Two-component interface material, system including interface material, and method thereof
A two-component thermal interface material with a carbamate-polyamine reaction and conductive fillers addresses thermal conductivity and cost issues, providing effective thermal management in battery systems with improved stability and gap filling.
Patent Information
- Application Number
- JP2021569020
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-05-21
- Filing Date
- 2020-05-08
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2040-05-08
AI Technical Summary
Existing thermal interface materials face challenges such as poor thermal conductivity, abrasive nature, high cost, manufacturing difficulties, and inadequate gap filling, particularly in two-component reactive compositions used for thermal management in battery cells and modules.
A two-component thermal interface material comprising a carbamate-containing prepolymer and a polyamine compound, with conductive fillers like aluminum hydroxide, that reacts at room temperature to form a matrix with high thermal conductivity and low viscosity, using a catalyst to enhance the reaction and minimize filler abrasiveness.
The material achieves high thermal conductivity (up to 3.0 W/mK), low viscosity for effective gap filling, and cost-effectiveness, with improved storage stability and reduced abrasiveness, suitable for thermal management in battery systems.
Smart Images

Figure 0007566788000016 
Figure 0007566788000017 
Figure 0007566788000018
Abstract
Description
[Technical field]
[0001] The teachings herein are directed to thermal interface materials having generally high thermal conductivity, components and articles including the thermal interface materials, and related methods. The thermal interface materials are preferably formed from a two-component composition, each component including a matrix phase that is liquid at room temperature and one or more thermally conductive fillers dispersed in the matrix phase. The matrix phase of the first component preferably includes a carbamate-containing compound, and the matrix phase of the second component preferably includes a carbamate-reactive compound. [Background technology]
[0002] In the automotive industry, a trend towards reducing the weight of vehicles has occurred over the past decade. This trend towards lighter weight is mainly due to the reduction in the CO 2 The trend towards a lightweight construction has been driven by regulations to reduce emissions. In recent years, the strategy of lightweight construction has been further driven by the increase in the number of electric vehicles. The combination of the growing automobile market and the growing market share of electric vehicles will result in a high growth in the number of electric vehicles. There is a need to provide batteries with high energy density and high range. Several battery strategies currently follow concepts that differ in detail, but all long-range endurance battery concepts have in common the need for thermal management. In particular, thermal interface materials based on two-component reactive compositions are required to thermally connect the battery cells or modules with the cooling units.
[0003] Various compositions including conductive fillers and two-part reactive compositions are described in PCT Publication Nos. WO 2001 / 041213 A1, WO 2014 / 047932 A1, WO 2015 / 148318 A1, WO 2016 / 145651 A1, WO 2017 / 091974 A1, WO 2018 / 34721, and WO 2006 / 016936 A1, European Patent Application No. 1438829 A1, Japanese Patent Publication No. 2010 / 0138357, and U.S. Patent Application Publication No. 2009 / 0250655 A1, each of which is incorporated herein by reference in its entirety. In these prior attempts, the compositions suffered from one or more of the following needs for inexpensive thermal interface materials: the composition has poor thermal conductivity, the composition is difficult to manufacture, the composition does not fill gaps properly resulting in poor contact, the components of the composition do not react at room temperature, one or both of the components have poor shelf life stability, the composition requires expensive materials, or the composition requires abrasive fillers that can damage processing equipment. Summary of the Invention [Problem to be solved by the invention]
[0004] There continues to be a need for thermal interface materials (and especially two-part compositions) that have both high thermal conductivity and low viscosity. There also continues to be a need for thermal interface materials with non-abrasive filler materials. There also continues to be a need for thermal interface materials that are more economical in terms of raw material costs and / or manufacturing / processing costs. There also continues to be a need for two-part compositions with high filler content that are capable of flowing and filling gaps at room temperature. There also continues to be a need for materials that meet one or more of the above needs and further have one or more of the following characteristics: storage stability (e.g., retaining the ability to flow at room temperature after aging), the ability to react at room temperature to polymerize, crosslink, or both, good thermal conductivity, substantially or completely avoid the use of abrasive fillers, or lightweight (e.g., having a specific gravity of about 3 or less, about 2.8 or less, about 2.6 or less, about 2.5 or less, or about 2.4 or less). [Means for solving the problem]
[0005] One or more of the above needs may be accomplished using thermal interface materials in accordance with the teachings herein.
[0006] A first aspect of the teachings herein is directed to a two-part composition for a thermal interface material that includes a first component comprising at least one prepolymer that includes two or more carbamate groups, and a second component comprising at least one or more polyamine compounds capable of reacting with the prepolymer. The composition preferably includes (in the first component, the second component, or both) one or more catalysts for catalyzing the reaction between the prepolymer and the polyamine compound, and 50 weight percent or more of one or more conductive fillers, based on the total weight of the two-part composition.
[0007] A second aspect of the invention is a method comprising disposing a layer of the thermal interface material of the invention between a first component and a second component and applying pressure such that the thermal interface material contacts both the first component and the second component and fills the gap between the two components.
[0008] The first aspect may further be characterized by one or any combination of the following features: the prepolymer is formed by blocking one or more of the isocyanate groups (preferably about each, or completely each, of the isocyanate groups) of an aromatic polyisocyanate prepolymer with a phenol group of a blocking compound; the blocked compound comprises a terminal phenol group (preferably a single terminal phenol group) attached to a linear hydrocarbon chain (preferably the linear hydrocarbon chain comprises 6 or more, 8 or more, 10 or more, or 12 or more carbon atoms) (preferably the linear hydrocarbon chain comprises 60 or fewer, 30 or fewer, or 20 or fewer carbon atoms); one or more polyamines, the prepolymer, or both, have an average functionality greater than 2; The thermally conductive filler is preferably selected from aluminum hydroxide, aluminum oxide, aluminum powder, zinc oxide, boron nitride, and mixtures thereof; the first component comprises 75 weight percent or more of a thermally conductive filler preferably selected from aluminum hydroxide, aluminum oxide, aluminum powder, zinc oxide, boron nitride, and mixtures thereof; the second component comprises 75 weight percent or more of a thermally conductive filler preferably selected from aluminum hydroxide, aluminum oxide, aluminum powder, zinc oxide, boron nitride, and mixtures thereof; preferably, the surface of the thermally conductive filler, e.g., aluminum hydroxide, is partially or completely coated with a surface modifier to reduce the hydrophilicity of the surface; the composition has a D of about 3 or more. 90 / D 50the composition preferably comprises one or more plasticizers; the composition preferably comprises a fatty acid or an ester of a fatty acid; the composition comprises an epoxy resin in the first component; the weight ratio of prepolymer to epoxy resin is about 0.5 or more, more preferably about 0.8 or more, and even more preferably about 1.0 or more; the weight ratio of prepolymer to epoxy resin is about 10 or less, about 5 or less, or about 4 or less; the composition is substantially free of isocyanate-containing compounds; the amount of NCO in the first component is about 0.10 weight percent or less, about 0.0 or less, based on the total weight of the first component. the molar ratio of carbamate groups in the first component to amine groups in the second component is about 0.1 or more, about 0.2 or more, about 0.3 or more, about 0.4 or more, about 0.5 or more, or about 0.6 or more; the molar ratio of carbamate groups in the first component to amine groups in the second component is about and / or about 10 or less, about 5.0 or less, about 3.5 or less, about 2.5 or less, about 2.0 or less, or about 1.7 or less; the first component comprises calcium carbonate; the amount of calcium carbonate in the first component and / or composition is about 0.1 weight percent or more, preferably about 0.5 weight percent or more, or about 1.0 weight percent or more; the first component comprises some or all of the catalyst; the composition is selected from the group consisting of ZFW The thermal interface materials are characterized by a thermal conductivity of about 2.0 W / mK or greater, preferably about 2.5 or greater, more preferably about 2.8 or greater, even more preferably about 2.9 or greater, and most preferably about 3.0 or greater on a Stuttgart Thermal Interface Material Tester, with testing performed in Spaltplus mode with a thickness of 1.8-1.2 mm. The thermal interface materials described are considered to be Type I (viscous liquid) as described in ASTM 5470-12. The upper contact is heated to about 40° C. and the lower contact is heated to about 10° C., resulting in a sample temperature of about 25° C.The A and B components are mixed in a static mixer as applied from a manual cartridge system; the two-part composition cures at room temperature (preferably as characterized by an increase in compression force of about 60% or more, or about 100% or more after aging for 24 hours after mixing); the first component is storage stable (e.g., as characterized by a compression force of the first component of less than 700 N after aging for 3 days at 55° C.); or the two-part composition is characterized by a specific gravity of about 2.5 or less.
