Inkjet textile printing ink
The core-shell structured inkjet textile ink with polyester resin and unopened oxazoline groups in the shell layer addresses ejection stability and washing fastness issues, ensuring stable and durable prints.
Patent Information
- Application Number
- JP2020128441
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-07-29
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2040-07-29
AI Technical Summary
Existing inkjet textile printing inks lack sufficient ejection stability and washing fastness.
The inkjet textile ink contains colored particles with a core-shell structure, where the core includes polyester resin and dye, and the shell layer is made of a specific resin with unopened oxazoline groups and amide ester groups, enhancing adhesion through covalent bonding.
The ink achieves excellent ejection stability and washing fastness by preventing dye dissolution and improving adhesion to the textile.
Smart Images

Figure 0007567254000001 
Figure 0007567254000002 
Figure 0007567254000003
Abstract
Description
[Technical field]
[0001] The present invention relates to an ink for ink-jet textile printing. [Background technology]
[0002] Inkjet printing inks are required to have excellent discharge stability and to be able to form printed items with excellent washing fastness. In order to form printed items with excellent washing fastness, for example, inkjet printing inks containing colored particles having a core-shell structure have been proposed (Patent Document 1). In addition, in order to form printed items with excellent washing fastness, for example, a method has been proposed in which an inkjet printing ink containing an unopened ring-containing oxazoline group-containing polymer is printed, and then the formed printed item is heated to crosslink the unopened ring-containing oxazoline group-containing polymer (Patent Document 2). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] WO 2003 / 55951 [Patent Document 2] JP 2000-109733 A Summary of the Invention [Problem to be solved by the invention]
[0004] However, the inkjet textile printing inks described in Patent Documents 1 and 2 do not have sufficient ejection stability.
[0005] The present invention has been made in consideration of the above problems, and an object of the present invention is to provide an ink-jet textile printing ink that has excellent ejection stability and is capable of forming a printed item that has excellent washing fastness. [Means for solving the problem]
[0006] The inkjet printing ink according to the present invention contains colored particles and an aqueous medium. The colored particles have a core and a shell layer covering the core. The core contains a polyester resin and a dye. The shell layer contains a specific resin having an unopened oxazoline group and an amide ester group. Effect of the Invention
[0007] The inkjet textile printing ink according to the present invention is excellent in ejection stability and can form printed textiles that are excellent in washing fastness. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] Hereinafter, an embodiment of the present invention will be described. In this specification, the volume median diameter (D 50 ) is a value measured using a dynamic light scattering particle size distribution analyzer (e.g., Zetasizer Nano ZS manufactured by Malvern Instruments) unless otherwise specified. Acrylic and methacrylic may be collectively referred to as "(meth)acrylic". Each component described in this specification may be used alone or in combination of two or more.
[0009] <Inkjet textile printing ink> An inkjet printing ink (hereinafter, sometimes referred to as ink) according to an embodiment of the present invention contains colored particles and an aqueous medium. The colored particles have a core and a shell layer that covers the core. The core contains a polyester resin and a dye. The shell layer contains a specific resin having an unopened oxazoline group and an amide ester group.
[0010] The ink of the present invention is suitable as an ink for use in direct printing (printing in which ink is directly ejected onto a printing object). The printing object using the ink of the present invention may be a woven fabric or a knitted fabric. Examples of the printing object include cotton fabric, silk fabric, linen fabric, acetate fabric, rayon fabric, nylon fabric, polyurethane fabric, and polyester fabric. The colored particles contained in the ink of the present invention contain a polyester resin, and therefore have excellent affinity with polyester fabrics. Therefore, polyester fabrics are preferred as the printing object.
[0011] The ink of the present invention, by being provided with the above-mentioned configuration, can form a printed item having excellent ejection stability and excellent washing fastness. The reason is presumed to be as follows. The ink of the present invention contains colored particles having a core-shell structure. Since the dye-containing core of the colored particles is covered with a shell layer, the dye is not exposed on the surface of the colored particles. Therefore, the dye is less likely to be dissolved in the printed item formed by the ink of the present invention during washing. In addition, the specific resin contained in the shell layer has an unopened ring oxazoline group. The unopened ring oxazoline group of the specific resin reacts with a carboxyl group present on the surface of the printed item to form a covalent bond, thereby improving the adhesion between the printed item and the colored particles. From the above, the printed item formed by the ink of the present invention has excellent washing fastness. Here, the colored particles are formed, for example, by treating the core with a polymer containing an unopened ring oxazoline group. The polymer containing an unopened ring oxazoline group has the property of undergoing a gradual crosslinking reaction even at room temperature. Therefore, the ink containing the unopened oxazoline group-containing polymer itself tends to have a decreased ejection stability due to the aggregation of the unopened oxazoline group-containing polymer. On the other hand, in the ink of the present invention, the specific resin contained in the shell layer is covalently bonded to the polyester resin contained in the core. Therefore, in the ink of the present invention, the specific resin is fixed to the colored particles and is not free in the aqueous medium. Also, in the ink of the present invention, the specific resin is unlikely to undergo a crosslinking reaction because a part of the unopened oxazoline group is consumed to form the above-mentioned covalent bond. For the above reasons, the specific resin contained in the ink of the present invention is unlikely to aggregate. Therefore, the ink of the present invention has excellent ejection stability.
