Toner and image reading method
The combination of PEDOT-PSS and gold nanorods in toner particles addresses the challenge of achieving both infrared readability and visible light invisibility, resulting in effective invisible image formation.
Patent Information
- Application Number
- JP2021030079
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-02-26
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2041-02-26
AI Technical Summary
Existing toners for invisible printing do not achieve optimal invisibility in the visible light region while maintaining readability in the infrared region, leading to potential color visibility issues.
A toner formulation containing poly(3,4-ethylenedioxythiophene)-poly(styrene sulfonic acid) (PEDOT-PSS) and gold nanorods, which are incorporated into the toner particles to enhance infrared absorption and reduce visible light absorption, thereby improving invisibility and readability.
The toner provides images with excellent readability in the infrared region and excellent invisibility in the visible light region, ensuring clear infrared detection without visible coloration.
Smart Images

Figure 0007566666000003 
Figure 0007566666000004 
Figure 0007566666000005
Abstract
Description
[Technical field]
[0001] The present disclosure relates to toner and an image reading method. [Background technology]
[0002] In recent years, "invisible printing," which embeds invisible information into printed matter, has been attracting attention for the purpose of strengthening security, such as copyright protection and counterfeit prevention. Since invisible printing does not deteriorate the appearance even when it is overlapped with a visible image, it is possible to use the embedded information while maintaining the quality of normal printed matter, and it is expected to be applied in many fields, including security.
[0003] Patent Document 1 discloses that by incorporating specific metal nanorods in toner, it is possible to form invisible images that are readable by irradiation with infrared light or the like and that do not impair the quality of visible images. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2007-219103 A [Non-patent literature]
[0005] [Non-Patent Document 1] Chemistry of Materials, 2003, No. 15, pp. 1957-1962 Summary of the Invention [Problem to be solved by the invention]
[0006] As a result of the inventors' investigation into the toner described in Patent Document 1, they realized that further improvement was required in terms of the invisibility of images formed using the toner.
[0007] One aspect of the present disclosure is directed to providing a toner that can provide images that can have good readability in the infrared range and good invisibility in the visible range.
[0008] Another aspect of the present disclosure is directed to providing a method for reading an image formed using the toner of the present disclosure. [Means for solving the problem]
[0009] According to one aspect of the present disclosure, there is provided a toner having toner particles containing a resin component, the toner particles contain poly(3,4-ethylenedioxythiophene)-poly(styrenesulfonic acid) (PEDOT-PSS) and gold nanorods; A toner is provided, which comprises:
[0010] According to another aspect of the present invention, there is provided an image reading method, comprising the steps of: There is provided an image reading method, comprising the step of reading an image formed using the toner according to the present disclosure, using a device equipped with a near-infrared sensor. Effect of the Invention
[0011] According to one aspect of the present disclosure, it is possible to provide a toner that can obtain an image that can have excellent readability in the infrared region and excellent invisibility in the visible light region.
[0012] According to another aspect of the present disclosure, a method for reading an image formed using the toner of the present disclosure can be provided. [Brief description of the drawings]
[0013] [Figure 1] Optical absorption spectrum of PEDOT-PSS [Diagram 2] Optical absorption spectrum of gold nanorods [Diagram 3] Illustration of how to read an image DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] The description of "xx or more and xx or less" or "xx to xx" expressing a numerical range means a numerical range including the lower and upper limits which are the endpoints, unless otherwise specified. When a numerical range is described in stages, the upper and lower limits of each numerical range can be arbitrarily combined.
[0015] The toner according to the present disclosure is preferably a toner for forming an invisible image.
[0016] In this disclosure, poly(3,4-ethylenedioxythiophene) is also referred to as PEDOT, and poly(styrenesulfonic acid) is also referred to as PSS. Furthermore, PEDOT-PSS according to this disclosure is treated as a composite of PEDOT and PSS.
[0017] <Background to the invention> The present inventors have found that when an image is formed using the toner according to Patent Document 1, the readability in the infrared region can be improved, but the fixed image may be lightly colored when observed visually. When the light absorption spectrum of the above image was measured, it was found that the above image exhibits absorption in the near infrared region, but also has a small light absorption peak around 530 nm, and this leads to the idea that a fixed image with a light color may be obtained. Naturally, a toner used to form an invisible image is required to be able to form an image that is difficult to see. Therefore, the present inventors have recognized that an improvement is necessary to make the color caused by the absorption around 530 nm difficult to see.
