Polylactate stereocomplex and its manufacturing method
A polylactate stereocomplex formed by a poly(L-lactate-3-hydroxypropionate) block copolymer and poly(D-lactate) addresses the limitations of polylactate resin, offering enhanced heat resistance and elongation properties while retaining biodegradability, suitable for general-purpose resin applications.
Patent Information
- Application Number
- JP2022564047
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-09-06
- Filing Date
- 2021-09-07
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2041-09-07
AI Technical Summary
Polylactate resin exhibits lower impact resistance and heat resistance than petroleum-based resins, limiting its application and use due to brittleness and poor elongation properties, while existing additive solutions often compromise biodegradability.
A polylactate stereocomplex is formed by combining a poly(L-lactate-3-hydroxypropionate) block copolymer with poly(D-lactate), where the block copolymer contains 10 to 50 parts by weight of poly(3-hydroxypropionate) repeating units per 100 parts by weight of poly(L-lactate) repeating units, and the poly(D-lactate) has a weight average molecular weight of 5,000 g/mol to 100,000 g/mol, enhancing heat resistance and elongation properties.
The polylactate stereocomplex demonstrates improved mechanical properties such as heat resistance and elongation, maintaining biodegradability, making it suitable for environmentally friendly general-purpose resin applications.
Smart Images

Figure 0007566401000001 
Figure 0007566401000002 
Figure 0007566401000003
Abstract
Description
[Technical field]
[0001] Cross-reference to related applications This application claims the benefit of priority based on Korean Patent Application No. 10-2020-0113936 filed on September 7, 2020, and Korean Patent Application No. 10-2021-0118336 filed on September 6, 2021, and all contents disclosed in the documents of said Korean patent applications are incorporated herein by reference.
[0002] The present invention relates to a polylactate stereocomplex containing a poly(L-lactate-3-hydroxypropionate) block copolymer and a method for producing the same. [Background technology]
[0003] Polylactate (polylactide or polylactic acid) resin is a plant-derived resin obtained from plants such as corn, and is attracting attention as an environmentally friendly material that has biodegradable properties and also has excellent tensile strength and elasticity. Specifically, unlike the currently used petroleum-based resins such as polystyrene resin, polyvinyl chloride (PVC) resin, and polyethylene, it has the effect of preventing the depletion of petroleum resources and suppressing carbon dioxide emissions, and therefore can reduce environmental pollution, which is a disadvantage of petroleum-based plastic products. Therefore, as the problem of environmental pollution caused by waste plastics and other substances has emerged as a social issue, efforts are being made to expand the scope of application to product areas where general plastics (petroleum-based resins) were used, such as food packaging materials and containers, and electronic product cases.
[0004] However, polylactate resin has limited application due to its lower impact resistance and heat resistance compared to existing petroleum-based resins.In addition, it has poor elongation properties and is easily brittle, limiting its use as a general-purpose resin.
[0005] In order to improve the elongation characteristics of polylactate resin, methods have been proposed in which additives are compounded or a copolymer is formed with a functional monomer, and methods have been proposed in which nucleating agents or inorganic additives are added to improve heat resistance. However, the additives used in these methods have a problem in that they are almost never biodegradable.
[0006] Therefore, there is a demand for the development of materials that exhibit improved heat resistance and elongation properties while maintaining biodegradability. Summary of the Invention [Problem to be solved by the invention]
[0007] An object of the present invention is to provide a polylactate stereocomplex having improved heat resistance and elongation properties while maintaining biodegradability, and a method for producing the same. [Means for solving the problem]
[0008] According to one embodiment of the present invention, A poly(L-lactate-3-hydroxypropionate) block copolymer containing 10 parts by weight to 50 parts by weight of poly(3-hydroxypropionate) repeating units per 100 parts by weight of poly(L-lactate) repeating units; and Provided is a polylactate stereocomplex comprising: poly(D-lactate) having a weight average molecular weight of 5,000 g / mol or more and less than 100,000 g / mol.
[0009] According to another embodiment of the present invention, A method for producing a polylactate stereocomplex is provided, which includes a step of mixing a poly(L-lactate-3-hydroxypropionate) block copolymer containing 10 to 50 parts by weight of poly(3-hydroxypropionate) repeating units per 100 parts by weight of poly(L-lactate) repeating units, and poly(D-lactate) having a weight average molecular weight of 5,000 g / mol or more and less than 100,000 g / mol. Effect of the Invention
[0010] The polylactate stereocomplex of the present invention has excellent mechanical properties such as heat resistance and elongation characteristics while maintaining biodegradability, and therefore can be suitably used as an environmentally friendly general-purpose resin. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] The terms used in this specification are merely used to describe exemplary embodiments and are not intended to limit the present invention. A singular expression includes a plural expression unless the context clearly indicates otherwise. In this specification, the terms "include", "comprise", "have" and the like are intended to specify the presence of an implemented feature, step, component, or combination thereof, and should be understood not to preclude the presence or additional possibility of one or more other features, steps, components, or combinations thereof.
