toner

The toner formulation with resin A and crystalline polyester in the binder resin addresses low-temperature fixability and scratch resistance issues by promoting heterogeneous nucleation and interfacial adhesion, ensuring effective image fixation and durability.

JP7566575B2Active Publication Date: 2024-10-15CANON KK
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2020177941
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-10-23
Publication Date
2024-10-15
Estimated Expiration
2040-10-23

AI Technical Summary

Technical Problem

Existing toners face challenges in achieving low-temperature fixability without compromising scratch resistance, as lowering the glass transition temperature (Tg) of the binder resin can lead to storage stability issues and offset on fixing members, while incorporating crystalline polyester can result in deteriorated scratch resistance over time.

Method used

A toner formulation with a binder resin containing resin A, which has a specific structure represented by formula (1) with a polymeric part and a monovalent group, and resin B with a crystalline polyester portion, promoting heterogeneous nucleation and improved interfacial adhesion through entanglement effects.

Benefits of technology

The toner achieves excellent low-temperature fixability and maintains scratch resistance over time by enhancing the compatibility and mobility of crystalline polyester within the binder resin, preventing large crystal growth and improving stress relaxation at the interface.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007566575000001
    Figure 0007566575000001
  • Figure 0007566575000002
    Figure 0007566575000002
  • Figure 0007566575000003
    Figure 0007566575000003
Patent Text Reader

Abstract

To provide a toner that is excellent in low temperature fixability and gives a fixed image having scratch resistance with time.SOLUTION: A toner comprises a toner particle containing a binder resin, a resin A and a resin B, where the resin A has a polymeric site and monovalent group that is bound to the polymeric site and is represented by the formula (1), and the resin B contains a crystalline polyester site. (In the formula (1), L1 is an alkylene group having 4 or less carbon atoms, -O-, -OR5-, -NH-, or -NHR6-, R1-R3 independently represent a hydrogen atom, a halogen atom, an alkyl group having one or more carbon atoms, an alkoxy group having one or more carbon atoms, an aryl group having 6 or more carbon atoms or a hydroxy group, and R5 and R6 each represent an alkylene group or a hydroxy alkylene group having 4 or less carbon atoms).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a toner used for forming a toner image by developing an electrostatic latent image formed by a dry electrostatic copying method such as electrophotography or electrostatic recording. [Background technology]

[0002] In recent years, energy saving has been considered a major technical issue in electrostatic copying electrophotography used in copiers, printers, faxes, etc., and a significant reduction in the amount of heat required for image fixing devices is desired. Therefore, there is an increasing need for toners that can fix images with less energy, that is, with so-called "low temperature fixability." Common methods for improving the low-temperature fixability of a toner include lowering the glass transition temperature (Tg) of the binder resin or reducing the molecular weight of the binder resin in order to soften the binder resin used. However, simply lowering the Tg of the binder resin or reducing the molecular weight can result in a decrease in the storage stability of the toner and offset to the fixing member due to insufficient releasability during fixing. Therefore, as a method for improving the fixability of a toner without lowering the Tg of a binder resin, Patent Document 1 proposes a toner containing a vinyl resin as a binder resin, which is a copolymer of a vinyl monomer and a silane coupling agent having an unsaturated double bond and an alkoxysilyl group. Patent Document 2 also proposes a toner in which a crystalline polyester resin is added to a binder resin. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Japanese Patent Application Publication No. 7-239573 [Patent Document 2] JP 2004-191927 A Summary of the Invention [Problem to be solved by the invention]

[0004] The toner described in Patent Document 1 has excellent anti-fixing offset properties and transferability from a photoreceptor due to the release effect specific to silicone resins caused by siloxane bonds generated when a silane coupling agent having an alkoxysilyl group is crosslinked. However, the toner described in Patent Document 1 has a problem in that it does not have sufficient low-temperature fixing properties. The toner described in Patent Document 2 has good low-temperature fixing properties, but has the problem that the abrasion resistance of the resulting fixed image decreases over time due to crystal growth of the crystalline polyester moiety. Furthermore, it was found that even if the crystalline polyester described in Patent Document 2 is directly contained in the toner described in Patent Document 1, the crystalline polyester portion undergoes crystal growth over time, resulting in a decrease in the abrasion resistance of the fixed image. In view of these problems, the present invention provides a toner that has excellent low-temperature fixing properties and can provide fixed images that have abrasion resistance even over time. [Means for solving the problem]

[0005] The present invention provides a toner having toner particles containing a binder resin, a resin A, and a resin B, The toner is characterized in that the resin A has a polymer moiety and a monovalent group represented by the following formula (1) bonded to the polymer moiety, and the resin B contains a crystalline polyester moiety.

[0006] [ka] (In formula (1), L 1 teeth- NH-, -NHR 6 - represents R 1 ~R 3 each independently represents a hydrogen atom, a halogen atom, an alkyl group having 1 or more carbon atoms, an alkoxy group having 1 or more carbon atoms, an aryl group having 6 or more carbon atoms, or a hydroxy group. 、R6 are each an alkylene group or a hydroxyalkylene group having 4 or less carbon atoms. Effect of the Invention

[0007] According to the present invention, it is possible to provide a toner which has excellent low-temperature fixing properties and can give a fixed image which has abrasion resistance even over time. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] The toner of the present invention will be specifically described below, but is not limited thereto.

[0009] In the present invention, the expressions "xx or more and xx or less" and "xx to xx" expressing a numerical range mean a numerical range including the lower and upper limit endpoints, unless otherwise specified.

[0010] The toner of the present invention is a toner having toner particles containing a binder resin, a resin A, and a resin B, wherein the resin A has a polymer portion and a monovalent group represented by the following formula (1) bonded to the polymer portion, and the resin B contains a crystalline polyester portion.

[0011] The present inventors have found that by employing a toner having the above-mentioned configuration, a fixed image having excellent low-temperature fixing properties and abrasion resistance even over time can be obtained.

[0012] The reason for this is speculated as follows.

[0013] When a toner containing a crystalline polyester moiety is heated to above the melting point of the crystalline polyester during fixing, the molten polyester dissolves in the binder resin, reducing the viscosity of the toner as it is fixed to paper.

[0014] When an image fixed with a conventional toner containing a crystalline polyester moiety is discharged from the printer body, the temperature drops rapidly from the fixing temperature to near room temperature. Because the time for this drop is short, the polyester tends to remain in a state of being compatible with the binder resin, rather than forming nuclei and growing crystals while phase-separating from the binder resin.

[0015] The polyester that exists in the compatible state has high mobility in the fixed image, so that over time, it will be arranged as polyester that exists in a crystallized state in the fixed image and will exist in a state of phase separation from the binder resin. The crystalline polyester that has grown large in this way is likely to have distortion at the interface with the binder resin as the crystals grow. For this reason, the interface portion is a relatively weak portion against external stress, and when a rubbing force (shear stress) is applied to the fixed image, the fixed image is destroyed along the interface portion, and the fixed image is easily peeled off from the paper.

[0016] In contrast, the toner of the present invention contains resin A. Since the carbonyl group of resin A and the ester group site of the crystalline polyester contained in resin B have a high affinity, resin A and resin B tend to be located close to each other in the toner after fixing. This is thought to promote the formation of heterogeneous nuclei of polyester with the silyl group in resin A as a nucleus, making it easier to form crystal nuclei of polyester. For this reason, more crystal nuclei of resin B tend to be formed than when resin A is not present, and in the fixed image, the crystals of resin B are present in a more finely dispersed state, reducing the growth of large crystals. The L in resin A of the present invention 1 is an alkylene group having 4 or less carbon atoms, -O-, -OR 5 -, -NH-, or -NHR 6 In the case of -, the distance between the carbonyl group of resin A and the silane moiety is sufficiently short, so that it is considered that the above-mentioned effect becomes more remarkable.

[0017] On the other hand, the binder resin has a polymer chain. Generally, polymer chains with long molecular chains tend to be entangled with each other. For this reason, the carbonyl group present in the resin A has a high affinity for the ester group portion of the resin B, while the polymer portion of the resin A tends to be entangled with the polymer chain of the binder resin. For this reason, in the crystal nucleus of the resin B formed from the silyl group, the polymer portion of the resin A is likely to exist in a state of being entangled with the binder resin, and the resin A is considered to exist in the interface region between the resin B and the binder resin.

[0018] Here, when an abrasion force (shear stress) is applied to the fixed image, the interfacial adhesion between the binder resin and resin B is improved due to the entanglement effect between the polymer portion of resin A and the binder resin, and therefore the stress applied to the interface is alleviated, and the abrasion resistance of the fixed image is improved.

[0019] As described above, the toner of the present invention contains a binder resin, a resin A having a specific structure represented by formula (1), and a resin B containing a crystalline polyester moiety, and thus can obtain a fixed image that has excellent low-temperature fixing property and abrasion resistance even over time.

[0020] Resin A of the present invention will be described in detail below.

[0021] Resin A of the present invention preferably contains a resin represented by formula (1), and more preferably is a resin represented by formula (1).

[0022] [ka] (In formula (1), L 1 is an alkylene group having 4 or less carbon atoms, -O-, -OR 5 -, -NH-, -NHR 6 - represents R 1 ~R 3 each independently represents a hydrogen atom, a halogen atom, an alkyl group having one or more carbon atoms, an alkoxy group having one or more carbon atoms, an aryl group having six or more carbon atoms, or a hydroxyl group; R 5 , R6 are each an alkylene group or a hydroxyalkylene group having 4 or less carbon atoms.

[0023] The content of silicon atoms in the resin A (silicon concentration) is preferably from 0.02% by mass to 10.0% by mass, and more preferably from 0.02% by mass to 5.0% by mass.

[0024] When the content of silicon atoms in the resin A is 0.02% by mass or more, the silyl groups in the resin A tend to become crystal nuclei.

[0025] On the other hand, if the content of silicon atoms in the resin A is 10.0% by mass or less, the polymer moiety (e.g., polymer moiety) in the resin A is easily oriented by the binder resin. If the content of silicon atoms is 5.0% by mass or less, the polymer moiety is more easily oriented with respect to the binder resin. The method for measuring the content of silicon atoms in the resin A will be described later.

[0026] L in the above formula (1) 1 is an alkylene group having 4 or less carbon atoms, -O-, -OR 5 -, -NH-, -NHR 6 In the case where L is -, the distance between the carbonyl group and the silyl group in the resin A becomes short as described above, and thus the heterogeneous nucleation of the crystalline polyester moiety contained in the resin B is promoted. 1 -O-, -OR 5 -, -NH-, -NHR 6 In the case where the group is -, since these groups are electron-withdrawing groups, the effect of attracting the ester group moiety of the crystalline polyester moiety contained in resin B is strengthened, which is preferable.

[0027] Also, R 5 , R 6are each an alkylene group or a hydroxyalkylene group having 4 or less carbon atoms. The number of carbon atoms in the alkylene group is preferably 1 or more and 3 or less, and more preferably 1 or 2. The number of carbon atoms in the hydroxyalkylene group is preferably 1 or more and 3 or less, and more preferably 1 or 2. Among these, R 5 , R 6 When R is a hydroxyalkylene group which is an electron-withdrawing group, the effect of attracting the ester group site of the crystalline polyester contained in Resin B is further strengthened, and this is more preferable.

[0028] R in the above formula (1) 1 ~R 3 each independently represents a hydrogen atom, a halogen atom, an alkyl group having one or more carbon atoms, an alkoxy group having one or more carbon atoms, an aryl group having six or more carbon atoms, or a hydroxy group.

[0029] The alkyl group preferably has 1 or more and 12 or less carbon atoms, more preferably has 1 or more and 4 or less carbon atoms, and further preferably has 1 or more and 3 or less carbon atoms.

[0030] The alkoxy group preferably has 1 or more and 6 or less, more preferably has 1 or more and 3 or less, and further preferably has 1 or 2 carbon atoms.

[0031] The aryl group preferably has 6 or more and 12 or less carbon atoms, and more preferably has 6 or more and 10 or less carbon atoms.

[0032] Among these, R in formula (1) 1 ~R 3 At least one of R in formula (1) is preferably an alkoxy group or a hydroxy group. 1 ~R 3 More preferably, each independently represents an alkoxy group or a hydroxy group.

[0033] These alkoxy groups or hydroxy groups have a higher affinity for the ester group site of resin B, and therefore tend to attract the crystalline polyester contained in resin B. This tends to further promote the above-mentioned heterogeneous nucleation reaction.

[0034] R in formula (1) 1 ~R 3 In order to make at least one of the groups a hydroxy group, for example, R 1 ~R 3 A resin in which one or more of the above groups are alkoxy groups may be hydrolyzed to convert the alkoxy groups to hydroxy groups.

[0035] The hydrolysis may be carried out by any method, for example, the following method.

