Exterior material for power storage device and power storage device using same
The exterior packaging material for power storage devices, featuring a semi-aromatic polyamide base with controlled elongation and a high-temperature adhesive, addresses deformation issues in high-temperature environments by maintaining structural integrity.
Patent Information
- Application Number
- JP2020095427
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-06-01
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2040-06-01
AI Technical Summary
Power storage devices, such as all-solid-state batteries, deform when used or stored in high-temperature environments, leading to structural issues that persist even after returning to normal temperatures.
An exterior packaging material comprising a base material with specific elongation limits in both MD and TD directions, made of semi-aromatic polyamide, and an adhesive layer that maintains adhesion at high temperatures, along with a barrier layer and sealant layer, to prevent deformation under high thermal stress.
The packaging material effectively suppresses deformation of power storage devices in high-temperature environments, maintaining structural integrity and preventing swelling even after exposure to high temperatures.
Smart Images

Figure 0007567214000002 
Figure 0007567214000003 
Figure 0007567214000004
Abstract
Description
[Technical field]
[0001] The present invention relates to an exterior material for an electricity storage device and an electricity storage device using the same. [Background technology]
[0002] Known examples of power storage devices include secondary batteries such as lithium ion batteries, nickel metal hydride batteries, and lead storage batteries, as well as electrochemical capacitors such as electric double layer capacitors. Due to the miniaturization of portable devices or the limitations of installation space, there is a demand for further miniaturization of power storage devices, and lithium ion batteries with high energy density have attracted attention. Metal cans have traditionally been used as exterior materials for lithium ion batteries, but multilayer films that are lightweight, have high heat dissipation properties, and can be produced at low cost have come to be used.
[0003] A lithium ion battery using the above multilayer film as an exterior material is called a laminated lithium ion battery. The exterior material covers the battery contents (positive electrode, separator, negative electrode, electrolyte, etc.) and prevents moisture from penetrating into the battery. A laminated lithium ion battery is manufactured, for example, by forming a recess in a part of the exterior material by cold forming, accommodating the battery contents in the recess, folding back the remaining part of the exterior material, and heat sealing the edges (see, for example, Patent Document 1). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2013-101765 A Summary of the Invention [Problem to be solved by the invention]
[0005] Meanwhile, research and development of a power storage device called an all-solid-state battery is being carried out as a next-generation battery of lithium-ion batteries. An all-solid-state battery is characterized by using a solid electrolyte as an electrolytic material, rather than an organic electrolyte. While a lithium-ion battery cannot be used at temperatures higher than the boiling point temperature of the electrolyte (about 80°C), an all-solid-state battery can be used at temperatures exceeding 100°C, and the conductivity of lithium ions can be increased by operating the all-solid-state battery under high temperature conditions (for example, 100 to 150°C). Since an all-solid-state battery can be used at such high temperatures, the space and cost required for a cooling system for cooling the battery can be reduced.
[0006] However, when the electric storage device is used or stored in a high-temperature environment, the electric storage device deforms, and the deformation does not return to normal even when the device is returned to a normal temperature environment. A deformed electric storage device not only has a poor appearance, but can also make it difficult to use as intended.
[0007] The present invention has been made based on these technical circumstances, and has an object to provide an electricity storage device and an exterior material for the electricity storage device that are less likely to deform even after long-term use or storage in a high-temperature environment. [Means for solving the problem]
[0008] In order to achieve the above object, the present disclosure provides an exterior material for an electricity storage device comprising at least a substrate, an outer adhesive layer, a barrier layer, and a sealant layer in this order, The present invention provides an exterior material for a storage battery device, characterized in that the substrate has a single layer structure, a sample of 20 mm in length and 10 mm in width is prepared from the substrate alone, and when a creep test is carried out on the sample by applying a constant load of 5 N for 3 hours in an environment of 150°C, the amount of elongation in both the MD and TD directions is 3 mm or less.
[0009] When an electricity storage device is used or stored in a high-temperature environment, the device expands for various reasons. For example, the battery contents themselves expand. In addition, residual gas remaining inside the electricity storage device expands. In addition, in batteries that use a sulfide-based solid electrolyte, moisture that has entered from the outside reacts with the solid electrolyte to form H. 2 Gases such as S gas are generated and cause expansion.
[0010] When the storage device is used or stored in a high-temperature environment, the storage device expands, and the internal pressure caused by this expansion is applied to the exterior material. Moreover, the inventors have found that the strength of the exterior material itself decreases in a high-temperature environment, so that the exterior material expands outward, and the deformation does not return to normal even when the environment returns to normal temperature. The inventors have found that the above problem can be solved by controlling the elongation amount within a specific range when the base material is subjected to a creep test. That is, according to the exterior material of the present disclosure, when a sample having a length of 20 mm and a width of 10 mm is made from the base material alone, and a creep test is performed in which a constant load of 5N is applied to the sample for 3 hours in a 150°C environment, the elongation amount in both the MD direction and the TD direction is 3 mm or less, so that the deformation can be suppressed even after long-term use or storage in a high-temperature environment.
[0011] In the exterior packaging material for a power storage device, the difference between the elongation in the MD direction and the elongation in the TD direction may be 2 mm or less. If either the MD direction or the TD direction is more likely to elongate, stress tends to concentrate in the more elongated direction. If the difference between the elongation in the MD direction and the elongation in the TD direction is 2 mm or less, such stress concentration can be prevented.
[0012] In the above-mentioned storage battery device exterior material, the above-mentioned substrate may be a biaxially stretched film. As described above, in a laminated lithium ion battery, a recess is formed in a part of the exterior material by cold forming, so in this case, the substrate needs to have molding performance that allows molding by cold forming. When the substrate is a biaxially stretched film, it exhibits excellent cold forming performance.
