Method for manufacturing a polarizer and a polarizing plate
The described method for manufacturing polarizers through dyeing, crosslinking, and stretching processes addresses display unevenness in image display devices by ensuring uniform dyeing and improving optical properties, resulting in high-quality polarizers.
Patent Information
- Application Number
- JP2021195644
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-12-01
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2041-12-01
AI Technical Summary
Existing polarizers in image display devices suffer from display unevenness, which is not adequately addressed by conventional manufacturing methods.
A method involving dyeing, crosslinking, and stretching steps for polyvinyl alcohol resin films, with specific absorbance ratios and processes to enhance uniformity, including auxiliary stretching and drying shrinkage, to produce polarizers with reduced thickness and improved optical properties.
The method effectively suppresses display unevenness in image display devices by ensuring uniform dyeing and enhancing optical properties, achieving high single transmittance and degree of polarization.
Smart Images

Figure 0007566720000002 
Figure 0007566720000003 
Figure 0007566720000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a polarizer and a method for producing a polarizing plate. [Background technology]
[0002] A polarizer is typically used in image display devices. For example, such a polarizer is formed on a resin substrate by forming a polyvinyl alcohol-based resin layer on the resin substrate, immersing a laminate including the resin substrate and the polyvinyl alcohol-based resin layer in an aqueous boric acid solution to insolubilize the polyvinyl alcohol-based resin layer, dyeing the polyvinyl alcohol-based resin layer with a dichroic substance, and then stretching the laminate in the aqueous boric acid solution (for example, Patent Document 1). In recent years, there has been a demand for higher definition image display devices using polarizers, and further reduction in display unevenness of the image display devices is desired. However, the image display device including the polarizer described in Patent Document 1 has room for improvement in reducing display unevenness. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] International Publication No. 2010 / 100917 Summary of the Invention [Problem to be solved by the invention]
[0004] The present invention has been made to solve the above-mentioned problems in the conventional art, and a main object of the present invention is to provide a method for producing a polarizer and a polarizing plate capable of suppressing display unevenness in an image display device. [Means for solving the problem]
[0005] A method for producing a polarizer according to an embodiment of the present invention includes a dyeing step of dyeing a polyvinyl alcohol-based resin film with a dichroic material, a crosslinking step of contacting the polyvinyl alcohol-based resin film after the dyeing step with an aqueous boric acid solution, and a stretching step of stretching the polyvinyl alcohol-based resin film after the crosslinking step in a stretching bath. A ratio of an orthogonal absorbance A580_c at a wavelength of 580 nm of the polyvinyl alcohol-based resin film after the crosslinking step and before the stretching step to an orthogonal absorbance A580_b at a wavelength of 580 nm of the polyvinyl alcohol-based resin film after the dyeing step and before the crosslinking step is 0.91 or more. In one embodiment, a polarizer having a single transmittance of 42% or more and 45% or less is produced. In one embodiment, the method for producing a polarizer includes, in this order, a laminate-preparing step of applying a coating liquid containing a polyvinyl alcohol-based resin and a halide onto a long thermoplastic resin substrate to prepare a laminate including a polyvinyl alcohol-based resin layer as the polyvinyl alcohol-based resin film and the thermoplastic resin substrate; an auxiliary stretching step of stretching the laminate in air; the dyeing step; the crosslinking step; the stretching step; and a drying shrinking step of shrinking the polyvinyl alcohol-based resin layer after the stretching step in a width direction perpendicular to the long direction while transporting the polyvinyl alcohol-based resin layer in the long direction. In one embodiment, the thermoplastic resin substrate is a polyethylene terephthalate film. In one embodiment, a polarizer having a thickness of 12 μm or less is produced. In one embodiment, the drawing bath is an aqueous solution of boric acid. A method for producing a polarizing plate according to another aspect of the present invention includes laminating a protective film to the polarizer produced by the above-described method for producing a polarizer. Effect of the Invention
[0006] According to the embodiment of the present invention, it is possible to manufacture a polarizer and a polarizing plate capable of suppressing display unevenness in an image display device. [Brief description of the drawings]
[0007] [Figure 1] FIG. 1 is a schematic diagram illustrating a method for producing a polarizer according to one embodiment of the present invention. [Diagram 2] Fig. 2(a) is a schematic cross-sectional view of one embodiment of the polyvinyl alcohol-based resin film shown in Fig. 1. Fig. 2(b) is a schematic cross-sectional view of another embodiment of the polyvinyl alcohol-based resin film shown in Fig. 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] Representative embodiments of the present invention will be described below, but the present invention is not limited to these embodiments.
