Friction charging unit, and friction power generation device and dust collection device equipped with said friction charging unit
Vinyl chloride resin is used as a negatively charged member to address the durability limitations of PTFE, enhancing triboelectric charging properties and durability for improved dust collection and power generation devices.
Patent Information
- Application Number
- JP2020118268
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-09-18
- Filing Date
- 2020-07-09
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2040-07-09
AI Technical Summary
Fluorine-containing resins like PTFE exhibit excellent triboelectric charging properties but lack sufficient durability, limiting their practical application in devices requiring both high charging efficiency and durability.
Employing vinyl chloride resin as the negatively charged member, which offers comparable triboelectric charging properties to PTFE while providing enhanced durability, through specific thickness and Vicat softening temperature ranges, and optionally incorporating additives for improved performance.
The vinyl chloride resin-based triboelectric charging unit achieves higher durability and charging efficiency, enabling effective dust collection and power generation with reduced maintenance needs.
Smart Images

Figure 0007567237000003 
Figure 0007567237000004 
Figure 0007567237000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a friction charging unit capable of charging an electric charge generated by friction. [Background technology]
[0002] Conventionally, a member has been charged by friction to collect fine dust in the air or to remove dirt from the member. For example, Patent Document 1 discloses a dust collection device that electrostatically collects dust using a dust collection plate that has been charged by friction.
[0003] In Patent Document 1, combinations of acrylic and nylon, and polyester and nylon are exemplified as the dust collecting plate and friction plate used in the dust collecting device, and it is said that the further away they are in the triboelectric series, the greater the charging force, making them preferable. Therefore, for dust collecting members that are charged by friction, PTFE (polytetrafluoroethylene) resin has almost always been used as a negatively charged material, because PTFE resin is the most likely to be negatively charged in the triboelectric series. (See Non-Patent Document 1.)
[0004] Therefore, it is understood that it is preferable to use PTFE resin as the negatively charged member because it can maximize the amount of charge when combined with any positively charged member for frictional charging. On the other hand, nylon is typically used as the positively charged member. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2002-336733 A [Non-patent literature]
[0006] [Non-Patent Document 1] Electrostatic Doctor "Charging Series", [online], Keyence Corporation, [Retrieved April 22, 2019], Internet <URL:https: / / www.keyence.co.jp / ss / products / static / static-electricity / basic / nature.jsp Summary of the Invention [Problem to be solved by the invention]
[0007] However, although fluorine-containing resins such as PTFE have excellent triboelectric charging properties, their durability is not sufficient. An object of the present invention is to provide a triboelectric charging unit that can achieve both triboelectric charging properties and durability. [Means for solving the problem]
[0008] The inventors of the present invention investigated materials that have the same level of triboelectric charging properties as when PTFE is used as a negatively charged member, while at the same time having durability equal to or greater than that of PTFE. They surprisingly found that the above-mentioned problems could be solved by using, as a negatively charged member, vinyl chloride resin, which is thought to have significantly inferior triboelectric charging properties as compared to PTFE, because its distance from a positively charged member is smaller in terms of the triboelectric charging order, and thus they arrived at the present invention. Furthermore, it has been found that by using a vinyl chloride resin having specific properties as a negatively charged member, it is possible to obtain a member having higher durability and superior charging properties.
[0009] The present invention includes the following. [1] A positively charged member and a negatively charged member arranged so as to be in contact with the positively charged member, a friction charging unit capable of charging by friction between the positively charged member and the negatively charged member, The negatively charged member is made of vinyl chloride resin. [2] The friction-charging unit according to [1], wherein the negatively charged member has a thickness of 0.1 μm or more and 5 mm or less. [3] The negatively charged member is made of a vinyl chloride resin having a Vicat softening temperature of 75° C. or higher. [1 ] or [2]. [4] The friction-charging unit according to any one of [1] to [3], wherein the negatively charged member is a coating-molded resin body. [5] A dust-collecting device comprising the frictional charging unit according to any one of [1] to [4]. [6] A power generating device comprising the friction charging unit described in any one of [1] to [4]. Effect of the Invention
[0010] According to the present invention, it is possible to provide a friction-charging unit having a negatively charged member and a positively charged member that generate high dust collection capacity. In a preferred embodiment, it is possible to provide a friction-charging unit that is more durable and has excellent charging properties. Furthermore, it is possible to provide a dust collection device or a power generation device that uses the friction-charging unit. [Brief description of the drawings]
[0011] [Figure 1] FIG. 1 is a schematic diagram showing an embodiment of a power generation device including a friction charging unit. [Diagram 2] 1A to 1C are schematic diagrams illustrating an example of a method for producing a negatively charged material-coated film body. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The present invention will be described in detail below. However, the description of the constituent elements described below is one example (representative example) of an embodiment of the present invention, and the present invention is not limited to these contents, and can be implemented in various modifications within the scope of the gist of the present invention.
