Toner and its manufacturing method
A toner with a specific resin structure enhances adhesion between the binder resin and silicon-containing particles, addressing cracking and chipping issues, thus maintaining low-temperature fixability and durability.
Patent Information
- Application Number
- JP2020177943
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-10-23
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2040-10-23
AI Technical Summary
Existing toners with low-temperature fixability tend to crack and chip during long-term use due to poor adhesion between the binder resin and silicon-containing particles, compromising both low-temperature fixability and durability.
A toner composition containing a binder resin with a substituted or unsubstituted silyl group and silicon-containing particles, such as silica or organosilicon polymers, is developed, where the resin A has a specific structure represented by formula (1) to enhance adhesion and dispersibility, thereby improving the toner's resistance to cracking and chipping.
The toner maintains low-temperature fixability while significantly reducing cracking and chipping during long-term use, ensuring improved durability and stability.
Smart Images

Figure 0007566577000001 
Figure 0007566577000002 
Figure 0007566577000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a toner for developing an electrostatic latent image formed by a method such as electrophotography, electrostatic recording, or toner jet recording, and a method for producing the toner. [Background technology]
[0002] In recent years, energy saving has been considered a major technical issue in electrostatic copying electrophotography used in copiers, printers, faxes, etc., and a significant reduction in the amount of heat required for image fixing devices is desired. Therefore, there is an increasing need for toners that can fix images with less energy, that is, with so-called "low temperature fixability." Common methods for improving the low-temperature fixability of a toner include lowering the glass transition temperature (Tg) of the binder resin or reducing the molecular weight of the binder resin in order to soften the binder resin used. However, simply lowering the Tg of the binder resin or reducing the molecular weight can result in a decrease in the storage stability of the toner and offset to the fixing member due to insufficient releasability during fixing. In order to increase the toner strength while maintaining the glass transition temperature (Tg), it is common to increase the molecular weight of the binder resin or to give the binder resin a crosslinked structure. However, if the toner strength is increased beyond a certain level using this method alone, the low-temperature fixability is inevitably impaired. For example, Patent Document 1 discloses a method of increasing toner strength by adding pearl necklace-like silica. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2009-42386 A Summary of the Invention [Problem to be solved by the invention]
[0004] According to Patent Document 1, it is possible to increase the toner strength compared to general silica. However, when the toner has good low-temperature fixing property, it is prone to cracking at the interface between the binder resin and the silica, and there is a problem of contamination of components due to cracking and chipping of the toner over long-term use. In view of these problems, the present invention provides a toner that is excellent in preventing cracking and chipping during long-term use without impairing low-temperature fixability. [Means for solving the problem]
[0005] The present invention relates to a toner containing toner particles, the toner particles containing a binder resin, a resin A, and silicon, The resin A teeth , The structure represented by the formula (1) described below (wherein L 1 has a linking group having a structure represented by formula (17) or a structure represented by formula (18) described below) , The toner is characterized in that the silicon-containing particles are at least one selected from the group consisting of silica and organosilicon polymers. The present invention also provides a method for producing the toner having the above-mentioned configuration, The present invention relates to a method for producing a toner, the method comprising the steps of dispersing the resin A, the silicon-containing particles, and a polymerizable monomer composition containing a polymerizable monomer in an aqueous medium, forming particles of the polymerizable monomer composition in the aqueous medium, and polymerizing the polymerizable monomer contained in the particles of the polymerizable monomer composition. Furthermore, the present invention provides a method for producing the toner having the above-mentioned configuration, The present invention relates to a method for producing a toner, comprising the steps of melt-kneading a mixture containing a binder resin, the resin A, and the silicon-containing particles to obtain a melt-kneaded product, and pulverizing the melt-kneaded product to obtain a pulverized product. Effect of the Invention
[0006] As described above, according to the present invention, it is possible to provide a toner that is excellent in preventing cracking and chipping even with long-term use without impairing low-temperature fixability. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0007] The toner of the present invention will be specifically described below, but is not limited thereto.
[0008] In the present invention, the expressions "xx or more and xx or less" and "xx to xx" expressing a numerical range mean a numerical range including the lower and upper limit endpoints, unless otherwise specified.
[0009] The toner of the present invention is a toner having toner particles containing a binder resin, a resin A, and silicon-containing particles, characterized in that the resin A has a substituted or unsubstituted silyl group in the molecule, the substituent of the substituted silyl group being at least one selected from an alkyl group having 1 or more carbon atoms, an alkoxy group having 1 or more carbon atoms, a hydroxy group, a halogen atom, and an aryl group having 6 or more carbon atoms, and the silicon-containing particles are at least one selected from silica or an organosilicon polymer.
[0010] The present inventors have found that by employing a toner having the above-mentioned configuration, low-temperature fixability is not impaired and cracking and chipping during long-term use are effectively prevented.
[0011] The reason for this is speculated as follows.
[0012] When a toner with good low-temperature fixing property is rubbed by a roller or a developing blade during image formation, the toner particles are soft and easily crushed. Therefore, in order to withstand the rubbing, it is necessary to increase the strength of the toner. It is generally known that the addition of particles containing silicon such as silica (filler effect) makes the toner particles harder. On the other hand, particles containing silicon such as silica have poor dispersibility within toner particles, so they need to be added in large amounts. Even if a large amount of particles containing silicon is added to increase the strength of the toner, the interface between the particles containing silicon and the binder resin is easily cracked and brittle, so there is a problem of cracking and chipping during long-term use. In addition, when a large amount of particles containing silicon is added, there is a problem that the low-temperature fixing property is impaired.
[0013] On the other hand, the toner of the present invention has a substituted or unsubstituted silyl group in the molecule of resin A. This improves the dispersibility of silicon-containing particles such as silica in the toner particles. It is also speculated that the adhesion between the binder resin and the silicon-containing particles is increased via this resin A, and the effect of suppressing cracking and chipping at the interface between the silicon-containing particles and the binder resin is exhibited. It is believed that this has produced a good effect in suppressing cracking and chipping of the toner during long-term use without impairing low-temperature fixability.
[0014] Preferred configurations of the present invention will now be described.
[0015] First, the binder resin used in the present invention will be described.
[0016] The binder resin used in the toner of the present invention is not particularly limited, and any conventionally known resin may be used. From the viewpoint of the development characteristics and durability of the toner, the binder resin is preferably a resin containing at least one unit selected from the group consisting of a styrene unit, an acrylic unit, and a methacrylic unit (hereinafter referred to as a styrene-acrylic copolymer portion), or a resin containing a polyester portion.
[0017] As long as it has a styrene-acrylic copolymer moiety, it may consist of only a styrene-acrylic copolymer, or it may be a block copolymer or graft copolymer of a styrene-acrylic copolymer and another polymer, or a mixture thereof.
[0018] Examples of styrene monomers constituting the styrene unit include styrene, α-methylstyrene, β-methylstyrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, 2,4-dimethylstyrene, divinylbenzene, etc. Although one type of styrene monomer can be used, two or more types selected from these can also be used in combination.
[0019] Examples of acrylic monomers constituting the acrylic unit include acrylic acid alkyl esters such as methyl acrylate, ethyl acrylate, n-propyl acrylate, isopropyl acrylate, n-butyl acrylate, isobutyl acrylate, tert-butyl acrylate, n-amyl acrylate, n-hexyl acrylate, 2-ethylhexyl acrylate, n-octyl acrylate, and n-nonyl acrylate; acrylic acid diesters such as diethylene glycol diacrylate, triethylene glycol diacrylate, tetraethylene glycol diacrylate, polyethylene glycol diacrylate, and 1,6-hexanediol diacrylate; and acrylic acid.
[0020] Examples of methacrylic monomers constituting the methacrylic unit include methacrylic acid alkyl esters such as methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, iso-propyl methacrylate, n-butyl methacrylate, iso-butyl methacrylate, tert-butyl methacrylate, n-amyl methacrylate, n-hexyl methacrylate, 2-ethylhexyl methacrylate, n-octyl methacrylate, and n-nonyl methacrylate; methacrylic acid, and the like.
[0021] The acrylic monomer and the methacrylic monomer may be used alone or in combination of two or more selected therefrom.
[0022] The resin having a styrene-acrylic copolymer moiety preferably contains a styrene-acrylic acid alkyl ester copolymer or a styrene-methacrylic acid alkyl ester copolymer.
[0023] Of the monomers forming the styrene-acrylic copolymer, the proportion of the styrene-based monomer is preferably 45% by mass or more and 80% by mass or less, and the proportion of the acrylic monomer (preferably an acrylic acid alkyl ester and a methacrylic acid alkyl ester) is preferably 20% by mass or more and 50% by mass or less.
[0024] The resin containing a polyester moiety may be a condensation polymer of a carboxylic acid component and an alcohol component as shown below. Examples of the carboxylic acid component include terephthalic acid, isophthalic acid, phthalic acid, fumaric acid, maleic acid, cyclohexanedicarboxylic acid, and trimellitic acid. Examples of the alcohol component include bisphenol A, hydrogenated bisphenol, an ethylene oxide adduct of bisphenol A, a propylene oxide adduct of bisphenol A, glycerin, trimethylolpropane, and pentaerythritol.
[0025] The polyester may be a polyester containing a urea group. It is preferable that the carboxyl groups at the terminals of the polyester are not capped.
[0026] The binder resin may contain a crosslinking agent.
[0027] As the crosslinking agent, a compound having two or more polymerizable double bonds is mainly used.
[0028] Examples of the vinyl compounds include aromatic divinyl compounds such as divinylbenzene and divinylnaphthalene; carboxylic acid esters having two double bonds such as ethylene glycol diacrylate, ethylene glycol dimethacrylate, 1,3-butanediol dimethacrylate, and 1,6-hexanediol diacrylate; divinyl compounds such as divinylaniline, divinyl ether, divinyl sulfide, and divinyl sulfone; and compounds having three or more vinyl groups.
[0029] These may be used alone or in combination of two or more. The amount of the crosslinking agent added is preferably 0.001 parts by mass or more and 15,000 parts by mass or less with respect to 100 parts by mass of the binder resin.
[0030] Resin A of the present invention will be described in detail below.
[0031] Resin A of the present invention is preferably a resin having a structure represented by the following formula (1).
[0032] [ka] (In formula (1), P 1 represents the polymer moiety, and L 1 represents a single bond or a divalent linking group, R 1 ~R 3 each independently represents a hydrogen atom, a halogen atom, an alkyl group, an alkoxy group, an aryl group, or a hydroxyl group; m represents a positive integer; and when m is 2 or more, 1 , multiple R 1 , multiple R 2 and multiple R 3 may be the same or different.)
[0033] In the resin represented by formula (1), silicon atoms (Si) are present in the side chains or terminals of the resin. This is believed to produce the effect of efficiently placing silicon-containing particles in the vicinity of resin A. Through this resin A, the adhesion between the binder resin and the silicon-containing particles is increased, suppressing cracking and chipping at the particle interface. As a result, it is believed that a good effect is realized in suppressing cracking and chipping of the toner over long-term use.
[0034] The content of the resin A in the toner particles is preferably 0.1% by mass or more and 10.0% by mass or less. By being in this range, low-temperature fixability is not impaired and good effects are shown in preventing cracking and chipping during long-term use.
