How to obtain convex laminated glazing

The application of a sacrificial layer on the second glass sheet during the bending process addresses optical distortions in convex laminated glazing by compensating for temperature differences, enhancing sensor performance.

JP7566893B2Active Publication Date: 2024-10-15SAINT GOBAIN VITRAGE SA
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2022519650
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-09-30
Filing Date
2020-09-30
Publication Date
2024-10-15
Estimated Expiration
2040-09-30

AI Technical Summary

Technical Problem

Convex laminated glazing exhibits optical distortions near enamel-coated areas due to temperature differences caused by the enamel's high infrared absorption, which affects the functionality of sensors and cameras in vehicles.

Method used

A sacrificial layer is applied on the second glass sheet along the enamel-coated area during bending, compensating for temperature differences and reducing optical distortions by absorbing or reflecting infrared radiation.

Benefits of technology

The sacrificial layer effectively reduces temperature differences between enamel-coated and non-coated areas, minimizing optical distortions and ensuring accurate sensor functionality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007566893000001
    Figure 0007566893000001
  • Figure 0007566893000002
    Figure 0007566893000002
  • Figure 0007566893000003
    Figure 0007566893000003
Patent Text Reader

Abstract

The present invention relates to a method for obtaining convex laminated glazing, comprising the steps of applying an enamel coating to a portion of a first surface (11) of a first glass sheet (1) so as to create at least one enameled area (12) and at least one non-enameled area (14, 16), applying a sacrificial layer (22) to a portion of a first surface (21) of a second glass sheet (2), referred to as the sacrificial area, simultaneously bending the first and second glass sheets (1, 2) so that the sacrificial area (22) is positioned along at least a portion of the enameled area (12), removing the sacrificial layer (22) during or after the bending process, and laminating the first glass sheet (1) and the second glass sheet (2) together using a thermoplastic interlayer (3).
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to the field of laminated glazing, and more particularly to a method that makes it possible to obtain a higher quality product in terms of optical properties by using a bending process. [Background technology]

[0002] Laminated glazing is a glazing comprising two glass sheets adhesively joined to each other by a thermoplastic interlayer. The interlayer makes it possible in particular to retain the glass fragments in case of breakage, but also provides other functionalities, in particular in terms of intrusion resistance and improved acoustic properties. Such glazing is used in particular as a windshield for automobiles and is then convex. The glass sheet arranged on the convex side, called the outer sheet since it is intended to be positioned outside the vehicle, comprises a face called "face 1" (outside the vehicle) and a face 2 in contact with the laminate interlayer, and the glass sheet arranged on the concave side, called the inner sheet, comprises a face 3 in contact with the laminate interlayer and a face 4 intended to be positioned inside the vehicle.

[0003] These laminated glazings generally comprise an enamel coating, which makes it possible to hide the mounting seals of the glazing, for example in openings in the body of the vehicle, and also to protect them from ultraviolet radiation. The enamel, which is often placed on face 2 or face 4, is generally in the form of a band placed on the periphery of the glass sheet.

[0004] The enamel comprises a glass frit and a pigment, often a black pigment. The enamel is generally applied by screen printing and then hardens during bending, during which the glass sheet is subjected to temperatures of at least 550° C. or even at least 600° C. This process takes place in a heating device, such as a furnace, in which the glass sheet is heated by convection and radiation.

[0005] It has been observed that convex laminated glazing can in certain cases have optical distortions, sometimes called "burn lines", in the immediate vicinity of the enamel coated areas.

[0006] These distortions are particularly troublesome when they are located near the area through which the light or image must be captured by the optical sensor, called the "camera area". This is the case, for example, of a windshield equipped with sensors and / or cameras, such as rain and brightness sensors or driver assistance cameras. These sensors or cameras are located in the interior of the vehicle, against the surface 4 of the glazing, for example in the area where the rear-view mirror is fixed to the windshield. An enamel coating is generally placed in this area to hide and protect the adhesive used to fix the rear-view mirror, but this enamelled area must provide a small window for the transmission of non-enamel coating so that light can reach the sensor. It is important that this camera area is free of optical distortions so that the captured image is not distorted and, in the unlikely event, inappropriately analyzed.

