Process cartridge and electrophotographic apparatus
The process cartridge with a conductive particle-enhanced surface protective layer and organosilicon polymer toner addresses toner scattering issues, ensuring stable image quality and transferability in electrophotographic devices at increased speeds.
Patent Information
- Application Number
- JP2022147173
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-08-16
- Filing Date
- 2022-09-15
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2042-09-15
AI Technical Summary
Existing electrophotographic devices face challenges in maintaining image quality and durability due to issues with toner chargeability, fluidity, and scattering, particularly at increased process speeds, leading to roughness in halftone images.
A process cartridge with an electrophotographic photoreceptor containing a surface protective layer with a specific volume content and resistivity of conductive particles, combined with toner particles having organosilicon polymer structures, enhances charge injection and distribution, reducing toner scattering and improving transferability.
The solution effectively suppresses image defects such as roughness in halftone images by ensuring proper charge injection and distribution, maintaining transferability and image quality even at higher process speeds.
Smart Images

Figure 0007566833000021 
Figure 0007566833000022 
Figure 0007566833000023
Abstract
Description
[Technical field]
[0001] The present invention relates to a process cartridge and an electrophotographic apparatus having an electrophotographic photosensitive member. [Background technology]
[0002] Electrophotographic devices (hereinafter also referred to as "image forming devices") are required to be faster, more compact, and have a longer life. To meet these demands, toner is increasingly required to have high durability that can withstand higher speeds, a long life, and the ability to stabilize image quality.
[0003] From the viewpoint of miniaturization, various attempts have been made to reduce the space required for the units. In particular, since improving the transferability of toner allows the size of a waste toner container for collecting the residual toner on the photosensitive drum to be reduced, various attempts have been made to improve the transferability.
[0004] In the transfer process, the toner on the photoconductor drum is transferred to a medium such as paper. In order to improve transferability, it is important to reduce the adhesive force between the photoconductor drum and the toner so that the toner can be easily separated from the photoconductor drum. One known technique for achieving this is to externally add large silica particles with a particle size of about 100 nm to 300 nm.
[0005] On the other hand, the external addition of large silica particles reduces the fluidity of the toner, which results in problems with chargeability, particularly in terms of charge start-up and chargeability under high temperature and high humidity conditions.
[0006] To address this issue, Patent Document 1 discloses a toner that aims to achieve both the effect of improving high chargeability and fluidity by using small silica particles and the effect of suppressing embedding of silica particles by using large silica particles. Patent Document 2 discloses a toner which combines large silica particles with organosilicon polymer microparticles of a specific particle size, and further controls the adhesion rate of the large silica particles and the organosilicon polymer microparticles to the toner particles to achieve a specific level, thereby achieving improved transferability, excellent fluidity, and reduced component contamination. Patent Document 3 discloses an electrophotographic photoreceptor in which a protective layer of the electrophotographic photoreceptor contains anatase-type titanium oxide containing niobium atoms, thereby improving the mechanical strength of the protective layer on the photoreceptor surface and maintaining stable electrical characteristics even under high-temperature and high-humidity environments. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2010-249995 A [Patent Document 2] JP 2020-106723 A [Patent Document 3] JP 2009-229495 A Summary of the Invention [Problem to be solved by the invention]
[0008] In the configuration described in Patent Document 1, although the durability performance is improved by using large-diameter silica particles, there are problems with the chargeability of the toner and the durability in the latter half of the running test.
[0009] The configuration described in Patent Document 2 certainly improves durability in the latter half of the durability test. However, the inventors of the present invention have further studied and confirmed that when the process speed of the image forming apparatus is increased, some of the toner developed on the electrophotographic photoreceptor has a low charge amount and scatters. As a result, it was found that when a halftone image is formed in particular, the poorly charged toner scatters, causing the halftone image to appear rough.
[0010] The configuration described in Patent Document 3 certainly improves the mechanical strength of the surface protection layer. However, after further intensive research, the present inventors have confirmed that there is room for improvement in the roughness of halftone images when the process of the image forming apparatus is accelerated. This is believed to be due to the lack of a mechanism for increasing the charge amount of the toner and sharpening the charge amount distribution of the toner by injecting charge from the electrophotographic photoreceptor into the toner. [Means for solving the problem]
[0011] The above object can be achieved by the present invention described below. The process cartridge of the present invention comprises: A process cartridge that is detachably mountable to a main body of an electrophotographic apparatus, The process cartridge comprises: An electrophotographic photoreceptor; a developing means having a toner storage section for storing toner and supplying the toner to the surface of the electrophotographic photoreceptor; having The electrophotographic photoreceptor has a conductive support, and a photosensitive layer and a surface protective layer formed on the conductive support in this order; The surface protective layer contains conductive particles, the content of the conductive particles is 5.0 vol% or more and 70.0 vol% or less with respect to the total volume of the surface protective layer, The volume resistivity of the surface protective layer is 1.0×10 9 Ω cm or more 1.0×10 14 Ω cm or less, The toner contained in the toner container is selected from the following (i) or (ii): (i) A toner having toner particles containing a binder resin and organosilicon polymer particles, (ii) A toner having toner particles containing a binder resin and having an organosilicon polymer on the surface thereof. It satisfies the provisions of The organosilicon polymer particles when the requirement (i) is satisfied, or the organosilicon polymer when the requirement (ii) is satisfied, A silicon atom having a T3 unit structure; At least one unit structure selected from the group consisting of a silicon atom having a T2 unit structure and a silicon atom having a T1 unit structure; It has The organosilicon polymer particles when the requirement (i) is satisfied, or the organosilicon polymer when the requirement (ii) is satisfied, are 29 In the measurement of Si-NMR, the ratio of the total area of the peaks derived from silicon atoms having a T2 unit structure and the peak area derived from silicon atoms having a T1 unit structure to the total area of the peaks derived from all silicon atoms is 0.10 or more and 0.40 or less. It is characterized by: Effect of the Invention
[0012] As described above, according to the present invention, it is possible to provide a process cartridge and an electrophotographic device which can improve transferability and suppress image defects (roughness in half-tone images) caused by toner scattering due to poor charging, which occurs when the process speed of an electrophotographic device is further increased. [Brief description of the drawings]
[0013] [Figure 1] 1 is a schematic diagram illustrating an example of a configuration of an electrophotographic photoreceptor according to the present invention. [Diagram 2] 1 is a diagram showing an example of a schematic configuration of a process cartridge in which an electrophotographic photosensitive member according to the present invention is mounted, and an electrophotographic apparatus including the process cartridge. [Diagram 3] FIG. 2 is a diagram showing an example of a comb-shaped electrode for measuring the volume resistivity of an electrophotographic photosensitive member. [Figure 4] FIG. 2 is a TEM image of an example of niobium-containing titanium oxide used in the present examples. [Diagram 5] FIG. 2 is a schematic diagram of an example of niobium-containing titanium oxide used in the present examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] The process cartridge of the present invention is a process cartridge that is detachably mountable to a main body of an electrophotographic apparatus, The process cartridge comprises: An electrophotographic photoreceptor; a developing means having a toner storage section for storing toner and supplying the toner to the surface of the electrophotographic photoreceptor; having The electrophotographic photoreceptor has a conductive support, and a photosensitive layer and a surface protective layer formed on the conductive support in this order; The surface protective layer contains conductive particles, the content of the conductive particles is 5.0 vol% or more and 70.0 vol% or less with respect to the total volume of the surface protective layer, The volume resistivity of the surface protective layer is 1.0×10 9 Ω cm or more 1.0×10 14 Ω cm or less, The toner contained in the toner container is selected from the following (i) or (ii): (i) A toner having toner particles containing a binder resin and organosilicon polymer particles, (ii) A toner having toner particles containing a binder resin and having an organosilicon polymer on the surface thereof. It satisfies the provisions of The organosilicon polymer particles when the requirement (i) is satisfied, or the organosilicon polymer when the requirement (ii) is satisfied, A silicon atom having a T3 unit structure; At least one unit structure selected from the group consisting of a silicon atom having a T2 unit structure and a silicon atom having a T1 unit structure; It has The organosilicon polymer particles when the requirement (i) is satisfied, or the organosilicon polymer when the requirement (ii) is satisfied, are 29In the measurement of Si-NMR, the ratio of the total area of the peaks derived from silicon atoms having a T2 unit structure and the peak area derived from silicon atoms having a T1 unit structure to the total area of the peaks derived from all silicon atoms is 0.10 or more and 0.40 or less. It is characterized by:
[0015] The inventors have investigated methods for improving transferability using the above-mentioned process cartridge, as well as suppressing image problems (roughness in half-tone images) caused by toner scattering due to poor charging that occurs when the process speed of an image forming device is further increased.
[0016] The inventors have confirmed that this phenomenon occurs when the process speed of an image forming apparatus is increased, and a portion of the toner developed on an electrophotographic photoreceptor has a low charge amount and scatters. As a result, it was found that when a halftone image is formed in particular, the poorly charged toner scatters, causing the halftone image to appear rough.
[0017] Therefore, the inventors have conducted extensive research into a process cartridge that can suppress image defects (roughness in half-tone images) caused by toner scattering due to poor charging that occurs when the process speed of an image forming apparatus is further increased, from the perspective of injecting a very small portion of the charge on the surface of an electrophotographic photosensitive member into the toner just before the toner is developed from the developer carrier onto the electrophotographic photosensitive member, thereby increasing the charge amount of the toner and sharpening its charge amount distribution.
[0018] The present inventors have made it possible for a small portion of the charge on the surface of the photoreceptor to be injected into the toner during development by incorporating an appropriate amount of conductive particles into the surface protective layer of the photoreceptor and controlling the volume resistivity of the surface protective layer of the photoreceptor.Furthermore, by making an organosilicon polymer present on the surface of the toner particles and making silanol groups present in part of the organosilicon polymer and controlling the amount of silanol groups, it has become possible for the charge on the surface of the electrophotographic photoreceptor to be rapidly injected into the toner via the organosilicon polymer, thereby making it possible to sharpen the charge amount and charge amount distribution of the toner. It was found that by using the above process cartridge, it is possible to maintain transferability while suppressing poor charging that occurs when the process speed of the image forming device is further increased, and to suppress image defects caused by toner scattering (roughness in half-tone images).
[0019] <Photoreceptor according to the present invention> The photoreceptor according to the present invention has a conductive support, a photosensitive layer, and a surface protective layer. The surface protective layer contains conductive particles, and the content of the conductive particles is 5.0 volume % or more and 70.0 volume % or less with respect to the total volume of the surface protective layer. Furthermore, the volume resistivity of the surface protective layer is 1.0×10 9 Ω cm or more 1.0×10 14 It is characterized by a resistivity of Ω·cm or less. Although the surface protective layer contains a large amount of conductive particles, the volume resistivity is kept relatively high, so that the charge retention is ensured and it is possible to inject electric charge into the toner according to the present invention through the conductive particles.
[0020] If the content of the conductive particles is less than 5.0% by volume, the charge injection property of the toner according to the present invention is reduced, and therefore poor charging during development at high speeds is likely to cause image problems due to toner scattering (roughness in halftone images). On the other hand, if the content exceeds 70.0% by volume, the surface protection layer itself becomes brittle, and the surface of the photoconductor is easily scraped off over long-term use. This reduces the charging uniformity of the photoconductor, and poor charging during development at high speeds is likely to cause image problems due to toner scattering. A more preferred content of the conductive particles is 5.0% by volume or more and 40.0% by volume or less. By setting the content in this preferred range, fogging in a high-temperature and high-humidity environment is also improved.
[0021] In addition, the volume resistivity of the surface protection layer is 1.0×10 9 Ω cm or more 1.0×10 14 It is characterized by a resistance of less than 1.0×10 9 If the resistivity is less than Ω·cm, the resistance of the surface protective layer is too low, making it difficult to maintain the potential, and the amount of charge of the toner decreases. As a result, the effect of the present invention cannot be obtained, and fogging in a high-temperature and high-humidity environment worsens. 14 If the resistance exceeds Ω·cm, the resistance of the surface protective layer becomes too high, and the charging ability of the toner is significantly deteriorated. As a result, the effect of the present invention cannot be obtained, and the fogging worsens due to poor charging caused by electrostatic cohesion between toner particles in a low temperature and low humidity environment.
[0022] The preferred volume resistivity of the surface protective layer is 1.0×10 11 Ω cm or more 1.0×10 14The volume resistivity of the surface protective layer is, for example, controlled by the particle diameter of the conductive particles. The particle diameter of the conductive particles is preferably 5 nm or more and 300 nm or less, more preferably 40 nm or more and 250 nm or less, in terms of number average particle diameter. If the number average particle diameter of the conductive particles is less than 5 nm, the specific surface area of the conductive particles increases, and moisture adsorption increases in the vicinity of the conductive particles on the surface of the surface protective layer, which tends to reduce the volume resistivity of the surface protective layer. If the number average particle diameter of the conductive particles exceeds 300 nm, the dispersion of the particles in the surface protective layer deteriorates and the area of the interface with the binder resin decreases, which increases the resistance at the interface and tends to deteriorate the charge injection property.
[0023] The conductive particles contained in the surface protective layer include particles of metal oxides such as titanium oxide, zinc oxide, tin oxide, and indium oxide. When metal oxides are used as the conductive particles, the metal oxides may be doped with elements such as niobium, phosphorus, and aluminum, or oxides thereof. In the present invention, titanium oxide is preferred from the viewpoint of charge injection from the charging member.
[0024] Furthermore, when titanium oxide contains niobium atoms, the injection property is improved, and the charge injection property can be improved with a small amount. The preferred niobium atom content is 0.5% by mass or more and 15.0% by mass or less, more preferably 2.6% by mass or more and 10.0% by mass or less, based on the total mass of the niobium atom-containing titanium oxide particles.
[0025] Particularly preferred conductive particles are titanium oxide particles containing niobium and having a configuration in which niobium is unevenly distributed near the particle surface. This is because the uneven distribution of niobium near the surface allows efficient transfer of electric charges. More specifically, titanium oxide particles are particles in which the concentration ratio calculated as "niobium atomic concentration / titanium atomic concentration" at 5% inside the maximum diameter of the particle from the surface of the particle is 2.0 times or more compared to the concentration ratio calculated as "niobium atomic concentration / titanium atomic concentration" at the center of the particle. By achieving such a state, electric charges can be efficiently transferred as described above. As a result, the charge injection property into the toner can be improved. Also, the decrease in the volume resistivity of the surface protective layer can be suppressed. This improves fogging in a high-temperature and high-humidity environment from the beginning to the end of durability in addition to the effects of the present invention. The niobium atomic concentration and titanium atomic concentration are obtained by a scanning transmission electron microscope (STEM) connected to an EDS analyzer (energy dispersive X-ray analyzer).
[0026] FIG. 4 shows a STEM image of an example of titanium oxide particles (X1) used in the examples of the present invention. The STEM image of FIG. 4 is shown diagrammatically in FIG. The niobium-containing titanium oxide particles used in the present invention can be prepared by coating titanium oxide particles as a core material with niobium-containing titanium oxide and then firing the coated titanium oxide. It is considered that the coated niobium-containing titanium oxide grows as niobium-doped titanium oxide along the crystals of the titanium oxide core material by so-called epitaxial growth. The niobium-containing titanium oxide prepared in this manner has a lower density near the surface compared to the density at the center of the particle, as shown in FIG. 4, and is in a core-shell form. In addition, in EDS analysis by STEM, since X-rays penetrate the entire particle, as shown in FIG. 5, the influence of the surface vicinity 32 is greater in EDS analysis at 5% of the primary particle diameter from the particle surface than in EDS analysis at the particle center 31. In addition, FIG. 5 is a schematic diagram showing an irradiation image of X-rays 33 for analyzing the center of a conductive particle and X-rays 34 for analyzing 5% of the maximum diameter of the measured particle from the particle surface.
[0027] The niobium atom-containing titanium oxide particles are preferably anatase or rutile titanium oxide particles, more preferably anatase titanium oxide particles. By using anatase titanium oxide, charge transfer within the surface protective layer becomes smooth, resulting in good charge injection. Anatase titanium oxide particles can be produced by the known sulfuric acid method, in which a solution containing titanium sulfate and titanyl sulfate is heated for hydrolysis to produce a hydrous titanium dioxide slurry, which is then dehydrated and fired. The degree of anatase conversion of anatase type titanium oxide is preferably 90 to 100%. A surface protective layer containing anatase type titanium oxide containing niobium atoms in the range specified in the present invention achieves good and stable rectification, and the above-mentioned effects of the present invention are well achieved. Here, the degree of anatase conversion is a value calculated by the following formula, measuring the intensity IA of the strongest interference line (plane index 101) of anatase and the intensity IR of the strongest interference line (plane index 110) of rutile in powder X-ray diffraction of titanium oxide. Anatase degree (%) = 100 / (1 + 1.265 × IR / IA) To produce titanium oxide with an anatase degree in the range of 90-100%, a solution containing titanium sulfate and titanyl sulfate as titanium compounds is heated and hydrolyzed to produce a hydrous titanium dioxide slurry, which is then dehydrated and fired. This method produces an anatase type titanium dioxide with an anatase degree of nearly 100%. Alternatively, an anatase type titanium dioxide with a high anatase degree can be obtained by neutralizing an aqueous titanium tetrachloride solution with an alkali.
