072] The method for cleaning the article on which the trivalent chromium plating film is formed is not particularly limited, and it is sufficient that the alkaline solution is brought into contact with the article on which the trivalent chromium plating film is formed. For example, there are a cleaning method in which the article on which the trivalent chromium plating film is formed is immersed in an alkaline solution, a method in which the article on which the trivalent chromium plating film is formed is sprayed with an alkaline solution, and the like.

[0073] The content of the alkaline compound in the alkaline solution is not particularly limited, and is preferably 0.01 to 10 mol / L, more preferably 0.1 to 7 mol / L, even more preferably 0.1 to 5 mol / L, and particularly preferably 1 to 5 mol / L. When the lower limit of the content of the alkaline compound is within the above range, the remaining trivalent chromium plating solution can be more effectively removed, and the corrosion of the article on which the trivalent chromium film is formed can be more effectively suppressed. In addition, when the upper limit of the content of the alkaline compound is within the above range, the adhesion of the alkaline compound to the article on which the trivalent chromium film is formed is suppressed, and the appearance of the trivalent chromium plating film is further improved.

[0074] The temperature of the alkaline solution is not particularly limited, and is preferably 20°C or higher, and more preferably 40°C or higher. When the lower limit of the alkaline solution temperature is within the above range, the remaining trivalent chromium plating solution can be more effectively removed, and the corrosion of the article on which the trivalent chromium film is formed can be more effectively suppressed. The upper limit of the alkaline solution temperature is not particularly limited as long as the evaporation of the alkaline solution can be suppressed, and is preferably 100°C or lower, more preferably 90°C or lower, and even more preferably 70°C or lower.

[0075] The cleaning time in the cleaning step is not particularly limited, and is preferably 1 minute or more, and more preferably 3 minutes or more. When the lower limit of the cleaning time is within the above range, the remaining trivalent chromium plating solution can be more effectively removed, and the corrosion of the article on which the trivalent chromium film is formed can be more effectively suppressed. The upper limit of the cleaning time is not particularly limited, and is preferably 30 minutes or less, and more preferably 15 minutes or less. When the upper limit of the cleaning time is within the above range, the adhesion of alkaline compounds to the article on which the trivalent chromium film is formed is suppressed, and the appearance of the trivalent chromium plating film is further improved.

[0076] 3. Articles on which a trivalent chromium plating film is formed by a trivalent chromium plating method By the above-described trivalent chromium plating method, an article having a trivalent chromium plating film formed thereon can be obtained. The article is not particularly limited, and an article that requires hardness, corrosion resistance, and abrasion resistance is preferable. Such articles include automobile parts, molding dies, various mechanical parts that are easily worn, tools, rolls used in printing, papermaking, rolling, film processing, and steelmaking, etc. EXAMPLES

[0077] The present invention will be specifically described below with reference to examples and comparative examples, but the present invention is not limited to the examples.

[0078] 1. Evaluation of trivalent chromium plating film An iron plate (60 mm × 90 mm × t0.3 mm) was prepared as the object to be plated, and chrome plating was performed according to the process shown in Table 1 below. The effective chrome plating area of ​​the object to be plated was 0.39 dm2 (60mm x 65mm).

[0079] [Table 1]

[0080] The chrome plating process of each of the examples and comparative examples will be described below.

[0081] Comparative Example 1 (Preparation of hexavalent chromium plating solution) 250 g / L of chromic anhydride and 2.5 g / L of sulfuric acid were added to water as a solvent to prepare 1 L of a hexavalent chromium plating solution.

[0082] (Hexavalent chromium plating) The hexavalent chromium plating solution of Comparative Example 1 was used on the object to be plated. The solution temperature was 40°C, and the applied current value was 4.68 A (cathode current density: 12 A / dm 2 ) and plating time: 180 minutes, and hexavalent chromium plating was performed to prepare test pieces.

[0083] Examples 1 to 20, Comparative Examples 2 to 4 The raw materials shown in Tables 2 and 3 were mixed in the proportions shown in each table to prepare 1 L of plating solution for each of the Examples and Comparative Examples.