[0012] The present invention can be modified in various ways and can have various forms, and will be described in detail below by taking specific examples as examples. However, it should be understood that this is not intended to limit the present invention to the specific disclosed forms, but rather to include all modifications, equivalents, or alternatives within the spirit and technical scope of the present invention.
[0013] As used herein, "poly(L-lactate-3-hydroxypropionate) block copolymer" refers to a block copolymer containing poly(L-lactate) repeat units derived from L-lactic acid and / or L-lactide monomers and poly(3-hydroxypropionate) repeat units derived from 3-hydroxypropionate monomers, and may be designated as "P(LLA-3-HP) block copolymer" or "P(LLA-b-3-HP)."
[0014] Furthermore, in this specification, "poly(L-lactate)" is a homopolymer of L-lactate monomers and / or L-lactide monomers and may be represented as "PLLA", and "poly(D-lactate)" is a homopolymer of D-lactic acid monomers and / or D-lactide monomers and may be represented as "PDLA".
[0015] The present invention will be described in detail below. Polylactate stereocomplex Polylactate resin is biodegradable and biocompatible, and is used as a representative biodegradable resin. However, it has low thermal stability and elongation, and its use as a general-purpose resin to replace polyolefins is limited.
[0016] Therefore, the present inventors conducted extensive research into a material that has excellent heat resistance and elongation properties while maintaining biodegradability, and as a result, discovered that a poly(L-lactate-3-hydroxypropionate) block copolymer having a poly(3-hydroxypropionate) repeating unit content of 10 to 50 parts by weight per 100 parts by weight of poly(L-lactate) repeating units can form a stereocomplex with poly(D-lactate). They confirmed that such a polylactate stereocomplex has significantly improved heat resistance and elongation properties compared to existing polylactate resins, and thus completed the present invention.
[0017] Therefore, according to one embodiment of the present invention, there is provided a polylactate stereocomplex comprising: a poly(L-lactate-3-hydroxypropionate) block copolymer containing 10 parts by weight to 50 parts by weight of poly(3-hydroxypropionate) repeating units per 100 parts by weight of poly(L-lactate) repeating units; and poly(D-lactate) having a weight average molecular weight of 5,000 g / mol or more and less than 100,000 g / mol.
[0018] The poly(L-lactate-3-hydroxypropionate) block copolymer exhibits superior flexibility and tensile properties compared to poly(L-lactate) homopolymer due to the poly(3-hydroxypropionate) repeating unit, while maintaining the crystallinity of the poly(L-lactate) repeating unit, and is therefore capable of forming a stereocomplex with poly(D-lactate).
[0019] In other words, the poly(L-lactate) portion in the poly(L-lactate-3-hydroxypropionate) block copolymer can be linked to the poly(D-lactate) like a zipper through intermolecular bonds such as hydrogen bonds, and therefore the polylactate stereocomplex of the present invention can exhibit excellent thermal stability and elongation properties.
[0020] In order to satisfy the above-mentioned characteristics, the poly(L-lactate-3-hydroxypropionate) block copolymer of the present invention preferably contains 10 parts by weight or more to 50 parts by weight or less of poly(3-hydroxypropionate) repeating units per 100 parts by weight of poly(L-lactate) repeating units, for example, 10 parts by weight or more, or 20 parts by weight or more, and 50 parts by weight or less, or 45 parts by weight or less, or 40 parts by weight or less.
[0021] If the content of poly(3-hydroxypropionate) repeating units is less than 10 parts by weight per 100 parts by weight of poly(L-lactate) repeating units, the effect of improving the physical properties such as the elongation of the polylactate stereocomplex cannot be ensured, and if it is 50 parts by weight or more, the rate of formation of the stereocomplex with poly(D-lactate) may be significantly reduced.
[0022] Meanwhile, the poly(L-lactate-3-hydroxypropionate) block copolymer may have a weight average molecular weight of 10,000 g / mol or more, or 50,000 g / mol or more, or 70,000 g / mol or more, and 400,000 g / mol or less, or 300,000 g / mol or less, or 200,000 g / mol or less, or 130,000 g / mol or less.
[0023] If the weight average molecular weight of the poly(L-lactate-3-hydroxypropionate) block copolymer is less than 10,000 g / mol, sufficient strength cannot be obtained when a stereocomplex is formed, and if the weight average molecular weight of the poly(L-lactate-3-hydroxypropionate) block copolymer exceeds 400,000 g / mol, processing becomes difficult, so it is preferable to satisfy the above range.