[0028] <Toner according to the present invention> The toner according to the present invention has the following (i) or (ii): (i) A toner having toner particles containing a binder resin and organosilicon polymer particles, (ii) A toner having toner particles containing a binder resin and having an organosilicon polymer on the surface thereof. It satisfies the provisions of the above. The organosilicon polymer particles satisfying the requirement (i), or the organosilicon polymer satisfying the requirement (ii), are A silicon atom having a T3 unit structure; At least one unit structure selected from the group consisting of a silicon atom having a T2 unit structure and a silicon atom having a T1 unit structure; It has. Furthermore, the organosilicon polymer particles when the requirement (i) is satisfied, or the organosilicon polymer when the requirement (ii) is satisfied, 29 In a Si-NMR measurement, the ratio of the total area of the peaks originating from silicon atoms having a T2 unit structure and the peak area originating from silicon atoms having a T1 unit structure to the total area of the peaks originating from all silicon atoms is 0.10 or more and 0.40 or less. A silicon atom having a T1 unit structure is a silicon atom that is bonded to one atom other than oxygen, three oxygen atoms, and only one of the three oxygen atoms is further bonded to another silicon atom. Generally, RaSi(O 1 / 2 )(OR)2 is a silicon atom. A silicon atom having a T2 unit structure is a silicon atom that is bonded to one atom other than oxygen, three oxygen atoms, and only two of the three oxygen atoms are further bonded to other silicon atoms. Generally, RaSi(O 1 / 2 )2(OR) is a silicon atom with a structure represented by the formula: A silicon atom having a T3 unit structure is a silicon atom that is bonded to one non-oxygen atom, three oxygen atoms, and all three oxygen atoms are further bonded to other silicon atoms. Generally, RaSi(O 1 / 2 )3 is a silicon atom having the structure represented by the formula: For example, Ra is an alkyl group having 1 to 6 carbon atoms or a phenyl group, and R is a hydrogen atom or an alkyl group having 1 to 6 carbon atoms.
[0029] (i) The case of a toner having toner particles containing a binder resin and organosilicon polymer particles will be described.
[0030] <Organosilicon Polymer Particles> In the above-mentioned configuration, when a toner having organosilicon polymer particles on the surface is used, there is no particular restriction on the method for forming the organosilicon polymer particles, and any conventionally known method can be used. The above-mentioned method is described below.
[0031] The organosilicon polymer particles have a structure in which silicon atoms and oxygen atoms are bonded alternately, and it is essential that the organosilicon polymer has at least one unit structure selected from the group consisting of silicon atoms having a T3 unit structure, silicon atoms having a T2 unit structure, and silicon atoms having a T1 unit structure.
[0032] In the above configuration, the method for producing the organosilicon polymer particles is not particularly limited, and can be obtained, for example, by dropping a silane compound represented by the following formula (Z) into water, carrying out hydrolysis and condensation reaction with a catalyst, and then filtering and drying the resulting suspension. Examples of the catalyst include acidic catalysts such as hydrochloric acid, hydrofluoric acid, sulfuric acid, and nitric acid, and basic catalysts such as ammonia water, sodium hydroxide, and potassium hydroxide, but are not limited to these. The following formula (Z) [ka] (In formula (Z), R a represents an organic functional group. 1 , R 2 and R 3 each independently represents a halogen atom, a hydroxy group, an acetoxy group, or an alkoxy group (preferably having 1 to 3 carbon atoms).
[0033] R a Examples of the carbon atom include a hydrocarbon group having 1 or more and 6 or less (preferably 1 to 3, more preferably 1 or 2) carbon atoms (preferably an alkyl group) and an aryl group (preferably a phenyl group). R 1 , R 2 and R 3are each independently a halogen atom, a hydroxyl group, an acetoxy group, or an alkoxy group. These are reactive groups that undergo hydrolysis, addition polymerization, and condensation to form a crosslinked structure. 1 , R 2 and R 3 The hydrolysis, addition polymerization and condensation of the above can be controlled by the reaction temperature, reaction time, reaction solvent and pH. a There are three reactive groups (R 1 , R 2 and R 3 ) are also called trifunctional silanes.
[0034] Examples of formula (Z) include the following: p-Styryltrimethoxysilane, methyltrimethoxysilane, methyltriethoxysilane, methyldiethoxymethoxysilane, methylethoxydimethoxysilane, methyltrichlorosilane, methylmethoxydichlorosilane, methylethoxydichlorosilane, methyldimethoxychlorosilane, methylmethoxyethoxychlorosilane, methyldiethoxychlorosilane, methyltriacetoxysilane, methyldiacetoxymethoxysilane, methyldiacetoxyethoxysilane, methylacetoxydimethoxysilane, methylacetoxymethoxyethoxysilane, methylacetoxydiethoxysilane, methyltrihydroxysilane, methylmethoxydihydroxysilane, methylethoxydihydroxysilane, methyldimethoxyhydroxysilane, methylethoxymethoxyhydroxysilane, methyldiethoxyhydroxysilane, trifunctional methylsilanes such as; ethyltrimethoxysilane, ethyltriethoxy Sisilane, trifunctional ethylsilane such as ethyltrichlorosilane, ethyltriacetoxysilane, ethyltrihydroxysilane; trifunctional propylsilane such as propyltrimethoxysilane, propyltriethoxysilane, propyltrichlorosilane, propyltriacetoxysilane, propyltrihydroxysilane; trifunctional butylsilane such as butyltrimethoxysilane, butyltriethoxysilane, butyltrichlorosilane, butyltriacetoxysilane, butyltrihydroxysilane; trifunctional hexylsilane such as hexyltrimethoxysilane, hexyltriethoxysilane, hexyltrichlorosilane, hexyltriacetoxysilane, hexyltrihydroxysilane; trifunctional phenylsilane such as phenyltrimethoxysilane, phenyltriethoxysilane, phenyltrichlorosilane, phenyltriacetoxysilane, phenyltrihydroxysilane. The organosilicon compound may be used alone or in combination of two or more.
[0035] In addition, the following may be used in combination with the organosilicon compound having the structure represented by formula (Z): an organosilicon compound having four reactive groups in one molecule (tetrafunctional silane), an organosilicon compound having two reactive groups in one molecule (bifunctional silane), or an organosilicon compound having one reactive group (monofunctional silane). The content of the structure represented by formula (Z) in the monomer forming the organosilicon polymer is preferably 50 mol% or more, more preferably 60 mol% or more.
[0036] The type of catalyst, the compounding ratio, the reaction initiation temperature, the drop time, etc. determine the degree of polymerization of the organosilicon polymer particles. 29 In the Si-NMR measurement, the ratio of the total area of the peaks derived from silicon having a T2 unit structure and the peak area derived from silicon having a T1 unit structure to the total area of the peaks derived from all silicon atoms can be controlled to be 0.10 or more and 0.40 or less.
[0037] By adjusting the pH, reaction temperature, and reaction time, 29 In the Si-NMR measurement, the ratio of the total area of the peaks originating from silicon atoms having T2 unit structure and the total area of the peaks originating from silicon atoms having T1 unit structure to the total area of the peaks originating from all silicon atoms can be controlled to 0.10 or more and 0.40 or less. If the ratio of the total area of the peaks originating from silicon having T2 unit structure and the total area of the peaks originating from silicon having T1 unit structure to the total area of the peaks originating from all silicon atoms is less than 0.10, the amount of silanol groups (and some alkoxysilane groups thereof) of the organosilicon polymer particles is small when the charge is injected from the photoreceptor according to the present invention to the toner, and the charge injection property is reduced. As a result, due to poor charging during development caused by high speed development, image problems due to toner scattering (roughness in halftone images) are likely to occur. Fog due to electrostatic aggregation in a low temperature and low humidity environment is aggravated.
[0038] On the other hand, if it exceeds 0.40, when charge is injected from the photoreceptor of the present invention into the toner, the amount of silanol groups (and some of the alkoxysilane groups) in the organosilicon polymer particles is large, and charge leakage is likely to occur due to the organosilicon polymer particles. As a result, the charge injection from the photoreceptor to the toner is reduced. As a result, poor charging during development caused by high speed development is likely to cause image problems (roughness in halftone images) due to toner scattering. Also, fogging in high temperature and high humidity environments is aggravated.
[0039] The organosilicon polymer particles 29 In the Si-NMR measurement, the ratio of the area of the peak originating from silicon atoms having T3 unit structure to the total area of the peak originating from all silicon atoms contained in the organosilicon polymer particles is preferably 0.50 or more and 0.90 or less.By being in the above range, the deterioration of the organosilicon polymer particles themselves is suppressed.As a result, when the speed is increased, the toner particles are less likely to be buried even during durable image output.Therefore, the charge injection from the photoconductor to the toner is good from the beginning to the long term.
[0040] It is preferable that the toner is a toner having toner particles containing a binder resin and organosilicon polymer particles, and the major axis of the organosilicon polymer particles is 30 nm or more and 300 nm or less. The toner has organosilicon polymer particles, so that the organosilicon polymer particles are present on the surface of the toner particles in a state in which they can roll.
[0041] As a result, when charge is injected from the photoreceptor into the toner particles via the organosilicon polymer particles, the organosilicon polymer particles roll on the surface of the toner particles, increasing the contact area between the toner particles and the organosilicon polymer particles per unit time, allowing charge to be injected efficiently from the photoreceptor to the toner.
[0042] Furthermore, when the major axis is 30 nm or more, the curvature of the organosilicon polymer particles is small, and when the speed is increased, the particles are less likely to be embedded in the toner particles even during durable image output. This improves the charge injection from the photoreceptor to the toner over a long period of time from the beginning. This makes it possible to suppress image defects (roughness in halftone images) caused by toner scattering over a long period of time from the beginning. Furthermore, toner deterioration is stably suppressed until the end of the cartridge life. As a result, stable fluidity can be maintained from the beginning to the end of the cartridge life. This improves fogging in a high-temperature, high-humidity environment from the beginning to the end of the cartridge life.
[0043] Furthermore, when the major axis is 300 nm or less, the toner particles can be stably present on the surface of the toner particles even at high speeds. Also, embedding in the toner particles is suppressed even during durable image output. This improves charge injection from the photoreceptor to the toner over a long period of time from the initial stage. Furthermore, toner deterioration is stably suppressed until the end of the cartridge life. As a result, stable fluidity can be maintained from the initial stage to the end of the cartridge life. This improves fogging in a high-temperature, high-humidity environment from the initial stage to the end of the cartridge life.
[0044] It is preferable that the adhesion rate of the organosilicon polymer particles to the toner particles during the water washing method is 25% or less. When the adhesion rate to the toner particles is 25% or less, most of the organosilicon polymer particles are present on the toner particle surface in a state where they can roll. By allowing the organosilicon polymer particles to roll on the toner particle surface, charge is efficiently injected from the photoreceptor into the toner, and the toner becomes uniformly charged. In addition, when the speed is increased, the toner particles are less likely to be embedded in the toner even during durable image output. This improves charge injection from the photoreceptor into the toner from the initial stage to the long term. As a result, image problems (roughness in halftone images) caused by toner scattering can be suppressed from the initial stage to the long term. Furthermore, toner deterioration is stably suppressed until the end of the cartridge life. As a result, stable fluidity can be maintained from the initial stage to the end of the cartridge life. This improves fogging in a high temperature and high humidity environment from the initial stage to the end of the cartridge life. Furthermore, the organosilicon polymer particles preferably have a silanol structure content of 98% by weight or more relative to the total content of alkoxysilane structures and silanol structures contained in the T1 and T2 unit structures, which further improves the charge injection properties into the toner, which is an effect of the present invention.
[0045] (ii) A case will be described in which a toner containing a binder resin and having toner particles having an organosilicon polymer on the surface is used.
[0046] In the above-mentioned constitution, when using a toner having toner particles with an organosilicon polymer on the surface, there is no particular restriction on the formation method, and a conventionally known method can be used. Among them, since it is possible to easily form an organosilicon polymer on the surface of the toner base particles, a method can be used in which the compound shown in the explanation of the organosilicon compound represented by the above formula (Z) is condensed in an aqueous medium in which the toner base particles are dispersed, and an organosilicon polymer is formed on the toner base particles. This method is described below.
[0047] When forming toner particles having an organosilicon polymer on the surface, it is preferable to include a step (step 1) of dispersing toner base particles in an aqueous medium to obtain a toner base particle dispersion, and a step (step 2) of mixing an organosilicon compound (or a hydrolyzate thereof) with the toner base particle dispersion and causing a condensation reaction of the organosilicon compound in the toner base particle dispersion to form an organosilicon polymer on the toner base particles.
[0048] In the above step 1, the method for obtaining the toner base particle dispersion may include a method of using the dispersion of toner base particles produced in an aqueous medium as is, and a method of putting dried toner base particles into an aqueous medium and dispersing them mechanically, etc. When dispersing dried toner base particles in an aqueous medium, a dispersion aid may be used.
[0049] As the dispersion aid, known dispersion stabilizers and surfactants can be used. Specifically, the dispersion stabilizer includes inorganic dispersion stabilizers such as tricalcium phosphate, hydroxyapatite, magnesium phosphate, zinc phosphate, aluminum phosphate, calcium carbonate, magnesium carbonate, calcium hydroxide, magnesium hydroxide, aluminum hydroxide, calcium metasilicate, calcium sulfate, barium sulfate, bentonite, silica, and alumina, and organic dispersion stabilizers such as polyvinyl alcohol, gelatin, methyl cellulose, methylhydroxypropyl cellulose, ethyl cellulose, sodium salt of carboxymethyl cellulose, and starch. In addition, the surfactant includes anionic surfactants such as alkyl sulfate ester salts, alkylbenzene sulfonates, and fatty acid salts, nonionic surfactants such as polyoxyethylene alkyl ethers and polyoxypropylene alkyl ethers, and cationic surfactants such as alkylamine salts and quaternary ammonium salts. Among them, it is preferable to include an inorganic dispersion stabilizer, and it is more preferable to include a dispersion stabilizer containing a phosphate such as tricalcium phosphate, hydroxyapatite, magnesium phosphate, zinc phosphate, or aluminum phosphate.
[0050] In the above step 2, the organosilicon compound may be added to the toner base particle dispersion liquid as it is, or may be added to the toner base particle dispersion liquid after hydrolysis. Among them, it is preferable to add it after hydrolysis, since the condensation reaction is easy to control and the amount of the organosilicon compound remaining in the toner base particle dispersion liquid can be reduced. The above hydrolysis is preferably carried out in an aqueous medium whose pH is adjusted using a known acid and base. It is known that the hydrolysis of an organosilicon compound is pH-dependent, and it is preferable to appropriately change the pH when carrying out the above hydrolysis depending on the type of the organosilicon compound. For example, when methyltriethoxysilane is used as the organosilicon compound, it is preferable that the pH of the above aqueous medium is 2.0 or more and 6.0 or less.
[0051] Specific examples of acids for adjusting the pH include inorganic acids such as hydrochloric acid, hydrobromic acid, hydroiodic acid, hypochlorous acid, chlorous acid, chloric acid, perchloric acid, hypobromous acid, bromous acid, bromic acid, perbromic acid, hypoiodous acid, iodous acid, iodic acid, periodic acid, sulfuric acid, nitric acid, phosphoric acid, and boric acid, and organic acids such as acetic acid, citric acid, formic acid, gluconic acid, lactic acid, oxalic acid, and tartaric acid.
[0052] Specific examples of bases for adjusting the pH include the following: alkali metal hydroxides such as potassium hydroxide, sodium hydroxide, lithium hydroxide, etc., and aqueous solutions of these; alkali metal carbonates such as potassium carbonate, sodium carbonate, lithium carbonate, etc., and aqueous solutions of these; alkali metal sulfates such as potassium sulfate, sodium sulfate, lithium sulfate, etc., and aqueous solutions of these; alkali metal phosphates such as potassium phosphate, sodium phosphate, lithium phosphate, etc., and aqueous solutions of these; alkaline earth metal hydroxides such as calcium hydroxide, magnesium hydroxide, etc., and aqueous solutions of these; and amines such as ammonia and triethylamine.
[0053] The condensation reaction in the step 2 is preferably controlled by adjusting the pH of the toner base particle dispersion. It is known that the condensation reaction of an organosilicon compound is pH-dependent, and the pH at which the condensation reaction is carried out is preferably changed as appropriate depending on the type of organosilicon compound. For example, when methyltriethoxysilane is used as the organosilicon compound, the pH of the aqueous medium is preferably 6.0 or more and 12.0 or less. As the acid and base for adjusting the pH, the acids and bases exemplified in the above hydrolysis section can be used.
[0054] By adjusting the pH, reaction temperature, and reaction time, 29 In Si-NMR measurements, the organosilicon polymer can control the ratio of the combined area of the peak derived from silicon atoms having a T2 unit structure and the peak area derived from silicon atoms having a T1 unit structure to the combined area of the peak derived from all silicon atoms to be 0.10 or more and 0.40 or less.
[0055] If the ratio of the total area of the peaks derived from silicon atoms having a T2 unit structure and the peaks derived from silicon atoms having a T1 unit structure to the total area of the peaks derived from all silicon atoms is less than 0.10, when charge is injected from the photoreceptor of the present invention into the toner, the amount of silanol groups (and some of the alkoxysilane groups) in the organosilicon polymer is small, and charge injection properties are reduced. As a result, poor charging during development at high speeds is likely to cause image problems due to toner scattering (roughness in half-tone images). Fog due to electrostatic aggregation in low-temperature, low-humidity environments is exacerbated.
[0056] On the other hand, if it exceeds 0.40, when charge is injected from the photoconductor of the present invention to the toner, the amount of silanol groups (and some of the alkoxysilane groups) in the organosilicon polymer is large, and charge leakage is likely to occur due to the organosilicon polymer. As a result, the charge injection from the photoconductor to the toner decreases, and due to poor charging during development caused by high speed development, image problems due to toner scattering (roughness in halftone images) are likely to occur. Also, fogging in high temperature and high humidity environments worsens.