[0013] In the exterior packaging material for an electricity storage device, the base material may be made of semi-aromatic polyamide.
[0014] In the exterior packaging material for a power storage device, the outer adhesive layer may be made of polyester polyurethane. In this case, the substrate and the barrier layer can be firmly bonded together in a high-temperature environment of, for example, 150° C. or higher. Effect of the Invention
[0015] According to the present invention, it is possible to provide an electricity storage device and an exterior material for the electricity storage device that are resistant to deformation even after long-term use or storage in a high-temperature environment. [Brief description of the drawings]
[0016] [Figure 1] 1 is a schematic cross-sectional view of an exterior material for a power storage device according to an embodiment of the present disclosure. [Diagram 2] 1 is a schematic cross-sectional view of an exterior material for a power storage device according to an embodiment of the present disclosure. [Diagram 3] 1 is a perspective view of an electricity storage device according to an embodiment of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] Hereinafter, preferred embodiments of the present disclosure will be described in detail with reference to the drawings. In the drawings, the same or corresponding parts are denoted by the same reference numerals, and duplicated explanations will be omitted. In addition, the dimensional ratios of the drawings are not limited to the ratios shown in the drawings.
[0018] [Exterior materials for power storage devices] Fig. 1 is a cross-sectional view showing a schematic diagram of an embodiment of the exterior material for a power storage device according to the present disclosure. As shown in Fig. 1, the exterior material (exterior material for a power storage device) 10 of this embodiment is a laminate including a substrate 11, an outer adhesive layer 12a provided on one side of the substrate 11, a barrier layer 13 having first and second corrosion prevention treatment layers 14a, 14b on both sides provided on the side of the outer adhesive layer 12a opposite the substrate 11, an inner adhesive layer 12b provided on the side of the barrier layer 13 opposite the outer adhesive layer 12a, and a sealant layer 16 provided on the side of the inner adhesive layer 12b opposite the barrier layer 13. Here, the first corrosion prevention treatment layer 14a is provided on the surface of the barrier layer 13 facing the substrate 11, and the second corrosion prevention treatment layer 14b is provided on the surface of the barrier layer 13 facing the sealant layer 16. In the packaging material 10, the substrate 11 is the outermost layer and the sealant layer 16 is the innermost layer. That is, the packaging material 10 is used with the substrate 11 facing the exterior side of the electricity storage device and the sealant layer 16 facing the interior side of the electricity storage device.
[0019] Each layer constituting the packaging material 10 will now be described in detail.
[0020] <Base material 11> The substrate 11 provides heat resistance in the sealing process when manufacturing the energy storage device and serves to prevent the occurrence of pinholes that may occur during molding and distribution, and also serves to withstand internal pressure when the energy storage device is used or stored in a high-temperature environment, thereby preventing subsequent deformation.
[0021] In order to fulfill this role, the substrate 11 has a single layer structure, and moreover, this single layer substrate 11 is in a standalone state without being laminated to any other layers. A sample 20 mm long and 10 mm wide is prepared with the length direction being the flow direction (MD direction) during film production and the width direction being the direction perpendicular to the flow direction (TD direction). When a creep test is conducted on this sample in an environment of 150°C under a constant load of 5N for 3 hours, the elongation in the length direction (MD elongation) must be 3 mm or less.
[0022] In addition, a sample 20 mm long and 10 mm wide is similarly prepared with the TD direction as the length direction and the MD direction as the width direction. When a creep test is conducted on this sample in an environment of 150°C under a constant load of 5N for 3 hours, the amount of elongation in the length direction (elongation in the TD direction) must be 3 mm or less.
[0023] Since the elongation in both MD and TD in creep tests is 3 mm or less, the material withstands the expansion pressure of the electricity storage device and suppresses deformation even when the electricity storage device is used or stored in a high-temperature environment. Of course, deformation is also suppressed after the electricity storage device is returned to room temperature.
[0024] In addition, the difference between the elongation in the MD direction and the elongation in the TD direction in the creep test is desirably 2 mm or less. When the difference between the elongation in the MD direction and the elongation in the TD direction is 2 mm or less, the concentration of the expansion pressure on one side can be prevented, and deformation of the electricity storage device can be further suppressed.
[0025] A film made of semi-aromatic polyamide is suitable as such a substrate 11. Semi-aromatic polyamide is a polyamide using both aromatic and aliphatic monomers as its monomers, and is characterized by having superior heat resistance compared to aliphatic polyamides using only aliphatic monomers. Terephthalic acid, hexamethylene isophthalamide, 2-methylpentamethylene terephthalamide, etc. are used as aromatic monomers. Examples of semi-aromatic polyamides using these aromatic monomers as a part of the monomers include Uniamide Ex manufactured by Unitika Ltd., HT-Nylon manufactured by Toray Industries, Ariene manufactured by Mitsui Chemicals, and Ultraamid manufactured by BASF.
[0026] It is preferable to use a biaxially stretched film as the substrate 11. When the substrate is a biaxially stretched film, it exhibits excellent cold forming performance and can be suitably used, for example, as an exterior material for a laminate-type lithium ion battery.
[0027] <Outer adhesive layer 12a> The outer adhesive layer 12a is a layer that bonds the substrate 11 and the barrier layer 13. Specific examples of materials constituting the outer adhesive layer 12a include polyurethane resins in which a difunctional or higher isocyanate compound (polyfunctional isocyanate compound) is allowed to act on a base material such as polyester polyol, polyether polyol, acrylic polyol, or carbonate polyol. Among polyurethane resins, polyester urethane resins using polyester polyol and difunctional or higher isocyanate compounds are preferred because they can firmly bond the substrate 11 and the barrier layer 13 even in a high-temperature environment of, for example, 150°C or higher.
[0028] The various polyols described above can be used alone or in combination of two or more kinds depending on the functions and performance required for the exterior material.