[0012] In the ink of the present invention, the content of unopened ring oxazoline groups measured by gas chromatography mass spectrometry is preferably 30 μmol / g or more and 100 μmol / g or less, more preferably 40 μmol / g or more and 60 μmol / g or less. By making the content of unopened ring oxazoline groups 30 μmol / g or more, the adhesion between the colored particles and the object to be printed can be improved. As a result, the washing fastness of the printed material formed by the ink of the present invention can be further improved. By making the content of unopened ring oxazoline groups 100 μmol / g or less, the aggregation of the colored particles can be suppressed. As a result, the ejection stability of the ink of the present invention can be further improved.
[0013] [Colored particles] The colored particles have a core and a shell layer that covers the core. In the ink of the present invention, the content of the colored particles is preferably from 1.0% to 25.0% by mass, and more preferably from 4.0% to 10.0% by mass.
[0014] The volume median diameter of the colored particles is preferably 20 nm or more and 300 nm or less, more preferably 80 nm or more and 200 nm or less. By making the volume median diameter of the colored particles 20 nm or more, it is possible to suppress the colored particles from aggregating. By making the volume median diameter of the colored particles 300 nm or less, it is possible to further improve the ejection stability of the ink of the present invention.
[0015] (core) The core includes a polyester resin and a dye. The core preferably includes only the polyester resin and the dye, but may further include other components (e.g., a resin other than the polyester resin, and an additive). In the core, the polyester resin forms a matrix. The dye is dispersed in the matrix formed by the polyester resin.
[0016] (polyester resin) The polyester resin is obtained by polycondensation of one or more polyhydric alcohols and one or more polycarboxylic acids. Examples of the polyhydric alcohols for synthesizing the polyester resin include dihydric alcohols (e.g., diol compounds and bisphenol compounds) and trivalent or higher alcohols. Examples of the carboxylic acids for synthesizing the polyester resin include divalent carboxylic acids and trivalent or higher carboxylic acids. In addition, in the synthesis of the polyester resin, instead of the polycarboxylic acid, a polycarboxylic acid derivative capable of forming an ester bond by polycondensation (e.g., dimethyl polycarboxylic acid, anhydride of polycarboxylic acid, and polycarboxylic acid halide) may be used.
[0017] Examples of diol compounds include ethylene glycol, diethylene glycol, triethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,4-butanediol, neopentyl glycol, 2-butene-1,4-diol, 1,5-pentanediol, 2-pentene-1,5-diol, 1,6-hexanediol, 1,4-cyclohexanedimethanol, dipropylene glycol, 1,4-benzenediol, polyethylene glycol, polypropylene glycol, and polytetramethylene glycol.
[0018] Examples of bisphenol compounds include bisphenol A, hydrogenated bisphenol A, ethylene oxide adducts of bisphenol A, and propylene oxide adducts of bisphenol A.
[0019] Examples of trihydric or higher alcohols include sorbitol, 1,2,3,6-hexanetetrol, 1,4-sorbitan, pentaerythritol, dipentaerythritol, tripentaerythritol, 1,2,4-butanetriol, 1,2,5-pentanetriol, glycerol, diglycerol, 2-methylpropanetriol, 2-methyl-1,2,4-butanetriol, trimethylolethane, trimethylolpropane, and 1,3,5-trihydroxymethylbenzene.
[0020] The polyhydric alcohol is preferably a bisphenol A propylene oxide adduct or ethylene glycol.
[0021] Examples of divalent carboxylic acids include maleic acid, fumaric acid, citraconic acid, itaconic acid, glutaconic acid, phthalic acid, isophthalic acid, 5-sodium sulfoisophthalate, terephthalic acid, naphthalenedicarboxylic acid (e.g., 2,6-naphthalenedicarboxylic acid), cyclohexanedicarboxylic acid, adipic acid, sebacic acid, azelaic acid, malonic acid, succinic acid, alkylsuccinic acids (e.g., n-butylsuccinic acid, isobutylsuccinic acid, n-octylsuccinic acid, n-dodecylsuccinic acid, and isododecylsuccinic acid), and alkenylsuccinic acids (e.g., n-butenylsuccinic acid, isobutenylsuccinic acid, n-octenylsuccinic acid, n-dodecenylsuccinic acid, and isododecenylsuccinic acid).
[0022] Examples of trivalent or higher carboxylic acids include 1,2,4-benzenetricarboxylic acid (trimellitic acid), 2,5,7-naphthalenetricarboxylic acid, 1,2,4-naphthalenetricarboxylic acid, 1,2,4-butanetricarboxylic acid, 1,2,5-hexanetricarboxylic acid, 1,3-dicarboxy-2-methyl-2-methylenecarboxypropane, 1,2,4-cyclohexanetricarboxylic acid, tetra(methylenecarboxy)methane, 1,2,7,8-octanetetracarboxylic acid, pyromellitic acid, and empol trimer acid.
[0023] The polyvalent carboxylic acid is preferably terephthalic acid, isophthalic acid, 2,6-naphthalenedicarboxylic acid or sodium 5-sulfoisophthalate.
[0024] Examples of the polyester resin include amorphous polyester resin and crystalline polyester resin. As the polyester resin, amorphous polyester resin is preferable. When the polyester resin contains an amorphous polyester resin, the ink of the present invention can form a printed material having excellent elasticity. When the core of the ink of the present invention contains an amorphous polyester resin, the heating temperature during the heat treatment after the image formation can be reduced.
[0025] In addition, the amorphous polyester resin has a property of having excellent affinity with anthraquinone-based disperse dyes, and therefore, when the polyester resin contains an amorphous polyester resin and the dye contains an anthraquinone-based disperse dye, the dispersibility of the amorphous polyester resin and the dye (anthraquinone-based disperse dye) in the core can be improved.