[0013] One embodiment of the present invention is a friction charging unit that has a positively charged member and a negatively charged member arranged so as to be in contact with the positively charged member, and that can be charged by friction between the positively charged member and the negatively charged member, and uses vinyl chloride resin as the negatively charged member. A positively charged member and a negatively charged member generate and become charged by sliding against each other and / or by repeatedly coming into contact and separating from each other. In this embodiment, vinyl chloride resin is used for the negatively charged member that charges the negative charge generated by friction. The generation of charge by such sliding and such contact and separation is referred to as "friction."
[0014] The positively charged member is not particularly limited as long as it can negatively charge the negatively charged member, and it is only necessary to avoid materials that are likely to be negatively charged themselves when combined with the vinyl chloride resin used as the negatively charged resin. Typically, nylon is used, but this is not limited thereto.
[0015] The present invention will now be described with reference to specific embodiments shown in the drawings. Fig. 1 shows an embodiment in which a frictional charging unit of the present invention is applied to a frictional power generation device. In the friction power generation device 10, a positively charged member 3 is supported on a substrate 1 for a positively charged member, and a negatively charged member 4 is supported on a substrate 2 for a negatively charged member. The positively charged member 3 and the negatively charged member 4 are not fixed, and as the positively charged member 3 and the negatively charged member 4 slide against each other and / or as the positively charged member 3 and the negatively charged member 4 repeatedly come into contact with and separate from each other, a positive charge is generated in the positively charged member 3 and a negative charge is generated in the negatively charged member 4. The friction between the positively charged member 3 and the negatively charged member 4 may be generated by moving the positively charged member 3 and the negatively charged member 4 using a known driving method.
[0016] The substrates 1 and 2 that support the charging members are conductive members, and the generated electricity can be taken out from the wiring 5 electrically connected to the substrates 1 and 2. When the heater is used as a dust collecting device, one end of the wiring electrically connected to the substrate may be earthed. The substrate 1 and the substrate 2 are not necessarily required, but are preferably provided in terms of handling and the like. In addition, there are no particular limitations as long as they have sufficient strength to support the charging member. In addition, an adhesive layer may be provided between the substrate and the charging member. In this case, the adhesive layer may be provided for the purpose of improving adhesion to the substrate, etc.
[0017] The negatively charged member 4 is made of vinyl chloride resin, and may be a laminate of vinyl chloride resin and other members, so long as at least the outermost layer in contact with the positively charged member 3 is made of vinyl chloride resin. The positively charged member 3 is not particularly limited as long as it is a member that can negatively charge the vinyl chloride resin used as the negatively charged member 4, and is typically nylon. The positively charged member 3 may be in the form of a film, or in the form of a brush in order to increase the amount of static electricity generated.
[0018] The vinyl chloride resin is a polymeric compound obtained by the polymerization reaction of vinyl chloride (chloroethylene), and is preferably a polymeric compound obtained by subjecting vinyl chloride resin to a chlorination treatment, which provides a high Vicat softening temperature. The weight average molecular weight is generally 3000 or more. In particular, when considering abrasion resistance, it is preferably 10000 or more.
[0019] The vinyl chloride resin is preferably stronger than Teflon (registered trademark) (fluororesin), and specifically, since the Shore D hardness of normal Teflon (registered trademark) (fluororesin) is about 50 to 55, it is preferable that the resin has a higher Shore D hardness than this, and preferably has a Shore D hardness of 55 or more, and more preferably 60 or more. There is no particular upper limit, but it is usually 85 or less.