[0009] Another embodiment in accordance with the teachings herein is directed to an article that includes a first component that generates heat, a second component for removing heat, and a layer of thermal interface material sandwiched between the first and second components, the thermal interface material providing a path for transferring heat from the first component to the second component. The thermal interface material is preferably formed by a two-part composition in accordance with the teachings herein.
[0010] Another embodiment in accordance with the teachings herein is directed to a method that includes disposing a layer of a thermal interface material between a first component and a second component and applying pressure such that the thermal interface material contacts both the first component and the second component and fills a gap between the two components. The thermal interface material is preferably formed from a two-part composition in accordance with the teachings herein. [Brief description of the drawings]
[0011] [Figure 1] FIG. 1 illustrates the characteristics of a composition having a filler with a generally narrow particle size distribution (A), a composition having a filler with a generally broad particle size distribution (B), and a composition having a surface-modified filler with a generally broad particle size distribution (C). [Diagram 2] FIG. 1 illustrates the characteristics of a reaction between a surface modifier and a conductive filler, for example, the surface modifier can change the hydrophobicity of the surface. [Diagram 3]FIG. 1 shows exemplary compositions having various amounts of filler, where filler (A) has a narrow particle size distribution, (B) has a broad particle size distribution, and (C) has a broad particle size distribution and a surface modifier to reduce or minimize bonding between the matrix phase material and the filler. [Figure 4] 1 is an optical micrograph of an exemplary conductive filler having a broad particle size distribution. [Diagram 5] 1A-1C illustrate exemplary features of a device including a thermal interface material. [Figure 6] FIG. 1 is an exemplary diagram of a battery including a thermal interface material. [Figure 7] FIG. 1 illustrates various chemical reactions that may be used or avoided in accordance with the teachings herein. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] Unless otherwise specified, the term "consisting essentially of" includes amounts of about 90 weight percent or more, about 95 weight percent or more, about 98 weight percent or more, or about 99 weight percent or more.
[0013] Unless otherwise specified, the terms "conductive" and "conductivity" refer to "thermally conductive" and "thermal conductivity."
[0014] The thermal interface material comprises two or more phases, preferably two phases. The first phase of the thermal interface material is a matrix phase. The matrix phase is preferably a continuous phase. However, the matrix phase may be a co-continuous phase and / or may comprise one or more subphases. Preferably, the matrix phase comprises, consists essentially of, or consists entirely of one or more polymers, oligomers, or polymerizable compounds. The matrix phase preferably comprises, consists essentially of, or consists entirely of one or more materials that are liquid at room temperature or require minimal heating to liquefy. The second phase is a discontinuous phase that is dispersed in the matrix phase. It will be understood that the discontinuous phase may be coated with one or more additional phases that provide an interface between the discontinuous phase and the matrix phase. Typically, the matrix phase comprises a material that generally has a low thermal conductivity (e.g., about 1 W / mK or less, or about 0.2 W / mK or less), so that the thermal conductivity of the composition depends primarily on the discontinuous phase. The discontinuous phase comprises one or more filler materials that are solid at room temperature. Because the filler phase is required to provide much of the heat transport, it is necessary to include high concentrations of filler to overcome the fact that the filler particles are generally dispersed in the matrix phase.
[0015] The thermal interface material may be formed from a single composition or may be formed by combining two or more components, each having a different composition. For example, the thermal interface material may be formed by mixing a first component (the A component) and a second component (i.e., the B component) of a two-component composition. Typically, upon mixing, the matrix phase of the composition is formed by combining the matrix phases of each component. The combined matrix phase is preferably reactive, resulting in an increase in the molecular weight of one or more compounds in the matrix phase. As an example, a compound in the first component may react with a compound in the second component. As another example, the reaction of a compound in the first component may be promoted by a catalyst in the second component. The reaction may be any reaction that increases the viscosity of the matrix phase. Preferably, the reaction includes a polymerization reaction, a crosslinking reaction, or both. In some applications, it is desirable to avoid the thermal interface material coming into contact with a temperature-sensitive component and heating the component to a temperature that may degrade or lose performance. Preferably, the reaction can proceed at a reaction temperature of about 50° C. or less, about 40° C. or less, about 30° C. or less, or about 23° C. or less. Preferably, the reaction can proceed at a reaction temperature of about -10° C. or more, about 0° C. or more, or about 10° C. or more. For example, the reaction can occur at about room temperature (e.g., about 23° C.). If the reaction is exothermic, the temperature rise due to the release of this energy is typically about 30° C. or less, about 20° C. or less, or about 10° C. or less. In some applications, it is desirable for the reaction to occur quickly (e.g., in about 1 hour or less). However, it is preferred that the reaction occur over a longer period of time so that a sudden temperature rise is avoided. Preferably, the reaction time may be about 30 minutes or more, more preferably about 1 hour or more, even more preferably about 4 hours or more, even more preferably about 8 hours or more, and most preferably about 24 hours or more. The reaction time is typically about 30 days or less, about 15 days or less, or about 7 days or less.
[0016] When the thermal interface material is provided as a two-component composition, the two components can be combined in any convenient volume ratio. The volume ratio of the first component to the second component can be about 100:1 or less, about 10:1 or less, about 3:1 or less, about 2:1 or less, or about 1:1 or less. The volume ratio of the first component to the second component can be about 1:100 or more, about 1:10 or more, about 1:3 or more, about 1:2 or more, or about 1:1 or more. The first component and the second component can be packaged separately. The first component and the second component can be packaged in a single container, and typically the two components are separated to avoid contact and / or mixing before use.
[0017] Thermal interface materials typically have a specific gravity of about 1.50 or more, or about 1.8 or more, due to the fillers in the composition. In some applications, such as during transportation, it may be desirable for the thermal interface material to be lightweight. Preferably, the thermal interface material has a specific gravity of about 4.0 or less, more preferably about 3.0 or less, even more preferably about 2.5 or less, even more preferably about 2.4 or less, and most preferably about 2.3 or less.
[0018] filling material The composition according to the teachings herein includes one or more fillers to increase the thermal conductivity of the composition. The fillers may include ultra-high conductive fillers (e.g., fillers having a thermal conductivity of about 100 W / mK), but such fillers are typically abrasive and / or expensive. Preferably, the one or more fillers include, consist essentially of, or consist entirely of one or more conductive fillers having a thermal conductivity of about 80 W / mK or less, about 50 W / mK or less, about 30 W / mK or less, about 20 W / mK or less, or about 15 W / mK or less. The conductive fillers preferably have a thermal conductivity of about 3 W / mK or more, about 4 W / mK or more, about 5 W / mK or more, or about 6 W / mK or more. The conductive fillers may be characterized by a thermal conductivity of about 10+ / -10%, about 10+ / -20%, or about 10+ / -30%. Preferably, the amount of superconductive filler in the composition is about 15 weight percent or less, more preferably about 4 weight percent or less, even more preferably about 1 weight percent or less, and most preferably about 0.3 weight percent or less, based on the total weight of the one or more fillers. The amount of superconductive filler in the composition can be about 0.0 weight percent or more, based on the total weight of the one or more fillers. The amount of conductive filler (i.e., superconductive filler) can be about 80 weight percent or more, about 85 weight percent or more, about 90 weight percent or more, about 93 weight percent or more, about 96 weight percent or more, about 98 weight percent or more, about 99 weight percent or more, or about 99.7 weight percent or more, based on the total weight of the one or more fillers. The amount of conductive filler can be about 100 weight percent or less, based on the total weight of the one or more fillers.
[0019] When present, the superconductive filler can be any filler that has a thermal conductivity of about 100 W / mK. Examples of superconductive fillers include boron nitride and aluminum powder.
[0020] The conductive filler can be any filler having thermal conductivity, such as those described herein. For example, the conductive filler can have a thermal conductivity of about 3 W / mK to about 80 W / mK. The conductive filler is preferably non-abrasive (e.g., less abrasive than boron nitride, less abrasive than aluminum powder, or both). An example of a non-abrasive conductive filler is aluminum hydroxide (i.e., ATH) powder. Aluminum hydroxide powder has a thermal conductivity of 3 to 80 W / mK (typically about 10 W / mK).
