toner

A toner with controlled organosilicon polymer coating on toner base particles, through a network index of -10000≦NI≦-2500, ensures development durability and uniform gloss across varying environmental conditions.

JP7566576B2Active Publication Date: 2024-10-15CANON KK
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020177942
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-10-23
Publication Date
2024-10-15
Estimated Expiration
2040-10-23

AI Technical Summary

Technical Problem

Existing toners fail to maintain development durability and image gloss uniformity across varying temperature and humidity environments, particularly at low temperatures, due to the organosilicon polymer not melting during heat fixing, leading to uneven gloss.

Method used

A toner with toner base particles coated by an organosilicon polymer, controlled through a network index (NI) of -10000≦NI≦-2500, achieved by specific pH treatments and sol-gel reactions, ensuring both development durability and gloss uniformity.

Benefits of technology

The toner maintains development durability under high-temperature, high-humidity and low-temperature, low-humidity conditions while achieving consistent image gloss, addressing the issues of uneven gloss and durability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007566576000012
    Figure 0007566576000012
  • Figure 0007566576000013
    Figure 0007566576000013
  • Figure 0007566576000001
    Figure 0007566576000001
Patent Text Reader

Abstract

To provide a toner which has excellent development durability under high temperature high humidity and low temperature low humidity and has excellent gloss uniformity of an output image.SOLUTION: A toner has toner particles containing toner base particles and organic silicon polymer bodies covering surfaces of the toner base particles, where a network index (NI) calculated by the following method of the toner particles is -10000≤NI≤-2500. With storage elastic modulus at 100°C of the toner to which the following treatments (i) to (iii) are applied as a vertical axis and treatment pH as a transversal axis, an inclination obtained when linear approximation in a least squares method is performed is NI. In treatment (i), the toner is dispersed in aqueous sodium hydroxide whose pH at 25°C is adjusted to 11.5, 12.0, 12.5 respectively to obtain aqueous dispersion. In treatment (ii), temperature of the aqueous dispersion of the toner obtained by the treatment (i) is adjusted to 55°C and agitation is performed for three hours. In treatment (iii), the aqueous dispersion treated in the treatment (ii) is filtered, washed in water, and dried up.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a toner used in electrophotography, electrostatic recording, and toner jet recording. [Background technology]

[0002] In recent years, there has been a demand for faster process speeds in laser beam printers (LBPs) and copiers. In addition, due to increasing global demand, there is a demand for stable image output in various temperature and humidity environments. In order to meet these performance requirements, it is necessary to improve the development durability of toners in high temperature and high humidity and low temperature and low humidity environments. Patent Document 1 discloses a technology for improving the development durability in each environment by forming a surface layer containing an organosilicon polymer on the surface layer of a toner. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2018-200487 A Summary of the Invention [Problem to be solved by the invention]

[0004] However, in recent years, due to the increasing demand for energy saving, there is a demand for improving the performance of the development durability and outputting stable images when fixed at lower temperatures. When the technology of the above-mentioned Patent Document 1 was examined, it was found that the gloss of the output image may become non-uniform when fixed at low temperatures. Therefore, there is a demand for a toner that has good development durability under high temperature and high humidity environments and low temperature and low humidity environments, and that provides good gloss uniformity of the image even when fixed at low temperatures. [Means for solving the problem]

[0005] The present invention relates to a toner having toner particles containing a toner base particle and an organosilicon polymer coating the surface of the toner base particle. 、 The toner base particles contain resin A, The resin A has a structure represented by the formula (1) described below (wherein P 1 (polyester moiety) The organosilicon polymer has a structure represented by formula (2) below, The toner particles have a network index (NI) of -10000≦NI≦-2500 as calculated by the following method. The storage modulus at 100°C of the toner that has been subjected to the following treatments (i) to (iii) is plotted on the vertical axis and the treatment pH on the horizontal axis, and the slope obtained by linear approximation using the least squares method is NI. Treatment (i) The toner is dispersed in aqueous sodium hydroxide solutions whose pH values ​​at 25° C. are adjusted to 11.5, 12.0 and 12.5, respectively, to obtain aqueous dispersions. Treatment (ii) The temperature of the water dispersion of the toner obtained in the above treatment (i) is adjusted to 55° C., and the mixture is stirred for 3 hours. Treatment (iii) The aqueous dispersion treated in the above treatment (ii) is filtered, washed with water, and then dried. Effect of the Invention

[0006] The present invention can provide a toner which has good development durability under high temperature and high humidity environments and low temperature and low humidity environments, and which provides output images with good gloss uniformity. [Brief description of the drawings]

[0007] [Figure 1] FIG. 2 is a diagram illustrating an image of a network on the surface of a toner particle. [Diagram 2] FIG. 1 is a schematic diagram of a graph showing a method for calculating NI. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] The toner of the present invention will be specifically described below.

[0009] The present invention is a toner having toner particles containing toner base particles and an organosilicon polymer coating the surfaces of the toner base particles, wherein the toner particles have a network index (NI) of -10000≦NI≦-2500 as calculated by the following method:

[0010] The storage modulus at 100°C of the toner that has been subjected to the following treatments (i) to (iii) is plotted on the vertical axis and the treatment pH on the horizontal axis, and the slope obtained by linear approximation using the least squares method is NI. Treatment (i) The toner is dispersed in aqueous sodium hydroxide solutions whose pH values ​​at 25° C. are adjusted to 11.5, 12.0 and 12.5, respectively, to obtain aqueous dispersions. Treatment (ii) The temperature of the water dispersion of the toner obtained by the above treatment (i) is adjusted to 55° C., and the mixture is stirred for 3 hours. Treatment (iii) The aqueous dispersion treated in the above treatment (ii) is filtered, washed with water, and then dried.

[0011] As described in Patent Document 1, the toner base particles are coated with an organosilicon polymer, which improves the development durability. However, the organosilicon polymer formed on the surface of the toner base particles does not melt during thermal fixing, and inhibits the toner base particles from spreading (deforming) when the toner is fixed, which tends to cause uneven gloss. It has been found that the toner of the present invention can achieve both development durability and gloss uniformity by controlling the structure of the organosilicon polymer formed on the surface of the toner base particles by controlling the network index (NI). The network index (NI) will be described in detail below.

[0012] The state in which the organosilicon polymer exists on the surface of the toner base particle may be in the form of a film, in the form of a mesh (network), or a mixture of both. If it is close to a film (thick network), the toner is less likely to deform during fixing. On the other hand, if it is formed in a network shape and each network is thin, it is thought that the network will be destroyed during fixing, which suggests that this is advantageous.

[0013] In the process (i) and process (ii) for calculating the NI of the present invention, the water dispersion (toner slurry) of the toner particles is exposed to a highly alkaline and heated (55°C) environment, so that a part of the organosilicon polymer on the surface of the toner mother particle can be dissolved. The higher the pH, the greater the amount of dissolution. When the network is thick or there is no network and it is in a film form, the film thickness of the organosilicon polymer gradually becomes thinner when the treatment pH is changed, so that the storage modulus of the toner particles after the treatment is considered to decrease gradually with the increase in pH. On the other hand, when the network is thin, it is hardly dissolved at low pH (pH = 11.5), so that the storage modulus of the toner particles after the treatment is high, but as the pH is increased to 12.0 and 12.5, the thin network is broken, so the decrease (slope) of the storage modulus becomes steep. Thus, when the NI is small (the slope is large), it is suggested that the network is thin. On the other hand, when the NI is large (the slope is small), it is suggested that the network is thick or close to a film form.

[0014] FIG. 1 shows an image of the network state when the NI of the present invention is large and when it is small. The toner of the present invention can achieve both development durability and gloss uniformity by controlling the NI to the range of -10000≦NI≦-2500. When the NI is larger than -2500, the network of the organosilicon polymer is thick and the toner is less deformed during fixing, resulting in poor gloss uniformity. When the NI is smaller than -10000, the network becomes too thin, resulting in poor development durability. The preferred range of NI is -8000≦NI≦-4000. A more detailed calculation method of NI, including the steps (i) to (iii), will be described later.

[0015] The method for controlling the NI of the present invention includes changing the conditions for forming the organosilicon polymer or the composition of the toner base particles. Of these, it is preferable to change the conditions for forming the organosilicon polymer. The method for forming the organosilicon polymer is described below.

[0016] The organosilicon polymer of the present invention may be formed by any method as long as the toner of the present invention satisfies -10000≦NI≦-2500, but the preferred methods are shown below.

[0017] The sol-gel method is an example of a method for forming an organosilicon polymer. The sol-gel method is a method in which liquid raw materials are used as starting materials, hydrolyzed and condensed to form a gel through a sol state, and is used to synthesize glass, ceramics, organic-inorganic hybrids, and nanocomposites. It is generally known that in a sol-gel reaction, the bond state of the siloxane bond formed varies depending on the acidity of the reaction medium. Specifically, when the reaction medium is acidic, a hydrogen ion electrophilically adds to the oxygen of one reactive group (e.g., an alkoxy group). Next, an oxygen atom in a water molecule coordinates to a silicon atom and becomes a hydroxyl group through a substitution reaction. When there is sufficient water, one hydrogen ion attacks one oxygen of a reactive group (e.g., an alkoxy group), so that as the content of hydrogen ions and reactive groups in the medium decrease with the progress of the reaction, the substitution reaction to a hydroxyl group slows down. Therefore, a polycondensation reaction occurs before all of the reactive groups attached to the silane are hydrolyzed, and one-dimensional linear polymers and two-dimensional polymers are relatively easily formed.

[0018] On the other hand, when the medium is alkaline, hydroxide ions are added to silicon via a pentacoordinate intermediate. This makes it easier for all reactive groups (e.g., alkoxy groups) to be eliminated and easily substituted with silanol groups. In particular, when a silicon compound having three or more reactive groups on the same silane is used, hydrolysis and polycondensation occur three-dimensionally, forming an organosilicon polymer with many three-dimensional cross-linking bonds. The reaction also finishes in a short time.

