How to install anti-static non-slip flooring

A non-slip floor with antistatic properties is constructed using a room temperature curable resin and single-walled carbon nanotubes, addressing the limitations of conductive aggregates by ensuring conductivity without them, thus improving design freedom and reducing costs.

JP7567278B2Active Publication Date: 2024-10-16SUMITOMO RUBBER INDUSTRIES LTD
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2020139803
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-08-21
Publication Date
2024-10-16
Estimated Expiration
2040-08-21

AI Technical Summary

Technical Problem

Existing non-slip floors with antistatic properties require conductive aggregates to form a conductive path between the undercoat and topcoat layers, limiting design freedom and increasing costs.

Method used

A method using a room temperature curable resin and single-walled carbon nanotubes as a conductive filler in both the undercoat and topcoat layers, eliminating the need for conductive aggregates.

Benefits of technology

The method achieves high electrical conductivity at the interface between the undercoat and topcoat layers without conductive aggregates, enhancing design freedom and reducing costs while maintaining antistatic performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007567278000001
    Figure 0007567278000001
  • Figure 0007567278000002
    Figure 0007567278000002
Patent Text Reader

Abstract

To provide a method capable of constructing a non-slip floor exhibiting antistatic performance without using conductive aggregate.SOLUTION: A method of constructing an antistatic non-slip floor comprises the steps of: forming an undercoating layer on a floor substrate by using an undercoating material; scattering an aggregate on the undercoating layer; and forming an overcoating layer on the undercoating layer on which the aggregate is scattered by using an overcoating material. The undercoating material and the overcoating material each contain a room-temperature curing resin and a single-wall carbon nanotube as a conductive filler.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for constructing a non-slip floor having antistatic properties. [Background technology]

[0002] Coating floors using hardening resins such as epoxy resins are often used for floors in production facilities such as factories. Among these coating floors, non-slip floors are known that have anti-slip properties due to unevenness using aggregate. The neat method is known as one of the construction methods for this non-slip floor. In the neat method, a coating floor material containing a hardening resin is applied to the floor base to form a resin material layer, aggregate is scattered on top of the resin material, and if necessary, a coating floor material is applied on top of the aggregate (for example, see Patent Documents 1 to 3).

[0003] On the other hand, since the curable resin used in the coated floor is electrically insulating, there is a problem that static electricity causes obstacles during work on the applied coated floor. Therefore, in order to impart antistatic properties to the coated floor, a conductive filler is added to the curable resin. For example, Patent Document 4 describes the use of conductive titanium oxide powder and carbon fiber as a conductive filler. Patent Document 5 describes the use of carbon fiber as a conductive filler. Patent Document 6 describes the use of conductive metal oxide such as conductive zinc oxide and stainless steel fiber as a conductive filler. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Publication No. 59-138657 [Patent Document 2] JP 2003-73454 A [Patent Document 3] JP 2003-105707 A [Patent Document 4] JP 2013-40446 A [Patent Document 5] JP 2017-48333 A [Patent Document 6] JP 2016-223252 A Summary of the Invention [Problem to be solved by the invention]

[0005] When the neat method is used to impart antistatic properties to a non-slip floor, a base coat layer is first formed using a base coat material containing a curable resin and a conductive filler, aggregate is then spread on the base coat layer, and then a top coat material containing a curable resin and a conductive filler is applied to form a top coat layer so that the aggregate is held in place. Here, the aggregate is scattered on the base coat layer, and the part of the base coat layer where the aggregate is not present comes into contact with the top coat layer, but the contact resistance is large at the contact interface between the base coat layer and the top coat layer, and conductivity is not obtained. Therefore, in the conventional technology, it is necessary to use a conductive aggregate as the aggregate in order to form a conductive path between the base coat layer and the top coat layer. Therefore, in the conventional technology, the conductive aggregate is essential, which causes problems such as limited freedom in designing non-slip floors or high costs.