[0007] It turns out that such distortions are due to the fact that enamel, especially when it is black, absorbs infrared radiation much more than bare glass. As a result, during bending, large temperature differences arise between the areas coated with enamel on the one hand and the glass areas not coated with enamel on the other hand, and these temperature differences are responsible for the observed distortions. Summary of the Invention [Problem to be solved by the invention]

[0008] The present invention aims to avoid these disadvantages by reducing or eliminating said optical distortions. [Means for solving the problem]

[0009] For that purpose, the invention is directed to a method for obtaining a convex laminated glazing having a concave side and a convex side, said glazing comprising a glass sheet, called the outer glass sheet, arranged on the convex side of the glazing, and a glass sheet, called the inner glass sheet, arranged on the concave side of the glazing, adhesively joined by a thermoplastic interlayer, said method comprising the steps of: - applying an enamel coating to a portion of a first surface of a first glass sheet to create at least one enameled area and at least one non-enameled area; - depositing a sacrificial layer on a portion of the first face of the second glass sheet, called the sacrificial area; - simultaneous bending of a first and a second glass sheet, the glass sheets being arranged during bending such that one of the first and second glass sheets is disposed above the other glass sheet, the respective first faces of the respective glass sheets being oriented towards the concave side of the glazing and the sacrificial area being disposed at least along at least a portion of the enamel-coated area, removing said sacrificial layer during or after the bending process; - laminating a first glass sheet and a second glass sheet with a thermoplastic interlayer; Includes.

[0010] In the majority of cases, which represent the most common bending methods, the first side of each respective glass sheet will be bent upward during bending. Similarly, in most cases, the laminate will be made such that the glass sheet placed on top during bending is the inner sheet.

[0011] According to a first embodiment, the inner glass sheet is the first glass sheet, in which case the enamel-coated glass sheet will generally be placed on top of the second glass sheet during bending, and the enamel coating will be placed on face 4 of the final glazing, and thus intended for use in contact with the interior of the vehicle in which the glazing will be installed.

[0012] According to a second embodiment, it is the outer glass sheet that is the first glass sheet. In this case, the second glass sheet will generally be placed on top of the enamel-coated glass sheet during bending, and the enamel coating will be placed on face 2 of the final glazing, i.e. in contact with the interlayer of the laminate.

[0013] In any case, in the final glazing, the enamel coating will generally be disposed on side 2, i.e., the inner surface of the outer sheet, or on side 4, i.e., the inner surface of the inner sheet.

[0014] The entirety of the following specification applies to these two embodiments, unless there are details to the contrary.

[0015] Each glass sheet is preferably flat before the bending step. The glass of the first and / or second glass sheet is typically soda-lime-silica glass, but other glasses, such as borosilicate and aluminosilicate glasses, can also be used. At least one glass sheet is preferably obtained by the float process, i.e. by flowing molten glass onto a bath of molten tin.

[0016] The at least one glass sheet may be transparent or tinted, for example green, blue, grey or bronze. The choice is made depending on the final use of the glazing. For example in the case of a motor vehicle windscreen, the light transmittance of the glazing (illuminant A, CIE-1931 colorimetric standard observer) is preferably at least 70%, or even 75%, and the at least one sheet then preferably comprises an iron oxide (expressed in the form Fe2O3) content of 0.5 to 0.9% by weight.

[0017] Each glass sheet preferably has a thickness comprised within the range of 0.7 to 6 mm, in particular 1 to 5 mm, in particular 2 to 4 mm. The glazing is preferably at least 1 mm thick. 2 It has an area of.

