Toner, toner manufacturing method, and image reading method

The toner with gold nanorods of specific aspect ratios and light absorption peaks enhances near-infrared readability and visible light invisibility, addressing the limitations of existing toners in invisible printing.

JP7566656B2Active Publication Date: 2024-10-15CANON KK
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2021020061
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-02-10
Publication Date
2024-10-15
Estimated Expiration
2041-02-10

AI Technical Summary

Technical Problem

Existing toners used for invisible printing do not provide sufficient invisibility in the visible light region while maintaining readability in the near-infrared region.

Method used

The toner contains gold nanorods with a specific aspect ratio distribution peak of 6.0 to 13.0 for near-infrared readability and gold nanorods or additives with a light absorption peak of 580 to 650 nm for visible light invisibility, along with a binder resin and optional additives for image formation.

Benefits of technology

The toner achieves excellent readability in the near-infrared region and excellent invisibility in the visible light region, facilitating secure and high-quality invisible image formation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007566656000004
    Figure 0007566656000004
  • Figure 0007566656000001
    Figure 0007566656000001
  • Figure 0007566656000002
    Figure 0007566656000002
Patent Text Reader

Abstract

To provide toner with which an invisible image that may have excellent invisibility in a visible light region and may have excellent readability in a near-infrared region can be obtained.SOLUTION: There is provided toner which has a toner particle. The toner contains a gold nanorod. The gold nanorod contains: a gold nanorod A which has a peak in a range of 6.0-13.0 in an aspect ratio in measurement of an aspect ratio distribution; and a gold nanorod B which has a peak in a range of 1.6-2.6 in an aspect ratio in measurement of the aspect ratio distribution. When measuring a light absorption wavelength of the gold nanorod B, the toner has a peak in a range of 580-650 nm.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a toner, a method for producing a toner, and a method for reading an image. [Background technology]

[0002] In recent years, "invisible printing," which embeds invisible information into printed matter, has been attracting attention for the purpose of strengthening security, such as copyright protection and counterfeit prevention. Since invisible printing does not deteriorate in appearance even when it is overlaid on a visible image, it is possible to use the embedded information while maintaining the quality of normal printed matter, and is expected to be applied in many fields, including security.

[0003] For example, Patent Document 1 discloses that by incorporating specific metal nanorods in toner, it is possible to form invisible images without impairing the quality of visible images. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2007-219103 A [Patent Document 2] JP 2006-118036 A [Patent Document 3] JP 2006-169544 A [Non-patent literature]

[0005] [Non-Patent Document 1] Y. Yuhoka, J. Phys. Chem. B, 101, 6661 (1997) [Non-Patent Document 2] NR Janahoka, J. Phys. Chem. B, 105, 4065 (2001) [Non-Patent Document 3] Chem.Commun.(2003),pp.2376-2377. [Non-Patent Document 4] Li.S et al., Nano Res.4, 723-728(2011) Summary of the Invention [Problem to be solved by the invention]

[0006] As a result of the inventors' investigation into the toner described in Patent Document 1, they realized that further improvement was required with respect to the invisibility of images in the visible light region.

[0007] One aspect of the present disclosure is directed to providing a toner that can provide images that can have excellent readability in the near infrared region and excellent invisibility in the visible light region.

[0008] Another aspect of the present disclosure is directed to providing a method for producing the toner according to the present disclosure.

[0009] Another aspect of the present disclosure is directed to providing a method for reading an image formed using the toner according to the present disclosure. [Means for solving the problem]

[0010] According to one aspect of the present disclosure, there is provided a toner having toner particles, The toner contains gold nanorods, The gold nanorods are In the measurement of the aspect ratio distribution, gold nanorod A has a peak in the aspect ratio range of 6.0 to 13.0, and In the aspect ratio distribution measurement, gold nanorod B has a peak in the aspect ratio range of 1.6 to 2.6. When the optical absorption wavelength of the gold nanorod B is measured, it has a peak in the range of 580 to 650 nm. A toner is provided, which comprises:

[0011] According to another aspect of the present disclosure, there is provided a toner having toner particles, the toner comprising: the toner contains gold nanorods and an additive; when the aspect ratio distribution of the gold nanorods contained in the toner is measured, the aspect ratio has a peak in the range of 6.0 to 13.0; When the light absorption wavelength of the additive is measured, it has a peak in the range of 580 to 650 nm. A toner is provided, which comprises:

[0012] According to another aspect of the present disclosure, there is provided a method for producing a toner having toner particles, the method comprising the steps of: The method includes a step of obtaining toner particles containing gold nanorods A and gold nanorods B, When the aspect ratio distribution of the gold nanorod A is measured, the aspect ratio has a peak in the range of 6.0 to 13.0, When the aspect ratio distribution of the gold nanorod B is measured, the aspect ratio has a peak in the range of 1.6 to 2.6; When the optical absorption wavelength of the gold nanorod B is measured, it has a peak in the range of 580 to 650 nm. The present invention provides a method for producing a toner comprising the steps of:

[0013] According to another aspect of the present disclosure, there is provided a method for producing a toner having toner particles, the method comprising the steps of: The method includes obtaining toner particles containing gold nanorods and an additive, When the aspect ratio distribution of the gold nanorods is measured, the aspect ratio has a peak in the range of 6.0 to 13.0; When the light absorption wavelength of the additive is measured, it has a peak in the range of 580 to 650 nm. The present invention provides a method for producing a toner comprising the steps of:

[0014] According to another aspect of the present disclosure, there is provided an image reading method, comprising: There is provided an image reading method, comprising the step of reading an image formed using the toner of the present disclosure with a device equipped with a near-infrared sensor. Effect of the Invention

[0015] According to one aspect of the present disclosure, it is possible to provide a toner that can obtain an image that can have excellent readability in the near infrared region and excellent invisibility in the visible light region.

[0016] According to another aspect of the present disclosure, a method for producing the toner according to the present disclosure can be provided.

[0017] Further, another aspect of the present disclosure can provide a method for reading an image formed using the toner according to the present disclosure. [Brief description of the drawings]

[0018] [Figure 1] FIG. 2 is an explanatory diagram of a method for reading an image. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] The description of "xx or more and xx or less" or "xx to xx" expressing a numerical range means a numerical range including the lower and upper limits which are the endpoints, unless otherwise specified. When a numerical range is described in stages, the upper and lower limits of each numerical range can be arbitrarily combined.