[0021] Conductive fillers typically contain one or more metal or metalloid atoms and one or more nonmetal atoms. Metalloid atoms include boron, silicon, germanium, arsenic, antimony, and tellurium. Preferred metal atoms include alkali metals, alkaline earth metals, transition metals, and post-transition metals. The amount of nonmetal atoms in the conductive filler should be high enough so that the conductive filler is not hard and abrasive. Examples of hard and abrasive metal or metalloid-containing fillers include SiC, TiC, and BN. These hard and abrasive abrasive fillers contain 50 atomic percent of metal or metalloid. Preferably, the concentration of nonmetal atoms in the conductive filler is greater than about 50 atomic percent of nonmetal atoms, more preferably about 65 percent or more, even more preferably about 75 percent or more, and most preferably about 80 percent or more, based on the total number of atoms in the conductive filler. The concentration of non-metallic atoms may be about 95 atomic percent or less, about 93 atomic percent or less, about 90 atomic percent or less, or about 88 atomic percent or less. The conductive filler preferably has a sufficient concentration of metal atoms such that the thermal conductivity is about 3 W / mK. The combined concentration of any metals and metalloids in the conductive filler is preferably about 5 atomic percent or more. The combined concentration of any metals and metalloids in the conductive filler may be less than 50 atomic percent, about 35 atomic percent or less, about 25 atomic percent or less, or about 20 atomic percent or less.
[0022] Preferred compositions include a sufficient amount of conductive filler such that the thermal conductivity of the composition is about 1.5 W / mK or greater, preferably about 2.0 W / mK or greater, more preferably about 2.5 W / mK or greater, and most preferably about 3.0 W / mK or greater. The thermal conductivity of the composition is typically about 10 W / mK or less, about 7 W / mK or less, or about 5 W / mK or less as measured on a ZFW Stuttgart Thermal Interface Materials Tester according to ASTM 5470-12, the test being performed in Spaltplus mode with a thickness of 1.8-1.2 mm, the described thermal interface material being considered to be Type I (viscous liquid) as described in ASTM 5470-12, the upper contact being heated to about 40° C. and the lower contact being heated to about 10° C., resulting in a sample temperature of about 25° C.
[0023] The A and B components are mixed in a static mixer when applied from a manual cartridge system. If the amount of conductive filler is too low, the composition will not be able to conduct enough heat to manage the temperature of the device. To achieve such high thermal conductivity of the composition, the composition typically has a high concentration of conductive filler. Preferably, the amount of conductive filler in the composition is about 60 weight percent or more, more preferably about 70 weight percent or more, even more preferably about 75 weight percent or more, even more preferably about 80 weight percent or more, even more preferably about 85 weight percent or more, and most preferably about 88 weight percent or more, based on the total weight of the composition. The amount of conductive filler in the composition should be low enough so that the conductive filler can be dispersed in the matrix. Typically, the amount of conductive filler is about 95 weight percent or less, more preferably about 92 weight percent or less, based on the total weight of the composition.
[0024] The conductive filler preferably has a Mohs hardness that is low enough so that the conductive filler is generally non-abrasive. Preferably, the conductive filler has a Mohs hardness of about 7.0 or less, preferably about 5.0 or less, and most preferably about 4.0 or less. The conductive filler may have a Mohs hardness of about 0.5 or more, about 1.5 or more, or about 2.0 or more.
[0025] Conductive fillers typically contain MX bonds, where M is a metal and X is a nonmetal. Preferably, the ratio of MX bonds to MM bonds (metal-metal bonds) in the filler can be about 2.0 or more, about 3.0 or more, or about 4.0 or more. It is understood that conductive fillers may not contain MM bonds. An example of a conductive filler that is generally free of MM bonds is aluminum hydroxide.
[0026] The one or more fillers in the composition preferably have an average specific gravity of about 3.5 or less, more preferably about 3.0 or less, even more preferably about 2.8 or less, even more preferably about 2.6 or less, and most preferably about 2.5 or less. The average specific gravity of the one or more fillers can be about 1.8 or more, about 2.2 or more, or about 2.4 or more. The average specific gravity of a filler comprising a mass fraction ma of filler A having a specific gravity va and a mass fraction mb of filler B having a specific gravity vb (where ma+mb=1) is defined as follows: 1 / [(ma / va)+(mb / vb)].
[0027] In addition to the thermally conductive filler, other fillers may include calcium carbonate and / or calcium oxide. If used, the total amount of calcium carbonate and calcium oxide is preferably about 20 weight percent or less, more preferably about 10 weight percent or less, and most preferably about 5 weight percent, based on the total weight of the one or more fillers in the composition (e.g., in a two-part composition). The total amount of calcium carbonate and calcium oxide may be about 0 weight percent or more, about 0.4 weight percent or more, or about 0.8 weight percent or more, based on the total weight of the one or more fillers in the composition (e.g., in a two-part composition).
[0028] Preferred fillers are selected from aluminum hydroxide, aluminum oxide, aluminum powder, zinc oxide, boron nitride, and mixtures thereof. Particularly preferred fillers are selected from aluminum hydroxide, aluminum oxide, and mixtures thereof. Most particularly preferred is aluminum hydroxide.
[0029] Particle size distribution To achieve a combination of high thermal conductivity of the composition and the ability to mix and process the composition, the conductive filler preferably has a broad particle size distribution.
[0030] A broad particle size distribution may allow particles to pack more efficiently. The particle size distribution is determined by D 10 , D 50 , and D 90 The particle size can be characterized by 2.24×10 -3 M solution (1 g Na in 1000 ml deionized water) 4 P 2 O 7 x10H 2 O) according to ISO 13320.
[0031] Fillers with a broad particle size distribution may be characterized by one or more of the following: Generally, a high D 90 / D 50 Ratio of, generally high D 90 / D 10 Ratio of, or generally high D 50 / D 10 or any combination thereof. Preferably, D 90 / D 50 is about 3 or more, about 4 or more, about 5 or more, about 6 or more, or about 8 or more. 90 / D 50 The ratio of D may be about 100 or less, or about 40 or less. 90 / D 10 is about 20 or more, about 40 or more, about 60 or more, or about 80 or more. 90 / D 10 The ratio may be about 1000 or less, or about 400 or less. 90 / D 50 The ratio of D may be about 100 or less, or about 40 or less. 50 / D 10 is about 8 or more, about 10 or more, or about 12 or more. 50 / D 10The ratio of large particles (D 90 The density (characterized by the D value) should be high enough to create sites for the filling of one or more small particles. 90 is about 10 μm or more, more preferably about 20 μm or more, even more preferably about 40 μm or more, and most preferably about 60 μm or more. 90 If D is too large, it may be difficult to process the composition. 90 is about 2000 μm or less, more preferably about 1000 μm or less, and most preferably about 500 μm or less. 10 The D values (characterized by the D value) should be small enough so that they can be incorporated into the sites between the large particles. 10 is about 4 μm or less, about 2 μm or less, or about 1 μm or less. Typically, it is difficult and expensive to make very small particles. Therefore, D 10 is preferably about 0.1 μm or greater, or about 0.25 μm or greater, although smaller particles may be used. The conductive filler may have a first portion having an average particle size of about 10 μm or less and a second portion having an average particle size of about 50 μm or greater (preferably, the first portion and the second portion are each present in an amount of about 25 weight percent or greater, about 30 weight percent or greater, or about 35 weight percent or greater of the conductive filler).
[0032] FIG. 1 illustrates the effect of having a broad particle size distribution 6 (B) on the ability to pack small particles 7 between large particles 8 compared to a filler with a narrow particle size distribution 4 (A). With a broad particle size distribution, the particles 2 are closer together as the particle concentration increases and there may be bridges between the two particles due to the matrix phase material 3. The adhesion and / or bridges of the matrix phase to the particle surface may reduce the ability to flow or process the composition. To improve processability, the particles preferably have a surface modifier. For example, (C) has a broad particle size distribution 6 and a coating 5 (e.g., of a surface modifier) to reduce or minimize bonding between the matrix phase material and the filler.
[0033] FIG. 2 shows the results of the study of aluminum hydroxide (i.e., Al(OH)), a conductive filler with a wide particle size distribution. 3 ) is an optical microscope photograph of an example of the present invention.
[0034] Filler surface modifier Although in many filled polymer systems it is desirable to have good compatibility and / or bonding between the matrix phase and the filler phase, the applicant has found that for these highly filled compositions, such compatibility and / or bonding can create bridges between adjacent filler particles that impede the flow of the composition. It is preferred that the matrix phase material does not bond with the surface of the filler. For example, covalent, ionic, and hydrogen bonds may be reduced, minimized, or even completely avoided. This can be achieved by the selection of the matrix phase material and the conductive filler material. Alternatively, the filler material may be treated with one or more surface modifiers to reduce, minimize, or eliminate bonding with the matrix phase material.