[0018] The enamel coating is preferably applied from a liquid enamel composition comprising glass frit, pigment and organic solvent, which is removed during the bending process and, if necessary, during a pre-hardening treatment of the enamel, allowing the enamel coating to harden. After hardening, the enamel coating thus essentially comprises pigment in a glassy matrix.

[0019] The glass frit or glass matrix is ​​preferably based on bismuth borosilicate and / or zinc borosilicate. The pigment preferably comprises one or more oxides selected from among chromium oxide, copper oxide, iron oxide, manganese oxide, cobalt oxide, nickel oxide. It may be, by way of example, copper chromate and / or iron chromate. The thickness of the enamel coating after the heat treatment step is preferably comprised within the range of 5-50 μm, in particular 10-40 μm.

[0020] The enamel-covered area preferably occupies 2-25%, in particular 3-20%, even more particularly 5-15% of the surface area of ​​the coating. The enamel-covered area is preferably in the form of a peripheral band. By "peripheral band" is meant a band closed on itself which extends from each point of the peripheral edge of the glass sheet towards the inside of the glass sheet with a specific width, typically 1-30 cm, often depending on the position.

[0021] The application of the enamel coating is preferably carried out by screen printing of a liquid enamel composition comprising glass frit, pigment and organic solvent. To do so, the enamel composition is applied onto the glass sheet through the mesh of a screen printing screen, in particular by means of a squeegee. The mesh of the screen is blocked in the areas of the glass sheet where no coating is desired, so that the enamel composition can only penetrate the screen in the areas to be printed according to a predefined pattern.

[0022] Other deposition techniques, such as digital printing techniques (eg inkjet printing or printing by transfer under the influence of laser radiation) are also possible.

[0023] Before curing, the enamel coating preferably has a thickness of 10 to 30 μm, in particular 15 to 25 μm. After curing, the thickness of the enamel coating is preferably 5 to 15 μm, in particular 7 to 13 μm.

[0024] The enamel is preferably black and advantageously has a colorimetric coordinate L in the reflection of the enamel surface of less than 10, in particular less than 5 and even less than 3. * has.

[0025] The sacrificial layer is deposited on the second glass sheet in a sacrificial area that will be disposed along (or in front of) at least a portion of the enamel-coated area during bending.

[0026] The presence of this layer on the second glass sheet makes it possible to compensate for the temperature difference appearing during bending at the boundary between the enameled and non-enameled areas of the first glass sheet and thus makes it possible to avoid the formation of the above-mentioned optical distortions.

[0027] The sacrificial layer may also be arranged along (ie in front of) a portion of the non-enameled area, in particular adjacent to the enameled area.

[0028] The sacrificial layer can be positioned along at least 5%, particularly at least 10%, even at least 20%, or even at least 30% or 40%, or even along at least 50% or 60% of the enamel coated area.

[0029] According to one example, the sacrificial region is disposed at least or exactly along the entirety of the enameled region, e.g., the sacrificial region is disposed along the entirety of the enameled region and along a portion of the non-enameled region adjacent to the enameled region.

[0030] According to another example, the sacrificial area is placed along the camera area, i.e. the area that includes the non-enamel area surrounded by the enameled area and a portion of the enameled area around the non-enamel area. As indicated above, the camera area refers to the area of ​​the glazing through which the sensor must capture light or an image in the final glazing as well as the adjacent enameled area.

[0031] In this case, the sacrificial area will generally be located along an area covering 0.5-10%, or even 1-5% of the enamel-covered area, and will therefore preferably be located along a non-enamel-covered area surrounded by this enamel-covered area.

[0032] The camera area preferably has a trapezoidal shape in its transparent portion. The area of ​​the transparent portion of the camera area is preferably 5 to 300 cm. 2 , especially 10~250cm 2 It is.

[0033] The sacrificial layer is preferably applied by screen printing, digital printing, pad printing, roller, curtain, or sputtering.