[0020] The toner according to the present disclosure is preferably a toner for forming an invisible image.

[0021] <Background to the invention> When an image is formed using a toner containing gold nanorods, an image that can be read in the near infrared region is easily obtained. As a result of the inventors' investigations into this toner, they found that when a toner containing gold nanorods with an aspect ratio distribution peak controlled to 6.0 to 13.0 is used, the amount of light absorbed in the near infrared region is increased, and therefore excellent image readability can be obtained.

[0022] On the other hand, the present inventors have found that when a fixed image formed using a toner containing gold nanorods with a controlled aspect ratio as described above is visually observed, the image may be lightly colored. When the optical absorption spectrum of the fixed image was measured, it was found that the image exhibited maximum absorption in the near infrared region, but also had a small optical absorption peak near 530 nm, which led to the conclusion that a fixed image with a lightly colored image may be obtained. Naturally, a toner used to form an invisible image is required to be able to form an image that is difficult to see. Therefore, the present inventors have recognized that an improvement is necessary to make it difficult to see the color caused by the optical absorption near 530 nm.

[0023] As a result of intensive research, the present inventors have found that a toner containing gold nanorod A with an aspect ratio distribution peak controlled to 6.0 to 13.0 and material B with a light absorption peak at 580 to 650 nm is effective for forming an image with the above-mentioned characteristics. The speculated mechanism and each of the constituent elements will be described in detail below.

[0024] <Presumed mechanism by which the effects of this disclosure manifest> By incorporating gold nanorods A, which have a distribution peak in the aspect ratio range of 6.0 to 13.0, into the toner, light in the near-infrared region (1000 to 1600 nm) is absorbed, making it easier to obtain images with excellent readability in the near-infrared region.

[0025] In addition, while the above gold nanorod A also partially absorbs light around 530 nm, by containing material B, which has a light absorption peak at 580 to 650 nm, it becomes easier to obtain an image with flatter light absorption characteristics in the visible light region, i.e., an image with lower saturation and less visible.

[0026] In the present disclosure, specific examples of the material B include: (i) Gold nanorod B having a light absorption peak at 580 to 650 nm and a distribution peak in the aspect ratio range of 1.6 to 2.6 (ii) Additive B having a light absorption peak at 580 to 650 nm He lists the following as examples.

[0027] <Gold nanorods> The toner according to the present disclosure contains gold nanorods. Furthermore, gold nanorods are considered to be nanorods with a gold content of 80% or more.

[0028] The arrangement of gold and metal elements other than gold in the gold nanorods may be an alloy composite at the atomic level, or a core-shell structure in which a nanorod of gold alone is coated with a metal element other than gold. The gold nanorods may also be coated with a shell made of, for example, silica or polystyrene. Furthermore, the surface of the gold nanorods may be modified with appropriate molecules such as surfactants depending on the purpose, such as dispersing the gold nanorods in a medium.

[0029] Gold nanorods refer to gold nanomaterials that have a long axis and a short axis in a TEM image. That is, gold nanorods are observed as approximately rectangular in a TEM image. In general, the length of the short axis is 1 nm to 60 nm, and the length of the long axis is 20 nm to 500 nm. The value obtained by dividing the length of the long axis of a gold nanorod by the length of the short axis is called the aspect ratio. In the present disclosure, a gold nanorod is considered to have an aspect ratio of 1.5 or more.

[0030] <Gold nanorod A> The toner contains gold nanorods, and the gold nanorods have gold nanorods A that have a peak in the aspect ratio range of 6.0 to 13.0 in a measurement of the aspect ratio distribution.

[0031] Here, the peak wavelength at which the light absorption of gold nanorods having a peak in the aspect ratio range of 6.0 to 13.0 in the aspect ratio distribution is maximum is likely to be in the range of 1000 to 1600 nm, and shows excellent absorption properties for wavelengths in the near infrared region. That is, when the light absorption wavelength of gold nanorod A is measured, it is preferable that the peak is in the range of 1000 to 1600 nm. For this reason, the toner having the above gold nanorods makes it easy to obtain invisible images that can have excellent readability in the near infrared region.

[0032] The aspect ratio is more preferably 9.0 or more and 11.0 or less.

[0033] In addition, the standard deviation of the aspect ratio distribution of the gold nanorods A contained in the toner is preferably 4.5 or less, more preferably 3.5 or less, and even more preferably 2.0 or less. There is no particular lower limit, and it is preferably 0.5 or more.

[0034] <Content of Gold Nanorod A> The content of gold nanorods A in the toner is preferably 0.001 to 0.200% by mass. If it is 0.001% by mass or more, the invisible image is easily visualized when irradiated with infrared light, and an image with excellent readability is easily obtained. Therefore, it is preferably 0.001% by mass or more, and more preferably 0.005% by mass or more. Also, if it is 0.200% by mass or less, the volume resistivity of the toner is less likely to decrease, an invisible image with high quality is easily obtained, and readability in the near-infrared region is easily excellent. Therefore, it is preferably 0.200% by mass or less, more preferably 0.100% by mass or less, and even more preferably 0.050% by mass or less.

[0035] <Material B> As described above, it has been discovered that an image that is difficult to see can be easily obtained by adding toner not only the above-mentioned gold nanorods A but also material B having a light absorption peak at 580 to 650 nm. Specific examples of material B in this disclosure include the following gold nanorods B and additive B.

[0036] <Gold nanorod B> One embodiment of the above material B is the following gold nanorod B. That is, the toner according to one embodiment of the present disclosure contains gold nanorods B having a peak in the aspect ratio range of 1.6 to 2.6 in the aspect ratio distribution measurement, and has a peak in the range of 580 to 650 nm when the light absorption wavelength of the gold nanorods B is measured. The aspect ratio range is preferably 2.0 to 2.2.

[0037] Gold nanorods with controlled aspect ratios as described above are preferred as material B because they tend to have a peak light absorption wavelength in the range of 580 to 650 nm, and images with excellent invisibility in the visible light region are easily obtained.

[0038] In addition, the standard deviation of the aspect ratio distribution of the gold nanorods B contained in the toner is preferably 4.5 or less, more preferably 3.5 or less, and even more preferably 2.0 or less. There is no particular lower limit, and it is preferably 0.5 or more.

[0039] From the viewpoint of invisibility in the visible light region and readability in the near infrared region, the mass ratio of gold nanorods A and gold nanorods B contained in the toner is preferably (0.99 / 0.01) to (0.85 / 0.15).