[0026] The amorphous polyester resin can be obtained by introducing a non-regular structure into the polyester resin, making it difficult for the polyester resin to form a crystalline structure. Specific methods for introducing a non-regular structure into the polyester resin include, for example, a method of using two or more types of polyhydric alcohols and two or more types of polycarboxylic acids in combination, a method of using a polyhydric alcohol or polycarboxylic acid having a steric hindrance, and a method of using a polyhydric alcohol (e.g., 1,3-propanediol) or polycarboxylic acid having an odd number of carbon atoms.
[0027] The raw material of the polyester resin preferably contains an aromatic dicarboxylic acid and an aromatic alcohol. In this case, the content ratio of the aromatic dicarboxylic acid and the aromatic alcohol in the polyester raw material is preferably 50 mass% or more. By containing the aromatic dicarboxylic acid and the aromatic alcohol in the raw material of the polyester resin, the affinity between the polyester resin and an oil-based dye (for example, a disperse dye) can be improved.
[0028] The polyester resin is preferably an amorphous polyester resin formed from raw materials in the following combination (a) or (b). Combination (a): dimethyl terephthalate (e.g., 20% by mass or more and 30% by mass or less), isophthalic acid (e.g., 15% by mass or more and 25% by mass or less), sodium 5-sulfoisophthalate (e.g., 1% by mass or more and 10% by mass or less), bisphenol A propylene oxide adduct (e.g., 25% by mass or more and 45% by mass or less), and ethylene glycol (e.g., 10% by mass or more and 20% by mass or less) Combination (b): dimethyl terephthalate (e.g., 10% by mass or more and 20% by mass or less), isophthalic acid (e.g., 10% by mass or more and 15% by mass or less), dimethyl 2,6-naphthalenedicarboxylate (e.g., 10% by mass or more and 20% by mass or less), sodium 5-sulfoisophthalate (e.g., 1% by mass or more and 10% by mass or less), bisphenol A propylene oxide adduct (e.g., 30% by mass or more and 40% by mass or less), and ethylene glycol (e.g., 10% by mass or more and 20% by mass or less)
[0029] The glass transition point (Tg) of the polyester resin is preferably 40° C. or higher and 75° C. or lower. By setting the glass transition point of the polyester resin to 40° C. or higher, the storage stability of the ink of the present invention can be improved. By setting the glass transition point of the polyester resin to 75° C. or lower, the adhesion of the colored particles to the printing target can be improved.
[0030] The content of the polyester resin in the core is preferably from 50.0% by mass to 90.0% by mass, and more preferably from 70.0% by mass to 85.0% by mass.
[0031] (dye) The dyes include, for example, yellow dyes, orange dyes, red dyes, blue dyes, purple dyes, and black dyes. The dyes are preferably disperse dyes. The yellow disperse dyes include, for example, CI Disperse Yellow (42, 49, 76, 83, 88, 93, 99, 119, 126, 160, 163, 165, 180, 183, 186, 198, 199, 200, 224, and 237). The orange disperse dyes include, for example, CI Disperse Orange (29, 30, 31, 38, 42, 44, 45, 53, 54, 55, 71, 73, 80, 86, 96, 118, and 119). Red disperse dyes include, for example, CI Disperse Red (73, 88, 91, 92, 111, 127, 131, 143, 145, 146, 152, 153, 154, 179, 191, 192, 206, 221, 258, 283, 302, 323, 328, and 359). Purple disperse dyes include, for example, CI Disperse Violet (26, 35, 48, 56, 77, and 97). Blue disperse dyes include, for example, CI Disperse Blue (27, 54, 60, 73, 77, 79, 79:1, 87, 143, 165, 165:1, 165:2, 181, 185, 197, 225, 257, 266, 267, 281, 341, 353, 354, 358, 364, 365, 368, 359, and 360).
[0032] Also preferred as the dye are dyes suitable for thermal transfer. Examples of yellow dyes suitable for thermal transfer include CI Disperse Yellow (51, 54, and 60) and CI Solvent Yellow 114. Examples of orange dyes suitable for thermal transfer include CI Disperse Orange (5, 7, 20, and 23) and CI Solvent Orange 67. Examples of red dyes suitable for thermal transfer include CI Disperse Red (50, 53, 59, 60, 239, and 240) and CI Solvent Red 146. Examples of purple dyes suitable for thermal transfer include CI Disperse Violet (8, 11, 17, 26, 27, 28, and 36). Blue dyes suitable for thermal transfer include, for example, CI Disperse Blue (3, 5, 26, 35, 55, 56, 72, 81, 91, 108 and 359) and CI Solvent Blue (36, 63, 83, 105 and 111).
[0033] In the colored particles, the content of the dye relative to 100 parts by mass of the polyester resin is preferably from 5 parts by mass to 80 parts by mass, and more preferably from 15 parts by mass to 45 parts by mass.
[0034] In the ink of the present invention, the content of the dye is preferably from 0.5% to 5.0% by mass, and more preferably from 1.5% to 3.0% by mass.
[0035] (Shell layer) The shell layer contains a specific resin having an unopened ring oxazoline group and an amide ester group. The specific resin is, for example, covalently bonded to the polyester resin contained in the core. The shell layer is formed, for example, by treating the core with an unopened ring oxazoline group-containing polymer. In detail, by treating the core with the unopened ring oxazoline group-containing polymer, the unopened ring oxazoline group-containing polymer covers the core, and the unopened ring oxazoline group contained in the unopened ring oxazoline group-containing polymer and the carboxy group contained in the polyester resin in the core are covalently bonded. As a result, the shell layer is formed.
[0036] In the colored particles, the content of the shell layer relative to 100 parts by mass of the core is preferably from 1 part by mass to 20 parts by mass, and more preferably from 5 parts by mass to 10 parts by mass.
