Coated substrate and vehicle window assembly
By using reflective elements arranged with absorption layers and low refractive index layers on the car window, the problem of HUD image display being disturbed by the outside environment is solved, and the display effect and driving safety are improved.
Patent Information
- Application Number
- CN202411175194.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-08-26
AI Technical Summary
Traditional head-up display (HUD) images are displayed in the light-transmitting area of the front windshield, which is susceptible to the brightness and interfering light outside the vehicle, reducing driving safety and visual comfort.
Using a reflective element composed of a stacked absorption layer and a low refractive index layer, combined with the optimized film thickness setting, improve the P polarized light reflectance, smooth the P polarized light reflection spectrum, and reduce the S polarized light reflectance, and reduce the center console. Reflection interference and color shift.
It improves the display effect, reduces the energy consumption of the projector, enhances the brightness and contrast of the projection display, weakens the reflection and glare of the instrument panel, and improves driving safety and visual comfort.
Smart Images

Figure CN119065039A_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the technical field of reflective elements, and specifically relates to a coated substrate and a vehicle window assembly. Background Art
[0002] Vehicles can provide various types of information to drivers and passengers, such as vehicle information, road information, social media information and even entertainment information. This can generally be achieved through the use of vehicle head-up displays (HUDs), instrument panels, central control screens, co-pilot display screens, and their combinations to meet multi-format, near- and far-level display requirements, thereby bringing passengers a more comfortable, safe, and intelligent experience and rich information.
[0003] The display of the instrument panel, central control screen, etc. requires the driver to lower his head to observe, and the human eye will temporarily leave the road, which will bring hidden dangers to driving safety. For the traditional head-up display (HUD), the HUD image is displayed in the light-transmitting area of the front windshield, and the outside environment is used as the display background of the HUD image. The ambient brightness outside the car and other interfering light will affect the driver's observation of the HUD image, thereby reducing driving safety and visual comfort. Summary of the invention
[0004] In view of this, the first aspect of the present application provides a coated substrate, comprising a substrate and a reflective element arranged on at least one surface of the substrate, the reflective element comprising at least one stacked structure, each of the stacked structures comprising an absorption layer and a low refractive index layer stacked in layers, the absorption layer having an extinction coefficient greater than 0.1 at a light having a wavelength of 550 nm, and the low refractive index layer having a refractive index less than 1.8 at a light having a wavelength of 550 nm.
[0005] Wherein, the extinction coefficient of the absorption layer at the light with a wavelength of 550 nm is ≥0.5, or ≥1, or ≥1.5, or ≥2, or ≥2.5, or ≥3, or ≥3.5.
[0006] The material of the absorption layer is selected from at least one of Si, Ni, Cr, Al, Ti, Nb, Mo, Sn, Zn, Zr and Mg as a single substance or an alloy.
[0007] Wherein, the physical thickness of the reflective element is 200nm-500nm, or 250nm-450nm, or 300nm-400nm.
[0008] Wherein, the total physical thickness of the absorption layer in the reflective element is 10 nm to 100 nm, or 25 nm to 85 nm, or 35 nm to 75 nm.
[0009] The reflective element includes 2 to 5 stacked structures, and the absorption layer in each stacked structure is closer to the substrate than the low refractive index layer.
[0010] Wherein, the total physical thickness of the low refractive index layer in the reflective element is 100 nm to 450 nm, or 200 nm to 400 nm, or 250 nm to 375 nm.
[0011] Wherein, the ratio between the total physical thickness of the absorption layer of the low refractive index layer in the reflective element and the total physical thickness of the absorption layer is 2-15, or 2.5-10.
[0012] Wherein, the reflective element comprises two stacked structures, and the two stacked structures are a first absorption layer, a first low refractive index layer, a second absorption layer and a second low refractive index layer;
[0013] The ratio of the physical thickness of the second absorption layer to the physical thickness of the first absorption layer is 1.5-4, and / or the ratio of the physical thickness of the second low refractive index layer to the physical thickness of the first low refractive index layer is 0.7-1.2.
[0014] Wherein, the reflective element comprises three stacked structures, and the three stacked structures are a first absorption layer, a first low refractive index layer, a second absorption layer, a second low refractive index layer, a third absorption layer and a third low refractive index layer;
[0015] The ratio of the physical thickness of the second absorption layer to the physical thickness of the first absorption layer is 0.7 to 5, and / or the ratio of the physical thickness of the third absorption layer to the physical thickness of the second absorption layer is 1 to 2, and / or the ratio of the physical thickness of the second low refractive index layer to the physical thickness of the first low refractive index layer is 0.8 to 4, and / or the ratio of the physical thickness of the third low refractive index layer to the physical thickness of the second low refractive index layer is 0.7 to 1.2.
[0016] Wherein, the physical thickness of the absorption layer in the reflective element farthest from the substrate is ≥15 nm, or ≥20 nm, or ≥25 nm.
[0017] Wherein, the reflective element further includes a barrier layer arranged between the substrate and the stacked structure.
[0018] Wherein, the material of the barrier layer is selected from at least one of a high refractive index material having a refractive index greater than or equal to 1.8 and a low refractive index material having a refractive index less than 1.8;
[0019] Wherein, the barrier layer is a single-layer structure, and the material of the single-layer structure is selected from the high-refractive index material;
[0020] Or, the barrier layer is composed of a first barrier sublayer and a second barrier sublayer which are stacked, and the materials of the first barrier sublayer and the second barrier sublayer are selected from the low refractive index material;
[0021] Alternatively, the barrier layer is composed of a first barrier sublayer and a second barrier sublayer which are stacked, the material of the first barrier sublayer is selected from the high refractive index material, and the material of the second barrier sublayer is selected from the low refractive index material.
[0022] Wherein, the material of the substrate is soda-lime glass, or high-aluminum glass, or lithium-aluminum glass, or borosilicate glass, or polyethylene terephthalate, or polycarbonate.
[0023] Wherein, the substrate is a 2.1 mm transparent glass plate, the transparent glass plate has a visible light transmittance TL0, and the coated substrate has a visible light transmittance TL1, TL0≥88%, TL1≤15%.
[0024] Wherein, the TL1 and the TL0 satisfy: TL1 / TL0≤0.15, or TL1 / TL0≤0.1, or TL1 / TL0≤0.05, or TL1 / TL0≤0.01, or TL1 / TL0≤0.005, or TL1 / TL0≤0.001.
[0025] A second aspect of the present application provides a vehicle window assembly, the vehicle window assembly comprising a vehicle window glass and a projection device, the vehicle window glass is the coated substrate provided in the first aspect of the present application, the vehicle window glass has at least one display area, the reflective element at least covers the display area, the display area has a P light reflectivity RLp for P polarized light with a wavelength of 380nm-780nm incident at an incident angle of 70°, and the RLp is ≥25%;
[0026] The projection device is used to generate projection light, the projection light contains at least 80% of P polarized light, the projection light is incident on the display area at an incident angle of 38° to 85°, and the display area reflects the projection light to form a display image.
[0027] A third aspect of the present application provides a vehicle window assembly, the vehicle window assembly comprising a laminated glass and a projection device, the laminated glass comprising a first glass plate, an adhesive layer, a second glass plate and a shielding layer, the second glass plate being the coated substrate provided in the first aspect of the present application; the laminated glass having a light-transmitting area and a shielding area, the light-transmitting area having a visible light transmittance greater than or equal to 70%, and the shielding area having a visible light transmittance less than or equal to 5%;
[0028] The first glass plate has a first surface and a second surface, the second glass plate has a third surface and a fourth surface, the adhesive layer connects the second surface and the third surface, the shielding layer is arranged in the shielding area, at least one display area is arranged in the shielding area, the reflective element is arranged in the shielding area and at least covers the display area, and the shielding layer is located between the first glass plate and the reflective element;
[0029] The display area has a P light reflectivity RLp for P polarized light with a wavelength of 380nm-780nm incident at an incident angle of 70°, and the RLp is ≥25%; the projection device is used to generate projection light, and the projection light contains at least 80% of P polarized light. The projection light is incident on the display area at an incident angle of 38° to 85°, and the display area reflects the projection light to form a display image.
[0030] The coated substrate and window assembly provided in the present application adopt a reflective element composed of a stacked absorption layer and a low refractive index layer, and cooperate with an optimizable film layer thickness setting, so that when the reflective element is arranged on the substrate, it can have a higher P-polarized light reflectivity, a smooth P-polarized light reflection spectrum, and a lower S-polarized light reflectivity, thereby achieving the effect of reducing the energy consumption of the projector, reducing the reflection interference of the center console, and making the reflected imaging neutral with little or no color deviation, thereby improving the display effect. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] In order to more clearly illustrate the technical solutions in the implementation modes of the present application, the drawings required for use in the implementation modes of the present application will be described below.
[0032] Figure 1 A schematic cross-sectional view of a reflective element with a laminated structure provided in the present application.
[0033] Figure 2 A schematic cross-sectional view of an example of a reflective element with two stacked structures provided in the present application.
[0034] Figure 3 A schematic cross-sectional view of another example of a reflective element with two stacked-layer structures provided in the present application.
[0035] Figure 4 A schematic cross-sectional view of an example of a reflective element with a laminated structure and a barrier layer provided in the present application.
[0036] Figure 5 A schematic cross-sectional view of another example of a reflective element with a laminated structure and a barrier layer provided in the present application.
[0037] Figure 6 A schematic top view of a laminated glass in one embodiment provided in the present application.