[0040] <Additive B> Another embodiment of the above material B is an additive (hereinafter also referred to as additive B) having a light absorption wavelength peak in the range of 580 to 650 nm. That is, a toner according to one embodiment of the present disclosure contains an additive, and when the light absorption wavelength of the additive is measured, the additive has a peak in the range of 580 to 650 nm.

[0041] From the viewpoint of invisibility in the visible light region and readability in the near infrared region, the mass ratio of the gold nanorods A to the additive B is preferably from (0.99 / 0.01) to (0.95 / 0.05).

[0042] As additive B having a light absorption peak wavelength in the range of 580 nm to 650 nm, a colorant for cyan toner or a colorant for magenta toner that satisfies the above can be used, with a colorant for cyan toner being more preferred.

[0043] Pigments for cyan toners include the following: CI Pigment Blue 2, 3, 15:2, 15:3, 15:4, 16, 17; CI Vat Blue 6; CI Acid Blue 45; copper phthalocyanine pigments having 1 to 5 phthalimidomethyl groups substituted on the phthalocyanine skeleton.

[0044] Dyes for cyan toners include CI Solvent Blue 70.

[0045] Magenta toner pigments include the following: CI Pigment Red 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 21, 22, 23, 30, 31, 32, 37, 38, 39, 40, 41, 48:2, 48:3, 48:4, 49, 50, 51, 52, 53, 54, 55, 57:1, 58, 60, 63, 64, 68, 81:1, 83, 87, 88, 89, 90, 112, 114, 122, 123, 146, 147, 150, 163, 184, 202, 206, 207, 209, 238, 269, 282; CI Pigment Violet 19; CI Bat Red 1, 2, 10, 13, 15, 23, 29, 35.

[0046] Dyes for magenta toners include solvent dyes such as CI Solvent Red 1, 3, 8, 23, 24, 25, 27, 30, 49, 81, 82, 83, 84, 100, 109, 121; CI Disperse Red 9; CI Solvent Violet 8, 13, 14, 21, 27; CI Disperse Violet 1; basic dyes such as CI Basic Red 1, 2, 9, 12, 13, 14, 15, 17, 18, 22, 23, 24, 27, 29, 32, 34, 35, 36, 37, 38, 39, 40; and CI Basic Violet 1, 3, 7, 10, 14, 15, 21, 25, 26, 27, 28.

[0047] In order to adjust the chromaticity, a colorant for yellow toner may be contained.

[0048] Yellow toner pigments include: CI Pigment Yellow 1, 2, 3, 4, 5, 6, 7, 10, 11, 12, 13, 14, 15, 16, 17, 23, 62, 65, 73, 74, 83, 93, 94, 95, 97, 109, 110, 111, 120, 127, 128, 129, 147, 151, 154, 155, 168, 174, 175, 176, 180, 181, 185; CI Vat Yellow 1, 3, 20.

[0049] Yellow toner dyes include CI Solvent Yellow 162.

[0050] Although a pigment may be used alone, it is more preferable to use a dye and a pigment in combination to improve the clarity of the color from the viewpoint of adjusting the chromaticity.

[0051] <Gold nanoparticles> It is preferable that the toner does not contain gold nanoparticles, or contains gold nanoparticles at a ratio of 30% or less by number relative to the number of gold nanorods. In the present disclosure, gold nanoparticles are treated as metal nanoparticles whose main component is gold. Metal nanoparticles are treated as nanoparticles whose aspect ratio is less than 1.5. Gold nanoparticles may be generated during the preparation of gold nanorods. Gold nanoparticles also exhibit absorption in the visible light region according to their particle size. For example, when the particle size is 20 nm, they exhibit light absorption around 520 nm. When the amount of gold nanoparticles in the toner is small, the light absorption rate in the visible light region corresponding to the absorption wavelength of the gold nanoparticles is small, and images with excellent invisibility are easily obtained.

[0052] The proportion of gold nanoparticles can be controlled by the reaction conditions and purification conditions described below.

[0053] <Preparation method of gold nanorods> Methods for preparing gold nanorods include electrolytic methods (Non-Patent Document 1) and chemical synthesis methods (Non-Patent Document 2).

[0054] For example, a method of synthesizing gold nanorod particles by reducing gold ions in an aqueous solution containing an excess of cetyltrimethylammonium bromide (CTAB), a quaternary ammonium salt, can be used. For details of this method, for example, Patent Document 2, Patent Document 3, Non-Patent Document 3, etc. can be referred to. In this method, first, an aqueous solution of CTAB is added to an aqueous solution of chloroauric acid tetrahydrate, and sodium borohydride is added to prepare a solution having seed particles. A solution of silver nitrate, chloroauric acid tetrahydrate, L-ascorbic acid, and CTAB is added to the solution and held for a certain period of time, or the solution is added little by little, which makes it easy to anisotropically grow seed particles as nuclei, and gold nanorods are obtained.

[0055] In addition, gold nanorods with a large aspect ratio can be obtained by adding benzyldimethylhexadecylammonium chloride when growing seed particles. In addition, gold nanorods with a large aspect ratio can be obtained by performing reduction with sodium borohydride, a strong reducing agent, in the first step, followed by reduction with triethylamine, a weak reducing agent.

[0056] Furthermore, the gold nanorods can be purified as necessary to adjust the aspect ratio distribution before use. Any of the commonly known methods can be used for purification, for example, density gradient ultracentrifugation. For details of this method, see, for example, Non-Patent Document 4. Specifically, first, mixed solutions of sucrose and CTAB with different concentrations are prepared and layered in a centrifuge tube in order of concentration gradient. A sample of gold nanorods is layered on top of this and centrifuged to separate them according to density and size. By separating and purifying in this way, the above-mentioned standard deviation σ is reduced, and gold nanorods with a narrower aspect ratio distribution can be obtained.

[0057] <Toner and toner particles> The toner particles preferably contain a binder resin. The binder resin is not particularly limited, and specific examples include vinyl resins, polyester resins, and epoxy resins, which can be used alone or in combination. The binder resin may be any of a resin having a linear molecular structure, a branched resin, and a crosslinked resin, or a mixture of these.

[0058] <Light absorptance in the near infrared region> The toner load is 0.30 mg / cm 2 In the spectroscopic analysis of the fixed image formed as above, it is preferable that the maximum light absorptance in the wavelength range of 900 nm to 1800 nm is 3% or more. This wavelength range corresponds to the near-infrared region, and if the light absorptance is 3% or more, it is easy to read the invisible image using a near-infrared camera or the like. It is more preferable that it is 10% or more, and even more preferable that it is 15% or more.