[0036] R in formula (1) 1 ~R 3 A resin in which one or more of the above groups are alkoxy groups is dissolved or suspended in a suitable solvent (which may be a polymerizable monomer), the pH is adjusted to acidic using an acid or alkali, and the mixture is mixed to cause hydrolysis.

[0037] Further, hydrolysis may occur during the production of toner particles.

[0038] Resin A has a polymer portion. The polymer portion is not particularly limited as long as it has a polymer structure. The polymer portion is likely to form an entangled structure with the molecular chain of the binder resin, so that when an abrasive force (shear stress) is applied to the fixed image, the stress relaxation effect at the interface between resin B and the binder resin increases, and the abrasion resistance is improved.

[0039] Specific examples of the polymer moiety in resin A include polyester moieties, vinyl polymer moieties such as styrene-acrylic acid copolymers, polyurethane moieties, polycarbonate moieties, phenolic resin moieties, polyolefin moieties, and the like.

[0040] Among these, it is preferable that the polymer segment contains a styrene-acrylic acid copolymer segment or a polyester segment.

[0041] The polymer moiety containing a styrene-acrylic acid copolymer moiety may be composed of only a styrene-acrylic acid copolymer, or may be a block copolymer or a graft copolymer of a styrene-acrylic acid copolymer and another polymer, or a mixture thereof. Here, the styrene-acrylic acid copolymer means a copolymer of a styrene-based monomer (styrene unit) and at least one monomer (unit) selected from the group consisting of an acrylic acid-based monomer (acrylic unit) and a methacrylic acid-based monomer (methacrylic unit).

[0042] Examples of the styrene monomer include styrene, α-methylstyrene, β-methylstyrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, 2,4-dimethylstyrene, divinylbenzene, etc. The styrene monomer may be used alone or in combination of two or more selected from these.

[0043] Examples of the acrylic acid monomer include acrylic acid alkyl esters such as methyl acrylate, ethyl acrylate, n-propyl acrylate, isopropyl acrylate, n-butyl acrylate, isobutyl acrylate, tert-butyl acrylate, n-amyl acrylate, n-hexyl acrylate, 2-ethylhexyl acrylate, n-octyl acrylate, and n-nonyl acrylate; acrylic acid diesters such as diethylene glycol diacrylate, triethylene glycol diacrylate, tetraethylene glycol diacrylate, polyethylene glycol diacrylate, and 1,6-hexanediol diacrylate; and acrylic acid.

[0044] Examples of the methacrylic acid monomer include methacrylic acid alkyl esters such as methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, iso-propyl methacrylate, n-butyl methacrylate, iso-butyl methacrylate, tert-butyl methacrylate, n-amyl methacrylate, n-hexyl methacrylate, 2-ethylhexyl methacrylate, n-octyl methacrylate, and n-nonyl methacrylate; methacrylic acid, and the like.

[0045] The acrylic acid monomer and the methacrylic acid monomer may be used alone or in combination of two or more selected therefrom.

[0046] The styrene-acrylic acid copolymer portion preferably contains a styrene-acrylic acid alkyl ester copolymer or a styrene-methacrylic acid alkyl ester copolymer.

[0047] In the total monomers forming the styrene-acrylic acid copolymer, the proportion of the styrene-based monomer is preferably 45% by mass or more and 80% by mass or less, while the proportion of at least one monomer selected from the group consisting of acrylic acid-based monomers and methacrylic acid-based monomers (e.g., acrylic acid alkyl ester and / or methacrylic acid alkyl ester) is preferably 20% by mass or more and 50% by mass or less.

[0048] Further, an embodiment in which the polymer moiety contains a polyester moiety will be described, but the present invention is not limited thereto.

[0049] The polyester moiety refers to a polymer moiety having an ester bond (-CO-O-) in the repeating unit of the main chain, such as a condensation polymer structure of a polyhydric alcohol (alcohol component) and a polycarboxylic acid (carboxylic acid component).

[0050] Examples of polyvalent carboxylic acids include oxalic acid, glutaric acid, succinic acid, maleic acid, adipic acid, β-methyladipic acid, azelaic acid, sebacic acid, nonanedicarboxylic acid, decanedicarboxylic acid, undecanedicarboxylic acid, dodecanedicarboxylic acid, fumaric acid, citraconic acid, diglycolic acid, cyclohexane-3,5-diene-1,2-dicarboxylic acid, hexahydroterephthalic acid, malonic acid, pimelic acid, phthalic acid, isophthalic acid, terephthalic acid, tetrachlorophthalic acid, chlorophthalic acid, nitrophthalic acid, p-carboxyphenylacetic acid, p-phenylene diacetic acid, m-phenylenediglycolic acid, p-phenylenediglycolic acid, o-phenylenediglycolic acid, diphenylacetic acid, diphenyl-p,p'-dicarboxylic acid, naphthalene-1,4-dicarboxylic acid, naphthalene-1,5-dicarboxylic acid, naphthalene-2,6-dicarboxylic acid, anthracene dicarboxylic acid, and cyclohexane dicarboxylic acid. Examples of polycarboxylic acids other than dicarboxylic acids include trimellitic acid, pyromellitic acid, naphthalene tricarboxylic acid, naphthalene tetracarboxylic acid, pyrene tricarboxylic acid, and pyrene tetracarboxylic acid.

[0051] Examples of polyhydric alcohols include ethylene glycol, diethylene glycol, triethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,4-butanediol, neopentyl glycol, 1,4-butenediol, 1,5-pentanediol, 1,6-hexanediol, 1,4-cyclohexanedimethanol, dipropylene glycol, polyethylene glycol, polypropylene glycol, polytetramethylene glycol, sorbitol, 1,2,3,6-hexanetetrol, 1,4-sorbitan, pentaerythritol, and dipentaerythritol. Examples of such esters include erythritol, tripentaerythritol, 1,2,4-butanetriol, 1,2,5-pentanetriol, glycerol, 2-methylpropanetriol, 2-methyl-1,2,4-butanetriol, trimethylolethane, trimethylolpropane, 1,3,5-trihydroxymethylbenzene, bisphenol A, bisphenol A ethylene oxide adduct, bisphenol A propylene oxide adduct, hydrogenated bisphenol A, hydrogenated bisphenol A ethylene oxide adduct, and hydrogenated bisphenol A propylene oxide adduct.

[0052] When the polymer moiety in the formula (1) and the binder resin have the same type of structure, the affinity between the polymer moiety and the binder resin becomes stronger.

[0053] That is, when the binder resin is a resin containing a styrene-acrylic acid copolymer and the polymer portion contains a styrene-acrylic acid copolymer, or when the binder resin is a resin containing a polyester portion and the polymer portion contains a polyester portion, the above-mentioned affinity is further strengthened. Therefore, when an abrasion force (shear stress) is applied to the fixed image, the stress relaxation effect at the interface between resin B and the binder resin is further increased, and the abrasion resistance is improved.

[0054] The resin having the structure of formula (1) can be formed by a method of reacting a carboxyl group in a polymer portion (e.g., a polymer portion) with an aminosilane, a method of reacting a hydroxyl group in the polymer resin with a carboxysilane, a method of reacting a hydroxyl group in the polymer resin with an isocyanate silane, a method of reacting an isocyanate group in the polymer resin with an aminosilane, or the like.

[0055] Examples of aminosilanes include, but are not limited to, aminomethylsilane, aminoethylsilane, 3-aminopropylsilane, 4-aminobutylsilane, aminomethyltrimethylsilane, aminoethyltrimethylsilane, 3-aminopropyltrimethylsilane, 4-aminobutyltrimethylsilane, aminomethyldimethoxymethylsilane, aminoethyldimethoxymethylsilane, 3-aminopropyldimethoxymethylsilane, 4-aminobutyldimethoxymethylsilane, aminomethyldiethoxymethylsilane, aminoethyldiethoxymethylsilane, 3-aminopropyldiethoxymethylsilane, 4-aminobutyldiethoxymethylsilane, aminomethyldimethoxyethylsilane, aminoethyldimethoxyethylsilane, 3-aminopropyldimethoxyethylsilane, 4-aminobutyldimethoxyethylsilane, aminomethyldiethoxyethylsilane, aminoethyldiethoxyethylsilane, 3-aminopropyldiethoxyethylsilane, 4-aminobutyldiethoxyethylsilane, aminomethyltrimethoxysilane, aminoethyltrimethoxysilane, 3-aminopropyltrimethoxysilane, 4-aminobutyltrimethoxysilane, aminomethyltriethoxysilane, aminoethyltriethoxysilane, 3-aminopropyltriethoxysilane, 4-aminobutyltriethoxysilane, trimethoxy[3-(methylamino)propyl]silane, and the like.

[0056] Examples of carboxysilanes include 3-carboxypropyltrimethoxysilane, β-carboxyethyltriethoxysilane, β-carboxyethylphenylbis(β-methoxyethoxy)silane, and N-β-(carboxymethyl)aminoethyl-γ-aminopropyltrimethoxysilane.

[0057] Examples of the isocyanate silane include isocyanate methyl trimethoxy silane, isocyanate ethyl triethoxy silane, 3-isocyanate propyl trimethoxy silane, 3-isocyanate propyl triethoxy silane, 3-isocyanate propyl dimethyl methoxy silane, 3-isocyanate propyl dimethyl ethoxy silane, 3-isocyanate propyl dimethoxy methyl silane, and 3-isocyanate propyl diethoxy methyl silane.

[0058] The weight average molecular weight (Mw) of the resin A is preferably 3,000 or more and 100,000 or less, and more preferably 5,000 or more and 30,000 or less.

[0059] If the weight average molecular weight is 3000 or more, the affinity between the polymer moiety bonded to the structure of formula (1) contained in resin A and the molecular chain of the binder resin is sufficient. In this case, when an abrasion force (shear stress) is applied to the fixed image, the fixed image has abrasion resistance due to the stress relaxation effect at the interface between resin B and the binder resin.

[0060] On the other hand, if the weight average molecular weight is 100,000 or less, the crystal growth of the crystalline polyester contained in the resin B is not hindered, and the crystallinity of the resin B is likely to be improved. The method for measuring the weight average molecular weight (Mw) will be described later.

[0061] The content of the resin A in the total resin of the toner particles is preferably 0.5% by mass or more, more preferably 1.0% by mass or more, and even more preferably 3.0% by mass or more. When the content of the resin A is within the above range, the heterogeneous nucleation of the resin B in the fixed image is sufficiently carried out, and the resin B is finely dispersed, resulting in good abrasion resistance. In addition, the content is preferably 20.0% by mass or less. When the content is 20.0% by mass or less, the viscosity reducing effect of the binder resin by the resin B becomes sufficient, and the toner has good low-temperature fixing properties.

[0062] The toner particles contain a binder resin. The binder resin is a resin component in the toner particles other than the resin A and the resin B. When the content of the binder resin in the total resin of the toner particles is 50.0% by mass or more, a fixed image having good fixability and abrasion resistance can be obtained, which is preferable.

[0063] The binder resin is not particularly limited, and any conventionally known binder resin can be used.

[0064] From the viewpoint of the developing characteristics and durability of the toner, the binder resin is preferably a resin containing a styrene-acrylic acid copolymer or a resin containing a polyester moiety.

[0065] The resin containing a styrene-acrylic acid copolymer may be a resin consisting of only a styrene-acrylic acid copolymer, or may be a block copolymer or graft copolymer of a styrene-acrylic acid copolymer and another polymer, or a mixture thereof, so long as it contains a styrene-acrylic acid copolymer.

[0066] Here, the styrene-acrylic acid copolymer means a copolymer of a styrene-based monomer and at least one monomer selected from the group consisting of an acrylic acid-based monomer and a methacrylic acid-based monomer.

[0067] Examples of the styrene monomer include styrene, α-methylstyrene, β-methylstyrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, 2,4-dimethylstyrene, divinylbenzene, etc. The styrene monomer may be used alone or in combination of two or more selected from these.

[0068] Examples of the acrylic acid monomer include acrylic acid alkyl esters such as methyl acrylate, ethyl acrylate, n-propyl acrylate, isopropyl acrylate, n-butyl acrylate, isobutyl acrylate, tert-butyl acrylate, n-amyl acrylate, n-hexyl acrylate, 2-ethylhexyl acrylate, n-octyl acrylate, and n-nonyl acrylate; acrylic acid diesters such as diethylene glycol diacrylate, triethylene glycol diacrylate, tetraethylene glycol diacrylate, polyethylene glycol diacrylate, and 1,6-hexanediol diacrylate; and acrylic acid.

[0069] Examples of the methacrylic acid monomer include methacrylic acid alkyl esters such as methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, iso-propyl methacrylate, n-butyl methacrylate, iso-butyl methacrylate, tert-butyl methacrylate, n-amyl methacrylate, n-hexyl methacrylate, 2-ethylhexyl methacrylate, n-octyl methacrylate, and n-nonyl methacrylate; methacrylic acid, and the like.