[0038] Figure 7 A schematic top view of a laminated glass in another embodiment provided in the present application.
[0039] Figure 8 Schematic top views of laminated glass in two other embodiments provided in the present application.
[0040] Fig. 9 This is a schematic cross-sectional view of the laminated glass provided in this application.
[0041] Fig.10 A partial cross-sectional schematic diagram showing that the shielding layer provided in the present application is located on the second surface.
[0042] Fig.11 A partial cross-sectional schematic diagram showing that the shielding layer provided in the present application is located on the fourth surface.
[0043] Fig.12 A partial cross-sectional schematic diagram showing that the shielding layer provided in the present application is composed of a first shielding sub-layer and a second shielding sub-layer.
[0044] Fig.13 A schematic cross-sectional view of a laminated glass with a heat insulation layer provided in the present application.
[0045] Fig.14 A partial cross-sectional schematic diagram of the reflective element provided in the present application located on the sixth surface.
[0046] Fig.15 A partial cross-sectional schematic diagram of the reflective element provided in the present application located on the fifth surface.
[0047] Fig.16 This is a graph of the P light reflection spectrum and the S light reflection spectrum of the laminated glass in Comparative Example 1 provided in the present application.
[0048] Fig.17 This is a graph of the P light reflection spectrum and the S light reflection spectrum of the laminated glass in Comparative Example 2 provided in the present application.
[0049] Fig.18 This is a graph of the P light reflection spectrum and the S light reflection spectrum of the laminated glass in Example 1 provided in the present application.
[0050] Fig.19 This is a graph of the P light reflection spectrum and the S light reflection spectrum of the laminated glass in Example 2 provided in the present application.
[0051] Fig. 20 This is a graph of the P light reflection spectrum and the S light reflection spectrum of the laminated glass in Example 3 provided in the present application.
[0052] Fig.21This is a graph of the P light reflection spectrum and the S light reflection spectrum of the laminated glass in Example 4 provided in the present application.
[0053] Fig. 22 This is a graph of the P light reflection spectrum and the S light reflection spectrum of the laminated glass in Example 5 provided in the present application.
[0054] Fig.23 This is a graph of the P light reflection spectrum and the S light reflection spectrum of the laminated glass in Example 6 provided in the present application.
[0055] Fig.24 This is a graph of the P light reflection spectrum and the S light reflection spectrum of the laminated glass in Example 7 provided in the present application.
[0056] Fig.25 This is a graph of the P light reflection spectrum and the S light reflection spectrum of the laminated glass in Example 8 provided in the present application.
[0057] Fig.26 This is a graph of the P light reflection spectrum and the S light reflection spectrum of the laminated glass in Example 9 provided in the present application.
[0058] Fig. 27 This is a graph of the P light reflection spectrum and the S light reflection spectrum of the laminated glass in Example 10 provided in the present application.
[0059] Fig.28 This is a graph of the P light reflection spectrum and the S light reflection spectrum of the laminated glass in Example 11 provided in the present application.
[0060] Fig.29 This is a graph of the P light reflection spectrum and the S light reflection spectrum of the laminated glass in Example 12 provided in the present application.
[0061] Description of reference numerals: laminated glass 10, light-transmitting area 101, shielding area 102, bottom shielding area 1021, left shielding area 1022, top shielding area 1023, right shielding area 1024, display area 103, first glass plate 11, first surface 111, second surface 112, adhesive layer 12, second glass plate 13, third surface 131, fourth surface 132, shielding layer 14, first shielding sublayer 141, second shielding sublayer 142, Reflective element 15, blocking layer 150, blocking lower sublayer 1501, blocking upper sublayer 1502, first absorption layer 151, first low refractive index layer 152, first low refractive index lower sublayer 1521, first low refractive index upper sublayer 1522, second absorption layer 153, second low refractive index layer 154, thermal insulation layer 16, ultra-thin substrate 17, fifth surface 171, sixth surface 172, connecting layer 18, projection device 20, projection light 201. DETAILED DESCRIPTION
[0062] The following are preferred implementations of the present application. It should be noted that, for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present application, and these improvements and modifications are also considered to be within the scope of protection of the present application.
[0063] Unless otherwise specified or there is a contradiction, the terms and phrases used in this application have the following meanings:
[0064] In this application, "first", "second", etc. are used only for descriptive purposes and should not be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, a feature defined as "first" or "second" may explicitly or implicitly include at least one of the features.
[0065] In this application, "one or several" refers to any one, any two or more of the listed items. Among them, "several" refers to any two or more of the listed items.
[0066] The value of x in the chemical formula: if it is clearly defined, it shall be within the defined range. If it is not clearly defined, it can be determined based on the deposition in a stoichiometric, substoichiometric or superstoichiometric manner in the magnetron sputtering process.
[0067] Refractive Index: The refractive index measured at a wavelength of 550 nm.
[0068] like Figure 1 , Figure 2 and Figure 3 As shown, the present application provides a coated substrate, including a substrate and a reflective element disposed on at least one surface of the substrate, the reflective element 15 of the present application includes at least one laminated structure, each of the laminated structures includes an absorption layer and a low refractive index layer stacked, the absorption layer has an extinction coefficient greater than 0.1 at a light with a wavelength of 550nm, and the low refractive index layer has a refractive index less than 1.8 at a light with a wavelength of 550nm. In each of the laminated structures, the absorption layer is closer to the substrate than the low refractive index layer.
[0069] The reflective element is provided on the substrate, and the material of the substrate is soda-lime glass, high-aluminum glass, lithium-aluminum glass, borosilicate glass, polyethylene terephthalate, or polycarbonate. The coated substrate can be used independently as a vehicle window glass, or can be made into a laminated glass and used as a vehicle window glass. Preferably, the coated substrate is applied to the front windshield of the vehicle. However, it is not limited to this, and the coated substrate can also be applied to the rear windshield or side window glass, thereby providing more display scene applications for the vehicle.
[0070] like Figure 1As shown in FIG. 1 , the reflective element 15 may be composed of only one laminated structure of “absorption layer / low refractive index layer”. The reflective element 15 may also include at least two laminated structures, such as Figure 2 As shown, it is composed of two stacked structures. It is understandable that it can also be composed of three stacked structures; or composed of four stacked structures. The reflective element includes 2 to 5 stacked structures, and the absorption layer in each stacked structure is closer to the substrate than the low refractive index layer. Specifically, the reflective element includes 2, 3, 4, or 5 stacked structures.
[0071] The extinction coefficient of the absorption layer at a wavelength of 550 nm can be 0.1, 0.15, 0.2, 0.3, 0.4, 0.5, 1, 1.5, 2, 2.5, 3, 3.5, etc. Preferably, the extinction coefficient of the absorption layer at a wavelength of 550 nm is ≥ 0.5, more preferably the extinction coefficient of the absorption layer at a wavelength of 550 nm is ≥ 1, and further preferably the extinction coefficient of the absorption layer at a wavelength of 550 nm is ≥ 1.5, or ≥ 2, or ≥ 2.5, or ≥ 3, or ≥ 3.5. The material of the absorption layer is selected from at least one of Si, Ni, Cr, Al, Ti, Nb, Mo, Sn, Zn, Zr, and Mg, or an alloy. Specific examples include NiCr, Si, TiZr, etc. In order to better achieve that the optical performance, mechanical performance and appearance color of the reflective element 15 meet the comprehensive requirements of vehicle window glass, the low refractive index layer can be a single-layer structure or a multi-layer structure, for example, including at least two low refractive index sub-layers. Figure 3 As shown, the first low refractive index layer 152 is composed of a first low refractive index lower sublayer 1521 and a first low refractive index upper sublayer 1522 which are stacked.
[0072] The physical thickness of the reflective element 15 of the present application is 200nm-500nm, and specifically can be 200nm, 250nm, 300nm, 350nm, 400nm, 450nm, 500nm, etc., preferably, the physical thickness of the reflective element 15 is 250nm-450nm, and more preferably, the physical thickness of the reflective element 15 is 300nm-400nm. Wherein, the total physical thickness of the absorption layer in the reflective element 15 is 10nm-100nm, and specifically can be 10nm, 12nm, 15nm, 18nm, 20nm, 25nm, 30nm, 35nm, 40nm, 45nm, 50nm, 55nm, 60nm, 65nm, 70nm, 75nm, 80nm, 85nm, 90nm, 95nm, 100nm, etc., preferably, the total physical thickness of the absorption layer is 25nm-85nm, and more preferably, the total physical thickness of the absorption layer is 35nm-75nm.
[0073] Moreover, the physical thickness of the absorption layer in the reflective element 15 farthest from the substrate is ≥15nm, and specific examples include 15nm, 20nm, 25nm, 30nm, etc. Preferably, the physical thickness of the absorption layer in the reflective element 15 farthest from the substrate is ≥20nm, and more preferably, the physical thickness of the absorption layer in the reflective element 15 farthest from the substrate is ≥25nm.
[0074] The total physical thickness of the low refractive index layer in the reflective element is 100nm to 450nm, specifically 100nm, 150nm, 200nm, 250nm, 300nm, 350nm, 400nm, 450nm, etc. Preferably, the total physical thickness of the low refractive index layer is 200nm to 400nm, and more preferably, the total physical thickness of the low refractive index layer is 250nm to 375nm. In addition, the ratio between the total physical thickness of the absorption layer of the low refractive index layer in the reflective element and the total physical thickness of the absorption layer is 2 to 15, specifically 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, etc. Preferably, the ratio between the total physical thickness of the absorption layer of the low refractive index layer and the total physical thickness of the absorption layer is 2.5 to 10.