[0018] Based on the above considerations, the present inventors have investigated a toner that can produce an image that is both readable and invisible in the infrared region. As a result, they have found that not only gold nanorods but also PEDOT-PSS, which will be described later, is effective in forming an image with the above-mentioned characteristics. The speculated mechanism and each of the constituent elements will be described in detail below.
[0019] <Presumed mechanism by which the effects of this disclosure manifest> The mechanism by which the toner having the configuration according to the present disclosure exerts the effects of the present disclosure will be described with reference to Figures 1 and 2. Figure 1 shows the light absorption spectrum of PEDOT-PSS used in the examples of the present disclosure, and Figure 2 shows the light absorption spectrum of gold nanorods used in the examples of the present disclosure.
[0020] As will be described in detail later, both PEDOT-PSS (Figure 1) and gold nanorods (Figure 2) exhibit excellent infrared absorption and have slight light absorption bands in the visible light region. Although both have slight light absorption bands in the visible light region, the wavelengths of these light absorption bands in the visible light region are different from each other. Therefore, when an image is formed using a toner containing both PEDOT-PSS and gold nanorods, it becomes easier to obtain an image with flatter light absorption characteristics in the visible light region, that is, an image with lower saturation and less visible.
[0021] In addition, as shown in Figures 1 and 2, since PEDOT-PSS and gold nanorods have excellent infrared absorption, when an image is formed using a toner containing both of them, an image having a high absorbance in the infrared region compared to the absorbance in the visible light region is likely to be obtained. Therefore, even when the content ratio of PEDOT-PSS and gold nanorods is reduced in order to further improve the invisibility of the image, an image having a sufficiently high absorbance in the infrared region and capable of achieving both excellent invisibility and readability is likely to be obtained.
[0022] <pedot-pss> PEDOT-PSS will be explained. When an electron acceptor or electron donor is added to a conjugated polymer, carriers (holes or electrons) are generated in the main chain of the conjugated polymer, forming a polymer complex with electrical conductivity. Such polymer complexes are generally called conductive polymers. Representative conjugated polymers include aliphatic conjugated polyacetylene, aromatic conjugated poly(p-phenylene), heterocyclic conjugated polypyrrole and polythiophene, and heteroatom conjugated polyaniline. Acceptors include halogens and Lewis acids, and donors include alkali metals and alkaline earth metals.
[0023] The conductive polymers exhibit infrared absorbing properties due to the plasma vibration of carriers. That is, it is believed that the infrared absorbing properties are exhibited by forming a polymer complex between a conjugated polymer and an electron acceptor or electron donor. In addition, since the infrared absorbing properties of a conductive polymer are proportional to the carrier density, the higher the conductivity of the conductive polymer, the higher the infrared absorbing properties are.
[0024] In the PEDOT-PSS contained in the toner according to the present disclosure, PEDOT is a conjugated polymer and PSS functions as an acceptor, forming a polymer complex, and therefore exhibits high infrared absorptivity.
[0025] The optical absorption spectrum of PEDOT-PSS is shown in Figure 1. PEDOT-PSS has a large optical absorption band in the infrared region due to the plasma oscillation of carriers. Here, the optical absorption caused by the plasma oscillation of carriers extends not only in the infrared region but also in the visible light region of 500 to 800 nm, so it exhibits a complementary color of blue to indigo.
[0026] PEDOT-PSS can be produced, for example, by oxidative polymerization of 3,4-ethylenedioxythiophene in the presence of PSS. In addition, a commercially available product (e.g., Denatron PT-300 (trade name), manufactured by Nagase Chemtex Corporation) can also be purchased and used.
[0027] <Gold nanorods> The toner contains gold nanorods. Here, gold nanorods refer to nanorods with a gold content of 80% or more.
[0028] Gold nanorods are fine metal materials that are mainly composed of gold and have a long axis and a short axis in a TEM image. In other words, gold nanorods are observed in a TEM image as being approximately rectangular. In general, the length of the short axis is 1 nm to 60 nm, and the length of the long axis is 20 nm to 500 nm. In addition, depending on the aspect ratio of the gold nanorod, which is the long axis length divided by the short axis length, the light absorption caused by the long axis appears at 650 nm to 2000 nm, and the larger the aspect ratio, the more the absorption wavelength shifts to the long wavelength side. On the other hand, it was found that the light absorption caused by the short axis is hardly affected by the aspect ratio and appears around 530 nm.