[0037] (Specific resin) The specific resin preferably has a first repeating unit (hereinafter sometimes referred to as repeating unit (1)) represented by the following general formula (A) and a second repeating unit (hereinafter sometimes referred to as repeating unit (2)) represented by the following general formula (B).
[0038] [ka]
[0039] In general formula (A), R 1 represents a hydrogen atom or an alkyl group having 1 to 10 carbon atoms which may be substituted with a phenyl group. 2 represents a hydrogen atom, or an alkyl group having 1 to 10 carbon atoms which may be substituted with a phenyl group. * represents a bonding site with an atom contained in the polyester resin contained in the core.
[0040] In the general formula (A) or (B), R 1 or R 2 Examples of the alkyl group having 1 to 10 carbon atoms, represented by the formula (I), include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, a sec-butyl group, a tert-butyl group, an n-pentyl group, an isopentyl group, a neopentyl group, a 1,2-dimethylpropyl group, a linear or branched chain hexyl group, a linear or branched chain heptyl group, a linear or branched chain octyl group, a linear or branched chain nonyl group, and a linear or branched chain decyl group.
[0041] In the general formula (A), R 1 Preferably, R represents a hydrogen atom, a methyl group, an ethyl group, or an isopropyl group. 2preferably represents a hydrogen atom, a methyl group, an ethyl group or an isopropyl group.
[0042] The specific resin may further have a repeating unit derived from a vinyl compound (hereinafter, may be referred to as repeating unit (3)). Here, the vinyl compound is a vinyl group (CH 2 =CH-), or a compound having a substituted vinyl group (a group in which at least one of the hydrogen atoms of a vinyl group is substituted with a substituent). Examples of the vinyl compound include ethylene, propylene, butadiene, vinyl chloride, (meth)acrylic acid, (meth)acrylic acid esters (preferably, (meth)acrylic acid alkyl esters), acrylonitrile, and styrene.
[0043] It is preferable that the specific resin further contains, as the repeating unit (3), a repeating unit derived from an alkyl (meth)acrylate ester or a repeating unit derived from styrene.
[0044] The specific resin preferably contains only the repeating unit (1), the repeating unit (2), and the repeating unit (3). However, the specific resin may further contain repeating units other than the repeating unit (1), the repeating unit (2), and the repeating unit (3).
[0045] [Method of manufacturing colored particles] Examples of the method for producing colored particles include a production method including a core-forming step of kneading and pulverizing a polyester resin and a dye, and a shell layer-forming step of reacting the obtained core with an unopened oxazoline group-containing polymer in an aqueous medium to form a shell layer.
[0046] (Core formation process) In this step, the polyester resin and the dye are mixed. The resulting mixture is then melt-kneaded using a melt-kneading device (for example, a single-screw or twin-screw extruder). The resulting kneaded product is then pulverized. This results in a core containing the polyester resin and the dye. The core may be dispersed in an aqueous medium as necessary before being subjected to the shell layer forming step.
[0047] Other methods for forming the core include, for example, a method of dissolving the polyester resin and the dye in an organic solvent (e.g., ethyl acetate and methyl ethyl ketone) and mixing them, and a method of dissolving the dye in a solution containing a monomer of the polyester resin and then polymerizing the monomer. However, the method of forming the core by the above-mentioned pulverization and kneading is preferred because it is less likely to cause the phenomenon in which only the dye separates and recrystallizes when the core is dispersed in an aqueous medium.
[0048] (Shell layer formation process) In this step, the core obtained in the pulverization step is reacted with the unopened ring-containing oxazoline group polymer in an aqueous medium. The unopened ring-containing oxazoline group polymer has, for example, the repeating unit (1) described above. The unopened ring-containing oxazoline group polymer has high hydrophilicity because it has the repeating unit (1) containing an oxazoline group, which is a group having high hydrophilicity. Therefore, the unopened ring-containing oxazoline group polymer is easily dissolved in an aqueous medium and easily reacts with the core in the aqueous medium. In addition, it is preferable that the unopened ring-containing oxazoline group polymer further has the repeating unit (3) described above. The unopened ring-containing oxazoline group polymer exhibits amphiphilicity by further having the repeating unit (3) having relatively high hydrophobicity. The unopened ring-containing oxazoline group polymer having amphiphilicity also functions as a dispersant and can react with the core even in an aqueous medium in which a dispersant (e.g., a surfactant) or an organic solvent is not present.
[0049] As a solution containing an unopened ring-containing oxazoline group polymer and an aqueous medium (hereinafter, sometimes referred to as a shell layer forming solution), for example, "Epocross (registered trademark) WS-300" or "Epocross (registered trademark) WS-700" manufactured by Nippon Shokubai Co., Ltd. can be used. Epocross (registered trademark) WS-300 contains a copolymer of 2-vinyl-2-oxazoline and methyl methacrylate (unopened ring-containing oxazoline group polymer). The mass ratio of the monomers constituting this copolymer is (2-vinyl-2-oxazoline):(methyl methacrylate)=9:1. Epocross (registered trademark) WS-700 contains a copolymer of 2-vinyl-2-oxazoline, methyl methacrylate, and butyl acrylate (unopened ring-containing oxazoline group polymer). The mass ratio of the monomers constituting the copolymer is (2-vinyl-2-oxazoline):(methyl methacrylate):(butyl acrylate)=5:4:1. 2-Vinyl-2-oxazoline is a compound represented by the following chemical formula (A-1).