[0075] The reflective element includes two stacked structures, which are a first absorption layer, a first low refractive index layer, a second absorption layer, and a second low refractive index layer; the ratio of the physical thickness of the second absorption layer to the physical thickness of the first absorption layer is 1.5 to 4, and / or the ratio of the physical thickness of the second low refractive index layer to the physical thickness of the first low refractive index layer is 0.7 to 1.2. The ratio of the physical thickness of the second absorption layer to the physical thickness of the first absorption layer can be specifically exemplified by 1.5, 2, 2.5, 3, 3.5, 4, etc. The ratio of the physical thickness of the second low refractive index layer to the physical thickness of the first low refractive index layer can be specifically exemplified by 0.7, 0.8, 0.9, 1, 1.1, 1.2, etc.
[0076] The reflective element includes three stacked structures, which are a first absorption layer, a first low refractive index layer, a second absorption layer, a second low refractive index layer, a third absorption layer and a third low refractive index layer; the ratio between the physical thickness of the second absorption layer and the physical thickness of the first absorption layer is 0.7-5, and / or the ratio between the physical thickness of the third absorption layer and the physical thickness of the second absorption layer is 1-2, and / or the ratio between the physical thickness of the second low refractive index layer and the physical thickness of the first low refractive index layer is 0.8-4, and / or the ratio between the physical thickness of the third low refractive index layer and the physical thickness of the second low refractive index layer is 0.7-1.2. Among them, the ratio between the physical thickness of the second absorption layer and the physical thickness of the first absorption layer can be specifically exemplified as 0.7, 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, 5, etc. The ratio between the physical thickness of the third absorption layer and the physical thickness of the second absorption layer can be specifically exemplified as 1, 1.2, 1.4, 1.6, 1.8, 2, etc. The ratio of the physical thickness of the second low refractive index layer to the physical thickness of the first low refractive index layer can be specifically exemplified as 0.8, 1, 1.5, 2, 2.5, 3, 3.5, 4, etc. The ratio of the physical thickness of the third low refractive index layer to the physical thickness of the second low refractive index layer can be specifically exemplified as 0.7, 0.8, 0.9, 1, 1.1, 1.2, etc.
[0077] The present application adopts a reflective element composed of a stacked absorption layer and a low refractive index layer, and cooperates with an optimizable film layer thickness setting, so that when the reflective element is set on the substrate, it can have a higher P-polarized light reflectivity, a smooth P-polarized light reflection spectrum, and a lower S-polarized light reflectivity, thereby achieving the effects of reducing the energy consumption of the projector, reducing the reflection interference of the center console, and making the reflected image neutral with little or no color deviation, thereby improving the display effect.
[0078] The reflective element 15 of the present application further includes a barrier layer 150 disposed between the substrate and the laminated structure. The reflective element 15 may be composed of only one laminated structure, which is a barrier layer 150, a first absorption layer 151, and a first low refractive index layer 152 laminated in sequence, that is, the barrier layer 150 is in direct contact with the substrate.
[0079] The material of the barrier layer 150 is selected from at least one of a high refractive index material with a refractive index greater than or equal to 1.8 and a low refractive index material with a refractive index less than 1.8. The high refractive index material of the barrier layer 150 is selected from nitrides, oxides, and oxynitrides of at least one element of Zn, Sn, Ti, Si, Al, Ni, Cr, Nb, Mg, Zr, Ga, Y, In, Sb, V, and Ta. Specific examples include SiNx, TiOx, NbOx, TiNx, ZnSnOx, AZO, and ZrOx. The low refractive index material of the barrier layer 150 is selected from oxides composed of one or more elements of Al, Mg, Zn, Si, Zr, Sn, Ca, and V. Specific examples include Al2O3 and SiO2.
[0080] Among them, Figure 4 As shown, the barrier layer 150 is a single-layer structure, and the material of the single-layer structure is selected from the high-refractive index material. In order to better achieve that the optical properties, mechanical properties, appearance color and other aspects of the reflective element 15 meet the comprehensive requirements of vehicle window glass, the barrier layer 150 can be a single-layer structure or a multi-layer structure, for example, including at least two barrier sub-layers. For example, the barrier layer 150 is composed of a first barrier sub-layer and a second barrier sub-layer that are stacked, and the materials of the first barrier sub-layer and the second barrier sub-layer are selected from the low-refractive index material. Alternatively, the barrier layer 150 is composed of a first barrier sub-layer and a second barrier sub-layer that are stacked, and the material of the first barrier sub-layer is selected from the high-refractive index material, and the material of the second barrier sub-layer is selected from the low-refractive index material. Specifically, as Figure 5 As shown, the barrier layer 150 is composed of a barrier lower sublayer 1501 and a barrier upper sublayer 1502 which are stacked.
[0081] like Figure 6 , Figure 7 and Figure 8 As shown, the coated substrate provided in the present application is applied to a vehicle window glass, wherein the vehicle window glass has a light-transmitting area 101 and a shielding area 102, wherein at least one display area 103 is arranged in the shielding area 102, the visible light transmittance of the light-transmitting area 101 is greater than or equal to 70%, and the visible light transmittance of the shielding area 102 is less than or equal to 5%, and the reflective element 15 is arranged in the shielding area 102 and at least covers the display area 103.
[0082] At least one display area 103 is provided in the shielding area 102 described in the present application. The display area 103 can display vehicle driving information, various patterns or play videos, etc., and can be used in various scenarios such as welcoming guests, creating atmosphere, watching movies and working. Optionally, it is used to display driving parameters, including vehicle speed, engine speed, fuel consumption, tire pressure, warning information, mileage, etc. It can also be used to display weather temperature, entertainment information, and can also be used for dynamic navigation, night vision, real-life maps, etc. The display area 103 is located in the shielding area 102, and the number of display areas 103 can be as follows: Figure 6 The one shown can also be Figure 7 Four are shown, and other quantities such as two, three or even more can also be designed according to actual products.
[0083] exist Figure 6 , Figure 7 and Figure 8 In the figure, the shielding area 102 includes a bottom shielding area 1021 located below the light-transmitting area 101, a left shielding area 1022 located on the left side of the light-transmitting area 101, a top shielding area 1023 located above the light-transmitting area 101, and a right shielding area 1024 located on the right side of the light-transmitting area 101. Preferably, the display area 103 is located in the bottom shielding area 1021.
[0084] In order to improve the shielding effect of the shielding area 102 and facilitate the observation of the display area 103 by the vehicle occupants, preferably, the ratio of the total area of the shielding area 102 to the area of the laminated glass 10 is 5% to 50%. Specifically, examples include 5%, 8%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, etc. More preferably, the ratio of the total area of the shielding area 102 to the area of the laminated glass 10 is 10% to 45%, or 15% to 40%, or 20% to 35%, so that the shielding effect of the shielding area 102 and the overall aesthetics of the laminated glass 10 can be well taken into account.
[0085] In order to improve the display effect of the display area 103 and facilitate the occupants to observe the display area 103, the ratio of the total area of the display area 103 to the area of the bottom shielding area 1021 is greater than or equal to 10%. Preferably, the ratio of the total area of the display area 103 to the area of the bottom shielding area 1021 is 10% to 110%, or 15% to 105%, or 20% to 100%, or 30% to 95%, or 40% to 90%, so that the display effect of the display area 103 and the overall aesthetics of the laminated glass 10 can be well taken into account. Specifically, the ratio can be 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85%, 90%, 95%, 100%, 105% or 110%, etc. When the number of the display areas 103 is greater than or equal to two, the total area of the display areas 103 is equal to the sum of the areas of all the display areas 103 .
[0086] exist Figure 8 In the figure, the display area 103 covers the entire bottom shielding area 1021, and even the upper boundary of the display area 103 is closer to the top shielding area 1023 than the upper boundary of the bottom shielding area 1021, that is, the ratio of the total area of the display area 103 to the area of the bottom shielding area 1021 is 100% to 110%, so as to form a through-type panoramic display effect from A-pillar to A-pillar.
[0087] The display area 103 described in the present application has a P light reflectivity RLp for P polarized light with a wavelength of 380nm-780nm incident at an incident angle of 70°, and the P light reflectivity RLp is ≥35%. Preferably, the P light reflectivity RLp is 35%-60%, and specific examples include 35%, 40%, 42%, 45%, 48%, 50%, 55%, 60%, etc. More preferably, the P light reflectivity RLp is 40%-60%, more preferably, the P light reflectivity RLp is 40%-50%, more preferably, the P light reflectivity RLp is 50%-60%, and further preferably, the P light reflectivity RLp is 42%-48%, thereby enhancing the brightness of the projection display, improving the energy utilization rate of the projection device 20, and thereby reducing the energy consumption of the projection device 20, which is beneficial to the miniaturization and heat dissipation design of the projection device 20.
[0088] The display area 103 described in the present application has an S light reflectivity RLs≤20% for S polarized light with a wavelength of 380nm-780nm incident at an incident angle of 70°. Specific examples include 20%, 17%, 15%, 13%, 10%, 8%, 6%, 5%, etc. Preferably, the S light reflectivity RLs≤15%, more preferably the S light reflectivity RLs≤10%, and further preferably the S light reflectivity RLs≤6%, thereby reducing or even eliminating the reflection of the dashboard in the display area 103 to avoid interfering with the field of vision of people in the car, and also reducing or even eliminating the glare caused by the excessive projection brightness of the projection device 20, thereby improving the display effect.