[0035] The polymer moiety P in the formula (1) 1 is not particularly limited, and examples thereof include a polyester moiety, a vinyl resin moiety, a polyurethane moiety, a polycarbonate moiety, a phenol resin moiety, a polyolefin moiety, etc. 1 The structure preferably contains a polyester portion or a vinyl resin portion, and among these, P 1It is more preferable that the structure contains a polyester moiety.
[0036] P 1 It is believed that when the structure of contains a polyester portion, it produces the effect of improving the dispersibility of the silicon-containing particles in the toner particles. Through this resin A, the adhesion between the binder resin and the silicon-containing particles is improved, and cracking and chipping at the particle interface is suppressed. As a result, it is believed that a good effect is realized in preventing cracking and chipping of the toner over long-term use.
[0037] P 1 An example in which the structure contains a polyester moiety will be described.
[0038] The polyester moiety is a condensation product of a dialcohol and a dicarboxylic acid. Examples of the polyester moiety include a condensation product of a unit of the following formula (12) and a unit (multiple units can be selected) selected from the following formulas (13) to (15), or a condensation polymer represented by a unit of the following formula (16).
[0039] [ka] [In formula (12), R 9 represents an alkylene group, an alkenylene group, or an arylene group.
[0040] [ka] [In formula (13), R 10 represents an alkylene group or a phenylene group.
[0041] [ka] [In formula (14), R 18 represents an ethylene group or a propylene group. x and y are each an integer value of 0 or more, and the average value of x+y is 2 or more and 10 or less.]
[0042] [ka] [In formula (16), R 11 represents an alkylene group or an alkenylene group.
[0043] R in the above formula (12) 9 Examples of the alkylene group in the formula (I) include the following: a methylene group, an ethylene group, a trimethylene group, a propylene group, a tetramethylene group, a hexamethylene group, a neopentylene group, a heptamethylene group, an octamethylene group, a nonamethylene group, a decamethylene group, an undecamethylene group, a dodecamethylene group, 1,3-cyclopentylene, 1,3-cyclohexylene, and 1,4-cyclohexylene group.
[0044] R in the above formula (12) 9 The alkenylene group in the formula (I) includes a vinylene group, a propenylene group, and a 2-butenylene group.
[0045] R in the above formula (12) 9 Examples of the arylene group in include a 1,4-phenylene group, a 1,3-phenylene group, a 1,2-phenylene group, a 2,6-naphthylene group, a 2,7-naphthylene group, and a 4,4'-biphenylene group.
[0046] R in the above formula (12) 9 may be substituted with a substituent. In this case, the substituent that may be substituted includes a methyl group, a halogen atom, a carboxyl group, a trifluoromethyl group, and combinations thereof.
[0047] R in the above formula (13) 10 Examples of the alkylene group in the formula (I) include the following: a methylene group, an ethylene group, a trimethylene group, a propylene group, a tetramethylene group, a hexamethylene group, a neopentylene group, a heptamethylene group, an octamethylene group, a nonamethylene group, a decamethylene group, an undecamethylene group, a dodecamethylene group, 1,3-cyclopentylene, 1,3-cyclohexylene, and 1,4-cyclohexylene group.
[0048] R in the above formula (13) 10 Examples of the phenylene group in include a 1,4-phenylene group, a 1,3-phenylene group, and a 1,2-phenylene group.
[0049] R in the above formula (13) 10 may be substituted with a substituent. In this case, the substituent that may be substituted includes a methyl group, an alkoxy group, a hydroxyl group, a halogen atom, and combinations thereof.
[0050] R in the above formula (16) 11 Examples of the alkylene group in the formula (I) include the following: a methylene group, an ethylene group, a trimethylene group, a propylene group, a tetramethylene group, a hexamethylene group, a neopentylene group, a heptamethylene group, an octamethylene group, a nonamethylene group, a decamethylene group, an undecamethylene group, a dodecamethylene group, and a 1,4-cyclohexylene group.
[0051] R in the above formula (16) 11 Examples of the alkenylene group in the above formula include the following: vinylene group, propenylene group, butenylene group, butadienylene group, pentenylene group, hexenylene group, hexadienylene group, heptenylene group, octanylene group, decenylene group, octadecenylene group, eicosenylene group, and triacontenylene group. These alkenylene groups may have any of a linear, branched, and cyclic structure. The position of the double bond may be any position, as long as there is at least one double bond.
[0052] R in the above formula (16) 11 may be substituted with a substituent. In this case, the substituent that may be substituted includes an alkyl group, an alkoxy group, a hydroxyl group, a halogen atom, and combinations thereof.
[0053] In addition, the P 1 When the structure contains a vinyl resin moiety, it is preferable that the resin contains a styrene-acrylic copolymer moiety.
[0054] L in the above formula (1) 1 is not particularly limited, but preferably has a partial structure represented by the following formulas (17) to (20).
[0055] [ka] [R in formula (17) 5 represents an alkylene group, an arylene group, or an alkylene group containing an -NH- group. (*) represents P in the above formula (1). 1 and (**) represents the bonding site to the silicon atom in formula (1).
[0056] [ka] [R in formula (18)] 6 represents an alkylene group or an arylene group. (*) represents P in the formula (1). 1 and (**) represents the bonding site to the silicon atom in formula (1).
[0057] [ka]
[0058] [ka] [R in formulas (19) and (20)] 7 and R 8 Each of the groups independently represents an alkylene group, an arylene group, or an oxyalkylene group. (*) represents P in the formula (1). 1 and (**) represents the bonding site to the silicon atom in formula (1).
[0059] Among these, L 1It was confirmed that the structure of the toner containing the amide bond represented by formula (17) produces excellent effects in preventing cracking and chipping during long-term use without impairing low-temperature fixing properties, and also improves tape peeling properties after toner fixing. This is presumably due to the high affinity of the amide bond with the hydroxyl groups of the cellulose that constitutes the paper fiber, which is the fixing medium.
[0060] The partial structure represented by the formula (17) is a divalent linking group containing an amide bond, and is formed, for example, by a reaction between a carboxy group in a resin and an aminosilane compound.
[0061] The aminosilane compound is not particularly limited, but examples thereof include γ-aminopropyltriethoxysilane, γ-aminopropyltrimethoxysilane, N-β(aminoethyl)γ-aminopropyltrimethoxysilane, N-β(aminoethyl)γ-aminopropylmethyldimethoxysilane, N-phenylγ-aminopropyltriethoxysilane, N-phenylγ-aminopropyltrimethoxysilane, N-β(aminoethyl)γ-aminopropyltriethoxysilane, N-6-(aminohexyl)3-aminopropyltrimethoxysilane, 3-aminopropyltrimethylsilane, and 3-aminopropylsilicon.
[0062] The partial structure represented by the formula (18) is a divalent linking group containing a urethane bond, and is formed, for example, by a reaction between a hydroxy group in a resin and an isocyanate silane compound.
[0063] The isocyanate silane compound is not particularly limited, but examples thereof include 3-isocyanate propyl trimethoxy silane, 3-isocyanate propyl methyl dimethoxy silane, 3-isocyanate propyl dimethyl methoxy silane, 3-isocyanate propyl triethoxy silane, 3-isocyanate propyl methyl diethoxy silane, and 3-isocyanate propyl dimethyl ethoxy silane.
[0064] The partial structure represented by the formula (19) or (20) is a divalent linking group containing a bond grafted to an ester bond in the resin.
[0065] The linking group is not limited to being formed by a reaction, but when it is reacted, it is formed, for example, by an insertion reaction of an epoxysilane compound.
[0066] The insertion reaction of an epoxysilane compound is the following reaction: It includes a step of inserting an epoxy group of an epoxysilane compound into an ester bond contained in the main chain of a resin.
[0067] The insertion reaction referred to here refers to, for example, the reaction described in Organic Synthesis Chemistry, Vol. 49, No. 3, p. 218, 1991, as "insertion reaction of an epoxy compound into an ester bond in a polymer chain."
[0068] This reaction mechanism can be expressed by a simple model formula as follows:
[0069] [ka] (D and E represent the constituent parts of the resin, and F represents the constituent part of the epoxy compound.)
[0070] In the above model formula, the ring-opening of the epoxy group can be either α-cleavage or β-cleavage, resulting in two types of compounds. In either case, the epoxy group is inserted into the ester bond in the resin; in other words, the components of the epoxy compound other than the epoxy moiety are grafted to the resin.
[0071] The epoxy silane compound is not particularly limited, but examples thereof include β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropylmethyldiethoxysilane, and the like.
[0072] In addition, R in the formula (1) 1 ~R3 At least one of R in the formula (1) is preferably an alkoxy group or a hydroxy group. 1 ~R 3 However, it is more preferable that each of them is independently an alkoxy group or a hydroxy group.
[0073] These alkoxy groups or hydroxy groups contain many Si-O-bonds, which is thought to enhance the adhesion between resin A and the silicon-containing particles. Through resin A, the adhesion between the binder resin and the silicon-containing particles is increased, and cracking and chipping at the particle interface is suppressed. As a result, it shows a good effect in suppressing cracking and chipping of the toner over long-term use.
[0074] In addition, R in the above formula (1) 1 ~R 3 In order to make one or more of R into a hydroxyl group, 1 ~R 3 A resin in which one or more of the above groups are alkoxy groups may be hydrolyzed to convert the alkoxy groups to hydroxy groups. The hydrolysis method may be any method, but examples thereof include the following methods.
[0075] R in the above formula (1) 1 ~R 3 A resin in which one or more of is an alkoxy group is dissolved or suspended in a suitable solvent (which may be a polymerizable monomer), and the pH is adjusted to acidic using an acid or alkali, and the mixture is mixed and hydrolyzed. Alternatively, hydrolysis may be caused during the production of toner particles.
[0076] Next, a suitable weight average molecular weight (Mw) of the resin A represented by the above formula (1) will be described.
[0077] The weight average molecular weight (Mw) of the resin A represented by the formula (1) is preferably 3000 or more and 100000 or less, more preferably 5000 or more and 30000 or less. By being in the above range, the polymer moiety (L 1 ) has sufficient affinity with the binder resin, and is effective in preventing cracking and chipping over long-term use.
[0078] The method for measuring the weight average molecular weight (Mw) of the resin A represented by the formula (1) will be described later.
[0079] Next, the silicon-containing particles of the present invention will be described.
[0080] The silicon-containing particles of the present invention are characterized in that they are at least one selected from the group consisting of silica and organosilicon polymers.
[0081] The silicon-containing particles are preferably contained in an amount of 0.040% by mass or more and 0.800% by mass or less based on the toner particles. By being in this range, low-temperature fixability is not impaired and good effects are shown in preventing cracking and chipping during long-term use.
[0082] The silicon-containing particles of the present invention are organosilicon polymers and preferably have a structure represented by the following formula (3). R-SiO 3 / 2 Formula (3) (In formula (3), R is an alkyl group having 1 to 4 carbon atoms.)
[0083] The organosilicon polymer having the structure of formula (3) has high affinity with resin A and also with the binder resin, which results in increased adhesion between the binder resin and the silicon-containing particles, suppressing cracking and chipping at the particle interface.
[0084] The organosilicon polymer having the structure of formula (3) is preferably a condensation polymer of an organosilicon compound having the structure represented by the following formula (4).