[0029] In this disclosure, gold nanorods are those with an aspect ratio of 1.5 or greater, and gold nanoparticles are those with an aspect ratio of less than 1.5.
[0030] The arrangement of gold and metal elements other than gold in the gold nanorods may be an alloy composite at the atomic level, or a core-shell structure in which a nanorod of gold alone is coated with a metal element other than gold. The gold nanorods may also be coated with a shell made of, for example, silica or polystyrene. Furthermore, the surface of the gold nanorods may be modified with appropriate molecules such as surfactants depending on the purpose, such as dispersing the gold nanorods in a medium.
[0031] In addition, since a toner having excellent invisibility is easily obtained, the ratio of the mass of the gold nanorods to the mass of the PEDOT-PSS contained in the toner is preferably 0.01 to 10.00, and more preferably 0.05 or more and 5.00 or less.
[0032] In addition, in order to easily obtain a toner having excellent infrared readability, it is preferable that the gold nanorods contained in the toner have a peak top in the wavelength range of 1000 to 1800 nm when the light absorption wavelength of the gold nanorods contained in the toner is measured.
[0033] <Preparation method of gold nanorods> Gold nanorods can be synthesized, for example, by a method proposed by B. Nikoobakft and MA El-Sayed (Non-Patent Document 1). Specifically, this method involves reducing chloroauric acid (HAuCl4) with ascorbic acid in an aqueous solution containing two types of surfactants (hexadecyltrimethylammonium bromide and benzyldimethylhexadecylammonium chloride). With this method, the surfactant is adsorbed to a specific crystal face of the gold nanoparticles, suppressing the growth of the crystal face, resulting in the synthesis of anisotropic gold nanorods.
[0034] The optical absorption spectrum of the gold nanorods synthesized by the above method is shown in Figure 2. The synthesized gold nanorods had a wide aspect ratio distribution, with the aspect ratio centered around 4 to 6, and showed large optical absorption in the wavelength range of 650 to 2000 nm. They also showed small optical absorption around 530 nm, and the gold nanorods were red to purple in color.
[0035] <Toner and toner particles> The toner particles contain a resin component. In addition, the ratio of the total mass of the gold nanorods and PEDOT-PSS contained in the toner to the mass of the resin component is preferably 0.01 to 1.00% by mass. If it is 0.01% by mass or more, the fixed image is likely to have sufficient infrared absorption properties, and an image with excellent readability is likely to be obtained. If it is 1.00% by mass or less, the brightness of the image is unlikely to be too low, and an image with excellent invisibility in the visible light region is likely to be obtained. In addition, the resin component is preferably a binder resin.
[0036] There is no particular limitation on the location and dispersion state of the PEDOT-PSS and gold nanorods in the toner. That is, the PEDOT-PSS and gold nanorods may be uniformly dispersed in the binder resin, or may be unevenly distributed in the center or surface. The PEDOT-PSS and gold nanorods may also be contained in wax or an external additive.
[0037] <Light absorptance in the infrared region> The toner load is 0.30 mg / cm 2 When the optical absorption spectrum of the fixed image formed as above is measured, the maximum absorptance in the wavelength range of 900 to 1800 nm is preferably 12% or more. This wavelength range corresponds to the infrared (near infrared to short wavelength infrared) range, and if the maximum absorptance is 12% or more, the invisible image can be easily and clearly read using an infrared camera or the like. It is more preferably 15% or more, and even more preferably 20% or more.
[0038] The light absorptance in the infrared region can be controlled by adjusting the masses of PEDOT-PSS and gold nanorods used in producing the toner.
[0039] <Resin component> The resin component contained in the toner particles is not particularly limited, and specifically includes vinyl resin, polyester resin, epoxy resin, etc., which can be used alone or in mixture. More preferably, it is at least one selected from the group consisting of vinyl resin and polyester resin. It is even more preferable that at least one resin selected from the group is the main binder. The resin component may be any of a resin having a linear molecular structure, a branched resin, and a crosslinked resin, or a mixture of these. It is preferable that the resin component is a binder resin.