[0006] In view of the above circumstances, an object of the present invention is to provide a method for constructing a non-slip floor that exhibits antistatic properties without using conductive aggregate. [Means for solving the problem]

[0007] The method for constructing a non-slip floor of the present invention includes the steps of forming an undercoat layer on a floor substrate using an undercoat material, scattering aggregate on the undercoat layer, and forming a topcoat layer on the undercoat layer on which the aggregate has been scattered using a topcoat material. The undercoat material and the topcoat material each contain a room temperature curing resin and single-walled carbon nanotubes as a conductive filler. Effect of the Invention

[0008] According to the present invention, it is possible to construct a non-slip floor that exhibits antistatic properties without using conductive aggregate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] The method for constructing a non-slip floor of the present invention includes a step of forming an undercoat layer on a floor substrate using an undercoat material (hereinafter also referred to as an "undercoat layer forming step"), a step of scattering aggregate on the undercoat layer (hereinafter also referred to as an "aggregate scattering step"), and a step of forming a topcoat layer on the undercoat layer on which the aggregate has been scattered using a topcoat material (hereinafter also referred to as an "topcoat layer forming step"). Here, the undercoat material and the topcoat material each contain a room temperature curing resin and single-walled carbon nanotubes as a conductive filler.

[0010] First, the undercoat layer forming step will be described. The floor underlay may be a conventionally known floor underlay, typically a concrete underlay. From the viewpoint of higher antistatic performance, usually, the surface of the floor underlay is given electrical conductivity. A suitable example of such a floor underlay is a underlay in which a conductive primer layer is formed on concrete. The underlay may further have a primer layer between the concrete and the conductive primer layer in order to improve the adhesion between them. This conductive primer layer and this primer layer may have the same configuration as those known in the art. For example, the conductive primer layer may be formed using a primer containing a room temperature curing resin and carbon black.

[0011] In the present invention, a floor coating material is used that contains a room temperature curing resin as an undercoat material and single-walled carbon nanotubes as a conductive filler.

[0012] The room temperature curing resin is a resin that can be cured at room temperature (for example, 0°C to 40°C, particularly 5°C to 35°C), which is the construction environment temperature, and known resins for floor coating applications can be used. As the room temperature curing resin, two-component curing type, moisture curing type, radical polymerization type, etc. can be used, and among these, two-component curing type is preferable. Specific examples of the room temperature curing resin include epoxy resin, urethane resin, acrylic resin, polyester resin, vinyl ester resin, etc., and among these, epoxy resin is preferable.

[0013] As the epoxy resin, any epoxy resin known in the art for use in floor coating materials can be used, and two-component curing type epoxy resins that are liquid at room temperature and cure by reaction with a curing agent are preferred.

[0014] Examples of epoxy resins include alicyclic epoxy resins such as 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexanecarboxylate; glycidyl ester type epoxy resins such as hexahydrophthalic acid diglycidyl ester; bisphenol type epoxy resins derived from bisphenols such as bisphenol A and bisphenol F and epihalohydrins; epoxidized novolac resins such as phenol novolac resin, cresol novolac resin, bisphenol A novolac resin, naphthol novolac resin, and biphenyl novolac resin; glycidyl ether type epoxy resins derived from dihydric alcohols such as hydrogenated bisphenol F, hydrogenated bisphenol A, 1,4-cyclohexanedimethanol, and alkylene oxide adducts of bisphenol A and epihalohydrins; and epoxy resins derived from polyhydric phenols such as hydroquinone and catechol and epihalohydrins. Among these, bisphenol type epoxy resins (particularly, bisphenol A type epoxy resins) are preferred. These can be used alone or in combination of two or more.

[0015] As the curing agent, those known in the application of floor coating materials can be used. Specific examples thereof include aliphatic amines such as diethylenetriamine, triethylenetetramine, pentaethylenehexamine, etc., or modified products thereof; aromatic amines such as m-phenylenediamine, m-xylylenediamine, diaminodiphenylmethane, etc., or modified products thereof; alicyclic amines such as 1,3-bis(aminomethyl)cyclohexane, isophoronediamine, etc., or modified products thereof; acid anhydrides such as phthalic anhydride, hexahydrophthalic anhydride, pyromellitic anhydride, etc.; polysulfides; acid amides; thiokol, etc. Among them, alicyclic amines, aromatic amines, and modified products thereof are preferred. Modified products include Mannich modified products, adduct modified products, etc. These can be used alone or in combination of two or more.