[0035] The surface modifier can partially or completely cover the surface of the conductive filler particle. The surface modifier can have one or more functional groups that react with the conductive filler particle. Thus, the surface modifier can be covalently bonded to the conductive filler. As an example, the conductive filler may include an M-OH group (wherein M is a metal atom), and the surface modifier may include a functional group that reacts with the M-OH group to form a direct or indirect bond between the surface modifier and M.
[0036] The surface of the conductive filler may be hydrophobized with a surface modifier. For example, the surface modifier may include an alkyl moiety and one or more functional groups at or near one end of the alkyl moiety. The alkyl moiety preferably includes about 6 or more carbon atoms, more preferably about 8 or more carbon atoms, even more preferably about 10 or more carbon atoms, and most preferably about 12 or more carbon atoms. The one or more functional groups may be selected to react with the surface of the conductive filler. For example, the one or more functional groups may include one or more alkoxysilanes. Such functional groups may be useful for bonding the surface modifier to conductive fillers that include M-OH groups, such as aluminum hydroxide, in particular. An example of a reaction between a conductive filler and a surface modifier is shown in FIG. 3.
[0037] It will be appreciated that the surface modifier may be added to the filler before or after the conductive filler is mixed with the matrix phase material. For example, the conductive filler may be coated and / or reacted with the surface modifier before mixing the conductive filler with the matrix phase material. As another example, the surface modifier may be mixed with the matrix phase material to form a premix, which is then combined with the conductive filler. As another example, the conductive filler may be mixed with the matrix phase material, and then the surface modifier may be added to the mixture.
[0038] Matrix Phase The matrix phase of the thermal interface material typically comprises, consists essentially of, or consists entirely of one or more liquid materials. For example, the matrix phase of the first component, the second component, or both may comprise one or more materials that are liquid at room temperature. The amount of liquid compounds in the first component, the second component, or both is preferably about 50 weight percent or more, more preferably about 70 weight percent or more, even more preferably about 85 weight percent or more, even more preferably about 95 weight percent or more, and most preferably about 98 weight percent or more, based on the total weight of the matrix phase of the components. The amount of liquid compounds in the first component, the second component, or both may be about 100 weight percent or less, based on the total weight of the matrix phase of the components. Since the matrix phase is preferably a minor phase (i.e., present in an amount of about 50 volume percent or less of the composition), the amount of liquid compounds in the first component, the second component, or both is preferably about 50 volume percent or less, based on the total weight of the components. The one or more liquids should be present in sufficient amounts so that the components can be mixed without disintegrating. Preferably, the weight percent of the one or more liquid compounds in the first component, the second component, or both is about 3 weight percent or more, about 5 weight percent or more, or about 7 weight percent or more, based on the total weight of the components. The one or more liquids should be present in a sufficiently small amount such that separation between filler particles is reduced and the thermal conductivity of the components or the overall composition is about 2.0 W / mK or more, about 2.5 W / mK or more, about 2.8 W / mK or more, about 2.9 W / mK or more, or about 3.0 W / mK or more, as measured on a ZFW Stuttgart thermal interface material tester according to ASTM 5470-12, the test being performed in Spaltplus mode at a thickness of 1.8-1.2 mm, and the described thermal interface material is considered to be Type I (viscous liquid) as described in ASTM 5470-12, with the upper contact heated to about 40° C. and the lower contact heated to about 10° C., resulting in a sample temperature of about 25° C.Preferably, the one or more liquid compounds in the first component, the second component, or both, is about 30 weight percent or less, more preferably about 25 weight percent or less, even more preferably about 20 weight percent or less, even more preferably about 15 weight percent or less, and most preferably about 13 weight percent or less, based on the total weight of the components.
[0039] The total amount of matrix phase in the thermal interface material (e.g., after mixing the first and second components and optionally reacting the two components) is preferably about 30 weight percent or less, more preferably about 25 weight percent or less, even more preferably about 20 weight percent or less, even more preferably about 15 weight percent or less, and most preferably about 13 weight percent or less, based on the total weight of the composition. The total amount of matrix phase in the thermal interface material (e.g., after mixing the first and second components and optionally reacting the two components) is preferably about 3 weight percent or more, more preferably about 5 weight percent or more, even more preferably about 7 weight percent or more, and most preferably about 8 weight percent or more, based on the total weight of the composition.
[0040] The first component (i.e., the carbamate-containing component) comprises one or more carbamate-containing compounds. The carbamate-containing compound may be any compound that contains a carbamate group, preferably two or more spaced apart carbamate groups. The spaced apart carbamate groups are typically spaced apart by 6 or more, 10 or more, or 15 or more atoms on the backbone of the compound. The carbamate-containing compound may be a monomeric, oligomeric compound. The oligomeric compound may be a prepolymer. The carbamate-containing compound may be prepared by reacting an isocyanate-containing compound with a phenol-containing compound to form a carbamate group. The carbamate-containing compound.
[0041] It will be appreciated that a carbamate-containing compound containing two or more carbamate groups can be formed by i) reacting an isocyanate group in an isocyanate-containing compound with a phenol-containing compound having a single phenol group, where the isocyanate-containing compound contains two or more spaced apart isocyanate groups, or ii) reacting each phenol group in a phenol-containing compound with an isocyanate-containing compound having a single isocyanate group, where the phenol-containing compound contains two or more spaced apart phenol groups. Typically, the spaced apart isocyanate groups or spaced apart phenol groups are separated by 6 or more, 10 or more, or 15 or more atoms on the backbone of the compound.
[0042] Preferably, the first component and / or the entire two-component composition are substantially free of isocyanate-containing compounds so that the components and compositions have good shelf-life stability. Without being bound by theory, it is believed that a high concentration of filler and / or a high amount of water in the filler may result in polymerization and / or crosslinking of the isocyanate-containing compounds, leading to an increase in the viscosity or even hardening of the first component. Preferably, the amount of isocyanate groups in the first component is about 0.10 weight percent or less, more preferably about 0.05 weight percent or less, even more preferably about 0.01 weight percent or less, and most preferably about 0.005 weight percent or less, based on the total weight of the first component or based on the total weight of the matrix phase of the first component. The first component may even be completely free of isocyanate groups. The molar ratio of isocyanate groups to carbamate groups in the first component is preferably about 0.35 or less, more preferably about 0.20 or less, even more preferably about 0.10 or less, even more preferably about 0.03 or less, and most preferably about 0.01 or less. The molar ratio of isocyanate groups to carbamate groups in the first component may be about 0.00 or more.
[0043] The carbamate-containing compound preferably has an equivalent weight (i.e., molecular weight divided by the number of carbamate groups) of about 10,000 g / eq or less, more preferably about 7,000 or less, even more preferably about 4,000 or less, even more preferably about 3,000 or less, and most preferably about 2,000 or less. The carbamate-containing compound may have an equivalent weight of about 300 g / eq or more, about 500 g / eq or more, or about 700 g / eq or more. The carbamate-containing compound preferably has a number average molecular weight of about 20,000 g / mole or less, more preferably about 10,000 or less, even more preferably about 7,000 or less, even more preferably about 6,000 or less, and most preferably about 5,000 or less. The carbamate-containing compound preferably has a number average molecular weight of about 500 g / mole or more, about 1000 g / mole or more, or about 1,500 g / mole or more. Molecular weight can be measured by gel permeation chromatography (GPC), for example using a Malvern Viscotek GPC max device. Tetrahydrofuran (THF) is preferably used as the eluent, and a PL GEL MIXED D (Ailent, 300×7.5 mm, 5 μm) can be used as the column, along with a refractive index and / or light scattering detector. For example, a MALVERN Viscotek TDA can be used as the detector.
[0044] The carbamate-containing compound may be prepared by reacting an isocyanate-containing compound containing one or more isocyanate groups with a phenol-containing compound containing one or more phenol groups, where the resulting compound contains two or more carbamate groups. The isocyanate-containing compound may be a prepolymer. The isocyanate-containing prepolymer may be formed by reacting a diisocyanate compound with a polyol, where an excess of isocyanate is used so that essentially all of the polyol is reacted. The diisocyanate may include an aromatic isocyanate, an aliphatic isocyanate, or both. Preferably, the diisocyanate comprises or consists essentially of an aromatic diisocyanate. It will be understood that the diisocyanate may be replaced by a compound containing more than two isocyanate groups. The polyol is preferably a polyether polyol. The polyol may have two or more OH groups. It will be understood that instead of using a prepolymer, the phenol-containing compound may be reacted directly with the diisocyanate. Phenol-containing compounds typically have a straight-chain hydrocarbon attached to the phenol group, providing the compound with some aliphatic character. The straight-chain hydrocarbon preferably contains about 3 or more carbon atoms, more preferably about 5 or more carbon atoms, even more preferably about 8 or more carbon atoms, and most preferably about 10 or more carbon atoms. The straight-chain hydrocarbon preferably contains about 50 or less carbon atoms, about 30 or less carbon atoms, about 24 or less carbon atoms, or about 18 or less carbon atoms. The phenol-containing compound is preferably a lipid.