[0040] <Various additives> If necessary, the toner may contain one or more additives selected from wax, charge control agents, external additives, etc. In addition, the toner according to the present disclosure preferably does not contain a coloring component that makes a fixed image a visible image.
[0041] <Wax> The wax is not particularly limited, but colorless or light-colored waxes are preferred, and examples thereof include the following.
[0042] Hydrocarbon wax, ester wax, amide wax, higher aliphatic alcohol, higher fatty acid, etc. One type of wax may be used alone, or multiple types may be used in combination.
[0043] <Charge control agent> The charge control agent is not particularly limited, but colorless or light-colored charge control agents are preferred, and examples thereof include the following.
[0044] Aromatic oxycarboxylic acids, metal compounds of aromatic oxycarboxylic acids, boron compounds, quaternary ammonium salts, calixarenes, resins having sulfonic acid (salt) groups, resins having sulfonic acid ester groups, etc. The charge control agents may be used alone or in combination.
[0045] <External additives> The external additive is not particularly limited, but colorless or light-colored ones are preferable, and the followings can be mentioned.
[0046] Silica, alumina, titanium oxide, strontium titanate, silicon nitride, polytetrafluoroethylene, zinc stearate, etc. The surface of the external additive may be subjected to a hydrophobic treatment.
[0047] <Method of manufacturing toner particles> The toner particles can be produced by a pulverization method, a polymerization method, or the like, but is not limited to these.
[0048] An example of a method for producing toner particles by a pulverization method will be described. After thoroughly mixing the binder resin, PEDOT-PSS, gold nanorods, and additives such as wax and charge control agent, the mixture is melted and kneaded using a device such as a three-roll type, single- or double-screw type, or Banbury mixer type to obtain a molten kneaded product. After cooling and solidifying the molten kneaded product, the mixture is pulverized and classified to obtain toner particles. The toner particles can be smoothed using a hybridization system (Nara Machinery Works) or a mechanofusion system (Hosokawa Micron Corporation), or sphericalized using a faculty (Hosokawa Micron Corporation). In addition, such a pulverization method may include a step of melting and kneading the resin to increase the content of PEDOT-PSS and gold nanorods in the resin to produce a master batch, and then further melting and kneading the master batch and the resin. This step can improve the dispersibility of PEDOT-PSS and gold nanorods in the toner particles.
[0049] An example of a method for producing toner particles by polymerization will be described. Representative polymerization methods are suspension polymerization and emulsion polymerization.
[0050] In the suspension polymerization method, a mixture of polymerizable monomers such as styrene and butyl acrylate, PEDOT-PSS, gold nanorods, and additives such as wax, charge control agent, polymerization initiator, and crosslinking agent is prepared. The prepared mixture is suspended in an aqueous phase containing a suspension stabilizer and a surfactant for dispersing the suspension stabilizer, using a homogenizer or the like. The suspension stabilizer can be an inorganic compound such as an alkaline earth metal phosphate, carbonate, or sulfate, or an organic compound such as polyvinyl alcohol, gelatin, or ethyl cellulose. By heating this suspension, the polymerizable monomers in the mixture suspended in the aqueous phase are polymerized to obtain toner particles.
[0051] In the emulsion polymerization method, polymerizable monomers such as styrene and butyl acrylate and surfactants are added to an aqueous phase in which a water-soluble polymerization initiator has been dissolved. The prepared mixture is heated and polymerized while applying strong shearing force to obtain resin particles. This dispersion of resin particles is mixed with additives such as PEDOT-PSS, gold nanorods, charge control agents, and wax, and then aggregating agents are added to generate aggregate particles in which the individual particles are aggregated. These aggregate particles are heated to above the glass transition temperature of the resin particles and fused to obtain toner particles.
[0052] If necessary, an external additive may be added to the toner particles produced by the pulverization method or the polymerization method.
[0053] <How to read an image> The method for reading an image formed using the toner according to the present disclosure is not particularly limited. Since an image formed using the toner according to the present disclosure is prone to absorbing wavelengths in the near-infrared region, it is preferable to use an apparatus equipped with a near-infrared sensor for the image reading method. More preferably, an apparatus equipped with an InGaAs sensor is used, and even more preferably, an InGaAs camera is used. In addition, it is preferable to use an image reading method that uses light in the wavelength region of 900 to 2500 nm. More preferably, it is the wavelength region of 900 to 1800 nm.