[0009] A. Overview of polarizer manufacturing method A method for producing a polarizer according to one embodiment of the present invention includes a dyeing step of dyeing a polyvinyl alcohol-based resin film (hereinafter referred to as a PVA-based resin film) with a dichroic material, a crosslinking step of contacting the PVA-based resin film after the dyeing step with an aqueous boric acid solution, and a stretching step of stretching the PVA-based resin film after the crosslinking step in a stretching bath. The ratio (A580_c / A580_b) of the orthogonal absorbance A580_c at a wavelength of 580 nm of the PVA-based resin film after the crosslinking step and before the stretching step to the orthogonal absorbance A580_b at a wavelength of 580 nm of the PVA-based resin film after the dyeing step and before the crosslinking step is 0.91 or more, preferably 0.92 or more, more preferably 0.97 or more, and particularly preferably 0.99 or more. In an image display device using a polarizer dyed with a dichroic material, non-uniformity in the dyeing of the polarizer can cause display unevenness in the image display device. The present inventors have therefore conducted extensive research into improving the uniformity of dyeing in the polarizer, and have found that streaky dyeing unevenness that can occur in the polarizer can be suppressed and the uniformity of dyeing in the polarizer can be improved by adjusting the ratio of the orthogonal absorbance before and after the crosslinking process to a specific range, thereby completing the present invention. More specifically, when the above-mentioned A580_c / A580_b is equal to or greater than the above lower limit, the dyeing unevenness in the polarizer can be significantly suppressed. In one embodiment, the upper limit of A580_c / A580_b is typically 2.5 or less, preferably 1.50 or less, and more preferably 1.15 or less. When A580_c / A580_b is equal to or less than the above upper limit, uneven dyeing in the polarizer can be more significantly suppressed. The orthogonal absorbance can be calculated from the orthogonal transmittance Tc, which will be described later, by the following formula. Orthogonal absorbance = log10(100 / Tc)
[0010] In one embodiment, the PVA-based resin film is brought into contact with a dye bath (dyeing solution) in the dyeing step without being brought into contact with an aqueous boric acid solution before the dyeing step. When the PVA-based resin film is brought into contact with an aqueous boric acid solution, the boric acid forms crosslinks, imparting water resistance to the PVA-based resin film. Therefore, in the method for producing a polarizer, the PVA-based resin film is generally brought into contact with an aqueous boric acid solution before the dyeing step to suppress dissolution of the PVA-based resin film in the dyeing solution. However, if the PVA-based resin film is previously contacted with a boric acid solution, the boric acid is released from the PVA-based resin film and eluted into the dyeing solution during the dyeing process, which may affect the distribution of the complex between the dichroic material and the PVA-based resin formed during the dyeing process, and therefore it is presumed that this will adversely affect the uniformity of dyeing in the polarizer. On the other hand, when the PVA-based resin film is brought into contact with a dye solution without being brought into contact with an aqueous boric acid solution prior to the dyeing step, the complex of the dichroic material and the PVA-based resin can be uniformly distributed, and uneven dyeing in the polarizer can be stably suppressed.
[0011] In one embodiment, the method for producing a polarizer includes a laminate preparation step, an auxiliary stretching step, the dyeing step, the crosslinking step, the stretching step, and a drying shrinkage step, in this order. In the laminate preparation step, a coating liquid containing a PVA-based resin and a halide is applied onto a long thermoplastic resin substrate to prepare a laminate including a PVA-based resin layer as a PVA-based resin film and a thermoplastic resin substrate. In the auxiliary stretching step, the laminate is stretched in air. In the drying shrinkage step, the PVA-based resin layer after the stretching step is shrunk in the width direction perpendicular to the long direction while being transported in the long direction. According to this method, a polarizer having a reduced thickness and excellent optical properties can be provided. That is, by introducing the auxiliary stretching process, even when the PVA-based resin is applied on the thermoplastic resin, it is possible to increase the crystallinity of the PVA-based resin, and it is possible to achieve high optical properties. In addition, by increasing the orientation of the PVA-based resin in advance at the same time, problems such as a decrease in the orientation and dissolution of the PVA-based resin when immersed in a liquid in the subsequent dyeing process can be prevented, and high optical properties can be achieved. In addition, since the PVA-based resin layer is contacted with an aqueous boric acid solution in the crosslinking process, it is possible to impart water resistance to the PVA-based resin layer, and it is possible to suppress the dissolution of the PVA-based resin layer in the stretching bath in the next stretching process. In addition, when the PVA-based resin layer is immersed in a liquid, the disorder of the orientation of the PVA-based resin molecules and the decrease in the orientation can be suppressed compared to when the PVA-based resin layer does not contain a halide. This can improve the optical properties of a polarizer obtained through a treatment process in which the laminate is immersed in a liquid, such as a dyeing process and a stretching process. Furthermore, by shrinking the PVA-based resin film in the width direction through a drying shrinkage step, the optical properties of the polarizer can be improved.
[0012] The above-mentioned method for producing a polarizer may include a hue adjusting step. In the hue adjustment step, typically, the PVA-based resin film after the stretching step (preferably the PVA-based resin film after the stretching step and before the drying shrinkage step) is immersed in a hue adjustment bath, whereby the PVA-based resin film can be washed and the polarizer can be adjusted to have a desired hue.
[0013] B. Details of polarizer manufacturing method 1 is a schematic diagram illustrating a method for producing a polarizer according to one embodiment of the present invention. In the illustrated example of the method for producing a polarizer, the above-mentioned dyeing step, crosslinking step, stretching step, hue adjusting step, and drying shrinkage step are carried out continuously. More specifically, a long PVA-based resin film 1 is transported from a raw roll 21 toward a take-up roll 22, and between the raw roll 21 and the take-up roll 22, a dyeing step, a crosslinking step, a stretching step, a hue adjusting step, and a drying shrinking step are sequentially performed on the PVA-based resin film 1. In one embodiment, the PVA-based resin film 1 is immersed in a dye bath 2B (dyeing liquid), a crosslinking bath 2C (crosslinking liquid), a stretching bath 2D (stretching liquid), and a hue adjusting bath 2E (hue adjusting liquid) in this order by a plurality of rollers 24, and then transported to pass through a heat drying section 23. Note that, as will be described later in detail, when the PVA-based resin film is a PVA-based resin layer included in a laminate, the laminate including the PVA-based resin layer is immersed in each of the above-mentioned baths (each liquid) to bring the PVA-based resin layer into contact with each bath (each liquid).
[0014] B-1. PVA resin film In the raw film roll 21, the PVA resin film 1 (hereinafter referred to as raw film 11) before each of the above-mentioned steps is wound in a roll shape. The crystallization index of the PVA-based resin in the raw film 11 is, for example, 1.6 or more, preferably 1.8 or more. If the crystallization index of the PVA-based resin is equal to or more than such a lower limit, even if the PVA-based resin film is immersed in a dye bath without contacting with an aqueous boric acid solution, the PVA-based resin film can be prevented from dissolving in the dye solution. The crystallization index of the PVA-based resin is typically 3.0 or less. The crystallization index of the PVA-based resin can be measured by the ATR method using a Fourier transform infrared spectrophotometer. The raw film 11 may be a single-layer resin film as shown in FIG. 2(a), or may be laminated to a thermoplastic resin substrate 12 (hereinafter referred to as resin substrate 12) as shown in FIG. 2(b).
