Two-component developer, replenishment developer, and image forming method

The two-component developer with silica fine particles and a resin-coated magnetic carrier, combined with a replenishment system, addresses environmental stability issues, providing stable high-definition images by enhancing charge followability and durability.

JP7566582B2Active Publication Date: 2024-10-15CANON KK
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2020179914
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-10-27
Publication Date
2024-10-15
Estimated Expiration
2040-10-27

AI Technical Summary

Technical Problem

Existing two-component developers face challenges in maintaining stable high-definition images under varying environmental conditions, particularly when transitioning from high temperature and high humidity to room temperature and low humidity, leading to color variations.

Method used

A two-component developer comprising toner with silica fine particles and a magnetic carrier with a resin coating layer containing a (meth)acrylic acid ester compound and phosphorus or sulfur elements, along with a replenishment developer to manage toner concentration, enhances environmental stability and durability.

Benefits of technology

The developer achieves stable high-definition images with reduced color variations across different environmental conditions by improving charge followability and durability, ensuring consistent image quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007566582000010
    Figure 0007566582000010
  • Figure 0007566582000011
    Figure 0007566582000011
  • Figure 0007566582000012
    Figure 0007566582000012
Patent Text Reader

Abstract

To provide a two-component developer that has satisfactory followability to an environmental change and durability, and even in an environment in which the developer is used at high temperature and high humidity and then left to stand and subsequently printing is performed at normal temperature and low humidity, can prevent a variation in hue and stably obtain a high-definition image.SOLUTION: A two-component developer includes toner and magnetic carrier. The toner is a toner having a toner particle, and silica fine particles A present on the surface of the toner particle. The number average particle diameter of primary particles of the silica fine particles A is 80 nm or more and 200 nm or less. After 1800 seconds from when the silica fine particles A are electrified in an environment of a temperature of 23°C and a relative humidity of 50%, the silica fine particles A have a charge attenuation constant α of 0.0005 or more and 0.0100 or less. The magnetic carrier is a magnetic carrier having a magnetic carrier particle having a resin coating layer. The resin coating layer contains a resin including a constitutional unit derived from a (meth)acrylate compound. The resin coating layer contains a phosphorus element or a sulfur element.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention relates to a two-component developer used in an image forming method for visualizing an electrostatic image by electrophotography, a replenishment developer, and an image forming method using the same. [Background technology]

[0002] Conventionally, electrophotographic image forming methods generally involve forming an electrostatic latent image on an electrostatic latent image carrier using various means, and then developing the electrostatic latent image by attaching toner to the electrostatic latent image. In this development, a two-component development method is widely used in which carrier particles called magnetic carriers are mixed with the toner, and the toner is frictionally charged to impart an appropriate amount of positive or negative charge to the toner, and the charge is used as a driving force for development.

[0003] The two-component development method has the advantage that the magnetic carrier can be given functions such as stirring, transporting, and charging the developer, so the division of functions between the magnetic carrier and the toner is clear, and therefore developer performance can be easily controlled.

[0004] On the other hand, in recent years, with the advancement of technology in the field of electrophotography, there has been an increasingly strict demand for not only higher speed and longer life of the device, but also higher definition and stable image quality. In order to meet such demands, there is a demand for higher performance of two-component developers.

[0005] As a magnetic carrier for achieving such a two-component developer, a magnetic carrier has been proposed that provides a two-component developer having a high charge amount, suppressing fluctuations in charge amount due to environmental changes, and excellent durability (see Patent Document 1). This magnetic carrier is characterized by containing phosphorus element in the coating layer of the magnetic carrier particles. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Japanese Patent Application Publication No. 2017-203852 Summary of the Invention [Problem to be solved by the invention]

[0007] The magnetic carrier of Patent Document 1 has improved issues such as durability and adaptability to environmental changes. However, there is an ever-increasing market demand for suppressing color variations during printing and stably obtaining high-resolution images in various environments. The two-component developer using the carrier of Patent Document 1 presents no problems in normal environments, but there is a concern that color variations may occur immediately after printing when subjected to severe environmental changes, such as when the developer is left in a high-temperature, high-humidity environment after use and then printed at room temperature and low humidity. Therefore, there is an urgent need to develop a two-component developer that suppresses color variations during printing and stably obtains high-resolution images in various environments.

[0008] An object of the present invention is to provide a two-component developer that solves these problems. Specifically, the developer has good adaptability to the required charge amount in environmental changes (hereinafter simply referred to as "adaptability to environmental changes") and durability for long-term use (hereinafter simply referred to as "durability"). Furthermore, the present invention is to provide a two-component developer that can suppress color variation and stably obtain high-resolution images even in severe environmental changes, such as when printing is performed at room temperature and low humidity after being left after use at high temperature and high humidity. [Means for solving the problem]

[0009] The present inventors have found that by using a two-component developer as described below, the developer has good adaptability to environmental changes and durability, and that color variations are suppressed even in harsh environments, such as when printing is performed at room temperature and low humidity after being left at high temperature and high humidity after use, and high-resolution images can be stably obtained.

[0010] That is, the present invention provides a two-component developer containing a toner and a magnetic carrier, The toner has toner particles containing a binder resin and silica fine particles A present on the surfaces of the toner particles, The silica fine particles A have a number average particle size of primary particles of 80 nm or more and 200 nm or less, The silica fine particles A have a charge decay constant α of 0.0005 or more and 0.0100 or less after 1800 seconds from being charged in an environment of a temperature of 23°C and a relative humidity of 50%, The magnetic carrier is a magnetic carrier having magnetic carrier particles having a magnetic carrier core and a resin coating layer formed on the surface of the magnetic carrier core, the resin coating layer contains a resin including a structural unit derived from a (meth)acrylic acid ester compound, The resin coating layer relates to a two-component developer characterized in that it contains phosphorus or sulfur.

[0011] The present invention also provides a replenishment developer for use in a two-component development method in which a replenishment developer is replenished to a developing device in response to a decrease in toner concentration of the two-component developer in the developing device, an electrostatic latent image formed on the surface of an electrostatic latent image carrier is developed using the two-component developer in the developing device, and excess magnetic carrier inside the developing device is discharged from the developing device as needed, The replenishment developer is characterized in that the amount of the toner relative to 1 part by mass of the magnetic carrier is 2 parts by mass or more and 50 parts by mass or less, and is the two-component developer according to the present invention.

[0012] The present invention also relates to an image forming method comprising a charging step of charging an electrostatic latent image carrier, an electrostatic latent image forming step of forming an electrostatic latent image on the surface of the electrostatic latent image carrier, a developing step of developing the electrostatic latent image with a two-component developer in a developing device to form a toner image, a transfer step of transferring the toner image to a transfer material with or without an intermediate transfer body, and a fixing step of fixing the transferred toner image to the transfer material, wherein the two-component developer used in the present invention is the two-component developer. [Effects of the Invention]

[0013] The two-component developer of the present invention has good adaptability to environmental changes and durability, and can suppress color fluctuations and stably obtain high-resolution images even in harsh environments, such as when printing is performed at room temperature and low humidity after being left at high temperature and high humidity after use. Furthermore, the effects can be similarly exhibited by the replenishment developer or image forming method of the present invention. [Brief explanation of the drawings]

[0014] [Figure 1] FIG. 1 is a schematic diagram of an image forming apparatus. [Figure 2] FIG. 1 is a schematic diagram of an image forming apparatus. [Figure 3] FIG. 2 is a schematic diagram of a device for measuring the resistivity of a magnetic carrier. DETAILED DESCRIPTION OF THE INVENTION

[0015] In the present invention, unless otherwise specified, the expressions "xx or more and xx or less" and "xx to xx" representing a numerical range mean a numerical range including the lower and upper limits, which are the endpoints. In the present invention, the (meth)acrylic acid ester means an acrylic acid ester and / or a methacrylic acid ester.

[0016] The two-component developer of the present invention is a two-component developer containing a toner and a magnetic carrier, The toner has toner particles containing a binder resin and silica fine particles A present on the surfaces of the toner particles, The silica fine particles A have a number average particle size of primary particles of 80 nm or more and 200 nm or less, The silica fine particles A have a charge decay constant α of 0.0005 or more and 0.0100 or less after 1800 seconds from being charged in an environment of a temperature of 23°C and a relative humidity of 50%, The magnetic carrier is a magnetic carrier having magnetic carrier particles having a magnetic carrier core and a resin coating layer formed on the surface of the magnetic carrier core, the resin coating layer contains a resin including a structural unit derived from a (meth)acrylic acid ester compound, The resin coating layer is characterized by containing phosphorus or sulfur.

[0017] The present inventors have conducted extensive research aimed at achieving a toner that has good adaptability and durability to environmental changes, and that can stably produce high-resolution images with reduced color variation even when subjected to severe environmental changes, such as when printing is performed at room temperature and low humidity after being left in a high-temperature and high-humidity environment after use. As a result, they have found that the combination of the magnetic carrier and toner having the above-mentioned configuration is important.

[0018] The mechanism by which the two-component developer of the present invention can solve the above problems is believed to be as follows. The magnetic carrier particles used in the two-component developer of the present invention have a resin coating layer on their surface that contains structural units derived from a (meth)acrylic acid ester compound, and the coating resin layer contains phosphorus or sulfur. The inclusion of structural units derived from a (meth)acrylic acid ester compound in the resin coating layer improves the hydrophobicity of the magnetic carrier particles, thereby suppressing a decrease in charge amount under high-temperature, high-humidity conditions. Furthermore, a resin coating layer containing such structural units has appropriate chargeability and mechanical strength, resulting in excellent durability. Furthermore, the positive chargeability of phosphorus or sulfur improves the charge-imparting properties of the magnetic carrier. Furthermore, by incorporating silica fine particles with a certain charge relaxation property into the toner particle surface, the silica fine particles themselves appropriately promote the transfer of charge possessed by the toner, resulting in a rapid charge buildup in the two-component developer. Therefore, even when the charge amount decreases due to exposure to high temperature and humidity, and then printing is performed in an environment where the charge amount is likely to increase, such as a room-temperature, low-humidity environment, charge transfer between the phosphorus or sulfur element and the silica fine particles is easily achieved. As a result, it is believed that the two-component developer exhibits good charge buildup, has good adaptability to environmental changes and durability, and can stably produce high-definition images with reduced color variation.

[0019] From the viewpoint of suppressing color variation, it is important that the number-average particle diameter of the primary particles of the silica fine particles A is 80 nm or more and 200 nm or less. If the number-average particle diameter of the primary particles of the silica fine particles A is less than 80 nm, the small number-average particle diameter of the primary particles increases the opportunities for contact between the magnetic carrier and the base part of the toner particles, which may broaden the charge distribution of the two-component developer and make color variation more likely. If the number-average particle diameter of the primary particles is greater than 200 nm, the time for charge migration within the silica fine particles increases, which delays the rise of charge in the two-component developer and makes color variation more likely.

[0020] From the same viewpoint, it is important that the charge decay constant α of the silica fine particles A after 1800 seconds from the charged state in an environment of 23°C temperature and 50% relative humidity is 0.0005 or more and 0.0100 or less. If the charge decay constant α is less than 0.0005, the charge buildup of the two-component developer is delayed, making color variation more likely. If it is greater than 0.0100, the charge amount decreases significantly after being left under high temperature and high humidity, and the difference between the initial charge amount and the saturated charge amount under normal temperature and low humidity during subsequent printing becomes larger, making color variation more likely.

[0021] The silica fine particles A used in the present invention are particles containing silica (i.e., SiO2) as a main component, and can be produced by known production methods such as a combustion method, a melting method, hydrothermal synthesis, etc. Among these, silica fine particles A produced by a combustion method or a melting method are more preferred in order to further enhance the effect of suppressing charge relaxation in a high-temperature, high-humidity environment, and from the viewpoint of high resistance and being less susceptible to the influence of humidity.

[0022] The combustion method is a method in which a siloxane compound is vaporized, and the resulting siloxane gas is introduced into a burner together with a carrier gas such as nitrogen, and the siloxane gas is diffused and mixed with a combustion-supporting gas such as oxygen, and then combusted to produce silica fine particles. Another combustion method is a method in which silicon tetrachloride is combusted at high temperature together with a mixed gas of oxygen, hydrogen, and a diluent gas such as nitrogen, to produce silica fine particles (fumed silica).

[0023] The melting method is a method in which a slurry of metal silicon particles is sprayed into a flame to cause an oxidation reaction and thereby sphericalize the particles, thereby obtaining silica particles.

[0024] In the present invention, from the viewpoint of controllability of the number average particle size of the primary particles of the silica fine particles A, a combustion method in which siloxane gas is burned to produce silica fine particles is cited as a preferred example.

[0025] Examples of the siloxane compound include hexamethylcyclotrisiloxane and octamethylcyclotetrasiloxane.

[0026] In the present invention, the silica fine particles A used in the present invention can be obtained by incorporating iron atoms, and preferably further incorporating aluminum atoms, into the silica fine particles A. The amount of iron atoms contained in the silica fine particles A is preferably 20 ppm or more and 2000 ppm or less, and more preferably 50 ppm or more and 1000 ppm or less, calculated as oxide. When the amount of iron atoms contained in the silica fine particles A is within this range, color variation can be suitably suppressed. As a method for incorporating these metal atoms into the silica fine particles A, it is possible to incorporate them by adjusting the purity of the siloxane compound.

[0027] Furthermore, the silica fine particles A are preferably surface-treated with a silane coupling agent, silicone oil, or the like to be hydrophobic. As the silane coupling agent, one that has been surface-treated with hexamethyldisilazane (HMDS) is more preferred. As the silicone oil, one that has been surface-treated with dimethyl silicone oil is more preferred.

[0028] The method of surface treatment with a silane coupling agent is not particularly limited, and known methods can be used. For example, a common and preferred method is to spray or vaporize the vaporized silane coupling agent onto a cloud of silica fine particles A formed by stirring the particles. The amount of the silane coupling agent used for the surface treatment is preferably in the range of 1 part by weight to 80 parts by weight per 100 parts by weight of the silica fine particles A.