[0084] [Table 2]

[0085] [Table 3]

[0086] Next, using the object to be plated shown in Table 4 as the cathode and the anode used in the electrolytic plating under the conditions shown in Table 4 below, test pieces were prepared.

[0087] [Table 4]

[0088] The test pieces prepared in the above Examples and Comparative Examples were used to carry out the following evaluations.

[0089] (Appearance of plating film) Cross-sectional photographs of the chromium plating film were taken and observed at a magnification of 1000 times using an inverted metallurgical microscope (Model ECLIPSE MA100, manufactured by Nikon Instech Corp.) and evaluated according to the following evaluation criteria. Cross-sectional photographs of the chromium plating film of Example 1 are shown in Fig. 1, Comparative Example 1 in Fig. 2, Comparative Example 2 in Fig. 3, Comparative Example 3 in Fig. 4, and Comparative Example 4 in Fig. 5. ○: The gloss appearance is uniform △: The plating film surface is uneven. ×: The plating film is brittle and uneven.

[0090] (Cathode current efficiency) The cathode current efficiency was calculated from the thickness of the chromium plating film obtained by observing the cross section of the chromium plating film. (Cathode current efficiency) = (amount of electricity (C) used to increase the amount of material in the chrome plating film) / (amount of electricity passed (C)) x 100 (%) It is calculated as follows.

[0091] In the examples and comparative examples, the amount of electricity applied is shown as 2.34 (A) x 3600 (s). The amount of electricity used to increase the amount of material in the chrome plating film is calculated by dividing the amount of material by the reaction time of chrome plating. 3+ +3e - → Cr three-electron reaction, and since the Faraday constant is 96500 C / mol, it is expressed as (amount of substance of the chromium plating film (mol)) × 3 × 96500 (C / mol). The amount of substance of the chromium plating film is calculated based on the density of chromium, which is 7.19 g / cm 3 Since the molar mass of chromium is 52.00 g / mol, the formula is [chrome plating thickness (μm) × 0.0001 × 39 (cm 2 )×7.19(g / cm 3)] / 52.00(g / mol). Therefore, the cathode current efficiency is calculated by the following formula:

[0092]

number

[0093] (Vickers hardness) Using a Vickers hardness tester (HM-200, manufactured by Mitutoyo Corporation), a diamond indenter was pressed against the cross section of the chrome plating film under a load of 0.05 kgf, and the hardness of the chrome plating film was calculated from the indentation.

[0094] (Wear resistance) Using a Suga abrasion tester (NUS-ISO-3 manufactured by Suga Test Instruments Co., Ltd.), the test was carried out under conditions of a load of 2000 gf, abrasive paper #240, and 500 abrasion cycles. The weight of the test piece before and after abrasion was measured, and the difference was calculated as the amount of abrasion to evaluate the abrasion resistance.

[0095] The results are shown in Tables 5 and 6.

[0096] [Table 5]

[0097] [Table 6]

[0098] From the results of Tables 5 and 6, it was found that in Examples 1 to 20 in which a trivalent chromium plating film was formed using a trivalent chromium plating solution containing the above components (A) to (D) and having a content of the metal halide as component (B) of 2 mol / L or more, the appearance of the plating film was excellent, and a trivalent chromium plating film excellent in hardness and abrasion resistance could be formed, and that the plating film showed excellent current efficiency.

[0099] In contrast, in Comparative Example 1, which did not contain the component (A), used a hexavalent chromium plating solution, and did not contain the components (B) to (D), the cathode current efficiency was low, indicating that the current efficiency was poor.

[0100] In addition, in Comparative Example 2, which did not contain the components (C) and (D), and Comparative Example 3, which did not contain the component (D), the trivalent chromium plating film became brittle, so the appearance of the plating film was poor, and it was impossible to measure the cathode current efficiency, the Vickers hardness, and the amount of wear in the wear resistance test.

[0101] Furthermore, in Comparative Example 4, which did not contain the component (C), the hardness of the trivalent chromium plating film was insufficient, and therefore the plating film had poor appearance, low Vickers hardness, and poor abrasion resistance.

[0102] 2. Evaluation of chlorine gas suppression by trivalent chromium plating method The raw materials shown in Table 7 were mixed in the proportions shown in Table 7 to prepare 1 L of the trivalent chromium plating solution of Example 21.