[0057] The organosilicon polymer 29 In the Si-NMR measurement, the ratio of the area of the peak derived from silicon having T3 unit structure to the total area of the peak derived from all silicon atoms contained in the organosilicon polymer is preferably 0.50 or more and 0.90 or less. By being in the above range, the deterioration of the organosilicon polymer itself is suppressed. As a result, when the speed is increased, the toner particles are less likely to be buried even during durable image output. This makes it possible to improve the charge injection from the photoreceptor to the toner from the initial stage to the long term.
[0058] Furthermore, the organosilicon polymer preferably has a silanol structure content of 98% by weight or more relative to the total content of alkoxysilane structures and silanol structures contained in the T1 and T2 unit structures, which further improves the charge injection properties into the toner, which is an effect of the present invention.
[0059] The average circularity of the toner is preferably 0.950 or more and 0.990 or less, and more preferably 0.970 or more and 0.990 or less. When the average circularity of the toner particles is within the above range, it means that the toner particles have a uniform shape. As a result, even when the speed is increased, image defects (roughness in halftone images) caused by toner scattering, which is an effect of the present invention, are suppressed, and transferability is improved. The average circularity of the toner can be controlled by adjusting the production conditions, and can be measured by the measurement method described later.
[0060] The configuration of the electrophotographic photoreceptor according to the present invention will be described below.
[0061] <Support> In the electrophotographic photoreceptor according to the present invention, the support is preferably a conductive support having electrical conductivity. The shape of the support may be cylindrical, belt-like, or sheet-like. Of these, a cylindrical support is preferable. The surface of the support may be subjected to electrochemical treatment such as anodization, blasting, cutting, or the like. The material of the support is preferably metal, resin, glass, or the like. Examples of metals include aluminum, iron, nickel, copper, gold, stainless steel, and alloys thereof. Of these, an aluminum support using aluminum is preferable. The resin or glass is preferably imparted with electrical conductivity by a treatment such as mixing or coating a conductive material.
[0062] <Conductive layer> In the electrophotographic photoreceptor according to the present invention, a conductive layer may be provided on the support. By providing the conductive layer, scratches and unevenness on the support surface can be concealed and light reflection on the support surface can be controlled. The conductive layer preferably contains conductive particles and a resin. Examples of the material of the conductive particles include metal oxides, metals, and carbon black.
[0063] Examples of metal oxides include zinc oxide, aluminum oxide, indium oxide, silicon oxide, zirconium oxide, tin oxide, titanium oxide, magnesium oxide, antimony oxide, bismuth oxide, etc. Examples of metals include aluminum, nickel, iron, nichrome, copper, zinc, silver, etc. Among these, it is preferable to use metal oxides as the conductive particles, and it is particularly preferable to use titanium oxide, tin oxide, or zinc oxide. When a metal oxide is used as the conductive particles, the surface of the metal oxide may be treated with a silane coupling agent or the like, or the metal oxide may be doped with an element such as phosphorus or aluminum or an oxide thereof. The conductive particles are preferably titanium oxide particles, barium sulfate particles, or zinc oxide particles having niobium atoms unevenly distributed near the surfaces. When a metal oxide is used as the conductive particles, the volume average particle size is preferably 1 nm or more and 500 nm or less, and more preferably 3 nm or more and 400 nm or less.
[0064] Examples of the resin include polyester resin, polycarbonate resin, polyvinyl acetal resin, acrylic resin, silicone resin, epoxy resin, melamine resin, polyurethane resin, phenol resin, alkyd resin, etc. The conductive layer may further contain silicone oil, resin particles, a masking agent such as titanium oxide, etc.
[0065] The conductive layer can be formed by preparing a conductive layer coating solution containing the above-mentioned materials and solvent, forming this coating film on a support, and drying it. Examples of the solvent used in the coating solution include alcohol-based solvents, sulfoxide-based solvents, ketone-based solvents, ether-based solvents, ester-based solvents, and aromatic hydrocarbon-based solvents. Examples of the dispersion method for dispersing the conductive particles in the conductive layer coating solution include a method using a paint shaker, a sand mill, a ball mill, and a liquid collision type high-speed disperser.
[0066] The average thickness of the conductive layer is preferably from 1 μm to 40 μm, and particularly preferably from 3 μm to 30 μm.
[0067] <Undercoat layer> In the electrophotographic photoreceptor according to the present invention, an undercoat layer may be provided on the support or the conductive layer. By providing the undercoat layer, the adhesion between layers is improved and a charge injection blocking function can be imparted. The undercoat layer preferably contains a resin. The undercoat layer may also be formed as a cured film by polymerizing a composition containing a monomer having a polymerizable functional group.
[0068] Examples of the resin include polyester resin, polycarbonate resin, polyvinyl acetal resin, acrylic resin, epoxy resin, melamine resin, polyurethane resin, phenol resin, polyvinyl phenol resin, alkyd resin, polyvinyl alcohol resin, polyethylene oxide resin, polypropylene oxide resin, polyamide resin, polyamic acid resin, polyimide resin, polyamideimide resin, and cellulose resin.
[0069] Examples of the polymerizable functional group contained in the monomer having a polymerizable functional group include an isocyanate group, a blocked isocyanate group, a methylol group, an alkylated methylol group, an epoxy group, a metal alkoxide group, a hydroxyl group, an amino group, a carboxyl group, a thiol group, a carboxylic anhydride group, and a carbon-carbon double bond group.
[0070] For the purpose of improving electrical properties, the undercoat layer may further contain an electron transporting material, a metal oxide, a metal, a conductive polymer, etc. Among these, it is preferable to use an electron transporting material or a metal oxide. Examples of the electron transport substance include a quinone compound, an imide compound, a benzimidazole compound, a cyclopentadienylidene compound, a fluorenone compound, a xanthone compound, a benzophenone compound, a cyanovinyl compound, an aryl halide compound, a silole compound, a boron-containing compound, etc. An electron transport substance having a polymerizable functional group may be used as the electron transport substance, and the undercoat layer may be formed as a cured film by copolymerizing the electron transport substance with the monomer having the polymerizable functional group described above. Examples of metal oxides include indium tin oxide, tin oxide, indium oxide, titanium oxide, zinc oxide, aluminum oxide, silicon dioxide, etc. Examples of metals include gold, silver, aluminum, etc.
[0071] The metal oxide particles contained in the undercoat layer may be surface-treated with a surface treatment agent such as a silane coupling agent. The surface treatment of the metal oxide particles can be carried out by a common method, such as a dry method or a wet method. In the dry method, metal oxide particles are stirred in a mixer capable of high-speed stirring, such as a Henschel mixer, while an alcohol aqueous solution, an organic solvent solution, or an aqueous solution containing a surface treatment agent is added to the metal oxide particles to uniformly disperse them, and then the particles are dried. In the wet method, the metal oxide particles and the surface treatment agent are stirred in a solvent or dispersed in a sand mill using glass beads or the like, and the solvent is removed by filtration or distillation under reduced pressure after dispersion. After removing the solvent, it is preferable to further bake the mixture at 100°C or higher.
[0072] The undercoat layer may further contain additives, for example, known materials such as metal powder such as aluminum, conductive materials such as carbon black, charge transport materials, metal chelate compounds, and organometallic compounds. Examples of the charge transport substance include quinone compounds, imide compounds, benzimidazole compounds, cyclopentadienylidene compounds, fluorenone compounds, xanthone compounds, benzophenone compounds, cyanovinyl compounds, aryl halide compounds, silole compounds, boron-containing compounds, etc. A charge transport substance having a polymerizable functional group may be used as the charge transport substance, and the undercoat layer may be formed as a cured film by copolymerizing the charge transport substance with the monomer having the polymerizable functional group.
[0073] The undercoat layer can be formed by preparing a coating solution for the undercoat layer containing the above-mentioned materials and solvent, forming a coating film of this on a support or a conductive layer, and drying and / or curing it. Examples of the solvent used in the coating solution for the undercoat layer include organic solvents such as alcohols, sulfoxides, ketones, ethers, esters, halogenated aliphatic hydrocarbons, aromatic compounds, etc. In the present invention, it is preferable to use alcohol-based and ketone-based solvents. Examples of a dispersion method for preparing a coating solution for the undercoat layer include methods using a homogenizer, an ultrasonic disperser, a ball mill, a sand mill, a roll mill, a vibration mill, an attritor, and a liquid collision type high-speed disperser. The average thickness of the undercoat layer is preferably from 0.1 μm to 10 μm, and more preferably from 0.1 μm to 5 μm.
[0074] <Photosensitive layer> The photosensitive layer of an electrophotographic photoreceptor is mainly classified into (1) a laminated type photosensitive layer and (2) a single-layer type photosensitive layer. (1) The laminated type photosensitive layer is a photosensitive layer having a charge generation layer containing a charge generation material and a charge transport layer containing a charge transport material. (2) The single-layer type photosensitive layer is a photosensitive layer containing both a charge generation material and a charge transport material.
[0075] (1) Laminated photosensitive layer The laminated type photosensitive layer has a charge generating layer and a charge transport layer.
[0076] (1-1) Charge generation layer The charge generating layer preferably contains a charge generating material and a resin.
[0077] Examples of the charge generating material include azo pigments, perylene pigments, polycyclic quinone pigments, indigo pigments, and phthalocyanine pigments. Among these, azo pigments and phthalocyanine pigments are preferred. Among phthalocyanine pigments, oxytitanium phthalocyanine pigments, chlorogallium phthalocyanine pigments, and hydroxygallium phthalocyanine pigments are preferred. The content of the charge generating material in the charge generating layer is preferably from 40% by mass to 85% by mass, and more preferably from 60% by mass to 80% by mass, based on the total mass of the charge generating layer.
[0078] Examples of the resin include polyester resin, polycarbonate resin, polyvinyl acetal resin, polyvinyl butyral resin, acrylic resin, silicone resin, epoxy resin, melamine resin, polyurethane resin, phenol resin, polyvinyl alcohol resin, cellulose resin, polystyrene resin, polyvinyl acetate resin, polyvinyl chloride resin, etc. Among these, polyvinyl butyral resin is more preferable.
[0079] The charge generating layer may further contain additives such as an antioxidant and an ultraviolet absorbing agent, etc. Specific examples of such additives include hindered phenol compounds, hindered amine compounds, sulfur compounds, phosphorus compounds, and benzophenone compounds.
[0080] The charge generating layer can be formed by preparing a coating solution for the charge generating layer containing the above-mentioned materials and solvent, forming a coating film of this on the undercoat layer, and drying it. Examples of the solvent used in the coating solution include alcohol-based solvents, sulfoxide-based solvents, ketone-based solvents, ether-based solvents, ester-based solvents, and aromatic hydrocarbon-based solvents. The average thickness of the charge generating layer is preferably from 0.1 μm to 1 μm, and more preferably from 0.15 μm to 0.4 μm.
[0081] (1-2) Charge transport layer The charge transport layer preferably contains a charge transport material and a resin.
[0082] Examples of the charge transport material include polycyclic aromatic compounds, heterocyclic compounds, hydrazone compounds, styryl compounds, enamine compounds, benzidine compounds, triarylamine compounds, resins having groups derived from these materials, etc. Among these, triarylamine compounds and benzidine compounds are preferred. The content of the charge transport material in the charge transport layer is preferably from 25% by weight to 70% by weight, and more preferably from 30% by weight to 55% by weight, based on the total weight of the charge transport layer.
[0083] Examples of the resin include polyester resin, polycarbonate resin, acrylic resin, polystyrene resin, etc. Among these, polycarbonate resin and polyester resin are preferable. As the polyester resin, polyarylate resin is particularly preferable. The content ratio (mass ratio) of the charge transport material to the resin is preferably from 4:10 to 20:10, and more preferably from 5:10 to 12:10.
[0084] The charge transport layer may also contain additives such as antioxidants, ultraviolet absorbers, plasticizers, leveling agents, slipping agents, and abrasion resistance improvers. Specific examples of such additives include hindered phenol compounds, hindered amine compounds, sulfur compounds, phosphorus compounds, benzophenone compounds, siloxane-modified resins, silicone oils, fluororesin particles, polystyrene resin particles, polyethylene resin particles, silica particles, alumina particles, and boron nitride particles.
[0085] The charge transport layer can be formed by preparing a coating solution for the charge transport layer containing the above-mentioned materials and solvent, forming the coating film on the charge generating layer, and drying it. Examples of the solvent used in the coating solution include alcohol-based solvents, ketone-based solvents, ether-based solvents, ester-based solvents, and aromatic hydrocarbon-based solvents. Among these solvents, ether-based solvents or aromatic hydrocarbon-based solvents are preferred. The average thickness of the charge transport layer is preferably from 3 μm to 50 μm, more preferably from 5 μm to 40 μm, and particularly preferably from 10 μm to 30 μm.
[0086] (2) Single-layer photosensitive layer The single-layer type photosensitive layer can be formed by preparing a coating solution for the photosensitive layer containing a charge generating material, a charge transporting material, a resin and a solvent, forming a coating film of this on the undercoat layer, and drying it. The charge generating material, the charge transporting material and the resin are the same as the examples of materials in "(1) Multi-layer type photosensitive layer" above.
[0087] <Surface protective layer> The surface protective layer may contain a polymer of a compound having a polymerizable functional group and a resin. Examples of the polymerizable functional group include an isocyanate group, a blocked isocyanate group, a methylol group, an alkylated methylol group, an epoxy group, a metal alkoxide group, a hydroxyl group, an amino group, a carboxyl group, a thiol group, a carboxylic anhydride group, a carbon-carbon double bond group, an alkoxysilyl group, a silanol group, etc. As a compound having a polymerizable functional group, a monomer having a charge transporting ability may be used. Examples of the resin include polyester resin, acrylic resin, phenoxy resin, polycarbonate resin, polystyrene resin, phenol resin, melamine resin, epoxy resin, etc. Among these, acrylic resin is preferable.
[0088] The material and particle size of the conductive particles contained in the surface protective layer are as described above. From the viewpoint of dispersibility and liquid stability, it is preferable to treat the surface of the metal oxide with a silane coupling agent or the like. The surface protective layer may contain additives such as antioxidants, ultraviolet absorbers, plasticizers, leveling agents, slipping agents, abrasion resistance improvers, etc. Specific examples of such additives include hindered phenol compounds, hindered amine compounds, sulfur compounds, phosphorus compounds, benzophenone compounds, siloxane-modified resins, silicone oils, fluororesin particles, polystyrene resin particles, polyethylene resin particles, silica particles, alumina particles, and boron nitride particles.
[0089] The surface protective layer can be formed by preparing a coating solution for the surface protective layer containing the above-mentioned materials and solvent, forming the coating film on the photosensitive layer, and drying and / or curing the coating film. Examples of the solvent used in the coating solution include alcohol-based solvents, ketone-based solvents, ether-based solvents, sulfoxide-based solvents, ester-based solvents, and aromatic hydrocarbon-based solvents. The average thickness of the surface protective layer is preferably from 0.2 μm to 5 μm, and more preferably from 0.5 μm to 3 μm. The constitution of the toner according to the present invention will be described below.
[0090] <Binding resin> The toner according to the present invention contains a binder resin. The content of the binder resin is preferably 50% by mass or more based on the total amount of resin components in the toner particles. The binder resin is not particularly limited, but examples thereof include styrene-acrylic resin, epoxy resin, polyester resin, polyurethane resin, polyamide resin, cellulose resin, polyether resin, mixed resin or composite resin thereof. Styrene-acrylic resin and polyester resin are preferred because they are inexpensive, easily available, and have excellent low-temperature fixing properties. Styrene-acrylic resin is more preferred because they have excellent development durability.
[0091] The polyester resin can be obtained by combining suitable compounds selected from polyvalent carboxylic acids, polyols, hydroxycarboxylic acids, etc., and synthesizing them using a conventionally known method such as an ester exchange method or a polycondensation method.
[0092] Polycarboxylic acids are compounds containing two or more carboxy groups in one molecule. Among them, dicarboxylic acids are compounds containing two carboxy groups in one molecule and are preferably used. Examples of the acid include oxalic acid, succinic acid, glutaric acid, maleic acid, adipic acid, β-methyladipic acid, azelaic acid, sebacic acid, nonanedicarboxylic acid, decanedicarboxylic acid, undecanedicarboxylic acid, dodecanedicarboxylic acid, fumaric acid, citraconic acid, diglycolic acid, cyclohexane-3,5-diene-1,2-carboxylic acid, hexahydroterephthalic acid, malonic acid, pimelic acid, suberic acid, phthalic acid, isophthalic acid, terephthalic acid, tetrachlorophthalic acid, chlorophthalic acid, nitrophthalic acid, p-carboxyphenylacetic acid, p-phenylenediacetic acid, m-phenylenediacetic acid, o-phenylenediacetic acid, diphenylacetic acid, diphenyl-p,p'-dicarboxylic acid, naphthalene-1,4-dicarboxylic acid, naphthalene-1,5-dicarboxylic acid, naphthalene-2,6-dicarboxylic acid, anthracenedicarboxylic acid, and cyclohexanedicarboxylic acid.
[0093] Examples of polyvalent carboxylic acids other than dicarboxylic acids include trimellitic acid, trimesic acid, pyromellitic acid, naphthalene tricarboxylic acid, naphthalene tetracarboxylic acid, pyrene tricarboxylic acid, pyrene tetracarboxylic acid, itaconic acid, glutaconic acid, n-dodecyl succinic acid, n-dodecenyl succinic acid, isododecyl succinic acid, isododecenyl succinic acid, n-octyl succinic acid, n-octenyl succinic acid, etc. These may be used alone or in combination of two or more.