[0089] The display area 103 of the present application has an S light reflectivity RLs for S polarized light with a wavelength of 380nm-780nm incident at an incident angle of 70°, and a ratio of the P light reflectivity RLp to the S light reflectivity RLs is RLp / RLs≥2.5, and specific examples include 2.5, 2.6, 2.7, 2.8, 2.9, 3.0, 3.1, 3.2, 3.3, 3.4, 3.5, 3.6, 3.7, 3.8, 3.9, 4.0, 4.1, 4.2, 4.3, 4.4, 4.5, 4.6, 4.7, 4.8, 4.9, 5.0, etc., preferably Preferably, the ratio of the P light reflectivity RLp to the S light reflectivity RLs is RLp / RLs≥3, more preferably the ratio of the P light reflectivity RLp to the S light reflectivity RLs is RLp / RLs≥4, and further preferably the ratio of the P light reflectivity RLp to the S light reflectivity RLs is RLp / RLs≥5, so that the reflectivity of the display area 103 to P polarized light is much greater than the reflectivity of the display area 103 to S polarized light, which can enhance the reflection of P polarized light to realize projection display, and reduce the reflection of S polarized light to weaken or even eliminate the reflection of the dashboard in the display area 103, thereby avoiding interfering with the field of vision of people in the car.
[0090] The display area 103 described in the present application has an S light reflection spectrum curve for S polarized light with a wavelength of 380nm-780nm incident at an incident angle of 70°, and the S light reflection spectrum curve has only one extreme point in the wavelength range of 450nm-650nm. The S light reflection spectrum curve in the wavelength range of 450nm-650nm can be understood as a U-shaped or U-shaped curve. At the extreme point, there is a minimum S light reflectivity RLsmin, and the minimum S light reflectivity RLsmin≤7.5%, and specific examples include 7.5%, 7%, 6.5%, 6%, 5.5%, 5%, 4.5%, 4%, 3.5%, 3%, 2.5%, 2%, 1%, etc. Preferably, the minimum S light reflectivity RLsmin≤5%, more preferably the minimum S light reflectivity RLsmin≤4%, and further preferably the minimum S light reflectivity RLsmin≤3%, so that there can be a smooth P polarized light reflection spectrum, thereby achieving the effects of reducing the energy consumption of the projector, reducing the reflection interference of the center console, and making the reflected imaging neutral with little or no color deviation, thereby improving the display effect.
[0091] The display area 103 described in the present application has a maximum P light reflectivity RLpmax and a minimum P light reflectivity RLpmin for P polarized light with a wavelength of 450nm-650nm incident at an incident angle of 70°, and the difference between the maximum P light reflectivity and the minimum P light reflectivity RLpmax-RLpmin≤5%, which can be 5%, 4.5%, 4%, 3.5%, 3%, 2.5%, 2%, 1.5%, 1%, 0.5%, etc. Preferably, the difference RLpmax between the maximum P light reflectivity and the minimum P light reflectivity is pmax-RLpmin≤4%, more preferably the difference between the maximum value and the minimum value of the P light reflectivity RLpmax-RLpmin≤3%, further preferably the difference between the maximum value and the minimum value of the P light reflectivity RLpmax-RLpmin≤1%, further preferably the difference between the maximum value and the minimum value of the P light reflectivity RLpmax-RLpmin≤0.5%, thereby achieving the effects of reducing the energy consumption of the projector, reducing the reflection interference of the central console, making the reflected imaging neutral with little or no color deviation, and improving the display effect.
[0092] In the present application, the substrate is a 2.1 mm transparent glass plate, and the 2.1 mm thick transparent glass plate has a visible light transmittance TL0 greater than or equal to 88%. A reflective element 15 with a thickness of 2.1 mm is arranged on the transparent glass plate, so that the transparent glass plate with a visible light transmittance greater than or equal to 88% has a visible light transmittance TL1 less than or equal to 15%, and TL1 can be specifically exemplified as 15%, 12%, 10%, 8%, 7%, 5%, 2.5%, 2%, 1.5%, 1%, 0.5%, etc. Preferably, the visible light transmittance TL1≤10%, more preferably the visible light transmittance TL1≤5%, and further preferably the visible light transmittance TL1≤2%, so that the reflection of the projection light 201 by the heat insulating layer 16 of the laminated glass 10 can be reduced or even eliminated to interfere with the image formed by the reflective element 15, and the materials used for the shielding layer 14 of the laminated glass can be saved to a certain extent or even partially replace the shielding layer 14, which is conducive to reducing the manufacturing cost of the laminated glass 10.
[0093] The TL1 and the TL0 described in the present application satisfy: TL1 / TL0≤0.15, and specific examples include 0.15, 0.1, 0.05, 0.01, 0.005, 0.001, etc. Preferably, TL1 / TL0≤0.1, more preferably TL1 / TL0≤0.05, further preferably TL1 / TL0≤0.01, or TL1 / TL0≤0.005, or TL1 / TL0≤0.001.
[0094] The present application also provides a vehicle window assembly, which includes a vehicle window glass and a projection device, wherein the vehicle window glass is the coated substrate provided above in the present application, and the vehicle window glass has at least one display area, and the reflective element at least covers the display area, and the display area has a P light reflectivity RLp for P polarized light with a wavelength of 380nm-780nm incident at an incident angle of 70°, and the RLp is ≥25%.
[0095] The projection device is used to generate projection light, the projection light contains at least 80% of P polarized light, the projection light is incident on the display area at an incident angle of 38° to 85°, and the display area reflects the projection light to form a display image.
[0096] The wavelength of the projection light 201 may be in the range of 380 nm to 780 nm. The projection light 201 may contain at least 80% of P-polarized light. The higher the proportion of P-polarized light in the projection light 201, the more conducive it is to meeting the use needs of drivers wearing sunglasses and the easier it is to eliminate the visual ghosting phenomenon of the displayed image. Exemplarily, the projection light 201 contains at least 85% of P-polarized light, or the projection light 201 contains at least 90% of P-polarized light, or the projection light 201 contains at least 95% of P-polarized light, or even the projection light 201 is 100% of P-polarized light, that is, the projection light 201 is substantially pure P-polarized light.
[0097] The present application also provides a vehicle window assembly, the vehicle window assembly comprising a laminated glass 10 and a projection device 20, the laminated glass 10 comprising a first glass plate 11, an adhesive layer 12, a second glass plate 13 and a shielding layer 14, the second glass plate 13 being the coated substrate provided in the present application; the laminated glass 10 has a light-transmitting area 101 and a shielding area 102, the light-transmitting area 101 has a visible light transmittance greater than or equal to 70%, and the shielding area 102 has a visible light transmittance less than or equal to 5%.
[0098] like Fig. 9 As shown, the laminated glass 10 includes a first glass plate 11, an adhesive layer 12, a second glass plate 13, and a shielding layer 14. The first glass plate 11 has a first surface 111 and a second surface 112. The second glass plate 13 has a third surface 131 and a fourth surface 132. The adhesive layer 12 connects the second surface 112 and the third surface 131. The shielding layer 14 is arranged in the shielding area 102. The reflective element 15 is arranged in the shielding area 102 and at least covers the display area 103. The shielding layer 14 is located between the first glass plate 11 and the reflective element 15.
[0099] Among them, the projection device 20 is used to generate projection light 201, and the projection light 201 contains at least 80% P polarized light. The projection light 201 is incident on the display area 103 at an incident angle of 38° to 85°. The display area 103 reflects the projection light 201 to form a display image that can be observed by people in the car. In particular, for the driver, the image can be observed without lowering the head, allowing the driver to have a better field of vision and a longer line of sight to observe external conditions. At the same time, the necessary information for assisted driving can be obtained more easily, greatly improving driving safety, thereby being able to partially replace or even completely replace the traditional instrument panel, or even eliminate the traditional instrument panel. At the same time, the shielding area 102 is also commonly referred to as the black border area. In the present application, the reflective element 15 is arranged in the shielding area 102 and the shielding layer 14 is located between the first glass plate 11 and the reflective element 15. The shielding layer 14 can block the reflective element 15 in the thickness direction of the laminated glass 10, so that the shielding layer 14 can be used as a display background for image display, which can better block external ambient light and avoid unnecessary interference in the line of sight. It can also improve the contrast between the displayed image and the display background and achieve a higher color gamut, making the image display clearer.
[0100] Specifically, the first glass plate 11 serves as the outer glass plate of the laminated glass 10, and the first glass plate 11 has a first surface 111 and a second surface 112. The first surface 111 is away from the adhesive layer 12 and is in contact with the outside environment of the vehicle, and the second surface 112 is close to the adhesive layer 12; the second glass plate 13 serves as the inner glass plate of the laminated glass 10, and the second glass plate 13 has a third surface 131 and a fourth surface 132. The third surface 131 is close to the adhesive layer 12, and the fourth surface 132 is away from the adhesive layer 12 and is in contact with the inside environment of the vehicle; the adhesive layer 12 connects the second surface 112 and the third surface 131.