[0070] The acrylic acid monomer and the methacrylic acid monomer may be used alone or in combination of two or more selected therefrom.

[0071] The resin containing a styrene-acrylic acid copolymer preferably contains a styrene-acrylic acid alkyl ester copolymer or a styrene-methacrylic acid alkyl ester copolymer.

[0072] In the total monomers forming the styrene-acrylic acid copolymer, the proportion of the styrene-based monomer is preferably 45% by mass or more and 80% by mass or less, while the proportion of at least one monomer selected from the group consisting of acrylic acid-based monomers and methacrylic acid-based monomers (e.g., acrylic acid alkyl ester and / or methacrylic acid alkyl ester) is preferably 20% by mass or more and 50% by mass or less.

[0073] The resin containing a polyester moiety may be a condensation polymer of a carboxylic acid component and an alcohol component as listed below. Examples of the carboxylic acid component include terephthalic acid, isophthalic acid, phthalic acid, fumaric acid, maleic acid, cyclohexanedicarboxylic acid, and trimellitic acid. Examples of the alcohol component include bisphenol A, hydrogenated bisphenol, an ethylene oxide adduct of bisphenol A, a propylene oxide adduct of bisphenol A, glycerin, trimethylolpropane, and pentaerythritol.

[0074] The polyester moiety may be a polyester containing a urea group. It is preferable that the carboxyl groups at the terminals of the polyester are not capped.

[0075] The content of the resin containing a styrene-acrylic acid copolymer or the resin containing a polyester moiety in the binder resin is preferably 50.0% by mass or more and 100.0% by mass or less, and more preferably 80.0% by mass or more and 100.0% by mass or less. When the content is within the above range, the viscosity reducing effect of the resin B described below on the binder resin becomes sufficient, and good low-temperature fixing properties are exhibited. These binder resins can be used alone or in combination.

[0076] The binder resin may contain a crosslinking agent. The inclusion of a crosslinking agent can increase the elasticity of the toner. If the toner has a sufficiently high elasticity, even if the viscosity reduction effect of the binder resin due to resin B is too large, the toner with reduced viscosity is expected to be less likely to adhere to the fixing roller, and low-temperature fixability is considered to be further improved.

[0077] As the crosslinking agent, a compound having two or more polymerizable double bonds is mainly used.

[0078] Examples of the vinyl compounds include aromatic divinyl compounds such as divinylbenzene and divinylnaphthalene; carboxylic acid esters having two double bonds such as ethylene glycol diacrylate, ethylene glycol dimethacrylate, 1,3-butanediol dimethacrylate, and 1,6-hexanediol diacrylate; divinyl compounds such as divinylaniline, divinyl ether, divinyl sulfide, and divinyl sulfone; and compounds having three or more vinyl groups.

[0079] These may be used alone or in combination of two or more. The content of the crosslinking agent is preferably 0.001 parts by mass or more and 15,000 parts by mass or less with respect to 100 parts by mass of the binder resin.

[0080] Resin B is a resin containing a crystalline polyester moiety. Here, the term "crystalline" in the resin containing a crystalline polyester moiety means a resin containing a polyester moiety that has a clear endothermic peak in measurement by a differential scanning calorimeter (DSC).

[0081] In addition, having a clear endothermic peak specifically means that in differential scanning calorimetry (DSC) measurement, the half-width of the endothermic peak is within 8°C when measured at a heating rate of 10°C / min.

[0082] The compound constituting the crystalline polyester moiety may be at least one polymer selected from the group consisting of a polymer obtained by condensation polymerization of an aliphatic diol having 2 to 16 carbon atoms and an aliphatic dicarboxylic acid having 2 to 16 carbon atoms, a polymer obtained by condensation polymerization of an aliphatic diol having 2 to 16 carbon atoms and an aromatic dicarboxylic acid having 8 to 16 carbon atoms, and a polymer obtained by condensation polymerization of an aromatic diol and an aliphatic dicarboxylic acid having 2 to 16 carbon atoms.

[0083] Examples of the aliphatic diols having 2 to 16 carbon atoms include ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,11-undecanediol, 1,12-dodecanediol, 1,13-tridecanediol, 1,14-tetradecanediol, 1,15-pentadecanediol, and 1,16-hexadecanediol.

[0084] Examples of aliphatic dicarboxylic acids having 2 to 16 carbon atoms include malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, 1,9-nonanedicarboxylic acid, 1,10-decanedicarboxylic acid, 1,11-undecanedicarboxylic acid, 1,12-dodecanedicarboxylic acid, 1,13-tridecanedicarboxylic acid, and 1,14-tetradecanedicarboxylic acid. In addition, examples include anhydrides of these acids and alkyl (having 1 to 3 carbon atoms) esters of these acids.

[0085] Aliphatic dicarboxylic acids having 2 to 16 carbon atoms are unsaturated aliphatic It may be a dicarboxylic acid, and examples thereof include fumaric acid and maleic acid.

[0086] The aromatic diol may be bisphenol A or an alkylene oxide adduct of bisphenol A.

[0087] Aromatic dicarboxylic acids having 8 to 16 carbon atoms include phthalic acid, isophthalic acid, and terephthalic acid. Aromatic dicarboxylic acids such as phthalic acid and the anhydrides of these acids, as well as their alkyl esters, the alkyl being methyl, ethyl, propyl, and isopropyl groups.

[0088] Furthermore, the resin containing a crystalline polyester moiety includes not only a resin whose component is composed only of a polymer having the above-mentioned polyester structure, but also a hybrid polymer (block copolymer, graft copolymer) composed of a component having the above-mentioned polyester structure and other components, provided that in the latter case, the component containing the crystalline polyester moiety in the resin constituting the hybrid polymer is 50 mass% or more.

[0089] The carbon number of the diol component of the resin containing a crystalline polyester moiety and the carbon number of the dicarboxylic acid can be determined, for example, by analyzing the toner particles by pyrolysis GC / MS.

[0090] The melting point of the resin B is preferably 20° C. or higher and 90° C. or lower, more preferably 40° C. or higher and 70° C. or lower, from the viewpoint of the balance between the storage stability and low-temperature fixability of the toner, and further preferably 50° C. or higher and 65° C. or lower. When the melting point of the resin B is 40° C. or higher, the storage stability of the toner increases, and when it is 90° C. or lower, sufficient low-temperature fixability can be obtained.

[0091] In the present invention, the content of resin B is preferably 2.0 parts by mass or more, more preferably 10.0 parts by mass or more, relative to 100.0 parts by mass of binder resin. If the content of resin B is 2.0 parts by mass or more, the viscosity reducing effect on the binder resin is good, and low-temperature fixability is exhibited. If the content of resin B is 10.0 parts by mass or more, the effect is further improved, and excellent low-temperature fixability is exhibited. On the other hand, the content of resin B is preferably 50.0 parts by mass or less, more preferably 30.0 parts by mass or less, relative to 100.0 parts by mass of binder resin. If the content of resin B is 50.0 parts by mass or less, the fixed image exhibits good abrasion resistance, and if it is 30.0 parts by mass or less, the fixed image exhibits even better abrasion resistance.

[0092] The weight average molecular weight (Mw) of the resin B is preferably 2000 or more and 50000 or less, more preferably 5000 or more and 30000 or less. If the weight average molecular weight of the resin B is 2000 or more, the crystallization degree of the resin B in the toner particles is improved, and low-temperature fixing properties can be obtained. On the other hand, if the weight average molecular weight is 50000 or less, crystal growth from the silyl group of the resin A as a nucleus is likely to proceed in the fixed image, and the fixed image can have abrasion resistance. The method for measuring the weight average molecular weight (Mw) of the resin B will be described later.

[0093] When the content of resin A in the toner is a% by mass and the content of resin B in the toner is b% by mass, the ratio (a / b) of resin A to resin B is preferably 0.1 to 10.0, more preferably 0.1 to 6.0. When (a / b) is in the above range, the heterogeneous nucleation reaction of resin B is easily caused, and resin B is easily finely dispersed in the fixed image. The calculation method of (a / b) will be described later.

[0094] The toner particles may contain a wax, if necessary, in order to improve releasability from paper. The wax is not particularly limited, and the following waxes can be exemplified.

[0095] Aliphatic hydrocarbon waxes such as low molecular weight polyethylene, low molecular weight polypropylene, microcrystalline wax, Fischer-Tropsch wax, and paraffin wax; oxides of aliphatic hydrocarbon waxes such as oxidized polyethylene wax, or block copolymers thereof; saturated straight-chain fatty acids such as palmitic acid, stearic acid, and montanic acid; unsaturated fatty acids such as brassidic acid, eleostearic acid, and parinaric acid; saturated alcohols such as stearyl alcohol, aralkyl alcohol, behenyl alcohol, carnaubyl alcohol, ceryl alcohol, and melissyl alcohol; polyhydric alcohols such as sorbitol; fatty acid amides such as linoleic acid amide, oleic acid amide, and lauric acid amide; methylene bisstearin Examples of such waxes include saturated fatty acid bisamides such as ethylene biscapric acid amide, ethylene bislauric acid amide, and hexamethylene bisstearic acid amide; unsaturated fatty acid amides such as ethylene bisoleic acid amide, hexamethylene bisoleic acid amide, N,N'dioleyl adipic acid amide, and N,N'dioleyl sebacic acid amide; aromatic bisamides such as m-xylene bisstearic acid amide and N,N'distearyl isophthalic acid amide; fatty acid metal salts (commonly known as metal soaps) such as calcium stearate, calcium laurate, zinc stearate, and magnesium stearate; and waxes obtained by grafting aliphatic hydrocarbon waxes with vinyl monomers such as styrene and acrylic acid. The waxes can be used alone or in combination of two or more.

[0096] Of these, it is preferable to contain a hydrocarbon wax.

[0097] The content of the wax is preferably 0.5 parts by mass or more and 20.0 parts by mass or less with respect to 100.0 parts by mass of the binder resin.

[0098] The toner particles may contain a colorant. The colorant is not particularly limited, and the following known colorants can be used.

[0099] Examples of yellow pigments that can be used include condensed azo compounds such as yellow iron oxide, navel yellow, naphthol yellow S, Hansa yellow G, Hansa yellow 10G, benzidine yellow G, benzidine yellow GR, quinoline yellow lake, permanent yellow NCG, and tartrazine lake, isoindolinone compounds, anthraquinone compounds, azo metal complexes, methine compounds, and allylamide compounds. Specific examples include the following.

[0100] CI Pigment Yellow 12, 13, 14, 15, 17, 62, 74, 83, 93, 94, 95, 109, 110, 111, 128, 129, 147, 155, 168, 180.

[0101] Orange pigments include the following:

[0102] Permanent Orange GTR, Pyrazolone Orange, Balkan Orange, Benzidine Orange G, Induthrene Brilliant Orange RK, Induthrene Brilliant Orange GK.

[0103] Examples of red pigments include condensed azo compounds such as red iron oxide, permanent red 4R, lithol red, pyrazolone red, watching red calcium salt, lake red C, lake D, brilliant carmine 6B, brilliant carmine 3B, eoxin lake, rhodamine lake B, and alizarin lake, diketopyrrolopyrrole compounds, anthraquinone compounds, quinacridone compounds, basic dye lake compounds, naphthol compounds, benzimidazolone compounds, thioindigo compounds, and perylene compounds. Specific examples include the following.

[0104] CI Pigment Red 2, 3, 5, 6, 7, 23, 48:2, 48:3, 48:4, 57:1, 81:1, 122, 144, 146, 166, 169, 177, 184, 185, 202, 206, 220, 221, 254.

[0105] Examples of blue pigments include alkali blue lake, Victoria blue lake, phthalocyanine blue, metal-free phthalocyanine blue, phthalocyanine blue partial chloride, fast sky blue, copper phthalocyanine compounds such as indanthrene blue BG and their derivatives, anthraquinone compounds, basic dye lake compounds, etc. Specific examples include the following.

[0106] CI Pigment Blue 1, 7, 15, 15:1, 15:2, 15:3, 15:4, 60, 62, 66.

[0107] Purple pigments include Fast Violet B and Methyl Violet Lake.

[0108] Green pigments include Pigment Green B, Malachite Green Lake, and Final Yellow Green G. White pigments include zinc oxide, titanium oxide, antimony white, and zinc sulfide.

[0109] Examples of black pigments include carbon black, aniline black, non-magnetic ferrite, magnetite, and pigments toned to black using the above-mentioned yellow, red and blue colorants. These colorants can be used alone or in combination, or in the form of a solid solution. If necessary, the colorants may be surface-treated.

[0110] The content of the colorant is preferably 1.0 part by mass or more and 15.0 parts by mass or less with respect to 100.0 parts by mass of the binder resin.