[0015] Specific examples of single-layer resin films include hydrophilic polymer films such as PVA films, partially formalized PVA films, and partially saponified ethylene-vinyl acetate copolymer films, and polyene-based oriented films such as dehydrated PVA and dehydrochlorinated polyvinyl chloride. When the raw film 11 is a single-layer resin film, the thickness is, for example, 20 μm or more, preferably 30 μm or more, and, for example, 65 μm or less, preferably 60 μm or less. In addition, when the raw film 11 is a single-layer resin film or a resin film supported by a resin substrate, an insolubilization step can be carried out to impart water resistance to the PVA-based resin film by contacting it with an aqueous boric acid solution before the dyeing step. The content of boric acid in the aqueous boric acid solution is, for example, 1 part by mass or more and 10 parts by mass or less with respect to 100 parts by mass of water. The temperature of the aqueous boric acid solution is, for example, 10° C. or more and 60° C. or less. The contact time between the PVA-based resin film and the aqueous boric acid solution is, for example, 10 seconds or more and 200 seconds or less. In the insolubilization step, the PVA-based resin film can also be stretched. When the raw film is a resin film supported by a single-layer resin film / resin substrate, A580_c / A580_b can be stably adjusted to the above range even if insolubilization treatment is performed, and the uniformity of dyeing in the polarizer can be ensured at a practical level. However, as described above, it is preferable not to contact the film with the boric acid aqueous solution before the dyeing step, because this can further reduce uneven dyeing in the polarizer.
[0016] When the original film 11 is laminated on a thermoplastic resin substrate 12, the original film 11 may be a PVA-based resin film supported on the resin substrate 12, or a PVA-based resin layer 13 formed by coating on the resin substrate 12. When the raw film 11 is a PVA-based resin layer 13 formed by coating on a resin substrate 12 , the PVA-based resin layer 13 is formed on the resin substrate 12 . More specifically, a coating liquid containing a PVA-based resin and a halide is applied onto a long resin substrate 12 by any appropriate method, and if necessary, dried at a temperature of, for example, 50°C or higher to produce a laminate 10 comprising a PVA-based resin layer 13 and the resin substrate 12.
[0017] Any appropriate material may be adopted as the constituent material of the resin substrate 12. The resin substrate is typically a polyethylene terephthalate film. Examples of the constituent material include amorphous (uncrystallized) polyethylene terephthalate-based resins, and preferably amorphous (hard to crystallize) polyethylene terephthalate-based resins. Specific examples of amorphous polyethylene terephthalate-based resins include copolymers further containing isophthalic acid as a dicarboxylic acid and copolymers further containing cyclohexanedimethanol as a glycol. The glass transition temperature (Tg) of the resin substrate is, for example, 170°C or less, preferably 120°C or less. When the Tg of the resin substrate is the above upper limit or less, the stretchability of the laminate can be sufficiently ensured while the crystallization of the PVA-based resin layer can be suppressed. The glass transition temperature (Tg) of the resin substrate is typically 60°C or more. This can suppress defects such as deformation of the resin substrate (for example, generation of unevenness, sagging, and wrinkles) when the coating liquid is applied to the resin substrate and dried. The glass transition temperature (Tg) is measured in accordance with JIS K 7121. The thickness of the resin substrate before stretching is, for example, 20 μm or more, preferably 50 μm or more, and for example, 300 μm or less, preferably 200 μm or less. The surface of the resin substrate may be subjected to any suitable surface treatment (e.g., corona treatment) or may have an easy-adhesion layer formed thereon, which can improve the adhesion between the resin substrate and the PVA-based resin layer.
[0018] The coating liquid is typically a solution in which a PVA resin and a halide are dissolved in a solvent. Any appropriate resin may be used as the PVA-based resin. Examples include polyvinyl alcohol and ethylene-vinyl alcohol copolymer. Polyvinyl alcohol is obtained by saponifying polyvinyl acetate. Ethylene-vinyl alcohol copolymer is obtained by saponifying ethylene-vinyl acetate copolymer. The saponification degree of the PVA-based resin is usually 85 mol% to 100 mol%, preferably 95.0 mol% to 99.95 mol%, more preferably 99.0 mol% to 99.93 mol%, and even more preferably 99.0 mol% to 99.5 mol%. The saponification degree can be measured in accordance with JIS K 6726-1994. By using a PVA-based resin with such a saponification degree, a thin polarizing film with excellent durability can be obtained. If the saponification degree is too high, gelation may occur.
[0019] The average degree of polymerization of the PVA resin can be appropriately selected depending on the purpose. The average degree of polymerization is, for example, 1000 or more, preferably 1500 or more, more preferably 2000 or more, and even more preferably 3000 or more, and is, for example, 10000 or less, preferably 6000 or less, and even more preferably 4300 or less. The average degree of polymerization can be measured in accordance with JIS K 6726-1994.
[0020] In one embodiment, the PVA-based resin may contain acetoacetyl-modified PVA. The content of acetoacetyl-modified PVA in the PVA-based resin is, for example, 5% by mass or more, preferably 8% by mass or more, and, for example, 20% by mass or less, preferably 12% by mass or less. If the PVA-based resin contains acetoacetyl-modified PVA, the mechanical strength of the polarizer can be improved.
[0021] The content of the PVA resin in the coating liquid is, for example, 3 to 20 parts by mass with respect to 100 parts by mass of the solvent. With such a resin concentration, a uniform coating film that adheres closely to the resin substrate can be formed.