[0029] Depending on the performance required for the adhesive, various other additives and stabilizers may be blended with the polyurethane resin described above.
[0030] In the polyurethane adhesive used to form the outer adhesive layer 12a containing the above-mentioned polyurethane resin, the ratio (NCO / OH) of the number of isocyanato groups contained in the polyfunctional isocyanate compound to the number of hydroxyl groups contained in the polyol may be 2 to 60, 5 to 50, or 10 to 40. When this ratio is 2 or more, the adhesive strength between the substrate 11 and the barrier layer 13 in a high temperature environment (for example, 150°C) can be further improved. When the ratio is 60 or less, it is possible to prevent unreacted hydroxyl groups from remaining in excess, and it is easy to further improve the adhesive strength between the substrate 11 and the barrier layer 13 in both room temperature and high temperature environments. The heat resistance of the cured product of the polyurethane adhesive (outer adhesive layer 12a) is improved by urea or biuret generated by the reaction of a trace amount of water contained in the air or the adhesive with the polyfunctional isocyanate compound. Therefore, the more the polyfunctional isocyanate compound, the more these units are increased, which increases Tg and tends to improve heat resistance.
[0031] The thickness of the outer adhesive layer 12a is not particularly limited, but is preferably 1 to 10 μm, more preferably 3 to 7 μm, from the viewpoint of obtaining the desired adhesive strength, followability, processability, etc. If the thickness of the outer adhesive layer 12a is 1 μm or more, high adhesive strength is easily obtained, and stress relaxation of the shear force generated during thermal expansion of the substrate 11 and the barrier layer 13 in a high temperature environment is easily achieved. On the other hand, if the thickness of the outer adhesive layer is 10 μm or less, the moldability of the exterior material can be further improved.
[0032] <Barrier layer 13> The barrier layer 13 has a water vapor barrier property that prevents moisture from penetrating into the inside of the electricity storage device. The barrier layer 13 may also have extensibility for deep drawing. As the barrier layer 13, for example, various metal foils such as aluminum, stainless steel, copper, etc., or metal vapor deposition films, inorganic oxide vapor deposition films, carbon-containing inorganic oxide vapor deposition films, films provided with these vapor deposition films, etc. can be used. As the film provided with the vapor deposition film, for example, an aluminum vapor deposition film or an inorganic oxide vapor deposition film can be used. These can be used alone or in combination of two or more. As the barrier layer 13, a metal foil is preferable, and an aluminum foil is more preferable, from the viewpoints of mass (specific gravity), moisture resistance, processability, and cost. Furthermore, the linear expansion coefficient of aluminum foil at 20 to 150°C is 23×10 -6 / ° C., and the difference with the linear expansion coefficient of the base material 11 can be easily reduced.
[0033] As the aluminum foil, a soft aluminum foil that has been annealed can be preferably used from the viewpoint of imparting desired ductility during molding, but it is more preferable to use an aluminum foil containing iron for the purpose of imparting further pinhole resistance and ductility during molding. The content of iron in the aluminum foil is preferably 0.1 to 9.0 mass%, more preferably 0.5 to 2.0 mass%, in 100 mass% of the aluminum foil. When the iron content is 0.1 mass% or more, an exterior material 10 having better pinhole resistance and ductility can be obtained. When the iron content is 9.0 mass% or less, an exterior material 10 having better flexibility can be obtained. As the aluminum foil, an untreated aluminum foil may be used, but it is preferable to use an aluminum foil that has been degreased in terms of imparting corrosion resistance. When the aluminum foil is degreased, the degreased treatment may be performed on only one side of the aluminum foil, or on both sides.
[0034] The thickness of the barrier layer 13 is not particularly limited, but taking into consideration the barrier properties, pinhole resistance, and processability, it is preferably 9 to 200 μm, and more preferably 15 to 100 μm.
[0035] <First and second corrosion prevention treatment layers 14a, 14b> The first and second corrosion prevention layers 14a, 14b are layers provided to prevent corrosion of the metal foil (metal foil layer) constituting the barrier layer 13. The first corrosion prevention layer 14a plays a role in increasing the adhesion between the barrier layer 13 and the outer adhesive layer 12a. The second corrosion prevention layer 14b plays a role in increasing the adhesion between the barrier layer 13 and the inner adhesive layer 12b. The first corrosion prevention layer 14a and the second corrosion prevention layer 14b may be layers of the same configuration or layers of different configurations. The first and second corrosion prevention layers 14a, 14b (hereinafter also simply referred to as "corrosion prevention layers 14a, 14b") are formed, for example, by degreasing treatment, hydrothermal conversion treatment, anodizing treatment, chemical conversion treatment, or a combination of these treatments.
[0036] Examples of the degreasing treatment include acid degreasing and alkaline degreasing. Examples of the acid degreasing include a method using an inorganic acid such as sulfuric acid, nitric acid, hydrochloric acid, or hydrofluoric acid alone or a mixture of these. In addition, by using an acid degreasing agent in which a fluorine-containing compound such as monosodium ammonium difluoride is dissolved in the inorganic acid as described above, not only can the aluminum be degreased, but also a passive aluminum fluoride can be formed, which is effective in terms of corrosion resistance, particularly when an aluminum foil is used for the barrier layer 13. Examples of the alkaline degreasing include a method using sodium hydroxide or the like.
[0037] An example of the hydrothermal modification treatment is a boehmite treatment in which an aluminum foil is immersed in boiling water containing added triethanolamine.
[0038] An example of the anodizing treatment is an alumite treatment.