[0034] Screen printing, digital printing or also pad printing methods make it possible to deposit the sacrificial layer only on defined areas. These localized deposition techniques are particularly useful when the invention aims to avoid optical distortions at the camera area, for example, since in this case only small areas of the glass sheet are involved in the method according to the invention.

[0035] The thickness of the sacrificial layer is preferably 100 nm to 80 μm, particularly preferably 1 μm to 30 μm, and further preferably 5 μm to 20 μm.

[0036] Preferably, the sacrificial layer absorbs a portion of the infrared radiation. The sacrificial layer advantageously comprises a pigment, in particular a black pigment, or carbon black. The pigment preferably comprises one or more oxides selected from among chromium oxide, copper oxide, iron oxide, manganese oxide, cobalt oxide, nickel oxide.

[0037] The sacrificial layer can selectively or cumulatively reflect a portion of the infrared radiation, in which case it can contain a pigment that reflects infrared radiation, in particular a pigment of titanium dioxide.

[0038] To allow the sacrificial layer to withstand various manipulations or handlings, such as transportation and contact with tools, the sacrificial layer preferably comprises a resin, which then acts as a binder allowing the layer to be temporarily fixed to the second glass sheet.

[0039] According to one embodiment, the sacrificial layer comprises a resin and a heat-resistant inorganic compound, such as a pigment or carbon black, and the removal of the sacrificial layer is carried out after the bending step, in particular by washing and / or brushing. By "heat-resistant" it is meant that these compounds do not melt and soften during bending.

[0040] According to another embodiment, the sacrificial layer comprises a resin and a combustible inorganic compound, and the removal of the sacrificial layer is performed simultaneously with the bending process. In this case, the combustible compound is removed by combustion during the bending process. By "combustible" inorganic it is certainly meant that these compounds can be burned during the bending process.

[0041] In both cases, the resin will generally be removed during bending or, if necessary, prior to bending by a pre-curing treatment of the enamel.

[0042] The resin content in the sacrificial layer is preferably at least 10% by weight, or at least 20% by weight, and / or at most 60% by weight.

[0043] The resins can be chosen among acrylic, epoxy, alkyd, polyurethane resins, either alone or as a mixture, in the aqueous or solvent phase. Copolymers of these different polymers are also available. The resins can be in the aqueous or solvent phase, typically with a solids content of 20-80% by weight, in particular 30-70% by weight.

[0044] The resin may be a crosslinkable resin under UV radiation, a solvent-free resin, or a resin in the aqueous or solvent phase, especially based on (meth)acrylates and possibly on photoinitiators. The resin does not have to be crosslinked if no handling of the glass sheet is required between the application of the sacrificial layer and the heat treatment. Otherwise it is preferable to provide for a drying step by UV radiation.

[0045] The resin may be in the form of a latex, i.e., a dispersion in water, or in the form of an aqueous emulsion. Drying may be carried out in air or in an oven, but the drying step may be omitted if no handling of the glass sheet is required between application of the sacrificial layer and heat treatment.

[0046] The resin may be a thermoplastic resin, such as a hot-melt resin or a thermoplastic elastomer, such as a SEBS (polystyrene-b-poly(ethylene-butylene)-b-polystyrene) copolymer.

[0047] The resin may be an organic solvent based resin for enamel compositions.

[0048] The bending preferably utilizes temperatures of 600-750° C., especially 620-700° C. If necessary, the bending can be followed by a heat strengthening treatment which further comprises rapid forced cooling of the surface of the glass, for example using air nozzles, to create surface compressive stresses which improve the mechanical strength of the glass sheet.

[0049] The bending can be carried out in a known manner, for example by gravity (the glass deforms under its own weight) or by pressing. During bending, the inner glass sheet (the first or second glass sheet, as the case may be) is often placed on top of the outer glass sheet (the second or first glass sheet, as the case may be). In order to prevent them from adhering to each other during bending, these glass sheets are preferably kept at a distance by placing between them an intercalation powder that ensures a space of several tens of micrometers, typically 20 to 50 μm. The intercalation powder is, for example, based on calcium carbonate and / or magnesium carbonate.