[0020] The vinyl chloride resin used in the present invention has a Vicat softening temperature of preferably 75° C. or higher, more preferably 78° C. or higher, and even more preferably 90° C. or higher. Although there is no particular upper limit, a resin having a Vicat softening temperature of 140° C. or lower is usually used, and preferably a resin having a temperature of 130° C. or lower. By setting the temperature within the above range, the chlorination rate of the chlorine contained in the resin tends to be high, which is preferable because it induces high negative triboelectric series characteristics and makes it easy to impart high triboelectric voltage and dust collection characteristics. More preferred specific structures include chlorinated polyvinyl chloride resins described in International Publication No. 2013 / 081133 and on page 74 of the non-patent document "PVC Fact Book" (published in February 2005 by the PVC Industry and Environment Association), which are preferred because they tend to achieve a high Vicat softening temperature of 80°C or higher.
[0021] If the Vicat softening temperature is significantly lower than 75°C, the moldability is excellent, but the chlorination rate is likely to be low, the negative triboelectric series characteristics are degraded, and the triboelectric charging characteristics are likely to be degraded. On the other hand, if the Vicat softening temperature is significantly higher than 140°C, the moldability is significantly degraded and thin film molding is difficult. In addition, a resin other than polyvinyl chloride can be blended as a method to obtain a high Vicat softening temperature, but the chlorination rate decreases as the resin is blended, and the triboelectric charging characteristics are likely to be degraded. The Vicat softening temperature is measured in accordance with JIS K7206. Unless there are particular problems, the B50 method is used.
[0022] In addition, auxiliary compounds may be added to the vinyl chloride resin within the range in which the characteristics of the present invention can be obtained. Plasticizers, fillers, lubricants, stabilizers, and further flame retardants, antioxidants, ultraviolet absorbers, etc. may also be added. As plasticizers, phthalates, adipates, epoxidized soybean oil (ESBO), etc. can be used. Although it depends on the molecular weight of the polyvinyl chloride resin that is the matrix, in order to achieve high abrasion resistance, the amount of additive should be 10% or less of the polyvinyl chloride resin. It is preferable that there is. As the filler, various pigments can be added to achieve the desired design. If the color is to be mainly white, calcium carbonate, titanium oxide, talc and other silicon-based compounds can be used. As the lubricant, those generally added such as hydrocarbon-based lubricants, fatty acid amides, fatty acid esters, and fatty acids may be used. As the stabilizer, lead-based, tin-based, zinc-based, etc. are used, and examples thereof include dibutyltin compounds and dioctyltin compounds.
[0023] Next, a manufacturing example of a vinyl chloride resin member which is a negatively charged member will be described. The shape of the vinyl chloride resin used as the negatively charged member in this embodiment is not particularly limited, but it is generally used in the form of a film having a thickness of 5 mm or less, but is not particularly limited and may be 2 mm or less. The lower limit is also not limited, and is usually 0.1 μm or more, may be 1 μm or more, or may be 5 μm or more. Particularly preferably, the film thickness is 0.1 mm or more and 1 mm or less, and further preferably, 0.3 mm or more and 0.8 mm or less, which tends to improve the charging characteristics.
[0024] The method for producing the vinyl chloride resin member can be a commonly known method and is not particularly limited. In order to form a film, compression molding, injection molding, coating molding, etc. can be used, but a vinyl chloride resin coated molded body in which a solvent or solventless vinyl chloride resin negatively charged material coating solution is applied to a substrate 1 or a temporary substrate at room temperature to 200°C, preferably room temperature to 150°C, is preferable because it has excellent in-plane uniformity that is effective for improving dust collection characteristics using frictional charging, and is particularly advantageous in terms of wear resistance when rubbed against a positively charged member for a long time, and can be obtained in a large area in a short time.
[0025] An example of a method for producing polyvinyl chloride resin using the coating molding method is shown in Figure 2. In the resin sheet deposition apparatus 20 shown in FIG. 2, a slit coater 22 is disposed on a substrate 24. The slit coater 22 or substrate 24 is movable horizontally in the drawing, and the negatively charged material coating solution 21 introduced into the slit coater is dripped onto the substrate 24 while the slit coater 22 or substrate 24 is moved horizontally in the drawing, thereby coating the negatively charged material coating solution onto the substrate 24. The coated negatively charged material coating solution is heated and / or dried as necessary to evaporate the solvent and harden, becoming a negatively charged sheet 25 (molded body). Thereafter, the negatively charged sheet laminate 23 is cut into a desired size by a cutting machine 26, and a negatively charged sheet laminate 23 is obtained that is individualized into a desired size.