[0094] A polyol is a compound containing two or more hydroxyl groups in one molecule. Among them, a diol is a compound containing two hydroxyl groups in one molecule, and is preferably used. Specifically, ethylene glycol, diethylene glycol, triethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,11-undecanediol, 1,12-dodecanediol, 1,13-tridecanediol, 1,14-tetradecanediol, 1,18-octadecanediol, 1,14-eicosane Examples of the alkylene glycol include decanediol, dipropylene glycol, polyethylene glycol, polypropylene glycol, polytetramethylene ether glycol, 1,4-cyclohexanediol, 1,4-cyclohexanedimethanol, 1,4-butenediol, neopentyl glycol, polytetramethylene glycol, hydrogenated bisphenol A, bisphenol A, bisphenol F, bisphenol S, and alkylene oxide (ethylene oxide, propylene oxide, butylene oxide, etc.) adducts of the above bisphenols. Among these, alkylene glycols having 2 to 12 carbon atoms and alkylene oxide adducts of bisphenols are preferred, and alkylene oxide adducts of bisphenols and combinations of these with alkylene glycols having 2 to 12 carbon atoms are particularly preferred.
[0095] Examples of trihydric or higher alcohols include glycerin, trimethylolethane, trimethylolpropane, pentaerythritol, hexamethylolmelamine, hexaethylolmelamine, tetramethylolbenzoguanamine, tetraethylolbenzoguanamine, sorbitol, trisphenol PA, phenol novolac, cresol novolac, alkylene oxide adducts of the above trihydric or higher alcohols, etc. These may be used alone or in combination of two or more.
[0096] Examples of the styrene-acrylic resin include homopolymers made of the following polymerizable monomers, copolymers obtained by combining two or more of these, and mixtures thereof: styrene derivatives such as styrene, α-methylstyrene, β-methylstyrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, 2,4-dimethylstyrene, pn-butylstyrene, p-tert-butylstyrene, pn-hexylstyrene, pn-octylstyrene, pn-nonylstyrene, pn-decylstyrene, pn-dodecylstyrene, p-methoxystyrene, and p-phenylstyrene; (Meth)acrylic derivatives such as methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, iso-propyl (meth)acrylate, n-butyl (meth)acrylate, iso-butyl (meth)acrylate, tert-butyl (meth)acrylate, n-amyl (meth)acrylate, n-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-octyl (meth)acrylate, n-nonyl (meth)acrylate, cyclohexyl (meth)acrylate, benzyl (meth)acrylate, dimethyl phosphate ethyl (meth)acrylate, diethyl phosphate ethyl (meth)acrylate, dibutyl phosphate ethyl (meth)acrylate and 2-benzoyloxyethyl (meth)acrylate, (meth)acrylonitrile, 2-hydroxyethyl (meth)acrylate, (meth)acrylic acid, maleic acid; Vinyl ether derivatives such as vinyl methyl ether and vinyl isobutyl ether; vinyl ketone derivatives such as vinyl methyl ketone, vinyl ethyl ketone and vinyl isopropenyl ketone; and polyolefins such as ethylene, propylene and butadiene.
[0097] The styrene acrylic resin may contain a polyfunctional polymerizable monomer as required. Examples of the polyfunctional polymerizable monomer include diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, 2,2'-bis(4-((meth)acryloxydiethoxy)phenyl)propane, trimethylolpropane tri(meth)acrylate, tetramethylolmethane tetra(meth)acrylate, divinylbenzene, divinylnaphthalene, and divinyl ether. In order to control the degree of polymerization, it is also possible to further add a known chain transfer agent and polymerization inhibitor.
[0098] Examples of the polymerization initiator for obtaining the styrene-acrylic resin include organic peroxide-based initiators and azo-based polymerization initiators. Examples of the organic peroxide initiator include benzoyl peroxide, lauroyl peroxide, di-α-cumyl peroxide, 2,5-dimethyl-2,5-bis(benzoylperoxy)hexane, bis(4-t-butylcyclohexyl)peroxydicarbonate, 1,1-bis(t-butylperoxy)cyclododecane, t-butylperoxymaleic acid, bis(t-butylperoxy)isophthalate, methyl ethyl ketone peroxide, tert-butylperoxy-2-ethylhexanoate, diisopropyl peroxycarbonate, cumene hydroperoxide, 2,4-dichlorobenzoyl peroxide, and tert-butylperoxypivalate. Examples of the azo polymerization initiator include 2,2'-azobis-(2,4-dimethylvaleronitrile), 2,2'-azobisisobutyronitrile, 1,1'-azobis(cyclohexane-1-carbonitrile), 2,2'-azobis-4-methoxy-2,4-dimethylvaleronitrile, azobismethylbutyronitrile, and 2,2'-azobis-(methyl isobutyrate).
[0099] Also, a redox initiator combining an oxidizing substance and a reducing substance can be used as the polymerization initiator. Examples of the oxidizing substance include hydrogen peroxide, inorganic peroxides such as persulfates (sodium salts, potassium salts, and ammonium salts), and oxidizing metal salts such as tetravalent cerium salts. Examples of the reducing substance include reducing metal salts (divalent iron salts, monovalent copper salts, and trivalent chromium salts), ammonia, lower amines (amines having 1 to 6 carbon atoms such as methylamine and ethylamine), amino compounds such as hydroxylamine, reducing sulfur compounds such as sodium thiosulfate, sodium hydrosulfite, sodium hydrogensulfite, sodium sulfite, and sodium formaldehyde sulfoxylate, lower alcohols (having 1 to 6 carbon atoms), ascorbic acid or its salts, and lower aldehydes (having 1 to 6 carbon atoms).
[0100] The polymerization initiator is selected with reference to its 10-hour half-life temperature and is used alone or in combination. The amount of the polymerization initiator to be added varies depending on the desired degree of polymerization, but is generally 0.5 parts by mass or more and 20.0 parts by mass or less per 100.0 parts by mass of the polymerizable monomer.
[0101] <Coloring agent> The toner according to the present invention may contain a colorant. As the colorant, there is no particular limitation, and conventionally known pigments and dyes of black, yellow, magenta, cyan, and other colors, magnetic materials, and the like can be used. Black colorants include black pigments such as carbon black.
[0102] Examples of yellow colorants include yellow pigments and yellow dyes such as monoazo compounds, disazo compounds, condensed azo compounds, isoindolinone compounds, benzimidazolone compounds, anthraquinone compounds, azo metal complexes, methine compounds, and allylamide compounds.Specific examples include CI Pigment Yellow 74, 93, 95, 109, 111, 128, 155, 174, 180, 185, and CI Solvent Yellow 162.
[0103] Examples of magenta colorants include magenta pigments and magenta dyes such as monoazo compounds, condensed azo compounds, diketopyrrolopyrrole compounds, anthraquinone compounds, quinacridone compounds, basic dye lake compounds, naphthol compounds, benzimidazolone compounds, thioindigo compounds, and perylene compounds. Specific examples include CI Pigment Red 2, 3, 5, 6, 7, 23, 48:2, 48:3, 48:4, 57:1, 81:1, 122, 144, 146, 150, 166, 169, 177, 184, 185, 202, 206, 220, 221, 238, 254, 269, and CI Pigment Violet Red 19.
[0104] Examples of cyan colorants include cyan pigments and cyan dyes such as copper phthalocyanine compounds and derivatives thereof, anthraquinone compounds, and basic dye lake compounds. Specifically, examples include CI Pigment Blue 1, 7, 15, 15:1, 15:2, 15:3, 15:4, 60, 62, and 66.
[0105] The content of the colorant is preferably 1.0 part by mass or more and 20.0 parts by mass or less with respect to 100.0 parts by mass of the binder resin or the polymerizable monomer.
[0106] The toner may also be made magnetic by incorporating a magnetic material, in which case the magnetic material may also function as a colorant. Examples of magnetic materials include iron oxides such as magnetite, hematite, and ferrite; metals such as iron, cobalt, and nickel; and alloys of these metals with metals such as aluminum, cobalt, copper, lead, magnesium, tin, zinc, antimony, beryllium, bismuth, cadmium, calcium, manganese, selenium, titanium, tungsten, and vanadium, and mixtures thereof.
[0107] <Wax> In the toner according to the present invention, known waxes can be used. Specifically, it can be exemplified by paraffin wax, microcrystalline wax, petroleum wax and its derivatives, montan wax and its derivatives, Fischer-Tropsch hydrocarbon wax and its derivatives, polyolefin wax and its derivatives, carnauba wax, candelilla wax and its natural wax and its derivatives, and the derivatives can be exemplified by oxides, block copolymers with vinyl monomers, and graft modified products.In addition, it can be exemplified by alcohols such as higher aliphatic alcohols; fatty acids such as stearic acid and palmitic acid or their acid amides, esters, and ketones; hydrogenated castor oil and its derivatives, vegetable waxes, and animal waxes.These can be used alone or in combination. The content of these waxes is preferably 1.0 part by mass or more and 30.0 parts by mass or less with respect to 100.0 parts by mass of the binder resin.
[0108] <Charge control agent> The toner according to the present invention may contain a charge control agent. As the charge control agent, any known charge control agent can be used without any particular limitation. Specific examples of the negative charge control agent include metal compounds of aromatic carboxylic acids such as salicylic acid, alkylsalicylic acid, dialkylsalicylic acid, naphthoic acid, and dicarboxylic acids, or polymers or copolymers having metal compounds of the aromatic carboxylic acids; polymers or copolymers having a sulfonic acid group, a sulfonate salt group, or a sulfonate ester group; metal salts or metal complexes of azo dyes or azo pigments; boron compounds, silicon compounds, and calixarenes.
[0109] On the other hand, examples of the positive charge control agent include the following: quaternary ammonium salts, polymeric compounds having quaternary ammonium salts in the side chains, guanidine compounds, nigrosine compounds, imidazole compounds, etc. As the polymer or copolymer having a sulfonate group or a sulfonate ester group, a homopolymer of a sulfonate group-containing vinyl monomer such as styrene sulfonic acid, 2-acrylamido-2-methylpropanesulfonic acid, 2-methacrylamido-2-methylpropanesulfonic acid, vinylsulfonic acid, or methacrylsulfonic acid, or a copolymer of the vinyl monomer shown in the section on binder resin and the above-mentioned sulfonate group-containing vinyl monomer, etc. can be used.
[0110] The content of the charge control agent is preferably 0.01 parts by mass or more and 5.0 parts by mass or less with respect to 100.0 parts by mass of the binder resin or polymerizable monomer.
[0111] <External additives> The toner according to the present invention may contain external additives. As the external additive, there is no particular limitation and any external additive known in the art can be used. Specific examples of the silica fine particles include: raw silica fine particles such as wet-process silica and dry-process silica, or surface-treated silica fine particles obtained by subjecting such raw silica fine particles to a surface treatment with a treating agent such as a silane coupling agent, a titanium coupling agent, or silicone oil; and resin fine particles such as vinylidene fluoride fine particles and polytetrafluoroethylene fine particles. The content of the external additive is preferably 0.1 parts by mass or more and 5.0 parts by mass or less with respect to 100.0 parts by mass of the toner particles.
[0112] <Production of toner base particles> The method for producing the toner base particles is not particularly limited, and may be a suspension polymerization method, a dissolution suspension method, an emulsion aggregation method, a pulverization method, etc. Among these, the suspension polymerization method is preferred.
[0113] As an example, a method for obtaining toner base particles by suspension polymerization will be described below. First, a polymerizable monomer capable of forming a binder resin and, if necessary, various additives are mixed, and the materials are dissolved or dispersed using a disperser to prepare a polymerizable monomer composition. The various additives include colorants, waxes, charge control agents, polymerization initiators, chain transfer agents, and the like. Examples of the dispersing machine include a homogenizer, a ball mill, a colloid mill, and an ultrasonic dispersing machine. Next, the polymerizable monomer composition is added to an aqueous medium containing poorly water-soluble inorganic fine particles, and droplets of the polymerizable monomer composition are prepared using a high-speed disperser such as a high-speed stirrer or an ultrasonic disperser (granulation process).
[0114] Thereafter, the polymerizable monomer in the droplets is polymerized to obtain toner base particles (polymerization step). The polymerization initiator may be mixed when preparing the polymerizable monomer composition, or may be mixed into the polymerizable monomer composition immediately before forming droplets in an aqueous medium. Alternatively, the polymerization initiator may be added in a dissolved state in the polymerizable monomer or another solvent, as necessary, during or after the granulation of the droplets, i.e., immediately before starting the polymerization reaction. After obtaining a binder resin by polymerizing the polymerizable monomer, a solvent removal treatment may be carried out as necessary to obtain a dispersion liquid of toner base particles.
[0115] When the binder resin is obtained by the emulsion aggregation method or the suspension polymerization method, the polymerizable monomer may be any conventionally known monomer without any particular limitation. Specifically, the vinyl monomers listed in the section on the binder resin may be used. As the polymerization initiator, any known polymerization initiator can be used without particular limitation. Specific examples thereof include those mentioned above.
[0116] [Process cartridges, electrophotographic devices] The process cartridge of the present invention comprises the electrophotographic photosensitive member and toner described above, and a developing means for accommodating the toner, and is characterized in that it is detachably mountable to the main body of the electrophotographic apparatus.
[0117] The developing means has a toner storage section that stores toner, and supplies the toner to the surface of the electrophotographic photosensitive member. In the present invention, the developing device is preferably a contact developing device that performs development by bringing a toner carrier carrying toner into contact with the photosensitive member. The electrophotographic device of the present invention is also characterized by having the process cartridge of the present invention.
[0118] FIG. 2 shows an example of a schematic configuration of an electrophotographic apparatus having a process cartridge equipped with an electrophotographic photosensitive member. A cylindrical (drum-shaped) electrophotographic photoreceptor (1 in FIG. 2) is driven to rotate around an axis 2 in the direction of an arrow at a predetermined peripheral speed (process speed). The surface of the electrophotographic photoreceptor is charged to a predetermined positive or negative potential by a charging means 3 during the rotation process. Note that, although a roller charging method using a roller-type charging member is shown in FIG. 2, a charging method such as a corona charging method, a proximity charging method, or an injection charging method may be adopted. Exposure light 4 is irradiated from an exposure means (not shown) onto the charged surface of the electrophotographic photoreceptor, and an electrostatic latent image corresponding to the target image information is formed. The exposure light 4 is light whose intensity is modulated in response to a time-series electric digital image signal of the target image information, and is output from an image exposure means such as a slit exposure or a laser beam scanning exposure. The electrostatic latent image formed on the surface of the electrophotographic photoreceptor is developed (normal development or reversal development) with toner contained in a developing means 5, and a toner image is formed on the surface of the electrophotographic photoreceptor 1. The toner image formed on the surface of the electrophotographic photoreceptor is transferred to a transfer material 7 by a transfer means 6. At this time, a bias voltage of a polarity opposite to the charge held by the toner is applied to the transfer means 6 from a bias power source (not shown). When the transfer material 7 is paper, the transfer material 7 is taken out from a paper feeder (not shown) and fed between the electrophotographic photosensitive member and the transfer means 6 in synchronization with the rotation of the electrophotographic photosensitive member 1. The transfer material 7 onto which the toner image has been transferred from the electrophotographic photosensitive member is separated from the surface of the electrophotographic photosensitive member and conveyed to a fixing means 8, where the toner image is fixed, and the image is printed out as an image formed product (print, copy) outside the electrophotographic device. The electrophotographic device may have a cleaning means 9 for removing deposits such as toner remaining on the surface of the electrophotographic photosensitive member after transfer. Alternatively, a so-called cleanerless system may be used in which the deposits are removed by a developing means or the like without providing a separate cleaning means. In the present invention, among the components selected from the above-mentioned electrophotographic photosensitive member, charging means 3, developing means 5, cleaning means 9, etc., a plurality of components are housed in a container and supported integrally to form a process cartridge, which can be configured to be detachably attached to the main body of the electrophotographic apparatus. For example, it can be configured as follows.At least one selected from the charging means 3, the developing means 5 and the cleaning means 9 is integrally supported together with the electrophotographic photosensitive member to form a cartridge. This can be made into a process cartridge 11 that is detachably attached to the main body of the electrophotographic apparatus using guide means 12 such as a rail of the main body of the electrophotographic apparatus. The electrophotographic apparatus may have a charge eliminating mechanism that eliminates charge on the surface of the electrophotographic photosensitive member by pre-exposure light 10 from a pre-exposure means (not shown). Also, guide means 12 such as a rail may be provided in order to attach and detach the process cartridge 11 of the present invention to the main body of the electrophotographic apparatus. The electrophotographic apparatus of the present invention is characterized by having the above-mentioned process cartridge.
[0119] The process cartridge of the present invention can be used in laser beam printers, LED printers, copiers, facsimiles, and multifunction machines thereof. EXAMPLES
[0120] The present invention will be described in more detail below using examples and comparative examples. The present invention is not limited to the following examples without departing from the gist of the present invention. In the following description of the examples, "parts" are by mass unless otherwise specified. The present invention will be described in more detail below with reference to examples. In the examples, "parts" means "parts by mass." The methods for measuring the various physical properties are described below. However, Examples 15 to 17 are reference examples.