[0039] The chemical conversion treatment may be of the immersion type or the coating type. Examples of the immersion type chemical conversion treatment include chromate treatment, zirconium treatment, titanium treatment, vanadium treatment, molybdenum treatment, calcium phosphate treatment, strontium hydroxide treatment, cerium treatment, ruthenium treatment, and various chemical conversion treatments consisting of a mixture of these. On the other hand, examples of the coating type chemical conversion treatment include a method in which a coating agent having corrosion prevention properties is applied onto the barrier layer 13.
[0040] When forming at least a part of the corrosion prevention layer by any of these corrosion prevention treatments, namely, hydrothermal conversion treatment, anodizing treatment, and chemical conversion treatment, it is preferable to perform the above-mentioned degreasing treatment in advance. When using a degreased metal foil, such as a metal foil that has been subjected to an annealing process, as the barrier layer 13, there is no need to perform a degreasing treatment again in forming the corrosion prevention layers 14a and 14b.
[0041] The coating agent used in the spray-type chemical conversion treatment preferably contains trivalent chromium. The coating agent may also contain at least one polymer selected from the group consisting of cationic polymers and anionic polymers, which will be described later.
[0042] Among the above treatments, particularly in hydrothermal conversion treatment and anodization treatment, the aluminum foil surface is dissolved by a treatment agent to form an aluminum compound (boehmite, alumite) having excellent corrosion resistance. Therefore, since a bicontinuous structure is formed from the barrier layer 13 using the aluminum foil to the corrosion prevention treatment layers 14a, 14b, the above treatment is included in the definition of chemical conversion treatment. On the other hand, as described later, it is also possible to form the corrosion prevention treatment layers 14a, 14b by a pure coating method that is not included in the definition of chemical conversion treatment. As an example of this method, a method using a sol of a rare earth element oxide such as cerium oxide with an average particle size of 100 nm or less can be mentioned, which has an aluminum corrosion prevention effect (inhibitor effect) and is also environmentally friendly. By using this method, it is possible to impart a corrosion prevention effect to metal foils such as aluminum foils even with a general coating method.
[0043] Examples of the rare earth element oxide sol include sols using various solvents such as water-based, alcohol-based, hydrocarbon-based, ketone-based, ester-based, ether-based, etc. Among these, water-based sols are preferred.
[0044] In order to stabilize the dispersion of the rare earth oxide sol, inorganic acids such as nitric acid, hydrochloric acid, phosphoric acid, etc. or their salts, and organic acids such as acetic acid, malic acid, ascorbic acid, lactic acid, etc. are usually used as dispersion stabilizers. Among these dispersion stabilizers, phosphoric acid in particular is expected to (1) stabilize the dispersion of the sol, (2) improve adhesion to the barrier layer 13 by utilizing the aluminum chelating ability of phosphoric acid, and (3) improve the cohesive force of the corrosion prevention treatment layers 14a, 14b (oxide layers) by easily causing dehydration condensation of phosphoric acid even at low temperatures.
[0045] The corrosion prevention layers 14a and 14b formed from the rare earth oxide sol are aggregates of inorganic particles, and therefore may lose their cohesive strength even after the drying and curing process. Therefore, it is preferable that the corrosion prevention layers 14a and 14b in this case are compounded with an anionic polymer or a cationic polymer to compensate for the cohesive strength.
[0046] The corrosion prevention treatment layers 14a and 14b are not limited to the above-mentioned layers. For example, they may be formed using a treatment agent in which phosphoric acid and a chromium compound are mixed with a resin binder (such as aminophenol), as in the case of coating-type chromate, which is a known technology. By using this treatment agent, a layer having both corrosion prevention function and adhesion can be obtained. In addition, although it is necessary to consider the stability of the coating liquid, a coating agent in which a rare earth oxide sol and a polycationic polymer or a polyanionic polymer are mixed in advance into a one-component solution can be used to obtain a layer having both corrosion prevention function and adhesion.
[0047] The mass per unit area of the corrosion prevention layers 14a and 14b is 0.005 to 0.200 g / m2 regardless of whether the layer has a multi-layer structure or a single-layer structure. 2 is preferable, and 0.010 to 0.100 g / m 2 It is more preferable that the mass per unit area is 0.005 g / m 2 If the mass per unit area is 0.200 g / m or more, it is easy to impart a corrosion prevention function to the barrier layer 13. 2 Even if the thickness exceeds 100 mm, the corrosion prevention function does not change much. On the other hand, when a rare earth oxide sol is used, if the coating is thick, the heat curing during drying may be insufficient, which may result in a decrease in cohesive force. The thickness of the corrosion prevention layers 14a and 14b can be calculated from their specific gravity.
[0048] From the viewpoint of easily maintaining the adhesion between the sealant layer and the barrier layer, the corrosion prevention treatment layers 14a, 14b may be in an embodiment containing, for example, cerium oxide, 1 to 100 parts by mass of phosphoric acid or a phosphate relative to 100 parts by mass of the cerium oxide, and a cationic polymer, or may be formed by subjecting the barrier layer 13 to a chemical conversion treatment, or may be formed by subjecting the barrier layer 13 to a chemical conversion treatment and contain a cationic polymer.
[0049] <Inner adhesive layer 12b> The inner adhesive layer 12b is a layer that bonds the barrier layer 13, on which the second corrosion prevention treatment layer 14b is formed, to the sealant layer 16. For the inner adhesive layer 12b, a general adhesive for bonding a barrier layer and a sealant layer can be used, and for example, the same adhesive as that for the outer adhesive layer 12a described above can be used.
[0050] The thickness of the inner adhesive layer 12b is not particularly limited, but from the viewpoint of obtaining the desired adhesive strength, processability, and the like, it is preferably 1 to 10 μm, and more preferably 3 to 7 μm.
[0051] <Sealant layer 16> The sealant layer 16 is a layer that provides heat sealing to the exterior material 10. Examples of the sealant layer 16 include resin films made of polyolefin resins or polyester resins. The resins constituting the sealant layer 16 (hereinafter also referred to as "base resins") may be used alone or in combination of two or more.