[0111] The toner particles may contain a charge control agent. Any known charge control agent can be used as the charge control agent. In particular, a charge control agent that has a high charging speed and can stably maintain a constant charge amount is preferred. Furthermore, when the toner particles are produced by a direct polymerization method, a charge control agent that has low polymerization inhibition properties and is substantially free of solubilized matter in an aqueous medium is particularly preferred.

[0112] As the charge control agent that controls the toner particles to have a negative charge, the following can be mentioned.

[0113] Organometallic compounds and chelating compounds include monoazo metal compounds, acetylacetone metal compounds, aromatic oxycarboxylic acids, aromatic dicarboxylic acids, oxycarboxylic acids and dicarboxylic acid-based metal compounds. Other examples include aromatic oxycarboxylic acids, aromatic mono- and polycarboxylic acids and their metal salts, anhydrides or esters, and phenol derivatives such as bisphenol. Further examples include urea derivatives, metal-containing salicylic acid compounds, metal-containing naphthoic acid compounds, boron compounds, quaternary ammonium salts, and calixarenes.

[0114] On the other hand, examples of charge control agents that control the toner particles to have a positive charge include the following.

[0115] Nigrosine and nigrosine modifications such as fatty acid metal salts; guanidine compounds; imidazole compounds; onium salts such as quaternary ammonium salts such as tributylbenzylammonium-1-hydroxy-4-naphthosulfonate, tetrabutylammonium tetrafluoroborate, and their analogues such as phosphonium salts, and lake pigments thereof; triphenylmethane dyes and lake pigments thereof (lake agents include phosphotungstic acid, phosphomolybdic acid, phosphotungstomolybdic acid, tannic acid, lauric acid, gallic acid, ferricyanide, ferrocyanide, etc.); metal salts of higher fatty acids; resin-based charge control agents.

[0116] These charge control agents may be contained alone or in combination of two or more. The content of these charge control agents is preferably 0.01 parts by mass or more and 10 parts by mass or less with respect to 100 parts by mass of the binder resin.

[0117] The toner particles may be used as they are as a toner, but in order to improve flowability, chargeability, cleaning properties, etc., so-called external additives such as a fluidizing agent and a cleaning aid may be added to the toner.

[0118] Examples of the external additive include inorganic oxide fine particles such as silica fine particles, alumina fine particles, and titanium oxide fine particles, inorganic stearic acid compound fine particles such as aluminum stearate fine particles and zinc stearate fine particles, and inorganic titanic acid compound fine particles such as strontium titanate and zinc titanate. These may be used alone or in combination of two or more.

[0119] These inorganic particles may be surface-treated with a silane coupling agent, a titanium coupling agent, a higher fatty acid, a silicone oil, etc., to improve heat resistance and storage stability and environmental stability. The BET specific surface area of ​​the external additive is 10 m 2 / g or more 450m 2 It is preferable that the molecular weight is not more than 1 / g.

[0120] The BET specific surface area can be determined by a low-temperature gas adsorption method using a dynamic constant pressure method in accordance with the BET method (preferably the BET multipoint method). For example, a specific surface area measuring device (product name: Gemini 2375 Ver. 5.0, manufactured by Shimadzu Corporation) is used to adsorb nitrogen gas onto the surface of a sample, and the BET multipoint method is used to measure the BET specific surface area (m 2 / g) can be calculated.

[0121] The content of these various external additives is preferably 0.05 parts by mass or more and 10 parts by mass or less, more preferably 0.1 parts by mass or more and 5 parts by mass or less, based on 100 parts by mass of the toner particles. In addition, various external additives may be used in combination.

[0122] The toner can be used as a magnetic or non-magnetic one-component developer, but may also be mixed with a carrier and used as a two-component developer.

[0123] As the carrier, for example, a magnetic material made of a known material such as a metal such as iron, ferrite, magnetite, or an alloy of such a metal with a metal such as aluminum or lead can be used. Of these, it is preferable to use ferrite. In addition, as the carrier, a coated carrier in which the surface of a magnetic material is coated with a coating agent such as a resin, or a resin dispersion type carrier in which magnetic fine particles are dispersed in a binder resin may be used.

[0124] The carrier preferably has a volume average particle size of 15 μm or more and 100 μm or less, and more preferably has a volume average particle size of 25 μm or more and 80 μm or less.

[0125] Known methods can be used for producing toner particles. For example, a dry production method such as a kneading and grinding method or a wet production method can be used. From the viewpoint of uniformity of particle size and shape controllability, a wet production method can be preferably used. Further, examples of the wet production method include a suspension polymerization method, a dissolution suspension method, an emulsion polymerization aggregation method, and an emulsion aggregation method.

[0126] For example, when toner particles are manufactured by a kneading and pulverizing method, a binder resin, resin A, resin B, and wax, as well as a colorant, a charge control agent, and other additives as necessary, are thoroughly mixed in a mixer such as a Henschel mixer, a ball mill, etc. Then, various materials are melt-kneaded using a thermal kneader such as a heating roll, a kneader, or an extruder to disperse or dissolve them, and toner particles are obtained through a cooling and solidifying process, a pulverizing process, a classification process, and a surface treatment process as necessary.

[0127] In the pulverization step, a known pulverization device such as a mechanical impact type or a jet type may be used. The order of the classification step and the surface treatment step is not important. In the classification step, it is preferable to use a multi-division classifier in terms of production efficiency.

[0128] Next, a description will be given of a case where toner particles are produced by a suspension polymerization method, which is a wet production method.

[0129] Hereinafter, examples of producing toner particles using the suspension polymerization method will be described step by step, but the present invention is not limited thereto.

[0130] (Preparation process of polymerizable monomer composition) In the suspension polymerization method, first, a polymerizable monomer for producing a binder resin, resin A, resin B, wax, and, if necessary, a colorant, a charge control agent, a crosslinking agent, a polymerization initiator, and other additives are uniformly dissolved or dispersed using a dispersing machine such as a ball mill or an ultrasonic dispersing machine to obtain a polymerizable monomer composition. Examples of the polymerizable monomer include those exemplified as the monomer for forming the styrene-acrylic acid copolymer described above.

[0131] (Dispersion process of polymerizable monomer composition (granulation process)) Next, the polymerizable monomer composition is charged into a previously prepared aqueous medium, and droplets of the polymerizable monomer composition are granulated to a desired toner particle size using a stirrer or disperser having high shear force.

[0132] The aqueous medium in the granulation step preferably contains a dispersion stabilizer in order to control the particle size of the toner particles, to sharpen the particle size distribution, and to suppress the coalescence of toner particles during the production process.

[0133] Dispersion stabilizers are generally broadly classified into polymers that exert a repulsive force due to steric hindrance and poorly water-soluble inorganic compounds that stabilize dispersion by electrostatic repulsive force.

[0134] Fine particles of poorly water-soluble inorganic compounds are preferably used because they dissolve in acids or alkalis and can be easily removed by washing with acids or alkalis after polymerization.

[0135] As the dispersion stabilizer of the poorly water-soluble inorganic compound, one containing any one of magnesium, calcium, barium, zinc, aluminum, and phosphorus is preferably used. More preferably, one containing any one of magnesium, calcium, aluminum, and phosphorus is desired. Specifically, the following can be mentioned.

[0136] Magnesium phosphate, tricalcium phosphate, aluminum phosphate, zinc phosphate, magnesium carbonate, calcium carbonate, magnesium hydroxide, calcium hydroxide, aluminum hydroxide, calcium metasilicate, calcium sulfate, barium sulfate, hydroxyapatide. When using the poorly water-soluble inorganic dispersant, it may be used as is, but in order to obtain finer particles, the inorganic dispersant particles can be generated in an aqueous medium and used. For example, in the case of tricalcium phosphate, a sodium phosphate aqueous solution and a calcium chloride aqueous solution are mixed under high speed stirring to generate water-insoluble calcium phosphate, which enables more uniform and fine dispersion.

[0137] The dispersion stabilizer may be used in combination with an organic compound such as polyvinyl alcohol, gelatin, methyl cellulose, methylhydroxypropyl cellulose, ethyl cellulose, sodium salt of carboxymethyl cellulose, or starch. These dispersion stabilizers are preferably used in an amount of 0.1 to 20.0 parts by mass per 100 parts by mass of the polymerizable monomer.

[0138] Furthermore, in order to make these dispersion stabilizers finer, a surfactant may be used in an amount of 0.1 to 10.0 parts by mass relative to 100 parts by mass of the polymerizable monomer. Specifically, commercially available nonionic, anionic, or cationic surfactants can be used. For example, sodium dodecyl sulfate, sodium tetradecyl sulfate, sodium pentadecyl sulfate, sodium octyl sulfate, sodium oleate, sodium laurate, potassium stearate, and calcium oleate are preferably used.

[0139] (Polymerization process) After the granulation step or while the granulation step is being carried out, the temperature is preferably set to 50° C. or more and 90° C. or less to polymerize the polymerizable monomers contained in the polymerizable monomer composition, thereby obtaining a toner particle dispersion liquid.

[0140] In the polymerization step, it is preferable to carry out a stirring operation so that the temperature distribution in the vessel becomes uniform. When a polymerization initiator is added, it can be added at any timing and for any required time. In addition, the temperature may be raised in the latter half of the polymerization reaction in order to obtain a desired molecular weight distribution, and further, in order to remove unreacted polymerizable monomers, by-products, etc. from the system, a part of the aqueous medium may be distilled off by a distillation operation in the latter half of the reaction or after the reaction is completed. The distillation operation can be carried out under normal pressure or reduced pressure.

[0141] The polymerization initiator used in the suspension polymerization method preferably has a half-life of 0.5 to 30 hours during the polymerization reaction. When the polymerization reaction is carried out using an initiator in an amount of 0.5 to 20 parts by mass relative to 100 parts by mass of the polymerizable monomer, a polymer having a molecular weight maximum between 5,000 and 50,000 can be obtained.

[0142] As the polymerization initiator, an oil-soluble initiator is generally used, for example, the following:

[0143] Examples of the initiator include azo compounds such as 2,2'-azobisisobutyronitrile, 2,2'-azobis-2,4-dimethylvaleronitrile, 1,1'-azobis(cyclohexane-1-carbonitrile), and 2,2'-azobis-4-methoxy-2,4-dimethylvaleronitrile; and peroxide initiators such as acetylcyclohexylsulfonyl peroxide, diisopropyl peroxycarbonate, decanonyl peroxide, lauroyl peroxide, stearoyl peroxide, propionyl peroxide, acetyl peroxide, tert-butylperoxy-2-ethylhexanoate, benzoyl peroxide, tert-butylperoxyisobutyrate, cyclohexanone peroxide, methyl ethyl ketone peroxide, dicumyl peroxide, tert-butyl hydroperoxide, di-tert-butyl peroxide, tert-butyl peroxypivalate, and cumene hydroperoxide.

[0144] As the polymerization initiator, a water-soluble initiator may be used as necessary, and examples thereof include the following.

[0145] Ammonium persulfate, potassium persulfate, 2,2'-azobis(N,N'-dimethyleneisobutyromidine) hydrochloride, 2,2'-azobis(2-aminodinopropane) hydrochloride, azobis(isobutylamidine) hydrochloride, 2,2'-azobisisobutyronitrile sodium sulfonate, ferrous sulfate, or hydrogen peroxide.

[0146] These polymerization initiators can be used alone or in combination of two or more. In order to control the degree of polymerization of the polymerizable monomer, it is also possible to further add a chain transfer agent, a polymerization inhibitor, etc.

[0147] (Solid-liquid separation process, washing process and drying process) For the purpose of removing the dispersion stabilizer attached to the surface of the toner particles, the toner particle dispersion may be treated with an acid or an alkali.

[0148] The solid-liquid separation for obtaining toner particles from the obtained toner particle dispersion can be performed by a general filtration method, and then, in order to remove foreign matter that has not been completely removed from the toner particle surface, it is preferable to perform further washing by reslurrying or washing with washing water. After sufficient washing, solid-liquid separation is performed again to obtain a toner cake. Thereafter, the toner is dried by a known drying means, and if necessary, a particle group having a particle size other than the specified particle size is separated by classification to obtain toner particles. The particle group having a particle size other than the specified particle size separated at this time may be reused to improve the final yield.

[0149] (External addition process) If necessary, an external additive may be added to the obtained toner particles. The external addition step is carried out by putting the external additive and the toner particles into a mixer equipped with a blade rotating at high speed and thoroughly mixing them.

[0150] When toner particles are obtained by the dissolution suspension method, a resin solution is prepared by uniformly dissolving or dispersing a binder resin, resin A, resin B, and wax, as well as other materials such as a colorant and a charge control agent, if necessary, in an organic solvent. The obtained resin solution is dispersed in an aqueous medium and granulated, and the organic solvent contained in the granulated particles is removed to obtain toner particles having a desired particle size.