[0026] The slit coater 22 may be any coating device capable of coating the coating solution on the substrate 24, such as a die coater or a roll coater. The negatively charged material coating solution may be prepared by dissolving the resin constituting the negatively charged material in an organic solvent, or may be prepared by dissolving the resin constituting the negatively charged material by heat. In this embodiment, the negatively charged material is vinyl chloride resin. Furthermore, the negatively charged sheet 25 may be stretched by a roll or tenter type stretching machine as necessary.
[0027] For example, when producing a biaxially stretched film, a vinyl chloride resin raw material is molten and extruded from a die in an extruder, and the molten sheet is cooled and solidified by a cooling roll to obtain an unstretched sheet. In this case, it is preferable to increase the adhesion between the sheet and the cooling roll in order to improve the flatness of the sheet, and an electrostatic application adhesion method or a liquid application adhesion method is preferably adopted.
[0028] Next, the unstretched sheet is stretched in one direction by a roll or tenter type stretching machine. The stretching temperature is usually 70 to 120° C., preferably 80 to 110° C., and the stretching ratio is usually 1.1 to 7 times, preferably 2 to 6 times. Next, the film is stretched in a direction perpendicular to the first-stage stretching direction, usually at 70 to 170°C, at a stretch ratio of usually 1.1 to 7 times, preferably 2 to 6 times. This is followed by heat treatment at a temperature of 80 to 270°C under tension or relaxation of 30% or less to obtain a biaxially oriented film. In the above stretching, a method of performing unidirectional stretching in two or more stages can also be adopted.
[0029] The principle of triboelectric generation will be described using as an example a friction generator that utilizes charging due to friction in a friction-charged dust collection unit, which is one embodiment of the present invention. The friction generator has a structure in which a pair of electrode members having an electrode and a charged member face each other. When the surfaces of the facing charged members slide against each other or repeatedly come into contact and separate, their surface layers are charged with opposite polarities. When the charged members repeatedly come into contact and separate, the electric fields formed by the positive and negative charges on the outside cancel each other out when the charged members are in contact with each other, so the potential difference between the electrodes is equal. When the charged members separate from each other, a potential difference occurs between the two electrodes. When the two electrodes are electrically connected via a load resistor, charges flow through the connection. The charges flow until the potential difference between the electrodes becomes zero, and this flow becomes a current.
[0030] When the charging caused by friction is utilized for dust collection, at least a negatively charged member and a positively charged member for charging the negatively charged member are provided. The sliding surface of the charging member becomes charged by friction between the surface of the charging member and the friction body, and this charged surface can be used to collect charged particles in the air. In addition, the negatively charged member preferably has releasability so that the charged particle aggregate in the air captured on the negatively charged member can be removed from the negatively charged member by the physical stimulation of the positively charged member.
[0031] The above-mentioned device using the friction charging unit of this embodiment is preferable because it has superior durability to conventional friction charging units that use PTFE as a negatively charged member, and therefore can reduce the frequency of replacement of the charging member. Furthermore, the frictional charging unit of this embodiment can also be used as a power generation source for a frictional power generation device, a power generation source for a sensor, a dust collection member for a dust collection device, and the like. Even when it is used as the power generation source for a sensor, it has a structure in which a pair of electrode members having an electrode and a charged member face each other, similar to the power generation source for a friction generator. It can also be used as a sensor by detecting, as a signal, the electric charge that flows when the surfaces of the charged members of the electrode members slide against each other or repeatedly come into contact and separate from each other. EXAMPLES
[0032] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the specific examples. <Example 1> As a negatively charged member, a PVC standard calibration plate (polyvinyl chloride resin) that is an accessory of a Sanhayato Co., Ltd. digital static electricity detector (static voltage measuring meter) with a thickness of 0.5 mm, width of 1.5 cm, length of 10 cm, and one end formed into a semicircular shape was used to perform the dust collection evaluation and static voltage strength evaluation described below.