[0085] [ka] (In formula (4), R 21 represents a hydrocarbon group having 1 to 4 carbon atoms, R 22 , R 23 and R 24each independently represents a halogen atom, a hydroxy group, an acetoxy group, or an alkoxy group.
[0086] From the viewpoint of improving the affinity with the binder resin, R 21 is preferably a hydrocarbon group having 1 to 4 carbon atoms, and more preferably a methyl group.
[0087] R 22 , R 23 and R 24 are each independently a halogen atom, a hydroxy group, an acetoxy group, or an alkoxy group (hereinafter also referred to as a reactive group). These reactive groups undergo hydrolysis, addition polymerization, and condensation polymerization to form a crosslinked structure, thereby making it possible to obtain a toner that is excellent in resistance to component contamination and development durability. From the viewpoints of mild hydrolysis at room temperature and deposition and coating properties on the surface of toner particles, an alkoxy group having 1 to 3 carbon atoms is preferred, and a methoxy group or an ethoxy group is more preferred. In addition, R 22 , R 23 and R 24 The hydrolysis, addition polymerization and condensation polymerization can be controlled by the reaction temperature, reaction time, reaction solvent and pH.
[0088] To obtain the organosilicon polymer used in the present invention, R 21 There are three reactive groups (R 22 , R 23 and R 24 ) (hereinafter also referred to as trifunctional silane) may be used alone or in combination of two or more.
[0089] Examples of the above formula (4) include the following.
[0090] Trifunctional methylsilanes such as methyltrimethoxysilane, methyltriethoxysilane, methyldiethoxymethoxysilane, methylethoxydimethoxysilane, methyltrichlorosilane, methylmethoxydichlorosilane, methylethoxydichlorosilane, methyldimethoxychlorosilane, methylmethoxyethoxychlorosilane, methyldiethoxychlorosilane, methyltriacetoxysilane, methyldiacetoxymethoxysilane, methyldiacetoxyethoxysilane, methylacetoxydimethoxysilane, methylacetoxymethoxyethoxysilane, methylacetoxydiethoxysilane, methyltrihydroxysilane, methylmethoxydihydroxysilane, methylethoxydihydroxysilane, methyldimethoxyhydroxysilane, methylethoxymethoxyhydroxysilane, and methyldiethoxyhydroxysilane.
[0091] Trifunctional silanes such as ethyltrimethoxysilane, ethyltriethoxysilane, ethyltrichlorosilane, ethyltriacetoxysilane, ethyltrihydroxysilane, propyltrimethoxysilane, propyltriethoxysilane, propyltrichlorosilane, propyltriacetoxysilane, propyltrihydroxysilane, butyltrimethoxysilane, butyltriethoxysilane, butyltrichlorosilane, butyltriacetoxysilane, and butyltrihydroxysilane.
[0092] In the present invention, silica particles can be used as the silicon-containing particles.
[0093] Methods for producing silica particles include a combustion method in which a silane compound is burned (i.e., a method for producing fumed silica), a deflagration method in which metal silicon powder is explosively burned, a wet method in which silica is obtained by a neutralization reaction between sodium silicate and a mineral acid (of these, those synthesized under alkaline conditions are called the precipitation method, and those synthesized under acidic conditions are called the gel method), and a sol-gel method (the so-called Stoeber method) in which silica particles are obtained by hydrolysis of alkoxysilanes such as hydrocarbyloxysilanes.
[0094] The number-average particle size of the silicon-containing particles in the present invention is preferably 5 nm to 200 nm, in which case the low-temperature fixability is not impaired and good cracking and chipping prevention effects are observed during long-term use.
[0095] Next, the colorant will be described.
[0096] The toner of the present invention may contain a colorant, if necessary. The colorant is not particularly limited, and the following known colorants may be used.
[0097] Examples of yellow pigments that can be used include condensed azo compounds such as yellow iron oxide, navel yellow, naphthol yellow S, Hansa yellow G, Hansa yellow 10G, benzidine yellow G, benzidine yellow GR, quinoline yellow lake, permanent yellow NCG, and tartrazine lake, isoindolinone compounds, anthraquinone compounds, azo metal complexes, methine compounds, and allylamide compounds. Specific examples include the following.
[0098] CI Pigment Yellow 12, 13, 14, 15, 17, 62, 74, 83, 93, 94, 95, 109, 110, 111, 128, 129, 147, 155, 168, 180.
[0099] Orange pigments include the following:
[0100] Permanent Orange GTR, Pyrazolone Orange, Balkan Orange, Benzidine Orange G, Induthrene Brilliant Orange RK, Induthrene Brilliant Orange GK.
[0101] Examples of red pigments include condensed azo compounds such as red iron oxide, permanent red 4R, lithol red, pyrazolone red, watching red calcium salt, lake red C, lake D, brilliant carmine 6B, brilliant carmine 3B, eoxin lake, rhodamine lake B, and alizarin lake, diketopyrrolopyrrole compounds, anthraquinone compounds, quinacridone compounds, basic dye lake compounds, naphthol compounds, benzimidazolone compounds, thioindigo compounds, and perylene compounds. Specific examples include the following.
[0102] CI Pigment Red 2, 3, 5, 6, 7, 23, 48:2, 48:3, 48:4, 57:1, 81:1, 122, 144, 146, 166, 169, 177, 184, 185, 202, 206, 220, 221, 254.
[0103] Examples of blue pigments include alkali blue lake, Victoria blue lake, phthalocyanine blue, metal-free phthalocyanine blue, phthalocyanine blue partial chloride, fast sky blue, copper phthalocyanine compounds such as indanthrene blue BG and their derivatives, anthraquinone compounds, basic dye lake compounds, etc. Specific examples include the following.
[0104] CI Pigment Blue 1, 7, 15, 15:1, 15:2, 15:3, 15:4, 60, 62, 66.
[0105] Purple pigments include Fast Violet B and Methyl Violet Lake.
[0106] Green pigments include Pigment Green B, Malachite Green Lake, and Final Yellow Green G. White pigments include zinc oxide, titanium oxide, antimony white, and zinc sulfide.
[0107] Examples of black pigments include carbon black, aniline black, non-magnetic ferrite, magnetite, and pigments toned to black using the above-mentioned yellow, red and blue colorants. These colorants can be used alone or in combination, or in the form of a solid solution.
[0108] If necessary, the colorant may be subjected to a surface treatment.
[0109] The content of the colorant is preferably 1.0 part by mass or more and 15.0 parts by mass or less with respect to 100.0 parts by mass of the binder resin.
[0110] Next, the wax will be described.
[0111] The toner of the present invention preferably contains a wax as necessary. Examples of wax include the following: aliphatic hydrocarbon waxes such as low molecular weight polyethylene, low molecular weight polypropylene, microcrystalline wax, Fischer-Tropsch wax, and paraffin wax; oxides of aliphatic hydrocarbon waxes such as oxidized polyethylene wax, or block copolymers thereof; waxes mainly composed of fatty acid esters such as carnauba wax and montanic acid ester wax, and partially or completely deoxidized fatty acid esters such as deoxidized carnauba wax; saturated straight-chain fatty acids such as palmitic acid, stearic acid, and montanic acid; unsaturated fatty acids such as brassidic acid, eleostearic acid, and parinaric acid; saturated alcohols such as stearyl alcohol, aralkyl alcohol, behenyl alcohol, carnaubyl alcohol, ceryl alcohol, and melissyl alcohol; polyhydric alcohols such as sorbitol; fatty acid amides such as linoleic acid amide, oleic acid amide, and lauric acid amide; methylene bismuth acid, methyl ... Examples of such waxes include saturated fatty acid bisamides such as stearic acid amide, ethylene biscapric acid amide, ethylene bislauric acid amide, and hexamethylene bisstearic acid amide; unsaturated fatty acid amides such as ethylene bisoleic acid amide, hexamethylene bisoleic acid amide, N,N'dioleyl adipic acid amide, and N,N'dioleyl sebacic acid amide; aromatic bisamides such as m-xylene bisstearic acid amide and N,N'distearyl isophthalic acid amide; fatty metal salts (generally known as metal soaps) such as calcium stearate, calcium laurate, zinc stearate, and magnesium stearate; waxes obtained by grafting aliphatic hydrocarbon waxes with vinyl monomers such as styrene and acrylic acid; partial esters of fatty acids and polyhydric alcohols such as behenic acid monoglyceride; and methyl ester compounds having hydroxyl groups obtained by hydrogenating vegetable oils and fats. The waxes mentioned above can be used alone or in combination of two or more.
[0112] Examples of aliphatic alcohols forming ester waxes include 1-hexanol, 1-heptanol, 1-octanol, 1-nonanol, 1-decanol, undecyl alcohol, lauryl alcohol, myristyl alcohol, 1-hexadecanol, stearyl alcohol, arachidyl alcohol, behenyl alcohol, and lignoceryl alcohol. Examples of aliphatic carboxylic acids include pentanoic acid, hexanoic acid, heptanoic acid, octanoic acid, nonanoic acid, decanoic acid, lauric acid, myristic acid, palmitic acid, stearic acid, arachidic acid, behenic acid, and lignoceric acid.
[0113] The content of the wax is preferably 0.5 parts by mass or more and 20.0 parts by mass or less with respect to 100.0 parts by mass of the binder resin or polymerizable monomer.
[0114] Next, the charge control agent will be described.
[0115] The toner particles of the present invention may contain a charge control agent. Any known charge control agent can be used. In particular, a charge control agent that has a high charging speed and can stably maintain a constant charge amount is preferred. Furthermore, when the toner particles are produced by a direct polymerization method, a charge control agent that has low polymerization inhibition properties and is substantially free of solubilized substances in an aqueous medium is particularly preferred.
[0116] As the charge control agent that controls the toner particles to have a negative charge, the following can be mentioned.
[0117] Organometallic compounds and chelating compounds include monoazo metal compounds, acetylacetone metal compounds, aromatic oxycarboxylic acids, aromatic dicarboxylic acids, oxycarboxylic acids and dicarboxylic acid-based metal compounds. Other examples include aromatic oxycarboxylic acids, aromatic mono- and polycarboxylic acids and their metal salts, anhydrides or esters, and phenol derivatives such as bisphenol. Further examples include urea derivatives, metal-containing salicylic acid compounds, metal-containing naphthoic acid compounds, boron compounds, quaternary ammonium salts, and calixarenes.
[0118] On the other hand, examples of charge control agents that control the toner particles to have a positive charge include the following.
[0119] Nigrosine and nigrosine modifications such as fatty acid metal salts; guanidine compounds; imidazole compounds; onium salts such as quaternary ammonium salts such as tributylbenzylammonium-1-hydroxy-4-naphthosulfonate, tetrabutylammonium tetrafluoroborate, and their analogues such as phosphonium salts, and lake pigments thereof; triphenylmethane dyes and lake pigments thereof (lake agents include phosphotungstic acid, phosphomolybdic acid, phosphotungstomolybdic acid, tannic acid, lauric acid, gallic acid, ferricyanide, ferrocyanide, etc.); metal salts of higher fatty acids; resin-based charge control agents.
[0120] These charge control agents may be contained alone or in combination of two or more kinds. The amount of these charge control agents added is preferably 0.01 parts by mass or more and 10 parts by mass or less with respect to 100 parts by mass of the binder resin.