[0016] The mixing amount of epoxy resin and curing agent may be set so that the molar amount of epoxy groups contained in the epoxy resin and the molar amount of active hydrogen contained in the curing agent are approximately equal, as in the conventional method. When a reactive diluent is used, which will be described later, the total molar amount of epoxy groups contained in the epoxy resin and the reactive diluent may be set so that the molar amount of active hydrogen contained in the curing agent is approximately equal.

[0017] The single-walled carbon nanotube (SWNT) used as the conductive filler has a structure in which one graphene sheet is rolled into a cylindrical shape. The single-walled carbon nanotube may be any of the armchair type, zigzag type, and chiral type. Since it can be easily dispersed in the floor coating material, it is preferable to use the single-walled carbon nanotube that is pre-dispersed, and in particular, it is preferable to use the single-walled carbon nanotube that is pre-dispersed in a diluent that is reactive with the room temperature curing resin. The single-walled carbon nanotube can be synthesized according to a known method, and is also available as a commercial product. A suitable example of the pre-dispersed single-walled carbon nanotube is "TUBALL MATRIX201" manufactured by OCSIAL. This "TUBALL MATRIX201" contains a fatty acid glycidyl ester as a reactive diluent. Therefore, when an epoxy resin is used as the room temperature curing resin, the fatty acid glycidyl ester can react with the curing agent together with the epoxy resin.

[0018] The content of single-walled carbon nanotubes in the coating floor material is not particularly limited, but if it is too small, the conductivity may be insufficient. Therefore, the content of single-walled carbon nanotubes in the coating floor material (i.e., relative to the total mass of the coating floor material; in the case of a two-component type room temperature curing resin, relative to the total mass of the coating floor material including the mass of the curing agent) is preferably 0.010% by mass or more, more preferably 0.015% by mass or more, and even more preferably 0.020% by mass or more. On the other hand, if the content of single-walled carbon nanotubes in the coating floor material is too high, the coating floor material may thicken and the finish may be impaired. Therefore, the content of single-walled carbon nanotubes in the coating floor material is preferably 0.040% by mass or less, more preferably 0.035% by mass or less, and even more preferably 0.030% by mass or less.

[0019] Here, single-walled carbon nanotubes have high conductivity, but are very prone to aggregation. Therefore, even if single-walled carbon nanotubes are added to a coating floor material as a conductive filler to improve conductivity, aggregation of single-walled carbon nanotubes occurs. Even if aggregation of single-walled carbon nanotubes occurs, the conductivity of the non-slip floor at 500V is obtained and the antistatic performance required in the current market can be satisfied, but the conductivity at low voltages (e.g., 50V, particularly 25V) is reduced. Therefore, in the present invention, it is preferable that the coating floor material contains at least one of a wetting dispersant and a phthalocyanine pigment as a component for dispersing the single-walled carbon nanotubes. In this case, conductivity is obtained even at low voltages (e.g., 50V, particularly 25V), and the antistatic performance of the non-slip floor can be further improved.

[0020] In the field of paints, wetting and dispersing agents are additives that act as surfactants to improve the wettability of coating films, and as dispersing agents that prevent particle aggregation through mechanisms such as electrical repulsion and steric hindrance. Among wetting and dispersing agents, wetting and dispersing agents that are polymer salts containing acidic and amino groups are preferred because they have particularly high dispersibility for single-walled carbon nanotubes. When a wetting and dispersing agent that is a polymer salt containing acidic and amino groups is included, the non-slip floor to be applied can exhibit particularly high conductivity even at low voltages such as 50V and even 25V.