[0050] The method may further comprise a pre-hardening treatment of the enamel before the bending step. This treatment then preferably utilizes temperatures between 550 and 650°C, in particular between 560 and 600°C. The pre-hardening treatment is particularly useful for enhancing the anti-adhesion properties of certain enamels. This embodiment is particularly appreciable when the first coating is an enamel intended to be on face 2 of the laminated glazing, said enamel then generally being destined to come into contact with the second glass sheet of the laminated glazing during the bending process.

[0051] As indicated previously, the method may include, after the bending step, a cleaning and / or brushing step, which makes it possible to remove potential organic and / or inorganic compounds or residues of the sacrificial layer, such as pigments.

[0052] After the bending step, the method includes a lamination step in which the glass sheets are bonded to one another by means of a thermoplastic interlayer.

[0053] Lamination can be carried out in known manner, for example by autoclaving at a temperature of 110-160° C. and a pressure of 10-15 bar. Prior to autoclaving, air trapped between the glass sheets and the laminate interlayer can be removed by calendering or by negative pressure.

[0054] The intermediate layer of the laminate preferably comprises at least one sheet of polyvinyl acetal, especially a sheet of polyvinyl butyral (PVB).

[0055] The intermediate layer of the laminate may be tinted or not, if necessary, to adjust the optical or thermal properties of the glazing. The intermediate layer of the laminate may advantageously have sound absorbing properties, for absorbing air-borne or solid-borne sound. For that purpose, the intermediate layer of the laminate may in particular consist of three polymeric sheets, of which two PVB sheets, called outer sheets, sandwich an inner polymeric sheet, possibly made of PVB, of lower hardness than that of the outer sheets. The intermediate layer of the laminate may also have thermal insulating properties, in particular infrared radiation reflecting properties. For that purpose, the intermediate layer of the laminate may comprise a thin coating with low emissivity, for example a coating comprising a thin layer of silver or a coating comprising alternating dielectric layers of different refractive index, applied on the PET inner sheet sandwiched by the two PVB outer sheets.

[0056] The thickness of the laminate interlayer is generally within the range of 0.3 to 1.5 mm, in particular 0.5 to 1 mm. The laminate interlayer may have a thickness that is smaller at the edge of the glazing than at the center of the glazing, in order to avoid the formation of double images when using a head-up display system, also called a HUD (head-up display).

[0057] According to one embodiment, a sensor is arranged on the inner glass sheet in front of a non-enamel-coated area (camera area) surrounded by a part of the enamel-coated area, for example a camera (especially a visible light camera and / or an infrared camera, especially a thermal camera) or a Lidar.

[0058] The resulting convex laminated glazing comprises two glass sheets adhesively joined by a thermoplastic interlayer, an enamel coating (especially black) advantageously arranged on the periphery of one of the glass sheets, on face 2 or face 4 of the glazing. The peripheral enamel makes it possible to conceal and protect the adhesives and seals that allow the fixing of the glazing in an opening in the vehicle body or the fixing of a rear-view mirror to the glazing. Preferably, the windshield comprises at least one sensor and the peripheral band of enamel comprises a non-enamel-coated window for transmission in front of said sensor. [Brief description of the drawings]

[0059] [Figure 1A] 1 is a schematic plan view of a first and second glass sheet before they are combined for bending purposes. [Figure 1B] 1B is a schematic cross-sectional view of a portion of a first and second glass sheet combined for bending purposes, taken along the cross section of the plan view shown in FIG. 1A. [Figure 1C] FIG. 2 is a cross-sectional view of the first and second glass sheets after bending. [Figure 1D] FIG. 2 is a cross-sectional view of the final laminated glazing. [Diagram 2] The temperature difference T1-T2 according to the temperature T1 is shown. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0060] The following examples illustrate the invention in a non-limiting manner in relation to the accompanying Figures 1 and 2.