[0050] [ka]
[0051] The details of the method of mixing the core and the shell layer forming solution are described below. When mixing the core and the shell layer forming solution, it is preferable to heat the mixed solution. The heating temperature is preferably a temperature at which the oxazoline group of the unopened oxazoline group-containing polymer reacts with the carboxyl group of the polyester resin to form an amide ester group or higher. A specific heating temperature is, for example, 70°C or higher and 100°C or lower. By mixing the core and the shell layer forming solution, a shell layer is formed on the surface of the core. As a result, a colored particle dispersion liquid containing colored particles and an aqueous medium is obtained.
[0052] In this step, the amount of the unopened oxazoline group-containing polymer added is preferably from 1 to 20 parts by mass, and more preferably from 5 to 10 parts by mass, per 100 parts by mass of the core.
[0053] [Aqueous medium] The aqueous medium contained in the ink of the present invention is a medium containing water. The aqueous medium may function as a solvent or as a dispersion medium. Specific examples of the aqueous medium include an aqueous medium containing only water, and an aqueous medium containing water and a water-soluble organic solvent.
[0054] In the ink of the present invention, the water content is preferably from 30.0% to 80.0% by mass, and more preferably from 40.0% to 60.0% by mass. By setting the water content to be from 30.0% to 80.0% by mass, the ejection stability of the ink of the present invention can be improved.
[0055] Examples of the water-soluble organic solvent contained in the ink of the present invention include glycol compounds, polyhydric alcohol ether compounds, lactam compounds, nitrogen-containing compounds, acetate compounds, thiodiglycol, glycerin, and dimethylsulfoxide.
[0056] Examples of glycol compounds include ethylene glycol, 1,3-propanediol, propylene glycol, diethylene glycol, triethylene glycol, and tetraethylene glycol.
[0057] Examples of the ether compounds of polyhydric alcohols include diethylene glycol diethyl ether, diethylene glycol monobutyl ether, ethylene glycol monomethyl ether, ethylene glycol monobutyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol diethyl ether, triethylene glycol monomethyl ether, triethylene glycol monoethyl ether, and propylene glycol monomethyl ether.
[0058] Lactam compounds include, for example, 2-pyrrolidone and N-methyl-2-pyrrolidone.
[0059] Examples of nitrogen-containing compounds include 1,3-dimethylimidazolidinone, formamide, and dimethylformamide.
[0060] An example of the acetate compound is diethylene glycol monoethyl ether acetate.
[0061] The water-soluble organic solvent contained in the ink of the present invention is preferably a glycol compound or glycerin, and more preferably propylene glycol or glycerin.
[0062] The content of the water-soluble organic solvent in the ink of the present invention is preferably from 10.0% to 60.0% by mass, and more preferably from 20.0% to 40.0% by mass. By setting the content of the water-soluble organic solvent to be from 10.0% to 60.0% by mass, the ejection stability of the ink of the present invention can be further improved.
[0063] [Surfactants] The ink of the present invention preferably further contains a surfactant. The surfactant improves the permeability (wettability) of the ink of the present invention to the object to be printed. Examples of the surfactant include anionic surfactants, cationic surfactants, and nonionic surfactants. The surfactant is preferably a nonionic surfactant.
[0064] Examples of the nonionic surfactant include polyoxyethylene dodecyl ether, polyoxyethylene hexadecyl ether, polyoxyethylene nonylphenyl ether, polyoxyethylene sorbitan monooleate ether, monodecanoyl sucrose, and ethylene oxide adducts of acetylene glycol. As the nonionic surfactant, ethylene oxide adducts of acetylene glycol are preferred.
[0065] When the ink of the present invention contains a surfactant, the content of the surfactant in the ink of the present invention is preferably from 0.05% to 3.0% by mass, and more preferably from 0.2% to 1.0% by mass.
[0066] [Other ingredients] The ink of the present invention may further contain known additives (more specifically, for example, a dissolution stabilizer, a drying inhibitor, an antioxidant, a viscosity adjuster, a pH adjuster, and an anti-mold agent) as necessary.
[0067] [Ink manufacturing method] The ink of the present invention is produced, for example, by mixing a colored particle dispersion liquid containing colored particles and water, a water-soluble organic solvent, and a component (e.g., a surfactant) that is added as needed, using a stirrer. The mixing time is, for example, 1 minute or more and 30 minutes or less. In preparing the ink of the present invention, after the components are uniformly mixed, foreign matter and coarse particles may be removed using a filter (e.g., a filter with a pore size of 5 μm). EXAMPLES
[0068] Examples of the present invention will be described below, but the present invention is not limited to the following examples.
[0069] In the examples, the volume median diameter (D 50 ) was measured using a dynamic light scattering particle size distribution analyzer ("Zetasizer Nano ZS" manufactured by Malvern Instruments).
[0070] [Synthesis of polyester resin] (Polyester resin (R-1)) A four-neck flask equipped with a distillation tube, a nitrogen inlet tube, a thermometer and a stirrer was used as a reaction vessel. 500 parts by mass of dimethyl terephthalate, 50 parts by mass of 5-sodium sulfoisophthalic acid, 300 parts by mass of ethylene glycol and 700 parts by mass of bisphenol A propylene oxide adduct as the first raw material, and 1 part by mass of zinc acetate as a reaction catalyst were added to the reaction vessel. Next, the internal temperature of the reaction vessel was raised to 130°C. Next, the internal temperature of the reaction vessel was raised from 130°C to 170°C over 2 hours. This resulted in an ester exchange reaction. Next, while the internal temperature of the reaction vessel was maintained at 170°C, 450 parts by mass of isophthalic acid and 1 part by mass of antimony trioxide were added to the reaction vessel as the second raw material. Next, the internal temperature of the reaction vessel was raised from 170°C to 200°C over 2 hours. This resulted in an esterification reaction. Next, the inside of the reaction vessel was gradually heated to 250°C, while gradually reducing the pressure inside the reaction vessel until the pressure inside the reaction vessel reached 666.6 Pa. After the inside temperature of the reaction vessel reached 250°C and the pressure inside the reaction vessel reached 666.6 Pa, this temperature and pressure were maintained for 1 hour. This allowed the polycondensation reaction to take place. As a result, a polyester resin (R-1) was obtained.