[0059] The above absorption rate can be controlled by adjusting the aspect ratio distribution of the gold nanorods.

[0060] <Weight average particle size of toner particles (D4)> The weight average particle diameter (D4) of the toner particles is preferably from 4.0 μm to 9.0 μm, more preferably from 5.0 μm to 7.0 μm, which is advantageous for forming high-definition images.

[0061] <Toner manufacturing method> The method for producing the toner is not particularly limited, but in one embodiment, it is preferable to include a step of obtaining toner particles containing the gold nanorods A and the gold nanorods B. In another embodiment, it is preferable to include a step of obtaining toner particles containing the gold nanorods A and the additive B.

[0062] Examples of the toner production method include the following toner production methods (1) to (3).

[0063] (1) Crushing method When producing toner by the pulverization method, first, gold nanorods are thoroughly mixed with a binder resin, which is a dispersion medium, and other additives using a mixer such as a Henschel mixer or a ball mill. The mixture is melted and kneaded using a thermal kneader that uses heat and mechanical shear force, such as a kneader or an extruder, to make the resins compatible with each other. The molten and kneaded mixture is cooled and solidified, and then the solidified product is pulverized and classified to obtain toner particles of the desired particle size.

[0064] (2) Polymerization method In the polymerization method, for example, gold nanorods, a polymerizable monomer capable of forming a binder resin, and optionally a polymerization initiator, a crosslinking agent, a charge control agent, and other additives are uniformly dispersed to obtain a polymerizable monomer composition. The obtained polymerizable monomer composition is then dispersed and granulated in a continuous layer (e.g., an aqueous phase) containing a dispersion stabilizer using an appropriate stirrer, and a polymerization reaction is carried out using a polymerization initiator to obtain toner particles having a desired particle size.

[0065] (3) Emulsion aggregation method When producing a toner by the emulsion aggregation method, first, materials such as gold nanorods, binder resin, and other additives are dispersed and mixed in an aqueous medium containing a dispersion stabilizer. A surfactant may be added to the aqueous medium. Then, an aggregating agent is added to aggregate the particles until the desired toner particle size is obtained, and then or simultaneously with the aggregation, the resin particles are fused together. If necessary, the shape is controlled by heat to form toner particles. Then, the toner particles are obtained through a filtration, washing, and drying process.

[0066] Furthermore, if necessary, a process for dispersing gold nanorods in a binder resin may be included in the series of toner production processes.

[0067] An example of a method for dispersing gold nanorods in a binder resin is a method using a masterbatch in a toner manufacturing process. That is, gold nanorods are mixed with a part of the binder resin so as to have a high concentration, and are melt-kneaded under high shear to produce a masterbatch in which the gold nanorods are finely dispersed. Then, the masterbatch is melt-kneaded while being diluted with the remaining binder resin. Examples of melt-kneading devices suitable for use in producing a masterbatch include a kneader, a Banbury mixer, a two-roll mill, and a three-roll mill, and these can be used alone or in combination. Examples of melt-kneading devices used in dilution kneading include a twin-screw kneader.

[0068] If necessary, a process for suppressing aggregation of gold nanorod particles may be provided during the toner production process.

[0069] An example of a method for suppressing the aggregation of gold nanorod particles during toner production is a method of rapidly cooling after the melt-kneading process. For example, the melt-kneaded material can be rapidly cooled by spreading it into a sheet on a water-cooled metal belt. Rapid cooling can suppress the aggregation of gold nanorods that occurs during cooling. Examples of suitable cooling devices for rapid cooling include the "High Viscosity NR Double Belt Cooler (manufactured by Nippon Belting Co., Ltd.)," the "Cooling Solidification Machine Belt Drum Flaker (manufactured by Nippon Coke and Engineering Co., Ltd.)," and the "Cooling Solidification Device Drum Flaker (manufactured by Katsuragi Kogyo Co., Ltd.)."

[0070] The step of dispersing gold nanorod particles in a binder resin and the method of suppressing aggregation of the gold nanorod particles may be used in combination.

[0071] <How to read an image> The method for reading an image formed using the toner according to the present disclosure is not particularly limited. Since an image formed using the toner according to the present disclosure is prone to absorbing wavelengths in the near infrared region, an image reading method using light with a wavelength of 900 to 2500 nm is preferred. More preferably, the wavelength is 900 to 1800 nm.

[0072] In addition, since light of that wavelength is easy to read, the image reading method is preferably an image reading method using a device equipped with a near-infrared sensor, more preferably an image reading method using a device equipped with an InGaAs sensor, and more preferably an InGaAs camera.

[0073] As an example of a method for reading an image, the operations carried out by the present inventors are shown below.

[0074] After forming an evaluation image using the toner according to the present disclosure, a light source 202 and a camera 203 were installed as shown in FIG. 1, and the evaluation image 201 was observed. That is, the evaluation image was placed on a desk, and infrared rays were irradiated from a distance of about 1 m at an angle of 15° to the evaluation image using the light source 202. In addition, the camera 203 was installed 15 cm directly above the evaluation image, and an image was taken. As the light source 202, a halogen lamp light source (product name: PCS-UHX-150, manufactured by Japan PI Corporation) equipped with a visible light cut filter unit was used. As the camera 203, a near-infrared camera (product name: NVU3VD, manufactured by IR Spec, InGaAs camera) with a filter for cutting wavelength components of 800 nm or less attached to the lens was used. The spectral sensitivity wavelength range of the near-infrared camera was 970 to 1650 nm.

[0075] <Various additives> The toner may contain, as necessary, one or more additives selected from wax, charge control agents, external additives, and the like.

[0076] <Wax> The wax is not particularly limited, but colorless or light-colored waxes are preferred, and examples thereof include the following.

[0077] Hydrocarbon wax, ester wax, amide wax, higher aliphatic alcohol, higher fatty acid, etc. One type of wax may be used alone, or multiple types may be used in combination.

[0078] <Charge control agent> The charge control agent is not particularly limited, but colorless or light-colored charge control agents are preferred, and examples thereof include the following.

[0079] Aromatic oxycarboxylic acids, metal compounds of aromatic oxycarboxylic acids, boron compounds, quaternary ammonium salts, calixarenes, resins having sulfonic acid (salt) groups, resins having sulfonic acid ester groups, etc. The charge control agents may be used alone or in combination.