[0101] The first glass plate 11 is transparent glass or tinted glass, the thickness of the first glass plate 11 is 0.7 mm to 4 mm, and the visible light transmittance of the first glass plate 11 is greater than or equal to 80%. The second glass plate 13 is transparent glass or tinted glass, the thickness of the second glass plate 13 is 0.7 mm to 4 mm, and the visible light transmittance of the second glass plate 13 is greater than or equal to 80%. The total iron content (in terms of Fe2O3) of the transparent glass is less than or equal to 0.1%, or even less than or equal to 0.05%, or further less than or equal to 0.01%, and the visible light transmittance of the transparent glass is 80% to 95%; the total iron content (in terms of Fe2O3) of the colored glass is 0.1% to 0.8%, preferably 0.1% to 0.5%, and the visible light transmittance of the colored glass is 80% to 90%. For example, the first glass plate 11 can be a transparent glass with a thickness of 2.1 mm and a visible light transmittance of 89%, and the second glass plate 13 can be a green glass with a thickness of 1.6 mm and a visible light transmittance of 83%, or a green glass with a thickness of 2.1 mm and a visible light transmittance of 80%.
[0102] Wherein, the bonding layer 12 is a transparent thermoplastic polymer film or a colored thermoplastic polymer film, and the thickness of the bonding layer 12 is 0.38mm to 2.28mm. For example, the thickness of the bonding layer 12 can be, but is not limited to, 0.38mm, or 0.76mm, or 1.14mm, or 1.52mm, or 1.9mm, or 2.28mm, or other values between 0.38mm and 2.28mm. The material of the thermoplastic polymer film can be selected from at least one of polyvinyl butyral (PVB), polyurethane (PU), ethylene-vinyl acetate copolymer (EVA) and ionic polymer (SGP). When the bonding layer 12 is a transparent thermoplastic polymer, the visible light transmittance of the transparent thermoplastic polymer is greater than or equal to 80%. For example, the visible light transmittance of the bonding layer 12 can be, but is not limited to, 80%, or 85%, or 90%, or 95%, etc. When the bonding layer 12 is a colored thermoplastic polymer film, the visible light transmittance of the colored thermoplastic polymer film is greater than or equal to 80%. For example, the visible light transmittance of the bonding layer 12 can be, but is not limited to, 80%, 85%, or 90%. The colored thermoplastic polymer film can be selected from a gray thermoplastic polymer film, a green thermoplastic polymer film, or a blue thermoplastic polymer film. Exemplarily, the bonding layer 12 can be a single-layer structure or a multi-layer structure, and the multi-layer structure can be exemplified by a double-layer structure, a three-layer structure, a four-layer structure, a five-layer structure, etc. The bonding layer 12 can also have other functions, such as providing at least one colored area as a shadow band to reduce the interference of sunlight to the human eye, or adding an infrared absorber to have a sunscreen or heat insulation function, or adding an ultraviolet absorber to have an ultraviolet light isolation function, or at least one layer of the multi-layer structure has a higher plasticizer content to have a sound insulation function.
[0103] The material of the shielding layer 14 is selected from at least one of dark ink, opaque polymer film, and dimming film.
[0104] like Fig.10 and Fig.12 As shown, the dark ink can be ceramic ink or ultraviolet ink, which is printed on the second surface 112, the third surface 131 and / or the fourth surface 132 by screen printing, inkjet printing or other processes, and is formed into a shielding layer 14 after curing or high-temperature sintering; the thickness of the shielding layer 14 formed by the dark ink is 5μm to 40μm.
[0105] The opaque polymer film can be a polymer film with body coloring, for example, black or brown coloring components are added during the manufacturing process of the polymer film; it can also be a polymer film with surface printed ink, paint or pigment, for example, black ink, black paint or brown pigment is printed on the surface of the polymer film; it can also be a dyed or colored polymer film, for example, black or brown dye is used to color the polymer film; the material of the polymer film can be polyvinyl butyral (PVB), polyethylene terephthalate (PET), polyvinyl chloride (PVC), polycarbonate (PC), polymethyl methacrylate (PMMA), etc.; the opaque polymer film is arranged in the bonding layer 12, for example, the bonding layer 12 can be two thermoplastic polymer films, and the opaque polymer film is sandwiched between the two thermoplastic polymer films.
[0106] The dimming film can be a polymer dispersed liquid crystal film (PDLC), a suspended particle film (SPD), an electrochromic film (EC), a dye liquid crystal film (LC), etc. The minimum visible light transmittance of the dimming film is less than or equal to 3%, such as 3%, 2%, 1%, 0.5%, 0%. In addition, the maximum visible light transmittance of the dimming film is set as needed, such as 10%, 20%, 30%, 50%, 70%, 80%, etc. For example: the visible light transmittance of the dimming film can be adjusted between 0% and 20%, between 0.5% and 50%, between 0% and 70%, etc. The dimming film can meet the requirements of visible light transmittance in multiple scenarios. For example, when black-border display is required, the dimming film is in an opaque state (visible light transmittance is less than or equal to 3%, or even 0%) to improve the contrast between the displayed image and the displayed background. When no display is performed, the dimming film is in a transparent state (visible light transmittance is greater than or equal to 70%) to achieve transparency in a larger area of the vehicle window glass. The dimming film is arranged in the bonding layer 12. For example, the bonding layer 12 can be two thermoplastic polymer films, and the dimming film is sandwiched between the two thermoplastic polymer films.
[0107] like Fig.12As shown, the shielding layer 14 in the bottom shielding area 1021 is composed of a first shielding sub-layer 141 and a second shielding sub-layer 142. The material of the first shielding sub-layer 141 is dark ink, and the material of the second shielding sub-layer 142 is an opaque polymer film or a dimming film. Preferably, the second shielding sub-layer 142 is a dimming film, which can better meet the requirements of visible light transmittance in multiple scenarios. For example, when image display is required, the dimming film is in an opaque state (visible light transmittance is less than or equal to 3%, or even 0%), which improves the contrast between the displayed image and the displayed background. When no display is performed, the dimming film is in a transparent state (visible light transmittance is greater than or equal to 70%), so that a larger area of the laminated glass 10 is transparent, thereby improving the field of vision of the occupants of the vehicle to observe the environment outside the vehicle. Specifically, the first shielding sublayer 141 is directly arranged on the second surface 112, and the second shielding sublayer 142 is arranged in the bonding layer 12; it can be understood that other forms can also be arranged according to actual conditions, for example, the second shielding sublayer 142 is arranged in the bonding layer 12, and the first shielding sublayer 141 is directly arranged on the third surface 131, and for example, the second shielding sublayer 142 is arranged in the bonding layer 12, and the first shielding sublayer 141 is directly arranged on the fourth surface 132.
[0108] like Fig.13 As shown, the laminated glass 10 described in the present application further includes a heat insulating layer 16. The heat insulating layer 16 can make the laminated glass 10 have excellent heat insulating properties, thereby improving the thermal comfort of the vehicle interior environment. Preferably, the total solar energy transmittance of the laminated glass 10 with the heat insulating layer 16 is less than or equal to 55%, more preferably less than or equal to 50%, or even less than or equal to 45%. The lower the total solar energy transmittance, the better the heat insulating properties of the laminated glass 10. The heat insulating layer 16 can be disposed on the second surface 112, or in the adhesive layer 12, or on the third surface 131, or on the fourth surface 132; and preferably, the heat insulating layer 16 and the reflective element 15 are not located on the same surface.
[0109] The heat insulation layer 16 can be at least one selected from single silver nano coating, double silver nano coating, triple silver nano coating, quadruple silver nano coating, ITO nano coating, FTO nano coating, infrared blocking micro coating.
[0110] The single silver nano coating, double silver nano coating, triple silver nano coating and quadruple silver nano coating can be deposited by magnetron sputtering process, and their physical thickness is preferably 100nm to 500nm. The single silver nano coating is a transparent nano coating having one silver layer and at least two dielectric layers, the double silver nano coating is a transparent nano coating having two silver layers and at least three dielectric layers, the triple silver nano coating is a transparent nano coating having three silver layers and at least four dielectric layers, and the quadruple silver nano coating is a transparent nano coating having four silver layers and at least five dielectric layers. Wherein, the material of the dielectric layer is selected from at least one oxide, nitride, or oxynitride of Zn, Ti, Si, Al, Sn, Se, Zr, Ni, In, Cr, W, Ca, Y, Nb, Cu, and Sm.
[0111] The ITO nano coating can be formed by magnetron sputtering deposition, the physical thickness of the ITO nano coating is preferably 100nm to 500nm, the ITO nano coating is a transparent nano coating having at least one ITO (indium tin oxide) functional layer and at least two dielectric layers, the material of the dielectric layer is selected from at least one oxide, nitride, or oxynitride of Zn, Ti, Si, Al, Sn, Se, Zr, Ni, In, Cr, W, Ca, Y, Nb, Cu, Sm. The FTO nano coating can be formed by chemical vapor deposition (CVD), the physical thickness of the FTO nano coating is preferably 50nm to 500nm, and the FTO nano coating is a transparent nano coating having at least one FTO (fluorine-doped tin oxide) functional layer.
[0112] The infrared blocking micro coating can be formed by sol-gel coating, the thickness of the infrared absorbing micro coating is 5 μm to 30 μm, the infrared blocking micro coating is a transparent micro coating with infrared blocking nano particles, and the material of the infrared blocking nano particles can be selected from at least one of ITO (indium tin oxide), FTO (fluorine-doped tin oxide), CWO (cesium-doped tungsten oxide), lanthanum hexaboride (LaB6) and vanadium pentoxide (V2O5). The average particle size of the infrared blocking nano particles is 20 nm to 100 nm.