[0029] Furthermore, from the viewpoint of adaptability to environmental changes and durability, it is important that the resin coating layer on the surface of the magnetic carrier core contains a structural unit derived from a (meth)acrylic acid ester compound. When the resin coating layer contains a structural unit derived from a (meth)acrylic acid ester compound, the hydrophobicity of the magnetic carrier particles is improved, and a decrease in the charge amount under high temperature and high humidity conditions is suppressed. Furthermore, since a resin coating layer containing such a structural unit has appropriate chargeability and mechanical strength, the magnetic carrier has excellent durability. From the viewpoint of further improving the adaptability to environmental changes and durability of a two-component developer, the (meth)acrylic acid ester compound is preferably an alicyclic (meth)acrylic acid ester compound. Furthermore, from the viewpoint of improving adaptability to environmental changes and durability, the alicyclic (meth)acrylic acid ester compound preferably has a cycloalkyl group having from 5 to 8 carbon atoms, and particularly preferably an alicyclic cyclohexyl (meth)acrylate having a cycloalkyl group having 6 carbon atoms.

[0030] The resin coating layer may be obtained by copolymerizing an alicyclic (meth)acrylic acid ester compound with another monomer. Examples of the other monomer include (meth)acrylic monomers such as chain or branched (meth)acrylic acid esters and aminoalkyl (meth)acrylate esters, and vinyl monomers such as styrene, vinyl acetate, and vinyl chloride. Among these, it is preferable to contain a (meth)acrylic monomer, and it is more preferable to contain a structural unit derived from a chain (meth)acrylic acid ester compound.

[0031] The content of the structural unit derived from the alicyclic (meth)acrylic acid ester compound in the coating resin layer is preferably 10.0% by mass or more and 90.0% by mass or less, and more preferably 20% by mass or more and 80% by mass or less. Within the above range, the environmental stability and durability of the charge amount of the magnetic carrier are further improved. The content of the structural unit is substantially the same as the content of the alicyclic (meth)acrylic acid ester compound relative to the total amount of monomers when producing the resin.

[0032] From the viewpoint of improving the charge-imparting property of the magnetic carrier, it is important that the resin coating layer contains phosphorus or sulfur, and it is more preferable that the resin coating layer contains phosphorus. The phosphorus may be present in the resin coating layer as part of the resin, or may be present in the resin coating layer as a compound containing phosphorus separately from the resin.

[0033] The phosphorus element is preferably contained in the resin coating layer as a phosphoric acid such as phosphoric acid, phosphorous acid, or phosphinic acid, or an organic phosphorus compound such as a phosphate ester or a phosphite ester, or a component derived therefrom. The phosphorus atom contained in such a component polarizes the phosphorus-oxygen bond (P=O, PO) due to the difference in electronegativity, so the resin coating layer is highly positively charged.

[0034] Among these, from the viewpoint of imparting an appropriate charge to the toner, organic phosphorus compounds are more preferred, and phosphoric acid esters are even more preferred. The phosphoric acid ester may be any of monoesters (P(=O)(OH)2(OR)), diesters (P(=O)(OH)(OR)2), and triesters (P(=O)(OR)3). In the above formula, R each independently represents any monovalent group other than a hydrogen atom and may be the same or different. That is, the magnetic carrier used in the two-component developer of the present invention preferably has a resin coating layer containing phosphorus as a phosphoric acid group (-OP(=O)(OH)2), an acidic phosphoric acid ester group (-OP(=O)(OH)(OR)), or a salt group thereof, or a phosphoric acid ester group (-OP(=O)(OR)2). In the above formula, R each independently represents any monovalent group other than a hydrogen atom and may be the same or different.

[0035] The presence of the above groups in the resin coating layer can be confirmed by using known mass spectrometry means such as TOF-MS or LC-MS.

[0036] The phosphorus content of the resin coating layer is preferably 0.0005 or more and 0.0200 or less, as the ratio (P / C) of the phosphorus content (P) to the carbon content (C), calculated by the measurement method described below. If it is 0.0005 or more, a decrease in the charge amount is suppressed under high temperature and high humidity. On the other hand, if it is 0.0200 or less, excessive charging is suppressed under low temperature and low humidity. Furthermore, from the viewpoint of achieving both environmental stability of the charge amount and durability at a good level, it is more preferably 0.0010 or more and 0.0150 or less, and particularly preferably 0.0010 or more and 0.0100 or less. Note that P / C can be controlled by adjusting the amount of the phosphorus-containing compound used, as described below.

[0037] The method for introducing phosphorus into the resin coating layer is not particularly limited, but a method of adding a compound containing phosphorus during the production of the resin is preferred, such as a method of producing the resin using a compound containing phosphorus as a surfactant or a monomer.

[0038] As one method for introducing phosphorus into the resin coating layer, it is preferable to produce the resin by emulsion polymerization using a surfactant containing phosphorus. The reasons for this preference are believed to be as follows: In resin particles produced by this method, the phosphorus is oriented on the outside of the resin particles. That is, these resin particles have a structure that is hydrophobic inside but easily absorbs moisture on the surface. A magnetic carrier produced using these resin particles can simultaneously reduce moisture adsorption under high-temperature, high-humidity conditions and improve moisture retention under low-temperature, low-humidity conditions. Therefore, while charge reduction under high-temperature, high-humidity conditions is suppressed, excessive charging under low-temperature, low-humidity conditions is also suppressed. It is believed that the magnetic carrier according to the present invention can impart a constant charge to the toner even when the temperature and humidity environment changes.

[0039] In this method, the P / C can be controlled within a desired range by appropriately adjusting the amount of phosphorus-containing surfactant used, the washing conditions for the produced resin, etc. Examples of methods for washing the resin include a method in which the resin is repeatedly filtered and redispersed in ion-exchanged water or an ion-exchanged water / alcohol mixed solvent. Furthermore, the phosphorus-containing surfactant may be added after the resin is produced. The surfactant containing phosphorus is preferably a phosphate surfactant such as an alkyl phosphate ester or a salt thereof, or a polyoxyethylene alkyl ether phosphate ester or a salt thereof. By using such a surfactant, the phosphorus element is localized on the surface of the resin particle, and thus a carrier having excellent charge-imparting properties can be obtained.

[0040] Alkyl phosphate esters are P(=O)(OH) 3-n (OR) nIn the formula, R is an alkyl group having from 4 to 30 carbon atoms, and n is 1 or 2. Specific examples include lauryl phosphate, tridecyl phosphate, myristyl phosphate, stearyl phosphate, oleyl phosphate, etc. These may be used alone or in combination of two or more.

[0041] Polyoxyethylene alkyl ether phosphate ester is [RO(CH2CH2O) m ] n P(=O)(OH) 3-n In the formula, R is an alkyl group having 4 to 30 carbon atoms, n is 1 or 2, and m is 1 to 50. Specific examples include polyoxyethylene tridecyl ether phosphate, polyoxyethylene lauryl ether phosphate, and the like. Of these, polyoxyethylene tridecyl ether phosphate is preferred from the viewpoint of resin productivity. These may be used alone or in combination of two or more.

[0042] The amount of the surfactant containing phosphorus used is preferably 0.1% by mass or more and 1.5% by mass or less, more preferably 0.2% by mass or more and 1.0% by mass or less, and even more preferably 0.3% by mass or more and 0.5% by mass or less, based on the total amount of monomers used to form the resin.

[0043] As one method for introducing phosphorus into the resin coating layer, it is also preferable to produce a resin by copolymerizing a monomer containing phosphorus with the above-mentioned alicyclic (meth)acrylic acid ester compound.

[0044] In this method, the P / C can be controlled within a desired range by appropriately adjusting the copolymerization ratio of the monomer containing phosphorus and the other monomer.

[0045] Examples of the monomer containing phosphorus element include 2-(meth)acryloyloxyethyl acid phosphate, 2-(meth)acryloyloxypropyl acid phosphate, etc. These may be used alone or in combination of two or more.

[0046] Another method for introducing phosphorus into the resin coating layer is to produce the resin using a polymerization initiator containing phosphorus. In this method, the P / C can be controlled within a desired range by appropriately adjusting the amount of the polymerization initiator used.

[0047] <Toner> In the toner of the present invention, a polyester resin is preferably used as a binder resin for toner particles. Examples of the polyester resin include amorphous polyester resin and crystalline polyester resin.

[0048] When a crystalline polyester resin is used, it is preferably used in an amount of 3.0 parts by mass or more and 15.0 parts by mass or less, and more preferably 4.0 parts by mass or more and 12.0 parts by mass or less, per 100.0 parts by mass of the non-crystalline polyester resin.

[0049] In the present invention, the crystalline polyester resin is a resin in which an endothermic peak is observed in differential scanning calorimetry (DSC).

[0050] The crystalline polyester resin can be obtained by the reaction of a divalent or higher polycarboxylic acid with a diol. Among them, a resin obtained by polycondensation of an aliphatic diol with an aliphatic dicarboxylic acid is preferred because it has a high degree of crystallinity. In the present invention, the crystalline polyester resin may be used alone or in combination with multiple types.

[0051] In the present invention, the crystalline polyester resin is preferably a resin obtained by condensation polymerization of an alcohol component containing at least one compound selected from the group consisting of aliphatic diols having from 2 to 22 carbon atoms and derivatives thereof, and a carboxylic acid component containing at least one compound selected from the group consisting of aliphatic dicarboxylic acids having from 2 to 22 carbon atoms and derivatives thereof.

[0052] Among these, the crystalline polyester resin is more preferably a crystalline polyester resin obtained by condensation polymerization of an alcohol component containing at least one compound selected from the group consisting of aliphatic diols having 6 to 12 carbon atoms and their derivatives, and a carboxylic acid component containing at least one compound selected from the group consisting of aliphatic dicarboxylic acids having 6 to 12 carbon atoms and their derivatives, from the viewpoints of low-temperature fixability and blocking resistance, as well as environmental response and durability.

[0053] The aliphatic diol having 2 to 22 carbon atoms (preferably 6 to 12 carbon atoms) is not particularly limited, but may be a chain (preferably linear) aliphatic diol.

[0054] Examples include ethylene glycol, diethylene glycol, triethylene glycol, 1,2-propylene glycol, dipropylene glycol, 1,3-propanediol, 1,4-butanediol, 1,4-butadiene glycol, 1,5-pentanediol, neopentyl glycol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,11-undecanediol, and 1,12-dodecanediol.

[0055] Among these, preferred examples include straight-chain aliphatic α,ω-diols such as 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,11-undecanediol, and 1,12-dodecanediol.

[0056] In the present invention, the derivative is not particularly limited as long as it can be obtained by the above-mentioned condensation polymerization with the same resin structure, for example, a derivative obtained by esterifying the above-mentioned diol.

[0057] In the present invention, in the alcohol component constituting the crystalline polyester resin, at least one compound selected from the group consisting of the aliphatic diols having 2 to 22 carbon atoms (preferably 6 to 12 carbon atoms) and their derivatives preferably accounts for 50% by mass or more, more preferably 70% by mass or more, of the total alcohol component.

[0058] In the present invention, polyhydric alcohols other than the above aliphatic diols can also be used. Among the polyhydric alcohols, examples of diols other than the above-mentioned aliphatic diols include aromatic alcohols such as polyoxyethylenated bisphenol A and polyoxypropylenated bisphenol A; 1,4-cyclohexanedimethanol; and the like. Furthermore, examples of the trivalent or higher polyhydric alcohols among the polyhydric alcohols include aromatic alcohols such as 1,3,5-trihydroxymethylbenzene; and aliphatic alcohols such as pentaerythritol, dipentaerythritol, tripentaerythritol, 1,2,4-butanetriol, 1,2,5-pentanetriol, glycerin, 2-methylpropanetriol, 2-methyl-1,2,4-butanetriol, trimethylolethane, and trimethylolpropane.

[0059] Furthermore, in the present invention, monohydric alcohols may be used to the extent that they do not impair the properties of the crystalline polyester resin. Examples of such monohydric alcohols include n-butanol, isobutanol, sec-butanol, n-hexanol, n-octanol, 2-ethylhexanol, cyclohexanol, and benzyl alcohol.

[0060] On the other hand, the aliphatic dicarboxylic acid having 2 to 22 carbon atoms (preferably 6 to 12 carbon atoms) is not particularly limited, but may be a chain (preferably linear) aliphatic dicarboxylic acid. Examples include oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, glutaconic acid, azelaic acid, sebacic acid, nonanedicarboxylic acid, decanedicarboxylic acid, undecanedicarboxylic acid, dodecanedicarboxylic acid, maleic acid, fumaric acid, mesaconic acid, citraconic acid, and itaconic acid. Also included are those obtained by hydrolyzing the acid anhydrides or lower alkyl esters of these.

[0061] In the present invention, the derivative is not particularly limited as long as it can provide a similar resin structure by the above-mentioned condensation polymerization. Examples thereof include acid anhydrides of the above-mentioned dicarboxylic acid components, and derivatives obtained by methyl esterification, ethyl esterification, or acid chloride of the dicarboxylic acid components.

[0062] In the present invention, in the carboxylic acid component constituting the crystalline polyester resin, at least one compound selected from the group consisting of the aliphatic dicarboxylic acids having 2 to 22 carbon atoms (preferably 6 to 12 carbon atoms) and their derivatives preferably accounts for 50% by mass or more, more preferably 70% by mass or more, of the total carboxylic acid component.

[0063] In the present invention, polycarboxylic acids other than the above-mentioned aliphatic dicarboxylic acids can also be used. Among the polycarboxylic acids, examples of dicarboxylic acids other than the above-mentioned aliphatic dicarboxylic acids include aromatic carboxylic acids such as isophthalic acid and terephthalic acid, aliphatic carboxylic acids such as n-dodecylsuccinic acid and n-dodecenylsuccinic acid, and alicyclic carboxylic acids such as cyclohexanedicarboxylic acid, as well as acid anhydrides or lower alkyl esters thereof.