[0080] <External additives> The external additive is not particularly limited, but colorless or light-colored ones are preferable, and the followings can be mentioned.

[0081] Silica, alumina, titanium oxide, strontium titanate, silicon nitride, polytetrafluoroethylene, zinc stearate, etc. The surface of the external additive may be subjected to a hydrophobic treatment.

[0082] Moreover, the average particle size of the primary particles of the external additive is preferably 1 / 10 or less of the weight average particle size (D4) of the toner particles.

[0083] <Developer> The toner can be used as a one-component developer, but may also be mixed with a carrier to be used as a two-component developer. As the carrier, magnetic particles made of known materials such as metals such as iron, ferrite, and magnetite, and alloys of these metals with metals such as aluminum and lead, can be used. In addition, a coated carrier in which the surface of the carrier is coated with a coating agent such as a resin, or a resin-dispersed carrier in which magnetic particles are dispersed in a binder resin may also be used. The volume average particle diameter of the carrier is preferably 15 μm or more and 100 μm or less, more preferably 25 μm or more and 80 μm or less.

[0084] <Various measurement methods, etc.> Various measurement methods etc. are described below.

[0085] <Method of measuring weight average particle size (D4) of toner particles> The weight average particle size (D4) of the toner particles is calculated as follows.

[0086] The measurement device used is a precision particle size distribution measurement device using the pore electrical resistance method, "Coulter Counter Multisizer 3" (registered trademark, manufactured by Beckman Coulter, Inc.), equipped with a 100 μm aperture tube. The measurement conditions are set and the measurement data is analyzed using the accompanying dedicated software "Beckman Coulter Multisizer 3 Version 3.51" (manufactured by Beckman Coulter, Inc.). The measurement is performed with an effective measurement channel count of 25,000.

[0087] The aqueous electrolyte solution used for the measurement can be prepared by dissolving special grade sodium chloride in ion-exchanged water to a concentration of approximately 1% by mass, for example, "ISOTON II" (manufactured by Beckman Coulter).

[0088] Before performing measurements and analysis, the dedicated software is set up as follows.

[0089] In the "Change Standard Measurement Method (SOM)" screen of the dedicated software, set the total count number in the control mode to 50,000 particles, the number of measurements to 1, and the Kd value to the value obtained using "Standard particle 10.0 μm" (Beckman Coulter). Press the "Threshold / Noise Level Measurement Button" to automatically set the threshold and noise level. In addition, set the current to 1600 μA, the gain to 2, the electrolyte to ISOTON II, and check "Flush aperture tube after measurement." In the "Pulse to particle size conversion setting" screen of the dedicated software, set the bin interval to logarithmic particle size, the particle size bin to 256 particle size bin, and the particle size range to 2 μm to 60 μm.

[0090] The specific measurement method is as follows.

[0091] (1) Pour about 200 mL of the above electrolyte solution into a 250 mL round-bottom glass beaker made exclusively for the Multisizer 3, set it on the sample stand, and stir the stirrer rod counterclockwise at 24 revolutions per second. Then, use the "aperture flush" function of the dedicated software to remove dirt and air bubbles from inside the aperture tube.

[0092] (2) Place about 30 mL of the above electrolyte solution in a 100 mL flat-bottom glass beaker. Add about 0.3 mL of a solution of "Contaminon N" (a 10% aqueous solution of a pH 7 neutral detergent for cleaning precision measuring instruments made of nonionic surfactants, anionic surfactants, and organic builders, manufactured by Fujifilm Wako Pure Chemical Industries) diluted about 3 times by mass with ion-exchanged water as a dispersant.

[0093] (3) Prepare an ultrasonic disperser "Ultrasonic Dispersion System Tetora150" (manufactured by Nikkaki Bios Co., Ltd.) that has two built-in oscillators with an oscillation frequency of 50 kHz and a phase shift of 180 degrees, and has an electrical output of 120 W. Place approximately 3.3 L of ion-exchanged water in the ultrasonic disperser's water tank, and add approximately 2 mL of Contaminon N to this water tank.

[0094] (4) The beaker (2) is set in the beaker fixing hole of the ultrasonic disperser, and the ultrasonic disperser is operated. Then, the height position of the beaker is adjusted so that the resonance state of the liquid surface of the electrolyte solution in the beaker is maximized.

[0095] (5) While the electrolyte solution in the beaker in (4) is irradiated with ultrasonic waves, about 10 mg of toner particles are added little by little to the electrolyte solution and dispersed. Then, ultrasonic dispersion treatment is continued for another 60 seconds. During ultrasonic dispersion, the water temperature in the water tank is appropriately adjusted to be 10°C or higher and 40°C or lower.

[0096] (6) Using a pipette, add the electrolyte solution (5) in which the toner particles are dispersed to the round-bottom beaker (1) placed in the sample stand, and adjust the measurement concentration to about 5%. Then, measurements are continued until the number of particles measured reaches 50,000.

[0097] (7) The measurement data is analyzed using the dedicated software that comes with the device, and the weight-average particle size (D4) is calculated. Note that when the dedicated software is set to Graph / Volume%, the "Average diameter" on the "Analysis / Volume Statistics (Arithmetic Mean)" screen is the weight-average particle size (D4).

[0098] <Method for measuring peak aspect ratio and standard deviation in aspect ratio distribution of gold nanorods> A measurement sample in which gold nanorods are dispersed in a solvent is dropped onto a support film and dried, and then TEM observation is performed using a transmission electron microscope such as the Technai F30 (manufactured by FEI). The peak aspect ratio and standard deviation in the aspect ratio distribution can be obtained by determining the lengths of the long and short axes of the observed gold nanorods using image processing software such as Photoshop.

[0099] When measuring the aspect ratio distribution of the gold nanorods contained in the toner, the gold nanorods contained in the toner are separated and collected before the above measurement.

[0100] The procedure is as follows: first, the toner is dissolved using a solvent capable of dissolving the binder resin. Next, the gold nanorods are allowed to settle by centrifugation, and the supernatant liquid is separated. New solvent is added and the centrifugation is repeated to separate the supernatant liquid. This process is repeated several times for washing, and finally the solvent is dried and removed, allowing the gold nanorods to be separated and recovered from the toner. The mass can also be measured before redispersing in the solvent. EXAMPLES

[0101] The present disclosure will be described in more detail below with reference to examples, but the present disclosure is not limited thereto.

