Polarizing plate, liquid crystal panel and display device

The polarizing plate design with controlled heat shrinkage deformation values and a stable structure addresses the issue of warping and light leakage in liquid crystal displays by using a hard coating layer and light-transmitting base material, ensuring durability and stability under high temperature and humidity.

JP7566630B2Active Publication Date: 2024-10-15XINMEI HOLDINGS (HONG KONG) CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2020542567
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-06-28
Filing Date
2019-07-01
Publication Date
2024-10-15
Estimated Expiration
2039-07-01

AI Technical Summary

Technical Problem

Polarizing plates in liquid crystal display devices suffer from heat-induced shrinkage and deformation, leading to warping and light leakage due to poor durability under high temperature and humidity conditions.

Method used

A polarizing plate design with a hard coating layer of 10 μm or less on one side and a light-transmitting base material on the other, where the ratio of heat shrinkage deformation values in perpendicular directions is controlled between 0.8 to 1.2, ensuring a stable internal structure and preventing cracks.

Benefits of technology

The design maintains structural integrity and prevents light leakage by adjusting heat shrinkage rates, providing durability and stability even under high temperature and humidity exposure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007566630000004
    Figure 0007566630000004
  • Figure 0007566630000005
    Figure 0007566630000005
  • Figure 0007566630000006
    Figure 0007566630000006
Patent Text Reader

Abstract

The present invention relates to a polarizing plate comprising: a polarizer; a hard coating layer having a thickness of 10 μm or less formed on one side of the polarizer; and an optical laminate comprising a light-transmitting substrate formed on the other side of the polarizer.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] Cross-reference to related applications This application claims the benefit of priority based on Korean Patent Application No. 10-2018-0075899 filed on June 29, 2018, Korean Patent Application No. 10-2018-0167778 filed on December 21, 2018, and Korean Patent Application No. 10-2019-0078374 filed on June 28, 2019, and all contents disclosed in the documents of these Korean patent applications are incorporated herein by reference.

[0002] The present invention relates to a polarizing plate, a liquid crystal panel, and a display device. [Background technology]

[0003] Liquid crystal display devices are displays that visualize polarized light using the switching effect of liquid crystals, and are used in a wide range of applications, from small and medium-sized displays for computers, notebook computers, electronic watches, and portable terminals to large TVs.

[0004] Currently, a considerable number of polarizing plates that are mass-produced for use in display devices are made by dyeing a polyvinyl alcohol film with a dichroic substance such as iodine or a dichroic dye, crosslinking it with a boron compound, and then stretching and aligning it to form a polarizing film (polarizer), on one or both sides of which an optically transparent protective film that has mechanical strength is bonded.

[0005] However, stretched polyvinyl alcohol films have a problem in that they easily undergo shrinkage deformation under durability conditions such as high temperature and high humidity. When the polarizer is deformed, the resulting stress affects the protective film and the liquid crystal cell, causing warping, which results in problems such as changes in the physical properties of the polarizing plate including the polarizer and light leakage in the liquid crystal display device. Summary of the Invention [Problem to be solved by the invention]

[0006] The object of the present invention is to provide a polarizing plate which has a well-balanced warpage and a stable internal structure by controlling the thermal shrinkage rate of the detailed constituent layers, and which can prevent cracks and light leakage in liquid crystal displays.

[0007] It is also an object of the present invention to provide a liquid crystal panel and a display device each including the polarizing plate. [Means for solving the problem]

[0008] The present specification provides a polarizing plate including: a polarizer; a hard coating layer having a thickness of 10 μm or less formed on one side of the polarizer; and an optical laminate including a light-transmitting substrate formed on the other side of the polarizer.

[0009] This specification also provides a polarizing plate comprising: a polarizer; a hard coating layer having a thickness of 10 μm or less formed on one side of the polarizer; and an optical laminate including a light-transmitting substrate formed on the other side of the polarizer; wherein a ratio of a thermal shrinkage deformation value of the optical laminate in a second direction perpendicular to the first direction to a thermal shrinkage deformation value of the optical laminate in a first direction is within a specific range.

[0010] The present specification also provides a polarizing plate comprising: an optical laminate including a polarizer; a hard coating layer having a thickness of 10 μm or less formed on one side of the polarizer; and a light-transmitting substrate formed on the other side of the polarizer; wherein a ratio of a thermal shrinkage deformation value of the optical laminate in a second direction perpendicular to the first direction to a thermal shrinkage deformation value of the optical laminate in a first direction is 0.8 to 1.2.

[0011] Further, the present specification provides a liquid crystal panel in which the polarizing plate is formed on at least one surface of a liquid crystal cell.

[0012] Also provided herein is a display device comprising the polarizer.

[0013] Hereinafter, a polarizing plate, a liquid crystal panel, and a display device according to specific embodiments of the invention will be described in more detail.

[0014] In the present invention, the terms "first", "second", etc. are used to describe various components, and the terms are used only to distinguish one component from another component.

[0015] Additionally, (meth)acryl is intended to include both acryl and methacryl.

[0016] Moreover, the inorganic nanoparticles having a hollow structure refer to particles having an empty space on the surface and / or inside the inorganic nanoparticles.

[0017] In addition, the term "(co)polymer" is intended to include both a copolymer and a homopolymer.