[0054] As an example of a method for reading an image, the operations carried out by the present inventors are shown below.
[0055] After forming an evaluation image using the toner according to the present disclosure, a light source 202 and a camera 203 were installed as shown in FIG. 3, and an evaluation image 201 was observed. That is, the evaluation image was placed on a desk, and infrared rays were irradiated from a distance of about 1 m at an angle of 15° to the evaluation image using the light source 202. In addition, a camera 203 was installed 15 cm directly above the evaluation image, and an image was taken. As the light source 202, a halogen lamp light source (product name: PCS-UHX-150, manufactured by Japan PI Corporation) equipped with a visible light cut filter unit was used. As the camera 203, a near-infrared camera (product name: NVU3VD, manufactured by IR Spec, InGaAs camera) equipped with a filter for cutting wavelength components of 800 nm or less was used in the lens part. The spectral sensitivity wavelength range of the near-infrared camera was 970 to 1650 nm.
[0056] <Toner analysis method> The method for quantifying the amount of PEDOT-PSS and gold nanorods contained in the toner is explained below. First, the resin components in the toner are dissolved in an organic solvent such as toluene, and this solution is centrifuged at 15,000 to 20,000 rpm to extract the high-density gold nanorods, whose mass can be measured. In addition, a liquid in which gold nanorods are dispersed in an appropriate solvent is dropped onto a dedicated grid, and after drying, the shape (major axis diameter, minor axis diameter, aspect ratio, etc.) and composition of the gold nanorods can be confirmed using a transmission electron microscope (TEM) and energy dispersive X-ray spectroscopy (EDX) mounted on the TEM.
[0057] In addition, water can be added to the organic solvent in which the toner is dissolved to extract hydrophilic PEDOT-PSS into the aqueous phase. The extracted PEDOT-PSS can be qualitatively and quantitatively analyzed by Fourier transform infrared spectroscopy (FT-IR), nuclear magnetic resonance spectroscopy (NMR), gas chromatography mass spectrometry (GC / MS), etc. From the mass of the dissolved resin component and the quantified masses of PEDOT-PSS and gold nanorods, the mass ratio of PEDOT-PSS and gold nanorods to the mass of the resin component, the mass ratio of gold nanorods to the mass of PEDOT-PSS, etc. can be calculated. EXAMPLES
[0058] The present disclosure will be described in more detail with reference to examples, but the present disclosure is not limited to the following examples.
[0059] <Example 1> [Preparation of gold nanorod dispersion] First, a seed particle solution was prepared. 500 L of 0.0005 mol / L chloroauric acid tetrahydrate (Kishida Chemical Co., Ltd.) aqueous solution was mixed with 500 mL of 0.2 mol / L cetyltrimethylammonium bromide (Kishida Chemical Co., Ltd.) aqueous solution. 60 mL of 0.01 mol / L sodium borohydride (Tokyo Chemical Industry Co., Ltd.) was added to this aqueous solution to obtain a seed particle solution (Solution A).
[0060] 3 g of cetyltrimethylammonium bromide was dissolved in 500 mL of 0.15 mol / L benzyldimethylhexadecylammonium chloride (Tokyo Chemical Industry Co., Ltd.) aqueous solution. 20 mL of 0.004 mol / L silver nitrate aqueous solution was added to the aqueous solution containing these two types of surfactants. 500 mL of 0.001 mol / L chloroauric acid tetrahydrate aqueous solution was added to this aqueous solution, and then 7 mL of 0.078 mol / L L-ascorbic acid aqueous solution (Kishida Chemical Co., Ltd.) was added. This solution was designated as solution B.
[0061] 1.2 mL of solution A was added dropwise to solution B. This solution was kept at 30° C. for one week, and seed particles serving as nuclei were grown anisotropically to obtain an aqueous dispersion of gold nanorods.
[0062] The dispersion medium of the above-mentioned gold nanorod aqueous dispersion was replaced with THF from water to obtain a gold nanorod THF dispersion. The optical absorption spectrum of the gold nanorods contained in the dispersion is shown in Figure 2. The spectrum was measured using a spectrophotometer (product name: V-670, JASCO Corporation).