[0102] <Production Example of Dispersion A Containing Gold Nanorods A According to the Present Disclosure> [Preparation of seed particle solution] 500 mL of a 0.0005 mol / L aqueous solution of chloroauric acid tetrahydrate (Kishida Chemical Co., Ltd.) was mixed with 500 mL of a 0.2 mol / L aqueous solution of cetyltrimethylammonium bromide (Kishida Chemical Co., Ltd.). 60 mL of 0.01 mol / L sodium borohydride (Tokyo Chemical Industry Co., Ltd.) was added to this aqueous solution to obtain a seed particle solution (Solution A).

[0103] [Step a] 10 g of cetyltrimethylammonium bromide was dissolved in 500 mL of 0.15 mol / L benzyldimethylhexadecylammonium chloride (Tokyo Chemical Industry Co., Ltd.) aqueous solution. 20 mL of 0.004 mol / L silver nitrate aqueous solution was added to the aqueous solution containing these two types of surfactants. 500 mL of 0.001 mol / L chloroauric acid tetrahydrate aqueous solution was added to this aqueous solution, and then 7 mL of 0.078 mol / L L-ascorbic acid aqueous solution (Kishida Chemical Co., Ltd.) was added. This solution was designated as solution B.

[0104] Next, 10 g of cetyltrimethylammonium bromide was dissolved in 500 mL of 0.15 mol / L benzyldimethylhexadecylammonium chloride (Tokyo Chemical Industry Co., Ltd.) aqueous solution. 20 mL of 0.004 mol / L silver nitrate aqueous solution was added to the aqueous solution containing these two types of surfactants. 500 mL of 0.0005 mol / L chloroauric acid tetrahydrate aqueous solution was added to this aqueous solution, and then 3.6 mL of 0.078 mol / L L-ascorbic acid aqueous solution (Kishida Chemical Co., Ltd.) was added. This solution was named solution C.

[0105] 1.2 mL of solution A was dropped into solution B, followed by the addition of 2.0 mL of solution C at a rate of 1.0 mL / 20 min, to anisotropically grow seed particles as nuclei. After centrifugation at 10,000×g for 5 min, the mixture was redispersed in THF to 99.98 parts by mass of THF and 0.02 parts by mass of gold nanorods, to obtain a particle dispersion.

[0106] [Refining process] 6 mL of the resulting particle dispersion was centrifuged at 10,000×g for 5 minutes, and the resulting pellet was resuspended in 0.05 mL of 0.01 M aqueous CTAB solution.

[0107] In addition, solutions were prepared by adding sucrose to a 0.01M CTAB solution to make 10 wt%, 15 wt%, 20 wt%, and 25 wt%. These solutions were layered in a 15-mL polyallomer tube in 3 mL portions in ascending order of sucrose concentration, and the resuspended particle dispersion was layered on top of each other. The solution was centrifuged at 25°C and 10,750 x g for 15 minutes using a high-speed refrigerated centrifuge Avanti JXN-30. After centrifugation, the solution was divided into fractions of 300 μL each. TEM images of the gold nanorods in each fraction were measured. The aspect ratio and standard deviation calculated from the TEM images of each fraction were confirmed, and the desired fractions were collected, and the collected solution was centrifuged at 10,000 x g for 5 minutes. The precipitate, the gold nanorods, were redispersed in a dispersion medium (THF) so that the gold nanorods were 0.02 parts by mass, and the final concentrations were 99.98 parts by mass of THF and 0.02 parts by mass of gold nanorods. In this way, dispersion A was prepared. The physical properties of the gold nanorods contained in dispersion A are shown in Table 1.

[0108] <Production Examples of Dispersions B to F Containing Gold Nanorods A According to the Present Disclosure> Dispersions B to F were obtained by carrying out the same operations as in the production example of dispersion A, except that the peak aspect ratio and standard deviation were changed as shown in Table 1 by adjusting the amount of solution C in step a, whether or not a purification step was performed, and which fractions were collected in the purification step. The physical properties of the gold nanorods contained in the dispersions are shown in Table 1.

[0109] However, for Dispersion D, styrene was used instead of THF as the final dispersion medium, and the final concentrations were 99.9 parts by mass of styrene and 0.1 parts by mass of gold nanorods.

[0110] <Production Example of Dispersion G Containing Gold Nanorods B According to the Present Disclosure> [Preparation of seed particle solution] First, a seed particle solution (Solution A) similar to that described above was prepared.

[0111] [Step b] 3.8 mL of 0.004 mol / L silver nitrate (Kishida Chemical Co., Ltd.) aqueous solution was added to 500 mL of 0.2 mol / L cetyltrimethylammonium bromide aqueous solution. 500 mL of 0.001 mol / L chloroauric acid tetrahydrate aqueous solution was added to this aqueous solution, and then 7 mL of 0.078 mol / L L-ascorbic acid aqueous solution (Kishida Chemical Co., Ltd.) was added. This solution was designated as solution B.

[0112] Then, 1.2 mL of solution A was dropped into solution B. This solution was kept at 30° C. for 20 minutes, and seed particles serving as nuclei were grown anisotropically to obtain a particle dispersion.

[0113] [Refining process] The same operation as in the purification step in the production example of Dispersion A was carried out using the particle dispersion obtained in step b to prepare Dispersion G. The physical properties of the gold nanorods contained in Dispersion G are shown in Table 1.

[0114] <Production Examples of Dispersions H to O Containing Gold Nanorods B According to the Present Disclosure> Dispersions H to O were obtained by carrying out the same operations as in the production example of dispersion G, except that the peak aspect ratio and standard deviation were changed as shown in Table 1 by adjusting the amount of silver nitrate aqueous solution added in step b and which fractions were recovered in the purification step. The physical properties of the gold nanorods contained in each dispersion are shown in Table 1.

[0115] However, for Dispersion O, styrene was used instead of THF as the final dispersion medium, and the final concentrations were 99.9 parts by mass of styrene and 0.1 parts by mass of gold nanorods.

[0116] <Production Example of Dispersion P Containing Additive B According to the Present Disclosure> Pigment (CI Pigment Blue 15:3) 1000 parts by weight Anionic surfactant 150 parts by weight Ion-exchanged water 9,000 parts by weight The above materials were mixed and dissolved, and then dispersed using a high-pressure impact disperser to obtain dispersion P. The physical properties of the pigment contained in the dispersion are shown in Table 1.