[0121] Next, the external additives will be described.
[0122] The toner particles of the present invention may be used as a toner as it is, but in order to improve the flowability, chargeability, cleaning properties, etc., so-called external additives such as a fluidizing agent and a cleaning aid may be added to the toner.
[0123] Examples of the external additive include inorganic oxide fine particles such as silica fine particles, alumina fine particles, and titanium oxide fine particles, inorganic stearic acid compound fine particles such as aluminum stearate fine particles and zinc stearate fine particles, and inorganic titanic acid compound fine particles such as strontium titanate and zinc titanate. These may be used alone or in combination of two or more.
[0124] These inorganic particles are preferably surface-treated with a silane coupling agent, a titanium coupling agent, a higher fatty acid, a silicone oil, etc., to improve heat resistance and storage stability and environmental stability. The BET specific surface area of the external additive is 10 m 2 / g or more 450m 2 It is preferable that the molecular weight is not more than 1 / g.
[0125] The BET specific surface area can be determined by a low-temperature gas adsorption method using a dynamic constant pressure method in accordance with the BET method (preferably the BET multipoint method). For example, a specific surface area measuring device (product name: Gemini 2375 Ver. 5.0, manufactured by Shimadzu Corporation) is used to adsorb nitrogen gas onto the surface of a sample, and the BET multipoint method is used to measure the BET specific surface area (m 2 / g) can be calculated.
[0126] The total amount of these various external additives added is preferably 0.05 parts by mass or more and 10 parts by mass or less, more preferably 0.1 parts by mass or more and 5 parts by mass or less, based on 100 parts by mass of the toner particles. Also, various external additives may be used in combination.
[0127] Next, the developer will be described.
[0128] The toner of the present invention can be used as a magnetic or non-magnetic one-component developer, but may also be mixed with a carrier and used as a two-component developer.
[0129] As the carrier, magnetic particles made of known materials such as metals such as iron, ferrite, magnetite, and alloys of these metals with metals such as aluminum and lead can be used. Of these, it is preferable to use ferrite particles. As the carrier, a coated carrier in which the surface of magnetic particles is coated with a coating agent such as resin, or a resin dispersion type carrier in which magnetic fine powder is dispersed in a binder resin can also be used.
[0130] The carrier preferably has a volume average particle size of 15 μm or more and 100 μm or less, and more preferably has a volume average particle size of 25 μm or more and 80 μm or less.
[0131] Next, the toner particles and the method for producing the toner will be described.
[0132] The toner particles can be produced by known means, and a kneading and pulverizing method or a wet production method can be used. Examples of the wet production method include a suspension polymerization method, a dissolution suspension method, an emulsion polymerization aggregation method, and an emulsion aggregation method. Among them, the suspension polymerization method and the kneading and pulverizing method are more preferable because they can efficiently cause silicon-containing particles to exist in the vicinity of the resin A in the toner particles.
[0133] Next, the production of toner particles by suspension polymerization will be described.
[0134] (Preparation process of polymerizable monomer composition) In the suspension polymerization method, first, a polymerizable monomer for producing a binder resin, resin A represented by the above formula (1), silicon-containing particles, and, if necessary, wax, a colorant, a charge control agent, a crosslinking agent, a polymerization initiator, and other additives are uniformly dissolved or dispersed using a dispersing machine such as a ball mill or an ultrasonic dispersing machine to obtain a polymerizable monomer composition. Examples of the polymerizable monomer include those exemplified as the monomers forming the above-mentioned styrene-acrylic copolymer.
[0135] The silicon-containing particles and colorant may be dispersed in advance in a polymerizable monomer or an organic solvent using a medium stirring mill or the like and then mixed with the other compositions, or may be dispersed after all of the compositions have been mixed.
[0136] The silicon-containing particles may be added alone, or may be added by reusing toner particles that already contain silicon-containing particles as a raw material.
[0137] (Dispersion process of polymerizable monomer composition (granulation process)) Next, the polymerizable monomer composition is poured into a previously prepared aqueous medium, and droplets of the polymerizable monomer composition are formed into a desired toner particle size using a stirrer or disperser having high shear force.
[0138] The aqueous medium in the granulation process preferably contains a dispersion stabilizer in order to control the particle size of the toner particles, sharpen the particle size distribution, and suppress the coalescence of the toner particles during the manufacturing process. Dispersion stabilizers are generally broadly classified into polymers that exhibit repulsive force due to steric hindrance and poorly water-soluble inorganic compounds that stabilize dispersion by electrostatic repulsive force. Since fine particles of poorly water-soluble inorganic compounds are dissolved by acid or alkali, they can be dissolved and easily removed by washing with acid or alkali after polymerization, and are therefore preferably used. As the dispersion stabilizer for poorly water-soluble inorganic compounds, one containing any of magnesium, calcium, barium, zinc, aluminum, and phosphorus is preferably used. More preferably, one containing any of magnesium, calcium, aluminum, and phosphorus is desired. Specifically, the following can be mentioned.
[0139] Magnesium phosphate, tricalcium phosphate, aluminum phosphate, zinc phosphate, magnesium carbonate, calcium carbonate, magnesium hydroxide, calcium hydroxide, aluminum hydroxide, calcium metasilicate, calcium sulfate, barium sulfate, hydroxyapatide. When using the poorly water-soluble inorganic dispersant, it may be used as it is, but in order to obtain finer particles, the inorganic dispersant particles can be generated in an aqueous medium and used. For example, in the case of tricalcium phosphate, a sodium phosphate aqueous solution and a calcium chloride aqueous solution are mixed under high speed stirring to generate water-insoluble calcium phosphate, which enables more uniform and fine dispersion.
[0140] The dispersion stabilizer may be used in combination with an organic compound such as polyvinyl alcohol, gelatin, methyl cellulose, methylhydroxypropyl cellulose, ethyl cellulose, sodium salt of carboxymethyl cellulose, or starch. The dispersion stabilizer is preferably used in an amount of 0.1 to 20.0 parts by mass per 100 parts by mass of the polymerizable monomer.
[0141] Furthermore, in order to make these dispersion stabilizers finer, a surfactant may be used in an amount of 0.1 to 10.0 parts by mass relative to 100 parts by mass of the polymerizable monomer. Specifically, commercially available nonionic, anionic, or cationic surfactants can be used. For example, sodium dodecyl sulfate, sodium tetradecyl sulfate, sodium pentadecyl sulfate, sodium octyl sulfate, sodium oleate, sodium laurate, potassium stearate, and calcium oleate are preferably used.
[0142] (Polymerization process) After the granulation step, or while the granulation step is being carried out, the temperature is preferably set to 50° C. or higher and 90° C. or lower to polymerize the polymerizable monomers contained in the polymerizable monomer composition, thereby obtaining a toner particle dispersion.
[0143] In the polymerization step, it is preferable to carry out a stirring operation so that the temperature distribution in the vessel becomes uniform. When a polymerization initiator is added, it can be added at any timing and for any required time. In addition, the temperature may be raised in the latter half of the polymerization reaction in order to obtain a desired molecular weight distribution, and further, in order to remove unreacted polymerizable monomers, by-products, etc. from the system, a part of the aqueous medium may be distilled off by a distillation operation in the latter half of the reaction or after the reaction is completed. The distillation operation can be carried out under normal pressure or reduced pressure.
[0144] The polymerization initiator used in the suspension polymerization method is preferably one having a half-life of 0.5 to 30 hours during the polymerization reaction. When the polymerization reaction is carried out using an amount of 0.5 to 20 parts by mass relative to 100 parts by mass of the polymerizable monomer, a polymer having a maximum molecular weight between 5,000 and 50,000 can be obtained. As the polymerization initiator, an oil-soluble initiator is generally used. For example, the following can be mentioned.
[0145] Examples of the initiator include azo compounds such as 2,2'-azobisisobutyronitrile, 2,2'-azobis-2,4-dimethylvaleronitrile, 1,1'-azobis(cyclohexane-1-carbonitrile), and 2,2'-azobis-4-methoxy-2,4-dimethylvaleronitrile; and peroxide initiators such as acetylcyclohexylsulfonyl peroxide, diisopropyl peroxycarbonate, decanonyl peroxide, lauroyl peroxide, stearoyl peroxide, propionyl peroxide, acetyl peroxide, tert-butylperoxy-2-ethylhexanoate, benzoyl peroxide, tert-butylperoxyisobutyrate, cyclohexanone peroxide, methyl ethyl ketone peroxide, dicumyl peroxide, tert-butyl hydroperoxide, di-tert-butyl peroxide, tert-butyl peroxypivalate, and cumene hydroperoxide.
[0146] As the polymerization initiator, a water-soluble initiator may be used as necessary, and examples thereof include the following.
[0147] Ammonium persulfate, potassium persulfate, 2,2'-azobis(N,N'-dimethyleneisobutyromidine) hydrochloride, 2,2'-azobis(2-aminodinopropane) hydrochloride, azobis(isobutylamidine) hydrochloride, 2,2'-azobisisobutyronitrile sodium sulfonate, ferrous sulfate, or hydrogen peroxide.
[0148] These polymerization initiators can be used alone or in combination of two or more. In order to control the degree of polymerization of the polymerizable monomer, a chain transfer agent, a polymerization inhibitor, etc. can also be further added.
[0149] (Solid-liquid separation process, washing process and drying process) For the purpose of removing the dispersion stabilizer attached to the surface of the toner particles, the toner particle dispersion may be treated with an acid or an alkali.
[0150] The solid-liquid separation for obtaining toner particles from the obtained toner particle dispersion can be carried out by a general filtration method, and then, in order to remove foreign matter that has not been completely removed from the toner particle surface, it is preferable to further wash the toner particles by reslurrying or washing with washing water. After sufficient washing, solid-liquid separation is again carried out to obtain a toner cake. Thereafter, the toner cake is dried by a known drying means, and if necessary, a particle group having a particle size other than the specified particle size is separated by classification to obtain toner particles.
[0151] Next, an example of producing toner particles using the kneading and pulverizing method will be described.
[0152] In the kneading and pulverizing method, first, a mixture containing a binder resin, resin A represented by the above formula (1), silicon-containing particles, and, if necessary, a wax, a colorant, a charge control agent, and other additives is thoroughly mixed by a mixer such as a Henschel mixer, a ball mill, etc. Then, the mixture is melt-kneaded using a thermal kneader such as a heating roll, a kneader, or an extruder to disperse or dissolve various materials to obtain a melt-kneaded product, which is then passed through a cooling and solidifying process, a pulverizing process, a classification process, and, if necessary, a surface treatment process to obtain toner particles.
[0153] In the pulverization step, a known pulverization device such as a mechanical impact type, a jet type, etc. may be used. The order of the classification step and the surface treatment step does not matter.
[0154] (External addition process) If necessary, an external additive may be added to the obtained toner particles. The external addition step is carried out by putting the external additive and the toner particles into a mixer equipped with a blade rotating at high speed and thoroughly mixing them.
[0155] The particle size of the toner particles of the present invention is preferably a weight average particle size of 3.0 μm or more and 10.0 μm or less from the viewpoint of obtaining a high-definition and high-resolution image. The weight average particle size of the toner can be measured by a capillary electrical resistance method. For example, it can be measured using a "Coulter Counter Multisizer 3" (manufactured by Beckman Coulter, Inc.).