[0064] Furthermore, among other polycarboxylic acids, examples of trivalent or higher polycarboxylic acids include aromatic carboxylic acids such as 1,2,4-benzenetricarboxylic acid (trimellitic acid), 2,5,7-naphthalenetricarboxylic acid, 1,2,4-naphthalenetricarboxylic acid, and pyromellitic acid, and aliphatic carboxylic acids such as 1,2,4-butanetricarboxylic acid, 1,2,5-hexanetricarboxylic acid, and 1,3-dicarboxyl-2-methyl-2-methylenecarboxypropane, as well as derivatives such as acid anhydrides and lower alkyl esters of these.

[0065] Furthermore, in the present invention, monocarboxylic acids may be used to the extent that they do not impair the properties of the crystalline polyester resin. Examples of such monocarboxylic acids include benzoic acid, naphthalenecarboxylic acid, salicylic acid, 4-methylbenzoic acid, 3-methylbenzoic acid, phenoxyacetic acid, biphenylcarboxylic acid, acetic acid, propionic acid, butyric acid, and octanoic acid.

[0066] In the present invention, the crystalline polyester resin can be produced by a conventional polyester synthesis method, for example, by subjecting the carboxylic acid component and the alcohol component to an esterification reaction or a transesterification reaction, followed by a conventional condensation polymerization reaction under reduced pressure or by introducing nitrogen gas.

[0067] The above esterification or transesterification reaction can be carried out, if necessary, using a conventional esterification catalyst or transesterification catalyst such as sulfuric acid, titanium butoxide, tin 2-ethylhexanoate, dibutyltin oxide, manganese acetate, or magnesium acetate.

[0068] The condensation polymerization reaction can be carried out using a conventional polymerization catalyst, such as titanium butoxide, tin 2-ethylhexanoate, dibutyltin oxide, tin acetate, zinc acetate, tin disulfide, antimony trioxide, germanium dioxide, etc. The polymerization temperature and the amount of catalyst are not particularly limited and may be determined appropriately.

[0069] In the esterification or transesterification reaction, or the polycondensation reaction, a method may be used in which all the monomers are charged at once in order to increase the strength of the resulting crystalline polyester resin, or a method in which a divalent monomer is reacted first and then a trivalent or higher monomer is added and reacted in order to reduce the amount of low molecular weight components.

[0070] The non-crystalline polyester resin can be produced in the same manner as the crystalline polyester resin, according to a conventional polyester synthesis method.

[0071] Monomers used in the production of amorphous polyester resins include polyhydric alcohols (dihydric, trihydric or higher alcohols), polycarboxylic acids (dihydric, trihydric or higher carboxylic acids), and their acid anhydrides or lower alkyl esters.

[0072] Here, when preparing a branched polymer, it is effective to partially crosslink the amorphous polyester resin molecule, and for this purpose, it is preferable to use a polyfunctional compound having a valence of three or more, that is, it is preferable to include, as a monomer, a carboxylic acid having a valence of three or more, an acid anhydride thereof or a lower alkyl ester thereof, and / or an alcohol having a valence of three or more.

[0073] Examples of the polyhydric alcohol and polycarboxylic acid used in the production of the amorphous polyester resin include the following.

[0074] Examples of dihydric alcohols include ethylene glycol, propylene glycol, 1,3-butanediol, 1,4-butanediol, 2,3-butanediol, diethylene glycol, triethylene glycol, 1,5-pentanediol, 1,6-hexanediol, neopentyl glycol, 2-ethyl-1,3-hexanediol, hydrogenated bisphenol A, bisphenols represented by the following formula (A) and derivatives thereof; and diols represented by the following formula (B). [ka] (In formula (A), R is an ethylene or propylene group, x and y are each an integer of 0 or more, and the average value of x+y is 0 or more and 10 or less.) [ka] (In formula (B), R' represents -CH2CH2-, -CH2-CH(CH3)-, or -CH2-C(CH3)2-, x' and y' are integers of 0 or more, and the average value of x'+y' is 0 or more and 10 or less.)

[0075] Examples of dicarboxylic acids include maleic acid, fumaric acid, citraconic acid, itaconic acid, glutaconic acid, phthalic acid, isophthalic acid, terephthalic acid, succinic acid, adipic acid, sebacic acid, azelaic acid, malonic acid, n-dodecenylsuccinic acid, isododecenylsuccinic acid, n-dodecylsuccinic acid, isododecylsuccinic acid, n-octenylsuccinic acid, n-octylsuccinic acid, isooctenylsuccinic acid, and isooctylsuccinic acid. Acid anhydrides and lower alkyl esters of these acids may also be used. Of these, maleic acid, fumaric acid, terephthalic acid, adipic acid, and n-dodecenylsuccinic acid are preferably used.

[0076] Examples of trihydric or higher alcohols include sorbitol, 1,2,3,6-hexanetetrol, 1,4-sorbitan, pentaerythritol, dipentaerythritol, tripentaerythritol, 1,2,4-butanetriol, 1,2,5-pentanetriol, glycerol, 2-methylpropanetriol, 2-methyl-1,2,4-butanetriol, trimethylolethane, trimethylolpropane, and 1,3,5-trihydroxymethylbenzene. Among these, glycerol, trimethylolpropane, and pentaerythritol are preferred examples.

[0077] Examples of trivalent or higher carboxylic acids include 1,2,4-benzenetricarboxylic acid, 2,5,7-naphthalenetricarboxylic acid, 1,2,4-naphthalenetricarboxylic acid, 1,2,4-butanetricarboxylic acid, 1,2,5-hexanetricarboxylic acid, 1,3-dicarboxyl-2-methyl-2-methylenecarboxypropane, 1,2,4-cyclohexanetricarboxylic acid, tetra(methylenecarboxyl)methane, 1,2,7,8-octanetetracarboxylic acid, pyromellitic acid, and empol trimer acid. Acid anhydrides and lower alkyl esters of these acids may also be used. Among these, 1,2,4-benzenetricarboxylic acid (trimellitic acid) or a derivative thereof is preferably used because it is inexpensive and the reaction can be easily controlled.

[0078] The dihydric alcohols and trihydric or higher alcohols can be used alone or in combination of two or more. Similarly, the dicarboxylic acids and trihydric or higher carboxylic acids can be used alone or in combination of two or more.

[0079] In the present invention, in terms of the molecular weight distribution of the tetrahydrofuran (THF)-soluble portion of the amorphous polyester resin measured by gel permeation chromatography (GPC), it is preferable that the peak molecular weight is from 4,000 to 13,000 from the viewpoints of environmental adaptability and durability. Furthermore, satisfying the above range is also preferable from the viewpoints of low-temperature fixability and hot offset resistance.

[0080] The acid value of the amorphous polyester resin is preferably 2 mgKOH / g or more and 30 mgKOH / g or less from the viewpoint of chargeability in a high-temperature, high-humidity environment.

[0081] Furthermore, the hydroxyl value of the amorphous polyester resin is preferably 2 mgKOH / g or more and 20 mgKOH / g or less from the viewpoint of low-temperature fixability and blocking resistance. In the present invention, the amorphous polyester resin preferably contains a low molecular weight amorphous polyester resin having a peak molecular weight of 4,500 or more and 7,000 or less, and a high molecular weight amorphous polyester resin having a peak molecular weight of 8,500 or more and 9,500 or less.

[0082] In this case, it is preferable that the mixing ratio (B / C) of the high molecular weight amorphous polyester resin to the low molecular weight amorphous polyester resin be 10 / 90 or more and 60 / 40 or less by mass, not only from the viewpoints of environmental change tracking ability and durability, but also from the viewpoints of low temperature fixability and hot offset resistance.

[0083] The peak molecular weight of the high-molecular-weight amorphous polyester resin is preferably from 8500 to 9500, not only from the viewpoint of environmental response and durability, but also from the viewpoint of hot offset resistance. The acid value of the high-molecular-weight amorphous polyester resin is preferably from 10 mgKOH / g to 30 mgKOH / g, not from the viewpoint of chargeability in a high-temperature, high-humidity environment.

[0084] The low-molecular-weight amorphous polyester resin preferably has a peak molecular weight of 4500 to 7000, both in terms of low-temperature fixability, durability, and environmental response. The low-molecular-weight amorphous polyester resin preferably has an acid value of 10 mgKOH / g or less, both in terms of chargeability in a high-temperature, high-humidity environment.

[0085] The acid value is the number of milligrams of potassium hydroxide required to neutralize the acid contained in 1 g of sample. The acid value of resins is measured in accordance with JIS K0070-1992. The hydroxyl value is the number of milligrams of potassium hydroxide required to neutralize the acetic acid bonded to the hydroxyl groups when 1 g of sample is acetylated. The hydroxyl value of amorphous polyesters is measured in accordance with JIS K0070-1992.

[0086] In the present invention, the toner particles may contain wax. Examples of the wax include the following.

[0087] Hydrocarbon waxes such as low molecular weight polyethylene, low molecular weight polypropylene, alkylene copolymers, microcrystalline wax, paraffin wax, and Fischer-Tropsch wax; oxides of hydrocarbon waxes such as oxidized polyethylene wax or their block copolymers; waxes whose main component is fatty acid esters such as carnauba wax; partially or completely deoxidized fatty acid esters such as deoxidized carnauba wax.

[0088] Further examples include saturated straight-chain fatty acids such as palmitic acid, stearic acid, and montanic acid; unsaturated fatty acids such as brassidic acid, eleostearic acid, and valinaric acid; saturated alcohols such as stearyl alcohol, aralkyl alcohol, behenyl alcohol, carnaubyl alcohol, ceryl alcohol, and melissyl alcohol; polyhydric alcohols such as sorbitol; esters of fatty acids such as palmitic acid, stearic acid, behenic acid, and montanic acid with alcohols such as stearyl alcohol, aralkyl alcohol, behenyl alcohol, carnaubyl alcohol, ceryl alcohol, and melissyl alcohol; fatty acid amides such as linoleic acid amide, oleic acid amide, and lauric acid amide; methylene bisstearic acid amide, ethylene biscapric acid amide, ethylene bislauric acid amide, and hexyl alcohol. Saturated fatty acid bisamides such as methylene bisstearamide; unsaturated fatty acid amides such as ethylene bisoleamide, hexamethylene bisoleamide, N,N-dioleyl adipamide, and N,N-dioleyl sebacamide; aromatic bisamides such as m-xylene bisstearamide and N,N-distearyl isophthalamide; fatty metal salts (commonly known as metal soaps) such as calcium stearate, calcium laurate, zinc stearate, and magnesium stearate; waxes grafted onto aliphatic hydrocarbon waxes using vinyl monomers such as styrene and acrylic acid; partial esters of fatty acids and polyhydric alcohols such as behenic acid monoglyceride; and methyl ester compounds having hydroxy groups obtained by hydrogenating vegetable oils and fats.

[0089] Among these waxes, hydrocarbon waxes such as low-molecular-weight polypropylene, paraffin wax, and Fischer-Tropsch wax, or fatty acid ester waxes such as carnauba wax are preferred from the viewpoint of improving low-temperature fixability and hot offset resistance. In the present invention, hydrocarbon waxes are more preferred from the viewpoint of further improving hot offset resistance.

[0090] In the present invention, the content of the wax is preferably 1.0 parts by mass or more and 20.0 parts by mass or less, and more preferably 3.0 parts by mass or more and 15.0 parts by mass or less, relative to 100.0 parts by mass of the binder resin.

[0091] Furthermore, the peak temperature of the wax's maximum endothermic peak measured using a differential scanning calorimeter (DSC) is preferably 45° C. or higher and 140° C. or lower, and more preferably 70° C. or higher and 100° C. or lower. If the peak temperature of the wax's maximum endothermic peak is within the above range, it is more preferable from the viewpoint of achieving both blocking resistance and hot offset resistance of the toner.

[0092] In the present invention, the toner particles may contain a colorant. Examples of the colorant that can be used include the following.

[0093] Examples of colorants for black toner include carbon black, and those toned to black using a yellow colorant, a magenta colorant, and a cyan colorant. As the colorant, a pigment may be used alone, but it is more preferable to use a dye and a pigment in combination to improve the clarity from the viewpoint of the image quality of full-color images.

[0094] Examples of pigments for magenta toner include CI Pigment Red 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 21, 22, 23, 30, 31, 32, 37, 38, 39, 40, 41, 48:2, 48:3, 48:4, 49, 50, 51, 52, 53, 54, 55, 57:1, 58, 60, 63, 64, 68, 81:1, 83, 87, 88, 89, 90, 112, 114, 122, 123, 146, 147, 150, 163, 184, 202, 206, 207, 209, 238, 269, 282; CI Pigment Violet 19; CI Bat Red 1, 2, 10, 13, 15, 23, 29, 35.

[0095] Dyes for magenta toner include solvent dyes such as CI Solvent Red 1, 3, 8, 23, 24, 25, 27, 30, 49, 81, 82, 83, 84, 100, 109, and 121; CI Disperse Red 9; CI Solvent Violet 8, 13, 14, 21, and 27; and CI Disperse Violet 1; and basic dyes such as CI Basic Red 1, 2, 9, 12, 13, 14, 15, 17, 18, 22, 23, 24, 27, 29, 32, 34, 35, 36, 37, 38, 39, and 40; and CI Basic Violet 1, 3, 7, 10, 14, 15, 21, 25, 26, 27, and 28.

[0096] Examples of pigments for cyan toner include CI Pigment Blue 2, 3, 15:2, 15:3, 15:4, 16, and 17; CI Vat Blue 6; and CI Acid Blue 45, and copper phthalocyanine pigments in which 1 to 5 phthalimidomethyl groups are substituted on the phthalocyanine skeleton. An example of a dye for cyan toner is CI Solvent Blue 70.