[0019] Therefore, to form an organosilicon polymer, it is preferable to carry out the sol-gel reaction in an alkaline reaction medium, and when produced in an aqueous medium, specifically, the pH is preferably 8.0 or higher. This allows the formation of an organosilicon polymer with higher strength and excellent durability. Furthermore, when controlling the network structure to satisfy the network index of the present invention, the pH is preferably 10.6 or higher. Specific examples are described below, but the method of obtaining the organosilicon polymer of the present invention using the sol-gel method is not limited to the following examples.

[0020] First, toner base particles are prepared, and an aqueous dispersion of the toner base particles is prepared. At this time, the solid content concentration in the aqueous dispersion of the toner base particles is preferably 10% by mass or more and 40% by mass or less. Next, the aqueous dispersion of the toner base particles is held at 45°C to 70°C, and the pH is adjusted using an aqueous sodium hydroxide solution. At this time, the pH is preferably in the range of 10.6 to 12.5 in order to obtain a desired NI. When the pH is 10.6 or more, the NI can be made smaller. When the pH is 12.5 or less, the NI can be made larger. When the holding temperature is 45°C or more, the NI can be made smaller. When the holding temperature is 70°C or less, the NI can be made larger.

[0021] After adjusting the temperature and pH, the organosilicon polymer is added to the aqueous dispersion of the toner base particles. The organosilicon polymer to be added is preferably one that has been hydrolyzed in advance. Hydrolysis is carried out by adding 5 to 100 parts by weight of an organosilicon compound to 100 parts by weight of ion-exchanged water or RO water, adjusting the pH to 1.0 to 7.0 and the temperature to 15 to 80°C, and stirring for 5 to 720 minutes. After adding the organosilicon polymer (or its hydrolyzed solution), the mixture is stirred for 60 minutes or more while maintaining the temperature, and the organosilicon polymer is formed on the surface of the toner base particles.

[0022] In the toner of the present invention, the toner base particles preferably contain a resin A having a structure represented by the following formula (1).

[0023] [ka] [In formula (1), P 1 is the polymer moiety, L 1 is a divalent linking group, R 1 ~R 3 Each independently represents a hydrogen atom, an alkyl group, an alkoxy group, or a hydroxyl group. m represents a positive value. 1 , R 1 ~R 3 may be independently different.]

[0024] When the toner base particles contain resin A, the structure represented by formula (1) has a silyl group, which improves the affinity with the organosilicon polymer, and increases the adhesion between the toner base particles and the organosilicon polymer formed on the surface, which tends to improve development durability. 1 Examples of the monomer are not particularly limited, but include polyester moieties, vinyl polymer moieties, polyurethane moieties, polycarbonate moieties, phenolic resin moieties, polyolefin moieties, etc. Among these, from the viewpoint of compatibility with gloss uniformity, polyester moieties or vinyl polymer moieties are preferred because they are easily deformed during fixing. Furthermore, in the case of polyester moieties, adhesion with organosilicon polymers is easily improved, and since they have moderate leak properties, development durability in low temperature and low humidity environments is easily improved. Polyvalent carboxylic acids and polyhydric alcohols can be used as condensation polymerization monomers that can be used to produce polyester moieties.

[0025] Examples of polyvalent carboxylic acids include oxalic acid, glutaric acid, succinic acid, maleic acid, adipic acid, β-methyladipic acid, azelaic acid, sebacic acid, nonanedicarboxylic acid, decanedicarboxylic acid, undecanedicarboxylic acid, dodecanedicarboxylic acid, fumaric acid, citraconic acid, diglycolic acid, cyclohexane-3,5-diene-1,2-dicarboxylic acid, hexahydroterephthalic acid, malonic acid, pimelic acid, phthalic acid, isophthalic acid, terephthalic acid, tetrachlorophthalic acid, chlorophthalic acid, nitrophthalic acid, p-carboxyphenylacetic acid, p-phenylene diacetic acid, m-phenylenediglycolic acid, p-phenylenediglycolic acid, o-phenylenediglycolic acid, diphenylacetic acid, diphenyl-p,p'-dicarboxylic acid, naphthalene-1,4-dicarboxylic acid, naphthalene-1,5-dicarboxylic acid, naphthalene-2,6-dicarboxylic acid, anthracene dicarboxylic acid, and cyclohexane dicarboxylic acid. Examples of polycarboxylic acids other than dicarboxylic acids include trimellitic acid, pyromellitic acid, naphthalene tricarboxylic acid, naphthalene tetracarboxylic acid, pyrene tricarboxylic acid, and pyrene tetracarboxylic acid.

[0026] Examples of polyhydric alcohols include ethylene glycol, diethylene glycol, triethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,4-butanediol, neopentyl glycol, 1,4-butenediol, 1,5-pentanediol, 1,6-hexanediol, 1,4-cyclohexanedimethanol, dipropylene glycol, polyethylene glycol, polypropylene glycol, polytetramethylene glycol, sorbitol, isosorbide, 1,2,3,6-hexanetetrol, 1,4-sorbitan, pentaerythritol, diphenyl ether, and the like. Examples of the bisphenol A include pentaerythritol, tripentaerythritol, 1,2,4-butanetriol, 1,2,5-pentanetriol, glycerol, 2-methylpropanetriol, 2-methyl-1,2,4-butanetriol, trimethylolethane, trimethylolpropane, 1,3,5-trihydroxymethylbenzene, bisphenol A, bisphenol A ethylene oxide adduct, bisphenol A propylene oxide adduct, hydrogenated bisphenol A, hydrogenated bisphenol A ethylene oxide adduct, and hydrogenated bisphenol A propylene oxide adduct.

[0027] The polyester moiety preferably has a structure represented by the following formula (3).

[0028] [ka]

[0029] When the compound has the structure of formula (3), adhesion to the organosilicon polymer tends to be further improved.

[0030] Examples of vinyl monomers that can be used to prepare the vinyl polymer portion include styrene derivatives such as styrene, α-methylstyrene, β-methylstyrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, 2,4-dimethylstyrene, pn-butylstyrene, p-tert-butylstyrene, pn-hexylstyrene, pn-octylstyrene, pn-nonylstyrene, pn-decylstyrene, pn-dodecylstyrene, p-methoxystyrene, and p-phenylstyrene; Acrylic polymerizable monomers such as methyl acrylate, ethyl acrylate, n-propyl acrylate, iso-propyl acrylate, n-butyl acrylate, iso-butyl acrylate, tert-butyl acrylate, n-amyl acrylate, n-hexyl acrylate, 2-ethylhexyl acrylate, n-octyl acrylate, n-nonyl acrylate, n-stearyl acrylate, cyclohexyl acrylate, benzyl acrylate, dimethyl phosphate ethyl acrylate, diethyl phosphate ethyl acrylate, dibutyl phosphate ethyl acrylate, and 2-benzoyloxyethyl acrylate; Methacrylic polymerizable monomers such as methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, iso-propyl methacrylate, n-butyl methacrylate, iso-butyl methacrylate, tert-butyl methacrylate, n-amyl methacrylate, n-hexyl methacrylate, 2-ethylhexyl methacrylate, n-octyl methacrylate, diethyl phosphate ethyl methacrylate, n-stearyl methacrylate, and dibutyl phosphate ethyl methacrylate;

[0031] In formula (1), R 1 ~R 3 R each independently represents a hydrogen atom, an alkyl group, an alkoxy group, or a hydroxy group, among which an alkoxy group or a hydroxy group is preferable. 1 ~R 3When is an alkoxy group or a hydroxy group, the presence of an Si-O- bond results in high affinity with the organosilicon polymer and improved adhesion, which tends to improve development durability.

[0032] L in formula (1) 1 represents a divalent linking group. 1 The structure is not particularly limited, but for example, linking groups represented by the following formulae (4) to (6) can be used.

[0033] [ka] [In formula (4), * represents P 1 , ** is the binding site to Si, R 5 represents an alkylene group.

[0034] [ka] [In formula (5), * represents P 1 , ** is the binding site to Si, R 6 represents an alkylene group.

[0035] [ka] [In formula (6), * represents P 1 , ** is the binding site to Si, R 7 represents an alkylene group.

[0036] Among these, L as in equation (4) and equation (5) 1 It is preferred that L contains a carbonyl group. 1 When the compound contains a carbonyl group, charge-up in a low-temperature, low-humidity environment is easily suppressed, and development durability is easily improved. For the same reason, it is more preferable that the compound has an amide bond. The linking group represented by formula (4) can be formed, for example, by the reaction of a carboxy group in the resin with an aminosilane.

[0037] The aminosilane is not particularly limited, but examples thereof include γ-aminopropyltriethoxysilane, γ-aminopropyltrimethoxysilane, N-β(aminoethyl)γ-aminopropyltrimethoxysilane, N-β(aminoethyl)γ-aminopropylmethyldimethoxysilane, N-phenylγ-aminopropyltriethoxysilane, N-phenylγ-aminopropyltrimethoxysilane, N-β(aminoethyl)γ-aminopropyltriethoxysilane, N-6-(aminohexyl)3-aminopropyltrimethoxysilane, 3-aminopropyltrimethylsilane, and 3-aminopropylsilane.

[0038] The linking groups represented by formula (5) and formula (6) can be formed, for example, by copolymerizing a silane coupling agent having a double bond with a monomer having a double bond.

[0039] Examples of the silane coupling agent having a double bond include vinyltriethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, vinyldiethoxymethoxysilane, vinylethoxydimethoxysilane, vinyltriacetoxysilane, vinyldiacetoxymethoxysilane, vinyldiacetoxyethoxysilane, vinylacetoxydimethoxysilane, vinylacetoxymethoxyethoxysilane, vinylacetoxydiethoxysilane, vinyltrihydroxysilane, vinylmethoxydihydroxysilane, vinylethoxydihydroxysilane, and vinyldimethoxyhydroxysilane. vinyl silanes such as vinyl ethoxy methoxy hydroxy silane and vinyl diethoxy hydroxy silane; (meth)acrylic silanes such as 3-[(meth)acryloxy] propyl trimethoxy silane, 3-[(meth)acryloxy] propyl triethoxy silane, (meth)acrylic acid (triethoxysilyl) methyl, (meth)acrylic acid 3-[dimethoxy (methyl) silyl] propyl, (meth)acrylic acid [dimethoxy (methyl) silyl] methyl, and 3-(methacryloyloxy) propyl tris (trimethylsilyloxy) silane; and p-styryl trimethoxy silane.

