Resin composition, cured molded product, fiber-reinforced plastic molding material, fiber-reinforced plastic, fiber-reinforced plastic laminate molded product, and method for producing same
A resin composition combining bifunctional epoxy and polycarbonate resins with a specific weight ratio and thermal crosslinking addresses the challenge of achieving high heat resistance and mechanical strength in FRP, enabling durable applications like aircraft parts and electrical equipment.
Patent Information
- Application Number
- JP2021509500
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-03-29
- Filing Date
- 2020-03-25
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2040-03-25
AI Technical Summary
Existing fiber-reinforced plastics (FRP) compositions face challenges in achieving both excellent heat resistance and mechanical strength, particularly due to issues with adhesion between polycarbonate resin and other resins, leading to potential peeling under stress and limited applications.
A resin composition comprising a first resin, such as a bifunctional epoxy resin with a weight average molecular weight of 4,000 or more, and a second resin, such as polycarbonate resin, with a specific weight ratio of 9:1 to 3:7, which undergoes thermal crosslinking to form a cured product with a glass transition temperature of 100°C or higher and no melting point, enhancing interlayer bonding through a crosslinking reaction.
The composition provides a cured product with superior heat resistance and mechanical strength, suitable for applications requiring structural integrity and durability, such as aircraft parts and electrical equipment.
Smart Images

Figure 0007566726000006 
Figure 0007566726000007 
Figure 0007566726000008
Abstract
Description
[Technical field]
[0001] The present invention relates to a resin composition, a cured molded product utilizing the resin composition, a fiber-reinforced plastic molding material, a fiber-reinforced plastic, a fiber-reinforced plastic laminate molded product, and a method for producing the same. [Background technology]
[0002] Fiber-reinforced plastics (FRP), typified by carbon fiber reinforced plastics (CFRP), are lightweight, high-strength materials that are widely used in a variety of applications, from sports goods such as bicycles and tennis rackets to various components for automobiles, railway vehicles, and aircraft.
[0003] Phenoxy resin, which is a thermoplastic resin, has good moldability and excellent adhesiveness, and can be made to exhibit properties similar to those of highly heat-resistant thermosetting resins by using a crosslinking agent. As a technology that uses phenoxy resin, for example, a powder of a resin composition in which phenoxy resin or phenoxy resin is mixed with a crystalline epoxy resin and an acid anhydride as a crosslinking agent is applied to a reinforced fiber substrate by a powder coating method to produce a prepreg, which is then molded and cured by a hot press to produce a fiber-reinforced plastic (FRP) (Patent Document 1).
[0004] On the other hand, polycarbonate resin, which is a thermoplastic resin, has excellent mechanical strength and heat resistance, and is widely used for industrial applications such as various electrical and electronic devices, automobiles, etc. In addition, polycarbonate resin reinforced with glass fiber has excellent strength and rigidity, and is used for the housings of various electrical and electronic devices.
[0005] For the purpose of improving the mechanical strength and other performance of FRP, for example, it has been proposed to mix a small amount of one or more hydroxyl group-containing polymers selected from a phenoxy resin or an epoxy resin with a polycarbonate resin (Patent Document 2).In addition, it has been proposed to mix a small amount of phenoxy resin with an aromatic polycondensation polymer such as polyarylethersulfone, polyaryletherketone, polycarbonate, or polyetherimide (Patent Document 3). However, Patent Document 2 states that if the ratio of the hydroxyl group-containing polymer in the resin component exceeds 50% by weight, sufficient mechanical strength cannot be obtained. Furthermore, Patent Document 3 states that the concentration of the phenoxy resin is about 30% by weight or less of the total composition weight including the fibers, which is even less than that of Patent Document 2. Furthermore, Patent Document 3 does not specifically disclose an example of adding a phenoxy resin to a polycarbonate resin.
[0006] In recent years, the use of thermoplastic resins has been actively considered in order to impart impact resistance, recyclability, etc. to CFRP. For example, rather than simply replacing the matrix resin with a thermoplastic resin, it has been proposed to blend thermoplastic resin particles into an epoxy resin matrix and to place a thermoplastic resin film in the intermediate layer of CFRP (Patent Document 4).
[0007] Other proposals include placing a layer containing phenoxy resin as an adhesive layer on the outermost layer of a CFRP that uses thermoplastic resin (Patent Document 5), and a CFRP molding material in which two different types of thermoplastic resins are placed on either side of a mat-like substrate made of short reinforcing fibers (Patent Document 6).
[0008] The polycarbonate resins described in Patent Documents 4 to 6 as resins that are preferably used are characterized by being particularly excellent in impact resistance among thermoplastic resins, but have the drawback of being somewhat inferior in adhesion to other resins. Therefore, when used in structural members, there is a risk that peeling may occur due to external stress, greatly reducing the strength of the structure, and the uses and locations of application are limited. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] International Publication No. WO2016 / 152856 [Patent Document 2] Patent No. 2968388 [Patent Document 3] Special Publication No. 2005-536597 [Patent Document 4] Patent No. 6278286 [Patent Document 5] WO2018 / 124215 [Patent Document 6] Patent No. 5626330 Summary of the Invention [Problem to be solved by the invention]
[0010] An object of the present invention is to provide a novel resin composition which has excellent heat resistance and mechanical strength and is useful as a material for, for example, FRP, and uses thereof. [Means for solving the problem]
[0011] The resin composition of the present invention is a resin composition that contains a first resin and a second resin different from the first resin and exhibits curability by thermal crosslinking. In the resin composition of the present invention, the first resin is at least one selected from the group consisting of a difunctional epoxy resin having a weight average molecular weight of 4,000 or more and a phenoxy resin, and the second resin is a polycarbonate resin.
[0012] In the resin composition of the present invention, the content ratio of the first resin to the second resin (first resin:second resin) may be within a range of 9:1 to 3:7 by weight.
[0013] In the resin composition of the present invention, both of the first resin and the second resin may have a bisphenol skeleton in the molecule.
[0014] The resin composition of the present invention may have a glass transition temperature (Tg) of 100°C or higher as measured by dynamic mechanical analysis (DMA) of a cured product obtained by thermally crosslinking the resin composition, and the cured product may not have a melting point (Tm).
[0015] The resin composition of the present invention may be such that the displacement of a probe after measurement at a temperature in the range of 25°C to 300°C in dynamic mechanical analysis (DMA) of a cured product obtained by thermally crosslinking the resin composition is less than -1 mm relative to the displacement before the measurement.
[0016] The cured molded product of the present invention comprises a cured product of any of the resin compositions described above.
[0017] The fiber-reinforced plastic molding material of the present invention comprises a reinforcing fiber substrate and a powder of any one of the above resin compositions adhered to the reinforcing fiber substrate.
[0018] The fiber-reinforced plastic of the present invention has a reinforcing fiber substrate and a cured product of any of the above-mentioned resin compositions adhered to the reinforcing fiber substrate.
[0019] The fiber-reinforced plastic laminate molding of the present invention is a fiber-reinforced plastic laminate molding that contains a phenoxy resin, a polycarbonate resin, and reinforcing fibers and is composed of multiple layers. The fiber-reinforced plastic laminate molding of the present invention is characterized in that it includes one or more interlayer bonding sites where the layer containing the phenoxy resin and the layer containing the polycarbonate resin are bonded by a crosslinking reaction at the lamination interface between the two layers.
[0020] The fiber-reinforced plastic laminate of the present invention may have layers containing the phenoxy resin and layers containing the polycarbonate resin laminated alternately.
[0021] In the fiber-reinforced plastic laminate of the present invention, the interlayer bonded portion bonded by the crosslinking reaction may have an interlayer shear strength of 40 MPa or more as measured by the ILSS method.
[0022] In the fiber-reinforced plastic laminate of the present invention, the reinforcing fibers may be continuous fibers selected from at least one type selected from carbon fibers, glass fibers, ceramic fibers, metal fibers, and organic fibers.
[0023] A method for producing a fiber-reinforced plastic laminate according to a first aspect of the present invention is a method for producing any one of the above fiber-reinforced plastic laminates, The material is characterized in that a fiber-reinforced plastic molding material having a phenoxy resin as a matrix resin and a fiber-reinforced plastic molding material having a polycarbonate resin as a matrix resin are laminated together and molded at a temperature of 260°C or higher.
[0024] A method for producing a fiber-reinforced plastic laminate according to a second aspect of the present invention is a method for producing any one of the above fiber-reinforced plastic laminates, A step of preparing a plurality of fiber-reinforced plastic molding materials, each of which has a reinforcing fiber substrate coated on one side with a phenoxy resin and coated on the other side with a polycarbonate resin; A step of laminating a plurality of the fiber-reinforced plastic molding materials so as to include a lamination boundary where the phenoxy resin and the polycarbonate resin are in contact with each other, and performing a molding process at a temperature of 260°C or higher; The present invention is characterized by comprising:
[0025] In the manufacturing method for a fiber-reinforced plastic laminate according to the second aspect of the present invention, a fiber-reinforced plastic molding material having a phenoxy resin as a matrix resin and / or a fiber-reinforced plastic molding material having a polycarbonate resin as a matrix resin may be interposed between the plurality of fiber-reinforced plastic molding materials.
[0026] In the method for producing a fiber-reinforced plastic laminate according to the second aspect of the present invention, a phenoxy resin film and / or a polycarbonate resin film may be interposed between the plurality of fiber-reinforced plastic molding materials.
[0027] A method for producing a fiber-reinforced plastic laminate according to a third aspect of the present invention is a method for producing any one of the fiber-reinforced plastic laminates described above, The material is characterized by being made by laminating a fiber-reinforced plastic molding material having a phenoxy resin as a matrix resin with a polycarbonate resin film, and then molding the laminate at a temperature of 260°C or higher.
[0028] A method for producing a fiber-reinforced plastic laminate according to a fourth aspect of the present invention is a method for producing any one of the above fiber-reinforced plastic laminates, This product is characterized by laminating a fiber-reinforced plastic molding material having a polycarbonate resin as a matrix resin and a phenoxy resin film, and then molding the laminate at a temperature of 260°C or higher.
[0029] The fiber-reinforced plastic molding material of the present invention comprises a reinforcing fiber substrate, a coating layer of phenoxy resin formed on one surface of the reinforcing fiber substrate, and a coating layer of polycarbonate resin formed on the other surface of the reinforcing fiber substrate.