[0022] Any suitable halide may be used as the halide. Representative examples of the halide include iodide and sodium chloride. Examples of the iodide include potassium iodide, sodium iodide, and lithium iodide, and preferably potassium iodide. The content of the halide in the coating solution is, for example, 5 parts by mass or more, preferably 10 parts by mass or more, and for example, 20 parts by mass or less, preferably 15 parts by mass or less, relative to 100 parts by mass of the PVA-based resin. When the content of the halide is within such a range, the finally obtained polarizer can be prevented from becoming cloudy.
[0023] Examples of the solvent include water, dimethylsulfoxide, dimethylformamide, dimethylacetamide, N-methylpyrrolidone, various glycols, polyhydric alcohols such as trimethylolpropane, and amines such as ethylenediamine and diethylenetriamine. These can be used alone or in combination. Of the solvents, water is preferred. The coating liquid may contain additives. Examples of additives include plasticizers and surfactants. Examples of plasticizers include polyhydric alcohols such as ethylene glycol and glycerin. Examples of surfactants include nonionic surfactants.
[0024] The thickness of the PVA-based resin layer formed from such a coating liquid before stretching is, for example, 3 μm or more, preferably 5 μm or more, and, for example, 40 μm or less, preferably 30 μm or less.
[0025] Moreover, the laminate 10 including the PVA-based resin layer 13 and the resin substrate 12 is preferably stretched in advance in the longitudinal direction at a predetermined stretch ratio in the air. That is, the auxiliary stretching step is carried out after the laminate preparation step and before the dyeing step. The stretching temperature in the auxiliary stretching step is typically equal to or higher than the glass transition temperature (Tg) of the PVA resin, for example, equal to or higher than 95° C., and preferably equal to or higher than 120° C. The stretching temperature in the auxiliary stretching step is typically equal to or lower than 150° C. The stretching ratio of the laminate in the auxiliary stretching step is 2.1 times or more, preferably 2.3 times or more. If the stretching ratio of the laminate is equal to or more than this lower limit, the orientation of the PVA-based resin layer contained in the laminate can be improved, and the PVA-based resin layer can be stably prevented from dissolving in the dyeing solution. The upper limit of the stretching ratio of the laminate in the auxiliary stretching step is typically 4 times or less. The air-stretching method in the auxiliary stretching step may be fixed-end stretching (e.g., a method of stretching using a tenter stretching machine) or free-end stretching (e.g., a method of uniaxially stretching the laminate by passing it between rolls having different peripheral speeds).
[0026] B-2. Dyeing process In the dyeing process, the PVA-based resin film 1 (raw film 11) is dyed with a dichroic material. Specifically, a dyeing solution is brought into contact with the PVA-based resin film 1 to adsorb the dichroic material. The dichroic material forms a complex with the PVA-based resin. In the dyeing process shown in the figure, the PVA-based resin film 1 is immersed in a dye bath (dyeing solution). In the following, the PVA-based resin film after the dyeing process and before the crosslinking process is referred to as dyed film 1b.
[0027] Examples of the dichroic substance include iodine and organic dyes. The dichroic substances can be used alone or in combination. Among the dichroic substances, iodine is preferable. The dye solution is typically an aqueous iodine solution. The iodine content in the dye solution is, for example, 0.05 parts by mass or more, preferably 0.5 parts by mass or more, and for example, 3 parts by mass or less, relative to 100 parts by mass of water. The staining solution preferably further contains an iodine compound. When the staining solution contains an iodine compound, the solubility of iodine in water can be improved. Examples of iodine compounds include potassium iodide, lithium iodide, sodium iodide, zinc iodide, aluminum iodide, lead iodide, copper iodide, barium iodide, calcium iodide, tin iodide, and titanium iodide. The iodine compounds can be used alone or in combination. Among the iodine compounds, potassium iodide is preferred. The mass ratio of iodine to the iodine compound in the dye solution (iodine:iodine compound) is, for example, 1:5 to 1:20, and preferably 1:5 to 1:10, which can impart excellent optical properties to the polarizer. The dyeing solution may also contain boric acid. The concentration of boric acid in the dyeing solution is, for example, 1.0% by mass or less, preferably 0.5% by mass or less, more preferably 0.45% by mass or less, particularly preferably 0.30% by mass or less, and is, for example, 0% by mass or more, preferably 0.1% by mass or more. If the concentration of boric acid in the dyeing solution is within the above range, uneven dyeing in the polarizer can be more stably suppressed.
[0028] The temperature of the dyebath is, for example, 10° C. or more, preferably 20° C. or more, and, for example, 50° C. or less, preferably 40° C. or less. The immersion time in the dyeing step is, for example, 5 seconds or more, preferably 30 seconds or more, and, for example, 300 seconds or less, preferably 90 seconds or less, more preferably 60 seconds or less. The method of adsorbing the dichroic material in the dyeing step is not limited to the above-mentioned immersion method. For example, the dyeing solution may be applied to the raw film, or the dyeing solution may be sprayed onto the raw film. When the raw film is a single-layer resin film or a resin film supported on a resin substrate, the PVA-based resin film may be stretched in the dyeing step.
[0029] B-3. Crosslinking process In the crosslinking step, the dyed film 1b is brought into contact with an aqueous solution of boric acid as a crosslinking liquid. Typically, the dyed film 1b is immersed in an aqueous solution of boric acid (crosslinking bath). In the following, the PVA-based resin film after the crosslinking step and before the stretching step is referred to as a crosslinked film 1c. When the dyed film is contacted with an aqueous solution of boric acid, the boric acid generates tetrahydroxyborate anions in the aqueous solution and crosslinks with the PVA resin by hydrogen bonding, or crosslinks with the hydroxyl group of the PVA resin by dehydration condensation to form a borate ester. This can prevent the PVA resin and the dichroic substance (preferably iodine) from eluting. Therefore, the ratio (A580_c / A580_b) of the orthogonal absorbance A580_c at a wavelength of 580 nm of the crosslinked film 1c to the orthogonal absorbance A580_b at a wavelength of 580 nm of the dyed film 1b can be adjusted to be equal to or higher than the lower limit.