[0021] The acidic group is preferably an acidic phosphate group. The polymer of the polymer salt may be a homopolymer or a copolymer. The polymer is preferably a graft copolymer in which one or more side chains (e.g., polyester chains) are introduced into a main chain (e.g., polyurethane chain). In this case, the dispersibility of the single-walled carbon nanotubes is improved due to the steric hindrance of the polymer chain. As the polymer salt, alkyl ammonium salts and phosphate salts are preferred, and alkyl ammonium salts are more preferred.

[0022] The wetting dispersant preferably has an acid value and an amine value of 10 mgKOH / g or more. From the viewpoint of storage stability, the acid value and the amine value of the wetting dispersant are more preferably 30 mgKOH / g or more, and even more preferably 35 mgKOH / g or more. The acid value refers to the acid value per 1 g of polymer dispersant solid content, and can be determined, for example, by potentiometric titration in accordance with JIS K0070. The amine value refers to the amine value per 1 g of polymer dispersant solid content, and can be determined, for example, by using a 0.1 N hydrochloric acid aqueous solution and converting the value determined by potentiometric titration into the equivalent amount of potassium hydroxide.

[0023] Specific examples of suitable wetting and dispersing agents include "BYK-9076", "BYK-9077", "DISPERBYK-142", and "DISPERBYK-2152" manufactured by BYK Japan Co., Ltd.; and "Disparlon DA-325" manufactured by Kusumoto Chemical Industries, Ltd. From the viewpoint of finish, "BYK-9076", "DISPERBYK-142", and "Disparlon DA-325" are preferred, and from the viewpoint of storage stability, "BYK-9076" and "DISPERBYK-142" are more preferred. Wetting and dispersing agents can be used alone or in combination of two or more.

[0024] The content of the wetting dispersant in the coating floor material is not particularly limited, but if it is too small, sufficient conductivity may not be obtained. In addition, the higher the content of the wetting dispersant, the higher the storage stability tends to be. Therefore, the content of the wetting dispersant in the coating floor material is preferably 0.04 mass% or more, more preferably 0.10 mass% or more, and even more preferably 0.15 mass% or more. On the other hand, if the content of the wetting dispersant in the coating floor material is too high, the conductivity may decrease. Therefore, the content of the wetting dispersant in the coating floor material is preferably 0.40 mass% or less, more preferably 0.32 mass% or less, and even more preferably 0.25 mass% or less.

[0025] In this specification, the term "phthalocyanine pigment" refers to a pigment having a phthalocyanine skeleton. The phthalocyanine skeleton of the phthalocyanine pigment allows single-walled carbon nanotubes to be stably dispersed, and thus, in the cured coating film formed using the floor coating material, a conductive path is formed even at low voltage, and high conductivity can be exhibited. The dispersion stabilization effect of the single-walled carbon nanotubes by the phthalocyanine pigment is exhibited for a long period of time, which also increases the storage stability of the floor coating material. In addition, when a new type of additive is used in the floor coating material, it may have a negative effect on other components. However, since pigments are components that are usually contained in floor coating materials, it is advantageous to be able to stably disperse single-walled carbon nanotubes and achieve conductivity at low voltage by using the phthalocyanine pigment, which is one type of pigment among a very large number of pigments, because the negative effect on other components is prevented.

[0026] The phthalocyanine skeleton (particularly, the phthalocyanine ring) may be unsubstituted or substituted. When the phthalocyanine skeleton is substituted, examples of the substituent include halogen atoms (e.g., fluorine atoms, chlorine atoms, bromine atoms, etc.), and among these, chlorine atoms are preferred. The phthalocyanine pigment may or may not have a coordinated metal. From the viewpoint of higher conductivity, the phthalocyanine pigment preferably has a coordinated metal. Examples of the coordinated metal include copper (Cu), cobalt (Co), zinc (Zn), nickel (Ni), iron (Fe), chromium (Cr), gallium (Ga), aluminum (Al), and the like. The coordinated metal is preferably copper (Cu).