[0045] An example of a carbamate-containing compound is the reaction product of an aromatic polyisocyanate prepolymer (based on toluene diisocyanate reacted with a polyether polyol having an NCO content of about 4-5% and an equivalent weight of about 500-1500 g / eq) and a phenol-containing lipid (such as cardanol). The compounds are preferably reacted in the presence of a catalyst, heat, and an inert atmosphere. The reaction temperature is preferably about 30° C. or higher, more preferably about 40° C. or higher. The reaction temperature is preferably about 130° C. or lower, more preferably about 100° C. or lower. The catalyst may be a Lewis acid or Lewis base catalyst. Particularly preferred catalysts are tin catalysts, especially dioctyltin dineodecanoate or amine catalysts, especially tertiary amine catalysts, such as DABCO (1,4-diazabicyclo[2.2.2]octane).
[0046] The carbamate-containing compound may be a blocked isocyanate compound in which the isocyanate group is blocked by a phenol group to form a carbamate group. Although such blocked isocyanate groups (i.e., isocyanate groups converted to carbamate groups) can be deblocked by heating, it may be desirable to avoid heating the two-component composition after the components are mixed and contacted with a device (e.g., a heat generating device). Thus, it may be desirable to react the carbamate group with a compound of the second component without deblocking the compound (i.e., without forming an isocyanate group). Thus, the second component preferably includes one or more carbamate-reactive compounds capable of reacting with the carbamate group to polymerize or crosslink at least the carbamate-containing compound. The carbamate-reactive compounds may react with the carbamate group to increase the viscosity of the composition.
[0047] The carbamate reactive compound may include any carbamate reactive group capable of reacting with a carbamate group. Preferably, the carbamate reactive compound includes one or more amine groups. The amine group may be any amine group (primary, secondary, or tertiary), with the preferred amine groups being primary and secondary amines, and the most preferred amine group being primary amines. The carbamate reactive compound is preferably a polyamine containing two or more amine groups. For example, the carbamate reactive compound may include a first polyamine having two amine groups and a second polyamine having more than two amine groups. The amine groups of the polyamine are typically spaced apart by two or more backbone atoms (i.e., the atoms that define the shortest covalent bond connecting the two groups). Preferably, each amine group is spaced apart from the other amine groups by 5 or more backbone atoms, more preferably about 6 or more backbone atoms, even more preferably about 8 or more backbone atoms, and most preferably about 10 or more backbone atoms.
[0048] The carbamate reactive component (e.g., the second component) may include one or more polyols. However, any reaction between the polyol and the first component may be minimized, especially for applications where heating the composition (e.g., after mixing) to a temperature of about 60° C. or higher (or about 100° C. or higher) is avoided. When a polyol is present in the second component, the molar ratio of hydroxyl groups (e.g., of the polyol) to amine groups (e.g., of the polyamine) is preferably about 1.5 or less, more preferably about 0.9 or less, even more preferably about 0.6 or less, and most preferably about 0.3 or less. The molar ratio of hydroxyl groups to amine groups in the second component may be about 0.0 or more, or about 0.01 or more.
[0049] Surface modifiers (for fillers) Although in many filled polymer systems it is desirable to have good compatibility and / or bonding between the matrix phase and the filler phase, it has surprisingly been found that for these highly filled compositions, such compatibility and / or bonding can create bridges between adjacent filler particles that prevent the composition from flowing. It is preferred that the matrix phase material does not bond with the surface of the filler. For example, covalent bonds, ionic bonds, and hydrogen bonds may be reduced, minimized, or even completely avoided. This can be achieved by the selection of the matrix phase material and the conductive filler material. Alternatively, the filler material may be treated with one or more surface modifiers to reduce, minimize, or eliminate bonding with the matrix phase material.
[0050] The surface modifier can partially or completely cover the surface of the conductive filler particle. The surface modifier can have one or more functional groups that react with the conductive filler particle. Thus, the surface modifier can be covalently bonded to the conductive filler. As an example, the conductive filler may include an M-OH group (wherein M is a metal atom), and the surface modifier may include a functional group that reacts with the M-OH group to form a direct or indirect bond between the surface modifier and M.
[0051] The surface of the conductive filler may be hydrophobized with a surface modifier. For example, the surface modifier may include an alkyl moiety and one or more functional groups at or near one end of the alkyl moiety. The alkyl moiety preferably includes about 6 or more carbon atoms, more preferably about 8 or more carbon atoms, even more preferably about 10 or more carbon atoms, and most preferably about 12 or more carbon atoms. The one or more functional groups may be selected to react with the surface of the conductive filler. For example, the one or more functional groups may include one or more alkoxysilanes. Such functional groups may be useful for bonding the surface modifier to conductive fillers that include M-OH groups, such as aluminum hydroxide, in particular. An example of a reaction between a conductive filler and a surface modifier is shown in FIG. 3.
[0052] It will be appreciated that the surface modifier may be added to the filler before or after the conductive filler is mixed with the matrix phase material. For example, the conductive filler may be coated and / or reacted with the surface modifier before mixing the conductive filler with the matrix phase material. As another example, the surface modifier may be mixed with the matrix phase material to form a premix, which is then combined with the conductive filler. As another example, the conductive filler may be mixed with the matrix phase material, and then the surface modifier may be added to the mixture.
[0053] As shown in Figure 4(A), when a conductive filler having a narrow particle size distribution is used, even at low filler loadings (e.g., only about 60 weight percent), the resulting composition may have a rough surface. As shown in Figure 4(B), the ability to increase filler loadings is improved by using fillers with a broad particle size distribution. As shown in Figure 4(C), the ability to increase filler loadings is further improved by using fillers with a broad particle size distribution and further by adding a surface modifier that reduces, minimizes, or eliminates bonding between the matrix phase material and the filler particles.
[0054] catalyst The composition preferably includes one or more catalysts for promoting the reaction between the carbamate-containing compound and the carbamate-reactive compound (such as the polyamine-containing compound). The catalyst may include a Lewis acid or Lewis base catalyst. The Lewis acid catalyst may be an organometallic compound that preferably includes one or more aliphatic groups. Each aliphatic group preferably includes 4 or more, 6 or more, or 8 or more carbon atoms. The organometallic compound is preferably a tin compound. An example of a tin-containing Lewis acid catalyst is dioctyltin dineodecanoate. The one or more catalysts may include an amine catalyst. The included amine catalyst may preferably include an aliphatic group, an aromatic group, or both. An example of an amine catalyst is tris-2,4,6-dimethylaminomethylphenol, or DABCO (1,4-diazabicyclo[2.2.2]octane). The catalyst should be used in an amount sufficient to promote the reaction between the carbamate-containing compound and the polyamine. Preferably, the amount of catalyst is about 0.05 weight percent or more, more preferably about 0.10 weight percent or more, even more preferably about 0.20 weight percent or more, even more preferably about 0.4 weight percent or more, and most preferably about 0.75 weight percent or more, based on the total weight of the matrix phase in the total composition (or based on the total weight of the liquid materials in the composition). Preferably, the amount of catalyst is about 10 weight percent or less, more preferably about 8 weight percent or less, even more preferably about 5 weight percent or less, and most preferably about 4 weight percent or less, based on the total weight of the matrix phase in the total composition (or based on the total weight of the liquid materials in the composition).
[0055] The catalyst may be provided in the first component, the second component, or both. As an example, the first component and the second component may each contain both an amine catalyst and an organometallic catalyst (e.g., a tin-containing Lewis acid catalyst). As another example, one component (e.g., the first component or the second component) may include an organometallic catalyst (e.g., a tin-containing Lewis acid catalyst) and the other component may include an amine catalyst. As another example, both the first component and the second component may include an organometallic catalyst (e.g., a tin-containing Lewis acid catalyst), which may be the same or different.
[0056] Preferred catalysts are liquid at room temperature.