[0030] In the fiber-reinforced plastic molding material of the present invention, the reinforcing fiber substrate may be a woven fabric made of continuous fibers or a UD material in which continuous fibers are aligned in one direction. Effect of the Invention
[0031] According to the resin composition of the present invention, it is possible to provide a resin material having excellent heat resistance and mechanical strength, and therefore the resin composition of the present invention can be preferably used for producing various resin molded products and composite materials such as FRP, which require heat resistance and strength. [Brief description of the drawings]
[0032] [Figure 1] 1 is a diagram for explaining an outline of a method for producing an FRP laminated body according to one embodiment of the present invention. [Diagram 2] 5 is a diagram for explaining an outline of a method for producing an FRP laminated body according to another embodiment of the present invention. [Diagram 3] 5 is a diagram for explaining an outline of a method for producing an FRP laminated body according to another embodiment of the present invention. [Figure 4] 5 is a diagram for explaining an outline of a method for producing an FRP laminated body according to still another embodiment of the present invention. [Diagram 5] 1 is a diagram showing the measurement results of viscosity of resin compositions obtained in Examples and Comparative Examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0033] Hereinafter, an embodiment of the present invention will be described in detail.
[0034] [Resin composition] The resin composition of the present embodiment is a resin composition that contains a first resin and a second resin different from the first resin and exhibits curability by thermal crosslinking. The first resin is at least one selected from a difunctional epoxy resin having a weight average molecular weight of 4,000 or more (hereinafter, sometimes referred to as a "difunctional epoxy resin") and a phenoxy resin. The second resin is a polycarbonate resin. The resin composition of the present embodiment is composed mainly of either one or both of the first resin and the second resin. Here, the term "main component" refers to the component that is contained in the largest amount among the resin components. In the resin composition of the present embodiment, in order to exhibit the effects of the invention, the total amount of the first resin and the second resin is preferably 50 parts by weight or more, and more preferably 80 parts by weight or more and 100 parts by weight or less, per 100 parts by weight of the total of the resin components. Note that the "resin component" includes thermoplastic resins and thermosetting resins other than bifunctional epoxy resins, phenoxy resins, and polycarbonate resins, but does not include non-resin components such as crosslinking agents.
[0035] <Difunctional epoxy resin> The bifunctional epoxy resin having a weight average molecular weight of 4,000 or more as the first resin means, more specifically, an epoxy resin having a linear high molecular weight with a weight average molecular weight (Mw) in the range of 4,000 or more and less than 10,000, and having epoxy groups at both ends of the molecular chain. Epoxy resins having Mw of less than 4,000 are not suitable because they have a low softening point, tend to block, and are difficult to work with during kneading and to handle as a resin composition. Bifunctional epoxy resins having Mw of 10,000 or more are generally handled as thermoplastic resins called phenoxy resins, which will be described later. The Mw is a value measured by gel permeation chromatography and converted using a standard polystyrene calibration curve.
[0036] As described above, the difunctional epoxy resin as the first resin may be any conventionally known linear difunctional epoxy resin having a weight-average molecular weight of 4,000 or more without any particular limitation, but is preferably a difunctional epoxy resin having a softening point of 90° C. or more and a bisphenol skeleton. Furthermore, the softening point of the difunctional epoxy resin is preferably 100° C. or more, and more preferably 110° C. or more. Examples of such bifunctional epoxy resins having a bisphenol skeleton include bisphenol A type epoxy resins (e.g., Epotohto YD-014, YD-017, YD-019 manufactured by Nippon Steel Chemical & Material Co., Ltd., JER1010 manufactured by Mitsubishi Chemical Corporation, etc.), bisphenol F type epoxy resins (e.g., Epotohto YDF-2005RL manufactured by Nippon Steel Chemical & Material Co., Ltd., JER4007P, JER4009P manufactured by Mitsubishi Chemical Corporation, etc.), bisphenol sulfide type epoxy resins (e.g., YSLV-120TE manufactured by Nippon Steel Chemical & Material Co., Ltd., etc.), etc., but are not limited thereto, and two or more of these may be used in combination.
[0037] In addition, bifunctional epoxy resins and phenoxy resins, which are high molecular weight materials suitable as the first resin, have almost the same chemical structure, but are distinguished from each other in the following points. (1) Phenoxy resins have a Mw of 10,000 or more (more commonly, a Mw of 40,000 or more), whereas epoxy resins have a Mw of less than 10,000 (more commonly, a Mw of around 4,000 to 6,000). (2) The epoxy equivalent of a high molecular weight bifunctional epoxy resin, which is the number of grams containing 1 gram equivalent of epoxy groups, is 700 to 5,000 g / eq, while that of a phenoxy resin is 6,000 g / eq or more. (3) Phenoxy resin has strong thermoplastic resin properties due to its large Mw, and is usually used without the need for a curing agent, whereas high molecular weight bifunctional epoxy resins require a curing agent in normal use. However, when a bifunctional epoxy resin is used in the resin composition of the present embodiment, no curing agent is used.
[0038] <Phenoxy resin> The phenoxy resin as the first resin is a thermoplastic polyhydroxypolyether resin obtained by a condensation reaction between a dihydric phenol compound and an epihalohydrin, or a polyaddition reaction between a dihydric phenol compound and a difunctional epoxy resin, and can be obtained by a conventionally known method in a solvent or without a solvent.
[0039] The phenoxy resin preferably used in the present invention is solid at room temperature and has a melt viscosity of 3,000 Pa·s or less at a temperature of 200° C. or more, more preferably 2,000 Pa·s or less, even more preferably 1,500 Pa·s or less, and most preferably 1,000 Pa·s or less. If the melt viscosity exceeds 3,000 Pa·s, the fluidity of the resin during molding decreases, and the resin does not spread sufficiently, which may cause voids, and is therefore undesirable.
[0040] Examples of dihydric phenol compounds used in the production of phenoxy resins include hydroquinone, resorcinol, 4,4-dihydroxybiphenyl, 4,4'-dihydroxydiphenyl ketone, 2,2-bis(4-hydroxyphenyl)propane (bisphenol A), 1,1-bis(4-hydroxyphenyl)cyclohexane, 1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane, bis(4-hydroxyphenyl)methane, 1,1-bis(4-hydroxyphenyl)ethane, 2,2-bis(4-hydroxyphenyl)butane, 1,1-bis(4-hydroxyphenyl)-1-phenylene, and the like. Examples of such arylethane include bis(4-hydroxyphenyl)diphenylmethane, 2,2-bis(4-hydroxy-3-methylphenyl)propane, 2,2-bis(3-phenyl-4-hydroxyphenyl)propane, 2,2-bis(4-hydroxy-3-tert-butylphenyl)propane, 1,3-bis(2-(4-hydroxyphenyl)propyl)benzene, 1,4-bis(2-(4-hydroxyphenyl)propyl)benzene, 2,2-bis(4-hydroxyphenyl)-1,1,1-3,3,3-hexafluoropropane, and 9,9'-bis(4-hydroxyphenyl)fluorene. Among these, 4,4-dihydroxybiphenyl, 4,4'-dihydroxydiphenyl ketone, 2,2-bis(4-hydroxyphenyl)propane (bisphenol A), or 9,9'-bis(4-hydroxyphenyl)fluorene is particularly preferred.
[0041] In addition, examples of bifunctional epoxy resins used in the production of the phenoxy resin include epoxy oligomers obtained by a condensation reaction between the above-mentioned dihydric phenol compounds and epihalohydrin, such as hydroquinone diglycidyl ether, resorcinol diglycidyl ether, bisphenol S type epoxy resin, bisphenol A type epoxy resin, bisphenol F type epoxy resin, methylhydroquinone diglycidyl ether, chlorohydroquinone diglycidyl ether, 4,4'-dihydroxydiphenyloxide diglycidyl ether, 2,6-dihydroxynaphthalene diglycidyl ether, dichlorobisphenol A diglycidyl ether, tetrabromobisphenol A type epoxy resin, and 9,9'-bis(4)-hydroxyphenyl)fluorene diglycidyl ether. Among these, bisphenol A type epoxy resin, bisphenol S type epoxy resin, hydroquinone diglycidyl ether, bisphenol F type epoxy resin, tetrabromobisphenol A type epoxy resin, or 9,9'-bis(4)-hydroxyphenyl)fluorene diglycidyl ether is preferred.
[0042] The production of the phenoxy resin can be carried out without a solvent or in the presence of a reaction solvent. As the reaction solvent, an aprotic organic solvent, for example, methyl ethyl ketone, dioxane, tetrahydrofuran, acetophenone, N-methylpyrrolidone, dimethyl sulfoxide, N,N-dimethylacetamide, sulfolane, etc. can be suitably used. In addition, the phenoxy resin obtained by the solvent reaction can be made into a solid resin that does not contain a solvent by performing a solvent removal treatment. In addition, in the production of the phenoxy resin, conventionally known polymerization catalysts such as alkali metal hydroxides, tertiary amine compounds, quaternary ammonium compounds, tertiary phosphine compounds, and quaternary phosphonium compounds can be suitably used as reaction catalysts.
[0043] The average molecular weight of the phenoxy resin is usually 10,000 to 200,000 as the weight average molecular weight (Mw), but is preferably 20,000 to 100,000, more preferably 30,000 to 100,000, and most preferably 40,000 to 80,000. If the Mw of the phenoxy resin is too low, the strength of the molded article is inferior, and if it is too high, the workability and processability are likely to be inferior. Note that Mw is a value measured by gel permeation chromatography and converted using a standard polystyrene calibration curve.
[0044] The hydroxyl equivalent (g / eq) of the phenoxy resin is usually 1000 or less, preferably 750 or less, and particularly preferably 500 or less. More specifically, the hydroxyl equivalent (g / eq) of the phenoxy resin is usually 50 to 1,000, preferably 100 to 750, and particularly preferably 200 to 500. If the hydroxyl equivalent is too low, the water absorption rate increases due to the increase in hydroxyl groups, and there is a concern that the mechanical properties will decrease. If the hydroxyl equivalent is too high, there is a concern that the crosslink density will be insufficient and the heat resistance of the cured product will decrease, which is not preferable. In addition, if the hydroxyl equivalent is too high, there are few hydroxyl groups, so the wettability with the reinforcing fiber substrate, especially carbon fiber, will decrease, and sufficient reinforcing effect cannot be expected when reinforcing carbon fiber. Here, the hydroxyl equivalent in this specification means a secondary hydroxyl equivalent. The polymer chain terminal functional group of the phenoxy resin may have either an epoxy group or a hydroxyl group, or both.
[0045] The glass transition temperature (Tg) of the phenoxy resin is preferably 65°C or more and 200°C or less, more preferably 180°C or less, and more preferably in the range of 65°C to 180°C. If the Tg of the phenoxy resin is higher than 200°C, the melt viscosity increases, and it becomes difficult to impregnate the resin composition of the present embodiment without defects such as voids when applied to, for example, FRP. In addition, if the Tg exceeds 200°C, the fluidity of the resin during molding processing decreases, and processing at a higher temperature is required, which is not very preferable. On the other hand, there is no particular limit to the lower limit of Tg as long as there is no problem with processability, but there is no problem if it is about 65°C. If the glass transition temperature is lower than 65°C, the moldability improves, but there is a risk that the tensile modulus retention rate and the dimensional change rate retention rate decrease. The glass transition temperature of the phenoxy resin is measured using a differential scanning calorimeter at a temperature rise rate of 10° C. / min in the range of 20 to 280° C., and is a value determined from the peak value of the second scan.