[0117] <Production Examples of Comparative Dispersions Q to T> Dispersions Q to T were obtained by carrying out the same operations as in the production example of dispersion G, except that the peak aspect ratio and standard deviation were changed as shown in Table 1 by adjusting the amount of silver nitrate aqueous solution added in step b and which fractions were recovered in the purification step. The physical properties of the gold nanorods contained in each dispersion are shown in Table 1.

[0118] [Table 1]

[0119] The peak aspect ratios and standard deviations in the aspect ratio distribution in Table 1 were measured by the measurement method described above.

[0120] Those with a peak light absorption wavelength in the range of 400 to 800 nm were measured using an ultraviolet, visible, near-infrared spectrophotometer (product name: UV-3600, manufactured by Shimadzu Corporation), and those with a peak light absorption wavelength in the range of 900 to 1800 nm were measured using an ultraviolet, visible, near-infrared spectrophotometer (product name: MV-3300, manufactured by JASCO Corporation).

[0121] <Example 1> <Production Example of Toner 1 (Melt Kneading Method)> [Production example of saturated polyester 1 dispersion] Saturated polyester 1 (polycondensate of ethylene oxide-modified bisphenol A and terephthalic acid, glass transition temperature 60°C, weight average molecular weight 29000, number average molecular weight 6000) 20.0 parts by mass ·THF 80.0 parts by mass The above materials were thoroughly mixed to obtain a saturated polyester 1 dispersion.

[0122] [Production Example of Toner Particle 1] ·Dispersion liquid I 2.0 parts by mass ·Dispersion B 31.0 parts by mass Saturated polyester 1 dispersion 67.0 parts by weight The above materials were thoroughly stirred using a magnetic stirrer, and reprecipitated by dropping them into heptane (Kishida Chemical Co., Ltd.). The precipitate was collected by suction filtration to obtain a mixture of gold nanorods and saturated polyester in powder form. 5.0 parts by mass of ester wax (melting point 73°C) was added to 100 parts by mass of this mixture, and the above materials were thoroughly mixed using an FM mixer (Nippon Coke Engineering Co., Ltd.), and then melt-kneaded using a PCM-30 type (Ikegai Co., Ltd.) set at a temperature of 130°C to obtain a kneaded product. The kneaded product obtained was spread in a sheet shape on a water-cooled metal belt and quenched, and then coarsely crushed to 1 mm or less using a hammer mill to obtain a coarsely crushed product. The obtained coarsely crushed product was finely crushed using a T-250 (Freund Turbo Co., Ltd.). It was further classified using a 200TSP (Hosokawa Micron Co., Ltd.), and toner particles 1 with a weight average particle size (D4) of 5.9 μm were obtained.

[0123] [External addition process] 100.0 parts by mass of the obtained toner particles 1 and 1.0 part by mass of hydrophobic silica fine powder (primary particle number average particle size 7 nm) surface-treated with hexamethyldisilazane were mixed using an FM mixer (manufactured by Nippon Coke and Engineering Co., Ltd.) to obtain toner 1.

[0124] [evaluation] Next, the obtained toner 1 was subjected to the following evaluations.

[0125] <Evaluation of invisibility in the visible light region> <Method for measuring light absorptance in the wavelength range of 400 nm to 800 nm> The image forming apparatus used was a color printer (product name: LBP652C, manufactured by Canon Inc.) that had been modified so that the development contrast could be freely changed, and the toner in the black developing unit was replaced with Toner 1. A4 size paper (product name: GF-C081, manufactured by Canon Marketing Japan Inc.) was used as the paper, and the amount of Toner 1 applied was 0.30 mg / cm2 in an environment of 25°C temperature and 60% relative humidity. 2A rectangular image of 1 cm x 10 cm was formed so as to obtain a sample image.

[0126] The image outputted as above was visually inspected and the invisibility was evaluated.

[0127] The evaluation criteria are as follows: A: Difficult to distinguish rectangular images B: Rectangular images are somewhat difficult to distinguish. C: Rectangular images are neither easy nor difficult to distinguish. D: Rectangular images are somewhat easy to distinguish. E: Rectangular images are easy to distinguish In the above evaluation criteria, those that received a rating of A or B were judged to have excellent invisibility.

[0128] <Evaluation of readability in the near infrared region> <Method for measuring light absorptance in the wavelength range of 900 nm to 1800 nm> The sample images used in the above invisibility evaluation were subjected to spectroscopic analysis measurement in the wavelength range of 900 nm to 1800 nm using an ultraviolet-visible near-infrared spectrophotometer (product name: MV-3300, manufactured by JASCO Corporation). The maximum absorptivity obtained from the measurement was taken as the measured value of the sample image. A measurement was also performed on a sheet of paper alone as a blank, and the value obtained by subtracting the measured value of the blank from the measured value of the sample image was taken as the infrared absorptivity (%), and this value was used to evaluate the readability of the toner 1. The results are shown in Table 3. It was determined that the effect of the present disclosure was obtained when the infrared absorptivity (%) was 3% or more. When an image with an infrared absorptivity of 3% was confirmed using a near-infrared camera (product name: NVU3VD, manufactured by IR Spec Co., Ltd.), it was found to be readable as an invisible image. On the other hand, when an image with an infrared absorptivity of 2% was confirmed using the above near-infrared camera, it was determined that it exceeded the level at which it could be read as an invisible image.

[0129] <Examples 2 to 10, 12 to 14> Toners 2 to 10 and 12 to 14 were produced and evaluated in the same manner as in Example 1, except that the type and amount of the dispersion liquid were changed as shown in Table 2. The evaluation results are shown in Table 3.

[0130] <Example 11> <Production Example of Toner 11 (Polymerization Method)> [Preparation of aqueous medium] A reaction vessel was charged with 1000.0 parts by mass of ion-exchanged water and 14.0 parts by mass of sodium phosphate 12-hydrate, and the mixture was kept at 65° C. for 1 hour while purging with nitrogen.

[0131] The mixture was stirred at 12,000 rpm using a high-speed stirrer "TK Homomixer" (manufactured by Primix Corporation). An aqueous calcium chloride solution, in which 9.2 parts by mass of calcium chloride dihydrate was dissolved in 20.0 parts by mass of ion-exchanged water, was added all at once to prepare an aqueous medium containing fine dispersion stabilizers.