[0018] According to one embodiment of the invention, there may be provided a polarizing plate comprising: a polarizer; a hard coating layer having a thickness of 10 μm or less formed on one side of the polarizer; and an optical laminate including a light-transmitting substrate formed on the other side of the polarizer; wherein a ratio of a thermal shrinkage deformation value of the optical laminate in a second direction perpendicular to the first direction to a thermal shrinkage deformation value in a first direction is 0.8 to 1.2.

[0019] Triacetyl cellulose (TAC) films, which are widely used as polarizer protective films for polarizing plates, have poor water resistance and can be twisted in high temperature / high humidity environments, causing defects such as light leakage. However, the inventors have confirmed through experiments that the polarizing plate of the above embodiment uses a light-transmitting substrate having the above-mentioned characteristics, thereby ensuring durability without significant changes in physical properties or shape even when exposed to high temperature and high humidity conditions for a long period of time, and have completed the invention.

[0020] In the polarizing plate of the above embodiment, the ratio (R) of the thermal shrinkage deformation value of the optical laminate in a second direction perpendicular to the first direction to the thermal shrinkage deformation value of the optical laminate in the first direction is 0.8 to 1.2, or 0.85 to 1.1. Therefore, even when a temperature of 60°C or more is applied during the manufacturing process, the thermal shrinkage rate or thermal shrinkage deformation rate between the fine layers of the polarizing plate is controlled, and the warping balance of the polarizing plate is also confirmed to be good, so that cracks in the polarizing plate can be prevented and light leakage phenomena in LCD devices can be prevented.

[0021] The ratio (R) may be defined by the following general formula 1:

[0022] [General formula 1] A ratio (R) of a thermal shrinkage deformation value of the optical laminate in a second direction perpendicular to the first direction to a thermal shrinkage deformation value of the optical laminate in a first direction = Heat shrinkage deformation value of the optical laminate in the second direction / Heat shrinkage deformation value of the optical laminate in the first direction

[0023] The thermal shrinkage deformation value of the optical laminate in the first direction and the thermal shrinkage deformation value of the optical laminate in the second direction may be a difference between the initial length of the optical laminate in the first direction and the length value measured after exposing the optical laminate for 80 to 120 hours at a temperature of 80 to 120° C. More specifically, the thermal shrinkage deformation value of the optical laminate in the first direction and the second direction may be a difference between the initial length of the optical laminate in the first direction and the length measured after exposing the optical laminate to a temperature of 100° C. for 96 hours.

[0024] The thermal shrinkage deformation value of the optical laminate in the first direction and the thermal shrinkage deformation value of the optical laminate in the second direction may be defined by the following General Formula 2 and General Formula 3, respectively.

[0025] [General formula 2] Heat shrinkage deformation value in a first direction of the optical laminate = Initial length of the optical laminate in the first direction (MD direction of PET) - Length of the optical laminate in the first direction (MD direction of PET) measured after exposure to a temperature of 80°C to 120°C for 80 to 120 hours

[0026] [General formula 3] Heat shrinkage deformation value in the second direction of the optical laminate = initial length of the optical laminate in the second direction (TD direction of PET) - length of the optical laminate in the second direction (TD direction of PET) measured after exposure to a temperature of 80°C to 120°C for 80 to 120 hours

[0027] The optical laminate may exhibit the greatest deformation in a temperature range of around 80°C, specifically in a temperature range of 80°C to 120°C. By providing a light-transmitting substrate on one side of the polarizer and a hard coating layer having a thickness of 10 μm or less on the other side, the ratio of the thermal shrinkage deformation value of the optical laminate in a second direction perpendicular to the first direction to the thermal shrinkage deformation value of the optical laminate in the first direction may satisfy 0.8 to 1.2, or 0.85 to 1.1.

[0028] In particular, when the light-transmitting substrate included in the optical laminate is a polymer film, for example, TAC, PET, acrylic resin, cycloolefin polymer (COP), polycarbonate, polymethyl methacrylate (PMMA), etc., the change in temperature rise or the heat shrinkage deformation value may be greater in a temperature range of about 80°C than in the previous temperature range. However, the polarizing plate may have a ratio of the heat shrinkage deformation value in the second direction of the optical laminate perpendicular to the first direction to the heat shrinkage deformation value in the first direction observed after being exposed to a temperature of 80°C to 120°C for 80 to 120 hours of 0.8 to 1.2, thereby achieving better durability against heat deformation or heat shrinkage and ensuring structural stability that is difficult to achieve in polarizing plates of other previously known structures.

[0029] In addition, the polarizing plate of the embodiment includes the optical laminate and a hard coating layer having a thickness of 10 μm or less formed on one side of the polarizer. This allows for a thinner thickness while appropriately controlling the thermal shrinkage rate and thermal shrinkage force between fine layers, thereby realizing a robust internal structure.

[0030] In particular, whereas previously known polarizing plates have a structure in which triacetyl cellulose (TAC) films are placed on both sides of a polarizer, the polarizing plate of the present embodiment has an optical laminate having the above-mentioned properties on one side and a hard coating layer having a thickness of 10 μm or less on the other side, which can block moisture transmission to the PVA film side and reduce the overall thickness of the polarizing film.

[0031] In this case, the first direction of the optical laminate may be a machine direction (MD) of the light-transmitting substrate, and the second direction of the optical laminate may be a transverse direction (TD) of the light-transmitting substrate.

