Highly antistatic floor coating materials and floor coatings
The combination of single-walled carbon nanotubes and phthalocyanine pigment in a coated flooring material ensures conductivity at low voltages, addressing the conductivity gap in existing floors and preventing electrostatic damage.
Patent Information
- Application Number
- JP2020139804
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-08-21
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2040-08-21
AI Technical Summary
Existing coated floors with conductive fillers do not exhibit conductivity at low voltages, failing to prevent static electricity hazards below 500V, which can cause electrostatic damage to electronic components.
A painted flooring material comprising a room temperature curable resin, single-walled carbon nanotubes, and a phthalocyanine pigment is used, where the phthalocyanine pigment stabilizes the dispersion of carbon nanotubes to enable conductivity even at low voltages.
The coated flooring material achieves high conductivity at voltages as low as 25V, effectively preventing electrostatic damage to electronic components and maintaining stability over time.
Smart Images

Figure 0007567279000001 
Figure 0007567279000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a coated floor material having improved antistatic performance. The present invention also relates to a coated floor including a cured coating film of the coated floor material. [Background technology]
[0002] Coating floors using curing resins such as epoxy resins are often used for floors in production facilities such as factories. However, since the curing resins used in coating floors are electrically insulating, problems occur in that static electricity occurs during work on the coated floors. Therefore, in order to impart antistatic properties to the coated floors, conductive fillers are added to the curing resins. For example, Patent Document 1 describes the use of conductive titanium oxide powder and carbon fibers as conductive fillers. Patent Document 2 describes the use of carbon fibers as conductive fillers. Patent Document 3 describes the use of conductive metal oxides such as conductive zinc oxide and stainless steel fibers as conductive fillers.
[0003] The leakage resistance when static electricity charged to the human body is grounded through a painted floor is 10 8 It is said that a resistance of about 10 Ω is sufficient. Therefore, an antistatic coating floor should have a resistance of 10 Ω or less when measured with an applied voltage of 500 V. 8 It has a conductivity of less than Ω. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2013-40446 A [Patent Document 2] JP 2017-48333 A [Patent Document 3] JP 2016-223252 A Summary of the Invention [Problem to be solved by the invention]
[0005] On the other hand, in production facilities, electrostatic damage such as the destruction of electronic components at low voltages may occur. In contrast, conventional coated floors have a sea-island structure in which the curable resin is the sea phase and the conductive filler is the island phase. In a sea-island structure, electricity flows between the island phases on either side of the sea phase, so a certain voltage or higher is required for electrical conduction. For this reason, conventional coated floors do not exhibit electrical conductivity at voltages much lower than 500V, and cannot prevent electrostatic damage at such low voltages. Therefore, there is a demand for the development of coated floors that exhibit electrical conductivity even at low voltages.
[0006] In view of the above circumstances, an object of the present invention is to provide a coated floor material in which a cured coating film exhibits electrical conductivity even at low voltage. [Means for solving the problem]
[0007] The present invention relates to a floor coating material containing a room temperature curable resin, single-walled carbon nanotubes, and a phthalocyanine pigment. Effect of the Invention
[0008] According to the present invention, it is possible to provide a coated floor material in which the cured coating film exhibits high electrical conductivity even at a low voltage. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] The coated floor material of the present invention contains a room temperature curing resin, single-walled carbon nanotubes, and a phthalocyanine pigment. Each component of the coated floor material of the present invention will be described in detail below.
[0010] [Room temperature curing resin] The room temperature curing resin is a resin that can be cured at room temperature (for example, 0°C to 40°C, particularly 5°C to 35°C), which is the construction environment temperature, and known resins for floor coating applications can be used. As the room temperature curing resin, two-component curing type, moisture curing type, radical polymerization type, etc. can be used, and among these, two-component curing type is preferable. Specific examples of the room temperature curing resin include epoxy resin, urethane resin, acrylic resin, polyester resin, vinyl ester resin, etc., and among these, epoxy resin is preferable.
[0011] As the epoxy resin, any epoxy resin known in the art for use in floor coating materials can be used, and two-component curing type epoxy resins that are liquid at room temperature and cure by reaction with a curing agent are preferred.