[0027] Suitable examples of phthalocyanine pigments include phthalocyanine green and phthalocyanine blue. Among these, phthalocyanine green is preferred from the viewpoint of higher conductivity. Specific examples of phthalocyanine pigments include CI Pigment Green 7, CI Pigment Green 38, CI Pigment Green 58, CI Pigment Green 59, CI Pigment Green 62, CI Pigment Green 63, CI Pigment Blue 15:3, CI Pigment Blue 15:4, CI Pigment Blue 15:6, and CI Pigment Blue 16. The phthalocyanine pigments can be used alone or in combination of two or more.

[0028] The content of the phthalocyanine pigment in the coating floor material is not particularly limited, but if it is too small, the electrical conductivity may be insufficient. Therefore, the content of the phthalocyanine pigment in the coating floor material is preferably 0.03 mass% or more, more preferably 0.05 mass% or more, and even more preferably 0.10 mass% or more. On the other hand, since the phthalocyanine pigment can be sufficiently colored even with a small amount, the content of the phthalocyanine pigment in the coating floor material is preferably 1.00 mass% or less, more preferably 0.80 mass% or less, and even more preferably 0.60 mass% or less.

[0029] When the floor coating material contains a phthalocyanine pigment, it may further contain an iron oxide pigment as a second pigment. The iron oxide pigment exhibits various hues, such as red, yellow, and black, depending on the difference in composition and crystal structure. The floor coating material contains a phthalocyanine pigment, and thus has the color tone exhibited by the phthalocyanine pigment. By blending an iron oxide pigment therein, this color tone can be adjusted. In addition, since the iron oxide pigment is an inorganic particle, it can improve the strength of the cured coating film. Examples of the iron oxide pigment include red iron oxide pigment (red iron oxide), black iron oxide pigment (iron black), and yellow iron oxide pigment (yellow iron). The iron oxide pigment can be used alone or in combination of two or more types.

[0030] The content of the iron oxide pigment in the coating material is not particularly limited and may be appropriately determined according to the desired color tone. The content of the iron oxide pigment in the coating material is, for example, 3% by mass or more and 20% by mass or less.

[0031] [Leveling Agent] The floor coating material may contain a leveling agent to improve the finish. The leveling agent may be a known one used in floor coating materials. Examples of the leveling agent include acrylic polymers. The leveling agent may be the "Polyflow" series manufactured by Kyoeisha Chemical Co., Ltd. The leveling agent may be used alone or in combination of two or more types.

[0032] The content of the leveling agent in the coating floor material is not particularly limited, but if it is too small, the finish may be deteriorated. Therefore, the content of the leveling agent in the coating floor material is preferably 0.03% by mass or more, more preferably 0.05% by mass or more, and even more preferably 0.07% by mass or more. On the other hand, if the content of the leveling agent in the coating floor material is too high, the conductivity may be insufficient. Therefore, the content of the leveling agent in the coating floor material is preferably 0.40% by mass or less, more preferably 0.30% by mass or less, and even more preferably 0.15% by mass or less. When the coating floor material contains a phthalocyanine pigment, the content of the leveling agent in the coating floor material is preferably 0.17% by mass or less, more preferably 0.15% by mass or less, and even more preferably 0.13% by mass or less.

[0033] [Antifoaming agent] The floor coating material may contain a defoaming agent to improve the finish. The defoaming agent may be a known agent used in floor coating materials. Examples of the defoaming agent include acrylic polymers, vinyl ether polymers, and mixtures thereof. The defoaming agent may be the "Florene" series manufactured by Kyoeisha Chemical Co., Ltd. The defoaming agent may be used alone or in combination of two or more types.