[0052] Examples of polyolefin resins include low-, medium- or high-density polyethylene; ethylene-α-olefin copolymers; polypropylene; block or random copolymers containing propylene as a copolymerization component; and propylene-α-olefin copolymers.
[0053] Examples of polyester-based resins include polyethylene terephthalate (PET) resin, polybutylene terephthalate (PBT) resin, polyethylene naphthalate (PEN) resin, polybutylene naphthalate (PBN) resin, and copolymers thereof.
[0054] The sealant layer 16 may contain a polyolefin-based elastomer. The polyolefin-based elastomer may be compatible with the above-mentioned base resin or may not be compatible with it, and may contain both a compatible polyolefin-based elastomer that is compatible and a non-compatible polyolefin-based elastomer that is not compatible with it. Being compatible (compatible system) means that the elastomer disperses in the base resin with a dispersed phase size of 1 nm or more and less than 500 nm. Not being compatible (non-compatible system) means that the elastomer disperses in the base resin with a dispersed phase size of 500 nm or more and less than 20 μm.
[0055] When the base resin is a polypropylene resin, the compatible polyolefin elastomer may be, for example, a propylene-butene-1 random copolymer, and the incompatible polyolefin elastomer may be, for example, an ethylene-butene-1 random copolymer. The polyolefin elastomers may be used alone or in combination of two or more.
[0056] Furthermore, the sealant layer 16 may contain, as additive components, for example, slip agents, antiblocking agents, antioxidants, light stabilizers, flame retardants, etc. The content of these additive components is preferably 5 parts by mass or less, assuming that the total mass of the sealant layer 16 is 100 parts by mass.
[0057] The thickness of the sealant layer 16 is not particularly limited, but from the viewpoint of achieving both a thin film and improved heat seal strength in a high-temperature environment, it is preferably in the range of 5 to 100 μm, more preferably in the range of 10 to 100 μm, and even more preferably in the range of 20 to 80 μm.
[0058] The sealant layer 16 may be either a single-layer film or a multi-layer film, and may be selected depending on the required function.
[0059] Although a preferred embodiment of the exterior material for a power storage device according to the present embodiment has been described in detail above, the present disclosure is not limited to such a specific embodiment, and various modifications and variations are possible within the scope of the gist of the present disclosure as described in the claims.
[0060] For example, FIG. 1 shows a case where anti-corrosion treatment layers 14a, 14b are provided on both sides of the barrier layer 13, but only one of the anti-corrosion treatment layers 14a, 14b may be provided, or no anti-corrosion treatment layer may be provided.
[0061] While Fig. 1 shows a case in which the barrier layer 13 and the sealant layer 16 are laminated using the inner adhesive layer 12b, the barrier layer 13 and the sealant layer 16 may be laminated using an adhesive resin layer 15 as in an exterior packaging material 20 for an electricity storage device shown in Fig. 2. Furthermore, in the exterior packaging material 20 for an electricity storage device shown in Fig. 2, an inner adhesive layer 12b may be provided between the barrier layer 13 and the adhesive resin layer 15.
[0062] <Adhesive resin layer 15> The adhesive resin layer 15 is generally composed of an adhesive resin composition as a main component and additive components as necessary. The adhesive resin composition is not particularly limited, but preferably contains a modified polyolefin resin.
[0063] The modified polyolefin resin is preferably a polyolefin resin graft-modified with an unsaturated carboxylic acid derivative derived from an unsaturated carboxylic acid, an acid anhydride, or an ester thereof.
[0064] Examples of polyolefin resins include low density polyethylene, medium density polyethylene, high density polyethylene, ethylene-α-olefin copolymer, homopolypropylene, block polypropylene, random polypropylene, and propylene-α-olefin copolymer.
[0065] The modified polyolefin resin is preferably a polyolefin resin modified with maleic anhydride. For example, "Admer" manufactured by Mitsui Chemicals, Inc. and "Modic" manufactured by Mitsubishi Chemical Corporation are suitable for the modified polyolefin resin. Since such modified polyolefin resins have excellent reactivity with various metals and polymers having various functional groups, the adhesive resin layer 15 can be given adhesion by utilizing the reactivity. In addition, the adhesive resin layer 15 may contain various additives such as various compatible and incompatible elastomers, flame retardants, slip agents, antiblocking agents, antioxidants, light stabilizers, and tackifiers, as necessary.
[0066] The thickness of the adhesive resin layer 15 is not particularly limited, but from the viewpoints of stress relaxation and moisture permeability, it is preferably the same as or less than that of the sealant layer 16 .
[0067] In addition, in the exterior packaging material 20 for a storage battery device, the total thickness of the adhesive resin layer 15 and the sealant layer 16 is preferably in the range of 5 to 100 μm, and more preferably in the range of 20 to 80 μm, from the viewpoint of achieving both a thin film and improved heat seal strength in a high-temperature environment.
[0068] [Exterior material manufacturing method] Next, there will be described an example of a method for manufacturing the exterior packaging material 10 shown in Fig. 1. Note that the method for manufacturing the exterior packaging material 10 is not limited to the following method.
[0069] The manufacturing method of the exterior material 10 of this embodiment is roughly composed of a step of providing corrosion prevention treatment layers 14a, 14b on the barrier layer 13, a step of bonding the substrate 11 and the barrier layer 13 using the outer adhesive layer 12a, a step of further laminating a sealant layer 16 via the inner adhesive layer 12b to produce a laminate, and a step of aging the obtained laminate, if necessary.
[0070] (Laminating process of corrosion prevention treatment layers 14a, 14b on barrier layer 13) This step is a step of forming the corrosion prevention treatment layers 14a, 14b on the barrier layer 13. As described above, examples of the method include subjecting the barrier layer 13 to a degreasing treatment, a hydrothermal conversion treatment, an anodizing treatment, or a chemical conversion treatment, or applying a coating agent having corrosion prevention properties.