[0030] In one embodiment, the ratio (A480_c / A480_b) of the orthogonal absorbance A480_c of the crosslinked film 1c at a wavelength of 480 nm to the orthogonal absorbance A480_b of the dyed film 1b at a wavelength of 480 nm is typically 1.10 or more, preferably 1.20 or more, and more preferably 1.24 or more. The upper limit of A480_c / A480_b is typically 2.5 or less, preferably 2.1 or less, and more preferably 1.50 or less. When the above-mentioned A580_c / A580_b is the above-mentioned lower limit or more and the above-mentioned A480_c / A480_b is the above-mentioned lower limit or more and / or the above-mentioned upper limit or less, uneven dyeing in the polarizer can be more significantly suppressed.
[0031] The content of boric acid in the crosslinking liquid is, for example, 1 part by mass or more, preferably 3 parts by mass or more, and for example, 10 parts by mass or less, preferably 8 parts by mass or less, relative to 100 parts by mass of water. The crosslinking liquid preferably further contains the above-mentioned iodine compound, which can prevent the iodine adsorbed to the dyed film from eluting. The content of the iodine compound in the crosslinking liquid is, for example, 0.1 parts by mass or more, preferably 1 part by mass or more, and for example, 8 parts by mass or less, preferably 5 parts by mass or less, relative to 100 parts by mass of water. The mass ratio of the iodine compound to boric acid in the crosslinking liquid (iodine compound:boric acid) is, for example, 1:1 to 1:3, preferably 1:1.5 to 1:2. The temperature of the crosslinking bath is, for example, 20° C. or more, preferably 30° C. or more, and, for example, 60° C. or less, preferably 50° C. or less. The immersion time in the crosslinking step is, for example, 5 seconds or more, preferably 10 seconds or more, and, for example, 200 seconds or less, preferably 60 seconds or less. When the raw film is a single-layer resin film or a resin film supported on a resin substrate, the PVA-based resin film may be stretched in the crosslinking step.
[0032] B-4.Stretching process In the stretching step, the crosslinked film 1c is stretched in the longitudinal direction in a stretching bath (stretching liquid). In the following, the PVA-based resin film after the stretching step is referred to as a stretched film 1d. The stretching ratio in the stretching step varies depending on whether or not the original film is subjected to an auxiliary stretching step. When the original film is not subjected to an auxiliary stretching step (i.e., when the original film is a single-layer resin film or a resin film supported by a resin substrate), the stretching ratio in the stretching step is, for example, 4.5 times or more and 7 times or less, preferably 5 times or more and 6.5 times or less. When the PVA-based resin film is stretched in the dyeing step and / or crosslinking step (and further insolubilization step as necessary), the stretching ratio in the stretching step is adjusted so that the product of the stretching ratio in these steps falls within the above range. When the auxiliary stretching step is performed on the raw film (i.e., when the raw film is a PVA-based resin layer formed by coating on a resin substrate), the stretching ratio in the stretching step is, for example, 1.5 to 4 times, preferably 1.5 to 3 times. The product of the stretching ratio in the auxiliary stretching step and the stretching ratio in the stretching step is, for example, 4.5 to 7 times, preferably 5 to 6.5 times. By stretching at the above-mentioned stretch ratio, it is possible to impart extremely excellent optical properties to the polarizer.
[0033] The stretching liquid is typically an aqueous solution of boric acid. The content of boric acid in the stretching liquid (aqueous solution of boric acid) is, for example, 1 part by mass or more, preferably 3 parts by mass or more, and for example, 10 parts by mass or less, preferably 8 parts by mass or less, relative to 100 parts by mass of water. The stretching liquid preferably further contains the above-mentioned iodine compound, which can prevent iodine adsorbed to the crosslinked film from being eluted. The content of the iodine compound in the stretching solution is, for example, 0.1 parts by mass or more, preferably 1 part by mass or more, and for example, 10 parts by mass or less, preferably 6 parts by mass or less, relative to 100 parts by mass of water. The mass ratio of boric acid to the iodine compound (boric acid:iodine compound) in the stretching solution is, for example, 1:0.5 to 1:1.2, preferably 1:0.6 to 1:1. The temperature of the stretching bath is, for example, 40° C. or more, preferably 60° C. or more, and, for example, 85° C. or less, preferably 80° C. or less. The immersion time in the stretching step is, for example, 15 seconds or more and 300 seconds or less.
[0034] B-5.Hue adjustment process In the hue adjusting step, typically, the stretched film 1d is immersed in a hue adjusting bath (hue adjusting liquid). In the following, the stretched film that has been subjected to the hue adjusting step is referred to as a hue adjusted film 1e. The hue adjusting liquid is typically an aqueous solution of an iodine compound. The aqueous solution of an iodine compound is a solution in which the above-mentioned iodine compound is dissolved in water. The aqueous solution of an iodine compound does not substantially contain boric acid. The content ratio of the iodine compound in the hue adjusting liquid is, for example, 0.5 parts by mass or more, preferably 2 parts by mass or more, and, for example, 10 parts by mass or less, preferably 6 parts by mass or less, relative to 100 parts by mass of water. The temperature of the hue adjusting bath is, for example, 0° C. or more, preferably 10° C. or more, and for example, 40° C. or less, preferably 30° C. or less. The immersion time in the hue adjusting step is, for example, 5 seconds or more, preferably 10 seconds or more, and for example, 200 seconds or less, preferably 60 seconds or less.