[0046] As the phenoxy resin, commercially available products can be used, and examples thereof include bisphenol A type phenoxy resin (e.g., Pheno Tohto YP-50, Pheno Tohto YP-50S, and Pheno Tohto YP-55U manufactured by Nippon Steel Chemical & Material Co., Ltd.), bisphenol F type phenoxy resin (e.g., Pheno Tohto FX-316 manufactured by Nippon Steel Chemical & Material Co., Ltd.), copolymer type phenoxy resin of bisphenol A and bisphenol F (e.g., YP-70 manufactured by Nippon Steel Chemical & Material Co., Ltd.), and special phenoxy resins such as brominated phenoxy resins, phosphorus-containing phenoxy resins, and sulfonic group-containing phenoxy resins other than the above (e.g., Pheno Tohto YPB-43C, Pheno Tohto FX293, and YPS-007 manufactured by Nippon Steel Chemical & Material Co., Ltd.). These can be used alone or in a mixture of two or more kinds.
[0047] <Polycarbonate resin> The polycarbonate resin as the second resin can be obtained, for example, by reacting a dihydric phenol, or a dihydric phenol and a small amount of a polyhydroxy compound, with a carbonate precursor. The method for producing the polycarbonate resin is not particularly limited, and polycarbonate resins produced by the conventionally known phosgene method (interfacial polymerization method) or melt method (ester exchange method) can be used.
[0048] Among polycarbonate resins, aromatic polycarbonate resins obtained from aromatic dihydroxy compounds are preferred in consideration of compatibility with bifunctional epoxy resins or phenoxy resins. Examples of aromatic dihydroxy compounds include 2,2-bis(4-hydroxyphenyl)propane (bisphenol A), bis(4-hydroxyphenyl)methane, 1,1-bis(4-hydroxyphenyl)ethane, 2,2-bis(4-hydroxyphenyl)butane, 4,4'-dihydroxydiphenyl ether, 4,4'-dihydroxy-3,3'-dimethyldiphenyl ether, bis(4-hydroxyphenyl)phenylmethane, 2,2-bis(4-hydroxyphenyl-3-methylphenyl)propane, 1,1-bis(4-hydroxy-3-tert-butylphenyl)propane, 1,1-bis(4-hydroxyphenyl)propane, 1,1-bis(4-hydroxyphenyl)but ... Bis(4-hydroxyphenyl)cyclopentane, 1,1-bis(4-hydroxyphenyl)cyclohexane, 4,4'-dihydroxydiphenyl sulfone, 4,4'-dihydroxy-3,3'-dimethyldiphenyl sulfone, 4,4'-dihydroxydiphenyl sulfide, 4,4'-dihydroxydiphenyl sulfoxide, 4,4'-dihydroxy-3,3'-dimethyldiphenyl sulfoxide, 2,2-bis(4-hydroxy-3-bromophenyl)propane, 2,2-bis(4-hydroxy-3,5-dibromophenyl)propane, 2,2-bis(4-hydroxy-3,5-dichlorophenyl)propane, etc. These can be used alone or in combination of two or more kinds.
[0049] The carbonate precursor may be a carbonyl halide, a carbonyl ester, or a haloformate, specifically phosgene, diphenyl carbonate, a dihaloformate of a dihydric phenol, or a mixture thereof. In producing the polycarbonate resin, a suitable molecular weight regulator or a catalyst for promoting the reaction may also be used. Two or more of the aromatic polycarbonate resins thus obtained may be mixed.
[0050] The polycarbonate resin may be linear or branched. To obtain a branched polycarbonate resin, a part of the above-mentioned dihydric phenol may be replaced with, for example, the following branching agents, that is, polyhydroxy compounds such as phloroglucin, 4,6-dimethyl-2,4,6-tri(4-hydroxyphenyl)heptene-2, 4,6-dimethyl-2,4,6-tri(4-hydroxyphenyl)heptane, 2,6-dimethyl-2,4,6-tri(4-hydroxyphenyl)heptene-3, 1,3,5-tri(4-hydroxyphenyl)benzene, 1,1,1-tri(4-hydroxyphenyl)ethane, and compounds such as 3,3-bis(4-hydroxyaryl)oxindole (=isatin bisphenol), 5-chloruisatin, 5,7-dichloruisatin, and 5-bromoisatin. The amount of these replacing compounds used is usually 0.01 to 10 mol%, preferably 0.1 to 2 mol%, based on the dihydric phenol.
[0051] Among the above-mentioned polycarbonate resins, polycarbonate resins derived from 2,2-bis(4-hydroxyphenyl)propane or polycarbonate copolymers derived from 2,2-bis(4-hydroxyphenyl)propane and other dihydroxy compounds are preferred. Also, copolymers mainly made of polycarbonate resins, such as copolymers with polymers or oligomers having a siloxane structure, may be used.
[0052] When a melting method is used to obtain a polycarbonate resin, the amount of OH groups at the polymer chain ends can be adjusted, but the terminal structure of the polycarbonate resin is not particularly limited in the present invention. Therefore, the terminal groups may be left as they are or may be capped with a terminal capping agent, and one or both ends may be capped.
[0053] The weight average molecular weight (Mw) of the polycarbonate resin is not particularly limited, and from the viewpoint of ensuring the mechanical strength of the molded article, it is preferably in the range of 10,000 to 250,000, more preferably in the range of 15,000 to 200,000, and most preferably in the range of 15,000 to 100,000. If the Mw of the polycarbonate resin is too low, the molded article may have poor mechanical properties and heat resistance, and if it is too high, it is likely to have poor workability and processability. If the Mw is less than 10,000, the strength of the molded article is poor, and if it is too high, it is likely to have poor workability and processability. The Mw is measured by gel permeation chromatography and is a value converted using a standard polystyrene calibration curve.
[0054] The polycarbonate resin preferably used in the present invention is solid at room temperature, and has a melt viscosity of 3,000 Pa·s or less at a temperature of 260°C or more, for example, 280°C, more preferably 2,000 Pa·s or less, and even more preferably 1,500 Pa·s or less. If the melt viscosity exceeds 3,000 Pa·s, the fluidity of the resin during molding processing decreases, the resin does not spread sufficiently, causing voids, or impregnation becomes insufficient, resulting in insufficient appearance and mechanical strength, which is not preferable. The lower limit of the melt viscosity is preferably higher than 100 Pa·s, more preferably 300 Pa·s or more, and most preferably 500 Pa·s or more. If the melt viscosity is 100 Pa·s or less, the matrix resin becomes brittle, and mechanical strength such as bending properties may not be sufficiently obtained.
[0055] The glass transition temperature (Tg) of the polycarbonate resin may be 200° C. or less, preferably in the range of 140° C. to 170° C., and more preferably in the range of 145° C. to 165° C. If the Tg of the polycarbonate resin is higher than 200° C., the melt viscosity becomes high, and it becomes difficult to impregnate the resin composition of the present embodiment without defects such as voids into a reinforcing fiber substrate when the resin composition is applied to, for example, FRP. On the other hand, there is no particular restriction on the lower limit of Tg as long as there is no problem with processability, but it is considered that it is sufficient to have a Tg of about 140° C. or more. Furthermore, the melting point (Tm) of the polycarbonate resin is preferably within the range of 200 to 300° C., more preferably 220 to 280° C., and even more preferably 240 to 260° C. If the melting point is less than 200° C., for example, when applied to FRP, there is a risk that the crosslinking reaction will start in a state where the impregnation into the reinforcing fiber substrate is insufficient, and if it exceeds 300° C., a molding machine with higher temperature specifications will be required for processing.
[0056] <Composition ratio> In the resin composition, the content ratio of the first resin to the second resin (first resin: second resin) is preferably within the range of 9:1 to 3:7 by weight. Within this composition ratio range, the cured product obtained by curing the resin composition by thermal crosslinking exhibits excellent heat resistance and mechanical properties. From this viewpoint, the content ratio (first resin: second resin) is more preferably within the range of 9:1 to 4:6, further preferably within the range of 8:2 to 4:6, and most preferably within the range of 8:2 to 5:5. If the content ratio (first resin: second resin) is outside of 3:7 and the first resin is small, or outside of 9:1 and the second resin is small, the crosslink density of the crosslinked cured product of the first resin and the second resin is reduced, and therefore a significant improvement in heat resistance and mechanical strength cannot be obtained.
[0057] A particularly preferred combination of the first and second resins is one in which both the first and second resins have a bisphenol skeleton in their molecules. By having both the first and second resins have a bisphenol skeleton in their molecules, compatibility is increased, making it easier to obtain a uniform cured product.
[0058] <Optional ingredients> The resin composition of the present embodiment may contain, as an optional component, a thermoplastic resin or a thermosetting resin other than the difunctional epoxy resin, the phenoxy resin, and the polycarbonate resin, as long as the effect of the invention is not impaired.
[0059] The optional thermoplastic resin may be crystalline, non-crystalline, or the like, and its properties are not particularly limited. For example, one or more of polyolefins and acid-modified products thereof, polystyrene, polymethyl methacrylate, AS resin, ABS resin, thermoplastic aromatic polyesters such as polyethylene terephthalate and polybutylene terephthalate, polyimide, polyamide, polyamideimide, polyetherimide, polyethersulfone, polyphenylene ether and modified products thereof, polyphenylene sulfide, polyoxymethylene, polyarylate, polyether ketone, polyether ether ketone, polyether ketone ketone, and the like can be used. As the optional thermosetting resin, for example, one or more types selected from vinyl ester resin, phenol resin, urethane resin, etc. can be preferably used.
[0060] However, since it is necessary to impart excellent heat resistance and mechanical strength to the cured product of the resin composition, the total amount of other thermoplastic resins and thermosetting resins as optional components is preferably less than 50 parts by weight, more preferably 0 to 20 parts by weight, per 100 parts by weight of the total amount of resin components. If the total amount of resins as optional components is 50 parts by weight or more, the effect of the invention may be impaired.
[0061] In addition, the resin composition of the present embodiment may contain, as optional components, for example, organic solvents, crosslinking agents, inorganic fillers, extender pigments, colorants, antioxidants, ultraviolet protection agents, flame retardants, flame retardant assistants, etc., within the scope of not impairing the effects of the invention.
[0062] <Form of Resin Composition> The resin composition of the present embodiment can be in any form, such as a solid, a powder, or a liquid form using an appropriate solvent. Examples of solvents capable of dissolving the first resin and the second resin include methanol, ethanol, butanol, dichloromethane, chloroform, tetrahydrofuran, toluene, xylene, acetone, ethyl acetate, dimethylformamide, N-methyl-2-pyrrolidone, and dimethylacetamide.