[0012] Examples of epoxy resins include alicyclic epoxy resins such as 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexanecarboxylate; glycidyl ester type epoxy resins such as hexahydrophthalic acid diglycidyl ester; bisphenol type epoxy resins derived from bisphenols such as bisphenol A and bisphenol F and epihalohydrins; epoxidized novolac resins such as phenol novolac resin, cresol novolac resin, bisphenol A novolac resin, naphthol novolac resin, and biphenyl novolac resin; glycidyl ether type epoxy resins derived from dihydric alcohols such as hydrogenated bisphenol F, hydrogenated bisphenol A, 1,4-cyclohexanedimethanol, and alkylene oxide adducts of bisphenol A and epihalohydrins; and epoxy resins derived from polyhydric phenols such as hydroquinone and catechol and epihalohydrins. Among these, bisphenol type epoxy resins (particularly, bisphenol A type epoxy resins) are preferred. These can be used alone or in combination of two or more.
[0013] As the curing agent, those known in the application of floor coating materials can be used. Specific examples thereof include aliphatic amines such as diethylenetriamine, triethylenetetramine, pentaethylenehexamine, etc., or modified products thereof; aromatic amines such as m-phenylenediamine, m-xylylenediamine, diaminodiphenylmethane, etc., or modified products thereof; alicyclic amines such as 1,3-bis(aminomethyl)cyclohexane, isophoronediamine, etc., or modified products thereof; acid anhydrides such as phthalic anhydride, hexahydrophthalic anhydride, pyromellitic anhydride, etc.; polysulfides; acid amides; thiokol, etc. Among them, alicyclic amines, aromatic amines, and modified products thereof are preferred. Modified products include Mannich modified products, adduct modified products, etc. These can be used alone or in combination of two or more.
[0014] The mixing amount of epoxy resin and curing agent may be set so that the molar amount of epoxy groups contained in the epoxy resin and the molar amount of active hydrogen contained in the curing agent are approximately equal, as in the conventional method. When a reactive diluent is used, which will be described later, the total molar amount of epoxy groups contained in the epoxy resin and the reactive diluent may be set so that the molar amount of active hydrogen contained in the curing agent is approximately equal.
[0015] [Single-walled carbon nanotubes] In the present invention, single-walled carbon nanotubes (SWNTs) are used as the conductive filler. SWNTs have a structure in which one graphene sheet is rolled into a cylindrical shape. The single-walled carbon nanotubes may be of any of the armchair type, zigzag type, and chiral type. Since they can be easily dispersed in the floor coating material, it is preferable to use pre-dispersed single-walled carbon nanotubes, and in particular, it is preferable to use those pre-dispersed in a diluent that is reactive with room temperature curing resins. Single-walled carbon nanotubes can be synthesized according to a known method and are also available as commercial products. A suitable example of pre-dispersed single-walled carbon nanotubes is "TUBALL MATRIX201" manufactured by OCSIAL. This "TUBALL MATRIX201" contains fatty acid glycidyl ester as a reactive diluent. Therefore, when an epoxy resin is used as the room temperature curing resin, the fatty acid glycidyl ester can react with the curing agent together with the epoxy resin.
[0016] The content of single-walled carbon nanotubes in the coating floor material is not particularly limited, but if it is too small, the conductivity may be insufficient. Therefore, the content of single-walled carbon nanotubes in the coating floor material (i.e., relative to the total mass of the coating floor material; in the case of a two-component type room temperature curing resin, relative to the total mass of the coating floor material including the mass of the curing agent) is preferably 0.010% by mass or more, more preferably 0.015% by mass or more, and even more preferably 0.020% by mass or more. On the other hand, if the content of single-walled carbon nanotubes in the coating floor material is too high, the coating floor material may thicken and the finish may be impaired. Therefore, the content of single-walled carbon nanotubes in the coating floor material is preferably 0.040% by mass or less, more preferably 0.035% by mass or less, and even more preferably 0.030% by mass or less. In addition, when the content of single-walled carbon nanotubes is 0.040% by mass or less, the color of the cured coating film of the coating floor material is hardly affected by the color of the single-walled carbon nanotubes.