[0071] (Polyester resins (R-2) to (R-4)) Polyester resins (R-2) to (R-4) were synthesized in the same manner as for the synthesis of polyester resin (R-1), except that the types and amounts of the first and second raw materials were changed as shown in Table 1. In Table 1, "DMT", "NDCN", "SSPIA", "BPO-PO", "EG" and "IPA" respectively represent dimethyl terephthalate, dimethyl 2,6-naphthalenedicarboxylate, sodium 5-sulfoisophthalate, bisphenol A propylene oxide adduct, ethylene glycol and isophthalic acid.
[0072] The glass transition points and melting points of the polyester resins (R-1) to (R-4) were measured using a differential scanning calorimeter (Shimadzu Corporation's "DSC-60") in accordance with a method conforming to JIS (Japanese Industrial Standards) K7121-2012. The polyester resins (R-1) to (R-4) had the glass transition points shown in Table 1 below. On the other hand, no clear melting points were measured for the polyester resins (R-1) to (R-4). In other words, the polyester resins (R-1) to (R-4) were all amorphous polyester resins.
[0073] [Table 1]
[0074] [Preparation of colored particle dispersion] Colored particle dispersions (A-1) to (A-12) were prepared by the following method. First, the dyes and shell layer forming solutions used in the preparation of the colored particle dispersions are shown below.
[0075] (dye) Dye (D-1): "Disperse Blue 359" manufactured by Santa Cruz Biotechnology, Inc. Dye (D-2): "Disperse Yellow 54" manufactured by Santa Cruz Biotechnology, Inc. Dye (D-3): "Disperse Red 60" manufactured by Santa Cruz Biotechnology, Inc.
[0076] (Shell layer forming solution) Shell layer forming solution (S-1): Emulsion containing a copolymer of 2-vinyl-2-oxazoline and methyl methacrylate (water-soluble crosslinking agent) ("Epocross (registered trademark) WS-300" manufactured by Nippon Shokubai Co., Ltd.), solid content concentration 10% Shell layer forming solution (S-2): Emulsion containing a copolymer of 2-vinyl-2-oxazoline, methyl methacrylate, and butyl acrylate (water-soluble crosslinking agent) ("Epocross (registered trademark) WS-700" manufactured by Nippon Shokubai Co., Ltd.), solid content concentration 25% Shell layer forming solution (S-3): Emulsion containing a styrene-acrylic resin having an oxazoline group ("Epocross (registered trademark) K-2020E" manufactured by Nippon Shokubai Co., Ltd.), solid content concentration 40% Shell layer forming solution (S-4): solution containing a polycarbodiimide resin to which a hydrophilic segment has been added ("Carbodilite (registered trademark) V-04" manufactured by Nisshinbo Chemical Inc.), solid content concentration 40%
[0077] (Colored particle dispersion (A-1)) 100 parts by mass of polyester resin (R-1) and 25 parts by mass of dye (D-1) were mixed in a high-speed mixer. The mixture obtained was subjected to a first kneading using a kneader ("KH-2-S" manufactured by Inoue Seisakusho Co., Ltd.) at a rotation speed of 100 rpm and a temperature of 85°C. The first kneaded product obtained by the first kneading was subjected to a second kneading using a twin-screw continuous kneader ("PCM-30" manufactured by Ikegai Co., Ltd.) at a material supply speed of 5 kg / hour, a shaft rotation speed of 150 rpm, and a cylinder temperature of 150°C.
[0078] The second kneaded product obtained in the second kneading was cooled and then finely pulverized with a pulverizer (Turbo Mill RS type, manufactured by Freund Turbo Corporation). This resulted in a core containing the polyester resin and the dye.
[0079] Into a four-neck flask equipped with a thermocouple, 200 g of core (components: 160 g of polyester resin (R-1) and 40 g of dye (D-1)), 700 g of ion-exchanged water, and 100 g of ethylene glycol monobutyl ether as a water-soluble organic solvent were added. The contents of the four-neck flask were then mixed for 2 hours at a stirring speed of 10,000 rpm and a temperature of 90° C. using a thin-film swirling high-speed mixer ("Filmix (registered trademark) 40-L" manufactured by Primix Corporation). Thereafter, the contents of the four-neck flask were cooled to room temperature while stirring to obtain a core dispersion.
[0080] A 1L three-neck flask equipped with a thermometer and stirring blade was used as a reaction vessel. 100g of core dispersion was added to the reaction vessel. Next, the internal temperature of the reaction vessel was maintained at 30°C using a water bath. Next, 14g (1.4g solid content) of shell layer forming solution (S-1) was added to the reaction vessel and thoroughly stirred. Next, the contents of the reaction vessel were stirred at a speed of 150 rpm for 1 hour. Next, 100g of ion-exchanged water was added to the reaction vessel. Next, while stirring the contents of the reaction vessel at 250 rpm, the internal temperature of the reaction vessel was raised to 80°C at a temperature increase rate of 0.5°C / min. Next, while maintaining the internal temperature of the reaction vessel at 80°C, the contents of the reaction vessel were stirred at 250 rpm for 1 hour. Next, the internal temperature of the reaction vessel was cooled to room temperature. This resulted in the colored particle dispersion (A-1).