[0063] The resin composition has a melt viscosity of 3000 Pa s or less in a temperature range below 260° C. If the melt viscosity exceeds 3000 Pa s in a temperature range below 260° C., the fluidity of the resin composition decreases, which is undesirable as it may cause voids after processing.
[0064] The resin composition has a melt viscosity of 8,000 Pa·s or more, preferably 10,000 to 1,000,000 Pa·s, and more preferably 20,000 to 1,000,000 Pa·s, in a temperature range of 260° C. or higher, and preferably 280° C. or higher. The resin composition begins to thicken at a temperature 10 to 20° C. above the melting point of the polycarbonate resin (about 250° C.), and the viscosity rises rapidly at temperatures of 260° C. or higher, reaching a range of 10,000 Pa·s. From the viewpoint of molding processing, the increase in melt viscosity of the resin composition, for example, at a temperature of 280°C, preferably reaches 10,000 Pa s or more within 30 minutes, and more preferably reaches 10,000 Pa s or more within 20 minutes. In this way, the resin composition behaves like a thermosetting resin due to thermal crosslinking, and hardens at a temperature range of 260 ° C or higher to form a hardened product. That is, although the first resin and the second resin constituting the resin composition are both thermoplastic resins, the resin composition is irreversibly hardened by heating to a temperature of 260 ° C or higher, for example, 280 to 320 ° C, preferably within a range of 280 to 300 ° C, and thereafter exhibits a characteristic behavior of being almost infusible. In this case, the hardening mechanism is not yet clear, but it is presumed that an ester exchange reaction occurs between the secondary hydroxyl group contained mainly in the bifunctional epoxy resin or the phenoxy resin and the ester group contained in the polycarbonate resin, and a crosslink is formed between the bifunctional epoxy resin chain or the phenoxy resin chain and the polycarbonate resin chain to form a three-dimensional network structure, and hardens.
[0065] <Preparation of Resin Composition> The resin composition of the present embodiment can be easily prepared by mixing the first resin, the second resin, and, if necessary, any optional components. The mixing method is not particularly limited, but examples thereof include a method of mixing the first resin and the second resin in a powdered state (dry blending), a method of mixing the first resin and the second resin while heating and melting them, and a method of dissolving the first resin and the second resin in a solvent and mixing them. In addition, when mixing each component, for example, various blenders, mixers, dry mills, single- or double-screw ruders, kneaders, etc. can be appropriately selected and used depending on the mixing form. When kneading is performed while heating and melting, it is preferable to perform it at a temperature at which a cured product described later is not formed. When the temperature is increased while kneading the first resin and the second resin, thickening begins at a temperature 10 to 20°C above the melting point of the polycarbonate resin (about 250°C), so the temperature of kneading performed to prepare the resin composition (kneading in an uncured state) is, for example, preferably 240°C or less, more preferably within the range of 200 to 240°C.
[0066] [Cured products and cured molded products] The cured product of the present embodiment is obtained by curing the above-mentioned resin composition by thermal crosslinking. The cured product of the present embodiment is obtained by heat-treating the resin composition at a temperature of 260° C. or higher, preferably 280° C. or higher. During the heat treatment, the resin composition can be shaped into a desired shape by, for example, compression molding, or injection molding or extrusion molding using a single- or double-screw extruder or kneader. Since the resin composition hardens due to a crosslinking reaction and loses its fluidity, the time from melting to molding is, for example, within 20 minutes after the temperature reaches 280° C., and preferably within 10 minutes.
[0067] The cured product of the present embodiment has a glass transition temperature (Tg) of 100°C or higher as measured by dynamic mechanical analysis (DMA). For example, in the DMA of the cured product, when the amount of bifunctional epoxy resin or phenoxy resin (first resin) is greater than the amount of polycarbonate resin (second resin) (the content ratio of phenoxy resin to polycarbonate resin is 8:2 or 9:1), the Tg of the first resin (for example, about 110 to 120°C) is detected, but the Tg of the second resin (for example, about 160 to 170°C) is not detected and has been confirmed to disappear. As the amount of the second resin increases, the Tg of the cured product shifts to the high temperature side and approaches the Tg of the polycarbonate resin used alone as the second resin. Furthermore, when the thermal crosslinking temperature is lower than 280°C, the Tg of the cured product is separated into a tan δ peak indicating the Tg of the first resin and a tan δ peak indicating the Tg of the second resin, and a clear bimodal peak is formed at least at 240°C or lower. Furthermore, the storage modulus E' and loss modulus E" of the cured product are significantly increased compared to those of the first resin or the second resin alone, and it has been confirmed that the storage modulus E' exhibits stable behavior even at temperatures higher than the Tm of the polycarbonate resin. Thus, the cured product of the resin composition of the present invention does not have a melting point and maintains a solid state even when heated.
[0068] Furthermore, in the case of the cured product of this embodiment, the amount of probe displacement after measurement in a DMA at temperatures ranging from 25° C. to 300° C. is less than −1 mm relative to the amount before measurement, which means that the cured product does not melt or soften even at 300° C., and has high heat resistance.
[0069] As described above, the cured product of the present embodiment has excellent heat resistance and mechanical strength. Therefore, the cured molded products molded into various shapes can be used for various applications such as aircraft parts, automobile parts, electric and electronic parts, building materials, various containers, sporting goods, daily necessities, household goods, and sanitary products. In particular, it can be preferably used for various applications requiring heat resistance and mechanical strength, such as aircraft engine peripheral parts, aircraft parts, automobile body parts and engine peripheral parts, intake and exhaust system parts, engine cooling water system parts, housing parts for notebook PCs, tablets, smartphones, etc., and electric and electronic equipment parts such as heat dissipation parts for LED lighting.
[0070] The cured product of the present embodiment can also be preferably used as a matrix resin in fiber-reinforced plastics, for example. In this case, the cured product has excellent adhesiveness and affinity with fibers derived from the first resin, and therefore has good impregnation into a reinforcing fiber substrate regardless of the presence or absence of sizing treatment, resulting in a fiber-reinforced plastic with excellent mechanical strength.
[0071] [Fiber reinforced plastic molding materials] The fiber-reinforced plastic molding material of the present embodiment (hereinafter, sometimes referred to as "FRP molding material") contains a reinforcing fiber base material and a powder of the above-mentioned resin composition adhered to the reinforcing fiber base material. In the FRP molding material of this embodiment, the reinforcing fiber is not particularly limited, but for example, carbon fiber, boron fiber, silicon carbide fiber, glass fiber, aramid fiber, etc. are preferable, and carbon fiber is more preferable. Regarding the type of carbon fiber, for example, PAN-based or pitch-based can be used, and these may be used alone or in combination depending on the purpose and use. In addition, as the reinforcing fiber substrate, for example, a nonwoven fabric substrate using chopped fiber, a cloth material using continuous fiber, a unidirectional reinforcing fiber substrate (UD material), etc. can be used, but from the viewpoint of reinforcing effect, the use of cloth material or UD material is preferable. When using cloth material or UD material, it is preferable that the fibers called filaments are opened. The weight of the reinforcing fiber base material is 40 to 250 g / m 2 It is preferable that the thickness is within the range of 40 g / m 2 At a basis weight of less than 250 g / m, the number of reinforcing fibers in the molded product is too small to obtain the desired mechanical properties. 2 If the amount exceeds this range, it becomes difficult to sufficiently impregnate the inside of the reinforcing fiber substrate with the resin, which is not preferable. The reinforcing fiber substrate can be used regardless of whether or not it has been subjected to a sizing treatment.
[0072] In the FRP molding material of this embodiment, the resin composition is attached to the reinforcing fiber substrate in a powder state. The FRP molding material is preferably prepared, for example, by a powder coating method in which fine powder of the resin composition is attached to the reinforcing fiber substrate. In the powder coating method, the raw resin composition is easily melted because of the fine particles, and the coating film after coating has a suitable amount of voids, which serve as an escape route for air, making it difficult for voids to occur in the resin after melting.
[0073] The powder coating method includes, for example, electrostatic coating, fluidized bed, and suspension coating. Among these, electrostatic coating and fluidized bed are suitable for thermoplastic resins, and are preferred because they are simple and have good productivity. In particular, electrostatic coating is the most suitable method because it provides good uniformity of adhesion of the fine powder raw resin composition to the reinforcing fiber substrate.
[0074] The average particle diameter of the fine powder raw resin composition used in the powder coating method is, for example, preferably in the range of 10 to 100 μm, more preferably in the range of 40 to 80 μm, and most preferably in the range of 40 to 50 μm. If the average particle diameter of the fine powder exceeds 100 μm, the energy when the fine powder collides with the fiber in the powder coating in an electrostatic field increases, and the adhesion rate to the reinforcing fiber substrate decreases. In addition, if the average particle diameter of the fine powder is less than 10 μm, the particles are scattered by the accompanying air flow, which reduces the adhesion efficiency, and the fine powder of the raw resin floating in the air may cause a deterioration of the working environment. The raw resin is preferably pulverized using a pulverizing mixer such as a low-temperature drying pulverizer (centrifuge dry mill), but is not limited thereto. In addition, when pulverizing the raw resin, multiple components as raw materials may be pulverized and then mixed, or multiple components may be blended in advance and then pulverized.
[0075] In powder coating, it is preferable to coat the reinforced fiber substrate with the amount of fine powder of raw resin (resin ratio: RC) in the range of 20 to 50%, more preferably in the range of 25 to 45%, and even more preferably in the range of 25 to 40%. If the RC exceeds 50%, the mechanical properties of the CFRP, such as the tensile and flexural modulus of elasticity, will decrease, and if it is below 20%, the amount of raw resin adhered will be extremely small, resulting in insufficient impregnation of the raw resin into the reinforced fiber substrate, and there is a concern that both the thermal properties and mechanical properties will be reduced.
[0076] [Fiber reinforced plastics] The fiber reinforced plastic (hereinafter sometimes referred to as "FRP") of the present embodiment has a reinforcing fiber substrate and a cured product of a resin composition as a matrix resin attached to the reinforcing fiber substrate. The method for producing FRP is not particularly limited, and may be, for example, an impregnation method or a film stack method, but it is preferable to prepare FRP by subjecting an FRP molding material (prepreg) having the resin composition of the above embodiment to a heating and pressurizing treatment. In the heating and pressurizing treatment, the powdery raw resin composition is completely melted by heating and becomes liquid, and is permeated into the prepreg by pressure. However, in the prepreg controlled to a predetermined air permeability, an escape route for air is secured, so the molten resin permeates while expelling the air, and the impregnation is completed in a short time even at a relatively low pressure, and the occurrence of voids can be avoided.