[0017] [Phthalocyanine pigments] In this specification, the term "phthalocyanine pigment" refers to a pigment having a phthalocyanine skeleton. Single-walled carbon nanotubes have high electrical conductivity, but are very prone to aggregation. Therefore, even if single-walled carbon nanotubes are added to a coating floor material as a conductive filler to improve electrical conductivity, aggregation of the single-walled carbon nanotubes occurs. As a result, in a cured coating film formed using the coating floor material, a conductive path is not formed at a low voltage, such as 100V or even 25V, and electrical conductivity is not obtained. Therefore, in the present invention, single-walled carbon nanotubes are used in combination with a phthalocyanine pigment. The phthalocyanine skeleton of the phthalocyanine pigment allows single-walled carbon nanotubes to be stably dispersed, and thus, in a cured coating film formed using the coating floor material, a conductive path is formed even at a low voltage, and high electrical conductivity can be expressed. The dispersion stabilization effect of the single-walled carbon nanotubes by the phthalocyanine pigment is exerted for a long period of time, which also increases the storage stability of the coating floor material. In addition, when a new type of additive is used in the coating floor material, it may have an adverse effect on other components. However, because pigments are a component commonly contained in coated flooring materials, the ability to stably disperse single-walled carbon nanotubes and achieve conductivity at low voltages using phthalocyanine pigments, which are just one type of pigment among the many types of pigments available, is advantageous because it prevents adverse effects on other components.
[0018] The phthalocyanine skeleton (particularly, the phthalocyanine ring) may be unsubstituted or substituted. When the phthalocyanine skeleton is substituted, examples of the substituent include halogen atoms (e.g., fluorine atoms, chlorine atoms, bromine atoms, etc.), and among these, chlorine atoms are preferred. The phthalocyanine pigment may or may not have a coordinated metal. From the viewpoint of higher conductivity, the phthalocyanine pigment preferably has a coordinated metal. Examples of the coordinated metal include copper (Cu), cobalt (Co), zinc (Zn), nickel (Ni), iron (Fe), chromium (Cr), gallium (Ga), aluminum (Al), and the like. The coordinated metal is preferably copper (Cu).
[0019] Suitable examples of phthalocyanine pigments include phthalocyanine green and phthalocyanine blue. Among these, phthalocyanine green is preferred from the viewpoint of higher conductivity. Specific examples of phthalocyanine pigments include CI Pigment Green 7, CI Pigment Green 38, CI Pigment Green 58, CI Pigment Green 59, CI Pigment Green 62, CI Pigment Green 63, CI Pigment Blue 15:3, CI Pigment Blue 15:4, CI Pigment Blue 15:6, and CI Pigment Blue 16. The phthalocyanine pigments can be used alone or in combination of two or more.
[0020] The content of the phthalocyanine pigment in the coating floor material is not particularly limited, but if it is too small, the electrical conductivity may be insufficient. Therefore, the content of the phthalocyanine pigment in the coating floor material is preferably 0.03 mass% or more, more preferably 0.05 mass% or more, and even more preferably 0.10 mass% or more. On the other hand, since the phthalocyanine pigment can be sufficiently colored even with a small amount, the content of the phthalocyanine pigment in the coating floor material is preferably 1.00 mass% or less, more preferably 0.80 mass% or less, and even more preferably 0.60 mass% or less.
[0021] [Iron oxide] The coated floor material of the present invention may contain an iron oxide pigment. The iron oxide pigment exhibits various hues, such as red, yellow, and black, depending on the difference in composition and crystal structure. The coated floor material of the present invention contains a phthalocyanine pigment, and thus has the color tone exhibited by the phthalocyanine pigment. By blending the iron oxide pigment therein, this color tone can be adjusted. In addition, since the iron oxide pigment is an inorganic particle, it can improve the strength of the cured coating film. Examples of the iron oxide pigment include red iron oxide pigment (red iron oxide), black iron oxide pigment (iron black), and yellow iron oxide pigment (yellow iron). The iron oxide pigment can be used alone or in combination of two or more types.
[0022] The content of the iron oxide pigment in the coating material is not particularly limited and may be appropriately determined according to the desired color tone. The content of the iron oxide pigment in the coating material is, for example, 3% by mass or more and 20% by mass or less.