[0081] (Colored particle dispersion (A-2)~(A-12)) Colored particle dispersions (A-2) to (A-12) were prepared in the same manner as in the preparation of colored particle dispersion (A-1), except for the following changes. In the preparation of colored particle dispersions (A-2) to (A-12), the type of polyester resin, the type of dye, the amount of ion-exchanged water added, the type and amount of water-soluble organic solvent, and the type and amount of shell layer-forming solution were changed so as to obtain the compositions shown in Tables 2 and 3 below. In addition, in the preparation of colored particle dispersion (A-11), no shell layer was formed. That is, the core dispersion having the composition shown in Table 3 below was used as colored particle dispersion (A-11) as it is.
[0082] In the following Tables 2 and 3, "EGBE," "MEK," and "IPA" respectively represent ethylene glycol monobutyl ether, methyl ethyl ketone, and isopropyl alcohol.
[0083] [Table 2]
[0084] [Table 3]
[0085] [Ink preparation] Inks (I-1) to (I-10) used in the examples and inks (I-11) to (I-13) used in the comparative examples were prepared by the following method.
[0086] (Ink (I-1)) 100 g of colored particle dispersion (A-1) (10% by mass of colored particles), 20 g of propylene glycol, 20 g of glycerin, and 0.5 g of a nonionic surfactant ("Surfynol (registered trademark) 104" manufactured by Nissin Chemical Industry Co., Ltd.) were mixed, and the resulting mixture was filtered using a filter with a pore size of 5 μm (filtration process). Ink (I-1) was thus obtained. The viscosity of ink (I-1) was 6.0 mPa s.
[0087] (Ink (I-2)~(I-12)) Inks (I-2) to (I-12) were prepared in the same manner as for ink (I-1), except that the type of color particle dispersion was changed as shown in Table 4 below.
[0088] (Ink (I-13)) 10.0 g (1.0 g in terms of solid content) of a pigment dispersion containing a disperse dye ("TB-416 Yellow" manufactured by Dainichiseika Chemical Industry Co., Ltd.), 20.0 g of propylene glycol, 20.0 g of glycerin, and 0.5 g of a nonionic surfactant ("Surfynol (registered trademark) 104" manufactured by Nissin Chemical Industry Co., Ltd.) were added to 49.5 g of ion-exchanged water to prepare a total amount of 100.0 g. The resulting mixture was filtered using a filter with a pore size of 5 μm (filtration process). As a result, a yellow ink, ink (I-13), was obtained.
[0089] (dispersibility) The dispersibility of the inks (I-1) to (I-13) was judged based on the state during the above-mentioned filtration process. In detail, during the filtration process of each ink, the presence or absence of clogging of the 5 μm pore size filter was confirmed. In addition, after the filtration process, the 5 μm pore size filter was visually observed. The dispersibility of the ink was judged based on the following criteria. The judgment results are shown in Table 4 below.
[0090] (Criteria for Dispersibility) A (good): No coarse particles remained on the filter, or some coarse particles remained on the filter but did not clog the filter. B (bad): Coarse particles remained on the filter and the filter became clogged.
[0091] (Volume Median Diameter Measurement) The volume median diameter (D 50 The measurement results are shown in Table 4 below.
[0092] (Measurement of the amount of unopened oxazoline groups) The amount of unopened oxazoline groups (Ox groups) contained in 1 g of ink was measured for inks (II) to (I-13) by the following method. The measurement results are shown in Table 4 below.
[0093] The measurement equipment used was a gas chromatograph mass spectrometer (Shimadzu Corporation, "GCMS-QP2010 Ultra") and a multi-shot pyrolyzer (Frontier Labs, Inc., "FRONTIER LAB Multi-functional Pyrolyzer (registered trademark) PY-3030D"). The column used was a GC column (Agilent Technologies, Inc., "Agilent (registered trademark) J&W Ultra Inert Capillary GC column DB-5ms", phase: arylene phase in which arylene is introduced into siloxane polymer to strengthen the polymer main chain, inner diameter: 0.25 mm, film thickness: 0.25 μm, length: 30 m).
[0094] (Gas Chromatograph) Carrier gas: Helium (He) gas Carrier flow rate: 1mL / min Vaporizer temperature: 210℃ Pyrolysis temperature: Heating furnace "600℃", interface part "320℃" Column oven temperature conditions: After holding at 40°C for 3 minutes, the temperature was increased from 40°C to 300°C at a rate of 10°C / min, and held at 300°C for 15 minutes.
[0095] (Mass spectrometry) Ionization method: EI (Electron Impact) method Ion source temperature: 200℃ Interface temperature: 320℃ Detection mode: Scan (measurement range: 45m / z~500m / z)
[0096] By analyzing the mass spectrum measured under the above conditions, the peaks derived from the unopened oxazoline groups were identified. Based on the peak area of the identified peaks, the amount of unopened oxazoline groups contained in 1 g of the measurement target (ink) was calculated. A calibration curve based on a standard substance was used for quantification.
[0097] <Evaluation> The ejection stability of the inks (I-1) to (I-13) and the washing fastness of the printed textiles formed were evaluated by the following methods. The evaluation results are shown in Table 4 below.