[0040] The silane coupling agent used in the above silane coupling reaction may be hydrolyzed before the reaction.

[0041] The content of the resin A is preferably 0.05% by mass or more and 20% by mass or less based on the toner base particles. The content of silicon atoms in the resin A is preferably 0.02% by mass or more and 5.00% by mass or less. When it is 0.02% by mass or more, the effect of improving development durability is easily achieved. When it is 5.00% by mass or less, the gloss uniformity is easily improved. More preferably, it is 0.15% by mass or more and 2.00% by mass or less.

[0042] The organosilicon polymer of the present invention preferably has the structure shown in formula (2). R 4 -SiO 3 / 2 Formula (2) [In formula (2), R 4 represents an alkyl group having 1 to 6 carbon atoms, or a phenyl group.

[0043] Of the four valence electrons of the Si atom in the structure represented by formula (2), one is R 4 The remaining three are involved in bonds with O atoms. The O atom has two valences that are both bonded to Si, that is, they form a siloxane bond (Si-O-Si). When considering the Si and O atoms as an organosilicon polymer, there are two Si atoms and three O atoms, so the bond is -SiO 3 / 2 When the organosilicon polymer of the present invention contains formula (2), the strength of the organosilicon polymer is high, and therefore the development durability is easily improved. In order to obtain a structure such as formula (2), it is advisable to use one or more types of organosilicon compounds having three reactive groups in one molecule (hereinafter also referred to as trifunctional silanes) in combination.

[0044] Trifunctional silanes include the following:

[0045] Trifunctional vinyl silanes such as vinyltrimethoxysilane, vinyltriethoxysilane, vinyldiethoxymethoxysilane, vinylethoxydimethoxysilane, vinyltrichlorosilane, vinylmethoxydichlorosilane, vinylethoxydichlorosilane, vinyldimethoxychlorosilane, vinylmethoxyethoxychlorosilane, vinyldiethoxychlorosilane, vinyltriacetoxysilane, vinyldiacetoxymethoxysilane, vinyldiacetoxyethoxysilane, vinylacetoxydimethoxysilane, vinylacetoxymethoxyethoxysilane, vinylacetoxydiethoxysilane, vinyltrihydroxysilane, vinylmethoxydihydroxysilane, vinylethoxydihydroxysilane, vinyldimethoxyhydroxysilane, vinylethoxymethoxyhydroxysilane, vinyldiethoxyhydroxysilane; Trifunctional allylsilanes such as allyltrimethoxysilane, allyltriethoxysilane, allyldiethoxymethoxysilane, allylethoxydimethoxysilane, allyltrichlorosilane, allylmethoxydichlorosilane, allylethoxydichlorosilane, allyldimethoxychlorosilane, allylmethoxyethoxychlorosilane, allyldiethoxychlorosilane, allyltriacetoxysilane, allyldiacetoxymethoxysilane, allyldiacetoxyethoxysilane, allylacetoxydimethoxysilane, allylacetoxymethoxyethoxysilane, allylacetoxydiethoxysilane, allyltrihydroxysilane, allylmethoxydihydroxysilane, allylethoxydihydroxysilane, allyldimethoxyhydroxysilane, allylethoxymethoxyhydroxysilane, allyldiethoxyhydroxysilane;p-Styryltrimethoxysilane, methyltrimethoxysilane, methyltriethoxysilane, methyldiethoxymethoxysilane, methylethoxydimethoxysilane, methyltrichlorosilane, methylmethoxydichlorosilane, methylethoxydichlorosilane, methyldimethoxychlorosilane, methylmethoxyethoxychlorosilane, methyldiethoxychlorosilane, methyltriacetoxysilane, methyldiacetoxymethoxysilane, methyldiacetoxyethoxysilane, methylacetoxydimethoxysilane, methylacetoxymethoxyethoxysilane, methylacetoxydiethoxysilane, methyltrihydroxysilane, methylmethoxydihydroxysilane, methylethoxydihydroxysilane, methyldimethoxyhydroxysilane, methylethoxymethoxyhydroxysilane, methyldiethoxyhydroxysilane, and other trifunctional methylsilanes; ethyltrimethoxysilane, ethyltriethoxy Trifunctional ethyl silanes such as silane, ethyl trichlorosilane, ethyl triacetoxysilane, and ethyl trihydroxysilane; trifunctional propyl silanes such as propyl trimethoxysilane, propyl triethoxysilane, propyl trichlorosilane, propyl triacetoxysilane, and propyl trihydroxysilane; trifunctional butyl silanes such as butyl trimethoxysilane, butyl triethoxysilane, butyl trichlorosilane, butyl triacetoxysilane, and butyl trihydroxysilane; trifunctional hexyl silanes such as hexyl trimethoxysilane, hexyl triethoxysilane, hexyl trichlorosilane, hexyl triacetoxysilane, and hexyl trihydroxysilane; trifunctional phenyl silanes such as phenyl trimethoxysilane, phenyl triethoxysilane, phenyl trichlorosilane, phenyl triacetoxysilane, and phenyl trihydroxysilane. The organosilicon compounds may be used alone or in combination of two or more.;

[0046] In addition to the above-mentioned organosilicon compounds, organosilicon compounds having four reactive groups in one molecule (tetrafunctional silane), organosilicon compounds having three reactive groups in one molecule (trifunctional silane), organosilicon compounds having two reactive groups in one molecule (bifunctional silane) or organosilicon compounds having one reactive group (monofunctional silane) may be used in combination. For example, the following may be mentioned.

[0047] Dimethyldiethoxysilane, tetraethoxysilane, hexamethyldisilazane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 3-glycidoxypropyltriethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-methacryloxypropylmethyldimethoxysilane, 3-methacryloxypropylmethyldiethoxysilane, 3-methacryloxypropyltriethoxysilane, 3-acryloxypropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, N-2-(aminoethyl)-3-aminopropyltriethoxysilane, N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, N-phenyl-3-aminopropyltrimethoxysilane silane, 3-ureidopropyltriethoxysilane, 3-chloropropyltrimethoxysilane, 3-anilinopropyltrimethoxysilane, 3-mercaptopropylmethyldimethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane, bis(triethoxysilylpropyl)tetrasulfide, trimethylsilyl chloride, triethylsilyl chloride, triisopropylsilyl chloride, t-butyldimethylsilyl chloride, N,N'-bis(trimethylsilyl)urea, N,O-bis(trimethylsilyl)trifluoroacetamide, trimethylsilyl trifluoromethanesulfonate, 1,3-dichloro-1,1,3,3-tetraisopropyldisiloxane, trimethylsilylacetylene, hexamethyldisilane, 3-isocyanatopropyltriethoxysilane, tetraisocyanatosilane, methyltriisocyanatosilane, vinyltriisocyanatosilane.

[0048] The content of the organosilicon polymer in the toner particles is preferably 0.50% by mass or more and 7.0% by mass or less. When the content of the organosilicon polymer is 0.50% by mass or more, the toner base particles can be sufficiently coated, so that the development durability is easily improved. When the content is 7.0% by mass or less, the film formation of the organosilicon polymer is easily suppressed, and the gloss uniformity is easily improved. More preferably, the content is 0.80% by mass or more and 5.0% by mass or less, and even more preferably, the content is 0.80% by mass or more and 2.0% by mass or less.

[0049] The toner particles of the present invention have a loss modulus of elasticity of 2×10 at 90° C., when treated by the following treatment method (iv), where G(90) is the loss modulus at 90° C. 4 ≦G(90)≦1×10 6 It is preferable that: (iv) The toner particles are dispersed in an aqueous NaOH solution of pH 13.5, heated at 50° C. for 3 hours, and then filtered, washed, and dried.

[0050] It is believed that the toner subjected to the above treatment (iv) has most of the organosilicon polymer dissolved, and reflects the deformation characteristics of the toner base particles. Therefore, when G(90) is within the above range, appropriate deformation occurs during fixing. G(90)≦1×10 6 When G(90) is 20000 or less, the toner base particles are sufficiently deformed during fixing, and the gloss uniformity is easily improved. When G(90) is 20000 or less, hot offset is easily suppressed, and the gloss uniformity is easily improved. A more preferable range of G(90) is 2×10 4 ≦G(90)≦1×10 5 G(90) can be controlled by changing the glass transition point (Tg) of the toner base particles, by changing the amount or type of wax (described later), by changing the amount or type of colorant such as a pigment (described later), by changing the peak molecular weight, weight average molecular weight, or crosslinking amount of the resin constituting the toner base particles, etc.

[0051] The toner base particles of the present invention preferably contain a binder resin, such as a polyester resin, a vinyl resin, a polyurethane resin, a polycarbonate resin, a phenol resin, a polyolefin resin, or an epoxy resin.

[0052] Among these, it is preferable to use polyester resins and vinyl resins from the viewpoint of development durability. The polyester resins can be produced in the same manner as in the synthesis of the polyester portion of the resin A described above. The vinyl resins can also be produced in the same manner as in the production of the vinyl polymer portion of the resin A. These binder resins can be added as polymers, or can be polymerized simultaneously with particle formation using a suspension polymerization method or an emulsion aggregation polymerization method.