[0023] [Leveling Agent] The coated floor material of the present invention may contain a leveling agent to improve the finish. The leveling agent may be a known one used in coated floor materials. Examples of the leveling agent include acrylic polymers. The leveling agent may be the "Polyflow" series manufactured by Kyoeisha Chemical Co., Ltd. The leveling agent may be used alone or in combination of two or more types.
[0024] The content of the leveling agent in the coating floor material is not particularly limited, but if it is too small, the finish may be deteriorated. Therefore, the content of the leveling agent in the coating floor material is preferably 0.03 mass% or more, more preferably 0.05 mass% or more, and even more preferably 0.07 mass% or more. On the other hand, if the content of the leveling agent in the coating floor material is too high, the conductivity may be insufficient. Therefore, the content of the leveling agent in the coating floor material is preferably 0.17 mass% or less, more preferably 0.15 mass% or less, and even more preferably 0.13 mass% or less.
[0025] [Antifoaming agent] The floor coating material of the present invention may contain a defoaming agent to improve the finish. The defoaming agent may be a known agent used in floor coating materials. Examples of the defoaming agent include acrylic polymers, vinyl ether polymers, and mixtures thereof. The defoaming agent may be the "Florene" series manufactured by Kyoeisha Chemical Co., Ltd. The defoaming agent may be used alone or in combination of two or more types.
[0026] The content of the defoaming agent in the coating floor material is not particularly limited, but if it is too small, the finish may be deteriorated. Therefore, the content of the defoaming agent in the coating floor material is preferably 0.25% by mass or more, more preferably 0.30% by mass or more, and even more preferably 0.35% by mass or more. On the other hand, if the content of the defoaming agent in the coating floor material is too high, the conductivity may be insufficient. Therefore, the content of the defoaming agent in the coating floor material is preferably 0.55% by mass or less, more preferably 0.50% by mass or less, and even more preferably 0.45% by mass or less.
[0027] The floor coating material of the present invention may further contain pigments other than those described above for the purpose of adjusting the color tone, etc. As the pigment, a known pigment used in floor coating materials may be used. The content of the pigment may be appropriately set according to the type of pigment and the desired color tone, etc.
[0028] The coated floor material of the present invention may contain an insulating filler for the purpose of improving strength, colorability, etc. As the insulating filler, a known one used in coated floor materials may be used. Examples thereof include calcium carbonate, magnesium carbonate, barium sulfate, calcium oxide, magnesium oxide, alumina, silica, kaolin, talc, mica, glass beads, glass microballoons, glass fiber, etc., and among them, calcium carbonate (particularly heavy calcium carbonate) is preferable. The content of the insulating filler may be appropriately set according to the desired strength, etc.
[0029] The floor coating material of the present invention may contain a reactive diluent, a non-reactive diluent, etc., for the purpose of viscosity adjustment, etc. Examples of reactive diluents include compounds having one or more reactive groups of the same type as the room temperature curing resin. Specifically, for example, when the room temperature curing resin is an epoxy resin, a compound having an epoxy group such as neopentyl glycol diglycidyl ether can be used. Examples of non-reactive diluents include compounds that do not have the same type of reactive group as the room temperature curing resin. Specifically, for example, when the room temperature curing resin is an epoxy resin, benzyl alcohol, etc. can be used. The content of these may be appropriately set according to the desired viscosity, etc.
[0030] The coated floor material of the present invention may further contain components other than those described above, provided that the effects of the present invention are not significantly impaired.
[0031] The method of preparing the floor coating material of the present invention is not particularly limited, and it can be prepared according to a known method. For example, each component of the floor coating material of the present invention may be mixed at once at the construction site or the like to prepare it. For example, the floor coating material of the present invention may be prepared as a two-liquid type in which the main agent containing components other than the hardener and the hardener are separated, and the main agent and the hardener are mixed and used at the construction site or the like. For example, it may be prepared as a two-liquid type, and the main agent component may be prepared without mixing the insulating filler or with a small amount of the insulating filler, and the insulating filler may be added to the main agent so that the mixing amount is determined in consideration of the condition of the base and the characteristics required for the floor coating, for example, at the construction site or the like.