[0132] [Preparation process of polymerizable monomer composition] The following materials were mixed to obtain a mixture. ·Dispersion liquid O 2.8 parts by mass ·Dispersion liquid D 42.0 parts by mass Styrene 128.9 parts by weight n-Butyl acrylate 34.0 parts by weight Aluminum salicylate compound (Bontron E-88, manufactured by Orient Chemical Industry Co., Ltd.) 1.0 part by mass Saturated polyester 2 (polycondensation product of propylene oxide modified bisphenol A and isophthalic acid, glass transition temperature 65°C, weight average molecular weight 10000, number average molecular weight 6000) 5.0 parts by mass Ester wax (peak temperature of maximum endothermic peak in DSC measurement = 70°C, Mn = 704) 10.0 parts by mass Divinylbenzene 0.1 parts by weight This mixture was kept at 65° C. and was dissolved and dispersed uniformly at 500 rpm using a TK homomixer to prepare a polymerizable monomer composition.

[0133] [Granulation process] The temperature of the aqueous medium containing the dispersion stabilizer was set to 70°C, and the rotation speed of the TK homomixer was kept at 12000 rpm, while the polymerizable monomer composition was added to the aqueous medium, and 10.0 parts by mass of t-butyl peroxypivalate, which is a polymerization initiator, was added. After that, the mixture was granulated for 10 minutes while maintaining the rotation speed at 12000 rpm.

[0134] [Polymerization process] After the granulation step, the agitator was replaced with a propeller agitator and the mixture was stirred at 150 rpm while maintaining the temperature at 70° C. for 5 hours to polymerize. The temperature was then raised to 85° C. and heated for 2 hours to complete the polymerization reaction.

[0135] [Washing and drying process] After the polymerization process was completed, the liquid temperature was cooled to room temperature, and diluted hydrochloric acid was added to adjust the pH to 1.5, followed by stirring for 3 hours. Thereafter, filtration and washing were repeated to obtain a toner cake.

[0136] The obtained toner cake was crushed, dried in an airflow dryer, and further, fine and coarse powder was removed using a multi-division classifier utilizing the Coanda effect, to obtain toner particles 11 having a weight average particle size (D4) of 6.3 μm.

[0137] [External addition process] 100.0 parts by mass of the obtained toner particles 11 were mixed with 1.0 part by mass of hydrophobic silica fine powder (primary particle number average particle size 7 nm) surface-treated with hexamethyldisilazane using a high-speed mixer "FM Mixer" (manufactured by Nippon Coke and Engineering Co., Ltd.) to obtain toner 11.

[0138] [evaluation] The obtained toner 11 was used for the same evaluation as in Example 1. The evaluation results are shown in Table 3.

[0139] <Comparative Examples 1 to 4> Toners 15 to 18 were produced and evaluated in the same manner as in Example 1, except that the type and amount of the dispersion liquid were changed as shown in Table 2. The evaluation results are shown in Table 3.

[0140]

Table 2

[0141]

Table 3

Claims

1. A toner having toner particles, The toner contains gold nanorods, The gold nanorods are Gold nanorod A having a peak in the aspect ratio range of 6.0 to 13.0 in the aspect ratio distribution measurement, In the aspect ratio distribution measurement, gold nanorod B has a peak in the aspect ratio range of 1.6 to 2.

6. When the optical absorption wavelength of the gold nanorod B is measured, it has a peak in the range of 580 to 650 nm. A toner characterized by:

2. 2. The toner according to claim 1, wherein the gold nanorods A have a peak in the range of 1000 to 1600 nm when the light absorption wavelength is measured.

3. 3. The toner according to claim 1, wherein the gold nanorods B are gold nanorods having a peak aspect ratio in the range of 2.0 to 2.2 in a measurement of aspect ratio distribution.

4. 4. The toner according to claim 1, wherein a mass ratio of the gold nanorods A and the gold nanorods B contained in the toner is from (0.99 / 0.01) to (0.85 / 0.15).

5. The toner according to any one of claims 1 to 4, wherein the content of the gold nanorods A in the toner is 0.001 to 0.200% by mass.

6. A toner having toner particles, The toner contains gold nanorods and an additive, when the aspect ratio distribution of the gold nanorods contained in the toner is measured, the aspect ratio has a peak in the range of 6.0 to 13.0; When the light absorption wavelength of the additive is measured, it has a peak in the range of 580 to 650 nm. A toner characterized by:

7. 7. The toner according to claim 6, wherein a mass ratio of the gold nanorods to the additive contained in the toner is from (0.99 / 0.01) to (0.95 / 0.05).

8. 8. The toner according to claim 6, wherein the content of the gold nanorods in the toner is 0.001 to 0.200% by mass.

9. 9. The toner according to claim 1, which is a toner for forming an invisible image.

10. Using the above toner, the toner loading amount was 0.30 mg / cm 2 10. The toner according to claim 1, wherein in a spectroscopic analysis of a fixed image formed as above, a maximum light absorptance in the wavelength range of 900 nm to 1800 nm is 3% or more.

11. A method for reading an image, comprising the steps of:

11. A method for reading an image, comprising the step of reading an image formed using the toner according to claim 1, using a device equipped with a near-infrared sensor.

12. 1. A method for producing a toner having toner particles, comprising: The method includes a step of obtaining toner particles containing gold nanorods A and gold nanorods B, When the aspect ratio distribution of the gold nanorod A was measured, the aspect ratio had a peak in the range of 6.0 to 13.0, When the aspect ratio distribution of the gold nanorods B is measured, the aspect ratio has a peak in the range of 1.6 to 2.6; When the optical absorption wavelength of the gold nanorod B is measured, it has a peak in the range of 580 to 650 nm. A method for producing a toner comprising the steps of:

13. 1. A method for producing a toner having toner particles, comprising: The method includes obtaining toner particles containing gold nanorods and an additive, When the aspect ratio distribution of the gold nanorods is measured, the aspect ratio has a peak in the range of 6.0 to 13.0; When the light absorption wavelength of the additive is measured, it has a peak in the range of 580 to 650 nm. A method for producing a toner comprising the steps of:

Citation Information

Patent Citations

  • Light absorption material and its formation composition

    JP2004238504A

  • White toner for non-contact fixing

    JP2005099295A

  • Metal particulate-containing composition and its application

    JP2006070300A

  • UV fixable color toner, invisible toner and image forming method

    JP2006079020A

  • Metal fine particle, method for producing metal fine particle, composition containing same, and application thereof

    JP2006118036A