[0033] <Comparative Example 1> As a negatively charged member, a PTFE resin member of "PTFE sheet" by Chukoh Chemical Industry Co., Ltd., measuring 1 mm in thickness, 1.5 cm in width, and 10 cm in length with one end formed into a semicircular shape, was used to perform the dust collection evaluation and static charge voltage strength evaluation described below.
[0034] <Method for evaluating triboelectric voltage> The negatively charged member of Example 1 was placed on an aluminum substrate (Al substrate) with a width of 200 mm and a length of 200 mm that was connected to earth, the non-semicircular end of the negatively charged member was connected to earth, and a weight of 73 g, a width of 20 mm, and a length of 50 mm was placed on the portion of the negatively charged member that was 5 cm from the semicircular end, after which the negatively charged member was held at the earthed end and with the weight placed on it, The negatively charged member was moved 40 mm at 10 mm per second. Next, the negatively charged member together with the weight was lifted away from the Al substrate, and after the weight was removed from the negatively charged member, the triboelectric voltage was measured at a portion 25 mm from the semicircular end of the surface of the negatively charged member that had been in contact with the aluminum using a static electricity voltage measuring instrument. This measurement operation was carried out within 10 seconds from the removal of the negatively charged member with the weight on it from the Al substrate to the end of the triboelectric voltage measurement. The results are shown in Table 1.
[0035] The triboelectric voltage was measured using the negatively charged member of Comparative Example 1 instead of the negatively charged member of Example 1. The results are shown in Table 1.
[0036] <Dust collection strength evaluation method> Similarly, at a temperature of 25°C and a humidity of 60%, a "Lawson Select" paper film manufactured by Oji Nepia Co., Ltd., weighing 53 mg, 30 mm wide and 150 mm long, was placed on the Al substrate used in the frictional charging voltage evaluation method, and one end was fixed with paper tape. The end of the film on the side that was not fixed and the film section up to 5 cm from the end were placed over the surface of the negatively charged member that had been charged in the same manner as in the frictional charging voltage evaluation method, the semicircular end and the section up to 50 mm from the end, which had been in contact with the Al substrate surface, and the negatively charged member was then raised at a speed of 10 mm per second. The end of the paper film adheres to the negatively charged member and is lifted up together with it, but as the paper film is lifted up, the weight of the paper increases, causing it to separate from the negatively charged member. The height of the negatively charged member at that time (adherence height) The results are shown in Table 1.
[0037] [Table 1]
[0038] As is clear from Table 1, the polyvinyl chloride resin plate can achieve a higher charging voltage than the PTFE resin plate, which is used in conventional products and whose charging order is considered to be on the more negative potential side, under the same film thickness and sliding conditions. Furthermore, with regard to component life, it is clear without even needing to conduct experiments that polyvinyl chloride resin is cheaper than PTFE, which is expensive and has limitations on how thick it can be made, and a wide range of types have been developed that offer flexibility and hardness, making it possible to appropriately select the thickness and other physical properties required for long life. Therefore, when used as a negatively charged component, for example for dust collection purposes, it is expected to collect more dust and have a longer life.
[0039] <Examples 2 to 6> As a negatively charged member, a vinyl chloride resin sheet having a thickness of 0.5 mm to 1.0 mm as shown in Table 2 below was used to prepare a negatively charged member sample having a width of 1.5 cm and a length of 10 cm, with one end formed into a semicircular shape, and the electrostatic charge voltage strength and dust collection were evaluated.
[0040] <Evaluation method for triboelectric voltage strength 2> -Measurement of triboelectric voltage of negatively charged sample: At a temperature of 25°C and a humidity of 40%, a Sanhayato Corporation digital static electricity detector EG-1 (static voltage measuring instrument) with an earthed case and a negatively charged sample were prepared. The negatively charged sample was placed on an aluminum substrate (Al substrate) that was 200 mm long and connected to earth, and the non-semicircular end of the negatively charged sample was connected to earth. An acrylic static elimination brush was used that was grounded to the part of the material that was 5 cm from the semicircular end of the negatively charged sample, and the brush was moved 50 mm at 10 mm per second so that the middle part of the brush bristles pressed the negatively charged sample with 100 g. This friction operation was repeated 15 times to make the sample saturated with electricity. Next, the negatively charged sample was lifted off the Al substrate and left for 1 minute, after which the triboelectric voltage was measured using a static electricity voltage measuring instrument at a portion 25 mm from the semicircular edge of the surface of the negatively charged sample that had been in contact with the aluminum. The measurement results are shown in Table 2.