[0121] <Calculation of primary particle size of conductive particles> First, the entire electrophotographic photoreceptor was immersed in methyl ethyl ketone (MEK) in a graduated cylinder and irradiated with ultrasonic waves to peel off the resin layer, and then the substrate of the electrophotographic photoreceptor was taken out. Next, the insoluble matter that does not dissolve in MEK (photosensitive layer and protective layer containing conductive particles) was filtered and dried in a vacuum dryer. Furthermore, the obtained solid was suspended in a mixed solvent of tetrahydrofuran (THF) / methylal at a volume ratio of 1:1, the insoluble matter was filtered, and the filtrate was collected and dried in a vacuum dryer. By this operation, conductive particles and the resin of the protective layer were obtained. Furthermore, the filtrate was heated to 500°C in an electric furnace so that the solid was only the conductive particles, and the conductive particles were collected. In order to secure the necessary amount of conductive particles for measurement, the same treatment was applied to multiple electrophotographic photoreceptors. A part of the collected conductive particles was dispersed in isopropanol (IPA), and the dispersion was dropped onto a grid mesh with a support film (Cu150J, manufactured by JEOL Co., Ltd.), and the conductive particles were observed in the STEM mode of a scanning transmission electron microscope (JEM2800, manufactured by JEOL Co., Ltd.). The observation was performed at a magnification of 500,000 to 1.2 million times to make it easier to calculate the particle diameter of the conductive particles, and STEM images of 100 conductive particles were taken. At this time, the acceleration voltage was set to 200 kV, the probe size was set to 1 nm, and the image size was set to 1024 x 1024 pixels. The primary particle diameter was measured using the obtained STEM image with the image processing software "Image-Pro Plus (manufactured by Media Cybernetics Co., Ltd.)". First, the scale bar displayed at the bottom of the STEM image was selected using the straight line tool (Straight Line) on the toolbar. In this state, when Set Scale is selected from the Analyze menu, a new window is opened and the pixel distance of the selected straight line is entered in the Distance in Pixels field. Enter the value of the scale bar (e.g., 100) in the Known Distance field of the window, enter the unit of the scale bar (e.g., nm) in the Unit of Measurement field, and click OK to complete the scale setting. Next, using the line tool, draw a line to represent the maximum diameter of the conductive particles, and calculate the particle diameter. The same operation was performed for 100 conductive particles, and the number average value of the obtained value (maximum diameter) was taken as the primary particle diameter of the conductive particles (hereinafter also referred to as the "number average particle diameter").
[0122] <Calculation of niobium atom / titanium atom concentration ratio> A sample piece measuring 5 mm square was cut from the photoreceptor and cut to a thickness of 200 nm using an ultrasonic ultramicrotome (Leica, UC7) at a cutting speed of 0.6 mm / s to prepare a thin sample. This thin sample was observed at magnifications of 500,000 to 1.2 million times using a scanning transmission electron microscope (JEOL, JEM2800) in STEM mode connected to an EDS analyzer (energy dispersive X-ray analyzer). Among the cross sections of the observed conductive particles, the cross sections of conductive particles having a maximum diameter of approximately 0.9 to 1.1 times the primary particle diameter calculated above were visually selected. Next, the constituent elements of the cross sections of the selected conductive particles were collected using an EDS analyzer to prepare EDS mapping images. The collection and analysis of the spectra were performed using an NSS (Thermo Fischer Scientific). The collection conditions were an acceleration voltage of 200 kV, a probe size of 1.0 nm or 1.5 nm appropriately selected so that the dead time was 15 to 30, a mapping resolution of 256 × 256, and 300 frames. EDS mapping images were obtained for 100 cross sections of conductive particles.
[0123] By analyzing the EDS mapping image obtained in this way, the ratio of the niobium atomic concentration (atomic %) to the titanium atomic concentration (atomic %) at the center of the particle and within 5% of the maximum diameter of the measured particle from the particle surface is calculated. Specifically, the "Line Extraction" button of the NSS is pressed first, a straight line is drawn to represent the maximum diameter of the particle, and information on the atomic concentration (atomic %) on the straight line from one surface through the inside of the particle to the other surface is obtained. If the maximum diameter of the particle obtained at this time is in the range of less than 0.9 times or more than 1.1 times the primary particle diameter calculated above, it is excluded from the subsequent analysis. (The analysis shown below was performed only on particles with a maximum diameter in the range of 0.9 times or more and less than 1.1 times the primary particle diameter.) Next, the niobium atomic concentration (atomic %) is read at the particle surface on both sides within 5% of the maximum diameter of the measured particle from the particle surface. In the same manner, the "titanium atomic concentration (atomic %) within 5% of the maximum diameter of the measured particle from the particle surface" is obtained. Next, using these values, the "concentration ratio of niobium atoms to titanium atoms within 5% of the maximum diameter of the measured particle from the particle surface" on both particle surfaces is calculated according to the following formula. Concentration ratio of niobium atoms to titanium atoms within 5% of the maximum diameter of the measured particle from the particle surface = (Niobium atomic concentration (atomic %) within 5% of the maximum diameter of the measured particle from the particle surface) / (Titanium atomic concentration (atomic %) within 5% of the maximum diameter of the measured particle from the particle surface) Of the two concentration ratios obtained, the smaller value is adopted as "the concentration ratio of niobium atoms to titanium atoms within 5% of the maximum diameter of the measured particle from the particle surface" in the present invention.
[0124] Also, the niobium atom concentration (atomic %) and titanium atom concentration (atomic %) are read at the position on the straight line that is the midpoint of the maximum diameter. Using these values, the "concentration ratio of niobium atoms to titanium atoms at the center of the particle" is calculated using the following formula. Concentration ratio of niobium atoms to titanium atoms in the particle center = (Niobium atom concentration at the center of the particle (atomic %)) / (Titanium atom concentration at the center of the particle (atomic %)) The "concentration ratio calculated as niobium atomic concentration / titanium atomic concentration at a portion 5% inside the maximum diameter of the measured particle from the particle surface to the concentration ratio calculated as niobium atomic concentration / titanium atomic concentration at the particle center" is calculated by the following formula. (Ratio of concentration of niobium atoms to titanium atoms within 5% of the maximum diameter of the measured particle from the particle surface) / (Ratio of concentration of niobium atoms to titanium atoms in the particle center)
[0125] <Calculation of conductive particle content> Next, four sample pieces of 5 mm square were cut out from the photoreceptor, and the protective layer was three-dimensionalized to 2 μm × 2 μm × 2 μm using FIB-SEM Slice & View. The particle content in the total volume of the protective layer was calculated from the difference in contrast of FIB-SEM Slice & View. In this example, the conditions for Slice & View were as follows. Analytical sample processing: FIB method Processing and observation equipment: SII / Zeiss NVision40 Slice interval: 10 nm Observation conditions: Acceleration voltage: 1.0 kV Sample tilt: 54° WD: 5mm Detector: BSE detector Aperture: 60μm, high current ABC:ON Image resolution: 1.25nm / pixel
[0126] The analysis area was 2 μm long x 2 μm wide, and the information for each cross section was integrated to obtain a 2 μm long x 2 μm wide x 2 μm thick (8 μm 3 The measurement environment is temperature: 23°C, pressure: 1×10 -4 Pa. As a processing and observation device, a Strata400S (sample inclination: 52°) manufactured by FEI can also be used. Information for each cross section was obtained by image analysis of the area of the identified conductive particles of the present invention. The image analysis was performed using image processing software: Image-Pro Plus manufactured by Media Cybernetics. Based on the obtained information, a volume of 2 μm × 2 μm × 2 μm (unit volume: 8 μm) was calculated for each of the four sample pieces. 3 The volume V of the conductive particles of the present invention in the sample was calculated. 3 / 8μm 3 × 100) was calculated. 3 / 8μm 3 × 100) was taken as the content [volume %] of the conductive particles of the present invention in the protective layer relative to the total volume of the protective layer. At this time, the thickness t (cm) of the protective layer was measured by processing all four sample pieces up to the boundary between the protective layer and the lower layer, and the value was used to calculate the volume resistivity ρv in the <Method for measuring the volume resistivity of the protective layer> described below.
[0127] <Quantitative Determination of Niobium Atoms Contained in Conductive Particles> The amount of niobium atoms contained in the conductive particles is determined as follows. The conductive particles collected from the photoconductor in the above <Calculation of the primary particle diameter of conductive particles> are pelletized by the press molding described below to prepare a sample. Using the prepared sample, measurement is performed with an X-ray fluorescence analyzer (XRF), and the niobium atom content of the entire conductive particles is quantified by the FP method. Specifically, the amount of niobium pentoxide is determined and converted into the amount of niobium atoms contained. (i) Example of equipment used: X-ray fluorescence analyzer 3080 (Rigaku Corporation) (ii) Sample preparation Samples are prepared using a sample press molding machine, MAEKAWA Testing Machine (manufactured by MFG Co, LTD.) 0.5 g of conductive particles are placed in an aluminum ring (model number: 3481E1), and the load is set to 5.0 tons. The sample is pressed for 1 minute to form a pellet. (iii) Measurement conditions Measurement diameter: 10φ Measurement potential, voltage 50kV, 50~70mA 2θ angle 25.12° Crystal plate LiF Measurement time: 60 seconds
[0128] <Powder X-ray diffraction measurement of conductive particles> A method for determining whether the conductive particles used in the electrophotographic photoreceptor of the present invention contain anatase type titanium oxide or rutile type titanium oxide will be described below. Identification is performed using the inorganic materials database (AtomWork) of the National Institute for Materials Science (NIMS) from a chart obtained by powder X-ray diffraction using CuKα X-rays. The conductive particles contained in the protective layer of the electrophotographic photoreceptor of the present invention are subjected to the above-mentioned process (quantitative determination of Nb atoms contained in the conductive particles) as an example. Measuring equipment used: Rigaku Electric Co., Ltd., X-ray diffraction device RINT-TTRII X-ray tube:Cu Tube voltage: 50KV Tube current: 300mA Scan method: 2θ / θ scan Scan speed: 4.0° / min Sampling interval: 0.02° Start angle (2θ): 5.0° Stop angle (2θ): 40.0° Attachment: Standard sample holder Filter: Not used Incident Monochrome:Use Counter monochromator: Not used Divergence slit: open Divergence vertical limit slit: 10.00mm Scattering slit: open Receiving slit: open Flat plate monochromator: Used Counter: Scintillation counter
[0129] <Method for measuring the volume resistivity of the surface protective layer> In the present invention, a picoampere meter (pA) was used to measure the volume resistivity. First, a gold comb-shaped electrode with an interelectrode distance (D) of 180 μm and a length (L) of 5.9 cm as shown in FIG. 3 was prepared by deposition on a PET film, and a surface protection layer with a thickness (T1) of 2 μm was provided on top of the electrode. Next, a direct current (I) was measured when a direct current voltage (V) of 100 V was applied between the comb-shaped electrodes in an environment of a temperature of 23° C. and a humidity of 50% RH, and the volume resistivity (temperature 23° C. / humidity 50% RH) was obtained by the following formula (7). Volume resistivity ρv(Ω cm)=V(V)×T1(cm)×L(cm) / {I(A)×D(cm)}(7)
[0130] When it is difficult to identify the composition of the conductive particles and binder resin of the surface protective layer, the surface resistivity of the surface of the electrophotographic photoreceptor is measured and converted to volume resistivity. When measuring the volume resistivity of the surface protective layer in a state in which it is coated on the surface of the photoreceptor, rather than the surface protective layer alone, it is desirable to measure the surface resistivity of the surface protective layer and convert it to volume resistivity from there. By measuring the DC current when a constant DC voltage is applied to a comb-shaped electrode that is gold-deposited on the surface protective layer in a state in which it is coated on the photoreceptor, the surface resistivity ρs can be calculated from the following formula (8). ρv=ρs×t (8) (t is the thickness of the charge injection layer)
[0131] In this measurement, since a minute amount of current is measured, it is preferable to use a resistance measuring device capable of measuring minute currents. For example, a picoammeter 4140B manufactured by Hewlett-Packard can be used. It is preferable to select the interdigital electrodes to be used and the voltage to be applied so that an appropriate signal-to-noise ratio is obtained according to the material and resistance value of the charge injection layer. In the present invention, comb-shaped gold electrodes with an interelectrode distance (D) of 180 μm and a length (L) of 5.9 cm are formed on the surface of an electrophotographic photoreceptor by deposition. Next, a direct current (I) is measured when a direct current voltage (V) of 1000 V is applied between the comb-shaped electrodes in an environment of temperature 23° C. / humidity 50% RH to obtain the surface resistivity ρs (temperature 23° C. / humidity 50% RH). Furthermore, the thickness T1 (cm) of the surface protection layer was measured by the above-mentioned <Calculation of the conductive particle content>. The volume resistivity ρv (temperature 23° C. / humidity 50% RH) was calculated by multiplying the surface resistivity ρs by the thickness T1 using the above formula.
[0132] <Method of measuring weight-average particle size (D4) and number-average particle size (D1) of toner particles> The weight average particle diameter (D4) and number average particle diameter (D1) of the toner particles are calculated as follows. The measurement device used is a precision particle size distribution measurement device using the pore electrical resistance method, "Coulter Counter Multisizer 3" (registered trademark, manufactured by Beckman Coulter, Inc.), equipped with a 100 μm aperture tube. The measurement conditions are set and the measurement data is analyzed using the accompanying dedicated software "Beckman Coulter Multisizer 3 Version 3.51" (manufactured by Beckman Coulter, Inc.). The measurement is performed with an effective measurement channel count of 25,000. The electrolyte solution used for the measurement is prepared by dissolving special grade sodium chloride in ion-exchanged water to a concentration of 1.0%, for example, "ISOTON II" (manufactured by Beckman Coulter, Inc.).
[0133] Before performing measurements and analysis, the dedicated software is set up as follows. In the "Change standard measurement method (SOMME)" screen of the dedicated software, set the total count number in the control mode to 50,000 particles, the number of measurements to 1, and the Kd value to the value obtained using "Standard particles 10.0 μm" (Beckman Coulter, Inc.). Press the "Threshold / Noise Level Measurement Button" to automatically set the threshold and noise level. Also, set the current to 1,600 μA, the gain to 2, the electrolyte to ISOTON II, and check "Flush aperture tube after measurement." In the "Pulse to particle size conversion setting" screen of the dedicated software, set the bin interval to logarithmic particle size, the particle size bin to 256 particle size bins, and the particle size range to 2 μm to 60 μm.
[0134] The specific measurement method is as follows. (1) Pour 200.0 mL of the electrolyte solution into a 250 mL round-bottom glass beaker made exclusively for the Multisizer 3, set it on the sample stand, and stir the stirrer rod counterclockwise at 24 revolutions per second. Then, remove dirt and air bubbles from inside the aperture tube using the "Aperture Tube Flush" function of the dedicated software. (2) 30.0 mL of the above electrolyte solution is placed in a 100 mL flat-bottom glass beaker, and 0.3 mL of a dilution of "Contaminon N" (a 10% aqueous solution of a neutral detergent for cleaning precision measuring instruments with a pH of 7, consisting of a nonionic surfactant, an anionic surfactant, and an organic builder, manufactured by Wako Pure Chemical Industries, Ltd.) diluted 3 times by mass with ion-exchanged water is added as a dispersant. (3) Prepare an ultrasonic disperser "Ultrasonic Dispersion System Tetra150" (manufactured by Nikkaki Bios Co., Ltd.) that has two built-in oscillators with an oscillation frequency of 50 kHz and a phase shift of 180 degrees and an electrical output of 120 W. Place 3.3 L of ion-exchanged water in the ultrasonic disperser's water tank and add 2.0 mL of Contaminon N to this tank. (4) The beaker (2) is set in the beaker fixing hole of the ultrasonic disperser, and the ultrasonic disperser is operated. Then, the height position of the beaker is adjusted so that the resonance state of the liquid surface of the electrolyte solution in the beaker is maximized. (5) While the electrolyte solution in the beaker in (4) is irradiated with ultrasonic waves, 10 mg of toner particles are added little by little to the electrolyte solution and dispersed. Then, ultrasonic dispersion treatment is continued for another 60 seconds. During ultrasonic dispersion, the water temperature in the water tank is appropriately adjusted to be 10°C or higher and 40°C or lower. (6) Using a pipette, the electrolyte solution (5) in which the toner particles are dispersed is dropped into the round-bottom beaker (1) placed in the sample stand, and the measurement concentration is adjusted to 5%. Then, measurements are continued until the number of particles measured reaches 50,000. (7) The measurement data is analyzed using the dedicated software that comes with the device, and the weight average particle size (D4) and number average particle size (D1) are calculated. Note that when the dedicated software is set to graph / volume %, the "average diameter" on the "analysis / volume statistics (arithmetic mean)" screen is the weight average particle size (D4), and when the dedicated software is set to graph / number %, the "average diameter" on the "analysis / number statistics (arithmetic mean)" screen is the number average particle size (D1).
[0135] <Measurement of the longest diameter of organosilicon polymer particles> A photograph of the surface of the toner particles was taken at a magnification of 30,000 times using an FE-SEMS-4800 (manufactured by Hitachi, Ltd.). The magnified photograph was used to measure the major axis of the organosilicon polymer particles, and those with a diameter of 30 nm or more and 300 nm or less were determined to be organosilicon polymers. Measurements were made on 100 or more toner particles, and the average value of the major axis of the organosilicon polymer particles was determined to be the major axis of the organosilicon polymer. It is also possible to handle toners that contain multiple types of external additives on the surface of the toner particles. When observing the backscattered electron image with the S-4800, it is possible to identify the elements of each particle using elemental analysis such as EDAX. It is also possible to select particles of the same type based on their shape characteristics. By performing the above measurements on particles of the same type, it is possible to calculate the major axis of each type of particle.