[0035] B-6. Drying shrinkage process In the drying shrinkage step, typically, the stretched film 1d (preferably the hue adjusting film 1e) is heated while being transported in the longitudinal direction. In the following, the stretched film that has been subjected to the drying shrinkage step is referred to as the dried shrinkage film 1f. In the illustrated example, the drying shrinkage step is performed by the heating and drying section 23. The heating and drying section may be of a zone heating type in which the entire inside of the heating and drying section is heated, or may be of a heated roll drying type in which the transport roll is heated. The heating and drying section preferably uses both of these. The internal temperature of the heating and drying section is, for example, 70° C. or higher, preferably 80° C. or higher, and, for example, 120° C. or lower, preferably 100° C. or lower. The surface temperature of the heating roll is, for example, 60° C. or more, preferably 70° C. or more, and, for example, 100° C. or less, preferably 80° C. or less. Drying with a heating roll efficiently suppresses the heat curl of the stretched film (laminate), and a polarizer with excellent appearance can be efficiently produced. In the drying shrinkage step, the stretched film is brought into contact with the heating roll and shrinks in the width direction perpendicular to the longitudinal direction. The shrinkage rate in the width direction of the stretched film in the drying shrinkage step is, for example, 2% or more, preferably 4% or more. If the shrinkage rate in the width direction is equal to or more than such a lower limit, the orientation of the PVA and the PVA / dichroic substance complex (iodine complex) can be improved, and the optical properties of the polarizer can be improved. The shrinkage rate of the stretched film in the width direction is typically 10% or less, preferably 8% or less, and more preferably 6% or less. When the shrinkage rate in the width direction is equal to or less than such an upper limit, the occurrence of defects in appearance such as wrinkles in the polarizer can be suppressed. Thereafter, the stretched film 1d (preferably the dry shrink film 1f) is wound into a roll as required to form a take-up roll 22.
[0036] C.Polarizer In this manner, a polarizer is manufactured. More specifically, when the raw film is a single-layer resin film, a single-layer polarizer is manufactured, and when the raw film is laminated on a resin substrate, a polarizing plate having a polarizer / resin substrate structure is manufactured (i.e., the resin substrate is used as a protective layer for the polarizer). The thickness of the polarizer is, for example, 80 μm or less, preferably 15 μm or less, more preferably 12 μm or less, and even more preferably 8 μm or less. When the raw film is a PVA-based resin layer formed by coating on a resin substrate, the thickness of the polarizer (i.e., the PVA-based resin layer) can be 12 μm or less, preferably 8 μm or less. The thickness of the polarizer is typically 1 μm or more, and preferably 3 μm or more.
[0037] The polarizer preferably exhibits absorption dichroism at any wavelength of 380 nm to 780 nm. Such a polarizer has excellent single transmittance and degree of polarization. The single transmittance of the polarizer is, for example, 41.0% or more and 46.0% or less, and preferably 42.0% or more and 45.0% or less. The degree of polarization of the polarizer is preferably 97.0% or more, more preferably 99.0% or more, and even more preferably 99.5% or more. According to the above-mentioned method for producing a polarizer, in a polarizer in which the single transmittance and the degree of polarization are each within the above range, uneven dyeing can be significantly suppressed.
[0038] A polarizer can also be manufactured by laminating any suitable protective film according to the purpose to the polarizer manufactured as described above. When the polarizer is laminated on a resin substrate, the resin substrate may be peeled off from the polarizer, and a protective film may be laminated on the peeled surface. Specific examples of materials that are the main components of the protective film include cellulose-based resins such as triacetyl cellulose (TAC), and transparent resins such as polyesters, polyvinyl alcohols, polycarbonates, polyamides, polyimides, polyethersulfones, polysulfones, polystyrenes, polynorbornenes, polyolefins, (meth)acrylics, and acetates. In addition, thermosetting resins or ultraviolet-curing resins such as (meth)acrylics, urethanes, (meth)acrylic urethanes, epoxy resins, and silicones are also included. Note that "(meth)acrylic resin" refers to acrylic resins and / or methacrylic resins. In addition, glassy polymers such as siloxane polymers are also included. In addition, the polymer films described in JP 2001-343529 A (WO01 / 37007) can also be used. The material for this film may be, for example, a resin composition containing a thermoplastic resin having a substituted or unsubstituted imide group in the side chain, and a thermoplastic resin having a substituted or unsubstituted phenyl group and a nitrile group in the side chain, such as a resin composition containing an alternating copolymer of isobutene and N-methylmaleimide, and an acrylonitrile-styrene copolymer. The polymer film may be, for example, an extrusion molded product of the above resin composition. EXAMPLES
[0039] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. The methods for measuring the various properties are as follows.
[0040] (1) Measurement of orthogonal absorbance in PVA resin film In each example and each comparative example, the cross transmittance Tc of the PVA-based resin film after the dyeing process and before the crosslinking process, and after the crosslinking process and before the stretching process was measured using an ultraviolet-visible spectrophotometer (V-7100 manufactured by JASCO Corporation). Tc is the Y value measured with a 2-degree visual field (C light source) according to JIS Z8701 and corrected for visibility. In addition, the orthogonal absorbance was calculated according to the following formula using the Tc measured at the wavelengths shown in Table 1. The results are shown in Table 1. Orthogonal absorbance = log10(100 / Tc)
[0041] (2) Measurement of single unit transmittance The single transmittance (Ts) of the polarizer film obtained in each Example and Comparative Example was measured using an ultraviolet-visible spectrophotometer (manufactured by JASCO Corporation, product name "V7100"). The results are shown in Table 1. When a polarizer was included in a polarizing plate, the resin substrate of the polarizing plate (test piece) was peeled off from the polarizer in advance.