[0034] The content of the defoaming agent in the coating floor material is not particularly limited, but if it is too small, the finish may be deteriorated. Therefore, the content of the defoaming agent in the coating floor material is preferably 0.05% by mass or more, more preferably 0.10% by mass or more, and even more preferably 0.15% by mass or more. On the other hand, if the content of the defoaming agent in the coating floor material is too high, the conductivity may be insufficient. Therefore, the content of the defoaming agent in the coating floor material is preferably 0.60% by mass or less, more preferably 0.40% by mass or less, and even more preferably 0.25% by mass or less. When the coating floor material contains a phthalocyanine pigment, the content of the defoaming agent in the coating floor material is preferably 0.25% by mass or more, more preferably 0.30% by mass or more, and even more preferably 0.35% by mass or more, while it is preferably 0.55% by mass or less, more preferably 0.50% by mass or less, and even more preferably 0.45% by mass or less.

[0035] The floor coating material may further contain pigments other than those described above for the purpose of adjusting the color tone, etc. As the pigment, a known pigment used in floor coating materials may be used. The content of the pigment may be appropriately set according to the type of pigment and the desired color tone, etc.

[0036] The floor coating material may contain an insulating filler for the purpose of improving strength, colorability, etc. As the insulating filler, a known one used in floor coating materials may be used. Examples thereof include calcium carbonate, magnesium carbonate, barium sulfate, calcium oxide, magnesium oxide, alumina, silica, kaolin, talc, mica, glass beads, glass microballoons, glass fiber, etc., and among them, calcium carbonate (particularly heavy calcium carbonate) is preferable. The content of the insulating filler may be appropriately set according to the desired strength, etc.

[0037] The floor coating material may contain a reactive diluent, a non-reactive diluent, etc., for the purpose of viscosity adjustment, etc. Examples of reactive diluents include compounds having one or more reactive groups of the same type as the room temperature curing resin. Specifically, for example, when the room temperature curing resin is an epoxy resin, a compound having an epoxy group such as neopentyl glycol diglycidyl ether can be used. Examples of non-reactive diluents include compounds that do not have the same type of reactive group as the room temperature curing resin. Specifically, for example, when the room temperature curing resin is an epoxy resin, benzyl alcohol, etc. can be used. The content of these may be appropriately set according to the desired viscosity, etc.

[0038] The coated floor material may further contain components other than those described above, within the range that does not significantly impair the effects of the present invention.

[0039] There is no particular limitation on the method of preparing the floor coating material, and it can be prepared according to a known method. For example, each component of the floor coating material may be mixed at once at the construction site or the like to prepare it. For example, the floor coating material may be prepared as a two-liquid type in which the main agent containing components other than the hardener and the hardener are separated, and the main agent and the hardener are mixed and used at the construction site or the like. For example, it may be prepared as a two-liquid type, and the main agent component may be prepared without mixing the insulating filler or with a small amount of the insulating filler, and the insulating filler may be added to the main agent so that the mixing amount is determined, for example, at the construction site or the like, taking into consideration the condition of the base and the characteristics required for the floor coating.

[0040] The undercoat layer can be formed by a known method using the above-mentioned floor coating material as the undercoat. For example, the undercoat layer can be formed by applying the undercoat material to the floor base by a pouring method. The amount of the undercoat material applied can be the same as in the past, for example, 1 m 2 The amount of coating should be between 1.0 kg and 1.5 kg per unit. In addition, when the particle size of the aggregate used in the next process is large, the amount of coating should be larger, and when the particle size of the aggregate is small, the amount of coating should be smaller.

[0041] Here, the mixture is left to stand for a predetermined period of time to allow drying and hardening of the room-temperature curing resin. However, as in the conventional neat method, it is preferable to carry out the next aggregate scattering step before the room-temperature curing resin has hardened, so that some of the aggregate particles will sink into the undercoat layer and improve adhesion.

[0042] Next, the aggregate scattering process will be described. In the present invention, it is not necessary to use conductive aggregate as the aggregate. Therefore, it is preferable to use insulating aggregate. The use of insulating aggregate can increase the freedom of designing the non-slip floor, and can also be advantageous in terms of cost.