[0077] The FRP of the present invention preferably has a fiber volume fraction (Vf) of the reinforcing fibers in the range of 40 to 65%. Vf is adjusted depending on the application of the FRP, but is more preferably 45 to 65%, and further preferably 45 to 60%. If Vf exceeds 65%, the amount of matrix resin becomes insufficient, and the strength of the FRP decreases. Also, if Vf is less than 40%, the reinforcing effect of the reinforcing fibers decreases.
[0078] In order to completely melt the fine powder of the raw resin composition and impregnate the entire reinforcing fiber substrate, the heating and pressurizing treatment is preferably performed at a temperature in the range of approximately 230°C to 350°C, which is equal to or higher than the melting point of the polycarbonate resin used as the second resin, and within this temperature range, a temperature of the melting point (Tm) of the polycarbonate resin used as the second resin + 10 to 60°C is more preferable. If the upper limit temperature is exceeded, excessive heat is applied, which may cause decomposition of the resin, and if the lower limit temperature is exceeded, not only may the melt viscosity be high and the reinforcing fiber substrate may not be sufficiently impregnated, but the crosslinking reaction between the first resin and the second resin may not occur, and a cured product having the desired strength and heat resistance cannot be obtained. In addition, when the melting point of the polycarbonate resin used as the second resin cannot be clearly confirmed, the glass transition temperature (Tg) + 100°C or more is a guideline for the heating and pressurizing treatment temperature.
[0079] The pressure of the heat and pressure treatment is, for example, preferably 3 MPa or more, and more preferably within the range of 3 to 5 MPa. If the pressure exceeds the upper limit, excessive pressure is applied, which may cause deformation or damage, and if the pressure is below the lower limit, the impregnation into the reinforcing fiber substrate is deteriorated.
[0080] The time for the heating and pressurizing treatment is preferably at least 5 minutes, and more preferably within the range of 5 to 20 minutes.
[0081] It is also possible to carry out molding into a desired shape simultaneously with the heating and pressurizing treatment. The molding process can also be carried out by quickly placing a material that has been heated to a desired temperature in a low-temperature pressurizing machine. After the heat and pressure treatment, any treatment such as post-cure can be performed. The post-cure is preferably performed at a temperature of 260° C. or higher, preferably 280° C. or higher, for about 10 to 30 minutes.
[0082] [Fiber reinforced plastic laminate] A fiber-reinforced plastic laminate (hereinafter, sometimes referred to as "FRP laminate") according to one embodiment of the present invention contains phenoxy resin, polycarbonate resin, and reinforcing fibers. In the FRP laminate of this embodiment, the phenoxy resin and the polycarbonate resin are laminated in layers, and the layer containing the phenoxy resin (hereinafter, sometimes referred to as "phenoxy resin-containing layer") and the layer containing the polycarbonate resin (hereinafter, sometimes referred to as "polycarbonate resin-containing layer") include one or more interlayer bonding sites where they are bonded by a crosslinking reaction at the lamination interface between the two layers. The FRP laminate of this embodiment preferably has an interlayer shear strength of 40 MPa or more as measured by the ILSS method.
[0083] The ILSS method is a method for evaluating interlaminar shear strength defined in JIS K 7078, and the FRP laminate of the present embodiment has an interlaminar shear strength of 40 MPa or more when measured by this method. FRP laminates are generally manufactured by stacking multiple sheets of FRP molding material known as prepregs and then heating and pressurizing them using a heat press or autoclave. However, if the interlaminar shear strength is less than 40 MPa, external stress on the FRP laminate will cause delamination, significantly reducing the strength of the FRP laminate. Incidentally, if the interlaminar shear strength is too high, there is a concern that it may result in a decrease in impact resistance, so that it is preferably within the range of 40 to 65 MPa, and more preferably within the range of 45 to 60 MPa.
[0084] The FRP laminated molding of this embodiment preferably has a matrix resin in a state in which the phenoxy resin and the polycarbonate resin are laminated in layers. The laminated state can have any structure depending on the desired properties of the FRP laminated molding, and the phenoxy resin-containing layer and the polycarbonate resin-containing layer may be alternately laminated, or may be randomly laminated. When the phenoxy resin-containing layer and the polycarbonate resin-containing layer are randomly laminated, they may be laminated so as to include at least one interlayer bonding site where the phenoxy resin-containing layer and the polycarbonate resin-containing layer are bonded, but in order to improve the mechanical strength of the FRP laminated molding, it is preferable that 10% or more, more preferably 50% or more, and even more preferably 70% to 100% of all interlayer bonding sites are interlayer bonding sites where the phenoxy resin-containing layer and the polycarbonate resin-containing layer are bonded. It is preferable that the phenoxy resin-containing layer and the polycarbonate resin-containing layer each contain reinforcing fibers at least in a portion thereof, but only one of the resin layers may contain reinforcing fibers.
[0085] The FRP laminated molding of this embodiment may contain a layer using any resin other than phenoxy resin and polycarbonate resin (for example, a layer derived from an FRP molding material made of any resin, a layer derived from a resin film made of any resin, etc.) within a range that does not impair the effects of the invention. Here, the arbitrary resin is not particularly limited, but a resin having good adhesion to phenoxy resin and polycarbonate resin is preferable. On the other hand, in order to maintain excellent mechanical strength, the FRP laminated molding of this embodiment preferably has a total ratio of phenoxy resin-containing layers and polycarbonate resin-containing layers to the number of all layers constituting the FRP laminated molding of, for example, 50% or more, more preferably 70% or more and 100% or less.
[0086] The fiber volume fraction (Vf) in the FRP laminate of this embodiment is preferably within a range of, for example, 45 to 67%. Here, Vf refers to the volume fraction of reinforcing fibers contained in the FRP laminate. It is preferable to set Vf within the above range from the viewpoint of the mechanical properties of the FRP laminate. If Vf is too high, the voids in the reinforcing fiber base material cannot be filled with the thermoplastic resin, and mechanical properties commensurate with the amount of fiber may not be obtained.
[0087] The FRP laminated molding of this embodiment includes an interlayer bonding site where the phenoxy resin and polycarbonate resin laminated in layers are firmly bonded by a crosslinking reaction at the contact interface between the two. This crosslinking reaction is confirmed by a significant increase in the melt viscosity of the mixture of the phenoxy resin and the polycarbonate resin, and the solidified product exhibits a higher elastic modulus than the polycarbonate resin alone. The crosslinking reaction becomes prominent when a heat history is given at 260°C or higher, for example, 280°C for 10 minutes or more, and is widely observed when the phenoxy resin and the polycarbonate resin are mixed in a ratio of 9:1 to 3:7. Although the details of the reaction mechanism are not clear at this time, since the crosslinking reaction occurs without any particular restriction on the terminal structure of the polycarbonate resin, it is speculated that the crosslinking is due to an ester exchange reaction between the phenoxy resin and the polycarbonate resin. That is, it is believed that the polymer chains of the phenoxy resin and polycarbonate resin form three-dimensional crosslinks due to an ester exchange reaction between the carbonate group -O(C=O)-O- of the polycarbonate resin and the hydroxyl group (-OH) present at the end or side chain of the phenoxy resin, resulting in a crosslinked cured product that is stronger and has higher heat resistance than the phenoxy resin alone or the polycarbonate resin alone.The FRP laminated molded product of this embodiment utilizes this crosslinking reaction at the interface between the phenoxy resin and the polycarbonate resin to improve mechanical strength.
[0088] The phenoxy resin-containing layer, the polycarbonate resin-containing layer, and the reinforcing fibers that constitute the FRP laminate of this embodiment will be described in detail below.
[0089] [Phenoxy resin-containing layer] The phenoxy resin-containing layer may contain reinforcing fibers (substrate), and may contain other components as necessary within the range that does not impair the effects of the present invention. Examples of other components that may be contained include flame retardants such as brominated phenoxy resins, release agents, dyes and pigments, antistatic agents, anti-dripping agents, impact strength improvers, and other thermoplastic resins (polyamide resins, polycarbonate resins, fluororesins, etc.). It is most preferable that the phenoxy resin-containing layer does not contain other resin components and that the resin components are composed only of phenoxy resin. However, when other resin components are contained, it is preferable that the phenoxy resin is contained in an amount of 60 parts by weight or more, more preferably 80 parts by weight or more, and even more preferably 90 parts by weight or more, of the total resin components in the phenoxy resin-containing layer, 100 parts by weight.
[0090] [Polycarbonate resin-containing layer] The polycarbonate resin-containing layer may contain reinforcing fibers (substrate), and may contain other components as necessary within the range that does not impair the effects of the present invention. Examples of other components that may be contained include phosphorus-based heat stabilizers such as phosphorous acid, phosphoric acid, phosphite esters, and phosphate esters, antioxidants such as hindered phenol-based antioxidants, release agents, ultraviolet absorbers, dyes and pigments, antistatic agents, flame retardants, drip prevention agents, impact strength improvers, and other thermoplastic resins (such as phenoxy resins). It is most preferable that the polycarbonate resin-containing layer does not contain other resin components and that the resin components are composed only of polycarbonate resin, but when other resin components are contained, it is preferable that the polycarbonate resin is contained in an amount of 80 parts by weight or more, and more preferably 90 parts by weight or more, of the total resin components in the polycarbonate resin-containing layer, 100 parts by weight.
[0091] [Reinforced fiber] In the FRP laminated molded body of this embodiment, the reinforcing fibers can be selected from a wide range of reinforcing fibers, such as carbon fibers, glass fibers, ceramic fibers such as boron, alumina, and silicon carbide, metal fibers such as stainless steel, and organic fibers such as aramid, and may be commercially available reinforcing fibers such as Tyranno Fiber (registered trademark). Among these, carbon fibers and glass fibers are preferably used, and it is most preferable to use carbon fibers with high strength and good thermal conductivity. Both pitch-based and PAN-based carbon fibers can be used, but pitch-based carbon fibers are not only high in strength but also high in thermal conductivity, and therefore can quickly diffuse generated heat, so they are preferable over PAN-based carbon fibers in applications where heat needs to be released. The form of the reinforcing fiber substrate is not particularly limited, and a woven fabric made of continuous fibers or a UD material in which continuous fibers are aligned in one direction is preferably used, and for example, a unidirectional material, a cloth such as a plain weave or twill weave, a three-dimensional cloth, or a tow made of several thousand or more filaments can be used. These reinforcing fiber substrates can be used alone or in combination of two or more types.
[0092] In order to improve the wettability of the matrix resin to the reinforcing fibers and ease of handling, the reinforcing fibers may be treated with a surface treatment agent such as a sizing agent (binding agent) or a coupling agent, or may be subjected to an oxidation treatment. Examples of the sizing agent include maleic anhydride compounds, urethane compounds, acrylic compounds, epoxy compounds, phenol compounds, and derivatives of these compounds, etc. Examples of the coupling agent include amino-, epoxy-, chlorine-, mercapto-, and cationic silane coupling agents, etc.