[0097] Yellow toner pigments include the following: CI Pigment Yellow 1, 2, 3, 4, 5, 6, 7, 10, 11, 12, 13, 14, 15, 16, 17, 23, 62, 65, 73, 74, 83, 93, 94, 95, 97, 109, 110, 111, 120, 127, 128, 129, 147, 151, 154, 155, 168, 174, 175, 176, 180, 181, 185; CI Vat Yellow 1, 3, 20. An example of a yellow toner dye is CI Solvent Yellow 162.

[0098] The content of the colorant is preferably 0.1 parts by mass or more and 30.0 parts by mass or less with respect to 100.0 parts by mass of the binder resin.

[0099] In the present invention, the toner particles may contain a charge control agent, if necessary. Although known charge control agents can be used as the charge control agent, metal compounds of aromatic carboxylic acids are particularly preferred because they are colorless, can charge toner quickly, and can stably maintain a constant charge amount.

[0100] Examples of negative charge control agents include metal salicylate compounds, metal naphthoate compounds, metal dicarboxylate compounds, polymeric compounds having sulfonic acid or carboxylic acid on the side chain, polymeric compounds having sulfonate salts or sulfonate esters on the side chain, polymeric compounds having carboxylate salts or carboxylate esters on the side chain, boron compounds, urea compounds, silicon compounds, and calixarenes.

[0101] Examples of the positive charge control agent include quaternary ammonium salts, polymeric compounds having the quaternary ammonium salts in the side chains, guanidine compounds, and imidazole compounds.

[0102] The charge control agent may be added internally or externally to the toner particles. The content of the charge control agent is preferably 0 parts by mass or more and 0.1 parts by mass or less with respect to 100.0 parts by mass of the binder resin.

[0103] The toner of the present invention may contain inorganic fine particles other than the silica fine particles A, if necessary. The inorganic fine particles may be added internally to the toner particles, or may be mixed with the toner particles as an external additive. When contained as an external additive, inorganic fine particles such as silica fine particles, titanium oxide fine particles, and aluminum oxide fine particles are preferred. The inorganic fine particles are preferably hydrophobized with a hydrophobizing agent such as a silane compound, silicone oil, or a mixture thereof.

[0104] When the inorganic fine particles are used to improve the fluidity of the toner, the specific surface area is 50 m 2 / g or more 400m 2 / g or less is preferable. On the other hand, when the inorganic fine particles are used to improve the durability of the toner, the specific surface area is 10 m 2 / g or more 50m 2 / g or less is preferable. In order to simultaneously improve the fluidity and durability, inorganic fine particles having a specific surface area within the above range may be used in combination.

[0105] When the inorganic fine particles are contained as an external additive, the amount thereof is preferably 0.1 parts by mass or more and 10.0 parts by mass or less relative to 100.0 parts by mass of toner particles. The toner particles and the inorganic fine particles may be mixed using a known mixer such as a Henschel mixer.

[0106] In the present invention, the method for producing the toner particles is not particularly limited, but it is preferable to use a melt-kneading method or an emulsion aggregation method, and it is more preferable to use a melt-kneading method. Here, the melt-kneading method is a method for producing toner particles that includes a process of melting and kneading a mixture containing a binder resin, a colorant, etc. to obtain a melt-kneaded product (hereinafter also simply referred to as the "melt-kneading process").

[0107] The procedure for producing toner particles using the melt-kneading method will be described below. First, in the raw material mixing step, predetermined amounts of polyester resin, colorant, etc. are weighed and blended as toner raw materials, and then mixed. Examples of the equipment used for the mixing include a Henschel mixer (manufactured by Nippon Coke Company); a Super Mixer (manufactured by Kawata Corporation); a Ribocone (manufactured by Okawara Manufacturing Co., Ltd.); a Nauta mixer, a Turbulizer, and a Cyclomix (manufactured by Hosokawa Micron Corporation); a Spiral Pin Mixer (manufactured by Pacific Machinery Works Co., Ltd.); and a Loedige mixer (manufactured by Matsubo Corporation). Next, the resulting mixture is melted and kneaded to melt the resins and disperse the colorant and other ingredients therein (melt-kneading step). Examples of the equipment used in the melt-kneading step include a TEM extruder (manufactured by Toshiba Machine Co., Ltd.), a TEX twin-screw kneader (manufactured by The Japan Steel Works, Ltd.), a PCM kneader (manufactured by Ikegai Iron Works Co., Ltd.), and a Kneedex (manufactured by Mitsui Mining Co., Ltd.) Continuous kneaders such as single-screw or twin-screw extruders are preferred over batch kneaders because of their advantages such as the ability to perform continuous production.

[0108] Next, the resulting molten kneaded product is rolled using a two-roll mill or the like, and cooled with water or the like. The cooled material is then crushed to a desired particle size by first coarsely crushing it using a crusher, hammer mill, or feather mill, and then finely crushing it using a Kryptron System (Kawasaki Heavy Industries, Ltd.) or a Super Rotor (Nisshin Engineering, Inc.) to obtain resin particles. The resulting resin particles may be classified to a desired particle size to produce toner particles. Apparatuses used for classification include Turboplex, Faculty, TSP, and TTSP (manufactured by Hosokawa Micron Corporation); Elbow Jet (manufactured by Nittetsu Mining Co., Ltd.), and the like. The weight average particle diameter of the obtained toner particles is preferably 3.0 μm or more and 8.0 μm or less, since the effect of the external additive according to the present invention can be fully obtained. Furthermore, the circularity of the toner particles may be increased by subjecting the toner particles to a treatment such as applying a mechanical impact force. In order to increase the opportunity for charge transfer and friction between toner particles and to increase the charge rise speed, the average circularity is preferably 0.946 or more and 0.972 or less.

[0109] <Magnetic carrier> Next, the magnetic carrier used in the present invention will be described. As the magnetic carrier core used in the magnetic carrier of the present invention, known magnetic carrier cores can be used. It is more preferable to use magnetic material-dispersed resin particles in which a magnetic material is dispersed in a resin component, or porous magnetic core particles containing a resin in the voids. These can reduce the true density of the magnetic carrier, thereby reducing the load on the toner. This reduces image quality degradation even over long periods of use, and reduces the frequency of replacing the developer composed of toner and carrier. However, the present invention is not limited to the above, and the effects of the present invention can be fully achieved even when a commercially available magnetic carrier core is used.

[0110] The magnetic material component used in the magnetic material-dispersed resin particles may be any of various magnetic iron compound particles, such as magnetite particles, maghemite particles, or magnetic iron oxide particles containing at least one selected from silicon oxide, silicon hydroxide, aluminum oxide, and aluminum hydroxide; magnetoplumbite ferrite particles containing barium, strontium, or barium-strontium; and spinel ferrite particles containing at least one selected from manganese, nickel, zinc, lithium, and magnesium. Among these, magnetic iron oxide particles are preferably used.

[0111] In addition to the magnetic material component, non-magnetic inorganic compound particles such as non-magnetic iron oxide particles such as hematite particles, non-magnetic ferric oxide hydrous particles such as goethite particles, titanium oxide particles, silica particles, talc particles, alumina particles, barium sulfate particles, barium carbonate particles, cadmium yellow particles, calcium carbonate particles, and zinc oxide particles may be used in combination with the magnetic iron compound particles. When the magnetic iron compound particles and the non-magnetic inorganic compound particles are mixed and used, the mixing ratio of these is preferably such that the magnetic iron compound particles account for at least 30 mass %. The magnetic iron compound particles are preferably wholly or partly treated with a lipophilic treatment agent. The lipophilic treatment agent used in this case may be an organic compound having one or more functional groups selected from the group consisting of an epoxy group, an amino group, a mercapto group, an organic acid group, an ester group, a ketone group, a halogenated alkyl group, and an aldehyde group, or a mixture thereof.

[0112] The organic compound having a functional group is preferably a coupling agent, more preferably a silane coupling agent, a titanium coupling agent, or an aluminum coupling agent, and particularly preferably a silane coupling agent.

[0113] The binder resin constituting the magnetic material dispersed resin particles is preferably a thermosetting resin. For example, phenol resin, epoxy resin, unsaturated polyester resin, etc. are available, but phenol resin is preferred because it is inexpensive and easy to manufacture, such as phenol-formaldehyde resin.

[0114] The content ratio of the binder resin and the magnetic iron compound particles (or a mixture of the magnetic iron compound particles and the non-magnetic inorganic compound particles) constituting the composite particles of the present invention is preferably 1% by mass or more and 20% by mass or less of the binder resin and 80% by mass or more and 99% by mass or less of the magnetic iron compound particles (or the mixture).

[0115] Next, a method for producing the magnetic material-dispersed resin particles will be described. As described in the Examples below, for example, composite particles can be produced by stirring phenols and aldehydes in an aqueous medium in the presence of magnetic or non-magnetic inorganic compound particles and a basic catalyst, followed by reacting and curing the phenols and aldehydes to produce composite particles containing inorganic compound particles such as magnetic iron oxide particles and a phenolic resin.

[0116] Alternatively, the magnetic carrier can be produced by a so-called kneading and grinding method in which a binder resin containing inorganic compound particles such as magnetic iron oxide particles is ground. The former method is preferred in order to easily control the particle size of the magnetic carrier and to obtain a sharp particle size distribution.

[0117] Next, the porous magnetic core particles will be described. The material of the porous magnetic core particles is preferably magnetite or ferrite, and more preferably ferrite, since this allows the porous structure of the porous magnetic core particles to be controlled and the resistance to be adjusted. The porous magnetic core particles used in the present invention preferably have a peak pore size in the pore size distribution range of 0.1 μm to 3.0 μm of 0.40 μm to 1.00 μm from the viewpoint of environmental response and durability. Similarly, the pore volume, which is the integral value of the differential pore volume in the range of 0.1 μm to 3.0 μm in the pore size distribution, is 58 mm 3 / g or more 100mm 3 / g or less is preferable from the viewpoint of adaptability to environmental changes and durability.

[0118] Ferrite is a sintered body represented by the following general formula: (M12O) x (M2O) y (Fe2O3) z (In the formula, M1 is a monovalent metal, M2 is a divalent metal, and when x + y + z = 1.0, x and y are each 0≦(x, y)≦0.8, and z is 0.2 <z<1.0である。) In the formula, M1 and M2 preferably use at least one metal atom selected from the group consisting of Li, Fe, Mn, Mg, Sr, Cu, Zn, and Ca. In addition, Ni, Co, Ba, Y, V, Bi, In, Ta, Zr, B, Mo, Na, Sn, Ti, Cr, Al, Si, and rare earth elements can also be used.

[0119] In the case of magnetic carriers, it is preferable to control the surface roughness of the porous magnetic core particles to maintain an appropriate level of magnetization and to set the pore diameter within a desired range. It is also preferable to be able to easily control the rate of the ferritization reaction and to suitably control the resistivity and magnetic force of the porous magnetic core particles. From these viewpoints, Mn-based ferrites, Mn-Mg-based ferrites, Mn-Mg-Sr-based ferrites, and Li-Mn-based ferrites containing Mn element are more preferable.

[0120] The manufacturing process when porous ferrite particles are used as the magnetic carrier core will be described in detail below. <Process 1 (weighing and mixing process)> The raw materials for the ferrite are weighed and mixed. Examples of ferrite raw materials include metal particles of the above metal elements, or oxides, hydroxides, oxalates, carbonates, and the like thereof. Examples of mixing devices include a ball mill, a planetary mill, a Giotto mill, and a vibration mill, with a ball mill being particularly preferred from the viewpoint of mixability. Specifically, the weighed ferrite raw material and balls are placed in a ball mill, and the mixture is pulverized and mixed, preferably for 0.1 to 20.0 hours.

[0121] <Step 2 (pre-firing step)> The crushed and mixed ferrite raw material is calcined in air or a nitrogen atmosphere, preferably at a calcination temperature of 700°C to 1200°C for preferably 0.5 to 5.0 hours to form ferrite. For calcination, the following furnaces are used, for example: burner-type incinerator, rotary-type calciner, electric furnace, etc.

[0122] <Process 3 (Crushing process)> The calcined ferrite produced in step 2 is pulverized in a pulverizer. The pulverizer is not particularly limited as long as it can produce the desired particle size, and examples thereof include a crusher, hammer mill, ball mill, bead mill, planetary mill, and Giotto mill. In order to obtain a pulverized ferrite product with a desired particle size, it is preferable to control, for example, the material, particle size, and operating time of the balls and beads used in a ball mill or a bead mill. Specifically, to reduce the particle size of the calcined ferrite slurry, balls with a heavy specific gravity can be used or the milling time can be extended. Furthermore, to widen the particle size distribution of the calcined ferrite, balls or beads with a heavy specific gravity can be used and the milling time can be shortened. Furthermore, calcined ferrite with a wide particle size distribution can also be obtained by mixing multiple calcined ferrites with different particle sizes. In addition, when using a ball mill or bead mill, the wet method is more preferable than the dry method because the crushed product does not fly up inside the mill and crushing efficiency is higher.

[0123] <Process 4 (granulation process)> To the pulverized calcined ferrite, water, a binder, and, if necessary, a pore adjuster, such as a foaming agent or resin particles, are added. Examples of foaming agents include sodium hydrogen carbonate, potassium hydrogen carbonate, lithium hydrogen carbonate, ammonium hydrogen carbonate, sodium carbonate, potassium carbonate, lithium carbonate, and ammonium carbonate. Examples of resin microparticles include polyester, polystyrene, styrene copolymers such as styrene-vinyltoluene copolymer, styrene-vinylnaphthalene copolymer, styrene-acrylic acid ester copolymer, styrene-methacrylic acid ester copolymer, styrene-α-chloromethyl methacrylate copolymer, styrene-acrylonitrile copolymer, styrene-vinyl methyl ketone copolymer, styrene-butadiene copolymer, styrene-isoprene copolymer, and styrene-acrylonitrile-indene copolymer; polyvinyl chloride, phenolic resin, modified phenolic resin, maleic resin, acrylic resin, methacrylic resin, polyvinyl acetate, and silicone resin; polyester resin having, as a structural unit, a monomer selected from aliphatic polyhydric alcohols, aliphatic dicarboxylic acids, aromatic dicarboxylic acids, aromatic dialcohols, and diphenols; polyurethane resin, polyamide resin, polyvinyl butyral, terpene resin, coumarone-indene resin, petroleum resin, and hybrid resin having a polyester unit and a vinyl polymer unit. As the binder, for example, polyvinyl alcohol is used.