[0043] Examples of insulating aggregates include natural aggregates such as silica sand, river sand, mountain sand, sea sand, corundum, garnet, and emery; ceramic aggregates such as alumina, zirconia, boron carbide, silicon carbide, and crushed ceramic; and glass powder. Among these, silica sand is preferred from the viewpoint of cost. Note that, in the present invention, it is not necessary to use a conductive aggregate, but a conductive aggregate (e.g., aluminum powder, aggregate obtained by coating the insulating aggregate with a conductive component (e.g., metal, etc.)) may be used.

[0044] The shape and particle size of the aggregate are not particularly limited and can be appropriately determined according to the desired coarseness of the non-slip floor. In general, insulating aggregates are more readily available in various shapes and particle sizes than conductive aggregates, so it is advantageous to be able to use insulating aggregates as aggregates in the present invention.

[0045] There is no particular restriction on the amount of aggregate to be spread; it may be determined appropriately depending on the type and shape of the aggregate, the desired coarseness of the non-slip floor, etc., and may be the same as the amount to be spread when constructing a non-slip floor using a known room temperature curing resin.

[0046] The method of scattering the aggregate on the undercoat layer is not particularly limited, and the aggregate may be scattered on the undercoat layer according to a known method. After scattering the aggregate, the undercoat layer is usually left to stand until the room temperature curing resin of the undercoat layer cures. After curing, it is preferable to remove the excess aggregate.

[0047] Next, the topcoat layer forming process will be described. As the topcoat material used in the topcoat layer forming process, a floor coating material containing room temperature curing resin and single-walled carbon nanotubes as conductive filler is used. The floor coating material is the same as the floor coating material used as the undercoat material. As the topcoat material, the same floor coating material as the undercoat material may be used, or a floor coating material different from the undercoat material may be used as long as it contains room temperature curing resin and single-walled carbon nanotubes as conductive filler.

[0048] The topcoat layer can be formed by a known method. For example, the topcoat layer can be formed by applying a coating to the undercoat layer by a casting method. The amount of coating of the topcoat material can be appropriately determined so that the aggregate is sufficiently covered and unevenness due to the aggregate is formed. For example, the amount of coating of the topcoat material can be determined so that the aggregate is sufficiently covered and unevenness is formed due to the aggregate. 2 The amount is 0.5 kg to 1.0 kg per coating. After coating, it is left to stand for a certain period of time to dry and harden the room temperature curing resin, completing a non-slip floor with antistatic properties.

[0049] In this manner, a non-slip floor having antistatic properties can be constructed. In the non-slip floor constructed by the method of the present invention, unlike the conventional technology, high conductivity is obtained even at the interface where the undercoat layer and the topcoat layer come into contact without any aggregate between them. Therefore, even without using conductive aggregate, a conductive path is formed between the undercoat layer and the topcoat layer, so antistatic properties can be exhibited. Therefore, compared to the conventional technology, the degree of freedom in designing the non-slip floor can be increased, and the cost can also be reduced.

[0050] The construction method of the present invention can be applied to floors in various buildings, including floors in various production facilities. The non-slip floor constructed by the construction method of the present invention can exhibit conductivity at 50V or even 25V, and such a non-slip floor that exhibits conductivity even at such low voltages can prevent electrostatic damage such as the destruction of electronic components at low voltages. Therefore, such a non-slip floor that exhibits conductivity even at low voltages is suitable for research facilities and production facilities for electronic components. EXAMPLES

[0051] Examples of the present invention will be described below, but it is not intended that the present invention be limited to those shown in these examples.

[0052] Examples 1 and 2, Comparative Example 1 and Reference Example 1 Conductive base agent A and conductive base agent B were prepared by mixing the components shown in Table 1. Using the conductive base agent A and conductive base agent B, the undercoat material and topcoat material shown in Table 2 were prepared, and the aggregate shown in Table 2 was also prepared. The primer layer and conductive primer layer (resistance: about 10 3 The undercoat material was applied with a trowel onto the flat plate on which the slab had been formed (Ω) to form a undercoat layer. Before the undercoat layer hardened, aggregate was scattered on the undercoat layer. After the undercoat layer hardened, the topcoat material was applied with a roller onto it to form a topcoat layer. In this way, a non-slip floor sample was prepared.