[0098] [Discharge stability] An inkjet printing device (a prototype manufactured by Kyocera Document Solutions Inc.) equipped with four line-type recording heads (KJ4B-QA manufactured by Kyocera Corporation, number of nozzles: 2656) and a conveyor belt was used as the evaluation machine. The recording head had a long shape, and its longitudinal direction was perpendicular to the conveying direction of the printing object. The conveyor belt of the evaluation machine had a suction unit that applied negative pressure to the printing object during conveyance in order to bring the conveyor belt and the printing object into close contact with each other. One of the recording heads of the evaluation machine was filled with the evaluation object (any of the inks (I-1) to (I-13)). Next, the ejection conditions of the recording head were set so that the amount of ink ejected per ink drop was 10.5 pL. Next, the negative pressure of the suction unit was set to 0.6 kPa.
[0099] Using the evaluation machine, a solid image was continuously formed over the entire surface of the printing target (a tetron pongee fabric using polyester fibers) for 30 minutes (continuous printing process). The evaluation machine was then left for 10 minutes. After 10 minutes, a nozzle check pattern was formed using the evaluation machine. This confirmed the presence or absence of non-ejecting nozzles that occurred during the continuous printing process. The ink ejection stability was judged based on the following criteria.
[0100] (Standard for discharge stability) A (Good): 0 to 3 non-ejecting nozzles B (defective): 4 or more non-ejecting nozzles
[0101] [Washing fastness] Using the evaluation machine, a solid image was formed on the entire surface of the printing target (a Tetron Pongee fabric using polyester fibers). Next, the printing target on which the solid image was formed was heated at 180°C for 60 seconds. This caused the polyester fibers and the ink to be integrated, and a printed product was obtained.
[0102] The above-mentioned printed fabric was subjected to a dye fastness test in accordance with JIS (Japanese Industrial Standards) L0844:2011. More specifically, first, an aqueous solution (soap concentration: 5 g / L) containing soap ("Shabondama Powder Soap" manufactured by Shabondama Soap Co., Ltd.) was prepared as a washing liquid. Next, the printed fabric was washed with the above-mentioned washing liquid using a washing tester, and the degree of discoloration of the printed fabric was judged using the gray scale for discoloration specified in JIS (Japanese Industrial Standards) L0804:2004. More specifically, the degree of discoloration of the printed fabric was judged in nine stages, namely, grade 1, grade 1-2, grade 2, grade 2-3, grade 3, grade 3-4, grade 4, grade 4-5, or grade 5. In the above judgment, grade 1 indicates the highest degree of discoloration, and grade 5 indicates the lowest degree of discoloration. The washing fastness was judged based on the following criteria.
[0103] (Standards for washing fastness) A (Good): The degree of discoloration is Grade 4, Grade 4-5, or Grade 5. B (bad): Discoloration level is grade 3 or 3-4 C (particularly poor): The degree of discoloration is grade 1, grade 1-2, grade 2, or grade 2-3.
[0104] [Table 4]
[0105] The inks (I-1) to (I-10) of Examples 1 to 10 contained colored particles and an aqueous medium. The colored particles had a core and a shell layer covering the core. The core contained a polyester resin and a dye. The shell layer contained a specific resin having an unopened oxazoline group and an amide ester group. The inks (I-1) to (I-10) of Examples 1 to 10 were excellent in ejection stability and were able to form printed items with excellent washing fastness.
[0106] On the other hand, the inks (I-11) to (I-13) of Comparative Examples 1 and 2 did not satisfy the above-mentioned requirements, and therefore were inferior in ejection stability or could not form printed items with excellent washing fastness.
[0107] Specifically, the colored particles in the ink (I-11) of Comparative Example 1 did not have a shell layer. The printed item formed using the ink (I-11) of Comparative Example 1 was judged to have poor washing fastness because the dye eluted from the core of the colored particles.
[0108] The ink (I-12) of Comparative Example 2 did not contain a specific resin in the shell layer. It is determined that the colored particles of the ink (I-12) of Comparative Example 2 did not have a stable core-shell structure. As a result, the ink (I-12) of Comparative Example 2 was inferior in ejection stability and was unable to form a printed item with excellent washing fastness.
[0109] The ink of Comparative Example 3 (I-13) used a disperse dye instead of colored particles, and therefore was unable to form a printed item with excellent washing fastness. [Industrial Applicability]
[0110] The ink according to the present invention can be used to form textile prints.
Claims
1. Contains colored particles and an aqueous medium, The coloring particles each include a core and a shell layer that covers the core, the core comprises a polyester resin and a dye; The shell layer comprises a specific resin having an unopened oxazoline group and an amide ester group.
2. The ink-jet textile printing ink according to claim 1 , wherein the polyester resin comprises an amorphous polyester resin.
3. The ink-jet printing ink according to claim 1 or 2, wherein the colored particles have a volume median diameter of 20 nm or more and 300 nm or less.
4. The ink-jet textile printing ink according to any one of claims 1 to 3, wherein the specific resin has a first repeating unit represented by general formula (A) below and a second repeating unit represented by general formula (B) below: 【Chemistry 1】 (In the above general formula (A), R 1 represents a hydrogen atom or an alkyl group having from 1 to 10 carbon atoms which may be substituted with a phenyl group, In the general formula (B), R 2 represents a hydrogen atom or an alkyl group having 1 to 10 carbon atoms which may be substituted with a phenyl group, and * represents a bonding site with an atom contained in the polyester resin contained in the core.
Citation Information
Patent Citations
Aqueous ink composition and formation of image and maintenance, and maintaining liquid
JP2000109733A
Colored fine particle dispersion and water-based ink containing the same
JP2004285215A
Ink for textile printing inkjet
JP2009215506A
Toner for electrostatic latent image development and method for manufacturing the same
JP2018124495A
Ink for inkjet printing and inkjet printing method, and method for manufacturing ink for inkjet printing
JP2019182941A