[0113] exist Fig.13 In the embodiment, the heat insulation layer 16 and the reflective element 15 are not located on the same surface, and the projection of the reflective element 15 on the heat insulation layer 16 at least partially overlaps with the heat insulation layer 16, and the heat insulation layer 16 is closer to the first surface 111 than the reflective element 15, which is conducive to simplifying the production process of the heat insulation layer 16 and the reflective element 15. Specifically, the heat insulation layer 16 is directly disposed on the third surface 131, and the reflective element 15 is directly disposed on the fourth surface 132. The present application can also cite embodiments in which the heat insulation layer 16 is directly disposed on the second surface 112, and the reflective element 15 is directly disposed on the fourth surface 132.
[0114] In other embodiments, the heat insulating layer 16 and the reflective element 15 are not located on the same surface, and the reflective element 15 and the heat insulating layer 16 do not overlap each other in the thickness direction of the laminated glass 10, thereby preventing the heat insulating layer 16 from reflecting the projection light 201 and interfering with the image formed by the reflective element 15.
[0115] In some other embodiments, the heat insulating layer 16 and the reflective element 15 are located on the same surface, and the reflective element 15 and the heat insulating layer 16 do not overlap each other, so as to avoid the heat insulating layer 16 reflecting the projection light 201 and interfering with the image formed by the reflective element 15 .
[0116] In other embodiments, the heat insulation layer 16 and the reflective element 15 are located on the same surface, and the projection of the reflective element 15 on the heat insulation layer 16 at least partially overlaps with the heat insulation layer 16, and the heat insulation layer 16 is closer to the first surface 111 than the reflective element 15. Specifically, the heat insulation layer 16 may be provided first, and then the reflective element 15 may be provided on a partial surface of the heat insulation layer 16.
[0117] In the present application, when the projection of the reflective element 15 on the insulation layer 16 at least partially overlaps with the insulation layer 16, preferably, the transparent glass plate with a thickness of 2.1 mm and a visible light transmittance greater than 88% provided with the reflective element 15 has a visible light transmittance less than or equal to 30%, and can also be preferably less than or equal to 25%, more preferably less than or equal to 20%, further preferably less than or equal to 15%, further preferably less than or equal to 10%, even less than or equal to 5%, and even less than or equal to 1%. In this way, the reflection of the projection light 201 by the insulation layer 16 and the interference with the image formed by the reflective element 15 can be weakened or even eliminated, and the material used for the shielding layer 14 can be saved to a certain extent or even the shielding layer 14 can be partially replaced, which is beneficial to reducing the manufacturing cost of the laminated glass 10.
[0118] like Fig.10 As shown, the reflective element 15 of the present application is directly disposed on the fourth surface 132. Alternatively, as Fig.11 As shown, the shielding layer 14 is disposed on the fourth surface 132, and the reflective element 15 is directly disposed on the surface of the shielding layer 14 away from the fourth surface 132. Fig.14 and Fig.15As shown, alternatively, an ultra-thin substrate 17 is arranged on the fourth surface 132, and the ultra-thin substrate 17 has a fifth surface 171 facing the fourth surface 132 and a sixth surface 172 away from the fourth surface 132, the reflective element 15 is directly arranged on the fifth surface 171 or the sixth surface 172, the thickness of the ultra-thin substrate 17 is 0.05mm to 1.0mm, and the material of the ultra-thin substrate 17 is soda-lime glass, or high aluminum glass, or lithium aluminum glass, or borosilicate glass, or polyethylene terephthalate, or polycarbonate.
[0119] When the reflective element 15 described in the present application is directly disposed on the fourth surface 132, as shown in FIG. Figure 1 As shown, the reflective element 15 may be composed of only one laminated structure, namely, a first absorption layer 151 and a first low refractive index layer 152 laminated in sequence; or Figure 2 As shown, the high-low refractive index stack is composed of two stacked structures, namely, the first absorption layer 151, the first low refractive index layer 152, the second absorption layer 153 and the second low refractive index layer 154 are stacked in sequence; or, the high-low refractive index stack is composed of three stacked structures, namely, the first absorption layer 151, the first low refractive index layer 152, the second absorption layer 153, the second low refractive index layer 154, the third absorption layer and the third low refractive index layer are stacked in sequence. Preferably, the layer in the reflective element 15 that is in direct contact with the fourth surface 132 is the absorption layer, that is, the first absorption layer 151 is in direct contact with the fourth surface 132, and the layer in the reflective element 15 that is farthest from the fourth surface 132 is the low refractive index layer, that is, the layer in the reflective element 15 that is in contact with the air is the low refractive index layer.
[0120] When the reflective element 15 is disposed on the sixth surface 172 of the ultra-thin substrate 17, the projection light 201 directly forms a reflected image, and the reflected image is clearer and has no ghosting. Alternatively, when the reflective element 15 is disposed on the fifth surface 171 of the ultra-thin substrate 17, the ultra-thin substrate 17 can better protect the reflective element 15. Since the thickness of the ultra-thin substrate 17 is extremely thin, the reflected secondary image formed by the sixth surface 172 for the high-angle incident projection light 201 is almost overlapped with the reflected primary image formed by the reflection of the reflective element 15, so that the reflected image can be visually viewed without ghosting.
[0121] like Fig.14 As shown, when the reflective element 15 is disposed on the sixth surface 172 of the ultra-thin substrate 17, the shielding layer 14 is disposed on the fourth surface 132, and the connecting layer 18 is disposed between the shielding layer 14 and the ultra-thin substrate 17 for bonding and connecting the shielding layer 14 and the ultra-thin substrate 17. Alternatively, as Fig.15 As shown, when the reflective element 15 is disposed on the fifth surface 171 of the ultra-thin substrate 17 , the connecting layer 18 is disposed between the fourth surface 132 and the reflective element 15 for bonding and connecting the fourth surface 132 and the reflective element 15 .
[0122] The material of the connecting layer 18 can be consistent with the material of the thermoplastic intermediate layer, such as PVB, EVA, SGP, or an adhesive such as OCA (Optically Clear Adhesive) optical adhesive and SCA (Solid Optically Clear Adhesive) optical adhesive. When the connecting layer 18 is transparent, the visible light transmittance of the transparent thermoplastic polymer is greater than or equal to 70%. For example, the visible light transmittance of the connecting layer 18 can be, but not limited to, 70%, 80%, or 90%. When the connecting layer 18 is opaque, for example, the visible light transmittance of the connecting layer 18 is less than or equal to 60%. For example, the visible light transmittance of the connecting layer 18 can be, but not limited to, 50%, 40%, 30%, 20%, or 10%. Preferably, the connecting layer 18 is opaque and has a visible light transmittance less than or equal to 5%.
[0123] The present application also provides a vehicle, comprising a vehicle body and the vehicle window assembly provided by the present application, wherein the projection device of the vehicle window assembly is installed inside the vehicle body, and the vehicle window assembly of the vehicle window assembly is installed at the opening of the vehicle body. When the vehicle window assembly is installed on the vehicle, it is preferably used as the front windshield of the vehicle. However, it is not limited thereto, and the vehicle window assembly can also be used as a rear windshield or side window glass, thereby providing more display scene applications for the vehicle.
[0124] In order to make the purpose and advantages of the present application clearer, the effects of the reflective element of the present application are further described in detail below in conjunction with specific embodiments.
[0125] In Comparative Examples 1-2 and Examples 1-12, the reflective element is disposed on a glass substrate for illustration.
[0126] The present application prepares a transparent glass plate with a thickness of 2.1 mm and a visible light transmittance of 90%, and deposits the reflective elements of Comparative Examples 1-2 and Examples 1-12 on the surface of the transparent glass plate. The specific film layer materials and physical thicknesses thereof are as follows:
[0127] Comparative Example 1: glass substrate / first high refractive index layer (TSO 23nm) / second low refractive index layer (SiO2 112nm) / third high refractive index layer (TZO 80nm) / fourth low refractive index layer (SiO2 98nm), the reflective element in Comparative Example 1 does not contain an absorption layer. Optionally, in TZO, the ratio of Ti to Zr is 65wt%:35wt%. In TSO, the ratio of Ti to Si is 92wt%:8wt%.
[0128] Comparative Example 2: glass substrate / first high refractive index layer (TiO2 57 nm) / second low refractive index layer (SiO2 132 nm) / third high refractive index layer (TiO2 59 nm). The reflective element in Comparative Example 2 does not contain an absorption layer.
[0129] Example 1: glass substrate / first absorption layer (NiCr 9 nm) / first low refractive index layer (SiO2 135 nm) / second absorption layer (NiCr 21 nm) / second low refractive index layer (SiO2 105 nm).
[0130] Example 2: glass substrate / first absorption layer (NiCr 11 nm) / first low refractive index layer (Al2O3 100 nm) / second absorption layer (NiCr 22 nm) / second low refractive index layer (SiO2 106 nm).
[0131] Example 3: glass substrate / first absorption layer (NiCr 11 nm) / first low refractive index lower sublayer (Al2O3 65 nm) / first low refractive index upper sublayer (SiO2 50 nm) / second absorption layer (NiCr 21 nm) / second low refractive index layer (SiO2 104 nm).
[0132] Example 4: glass substrate / blocking lower sublayer (Al2O3 91nm) / blocking upper sublayer (SiO2 32nm) / first absorption layer (NiCr 10nm) / first low refractive index lower sublayer (Al2O3 39nm) / first low refractive index upper sublayer (SiO2 81nm) / second absorption layer (NiCr 22nm) / second low refractive index layer (SiO2 104nm).
[0133] Example 5: glass substrate / barrier layer (SiNx 45nm) / first absorption layer (NiCr 8nm) / first low refractive index layer (Al2O3 100nm) / second absorption layer (NiCr 20nm) / second low refractive index layer (SiO2 99nm).