[0053] For this non-slip floor sample, the resistance was measured using an insulation tester at applied voltages of 500 V and 25 V in accordance with the NFPA method and JIS A1454:2016 to evaluate the electrical conductivity. Note that 2.25 kg iron cylinders were used as electrodes, and the distance between the electrodes was 3 feet (approximately 91 cm). The measurement results are shown in Table 2.

[0054] [Table 1]

[0055] The values ​​for each component in the table indicate parts by mass. Polyflow #85: Kyoeisha Chemical Co., Ltd.'s leveling agent "Polyflow #85" FLORON AC324: Defoamer "FLORON AC324" manufactured by Kyoeisha Chemical Co., Ltd. MATRIX201: OCSIAL's "TUBALL MATRIX201" (contains single-walled carbon nanotubes: fatty acid glycidyl ester (reactive diluent) in a mass ratio of 1:9) BYK-9076: Wetting and dispersing agent "BYK-9076" manufactured by BYK Japan (alkyl ammonium salt of a polymer in which a polyester chain is grafted onto a polyurethane main chain; acid value = 38 mg KOH / g, amine value = 44 mg KOH / g)

[0056] [Table 2]

[0057] The values ​​of each component in the table are for 1 m2 of construction area. 2 Indicates the mass (kg) per unit.

[0058] As shown in Table 1, the coated floor material using conductive base agents A and A' is a coated floor material containing room temperature curing resin and single-walled carbon nanotubes, and the coated floor material using conductive base agent B is a coated floor material using a conventional conductive filler.

[0059] Comparative Example 1 and Reference Example 1 are test examples in which conventional floor coating materials were used as undercoats and topcoats. As the results of Comparative Example 1 and Reference Example 1 show, when conventional floor coating materials were used as undercoats and topcoats, electrical conductivity was obtained by using conductive aluminum powder as aggregate, but electrical conductivity was not obtained by using insulating silica sand as aggregate.

[0060] On the other hand, in Examples 1 to 4, in which floor coating materials containing room temperature curing resin and single-walled carbon nanotubes were used as undercoat and topcoat materials, electrical conductivity was obtained even though insulating silica sand was used as aggregate. That is, in Examples 1 to 4, antistatic performance could be imparted to the non-slip floor without using conductive aggregate. From this, it can be seen that according to the present invention, it is possible to construct a non-slip floor that exhibits antistatic performance without using conductive aggregate. In addition, the No. 5 silica sand used in Examples 1 and 2 and the No. 6 silica sand used in Examples 3 and 4 have different particle coarseness. From this, it can be said that it is easy to make the non-slip floor have the desired coarseness, and it can be seen that according to the present invention, the degree of freedom in designing the non-slip floor is increased.

Claims

1. A step of forming a primer layer on the floor substrate using a primer material; Spreading aggregate on the undercoat layer; and A step of forming a topcoat layer using a topcoat material on the undercoat layer on which the aggregate has been spread. Inclusive of The undercoat material and the topcoat material each contain a room temperature curing resin and single-walled carbon nanotubes (excluding modified single-walled carbon nanotubes whose surfaces are carboxylated) as a conductive filler, The undercoat material and the topcoat material each contain at least one of a wetting and dispersing agent and a phthalocyanine pigment; the wetting and dispersing agent is a polymer salt containing acidic and amino groups, The phthalocyanine pigment is phthalocyanine green containing copper as a coordination metal or phthalocyanine blue containing copper as a coordination metal. How to install a non-slip floor.

2. 2. The method of claim 1, wherein the aggregate is insulating.

Citation Information

Patent Citations

  • Novel antistatic terrace system and production method

    CN107652845A

  • Construction of Anti-slip floor

    JP1984138657A

  • Technique for laminating floor moisture-permeable coating film

    JP2001340806A

  • Curable composition for neat construction and cured material thereof

    JP2003073454A

  • Resin composition for road and its constructing method and pavement structure

    JP2003105707A