[0032] The coated floor material of the present invention can be applied and used according to a known method. For example, the coated floor material of the present invention can be applied to the floor to be applied by a pouring method, and then left to stand for a predetermined time to dry and harden the epoxy resin, thereby forming a coated floor. The applied coated floor may be a single layer of the layer formed by the coated floor material of the present invention (i.e., the layer of the cured coating film of the coated floor material of the present invention), or may be a multi-layer structure combining the layer formed by the coated floor material of the present invention and a primer layer.
[0033] According to the floor coating material of the present invention, by combining single-walled carbon nanotubes with phthalocyanine pigments, the cured coating film exhibits high conductivity even at voltages far lower than 500 V (for example, 100 V or even 25 V). In particular, the cured coating film has a resistance value of 10 at 25 V. 7 It can show a conductivity of less than Ω. Therefore, the coated floor material of the present invention has a much higher antistatic performance than conventional ones (so it can be called a "highly antistatic coated floor material"), and can prevent not only conventional antistatic but also electrostatic damage such as destruction of electronic components at low voltage. In addition, the coated floor material of the present invention has good storage stability.
[0034] Therefore, from another perspective, the present invention is a coated floor having a cured coating film of the above-mentioned coated floor material. The coated floor may have a primer layer. The thickness of the cured coating film of the above-mentioned coated floor material is not particularly limited, but is, for example, 1.0 mm or more and 3.0 mm or less, preferably 1.0 mm or more and 2.0 mm or less. The coated floor of the present invention exhibits high conductivity even at 25 V. Therefore, it is possible to prevent electrostatic damage such as the destruction of electronic components at low voltage. The coated floor of the present invention can be used in various buildings, and is particularly suitable for research facilities and production facilities for electronic components. EXAMPLES
[0035] Examples of the present invention will be described below, but it is not intended that the present invention be limited to those shown in these examples.
[0036] [Test Example 1: Comparison with conventional products] Example 1 and Comparative Example 1 The components listed in Table 1 were mixed to prepare a two-liquid type coating floor material consisting of a base agent and a hardener. Specifically, in Example 1, an epoxy resin was weighed and added to a stirring vessel. A non-reactive diluent was weighed and added to the stirring vessel and stirred at 1500 rpm. Furthermore, calcium carbonate was weighed and added to the stirring vessel and stirred at 1500 rpm. Meanwhile, a mixture of a pigment, a carbon nanotube dispersion, a small amount of epoxy resin, and a reactive diluent was added to the stirring vessel and stirred at 1500 rpm. A leveling agent and an antifoaming agent were added to the stirring vessel and stirred at 1500 rpm. After that, the mixture was stirred for another 20 minutes to obtain a base agent. The base agent and hardener were mixed in a mass ratio of 5:1 to prepare a paint. The values for each component in Table 1 indicate parts by mass. The total of the base agent and hardener is about 120 parts by mass.
[0037] [Conductivity evaluation] Primer layer and conductive primer layer (resistance: approx. 10 3 A floor coating material of each Example and Comparative Example was applied to a flat plate having a surface roughness of 1000 Ω, and the epoxy resin was allowed to harden for 24 hours or more to prepare a test sample. The resistance of this test sample was measured using an insulation resistance meter when an applied voltage of 500 V and 25 V was set in accordance with the NFPA method and JIS A1454:2016. Note that 2.25 kg iron cylinders were used as electrodes, and the distance between the electrodes was 3 feet (approximately 91 cm). The measurement results are shown in Table 1.
[0038] [Table 1]
[0039] Polyflow #85: Kyoeisha Chemical Co., Ltd.'s leveling agent "Polyflow #85" FLORON AC324: Defoamer "FLORON AC324" manufactured by Kyoeisha Chemical Co., Ltd. MATRIX201: OCSIAL's "TUBALL MATRIX201" (contains single-walled carbon nanotubes: fatty acid glycidyl ester (reactive diluent) in a mass ratio of 1:9)
[0040] Comparative Example 1 is an example of the prior art in which conductive zinc oxide, metal fiber, and carbon fiber are used as conductive fillers. As shown in the results in Table 1, in Comparative Example 1, which corresponds to the prior art, the resistance value was 10 5 It has low conductivity of 10 Ω, but at 25 V the resistance is 10 9 In contrast, in Example 1, which is an example of the present invention, the resistance value is 10 6 It can be seen that the electrical conductivity is low at only Ω. Therefore, it can be seen that the present invention has realized a coated floor material in which the cured coating film exhibits high electrical conductivity even at low voltages (especially 25 V).