[0156] The methods for measuring the various physical properties of the toner of the present invention will be described below.
[0157] <Separation of toner and additives> In the case of a toner having an external additive on the surface of the toner particles, the toner particles and the external additive are separated by the following method to obtain toner particles.
[0158] Add 160 g of sucrose (Kishida Chemical) to 100 mL of ion-exchanged water and dissolve in a hot water bath to prepare a concentrated sucrose solution. Add 31 g of the concentrated sucrose solution and 6 mL of Contaminon N (a 10% aqueous solution of a pH 7 neutral detergent for cleaning precision measuring instruments, consisting of a nonionic surfactant, an anionic surfactant, and an organic builder, manufactured by Wako Pure Chemical Industries, Ltd.) to a centrifuge tube (volume 50 mL) to prepare a dispersion. Add 1.0 g of toner to this dispersion and break up the toner clumps with a spatula or the like.
[0159] The centrifuge tube is shaken in a shaker at 350 strokes per minute (spm) for 20 minutes. After shaking, the solution is transferred to a glass tube for a swing rotor (capacity 50 mL) and separated in a centrifuge (H-9R, manufactured by Kokusan Co., Ltd.) at 3500 rpm for 30 minutes. This operation separates the toner particles from the removed external additives. It is visually confirmed that the toner and the aqueous solution are sufficiently separated, and the toner separated in the top layer is collected with a spatula or the like. The collected toner is filtered with a vacuum filter and then dried in a dryer for at least 1 hour to obtain toner particles. This operation is carried out multiple times to obtain the required amount of toner particles.
[0160] <Extraction of Resin A represented by Formula (1) from Toner Particles> The resin represented by formula (1) in the toner particles was extracted with tetrahydrofuran (THF) and separated by a solvent gradient elution method. The preparation method is shown below.
[0161] 10.0 g of toner particles were weighed, placed in a cylindrical filter paper (Toyo Roshi No. 86R) and subjected to a Soxhlet extractor. Extraction was performed for 20 hours using 200 mL of THF as a solvent, and the solid obtained by removing the solvent from the extract is the THF-soluble fraction. The THF-soluble fraction contains the resin represented by formula (1). This was repeated multiple times to obtain the required amount of THF-soluble fraction.
[0162] For the solvent gradient elution, gradient preparative HPLC (Shimadzu LC-20AP high pressure gradient preparative system, Waters SunFire preparative column 50mmφ250mm) was used, and separation was performed at a flow rate of 50ml / min. THF, chloroform, and toluene were appropriately selected as good solvents for the mobile phase, and acetonitrile, acetone, methanol, and n-hexane were appropriately selected as poor solvents. By repeating the solvent gradient elution as necessary, resin A represented by formula (1) was obtained.
[0163] <Method for measuring silicon concentration in resin A represented by formula (1)> The silicon content in resin A represented by formula (1) is measured using a wavelength dispersive X-ray fluorescence analyzer "Axios" (PANalytical) and the accompanying dedicated software "SuperQ ver.4.0F" (PANalytical) for setting measurement conditions and analyzing measurement data. Rh is used as the anode of the X-ray tube, the measurement atmosphere is vacuum, the measurement diameter (collimator mask diameter) is 27 mm, and the measurement time is 10 seconds.
[0164] As a measurement sample, resin A represented by formula (1) itself is used, or resin A extracted from toner particles by the above-mentioned extraction method is used.
[0165] For 100.00 parts by mass of the measurement sample, silica (SiO 2 ) fine powder [product name: AEROSIL NAX50, specific surface area: 40±10, carbon content: 0.45-0.85%; manufactured by Nippon Aerosil Co., Ltd.] was added to the mixture so that the amount was 0.50 parts by mass, and thoroughly mixed using a coffee mill. Similarly, silica fine powder was mixed with the measurement sample so that the amount was 5.00 parts by mass, 10.00 parts by mass, and 15.00 parts by mass, respectively, and these were used as samples for the calibration curve. The measurement pellets were prepared using a tablet molding compression machine "BRE-32" (manufactured by Maekawa Test Machinery Manufacturing Co., Ltd.). 4 g of the measurement sample was placed in a dedicated aluminum ring for pressing, flattened, and pressed at 20 MPa for 60 seconds to obtain measurement pellets molded to a thickness of 2 mm and a diameter of 39 mm.
[0166] For each measurement pellet, the count rate (unit: cps) of the Si-Kα ray observed at a diffraction angle (2θ) = 109.08° when PET is used as the analyzing crystal is measured. The acceleration voltage and current of the X-ray generator are 24 kV and 100 mA, respectively. A linear calibration curve is obtained by plotting the obtained X-ray count rate on the vertical axis and the Si concentration in each calibration curve sample on the horizontal axis.
[0167] Next, a measurement pellet is similarly prepared for the measurement sample, and the count rate of the Si-Kα ray is measured. Then, the silicon concentration (mass%) in the resin, which is represented by the formula (1), is calculated from the obtained calibration curve.
[0168] <Confirmation of the structure of resin A represented by formula (1) (R 1 ~R 3 )> Functional groups contained in resin A represented by formula (1) and polymer moieties P in the structure represented by formula (1) 1 , L 1 Part, R 1 ~R 3 The part is, 1 H-NMR analysis, 13 C-NMR analysis, 29 The measurement is performed using Si-NMR analysis and FT-IR analysis. The measurement sample is either Resin A itself or Resin A extracted from the toner particles by the above-mentioned extraction method.
[0169] L 1 When the compound contains an amide bond as represented by the formula (17), 1 It can be identified by H-NMR analysis. Specifically, it can be identified by the chemical shift value of the proton at the NH site of the amide group, and the amount of the amide group can be quantified by calculating the integral value.
[0170] In addition, R in the structure represented by formula (1) 1 ~R 3 When contains an alkoxy group or a hydroxy group, 29 The valence of the alkoxy group or hydroxy group relative to the silicon atom can be determined by the method shown in "Si-NMR (solid) measurement conditions."
[0171] ( 29 Si-NMR (solid state) measurement conditions Equipment: JEOL RESONANCE JNM-ECX500II Sample tube: 3.2mmφ Sample: 150 mg of resin A represented by formula (1) Measurement temperature: room temperature Pulse mode: CP / MAS Measured nuclear frequency: 97.38MHz (29Si) Reference material: DSS (external standard: 1.534ppm) Sample rotation speed: 10kHz Contact time: 10ms Delay time: 2s Accumulation count: 8192 times
[0172] The above measurement allows the abundance ratio of multiple silane components according to the number of oxygen atoms bonded to silicon to be determined by peak separation and integration using curve fitting. In this way, the abundance ratio of R 1 ~R 3 The number of alkoxy or hydroxy groups can be confirmed.
[0173] <Confirmation of the structure of resin A represented by formula (1) (P 1 and L 1 )> P in the resin represented by formula (1) 1 , L 1 and R 1 ~R 3 The structure of 13 This can be confirmed by C-NMR (solid state) measurement. The measurement conditions are as follows.
[0174] ( 13 C-NMR (solid state) measurement conditions Equipment: JEOL RESONANCE JNM-ECX500II Sample tube: 3.2mmφ Sample size: 150mg Measurement temperature: room temperature Pulse mode: CP / MAS Measurement nuclear frequency: 123.25MHz ( 13 C) Reference substance: Adamantane (external standard: 29.5ppm) Sample rotation speed: 20kHz Contact time: 2ms Delay time: 2s Number of times accumulated: 1024
[0175] ( 1 H-NMR analysis (solution) measurement conditions Equipment: JEOL RESONANCE JNM-EX400 Sample tube: 3.2mmφ Sample size: 10mg Solvent: CDCl 3 Measurement temperature: room temperature Measurement frequency: 400MHz Pulse condition: 5.0μs Frequency range: 10500Hz Number of times accumulated: 64 P in formula (1) 1 , L 1 and R 1 ~R 3 The various peaks are separated according to the type of 1 , L 1 and R 1 ~R 3 Determine the type of.
[0176] <Method for identifying organosilicon polymer having the structure of formula (3)> To confirm the structure of the organosilicon polymer contained in the toner particles represented by formula (3), the organosilicon polymer represented by formula (3) itself can be used, or the organosilicon polymer extracted from the toner particles by the method described below can be used.
[0177] 1 g of the toner particles collected by the method described above is placed in a vial, dissolved in 31 g of chloroform, and dispersed in an ultrasonic homogenizer for 30 minutes to prepare a dispersion liquid. Ultrasonic processing device: Ultrasonic homogenizer VP-050 (manufactured by Taitec Co., Ltd.) Microchip: Step type microchip, tip diameter φ2mm Microchip tip position: Center of glass vial, 5 mm above the bottom of the vial Ultrasonic conditions: intensity 30%, 30 minutes. During this time, ultrasonic waves are applied while cooling the vial with ice water to prevent the dispersion from heating up.
[0178] The dispersion liquid was transferred to a glass tube (50 mL) for a swing rotor and centrifuged at 58.33 S in a centrifuge (H-9R; manufactured by Kokusan Co., Ltd.). -1Centrifugation is performed under conditions of 100°C for 30 minutes. After centrifugation, organosilicon polymer particles are separated in the glass tube. These are extracted and dispersed again in 10g of chloroform for washing, and the organosilicon polymer particles are separated using a centrifuge. After washing again, the extracted organosilicon polymer particles are vacuum dried (40°C / 24 hours) to remove the chloroform and prepare the sample.
[0179] The resulting sample is weighed to determine the content of the organosilicon polymer particles in the toner particles.
[0180] The presence or absence of an alkyl group represented by R in formula (3) is 13 The detailed structure of formula (1) is 1 H-NMR, 13 C-NMR and 29 The measurement was confirmed by Si-NMR. The equipment and measurement conditions used are as follows:
[0181] (Measurement conditions) Equipment: BRUKER AVANCE III 500 Probe: 4mm MAS BB / 1H Measurement temperature: room temperature Sample rotation speed: 6kHz Sample: 150 mg of a measurement sample (tetrahydrofuran (THF)-insoluble portion of toner particles for NMR measurement) is placed in a sample tube with a diameter of 4 mm.
[0182] Using this method, the presence or absence of an alkyl group represented by R in formula (3) is confirmed. If a signal is confirmed, the structure of formula (3) is deemed to be "present."
[0183] ( 13 C-NMR (solid state) measurement conditions Equipment: JEOL RESONANCE JNM-ECX500II Measurement nuclear frequency: 125.77MHz Reference substance: Glycine (external standard: 176.03ppm) Observation width: 37.88kHz Measurement method: CP / MAS Contact time: 1.75ms Repeat time: 4s Accumulation count: 2048 times LB value: 50Hz
[0184] ( 29 Si-NMR (solid state) measurement method (Measurement conditions) Equipment: BRUKER AVANCE III 500 Probe: 4mm MAS BB / 1H Measurement temperature: room temperature Sample rotation speed: 6kHz Sample: 150 mg of a measurement sample (THF insoluble portion of toner particles for NMR measurement) is placed in a sample tube with a diameter of 4 mm. Measurement nuclear frequency: 99.36MHz Reference material: DSS (external standard: 1.534ppm) Observation width: 29.76kHz Measurement method: DD / MAS, CP / MAS 29 Si 90° Pulse width: 4.00μs@-1dB Contact time: 1.75ms~10ms Repeat time: 30s (DD / MASS), 10s (CP / MAS) Accumulation count: 2048 times LB value: 50Hz
[0185] <How to confirm the number-average particle size of silicon-containing particles> The number average particle size of the silicon-containing particles is measured by scanning electron microscope (SEM) observation. The SEM observation method is as follows. Images taken with a Hitachi ultra-high resolution field emission scanning electron microscope S-4800 (Hitachi High-Technologies Corporation) are used. The image taking conditions for the S-4800 are as follows.