[0024] Furthermore, the poly(L-lactate-3-hydroxypropionate) block copolymer may have a melting temperature (Tm) of 145° C. or more, 150° C. or more, or 160° C. or more. The melting temperature of the poly(L-lactate-3-hydroxypropionate) block copolymer may be, for example, 180° C. or less.
[0025] A poly(L-lactate-3-hydroxypropionate) block copolymer satisfying the content of the poly(3-hydroxypropionate) repeating unit may be prepared by forming the poly(L-lactate) repeating unit and the poly(3-hydroxypropionate) repeating unit by ring-opening polymerization of an L-lactide monomer in the presence of a poly(3-hydroxypropionate) initiator.
[0026] In this case, the poly(3-hydroxypropionate) initiator preferably has a weight average molecular weight of 1,500 g / mol to 50,000 g / mol, 2,000 g / mol to 40,000 g / mol, 4,000 g / mol to 45,000 g / mol, or 5,000 g / mol to 30,000 g / mol in order to prevent a decrease in polymerization activity and to provide excellent physical properties for the block copolymer.
[0027] A poly(L-lactate-3-hydroxypropionate) block copolymer produced from a poly(3-hydroxypropionate) initiator satisfying the above molecular weight range can form a stereocomplex with poly(D-lactate) since the crystallinity of the poly(L-lactate) repeating unit (block) is maintained.
[0028] The method for producing the poly(L-lactate-3-hydroxypropionate) block copolymer suitable for forming the polylactate stereocomplex of the present invention will be described in more detail in the section on the method for producing the polylactate stereocomplex.
[0029] The poly(D-lactate) that forms a stereocomplex with the poly(L-lactate-3-hydroxypropionate) block copolymer may be a homopolymer of D-lactic acid monomer and / or D-lactide monomer and have an optical purity of 90% or more, 95% or more, or 98% or more.
[0030] The poly(D-lactate) has a weight average molecular weight of 5,000 g / mol or more, or 7,000 g / mol or more, or 10,000 g / mol or more, or 15,000 g / mol or more, and is preferably 100,000 g / mol or less, 70,000 g / mol or less, or 50,000 g / mol or less. If the weight average molecular weight of poly(D-lactate) is less than 5,000 g / mol, there is a problem that it does not have sufficient crystallinity, and if it exceeds 100,000 g / mol, the tensile elongation property of the stereocomplex produced is significantly reduced and the effect of the present invention cannot be achieved, so it is preferable to satisfy the above range.
[0031] The weight average molecular weights of the poly(3-hydroxypropionate) initiator, poly(L-lactate-3-hydroxypropionate) block copolymer, and poly(D-lactate) can be measured by gel permeation chromatography (GPC) as described in the Examples below.
[0032] The polylactate stereocomplex may contain 70 to 90 parts by weight of poly(L-lactate-3-hydroxypropionate) block copolymer; and 10 to 30 parts by weight of poly(D-lactate). When the content of poly(L-lactate-3-hydroxypropionate) block copolymer is high, the mechanical properties of the polylactate stereocomplex produced can be further improved. More preferably, the polylactate stereocomplex contains 80 to 90 parts by weight of poly(L-lactate-3-hydroxypropionate) block copolymer; and 10 to 20 parts by weight of poly(D-lactate).
[0033] The polylactate stereocomplex of the present invention is a complex of the above-mentioned poly(L-lactate-3-hydroxypropionate) block copolymer and poly(D-lactate), and exhibits significantly improved heat resistance and elongation properties compared to existing polylactate resins.
[0034] Specifically, the melting temperature (Tm) of the polylactate stereocomplex can be 200°C or more and 270°C or less, 260°C or less, 240°C or less, or 220°C or less.
[0035] When the melting temperature is 200° C. or more, it can be determined that a polylactate stereocomplex is formed, and in this case, it can be determined that the higher the melting enthalpy, the higher the stereocomplex formation rate, i.e., the ratio of each polymer participating in the stereocomplex formation. Thus, the polylactate stereocomplex according to one embodiment of the present invention may have a melting enthalpy of 11 J / g or more, or 20 J / g or more, and 50 J / g or less, or 45 J / g or less.
[0036] The melting temperature and melting enthalpy can be measured by differential scanning calorimetry.
[0037] Meanwhile, the polylactate stereocomplex has an elongation of 30% or more, 45% or more, or 55% or more as measured by a tensile strength tester according to IPC-TM-650 after preparing a dogbone test specimen according to ASTM D638 Type V, and thus exhibits a significantly superior elongation compared to existing stereocomplexes of poly(L-lactate) and poly(D-lactate). The upper limit of the elongation is not particularly limited, but may be, for example, 150% or less, or 110% or less.
[0038] Methods for determining the melt temperature, melt enthalpy, and elongation properties of the polylactate stereocomplexes are described in more detail in the Examples below.