[0042] (3) Measurement of crystallization index In each of the Examples and Comparative Examples, the crystallization index of the PVA-based resin layer (PVA-based resin film) was measured by the ATR method using a Fourier transform infrared spectrophotometer. Specifically, the measurement was performed using polarized light as the measurement light, and the 1141 cm -1 Intensity (IC) and 1440cm -1 The crystallization index was calculated according to the following formula (1) using the intensity (IR). Crystallization index = (IC / IR) (1)
[0043] (4) Evaluation of dye unevenness The state of uneven dyeing (streaks) of the polarizers obtained in each of the Examples and Comparative Examples was visually observed from a distance of 50 mm in the perpendicular direction and evaluated according to the following criteria. The results are shown in Table 1. A: No unevenness is visible. B: Slight unevenness is visible. C: Unevenness is visible.
[0044] <<Example 2 ~ 5 and reference examples 1、 6>> As a thermoplastic resin substrate, a long amorphous isophthalic copolymerized polyethylene terephthalate film (thickness: 100 μm) having a Tg of about 75° C. was used, and one side of the resin substrate was subjected to a corona treatment. A PVA aqueous solution (coating solution) was prepared by adding 13 parts by mass of potassium iodide to 100 parts by mass of a PVA-based resin prepared by mixing polyvinyl alcohol (polymerization degree 4200, saponification degree 99.2 mol%) and acetoacetyl-modified PVA (manufactured by Nippon Synthetic Chemical Industry Co., Ltd., product name "GOHSEFFIMER") in a 9:1 ratio. The solution was dissolved in water. The above PVA aqueous solution was applied to the corona-treated surface of a resin substrate and dried at 60° C. to form a PVA-based resin layer with a thickness of 13 μm, thereby producing a laminate (laminate production step). The obtained laminate was uniaxially stretched in the longitudinal direction (longitudinal direction) at an auxiliary stretching ratio of 2.4 times in an oven at 130°C (auxiliary stretching step). The PVA-based resin layer contained in the laminate after the auxiliary stretching and before the dyeing step was subjected to the measurement of the crystallization index described above. The crystallization index of the PVA-based resin layer was 1.82. Next, the laminate was immersed in a dye bath (an aqueous iodine solution obtained by mixing iodine and potassium iodide in a mass ratio of 1:7 with respect to 100 parts by mass of water) at a liquid temperature of 30° C. for 60 seconds (dyeing step). In Examples 2 to 5 and Reference Example 6, the dye bath contained boric acid. Table 1 shows the concentration of boric acid in the dye solution. Next, the laminate was immersed in a crosslinking bath (a boric acid aqueous solution obtained by mixing 3 parts by mass of potassium iodide and 5 parts by mass of boric acid with respect to 100 parts by mass of water) at a liquid temperature of 40° C. for 30 seconds (crosslinking step). The PVA-based resin layer included in the laminate was subjected to the above-mentioned orthogonal absorbance measurement after the dyeing step and before the crosslinking step, and after the crosslinking step and before the stretching step. Thereafter, the laminate was immersed in a stretching bath (a boric acid aqueous solution obtained by blending 5 parts by mass of potassium iodide and 4 parts by mass of boric acid with respect to 100 parts by mass of water) at a liquid temperature of 70°C, and uniaxially stretched in the longitudinal direction (longitudinal direction) between rolls with different peripheral speeds so that the total stretch ratio was 5.5 times (stretching process). Thereafter, the laminate was immersed in a hue adjusting bath (an aqueous solution obtained by mixing 4 parts by mass of potassium iodide with 100 parts by mass of water) having a liquid temperature of 20° C. (hue adjusting step). Thereafter, the laminate was brought into contact with a SUS heated roll having a surface temperature maintained at about 75° C. while being dried in an oven maintained at about 90° C. (drying shrinkage process). In this way, a polarizer having a thickness of about 5 μm was formed on the resin substrate, and a polarizing plate having a polarizer / resin substrate structure was obtained. The polarizer included in the polarizing plate was subjected to the measurement of the single transmittance described above. In addition, the uneven dyeing (striped unevenness) of the polarizer was evaluated as described above.
[0045] << Reference example 7>> A polarizing plate having a polarizer / resin substrate structure was obtained in the same manner as in Example 1, except that the proportion of water was adjusted so that the single transmittance was 44%. The polarizer included in the polarizing plate was subjected to the measurement of the single transmittance described above. In addition, the uneven dyeing (streaky unevenness) of the polarizer was evaluated as described above.
[0046] << reference Example 8>> A polyvinyl alcohol-based film (PVA-based resin film) having a thickness of 30 μm was used as the raw film. The PVA-based resin film was subjected to the following steps in the following order. (Insolubilization step) A 4% by mass aqueous solution of boric acid was used as the treatment liquid for the insolubilization bath. The PVA-based resin film was transported to the insolubilization bath (aqueous boric acid solution), immersed in the boric acid solution adjusted to 30°C for 60 seconds, swollen, and further uniaxially stretched to a stretching ratio of 1.6 times. (Dyeing process) As a treatment liquid for the dye bath, an iodine dyeing solution with a concentration of 0.3% by mass of iodine:potassium iodide (mass ratio = 0.5:8) was used. The insolubilized PVA resin film was transported to the dye bath and dyed while immersed in the iodine dyeing solution adjusted to 30°C for 60 seconds and uniaxially stretched to a stretch ratio of 2.4 times the original length. (Crosslinking step) A boric acid aqueous solution containing 5% by mass of boric acid and 3% by mass of potassium iodide was used as the treatment liquid for the crosslinking bath. The dyed PVA resin film was transported to the crosslinking bath and crosslinked with boric acid while immersing for 45 seconds in the boric acid aqueous solution adjusted to 40°C and uniaxially stretching to a total stretch ratio of 3.3 times the original length. The PVA-based resin film was subjected to the above-mentioned orthogonal absorbance measurement after the dyeing step and before the crosslinking step, and after the crosslinking step and before the stretching step. (Stretching step) A boric acid aqueous solution containing 4% by mass of boric acid and 5% by mass of potassium iodide was used as the treatment liquid for the stretching bath. The crosslinked PVA resin film was transported to the stretching bath and uniaxially stretched to a total stretch ratio of 6 times the original length while being immersed in the boric acid aqueous solution adjusted to 60°C for 30 seconds. (Hue Adjustment Step) As a treatment liquid for the hue adjustment bath, an aqueous solution containing 3% by mass of potassium iodide was used. The PVA resin film subjected to the stretching treatment was transported to the hue adjustment bath and immersed in the aqueous solution adjusted to 27° C. for 10 seconds. (Drying and shrinking step) Next, the PVA-based resin film that had been subjected to the above-mentioned hue adjustment treatment was dried in an oven at 60° C. for 4 minutes to obtain a polarizer. In this way, a polarizer made of a PVA-based resin film was obtained. The polarizer was subjected to the measurement of the single-piece transmittance as described above. In addition, the uneven dyeing (streaky unevenness) of the polarizer was evaluated as described above.