[0041] The triboelectrically charged voltage values of the negatively charged samples of Examples 2 to 6 were divided by the triboelectrically charged voltage value of the negatively charged sample of Example 6 to determine the relative triboelectrically charged voltage. A higher evaluation value indicates higher charging characteristics. The measurement results are shown in Table 2.
[0042] <Dust collection strength evaluation method 2> Similarly, at a temperature of 25°C and a humidity of 40%, a paper film "Lawson Select" manufactured by Oji Nepia Co., Ltd., weighing 53 mg, 30 mm wide and 150 mm long, was placed on the Al substrate used in the frictional charging voltage strength evaluation method, and one end was fixed with paper tape. The end of the film on the side that was not fixed and the film section up to 5 cm from the end were placed on the surface of the negatively charged sample that had been charged in the same manner as in the frictional charging voltage strength evaluation method, which had been in contact with the Al substrate surface, and the negatively charged member sample was then raised at a speed of 10 mm per second. The end of the paper film was placed on the semicircular end of the negatively charged member sample and the section up to 50 mm from the end. The end of the paper film was attached to the negatively charged member sample and lifted up together with it, but as the height increased, it separated from the negatively charged member sample. The height at which the paper film and the negatively charged member sample separated (attachment height) was Measured. Next, the charging voltage and the adhesion height of the negatively charged member sample in Examples 2 to 5 were divided by the charging voltage (-7 kV) and the adhesion height (6.5 cm) of the negatively charged member sample in Example 6 to obtain the relative dust collection strength. The higher the evaluation value, the higher the dust collection characteristics. The measurement results are shown in Table 2.
[0043] [Table 2]
[0044] From these results, it is understood that the higher the Vicat softening temperature, the higher the charging voltage and the better the dust collection rate. The reason for this is that the chlorine introduced into the ethenyl skeleton of PVC resin bonds to the carbon on the ethenyl skeleton. When these two chlorines are combined, they form a carbon-chlorine group with high polarity, or a chlorine-carbon-chlorine group with two chlorines bonded to one carbon. These highly polar groups have strong mutual interactions, so they suppress movements such as rotation and vibration between polyvinyl chloride resin molecules, resulting in an increase in the Vicat softening temperature. On the other hand, the increase in the negative polarity of the chlorine generates high negative triboelectric series characteristics for the polyvinyl chloride resin, which in turn increases the triboelectric series difference with the triboelectric charging brush, resulting in a high triboelectric voltage and high dust collection characteristics. [Explanation of symbols]
[0045] 10 Power generation devices 1, 2 Base material 3 Positively charged member 4 Negatively charged member 5. Wiring 20 Resin sheet deposition device 21 Negatively charged material coating solution 22 Slit Coater 23 Negatively charged sheet laminate 24 Base material 25 Negatively charged sheet 26 Cutting machine
Claims
1. A friction charging unit having a positively charged member and a negatively charged member arranged so as to be in contact with the positively charged member, the friction charging unit being capable of charging the positively charged member by friction between the positively charged member and the negatively charged member, the positively charged member is in the form of a film, The negatively charged member is a film-shaped vinyl chloride resin having a Vicat softening temperature of 75° C. or higher.
2. A frictional charging unit as described in claim 1, wherein the positively charged member is supported on a substrate for a positively charged member, the negatively charged member is supported on a substrate for a negatively charged member, and the substrate is a conductive member.
3. 3. The frictional charging unit according to claim 1, wherein the negatively charged member has a thickness of 0.1 μm or more and 5 mm or less.
4. 4. The frictional charging unit according to claim 1, wherein the negatively charged member is a coating-molded resin body.
5. A dust-collecting device comprising the friction charging unit according to any one of claims 1 to 4.
6. A power generation device comprising the friction charging unit according to any one of claims 1 to 4.
Citation Information
Patent Citations
JP1973102224U
Window for car
JP1984182731A
Dust collector and air conditioner having the dust collector mounted thereon
JP2002336733A
Sucking utensil for vacuum cleaner and vacuum cleaner using the same
JP2003304990A
Developer for hybrid development and image forming apparatus
JP2010026388A