[0061] 1A-1D show a schematic representation of one embodiment of the method of the present invention, which seeks to reduce optical distortions in the camera area of ​​a car windshield.

[0062] FIG. 1A is a schematic plan view of a first and second glass sheet before they are combined for bending purposes.

[0063] A first glass sheet 1 is coated on its first face 11 with a peripheral band 12 of black enamel which surrounds a non-enamelled area 14 (the central area of ​​the glass sheet) and creates a camera area 16 in the upper central part of the glass sheet, which comprises a non-enamelled transparent part surrounded by the enameled part. The application of the enamel is carried out, for example, by screen printing. At this stage the enamel has not yet hardened.

[0064] The second glass sheet 2 is covered on its first side 21 with a sacrificial layer 22, which is arranged in a sacrificial area intended to be located along (in front of) the camera area 16 during assembly of the glass sheets for bending. In an embodiment, the sacrificial layer extends along the transparent, i.e. non-enamelled, part of the camera area 16 as well as along the enamelled part located around this transparent part.

[0065] The sacrificial layer 22 includes, for example, a resin and a black pigment.

[0066] Figure 1B is a schematic cross-sectional view of a portion of a first and a second glass sheet combined for bending purposes, along the section of the plan view shown in Figure 1A. Here, the second glass sheet 2 is arranged on the first glass sheet 1. In the final glazing, the second glass sheet 2 will thus be the inner glass sheet and the first glass sheet 1 will thus be the outer glass sheet, and the enamel coating will then be found on face 2 of the glazing. As indicated above, the reverse arrangement is also possible, depending on whether the enamel is intended to be on face 2 or on face 4 of the final laminated glazing. The intercalating powder, which is generally present between the two glass sheets, is not shown here.

[0067] The first faces 11 and 21 are oriented towards what will become the concave side of the glazing during bending. Since gravity bending is discussed here, the first faces 11 and 21 are bent towards the top. Other arrangements are possible depending on the bending method utilized.

[0068] 1C is a cross-sectional view of the first and second glass sheets after bending. In the given example of a sacrificial layer, the burning of the resin has left a black pigment, indicated by reference symbol 24, on the first face 21 of the second glass sheet 2, which can be removed from face 21 by brushing.

[0069] Figure ID shows a cross-section of the final laminated glazing. After bending, the two glass sheets are separated and then laminated together with a thermoplastic interlayer 3, typically made of PVB.

[0070] 1A to 1D show only one embodiment of the method according to the invention, other configurations are of course possible, for example the deposition of the sacrificial layer 22 can be achieved along the entire enamel-coated area 12 so as to eliminate the optical distortions present in the boundary area between the enamel-coated area 12 and the non-enamel-coated area 14.

[0071] The examples which follow demonstrate the advantages of the present invention.

[0072] A first glass sheet was covered on half of its first surface with a black enamel coating by screen printing. A second glass sheet was then placed on top of the first glass sheet and the whole was then heat treated by placing it for 180 seconds in an oven heated to a temperature of 710° C. The change in temperature of the glass in the enamel-coated area (T1) and in the non-enamel-coated area (T2) (measured by thermocouples located on the first glass sheet) was measured.

[0073] In experiment 1A, the first side of the second glass sheet (which will be bent upwards during the heat treatment) was previously covered by screen printing with a composition consisting of an inorganic black pigment based on copper oxide (37% by weight), iron oxide (17% by weight) and manganese oxide (46% by weight) and an organic solvent. The wet thickness was 15 μm. In this example, the heat treatment made it possible to remove the sacrificial layer by burning off the resin, leaving the pigment on the surface of the second glass sheet, which was then removed by washing.

[0074] In Experiment 1B (Comparative), no sacrificial layer was deposited.