[0047] <<Reference example 9>> Except that the insolubilization step was not performed, the laminate after the auxiliary stretching step was subjected to the dyeing step. Reference example A polarizer was obtained in the same manner as in Example 8. The polarizer was subjected to the measurement of the single transmittance as described above. In addition, the uneven dyeing (streaky unevenness) of the polarizer was evaluated as described above.
[0048] <<Comparative Example 1>> A polarizing plate having a polarizer / resin substrate structure was obtained in the same manner as in Example 1, except that after the auxiliary stretching and before the dyeing step, the laminate was immersed in an insolubilizing bath (a boric acid aqueous solution obtained by mixing 4 parts by mass of boric acid with 100 parts by mass of water) having a liquid temperature of 40°C for 30 seconds (i.e., the insolubilizing step was performed). The polarizer included in the polarizing plate was subjected to the measurement of the single transmittance described above. In addition, the uneven dyeing (striped unevenness) of the polarizer was evaluated as described above.
[0049] <<Comparative Example 2>> After the auxiliary stretching and before the dyeing step, the laminate was immersed in an insolubilizing bath (a boric acid aqueous solution obtained by mixing 4 parts by mass of boric acid with 100 parts by mass of water) having a liquid temperature of 40° C. for 30 seconds (i.e., an insolubilizing step was performed). Reference example A polarizing plate having a polarizer / resin substrate structure was obtained in the same manner as in 7. The polarizer included in the polarizing plate was subjected to the measurement of the single transmittance described above. In addition, the uneven dyeing (streaky unevenness) of the polarizer was evaluated as described above.
[0050] [Table 1]
[0051] [evaluation] As is clear from Table 1, when the ratio (A580_c / A580_b) of the orthogonal absorbance A580_c of the PVA-based resin film after the crosslinking process and before the stretching process to the orthogonal absorbance A580_b of the PVA-based resin film after the dyeing process and before the crosslinking process is 0.91 or more, a polarizer with suppressed dyeing unevenness can be produced. [Industrial Applicability]
[0052] The manufacturing method according to the embodiment of the present invention can be suitably used for manufacturing polarizers and polarizing plates applied to image display devices. [Explanation of symbols]
[0053] 1 PVA resin film 10 Laminate 12 Thermoplastic resin substrate
Claims
1. A dyeing step of dyeing the polyvinyl alcohol-based resin film with a dichroic substance; a crosslinking step of contacting the polyvinyl alcohol-based resin film after the dyeing step with an aqueous boric acid solution; A stretching step of stretching the polyvinyl alcohol-based resin film after the crosslinking step in a stretching bath, a ratio of an orthogonal absorbance A580_c at a wavelength of 580 nm of the polyvinyl alcohol-based resin film after the crosslinking step and before the stretching step to an orthogonal absorbance A580_b at a wavelength of 580 nm of the polyvinyl alcohol-based resin film after the dyeing step and before the crosslinking step is 0.92 or more and less than 1.21; a ratio of an orthogonal absorbance A480_c at a wavelength of 480 nm of a polyvinyl alcohol-based resin film after the crosslinking step and before the stretching step to an orthogonal absorbance A480_b at a wavelength of 480 nm of a polyvinyl alcohol-based resin film after the dyeing step and before the crosslinking step is 1.50 or less.
2. The method for producing a polarizer according to claim 1 , wherein the method produces a polarizer having a single transmittance of 42% or more and 45% or less.
3. a laminate preparation step of applying a coating liquid containing a polyvinyl alcohol-based resin and a halide onto a long thermoplastic resin substrate to prepare a laminate including a polyvinyl alcohol-based resin layer as the polyvinyl alcohol-based resin film and the thermoplastic resin substrate; an auxiliary stretching step of stretching the laminate in air; The dyeing step; The crosslinking step; The stretching step; a drying shrinking step of shrinking the polyvinyl alcohol-based resin layer after the stretching step in a width direction perpendicular to the longitudinal direction while transporting the polyvinyl alcohol-based resin layer in the longitudinal direction, in that order.
4. The method for producing a polarizer according to claim 3 , wherein the thermoplastic resin substrate is a polyethylene terephthalate film.
5. The method for producing a polarizer according to claim 3 or 4, wherein a polarizer having a thickness of 12 μm or less is produced.
6. The method for producing a polarizer according to any one of claims 1 to 5, wherein the stretching bath is an aqueous solution of boric acid.
7. A method for producing a polarizing plate, comprising laminating a protective film to a polarizer produced by the method for producing a polarizer according to any one of claims 1 to 6.
Citation Information
Patent Citations
Polarizing film, optical film laminate including polarizing film, extended laminate to be used for manufacturing optical film laminate including polarizing film, method for manufacturing these laminates, and organic el display device having polarizing film
JP2017068282A
JPB23145747B
Highly functional thin polarizing film and process for producing same
WO2010100917A1
Layered object, polarizing film, and process for producing polarizing film
WO2014024712A1
Raw film for manufacturing optical films
WO2015104966A1