[0093] The content of the sizing agent and coupling agent, which are surface treatment agents, is preferably 0.1 to 10 parts by weight, more preferably 0.5 to 6 parts by weight, relative to 100 parts by weight of the reinforcing fibers. If the content of the sizing agent and coupling agent is 0.1 to 10 parts by weight, the wettability with the matrix resin and the handleability are better.
[0094] [Manufacturing method for FRP laminated bodies] The FRP laminated molded product of this embodiment can be obtained, for example, by the following manufacturing methods (1) to (3). Details of these manufacturing methods will be described below as representative examples, but the manufacturing method of the FRP laminated molded product of this embodiment is not limited to these.
[0095] [Manufacturing method (1)] Prepreg Lamination: As shown in FIG. 1, this method involves preparing a plurality of sheet-like phenoxy resin FRP molding materials 10 containing phenoxy resin as a matrix resin and a reinforcing fiber base material, and a plurality of sheet-like polycarbonate resin FRP molding materials 20 containing polycarbonate resin as a matrix resin and a reinforcing fiber base material, stacking the two alternately or randomly, and pressure-molding while heating to obtain an FRP laminated molded product 30.
[0096] The phenoxy resin FRP molding material 10 and polycarbonate resin FRP molding material 20 used in the manufacturing method (1) can be used without any problem if they are obtained by a known method, but it is preferable that they are produced by a method that does not use a solvent. Examples of such methods include a method of pressurizing and impregnating a molten resin composition into a reinforcing fiber substrate (film stack method), a method of spraying or coating a powdered resin composition on a reinforcing fiber substrate (powder coating method), and a method of mixing and weaving continuous fibers spun from a resin composition with reinforcing fibers (comingle method).
[0097] The resin ratio (RC) of the phenoxy resin FRP molding material 10 or the polycarbonate resin FRP molding material 20 is preferably within the range of 25 to 50%, and more preferably within the range of 30 to 50%, so as to ensure that a molten mixed state of the phenoxy resin and the polycarbonate resin is formed at the layer boundary in the subsequent heating and pressure molding process.
[0098] The phenoxy resin FRP molding material 10 and the polycarbonate resin FRP molding material 20 are laminated alternately or randomly to a desired molded body thickness, and then heated and pressurized to be processed into the FRP laminated molding 30 of this embodiment. When the phenoxy resin FRP molding material 10 and the polycarbonate resin FRP molding material 20 are randomly laminated, they may be laminated so as to include at least one lamination boundary where the phenoxy resin and the polycarbonate resin contact each other, but in order to improve the mechanical strength of the FRP laminated molding 30 to be produced, it is preferable to laminate them so that 10% or more of all lamination boundaries, more preferably 50% or more, and even more preferably 70% to 100% of all lamination boundaries are lamination boundaries where the phenoxy resin and the polycarbonate resin contact each other. Furthermore, if necessary, FRP molding materials or resin films made of resins other than phenoxy resin and polycarbonate resin may be inserted between the layers of the phenoxy resin FRP molding material 10 and the polycarbonate resin FRP molding material 20. In this case as well, lamination may be performed so that at least a portion of the lamination boundary where the phenoxy resin and polycarbonate resin come into contact is included, but in order to improve the mechanical strength of the FRP laminated molding 30 to be produced, it is preferable to laminate so that 70% or more, and more preferably 75% or more but less than 100%, of all lamination boundaries are lamination boundaries where the phenoxy resin comes into contact with the polycarbonate resin. For molding, a common pressure molding machine for molding FRP, such as a flat plate type heat press, belt press, roll press, or autoclave, can be used, but processing conditions of 5 minutes or more at a molding temperature of 260° C. or higher are required. Processing conditions are preferably within the range of a molding temperature of 260 to 300° C. and 5 to 30 minutes, and more preferably within the range of 280 to 290° C. and 10 to 20 minutes. Furthermore, if the molding temperature is less than 260°C or the processing time is less than 5 minutes, the crosslinking reaction between the phenoxy resin and the polycarbonate resin will be insufficient, resulting in a weak interface between the two and insufficient mechanical strength for the FRP laminated molding.
[0099] [Manufacturing method (2)] Film Insertion: As shown in Figure 2 or Figure 3, this method involves preparing a phenoxy resin FRP molding material 10 or a polycarbonate resin FRP molding material 20 and any resin film not used in the FRP molding material, laminating these alternately, and performing pressure molding while heating to obtain an FRP laminated molding 50A or 50B. That is, in manufacturing method (2), as shown in Figure 2, a polycarbonate resin film 40 may be laminated onto the phenoxy resin FRP molding material 10 to produce an FRP laminated molding 50A, or as shown in Figure 3, a phenoxy resin film 60 may be laminated onto the polycarbonate resin FRP molding material 20 to produce an FRP laminated molding 50B.
[0100] The phenoxy resin FRP molding material 10 and polycarbonate resin FRP molding material 20 used in manufacturing method (2) can be the same as those used in manufacturing method (1). There is no particular limitation on the manufacturing method of the phenoxy resin film 60 or polycarbonate resin film 40, and they may be manufactured by themselves using, for example, the T-die method or the inflation method, or a commercially available film may be used. There are no particular limitations on the thickness of the phenoxy resin film 60 and polycarbonate resin film 40, but a) ensuring a sufficient amount of resin to generate a sufficient melt-mixed state at the interface with the phenoxy resin FRP molding material 10 or the polycarbonate resin FRP molding material 20; b) The thickness of the portion consisting only of resin and not of reinforcing fibers is minimized to ensure mechanical strength without decreasing Vf of the resulting FPC laminates 50A and 50B. From this viewpoint, for example, the range of 10 to 200 μm is preferable, and the range of 20 to 150 μm is more preferable.
[0101] In the manufacturing method (2), the FRP molding material and the resin film are laminated alternately or randomly to the desired molded body thickness as in the manufacturing method (1), and then heated and pressurized to be processed into the FRP laminated molded bodies 50A and 50B of the present embodiment. When the FRP molding material and the resin film are randomly laminated, they may be laminated so as to include at least one lamination boundary where the phenoxy resin and the polycarbonate resin come into contact, but laminating a resin film that does not contain reinforcing fibers reduces the Vf of the FRP laminated molded bodies 50A and 50B. Therefore, in order to improve the mechanical strength of the manufactured FRP laminated molded bodies 50A and 50B, it is preferable to laminate them so that 25% or more, more preferably 25% to 100%, of all lamination boundaries are lamination boundaries where the phenoxy resin comes into contact with the polycarbonate resin. Also, if necessary, FRP molding materials or resin films made of resins other than phenoxy resin and polycarbonate resin may be inserted between the layers. In this case, too, lamination may be performed so that at least a portion of the lamination boundary where the phenoxy resin and polycarbonate resin come into contact is included, but in order to improve the mechanical strength of the FRP laminated moldings 50A and 50B to be produced, it is preferable to laminate so that 25% or more, more preferably 25% or more but less than 100%, of all lamination boundaries are lamination boundaries where the phenoxy resin comes into contact with the polycarbonate resin. For molding, a common pressure molding machine for molding FRP, such as a flat plate type heat press, belt press, roll press, or autoclave, can be used, but processing conditions of 5 minutes or more at a molding temperature of 260° C. or higher are required. Processing conditions are preferably within the range of a molding temperature of 260 to 300° C. and 5 to 30 minutes, and more preferably within the range of 280 to 290° C. and 10 to 20 minutes. Furthermore, if the molding temperature is less than 260°C or the processing time is less than 5 minutes, the crosslinking reaction between the phenoxy resin and the polycarbonate resin will be insufficient, resulting in a weak interface between the two and insufficient mechanical strength being obtained for the FRP laminated moldings 50A, 50B.
[0102] [Manufacturing method (3)] Use of hybrid moulding materials: As shown in FIG. 4, this method involves preparing a hybrid FRP molding material 80 in which one side of a reinforcing fiber substrate 70 is covered with phenoxy resin and the other side is covered with polycarbonate resin, and then stacking multiple sheets of this hybrid FRP molding material 80 and subjecting them to heat and pressure molding to obtain an FRP laminated molded product 90.
[0103] The hybrid FRP molding material 80 used in manufacturing method (3) differs from manufacturing methods (1) and (2) in that one side of the reinforcing fiber substrate 70 is covered with phenoxy resin and the other side is covered with polycarbonate resin. Here, the phenoxy resin coating layer on one side of the hybrid FRP molding material 80 is the part that will become the "phenoxy resin-containing layer" in the FRP laminated product 90, and the polycarbonate resin coating layer on the other side is the part that will become the "polycarbonate resin-containing layer" in the FRP laminated product 90. The phenoxy resin and polycarbonate resin coating the reinforcing fiber substrate 70 may coat the surface of the reinforcing fiber substrate 70 in the form of a film, or may coat the surface of the reinforcing fiber substrate 70 in a state in which resin powder has accumulated and adhered thereto; however, a film-like coating is preferred from the standpoint of productivity of the hybrid FRP molding material 80, etc.
[0104] The hybrid FRP molding material 80 is obtained by applying pressure to the reinforcing fiber substrate 70 while the phenoxy resin and polycarbonate resin are heated to a temperature above the melting or softening temperature of the resin, respectively, to coat the surface of the reinforcing fiber substrate 70. Specifically, (i) As shown by the downward arrow in FIG. 4, a phenoxy resin film 60 and a polycarbonate resin film 40 are superimposed on both sides of the reinforcing fiber substrate 70 in the thickness direction, and the resin component is melt-impregnated into the reinforcing fiber substrate 70 while applying heat and pressure. (ii) As shown by the upward arrow in FIG. 4, a phenoxy resin FRP molding material 10 and a polycarbonate resin FRP molding material 20 are overlapped, and the resin components are melt-impregnated while being heated and pressurized, thereby integrating the two materials. Examples include: As equipment for carrying out the above method, for example, a pressure molding machine, a belt press or a roll press can be suitably used. In the above (i) and (ii), the temperature at which the phenoxy resin and polycarbonate resin are melt-impregnated into the reinforcing fiber substrate 70 is less than 260° C., and preferably in the range of 200° C. to 240° C. Processing at a temperature of 260° C. or higher is not preferable because it causes a crosslinking reaction between the phenoxy resin and the polycarbonate resin, thereby reducing the formability of the hybrid FRP molding material 80. The resin ratio (RC) of the hybrid FRP molding material 80 is preferably within the range of 25 to 50%, for example, and more preferably within the range of 30 to 50%, in order to ensure that a molten mixed state of the phenoxy resin and polycarbonate resin is formed in the subsequent heating and pressure molding process.