[0124] In step 3, when wet pulverization is performed, it is preferable to add a binder and, if necessary, a pore adjuster, taking into consideration the water contained in the ferrite slurry. The obtained ferrite slurry is dried and granulated using a spray dryer, preferably in a heated atmosphere at 100° C. to 200° C. The spray dryer is not particularly limited as long as it can obtain the desired particle size of the porous magnetic core particles. For example, a spray dryer can be used.

[0125] <Step 5 (baking step)> Next, the granulated product is fired preferably at a temperature of 800° C. or higher and 1400° C. or lower, preferably for 1 hour or higher and 24 hours or lower. By increasing the firing temperature and lengthening the firing time, the firing of the porous magnetic core particles progresses, resulting in a smaller pore size and a reduced number of pores.

[0126] <Process 6 (Sorting Process)> After the calcined particles are crushed as described above, they may be classified or sieved to remove coarse particles and fine particles, if necessary. From the viewpoint of suppressing carrier adhesion to images and roughness, the volume distribution based 50% particle size (D50) of the magnetic core particles is preferably 18.0 μm or more and 68.0 μm or less.

[0127] <Process 7 (filling process)> The physical strength of porous magnetic core particles may be reduced depending on the internal pore volume, and therefore, in order to increase the physical strength as a magnetic carrier, it is preferable to fill at least a portion of the voids of the porous magnetic core particles with a resin. The amount of resin filled in the porous magnetic core particles is preferably 2% by mass or more and 15% by mass or less of the porous magnetic core particles. As long as there is little variation in the resin content of each magnetic carrier, it is acceptable for the resin to fill only a portion of the internal voids, for the resin to fill only the voids near the surface of the porous magnetic core particle and leave voids inside, or for the internal voids to be completely filled with resin.

[0128] The method for filling the voids of the porous magnetic core particles with a resin is not particularly limited, but examples thereof include a method in which the porous magnetic core particles are impregnated with a resin solution by a coating method such as a dipping method, a spraying method, a brush coating method, or a fluidized bed coating method, and then the solvent is evaporated. Alternatively, a method in which the resin is diluted in a solvent and then added to the voids of the porous magnetic core particles can be used. The solvent used here may be any solvent that can dissolve the resin. In the case of a resin that is soluble in an organic solvent, examples of the organic solvent include toluene, xylene, cellosolve butyl acetate, methyl ethyl ketone, methyl isobutyl ketone, and methanol. In the case of a water-soluble resin or an emulsion-type resin, water may be used as the solvent. The amount of resin solids in the resin solution is preferably 1% by mass or more and 50% by mass or less, more preferably 1% by mass or more and 30% by mass or less. If it is 50% by mass or less, the viscosity is not too high and the resin solution easily penetrates uniformly into the voids of the porous magnetic core particles. On the other hand, if it is 1% by mass or more, the amount of resin is appropriate, and the adhesion of the resin to the porous magnetic core particles is good.

[0129] The resin to be filled into the voids of the porous magnetic core particles may be either a thermoplastic resin or a thermosetting resin. It is preferable that the resin has a high affinity for the porous magnetic core particles. When a resin with a high affinity is used, the surface of the porous magnetic core particles can be covered with the resin at the same time as the resin is filled into the voids of the porous magnetic core particles.

[0130] Examples of the resin to be filled include the following thermoplastic resins: novolac resin, saturated alkyl polyester resin, polyarylate, polyamide resin, and acrylic resin. Examples of the thermosetting resin include phenolic resins, epoxy resins, unsaturated polyester resins, and silicone resins.

[0131] The method for coating the surfaces of the magnetic carrier core particles with a resin is not particularly limited, but examples thereof include coating methods such as dipping, spraying, brushing, dry coating, and fluidized bed coating. Furthermore, the resin coating layer may contain conductive particles or particles or materials with charge control properties. Examples of conductive particles include carbon black, magnetite, graphite, zinc oxide, and tin oxide. The amount of conductive particles added is preferably 0.1 parts by mass or more and 10.0 parts by mass or less relative to 100 parts by mass of the coating resin in order to adjust the resistance of the magnetic carrier. Examples of particles having charge control properties include organic metal complex particles, organic metal salt particles, chelate compound particles, monoazo metal complex particles, acetylacetone metal complex particles, hydroxycarboxylic acid metal complex particles, polycarboxylic acid metal complex particles, polyol metal complex particles, polymethyl methacrylate resin particles, polystyrene resin particles, melamine resin particles, phenolic resin particles, nylon resin particles, silica particles, titanium oxide particles, and alumina particles. The amount of particles having charge control properties added is preferably 0.5 parts by mass or more and 50.0 parts by mass or less per 100 parts by mass of the coating resin in order to adjust the amount of triboelectric charge. The content of the resin coating layer present on the magnetic carrier surface is preferably 1.0 to 3.0 parts by mass per 100 parts by mass of the magnetic carrier core. When the content is 1.0 part by mass or more, the toughness and abrasion resistance of the resin are increased, and changes in image density are suppressed. On the other hand, when the content is 3.0 parts by mass or less, the charging relaxation is further increased, and density unevenness within the image surface and deterioration of fine line reproducibility are further suppressed.

[0132] The magnetic carrier preferably has a current value of 10.0 μA or more and 100.0 μA or less when 500 V is applied. A current value of 10.0 μA or more further suppresses uneven density within the image surface and deterioration of character quality. On the other hand, a current value of 100.0 μA or less can suppress so-called "fogging," in which insufficiently charged toner transfers to non-image areas. The magnetic carrier has a specific resistance of 1.0 x 10 at an electric field strength of 2000 V / cm. 5 Ω cm or more 1.0×10 10 It is preferable that the resistivity is 1.0×10 Ω·cm or less. 5 At Ω·cm or higher, "fogging" is suppressed and the resistivity is 1.0×10 10 At Ω·cm or less, uneven density within the image and deterioration of character quality are further suppressed.

[0133] When the toner of the present invention is mixed with a magnetic carrier to be used as a two-component developer, good results are usually obtained when the carrier mixing ratio is 2% by mass to 15% by mass, preferably 4% by mass to 13% by mass, in terms of toner concentration in the developer. If the toner concentration is less than 2% by mass, the image density tends to decrease, and if it exceeds 15% by mass, fogging and scattering in the machine tend to occur.

[0134] In addition, in the case of a replenishment developer to be replenished to a developing device in response to a decrease in the toner concentration of the two-component developer in the developing device, the amount of toner is 2 parts by mass or more and 50 parts by mass or less per 1 part by mass of the replenishment magnetic carrier. The replenishment developer is a developer that is replenished to a developing device in response to a decrease in the toner concentration of the two-component developer in the developing device, and is intended for use in a two-component development method in which an electrostatic latent image formed on the surface of an electrostatic latent image carrier is developed using the two-component developer in the developing device, and excess magnetic carrier inside the developing device is discharged from the developing device as needed.

[0135] Next, an image forming apparatus equipped with a developing device that uses a two-component developer and a replenishment developer will be described as an example, but the present invention is not limited to this.

[0136] <Image forming method> In Figure 1, electrostatic latent image carrier 1 rotates in the direction of the arrow in the figure. Electrostatic latent image carrier 1 is charged by charger 2, which is a charging means (charging step), and the surface of the charged electrostatic latent image carrier 1 is exposed by exposure device 3, which is an electrostatic latent image forming means, to form an electrostatic latent image (electrostatic latent image forming step). Developing device 4 has a developer container 5 that contains a two-component developer, and developer carrier 6 is rotatably arranged, and developer carrier 6 contains magnet 7 as a magnetic field generating means. At least one of the magnets 7 is positioned so as to face electrostatic latent image carrier 1.

[0137] The two-component developer is held on the developer carrier 6 by the magnetic field of the magnet 7, and the amount of the two-component developer is regulated by a regulating member 8 before being transported to the development section facing the electrostatic latent image carrier 1. In the development section, a magnetic brush is formed by the magnetic field generated by the magnet 7. Then, by applying a development bias consisting of an alternating electric field superimposed on a direct current electric field, the electrostatic latent image is visualized as a toner image using the two-component developer in the developer (development process). The toner image formed on the electrostatic latent image carrier 1 is electrostatically transferred to a recording medium 12 by a transfer charger 11 without using an intermediate transfer body (transfer process).

[0138] 2, the image may be transferred from the electrostatic latent image carrier 1 to an intermediate transfer member 9 (via the intermediate transfer member) and then electrostatically transferred to a transfer material (recording medium) 12. The recording medium 12 is then transported to a fixing device 13, where the toner is fixed onto the recording medium 12 by heating and pressing (fixing process). The recording medium 12 is then discharged outside the apparatus as an output image. After the transfer process, any toner remaining on the electrostatic latent image carrier 1 is removed by a cleaner 15.

[0139] Thereafter, the electrostatic latent image carrier 1 cleaned by the cleaner 15 is electrically initialized by light irradiation from the pre-exposure 16, and the above image forming operation is repeated.

[0140] FIG. 2 shows an example of a full-color image forming apparatus. The arrangement of image forming units such as K, Y, C, and M and the arrows indicating their rotation directions in the figure are not limited to these. Incidentally, K represents black, Y represents yellow, C represents cyan, and M represents magenta. In Figure 2, electrostatic latent image carriers 1K, 1Y, 1C, and 1M rotate in the direction of the arrows in the figure. Each electrostatic latent image carrier is charged by chargers 2K, 2Y, 2C, and 2M, which serve as charging means, and the surface of each charged electrostatic latent image carrier is exposed by exposure devices 3K, 3Y, 3C, and 3M, which serve as electrostatic latent image forming means, to form an electrostatic latent image.

[0141] The electrostatic latent image is then visualized as a toner image by two-component developers carried on developer carriers 6K, 6Y, 6C, and 6M provided in developing devices 4K, 4Y, 4C, and 4M, which serve as developing means. The toner image is then transferred to intermediate transfer body 9 by intermediate transfer chargers 10K, 10Y, 10C, and 10M, which serve as transfer means. The toner image is then transferred to recording medium 12 by transfer charger 11, which also serves as transfer means, and the recording medium 12 is fixed by heat and pressure by fixing device 13, which serves as fixing means, and output as an image. An intermediate transfer body cleaner 14, which is a cleaning member for intermediate transfer body 9, collects residual toner and the like after transfer.

[0142] Specifically, the development method preferably involves applying an AC voltage to the developer carrier 6 to form an AC electric field in the development area while the magnetic brush is in contact with the photosensitive member. The distance (SD distance) between the developer carrier (developing sleeve) 6 and the electrostatic latent image carrier 1 is preferably 100 μm or more and 1000 μm or less, which is favorable for preventing carrier adhesion and improving dot reproducibility. A distance of 100 μm or more ensures sufficient developer supply and good image density. A distance of 1000 μm or less prevents the magnetic field lines from the magnetic pole S1 from spreading, improving the density of the magnetic brush and improving dot reproducibility. Furthermore, the force that binds the magnetically coated carrier is increased, suppressing carrier adhesion.

[0143] The peak-to-peak voltage (Vpp) of the alternating electric field is preferably 300 V or more and 3000 V or less, more preferably 500 V or more and 1800 V or less. The frequency is preferably 500 Hz or more and 10000 Hz or less, more preferably 1000 Hz or more and 7000 Hz or less, and can be appropriately selected depending on the process.

[0144] In this case, the waveform of the AC bias for forming the AC electric field can be a triangular wave, a square wave, a sine wave, or a waveform with a varied duty ratio. To accommodate changes in the toner image formation speed, it is preferable to apply a development bias voltage (intermittent AC superimposed voltage) having a discontinuous AC bias voltage to the developer carrier for development. When the applied voltage is 300 V or higher, sufficient image density is easily obtained, and fogging toner in non-image areas is easily collected. Furthermore, when the voltage is 3000 V or lower, disturbance of the latent image via the magnetic brush is unlikely to occur, resulting in good image quality.

[0145] By using a two-component developer with a well-charged toner, the fog removal voltage (Vback) can be lowered, and the primary charge of the photoreceptor can be reduced, thereby extending the life of the photoreceptor. Vback, although it depends on the development system, is preferably 200 V or less, more preferably 150 V or less. The contrast potential is preferably 100 V or more and 400 V or less to produce sufficient image density.

[0146] Although a frequency lower than 500 Hz affects the process speed, the electrostatic latent image carrier may have the same structure as a photoreceptor typically used in an image-forming apparatus, such as a photoreceptor having a conductive substrate made of aluminum, stainless steel, or the like, on which a conductive layer, an undercoat layer, a charge generation layer, a charge transport layer, and optionally a charge injection layer are provided in this order. The conductive layer, undercoat layer, charge generating layer, and charge transport layer may be layers that are generally used in photoreceptors. As the outermost surface layer of the photoreceptor, for example, a charge injection layer or a protective layer may be used. The methods for measuring physical properties related to the present invention will be described below.

[0147] <Measurement of weight average particle size (D4) of toner particles> The weight-average particle size (D4) of the toner particles is measured with an effective number of 25,000 measurement channels using a precision particle size distribution measuring device equipped with a 100 μm aperture tube and using the narrow-pore electrical resistance method, the Coulter Counter Multisizer 3 (registered trademark, manufactured by Beckman Coulter, Inc.), and the accompanying dedicated software for setting measurement conditions and analyzing measurement data, the Beckman Coulter Multisizer 3 Version 3.51 (manufactured by Beckman Coulter, Inc.), and the measurement data is analyzed and calculated. The aqueous electrolyte solution used for the measurement is prepared by dissolving special grade sodium chloride in ion-exchanged water to a concentration of approximately 1% by mass, such as "ISOTON II" (manufactured by Beckman Coulter).