[0032] If the ratio of the thermal shrinkage deformation value of the optical laminate in a second direction perpendicular to the first direction to the thermal shrinkage deformation value of the optical laminate in a first direction is excessively small or large, stress transfer at high temperature and humidity may occur unevenly, the adhesion between the fine layers may decrease, the polarizer and the optical laminate may be lifted, cracks may occur in the polarizing plate, and light leakage phenomena may occur in the LCD device, which may be technically disadvantageous.

[0033] The light-transmitting substrate may have a transmittance of 50% or more at wavelengths of 300 nm or more.

[0034] Meanwhile, an example of a polarizing plate 100 according to the embodiment is shown in Fig. 1. The polarizing plate 100 shown in Fig. 1 includes a polarizer 20, a hard coating layer 30 having a thickness of 10 µm or less and positioned to face the polarizer with respect to the center, and a light-transmitting substrate 10.

[0035] Meanwhile, the light-transmitting substrate may have a retardation (Rth) in the thickness direction measured at a wavelength of 400 nm to 800 nm of 3,000 nm or more.

[0036] By controlling the retardation of the light-transmitting substrate to 3,000 nm or more, 4,000 to 15,000 nm, or 5,000 to 10,000 nm, rainbow phenomenon due to destructive interference is suppressed, and the visibility of the image display device can be improved to be comparable to that of a cellulose ester film.

[0037] The retardation is determined by the refractive index in the slow axis direction, which is the direction in the plane of the light-transmitting substrate that has the largest refractive index (n x ), the refractive index in the fast axis direction perpendicular to the slow axis direction (n y ) and the thickness d (unit: nm) of the light-transmitting substrate may be substituted into the following mathematical formula 1 to calculate the light-transmitting coefficient:

[0038] [Formula 1] Re = (n x -n y )×d

[0039] The retardation may be a value measured using, for example, an automatic birefringence meter (KOBRA-WR, measurement angle: 0°, measurement wavelength: 548.2 nm). Alternatively, the retardation may be obtained by the following method. First, two polarizing plates are used to provide the light-transmitting substrate with the alignment axis direction, and two axial refractive indices (n x , n y ) is obtained using an Abbe refractometer (NAR-4T). At this time, the axis showing the larger refractive index is defined as the slow axis. In addition, the thickness of the light-transmitting substrate is measured using, for example, an electric micrometer, and the refractive index difference (n x -n y )(Hereinafter, n x -n y The difference in refractive index (Δn) is calculated, and the retardation can be calculated by multiplying this difference in refractive index (Δn) by the thickness d (nm) of the light-transmitting substrate.

[0040] Since the retardation of the light-transmitting substrate is 3000 nm or more, the refractive index difference (Δn) may be 0.05 or more, 0.05 to 0.20, or 0.08 to 0.13. If the refractive index difference (Δn) is less than 0.05, the thickness of the light-transmitting substrate required to obtain the above-mentioned retardation value may be large. On the other hand, if the refractive index difference (Δn) exceeds 0.20, the stretching ratio needs to be excessively increased, and the light-transmitting substrate is easily broken and destroyed, so that the practicality as an industrial material may be significantly reduced, and the moist heat resistance may be reduced.

[0041] The refractive index (n x ) may be 1.60 to 1.80 or 1.65 to 1.75. On the other hand, the refractive index (n y ) may be between 1.50 and 1.70, or between 1.55 and 1.65.

[0042] On the other hand, as the light-transmitting substrate, a polyethylene terephthalate (PET) film having excellent water resistance, almost no possibility of inducing light leakage phenomenon, and excellent mechanical properties can be used.

[0043] Meanwhile, the light-transmitting substrate may have a retardation (Rth) in the thickness direction of 3,000 nm or more measured at a wavelength of 400 nm to 800 nm, and may also have low moisture permeability. More specifically, the light-transmitting substrate may have a moisture permeability of 100 g / m2 or less when the moisture permeability is measured for 24 hours under conditions of 40° C. and 100% humidity. 2 or less than 10 to 100 g / m 2 may be also possible.

[0044] Meanwhile, the thickness of the light-transmitting substrate is not particularly limited, and may be 10 to 150 μm, 20 to 120 μm, or 30 to 100 μm. If the thickness of the light-transmitting substrate is less than 10 μm, it is too thin compared to the thickness of the hard coating layer, and warping may occur, and the flexibility of the light-transmitting substrate may decrease, making it difficult to control the process. In addition, if the light-transmitting substrate is too thick, the transmittance of the light-transmitting substrate may decrease, deteriorating the optical properties, and there is a problem that it is difficult to make the image display device including the light-transmitting substrate thin.

[0045] In order to make the internal structure of the polarizing plate more robust and prevent problems such as warping even when exposed to high temperature conditions, the ratio of the thickness of the hard coating layer to the thickness of the light-transmitting substrate may be 0.02 to 0.25.

[0046] As described above, if the thickness of the light-transmitting substrate is not within the appropriate range with respect to the thickness of the hard coating layer, the polarizing plate may warp, and the flexibility of the light-transmitting substrate may decrease, making it difficult to control the process.

[0047] Meanwhile, the polarizing plate of the embodiment may achieve a robust structure even with a thinner thickness compared to other previously known polarizing plate structures, and may have characteristics that the durability and physical properties are not significantly affected by external heat.

[0048] More specifically, the combined thickness of the polarizer, the hard coating layer, and the light-transmitting substrate may be 200 μm or less. For example, the polarizer may have a thickness of 40 μm or less, or from 1 to 40 μm, the hard coating layer may have a thickness of 10 μm or less, or from 1 to 10 μm, and the light-transmitting substrate may have a thickness of 150 μm or less.