[0103] [Table 7]

[0104] Next, the electrolytic plating tank shown in FIG. Electrolytic plating was performed under the conditions shown in Table 8 below. FIG. 6 is a schematic diagram showing an example of a trivalent chromium plating method using the trivalent chromium plating solution of Example 21. In FIG. 6, the electrolytic plating was performed by immersing the plated object 1 shown in Table 8 as the cathode used in the electrolytic plating and the anode 2 in the trivalent chromium plating solution 3. Trivalent chromium plating was performed using the anodes shown in No. 1 to No. 5 in Table 9 below as the anodes 2. For each anode, as shown in FIG. 6, the detection port 5 of the gas detector tube 4 was installed at a position where the height h was 1 cm from the liquid interface of the trivalent chromium plating solution near the anode 2 to detect chlorine gas and measure the concentration of chlorine gas. The gas detector tube used was a gas detector tube (chlorine passive dositube (No. 8D), manufactured by Gastec Co., Ltd.). The measurement was performed three times, and the average chlorine gas concentration was calculated to obtain the measurement result. The results are shown in Table 9.

[0105] [Table 8]

[0106] [Table 9]

[0107] From the results in Table 9, it was found that even when the concentration of the metal halide, which is component (B) in the trivalent chromium plating solution, is as high as 2 mol / L or more, the generation of harmful chlorine gas is further suppressed by using a soluble anode made of metallic chromium. [Explanation of symbols]

[0108] 1.Item to be plated (cathode) 2. Anode 3. Trivalent chromium plating solution 4. Gas detector 5. Gas detector tube detection port h. Height from the liquid interface to the detection port of the gas detector

Claims

1. (A) trivalent chromium ions, (B) at least one metal halide selected from the group consisting of alkali metal halides and alkaline earth metal halides; (C) a boron compound, and (D) At least one dispersant selected from the group consisting of glycols, water-soluble polymers, anionic surfactants, amphoteric surfactants, and fluorine-based surfactants. Including, the metal halide is at least one selected from the group consisting of calcium chloride and lithium chloride; The content of the metal halide is 2 mol / L or more. A trivalent chromium plating solution comprising:

2. 2. The trivalent chromium plating solution according to claim 1, wherein the content of the metal halide is 4 mol / L or more.

3. 3. The trivalent chromium plating solution according to claim 1, wherein the metal halide comprises calcium chloride.

4. The trivalent chromium plating solution according to any one of claims 1 to 3, wherein the boron compound is at least one selected from the group consisting of boric acid, a borate salt, and boron oxide.

5. The trivalent chromium plating solution according to any one of claims 1 to 4, wherein the content of the boron compound is 5 to 100 g / L.

6. The trivalent chromium plating solution according to any one of claims 1 to 5, wherein the dispersant is a water-soluble polymer.

7. The trivalent chromium plating solution according to any one of claims 1 to 6, wherein the content of the dispersant is 0.01 to 100 g / L.

8. (A) trivalent chromium ions, (B) at least one metal halide selected from the group consisting of alkali metal halides and alkaline earth metal halides; (C) a boron compound, and (D) At least one dispersant selected from the group consisting of glycols, water-soluble polymers, anionic surfactants, amphoteric surfactants, and fluorine-based surfactants. The method includes a step of immersing an object to be plated as a cathode in a trivalent chromium plating solution containing the above-mentioned, and also immersing an anode in the solution to perform electrolytic plating, the metal halide is at least one selected from the group consisting of calcium chloride and lithium chloride; The content of the metal halide in the trivalent chromium plating solution is 2 mol / L or more. A method for trivalent chromium plating comprising the steps of:

9. 9. The trivalent chromium plating method according to claim 8, wherein the anode is a soluble anode containing metallic chromium.

Citation Information

Patent Citations

  • Electroplating solution and anode device thereof

    JP1979134038A

  • A photoresist layer on a substrate of the thermal imaging method

    JP1988501744A

  • Trivalent chromium plating bath

    JP2002285375A

  • Crystalline chromium alloy deposits

    JP2010540781A

  • Flexible color adjustment for dark cr(iii) plating

    JP2018528327A