[0148] Before carrying out the measurements and analysis, the dedicated software is set up as follows. In the "Change Standard Measurement Method (SOM) screen" of the dedicated software, set the total count in control mode to 50,000 particles, the number of measurements to 1, and the Kd value to the value obtained using "Standard Particle 10.0 μm" (Beckman Coulter). Press the threshold / noise level measurement button to automatically set the threshold and noise level. Also, set the current to 1600 μA, the gain to 2, the electrolyte solution to ISOTON II, and check "Flush aperture tube after measurement." In the dedicated software's "Pulse to particle size conversion setting screen," set the bin interval to logarithmic particle size, the particle size bin to 256 particle size bins, and the particle size range to 2 μm or more and 60 μm or less.

[0149] The specific measurement method is as follows. (1) Pour approximately 200 ml of the electrolyte solution into a 250 ml round-bottom glass beaker made specifically for the Multisizer 3, set it on the sample stand, and stir the stirrer rod counterclockwise at 24 revolutions per second. Then, use the "aperture flush" function of the dedicated software to remove any dirt and air bubbles from inside the aperture tube.

[0150] (2) Approximately 30 ml of the above-mentioned aqueous electrolyte solution is placed in a 100 ml flat-bottom glass beaker, and approximately 0.3 ml of a dilution obtained by diluting "Contaminon N" (a 10% by weight aqueous solution of a neutral detergent for cleaning precision measuring instruments, pH 7, consisting of a nonionic surfactant, anionic surfactant, and organic builder, manufactured by Wako Pure Chemical Industries, Ltd.) three times by weight with ion-exchanged water is added as a dispersant.

[0151] (3) A predetermined amount of ion-exchanged water is placed in the water tank of an ultrasonic disperser, "Ultrasonic Dispersion System Tetora150" (manufactured by Nikkaki Bios Co., Ltd.), which has two built-in oscillators with an oscillation frequency of 50 kHz and a phase difference of 180 degrees and an electrical output of 120 W, and approximately 2 ml of the Contaminon N is added to this water tank.

[0152] (4) Set the beaker (2) in the beaker fixing hole of the ultrasonic disperser, operate the ultrasonic disperser, and adjust the height of the beaker so that the resonance state of the liquid surface of the electrolytic solution in the beaker is maximized.

[0153] (5) While ultrasonic waves are irradiated to the electrolyte solution in the beaker in (4), approximately 10 mg of toner particles are added little by little to the electrolyte solution and dispersed. The ultrasonic dispersion process is then continued for another 60 seconds. During the ultrasonic dispersion, the water temperature in the water tank is appropriately adjusted to be between 10°C and 40°C.

[0154] (6) Using a pipette, the electrolytic solution (5) containing the dispersed toner is dropped into the round-bottom beaker (1) placed in the sample stand, and the measurement concentration is adjusted to approximately 5%. Then, measurements are continued until the number of particles measured reaches 50,000.

[0155] (7) The measurement data is analyzed using the dedicated software provided with the device, and the weight-average particle size (D4) is calculated. Note that when the dedicated software is set to Graph / Volume %, the "Average diameter" on the Analysis / Volume Statistics (Arithmetic Mean) screen is the weight-average particle size (D4).

[0156] <Method for measuring average circularity> The average circularity of the toner particles is measured using a flow particle image analyzer "FPIA-3000" (manufactured by Sysmex Corporation) under the measurement and analysis conditions used during the calibration process. The specific measurement method is as follows. First, approximately 20 ml of ion-exchanged water, from which impurities such as solids have been removed, is placed in a glass container. Approximately 0.2 ml of a solution prepared by diluting Contaminon N (a 10% by weight aqueous solution of a pH 7 neutral detergent for cleaning precision measuring instruments, consisting of a nonionic surfactant, an anionic surfactant, and an organic builder, manufactured by Wako Pure Chemical Industries, Ltd.) approximately three times by weight with ion-exchanged water is added. Approximately 0.02 g of the sample to be measured is then added, and the mixture is dispersed for two minutes using an ultrasonic disperser to obtain a dispersion for measurement. The dispersion is then cooled appropriately so that its temperature is between 10°C and 40°C. A tabletop ultrasonic cleaner disperser (VS-150, manufactured by Vervoclear) with an oscillation frequency of 50 kHz and an electrical output of 150 W is used as the ultrasonic disperser. A predetermined amount of ion-exchanged water is placed in the water tank, and approximately 2 ml of Contaminon N is added to the water tank.

[0157] The measurement was performed using the flow particle image analyzer equipped with a standard objective lens (10x magnification), and a particle sheath "PSE-900A" (manufactured by Sysmex Corporation) was used as the sheath liquid. The dispersion prepared according to the procedure described above was introduced into the flow particle image analyzer, and 3,000 toner particles were measured in HPF measurement mode and total count mode. The binarization threshold for particle analysis was set to 85%, and the analyzed particle diameter was limited to a circle-equivalent diameter of 1.985 μm or more and less than 39.69 μm, and the average circularity of the toner particles was determined.

[0158] Before starting the measurement, automatic focus adjustment is performed using standard latex particles (Duke Scientific's "RESEARCH AND TEST PARTICLES Latex Microsphere Suspensions 5200A" diluted with ion-exchanged water). After that, it is preferable to perform focus adjustment every two hours from the start of the measurement.

[0159] In the examples of the present application, a flow-type particle image analyzer was used that had been calibrated by Sysmex Corporation and had a calibration certificate issued by Sysmex Corporation. Measurements were carried out under the same measurement and analysis conditions as when the calibration certificate was received, except that the particle diameter to be analyzed was limited to a circle-equivalent diameter of 1.985 μm or more and less than 39.69 μm.

[0160] <Measurement of magnetic carrier resistivity> The resistivity of the magnetic carrier is measured using a measuring device shown in Fig. 3. The resistivity of the magnetic carrier is measured at an electric field strength of 2000 (V / cm). Resistance measurement cell A has a cross-sectional area of ​​2.4 cm 2 The device is composed of a cylindrical container (made of PTFE resin) 17 with a hole, a lower electrode (made of stainless steel) 18, a support base (made of PTFE resin) 19, and an upper electrode (made of stainless steel) 20. The cylindrical container 17 is placed on the support base 19, and a sample (magnetic carrier) 21 is filled to a thickness of approximately 1 mm. The upper electrode 20 is placed on the filled sample 21, and the thickness of the sample is measured. As shown in Figure 3(a), the gap when there is no sample is d1, and as shown in Figure 3(b), the gap when the sample is filled to a thickness of approximately 1 mm is d2. The sample thickness d can be calculated using the following formula. d = d2 - d1 (mm) At this time, the mass of the sample is appropriately changed so that the thickness d of the sample is 0.95 mm or more and 1.04 mm or less.

[0161] The resistivity of the sample can be determined by applying a DC voltage between the electrodes and measuring the current that flows at that time. For the measurement, an electrometer 22 (Kesley 6517A, manufactured by Kesley) and a processing computer 23 for control are used. The control system and control software (LabVEIW, National Instruments) manufactured by National Instruments are used for the control processing computer. The measurement conditions were: contact area between the sample and the electrode S = 2.4 cm 2 The measured value d is input so that the thickness of the sample is between 0.95 mm and 1.04 mm. The load on the upper electrode is set to 270 g, and the maximum applied voltage is set to 1000 V. Resistivity (Ω·cm) = (applied voltage (V) / measured current (A)) × S (cm 2 ) / d(cm) Electric field strength (V / cm) = applied voltage (V) / d (cm) The resistivity of the magnetic carrier at the electric field strength is read from the graph as the resistivity at the electric field strength on the graph.

[0162] <Measurement of pore diameter and pore volume of porous magnetic core particles> The pore size distribution of the porous magnetic core particles is measured by mercury intrusion porosimetry. The measurement principle is as follows. In this measurement, the pressure applied to the mercury is varied, and the amount of mercury that penetrates into the pores is measured. The conditions under which mercury can penetrate into the pores can be expressed from the balance of forces as PD = -4σCOSθ, where P is the pressure, D is the pore diameter, θ is the contact angle of the mercury, and σ is the surface tension. If the contact angle and surface tension are constants, then the pressure P and the pore diameter D into which mercury can penetrate at that time are inversely proportional. For this reason, the pressure P and the amount of infiltrated liquid V at that time are measured by varying the pressure, and the horizontal axis P of the PV curve, obtained by this measurement, is then directly substituted for the pore diameter in this equation to determine the pore distribution.

[0163] Measurement can be performed using a measuring device such as a fully automatic multi-function mercury porosimeter PoreMaster series or PoreMaster-GT series manufactured by Yuasa Ionics Co., Ltd., or an automatic porosimeter Autopore IV 9500 series manufactured by Shimadzu Corporation. Specifically, the measurement is carried out using an Autopore IV9520 manufactured by Shimadzu Corporation under the following conditions and procedures. Measurement conditions Measurement environment: 20℃ Measurement cell sample volume 5cm 3 , indentation volume 1.1cm 3 , Application for powder Measurement range: 2.0 psia (13.8 kPa) or more, 59989.6 psia (413.7 kPa) or less Measurement steps: 80 steps (When the pore diameter is calculated logarithmically, the steps are spaced at equal intervals.) Pressing Parameter - Exhaust Pressure 50 μmHg Exhaust Time 5.0 min Mercury Injection Pressure 2.0 psia (13.8 kPa) Equilibration Time 5 secs High Pressure Parameter - Equilibration Time 5 secs Mercury Parameter - Advancing Contact Angle 130.0 degrees Receding Contact Angle 130.0 degrees Surface Tension 485.0 mN / m (485.0 dynes / cm) Mercury Density 13.5335 g / mL

[0164] Measurement Procedure (1) Weigh approximately 1.0 g of porous magnetic core particles and place them in the sample cell. Enter the weighed value. (2) Measure in the low-pressure section within the range of 2.0 psia (13.8 kPa) or more and 45.8 psia (315.6 kPa) or less. <00​​​​​​​​​​​​​​​​Specifically, quantitative analysis of phosphorus and carbon elements is performed using an X-ray photoelectron spectrometer "K-Alpha" (manufactured by Thermo Fisher Scientific) under the following analytical conditions, and the surface element concentration is calculated using the relative sensitivity factor from each atomic peak area, and the ratio (P / C) of the surface element concentration of phosphorus (P) to the surface element concentration of carbon (C) is calculated.

[0166] (Sample preparation) The dried resin is placed in a hole (diameter 3 mm, depth 1 mm) in a powder measurement plate, and the surface is scraped off to obtain the measurement sample.

[0167] (Measurement conditions) X-ray: Al monochromatic source Acceleration: 12kV, 6mA Beam system: 400 μm Pass energy: 50 eV Step size: 0.1 eV

[0168] <Method for measuring the number average particle size of primary particles of silica fine particles A> The number average particle size of the primary particles of silica fine particles A is calculated from an image of silica fine particles A on the surface of a toner particle taken with a Hitachi ultra-high resolution field emission scanning electron microscope S-4800 (Hitachi High-Technologies Corporation). The image taking conditions for the S-4800 are as follows: The S-4800 observation conditions are set to calculate the number-average particle size of the primary particles of silica fine particle A using images obtained by backscattered electron image observation with the S-4800. Because backscattered electron images have less particle charging than secondary electron images, particle size can be measured with high precision. The average particle size is determined by measuring the particle sizes of at least 300 silica fine particles A on the surface of the toner particles. Here, since some silica fine particles A exist as agglomerates, the maximum diameter of those that can be confirmed as primary particles is determined, and the number-average particle size of the primary particles of silica fine particles A is obtained by arithmetically averaging the obtained maximum diameters.

[0169] <Method for measuring the content of metal elements in silica fine particles A> <Extraction of silica particles A from toner> Silica fine particles A are extracted from the toner by a water washing treatment method. Specifically, a sucrose aqueous solution prepared by dissolving 31.1 g of sucrose (manufactured by Kishida Chemical Co., Ltd.) in 10.3 g of ion-exchanged water is added to 6 mL of Contaminon N (described below) in a 30 mL glass vial and mixed thoroughly to prepare a dispersion. Contaminon N: A neutral detergent for cleaning precision measuring instruments with a pH of 7, consisting of a nonionic surfactant, an anionic surfactant, and an organic builder. Manufactured by Wako Pure Chemical Industries, Ltd. Glass vial: Nichiden Rika Glass Co., Ltd., VCV-30, outer diameter: 35 mm, height: 70 mm 1.0 g of toner is added to this glass vial and allowed to stand until the toner settles naturally, producing a pre-treatment dispersion. This dispersion is shaken at 200 rpm for 5 minutes in a shaker (YS-8D model, manufactured by Yayoi Co., Ltd.) to separate the silica fine particles A from the surface of the toner particles. The toner particles and the silica fine particles A that have been separated from the surface of the toner particles are separated using a centrifuge. The centrifugation process is carried out at 3700 rpm for 30 minutes. The silica fine particles A that have been separated from the surface of the toner particles and the toner are each collected by suction filtration and dried to obtain the silica fine particles A and the toner after washing with water.

[0170] <Measurement of metal element content in silica fine particles A> The silica fine particles A obtained by repeatedly performing the above water washing treatment are subjected to fluorescent X-ray measurement to calculate the iron atom content. The X-ray fluorescence measurement of each element conforms to JIS K 0119-1969, and specifically is as follows: As a measuring device, for example, a wavelength dispersive X-ray fluorescence analyzer "Axios" (manufactured by PANalytical) is used. Two grams of sample was weighed into a cup specifically designed for powder measurement, recommended by PANalytical, with a special PP (polypropylene) film attached to the bottom. A uniform layer was formed on the bottom and the lid was then placed on the cup. Elements from Na to U in the silica particles were then measured using the FP method under atmospheric pressure He atmosphere. All detected elements were assumed to be oxides, with their total mass taken as 100%. The content (mass%) of Fe2O3 relative to the total mass was calculated as an oxide equivalent value using the SpectraEvaluation software (version 5.0L).