[0049] Meanwhile, the hard coating layer is not particularly limited in terms of its specific composition, but may include, for example, a binder resin; and organic fine particles having a particle size of 0.5 μm to 10 μm or inorganic fine particles having a particle size of 1 nm to 500 nm dispersed in the binder resin.

[0050] The binder resin in the hard coating layer may include a photocurable resin, which refers to a polymer of a photopolymerizable compound that can undergo a polymerization reaction when irradiated with light such as ultraviolet light.

[0051] Examples of the photocurable resin include polymers or copolymers formed from a group of reactive acrylate oligomers consisting of urethane acrylate oligomers, epoxy acrylate oligomers, polyester acrylates, and polyether acrylates; and a group of polyfunctional acrylate monomers consisting of dipentaerythritol hexaacrylate, dipentaerythritol pentaacrylate, pentaerythritol tetraacrylate, pentaerythritol triacrylate, trimethylolpropane triacrylate, glycerin propoxylate triacrylate, trimethylpropane ethoxylate triacrylate, trimethylpropyl triacrylate, 1,6-hexanediol diacrylate, tripropylene glycol diacrylate, and ethylene glycol diacrylate; and epoxy resins containing an epoxy group containing an epoxy group, a ring-type epoxy group, a glycidyl group epoxy group, or an oxetane group.

[0052] The binder resin may further include a (co)polymer having a weight average molecular weight of 10,000 g / mol or more (hereinafter, referred to as a high molecular weight (co)polymer) in addition to the above-mentioned photocurable resin. The high molecular weight (co)polymer may include, for example, one or more polymers selected from the group consisting of cellulose-based polymers, acrylic-based polymers, styrene-based polymers, epoxide-based polymers, nylon-based polymers, urethane-based polymers, and polyolefin-based polymers.

[0053] The particle size of the organic or inorganic fine particles is not specifically limited, but for example, the organic fine particles may have a particle size of 1 to 10 μm, and the inorganic particles may have a particle size of 1 nm to 500 nm, or 1 nm to 300 nm.

[0054] In addition, specific examples of the organic or inorganic fine particles contained in the hard coating layer are not limited, but for example, the organic or inorganic fine particles may be organic fine particles made of acrylic resin, styrene resin, epoxide resin, or nylon resin, or inorganic fine particles made of silicon oxide, titanium dioxide, indium oxide, tin oxide, zirconium oxide, or zinc oxide.

[0055] The polarizing plate of the embodiment includes a polarizer.

[0056] The polarizer may be a film made of polyvinyl alcohol (PVA) containing iodine or a dichroic dye, which is well known in the art. In this case, the polarizer may be manufactured by dyeing a polyvinyl alcohol film with iodine or a dichroic dye and stretching the film, but the manufacturing method is not particularly limited.

[0057] Meanwhile, when the polarizer is a polyvinyl alcohol film, the polyvinyl alcohol film can be used without any particular limitation as long as it contains a polyvinyl alcohol resin or a derivative thereof. In this case, the derivative of the polyvinyl alcohol resin can be, but is not limited to, a polyvinyl formal resin, a polyvinyl acetal resin, etc. Alternatively, the polyvinyl alcohol film can be a commercially available polyvinyl alcohol film that is generally used in the manufacture of polarizers in the art, such as P30, PE30, PE60 from Kuraray Co., Ltd., M3000, M6000 from Nippon Gosei Co., Ltd., etc.

[0058] Meanwhile, the polyvinyl alcohol film may have a degree of polymerization of, but is not limited to, 1000 to 10000 or 1500 to 5000. When the degree of polymerization satisfies the above range, the molecules are free to move and can be flexibly mixed with iodine or dichroic dyes. The polarizer may have a thickness of 40 μm or less, 30 μm or less, 20 μm or less, 1 to 20 μm, or 1 to 10 μm. In this case, devices such as polarizing plates and image display devices including the polarizer can be made thin and lightweight.

[0059] Meanwhile, the optical laminate may further include a second hard coating layer having a thickness of 1 to 100 μm formed on one surface of the light-transmitting substrate to face the polarizer.

[0060] By forming the second hard coating layer, the optical laminate can realize a predetermined optical property or functionality on one surface of the polarizing layer. For example, the second hard coating layer can function as an anti-glare layer, a high refractive index layer, a medium refractive index layer, or a general hard coating layer.

[0061] Although a specific example of the second hard coating layer is not limited, the second hard coating layer may also include a binder resin and organic fine particles having a particle size of 0.5 μm to 10 μm or inorganic fine particles having a particle size of 1 nm to 500 nm dispersed in the binder resin, such as "a hard coating layer having a thickness of 10 μm or less formed on one side of the polarizer".

[0062] Also, the optical laminate may further include a low refractive layer having a refractive index of 1.20 to 1.60 in a wavelength range of 380 nm to 780 nm formed on another surface of the second hard coating layer.

[0063] The polarizing plate may further include an anti-reflection film formed on one surface of the light-transmitting substrate to face the polarizer.

[0064] Another example of the polarizing plate 100 according to the embodiment is shown in Fig. 2. The polarizing plate 100 shown in Fig. 2 includes a polarizer 20, a hard coating layer 30 having a thickness of 10 µm or less and positioned to face the polarizer with respect to the center, and a light-transmitting substrate 10, and an anti-reflection film 40 formed on one surface of the light-transmitting substrate 10.