[0057] Plasticizer The first component, the second component, or both components may include one or more plasticizers. The plasticizer is preferably a compound that does not react with the carbamate groups of the first component. The plasticizer is preferably a compound that does not react with the amine groups of the second component. The plasticizer is liquid at room temperature and forms part of the matrix phase. The plasticizer may be present in the first component, the second component, or both in an amount of about 0 weight percent or more, preferably about 10 weight percent or more, more preferably about 20 weight percent or more, and most preferably about 25 weight percent or more, based on the total weight of the matrix phase of the components. The plasticizer may be present in the first component, the second component, or both in an amount of about 75 weight percent or less, preferably about 65 weight percent or less, more preferably about 60 weight percent or less, and most preferably about 55 weight percent or less, based on the total weight of the matrix phase of the components.
[0058] Preferred plasticizers have a weight average molecular weight of about 2,000 g / mol or less, more preferably about 1,000 g / mol or less, even more preferably about 800 g / mol or less, and most preferably about 600 g / mol or less. The plasticizers are liquid at a temperature of about 100° C. Preferred plasticizers have a molecular weight of about 125 g / mol, more preferably about 175 g / mol, and most preferably about 225 g / mol.
[0059] Coloring agent The composition may optionally include a dye, pigment, or other colorant to provide the composition with a predetermined color. When used, the colorant may be included in the first component, the second component, or both. The colorant is typically present in an amount of about 1 weight percent or less, about 0.5 weight percent or less, or about 0.2 weight percent or less, based on the total weight of the two-part composition. The colorant may be provided as a neat material or may be mixed with a carrier material (typically a carrier liquid). The carrier material is preferably a material described herein for use in the first component and / or the second component. For example, the carrier material may be an epoxy resin, a carbamate-containing compound, a plasticizer, a polyol, a catalyst, a carbamate-reactive compound, or a surface modifier, in accordance with the teachings herein.
[0060] The matrix phase of the first component (e.g., defined by a composition including liquid compounds and / or fillers) preferably includes a significant amount of a carbamate-containing compound. Preferably, the amount of the carbamate-containing compound in the first component is about 10 weight percent or more, more preferably about 15 weight percent or more, and most preferably about 18 weight percent or more, based on the total weight of the liquid compounds in the first component. The amount of the carbamate-containing compound in the first component may be about 90 weight percent or less, about 80 weight percent or less, about 70 weight percent or less, about 60 weight percent or less, or about 50 weight percent or less, based on the total weight of the liquid compounds in the first component.
[0061] The matrix phase of the second component (e.g., defined by a composition including liquid compounds and / or fillers) preferably includes a significant amount of a carbamate-reactive compound (e.g., a polyamine). Preferably, the amount of carbamate-reactive compound in the second component is about 10 weight percent or more, more preferably about 15 weight percent or more, even more preferably about 20 weight percent or more, and most preferably about 25 weight percent or more, based on the total weight of the liquid compounds in the second component. The amount of carbamate-reactive compound (e.g., a polyamine) in the second component may be about 90 weight percent or less, about 80 weight percent or less, about 70 weight percent or less, about 60 weight percent or less, or about 50 weight percent or less, based on the total weight of the liquid compounds in the second component.
[0062] The total amount of the carbamate-containing compound, one or more catalysts, the carbamate-reactive compound, the surface modifier, the one or more fillers, and the plasticizer is preferably about 95 weight percent or more, more preferably about 97 weight percent or more, even more preferably about 98 weight percent or more, even more preferably about 99 weight percent or more, and most preferably about 99.5 weight percent or more, based on the total weight of the composition. The total amount of the carbamate-containing compound, one or more catalysts, the polyamine compound, the alkoxysilane surface modifier, the ATH, the optional calcium carbonate and calcium oxide, and the plasticizer is preferably about 95 weight percent or more, more preferably about 97 weight percent or more, even more preferably about 98 weight percent or more, even more preferably about 99 weight percent or more, and most preferably about 99.5 weight percent or more, based on the total weight of the composition.
[0063] The molar ratio of carbamate groups in the first component to amine groups in the second component is preferably about 0.1 or more, about 0.2 or more, about 0.3 or more, about 0.4 or more, about 0.5 or more, or about 0.6 or more. The molar ratio of carbamate groups in the first component to amine groups in the second component is preferably about 10 or less, about 5.0 or less, about 3.5 or less, about 2.5 or less, about 2.0 or less, or about 1.7 or less.
[0064] Gap filling properties The two-component composition should be able to fill the gap between the components to provide a thermally conductive path between the two components. Typically, the two-component composition, after mixing (i.e., the thermal interface material), is placed on one of the components, followed by pressing the other component into the mixture. Each of the two components of the thermal interface material preferably has a low enough viscosity so that the material can be mixed with the other component and the component can be easily pressed into the mixture. The two-component composition should have a high enough viscosity after mixing so that the mixture does not flow out of the area where it is applied (e.g., before pressing the second component into the mixture). The viscosity of one of the components, or the mixture, can be characterized by the pressing force described herein. Preferably, the first component, the second component, the mixture, or any combination thereof, is characterized by a pressing force (initial, measured at 23° C.) of about 1000 N or less, about 900 N or less, about 800 N or less, about 700 N or less, about 600 N or less, about 500 N or less, or about 400 N or less. Preferably, the first component, the second component, the mixture, or any combination thereof, is characterized by an compression force (initial, measured at 23° C.) of about 5 N or more, about 10 N or more, about 30 N or more, about 60 N or more, about 80 N or more, about 90 N or more, or about 100 N or more.
[0065] Storage stability Materials according to the teachings herein may be required to be storage stable at room temperature and / or shipping temperature. The storage stability of a material may be characterized by accelerated testing in which the material is exposed to a temperature of about 55° C. for 3 days. Preferably, each component of the two-part composition maintains its good viscosity even after aging at a temperature of about 55° C. for about 3 days before mixing. Specifically, the first component, the second component, or both should be selected such that there is little or no increase in viscosity after aging at 55° C. for 3 days. Preferably, each component is characterized by a ratio of the compression force after aging (e.g., 3 days at 55° C.) to the initial compression force of about 4.0 or less, about 3.0 or less, about 2.0 or less, about 1.5 or less, or about 1.3 or less. Typically, the ratio of the compression force after aging to the initial compression force is about 0.5 or more, 0.75 or more, or about 1.0 or more, although values of 0.5 or less are also possible. After aging (e.g., 3 days at 55°C), the press-in force of the first component, the second component, or both, is preferably about 1000N or less, about 900N or less, about 800N or less, about 700N or less, about 600N or less, about 500N or less, or about 400N or less.
[0066] Purpose Thermal interface materials according to the teachings herein can be used in any device or system requiring a polymeric or oligomeric material with good thermal conductivity. FIG. 5 is a diagram illustrating features of a device 10 including a thermal interface material 12. The device may require a heat flow 20 from a first component 14 of the device to a second component 16 of the device 10. As shown in FIG. 5, the heat flow may pass through the thermal interface material 12. The second component 16 of the device may have a surface 20 (internal or external) that allows for the removal of heat from the second component.
[0067] The thermal interface material can be used as a gap filling material. The thermal interface material can be used as a sealing material. In some applications, it may be necessary to apply a thin layer of the thermal interface material (e.g., about 2 mm or less, about 1 mm or less, about 0.5 mm or less, or about 0.3 mm or less). Thus, the thermal interface material preferably has a low viscosity and / or good mixing behavior (e.g., has a smooth appearance that does not crumble after mixing) so that thin areas or layers can be prepared.
[0068] An article including one or more battery cells, a cooling unit, or a cell cover having a surface for contacting a circulating coolant preferably has a thermal interface material sandwiched between the battery cells and the cell cover. The thermal interface material provides a path for conducting thermal energy from the battery cells to the cell cover to manage the temperature of the battery cells. The battery cells may be provided as one or more modules. Without the thermal interface material, there may be gaps (at least in some areas) between the battery modules and a conductive plate (e.g., of the housing). FIG. 6 is a diagram illustrating features that may be used for thermal management of one or more battery modules. The battery / thermal management system 30 includes a thermal interface material 32 for filling gaps between one or more battery modules 34 and a metal surface 36. The thermal interface material may be applied by placing it on a surface of the battery module or by placing it on a metal surface. The metal surface may be a cooling plate or other component configured to evacuate heat from the system.
[0069] Test Method Particle size distribution. Unless otherwise specified, the particle size distribution of the fillers is measured by laser diffraction in acetone.