[0039] Method for producing polylactate stereocomplex Meanwhile, according to another embodiment of the present invention, there is provided a method for producing the above-mentioned polylactate stereocomplex.
[0040] Specifically, the polylactate stereocomplex can be prepared by a method including a step of mixing a poly(L-lactate-3-hydroxypropionate) block copolymer containing 10 parts by weight to 50 parts by weight of a poly(3-hydroxypropionate) repeating unit per 100 parts by weight of a poly(L-lactate) repeating unit, and poly(D-lactate).
[0041] The characteristics of the poly(L-lactate-3-hydroxypropionate) block copolymer and poly(D-lactate) are as described above.
[0042] The method for producing the poly(L-lactate-3-hydroxypropionate) block copolymer and poly(D-lactate) is not particularly limited, and known methods can be applied.
[0043] As an example, the poly(L-lactate-3-hydroxypropionate) block copolymer can be prepared by forming the poly(L-lactate) repeat unit and the poly(3-hydroxypropionate) repeat unit by ring-opening polymerization of L-lactide monomer in the presence of a poly(3-hydroxypropionate) initiator.
[0044] The poly(3-hydroxypropionate) initiator contains a hydroxy group and / or an alkoxy group at its terminal. When the poly(3-hydroxypropionate) initiator is added to the ring-opening polymerization reaction of the lactide monomer, the lactide monomer begins to be inserted from the terminal of the poly(3-hydroxypropionate) initiator, resulting in the production of a poly(L-lactate-3-hydroxypropionate) block copolymer.
[0045] Therefore, when a ring-opening polymerization reaction of lactide monomer is carried out in the presence of the poly(3-hydroxypropionate) initiator, the poly(3-hydroxypropionate) not only serves as a polymerization initiator but is also included as a repeating unit in the block copolymer, thereby improving mechanical properties such as flexibility and impact strength of the final block copolymer. Specifically, the poly(3-hydroxypropionate) is included in the final block copolymer, thereby decreasing the glass transition temperature (Tg) of the block copolymer and increasing its flexibility.
[0046] In this case, the content of the poly(3-hydroxypropionate) initiator may be selected within an appropriate range in consideration of the content of the poly(3-hydroxypropionate) repeating unit contained in the final block copolymer and the minimum molar ratio of the hydroxyl group and / or alkoxy group of the initiator required to initiate polymerization.
[0047] Specifically, in order to optimize flexibility and mechanical properties while maintaining the crystallinity of the poly(L-lactate) repeating unit of the final block copolymer, and in consideration of the minimum content required for the role of an initiator in the ring-opening polymerization reaction, the poly(3-hydroxypropionate) initiator may be added in an amount of 10 parts by weight or more, or 20 parts by weight or more, and 50 parts by weight or less, or 40 parts by weight or less, per 100 parts by weight of L-lactide monomer.
[0048] The poly(3-hydroxypropionate) initiator may have a weight average molecular weight of 1,500 g / mol to 50,000 g / mol, 2,000 g / mol to 40,000 g / mol, 4,000 g / mol to 45,000 g / mol, or 5,000 g / mol to 30,000 g / mol so that the block copolymer exhibits excellent physical properties without reducing the polymerization activity. If the weight average molecular weight of the poly(3-hydroxypropionate) initiator is less than 1,500 g / mol, the content of poly(3-hydroxypropionate) may be reduced, and if it exceeds 50,000 g / mol, the polymerization activity may be reduced.
[0049] Meanwhile, prior to the ring-opening polymerization step, 3-hydroxypropionate may be condensation-polymerized to prepare the poly(3-hydroxypropionate) initiator. The prepared poly(3-hydroxypropionate) initiator and lactide monomer-containing reactant may be dried, and then the dried poly(3-hydroxypropionate) initiator and lactide monomer may be ring-opening-polymerized to prepare the block copolymer.
[0050] The catalyst used in the ring-opening polymerization may be any catalyst commonly used in the preparation of polylactate resins by ring-opening polymerization of lactide monomers. For example, the ring-opening polymerization may be carried out in the presence of one or more catalysts selected from the group consisting of organometallic complex catalysts and organic catalysts.
[0051] The organometallic complex catalyst may be any catalyst that is commonly used in the manufacture of a polylactate resin by ring-opening polymerization of a lactide monomer, without being limited in its composition. For example, the organometallic complex catalyst may be a catalyst represented by the following Chemical Formula 1:
[0052] [Chemical formula 1] MA 1 p A 2 2-p In the above formula 1, M is Al, Mg, Zn, Ca, Sn, Fe, Y, Sm, Lu, Ti or Zr, p is an integer of 0 to 2, and A 1 and A 2 are each independently an alkoxy or carboxyl group.
[0053] More specifically, the MA 1 p A 2 2-p can be tin(II) 2-ethylhexanoate (Sn(Oct)2).