[0053] The toner base particles of the present invention may contain a wax for the purpose of controlling G(90) in addition to improving the releasability of the toner. Examples of wax include aliphatic hydrocarbon waxes, oxides of aliphatic hydrocarbon waxes, block copolymers of aliphatic hydrocarbon waxes, waxes mainly composed of fatty acid esters, partially or completely deoxidized fatty acid esters such as deoxidized carnauba wax, partial esters of fatty acids and polyhydric alcohols, and methyl ester compounds having hydroxyl groups obtained by hydrogenating vegetable oils and fats. Among the above, examples of ester waxes that can be used for the purpose of controlling G(90) include the following. Esters of monohydric alcohols and aliphatic carboxylic acids, such as behenyl behenate, stearyl stearate, and palmityl palmitate; esters of dihydric alcohols and aliphatic carboxylic acids, such as ethylene glycol distearate, dibehenyl sebacate, and hexanediol dibehenate; esters of trihydric alcohols and aliphatic carboxylic acids, such as glycerol tribehenate, or esters of trihydric carboxylic acids and aliphatic alcohols; pentaerythritol tetrastearate esters of tetrahydric alcohols and aliphatic carboxylic acids, such as pentaerythritol tetrapalmitate, or esters of tetrahydric carboxylic acids and aliphatic alcohols; esters of hexahydric alcohols and aliphatic carboxylic acids, such as dipentaerythritol hexastearate, dipentaerythritol hexapalmitate, or esters of hexahydric carboxylic acids and aliphatic alcohols; esters of polyhydric alcohols and aliphatic carboxylic acids, such as polyglycerin behenate, or esters of polyhydric carboxylic acids and aliphatic alcohols; and natural ester waxes, such as carnauba wax and rice wax. The wax content is preferably 1.50 parts by mass or more and 30.00 parts by mass or less, relative to 100 parts by mass of toner particles. The ester wax may be used alone or in combination with an aliphatic hydrocarbon wax or the like.

[0054] The toner base particles of the present invention may contain a colorant. The colorant is not particularly limited, and for example, the following known colorants can be used.

[0055] Examples of yellow pigments that can be used include condensed azo compounds such as yellow iron oxide, navel yellow, naphthol yellow S, Hansa yellow G, Hansa yellow 10G, benzidine yellow G, benzidine yellow GR, quinoline yellow lake, permanent yellow NCG, and tartrazine lake, isoindolinone compounds, anthraquinone compounds, azo metal complexes, methine compounds, and allylamide compounds. Specific examples include the following.

[0056] CI Pigment Yellow 12, 13, 14, 15, 17, 62, 74, 83, 93, 94, 95, 109, 110, 111, 128, 129, 147, 155, 168, 180, 185.

[0057] Orange pigments include the following:

[0058] Permanent Orange GTR, Pyrazolone Orange, Balkan Orange, Benzidine Orange G, Induthrene Brilliant Orange RK, Induthrene Brilliant Orange GK.

[0059] Examples of red pigments include condensed azo compounds such as red iron oxide, permanent red 4R, lithol red, pyrazolone red, watching red calcium salt, lake red C, lake D, brilliant carmine 6B, brilliant carmine 3B, eoxin lake, rhodamine lake B, and alizarin lake, diketopyrrolopyrrole compounds, anthraquinone compounds, quinacridone compounds, basic dye lake compounds, naphthol compounds, benzimidazolone compounds, thioindigo compounds, and perylene compounds. Specific examples include the following.

[0060] CI Pigment Red 2, 3, 5, 6, 7, 23, 48:2, 48:3, 48:4, 57:1, 81:1, 122, 144, 146, 150, 166, 169, 177, 184, 185, 202, 206, 220, 221, 254, 269.

[0061] Examples of blue pigments include alkali blue lake, Victoria blue lake, phthalocyanine blue, metal-free phthalocyanine blue, phthalocyanine blue partial chloride, fast sky blue, copper phthalocyanine compounds such as indanthrene blue BG and their derivatives, anthraquinone compounds, basic dye lake compounds, etc. Specific examples include the following: CI Pigment Blue 1, 7, 15, 15:1, 15:2, 15:3, 15:4, 60, 62, 66.

[0062] Examples of black pigments include carbon black, aniline black, non-magnetic ferrite, magnetite, and pigments toned to black using the above-mentioned yellow, red and blue colorants. These colorants can be used alone or in combination, or in the form of a solid solution.

[0063] The toner base particles of the present invention may contain a charge control agent. Any known charge control agent can be used as the charge control agent. There are charge control agents that control the toner to be negatively charged and charge control agents that control the toner to be positively charged. Examples of charge control agents that control the toner to be negatively charged include the following.

[0064] Monoazo metal compounds, acetylacetone metal compounds, aromatic oxycarboxylic acids, aromatic dicarboxylic acids, oxycarboxylic and dicarboxylic acid-based metal compounds, aromatic oxycarboxylic acids, aromatic mono- and polycarboxylic acids and their metal salts, anhydrides, esters, phenol derivatives such as bisphenol, urea derivatives, metal-containing salicylic acid compounds, metal-containing naphthoic acid compounds, boron compounds, quaternary ammonium salts, calixarenes, and resin-based charge control agents.

[0065] On the other hand, examples of toner that can be controlled to have a positive charge include the following.

[0066] Nigrosine and nigrosine modifications such as fatty acid metal salts; guanidine compounds; imidazole compounds; onium salts such as quaternary ammonium salts such as tributylbenzylammonium-1-hydroxy-4-naphthosulfonate, tetrabutylammonium tetrafluoroborate, and their analogues such as phosphonium salts, and lake pigments thereof; triphenylmethane dyes and lake pigments thereof (lake agents include phosphotungstic acid, phosphomolybdic acid, phosphotungstomolybdic acid, tannic acid, lauric acid, gallic acid, ferricyanide, ferrocyanide, etc.); metal salts of higher fatty acids; resin-based charge control agents.

[0067] The method for producing the toner base particles of the present invention will be described. The toner base particles of the present invention can be produced by a conventionally known method. For example, a suspension polymerization method in which a polymerizable monomer composition containing resin A, a polymerizable monomer constituting a binder resin, wax, a colorant, etc. is suspended in an aqueous medium, granulated, and the polymerizable monomer in the polymerizable monomer composition is polymerized; a kneading and grinding method in which various toner constituent materials such as resin A, binder resin, wax, and colorant are kneaded, pulverized, and classified; an emulsion aggregation method in which a dispersion of resin A, binder resin, wax, colorant, etc. is mixed, aggregated, and heat-fused to obtain toner particles; an emulsion polymerization aggregation method in which a dispersion formed by emulsion-polymerizing a polymerizable monomer constituting a binder resin is mixed with a dispersion in which resin A is emulsified and dispersed, and an emulsion dispersion of wax, colorant, etc. are mixed, aggregated, and heat-fused to obtain toner particles; a dissolution suspension method in which an organic solvent dispersion containing resin A, binder resin, wax, colorant, etc. in an organic solvent is suspended in an aqueous medium, and granulated; and the like can be used.

[0068] Among the above manufacturing methods, it is preferable to use the suspension polymerization method, and more preferably, the organosilicon polymer is formed by directly using the aqueous dispersion of the toner base particles obtained by the suspension polymerization method, since this makes it easier for the organosilicon polymer to precipitate uniformly on the surface of the toner particles.

[0069] In order to control the molecular weight of the binder resin constituting the toner particles, a crosslinking agent may be added during polymerization of the polymerizable monomer. Examples of crosslinkable monomers include the following: divinylbenzene, bis(4-acryloxypolyethoxyphenyl)propane, ethylene glycol diacrylate, 1,3-butylene glycol diacrylate, 1,4-butanediol diacrylate, 1,5-pentanediol diacrylate, 1,6-hexanediol diacrylate, neopentyl glycol diacrylate, diethylene glycol diacrylate, triethylene glycol diacrylate, tetraethylene glycol diacrylate, polyethylene glycol #200, #400, #600 diacrylates, dipropylene glycol diacrylate, polypropylene glycol diacrylate, polyester type diacrylate (MANDA Nippon Kayaku), and those in which the above acrylates are replaced with methacrylates. Examples of polyfunctional crosslinkable monomers include the following: Pentaerythritol triacrylate, trimethylolethane triacrylate, trimethylolpropane triacrylate, tetramethylolmethane tetraacrylate, oligoester acrylate and its methacrylate, 2,2-bis(4-methacryloxy-polyethoxyphenyl)propane, diacryl phthalate, triallyl cyanurate, triallyl isocyanurate, triallyl trimellitate, diaryl chlorendate. The preferred amount is 0.001 to 15,000 parts by mass relative to 100 parts by mass of the polymerizable monomer.

[0070] In the present invention, an external additive may be added to the toner particles to improve the image quality of the toner. As the external additive, inorganic fine powder such as silica fine powder, titanium oxide fine powder, or aluminum oxide fine powder is preferably used. These inorganic fine powders are preferably hydrophobized with a hydrophobizing agent such as a silane coupling agent, silicone oil, or a mixture thereof. Furthermore, the toner of the present invention may, if necessary, mix external additives other than those mentioned above into the toner particles. The amount of inorganic fine powder added is preferably 0.50 parts by mass or more and 5.0 parts by mass or less with respect to 100 parts by mass of the toner particles.

[0071] The methods for measuring the various physical properties of the toner will be described below.

[0072] <How to calculate the Network Index (NI)> (Toner Processing Method) In order to obtain the NI of the present invention, the toner was treated in the following steps (i) to (iii). Process (i): 20 g of RO water is weighed into a container containing a stirrer tip, and the temperature is adjusted to 25°C. The pH is adjusted to 11.5, 12.0, and 12.5 using a 2M aqueous solution of sodium hydroxide. One drop of Contaminon N (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) is added to each of the adjusted aqueous solutions, and 2.0 g of toner is added. Dispersion processing is performed for 5 minutes using an ultrasonic homogenizer (VP-050, manufactured by TAITEC Co., Ltd.) at 20% output, and an aqueous dispersion of the toner is obtained. Treatment (ii): The temperature of the aqueous dispersion of the toner having a different pH obtained in the treatment (i) is adjusted to 55° C., and the dispersion is stirred for 3 hours using a magnetic stirrer. Treatment (iii): The aqueous dispersion treated in treatment (ii) is filtered under reduced pressure, washed five times with 40 g of RO water, and then dried in a vacuum dryer for 24 hours.

[0073] The storage modulus of the toner treated in the steps (i) to (iii) was measured by the following method.

[0074] (Method for measuring storage modulus) The storage modulus was measured using MCR302 (manufactured by Anton Paar).