[0186] (1) Sample preparation A thin layer of conductive paste (TED PELLA, Inc., Product No. 16053, PELCO Colloidal Graphite, Isopropanol base) is applied to a sample stage (aluminum sample stage 15 mm x 6 mm), and the target sample is sprayed onto it. After removing excess sample from the sample stage with air blowing, platinum is evaporated at 15 mA for 15 seconds. The sample stage is set in the sample holder, and the sample stage height is adjusted to 30 mm using the sample height gauge.
[0187] (2) S-4800 observation condition setting Pour liquid nitrogen into the anti-contamination trap attached to the S-4800 housing until it overflows, and leave it for 30 minutes. Start the S-4800's "PC-SEM" and perform flushing (cleaning the FE chip, which is the electron source). Click the accelerating voltage display area on the control panel on the screen, and press the [Flushing] button to open the flushing execution dialog. Check that the flushing intensity is 2, and execute it. Check that the emission current due to flushing is 20 to 40 μA. Insert the sample holder into the sample chamber of the S-4800 housing. Press [Origin] on the control panel to move the sample holder to the observation position.
[0188] Click the accelerating voltage display to open the HV setting dialog, and set the accelerating voltage to [2.0 kV] and the emission current to [10 μA]. In the [Basic] tab of the operation panel, set the signal selection to [SE], select the SE detector to [Bottom (L)], and set the mode to observe the backscattered electron image. In the same [Basic] tab of the operation panel, set the probe current in the electron optical system condition block to [Normal], the focus mode to [UHR], and the WD to [8.0 mm]. Press the [ON] button in the accelerating voltage display on the control panel to apply the accelerating voltage.
[0189] (3) Focus adjustment Drag within the magnification display on the control panel to set the magnification to 5000 (5k). Rotate the focus knob [COARSE] on the operation panel to adjust the aperture alignment once the image is in focus to a certain extent. Click [Align] on the control panel to display the alignment dialog and select [Beam]. Rotate the STIGMA / ALIGNMENT knobs (X, Y) on the operation panel to move the displayed beam to the center of the concentric circles.
[0190] Next, select [Aperture] and turn the STIGMA / ALIGNMENT knobs (X,Y) one by one to stop the image movement or adjust it so that it moves as little as possible. Close the Aperture dialog and use autofocus to adjust the focus. Repeat this operation two more times to adjust the focus. With the midpoint of the maximum diameter of the observed particle aligned with the center of the measurement screen, drag within the magnification display area of the control panel to set the magnification to 10,000 (10k). Turn the focus knob [COARSE] on the operation panel until the image is in focus to a certain extent, then adjust the aperture alignment. Click [Align] on the control panel to display the alignment dialog and select [Beam]. Turn the STIGMA / ALIGNMENT knobs (X,Y) on the operation panel to move the displayed beam to the center of the concentric circles.
[0191] Next, select [Aperture] and turn the STIGMA / ALIGNMENT knobs (X, Y) one by one to stop the image movement or adjust it so that the movement is minimized. Close the Aperture dialog and adjust the focus using autofocus. After that, set the magnification to 100000 (100k) times and adjust the focus using the focus knob and STIGMA / ALIGNMENT knob as above, then use autofocus to focus again. Repeat this operation to adjust the focus.
[0192] (4) Image storage Adjust the brightness in ABC mode, then take and save a photo with a size of 640 x 480 pixels.
[0193] From the obtained SEM observation results, the number-average particle size (D1) of 500 silicon-containing particles is calculated using image processing software (Image J). The measurement method is as follows. Measurement of organosilicon polymer particles From the measurement commands, select the maximum length of the selected shape and measure the particle size of the organosilicon polymer particles. This operation is repeated several times to obtain the average value of 500 points, thereby calculating the number average particle size of the silicon-containing particles.
[0194] <Method of measuring weight average molecular weight (Mw)> The weight average molecular weight (Mw) of the resin A represented by formula (1) is measured by gel permeation chromatography (GPC) as follows.
[0195] First, a sample is dissolved in tetrahydrofuran (THF) at room temperature for 24 hours. The resulting solution is then filtered through a solvent-resistant membrane filter "Myshoridisc" (manufactured by Tosoh Corporation) with a pore size of 0.2 μm to obtain a sample solution. The sample solution is prepared so that the concentration of components soluble in THF is 0.6% by mass or more and 1.0% by mass or less. This sample solution is used to perform measurements under the following conditions. Equipment: HLC8120 GPC (detector: RI) (Tosoh Corporation) Column: Shodex KF-801, 802, 803, 804, 805, 806, 807 (Showa Denko) Eluent: tetrahydrofuran (THF) Flow rate: 1.0mL / min Oven temperature: 40.0℃ Sample injection volume: 0.10 mL
[0196] In calculating the molecular weight of the sample, a molecular weight calibration curve prepared using standard polystyrene resins (product names: "TSK Standard Polystyrene F-850, F-450, F-288, F-128, F-80, F-40, F-20, F-10, F-4, F-2, F-1, A-5000, A-2500, A-1000, A-500", manufactured by Tosoh Corporation) is used.
[0197] <Method for measuring the acid value of resin> The acid value is the number of milligrams of potassium hydroxide required to neutralize the acid contained in 1 g of a sample. The acid value of a resin is measured in accordance with JIS K 0070-1992, and specifically, it is measured according to the following procedure.
[0198] (1) Preparation of reagents Dissolve 1.0 g of phenolphthalein in 90 mL of ethyl alcohol (95% by volume), and add ion-exchanged water to make 100 mL to obtain a phenolphthalein solution.
[0199] Dissolve 7 g of special grade potassium hydroxide in 5 mL of water and add ethyl alcohol (95% by volume) to make 1 L. Place in an alkali-resistant container to avoid contact with carbon dioxide, etc., leave for 3 days, then filter to obtain potassium hydroxide solution. Store the resulting potassium hydroxide solution in an alkali-resistant container.
[0200] The factor of the potassium hydroxide solution is calculated by taking 25 mL of 0.1 mol / L hydrochloric acid in an Erlenmeyer flask, adding a few drops of the phenolphthalein solution, titrating with the potassium hydroxide solution, and calculating the amount of the potassium hydroxide solution required for neutralization. The 0.1 mol / L hydrochloric acid used is prepared in accordance with JIS K 8001-1998.
[0201] (2) Operation (A) Main Test Weigh out 2.0 g of the crushed sample into a 200 ml Erlenmeyer flask, add 100 ml of a toluene / ethanol (2:1) mixed solution, and dissolve for 5 hours. Next, add a few drops of the phenolphthalein solution as an indicator, and titrate with the potassium hydroxide solution. The end point of the titration is when the light red color of the indicator continues for about 30 seconds. (B) Blank test The titration is carried out in the same manner as above, except that no sample is used (i.e., only the toluene / ethanol (2:1) mixed solution is used).
[0202] (3) The obtained result is substituted into the following formula to calculate the acid value. A = [(CB) × f × 5.61] / S Here, A is the acid value (mgKOH / g), B is the amount of potassium hydroxide solution added for the blank test (ml), C is the amount of potassium hydroxide solution added for the main test (ml), f is the factor of the potassium hydroxide solution, and S is the mass of the sample (g).
[0203] <Method of measuring weight average particle size (D4)> The weight average particle diameter (D4) of the toner particles is measured as follows.
[0204] The measurement device used is a precision particle size distribution measurement device using the pore electrical resistance method, "Coulter Counter Multisizer 3" (registered trademark, manufactured by Beckman Coulter, Inc.), equipped with a 100 μm aperture tube. The measurement conditions are set and the measurement data is analyzed using the accompanying dedicated software "Beckman Coulter Multisizer 3 Version 3.51" (manufactured by Beckman Coulter, Inc.). The measurement is performed with an effective measurement channel count of 25,000.
[0205] The aqueous electrolyte solution used for the measurement is prepared by dissolving special grade sodium chloride in ion-exchanged water to a concentration of 1% by mass, for example, "ISOTON II" (manufactured by Beckman Coulter).
[0206] Before performing measurements and analysis, the dedicated software is set up as follows.
[0207] In the "Change Standard Measurement Method (SOM)" screen of the dedicated software, set the total count number in the control mode to 50,000 particles, the number of measurements to 1, and the Kd value to the value obtained using "Standard particle 10.0 μm" (Beckman Coulter). Press the "Threshold / Noise level measurement button" to automatically set the threshold and noise level. In addition, set the current to 1600 μA, the gain to 2, the electrolyte to ISOTON II, and check "Flush aperture tube after measurement."
[0208] In the "Pulse to particle size conversion setting" screen of the dedicated software, set the bin interval to logarithmic particle size, the particle size bin to 256 particle size bins, and the particle size range to 2 μm to 60 μm.
[0209] The specific measurement method is as follows. (1) Pour 200 mL of electrolyte solution into a 250 mL round-bottom glass beaker made exclusively for the Multisizer 3, set it on the sample stand, and stir the stirrer rod counterclockwise at 24 revolutions per second. Then, use the "Aperture tube flush" function of the dedicated software to remove dirt and air bubbles from inside the aperture tube. (2) Put 30 mL of the electrolyte solution into a 100 mL flat-bottom glass beaker. Add 0.3 mL of a solution of "Contaminon N" (a 10% aqueous solution of a pH 7 neutral detergent for cleaning precision measuring instruments made from a nonionic surfactant, anionic surfactant, and organic builder, manufactured by Wako Pure Chemical Industries, Ltd.) diluted 3 times with ion-exchanged water as a dispersant. (3) Prepare an ultrasonic disperser "Ultrasonic Dispersion System Tetora150" (manufactured by Nikkaki Bios Co., Ltd.) that has two built-in oscillators with an oscillation frequency of 50 kHz and a phase shift of 180 degrees, and has an electrical output of 120 W. Place 3.3 L of ion-exchanged water in the ultrasonic disperser's water tank, and add 2 mL of Contaminon N to this water tank. (4) Set the beaker (2) in the beaker fixing hole of the ultrasonic disperser, operate the ultrasonic disperser, and adjust the height of the beaker so that the resonance state of the electrolyte solution in the beaker is maximized. (5) While the electrolyte solution in the beaker in (4) is irradiated with ultrasonic waves, 10 mg of toner particles are added little by little to the electrolyte solution and dispersed. Then, ultrasonic dispersion treatment is continued for another 60 seconds. During ultrasonic dispersion, the water temperature in the water tank is appropriately adjusted to be 10°C or higher and 40°C or lower. (6) Using a pipette, the electrolyte solution (5) in which the toner particles are dispersed is dropped into the round-bottom beaker (1) placed in the sample stand, and the measurement concentration is adjusted to 5%. Then, measurements are continued until the number of particles measured reaches 50,000. (7) The measurement data is analyzed using the dedicated software that comes with the device, and the weight-average particle diameter (D4) is calculated. Note that when the dedicated software is set to Graph / Volume%, the "Average diameter" on the "Analysis / Volume Statistics (Arithmetic Mean)" screen is the weight-average particle diameter (D4). EXAMPLES
[0210] The present invention will be specifically described below with reference to examples, but the present invention is not limited to these examples. Example 18 is a reference example. In the examples and comparative examples, the "parts" of each material are all based on mass unless otherwise specified.