[0054] Meanwhile, the organic catalyst may be any one generally used in the manufacture of polylactate resins by ring-opening polymerization of lactide monomers, without limitation of its constitution. For example, the organic catalyst may be one or more selected from the group consisting of 1,5,7-triazabicyclo-[4,4,0]dec-5-ene (TBD), 1,8-diazabicyclo[5.4.0]undec-7-ene (DBU), 7-methyl-1,5,7-triazabicyclo[4.4.0]dec-5-ene (MTBD), 4-dimethylaminopyridine (DMAP), 4-(1-pyrrolidinyl)pyridine (PPY), imidazole, triazolium, thiourea, tertiary amine, and creatinine. [ka]
[0055] The imidazole may be one or more selected from the group consisting of the following compounds: [ka]
[0056] The triazolium may be the following compound: [ka]
[0057] The thiourea may be one or more selected from the group consisting of the following compounds: [ka]
[0058] The tertiary amine may be one or more selected from the group consisting of the following compounds: [ka]
[0059] When lactide ring-opening polymerization is carried out in the presence of the above-mentioned catalyst, depolymerization or decomposition of the final block copolymer can be suppressed, and poly(L-lactate-3-hydroxypropionate) block copolymers having higher molecular weights and excellent mechanical properties can be obtained at higher conversion rates.
[0060] In the method for producing a block copolymer according to the embodiment, the content of the catalyst may be 0.01 mol% to 10 mol%, 0.05 mol% to 8 mol%, 0.07 mol% to 5 mol%, or 0.09 mol% to 3 mol% based on 100 mol% of the lactide monomer. If the content of the catalyst based on 100 mol% of the lactide monomer is less than 0.01 mol%, the polymerization activity may be insufficient, and if it exceeds 10 mol%, the amount of residual catalyst in the produced poly(L-lactate-3-hydroxypropionate) block copolymer may become large, which may lead to decomposition of the copolymer or a decrease in molecular weight due to depolymerization such as a transesterification reaction.
[0061] The ring-opening polymerization can be carried out at 150° C. to 200° C. for 5 minutes to 10 hours.
[0062] In addition, the ring-opening polymerization reaction can be carried out by bulk polymerization, which does not substantially use a solvent. In this case, the term "substantially does not use a solvent" can include the use of a small amount of solvent to dissolve the catalyst, for example, a maximum of less than 1 ml of solvent per 1 kg of lactide monomer used. By carrying out the ring-opening polymerization by bulk polymerization, it is possible to omit a process for removing the solvent after polymerization, and decomposition or loss of the resin during such a solvent removal process can be suppressed. In addition, the poly(L-lactate-3-hydroxypropionate) block copolymer can be obtained at a high conversion rate and yield by the bulk polymerization.
[0063] The poly(L-lactate-3-hydroxypropionate) block copolymer prepared as above maintains the crystallinity of the poly(L-lactate) repeating unit, and can be polymerized with poly(D-lactate) to form a polylactate stereocomplex.
[0064] Meanwhile, poly(D-lactate) can be prepared by using a commercially available product or by a known synthesis method. In one embodiment, poly(D-lactate) can be prepared by polycondensation of D-lactic acid monomer in the presence of a catalyst.
[0065] Next, the poly(L-lactate-3-hydroxypropionate) block copolymer and poly(D-lactate) are mixed to prepare a stereocomplex. At this time, a melt mixing method can be used, and in this case, the molecular weight of the prepared polylactate stereocomplex may be slightly reduced, but the stereocomplex can be formed in a short time and the formation rate of the complex can be high.
[0066] The melt mixing can be carried out at a temperature of 140°C to 200°C, or 150°C to 200°C, or 170°C to 200°C. If the temperature during melt mixing is less than 140°C, the rate of stereocomplex formation may decrease, and if it is too high and exceeds 200°C, the polymer may be thermally deformed, so it is preferable to satisfy the above-mentioned range. The melt mixing can be carried out under normal pressure, that is, within a pressure range of 700 Torr to 800 Torr. Under the above-mentioned temperature and pressure conditions, poly(L-lactate-3-hydroxypropionate) block copolymer and poly(D-lactate) can be stirred for 20 minutes or more, or 30 minutes to 1 hour to prepare a polylactate stereocomplex.
[0067] Hereinafter, preferred examples will be presented for understanding the present invention. However, the following examples are merely illustrative of the present invention, and it will be apparent to those skilled in the art that various changes and modifications are possible within the scope of the scope and technical idea of the present invention. It is natural that such changes and modifications fall within the scope of the appended claims. EXAMPLES
[0068] [Production Example] Production Example 1-1: Production of poly(L-lactate-3-hydroxypropionate) block copolymer
[0069] (1) Preparation of poly(3-hydroxypropionate) oligomers 30 g (416 mmol) of 3-hydroxypropionate was dried and then subjected to a polycondensation reaction in the presence of 0.012 g of p-toluenesulfonic acid (p-TSA) catalyst at a temperature of 110° C. and a reduced pressure of 0.1 Torr for 12 hours to produce poly(3-hydroxypropionate) oligomer.