[0075] FIG. 2 shows the temperature difference T1-T2 as a function of the temperature T1.

[0076] The results show that the sacrificial layer on the second glass sheet makes it possible to significantly reduce the temperature difference at high temperatures between the enameled and non-enameled areas, which in the case of Example 1A is a maximum of 10°C in absolute value, whereas in the absence of the sacrificial layer this difference can be up to 35°C or more. [Explanation of symbols]

[0077] 1. First Glass Sheet 2. Second Glass Sheet 3 Thermoplastic Interlayer 11 Front page 12 Enamel-coated area 16 Camera Area 21 Front page 22 Sacrificial Layer

Claims

1. A method for obtaining a convex laminated glazing having a concave side and a convex side, said glazing comprising a glass sheet, called the outer glass sheet, placed on the convex side of the glazing, and a glass sheet, called the inner glass sheet, placed on the concave side of the glazing, adhesively joined by a thermoplastic intermediate layer (3), said method comprising the steps of: - applying an enamel coating to a portion of a first face (11) of a first glass sheet (1) so as to create at least one enamel-coated area (12) and at least one non-enamel-coated area (14, 16); - depositing a sacrificial layer (22) on a part of the first face (21) of the second glass sheet (2), called the sacrificial area, such that it absorbs a part of the infrared radiation; - simultaneous bending of a first and a second glass sheet (1, 2), the glass sheets being arranged during bending such that one of the first and second glass sheets is placed on top of the other glass sheet, the respective first faces (11, 21) of each glass sheet (1, 2) being oriented towards the concave side of the glazing and the sacrificial areas (22) being arranged along at least a part of the enamelled areas (12) and along at least a part of the non-enamelled areas adjacent to the enamelled areas (12); - removing said sacrificial layer (22) during or after the bending process, - laminating a first glass sheet (1) and a second glass sheet (2) with a thermoplastic interlayer (3), A method for obtaining a convex laminated glazing, comprising:

2. 2. The method of claim 1, wherein the inner glass sheet is the first glass sheet (1).

3. 2. The method of claim 1, wherein the outer glass sheet is the first glass sheet (1).

4. 4. The method according to claim 1, wherein the enamelled area (12) is in the form of a peripheral band.

5. 5. The method of claim 1, wherein the enamel coating is applied from a liquid enamel composition comprising glass frit, pigment and an organic solvent.

6. The method according to any one of claims 1 to 5, wherein the sacrificial area (12) is arranged along the camera area (16).

7. The method of any one of claims 1 to 6, wherein the sacrificial layer is deposited by screen printing, digital printing, pad printing, roller, curtain, or sputtering.

8. The method according to any one of the preceding claims, wherein the sacrificial layer (22) comprises a pigment, in particular a black pigment, or carbon black.

9. 9. The method according to any one of claims 1 to 8, wherein the sacrificial layer (22) comprises a resin and a heat-resistant inorganic compound, and removal of the sacrificial layer (22) is carried out after the bending step, in particular by washing and / or brushing.

10. 9. The method according to any one of claims 1 to 8, wherein the sacrificial layer (22) comprises a resin and a combustible inorganic compound, and the removal of the sacrificial layer (22) is performed simultaneously with the bending process.

11. 11. The method according to any one of claims 1 to 10, further comprising a pre-hardening treatment of the enamel (12) before the bending step.

12. 12. The method according to any one of the preceding claims, wherein the glazing is a motor vehicle windscreen.

13. 13. The method according to any one of claims 1 to 12, wherein at least one sensor is arranged on the inner glass sheet in front of a non-enamel-coated area (16) surrounded by a part of the enamelled area (12).

14. 14. The method according to claim 13, wherein the at least one sensor is a camera, in particular a visible light camera and / or an infrared camera, in particular a thermal camera, or a Lidar.

Citation Information

Patent Citations

  • Method for bending glass sheets

    WO2005068381A1

  • Laminated glass

    WO2017159452A1