[0211] <Production Example of Polyester Resin (a-1)> The polyester resin (a-1) was synthesized according to the following procedure.
[0212] The following materials were charged into an autoclave equipped with a pressure reducing device, a water separating device, a nitrogen gas introducing device, a temperature measuring device, and a stirrer, and a reaction was carried out under a nitrogen atmosphere at normal pressure and 200°C for 5 hours. Bisphenol A-propylene oxide 2.1 mole adduct: 39.6 parts Terephthalic acid: 8.0 parts Isophthalic acid: 7.6 parts Tetrabutoxytitanate: 0.1 parts Thereafter, 0.01 part of trimellitic acid and 0.12 part of tetrabutoxy titanate were added, and the mixture was reacted at 220° C. for 3 hours, and then reacted under reduced pressure of 10 to 20 mmHg for 2 hours to obtain a polyester resin (a-1).
[0213] The resulting polyester resin (a-1) had an acid value of 6.1 and Mw=10,200.
[0214] <Production example of styrene acrylic resin (a-2)> Styrene-acrylic resin (a-2) was synthesized according to the following procedure.
[0215] 100.0 parts of propylene glycol monomethyl ether was heated while replacing with nitrogen, and refluxed at a liquid temperature of 120°C or higher. A mixture of 83.4 parts of styrene, 20.9 parts of butyl acrylate, 1.0 parts of acrylic acid, and 0.6 parts of tert-butyl peroxybenzoate [manufactured by NOF Corp., trade name: Perbutyl Z] as a polymerization initiator was added dropwise over 3 hours. After the dropwise addition was completed, the solution was stirred for 3 hours, and then distilled at normal pressure while raising the liquid temperature to 170°C. After the liquid temperature reached 170°C, the pressure was reduced to 1 hPa, and the solvent was removed by distillation for 1 hour to obtain a resin solid. The resin solid was dissolved in tetrahydrofuran, reprecipitated with n-hexane, and the precipitated solid was filtered to obtain a styrene-acrylic resin (a-2).
[0216] The resulting styrene-acrylic resin (a-2) had an acid value of 10.6 and Mw=13,000.
[0217] <Production Example of Resin A (A-1) Represented by Formula (1)> Resin A (A-1) represented by formula (1) was synthesized according to the following procedure.
[0218] 50.00 parts of polyester resin (a-1) was dissolved in 200.00 parts of N,N-dimethylacetamide, and 1.20 parts of 3-aminopropyltriethoxysilane, 1.70 parts of triethylamine, and 1.70 parts of DMT-MM (4-(4,4-dimethoxy-1,3,5-triazin-2-yl)-4-methylmorpholinium chloride) were added as silane compounds, and the mixture was stirred at room temperature for 5 hours. After the reaction was completed, the solution was dropped into methanol, reprecipitated, and filtered to obtain resin A (A-1) represented by formula (1). The weight average molecular weight Mw of the resin A (A-1) represented by formula (1) obtained was 10400. The physical properties of the resin A (A-1) represented by formula (1) obtained above are shown in Table 2.
[0219] <Production Example of Resin A (A-2) Represented by Formula (1)> Resin A (A-2) represented by formula (1) was obtained in the same manner as in the synthesis of Resin A (A-1) represented by formula (1) above, except that the silane compound was changed as shown in Table 1. The physical properties are shown in Table 2.
[0220] <Production Example of Resin A (A-3) Represented by Formula (1)> The solution of 10.0 parts of resin A (A-1) represented by the formula (1) was dissolved in 90.0 parts of toluene, mixed with 400.0 parts of pure water and stirred, adjusted to pH 4.0 with dilute hydrochloric acid, stirred at room temperature for 10.8 hours, stopped stirring, transferred to a separatory funnel, and extracted the oil phase. The oil phase was concentrated and reprecipitated with methanol to obtain resin A (A-3) represented by the formula (1).
[0221] The obtained resin A (A-3) represented by formula (1) 29 When analyzed by Si-NMR (solid state) measurement, R in formula (1) 1 ~R 3 The physical properties are shown in Table 2.
[0222] <Production Example of Resin A (A-4) Represented by Formula (1)> Resin A (A-4) represented by formula (1) was synthesized according to the following procedure.
[0223] 50.00 parts of polyester resin (a-1) was dissolved in 500.00 parts of chloroform, and 1.30 parts of 3-isocyanatepropyltriethoxysilane and 0.50 parts of titanium (IV) tetraisopropoxide were added under a nitrogen atmosphere and stirred at room temperature for 5 hours. After the reaction was completed, the solution was dropped into methanol, reprecipitated, and filtered to obtain resin A (A-4) represented by formula (1). The physical properties are shown in Table 2.
[0224] <Production Example of Resin A (A-5) Represented by Formula (1)> Resin A (A-5) represented by formula (1) was obtained in the same manner as in the synthesis of Resin A (A-1) represented by formula (1) above, except that polyester resin (a-1) was replaced with styrene acrylic resin (a-2). The physical properties are shown in Table 2.
[0225] <Production Example of Resin A (A-6) Represented by Formula (1)> Resin A (A-6) represented by formula (1) was obtained in which a linking group represented by the following formula (19) or formula (20) was formed by an insertion reaction of an epoxy group in an epoxysilane with an ester bond in a polyester resin (a-1).
[0226] 50.0 parts of the polyester resin (A-2) was dissolved in 100.0 parts of anisole, and 2.90 parts of 5,6-epoxyhexyltrimethoxysilane and 10.00 parts of tetrabutylphosphonium bromide were added under a nitrogen atmosphere and stirred at 140°C for 5 hours. After cooling, the reaction mixture was dissolved in 200 ml of chloroform, dropped into methanol, reprecipitated, and filtered to obtain resin A (A-6). The physical properties are shown in Table 2.
[0227] <Synthesis of Comparative Resin> As a comparative example of resin A, polyester resin (a-1) was used as resin A (A-7).
[0228] [Table 1]
[0229] [Table 2]
[0230] [ka] [The (*) in formula (17) represents P in formula (1) 1 and (**) represents the bonding site to the silicon atom in formula (1).
[0231] [ka] [The (*) in formula (18) represents P in formula (1) 1 and (**) represents the bonding site to the silicon atom in formula (1).
[0232] [ka]
[0233] [ka] [In formulas (19) and (20), (*) represents P in formula (1) 1 and (**) represents the bonding site to the silicon atom in formula (1).
[0234] In Table 2, the silicon concentration indicates the content (mass %) of silicon atoms in the resin A.
[0235] <Production Example of Organosilicon Polymer Particle 1 Represented by Formula (3)> Organosilicon polymer particles 1 represented by formula (3) were synthesized according to the following procedure.
[0236] A container equipped with a stirrer and a nitrogen pipe was placed in a water bath at 25° C., and 800 parts of an aqueous hydrochloric acid solution adjusted to pH 3.0 was prepared. 100 parts of methyltriethoxysilane was added thereto, and the mixture was stirred for 120 minutes to obtain a hydrolyzed solution of methyltriethoxysilane.
[0237] Meanwhile, 1620 parts of water was placed in a vessel equipped with a stirrer and heated to 70°C in a warm bath, after which 1.0 mol / L sodium hydroxide solution was added to adjust the pH to 9.0. The above hydrolysis solution was added thereto over 1 hour, and condensation polymerization was carried out for 1 hour while maintaining the temperature at 70°C. After that, 0.1 mol / L sodium hydroxide solution was gradually added to adjust the pH to 10.5, and condensation polymerization was carried out at 70°C for an additional 3 hours to obtain a dispersion of organosilicon polymer particles 1.
[0238] The resulting dispersion of organosilicon polymer particles 1 was centrifuged to remove coarse particles, and then filtered, washed, and dried to obtain organosilicon polymer particles 1.
[0239] The number average particle size of organosilicon polymer particles 1 was 40 nm. The details of organosilicon polymer particles 1 are shown in Table 3.
[0240] <Production Examples of Organosilicon Polymer Particles 2 and 3 Represented by Formula (3)> Organosilicon polymer particles 2 and 3 were obtained in the same manner as in the preparation example of organosilicon polymer particles 1, except for the changes shown in Table 3 below.
[0241] [Table 3] The abbreviations in the table are as follows. MTES: Methyltriethoxysilane PrTMS: Propyltrimethoxysilane
[0242] The silica particles used were those shown in Table 4 below.
[0243] [Table 4]
[0244] <Production of Toner Particle 1> In a reaction vessel equipped with a stirrer, a thermometer, and a reflux tube, 390.0 parts of ion-exchanged water and 14.0 parts of sodium phosphate (12-hydrate) (manufactured by Rasa Kogyo Co., Ltd.) were added, and the mixture was kept at 65°C for 1.0 hours while being purged with nitrogen. Next, an aqueous calcium chloride solution in which 9.2 parts of calcium chloride (dihydrate) was dissolved in 10.0 parts of ion-exchanged water was added all at once using a TK homomixer (manufactured by Tokushu Kika Kogyo Co., Ltd.) while stirring at 12,000 rpm, to prepare an aqueous medium containing a dispersion stabilizer. Furthermore, hydrochloric acid was added to the aqueous medium to adjust the pH to 6.0, and aqueous medium 1 was obtained.
[0245] On the other hand, the following materials were placed in an attritor (manufactured by Nippon Coke & Engineering Co., Ltd.), and then zirconia particles having a diameter of 1.7 mm were added and dispersed at 220 rpm for 5.0 hours. After that, the zirconia particles were removed to prepare Dispersion 1 in which the colorant was dispersed. Styrene 60.0 parts Colorant (CI Pigment Blue 15:3) 6.5 parts Next, the following materials were added to the prepared dispersion liquid 1. Styrene 15.0 parts ・25.0 parts n-butyl acrylate Resin A (A-1) 4.0 parts Organosilicon polymer particles 1 0.2 parts Divinylbenzene 0.3 parts Wax (Fischer-Tropsch wax, melting point: 78°C) 3.0 parts Wax (ethylene glycol distearate) 10.0 parts The mixture was kept at 65° C. and uniformly dissolved and dispersed using a TK homomixer at 500 rpm to prepare a polymerizable monomer composition 1.
[0246] While maintaining the temperature of the aqueous medium 1 at 72° C. and the rotation speed of the stirring device at 12,000 rpm, the polymerizable monomer composition 1 was charged into the aqueous medium 1, and 9.0 parts of t-butyl peroxypivalate was added as a polymerization initiator. Granulation was continued for 10 minutes while maintaining the stirring speed at 12,000 rpm.
[0247] The stirrer was changed to a stirrer equipped with a propeller stirring blade, and polymerization was carried out for 5.0 hours while stirring at 150 rpm and maintaining the temperature at 72°C, and then the temperature was raised to 85°C and maintained at this temperature for 2.0 hours.