[0171] <Method for measuring the charge decay constant α of silica fine particles A> The charge decay constant α of the external additive used in each of the magnetic carrier and toner is calculated using an attachment of an electrostatic diffusion rate measuring device (product name: NS-D100, manufactured by Nano Seeds Co., Ltd.) according to a method in accordance with JIS C 61340-2-1. -Setting the sample The external additive is placed in an aluminum sample pan (with an inner diameter of 10 mm and a recess of 1 mm depth). Thereafter, the external additive is pressed in from above using a flat plate until it is filled to the brim. ·Environmental neglect The sample pan filled with the external additive is placed on an aluminum sample cell and left to stand for 12 hours or more in an environment of 23°C and 50% relative humidity. Charging The grounded sample cell is placed in the measuring instrument, and the sample is charged by corona discharge for 0.1 seconds. Potential measurement The surface potential is measured for 1800 seconds immediately after the end of the corona discharge. The surface potential at the start of the measurement is taken as the initial surface potential V0, and the charge decay constant α is calculated from the change in surface potential up to 1800 seconds using the following formula. ln(Vt / V0)=-αt(1 / 2) (In the above formula, V represents the surface potential (V), V represents the surface potential (V) after t seconds, V represents the initial surface potential (V), α represents the charge decay constant (1 / s(1 / 2)), and t represents the decay time (seconds).) [Example]

[0172] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. In the following formulations, parts are by weight unless otherwise specified. Moreover, Examples 23 to 28 are reference examples.

[0173] <Production example of silica fine particles A1> Silica fine particles A1 were produced by the diffusion combustion method as follows. To produce silica microparticles A1, a hydrocarbon-oxygen mixed burner with a double-tube structure, which forms an inner flame and an outer flame, was used as the combustion furnace. This burner was configured so that a two-fluid nozzle for injecting slurry was grounded in the center of the burner, allowing the raw silicon compound to be introduced. In addition, a flammable hydrocarbon-oxygen gas was injected from around the two-fluid nozzle, forming an inner flame and an outer flame, which constitute a reducing atmosphere. The atmosphere, temperature, and flame length could be adjusted by controlling the amount and flow rate of the flammable gas and oxygen. In the flame, silica fine particles are generated from the raw silicon compound, and the silica fine particles can be fused until they reach the desired particle size. After that, they are cooled and the generated silica fine particles are collected using a bag filter or the like to obtain silica fine particles A of the desired particle size. Silica fine particles A1 were produced using a hexamethylcyclotrisiloxane compound containing 150 ppm of iron atoms as the silicon compound raw material. Next, 100 parts by mass of the obtained silica fine particles A were subjected to a surface treatment with 4% by mass of hexamethyldisilazane to obtain silica fine particles A1. The number average particle size of the primary particles of the obtained silica fine particles A1 is shown in Table 1. Table 1 also shows the iron content and charge decay constant α of the silica fine particles A1 in an environment of 23° C. and 50% RH.

[0174] <Production Examples of Silica Fine Particles A2 to A13> In the production example of silica microparticles A1, the number-average particle size of the primary particles and the iron content were changed to obtain silica microparticles A2 to A13. Table 1 shows the number-average particle size of the primary particles, the silica aggregate particle size, the iron content, and the charge decay constant α under an environment of 23°C and 50% RH for each silica microparticle.

[0175] [Table 1]

[0176] <Toner manufacturing example> <Production example of amorphous polyester resin> <Production example of low molecular weight amorphous polyester resin (L)> Polyoxypropylene(2.8)-2,2-bis(4-hydroxyphenyl)propane :76.6 copies (0.17 mol; 100.0 mol% based on the total number of moles of polyhydric alcohol) Terephthalic acid: 17.4 parts (0.10 mol; 72.0 mol% based on the total number of moles of polycarboxylic acids) Adipic acid: 6.0 parts (0.04 mol; 28.0 mol% based on the total number of moles of polycarboxylic acids) Titanium tetrabutoxide (esterification catalyst): 0.5 parts The above materials were weighed and placed in a reaction vessel equipped with a condenser, a stirrer, a nitrogen inlet tube, and a thermocouple. Next, the atmosphere inside the reaction vessel was replaced with nitrogen gas, and the temperature was gradually raised with stirring, and the mixture was allowed to react for 4 hours at a temperature of 200°C with stirring. Furthermore, the pressure inside the reaction vessel was reduced to 8.3 kPa and maintained at that level for 1 hour, after which the vessel was cooled to 180°C and returned to atmospheric pressure (first reaction step). tert-Butylcatechol (polymerization inhibitor): 0.1 parts The above materials were then added, the pressure in the reactor was reduced to 8.3 kPa, and the reaction was continued for 1 hour while maintaining the temperature at 180°C. Once the softening point of the reaction product, measured according to ASTM D36-86, reached 90°C, the temperature was reduced to stop the reaction (second reaction step), yielding amorphous polyester resin (L). The resulting amorphous polyester resin (L) had a peak molecular weight (Mp) of 5,000, a softening point (Tm) of 90°C, a glass transition temperature (Tg) of 52°C, an acid value of 5 mgKOH / g, and a hydroxyl value of 10 mgKOH / g.

[0177] <Production example of high molecular weight amorphous polyester resin (H)> Polyoxyethylene (2.2)-2,2-bis(4-hydroxyphenyl)propane :72.2 copies (0.20 mol; 100.0 mol% based on the total number of moles of polyhydric alcohol) Terephthalic acid: 13.2 parts (0.08 mol; 48.0 mol% based on the total number of moles of polycarboxylic acids) Adipic acid: 8.2 parts (0.06 mol; 34.0 mol% based on the total number of moles of polycarboxylic acids) Titanium tetrabutoxide (esterification catalyst): 0.5 parts by mass The above materials were weighed and placed in a reaction vessel equipped with a condenser, a stirrer, a nitrogen inlet tube, and a thermocouple. Next, the inside of the reaction vessel was replaced with nitrogen gas, and the temperature was gradually raised with stirring, and the mixture was reacted at 200°C for 2 hours with stirring. Furthermore, the pressure inside the reaction vessel was reduced to 8.3 kPa and maintained for 1 hour, after which it was cooled to 160 and returned to atmospheric pressure (first reaction step). Trimellitic acid: 6.3 parts (0.03 mol; 18.0 mol% based on the total number of moles of polycarboxylic acids) tert-Butylcatechol (polymerization inhibitor): 0.1 parts The above materials were then added, the pressure in the reactor was reduced to 8.3 kPa, and the reaction was continued for 15 hours while maintaining the temperature at 160°C. After confirming that the softening point of the reaction product, measured according to ASTM D36-86, reached 140°C, the temperature was reduced to stop the reaction (second reaction step), yielding amorphous polyester resin (H). The resulting amorphous polyester resin (H) had a peak molecular weight (Mp) of 8700, a softening point (Tm) of 142°C, a glass transition temperature (Tg) of 57°C, an acid value of 20 mgKOH / g, and a hydroxyl value of 10 mgKOH / g.

[0178] <Toner 1 manufacturing example> Low molecular weight amorphous polyester resin (L) 70.0 parts High molecular weight amorphous polyester resin (H) 30.0 parts Fischer-Tropsch wax 5.0 parts (Hydrocarbon wax, maximum endothermic peak temperature is 90℃) CI Pigment Blue 15:3 7.0 parts The above materials were mixed in a Henschel mixer (FM-75 model, manufactured by Nippon Coke & Engineering Co., Ltd.) at a rotation speed of 20 s -1 After mixing for 5 minutes, the mixture was melted and kneaded in a twin-screw kneader (PCM-30, manufactured by Ikegai Iron Works Co., Ltd.) set at a temperature of 150°C. The resulting molten mixture was cooled and coarsely crushed to 1 mm or less using a hammer mill to obtain a coarsely crushed product. The coarsely crushed product was then finely crushed using a mechanical crusher (T-250, manufactured by Turbo Kogyo Co., Ltd.). Further, classification was carried out using a Faculty F-300 (manufactured by Hosokawa Micron Corporation) to obtain toner base particles 1. The operating conditions of the Faculty F-300 were a classification rotor rotation speed of 130 s -1 , distributed rotor rotation speed 120s -1 It was decided. 100 parts of toner base particles 1, 1.0 part of hydrophobic silica (number average particle size: 20 nm) and 2.0 parts of silica fine particles A1 were mixed in a Henschel mixer (FM-75, manufactured by Nippon Coke & Engineering Co., Ltd.) at a rotation speed of 30 s. -1 The mixture was mixed at a rotation time of 10 minutes to obtain Toner 1. Toner 1 had a weight average particle size (D4) of 6.5 μm and an average circularity of 0.950.

[0179] <Production Examples of Toners 2 to 13> Toners 2 to 13 were obtained in the same manner as in the production example of Toner 1, except that the type of silica fine particles A was changed as shown in Table 2. Toners 2 to 13 had a weight average particle size (D4) of 6.5 μm and an average circularity of 0.950.

[0180] [Table 2]

[0181] <Manufacturing example of magnetic carrier core 1> Process 1 (weighing and mixing process) Fe2O368.3% by mass MnCO328.5% by mass Mg(OH)22.0% by mass SrCO31.2% by mass The ferrite raw materials were weighed, and 80 parts of the ferrite raw materials were mixed with 20 parts of water, followed by wet mixing for 3 hours in a ball mill using zirconia with a diameter (φ) of 10 mm to prepare a slurry with a solid content of 80 mass%.

[0182] Process 2 (pre-firing process) The mixed slurry was dried using a spray dryer (manufactured by Okawahara Kakoki Co., Ltd.) and then fired in a batch electric furnace in a nitrogen atmosphere (oxygen concentration 1.0% by volume) at a temperature of 1050°C for 3.0 hours to produce calcined ferrite.

[0183] Process 3 (crushing process) The calcined ferrite was crushed to about 0.5 mm using a crusher, and water was then added to prepare a slurry. The solid content of the slurry was adjusted to 70% by mass. The slurry was crushed for 3 hours using a wet ball mill with 1 / 8-inch stainless steel beads to obtain a slurry. This slurry was further crushed for 4 hours using a wet bead mill with 1 mm diameter zirconia to obtain a calcined ferrite slurry with a volume-based 50% particle size (D50) of 1.3 μm.

[0184] Process 4 (granulation process) To 100 parts of the calcined ferrite slurry, 1.0 part of ammonium polycarboxylate as a dispersant and 1.5 parts of polyvinyl alcohol as a binder were added, and the mixture was granulated into spherical particles using a spray dryer (manufactured by Okawara Kakoki Co., Ltd.) and dried. The resulting granules were subjected to particle size adjustment and then heated at 700°C for 2 hours in a rotary electric furnace to remove organic substances such as the dispersant and binder.

[0185] Step 5 (baking process) The material was fired in a nitrogen atmosphere (oxygen concentration 1.0% by volume) over a period of 2 hours from room temperature to the firing temperature (1100°C), and then held at 1100°C for 4 hours. The temperature was then lowered to 60°C over 8 hours, and the material was returned from the nitrogen atmosphere to the air and removed when the temperature was below 40°C.

[0186] Process 6 (sorting process) After crushing the agglomerated particles, they were sieved through a sieve with 150 μm openings to remove coarse particles, air classification to remove fine powder, and further magnetic separation to remove low magnetic force particles, thereby obtaining porous magnetic core particles 1. The resulting porous magnetic core particles had a peak pore diameter of 0.60 μm and a pore volume of 75 mm 3 / g. 100 parts of porous magnetic core particles 1 were placed in the stirring vessel of a mixer / stirrer (NDMV type universal stirrer manufactured by Dalton), the temperature was maintained at 60°C, and 5 parts of a filling resin consisting of 95.0% by mass of methyl silicone oligomer and 5.0% by mass of γ-aminopropyltrimethoxysilane was added dropwise at normal pressure. After the dropwise addition was completed, stirring was continued while adjusting the time, and the temperature was raised to 70°C, filling the resin composition into the particles of each porous magnetic core. After cooling, the resulting resin-filled magnetic core particles were transferred to a mixer (a UD-AT drum mixer manufactured by Sugiyama Heavy Industries Co., Ltd.) equipped with a spiral blade in a rotatable mixing container, and the temperature was raised to 140°C at a rate of 2°C / min while stirring under a nitrogen atmosphere. Heating and stirring were then continued at 140°C for 50 minutes. The resin-filled and hardened ferrite particles were then cooled to room temperature, and non-magnetic materials were removed using a magnetic separator. Coarse particles were then removed using a vibrating sieve to obtain resin-filled magnetic carrier cores 1.

[0187] <Manufacturing example of magnetic carrier core 2> To 100.0 parts of magnetite powder with a number average particle size of 0.30 μm, 4.0 parts of a silane coupling agent (3-(2-aminoethylamino)propyltrimethoxysilane) was added, and the mixture was mixed and stirred at high speed in a container at 100°C or higher to treat the fine particles. Phenol 10 parts 6 parts formaldehyde solution (40% formaldehyde, 10% methanol, 50% water) 84 parts treated magnetite The above materials, 5 parts of 28% aqueous ammonia, and 20 parts of water were placed in a flask, and the mixture was heated to 85°C over 30 minutes and maintained at that temperature while stirring and mixing. A polymerization reaction was carried out for 3 hours, and the resulting phenolic resin was cured. The cured phenolic resin was then cooled to 30°C, and more water was added. The supernatant was removed, and the precipitate was washed with water and air-dried. This was then dried at 60°C under reduced pressure (5 mmHg or less) to obtain spherical magnetic carrier cores 2 with the magnetic material dispersed therein.