[0071] Furthermore, when the corrosion prevention treatment layers 14a, 14b are multiple layers, for example, a coating liquid (coating agent) constituting the lower corrosion prevention treatment layer (barrier layer 13 side) may be applied to the barrier layer 13 and baked to form a first layer, and then a coating liquid (coating agent) constituting the upper corrosion prevention treatment layer may be applied to the first layer and baked to form a second layer.
[0072] The degreasing treatment may be performed by spraying or immersion. The hydrothermal conversion treatment and anodizing treatment may be performed by immersion. The chemical conversion treatment may be performed by an appropriate method such as immersion, spraying, or coating, depending on the type of chemical conversion treatment.
[0073] Regarding the coating method of the coating agent having corrosion prevention properties, various methods such as gravure coating, reverse coating, roll coating, bar coating, etc. can be used.
[0074] As described above, the various treatments may be performed on either one or both sides of the metal foil, but in the case of one-sided treatment, the treated side is preferably the side on which the sealant layer 16 is laminated. If required, the surface of the substrate 11 may also be subjected to the above treatments.
[0075] The amount of coating agent applied to form the first layer and the second layer is 0.005 to 0.200 g / m 2 is preferable, and 0.010 to 0.100 g / m 2 is more preferred.
[0076] Furthermore, when dry curing is required, it can be performed at a base material temperature in the range of 60 to 300° C. depending on the drying conditions of the corrosion prevention treatment layers 14a and 14b used.
[0077] (Step of bonding the substrate 11 and the barrier layer 13) This step is a step of bonding the barrier layer 13 provided with the corrosion prevention treatment layers 14a, 14b to the substrate 11 via the outer adhesive layer 12a. The bonding method may be dry lamination, non-solvent lamination, wet lamination, or the like, and the two are bonded together using the material constituting the outer adhesive layer 12a described above. The outer adhesive layer 12a has a dry coating amount of 1 to 10 g / m 2 More preferably, the range is 2 to 7 g / m 2 It is set within the range.
[0078] (Laminating process of the inner adhesive layer 12b and the sealant layer 16) This step is a step of bonding the sealant layer 16 via the inner adhesive layer 12b to the second corrosion prevention treatment layer 14b side of the barrier layer 13. Examples of the bonding method include a wet process and dry lamination.
[0079] In the case of the wet process, a solution or dispersion of the adhesive constituting the inner adhesive layer 12b is applied onto the second corrosion prevention treatment layer 14b, and the solvent is removed at a predetermined temperature to form a dry film, or a baking process is performed as necessary after the dry film is formed. Then, the sealant layer 16 is laminated to produce the exterior material 10. Examples of the coating method include the various coating methods exemplified above. The preferred dry coating amount of the inner adhesive layer 12b is the same as that of the outer adhesive layer 12a.
[0080] In this case, the sealant layer 16 can be produced, for example, by a melt extrusion molding machine using a resin composition for forming a sealant layer that contains the above-mentioned components of the sealant layer 16. In the melt extrusion molding machine, the processing speed can be set to 80 m / min or more from the viewpoint of productivity.
[0081] (Aging process) This step is a step of aging (curing) the laminate. By aging the laminate, it is possible to promote adhesion between the barrier layer 13 / the second corrosion prevention treatment layer 14b / the inner adhesive layer 12b / the sealant layer 16. The aging treatment can be carried out at a temperature range of room temperature to 100° C. The aging time is, for example, 1 to 10 days.
[0082] In this manner, the exterior packaging material 10 of the present embodiment as shown in FIG. 1 can be manufactured.
[0083] Next, a description will be given of an example of a method for manufacturing the exterior material 20 shown in Fig. 2. Note that the method for manufacturing the exterior material 20 is not limited to the following method. The manufacturing method of the exterior material 20 of this embodiment is roughly composed of the steps of providing corrosion prevention treatment layers 14a, 14b on the barrier layer 13, bonding the substrate 11 and the barrier layer 13 together using the outer adhesive layer 12a, further laminating an adhesive resin layer 15 and a sealant layer 16 to produce a laminate, and, if necessary, heat treating the obtained laminate.
[0084] The process up to the step of bonding the substrate 11 and the barrier layer 13 can be carried out in the same manner as the manufacturing method of the packaging material 10 described above.
[0085] (Laminating Step of Adhesive Resin Layer 15 and Sealant Layer 16) This step is a step of forming an adhesive resin layer 15 and a sealant layer 16 on the second corrosion prevention treatment layer 14b formed in the previous step. The method includes a method of sand laminating the adhesive resin layer 15 together with the sealant layer 16 using an extrusion laminator. Furthermore, lamination is also possible by a tandem lamination method in which the adhesive resin layer 15 and the sealant layer 16 are extruded, or a co-extrusion method. In forming the adhesive resin layer 15 and the sealant layer 16, for example, each component is blended so as to satisfy the above-mentioned configuration of the adhesive resin layer 15 and the sealant layer 16. The above-mentioned resin composition for forming the sealant layer is used to form the sealant layer 16.
[0086] This process produces a laminate in which the layers are stacked in the following order: substrate 11 / outer adhesive layer 12a / first corrosion prevention treatment layer 14a / barrier layer 13 / second corrosion prevention treatment layer 14b / adhesive resin layer 15 / sealant layer 16, as shown in FIG. 2.
[0087] The adhesive resin layer 15 may be laminated by directly extruding the materials dry-blended to have the above-mentioned material composition using an extrusion laminator. Alternatively, the adhesive resin layer 15 may be laminated by extruding the granulated material, which has been melt-blended in advance using a melt kneading device such as a single-screw extruder, a twin-screw extruder, or a Brabender mixer, using an extrusion laminator.