[0151] The obtained toner particles may be subjected to a solid-liquid separation step, a washing step, a drying step, and an external addition step, if necessary, in the same manner as in the above-mentioned suspension polymerization method.

[0152] The organic solvent used in the resin solution in the dissolution suspension method is not particularly limited as long as it is compatible with the raw materials of the toner particles, such as the binder resin, resin A, resin B, and wax. From the viewpoint of solvent removal, however, it is preferable that the organic solvent has a certain degree of vapor pressure even at or below the boiling point of water.

[0153] For example, toluene, xylene, ethyl acetate, butyl acetate, methyl ethyl ketone, methyl isobutyl ketone, etc. can be used.

[0154] When obtaining toner particles by the emulsion aggregation method, first, fine particles of binder resin, fine particles of resin A, fine particles of wax, and, if necessary, fine particles of other materials such as colorant and charge control agent are dispersed and mixed in an aqueous medium containing a dispersion stabilizer. A surfactant may be added to the aqueous medium. Then, a known aggregating agent is added to aggregate the particles to the desired toner particle size, and then or simultaneously with the aggregation, the resin fine particles are fused together. If necessary, shape control is performed by heat.

[0155] The obtained toner particles may be subjected to a solid-liquid separation process, a washing process, a drying process, and an external addition process as necessary in the same manner as the suspension polymerization method. In the washing process, impurities in the toner particles can be removed by repeatedly washing and filtering the obtained particles. Specifically, it is preferable to wash the toner particles using an aqueous solution containing a chelating agent such as ethylenediaminetetraacetic acid (EDTA) and its Na salt, and further wash the toner particles several times with pure water.

[0156] From the viewpoint of obtaining a high-definition and high-resolution image, the toner particles and the particle size of the toner preferably have a weight average particle size of 3.0 μm or more and 10.0 μm or less. The weight average particle size of the toner particles and the toner can be measured by a capillary electrical resistance method. For example, it can be measured using a "Coulter Counter Multisizer 3" (manufactured by Beckman Coulter, Inc.).

[0157] The methods for measuring the various physical properties of the toner will be described below.

[0158] <Method for measuring the glass transition temperature (Tg) of toner> The glass transition temperature (Tg) of the toner is measured in accordance with ASTM D3418-82 using a differential scanning calorimeter "Q1000" (manufactured by TA Instruments). The melting points of indium and zinc are used for temperature correction of the detector of the device, and the heat of fusion of indium is used for heat correction. Specifically, 10 mg of toner is precisely weighed and placed in an aluminum pan, and an empty aluminum pan is used as a reference, and measurement is performed at a temperature rise rate of 10°C / min in the measurement temperature range of 30 to 200°C. In the measurement, the temperature is raised to 200°C once, then lowered to 30°C, and then raised again. During this second temperature rise process, a specific heat change is obtained in the temperature range of 40°C to 100°C. The intersection of the line at the midpoint of the baseline before and after the specific heat change occurs and the differential heat curve is taken as the glass transition temperature (Tg) of the binder resin.

[0159] <Method of measuring weight average particle size (D4) of toner> The weight average particle diameter (D4) of the toner is calculated as follows. The measurement device used is a precision particle size distribution measurement device using the pore electrical resistance method, "Coulter Counter Multisizer 3" (registered trademark, manufactured by Beckman Coulter, Inc.), equipped with a 100 μm aperture tube. The measurement conditions are set and the measurement data is analyzed using the accompanying dedicated software "Beckman Coulter Multisizer 3 Version 3.51" (manufactured by Beckman Coulter, Inc.). The measurement is performed with an effective measurement channel count of 25,000 channels.

[0160] The aqueous electrolyte solution used for the measurement is prepared by dissolving special grade sodium chloride in ion-exchanged water to a concentration of 1% by mass, for example, "ISOTON II" (manufactured by Beckman Coulter).

[0161] Before carrying out the measurements and analyses, the dedicated software is set up as follows.

[0162] In the "Change Standard Measurement Method (SOM)" screen of the dedicated software, set the total count number in the control mode to 50,000 particles, the number of measurements to 1, and the Kd value to the value obtained using "Standard Particle 10.0 μm" (Beckman Coulter). Press the "Threshold / Noise Level Measurement Button" to automatically set the threshold and noise level. In addition, set the current to 1600 μA, the gain to 2, the electrolyte to ISOTON II, and check "Flush aperture tube after measurement."

[0163] In the "Pulse to particle size conversion setting" screen of the dedicated software, the bin interval is set to logarithmic particle size, the particle size bin is set to 256 particle size bins, and the particle size range is set to 2 μm to 60 μm.

[0164] The specific measurement method is as follows.

[0165] (1) Pour 200 ml of the electrolyte solution into a 250 ml round-bottom glass beaker made exclusively for the Multisizer 3, set it on the sample stand, and stir the stirrer rod counterclockwise at 24 revolutions per second. Then, remove dirt and air bubbles from inside the aperture tube using the "Aperture Tube Flush" function of the dedicated software. (2) 30 ml of the electrolyte solution is placed in a 100 ml flat-bottom glass beaker, and 0.3 ml of a dilution of "Contaminon N" (a 10% aqueous solution of a pH 7 neutral detergent for cleaning precision measuring instruments made of a nonionic surfactant, anionic surfactant, and organic builder, manufactured by Wako Pure Chemical Industries, Ltd.) diluted 3 times by mass with ion-exchanged water is added as a dispersant. (3) Prepare an ultrasonic disperser "Ultrasonic Dispersion System Tetora150" (manufactured by Nikkaki Bios Co., Ltd.) that has two built-in oscillators with an oscillation frequency of 50 kHz and a phase shift of 180 degrees, and has an electrical output of 120 W. Place 3.3 L of ion-exchanged water in the ultrasonic disperser's water tank, and add 2 mL of Contaminon N to this water tank. (4) The beaker (2) is set in the beaker fixing hole of the ultrasonic disperser, and the ultrasonic disperser is operated. Then, the height position of the beaker is adjusted so that the resonance state of the liquid surface of the electrolyte solution in the beaker is maximized. (5) While the electrolyte solution in the beaker in (4) is irradiated with ultrasonic waves, 10 mg of toner is added little by little to the electrolyte solution and dispersed. Then, ultrasonic dispersion treatment is continued for another 60 seconds. During ultrasonic dispersion, the water temperature in the water tank is appropriately adjusted to be 10°C or higher and 40°C or lower. (6) Using a pipette, the electrolytic solution (5) in which the toner is dispersed is dropped into the round-bottom beaker (1) placed in the sample stand, and the measurement concentration is adjusted to 5%. Then, measurements are continued until the number of particles measured reaches 50,000. (7) The measurement data is analyzed using the dedicated software that comes with the device, and the weight-average particle diameter (D4) is calculated. Note that when the dedicated software is set to Graph / Volume%, the "Average diameter" on the "Analysis / Volume Statistics (Arithmetic Mean)" screen is the weight-average particle diameter (D4).

[0166] <Separation of toner and additives> In the case of a toner having an external additive on the surface of the toner particles, the toner particles and the external additive are separated by the following method to obtain toner particles.

[0167] Add 160 g of sucrose (Kishida Chemical) to 100 mL of ion-exchanged water and dissolve in a hot water bath to prepare a concentrated sucrose solution. Add 31 g of the concentrated sucrose solution and 6 mL of Contaminon N (a 10% aqueous solution of a pH 7 neutral detergent for cleaning precision measuring instruments, consisting of a nonionic surfactant, an anionic surfactant, and an organic builder, manufactured by Wako Pure Chemical Industries, Ltd.) to a centrifuge tube (volume 50 mL) to prepare a dispersion. Add 1.0 g of toner to this dispersion and break up the toner clumps with a spatula or the like.

[0168] The centrifuge tube is shaken in a shaker at 350 strokes per minute (spm) for 20 minutes. After shaking, the solution is transferred to a glass tube for a swing rotor (50 mL capacity) and separated in a centrifuge (H-9R, manufactured by Kokusan Co., Ltd.) at 3500 rpm for 30 minutes. This operation separates the toner particles from the removed external additives. It is visually confirmed that the toner and the aqueous solution are sufficiently separated, and the toner separated in the top layer is collected with a spatula or the like. The collected toner particles are filtered with a vacuum filter and then dried in a dryer for at least 1 hour to obtain toner particles. This operation is carried out multiple times to obtain the required amount of toner particles.

[0169] <Method of extracting resin A from toner particles> Resin A in the toner particles is extracted by separating the extract using tetrahydrofuran (THF) using a solvent gradient elution method. The preparation method is shown below.

[0170] Weigh out 10.0 g of toner particles, place them in a cylindrical filter paper (Toyo Roshi No. 84) and place them in a Soxhlet extractor. Extract for 20 hours using 200 mL of THF as the solvent, and the solid obtained by removing the solvent from the extract is the THF-soluble fraction. The THF-soluble fraction contains resin A. Repeat this process multiple times to obtain the required amount of THF-soluble fraction.

[0171] For the solvent gradient elution method, gradient preparative HPLC (Shimadzu LC-20AP high pressure gradient preparative system, Waters SunFire preparative column 50 mm φ 250 mm) is used. The column temperature is 30°C, the flow rate is 50 mL / min, and THF, chloroform, and toluene are appropriately selected as good solvents for the mobile phase, and acetonitrile, acetone, methanol, and n-hexane are appropriately selected as poor solvents. 0.02 g of the THF soluble fraction is dissolved in 1.5 ml of good solvent and used as a sample for gradient preparative HPLC. The mobile phase starts with a composition of 100% poor solvent, and 5 minutes after the sample injection, the ratio of good solvent is increased by 4% every minute, until the composition of the mobile phase is 100% good solvent over 25 minutes. The obtained fraction is dried to obtain resin A. Which fractional section is resin A can be determined by measuring the silicon atom content described later, and 13 This can be determined by C-NMR measurement. If necessary, the solvent gradient elution is repeated to obtain the required amount of resin A.

[0172] <Method for measuring the content of silicon atoms in resin A> The content of silicon atoms in resin A is measured using a wavelength dispersive X-ray fluorescence analyzer "Axios" (PANalytical). The measurement conditions are set and the measurement data is analyzed using the accompanying dedicated software "SuperQ ver.4.0F" (PANalytical).

[0173] The anode of the X-ray tube is Rh, and the acceleration voltage and current are 24 kV and 100 mA, respectively.

[0174] The measurement atmosphere is vacuum, the measurement diameter (collimator mask diameter) is 27 mm, and the measurement time is 10 seconds. A proportional counter (PC) is used as the detector. The measurement is performed by measuring the count rate (unit: cps) of Si-Kα rays observed at a diffraction angle (2θ) = 109.08° when PET is used as the analyzing crystal, and calculating using the following calibration curve.

[0175] As the measurement sample, resin A (or the resin represented by formula (1)) itself is used, or a resin extracted from toner particles by the above-mentioned extraction method is used.

[0176] The pellets for measurement are made using a tablet molding and compression machine "BRE-32" (Maekawa Testing Machinery Manufacturing Co., Ltd.) 4 g of the measurement sample is placed in a dedicated aluminum ring for pressing, flattened, and pressed at 20 MPa for 60 seconds to form pellets with a thickness of 2 mm and a diameter of 39 mm.

[0177] As pellets for creating a calibration curve to determine the content, binder [product name: Spectro Blend, components: C 81.0, O 2.9, H 13.5, N 2.6 (mass%), chemical formula: C 19 H 38 To 100 parts by mass of SiO2 (hydrophobic fumed silica) [product name: AEROSIL NAX50, specific surface area: 40±10, carbon content: 0.45-0.85%; manufactured by Nippon Aerosil Co., Ltd.], add 0.50 parts by mass of SiO2, mix thoroughly using a coffee mill, and mold into pellets. In the same manner, mix and mold into pellets so that the SiO2 amounts are 5.00 parts by mass, 10.00 parts by mass, and 15.00 parts by mass, respectively.

[0178] A linear calibration curve is obtained by plotting the count rate of the obtained X-rays on the vertical axis and the concentration of Si added in each calibration sample on the horizontal axis.

[0179] Next, the count rate of the Si-Kα ray is measured for the measurement sample in the same manner, and the silicon atom content (mass%) is calculated from the obtained calibration curve.

[0180] <Confirmation of the structure of the resin represented by formula (1) (R 1 ~R 3 )> R in the resin represented by formula (1) 1 ~R 3 The structure of 29 Si-NMR (solid state) measurement, and 13 The measurement conditions are as follows: Resin A (or the resin represented by formula (1)) itself is used as a measurement sample, or a resin extracted from a toner particle by the above-mentioned extraction method is used.