[0075] 120 mg of the toner was weighed out and molded for 1 minute at 20 kN using a tablet molding machine to obtain a disk-shaped sample with a diameter of 8 mm.

[0076] The obtained sample was set in a measuring jig under the following conditions. Measuring jig name: Measuring plate PP08 / SD:8mm sandblasted Setting conditions: 80℃ 0.1N

[0077] Next, viscoelasticity measurement was performed under the following conditions.

[0078] With the settings of a frequency of 1 Hz and a normal force of 100 mN, while changing the applied strain from 0.5% to 7.0 at 0.22% / min, the temperature was raised from 70 °C to 130 °C at 2 °C / min, and measurement was performed for 30 minutes. The sampling pitch at this time was 1 point / 0.5 min.

[0079] In the above measurement, NI was calculated using the value of the storage modulus at 100 °C calculated.

[0080] (Calculation method of NI) When the storage moduli at 100 °C of the toners treated at pH 11.5, 12.0, and 12.5 are G(11.5), G(12.0), and G(12.5) respectively, with pH (11.5, 12.0, 12.5) on the horizontal axis and the corresponding storage moduli G(11.5), G(12.0), and G(12.5) on the vertical axis, a graph is created. Linear approximation is performed on the three plotted points using the least squares method. The slope of the obtained approximate curve is defined as NI. A schematic diagram of the graph is shown in Figure 2.

[0081] <Calculation method of G(90)> A water dispersion of the toner with the pH adjusted to 13.5 is obtained in the same manner as the above NI calculation method.

[0082] The obtained toner is heated to 50 °C and stirred for 3 hours. The treated toner dispersion is filtered, washed, and dried, and measured in the same manner as the measurement method of the storage modulus in the above NI calculation method. The value of the loss modulus (Pa) at 90 °C of the obtained data is read and defined as G(90).

[0083] <Adjustment method for the tetrahydrofuran-insoluble content of toner particles (extraction of organosilicon polymer)> First, when the surface of the toner particles is treated with an external additive or the like, the external additive is removed by the following method to obtain toner particles.

[0084] Add 160g of sucrose (Kishida Chemical) to 100mL of ion-exchanged water and dissolve in a hot water bath to prepare a concentrated sucrose solution. Add 31g of the concentrated sucrose solution and 6mL of Contaminon N (Fujifilm Wako Pure Chemicals) to a centrifuge tube (capacity 50mL) to prepare a dispersion. Add 1.0g of toner to this dispersion and break up any clumps of toner with a spatula or similar.

[0085] The centrifuge tube is shaken in a shaker at 350 strokes per minute (spm) for 20 minutes. After shaking, the solution is transferred to a glass tube for a swing rotor (capacity 50 mL) and separated in a centrifuge (H-9R, manufactured by Kokusan Co., Ltd.) at 3500 rpm for 30 minutes. This operation separates the toner particles from the removed external additives. It is visually confirmed that the toner and the aqueous solution are sufficiently separated, and the toner separated in the top layer is collected with a spatula or the like. The collected toner is filtered with a vacuum filter and then dried in a dryer for at least 1 hour to obtain toner particles. This operation is carried out multiple times to ensure the required amount.

[0086] Next, the tetrahydrofuran (THF) insoluble content of the toner particles is prepared as follows.

[0087] Weigh out 10.0 g of toner particles, place them in a cylindrical filter paper (Toyo Roshi No. 84) and place them in a Soxhlet extractor. Extract for 20 hours using 200 mL of THF as the solvent. Replace with 200 mL of fresh THF and extract for another 20 hours. Finally, replace with 200 mL of fresh THF again and extract for another 20 hours (total amount of THF used is 600 mL, total extraction time is 60 hours).

[0088] The filtered material in the cylindrical filter paper was vacuum dried at 40°C for several hours to obtain the tetrahydrofuran insoluble matter.

[0089] Furthermore, if necessary, insoluble matters such as pigments can be removed from the tetrahydrofuran insoluble matter to isolate the organosilicon polymer, using a method similar to that used to remove the external additives described above (using "tetrahydrofuran insoluble matter" instead of the above-mentioned "toner"; the organosilicon polymer is often isolated in the lower layer after centrifugation).

[0090] <Adjustment of tetrahydrofuran soluble content of toner particles (extraction of resin A)> Resin A in the toner particles is extracted by separating the extract using tetrahydrofuran (THF) using a solvent gradient elution method. The preparation method is shown below.

[0091] Weigh out 10.0 g of toner particles, place them in a cylindrical filter paper (Toyo Roshi No. 84) and place them in a Soxhlet extractor. Extract for 20 hours using 200 mL of THF as the solvent, and the solid obtained by removing the solvent from the extract is the THF-soluble fraction. The THF-soluble fraction contains resin A. Repeat this process multiple times to obtain the required amount of THF-soluble fraction.

[0092] For the solvent gradient elution method, gradient preparative HPLC (Shimadzu LC-20AP high pressure gradient preparative system, Waters SunFire preparative column 50mmφ250mm) is used. The column temperature is 30°C, the flow rate is 50mL / min, and the mobile phase uses acetonitrile as a poor solvent and THF as a good solvent. 0.02g of the THF soluble matter obtained by extraction is dissolved in 1.5mL of THF to prepare the sample for separation. The mobile phase starts with a composition of 100% acetonitrile, and 5 minutes after the sample injection, the ratio of THF is increased by 4% per minute until the mobile phase composition becomes 100% THF over 25 minutes. The components can be separated by drying the obtained fraction. This allows resin A to be obtained. Which fraction component is resin A can be determined by measuring the silicon atom content and 13 It can be distinguished by C-NMR measurement.

[0093] <Method for measuring silicon content in resin A> The content of the organosilicon polymer and the silicon content in Resin A are measured using a wavelength dispersive X-ray fluorescence analyzer "Axios" (PANalytical) and the accompanying dedicated software "SuperQ ver.4.0F" (PANalytical) for setting measurement conditions and analyzing measurement data. Rh is used as the anode of the X-ray tube, the measurement atmosphere is vacuum, the measurement diameter (collimator mask diameter) is 27 mm, and the measurement time is 10 seconds. A proportional counter (PC) is used to measure light elements, and a scintillation counter (SC) is used to measure heavy elements.

[0094] The measurement sample was prepared by placing 4 g of Resin A alone or the tetrahydrofuran soluble portion obtained by the above-mentioned preparation method, or 4 g of the organosilicon polymer or the tetrahydrofuran insoluble portion in a dedicated aluminum ring for pressing, flattening it, and pressing it at 20 MPa for 60 seconds using a tablet molding compression machine "BRE-32" (Maekawa Test Machinery Manufacturing Co., Ltd.) to form a pellet with a thickness of 2 mm and a diameter of 39 mm.

[0095] In addition, binder particles [product name: Spectro Blend, components: C81.0% by mass, O2.9% by mass, H13.5% by mass, N2.6% by mass, chemical formula: C 19 H 38 SiO2 particles (hydrophobic fumed silica) [product name: AEROSIL NAX50, specific surface area: 40±10 m2] per 100 parts by mass of SiO2 particles (hydrophobic fumed silica) [product name: AEROSIL NAX50, specific surface area: 40±10 m2] 2 0.5 parts by mass of SiO2 particles (0.01g / g, carbon content: 0.45% to 0.85%; manufactured by Nippon Aerosil Co., Ltd.) was added and thoroughly mixed using a coffee mill. Similarly, 5.0 parts by mass and 10.0 parts by mass of the SiO2 particles were mixed with the binder particles, respectively, to prepare samples for the calibration curve.

[0096] For each sample, a pellet of the calibration curve sample is prepared as described above using a tablet press, and the count rate (unit: cps) of the Si-Kα ray observed at a diffraction angle (2θ) = 109.08° when PET is used as the analyzing crystal is measured. In this case, the acceleration voltage and current value of the X-ray generator are 24 kV and 100 mA, respectively. A linear function calibration curve is obtained by plotting the obtained X-ray count rate on the vertical axis and the amount of SiO2 particles added in each calibration curve sample on the horizontal axis.

[0097] Next, the resin A to be analyzed or the tetrahydrofuran soluble portion obtained by the above preparation method, or the organosilicon polymer or the tetrahydrofuran insoluble portion, is pelletized using a tablet molding compression machine as described above, and the count rate of the Si-Kα radiation is measured. The silicon atom content in resin A is then calculated from the above calibration curve.

[0098] <Method for measuring the content of organosilicon polymer in toner> The silicon content in Resin A was measured in the same manner as above, except that the measurement sample was changed to a toner, and the organosilicon polymer content in the toner was measured.

[0099] <Method of confirming the structure represented by formula (2)> The structure represented by formula (2) in the organosilicon polymer contained in the toner particles is confirmed by the following method.

[0100] R in Equation (2) 4 The alkyl group represented by the formula: 13 Confirm by C-NMR.

[0101] ( 13 C-NMR (solid state) measurement conditions Equipment: JEOL RESONANCE JNM-ECX500II Sample tube: 3.2mmφ Sample: 150 mg of tetrahydrofuran insoluble matter obtained by the above preparation method Measurement temperature: room temperature Pulse mode: CP / MAS Measurement nuclear frequency: 123.25MHz (13 C) Reference substance: Adamantane (external standard: 29.5ppm) Sample rotation speed: 20kHz Contact time: 2ms Delay time: 2s Accumulation count: 8000 times

[0102] In this method, methyl groups (Si-CH3), ethyl groups (Si-C2H5), propyl groups (Si-C3H7), butyl groups (Si-C4H9), and pentyl groups (Si-C5H 11 ), hexyl group (Si-CH 13 ) or phenyl group (Si-C6H5-) depending on the presence or absence of a signal due to R in formula (2). 4 The alkyl group represented by the formula:

[0103] <Identification of the structure represented by formula (1)> Polymer moiety P in the structure represented by formula (1) 1 , L 1 Part, R 1 ~R 3 The part is, 1 H-NMR analysis, 13 C-NMR analysis, 29 The analysis is carried out using Si-NMR analysis and FT-IR analysis. The tetrahydrofuran soluble fraction obtained by the above preparation method or resin A synthesized separately is used as the analysis sample.