[0070] The weight average molecular weight of the produced poly(3-hydroxypropionate) oligomer (P3HP) was 10,000 g / mol.
[0071] (2) Preparation of poly(L-lactate-3-hydroxypropionate) block copolymer Into a 100 mL round flask, 100 parts by weight of L-lactide, 10 parts by weight of the poly(3-hydroxypropionate) oligomer produced in (1) above, and 0.01 mol% of tin(II) 2-ethylhexanoate (based on 100% by weight of L-lactide) were placed, and sufficient vacuum was applied to dry the mixture at room temperature for 4 hours.
[0072] The flask was then placed in a 130°C pre-heated oil bath, and the temperature was raised to 180°C, after which ring-opening polymerization reaction was carried out for 60 to 90 minutes. After the reaction was terminated, the reactants were dissolved in chloroform and extracted with methanol to recover P(LLA-b-3HP) copolymer with a weight average molecular weight of 124,000 g / mol.
[0073] Production Example 1-2: Production of poly(L-lactate-3-hydroxypropionate) block copolymer
[0074] A P(LLA-b-3HP) copolymer having a weight average molecular weight of 80,000 g / mol was prepared in the same manner as in Preparation Example 1-1, except that 100 parts by weight of L-lactide, 20 parts by weight of poly(3-hydroxypropionate) oligomer, and 0.01 mol% of tin(II) 2-ethylhexanoate (based on 100% by weight of L-lactide) were used in step (2) of Preparation Example 1-1.
[0075] Production Example 1-3: Production of poly(L-lactate-3-hydroxypropionate) block copolymer
[0076] (1) Preparation of poly(3-hydroxypropionate) oligomers 30 g (416 mmol) of 3-hydroxypropionate was dried and then subjected to a polycondensation reaction in the presence of 0.012 g of p-toluenesulfonic acid (p-TSA) catalyst at a temperature of 110° C. and a reduced pressure of 0.1 Torr for 24 hours to produce poly(3-hydroxypropionate) oligomer.
[0077] The weight average molecular weight of the poly(3-hydroxypropionate) oligomer produced was 25,000 g / mol.
[0078] (2) Preparation of poly(L-lactate-3-hydroxypropionate) block copolymer Into a 100 mL round flask, 100 parts by weight of L-lactide, 20 parts by weight of the poly(3-hydroxypropionate) oligomer produced in (1) above, and 0.01 mol% of tin(II) 2-ethylhexanoate (based on 100% by weight of L-lactide) were placed, and sufficient vacuum was applied to dry the mixture at room temperature for 4 hours.
[0079] Then, the flask was placed in a pre-heated oil bath at 130° C., and the temperature was raised to 180° C., after which ring-opening polymerization reaction was carried out for 90 minutes. After the reaction was terminated, the reactants were dissolved in chloroform and extracted with methanol to recover P(LLA-b-3HP) copolymer with a weight average molecular weight of 115,100 g / mol.
[0080] Production Example 1-4: Production of poly(L-lactate-3-hydroxypropionate) block copolymer
[0081] A P(LLA-b-3HP) copolymer having a weight average molecular weight of 70,000 g / mol was prepared in the same manner as in Preparation Example 1-3, except that 100 parts by weight of L-lactide, 40 parts by weight of poly(3-hydroxypropionate) oligomer, and 0.01 mol% of tin(II) 2-ethylhexanoate (based on 100% by weight of L-lactide) were used in step (2) of Preparation Example 1-3.
[0082] Production Example 1-5: Production of poly(L-lactate-3-hydroxypropionate) block copolymer
[0083] A P(LLA-b-3HP) copolymer having a weight average molecular weight of 30,000 g / mol was prepared in the same manner as in Preparation Example 3, except that 100 parts by weight of L-lactide, 70 parts by weight of poly(3-hydroxypropionate) oligomer, and 0.01 mol% of tin(II) 2-ethylhexanoate (based on 100% by weight of L-lactide) were used in step (2) of Preparation Example 1-3.
[0084] Production Example 1-6: Production of poly(L-lactate)
[0085] 25 g of L-lactide and 11.2 μl of tin(II) 2-ethylhexanoate (0.01 mol % relative to 100 wt % L-lactide) were placed in a 500 mL round flask, and sufficient vacuum was applied to dry the mixture at room temperature (25° C.) for 4 hours.