[0181] ( 29 Si-NMR (solid state) measurement conditions Equipment: JEOL RESONANCE JNM-ECX500II Sample tube: 3.2mmφ Sample size: 150mg Measurement temperature: room temperature Pulse mode: CP / MAS Measurement nuclear frequency: 97.38MHz ( 29 Si) Reference material: DSS (external standard: 1.534ppm) Sample rotation speed: 10kHz Contact time: 10ms Delay time: 2s Number of times: 2000 to 8000

[0182] By the above measurement, the abundance ratio of multiple silane components according to the number of oxygen atoms bonded to silicon can be obtained by peak separation and integration by curve fitting. In this way, the R 1 ~R 3 The number of alkoxy or hydroxy groups can be confirmed.

[0183] ( 13 C-NMR (solid state) measurement conditions Equipment: JEOL RESONANCE JNM-ECX500II Sample tube: 3.2mmφ Sample size: 150mg Measurement temperature: room temperature Pulse mode: CP / MAS Measurement nuclear frequency: 123.25MHz ( 13 C) Reference substance: Adamantane (external standard: 29.5ppm) Sample rotation speed: 20kHz Contact time: 2ms Delay time: 2s Number of times accumulated: 1024

[0184] By the above measurement, R in formula (1) 1 ~R 3 The various peaks are separated according to the type of 1 ~R 3 Determine the structure of.

[0185] <Confirmation of the structure of resin A (polymer portion and L in formula (1) 1 )> The polymer moiety in resin A and L in formula (1) 1 The structure of 13 This can be confirmed by C-NMR (solid state) measurement. The measurement conditions are as above ( 13 The measurement conditions are the same as those for C-NMR (solid). The measurement sample is either Resin A (or the resin represented by formula (1)) itself, or a resin extracted from a toner particle by the above-mentioned extraction method.

[0186] By the above measurement, the polymer moiety in resin A and L in formula (1) 1 The peaks are separated according to the type of the compound, and each peak is identified to identify the polymer moiety in resin A and the L 1 Determine the structure of.

[0187] <Method of extracting resin B from toner particles> On the other hand, resin B in the toner particles is extracted by separating the extract using THF using a solvent gradient elution method. The required amount of THF-soluble matter is obtained by the same operation as in the above <Method for extracting resin A from toner particles>. The THF-soluble matter contains resin B.

[0188] For the mobile phase, THF, chloroform, or toluene is appropriately selected as a good solvent, and acetone or methanol is appropriately selected as a poor solvent. The fractions are dried and solidified in the same manner as in the above <Method of extracting resin A from toner particles> to obtain resin B. Which fractional section is the crystalline polyester that constitutes resin B can be determined by: 1 H-NMR analysis, 13 The type and structure of the crystalline polyester contained in the resin B in the toner particles can be identified by known analytical methods such as C-NMR analysis, FT-IR analysis, GC-MS analysis, and GPC analysis. The type and structure of the crystalline polyester contained in the resin B in the toner particles can be identified by the above analytical methods. The resin B may be obtained by synthesizing the resin B separately.

[0189] <Method of measuring weight average molecular weight (Mw)> The weight average molecular weight (Mw) of the resin A, the resin B, or the toner particles is measured by gel permeation chromatography (GPC) as follows.

[0190] First, the sample is dissolved in tetrahydrofuran (THF) at room temperature for 24 hours. The resulting solution is then filtered through a solvent-resistant membrane filter "Myshoridisc" (manufactured by Tosoh Corporation) with a pore size of 0.2 μm to obtain a sample solution. The sample solution is prepared so that the concentration of components soluble in THF is 0.8 mass%. This sample solution is used to perform measurements under the following conditions. Equipment: HLC8120 GPC (detector: RI) (Tosoh Corporation) Column: Shodex KF-801, 802, 803, 804, 805, 806, 807 (Showa Denko) Eluent: tetrahydrofuran (THF) Flow rate: 1.0mL / min Oven temperature: 40.0℃ Sample injection volume: 0.10 mL

[0191] In calculating the molecular weight of the sample, a molecular weight calibration curve prepared using standard polystyrene resins (product names: "TSK Standard Polystyrene F-850, F-450, F-288, F-128, F-80, F-40, F-20, F-10, F-4, F-2, F-1, A-5000, A-2500, A-1000, A-500", manufactured by Tosoh Corporation) is used.

[0192] <Method for measuring the acid value of resin> The acid value is the number of milligrams of potassium hydroxide required to neutralize the acid contained in 1 g of a sample. The acid value of a resin is measured in accordance with JIS K 0070-1992, and specifically, it is measured according to the following procedure.

[0193] (1) Preparation of reagents Dissolve 1.0 g of phenolphthalein in 90 mL of ethyl alcohol (95% by volume), and add ion-exchanged water to make 100 mL to obtain a phenolphthalein solution.

[0194] Dissolve 7 g of special grade potassium hydroxide in 5 mL of water and add ethyl alcohol (95% by volume) to make 1 L. Place in an alkali-resistant container to avoid contact with carbon dioxide, etc., leave for 3 days, then filter to obtain potassium hydroxide solution. Store the resulting potassium hydroxide solution in an alkali-resistant container.

[0195] The factor of the potassium hydroxide solution is calculated by taking 25 mL of 0.1 mol / L hydrochloric acid in an Erlenmeyer flask, adding a few drops of the phenolphthalein solution, titrating with the potassium hydroxide solution, and calculating the amount of the potassium hydroxide solution required for neutralization. The 0.1 mol / L hydrochloric acid used is prepared in accordance with JIS K 8001-1998.

[0196] (2) Operation (A) Main Test Weigh out 2.0 g of the crushed sample into a 200 ml Erlenmeyer flask, add 100 ml of a toluene / ethanol (2:1) mixed solution, and dissolve for 5 hours. Next, add a few drops of the phenolphthalein solution as an indicator, and titrate with the potassium hydroxide solution. The end point of the titration is when the light red color of the indicator continues for about 30 seconds. (B) Blank test The titration is carried out in the same manner as above, except that no sample is used (i.e., only the toluene / ethanol (2:1) mixed solution is used).

[0197] (3) The obtained result is substituted into the following formula to calculate the acid value. A = [(CB) × f × 5.61] / S Here, A is the acid value (mgKOH / g), B is the amount of potassium hydroxide solution added for the blank test (ml), C is the amount of potassium hydroxide solution added for the main test (ml), f is the factor of the potassium hydroxide solution, and S is the mass of the sample (g).

[0198] <Measuring method for melting point of resin B> The melting point of resin B (peak temperature of maximum endothermic peak) is measured using a differential scanning calorimeter "Q1000" (manufactured by TA Instruments) in accordance with ASTM D3418-82. The melting points of indium and zinc are used for temperature correction of the detector of the device, and the heat of fusion of indium is used for heat correction. Specifically, 10 mg of toner is precisely weighed and placed in an aluminum pan, and an empty aluminum pan is used as a reference, and measurement is performed at a temperature rise rate of 10°C / min in the measurement temperature range of 30 to 200°C. In the measurement, the temperature is raised to 200°C once, then lowered to 30°C, and then raised again. The maximum endothermic peak of the DSC curve in the temperature range of 30 to 200°C during this second temperature rise process is taken as the melting point of resin B of the present invention.

[0199] <How to calculate the ratio (a / b) of the content a of resin A to the content b of resin B> The content a of resin A in the toner can be obtained in the process of extracting resin A from the toner. The content a of resin A in the toner can be calculated from the weighed toner mass in the <Method for extracting resin A from toner particles> and the mass of resin A obtained from the toner.

[0200] The content b of resin B in the toner can be determined in the process of extracting resin B from the toner. In the <Method for extracting resin B from toner particles>, the content b of resin B in the toner can be calculated from the weighed toner mass and the mass of resin B obtained from the toner. The ratio (a / b) is calculated from the obtained values ​​of a and b. EXAMPLES

[0201] The present invention will be specifically described below with reference to examples and comparative examples, but the present invention is not limited to these examples and comparative examples. Unless otherwise specified, the "parts" and "%" of each material in the examples and comparative examples are all based on mass.

[0202] <Production Example of Styrene-Acrylic Acid Copolymer (a-1)> A styrene-acrylic acid copolymer (a-1) was produced by the following procedure.

[0203] 100.0 parts of propylene glycol monomethyl ether was heated while replacing with nitrogen, and refluxed at a liquid temperature of 120°C or higher. A mixture of 83.4 parts of styrene, 20.9 parts of butyl acrylate, 1.0 parts of acrylic acid, and 0.6 parts of tert-butyl peroxybenzoate [manufactured by NOF Corp., trade name: Perbutyl Z] as a polymerization initiator was added dropwise over 3 hours. After the dropwise addition was completed, the solution was stirred for 3 hours, and then distilled at normal pressure while raising the liquid temperature to 170°C. After the liquid temperature reached 170°C, the pressure was reduced to 1 hPa, and the solvent was removed by distillation for 1 hour to obtain a resin solid. The resin solid was dissolved in tetrahydrofuran, reprecipitated with n-hexane, and the precipitated solid was filtered off to obtain a styrene-acrylic acid copolymer (a-1).

[0204] The resulting styrene-acrylic acid copolymer (a-1) had an acid value of 10.6 mgKOH / g and a weight average molecular weight (Mw) of 13,000.

[0205] <Production Example of Styrene-Acrylic Acid Copolymer (a-2)> In the production example of styrene-acrylic acid copolymer (a-1), the polymerizable monomers were changed to 82.0 parts of styrene, 10.0 parts of methacrylic acid, and 8.0 parts of acrylic acid, and the amount of the polymerization initiator was changed to 1.0 part, respectively. In the same manner as in the production example of styrene-acrylic acid copolymer (a-1), styrene-acrylic acid copolymer (a-2) was obtained.

[0206] The resulting styrene-acrylic acid copolymer (a-2) had an acid value of 161.0 mgKOH / g and a weight average molecular weight (Mw) of 46,000.

[0207] <Production example of polyester part (a-3)> The polyester portion (a-3) was produced by the following procedure.

[0208] The following materials were charged into a reaction vessel equipped with a pressure reducing device, a water separating device, a nitrogen gas introducing device, a temperature measuring device, and a stirring device, and the reaction was carried out under a nitrogen atmosphere at normal pressure and 200°C for 5 hours. Bisphenol A-propylene oxide 2.1 mole adduct: 39.6 parts Terephthalic acid: 8.0 parts Isophthalic acid: 7.6 parts Tetrabutoxytitanate: 0.1 parts Thereafter, 0.01 part of trimellitic acid and 0.12 part of tetrabutoxy titanate were added, and the mixture was reacted at 220° C. for 3 hours, and then reacted under reduced pressure of 10 to 20 mmHg for 2 hours to obtain a polyester resin (a-3).

[0209] The resulting polyester portion (a-3) had an acid value of 6.1 mgKOH / g and a weight average molecular weight (Mw) of 10,200.

[0210] <Production Examples of Polyester Moieties (a-4) and (a-5)> The polyester moieties (a-4) and (a-5) were produced in the same manner as in the production example of the polyester moiety (a-3), except that the reaction pressure, reaction temperature, and reaction time were appropriately adjusted in order to obtain a lower molecular weight substance or a higher molecular weight substance.

[0211] The resulting polyester portion (a-4) had an acid value of 28.0 mgKOH / g and a weight average molecular weight (Mw) of 3,100.

[0212] The acid value of the resulting polyester portion (a-5) was 1.2 mgKOH / g and the weight average molecular weight (Mw) was 99,500.

[0213] <Resin A: Production Example of Resin (A-1) Represented by Formula (1)> Resin (A-1) represented by formula (1) was produced according to the following procedure.

[0214] 50.00 parts of styrene-acrylic acid copolymer (a-1) was dissolved in 200.00 parts of N,N-dimethylacetamide, and 1.20 parts of 3-aminopropyltriethoxysilane, 2.90 parts of triethylamine, and 2.90 parts of DMT-MM [4-(4,6-dimethoxy-1,3,5-triazin-2-yl)-4-methylmorpholinium chloride] were added as a silane compound, and the mixture was stirred at room temperature for 5 hours. After the reaction was completed, the solution was dropped into methanol, reprecipitated, and filtered to obtain a resin (A-1) represented by formula (1). The weight average molecular weight Mw of the obtained resin (A-1) represented by formula (1) was 13200.

[0215] <Resin A: Production Examples of Resins (A-2) to (A-10), (A-12) to (A-14), (A-16), and (A-18) Represented by Formula (1)> Resins (A-2) to (A-10), (A-12) to (A-14), (A-16) and (A-18) represented by formula (1) were obtained in the same manner as in the production example of resin (A-1) represented by formula (1), except that the type of polymer moiety of resin A, the type and amount of silane compound added, and the amount of triethylamine and DMT-MM added were changed as shown in Table 1.