[0063] [Toner particle manufacturing process] Polyester 1 (polycondensate of ethylene oxide-modified bisphenol A and terephthalic acid, glass transition temperature 60°C, weight average molecular weight 29000, number average molecular weight 6000) 5 parts by weight Material A: PEDOT-PSS (Denatron PT-300, Nagase ChemteX Corporation) 0.727 parts by mass Material B: Gold nanorod THF dispersion (Use gold nanorod THF dispersion so that the gold nanorod solid content is 0.073 parts by mass) A mixture of the above materials was prepared. In this case, PEDOT-PSS was freeze-dried and then finely ground in a ball mill before use. The optical absorption spectrum of the PEDOT-PSS is shown in Figure 1. A spectrophotometer (product name: V-670, JASCO Corporation) was used to measure the optical absorption spectrum.
[0064] After evaporating the THF from the above mixture, the mixture was coarsely pulverized using a hammer mill to obtain a coarsely pulverized product. Note that the above Denatron PT-300 is PEDOT-PSS.
[0065] To the obtained coarsely ground product, 95 parts by mass of polyester 1 and 5 parts by mass of ester wax were added and mixed in a mixer (FM Mixer, manufactured by Nippon Coke & Engineering Co., Ltd.), and then melt-kneaded in a twin-screw kneader (PCM30, manufactured by Ikegai Corporation) set at a temperature of 130°C to obtain a kneaded product. The kneaded product was cooled and solidified, coarsely ground in a hammer mill, and then finely ground in a dry grinder (T250, manufactured by Freund Turbo Corporation). This powder was classified using a rotary classifier (200TSP, manufactured by Hosokawa Micron Corporation) to obtain toner particles.
[0066] [External addition process] 100 parts by mass of the obtained toner particles and 1 part by mass of hydrophobic silica fine powder (primary particle number average particle size 7 nm) that had been surface-treated with hexamethyldisilazane were mixed in a mixer to obtain toner 1.
[0067] [evaluation] The obtained toner 1 was subjected to the following evaluations.
[0068] (1) Evaluation of readability in the infrared region As an image forming device, a color printer (product name: LBP652C, manufactured by Canon Inc.) modified so that the development contrast could be freely changed was used, and the toner in the black developing device was replaced with toner 1. A4 paper (product name: GF-C081, manufactured by Canon Marketing Japan Inc.) was used as the output paper, and the following sample images were output in an environment of a temperature of 25° C. and a relative humidity of 60%. Sample image: Toner 1 loading amount is 0.30mg / cm 2 A rectangular image of 1cm x 10cm.
[0069] The above sample image was subjected to spectroscopic analysis measurement in the wavelength region of 900 to 1800 nm using an ultraviolet-visible near-infrared spectrophotometer (product name: MV-3300, manufactured by JASCO Corporation). The maximum absorptivity obtained from the measurement was taken as the measured value of the sample image. Spectroscopic analysis measurement was also performed on a single sheet of paper as a blank, and the value obtained by subtracting the measured value of the blank from the measured value of the sample image was taken as the infrared absorptivity (%), and this value was used to evaluate the readability of Toner 1. The results are shown in Table 2. It was determined that the effect of the present disclosure was obtained when the infrared absorptivity (%) was 12% or more.
[0070] (2) Invisibility assessment The above sample images were visually inspected and evaluated for invisibility. The evaluation criteria were as follows: A: Difficult to distinguish rectangular images B: Rectangular images are somewhat difficult to distinguish. C: Rectangular images are neither easy nor difficult to distinguish. D: Rectangular images are somewhat easy to distinguish. E: Rectangular images are easy to distinguish In the above evaluation criteria, those that received a rating of A or B were judged to have excellent invisibility.
[0071] <Examples 2 and 3> Toners 2 and 3 were produced and evaluated in the same manner as in Example 1, except that the types and amounts of materials A and B were changed as shown in Table 1. The evaluation results are shown in Table 2.
[0072] <Example 4> [Preparation of aqueous medium] 14 parts by mass of sodium phosphate dodecahydrate were dissolved in 1000 parts by mass of ion-exchanged water, and the mixture was kept at 65°C for 1 hour while purging with nitrogen. After that, it was stirred at 12000 rpm using a high-speed emulsifier / disperser (Primix Corporation homomixer). An aqueous calcium chloride solution in which 9.2 parts by mass of calcium chloride dihydrate were dissolved in 20 parts by mass of ion-exchanged water was added all at once to prepare an aqueous medium containing fine dispersion stabilizers.