[0136] <Analysis method for organosilicon polymer particles or organosilicon polymer> solid 29In Si-NMR, peaks are detected in different shift regions depending on the structure of the functional group bonded to Si in the organosilicon polymer fine particles or the constituent compounds of the organosilicon polymer. The structure bonded to Si can be identified by identifying the position of each peak using a standard sample. In addition, the abundance ratio of each constituent compound can be calculated from the obtained peak area. This allows the area values of the peaks derived from the T3 unit structure, the T2 unit structure, and the T1 unit structure to be calculated. solid 29 Specifically, the Si-NMR measurement conditions are as follows: Equipment: JNM-ECX5002 (JEOL RESONANCE) Temperature: room temperature Measurement method: DDMAS method 29 Si 45° Sample tube: Zirconia 3.2mmφ Sample: Powdered material filled into test tube Sample rotation speed: 10kHz Relaxation delay: 180s Scan:2000
[0137] ( 13 C-NMR (solid state) measurement conditions solid 13 C-NMR (solid state) can be used to quantify the amount of alkyl groups and alkoxy groups bonded to silicon atoms in organosilicon polymer fine particles or in the constituent compounds of the organosilicon polymer. Equipment: JEOL RESONANCE JNM-ECX500II Sample tube: 3.2mmφ Sample: 150 mg of tetrahydrofuran insoluble matter obtained by the above preparation method Measurement temperature: room temperature Pulse mode: CP / MAS Measurement nuclear frequency: 123.25MHz (13C) Reference substance: Adamantane (external standard: 29.5ppm) Sample rotation speed: 20kHz Contact time: 2ms Delay time: 2s Number of times: 2000 to 8000 and, 29 Si-NMR results and 13 By combining this with the results of C-NMR, the amount of alkyl groups and alkoxy groups bonded to silicon atoms having each structure can be determined, and the amount of OH groups bonded can be calculated from the results. The mass ratio of alkoxysilane (-Si-OR) and silanol group (-Si-OH) is calculated based on the amount of alkoxy groups and OH groups bonded obtained. This makes it possible to determine the proportion of silanol structures relative to the total of alkoxysilane structures and silanol structures in the T1 unit structures or T2 unit structures in the organosilicon polymer particles or organosilicon polymer. Specifically, the "ratio of the content of silanol structures to the total content of alkoxysilane structures and silanol structures contained in the T1 unit structure or the T2 unit structure" is any one of A to D below: A = content of alkoxysilane structure in T1 unit structure B = the amount of silanol structures contained in the T1 unit structure C=Alkoxysilane structure content in T2 unit structure D = the amount of silanol structures contained in the T2 unit structure When expressed using (B+C) / (A+B+C+D)×100 It is best to be able to completely quantify the amount, but even if it is difficult to quantify the amount, it is possible to calculate the amount if the ratio of each can be obtained. In that case, the "content" in the above formula can be calculated as the "content ratio".
[0138] <Method for measuring adhesion rate of organosilicon polymer fine particles or silica fine particles to toner particles by water washing method> (Water washing process) 20 g of "Contaminon N" (a 30% by weight aqueous solution of a neutral detergent for cleaning precision measuring instruments, consisting of a nonionic surfactant, anionic surfactant, and organic builder, with a pH of 7) is weighed out into a 50 mL vial and mixed with 1 g of toner. The vial is then placed in a "KM Shaker" (model: V.SX) manufactured by Iwaki Sangyo Co., Ltd., and shaken for 120 seconds at a speed of 50. Depending on the adhesion state of the organosilicon polymer fine particles or silica fine particles, this causes the organosilicon polymer fine particles to migrate from the surface of the toner particles to the dispersion liquid side. The mixture is then centrifuged in a centrifuge (H-9R; manufactured by Kokusan Co., Ltd.) (16.67 S -1 The toner is separated from the organosilicon polymer fine particles or silica fine particles that have migrated to the supernatant by vacuum drying (40°C / 24 hours) to dry the precipitated toner, leaving the washed toner. Next, a Hitachi ultra-high resolution field emission scanning electron microscope S-4800 (Hitachi High-Technologies Corporation) is used to photograph the toner that has not been subjected to the above washing process (toner before washing) and the toner obtained through the above washing process (toner after washing). The photographed toner surface images are then analyzed using image analysis software Image-Pro Plus ver. 5.0 (Nippon Roper Co., Ltd.) to calculate the coverage rate.
[0139] The imaging conditions for the S-4800 are as follows: (1) Sample preparation Apply a thin layer of conductive paste to a sample stage (aluminum sample stage 15 mm x 6 mm) and spray toner onto it. Then use air to remove excess toner from the sample stage and dry thoroughly. Set the sample stage in the sample holder and adjust the sample stage height to 36 mm using the sample height gauge.
[0140] (2) S-4800 observation condition setting When measuring the coverage rate, elemental analysis by the above-mentioned energy dispersive X-ray analysis (EDS) is carried out in advance to distinguish between the organosilicon polymer fine particles and the silica fine particles on the surface of the toner particles, and then the measurement is carried out. Pour liquid nitrogen into the anti-contamination trap attached to the S-4800 housing until it overflows, and leave it for 30 minutes. Start the S-4800's "PC-SEM" and perform flushing (cleaning the FE chip, which is the electron source). Click the accelerating voltage display area on the control panel on the screen, and press the [Flushing] button to open the flushing execution dialog. Check that the flushing intensity is 2, and execute it. Check that the emission current due to flushing is 20 to 40 μA. Insert the sample holder into the sample chamber of the S-4800 housing. Press [Origin] on the control panel to move the sample holder to the observation position. Click the accelerating voltage display to open the HV setting dialog, and set the accelerating voltage to [1.1kV] and the emission current to [20μA]. In the [Basic] tab of the operation panel, set the signal selection to [SE], select the SE detector to [Upper (U)] and [+BSE], select [LA100] in the [+BSE] selection box, and set the mode to observation with backscattered electron images. In the same [Basic] tab of the operation panel, set the probe current in the electron optical system condition block to [Normal], the focus mode to [UHR], and the WD to [4.5mm]. Press the [ON] button in the accelerating voltage display on the control panel to apply the accelerating voltage.
[0141] (3) Calculation of the number-average particle size (D1) of toner Drag within the magnification display area on the control panel to set the magnification to 5000 (5k). Rotate the focus knob [COARSE] on the operation panel to adjust the aperture alignment once the image is in focus to a certain extent. Click [Align] on the control panel to display the alignment dialog and select [Beam]. Rotate the STIGMA / ALIGNMENT knobs (X, Y) on the operation panel to move the displayed beam to the center of the concentric circles. Next, select [Aperture] and rotate the STIGMA / ALIGNMENT knobs (X, Y) one by one to stop the image movement or adjust it so that it moves as little as possible. Close the aperture dialog and use autofocus to adjust the focus. Repeat this operation two more times to adjust the focus. After that, measure the particle size of 300 toner particles to obtain the number average particle size (D1). The particle size of each particle is the maximum diameter when the toner particles are observed.
[0142] (4) Focus adjustment For the particles with a number-average particle size (D1) of ±0.1 μm obtained in (3), set the magnification to 10,000 (10k) by dragging within the magnification display area of the control panel while aligning the midpoint of the maximum diameter with the center of the measurement screen. Rotate the focus knob [COARSE] on the operation panel, and adjust the aperture alignment once the image is in focus to a certain extent. Click [Align] on the control panel to display the alignment dialog, and select [Beam]. Rotate the STIGMA / ALIGNMENT knobs (X, Y) on the operation panel to move the displayed beam to the center of the concentric circles. Next, select [Aperture] and rotate the STIGMA / ALIGNMENT knobs (X, Y) one by one to stop the image movement or adjust it so that it moves as little as possible. Close the aperture dialog and use autofocus to adjust the focus. After that, set the magnification to 50,000 (50k) times, adjust the focus using the focus knob and STIGMA / ALIGNMENT knob as above, and use autofocus to focus again. Repeat this operation to adjust the focus. Here, if the tilt angle of the observation surface is large, the measurement accuracy of the coverage rate is likely to be low, so when adjusting the focus, select one where the entire observation surface is in focus at the same time, and select one with as little surface tilt as possible for analysis.
[0143] (5) Image storage Adjust the brightness in ABC mode, take a photo with a size of 640 x 480 pixels, and save it. Use this image file to perform the following analysis. Take one photo for each toner, and obtain images for 25 toner particles.
[0144] (6) Image analysis The image obtained by the above method is binarized using the following analysis software to calculate the coverage. At this time, the above screen is divided into 12 squares and each is analyzed. The analysis conditions for the image analysis software Image-Pro Plus ver.5.0 are as follows. However, if the divided section contains organosilicon polymer fine particles with a particle size of less than 30 nm and more than 300 nm (when measuring the coverage of organosilicon polymer fine particles), or silica fine particles with a particle size of less than 100 nm and more than 300 nm (when measuring the coverage of silica fine particles), the coverage of that section is not calculated. From the "Measurement" menu on the Image-ProPlus5.1J software toolbar, select "Count / Size" and then "Options" to set the binarization conditions. Select 8-connected in the object extraction options and set smoothing to 0. In addition, do not select pre-sort, fill holes, or enclosing lines, and set "Exclude borders" to "None." From the "Measurement" menu on the toolbar, select "Measurement item" and enter 2 to 107 in the selection range for area. The coverage rate is calculated by enclosing a square region. In this case, the area of the region (C) should be 24,000 to 26,000 pixels. Automatic binarization is performed using "Processing" - Binarization, and the total area of regions without organosilicon polymer microparticles or silica microparticles (D) is calculated. The coverage rate can be calculated using the following formula from the area C of the square region and the total area D of regions without organosilicon polymer microparticles or silica microparticles. Coverage rate (%)=100-(D / C×100) The arithmetic average of all the data obtained is taken as the coverage rate. Then, the coverage rates of the toner before and after washing are calculated, [Toner coverage after washing] / [Toner coverage before washing] x 100 is defined as the "sticking rate" in the present invention.
[0145] <Method for measuring average circularity> The average circularity of toner particles is measured using a flow-type particle image analyzer "FPIA-3000" (manufactured by Sysmex Corporation) under the measurement and analysis conditions during the calibration work. The specific measurement method is as follows. First, about 20 ml of ion-exchanged water from which impurities such as solids have been removed in advance is placed in a glass container. About 0.2 ml of a dilution solution obtained by diluting "Contaminon N" (a 10% aqueous solution of a pH 7 neutral detergent for cleaning precision measuring instruments made of nonionic surfactants, anionic surfactants, and organic builders, manufactured by Wako Pure Chemical Industries, Ltd.) about 3 times by mass with ion-exchanged water is added as a dispersant. About 0.02 g of the measurement sample is further added, and the dispersion process is performed for 2 minutes using an ultrasonic disperser to obtain the dispersion for measurement. At this time, the dispersion is appropriately cooled so that the temperature of the dispersion is between 10°C and 40°C. As the ultrasonic disperser, a tabletop ultrasonic cleaner disperser (e.g., "VS-150" (manufactured by Vervoclear)) with an oscillation frequency of 50 kHz and an electric output of 150 W is used, a predetermined amount of ion-exchanged water is placed in the water tank, and about 2 ml of the Contaminon N is added to the water tank. For the measurement, the flow type particle image analyzer equipped with "UPlanApro" (magnification 10 times, numerical aperture 0.40) is used as the objective lens, and the particle sheath "PSE-900A" (manufactured by Sysmex Corporation) is used as the sheath liquid. The dispersion liquid adjusted according to the above procedure is introduced into the flow type particle image analyzer, and 3000 toner particles are measured in HPF measurement mode and total count mode. Then, the binarization threshold during particle analysis is set to 85%, and the analyzed particle diameter is limited to a circle equivalent diameter of 1.985 μm or more and less than 39.69 μm, and the average circularity of the toner particles is obtained. Before starting the measurement, automatic focus adjustment is performed using standard latex particles (e.g., Duke Scientific's "RESEARCH AND TEST PARTICLES Latex Microsphere Suspensions 5200A" diluted with ion-exchanged water). After that, focus adjustment is performed every 2 hours from the start of the measurement.
[0146] (Production Examples of Anatase-Type Titanium Oxide Particles 1 to 7) A solution containing titanyl sulfate was heated to hydrolyze the solution and produce a hydrous titanium dioxide slurry, which was then dehydrated and fired to obtain anatase-type titanium dioxide particles. The number-average particle size of the anatase-type titanium dioxide particles was controlled by controlling the titanyl sulfate solution concentration, and anatase-type titanium dioxide particles 1 to 7 shown in Table 1 were obtained.
[0147] [Table 1]
[0148] <Production of conductive particles> (Production of Conductive Particles 1) 100 g of anatase-type titanium oxide particles 1 were dispersed in water, and heated to 60°C to form a 1L aqueous suspension. A titanium niobate solution (the weight ratio of niobium atoms to titanium atoms in the solution was 1.0 / 33.7) was mixed with 600 mL of titanium sulfate solution containing 33.7 g of titanium, and a 10.7 mol / L aqueous sodium hydroxide solution was added dropwise (parallel addition) over 3 hours so that the pH of the suspension was 2 to 3. After the dropwise addition was completed, the suspension was filtered, washed, and dried at 110°C for 8 hours. This dried product was heated (calcined) at 800°C for 1 hour in an air atmosphere to obtain niobium atom-containing titanium oxide particles 1. next, Niobium-containing titanium oxide particles 1 100.0 parts Surface treatment agent 1 (formula (S-1) below) (product name: KBM-3033, manufactured by Shin-Etsu Chemical Co., Ltd.) 3.0 parts [ka] Toluene 200.0 parts These were mixed and stirred for 4 hours with a stirrer, then filtered, washed, and further heat-treated at 130° C. for 3 hours to obtain conductive particles 1. The surface properties and particle size of the conductive particles are shown in Table 2.
[0149] (Production of conductive particles 2 to 9 and 14) In the production of conductive particle 1, the type of core material used, the concentration and amount of the titanium niobate liquid, and the coating conditions were appropriately changed. Otherwise, powders of conductive particles 2 to 9 and 14 were obtained in the same manner as in the production of conductive particle 1. The contents in Table 2 are the contents of niobium atoms in the niobium atom-containing titanium oxide particles, and are values obtained by measurement using X-ray fluorescence elemental analysis (XRF). Conductive particle 9 is the same as anatase type titanium oxide particle 7.
[0150] (Production of conductive particles 10) The following materials were prepared: Tin oxide particles (product name: S-2000, manufactured by Mitsubishi Materials Corporation) 100.0 parts Surface treatment agent 2 (formula (S-2) below) (trade name: decyltrimethoxysilane, manufactured by Tokyo Chemical Industry Co., Ltd.) 20.0 parts Toluene 200.0 parts These were mixed and stirred for 4 hours in a stirrer, then filtered and washed, and then further heat-treated at 130° C. for 3 hours for surface treatment. The surface properties and particle diameter of the conductive particles are shown in Table 2. [ka]
[0151] (Production of conductive particles 11) Approximately spherical anatase type titanium dioxide particles 8 having a number average particle size of 6 nm and a niobium atom content of 0.50 mass % were used as the conductive particles 11. The physical properties of the conductive particles 11 are shown in Table 2.
[0152] (Production of conductive particles 12) In the production of conductive particles 1, the core material used was an approximately spherical anatase type titanium oxide 9 with a number average particle size of 150 nm and a niobium atom content of 0.20 mass %, and the coating conditions in the production of conductive particles 1 were changed. The rest of the process was the same as in the production of conductive particles 1. The physical properties of conductive particles 12 are shown in Table 2.
[0153] (Production of conductive particles 13) Niobium sulfate (a water-soluble niobium compound) was added to a titanium dioxide hydrous slurry obtained by hydrolysis of an aqueous titanyl sulfate solution. The amount of niobium sulfate added was 0.2% by mass as niobium ions relative to the amount of titanium in the slurry (converted to titanium dioxide). A titanium dioxide hydrous slurry was obtained by hydrolyzing an aqueous titanyl sulfate solution to which niobium sulfate was added at a ratio of 0.2% by mass as niobium ions. Next, the titanium dioxide hydrous slurry containing niobium ions and the like was dehydrated and fired at a firing temperature of 1000°C. As a result, anatase-type titanium dioxide particles 10 having a number-average particle size of 130 nm and containing 0.2% by mass of niobium atoms were obtained. 100 g of spherical anatase-type titanium oxide particles 10 with a number-average particle size of 130 nm and a concentration of 0.2 wt % were dispersed in water to prepare 1 L of water suspension, which was then heated to 60° C. A titanic acid solution mixed with 600 mL of titanium sulfate solution containing 33.7 g of titanium and a 10.7 mol / L sodium hydroxide solution were simultaneously dropped (added in parallel) over a period of 3 hours so that the pH of the suspension became 2 to 3. After the dropping was completed, the suspension was filtered, washed, and dried at 110° C. for 8 hours. The dried product was subjected to a heat treatment at 800° C. for 1 hour in an air atmosphere. As a result, conductive particles 13 were obtained. The physical properties of the conductive particles 13 are shown in Table 2.
[0154] [Table 2] In the table, A is the "concentration ratio of niobium atoms to titanium atoms within 5% of the maximum diameter of the measured particle from the particle surface," and B is the "concentration ratio of niobium atoms to titanium atoms in the particle center."
[0155] [Electrophotographic Photoreceptor Manufacturing Example 1] An aluminum cylinder (JIS-A3003, aluminum alloy) having a diameter of 24 mm and a length of 257.5 mm was used as a support (conductive support).
[0156] (Conductive Layer Manufacturing Example 1) Next, the following materials were prepared: 214 parts of titanium oxide (TiO2) particles (volume average particle size 230 nm) coated with oxygen-deficient tin oxide (SnO2) as metal oxide particles Phenolic resin as a binder (phenolic resin monomer / oligomer) (product name: Plyofen J-325, manufactured by Dainippon Ink and Chemicals, Inc., resin solid content: 60% by mass) 132 parts 98 parts of 1-methoxy-2-propanol as solvent These were placed in a sand mill using 450 parts of glass beads with a diameter of 0.8 mm, and dispersion treatment was carried out under the conditions of a rotation speed of 2000 rpm, a dispersion treatment time of 4.5 hours, and a cooling water temperature setting of 18° C., to obtain a dispersion liquid. The glass beads were removed from this dispersion liquid using a mesh (mesh opening: 150 μm). Silicone resin particles (trade name: Tospearl 120, manufactured by Momentive Performance Materials, Inc., average particle size 2 μm) were added to the obtained dispersion as a surface roughening agent. The amount of silicone resin particles added was 10 mass% of the total mass of the metal oxide particles and binding material in the dispersion after removing the glass beads. In addition, silicone oil (trade name: SH28PA, manufactured by Dow Corning Toray Co., Ltd.) was added as a leveling agent to the dispersion so that the amount was 0.01 mass% of the total mass of the metal oxide particles and binding material in the dispersion. Next, a mixed solvent of methanol and 1-methoxy-2-propanol (mass ratio 1:1) was added to the dispersion so that the total mass of the metal oxide particles, the binder material, and the surface roughening agent in the dispersion (i.e., the mass of the solid content) was 67 mass% relative to the mass of the dispersion. Then, the mixture was stirred to prepare a coating liquid for a conductive layer. The coating liquid for a conductive layer was dip-coated on a support and heated at 140°C for 1 hour to form a conductive layer with a thickness of 30 μm.