[0104] L 1 When the compound contains an amide bond as represented by the formula (4), 1 It can be identified by H-NMR analysis. Specifically, it can be identified by the chemical shift value of the proton at the NH site of the amide group, and the amount of the amide group can be quantified by calculating the integral value.

[0105] In addition, R in the structure represented by formula (1) 1 ~R 3 When contains an alkoxy group or a hydroxy group, 29The valence of the alkoxy group or hydroxy group relative to the silicon atom can be determined by the same method as in "Si-NMR (solid) measurement conditions". The tetrahydrofuran soluble fraction obtained by the above preparation method or resin A synthesized separately is used as the analysis sample.

[0106] <Method of measuring weight average molecular weight (Mw)> The weight average molecular weight (Mw) of a resin is measured by gel permeation chromatography (GPC) as follows.

[0107] First, the sample is dissolved in tetrahydrofuran (THF) at room temperature for 24 hours. The resulting solution is then filtered through a solvent-resistant membrane filter "Myshoridisc" (manufactured by Tosoh Corporation) with a pore size of 0.2 μm to obtain a sample solution. The sample solution is prepared so that the concentration of components soluble in THF is approximately 0.8 mass%. This sample solution is used to perform measurements under the following conditions. Equipment: HLC8120 GPC (detector: RI) (Tosoh Corporation) Column: Shodex KF-801, 802, 803, 804, 805, 806, 807 (Showa Denko) Eluent: tetrahydrofuran (THF) Flow rate: 1.0mL / min Oven temperature: 40.0℃ Sample injection volume: 0.10 mL

[0108] In calculating the molecular weight of the sample, a molecular weight calibration curve prepared using standard polystyrene resins (product names: "TSK Standard Polystyrene F-850, F-450, F-288, F-128, F-80, F-40, F-20, F-10, F-4, F-2, F-1, A-5000, A-2500, A-1000, A-500", manufactured by Tosoh Corporation) is used.

[0109] <Method for measuring the acid value of resin> The acid value is the number of milligrams of potassium hydroxide required to neutralize the acid contained in 1 g of a sample. The acid value of a resin is measured in accordance with JIS K 0070-1992, and specifically, it is measured according to the following procedure.

[0110] (1) Preparation of reagents Dissolve 1.0 g of phenolphthalein in 90 mL of ethyl alcohol (95% by volume), and add ion-exchanged water to make 100 mL to obtain a phenolphthalein solution.

[0111] Dissolve 7 g of special grade potassium hydroxide in 5 mL of water and add ethyl alcohol (95% by volume) to make 1 L. Place in an alkali-resistant container to avoid contact with carbon dioxide, etc., leave for 3 days, then filter to obtain potassium hydroxide solution. Store the resulting potassium hydroxide solution in an alkali-resistant container.

[0112] The factor of the potassium hydroxide solution is calculated by taking 25 mL of 0.1 mol / L hydrochloric acid in an Erlenmeyer flask, adding a few drops of the phenolphthalein solution, titrating with the potassium hydroxide solution, and calculating the amount of the potassium hydroxide solution required for neutralization. The 0.1 mol / L hydrochloric acid used is prepared in accordance with JIS K 8001-1998.

[0113] (2) Operation (A) Main Test Weigh out 2.0 g of the crushed sample into a 200 ml Erlenmeyer flask, add 100 ml of a toluene / ethanol (2:1) mixed solution, and dissolve for 5 hours. Next, add a few drops of the phenolphthalein solution as an indicator, and titrate with the potassium hydroxide solution. The end point of the titration is when the light red color of the indicator continues for about 30 seconds. (B) Blank test The titration is carried out in the same manner as above, except that no sample is used (i.e., only the toluene / ethanol (2:1) mixed solution is used).

[0114] (3) The obtained result is substituted into the following formula to calculate the acid value. A = [(CB) × f × 5.61] / S Here, A is the acid value (mgKOH / g), B is the amount of potassium hydroxide solution added for the blank test (ml), C is the amount of potassium hydroxide solution added for the main test (ml), f is the factor of the potassium hydroxide solution, and S is the mass of the sample (g).

[0115] <Method of measuring weight average particle size (D4)> The weight average particle diameter (D4) of the toner is calculated as follows. The measurement device used is a precision particle size distribution measurement device using the narrow hole electrical resistance method, "Coulter Counter Multisizer 3" (registered trademark, manufactured by Beckman Coulter, Inc.), equipped with a 100 μm aperture tube. The measurement conditions are set and the measurement data is analyzed using the accompanying dedicated software "Beckman Coulter Multisizer 3 Version 3.51" (manufactured by Beckman Coulter, Inc.). The measurement is performed with an effective measurement channel count of 25,000 channels.

[0116] The aqueous electrolyte solution used for the measurement is prepared by dissolving special grade sodium chloride in ion-exchanged water to a concentration of 1% by mass, for example, "ISOTON II" (manufactured by Beckman Coulter).

[0117] Before carrying out the measurements and analyses, the dedicated software is set up as follows.

[0118] In the "Change Standard Measurement Method (SOM)" screen of the dedicated software, set the total count number in the control mode to 50,000 particles, the number of measurements to 1, and the Kd value to the value obtained using "Standard Particle 10.0 μm" (Beckman Coulter). Press the "Threshold / Noise Level Measurement Button" to automatically set the threshold and noise level. In addition, set the current to 1600 μA, the gain to 2, the electrolyte to ISOTON II, and check "Flush aperture tube after measurement."

[0119] In the "Pulse to particle size conversion setting" screen of the dedicated software, the bin interval is set to logarithmic particle size, the particle size bin is set to 256 particle size bins, and the particle size range is set to 2 μm to 60 μm.

[0120] The specific measurement method is as follows. (1) Pour 200 ml of the electrolyte solution into a 250 ml round-bottom glass beaker made exclusively for the Multisizer 3, set it on the sample stand, and stir the stirrer rod counterclockwise at 24 revolutions per second. Then, remove dirt and air bubbles from inside the aperture tube using the "Aperture Tube Flush" function of the dedicated software. (2) 30 ml of the electrolyte solution is placed in a 100 ml flat-bottom glass beaker, and 0.3 ml of a dilution of "Contaminon N" (a 10% aqueous solution of a pH 7 neutral detergent for cleaning precision measuring instruments made of a nonionic surfactant, anionic surfactant, and organic builder, manufactured by Wako Pure Chemical Industries, Ltd.) diluted 3 times by mass with ion-exchanged water is added as a dispersant. (3) Prepare an ultrasonic disperser "Ultrasonic Dispersion System Tetora150" (manufactured by Nikkaki Bios Co., Ltd.) that has two built-in oscillators with an oscillation frequency of 50 kHz and a phase shift of 180 degrees, and has an electrical output of 120 W. Place 3.3 L of ion-exchanged water in the ultrasonic disperser's water tank, and add 2 mL of Contaminon N to this water tank. (4) The beaker (2) is set in the beaker fixing hole of the ultrasonic disperser, and the ultrasonic disperser is operated. Then, the height position of the beaker is adjusted so that the resonance state of the liquid surface of the electrolyte solution in the beaker is maximized. (5) While the electrolyte solution in the beaker in (4) is irradiated with ultrasonic waves, 10 mg of toner is added little by little to the electrolyte solution and dispersed. Then, ultrasonic dispersion treatment is continued for another 60 seconds. During ultrasonic dispersion, the water temperature in the water tank is appropriately adjusted to be 10°C or higher and 40°C or lower. (6) Using a pipette, the electrolytic solution (5) in which the toner is dispersed is dropped into the round-bottom beaker (1) placed in the sample stand, and the measurement concentration is adjusted to 5%. Then, measurements are continued until the number of particles measured reaches 50,000. (7) The measurement data is analyzed using the dedicated software that comes with the device, and the weight-average particle diameter (D4) is calculated. Note that when the dedicated software is set to Graph / Volume%, the "Average diameter" on the "Analysis / Volume Statistics (Arithmetic Mean)" screen is the weight-average particle diameter (D4). EXAMPLES

[0121] The present invention will be specifically described below by way of examples, but the present invention is not limited to these examples. Examples 6 to 8, 17, 22 and 24 are reference examples. In the examples and comparative examples, the "parts" of each material are all based on mass unless otherwise specified.

[0122] <Synthesis of resin (P-1)> Resin (P-1) was synthesized according to the following procedure.

[0123] The following materials were charged into an autoclave equipped with a pressure reducing device, a water separating device, a nitrogen gas introducing device, a temperature measuring device, and a stirrer, and a reaction was carried out under a nitrogen atmosphere at normal pressure and 200°C for 5 hours. Bisphenol A-propylene oxide 2.1 mole adduct: 22.7 parts Terephthalic acid: 15.6 parts Isosorbide: 0.58 parts Ethylene glycol: 1.86 parts Tetrabutoxytitanate: 0.1 parts Thereafter, 1.05 parts of trimellitic acid and 0.12 parts of tetrabutoxy titanate were added, and the mixture was reacted at 220° C. for 3 hours, and then reacted under reduced pressure of 10 mmHg to 20 mmHg for 2 hours to obtain a resin (P-1).

[0124] The resulting polyester (P-1) had an acid value of 6.2 mgKOH / g and Mw=14,500.

[0125] <Synthesis of resin (P-2)> Resin (P-2) was synthesized according to the following procedure.

[0126] The following materials were charged into an autoclave equipped with a pressure reducing device, a water separating device, a nitrogen gas introducing device, a temperature measuring device, and a stirrer, and a reaction was carried out under a nitrogen atmosphere at normal pressure and 200°C for 5 hours. Bisphenol A-propylene oxide 2.1 mole adduct: 39.6 parts Terephthalic acid: 8.0 parts Isophthalic acid: 7.6 parts Tetrabutoxytitanate: 0.1 parts Thereafter, 0.01 parts of trimellitic acid and 0.12 parts of tetrabutoxy titanate were added, and the mixture was reacted at 220° C. for 3 hours, and further reacted under reduced pressure of 10 mmHg to 20 mmHg until a desired molecular weight was obtained, to obtain a resin (P-2).