[0070] Thermal Conductivity Thermal conductivity is measured on a ZFW Stuttgart Thermal Interface Material Tester according to ASTM 5470-12. Tests are performed in Spaltplus mode with thicknesses of 1.8-1.2 mm. The described thermal interface material is considered to be Type I (viscous liquid) as described in ASTM 5470-12. The upper contact is heated to about 40°C and the lower contact is heated to about 10°C, resulting in a sample temperature of about 25°C. The A and B components are mixed in a static mixer as they are applied from a manual cartridge system. This is the method used in the examples of this application.
[0071] Press-in force The press-in force is measured with a tensometer (Zwick). The composition (e.g., gap filling material) is placed on the metal surface. An aluminum piston with a diameter of about 40 mm is placed on top and the material is compressed to an initial position of 5 mm. The material is then compressed from 5 mm to 0.3 mm at a speed of about 1 mm / s, and the force-deflection curve is recorded. The force (N) at a thickness of 0.5 mm is then recorded in a data table and considered as the press-in force. A material with low viscosity has a press-in force of 700 N or less. A material with high viscosity has a press-in force of more than 700 N or about 800 N or more. A material with low viscosity has a press-in force of preferably about 600 N or less, even more preferably about 500 N or less, and most preferably about 400 N or less.
[0072] mixing ability The ability to mix the compositions was judged by the ability to produce a single mass of material with a smooth surface. Such a material has a "good" mix. If the surface is rough and / or the material falls apart when removed from the mixer, the mix is poor.
[0073] material
[0074] [Table 1]
[0075] [Table 2]
[0076] [Table 3] EXAMPLES
[0077] Carbamate Prepolymer 1 Carbamate Prepolymer 1 is prepared with the composition shown in Table 2. Cardanol and Polyisocyanate Prepolymer 1 are added to a reactor and heated to about 60° C. with continuous mixing. Dibutyltin dilaurate catalyst is then added and the reaction is carried out for about 45 minutes under nitrogen at a temperature of about 80° C. After 45 minutes, vacuum is applied for 10 minutes and then the reactor is cooled to room temperature. The reaction product (Carbamate Prepolymer 1) has the following properties shown in Table 2. The molecular weight data of the polyurethane prepolymer was determined by gel permeation chromatography (GPC) using a Malvern Viscotek GPC max instrument. EMSURE-THF (ACS, Reag.Ph EUR, analytical grade) was used as the eluent, PL GEL MIXED D (Ailent, 300×7.5 mm, 5 μm) was used as the column and MALVERN Viscotek TDA was used as the detector.
[0078] [Table 4]
[0079] Examples A-1, A-2, A-3, and A-4 are Component A compositions containing an isocyanate prepolymer. These compositions are prepared by first mixing the liquid components and then adding the filler in the amounts shown in Table 3. A planetary mixer is used to mix all of the Component A composition and all of the Component B composition materials. As shown in Table 3, Examples A-1, A-2, A-3, and A-4 all had high initial compression forces and further solidified after 3 days at 55°C.
[0080] Thermal conductivity was measured on a ZFW Stuttgart Thermal Interface Material Tester according to ASTM 5470-12, the test was performed in Spaltplus mode with a thickness of 1.8-1.2 mm, the thermal interface material described is considered to be Type I (viscous liquid) as described in ASTM 5470-12, the top contact was heated to about 40°C and the bottom contact was heated to about 10°C, resulting in a sample temperature of about 25°C.
[0081] [Table 5]
[0082] In Examples A-4, A-5, A-6, A-7, and A-8, the addition of additional silane compound and / or more dimethyl malonate appears to reduce the initial press-in force, however, all of these materials have poor storage stability as indicated by the solidification of the compositions after 3 days at 55° C. as shown in Table 4, so the press-in force of the compositions cannot be tested further.
[0083] [Table 6]
[0084] Example B-1 is a Component B composition that includes a polyol component and has the composition shown in Table 5.
[0085] [Table 7]
[0086] Examples A-9, A-10, A-11, A-12, A-13, A-14, A-15, A-16, A-17, A-18, A-19, and A-20 are Component A compositions prepared using carbamate prepolymer 1, the compositions and properties of which are shown in Tables 7, 8, and 9. It can be seen herein that it is possible to prepare Component A compositions having low initial viscosity, good thermal stability, and high thermal conductivity.
[0087] [Table 8]
[0088] [Table 9]
[0089] Examples B-2, B-3, B-4, B-5, B-6, B-7, and B-8 are Component B compositions that include a carbamate-reactive compound (e.g., a polyamine) that can react with a Component A composition that includes a carbamate-containing compound.
[0090] [Table 10]
[0091] [Table 11]
[0092] Examples 1 and 2 are two-component compositions based on a first component containing an isocyanate and a second component containing a polyol capable of reacting with the isocyanate. These compositions are shown in Table 11.
[0093] [Table 12]
[0094] Examples 3-14 are thermal interface materials based on a carbamate-containing A component and a polyamine-containing B component. As shown in Tables 12 and 13, when the carbamate-containing A component and the polyamine-containing B component are mixed, the compositions generally have a low initial press-in force, which allows gap filling. This is possible even when the thermal conductivity is about 3 W / mK. For example, when the composition has an aluminum hydroxide concentration of more than 85 weight percent and / or a total filler concentration of 89 weight percent or more.
[0095] [Table 13]
[0096] [Table 14]
[0097] Table 14 shows the importance of having a catalyst in the A and / or B parts to affect the viscosity increase (characterized by the force of compression) at room temperature.
[0098] [Table 15] The invention as originally claimed in the present application is set forth below. [1] i) at least: a) a first component comprising a prepolymer containing two or more carbamate groups; ii) at least: b) a second component comprising one or more polyamine compounds capable of reacting with the prepolymer, The composition comprises: c) one or more catalysts for catalyzing the reaction between the prepolymer and the polyamine compound; d) 50 weight percent or more of one or more conductive fillers, based on the total weight of the two-part composition. [2] The two-component composition according to [1], wherein the prepolymer is formed by blocking one or more of the isocyanate groups of an aromatic polyisocyanate prepolymer (preferably substantially each, or completely each, of the isocyanate groups) with a phenol group of a blocking compound. [3] The two-component composition of [2], wherein the blocked compound comprises a terminal phenol group (preferably a single terminal phenol group) attached to a linear hydrocarbon chain (preferably the linear hydrocarbon chain contains 6 or more, 8 or more, 10 or more, or 12 or more carbon atoms) (preferably the linear hydrocarbon chain contains 60 or fewer, 30 or fewer, or 20 or fewer carbon atoms). [4] The two-component composition according to any one of [1] to [3], wherein the one or more polyamines, the prepolymer, or both have an average functionality of greater than 2. [5] The two-component composition according to any one of [1] to [4], wherein the one or more thermally conductive fillers include a filler selected from aluminum hydroxide, aluminum oxide, aluminum powder, zinc oxide, boron nitride, and / or a mixture of any of these. [6] The two-component composition according to any one of [1] to [4], wherein the one or more thermally conductive fillers include a filler selected from aluminum hydroxide, aluminum oxide, and / or a mixture of any of these. [7] The two-component composition according to any one of [1] to [4], wherein the one or more thermally conductive fillers are aluminum hydroxide. [8] The two-component composition according to any one of [1] to [7], wherein the one or more conductive fillers comprise aluminum hydroxide. [9] The two-component composition according to any one of [1] to [8], wherein the first component contains 75 weight percent or more of aluminum hydroxide, and the second component contains 75 weight percent or more of aluminum hydroxide.
[10] The two-component composition according to any one of [1] to [9], wherein the surface of the aluminum hydroxide is partially or completely coated with a surface modifier to reduce the hydrophilicity of the surface.
[11] The composition has a D of about 3 or more. 90 / D 50 The aluminum hydroxide has a wide particle size distribution including a ratio of 2.24×10 to 100% of tetrasodium pyrophosphate decahydrate as a dispersion medium. -3 M solution (1 g Na in 1000 ml deionized water) 4 P 2 O 7 ×10H2 The two-component composition according to any one of [1] to
[10] , wherein the two-component composition is measured according to ISO 13320 using 0).
[12] The two-component composition according to any one of [1] to
[11] , wherein the composition contains one or more plasticizers.
[13] The two-component composition according to any one of [1] to
[12] , wherein the composition contains a fatty acid or an ester of a fatty acid.
[14] The two-component composition according to any one of [1] to
[13] , wherein the composition comprises an epoxy resin in the first component, and preferably, the weight ratio of the prepolymer to the epoxy resin is about 0.5 or more, more preferably about 0.8 or more, and even more preferably about 1.0 or more (preferably, the weight ratio of the prepolymer to the epoxy resin is about 10 or less, about 5 or less, or about 4 or less).