[0134] Example 6: glass substrate / blocking lower sublayer (SiNx 65nm) / blocking upper sublayer (SiO2 66nm) / first absorption layer (NiCr7nm) / first low refractive index layer (SiO2 134nm) / second absorption layer (NiCr 21nm) / second low refractive index layer (SiO2 109nm).
[0135] Specifically, the reflective element in Examples 1-6 includes two laminated structures, each of which includes an absorption layer and a low refractive index layer stacked in sequence, the refractive index of the low refractive index layer is less than 1.8, and the extinction coefficient of the absorption layer at 550nm is 3.5. The material of the absorption layer is selected from at least one element or alloy of Si, Ni, Cr, Al, Ti, Nb, Mo, Sn, Zn, Zr, and Mg, such as NiCr, Si, TiZr, etc. The physical thickness of the absorption layer farthest from the glass substrate in the reflective element in Examples 1-6, i.e., the second absorption layer, is greater than or equal to 15nm, preferably greater than or equal to 20nm. The first low refractive index layer in Examples 3 and 6 includes two sublayers, i.e., a first low refractive index lower sublayer and a first low refractive index upper sublayer.
[0136] The barrier layer of Example 4 comprises two sublayers, each of which is made of a low refractive index material, namely, a lower barrier sublayer and an upper barrier sublayer. The barrier layer of Example 5 is a single-layer structure, and its material is a high refractive index material. The barrier layer of Example 6 comprises two sublayers, namely, a lower barrier sublayer and an upper barrier sublayer, the material of the lower barrier sublayer is a high refractive index material, and the material of the upper barrier sublayer is a low refractive index material.
[0137] Example 7: glass substrate / first absorption layer (NiCr 23nm) / first low refractive index layer (SiO2 44nm) / second absorption layer (NiCr 23nm) / second low refractive index layer (SiO2 125nm) / third absorption layer (NiCr 31nm) / third low refractive index layer (SiO2 98nm).
[0138] Example 8: glass substrate / first absorption layer (NiCr 27nm) / first low refractive index layer (Al2O3 39nm) / second absorption layer (NiCr 24nm) / second low refractive index layer (SiO2 94nm) / third absorption layer (NiCr 29nm) / third low refractive index layer (SiO2 102nm).
[0139] Example 9: glass substrate / first absorption layer (NiCr 31nm) / first low refractive index lower sublayer (Al2O3 27nm) / first low refractive index upper sublayer (SiO2 14nm) / second absorption layer (NiCr 23nm) / second low refractive index lower sublayer (Al2O359nm) / second low refractive index upper sublayer (SiO2 51nm) / third absorption layer (NiCr 28nm) / third low refractive index layer (SiO2105nm).
[0140] Example 10: glass substrate / barrier layer (SiNx 31nm) / first absorption layer (NiCr 6nm) / first low refractive index layer (SiO2 117nm) / second absorption layer (NiCr 16nm) / second low refractive index layer (SiO2 139nm) / third absorption layer (NiCr23nm) / third low refractive index layer (SiO2 105nm).
[0141] Example 11: glass substrate / barrier layer (SiNx 33nm) / first absorption layer (NiCr 7nm) / first low refractive index layer (Al2O3 96nm) / second absorption layer (NiCr 17nm) / second low refractive index layer (Al2O3 105nm) / third absorption layer (NiCr24nm) / third low refractive index layer (SiO2 110nm).
[0142] Example 12: glass substrate / barrier layer (SiNx 32nm) / first absorption layer (NiCr 4nm) / first low refractive index lower sublayer (Al2O3 45nm) / first low refractive index upper sublayer (SiO2 87nm) / second absorption layer (NiCr 18nm) / second low refractive index lower sublayer (Al2O3 66nm) / second low refractive index upper sublayer (SiO2 50nm) / third absorption layer (NiCr 25nm) / third low refractive index layer (SiO2 108nm).
[0143] Specifically, the reflective element in Examples 7-12 includes three stacked structures, each of which includes an absorption layer and a low refractive index layer stacked in sequence, the refractive index of the low refractive index layer is less than 1.8, and the extinction coefficient of the absorption layer at 550nm is 3.5. The physical thickness of the absorption layer farthest from the glass substrate in the reflective element in Examples 7-12, i.e., the third absorption layer, is greater than or equal to 15nm, preferably greater than or equal to 20nm, and more preferably greater than or equal to 25nm. The first low refractive index layer in Examples 9 and 12 includes two sublayers, i.e., a first low refractive index lower sublayer and a first low refractive index upper sublayer. The second low refractive index layer in Examples 9 and 12 includes two sublayers, i.e., a second low refractive index lower sublayer and a second low refractive index upper sublayer. The barrier layer in Examples 10-12 is a single-layer structure, and its material is a high refractive index material.
[0144] The 2.1 mm thick transparent glass plates with film layer structures of Comparative Examples 1-2 and Examples 1-12 were subjected to high temperature heat treatment at least 500° C., and then their visible light transmittances were measured, and the measurement results were recorded in Table 1.
[0145] Visible light transmittance: measured and calculated in accordance with ISO 9050 within the wavelength range of 380nm to 780nm.
[0146] Table 1: Visible light transmittance of the transparent glass plates with reflective elements of Comparative Examples 1-2 and Examples 1-12
[0147]
[0148]
[0149] As can be seen from Table 1, a transparent glass plate with a thickness of 2.1 mm has a visible light transmittance TL0 greater than 88%, and a transparent glass plate with a thickness of 2.1 mm and a visible light transmittance greater than 88% provided with a reflective element has a visible light transmittance TL1 less than 15%. Preferably, a transparent glass plate with a thickness of 2.1 mm and a visible light transmittance greater than 88% provided with the reflective element of Examples 1-12 has a visible light transmittance TL1 less than or equal to 10%. Exemplarily, TL1 is less than or equal to 5%. Exemplarily, TL1 is less than or equal to 1%. Further exemplary, TL1 is less than or equal to 0.5%. Further exemplary, TL1 is less than or equal to 0.1%. In this way, the reflection of the projection light by the heat insulating layer of the laminated glass and the interference with the image formed by the reflective element can be reduced or even eliminated, and the materials used for the shielding layer of the laminated glass can be saved to a certain extent or even partially replace the shielding layer, which is conducive to reducing the manufacturing cost of the laminated glass.
[0150] Prepare another transparent glass plate with a thickness of 2.1 mm and a visible light transmittance greater than 88%, print black ceramic ink on the surface through a screen printing process, and form a shielding layer after high-temperature sintering;
[0151] Prepare another piece of transparent PVB with a thickness of 0.76 mm, and laminate the transparent glass plates with the reflective elements of Comparative Examples 1-2 and Examples 1-12 with the transparent PVB and the transparent glass plates with the shielding layer according to the automobile glass production process, and then treat them in an autoclave, etc., to finally obtain laminated glass with the reflective elements of Comparative Examples 1-2 and Examples 1-12.
[0152] A transparent glass plate with a shielding layer is used as an outer glass plate of a laminated glass, and a transparent glass plate with a reflective element of comparative examples 1-2 and embodiments 1-12 is used as an inner glass plate of a laminated glass, the shielding layer is located on the second surface of the laminated glass and forms a shielding area, the reflective element is arranged on the fourth surface of the laminated glass and is located in the bottom shielding area, and the reflective element forms a display area in the bottom shielding area.
[0153] The P light reflection spectrum curve, P light reflectivity RLp, S light reflection spectrum curve, S light reflectivity RLs, and S light reflectivity minimum value RLsmin of the laminated glass having the reflective elements of Comparative Examples 1-2 and Examples 1-12 were measured, and the measurement results were recorded in Table 2.
[0154] P-light reflection spectrum curve: The reflection spectrum of P-polarized light of 380nm-780nm is measured by a spectrophotometer.
[0155] P-light reflectivity RLp: According to standard ISO9050, the reflectivity of the display area to P-polarized light with a wavelength of 380nm-780nm incident at an incident angle of 70° is measured and calculated from the side of the fourth surface.
[0156] P light reflectance extreme difference ΔP: According to the P light reflectance spectrum curve, the maximum value RLpmax and the minimum value RLpmin of the P light reflectance are measured and calculated within the wavelength range of 450nm-650nm, ΔP=RLpmax-RLpmin.
[0157] S-light reflection spectrum curve: The reflection spectrum of S-polarized light of 380nm-780nm is measured by a spectrophotometer.
[0158] S light reflectivity RLs: According to standard ISO9050, the reflectivity of the display area to S polarized light with a wavelength of 380nm-780nm incident at an incident angle of 70° is measured and calculated from the side of the fourth surface.
[0159] Whether there is an extreme point: Based on the S light reflection spectrum curve, measure and calculate whether there is an extreme point in the wavelength range of 450nm-650nm. The extreme point is the point where the first-order derivative of the curvature in the S light reflection spectrum curve is zero, and the extreme point has a local maximum or local minimum value of the S light reflectivity.
[0160] S light reflectivity minimum value RLsmin: If the S light reflectivity spectrum curve has an extreme point in the wavelength range of 450nm-650nm, and has a local minimum value of the S light reflectivity at the extreme point, the local minimum value is recorded as the S light reflectivity minimum value RLsmin.