[0127] The resulting resin (P-2) had an acid value of 5.8 mgKOH / g and Mw=15,500.

[0128] <Synthesis of resin (P-3)> Resin (P-3) was obtained in the same manner as in the synthesis of resin (P-1), except that trimellitic acid was not added, terephthalic acid: 15.6 parts was changed to 16.3 parts, and the reaction time was changed. The acid value of the obtained resin (P-3) was 0.4 mg KOH / g, and Mw = 90000.

[0129] <Synthesis of resin (P-4)> A styrene-acrylic resin (P-4) was synthesized as follows.

[0130] 100.0 parts of propylene glycol monomethyl ether was heated while replacing with nitrogen, and refluxed at a liquid temperature of 120° C. or higher. A mixture of 72.9 parts of styrene, 21.6 parts of acrylic acid, and 1.0 part of tert-butyl peroxybenzoate [organic peroxide polymerization initiator, manufactured by NOF Corporation, product name: Perbutyl Z] was added dropwise thereto over 3 hours.

[0131] After the dropwise addition, the solution was stirred for 3 hours, and then distilled at normal pressure while increasing the liquid temperature to 170°C. After the liquid temperature reached 170°C, the pressure was reduced to 1 hPa, and the solvent was removed by distillation for 1 hour to obtain a resin solid. The resin solid was dissolved in tetrahydrofuran, reprecipitated with n-hexane, and the precipitated solid was filtered to obtain a resin (P-4). The acid value of the obtained resin (P-4) was 159 mgKOH / g, and Mw=21000.

[0132] <Synthesis of Resin (A-1)> The carboxy group in the resin (P-1) and the amino group in the aminosilane were amidated to synthesize the resin (A-1) as follows.

[0133] 40.0 parts of resin (P-1) was dissolved in 200.0 parts of N,N-dimethylacetamide, 0.98 parts of 3-aminopropyltriethoxysilane, 1.4 parts of DMT-MM (4-(4,6-dimethoxy-1,3,5-triazin-2-yl)-4-methylmorpholinium chloride) as a condensing agent, and 1.12 parts of triethylamine were added, and the mixture was stirred at room temperature for 5 hours. After the reaction was completed, the solution was dropped into methanol, reprecipitated, and filtered to obtain resin (A-1). The physical properties of the obtained resin (A-1) are shown in Table 2.

[0134] <Synthesis of Resin (A-2)> Resin (A-2) was synthesized in the same manner as in the synthesis of resin (P-4), except that 72.9 parts of styrene were replaced with 98.0 parts of styrene and 21.6 parts of acrylic acid were replaced with 2.0 parts of vinyltriethoxysilane. The physical properties of the obtained resin (A-2) are shown in Table 2.

[0135] <Synthesis of Resin (A-3)> Resin (A-3) was synthesized in the same manner as in the synthesis of Resin (A-2), except that 2.0 parts of vinyltriethoxysilane was replaced with 2.0 parts of 3-methacryloxypropyltrimethoxysilane. The physical properties of the obtained Resin (A-3) are shown in Table 2.

[0136] <Synthesis of Resin (A-4)> A solution of 10.0 parts of resin (A-1) dissolved in 90.0 parts of toluene was mixed with 400.0 parts of pure water and stirred, and the pH was adjusted to 4.0 using dilute hydrochloric acid. After stirring at room temperature for 10 hours, the stirring was stopped and the mixture was transferred to a separatory funnel to extract the oil phase. The oil phase was concentrated and reprecipitated with methanol to obtain resin (A-4). The physical properties of the obtained resin (A-4) are shown in Table 2.

[0137] <Synthesis of Resins (A-5), (A-7) to (A-9)> Resins (A-5), (A-7) to (A-9) were synthesized in the same manner as in the synthesis of resin (A-1), except that the base resin type, silane coupling agent type and amount, condensation agent amount, and base amount were changed as shown in Table 1. The physical properties of the obtained resins (A-5), (A-7) to (A-9) are shown in Table 2.

[0138] <Synthesis of Resin (A-6)> Resin (A-6) was synthesized in the same manner as in the synthesis of Resin (A-3), except that tert-butyl peroxybenzoate was changed from 1.0 part to 0.2 parts and the reaction time was changed. The physical properties of the obtained Resin (A-6) are shown in Table 2.

[0139] [Table 1]

[0140] In Table 1, 3-APTES represents 3-aminopropyltriethoxysilane, 3-APTMS represents 3-aminopropyltrimethylsilane, DMT-MM represents 4-(4,6-dimethoxy-1,3,5-triazin-2-yl)-4-methylmorpholinium chloride, and TEA represents triethylamine.

[0141] [Table 2]

[0142] <Production Example of Toner Base Particle 1> (Preparation process of aqueous medium 1) 14.0 parts of sodium phosphate was added to 1000.0 parts of ion-exchanged water in a reaction vessel, and the mixture was kept at 65°C for 1 hour while purging with nitrogen. Using a TK homomixer (manufactured by Tokushu Kika Kogyo Co., Ltd.), an aqueous calcium chloride solution in which 9.2 parts of calcium chloride (dihydrate) was dissolved in 10.0 parts of ion-exchanged water was added all at once while stirring at 12000 rpm to prepare an aqueous medium containing a dispersion stabilizer. Furthermore, 10% by mass of hydrochloric acid was added to the aqueous medium to adjust the pH to 6.0, and aqueous medium 1 was obtained.

[0143] (Preparation process of polymerizable monomer composition) Styrene: 60.0 parts CI Pigment Blue 15:3:6.5 parts The above materials were charged into an attritor (manufactured by Mitsui Miike Chemical Engineering Co., Ltd.), and further dispersed at 220 rpm for 5 hours using zirconia particles having a diameter of 1.7 mm to prepare a pigment dispersion. The following materials were added to the above pigment dispersion. Styrene: 14.0 parts n-Butyl acrylate: 26.0 parts Crosslinking agent (divinylbenzene): 0.20 parts Resin (A-1): 6.0 parts Fischer-Tropsch wax (melting point 78°C): 10.0 parts Behenyl behenate: 10.0 parts Charge control agent: 0.5 parts (Aluminum compound of 3,5-di-tert-butylsalicylic acid) The mixture was kept at 65° C. and was uniformly dissolved and dispersed at 500 rpm using a TK homomixer (manufactured by Tokushu Kika Kogyo Co., Ltd.) to prepare a polymerizable monomer composition.

[0144] (granulation process) While maintaining the temperature of the aqueous medium 1 at 70° C. and the rotation speed of the stirring device at 12,000 rpm, the polymerizable monomer composition was charged into the aqueous medium 1, and 9.0 parts of t-butyl peroxypivalate as a polymerization initiator was added. Granulation was continued for 10 minutes while maintaining the stirring device at 12,000 rpm.

[0145] (polymerization process) The agitator was changed from the high-speed agitator to a propeller agitator blade, and polymerization was carried out for 5 hours while stirring at 150 rpm and maintaining the temperature at 70°C. The temperature was then raised to 95°C and heated for 2 hours to carry out the polymerization reaction, thereby obtaining a dispersion of toner base particles 1.

[0146] <Production Example of Toner Base Particle 2> A dispersion liquid of toner base particles 2 was obtained in the same manner as in the production example of toner base particles 1, except that resin A was not added.

[0147] <Production Examples of Toner Base Particles 3 to 6, 11 to 14> In the same manner as in the production example of toner base particles 1, except that the type of resin A was changed as shown in Table 3, dispersions of toner base particles 3 to 6 and 11 to 14 were obtained.

[0148] <Production Example of Toner Base Particle 7> A dispersion of toner base particles 7 was obtained in the same manner as in the production example of toner base particles 1, except that the amount of behenyl behenate was changed from 10.0 parts to 5.0 parts and the amount of divinylbenzene was changed from 0.20 parts to 0.40 parts.

[0149] <Production Example of Toner Base Particle 8> A dispersion liquid of toner base particles 8 was obtained in the same manner as in the production example of toner base particles 1, except that behenyl behenate was not added and the amount of divinylbenzene was changed from 0.20 parts to 0.50 parts.

[0150] <Production Example of Toner Base Particle 9> A dispersion liquid of toner base particles 9 was obtained in the same manner as in the production example of toner base particles 1, except that the amount of behenyl behenate was changed from 10.0 parts to 20 parts and the amount of divinylbenzene was changed from 0.20 parts to 0.10 parts.

[0151] <Production Example of Toner Base Particles 10> A dispersion of toner base particles 10 was obtained in the same manner as in the production example of toner base particles 1, except that the amount of behenyl behenate was changed from 10.0 parts to 25.0 parts, divinylbenzene was not added, styrene was changed from 14.0 parts to 5.0 parts, and butyl acrylate was changed from 26.0 parts to 35.0 parts.

[0152] <Production Example of Toner Base Particle 15> A dispersion liquid of toner base particles 15 was obtained in the same manner as in the production example of toner base particles 2, except that 9.0 parts of methyltriethoxylane was added to the pigment dispersion liquid.

[0153] <Production Example of Toner Base Particles 16> A dispersion liquid of toner base particles 16 was obtained in the same manner as in the production example of toner base particles 2, except that behenyl behenate was not added.

[0154] <Preparation of organosilicon compound aqueous solution 1> 60.0 parts of ion-exchanged water was weighed into a reaction vessel equipped with a stirrer and a thermometer, and the pH was adjusted to 3.0 using 10% by mass hydrochloric acid. This was heated with stirring until the temperature reached 40° C. Then, 40.0 parts of methyltriethoxysilane was added and stirred for 120 minutes to obtain an aqueous solution of an organosilicon compound 1.

[0155] <Preparation of organosilicon compound aqueous solution 2> An organosilicon compound aqueous solution 2 was obtained in the same manner as in the preparation of the organosilicon compound aqueous solution 1, except that 8.0 parts of tetraethoxysilane was added in addition to 40.0 parts of methyltriethoxysilane.