[0088] The sealant layer 16 may be laminated by directly extruding the materials dry-blended to have the above-mentioned material composition as the constituents of the resin composition for forming the sealant layer using an extrusion laminator. Alternatively, the adhesive resin layer 15 and the sealant layer 16 may be laminated by a tandem lamination method in which the adhesive resin layer 15 and the sealant layer 16 are extruded using an extrusion laminator using a granulated product obtained by melt blending in advance using a melt kneading device such as a single screw extruder, a twin screw extruder, or a Brabender mixer, or by a co-extrusion method. Alternatively, a sealant monolayer may be formed in advance as a cast film using the resin composition for forming the sealant layer, and this film may be laminated together with an adhesive resin by a method of sand lamination. The forming speed (processing speed) of the adhesive resin layer 15 and the sealant layer 16 may be, for example, 80 m / min or more from the viewpoint of productivity.
[0089] (Heat treatment process) This step is a step of heat-treating the laminate. Heat-treating the laminate can improve adhesion between the barrier layer 13, the second corrosion prevention treatment layer 14b, the adhesive resin layer 15, and the sealant layer 16. As a method of heat treatment, it is preferable to treat at a temperature at least equal to or higher than the melting point of the adhesive resin layer 15.
[0090] In this manner, the exterior packaging material 20 of this embodiment as shown in FIG. 2 can be manufactured.
[0091] Although preferred embodiments of the exterior material for a power storage device according to the present disclosure have been described in detail above, the present disclosure is not limited to such specific embodiments, and various modifications and variations are possible within the scope of the gist of the present disclosure as described in the claims.
[0092] The exterior material for an electricity storage device according to the present disclosure can be suitably used as an exterior material for an electricity storage device such as, for example, a secondary battery such as a lithium ion battery, a nickel-metal hydride battery, and a lead-acid battery, and an electrochemical capacitor such as an electric double layer capacitor, etc. In particular, the exterior material for an electricity storage device according to the present disclosure is suitable as an exterior material for an all-solid-state battery using a solid electrolyte.
[0093] [Electricity storage device] FIG. 3 is a perspective view showing one embodiment of a power storage device produced using the above-mentioned exterior material. As shown in FIG. 3, the power storage device 50 includes a battery element (power storage device main body) 52, two metal terminals (current extraction terminals) 53 for extracting current from the battery element 52 to the outside, and an exterior material 10 that hermetically encloses the battery element 52. The exterior material 10 is the exterior material 10 according to the present embodiment described above. In the exterior material 10, the base material 11 is the outermost layer, and the sealant layer 16 is the innermost layer. That is, the exterior material 10 is folded in two so that the base material 11 is on the outer side of the power storage device 50 and the sealant layer 16 is on the inner side of the power storage device 50, one of which is cold-molded, and then heat-sealed to accommodate and seal the battery element 52 inside. Alternatively, one of the two exterior materials 10 may be cold-formed, and then the other exterior material 10 may be placed on top of it and heat-sealed to form a power storage device 50 that contains and seals the battery element 52 therein. Note that in the power storage device 50, an exterior material 20 may be used instead of the exterior material 10.
[0094] The battery element 52 is formed by interposing an electrolyte between a positive electrode and a negative electrode. The metal terminal 53 is a part of the current collector taken out from the exterior material 10, and is made of a metal foil such as a copper foil or an aluminum foil.
[0095] The electricity storage device 50 of this embodiment may be an all-solid-state battery. In this case, a solid electrolyte such as a sulfide-based solid electrolyte is used as the electrolyte of the battery element 52. Since the electricity storage device 50 of this embodiment uses the exterior material 10 of this embodiment, it is possible to suppress the occurrence of the base material peeling off from the barrier layer even when used in a high-temperature environment (for example, 150°C). EXAMPLES
[0096] The present disclosure will be described more specifically below based on examples, but the present disclosure is not limited to the following examples.
[0097] [Materials used] The materials used in the examples and comparative examples are shown below.
[0098] As the substrate 11, three types of films were prepared.
[0099] First, the first base material 11 is a simultaneously biaxially stretched semi-aromatic polyamide film (manufactured by Unitika Ltd., product name: Uniamide Ex, thickness: 25 μm).
[0100] The second base material 11 is a sequentially biaxially stretched easily moldable polyethylene terephthalate film (manufactured by Unitika Ltd., thickness: 25 μm).
[0101] The third substrate 11 is a polybutylene terephthalate film (manufactured by Kojin Film & Chemical Co., Ltd., product name: Boblet, thickness: 25 μm) produced by the tubular method.
[0102] Next, as the urethane-based adhesive to be used for the outer adhesive layer 12a, a polyester urethane-based adhesive was used which was prepared by mixing polyester urethane: polyester polyol (manufactured by Toyo Morton, product name: TMK-55) and isocyanate (TDI-adduct, manufactured by Toyo Morton, product name: CAT-10L) and diluting it with a solvent.
[0103] As the barrier layer 13, an aluminum foil (thickness: 40 μm) having anti-corrosion treatment layers on both sides was used.
[0104] An acid-modified polypropylene resin was used as the resin for the adhesive resin layer 15. The thickness of the adhesive resin layer was 27 μm.
[0105] Polypropylene resin was used as the resin for the sealant layer 16. The thickness of the sealant layer 16 was 53 μm.
[0106] [Creating exterior materials] Example 1 First, one side of the barrier layer, which had anti-corrosion treatment layers on both sides, was attached to the substrate using a polyester urethane adhesive (outer adhesive layer) by dry lamination. The barrier layer and substrate were laminated by applying the polyester urethane adhesive to one side of the barrier layer, drying it at 80°C for 1 minute, laminating it with the substrate, and aging it at 80°C for 120 hours.