[0161] Table 2: Performance parameters of laminated glass with reflective elements of Comparative Examples 1-2 and Examples 1-12
[0162]
[0163] The P light reflection spectrum curves of the laminated glasses of Comparative Examples 1-2 and Examples 1-12 in the wavelength range of 400nm-700nm, and the S light reflection spectrum curves in the wavelength range of 400nm-700nm are as follows: Figure 16-Figure 29 As shown, the thick line represents the P light reflection spectrum curve, and the thin line represents the S light reflection spectrum curve.
[0164] From Table 2, and Figure 16-Figure 29It can be seen that in the laminated glass of Comparative Example 1 and Comparative Example 2, RLp is less than 30%, RLs is greater than 20%, RLp / RLs is less than 1.5, and the 450nm-650nmP light reflection extreme difference ΔP of Comparative Example 1 is greater than 5%, and the S light reflection spectrum curve of Comparative Example 2 does not have a minimum value, resulting in only a low-brightness image that can be obtained by projection display in the display area, which reduces driving safety and visual comfort. If a bright image is to be obtained, the energy consumption of the projection device needs to be greatly increased, which is not conducive to the miniaturization of the projection device and the heat dissipation design.
[0165] In the laminated glass of Examples 1-12, RLp ≥ 35% or even ≥ 40%, RLs ≤ 15% or even ≤ 10%, RLp / RLs > 2 or ≥ 3 or even ≥ 4, and the extreme difference ΔP of P light reflection from 450nm to 650nm is ≤ 1% or even ≤ 0.5%, and it has only one minimum value in the wavelength range of 450nm-650nm, and RLsmin is less than 7.5% or even ≤ 5%. By adopting a reflective element composed of a stacked arrangement of an absorption layer and a low refractive index layer, and cooperating with an optimizable film thickness setting, when the reflective element is arranged on the laminated glass, it has a higher P-polarized light reflectivity, a smooth P-polarized light reflection spectrum, and a lower S-polarized light reflectivity, thereby achieving the effects of reducing the energy consumption of the projector, reducing the reflection interference of the center console, and making the reflected imaging neutral with little or no color deviation, thereby improving the display effect.
[0166] The above is a detailed introduction to the contents provided in the implementation mode of the present application. This article explains and illustrates the principles and implementation modes of the present application. The above explanation is only used to help understand the method and core idea of the present application. At the same time, for those skilled in the art, according to the idea of the present application, there will be changes in the specific implementation mode and application scope. In summary, the contents of this specification should not be understood as limiting the present application.
Claims
1. A film-coated substrate, characterized in that: The invention comprises a substrate and a reflective element arranged on at least one surface of the substrate, wherein the reflective element comprises at least one stacked structure, each of the stacked structures comprises an absorption layer and a low refractive index layer stacked in layers, the extinction coefficient of the absorption layer at a light with a wavelength of 550 nm is greater than 0.1, and the refractive index of the low refractive index layer at a light with a wavelength of 550 nm is less than 1.
8.
2. The coated substrate according to claim 1, characterized in that: The extinction coefficient of the absorption layer at the light with a wavelength of 550 nm is ≥0.5, or ≥1, or ≥1.5, or ≥2, or ≥2.5, or ≥3, or ≥3.
5.
3. The film-coated substrate according to claim 1, characterized in that: The material of the absorption layer is selected from at least one of Si, Ni, Cr, Al, Ti, Nb, Mo, Sn, Zn, Zr, and Mg, or an alloy thereof.
4. The coated substrate according to claim 1, characterized in that: The physical thickness of the reflective element is 200nm-500nm, or 250nm-450nm, or 300nm-400nm.
5. The coated substrate according to claim 1, characterized in that: The total physical thickness of the absorption layer in the reflective element is 10 nm to 100 nm, or 25 nm to 85 nm, or 35 nm to 75 nm.
6. The coated substrate according to claim 1, characterized in that: The reflective element includes 2 to 5 stacked structures, and the absorption layer in each stacked structure is closer to the substrate than the low refractive index layer.
7. The film-coated substrate according to claim 1, characterized in that: The total physical thickness of the low refractive index layer in the reflective element is 100 nm to 450 nm, or 200 nm to 400 nm, or 250 nm to 375 nm.
8. The coated substrate according to claim 1, characterized in that: The ratio between the total physical thickness of the absorption layer of the low refractive index layer in the reflective element and the total physical thickness of the absorption layer is 2-15, or 2.5-10.
9. The film-coated substrate according to claim 1, characterized in that: The reflective element comprises two stacked-layer structures, wherein the two stacked-layer structures are a first absorption layer, a first low-refractive-index layer, a second absorption layer, and a second low-refractive-index layer; The ratio of the physical thickness of the second absorption layer to the physical thickness of the first absorption layer is 1.5-4, and / or the ratio of the physical thickness of the second low refractive index layer to the physical thickness of the first low refractive index layer is 0.7-1.
2.
10. The film-coated substrate according to claim 1, characterized in that: The reflective element comprises three stacked structures, wherein the three stacked structures are a first absorption layer, a first low refractive index layer, a second absorption layer, a second low refractive index layer, a third absorption layer and a third low refractive index layer; The ratio of the physical thickness of the second absorption layer to the physical thickness of the first absorption layer is 0.7 to 5, and / or the ratio of the physical thickness of the third absorption layer to the physical thickness of the second absorption layer is 1 to 2, and / or the ratio of the physical thickness of the second low refractive index layer to the physical thickness of the first low refractive index layer is 0.8 to 4, and / or the ratio of the physical thickness of the third low refractive index layer to the physical thickness of the second low refractive index layer is 0.7 to 1.
2.
11. The film-coated substrate according to claim 1, characterized in that: The physical thickness of the absorption layer in the reflective element farthest from the substrate is ≥15 nm, or ≥20 nm, or ≥25 nm.
12. The film-coated substrate according to claim 1, characterized in that: The reflective element further includes a barrier layer disposed between the substrate and the stacked structure.
13. The film-coated substrate according to claim 12, characterized in that: The material of the barrier layer is selected from at least one of a high refractive index material having a refractive index greater than or equal to 1.8 and a low refractive index material having a refractive index less than 1.8; Wherein, the barrier layer is a single-layer structure, and the material of the single-layer structure is selected from the high-refractive index material; Or, the barrier layer is composed of a first barrier sublayer and a second barrier sublayer which are stacked, and the materials of the first barrier sublayer and the second barrier sublayer are selected from the low refractive index material; Alternatively, the barrier layer is composed of a first barrier sublayer and a second barrier sublayer which are stacked, the material of the first barrier sublayer is selected from the high refractive index material, and the material of the second barrier sublayer is selected from the low refractive index material.
14. The film-coated substrate according to claim 12, characterized in that: The material of the substrate is soda-lime glass, high-aluminum glass, lithium-aluminum glass, borosilicate glass, polyethylene terephthalate, or polycarbonate.
15. The film-coated substrate according to claim 1, characterized in that: The substrate is a 2.1 mm transparent glass plate, the transparent glass plate has a visible light transmittance TL0, and the coated substrate has a visible light transmittance TL1, TL0≥88%, TL1≤15%.
16. The film-coated substrate according to claim 15, characterized in that: The TL1 and the TL0 satisfy: TL1 / TL0≤0.15, or TL1 / TL0≤0.1, or TL1 / TL0≤0.05, or TL1 / TL0≤0.01, or TL1 / TL0≤0.005, or TL1 / TL0≤0.
001.
17. A vehicle window assembly, characterized in that: The vehicle window assembly comprises a vehicle window glass and a projection device, wherein the vehicle window glass is a coated substrate according to any one of claims 1 to 16, the vehicle window glass has at least one display area, the reflective element at least covers the display area, the display area has a P light reflectivity RLp for P polarized light with a wavelength of 380nm-780nm incident at an incident angle of 70°, and the RLp is ≥25%; The projection device is used to generate projection light, the projection light contains at least 80% of P polarized light, the projection light is incident on the display area at an incident angle of 38° to 85°, and the display area reflects the projection light to form a display image.
18. A vehicle window assembly, characterized in that: The vehicle window assembly comprises a laminated glass and a projection device, wherein the laminated glass comprises a first glass plate, an adhesive layer, a second glass plate and a shielding layer, wherein the second glass plate is a coated substrate according to any one of claims 1 to 16; the laminated glass has a light-transmitting area and a shielding area, wherein the visible light transmittance of the light-transmitting area is greater than or equal to 70%, and the visible light transmittance of the shielding area is less than or equal to 5%; The first glass plate has a first surface and a second surface, the second glass plate has a third surface and a fourth surface, the adhesive layer connects the second surface and the third surface, the shielding layer is arranged in the shielding area, at least one display area is arranged in the shielding area, the reflective element is arranged in the shielding area and at least covers the display area, and the shielding layer is located between the first glass plate and the reflective element; The display area has a P light reflectivity RLp for P polarized light with a wavelength of 380nm-780nm incident at an incident angle of 70°, and the RLp is ≥25%; the projection device is used to generate projection light, and the projection light contains at least 80% of P polarized light. The projection light is incident on the display area at an incident angle of 38° to 85°, and the display area reflects the projection light to form a display image.
Citation Information
Patent Citations
Solar control glazing
CN105008299A
Coated glass and laminated glass
CN114057407A
Black edge display vehicle window and vehicle
CN117465203A
Glass panel comprising a solar control layer
US20160031751A1
Glazing comprising a functional coating and an absorbing coating having a colorimetric adjustment
US20210347685A1
Cited By
Laminated glass and vehicle
CN119872026A
Laminated glass and vehicle
CN119872026B
Laminated glass and projection system