[0041] Furthermore, after preparing the floor coating material of Example 1, it was left for two weeks and then the above-mentioned conductivity evaluation was carried out. 5 It was confirmed that the electrical conductivity did not decrease, and the resistance value of the single-walled carbon nanotubes was Ω. This shows that the good dispersion state of the single-walled carbon nanotubes is maintained for a long period of time in the floor coating material of the present invention, and the storage stability is also excellent.
[0042] [Test Example 2: Study of phthalocyanine pigments] Examples 2 to 10 The components listed in Table 2 were mixed to prepare a two-liquid type coating floor material consisting of a base agent and a hardener. Specifically, in Example 1, an epoxy resin paint was weighed and added to a stirring vessel. A carbon nanotube dispersion was weighed and added to the stirring vessel, and stirred at 4000 rpm. The resulting mixture was divided into small portions, and T16 and a phthalocyanine pigment were weighed and stirred to obtain a base agent. The base agent and hardener were mixed in a mass ratio of 5:1 to prepare a coating material. The values for each component in Table 2 indicate parts by mass. The above-mentioned conductivity evaluation was performed on this coating floor material. However, the voltage during the evaluation was 100V.
[0043] [Table 2]
[0044] C450A: Uncolored paint (pigment-free version of Sumitomo Rubber Industries' epoxy resin paint "C450A"; paint containing epoxy resin, reactive diluent, non-reactive diluent, heavy calcium carbonate, leveling agent, defoamer, dispersant, and anti-settling agent) T16: Iron oxide pigments H506SA: Modified polyamine-based hardener "H506SA" manufactured by Sumitomo Rubber Industries, Ltd.
[0045] The so-called "copper phthalocyanine" in Examples 2 to 9 is a phthalocyanine pigment containing copper as a coordinated metal, and the so-called "metal-free phthalocyanine" in Example 10 is a phthalocyanine pigment that does not contain a coordinated metal. From these comparisons, it can be seen that when the phthalocyanine pigment contains copper as a coordinated metal, higher conductivity can be obtained at low voltage. It can also be seen that the use of phthalocyanine green generally results in higher conductivity than the use of phthalocyanine blue.
Claims
1. The composition contains an epoxy resin which is a room temperature curing resin, single-walled carbon nanotubes (however, excluding modified single-walled carbon nanotubes whose surfaces are carboxylated and carbon nanotubes which are dispersed in an aqueous resin and then the aqueous resin is precipitated to treat the surfaces with the resin), and a phthalocyanine pigment, The phthalocyanine pigment is phthalocyanine green containing copper as a coordination metal or phthalocyanine blue containing copper as a coordination metal.
2. The coated floor material according to claim 1, wherein the content of the phthalocyanine pigment is 0.03% by mass or more and 1.00% by mass or less.
3. The floor coating material according to claim 1 or 2, wherein the content of the single-walled carbon nanotubes is 0.010% by mass or more and 0.040% by mass or less.
4. A floor coating material according to any one of claims 1 to 3, wherein the single-walled carbon nanotubes are pre-dispersed in a diluent reactive with the room temperature curing resin.
5. The floor coating material according to any one of claims 1 to 4, wherein the phthalocyanine pigment is phthalocyanine green.
6. The floor coating material according to any one of claims 1 to 5, further comprising an iron oxide pigment.
7. A method for forming a coated floor, comprising a step of applying the coated floor material according to any one of claims 1 to 6.
Citation Information
Patent Citations
Novel antistatic terrace system and production method
CN107652845A
Facilities for preventing infection
JP1996107913A
Coating liquid
JP2008280450A
carbon nanotube dispersion
JP2012502144A
Floor coating material formed through flow-spreading technique and antistatic coated floor
JP2013040446A