[0156] <Preparation of Organosilicon Compound Aqueous Solution 3> An organosilicon compound aqueous solution 3 was obtained in the same manner as in the preparation of the organosilicon compound aqueous solution 1, except that 40.0 parts of methyltriethoxysilane was changed to 40.0 parts of hexyltriethoxysilane.

[0157] <Preparation of Organosilicon Compound Aqueous Solution 4> An organosilicon compound aqueous solution 4 was obtained in the same manner as in the preparation of the organosilicon compound aqueous solution 1, except that 40.0 parts of methyltriethoxysilane was changed to 40.0 parts of tetraethoxysilane.

[0158] <Toner 1 Manufacturing Example> (Organosilicon Polymer Formation Process) The pH of 11.5 was adjusted to 11.5 using an aqueous sodium hydroxide solution for 1100 parts of the dispersion of the toner base particles 1. This was heated to 60° C., and the aqueous organosilicon compound solution 1 was added thereto with stirring. After the addition, the temperature was kept at 60° C. for 300 minutes while stirring was continued to carry out a condensation reaction.

[0159] (Washing and drying process) The toner particle dispersion liquid after the organosilicon polymer formation process was cooled, the toner particle hydrochloric acid was added to adjust the pH to 1.5 or less, and the mixture was left to stir for 1 hour before being subjected to solid-liquid separation using a pressure filter to obtain a toner cake. This was reslurried in ion-exchanged water to make a dispersion again, and then subjected to solid-liquid separation using the aforementioned filter. The reslurry and solid-liquid separation were repeated until the electrical conductivity of the filtrate was 5.0 μS / cm or less, after which the mixture was finally subjected to solid-liquid separation to obtain a toner cake.

[0160] The obtained toner cake was dried using a flash jet dryer (manufactured by Seishin Enterprises), and further, fine and coarse powders were removed using a multi-division classifier utilizing the Coanda effect, to obtain toner particles 1.

[0161] The drying conditions were a blowing temperature of 90°C, a dryer outlet temperature of 40°C, and the toner cake supply speed was adjusted according to the moisture content of the toner cake so that the outlet temperature did not deviate from 40°C.

[0162] The resulting toner particles were used without any external addition to obtain Toner 1. The physical properties of Toner 1 obtained are shown in Table 4.

[0163] <Production Examples of Toners 2 to 25, and Comparative Toners 3 and 5> Toners 2 to 25 and comparative toners 3 and 5 were produced in the same manner as in the production example of toner 1, except that the composition, amount, and formation conditions of the toner base particles and organosilicon polymer were changed as shown in Table 3. The physical properties of the obtained toners 2 to 25 and comparative toners 3 and 5 are shown in Table 4.

[0164] <Production Example of Comparative Toner 1> The dispersion of toner base particles 15 was adjusted to pH 9.0 using an aqueous sodium hydroxide solution, heated to 60° C., and stirred for 300 minutes. After that, a washing and drying process was performed to obtain comparative toner 1. The physical properties of the obtained comparative toner 1 are shown in Table 4.

[0165] <Production Example of Comparative Toner 2> Comparative toner 2 was obtained in the same manner as in the production example of toner 6, except that 8.0 parts of methyltriethoxysilane was added directly without using the aqueous solution of organosilicon compound 1, and the step of adjusting the pH to 11.5 using an aqueous sodium hydroxide solution was changed to a pH of 9.0. The physical properties of the obtained comparative toner 2 are shown in Table 4.

[0166] <Production Example of Comparative Toner 4> The dispersion of toner base particles 16 was washed and dried in the same manner as in the manufacturing example of toner 1. 10 parts of the obtained toner particles were dispersed in 100 parts of 0.3% by mass sodium dodecyl sulfate aqueous solution using an ultrasonic disperser to obtain a toner dispersion. Next, in a separate container, 30 parts of methyltriethoxysilane were dispersed in 100 parts of 0.3% by mass sodium dodecyl sulfate aqueous solution using an ultrasonic disperser, and the temperature was maintained at 25°C. The toner dispersion was then poured into the toner dispersion. After the addition, the pH was adjusted to 11.4 using an aqueous sodium hydroxide solution, and the reaction was carried out for 24 hours while maintaining the temperature at 25°C. After washing with ethanol, the mixture was repeatedly washed with ion-exchanged water until the electrical conductivity of the filtrate was 5.0 μS / cm or less, and then filtered and dried. The physical properties of the obtained comparative toner 4 are shown in Table 4.

[0167] [Table 3] (In Table 3, MTES stands for methyltriethoxysilane, TEOS stands for tetraethoxysilane, and HTES stands for hexyltriethoxysilane.)

[0168] [Table 4]

[0169] [Examples 1 to 25] In Examples 1 to 25, the development durability and gloss uniformity were evaluated using Toners 1 to 25.

[0170] [Comparative Examples 1 to 5] In Comparative Examples 1 to 5, comparative toners 1 to 5 were used to evaluate the development durability and gloss uniformity.

[0171] [Evaluation method for development durability] The durability was evaluated using a commercially available Canon printer LBP-712Ci.

[0172] The evaluation cartridge was a commercially available cartridge in which the toner was removed, the inside was cleaned with an air blower, and then filled with 100 g of the above toner.

[0173] Before evaluation, the cartridges were left for 24 hours in a high temperature and high humidity (H / H) environment (30°C, 80% RH) and a low temperature and low humidity (L / L) environment (15°C, 10% RH).

[0174] The above cartridge was mounted in the cyan station, and dummy cartridges were mounted in the other stations to carry out the evaluation.

[0175] Under H / H and L / L environments, 10,000 images with a print coverage rate of 1% were printed using Canon Oce Red Label (80g / m2).

[0176] After the above image output, a full solid image was output on one sheet, and the density was measured.

[0177] The density was measured using an X-Rite color reflection densitometer (X-Rite Corporation). The evaluation criteria are as follows:

[0178] The evaluation results are shown in Table 5.

[0179] (Evaluation Criteria) A: Concentration is 1.45 or more B: Density is 1.35 or more C: Density is 1.25 or more D: Density is less than 1.25

[0180] Subsequently, a solid white image was output, the worst reflection density of the white background was taken as Ds, the average reflection density of the transfer material before image formation was taken as Dr, and Dr-Ds was taken as the fog value.

[0181] The reflection density of the white background was measured using a reflection densitometer (Reflectometer Model TC-6DS, manufactured by Tokyo Denshoku Co., Ltd.) and an amber light filter was used.

[0182] The smaller the value, the better the evaluation. The evaluation criteria are as follows. The evaluation results are shown in Table 5.

[0183] (Evaluation Criteria) A: 0.5% or less B: More than 0.5% and 1.0% C: 1.0% or more and 2.0% or less D: greater than 2.0%

[0184] [Evaluation of gloss uniformity] The LBP-712Ci used in the evaluation of the above-mentioned development durability was modified so that the toner amount on the paper could be adjusted, and the fixing unit was removed.

[0185] Using the same cartridge as that used in the evaluation of the development durability, media (GF-C081, 81.4 g / m 2 ) toner amount 0.45mg / cm 2A full solid image was output using a 100% inkjet printer. The removed fixing unit was then modified so that the fixing temperature and process speed could be adjusted, and the process speed was set to 280 mm / s in a normal temperature and humidity (N / N) environment (23°C, 60% RH). The unfixed image was fixed using an external fixing device with a temperature setting of 135°C. The glossiness of the fixed image was measured at a total of nine points, including three points on the top row, three points on the middle row, and three points on the bottom row. A PG-3D (manufactured by Nippon Denshoku Industries Co., Ltd.) was used for the measurements. The difference (Gmax-Gmin) between the highest glossiness value (Gmax) and the lowest glossiness value (Gmin) measured was used as the evaluation standard for gloss uniformity.

[0186] (Evaluation Criteria) A: 1.0% or less B: More than 1.0% and 2.0% or less C: 2.0% or more and 3.0% or less D: greater than 3.0%

[0187] [Table 5]

Claims

1. A toner having toner particles containing toner base particles and an organosilicon polymer coating the surfaces of the toner base particles, The toner base particles contain a resin A, The resin A has a structure represented by the following formula (1): The organosilicon polymer has a structure represented by formula (2): The toner particles have a network index (NI) of -10,000≦NI≦-2,500 as calculated by the following method: The storage modulus at 100° C. of the toner that has been subjected to the following treatments (i) to (iii) is plotted on the vertical axis and the treatment pH on the horizontal axis, and the slope obtained by linear approximation using the least squares method is NI. Treatment (i) The toner is dispersed in aqueous sodium hydroxide solutions whose pH values ​​at 25° C. are adjusted to 11.5, 12.0 and 12.5, respectively, to obtain aqueous dispersions. Treatment (ii) The temperature of the water dispersion of the toner obtained in the above treatment (i) is adjusted to 55° C., and the mixture is stirred for 3 hours. Treatment (iii) The aqueous dispersion treated in the above treatment (ii) is filtered, washed with water, and then dried. 【Chemistry 1】 [In formula (1), P 1 represents a polyester moiety, L 1 represents a divalent linking group, and R 1 to R 3 each independently represent a hydrogen atom, an alkyl group, an alkoxy group, or a hydroxyl group. m represents a positive value. The respective structures of m L 1 s and R 1 to R 3 may be independently different.] R 4 -SiO 3 / 2 Formula (2) [In formula (2), R 4 represents an alkyl group having 1 to 6 carbon atoms, or a phenyl group.]

2. 2. The toner according to claim 1, wherein the content of said organosilicon polymer in said toner particles is from 0.50% by weight to 7.0% by weight.

3. When the toner particles are treated by the following treatment method (iv), the loss modulus at 90° C. is defined as G(90), and the range is 20,000≦G(90)≦1×10 6 3. The toner according to claim 1, wherein Treatment (iv) The toner particles are dispersed in an aqueous NaOH solution of pH 13.5, heated at 50° C. for 3 hours, filtered, washed and dried.

Citation Information

Patent Citations

  • Toner for electrostatic charge image development

    JP2013205579A

  • toner

    JP2016027399A

  • Method for manufacturing toner particle

    JP2017134367A

  • toner

    JP2017138592A

  • toner

    JP2017203889A