[15] The two-component composition according to any one of [1] to
[14] , wherein the composition is substantially free of an isocyanate-containing compound (e.g., the amount of NCO in the first component is preferably about 0.10 weight percent or less, about 0.05 weight percent or less, or about 0.01 weight percent or less, based on the total weight of the first component).
[16] The two-component composition according to any one of [1] to
[15] , wherein the molar ratio of the carbamate groups in the first component to the amine groups in the second component is about 0.1 or more, about 0.2 or more, about 0.3 or more, about 0.4 or more, about 0.5 or more, or about 0.6 or more, and / or about 10 or less, about 5.0 or less, about 3.5 or less, about 2.5 or less, about 2.0 or less, or about 1.7 or less.
[17] The two-component composition according to any one of [1] to
[16] , wherein the first component contains calcium carbonate (preferably in an amount of about 0.1 weight percent or more, more preferably about 0.5 weight percent or more, and most preferably about 1.0 weight percent or more, based on the total weight of the first component).
[18] The two-component composition according to any one of [1] to
[17] , wherein the catalyst is a Lewis acid or a Lewis base.
[19] The two-component composition according to any one of [1] to
[18] , wherein the catalyst is a tin catalyst.
[20] The two-component composition according to any one of [1] to
[18] , wherein the catalyst is an amine catalyst.
[21] The two-component composition according to any one of [1] to
[20] , wherein the catalyst is DABCO (1,4-diazabicyclo[2.2.2]octane).
[22] The two-component composition according to any one of [1] to
[21] , wherein the first component contains a part or all of the catalyst.
[23] The two-component composition of any of [1] to
[22] , wherein the composition is characterized by a thermal conductivity of about 2.0 W / mK or more (preferably about 2.5 or more, more preferably about 2.8 or more, even more preferably about 2.9 or more, and most preferably about 3.0 or more) as measured on a ZFW Stuttgart thermal interface material tester in accordance with ASTM 5470-12, the test being performed in Spaltplus mode with a thickness of 1.8 to 1.2 mm, the described thermal interface material being considered to be Type I (viscous liquid) as described in ASTM 5470-12, and the upper contact is heated to about 40° C. and the lower contact is heated to about 10° C., resulting in a sample temperature of about 25° C.
[24] The two-component composition according to any one of [1] to
[23] , wherein the two-component composition cures at room temperature (preferably as characterized by an increase in compression force of about 100% or more after aging for 24 hours after mixing).
[25] The two-component composition according to any of [1] to
[24] , wherein the first component is storage stable (e.g., as characterized by a compression force of the first component of less than 700 N after aging for 3 days at 55° C.).
[26] An article comprising a first component for generating heat, a second component for removing heat, and a layer of a thermal interface material sandwiched between the first component and the second component, the thermal interface material providing a path for transferring heat from the first component to the second component, and formed from the two-component composition described in any of [1] to
[25] .
[27] A method comprising the steps of disposing a layer of a thermal interface material between a first component and a second component, and applying pressure such that the thermal interface material contacts both the first component and the second component and fills a gap between the two components, wherein the thermal interface material is formed from a two-component composition described in any of [1] to
[25] .
Claims
1. i) at least a) a first component comprising a prepolymer containing two or more carbamate groups; ii) at least b) a second component comprising one or more polyamine compounds capable of reacting with the prepolymer, The composition comprises: c) one or more catalysts for catalyzing the reaction between the prepolymer and the polyamine compound; d) at least 50 weight percent of one or more thermally conductive fillers, based on the total weight of the two-part composition; The prepolymer comprises an aromatic polyisocyanate prepolymer in which one or more of the isocyanate groups are blocked with a phenol group of a blocking compound. Two-part composition.
2. The two-component composition described in claim 1, wherein each of the isocyanate groups of the aromatic polyisocyanate prepolymer is blocked with a phenol group of a blocking compound.
3. 3. The two-part composition of claim 1, wherein the blocked compound comprises a terminal phenol group attached to a linear hydrocarbon chain.
4. The two-part composition of any one of claims 1 to 3, wherein the one or more polyamines, the prepolymer, or both, have an average functionality greater than two.
5. 5. The two-part composition of claim 1, wherein the one or more thermally conductive fillers comprise a filler selected from aluminum hydroxide, aluminum oxide, aluminum powder, zinc oxide, boron nitride, and / or mixtures of any thereof.
6. 5. The two-part composition of claim 1, wherein the one or more thermally conductive fillers comprise a filler selected from aluminum hydroxide, aluminum oxide, and / or any mixture thereof.
7. The two-part composition of any one of claims 1 to 4, wherein the one or more thermally conductive fillers is aluminum hydroxide.
8. The two-part composition of any one of claims 1 to 7, wherein the one or more thermally conductive fillers comprise aluminum hydroxide.
9. The two-part composition of any one of claims 1 to 8, wherein the first component comprises at least 75 weight percent aluminum hydroxide and the second component comprises at least 75 weight percent aluminum hydroxide.
10. 10. The two-part composition according to any one of claims 1 to 9, wherein the surface of the aluminium hydroxide is partially or completely coated with a surface modifier to reduce the hydrophilicity of the surface.
11. The composition has a D 90 / D 50 The aluminum hydroxide has a wide particle size distribution including a ratio of 2.24×10 to 1.001 of tetrasodium pyrophosphate decahydrate as a dispersion medium. -3 M solution (1 g Na in 1000 ml deionized water) 4 P 2 O 7 x10H 2 The two-part composition according to any one of claims 1 to 10, wherein the viscosity is measured according to ISO 13320 using 0).
12. The two-part composition of any one of claims 1 to 11, wherein the composition comprises one or more plasticizers.
13. The two-part composition of any one of claims 1 to 12, wherein the composition comprises a fatty acid or an ester of a fatty acid.
14. The two-part composition according to any one of claims 1 to 13, wherein the composition comprises an epoxy resin in the first component.
15. The two-part composition of claim 1, wherein the NCO amount of the first component is 0.10 weight percent or less, based on the total weight of the first component.
16. 16. The two-part composition according to claim 1, wherein a molar ratio of the carbamate groups in the first component to the amine groups in the second component is 0.1 or more, 0.2 or more, 0.3 or more, 0.4 or more, 0.5 or more, or 0.6 or more, and / or 10 or less, 5.0 or less, 3.5 or less, 2.5 or less, 2.0 or less, or 1.7 or less.
17. The two-part composition of any one of claims 1 to 16, wherein the first component comprises calcium carbonate.
18. The two-part composition according to any one of claims 1 to 17, wherein the catalyst is a Lewis acid or a Lewis base.
19. The two-part composition of any one of claims 1 to 18, wherein the catalyst is a tin catalyst.
20. The two-part composition of any one of claims 1 to 18, wherein the catalyst is an amine catalyst.
21. The two-part composition of any one of claims 1 to 20, wherein the catalyst is DABCO (1,4-diazabicyclo[2.2.2]octane).
22. The two-part composition of any one of claims 1 to 21, wherein the first component comprises some or all of the catalyst.
23. 23. The two-part composition of any one of claims 1 to 22, wherein the composition is characterized by a thermal conductivity of 2.0 W / mK or greater as measured on a ZFW Stuttgart thermal interface material tester according to ASTM 5470-12, the test being performed in Spaltplus mode with a thickness of 1.8-1.2 mm, and the described thermal interface material is considered to be Type I (viscous liquid) as described in ASTM 5470-12, with the top contact heated to 40°C and the bottom contact heated to 10°C, resulting in a sample temperature of 25°C.
24. The two-part composition of any one of claims 1 to 23, wherein the two-part composition cures at room temperature.
25. The two-part composition of any one of claims 1 to 24, wherein the first component is storage stable.
26. 26. An article comprising a first component for generating heat, a second component for removing heat, and a layer of thermal interface material sandwiched between the first and second components, the thermal interface material providing a path for transferring heat from the first component to the second component, and formed from the two-part composition of any one of claims 1 to 25.
27. 26. A method comprising the steps of disposing a layer of thermal interface material between a first component and a second component and applying pressure such that the thermal interface material contacts both the first component and the second component to fill a gap between the two components, wherein the thermal interface material is formed from the two-part composition of any one of claims 1 to 25.
Citation Information
Patent Citations
battery coating
JP2017505507A
Polymer compound for film and self-healable heat-dissipation film using the same
KR101830523B1