[0216] <Resin A: Production Example of Resin (A-11) Represented by Formula (1)> A solution of 10.0 parts of resin (A-1) represented by formula (1) dissolved in 90.0 parts of toluene was mixed with 400.0 parts of pure water and stirred, and the pH was adjusted to 4.0 using dilute hydrochloric acid. After stirring at room temperature for 10.8 hours, the stirring was stopped and the mixture was transferred to a separatory funnel to extract the oil phase. The oil phase was concentrated and reprecipitated with methanol to obtain resin (A-11) represented by formula (1).

[0217] The obtained resin (A-11) 29 When analyzed by Si-NMR (solid state) measurement, R in formula (1) of resin (A-11) was 1 ~R 3 were all hydroxy groups.

[0218] <Resin A: Production Example of Resin (A-15) Represented by Formula (1)> Resin (A-15) represented by formula (1) was produced according to the following procedure.

[0219] 50.00 parts of polyester portion (a-3) was dissolved in 500.00 parts of chloroform, and 1.20 parts of 3-isocyanatepropyltriethoxysilane and 1.00 parts of titanium (IV) tetraisopropoxide were added under a nitrogen atmosphere and stirred at room temperature for 5 hours. After the reaction was completed, the solution was dropped into methanol, reprecipitated, and filtered to obtain resin (A-15) represented by formula (1).

[0220] <Resin A: Production Example of Resin (A-17) Represented by Formula (1)> Resin (A-17) represented by formula (1) was obtained in the same manner as in the production example of resin (A-15) represented by formula (1), except that the type of silane compound was changed to 6-isocyanatehexyltriethoxysilane.

[0221] The structures and physical properties of the obtained resin A; resins (A-1) to (A-18) represented by formula (1) are shown in Table 2.

[0222] [Table 1]

[0223] [Table 2]

[0224] <Resin B: Production example of crystalline polyester (B-1)> Resin B (B-1) was produced according to the following procedure.

[0225] The following materials were charged into a reaction vessel equipped with a pressure reducing device, a water separating device, a nitrogen gas introducing device, a temperature measuring device, and a stirring device. 1,6-Hexanediol: 64.2 parts Sebacic acid: 100.0 parts After the system was substituted with nitrogen by a decompression operation, the system was immersed in an oil bath at 160°C with nitrogen flowing. After the raw materials were melted, 0.19 parts of tetrabutyl orthotitanate was added to the system and stirred with a mechanical stirrer for 3 hours. Then, while continuing to stir, the temperature was gradually raised to 180°C under reduced pressure and maintained for another 3.5 hours. When the mixture became viscous, heating was stopped, nitrogen was introduced into the system to cool it, and the reaction was stopped. Chloroform was added to the system to dissolve the product, which was then poured into a large amount of methanol. The precipitate was filtered and vacuum dried to obtain resin B (B-1). The weight average molecular weight (Mw) of the obtained resin B (B-1) was 20,000 and the melting point was 64°C.

[0226] <Resin B: Production example of crystalline polyester (B-2)> Resin B: Resin B (B-2) was obtained by the same procedure as in the production example of crystalline polyester (B-1), except that 1,6-hexanediol was replaced with 110.0 parts of 1,12-dodecanediol. The weight average molecular weight (Mw) of the obtained resin B (B-2) was 20300 and the melting point was 83°C.

[0227] <Resin B: Production example of resin (B-3) containing crystalline polyester> Into a reaction vessel equipped with a pressure reducing device, a water separating device, a nitrogen gas introducing device, a temperature measuring device, and an agitating device, 64.2 parts of the crystalline polyester (B-1) was placed, and after replacing with nitrogen, 140.0 parts of dehydrated chloroform (manufactured by Kanto Chemical) was added and stirred to completely dissolve.

[0228] Next, while cooling the reaction vessel in an ice bath, 2.3 parts of triethylamine (manufactured by Kanto Chemical Co., Ltd.) that had been dehydrated in advance was added and thoroughly stirred. After that, 7.0 parts of 2-bromoisobutyryl bromide (manufactured by Aldrich Co., Ltd.) was gradually added dropwise while cooling the flask in an ice bath so that the temperature of the solution was kept below 10°C, and after the addition was completed, the mixture was stirred at room temperature for 24 hours under a nitrogen flow. After the stirring was completed, the contents of the reaction vessel were poured into a large amount of ethanol, and the precipitate was collected. The precipitate was dried under reduced pressure to obtain a resin (B-3) precursor containing a crystalline polyester.

[0229] The following ingredients were then charged into the reaction vessel: Styrene: 220.0 parts Crystalline polyester-containing resin (B-3) precursor: 10.0 parts Dimethylformamide: 40.0 parts N,N,N',N”,N”-Pentamethyldiethylenetriamine (PMDETA; Aldrich): 0.4 parts After stirring the inside of the system to dissolve, vacuum freeze degassing treatment was repeated three times using liquid nitrogen, and stirring was performed again to dissolve everything, and then nitrogen replacement was performed for one hour. Then, 0.34 parts of copper bromide (I) (CuBr; manufactured by Aldrich) was added under nitrogen flow, and after stirring for one minute, the polymerization reaction was started in an oil bath at 100°C. The contents of the reaction vessel sampled at different polymerization reaction times were each poured into a large amount of ethanol, and the precipitates were collected. These precipitates were dried under reduced pressure to obtain multiple types of block polymers consisting of styrene and crystalline polyester (B-1). Among the obtained block polymers, one with a weight average molecular weight (Mw) of 32,000 was used as resin (B-3) containing crystalline polyester. The melting point of the resin (B-3) was 66°C.

[0230] <Production Example of Amorphous Polyester Resin C> A non-crystalline polyester resin C was produced according to the following procedure.

[0231] The following materials were charged into a reaction vessel equipped with a pressure reducing device, a water separating device, a nitrogen gas introducing device, a temperature measuring device, and a stirring device, and stirred under a nitrogen atmosphere at normal pressure and 190° C. for 1 hour. Ethylene glycol: 48.6 parts Neopentyl glycol: 65.0 parts Terephthalic acid: 95.7 parts Then, 0.12 parts of dibutyltin oxide was added, and the mixture was reacted at 220°C for 3 hours, and further reacted at 230°C for 4 hours under reduced pressure of 10 to 20 mmHg to obtain amorphous polyester resin C. The obtained amorphous polyester resin C had a glass transition temperature (Tg) of 58°C and a weight average molecular weight (Mw) of 9,800.

[0232] <Production Example of Toner Particle 1> Into a reaction vessel, 390.0 parts of ion-exchanged water and 14.0 parts of sodium phosphate (12-hydrate) (manufactured by Rasa Kogyo Co., Ltd.) were added, and the mixture was kept at 65°C for 1.0 hours while being purged with nitrogen. Next, an aqueous calcium chloride solution in which 9.2 parts of calcium chloride (dihydrate) was dissolved in 10.0 parts of ion-exchanged water was added all at once using a TK homomixer (manufactured by Tokushu Kika Kogyo Co., Ltd.) while stirring at 12,000 rpm, to prepare an aqueous medium containing a dispersion stabilizer. Furthermore, hydrochloric acid was added to the aqueous medium to adjust the pH to 6.0, and aqueous medium 1 was obtained.

[0233] On the other hand, the following materials were placed in an attritor (manufactured by Nippon Coke & Engineering Co., Ltd.), and then zirconia particles having a diameter of 1.7 mm were added and dispersed at 220 rpm for 5.0 hours. After that, the zirconia particles were removed to prepare Dispersion 1 in which the colorant was dispersed. Styrene 60.0 parts Colorant (CI Pigment Blue 15:3) 6.5 parts Next, the following materials were added to the prepared dispersion liquid 1. Styrene 15.0 parts ・25.0 parts n-butyl acrylate Styrene-acrylic acid copolymer (a-1) 4.0 parts Resin A (A-1) 8.0 parts ·Resin B (B-1) 20.0 parts Divinylbenzene 0.6 parts Wax (Fischer-Tropsch wax, melting point: 78°C) 3.0 parts The mixture was kept at 65° C. and uniformly dissolved and dispersed using a TK homomixer at 500 rpm to prepare a polymerizable monomer composition 1.

[0234] While maintaining the temperature of the aqueous medium 1 at 70° C. and the rotation speed of the stirring device at 12,000 rpm, the polymerizable monomer composition 1 was charged into the aqueous medium 1, and 9.0 parts of t-butyl peroxypivalate was added as a polymerization initiator. Granulation was continued for 10 minutes while maintaining the stirring speed at 12,000 rpm.

[0235] The stirring device was changed to a stirrer equipped with a propeller stirring blade, and polymerization was carried out for 5.0 hours while stirring at 150 rpm and maintaining the temperature at 70° C., and then the temperature was raised to 85° C. and maintained at that temperature for 2.0 hours. Thereafter, the aqueous dispersion was cooled to 55° C., maintained at that temperature for 6.0 hours, and then cooled to room temperature to obtain toner particle dispersion 1.

[0236] Hydrochloric acid was added to the obtained toner particle dispersion liquid 1 to adjust the pH to 1.4 or less, and the dispersion stabilizer was dissolved therein. The resulting mixture was filtered, washed, and dried to obtain toner particles 1.

[0237] <Production Example of Toner Particle 2> In a reaction vessel equipped with a reflux condenser, a stirrer, and a nitrogen inlet tube, the following materials were placed under a nitrogen atmosphere. Toluene 100.0 parts Styrene 75.0 parts ・25.0 parts n-butyl acrylate Divinylbenzene 0.6 parts t-Butyl peroxypivalate 3.0 parts The inside of the reaction vessel was stirred at 200 revolutions per minute, heated to 70° C. and maintained for 10 hours, to obtain a resin solution 2.

[0238] Next, ·Resin solution 2 203.6 parts Styrene-acrylic acid copolymer (a-1) 4.0 parts Resin A (A-1) 8.0 parts ·Resin B (B-1) 20.0 parts Wax (Fischer-Tropsch wax, melting point: 78°C) 3.0 parts Colorant (CI Pigment Blue 15:3) 6.5 parts Zirconia particles having a diameter of 1.7 mm were added to the above components and dispersed at 220 rpm for 10.0 hours, after which the zirconia particles were removed to obtain a resin composition solution 2.

[0239] Next, the resin composition solution 2 was added to an aqueous medium 1 obtained by the same operation as in the production of toner particles 1, and a granulation process was carried out for 10 minutes while maintaining the rotation speed at 15,000 rpm in Clearmix, thereby obtaining a resin composition dispersion 2.

[0240] The resin composition dispersion 2 was heated to 95° C. and stirred for 120 minutes to remove toluene from the resin composition dispersion 2. Thereafter, the resin composition dispersion 2 was cooled to 55° C., held at that temperature for 6.0 hours, and then cooled to room temperature to obtain a toner particle dispersion 2.

[0241] Hydrochloric acid was added to the obtained toner particle dispersion liquid 2 to adjust the pH to 1.4 or less, and the dispersion stabilizer was dissolved. The resulting mixture was filtered, washed, and dried to obtain toner particles 2.

[0242] <Production Example of Toner Particle 3> The following materials were placed in a reaction vessel and dissolved: Styrene 75.0 parts ・25.0 parts n-butyl acrylate Styrene-acrylic acid copolymer (a-1) 4.0 parts Resin A (A-1) 8.0 parts ·Resin B (B-1) 20.0 parts Divinylbenzene 0.6 parts n-Lauryl mercaptan 3.2 parts Next, an aqueous solution consisting of 1.5 parts of Neogen RK (manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) and 150.0 parts of ion-exchanged water was added and dispersed. Furthermore, an aqueous solution consisting of 0.3 parts of potassium persulfate and 10.0 parts of ion-exchanged water was added while slowly stirring. After the reaction vessel was substituted with nitrogen, emulsion polymerization was carried out at 70°C for 6 hours. After the polymerization was completed, the reaction liquid was cooled to room temperature and ion-exchanged water was added to obtain a resin particle dispersion liquid having a solid content concentration of 12.5% ​​by mass and a weight average particle size of 0.2 μm.

[0243] In addition, 100.0 parts of Fischer-Tropsch wax (melting point: 78°C) and 15.0 parts of NEOGEN RK were mixed with 385.0 parts of ion-exchanged water, and dispersed for 1 hour using a wet jet mill JN100 (manufactured by Jokou Co., Ltd.) Ion-exchanged water was added to the obtained dispersion to obtain a wax dispersion having a solid content concentration of 20.0 mass%.

[0244] As a colorant, 100.0 parts of CI Pigment Blue 15:3, 15.0 parts of Neogen RK, and 885.0 parts of ion-exchanged water were mixed and dispersed for 1 hour using a wet jet mill JN100. Ion-exchanged water was added to the obtained dispersion to obtain a colorant dispersion having a solid content concentration of 10.0% by mass.