[0105] The hybrid FRP molding material 80 is laminated to the desired molded body thickness in the same manner as in the manufacturing methods (1) and (2). At this time, there is no particular restriction on the orientation of the hybrid FRP molding material 80, and it is sufficient to laminate it so that at least a portion of the laminate boundary where the phenoxy resin and the polycarbonate resin come into contact is included, but in order to make the mechanical strength of the manufactured FRP laminated molded body 90 excellent, it is preferable to laminate it so that 50% or more of all the laminate boundaries, more preferably 75% or more and 100% or less, are the laminate boundaries where the phenoxy resin comes into contact with the polycarbonate resin. Furthermore, if necessary, FRP molding materials or resin films made of phenoxy resin or polycarbonate resin, or FRP molding materials or resin films made of resins other than phenoxy resin and polycarbonate resin, may be inserted between layers of multiple hybrid FRP molding materials 80. In this case as well, lamination may be performed so that at least a portion of the lamination boundary where the phenoxy resin and polycarbonate resin come into contact is included, but in order to improve the mechanical strength of the FRP laminated molding 90 to be produced, it is preferable to laminate so that 50% or more, and more preferably 75% or more and 100% or less of all lamination boundaries are lamination boundaries where the phenoxy resin comes into contact with the polycarbonate resin.
[0106] The laminated body, which is laminated so as to include a plurality of hybrid FRP molding materials 80, is heated and pressurized to be processed into the FRP laminated body 90 of this embodiment. For molding, a common pressurizing machine for molding FRP, such as a flat plate type heat press, belt press, roll press, or autoclave, can be used, but processing conditions of a molding temperature of 260°C or higher and a processing time of 5 minutes or more are required. Processing conditions are preferably within a molding temperature range of 260 to 300°C for 5 to 30 minutes, and more preferably within a range of 280 to 290°C for 10 to 20 minutes. Furthermore, if the molding temperature is less than 260°C or the processing time is less than 5 minutes, the cross-linking reaction between the phenoxy resin and the polycarbonate resin will be insufficient, the interface between the two will be weak, and the FRP laminated molding 90 will not have sufficient mechanical strength. In addition, the hot and pressurized molding may cause the coated phenoxy resin and coated polycarbonate resin that have penetrated into the hybrid FRP molding material 80 to become mixed near the center in the thickness direction of the hybrid FRP molding material 80 (inside the reinforcing fiber substrate 70), resulting in the formation of crosslinks; however, this inside of the reinforcing fiber substrate 70 is not included in the "interlayer bonding site."
[0107] The FRP laminated molded bodies 30, 50A, 50B, 90 obtained in this manner can then be painted, or post-processed such as by drilling holes for fastening to other components, or by inserting them into an injection molding die and molding ribs, etc.
[0108] The FRP laminated moldings 30, 50A, 50B, 90 obtained as described above have a stable and strong interlayer bond and high mechanical properties because the phenoxy resin and the polycarbonate resin are mixed at the joints by laminating layers containing phenoxy resin and layers containing polycarbonate resin. Therefore, the FRP laminated moldings 30, 50A, 50B, 90 have both the excellent impact resistance characteristic of polycarbonate resin and the good adhesion to other members characteristic of phenoxy resin, and are also excellent in processability such as bending. Therefore, the FRP laminated moldings 30, 50A, 50B, 90 can be suitably used as mounting members in applications such as automobile members, electrical and electronic equipment housings, and aircraft members.
[0109] The uses of the FRP laminated molded body of the present embodiment are not particularly limited, and examples thereof include sporting goods, portable information terminals, and electric / electronic device parts, civil engineering and building material parts, structural parts for automobiles and motorcycles, and aircraft parts. From the viewpoint of its mechanical properties, it can be preferably used in electrical / electronic device casings, structural materials for bicycles and sporting goods, and interior and exterior members for automobiles, aircraft, etc., which require high mechanical strength. EXAMPLES
[0110] The present invention will be described in more detail with reference to the following examples, but the present invention is not limited to the descriptions of these examples. The methods for testing and measuring various physical properties in the examples are as follows.
[0111] [Average particle diameter (D50)] The average particle size was measured using a laser diffraction / scattering particle size distribution measuring device (Microtrac MT3300EX, manufactured by Nikkiso Co., Ltd.) as the particle size at which the cumulative volume was 50% on a volume basis.
[0112] [Dynamic Mechanical Analysis (DMA)] The measurements were carried out using a dynamic viscoelasticity measuring device (DMA 7e, manufactured by Perkin Elmer). The amount of probe displacement of the cured product was measured at temperatures ranging from 25° C. to 300° C., and the amount of probe displacement after DMA measurement was compared with the position before measurement. To measure the Tg of the cured product, a test piece 10 mm wide and 10 mm long was cut out from the cured product using a diamond cutter, and the temperature was measured in the range of 25°C to 300°C at a temperature increase rate of 5°C / min. The maximum peak of tan δ was taken as the Tg.
[0113] [Melt Viscosity] Using a rheometer (MCR302 manufactured by Anton Paar), approximately 300 mg of the measurement sample was sandwiched between parallel plates and heated to 280°C at a rate of 50°C / min. After that, the temperature was maintained at 280°C and the minimum melt viscosity and the melt viscosity at 280°C or higher were measured under the conditions of a frequency of 1 Hz, an oscillation angle of 0.5%, and a normal force of 0.1 N.
[0114] [Resin ratio (RC:%)] The weight was calculated using the following formula from the weight (W1) of the reinforcing fiber substrate before the matrix resin was attached and the weight (W2) of the CFRP molding material after the resin was attached. Resin ratio (RC:%) = (W2-W1) / W2 x 100 W1: Weight of reinforcing fiber substrate before resin adhesion W2: Weight of CFRP molding material after resin adhesion
[0115] [Fiber volume content (Vf:%)] The measurements were made using a combustion method based on JIS K 7075:1991 Test method for fiber content and void content of carbon fiber reinforced plastics.
[0116] [Mechanical strength measurement] The mechanical properties (stress at break and elastic modulus) of the obtained CFRP molded bodies were measured based on JIS K 7074:1988 Bending test method for carbon fiber reinforced plastics. Specifically, the laminated molded product was cut into a rectangular shape with a total length of 80 mm and a width of 15 mm to be used as a test specimen, with a support distance of 40 mm. The test was performed using a Tensilon universal material testing machine (RTA250 manufactured by A&D) at a test speed of 2 mm / min.
[0117] [Measurement of interlaminar shear strength] Based on JIS K 7078:1991 Interlaminar shear test method for carbon fiber reinforced plastics, test pieces of 21 mm length x 10 mm width x 3 mm thickness were measured using a universal strength testing machine (Autograph AG-Xplus100kN, manufactured by Shimadzu Corporation).
[0118] [Evaluation of mechanical strength of FRP laminated bodies] The mechanical properties (flexural strength, flexural modulus) of the resulting FRP laminate were measured based on JIS K 7074:1988 Bending test method for carbon fiber reinforced plastics.
[0119] [Measurement of deflection temperature under load] Based on the C method in JIS K 7191-2:2015 Plastics - Determination of deflection temperature under load, the deflection temperature under load of a test piece with a length of 80 mm, width of 10 mm, and thickness of 1 mm was measured using a Toyo Seiki Seisakusho HDT Tester 3M-2V.
[0120] <Phenoxy resin> A-1: PhenoToto YP-50S (bisphenol A type, manufactured by Nippon Steel Chemical & Material Co., Ltd., Mw = 60,000, hydroxyl equivalent = 284 g / eq), melt viscosity at 200°C = 400 Pa s, Tg = 84°C
[0121] <Difunctional epoxy resin> A-2: Epotohto YP-017 (bisphenol A type, Mw=4000, manufactured by Nippon Steel Chemical & Material Co., Ltd.), softening point=117℃
[0122] <Polycarbonate resin> B-1: Iupilon S3000 (Mitsubishi Engineering Plastics Corporation, Mw = 45,000), melt viscosity at 280°C = 1,020 Pa s, Tg = 149°C, Tm = 240°C B-2: Novarex 7022R (Mitsubishi Engineering Plastics Corporation, Mw = 21,000), melt viscosity at 280°C = 1,200 Pa·s, Tg = 160°C, Tm = 230-260°C
[0123] [Example 1] 90 parts by weight of phenoxy resin A-1 and 10 parts by weight of polycarbonate resin B-1 were prepared, and each was crushed and classified to obtain a powder with an average particle diameter D50 of 80 μm. The powder was dry-blended in a dry powder mixer (Aichi Electric Co., Ltd., rocking mixer) to prepare resin composition E1. The resulting resin composition E1 was cured by kneading for 15 minutes at 280° C. using a Labo Blast Mill (manufactured by Toyo Seiki Seisakusho), to obtain a cured product E1.
[0124] [Examples 2 to 7] Resin compositions E2 to E7 and cured products E2 to E7 were obtained in the same manner as in Example 1, except that the compounding ratio of the phenoxy resin A-1 and the polycarbonate resin B-1 was changed as shown in Table 1.
[0125] [Example 8] A resin composition E8 and a cured product E8 were obtained in the same manner as in Example 1, except that polycarbonate resin B-2 was used instead of polycarbonate resin B-1 and the blending ratio was the same as in Example 2.
[0126] [Example 9] Resin composition E9 and cured product E9 were obtained in the same manner as in Example 1, except that bifunctional epoxy resin A-2 was used instead of phenoxy resin A-1, polycarbonate resin B-2 was used instead of polycarbonate resin B-1, and the blending ratios were the same as in Example 3.
[0127] [Examples 10 and 11] Resin compositions E10 and E11 were prepared in the same manner as in Example 1, except that the compounding ratio of the phenoxy resin A-1 and the polycarbonate resin B-1 was changed as shown in Table 1. The resulting resin compositions E10 and E11 were cured by kneading for 15 minutes at 280° C. using a Labo Blast Mill (manufactured by Toyo Seiki Seisakusho), to obtain cured products E10 and E11.
[0128] DMA measurement and melt viscosity measurement were carried out for the resin compositions E1 to E11 and the cured products E1 to E11 obtained in Examples 1 to 11. The results are shown in Table 1. In all of the Examples, an increase in melt viscosity due to the crosslinking reaction between the phenoxy resin and the polycarbonate resin was confirmed, but in particular, the cured products E1 to E9 did not have a melting point and maintained a solid state even when heated.
[0129] [Comparative Example 1] The solidified product R1 of the phenoxy resin A-1 was subjected to DMA measurement and melt viscosity measurement. The results are shown in Table 1.
[0130] [Comparative Example 2] The solidified product R2 of the polycarbonate resin B-1 was subjected to DMA measurement and melt viscosity measurement. The results are shown in Table 1.