[0065] The anti-reflection film may have an average reflectance of 2% or less in the wavelength region of 380 nm to 780 nm.

[0066] The anti-reflection film may include a hard coating layer having a thickness of 1 to 100 μm and a low reflection layer having a refractive index of 1.20 to 1.60 in the wavelength region of 380 nm to 780 nm.

[0067] Although a specific example of the hard coating layer included in the anti-reflection film is not limited, the hard coating layer included in the anti-reflection film may also include a binder resin; and organic fine particles having a particle size of 0.5 μm to 10 μm and / or inorganic fine particles having a particle size of 1 nm to 500 nm dispersed in the binder resin, such as "a hard coating layer having a thickness of 10 μm or less and positioned to face the polarizer from the center".

[0068] The binder resin and the organic fine particles having a particle size of 0.5 μm to 10 μm or the inorganic fine particles having a particle size of 1 nm to 500 nm contained in the hard coating layer of the anti-reflection film include the above-mentioned contents.

[0069] The low reflective layer having a refractive index of 1.20 to 1.60 in the wavelength region of 380 nm to 780 nm may include a binder resin and organic or inorganic particles dispersed in the binder resin, and may optionally further include a fluorine-containing compound having a photoreactive functional group and / or a silicone-based compound having a photoreactive functional group.

[0070] The binder resin comprises a (co)polymer containing multifunctional (meth)acrylate repeats, which may be derived from a multifunctional (meth)acrylate compound such as, for example, trimethylolpropane triacrylate (TMPTA), trimethylolpropane ethoxy triacrylate (TMPEOTA), glycerol propoxylate triacrylate (GPTA), pentaerythritol tetraacrylate (PETA), or dipentaerythritol hexaacrylate (DPHA).

[0071] The photoreactive functional group contained in the fluorine-containing compound or silicone-based compound may include one or more functional groups selected from the group consisting of a (meth)acrylate group, an epoxide group, a vinyl group, and a thiol group.

[0072] The fluorine-containing compound containing a photoreactive functional group may be one or more compounds selected from the group consisting of: i) an aliphatic compound or an aliphatic ring compound substituted with one or more photoreactive functional groups and at least one carbon substituted with one or more fluorines; ii) a heteroaliphatic compound or a heteroaliphatic ring compound substituted with one or more photoreactive functional groups, at least one hydrogen substituted with fluorine, and at least one carbon substituted with silicon; iii) a polydialkylsiloxane-based polymer substituted with one or more photoreactive functional groups and at least one silicone substituted with one or more fluorines; and iv) a polyether compound substituted with one or more photoreactive functional groups and at least one hydrogen substituted with fluorine.

[0073] The low reflection layer may also include hollow inorganic nanoparticles, solid inorganic nanoparticles and / or porous inorganic nanoparticles.

[0074] The hollow inorganic nanoparticles refer to particles having a maximum diameter of less than 200 nm and having open spaces on the surface and / or inside thereof. The hollow inorganic nanoparticles may include at least one type selected from the group consisting of inorganic fine particles having a number average particle diameter of 1 to 200 nm or 10 to 100 nm. The hollow inorganic nanoparticles may have a particle diameter of 1.50 g / cm. 3 ~3.50g / cm 3 The density of the powder may be 0.01 to 0.01.

[0075] The hollow inorganic nanoparticles may have at least one reactive functional group selected from the group consisting of (meth)acrylate groups, epoxide groups, vinyl groups, and thiol groups on the surface. By having the reactive functional groups on the surface of the hollow inorganic nanoparticles, a higher degree of crosslinking can be achieved.

[0076] The solid type inorganic nanoparticles may include at least one selected from the group consisting of solid type inorganic fine particles having a number average particle size of 0.5 to 100 nm.

[0077] The porous inorganic nanoparticles may include at least one selected from the group consisting of inorganic fine particles having a number average particle size of 0.5 to 100 nm.

[0078] The low reflection layer may contain 10 to 400 parts by weight of the inorganic nanoparticles and 20 to 300 parts by weight of the fluorine-containing compound and / or silicone-based compound having a photoreactive functional group, relative to 100 parts by weight of the (co)polymer.

[0079] The polarizing plate may further include an adhesive layer located between the polarizer and the light-transmitting substrate and having a thickness of 0.1 μm to 5 μm.

[0080] The adhesive layer may be formed using various adhesives for polarizing plates used in the art, such as polyvinyl alcohol-based adhesives, polyurethane-based adhesives, acrylic-based adhesives, cationic or radical-based adhesives, etc., without limitation.

[0081] Meanwhile, the polarizing plate may further include an adhesive layer formed on another surface of the hard coating film in contact with the polarizer.

[0082] The adhesive layer may enable the polarizing plate of the embodiment to be attached to an image panel of an image display device. The adhesive layer may be formed using various adhesives well known in the art, and the type is not particularly limited. For example, the adhesive layer may be formed using a rubber-based adhesive, an acrylic-based adhesive, a silicone-based adhesive, a urethane-based adhesive, a polyvinyl alcohol-based adhesive, a polyvinylpyrrolidone-based adhesive, a polyacrylamide-based adhesive, a cellulose-based adhesive, a vinyl alkyl ether-based adhesive, or the like.