[0188] <Manufacturing example of magnetic carrier core 3> The raw materials were weighed to a concentration of 35 mol% MnO, 14.5 mol% MgO, 50 mol% Fe2O3, and 0.5 mol% SrO, mixed with water, and milled for 5 hours in a wet media mill to obtain a slurry. The resulting slurry was dried in a spray dryer to obtain spherical particles. The mixture was heated to 950°C for 2 hours and calcined. It was then milled in a wet ball mill using 0.5 cm diameter stainless steel beads for 1 hour, and then further milled using 0.3 cm diameter zirconia beads for 4 hours. An appropriate amount of dispersant was added to the slurry, and 0.8 mass% of polyvinyl alcohol resin (PVA) was added as a binder to ensure the strength of the granulated particles. The mixture was then granulated and dried using a spray dryer. It was then calcined in an electric furnace at 1275°C and an oxygen concentration of 2.5% by volume (nitrogen gas atmosphere) for 5 hours. Thereafter, the mixture was crushed and further classified to adjust the particle size, and then low magnetic force products were separated by magnetic separation to prepare magnetic carrier cores 3.

[0189] <Production example of coating resin 1> Monomer A and Monomer B shown in Table 3 were added to a four-necked flask equipped with a reflux condenser, a thermometer, a nitrogen suction tube and a rotary stirrer, and then 3.0 parts of toluene, 3.0 parts of methyl ethyl ketone and 0.072 parts of azobisisovaleronitrile were added. The mixture was kept at 80°C for 10 hours under a nitrogen stream, and then potassium polyoxyethylene alkyl ether phosphate was added as a compound containing phosphorus or sulfur in the amount shown in Table 3 to obtain a coating resin 1 solution (solid content 35% by mass). Furthermore, using the raw materials shown in Table 3, coating resins 2 to 20 were obtained in the same manner.

[0190] [Table 3]

[0191] <Magnetic Carrier 1 Manufacturing Example> 100 magnetic carrier cores Coating resin 1 3.00 parts Coating resin 1 was diluted with toluene to a resin content of 5% for 1:100 parts of magnetic carrier cores, and the resulting solution was thoroughly stirred. Magnetic carrier cores 1 were then placed in a planetary mixer (Nauta Mixer VN, manufactured by Hosokawa Micron Corporation) maintained at 60°C, and the resin solution was added. Half the resin solution was added, and the solvent was removed and applied for 30 minutes. Another half of the resin solution was then added, and the solvent was removed and applied for 40 minutes. The magnetic carrier coated with the resin coating layer was then transferred to a mixer (UD-AT type drum mixer manufactured by Sugiyama Heavy Industries Co., Ltd.) equipped with spiral blades in a rotatable mixing container, and heat-treated for 2 hours at 120°C in a nitrogen atmosphere while stirring at 10 revolutions per minute. The obtained magnetic carrier was separated into low magnetic carriers by magnetic separation, passed through a sieve with 150 μm openings, and then classified with an air classifier to obtain magnetic carrier 1. The resistivity of magnetic carrier 1 was 8.0 x 10 9 The resistance was Ω·cm.

[0192] <Manufacturing Examples of Magnetic Carriers 2 to 22> Magnetic Carriers 2 to 22 were obtained in the same manner as in the production example of Magnetic Carrier 1, except that the types of magnetic carrier core and coating resin were changed as shown in Table 4. The specific resistance values ​​of Magnetic Carriers 2 to 22 were 8.0×10 9 The resistance was Ω·cm.

[0193] [Table 4]

[0194] Toners 1 to 13 and magnetic carriers 1 to 22 were shaken in a shaker (YS-8D model, manufactured by Yayoi Co., Ltd.) to a toner concentration of 8% by mass to prepare 300 g of two-component developer. The vibration conditions of the shaker were 200 rpm and 2 minutes.

[0195] On the other hand, toners 1 to 13 and magnetic carriers 1 to 22 were mixed in a V-type mixer for 5 minutes in an environment of room temperature and humidity 23°C / 50%RH so that the carrier concentration was 8% by mass, to obtain a replenishment developer. Details of the two-component developers are shown in Table 5, and details of the replenishment developers are shown in Table 6.

[0196] [Table 5]

[0197] [Table 6]

[0198] <Examples 1 to 28 and Comparative Examples 1 to 6> The obtained two-component developer and replenishment developer were evaluated as follows. The image forming apparatus used was a modified Canon imagePRESS C850 color copier.

[0199] During image formation, the developer contained in the cyan developing machine was replaced with the above-mentioned two-component developers 1 to 34, and the replenishment developer contained in the cyan replenishment developer container was replaced with the above-mentioned replenishment developers 1 to 34. The modifications were as follows: (1) The development contrast can be adjusted to any value, and the automatic correction by the main unit is prevented from operating. (2) The AC component of the developing bias was modified to have a frequency of 2.0 kHz, and the peak-to-peak voltage (Vpp) was changed in 0.1 kV increments from 0.7 kV to 1.8 kV. (3) It was modified to enable monochrome image formation. Using the above modified machine, laser beam printer paper CS-814 (81.4 g / m 2 ) (available from Canon Marketing Japan Inc.), a cyan monochromatic image was formed, and the following evaluation tests were carried out.

[0200] The evaluation items are shown below. (1) Initial environmental difference assessment After leaving the evaluation device in an N / L environment (temperature 23°C / humidity 5RH%) and an H / H environment (temperature 30°C / humidity 80RH%) for 48 hours, 100 sheets of an FFH output chart with an image ratio of 5% were printed. FFH is a value that represents 256 gradations in hexadecimal, with 00h being the first gradation (white background) of the 256 gradations and FFH being the 256th gradation (solid area) of the 256 gradations. After 100 sheets were printed, an image was printed with nine 1cm x 1cm patches of FFH density arranged evenly spaced vertically and horizontally on the paper. The reflection density of all patches was measured using an X-Rite color reflection densitometer (500 series: manufactured by X-Rite), the average value was calculated, and the difference in image density between the N / L environment and the H / H environment was calculated. This density difference was evaluated based on the following evaluation criteria. (Evaluation criteria) A: Density difference: less than 0.03 B: Density difference: 0.03 or more and less than 0.06 C: Density difference: 0.06 or more and less than 0.10 D: Density difference: 0.10 or more and less than 0.13 E: Density difference: 0.13 or more and less than 0.16 F: Density difference: 0.16 or more and less than 0.20 G: Density difference: 0.20 or more and less than 0.25 H: Concentration difference: 0.25 or more

[0201] (2) Durability evaluation After 48 hours of storage in an N / N environment (temperature 23°C / humidity 50%) and an H / H environment (temperature 30°C / humidity 80%), 300,000 images were printed using a 5% image ratio FFH output chart in the N / N environment and a 40% image ratio FFH output chart in the H / H environment. Every 1,000 sheets during the durability test, nine 1cm x 1cm FFH density patches were printed, evenly spaced vertically and horizontally. The reflection density of all patches was measured using an X-Rite color reflection densitometer (500 series, manufactured by X-Rite), and the average was calculated as the image density for that number of sheets. The standard deviation of all image density fluctuations during the durability test was then calculated. This standard deviation of image density fluctuation was evaluated based on the following criteria. During the 300,000-sheet continuous paper feed period, paper was fed under the same development and transfer conditions (without calibration) as the first sheet. (Evaluation criteria) A: Standard deviation: less than 0.02 B: Standard deviation: 0.02 or more and less than 0.04 C: Standard deviation: 0.04 or more and less than 0.06 D: Standard deviation: 0.06 or more and less than 0.08 E: Standard deviation: 0.08 or more and less than 0.10 F: Standard deviation: 0.10 or more and less than 0.15 G: Standard deviation: 0.15 or more and less than 0.20 H: Standard deviation: 0.20 or more

[0202] (3) Evaluation of storage characteristics under high temperature and humidity After the durability test under the H / H environment in (2) above, the test piece was left in the same environment for 48 hours, and then an image was printed on a sheet of paper with nine 1cm x 1cm patches of FFH density arranged at equal intervals vertically and horizontally. The reflection density of all patches was measured using an X-Rite color reflection densitometer (500 series: manufactured by X-Rite), the average value was calculated, and the density difference from immediately after passing 300,000 sheets was calculated. This density difference was evaluated based on the following evaluation criteria. (Evaluation criteria) A: Density difference: less than 0.03 B: Density difference: 0.03 or more and less than 0.06 C: Density difference: 0.06 or more and less than 0.10 D: Density difference: 0.10 or more and less than 0.13 E: Density difference: 0.13 or more and less than 0.16 F: Density difference: 0.16 or more and less than 0.20 G: Density difference: 0.20 or more and less than 0.25 H: Concentration difference: 0.25 or more

[0203] (4) Evaluation of color change after storage After the evaluation in (3) above, the evaluation machine was moved to a non-returnable environment and left for 24 hours. Then, 100 sheets of a 5% image ratio FFH output chart were run through the machine, and the reflection density of the printed area on all 100 sheets was measured. The standard deviation of the image density fluctuations between the first sheet and the 50th sheet, and between the 51st sheet and the 100th sheet, was calculated. This standard deviation of the image density fluctuations was evaluated based on the following evaluation criteria. During the test, the sheets were run through under the same development and transfer conditions (without calibration) as the first sheet. (Evaluation criteria) A: Standard deviation: less than 0.02 B: Standard deviation: 0.02 or more and less than 0.04 C: Standard deviation: 0.04 or more and less than 0.06 D: Standard deviation: 0.06 or more and less than 0.08 E: Standard deviation: 0.08 or more and less than 0.10 F: Standard deviation: 0.10 or more and less than 0.15 G: Standard deviation: 0.15 or more and less than 0.20 H: Standard deviation: 0.20 or more

[0204] The evaluation results are shown in Table 7. [Table 7] [Explanation of symbols]

[0205] 1, 1K, 1Y, 1C, 1M: electrostatic latent image carrier, 2, 2K, 2Y, 2C, 2M: charger, 3, 3K, 3Y, 3C, 3M: exposure device, 4, 4K, 4Y, 4C, 4M: developer, 5: developer container, 6, 6K, 6Y, 6C, 6M: developer carrier, 7: magnet, 8: regulating member, 9: intermediate transfer body, 10K, 10Y, 10C, 10M: intermediate transfer charger, 11: transfer charger, 12: transfer material (recording medium), 13: fixing device, 14: intermediate transfer body cleaner, 15, 15K, 15Y, 15C, 15M: cleaner, 16: pre-exposure, 17: cylindrical container, 18: lower electrode, 19: support base, 20: upper electrode, 21: magnetic carrier or carrier core, 22: electrometer, 23: processing computer, d1: gap when no sample is present, d2: gap when sample is filled

Claims

1. A two-component developer including a toner and a magnetic carrier, The toner has toner particles containing a binder resin and silica fine particles A present on the surfaces of the toner particles, The silica fine particles A have a number average particle size of primary particles of 80 nm or more and 200 nm or less, The silica fine particles A contain iron atoms in an amount of 50 ppm or more and 1000 ppm or less in terms of oxide, The silica fine particles A have a charge decay constant α of 0.0005 or more and 0.0100 or less 1800 seconds after being charged in an environment having a temperature of 23° C. and a relative humidity of 50%, The magnetic carrier is a magnetic carrier having magnetic carrier particles having a magnetic carrier core and a resin coating layer formed on the surface of the magnetic carrier core, The resin coating layer contains a resin including a structural unit derived from a (meth)acrylic acid ester compound, The two-component developer is characterized in that the resin coating layer contains phosphorus or sulfur.

2. A two-component developer as described in Claim 1, wherein the silica fine particles A have a charge decay constant α of 0.0010 or more and 0.0050 or less.

3. A two-component developer according to claim 1 or 2, wherein the content of iron atoms in the silica fine particles A is 150 ppm or more and 1000 ppm or less in terms of oxide.

4. The two-component developer according to any one of claims 1 to 3, wherein the (meth)acrylic acid ester compound is an alicyclic (meth)acrylic acid ester compound.

5. The two-component developer according to claim 4 , wherein the alicyclic (meth)acrylic acid ester compound has a cycloalkyl group having 5 to 8 carbon atoms.

6. The two-component developer according to claim 5, wherein the alicyclic (meth)acrylic acid ester compound is cyclohexyl (meth)acrylate.

7. 7. The two-component developer according to claim 2, wherein the resin coating layer further contains a structural unit derived from a chain (meth)acrylic acid ester compound.

8. The two-component developer according to any one of claims 2 to 7, wherein the content of the constitutional unit derived from the alicyclic (meth)acrylic acid ester compound in the resin coating layer is 10.0% by mass or more and 90.0% by mass or less.

9. The two-component developer according to any one of claims 1 to 8, wherein the resin coating layer contains a phosphorus element.

10. 10. The two-component developer according to claim 9, wherein the ratio (P / C) of the phosphorus content (P) to the carbon content (C) in the resin coating layer is 0.0010 or more and 0.0100 or less.

11. 11. The two-component developer according to claim 9, wherein the resin coating layer contains the phosphorus element as a phosphoric acid group, an acidic phosphoric acid ester group or a salt thereof, or a phosphoric acid ester group.

12. A replenishment developer for use in a two-component developing method in which a replenishment developer is replenished to a developing device in response to a decrease in toner concentration of the two-component developer in the developing device, an electrostatic latent image formed on a surface of an electrostatic latent image carrier is developed using the two-component developer in the developing device, and an excess magnetic carrier inside the developing device is discharged from the developing device as necessary, The replenishing developer is characterized in that the amount of the toner per 1 part by mass of the magnetic carrier is 2 parts by mass or more and 50 parts by mass or less, and the replenishing developer is a two-component developer according to any one of claims 1 to 11.

13. 12. An image forming method comprising: a charging step of charging an electrostatic latent image carrier; an electrostatic latent image forming step of forming an electrostatic latent image on the surface of the electrostatic latent image carrier; a developing step of developing the electrostatic latent image with a two-component developer in a developing device to form a toner image; a transfer step of transferring the toner image to a transfer material with or without an intermediate transfer body; and a fixing step of fixing the transferred toner image to the transfer material, wherein the two-component developer according to any one of claims 1 to 11 is used as the two-component developer.

Citation Information

Patent Citations

  • Developer and developing method

    JP1999223960A

  • Toner and electrophotographic device

    JP2003043727A

  • Carrier for electrostatic charge image development, and two-component developer for electrostatic charge image development