[0131] [Comparative Example 3] Resin composition R3 was prepared in the same manner as in Example 1, except that a polyamide resin (Polyamide 6, CM1013, manufactured by Toray Industries, Inc.) was used in place of polycarbonate resin B-1 and the blending ratio was as shown in Table 1. The obtained resin composition R3 was kneaded at 280° C. for 15 minutes in the same manner as in Example 1, but since no significant increase in viscosity was observed, the resin composition was cooled as it was to obtain a solidified material R3. The results are shown in Table 1.
[0132] [Reference examples 1 and 2] The resin composition E2 obtained in Example 2 was cured by kneading for 15 minutes at 260° C. (Reference Example 1) and 240° C. (Reference Example 2), respectively, to obtain cured products R4 and R5. The results are shown in Table 1.
[0133] [Table 1]
[0134] Furthermore, for the resin compositions E1 to E11, R1, and R2 obtained in the above Examples 1 to 11 and Comparative Examples 1 and 2, the viscosity was measured using a rheometer 0 minutes, 10 minutes, 20 minutes, 30 minutes, 40 minutes, 50 minutes, 60 minutes, 70 minutes, 80 minutes, 90 minutes, and 100 minutes after the temperature reached 280°C. The results are shown in FIG. 5.
[0135] [Example 12] Resin composition E1 obtained in Example 1 was powder coated on SA3202 (manufactured by Sakai Ovex Co., Ltd., plain woven open carbon fiber cloth material) from which the sizing agent had been removed as a reinforcing fiber substrate in an electrostatic field under conditions of a charge of 60 kV and an air blowing rate of 60 L / min so that Vf after molding was 60%. After that, the resin composition was heat-melted to the carbon fiber by heating at 250°C for 3 minutes in an oven to produce CFRP prepreg A with a thickness of 0.9 mm and a resin ratio (RC) of 30%. 13 sheets of the obtained CFRP prepreg A were used and pressed at 5 MPa for 10 minutes in a press machine heated to 280°C to produce a CFRP molded body X1. After cooling, the obtained CFRP molded body X1 was subjected to measurement of mechanical properties (stress at break and elastic modulus). The results are shown in Table 2.
[0136] [Examples 13 to 22, Comparative Examples 4 to 6] CFRP prepregs B to K of the Examples and CFRP prepregs L to N of the Comparative Examples were produced in the same manner as in Example 12, except that the resin compositions (or resins) obtained in Examples 2 to 11 and Comparative Examples 1 to 3 were used. Furthermore, CFRP molded bodies X2 to X11 of the Examples and CFRP molded bodies W1 to W3 of the Comparative Examples were produced, and mechanical properties (stress at break and elastic modulus) were measured. The results are shown in Table 2. The corresponding relationships with the resin compositions used are also shown in Table 2.
[0137] [Reference examples 3 and 4] A CFRP prepreg B was produced in the same manner as in Example 12, except that the resin composition E2 obtained in Example 2 was used, and further, CFRP molded bodies W4 and W5 were produced in the same manner as in Example 12, except that the pressing temperature was changed to 260°C (Reference Example 3) or 240°C (Reference Example 4), and mechanical properties (stress at break and elastic modulus) were measured. The results are shown in Table 2. The correspondence with the resin compositions used is also shown in Table 2.
[0138] [Table 2]
[0139] [Examples 23 to 33, Comparative Examples 7 and 8] CFRP prepregs a to k of the examples and CFRP prepregs l and m of the comparative examples were obtained in the same manner as in Examples 12 to 22 and Comparative Examples 4 and 5, except that SA3202 from which the sizing agent had not been removed was used as the reinforcing fiber base material. The obtained CFRP prepregs a to k, CFRP prepregs l, and m were pressed for 10 minutes at 5 MPa in a press machine heated to 280°C to produce CFRP molded bodies Y1 to Y11 of the examples and CFRP molded bodies Z1 and Z2 of the comparative examples, and the mechanical properties (stress at break and elastic modulus) were measured. The results are shown in Table 3. The correspondence with the resin compositions used is also shown in Table 3.
[0140] [Table 3]
[0141] Furthermore, the interlaminar shear strength and deflection temperature under load were measured for the CFRP molded body X2 obtained in Example 13 and the CFRP molded body X10 obtained in Example 21. The results are shown in Table 4.
[0142] [Table 4]
[0143] [Example 34] Phenoxy resin and polycarbonate resin were crushed and classified to produce two types of matrix resin powders with an average particle size D50 of 80μm. Next, a plain-woven reinforced fiber substrate made of opened carbon fiber (T700, manufactured by Toray Industries, Inc.) was prepared and powder-coated with each matrix resin powder separately in an electrostatic field under conditions of a charge of 100kV and a spray air pressure of 0.1MPa. After that, the phenoxy resin was heated and melted in an oven at 200℃ and the polycarbonate resin was heated and melted at 260℃ for 3 minutes each to heat-seal the resins, obtaining a phenoxy resin FRP molding material and a polycarbonate resin FRP molding material. The resin ratio (RC) of the obtained FRP molding material was 33% for the phenoxy resin FRP molding material and 32% for the polycarbonate resin FRP molding material. The phenoxy resin FRP molding material and the polycarbonate resin FRP molding material were laminated alternately so that the outermost layer was the phenoxy resin FRP molding material, and then heated and pressurized in a hot press at 5 MPa, 280°C, and 10 minutes, and the various physical properties of the resulting FRP laminate were measured. The results are shown in Table 5.
[0144] [Example 35] An FRP laminate was produced in the same manner as in Example 34, except that the hot-press molding temperature was 260° C., and various physical properties were measured. The results are shown in Table 5.
[0145] [Example 36] Phenoxy resin A-1 was extruded using a T-die extrusion molding machine under the conditions of a die width of 150 mm, a coat hanger die, and a lip width of 0.2 mm to obtain a phenoxy resin film having a thickness of 20 μm. The polycarbonate resin FRP molding material prepared in Example 34 and the above-mentioned phenoxy resin film were laminated together so that the outermost layer was the polycarbonate resin FRP molding material. The polycarbonate resin FRP molding material and the phenoxy resin film were laminated in such a way that one sheet of phenoxy resin film was laminated for every three sheets of polycarbonate resin FRP molding material, for a total of 51 sheets of both. The laminate was then heated and pressurized in a hot press at 5 MPa, 280° C., and 10 minutes, and the physical properties of the resulting FRP laminate were measured. The results are shown in Table 5.
[0146] [Example 37] An FRP laminate was prepared in the same manner as in Example 36, except that four sheets of polycarbonate resin FRP molding material were placed on the outermost layers, and one sheet of phenoxy resin film was placed on every six sheets of polycarbonate FRP molding material, for a total of 46 sheets of both, and various physical properties were measured. The results are shown in Table 5.
[0147] [Comparative Example 9] An FRP laminate was produced in the same manner as in Example 34, except that the hot-press molding temperature was 240° C., and various physical properties were measured. The results are shown in Table 5.
[0148] [Comparative Example 10] An FRP laminate was produced in the same manner as in Example 36, except that the hot-press molding temperature was 240° C., and various physical properties were measured. The results are shown in Table 5.
[0149] [Comparative Example 11] An FRP laminate was produced in the same manner as in Example 37, except that the hot-press molding temperature was 240° C., and various physical properties were measured. The results are shown in Table 5.
[0150] [Reference example 5] An FRP laminate was produced in the same manner as in Example 34, except that only the phenoxy resin FRP molding material was used, and various physical properties were measured. The results are shown in Table 5.
[0151] [Reference example 6] An FRP laminate was produced in the same manner as in Example 34, except that only the polycarbonate resin FRP molding material was used, and various physical properties were measured. The results are shown in Table 5.
[0152] [Table 5]
[0153] In the FRP laminate of the present invention, a strong adhesive interface is formed by the crosslinking reaction between the phenoxy resin and the polycarbonate resin, and therefore the interlaminar shear strength is greater than that of an FRP laminate in an insufficiently crosslinked state such as in Comparative Example 9, and the product can exhibit high mechanical properties that make it suitable for use as a structural material.
[0154] Although the embodiment of the present invention has been described in detail above for the purpose of illustration, the present invention is not limited to the above embodiment.
[0155] This application claims priority based on Japanese Patent Application No. 2019-057952 filed in Japan on March 26, 2019, and Japanese Patent Application No. 2019-066082 filed in Japan on March 29, 2019, the entire contents of which are incorporated herein by reference. [Explanation of symbols]
[0156] 10: Phenoxy resin FRP molding material 20: Polycarbonate resin FRP molding material 30: FRP laminated body (prepreg laminate) 40: Polycarbonate resin film 50A, 50B: FRP laminated body (film inserted laminate) 60: Phenoxy resin film 70: Reinforced fiber base material 80: Hybrid FRP molding material 90: FRP laminated molding (hybrid prepreg laminate)
Claims
1. A resin composition exhibiting curability by thermal crosslinking, comprising a first resin and a second resin different from the first resin, the first resin is a polyhydroxy polyether, and is at least one selected from the group consisting of a bifunctional epoxy resin having a weight average molecular weight of 4,000 or more and less than 10,000, and a phenoxy resin having a weight average molecular weight of 10,000 or more and 200,000 or less; the second resin is a polycarbonate resin; The resin composition is characterized in that the content ratio of the first resin to the second resin (first resin:second resin) is within a range of 9:1 to 3:7 by weight, and the resin composition is irreversibly crosslinked and cured at a temperature within a range of 280°C to 320°C.
2. The resin composition according to claim 1 , wherein the first resin and the second resin each have a bisphenol skeleton in the molecule.
3. 2. The resin composition according to claim 1, wherein the cured product obtained by thermally crosslinking the resin composition has a glass transition temperature (Tg) of 100° C. or higher as measured by dynamic mechanical analysis (DMA), and the cured product does not have a melting point (Tm).
4. The resin composition according to claim 1, wherein the displacement of a probe after measurement at a temperature in the range of 25°C to 300°C in dynamic mechanical analysis (DMA) of a cured product obtained by thermally crosslinking the resin composition is less than -1 mm based on the displacement before the measurement.
5. A cured molded product comprising the cured product of the resin composition according to claim 1.
6. A fiber-reinforced plastic molding material comprising a reinforcing fiber substrate and a powder of the resin composition according to claim 1 adhered to the reinforcing fiber substrate.
7. A fiber-reinforced plastic comprising a reinforcing fiber substrate and a cured product of the resin composition according to claim 1 adhered to the reinforcing fiber substrate.
Citation Information
Patent Citations
Electromagnetic relay
JP1981026330A
Production of light blocking film
JP1987078286A
Polycarbonate resin composition
JP1993302025A
Transfer sheet for thermal transfer recording
JP2000177256A
Aromatic polycondensation polymer compositions exhibiting enhanced strength properties
JP2005536597A