[0073] [Preparation process of polymerizable monomer composition] A styrene dispersion of PEDOT-PSS and gold nanorods was obtained by treating 113.8 parts by mass of styrene, 0.133 parts by mass of the above PEDOT-PSS, and 0.067 parts by mass of the above gold nanorods using a wet fine grinding machine (Attritor, manufactured by Nippon Coke & Engineering Co., Ltd.) at 220 rpm for 5 hours. A mixture was obtained by adding 45 parts by mass of styrene, 34 parts by mass of n-butyl acrylate, 1 part by mass of an aluminum salicylate compound, 5 parts by mass of polyester 1, 10 parts by mass of ester wax, and 0.1 parts by mass of divinylbenzene to the obtained styrene dispersion. This mixture was dispersed at 500 rpm while maintaining the temperature at 65°C using a high-speed emulsifier / disperser to prepare a polymerizable monomer composition.
[0074] [Granulation process] While maintaining the temperature of the aqueous medium at 70°C and operating the high-speed emulsifier / disperser at 12,000 rpm, the polymerizable monomer composition and 10 parts by mass of t-butyl peroxypivalate were added to the aqueous medium, and granulated for 10 minutes.
[0075] [Polymerization process] After granulation, polymerization was carried out for 5 hours while maintaining the temperature at 70° C. and stirring at 150 rpm, and then the temperature was raised to 85° C. and heated for 2 hours to complete the polymerization reaction.
[0076] [Washing and drying process] After the polymerization process was completed, the liquid temperature was lowered to room temperature, and diluted hydrochloric acid was added dropwise to adjust the pH to 1.5, followed by stirring for 3 hours. After that, filtration and washing were repeated to obtain a toner cake. After crushing the toner cake, it was dried in an airflow dryer, and further classified using a multi-division classifier utilizing the Coanda effect to obtain toner particles.
[0077] [External addition process] 100 parts by mass of the obtained toner particles and 1 part by mass of hydrophobic silica fine powder (primary particle number average particle size 7 nm) that had been surface-treated with hexamethyldisilazane were mixed in a mixer to obtain toner 4.
[0078] [evaluation] The obtained toner 4 was used for the same evaluation as in Example 1. The results are shown in Table 2.
[0079] <Examples 5 and 6> Toners 5 and 6 were produced and evaluated in the same manner as in Example 4, except that the amounts of PEDOT-PSS and gold nanorods added were changed as shown in Table 1. The evaluation results are shown in Table 2.
[0080] <Comparative Examples 1 to 4> Toners 7 to 10 were produced and evaluated in the same manner as in Example 1, except that the types and amounts of materials A and B were changed as shown in Table 1. The evaluation results are shown in Table 2.
[0081] [Table 1]
[0082] [Table 2]
Claims
1. A toner having toner particles containing a resin component, the toner contains poly(3,4-ethylenedioxythiophene)-poly(styrenesulfonic acid) (PEDOT-PSS) and gold nanorods; A toner characterized by:
2. 2. The toner according to claim 1, wherein a ratio of a total mass of the gold nanorods and the PEDOT-PSS contained in the toner to a mass of the resin component is 0.01 to 1.00% by mass.
3. 3. The toner according to claim 1, wherein a ratio of the mass of the gold nanorods to the mass of the PEDOT-PSS contained in the toner is 0.01 to 10.
00.
4. Using the above toner, the toner loading amount was 0.30 mg / cm 2 When the optical absorption spectrum of the fixed image formed as above was measured, 4. The toner according to claim 1, which has a maximum absorptivity of 15% or more in a wavelength region of 900 to 1800 nm.
5. 5. The toner according to claim 1, wherein, when the light absorption wavelength of the gold nanorods is measured, the gold nanorods have a peak top in a wavelength range of 1000 to 1800 nm.
6. 6. The toner according to claim 1, which is a toner for forming an invisible image.
7. A method for reading an image, comprising the steps of:
7. A method for reading an image, comprising the step of reading an image formed using the toner according to claim 1, using a device equipped with a near-infrared sensor.
Citation Information
Patent Citations
UV fixable color toner, invisible toner and image forming method
JP2006079020A
Electrophotographic toner, electrophotographic developer and image forming method
JP2007219103A
Conductive nanocomposite
JP2018528312A
Toner, image forming apparatus, and image forming method
JP2019138936A
Coagulating ink
JP2019500458A