[0083] Another example of the polarizing plate 100 of the embodiment is shown in Fig. 3. The polarizing plate 100 shown in Fig. 3 includes a polarizer 20, a hard coating layer 30 having a thickness of 10 µm or less and positioned to face the polarizer at the center, and a light-transmitting substrate 10, an anti-reflection film 40 formed on one surface of the light-transmitting substrate 10, an adhesive layer 50 positioned between the polarizer and the light-transmitting substrate, and an adhesive layer 60 formed on the other surface of the hard coating film in contact with the polarizer.

[0084] The thickness of the adhesive layer is not particularly limited, and may be, for example, 1 to 50 μm.

[0085] According to still another embodiment of the present invention, there may be provided a liquid crystal panel having a polarizing plate formed on at least one surface of a liquid crystal cell.

[0086] An example of a liquid crystal panel 200 according to the embodiment is shown in Fig. 4. The liquid crystal panel 200 shown in Fig. 4 has a structure in which the polarizing plate 100 is formed on one surface of a liquid crystal panel.

[0087] Another example of the liquid crystal panel 200 of the embodiment is shown in Fig. 5. The liquid crystal panel 200 shown in Fig. 5 has a structure in which the polarizing plates 100 are formed on both sides of a liquid crystal panel.

[0088] In the liquid crystal panel, the polarizing plate according to claim 1 may be formed on both sides of the liquid crystal cell, and the two polarizing plates may be positioned such that the MD direction of the polarizer of the polarizing plate formed on one side of the liquid crystal cell and the MD direction of the polarizer of the polarizing plate formed on the other side are perpendicular to each other.

[0089] According to yet another embodiment of the invention, there may be provided a display device including the polarizer described above.

[0090] The display device is not limited to a specific example, and may be, for example, a liquid crystal display device, a plasma display device, an organic light emitting diode device, or the like.

[0091] For example, the display device may be a liquid crystal display device including a pair of polarizing plates facing each other; a thin film transistor, a color filter, and a liquid crystal cell sequentially stacked between the pair of polarizing plates; and a backlight unit.

[0092] In the display device, the anti-reflection film may be provided on the outermost surface of the display panel on the viewer side or on the backlight side.

[0093] In the display device including the anti-reflection film, the anti-reflection film may be disposed on one surface of a polarizing plate that is relatively far from a backlight unit, out of a pair of polarizing plates.

[0094] As another example, the display device may include a display panel; and the polarizer disposed on at least one surface of the display panel.

[0095] The display device may be a liquid crystal display device including a liquid crystal panel and an optical laminate provided on each side of the liquid crystal panel, and at least one of the polarizing plates may be a polarizing plate including a polarizer according to one embodiment of the present specification. At this time, the type of liquid crystal panel included in the liquid crystal display device is not particularly limited, and any known panel such as a manual matrix type panel such as a TN (twisted nematic) type, STN (super twisted nematic) type, F (ferroelectric) type, or PD (polymer dispersed) type; an active matrix type panel such as a two terminal type or a three terminal type; an in-plane switching (IPS) panel, and a vertical alignment (VA) panel may be applied. Effect of the Invention

[0096] According to the present invention, there can be provided a polarizing plate having a good warp balance and a stable internal structure by controlling the thermal shrinkage rate of the detailed constituent layers, and capable of preventing cracks and light leakage in a liquid crystal display device, and a liquid crystal panel and a display device including the polarizing plate. [Brief description of the drawings]

[0097] [Figure 1] 1 is a diagram showing an example of a polarizing plate according to an embodiment of the present invention. [Diagram 2] 1 is a diagram showing another example of a polarizing plate according to an embodiment of the present invention. [Diagram 3] 1 is a diagram showing still another example of a polarizing plate according to an embodiment of the present invention. [Figure 4]1 is a diagram showing an example of a liquid crystal panel according to an embodiment of the present invention. [Diagram 5] 1 is a diagram showing another example of a liquid crystal panel according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0098] The embodiments of the present invention will be described in more detail in the following examples, however, the following examples are merely illustrative of the present invention and are not intended to limit the scope of the present invention.

[0099] [Production Example] Manufacturing Example 1: Manufacturing of optical laminate (1) Manufacturing of coating solution for forming hard coating layer The components shown in Table 1 below were mixed to prepare coating solutions (B1, B2) for forming hard coating layers of optical laminates.

[0100] [Table 1]

[0101] TMPTA: Trimethylolpropane triacrylate PETA: Pentaerythritol triacrylate UA-306T: A urethane acrylate, a reaction product of toluene diisocyanate and pentaerythritol triacrylate (Kyoeisha product) SC2152: Compound in which hexamethylene diisocyanate (HMDI) and acrylate compounds are linked by urethane bonds [Mass average molecular weight 20,000 / Manufacturer: Miwon Chemical] IRG-184: Initiator (Irgacure 184, Ciba) Tego wet 270: Tego leveling agent BYK350: BYK leveling agent 2-butanol Butyl alcohol IPA Isopropyl Alcohol XX-103BQ (2.0 μm, refractive index 1.515): Copolymer particles of polystyrene and polymethyl methacrylate (Sekisui Plastic product) XX-113BQ (2.0 μm, refractive index 1.555): Copolymer particles of polystyrene and polymethyl methacrylate (Sekisui Plastic product) MA-ST (30% in MeOH): Dispersion of nano-silica particles with a size of 10-15 nm in methyl alcohol (Nissan Chemical product)

[0102] (2) Production of coating solution (C) for forming low reflection layer A coating solution for forming a low reflection layer was prepared by diluting 100 g of trimethylolpropane triacrylate (TMPTA), 283 g of hollow silica nanoparticles (diameter range: about 42 nm to 66 nm, JSC Catalyst and Chemicals product), 59 g of solid silica nanoparticles (diameter range: about 12 nm to 19 nm), 115 g of a first fluorine-containing compound (X-71-1203M, ShinEtsu Co., Ltd.), 15.5 g of a second fluorine-containing compound (RS-537, DIC Co., Ltd.) and 10 g of an initiator (Irgacure 127, Ciba Co., Ltd.) in a MIBK (methyl isobutyl ketone) solvent to a solid content concentration of 3 wt %.