[0086] Then, the flask was placed in a pre-heated oil bath at 130° C., and the temperature was raised to 180° C., after which ring-opening polymerization reaction was carried out for 90 minutes. After the reaction was completed, the reactant was dissolved in chloroform and extracted with methanol to recover a PLLA polymer having a weight average molecular weight of 118,000 g / mol.
[0087] Production Example 2-1: Production of poly(D-lactate) 20 g of D-lactic acid and 6 g of p-toluenesulfonic acid catalyst were placed in a 100 mL round flask and reacted at 50 mbar and 110°C for 3 hours and at 20 mbar and 140°C for 15 hours to obtain a PDLA polymer with a weight average molecular weight of 14,690 g / mol.
[0088] Production Example 2-2: Production of poly(D-lactate) 10 g (70 mmol) of D-lactide, 0.036 g (0.2 mmol) of 1-octanol, and 0.01 mol% of tin(II) 2-ethylhexanoate (based on 100% by weight of D-lactide) were placed in a 100 mL round flask, and sufficient vacuum was applied to dry the mixture at room temperature for 4 hours.
[0089] Then, the flask was placed in a pre-heated oil bath at 130° C., and the temperature was raised to 180° C., after which ring-opening polymerization reaction was carried out for 90 minutes. After the reaction was completed, the reactant was dissolved in chloroform and extracted with methanol to recover a PDLA polymer having a weight average molecular weight of 50,000 g / mol.
[0090] Production Example 2-3: Production of poly(D-lactate) 10 g (70 mmol) of D-lactide, 0.016 g (0.1 mmol) of 1-octanol, and 0.01 mol% of tin(II) 2-ethylhexanoate (based on 100% by weight of D-lactide) were placed in a 100 mL round flask, and sufficient vacuum was applied to dry the mixture at room temperature for 4 hours.
[0091] Then, the flask was placed in a pre-heated oil bath at 130° C., and the temperature was raised to 180° C., after which ring-opening polymerization reaction was carried out for 90 minutes. After the reaction was completed, the reactant was dissolved in chloroform and extracted with methanol to recover a PDLA polymer having a weight average molecular weight of 120,000 g / mol.
[0092] Example 1 90 parts by weight of the P(LLA-b-3HP) copolymer prepared in Preparation Example 1-1 and 10 parts by weight of the PDLA polymer prepared in Preparation Example 2-1 were placed in a reactor capable of stirring, and stirred at 200° C. for 30 minutes under normal pressure (760 Torr) to prepare a polylactate stereocomplex.
[0093] Examples 2 to 6 and Comparative Examples 1 to 3 A polylactate stereocomplex was prepared in the same manner as in Example 1, except that the substances shown in Table 2 below were used as P(LLA-b-3HP) (or PLLA) and PDLA, and the content of PDLA was adjusted as shown in Table 2 below.
[0094] Comparative Example 4 A commercially available PLLA polymer, Ingeo® Biopolymer 2003D (PLA 2003D) from Nature Works, Inc., was used as Comparative Example 2.
[0095] [Experimental Example] The physical properties of the polymers prepared in the above Preparation Examples and the polylactate stereocomplexes of the Examples and Comparative Examples were evaluated by the following methods. The results are shown in Tables 1 and 2.
[0096] Experimental Example 1: GPC (Gel Permeation Chromatography) Analysis The weight average molecular weight (Mw) and number average molecular weight (Mn) of the polymer were determined by gel permeation chromatography (GPC) (Waters: Waters 707), and the polydispersity index (PDI) was calculated by dividing the measured weight average molecular weight by the number average molecular weight.
[0097] The polymer to be measured was dissolved in chloroform to a concentration of 4000 ppm, and 100 μl was injected into the GPC. Chloroform was used as the mobile phase for GPC, and the flow rate was 1.0 mL / min. Analysis was performed at 35°C. Four columns, Waters HR-05, 1, 2, and 4E, were connected in series. RI and PAD detectors were used as detectors, and measurements were performed at 35°C.
[0098] Experimental Example 2: Differential Scanning Calorimetry The melting enthalpy and melting temperature were measured using a Differential Scanning Calorimeter (DSC, manufacturer: Mettler Toledo) by the following method.
[0099] The polymer (or stereocomplex) was heated to 230°C, maintained at this temperature for 5 minutes, and then cooled to -40°C to remove the thermal history. The melting temperature (Tm) and melting enthalpy (ΔH) were measured from the peak in the second heating by heating to 230°C again. The temperature increase and decrease rates were controlled at 10°C / min, respectively.
[0100] Experimental example 3: Elongation measurement The stereocomplexes of Examples 1 and 3 and Comparative Example 1 and the P(LLA-b-3HP) copolymer of Preparation Example 3 were measured for elongation by the following method.
[0101] Dog-bone test pieces conforming to ASTM D638 Type V were prepared at 170°C using a hot press (Limotem QM900S).