[0248] The reflux tube of the reaction vessel was replaced with a cooling tube, and the slurry was heated to 100° C. to perform distillation for 6 hours to distill off the unreacted polymerizable monomer, thereby obtaining toner particle dispersion liquid 1.
[0249] Hydrochloric acid was added to the obtained toner particle dispersion liquid 1 to adjust the pH to 1.4 or less, and the dispersion stabilizer was dissolved therein. The resulting mixture was filtered, washed, dried, and classified to obtain toner particles 1.
[0250] <Production Examples of Toner Particles 2 to 4 and 6 to 23> Toner particles 2 to 4 and 6 to 23 were obtained in the same manner as in the production example of toner particle 1, except that the resin A represented by formula (1) and the silicon compound-containing particles were changed as shown in Table 5 below.
[0251] The physical properties of the obtained toner particles 2 to 4 and 6 to 23 are shown in Table 5.
[0252] <Production Example of Toner Particle 5> Preparation of binder resin Bisphenol A propylene oxide 2.2 mole adduct 1200 parts Bisphenol A ethylene oxide 2.2 mole adduct 475 parts Terephthalic acid 250 parts Trimellitic anhydride 190 parts Fumaric acid 290 parts Dibutyltin oxide 0.1 parts The mixture was placed in a 4-liter, 4-necked glass flask, equipped with a thermometer, a stirring rod, a condenser, and a nitrogen inlet tube, and placed in a mantle heater. The mixture was reacted at 220° C. for 5 hours under a nitrogen atmosphere to obtain a binder resin. Next, 100.0 parts of the above binder resin Colorant (CI Pigment Blue 15:3) 6.5 parts Resin A (A-1) 4.0 parts Organosilicon polymer particles 1 0.2 parts Wax (Fischer-Tropsch wax, melting point: 78°C) 3.0 parts Wax (ethylene glycol distearate) 10.0 parts The above toner materials were thoroughly premixed in a Henschel mixer, melted and kneaded in a twin-screw extruder, cooled, and then roughly pulverized to a particle size of about 1 to 2 mm using a hammer mill. The mixture was then finely pulverized in an air jet type fine pulverizer. The resulting finely pulverized material was then classified using a multi-division classifier to obtain toner particles 5.
[0253] [Examples 1 to 18 and Comparative Examples 1 to 5] <Production of Toners 1 to 18 and Comparative Toners 19 to 23> For each of 100.0 parts of the obtained toner particles 1 to 23, silica fine particles (hydrophobized with hexamethyldisilazane, number average particle size of primary particles: 8 nm, BET specific surface area: 160 m 2 The mixture was mixed in a Henschel mixer (manufactured by Mitsui Miike Chemical Engineering Co., Ltd.) with 0.8 parts of glycerin (1.0 parts / g).
[0254] After the above-mentioned mixing treatment, the mixture was sieved through a mesh having an opening of 200 μm to obtain toners 1 to 18 and comparative toners 19 to 23. The physical properties of the obtained toners are shown in Table 5.
[0255] [Table 5]
[0256] The performance of each of the obtained toners was evaluated according to the following method.
[0257] <Evaluation of contamination of developing components> After 100 g of the toner was left in an environment of 23° C. / relative humidity 50% for 24 hours, an image was evaluated using an LBP712Ci (Canon) image forming apparatus at a temperature of 23° C. and a relative humidity of 50%.
[0258] An image forming apparatus (LBP712Ci (Canon)) was prepared, the toner was removed from the cyan cartridge, and the toner to be evaluated was filled in place of the cyan cartridge. Evaluation was also performed by mounting a dummy cartridge.
[0259] The process speed was set to 240 mm / s in cyan monochrome mode. 500 copies of the letter "E" (image printing rate 1%) were printed out in intermittent printing mode (2-second pause after every 2 copies).
[0260] The cyan cartridge was removed, and the developing roller was removed. The newly prepared toner and developing roller were then attached to the cyan cartridge from which the developing roller had been removed.
[0261] Next, the image forming apparatus was modified so that an image could be output even if the toner was not loaded.
[0262] This creates a state in which the toner coated on the developing roller is repeatedly rubbed by the developing blade.
[0263] After the toner on the developing member was rubbed with this cartridge for 150 printed sheets, the developing member was removed and air was blown to remove the toner on the developing member. The developing roller was taped and then printed with A4 color laser copier paper (Canon, 80 g / m 2 ) and pasted it.
[0264] The density of this tape was measured at five points, and the average value was used as an index of the degree of contamination of the component. The image density was measured using a "504 Spectrodensitometer" (manufactured by X-Rite Corporation), and the evaluation was performed with the image density without taping of the developing roller set as 0.00. The results are shown in Table 6.
[0265] (Evaluation Criteria) A: The difference in concentration from the standard is less than 0.050 B: The difference in concentration from the standard is 0.050 or more and less than 0.100 C: The difference in concentration from the standard is 0.100 or more and less than 0.200 D: The difference in concentration from the standard is 0.200 or more
[0266] <Low temperature fixability evaluation> After 100 g of the toner was left in an environment of 23° C. / relative humidity 50% for 24 hours, an image was evaluated using an LBP712Ci (Canon) image forming apparatus at a temperature of 23° C. and a relative humidity of 50%.
[0267] An image forming apparatus (LBP712Ci (manufactured by Canon)) was prepared, the toner was removed from the cyan cartridge, and the toner to be evaluated was filled in place of the cyan cartridge.
[0268] Next, the image receiving paper (HP Laser Jet90, manufactured by HP, 90 g / m 2 ) with an unfixed toner image of 2.0 cm length x 15.0 cm width (toner loading: 0.9 mg / cm 2 ) was formed at a position 1.0 cm from the upper end in the paper feed direction.
[0269] Next, the removed fixing unit was modified so that the fixing temperature and process speed could be adjusted, and a fixing test of an unfixed image was carried out using this.
[0270] First, in a normal temperature and humidity environment (23°C / relative humidity 60%), the process speed was set to 300 m / s, and the initial temperature was 120°C, and the set temperature was increased by 2°C each time, and the unfixed image was fixed at each temperature.
[0271] The evaluation criteria for low temperature fixability are as follows.
[0272] The low temperature side fixing start point is the lowest temperature at which the low temperature offset phenomenon (the phenomenon in which part of the toner adheres to the fixing device) is not observed. The results are shown in Table 6.
[0273] (Evaluation Criteria) A: The low temperature side fixing start point is less than 140℃ B: The low-temperature side fixing start point is 140°C or higher and less than 150°C. C: The low temperature side fixing start point is 150℃ or more and less than 160℃ D: The low temperature side fixing start point is 160°C or higher
[0274] <Evaluation of tape peelability> An image forming apparatus (LBP712Ci (manufactured by Canon)) was prepared, the toner was removed from the cyan cartridge, and the toner to be evaluated was filled in place of the cyan cartridge.
[0275] The image forming device used was modified to allow the development bias to be adjusted, and the fixing media used was FOX RIVER BOND paper (110 g / m 2 ) was used.
[0276] The image to be evaluated is a line image. The amount of toner on the image is increased by adjusting the developing bias to set a high image density, and by using thick paper with large surface irregularities, the toner in the recesses of the paper and the lower part of the toner layer is less likely to melt during the fixing process, allowing for strict evaluation of peeling.
[0277] First, the image forming apparatus was left overnight in a low temperature and low humidity environment (15°C, 10% RH). If the evaluation environment is low, the fixing unit does not warm up easily, resulting in a strict evaluation.
[0278] Then, a horizontal line image was printed using FOX RIVER BOND paper with the development bias adjusted so that the line width was 180 μm. After leaving it in a low temperature and low humidity environment for 1 hour, a polypropylene tape (Klebeband 19 mm × 10 mm, manufactured by tesa) was attached to the horizontal line image and slowly peeled off. After peeling, the image was observed visually and under a microscope and evaluated according to the following evaluation criteria. The results are shown in Table 6.
[0279] (Evaluation Criteria) A: No defects B: Slight defects are visible, but not visible to the naked eye. C: Slight defects visible to the naked eye D: There is a visible defect and the line is broken.
[0280] [Table 6]
Claims
1. A toner containing toner particles, the toner particles containing a binder resin, a resin A, and silicon, The resin A has a structure represented by the following formula (1): The toner is characterized in that the silicon-containing particles are at least one selected from the group consisting of silica and organosilicon polymers. 【Chemistry 1】 (In formula (1), P 1 represents a polymer moiety, L 1 represents a divalent linking group having a structure represented by formula (17) or a structure represented by formula (18), R 1 to R 3 each independently represent a hydrogen atom, a halogen atom, an alkyl group, an alkoxy group, an aryl group or a hydroxyl group, m represents a positive integer, and when m is 2 or more, a plurality of L 1 s, a plurality of R 1 s, a plurality of R 2 s and a plurality of R 3 s may be the same or different.) 【Chemistry 2】 [R 5 in formula (17) represents an alkylene group, an arylene group, or an alkylene group containing an --NH-- group. (*) represents the bonding site to P 1 in formula (1), and (**) represents the bonding site to the silicon atom in formula (1)] 【Chemistry 3】 [R 6 in formula (18) represents an alkylene group or an arylene group, (*) represents the bonding site to P 1 in formula (1), and (**) represents the bonding site to the silicon atom in formula (1)]
2. The toner according to claim 1, wherein the content of the resin A in the toner particles is from 0.1% by mass to 10.0% by mass.
3. P in the formula (1) 1 3. The toner according to claim 1, wherein the monomer unit is a polyester moiety.
4. R in the above formula (1) 1 ~R 3 4. The toner according to claim 1, wherein at least one of the groups is an alkoxy group or a hydroxy group.
5. 5. The toner according to claim 1, wherein the silicon-containing particles are present in an amount of 0.040% by mass or more and 0.800% by mass or less based on the toner particles.
6. 6. The toner according to claim 1, wherein the silicon-containing particles are an organosilicon polymer and have a structure represented by the following formula (3): R-SiO 3 / 2 Formula (3) (In formula (3), R is an alkyl group having 1 to 4 carbon atoms.)
7. A method for producing the toner according to any one of claims 1 to 6, comprising the steps of: A toner manufacturing method comprising the steps of: dispersing the resin A, the silicon-containing particles, and a polymerizable monomer composition containing a polymerizable monomer in an aqueous medium; forming particles of the polymerizable monomer composition in the aqueous medium; and polymerizing the polymerizable monomer contained in the particles of the polymerizable monomer composition.
8. A method for producing the toner according to any one of claims 1 to 6, comprising the steps of: A method for producing a toner, comprising the steps of melt-kneading a mixture containing a binder resin, the resin A, and the silicon-containing particles to obtain a melt-kneaded product, and pulverizing the melt-kneaded product to obtain a pulverized product.
Citation Information
Patent Citations
Electrostatic charge image developing toner
JP2006259359A
Electrostatic charge image developing toner, electrostatic charge image developer and image forming apparatus
JP2009042386A
Toner for electrostatic charge image development, electrostatic charge image developer, toner cartridge, process cartridge and image forming apparatus
JP2011203511A
toner
JP2016200815A
Manufacturing method of toner
JP2017044933A