[0103] (2) Production of an optical laminate in which a hard coating layer is formed on a light-transmitting substrate 1) Measurement of the heat shrinkage ratio The ratio of the heat shrinkage rate in the MD direction to the heat shrinkage rate in the TD direction of the polyethylene terephthalate (PET) films used in each of the Examples and Comparative Examples was calculated by cutting each PET film into a size of 10 cm x 10 cm (width x length) and leaving it at 80°C for 30 minutes, and then determining the heat shrinkage rate (deformed length / initial length) in each of the MD and TD directions. PET1: Heat shrink ratio (MD / TD) is about 1 PET2: Heat shrink ratio (MD / TD) is about 0.5

[0104] 2) Manufacturing of optical laminates The prepared coating solutions (B1, B2) for forming hard coating layers were coated on the polyethylene terephthalate (PET) films shown in Tables 2 and 3 below using a #12 Mayer bar, then dried for 2 minutes at the temperatures shown in Tables 2 and 3 below, and cured with UV to form hard coating layers (coating thickness 5 μm). The UV lamp used was an H bulb, and the curing reaction was carried out under a nitrogen atmosphere. The UV light dose irradiated during curing was 150 mJ / cm. 2 It is.

[0105] The coating solution (C) for forming a low reflection layer was coated on the hard coating film using a #4 Mayer bar to a thickness of about 110 to 120 nm, and then dried and cured for 1 minute at the temperatures shown in Tables 2 and 3 below. During the curing, the dried coating was purged with nitrogen and was subjected to a radiation dose of 252 mJ / cm2. 2 The specimen was exposed to ultraviolet light of 1000 nm.

[0106] 3) Measurement of thermal shrinkage deformation value of optical laminate The optical laminate was cut into a length of 12 cm in each of the MD and TD directions of the polyethylene terephthalate (PET) film to prepare a sample for measuring thermal shrinkage deformation.

[0107] The prepared sample was left at 100° C. for 96 hours, and then the lengths in the MD and TD directions were measured to determine the thermal shrinkage deformation in each direction.

[0108] [General formula 2-1] Heat shrinkage deformation value in the first direction of the optical laminate (MD direction of PET) = Initial length of the optical laminate in the first direction (MD direction of PET) - Length of the optical laminate in the first direction (MD direction of PET) measured after exposure to a temperature of 100°C for 96 hours

[0109] [General formula 3-1] Thermal shrinkage deformation in the second direction (TD direction of PET) of the optical laminate = initial length of the optical laminate in the second direction (TD direction of PET) minus the length of the optical laminate in the second direction (TD direction of PET) measured after exposure to a temperature of 100° C. for 96 hours

[0110] Then, the ratio (R) of the thermal shrinkage deformation value of the optical laminate in the second direction (TD direction of PET) to the thermal shrinkage deformation value of the optical laminate in the first direction (MD direction of PET) was determined.

[0111] [General formula 1-1] Ratio (R) = Heat shrinkage deformation value in the second direction of the optical laminate (TD direction of PET) / Heat shrinkage deformation value in the first direction of the optical laminate (MD direction of PET)

[0112] Preparation Example 2: Preparation of coating solution for forming hard coating layer and preparation of polarizer having hard coating layer formed thereon (1) Preparation of coating solution (A) for forming hard coating layer A hard coating composition was prepared by uniformly mixing 28 g of trimethyloylpropane triacrylate, 2 g of KBE-403, 0.1 g of initiator KIP-100f, and 0.06 g of leveling agent (Tego wet 270).

[0113] [Examples and Comparative Examples: Production of Polarizing Plates and Liquid Crystal Panels] (1) Manufacture of polarizing plates A polyvinyl alcohol polarizer (thickness: 25 μm, manufactured by LG Chem) was bonded to the light-transmitting substrate side of the optical laminate manufactured in Manufacturing Example 1 using a UV adhesive, and then the coating solution (A) for forming the hard coating layer manufactured in the above-mentioned manufacturing example was applied to the opposite side of the light-transmitting substrate to a thickness of 7 μm, and the coating was dried under nitrogen purging and then subjected to a 500 mJ / cm 2 The hard coating layer was formed by irradiating the film with ultraviolet light of 1000 nm.

[0114] (2) Manufacturing samples for thermal shock evaluation The polarizing plate cut into a square with a side length of 10 cm is bonded to one side of a TV glass (12 cm wide, 12 cm long, 0.7 mm thick) using an adhesive to prepare a sample for thermal shock evaluation. At this time, the polarizing plate is cut so that the MD direction of the polarizer is parallel to one side of the square.

[0115] [Experimental example: Thermal shock evaluation] A thermal shock test was performed on the prepared polarizer and an evaluation sample having a bonded polarizer under the following conditions, and the following three items were measured and confirmed.