[0102] The elongation of the prepared test pieces was measured using a tensile strength measuring instrument (manufacturer: Instron, model name: 3345 UTM) according to the measurement method of IPC-TM-650.
[0103] [Table 1]
[0104] [Table 2]
[0105] Referring to Table 2, it can be seen that the stereocomplexes of Examples 1 to 6 exhibit significantly improved heat resistance compared to the P(LLA-b-3HP) copolymer alone or a commercially available polylactate resin, and have significantly improved tensile elongation compared to the stereocomplex of Comparative Example 1 prepared from poly(L-lactate) and poly(D-lactate).
[0106] On the other hand, in Comparative Example 2, in which P(LLA-b-3HP) containing more than 50 parts by weight of poly(3-hydroxypropionate) repeating units was used, the melting temperature did not reach 200° C., indicating that no complex was formed. In Comparative Example 3, in which PDLA with a weight-average molecular weight of more than 100,000 g / mol was used, stereocomplex formation occurred, but the tensile elongation properties were significantly lower than those of Examples 1 to 6.
[0107] From the above results, it can be confirmed that it is possible to manufacture a stereocomplex with excellent heat resistance and tensile elongation by using P(LLA-b-3HP) having a poly(3-hydroxypropionate) repeating unit content of 10 parts by weight or more and 50 parts by weight or less, and PDLA having a weight average molecular weight of 5,000 g / mol or more and less than 100,000 g / mol.
Claims
1. A polylactate stereocomplex comprising 70 to 90 parts by weight of a poly(L-lactate-3-hydroxypropionate) block copolymer and 10 to 30 parts by weight of poly(D-lactate), the poly(L-lactate-3-hydroxypropionate) block copolymer contains 10 to 50 parts by weight of poly(3-hydroxypropionate) repeating units per 100 parts by weight of poly(L-lactate) repeating units; The poly(D-lactate) has a weight average molecular weight of 5,000 g / mol or more and less than 100,000 g / mol. Polylactate stereocomplex.
2. The poly(L-lactate-3-hydroxypropionate) block copolymer is contained in an amount of 80 parts by weight to 90 parts by weight, 2. The polylactate stereocomplex according to claim 1, comprising 10 to 20 parts by weight of said poly(D-lactate).
3. The polylactate stereocomplex according to claim 1 or 2, wherein the poly(L-lactate-3-hydroxypropionate) block copolymer has a weight average molecular weight of 10,000 g / mol to 400,000 g / mol.
4. The polylactate stereocomplex according to any one of claims 1 to 3, wherein the poly(D-lactate) has a weight average molecular weight of 15,000 g / mol to 50,000 g / mol.
5. 5. The polylactate stereocomplex according to claim 1, having a melting temperature of 200° C. or higher.
6. 6. The polylactate stereocomplex according to claim 1, having a melting enthalpy of 11 J / g or more.
7. The polylactate stereocomplex according to any one of claims 1 to 6, wherein the polylactate stereocomplex has an elongation of 10% or more as measured by a tensile strength tester according to IPC-TM-650 after preparing an ASTM D638 Type V dog-bone test piece.
8. A method for producing a polylactate stereocomplex, comprising mixing 70 to 90 parts by weight of a poly(L-lactate-3-hydroxypropionate) block copolymer and 10 to 30 parts by weight of poly(D-lactate), the poly(L-lactate-3-hydroxypropionate) block copolymer contains 10 to 50 parts by weight of poly(3-hydroxypropionate) repeating units per 100 parts by weight of poly(L-lactate) repeating units; The weight average molecular weight of poly(D-lactate) is 5,000 g / mol or more and less than 100,000 g / mol; A method for producing a polylactate stereocomplex.
9. The method for producing a polylactate stereocomplex according to claim 8, wherein the poly(L-lactate-3-hydroxypropionate) block copolymer is produced by ring-opening polymerization of lactide monomer in the presence of a poly(3-hydroxypropionate) initiator.
10. The method for producing a polylactate stereocomplex according to claim 9, wherein the poly(3-hydroxypropionate) initiator has a weight average molecular weight of 1,500 g / mol to 50,000 g / mol.
11. The method for producing a polylactate stereocomplex according to claim 9 or 10, wherein the content of the poly(3-hydroxypropionate) initiator is 10 parts by weight or more based on 100 parts by weight of the lactide monomer.
Citation Information
Patent Citations
Polyactic acid resin composition, production method thereof and molded article
JP2003096285A
Lactic acid based resin composition containing copolymer and its molded article
JP2006299133A
Polylactic acid stereocomplex resin composition, method for molding polylactic acid stereocomplex resin composition, and molded product
JP2015004050A
Polymeric piezoelectric material and manufacturing method therefor
JP2016138239A
Stereocomplex multi-block copolymer and molded body
JP2016210894A