[0107] Next, the barrier layer and the sealant layer were bonded together using a sand lamination method, that is, a molten acid-modified polypropylene resin was extruded between the barrier layer and the sealant layer, and the whole was pressure-bonded to be integrated.
[0108] (Examples 2 and 3 and Comparative Examples 1 to 3) Exterior materials of Examples 2 and 3 and Comparative Examples 1 to 3 (laminates of substrate / outer adhesive layer / first corrosion prevention treatment layer / barrier layer / second corrosion prevention treatment layer / inner adhesive layer / sealant layer) were prepared in the same manner as in Example 1, except that the substrate and / or outer adhesive layer was changed to the configuration shown in Table 1.
[0109] [Measurement of elongation by creep test] The three types of substrates were cut to prepare samples with a length of 20 mm and a width of 10 mm. The first type of sample had the length direction in the MD direction and the width direction in the TD direction.
[0110] A constant load of 5N was applied to the sample for 3 hours in a 150°C environment using a thermomechanical analyzer (product name: DMA7100) manufactured by Hitachi High-Tech Science Corporation, and the amount of elongation (MD elongation) was measured.
[0111] Next, a sample 20 mm long and 10 mm wide was similarly prepared with the TD direction as the length direction and the MD direction as the width direction, and a constant load of 5 N was applied to the sample for 3 hours in a 150°C environment, and the amount of elongation (TD direction elongation) was measured.
[0112] [Evaluation of deformation of electricity storage device in 150℃ environment] The exterior materials of Examples 2 and 3 and Comparative Examples 1 to 3 were cut into rectangular shapes of 120 mm in the TD direction × 200 mm in the MD direction, and placed in a molding device so that the sealant layer faced upward. The molding depth of the molding device was set to 4.0 mm, the holding pressure was set to 0.8 MPa, and cold molding was performed in an environment of room temperature 23 ° C and dew point temperature -35 ° C. The punch mold had a rectangular cross section of 80 mm × 70 mm, a punch radius (RP) of 1 mm on the bottom, and a punch corner radius (RCP) of 1 mm on the side. The die mold had a die radius (RD) of 1 mm on the upper surface of the opening. The clearance between the punch mold and the die mold was 170 μm. The molding area was approximately the center of one half of the cut exterior material divided at approximately the center in the longitudinal direction (MD direction), and the longitudinal direction of the punch mold was aligned with the TD direction of the exterior material.
[0113] The electricity storage device thus manufactured was stored in an environment of 150° C. for one week, and then returned to room temperature and visually inspected for its appearance. The evaluation criteria were as follows: A: There was no change in appearance before and after storage. B: After storage, some parts swelled and became deformed. C: After storage, the product swelled and deformed overall.
[0114] [Evaluation of moldability] The exterior materials of Examples 2 and 3 and Comparative Examples 1 to 3 were cold-molded and evaluated for the presence or absence of pinholes and cracks. The number of samples was 10. The molding conditions were as described above. The evaluation criteria were as follows. A: Neither pinholes nor cracks were found in any of the 10 exterior materials. B: Neither pinholes nor cracks occurred in 8 or more exterior materials. C: Pinholes and / or cracks occurred in three or more exterior materials.
[0115] [Evaluation of peel resistance in a 150℃ environment] The exterior materials of Examples 2 and 3 and Comparative Examples 1 to 3 were cold-molded and stored in an environment of 150°C for 3 days, and then measured by a 90-degree peel test using a tensile tester (manufactured by Shimadzu Corporation) at a tensile speed of 50 mm / min. The evaluation criteria were as follows: A: Peel strength is 1N / 15mm or more. C: The peel strength is less than 1N / 15mm.
[0116] [Table 1] [Explanation of symbols]
[0117] Reference Signs List 10: Exterior material for power storage device 11: Substrate 12a: Outer adhesive layer 12b: Inner adhesive layer 13: Barrier layer 14a: First corrosion prevention treatment layer 14b: Second corrosion prevention treatment layer 15: Adhesive resin layer 16: Sealant layer 20...Exterior materials for power storage devices 50...electricity storage device, 52...battery element, 53...metal terminal
Claims
1. An exterior material for an electricity storage device comprising at least a substrate, an outer adhesive layer, a barrier layer, and a sealant layer in this order, The exterior material for a storage battery device is characterized in that the substrate has a single layer structure and is made of semi-aromatic polyamide, and when a sample of 20 mm in length and 10 mm in width is prepared from the substrate alone and a creep test is conducted on the sample by applying a constant load of 5 N for 3 hours in an environment of 150°C, the amount of elongation in both the MD direction and the TD direction is 3 mm or less.
2. 2 . The packaging material for an electricity storage device according to claim 1 , wherein a difference between the amount of elongation in the MD direction and the amount of elongation in the TD direction is 2 mm or less.
3. 3. The packaging material for an electricity storage device according to claim 1, wherein the substrate is a biaxially oriented film.
4. 4. The exterior packaging material for an electricity storage device according to claim 1, wherein the outer adhesive layer is made of polyester polyurethane.
5. The exterior material for a storage battery device according to any one of claims 1 to 4, which is for an all-solid-state battery.
6. A power storage device main body; a current extracting terminal extending from the power storage device body; The exterior material for an electricity storage device according to any one of claims 1 to 5, which holds the current extracting terminal and houses the electricity storage device main body; A power storage device comprising:
Citation Information
Patent Citations
External facing material for power storage device
JP2013101765A
Composite film and its manufacturing method
JP2016524552A
Cast polypropylene-based film and outer package material for power storage device, including the same as sealant layer
JP2019029221A
Battery packaging material, method of producing the same and battery
JP2019071262A
Layered body, bag, and lithium ion cell
WO2016148071A1