[0157] (Preparation Example 1 of Undercoat Layer) Next, the following materials were prepared: 3.11 parts of an electron transport material represented by the following formula (E-1): Blocked isocyanate (product name: Duranate SBB-70P, manufactured by Asahi Kasei Chemicals Corporation) 6.49 parts Styrene-acrylic resin (product name: UC-3920, manufactured by Toagosei) 0.4 parts ·1.8 parts of silica slurry (product name: IPA-ST-UP, manufactured by Nissan Chemical Industries, solid content concentration: 15% by mass, viscosity: 9mPa·s) These were dissolved in a mixed solvent of 48 parts of 1-butanol and 24 parts of acetone to prepare a coating solution for an undercoat layer. The coating solution for an undercoat layer was dip-coated onto the conductive layer, and heated at 170° C. for 30 minutes to form an undercoat layer with a thickness of 0.7 μm. [ka] Next, 10 parts of hydroxygallium phthalocyanine in a crystalline form having peaks at 7.5° and 28.4° in a chart obtained by CuKα characteristic X-ray diffraction and 5 parts of polyvinyl butyral resin (product name: S-LEC BX-1, manufactured by Sekisui Chemical Co., Ltd.) were prepared. These were added to 200 parts of cyclohexanone and dispersed for 6 hours using a sand mill device using glass beads with a diameter of 0.9 mm. This was further diluted with 150 parts of cyclohexanone and 350 parts of ethyl acetate to obtain a coating liquid for a charge generating layer. The obtained coating liquid was dip-coated on the undercoat layer and dried at 95°C for 10 minutes to form a charge generating layer with a film thickness of 0.20 μm.
[0158] The X-ray diffraction measurements were carried out under the following conditions. [Powder X-ray diffraction measurement] Measuring equipment used: Rigaku Electric Co., Ltd., X-ray diffraction device RINT-TTRII X-ray tube: Cu Tube voltage: 50KV Tube current: 300mA Scan method: 2θ / θ scan Scan speed: 4.0° / min Sampling interval: 0.02° Start angle (2θ): 5.0° Stop angle (2θ): 40.0° Attachment: Standard sample holder Filter: Not used Incident Monochrome:Use Counter monochromator: Not used Divergence slit: open Divergence vertical limit slit: 10.00mm Scattering slit: open Receiving slit: open Flat plate monochromator: Used Counter: Scintillation counter
[0159] (Photosensitive Layer Production Example 1) Next, the following materials were prepared: 6 parts of a charge transport material (hole transport material) represented by the following formula (C-1): Three parts of a charge transport material (hole transport material) represented by the following formula (C-2): One part of a charge transport material (hole transport material) represented by the following formula (C-3): Polycarbonate (product name: Iupilon Z400, manufactured by Mitsubishi Engineering Plastics Co., Ltd.) 10 parts 0.02 parts of polycarbonate resin having copolymer units of the following formula (C-4) and the following formula (C-5) (x / y=0.95 / 0.05: viscosity average molecular weight=20000) These were dissolved in a mixed solvent of 25 parts of orthoxylene, 25 parts of methyl benzoate, and 25 parts of dimethoxymethane to prepare a coating solution for the charge transport layer. The coating solution for the charge transport layer was dip-coated onto the charge generating layer to form a coating film, and the coating film was dried at 120°C for 30 minutes to form a charge transport layer with a thickness of 12 μm. [ka] [ka] [ka] [ka] [ka]
[0160] (Surface protection layer manufacturing example 1) Next, the following materials were prepared: 100.0 parts of a compound represented by the following structural formula (O-1) as a binder resin Conductive particles 1: 100.0 parts of the above surface-treated niobium atom-containing titanium oxide particles These were mixed in a mixed solvent of 100 parts 1-propanol / 100 parts cyclohexane, and stirred with a stirrer for 6 hours. In this way, a coating solution for a surface protective layer was prepared. This coating solution for a surface protective layer was dip-coated on the charge transport layer to form a coating film, and the resulting coating film was dried at 50°C for 6 minutes. Thereafter, the coating film was irradiated with an electron beam for 1.6 seconds under a nitrogen atmosphere, while rotating the support (irradiated body) at a speed of 300 rpm under conditions of an acceleration voltage of 70 kV and a beam current of 5.0 mA. The dose at the surface protective layer position was 15 kGy. Thereafter, in a nitrogen atmosphere, the temperature of the coating film was raised to 117° C. The oxygen concentration from the electron beam irradiation to the subsequent heat treatment was 10 ppm. Next, the coating film was naturally cooled in the atmosphere until the temperature of the coating film reached 25° C., and then heat treatment was performed for 1 hour under conditions such that the temperature of the coating film reached 120° C., thereby forming a surface protective layer with a thickness of 2 μm. In this manner, the electrophotographic photoreceptor 1 was produced. [ka]
[0161] (Electrophotographic Photoreceptor Manufacturing Examples 2 to 20, 24, and 25) Electrophotographic photoreceptors 2 to 20, 24, and 25 were produced in the same manner as in Electrophotographic Photoreceptor Production Example 1, except that the type of conductive particles and the number of conductive particles added in the surface protective layer were appropriately changed, so that the volume resistivity of the surface protective layer and the content (volume %) of the conductive particles in the protective layer were as shown in Table 3.
[0162] (Electrophotographic Photoreceptor Manufacturing Example 21) A coating solution for a surface protective layer was prepared as follows: First, the following materials were prepared. As a binder resin, 100.0 parts of radical polymerizable monomer (product name: TMPTA, manufactured by Tokyo Chemical Industry Co., Ltd.) 50.0 parts of a compound represented by the following formula (H-1) 1.5 parts of a compound represented by the following formula (H-2) 1.5 parts of a compound represented by the following formula (H-3) Fluoropolymer particles (product name: MPE-056, manufactured by Mitsui DuPont Fluorochemicals Co., Ltd.) 15.0 parts Photopolymerization initiator (product name: Irgacure 184, manufactured by BASF Japan Ltd.) 7.5 parts [ka] [ka] [ka] These were mixed with 1000 parts of tetrahydrofuran and stirred with a stirrer for 6 hours to prepare a coating solution for surface protective layer. This coating solution for surface protective layer was applied to the charge transport layer by spray coating in a nitrogen gas flow to form a coating film, which was then left in the nitrogen gas flow for 10 minutes and dried to the touch. After that, ultraviolet irradiation was performed under the following conditions in an ultraviolet light irradiation booth in which the inside of the booth was replaced with nitrogen gas so that the oxygen concentration was 2% or less. Metal halide lamp: 160W / cm Irradiation distance: 120mm Irradiation intensity: 700mW / cm 2 Irradiation time: 60 seconds Furthermore, the coating was dried at 130° C. for 20 minutes to form a surface protective layer with a thickness of 5 μm. Except for the above, the same procedure as in Example 1 was carried out to obtain an electrophotographic photoreceptor 21.
[0163] (Electrophotographic Photoreceptor Manufacturing Example 22) Electrophotographic photoreceptor 22 was obtained in the same manner as in electrophotographic photoreceptor manufacturing example 21, except that in preparing the coating liquid for the surface protective layer, the number of parts added was changed so that the content of the conductive particles was 42.0% of the total volume of the surface protective layer.
[0164] (Electrophotographic Photoreceptor Manufacturing Example 23) Conductive particles 11 100.0 parts 100.0 parts of a compound represented by the following formula (H-7) Polymerization initiator (1-hydroxycyclohexyl(phenyl)methanone) 10 parts These were mixed with 400.0 parts of n-propyl alcohol and dispersed for 2 hours with a sand mill to prepare a coating solution for a protective layer. An electrophotographic photoreceptor was produced in the same manner as in Production Example 21 of an electrophotographic photoreceptor, except that this coating solution for a protective layer was used, to obtain an electrophotographic photoreceptor 23. [ka]
[0165] [Table 3]
[0166] <Toner manufacturing example> <Production Example of Toner Base Particle Dispersion> <Toner base particle dispersion 1> 11.2 parts of sodium phosphate (12-hydrate) was added to a reaction vessel containing 390.0 parts of ion-exchanged water, and the mixture was kept at 65°C for 1.0 hours while purging with nitrogen. The mixture was stirred at 12000 rpm using a TK homomixer (manufactured by Tokushu Kika Kogyo Co., Ltd.). While maintaining the stirring, an aqueous calcium chloride solution in which 7.4 parts of calcium chloride (2-hydrate) was dissolved in 10.0 parts of ion-exchanged water was added to the reaction vessel all at once to prepare an aqueous medium containing a dispersion stabilizer. Furthermore, 1.0 mol / L of hydrochloric acid was added to the aqueous medium in the reaction vessel to adjust the pH to 6.0, and aqueous medium 1 was prepared.
[0167] (Preparation of Polymerizable Monomer Composition) Styrene 60.0 parts ·CIPigment Blue15:3 6.5 copies The above materials were placed in an attritor (manufactured by Nippon Coke & Engineering Co., Ltd.), and further dispersed using zirconia particles having a diameter of 1.7 mm at 220 rpm for 5.0 hours to prepare a colorant dispersion in which the pigment was dispersed. The following materials were then added to the colorant dispersion: Styrene 10.0 parts 30.0 parts n-butyl acrylate Polyester resin 5.0 parts (condensation polymer of terephthalic acid and 2 moles of propylene oxide adduct of bisphenol A, weight average molecular weight Mw=10000, acid value: 8.2mgKOH / g) Release wax: HNP9 (melting point: 76°C, manufactured by Nippon Seiro Co., Ltd.) 5.0 parts Plastic wax: 10.0 parts ethylene glycol distearate The above materials were kept at 65° C. and uniformly dissolved and dispersed at 500 rpm using a TK homomixer to prepare a polymerizable monomer composition.
[0168] (granulation process) While maintaining the temperature of the aqueous medium 1 at 70° C. and the rotation speed of the stirring device at 12,500 rpm, the polymerizable monomer composition was charged into the aqueous medium 1, and 8.0 parts of t-butyl peroxypivalate as a polymerization initiator was added. Granulation was continued for 10 minutes while maintaining the stirring device at 12,500 rpm.
[0169] (Polymerization process) The high-speed stirring device was changed to a stirrer equipped with a propeller stirring blade, and polymerization was carried out for 5.0 hours while maintaining 70°C with stirring at 200 rpm, and then the temperature was raised to 85°C and heated for 2.0 hours to carry out the polymerization reaction. The temperature was then raised to 98°C and heated for 3.0 hours to remove residual monomers, and ion-exchanged water was added to adjust the toner base particle concentration in the dispersion to 30.0%, obtaining toner base particle dispersion 1 in which toner base particles 1 are dispersed.
[0170] <Preparation of organosilicon polymer particles> Organosilicon polymerized microparticles 1 were prepared by the following procedure. In the first step, 360 parts of water was placed in a reaction vessel equipped with a thermometer and a stirrer, and 17 parts of hydrochloric acid with a concentration of 5.0% by mass was added to obtain a homogeneous solution. 136 parts of methyltrimethoxysilane was added while stirring at a temperature of 25°C, and the mixture was stirred for 5 hours, and then filtered to obtain a transparent reaction liquid containing a silanol compound or a partial condensate thereof. In the second step, 540 parts of water was placed in a reaction vessel equipped with a thermometer, agitator, and a dropping device, and 19 parts of 10.0% by weight ammonia water was added to obtain a homogeneous solution. While stirring at a temperature of 30°C, 100 parts of the reaction liquid obtained in the first step was dropped over 0.60 hours, and the mixture was stirred for 6 hours to obtain a suspension. The suspension was centrifuged to precipitate and remove the fine particles, and then dried in a dryer at a temperature of 180°C for 24 hours to obtain organosilicon polymer particles 1.
[0171] <Preparation of organosilicon polymer fine particles 2-11> Organosilicon polymer fine particles 2 to 11 were obtained in the same manner as in the preparation of organosilicon polymer fine particles 1, except that the parts used were as shown in Table 4 and the production conditions were changed as shown in Table 4.
[0172] [Table 4]
[0173] <Toner particle manufacturing example> <Toner particle 1> The pH of the toner base particle dispersion 1 was adjusted to 1.5 with 1 mol / L hydrochloric acid, and the mixture was stirred for 1.0 hour, and then the mixture was washed with ion-exchanged water, filtered, and dried. The obtained powder was classified with an air classifier to obtain toner particles 1. The toner particles 1 had a number average particle size (D1) of 6.2 μm, a weight average particle size (D4) of 6.7 μm, and an average circularity of 0.985.
[0174] <Toner particles 2> The following materials were weighed, mixed and dissolved: Styrene 70.0 parts 25.1 parts n-butyl acrylate Acrylic acid 1.3 parts Hexanediol diacrylate 0.4 parts n-Lauryl mercaptan 3.2 parts A 10% aqueous solution of NEOGEN RK (manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) was added to this solution and dispersed, and an aqueous solution of 0.15 parts of potassium persulfate dissolved in 10.0 parts of ion-exchanged water was added while slowly stirring for another 10 minutes. After replacing with nitrogen, emulsion polymerization was carried out for 6.0 hours at a temperature of 70° C. After the polymerization was completed, the reaction liquid was cooled to room temperature, and ion-exchanged water was added to obtain a resin particle dispersion liquid with a solid content concentration of 12.5% and a number average particle size of 0.2 μm.
[0175] The following materials were weighed and mixed: Release wax: HNP9 (melting point: 76°C, manufactured by Nippon Seiro Co., Ltd.) 15.0 parts Plastic wax: 45.0 parts ethylene glycol distearate Ionic surfactant Neogen RK (manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) 2.0 parts 240.0 parts of ion-exchanged water The above was heated to 100°C and thoroughly dispersed using an IKA Ultra Turrax T50, and then the mixture was heated to 115°C using a pressure discharge type Gaulin homogenizer and dispersed for 1 hour to obtain a release agent particle dispersion with a volume average particle size of 150 nm and a solid content of 20%.
[0176] The following materials were weighed and mixed: ·CIPigment Blue15:3 45.0 copies · 5.0 parts of Neogen RK Ion-exchanged water 190.0 parts The above components were mixed and dispersed for 10 minutes using a homogenizer (IKA Ultra Turrax), and then dispersed for 20 minutes at a pressure of 250 MPa using an Ultimizer (opposed collision type wet grinder: Sugino Machine Ltd.) to obtain a colorant particle dispersion having a volume average particle size of 120 nm and a solid content of 20%.
[0177] ·Resin particle dispersion liquid 160.0 parts Wax particle dispersion 33.4 parts Colorant particle dispersion 14.4 parts Magnesium sulfate 0.3 parts The above materials were dispersed using a homogenizer (IKA), and then heated to 65°C while stirring. After stirring at 65°C for 1.0 hour, it was confirmed by observation with an optical microscope that aggregate particles with a number-average particle size of 6.0 μm had been formed. After adding 2.5 parts of NEOGEN RK (Dai-ichi Kogyo Seiyaku Co., Ltd.), the temperature was raised to 80°C and stirred for 2.0 hours to obtain fused colored resin particles.
[0178] After cooling, the mixture was filtered, and the solid matter separated was washed with 2500.0 parts of ion-exchanged water by stirring for 1.0 hour. The dispersion liquid containing the colored resin was filtered and then dried. The obtained powder was classified by an air classifier to obtain toner particles 2. The number average particle size (D1) of toner particles 2 was 6.2 μm, and the weight average particle size (D4) was 6.7 μm.
[0179] <Toner particles 3> Binder resin: styrene-n-butyl acrylate copolymer: 100.0 parts (styrene-n-butyl acrylate copolymer ratio = 70:30, Mp = 22000, Mw = 35000, Mw / Mn = 2.4 ·CIPigment Blue15: 6.5 copies Amorphous polyester resin (condensation product of terephthalic acid and propylene oxide modified bisphenol A, Mw: 7800, Tg: 70°C, acid value 8.0mgKOH / g): 5.0 parts Release wax: HNP9 (melting point: 76°C, manufactured by Nippon Seiro Co., Ltd.) 5.0 parts Plastic wax: 10.0 parts ethylene glycol distearate The above materials were premixed in an FM mixer (manufactured by Nippon Coke and Engineering Co., Ltd.), and then melt-kneaded in a twin-screw kneader (PCM-30 model, manufactured by Ikegai Iron Works, Ltd.) to obtain a kneaded mixture. The kneaded mixture obtained was cooled, coarsely pulverized in a hammer mill (manufactured by Hosokawa Micron Corporation), and then pulverized in a mechanical pulverizer (T-250, manufactured by Turbo Kogyo Co., Ltd.) to obtain a finely pulverized powder. The finely pulverized powder obtained was classified using a multi-division classifier (EJ-L-3 model, manufactured by Nittetsu Mining Co., Ltd.) that utilizes the Coanda effect, to obtain toner particles 3. The number-average particle size (D1) of toner particles 3 was 6.2 μm, and the weight-average particle size (D4) was 6.7 μm.