[0116] -Measurement conditions: The polarizing plate and the evaluation sample were placed vertically in a thermal shock chamber. The temperature was raised from room temperature to 80°C and left for 30 minutes, then the temperature was lowered to -30°C and left for 30 minutes, and then the temperature was adjusted to room temperature. This cycle was repeated 100 times in total.

[0117] (1) Number of cracks The cracks and gaps between the polarizers of the evaluation sample were checked with the naked eye, and the number of cracks having a length of 1 cm or more was counted.

[0118] (2) Air bubbles The number of bubbles having a diameter of 5 mm or more was counted by visually checking for bubbles generated between the polarizer and the protective film and between the polarizer and the hard coating layer of the evaluation sample.

[0119] (3) Apex float (mm), 10x10 / film The four corners of the polarizing plate sample were observed to observe lifting between the coating layer and the polarizer, peeling between the polarizer and the protective film, and peeling and warping between the hard coating and the adhesive layer. If lifting and warping occurred, the sample was placed flat on the bottom and the height of the warp from the bottom was measured to calculate the average.

[0120] [Table 2]

[0121] [Table 3]

[0122] As shown in Tables 2 and 3, the polarizer of the embodiment has a controlled thermal shrinkage ratio or thermal shrinkage deformation between the fine layers even when a temperature of 60°C or more is applied during the manufacturing process, and in particular, the ratio of the thermal shrinkage deformation in the second direction of the optical laminate perpendicular to the first direction to the thermal shrinkage deformation in the first direction is within 0.8 to 1.2. As a result, it is confirmed that the polarizer of the embodiment has a good warpage balance, and it is possible to prevent cracks in the polarizer and prevent light leakage in LCD devices. [Explanation of symbols]

[0123] 10 Light-transparent base material 20 Polarizer 30 Hard Coating Layer 40 Anti-reflective film 50 Adhesive layer 60 Adhesive layer 70 Liquid crystal cell 100 Polarizing Plate 200 LCD Panel

Claims

1. A polarizer having a thickness of 25 to 40 μm; A hard coating layer having a thickness of 10 μm or less formed on one side of the polarizer; and an optical laminate including a light-transmitting substrate formed on the other side of the polarizer; The light-transmitting substrate has a retardation (Rth) in a thickness direction of 3,000 nm or more measured at any one wavelength in a wavelength range of 400 nm to 800 nm; the light-transmitting substrate is a polyethylene terephthalate (PET) film; the hard coating layer is in contact with the polarizer, the ratio of the thickness of the hard coating layer to the thickness of the light-transmitting substrate is 0.02 to 0.25; the hard coating layer includes a binder resin; and organic fine particles having a particle size of 0.5 μm to 10 μm and inorganic fine particles having a particle size of 1 nm to 500 nm, the organic fine particles being dispersed in the binder resin; a second hard coating layer having a thickness of 1 to 100 μm formed on one surface of the light-transmitting substrate to face the polarizer; A ratio of a thermal shrinkage deformation value of the optical laminate in a second direction perpendicular to the first direction to a thermal shrinkage deformation value of the optical laminate in the first direction is 0.8 to 1.2; The thermal shrinkage deformation value of the optical laminate in the first direction and the thermal shrinkage deformation value of the optical laminate in the second direction are each a difference in length values ​​measured after exposing the optical laminate to a temperature of 100° C. for 96 hours for the initial lengths of the optical laminate in the first direction and the second direction, respectively; The first direction of the optical laminate is a machine direction (MD) of the light-transmitting substrate, The second direction of the optical laminate is the transverse direction (TD) of the light-transmitting substrate, Polarizing plate.

2. The moisture permeability of the light-transmitting substrate measured for 24 hours under conditions of 40° C. and 100% humidity is 100 g / m 2 2. The polarizing plate according to claim 1, wherein:

3. 3. The polarizing plate according to claim 1, wherein the light-transmitting substrate has a thickness of 10 to 150 [mu]m.

4. 4. The polarizing plate according to claim 1, wherein the combined thickness of the polarizer, the hard coating layer, and the light-transmitting substrate is 200 μm or less.

5. The polarizing plate of any one of claims 1 to 4, wherein the optical laminate further comprises a low refractive layer having a refractive index of 1.20 to 1.60 in a wavelength range of 380 nm to 780 nm, the low refractive layer being formed on another surface of the second hard coating layer.

6. 6. The polarizing plate according to claim 1, further comprising: an adhesive layer located between the polarizer and the light-transmitting substrate, the adhesive layer having a thickness of 0.1 μm to 5 μm.

7. A liquid crystal panel having a liquid crystal cell on at least one side thereof, the polarizing plate according to any one of claims 1 to 6 being formed thereon.

8. a polarizing plate according to any one of claims 1 to 6 formed on both sides of the liquid crystal cell, The liquid crystal panel of claim 7, wherein the two polarizing plates are positioned such that the MD direction of the polarizer of the polarizing plate formed on one side of the liquid crystal cell and the MD direction of the polarizer of the polarizing plate formed on the other side are perpendicular to each other.

9. A display device comprising the polarizing plate according to any one of claims 1 to 6.

Citation Information

Patent Citations

  • Optical functional film, manufacturing method of the same and polarizing plate using the same, and image display device

    JP2006251043A

  • Polarizing plate and image display device using the same

    JP2008107432A

  • Optical polyester film, and polarization plate and transparent conductive film using the same

    JP2015215593A

  • Polarizing film, polarizing plate, and liquid crystal panel

    JP2015222368A

  • Polarizing plate and display device including the same

    JP2015532459A