[0245] The resin particle dispersion (80.0 parts), wax dispersion (9.0 parts), and colorant dispersion (6.0 parts) obtained by the above operation were placed in a reaction vessel and stirred using a homogenizer (IKA: Ultra Turrax T50). Next, the temperature in the reaction vessel was adjusted to 30°C while stirring, and a 1 mol / L aqueous sodium hydroxide solution was added to adjust the pH to 8.0. Next, an aqueous solution of 0.3 parts of magnesium sulfate dissolved in 10.0 parts of ion-exchanged water was added as a flocculant over 10 minutes while stirring at 30°C.

[0246] After another 3 minutes had elapsed, the temperature was increased to 50° C., and aggregated particles were generated. The particle size of the aggregated particles was measured using a Coulter Counter Multisizer 3 (registered trademark, manufactured by Beckman Coulter, Inc.).

[0247] When the weight average particle size of the aggregated particles reached 6.0 μm, 0.9 parts of sodium chloride and 5.0 parts of NEOGEN RK were added to the reaction vessel to stop the particle growth of the aggregated particles.

[0248] Thereafter, the reaction vessel was heated to 65°C and held for 8 hours, then heated to 85°C and held for 1 minute, cooled to 55°C, held for a further 6.0 hours, and then cooled to room temperature, thereby obtaining toner particle dispersion liquid 3.

[0249] The toner particle dispersion 3 thus obtained was filtered and washed, and this process was repeated several times, followed by drying, thereby obtaining toner particles 3.

[0250] <Production Example of Toner Particle 4> Toner particles 4 were obtained in the same manner as in the production example of toner particles 1, except that the type of resin A was changed from (A-1) to (A-12).

[0251] <Production Example of Toner Particle 5> Toner particles 4 were obtained in the same manner as in the production example of toner particles 1, except that the type of resin A was changed from (A-1) to (A-13).

[0252] <Production Examples of Toner Particles 9-13, 17-21, and 24-35> In the production example of toner particle 1, toner particles 9 to 13, 17 to 21, and 24 to 35 were obtained in the same manner, except that the type and added amount of resin A, and the type and added amount of resin B were changed as shown in Table 3.

[0253] <Production Example of Toner Particle 6> The following materials were placed in a reaction vessel, and then zirconia particles having a diameter of 1.7 mm were added. The mixture was dispersed at 220 rpm for 10.0 hours, after which the zirconia particles were removed to obtain a resin composition solution 6. Toluene 100.0 parts Amorphous polyester resin C 100.0 parts Polyester part (a-3) 4.0 parts Resin A (A-3) 8.0 parts ·Resin B (B-1) 20.0 parts Wax (Fischer-Tropsch wax, melting point: 78°C) 3.0 parts Colorant (CI Pigment Blue 15:3) 6.5 parts Next, the resin composition solution 6 was added to the aqueous medium 1 obtained by the same operation as in the production example of the toner particles 1, and a granulation process was carried out for 10 minutes while maintaining the rotation speed at 15,000 rpm in the Clearmix, thereby obtaining a resin composition dispersion 6.

[0254] The resin composition dispersion liquid 6 was heated to 95° C. and stirred for 120 minutes to remove toluene from the resin composition dispersion liquid 6. Thereafter, the resin composition dispersion liquid 6 was cooled to 55° C., and was kept at that temperature for 6.0 hours, and then cooled to room temperature to obtain a toner particle dispersion liquid 6.

[0255] Hydrochloric acid was added to the obtained toner particle dispersion liquid 6 to adjust the pH to 1.4 or less, and the dispersion stabilizer was dissolved. The resulting mixture was filtered, washed, and dried to obtain toner particles 6.

[0256] <Production Example of Toner Particle 7> Toner particles 7 were obtained in the same manner as in the production example of toner particles 6, except that resin (A-1) was used instead of resin (A-3).

[0257] <Production Example of Toner Particle 8> Toner particles 8 were obtained by the same procedure as in the production example of toner particles 2, except that the resin solution 2 was changed to 101.8 parts, the styrene-acrylic acid copolymer (a-1) was changed to the polyester portion (a-3), and 50.0 parts of amorphous polyester resin C was added.

[0258] <Production Example of Toner Particle 14> Toner particles 14 were obtained by the same procedure as in the production example of toner particles 2, except that the styrene-acrylic acid copolymer (a-1) was changed to the polyester portion (a-3), the number of parts of resin A (A-3) was changed to 20.0 parts, and the number of parts of resin B (B-1) was changed to 10.0 parts.

[0259] <Production Example of Toner Particle 15> Toner particles 15 were obtained in the same manner as in the production example of toner particles 14, except that the amount of resin B (B-1) was changed to 2.0 parts.

[0260] <Production Example of Toner Particle 16> Toner particles 16 were obtained by the same procedure as in the production example of toner particles 14, except that the parts of resin A (A-3) was changed to 30.0 parts and the parts of resin B (B-1) was changed to 2.0 parts.

[0261] <Production Example of Toner Particles 22> Toner particles 22 were obtained by the same procedure as in the production example of toner particles 14, except that the parts of resin A (A-3) was changed to 8.0 parts and the parts of resin B (B-1) was changed to 50.0 parts.

[0262] <Production Example of Toner Particle 23> Toner particles 23 were obtained by the same procedure as in the production example of toner particles 22, except that the amount of resin B (B-1) was changed to 60.0 parts.

[0263] <Production Example of Toner Particle 36> Toner particles 36 were obtained in the same manner as in the production example of toner particles 1, except that 8.0 parts of resin A (B-1) was changed to 4.0 parts of trimethoxyvinylsilane.

[0264] <Production Example of Toner Particle 37> Toner particles 37 were obtained in the same manner as in the production example of toner particles 1, except that 8.0 parts of resin A (B-1) was changed to 4.0 parts of 3-methacryloxypropyltrimethoxysilane.

[0265] <Production Example of Toner Particle 38> Toner particles 38 were obtained in the same manner as in the production example of toner particles 1, except that resin B was not used.

[0266] [Table 3]

[0267] Here, TMVS stands for trimethoxyvinylsilane, and MPTMS stands for methacryloxypropyltrimethoxysilane.

[0268] <Production Examples of Toners 1 to 32 and Comparative Toners 1 to 6> For 100.0 parts of each of the obtained toner particles 1 to 32 and toner particles 33 to 38, a BET value of 200 m 2 / g and 0.6 parts of hydrophobic silica fine particles having a number average particle size of primary particles of 8 nm were mixed in a Henschel mixer (manufactured by Mitsui Miike Chemical Engineering Co., Ltd.).

[0269] After the above-mentioned mixing treatment, the mixture was sieved through a mesh having an opening of 150 μm to obtain toners 1 to 32 and comparative toners 1 to 6.

[0270] [Examples 1 to 32 and Comparative Examples 1 to 6] The performance of the obtained toners 1 to 32 and comparative toners 1 to 6 was evaluated according to the following method. The evaluation results are shown in Table 4.

[0271] [Evaluation of low-temperature fixability] A color laser printer (HP Color LaserJet 3525dn, manufactured by HP) with the fixing unit removed was prepared as an image forming apparatus, the toner was removed from the cyan cartridge, and the toner to be evaluated was filled instead. Next, a receiving paper (HP Laser Jet90, manufactured by HP, 90 g / m 2 ) using the filled toner, an unfixed toner image of 2.0 cm length x 15.0 cm width (toner loading amount: 0.9 mg / cm 2) was formed at a position 1.0 cm from the upper end in the paper feed direction. Next, the removed fixing unit was modified so that the fixing temperature and process speed could be adjusted, and a fixing test of an unfixed image was carried out using this.

[0272] First, in a normal temperature and humidity environment (temperature 23°C, relative humidity 60%), the process speed was set to 335 mm / s, and the initial temperature was 140°C, and the set temperature was increased in increments of 5°C, while the unfixed image was fixed at each temperature.

[0273] The evaluation criteria for low-temperature fixability are as follows: The low-temperature fixation starting point is the lowest temperature at which the low-temperature offset phenomenon (the phenomenon in which part of the toner adheres to the fixing device) is not observed.

[0274] A rating of C or above was considered good.

[0275] (Evaluation Criteria) A: The low temperature side fixing start point is 165℃ or less B: The low temperature side fixing start point is 170℃ or more and 180℃ or less C: Low temperature side fixing start point is 185℃ or more and 195℃ or less D: The low-temperature side fixing start point is 200°C or higher and 210°C or lower E: The low temperature side fixing start point is 215℃ or higher

[0276] [Evaluation of abrasion resistance] Using the fixed images obtained in the evaluation of low-temperature fixability, evaluation of abrasion resistance was carried out.

[0277] The fixed image obtained by the above evaluation was left to stand for 30 days under normal temperature and humidity conditions (temperature 23°C, relative humidity 60%). 2 The fixed image was rubbed back and forth five times with a sand eraser to which a load of 63.7 kPa was applied, and the image density reduction rate before and after rubbing was calculated.

[0278] The image density was measured by the following procedure. Using a Macbeth reflection densitometer RD918 (manufactured by Macbeth), the relative density was measured for the image of a white background portion with an image density of 0.00 according to the attached instruction manual. The relative density was measured at five different points on the fixed image, and the average value was taken as the image density value before the rubbing test.

[0279] From these results, the abrasion resistance of the fixed image was evaluated, and a rating of C or higher was judged to be good.

[0280] (Evaluation Criteria) A: Image density reduction rate is less than 15.0% B: Image density reduction rate is 15.0% or more and less than 20.0% C: Image density reduction rate is 20.0% or more and less than 25.0% D: Image density reduction rate is 25.0% or more and less than 30.0% E: Image density reduction rate is 30.0% or more

[0281] [Evaluation of storage stability] 5 g of each toner was placed in a 50 ml resin cup, and left to stand for 5 days at a temperature of 50° C. and a relative humidity of 10%, and the presence or absence of aggregates was checked and evaluated according to the following criteria. A rating of C or higher was considered to be good.

[0282] (Evaluation Criteria) A: No clumps formed B: Slight clumps formed, which can be broken down by gentle shaking C: Slight clumps formed, crumbles when lightly pressed with finger D: Agglomerates form, but do not crumble even when lightly pressed with fingers E: Completely aggregated

[0283] Table 4 shows the physical properties and performance evaluation results of each of the obtained toners.

[0284] [Table 4]

Claims

1. A toner having toner particles containing a binder resin, a resin A, and a resin B, The toner is characterized in that the resin A has a polymer portion and a monovalent group represented by the following formula (1) bonded to the polymer portion, and the resin B contains a crystalline polyester portion: [Formula 1] (In formula (1), L 1 -NH-, -NHR 6 - represents R 1 ~R 3 each independently represents a hydrogen atom, a halogen atom, an alkyl group having 1 or more carbon atoms, an alkoxy group having 1 or more carbon atoms, an aryl group having 6 or more carbon atoms, or a hydroxy group, and R6 is an alkylene group or a hydroxyalkylene group having 4 or less carbon atoms.

2. The R 1 ~R 3 The toner according to claim 1 , wherein at least one of:

3. 3. The toner according to claim 1, wherein the content of the resin B is 2.0 parts by mass or more and 50.0 parts by mass or less with respect to 100 parts by mass of the binder resin.

4. 4. The toner according to claim 1, wherein the resin A has a silicon concentration of 0.02% by mass or more and 10.0% by mass or less.

5. 5. The toner according to claim 1, wherein a ratio (a / b) of a content a of the resin A to a content b of the resin B in the toner is 0.1 or more and 10.0 or less.

6. The toner according to any one of claims 1 to 5, wherein the resin A has a weight average molecular weight of 3,000 or more and 100,000 or less.

7. The toner according to claim 1, wherein the content of said resin A in the total resin of said toner particles is 0.5% by mass or more and 20.0% by mass or less.

8. The toner according to claim 1, wherein the content of the binder resin in the total resin of the toner particles is 50.0 mass % or more.

9. The toner according to any one of claims 1 to 8, wherein the binder resin contains at least one unit selected from the group consisting of a styrene unit, an acrylic unit, and a methacrylic unit, and the polymer portion in the resin A contains at least one unit selected from the group consisting of a styrene unit, an acrylic unit, and a methacrylic unit.

10. 9. The toner according to claim 1, wherein the binder resin contains a polyester moiety, and the polymer moiety in the resin A contains a polyester moiety.

Citation Information

Patent Citations

  • Electrophotographic toner

    JP1995239573A

  • Electrostatic charge image developing toner, method of manufacturing the same, and electrostatic charge image developer, and image forming method using the same

    JP2004191927A

  • Toner for developing electrostatic latent image, method for manufacturing therefor, and process cartridge

    JP2008250294A

  • Toner

    JP2015096949A

  • Manufacturing method of resin particle and manufacturing method of toner

    JP2017015916A