[0180] <Toner Production Example 1> 100 parts of toner particles 1 and 2.0 parts of organosilicon polymer fine particles 1 were mixed for 5 minutes in a Henschel mixer (manufactured by Mitsui Miike Chemical Engineering Co., Ltd.) to obtain toner 1. The jacket temperature of the Henschel mixer was set to 10° C., and the peripheral speed of the rotating blades was set to 38 m / sec.
[0181] <Toner Production Examples 2 to 13, 16, and 17> In Toner Production Example 1, except that the type of toner particles and the organosilicon polymer fine particles were changed according to Table 5, the same production as for Toner 1 was carried out to obtain Toners 2 to 13, and Toners 16 and 17.
[0182] <Toner Production Example 14> <Production example of organosilicon compound liquid 1> 70.0 parts of ion-exchanged water Methyltriethoxysilane 30.0 parts The above materials were weighed into a 200 mL beaker, and the pH was adjusted to 3.5 with 10% hydrochloric acid. After that, the mixture was stirred for 1.0 hour while controlling the temperature at 30° C. in a water bath, to prepare organosilicon compound liquid 1. The following samples were weighed and placed in a reaction vessel, and mixed using a propeller agitator. Toner base particle dispersion 1 500.0 parts Organosilicon compound liquid 1 35.0 parts Next, the pH of the resulting mixture was adjusted to 6.0 using 1 mol / L NaOH aqueous solution, and the temperature of the mixture was adjusted to 50°C, and the mixture was held for 1.0 hour while being mixed using a propeller stirring blade. Thereafter, the pH of the mixture was adjusted to 9.5 using 1 mol / L NaOH aqueous solution, and the mixture was held for 4.0 hours. After the temperature was lowered to 25°C, the pH was adjusted to 1.5 using 1 mol / L hydrochloric acid, and the mixture was stirred for 1.0 hour, and then the mixture was washed with ion-exchanged water, filtered, and then dried. The resulting powder was classified using an air classifier to obtain toner 14. The number average particle size (D1) of toner 14 was 6.2 μm, and the weight average particle size (D4) was 6.7 μm. The physical properties of the resulting toner 14 are shown in Table 5.
[0183] <Toner Production Example 15> The following samples were weighed and placed in a reaction vessel, and mixed using a propeller agitator. Toner base particle dispersion 1 500.0 parts Organosilicon compound liquid 1 35.0 parts Next, the pH of the resulting mixture was adjusted to 6.0 using a 1 mol / L NaOH aqueous solution, and the temperature of the mixture was raised to 45° C., after which it was held for 1.0 hour while being mixed using a propeller stirring blade. Thereafter, the pH of the mixture was adjusted to 8.0 using a 1 mol / L NaOH aqueous solution, and held for 4.0 hours. After lowering the temperature to 25°C, the pH was adjusted to 1.5 with 1 mol / L hydrochloric acid and stirred for 1.0 hour, then the mixture was washed with ion-exchanged water, filtered, and dried. The resulting powder was classified using an air classifier to obtain toner 15. The number-average particle size (D1) of toner 15 was 6.2 μm, and the weight-average particle size (D4) was 6.7 μm. The physical properties of the obtained toner 15 are shown in Table 5.
[0184] <Toner Production Example 18> The following samples were weighed and placed in a reaction vessel, and mixed using a propeller agitator. Toner base particle dispersion 1 500.0 parts Organosilicon compound liquid 1 35.0 parts Next, the pH of the resulting mixture was adjusted to 6.0 using a 1 mol / L NaOH aqueous solution, and the temperature of the mixture was raised to 45° C., after which it was held for 1.0 hour while being mixed using a propeller agitator. Thereafter, the pH of the mixture was adjusted to 7.0 using a 1 mol / L NaOH aqueous solution, and held for 4.0 hours. After lowering the temperature to 25°C, the pH was adjusted to 1.5 with 1 mol / L hydrochloric acid and stirred for 1.0 hour, then the mixture was washed with ion-exchanged water, filtered, and dried. The resulting powder was classified using an air classifier to obtain toner 18. The number-average particle size (D1) of toner 18 was 6.2 μm, and the weight-average particle size (D4) was 6.7 μm. The physical properties of the obtained toner 18 are shown in Table 5.
[0185] <Toner Production Example 19> 100 parts of toner particles 1, 2.0 parts of organosilicon polymer microparticles 1, and 1.0 part of silica particles having a number average particle size of 100 nm were mixed for 5 minutes in a Henschel mixer (manufactured by Mitsui Miike Chemical Engineering Co., Ltd.) to obtain toner 19. The jacket temperature of the Henschel mixer was set to 10° C., and the peripheral speed of the rotating blades was set to 38 m / sec.
[0186] [Table 5]
[0187] <Evaluation> A modified LBP712Ci (Canon) was used as the image forming apparatus. The process speed of the main body was modified to 320 mm / sec. Necessary adjustments were made so that image formation was possible under these conditions. The toner was removed from the cyan cartridge, and 100 g of the toner to be evaluated was filled instead. Furthermore, the electrophotographic photoreceptor was changed to the electrophotographic photoreceptor 1 according to the present invention. The toner cartridge thus prepared was installed in the black station, and dummy cartridges were installed in the other stations, and the following image output test was carried out. The evaluation results are shown in Table 6.
[0188] <Halftone roughness evaluation> In a high temperature and humidity environment (temperature 30.0°C / humidity 80%RH), 1000 sheets of an image with a 1% coverage rate of horizontal lines were printed out, and then a halftone image was output, and the fineness of the image was visually evaluated. After that, 10000 sheets of an image with a 1% coverage rate of horizontal lines were printed out, and then a halftone image was output, and the fineness of the image was visually evaluated. Canon color laser copier paper (A4: 81.4 g / m 2 (Hereafter, unless otherwise specified, this form is assumed to be used.) (Evaluation Criteria) A: Uniformly fine grained. B: The image is slightly hazy. C: The image is hazy. D: A defective image with noticeable unevenness in density was generated.
[0189] <Fog rating: 1> Under a low temperature and low humidity environment (temperature 15°C / humidity 10% RH) and a high temperature and high humidity environment (temperature 30°C / humidity 80% RH), 10,000 sheets of an image with a horizontal line and a printing rate of 1% were printed out, and then left for 48 hours, after which the reflectance (%) of the non-image area of the image with a horizontal line and a printing rate of 1% was measured using a "REFLECTOMETER MODEL TC-6DS" (manufactured by Tokyo Denshoku Co., Ltd.). The reflectance obtained was subtracted from the reflectance (%) of unused printout paper (standard paper) measured in the same manner, and the value (%) was used for evaluation. The smaller the value, the more suppressed the image fog. The evaluation was performed in gloss paper mode using plain paper (HP Brochure Paper 200g, Glossy, manufactured by HP, 200g / m 2 ) was used. (Evaluation Criteria) A: 0.5% or less B: More than 0.5% and less than 1.5% C: More than 1.5% and less than 3.0% D: More than 3.0%
[0190] <Fog rating 2> In a high temperature and humidity environment (temperature 30°C / humidity 80%RH), 12,000 sheets of an image with a 1% printing rate in horizontal lines were printed out, and then left for 48 hours. The reflectance (%) of the non-image area of the image with a 1% printing rate in horizontal lines was measured using a "REFLECTOMETER MODEL TC-6DS" (manufactured by Tokyo Denshoku Co., Ltd.). The evaluation was performed using the same method and criteria as in Fog Evaluation 1.
[0191] <Evaluation of transferability (transfer efficiency)> The transfer efficiency is an index of transferability that indicates what percentage of the toner developed on the photosensitive drum is transferred onto the intermediate transfer belt. The transfer efficiency was evaluated by continuously forming solid images on the recording medium. First, the measurement was performed in a low temperature and low humidity environment (temperature 15°C, humidity 10% RH), and 1,000 sheets of horizontal line images with a printing rate of 1% were printed out, after which 10 solid images were formed continuously on the recording medium. After forming 10 sheets of the above image, the toner transferred onto the intermediate transfer belt and the toner remaining on the photosensitive drum after transfer were peeled off with a transparent polyester adhesive tape. The density difference was calculated by subtracting the toner density of the paper with only the adhesive tape attached from the toner density of the paper with the peeled adhesive tape attached. The transfer efficiency is the ratio of the toner density difference on the intermediate transfer belt when the sum of the respective toner density differences is set to 100, and the higher this ratio, the better the transfer efficiency. The transfer efficiency was evaluated according to the following criteria. The toner density was measured with an X-Rite color reflection densitometer (500 series). A: Transfer efficiency is 95% or more B: Transfer efficiency is 90% or more but less than 95% C: Transfer efficiency is less than 90%
[0192] [Table 6]
[0193] The disclosure of this embodiment includes the following configuration. (Configuration 1) A process cartridge that is detachably mountable to a main body of an electrophotographic apparatus, The process cartridge comprises: An electrophotographic photoreceptor; a developing means having a toner storage section for storing toner and supplying the toner to the surface of the electrophotographic photoreceptor; having The electrophotographic photoreceptor has a conductive support, and a photosensitive layer and a surface protective layer formed on the conductive support in this order; The surface protective layer contains conductive particles, the content of the conductive particles is 5.0 vol% or more and 70.0 vol% or less with respect to the total volume of the surface protective layer, The volume resistivity of the surface protective layer is 1.0×10 9 Ω cm or more 1.0×10 14 Ω cm or less, The toner contained in the toner container is selected from the following (i) or (ii): (i) A toner having toner particles containing a binder resin and organosilicon polymer particles, (ii) A toner having toner particles containing a binder resin and having an organosilicon polymer on the surface thereof. It satisfies the provisions of The organosilicon polymer particles when the requirement (i) is satisfied, or the organosilicon polymer when the requirement (ii) is satisfied, A silicon atom having a T3 unit structure; At least one unit structure selected from the group consisting of a silicon atom having a T2 unit structure and a silicon atom having a T1 unit structure; It has The organosilicon polymer particles when the requirement (i) is satisfied, or the organosilicon polymer when the requirement (ii) is satisfied, are 29 In the measurement of Si-NMR, the ratio of the total area of the peak area originating from silicon atoms having a T2 unit structure and the peak area originating from silicon atoms having a T1 unit structure to the total area of the peaks originating from all silicon atoms is 0.10 or more and 0.40 or less. A process cartridge comprising: (Configuration 2) The organosilicon polymer particles or the organosilicon polymer 29 The process cartridge according to Configuration 1, wherein, in Si-NMR measurement, the ratio of the area of the peak derived from silicon atoms having a T3 unit structure to the total area of the peaks derived from all silicon atoms contained in the organosilicon polymer particle or the organosilicon polymer is 0.50 or more and 0.90 or less. (Configuration 3) 3. The process cartridge according to claim 1, wherein the toner is a toner having toner particles containing a binder resin and organosilicon polymer particles, the major axis of the organosilicon polymer particles being 30 nm or more and 300 nm or less. (Configuration 4) 4. A process cartridge according to claim 3, wherein the rate of adhesion of the organosilicon polymer particles to the toner particles in a water washing method is 25% or less. (Configuration 5) 5. The process cartridge according to any one of Configurations 1 to 4, wherein the toner has an average circularity of 0.950 or more and 0.990 or less. (Configuration 6) The process cartridge according to any one of Configurations 1 to 5, wherein the content of silanol structures relative to the total content of alkoxysilane structures and silanol structures contained in the organosilicon polymer particles, or the T1 unit structures and T2 unit structures in the organosilicon polymer, is 98 mass% or more. (Configuration 7) 7. The process cartridge according to any one of Configurations 1 to 6, wherein the conductive particles are titanium oxide particles. (Configuration 8) 8. The process cartridge according to claim 7, wherein the titanium oxide particles are niobium atom-containing titanium oxide particles. (Configuration 9) 9. The process cartridge according to claim 8, wherein the niobium-atom-containing titanium oxide particles have a concentration ratio calculated as niobium atom concentration / titanium atom concentration at a portion within 5% of the maximum diameter of the measured particle from the particle surface, which is 2.0 times or more, compared to a concentration ratio calculated as niobium atom concentration / titanium atom concentration at a center of the particle. (Configuration 10) The process cartridge according to Configuration 8 or 9, wherein the niobium atom content of the niobium atom-containing titanium oxide particles is 2.6% by mass or more and 10.0% by mass or less based on the total mass of the niobium atom-containing titanium oxide particles. (Configuration 11) the content of the conductive particles is 5.0 vol% or more and 40.0 vol% or less with respect to the total volume of the surface protective layer, The volume resistivity of the surface protective layer is 1.0×10 11 Ω cm or more 1.0×10 14 11. The process cartridge according to any one of configurations 1 to 10, wherein the resistivity is Ω·cm or less. (Configuration 12) 12. The process cartridge according to any one of configurations 1 to 11, wherein the developing means is a contact developing device that performs development by bringing a toner carrying member carrying the toner into contact with the electrophotographic photosensitive member. (Configuration 13) 13. An electrophotographic apparatus comprising the process cartridge according to any one of configurations 1 to 12. [Explanation of symbols]
[0194] 21 Support 22 Undercoat layer 23 Charge generation layer 24 Charge transport layer 25 Surface protective layer 1. Electrophotographic photoreceptor 2-axis 3. Charging means 4 Exposure light 5. Developing method 6 Transfer Method 7 Transfer material 8 Fixing Method 9 Cleaning Method 10 Pre-exposure light 11 Process cartridge 12 Guidance means 31 Center of conductive particle 32 Near the surface of conductive particles 33 X-rays to analyze the core of conductive particles 34 X-rays that analyze the interior of conductive particles within 5% of their maximum diameter from the surface
Claims
1. A process cartridge that is detachably mountable to a main body of an electrophotographic apparatus, The process cartridge comprises: An electrophotographic photoreceptor; a developing means having a toner storage section for storing toner and supplying the toner to the surface of the electrophotographic photoreceptor; having The electrophotographic photoreceptor has a conductive support, and a photosensitive layer and a surface protective layer formed on the conductive support in this order; The surface protective layer contains conductive particles, the conductive particles are titanium oxide particles, The titanium oxide particles are niobium atom-containing titanium oxide particles, the content of the conductive particles is 5.0 vol% or more and 70.0 vol% or less with respect to the total volume of the surface protective layer, The volume resistivity of the surface protective layer is 1.0×10 9 Ω・cm or more 1.0×10 14 Ω cm or less, The toner contained in the toner container is selected from the following (i) or (ii): (i) A toner having toner particles containing a binder resin and organosilicon polymer particles, (ii) A toner having toner particles containing a binder resin and having an organosilicon polymer on the surface thereof, It satisfies the provisions of The organosilicon polymer particles when the condition (i) is satisfied, or the organosilicon polymer when the condition (ii) is satisfied, A silicon atom having a T3 unit structure; At least one unit structure selected from the group consisting of a silicon atom having a T2 unit structure and a silicon atom having a T1 unit structure; It has The organosilicon polymer particles when the condition (i) is satisfied, or the organosilicon polymer when the condition (ii) is satisfied, are 29In a Si-NMR measurement, the ratio of the total area of the peaks derived from silicon atoms having a T2 unit structure and the peak area derived from silicon atoms having a T1 unit structure to the total area of the peaks derived from all silicon atoms is 0.10 or more and 0.40 or less. A process cartridge comprising:
2. The organosilicon polymer particles or the organosilicon polymer 29 2. The process cartridge according to claim 1, wherein, in Si-NMR measurement, the ratio of the area of the peak derived from silicon atoms having a T3 unit structure to the total area of the peaks derived from all silicon atoms contained in said organosilicon polymer particles or said organosilicon polymer is 0.50 or more and 0.90 or less.
3. 2. A process cartridge according to claim 1, wherein said toner comprises toner particles containing a binder resin and organosilicon polymer particles, the major axis of said organosilicon polymer particles being 30 nm or more and 300 nm or less.
4. 4. A process cartridge according to claim 3, wherein the rate of adhesion of said organosilicon polymer particles to said toner particles in a water washing method is 25% or less.
5. 2. The process cartridge according to claim 1, wherein the toner has an average circularity of 0.950 or more and 0.990 or less.
6. 2. The process cartridge according to claim 1, wherein the content of silanol structures relative to the total content of alkoxysilane structures and silanol structures contained in said organosilicon polymer particles or in the T1 unit structures and T2 unit structures in said organosilicon polymer is 98% by mass or more.
7. 2. The process cartridge according to claim 1, wherein the niobium-atom-containing titanium oxide particles have a concentration ratio calculated as niobium atom concentration / titanium atom concentration at a portion within 5% of the maximum diameter of the measured particle from the particle surface, which is 2.0 times or more, relative to a concentration ratio calculated as niobium atom concentration / titanium atom concentration at a center of the particle.
8. 2. The process cartridge according to claim 1, wherein the niobium atom content of said niobium atom-containing titanium oxide particles is from 2.6% by mass to 10.0% by mass based on the total mass of said niobium atom-containing titanium oxide particles.
9. the content of the conductive particles is 5.0 vol% or more and 40.0 vol% or less with respect to the total volume of the surface protective layer, The volume resistivity of the surface protective layer is 1.0×10 11 Ω・cm or more 1.0×10 14 2. The process cartridge according to claim 1, wherein the surface tension is Ω·cm or less.
10. 2. A process cartridge according to claim 1, wherein said developing means is a contact developing device which performs development by bringing a toner carrying member carrying said toner into contact with said electrophotographic photosensitive member.
11. An electrophotographic apparatus comprising the process cartridge according to any one of claims 1 to 10.
Citation Information
Patent Citations
Electrophotographic photoreceptor, image forming method and image forming apparatus
JP2009229495A
Toner for electrostatic charge image development and method for forming image of the toner
JP2010249995A
Toner
JP2020106723A
toner
JP2020109506A
Process cartridge and electrophotographic device
JP2021021941A