Biaxially oriented polyester film
A biaxially oriented polyester film with specific diol components and a biobased synthetic polymer content addresses flexibility, bending resistance, and rainbow unevenness issues, ensuring high-quality display performance in flexible and foldable applications.
Patent Information
- Application Number
- JP2020161694
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-09-28
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2040-09-28
AI Technical Summary
Conventional biaxially oriented polyester films lack flexibility, bending resistance, and exhibit rainbow unevenness and poor heat resistance, making them unsuitable for flexible and foldable display applications.
A biaxially oriented polyester film composed of an aromatic dicarboxylic acid component and a diol component with a specific molar ratio of diol components having even and odd numbers of carbon atoms in the main chain, along with a biobased synthetic polymer content, to enhance flexibility, heat resistance, and reduce rainbow unevenness.
The film achieves high-quality display performance with both flexibility and heat resistance, suitable for flexible displays that require repeated bending, while minimizing rainbow unevenness and maintaining excellent mechanical properties.
Smart Images

Figure 0007567322000011 
Figure 0007567322000012 
Figure 0007567322000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a biaxially oriented polyester film. [Background technology]
[0002] Thermoplastic resin films, especially biaxially oriented polyester films, are widely used as substrate films in many applications such as magnetic recording materials and packaging materials because of their excellent mechanical properties, electrical properties, dimensional stability, transparency, and chemical resistance. In particular, in recent years, in the fields of flat panel displays and touch panels, there has been an increasing demand for various optical films, such as cover films that prevent scratches on the display surface of flexible displays. Image display devices using self-illuminating bodies called organic light-emitting diodes (hereinafter referred to as "organic electroluminescent display devices") have been put into practical use, and since these organic electroluminescent display devices use self-illuminating bodies compared to conventional liquid crystal display devices, they are not only superior in terms of visibility and response speed, but also do not require auxiliary lighting devices such as backlights, making it possible to make the display devices thinner and more flexible. For this reason, the development of flexible display devices that can be folded or rolled has accelerated, and folding resistance is required. In addition, for polarizer protective film applications, the replacement of conventional TAC (triacetyl cellulose) films with biaxially oriented polyester films has been actively considered for the purpose of reducing costs. For example, a hard coat film in which hard coat layers are laminated on both sides of a substrate containing a polyester film has been proposed as a method for improving scratch resistance for image display devices (Patent Document 1). Also, an antireflection film in which an antireflection layer is provided on at least one side of a flexible transparent resin film containing a polyester film has been proposed for flexible displays (Patent Document 2).
[0003] In addition, when a biaxially oriented film is used as a polarizer protective film, rainbow unevenness is visually observed when viewed obliquely due to the large birefringence in the plane direction and thickness direction. For this reason, a method is known for suppressing the orientation in the plane direction of biaxially oriented polyester films that have been studied in the past to keep the birefringence low and suppress rainbow unevenness (Patent Document 3). In addition, a method has been devised to make rainbow unevenness invisible to the naked eye by largely orienting in one axis direction and largely controlling the birefringence (Patent Documents 4 and 5). Furthermore, for flexible display devices, an antireflection film has been proposed in which an antireflection layer is provided on at least one surface of a flexible transparent resin film containing a biaxially oriented polyester film (for example, Patent Document 6). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2015-61750 A [Patent Document 2] JP 2016-75869 A [Patent Document 3] International Publication No. 2015 / 093307 [Patent Document 4] JP 2013-200435 A [Patent Document 5] JP 2016-21000 A [Patent Document 6] JP 2016-75869 A Summary of the Invention [Problem to be solved by the invention]
[0005] When the above conventional techniques are used as films for image display devices, they are characterized by a hard coat layer and an anti-reflection layer, and the substrate film does not take into consideration bending resistance, making it difficult to apply them to flexible displays. Although they are effective in suppressing rainbow unevenness, they also have issues with heat resistance due to low orientation characteristics and are difficult to apply to foldable applications that require repeated folding due to strong anisotropy.
[0006] Therefore, the present invention aims to eliminate the above-mentioned drawbacks and provide a biaxially oriented polyester film that is flexible, resistant to bending, has little visible iridescent unevenness, and has excellent heat resistance. [Means for solving the problem]
[0007] In order to solve the above problems, the biaxially oriented polyester film of the present invention has the following configuration. (1) A biaxially oriented polyester film having as its main components an aromatic dicarboxylic acid component and a diol component, wherein the diol component comprises a diol component (Ev) having an even number of carbon atoms in its main chain and a diol component (Od) having an odd number of carbon atoms in its main chain, and wherein the molar ratio (Ev) / (Od) of the diol component (Ev) to the diol component (Od) is 88 / 12 to 50 / 50, and wherein the difference ΔT between the maximum and minimum values of the spectral transmittance at a wavelength of 400 to 800 nm measured by the following measuring method is 0% or more and 30% or less. (Measurement method) The film was cut into a length of 4.0 cm and a width of 5.0 cm, and the film was sandwiched between two polarizing plates (Kenis Co., Ltd., polarizing film thin S size, transmittance 0.43, polarization rate 0.9999) so that the absorption axis of the polarizing plate was parallel to the length of the film to prepare a measurement sample. The measurement was performed using a Hitachi High-Technologies Corporation spectrophotometer U-4100 equipped with an attached U-4100 type spectrophotometer angle variable transmission accessory, a light source mask of 8 mm (H) x 5 mm (W), and a mirror-based normal incidence detector to measure the light transmittance of 400 to 800 nm. The measurement conditions were a scanning speed of 600 nm / min, a sampling pitch of 1 nm, and high-resolution measurement mode. During measurement, the angle of the angle-variable transmission accessory is set to 30°, and the sample is placed so that the angle between the film width direction and the horizontal plane is 30°, based on the state where the absorption axis of the polarizing plate coincides with the horizontal plane. For baseline measurement, two polarizing plates alone are stacked so that their absorption axes coincide with each other, and the measurement is performed in the same manner as above. The difference between the maximum and minimum light transmittance at wavelengths of 400 to 800 nm is calculated as ΔT. In the above evaluation, if the longitudinal direction and width direction are unknown, an arbitrary direction is set as 0° as the reference, and the refractive index is measured from 0 to 360° in 15° increments from there, and the direction with the highest refractive index is set as the longitudinal direction, and the direction perpendicular to that is the width direction. The refractive index is measured using an Abbe refractometer with sodium D line (wavelength 589 nm) as a light source. (2) The spectral transmittance is 60% or more at any wavelength from 400 to 800 nm. (3) The diol component (Od) includes at least one diol component having a main chain carbon number of 3, 5, or 7. (4) The diol component (Od) is trimethylene glycol. (5) The bio-based synthetic polymer content is 10 mol % or more. (6) The bending stiffness obtained from a loop stiffness tester is 0.1 mN or more and 1.0 mN or less. (7) The tear strength in both the longitudinal and transverse directions is 3.0 mN / mm or more. (8) The crystalline melting energy ΔHm of the film is 25 J / g or more and 55 J / g or less. (9) Used in flexible displays. Effect of the Invention
[0008] The biaxially oriented polyester film of the present invention can display high quality images even when mounted on a display device such as a flat panel display, and since it has both flexibility and heat resistance, it is particularly suitable for use in displays that involve repeated bending. [Brief description of the drawings]
[0009] [Figure 1] FIG. 2 is a diagram showing a schematic diagram of measurement of spectral transmittance. [Diagram 2] FIG. 2 is a diagram showing a schematic diagram of measurement of spectral transmittance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The biaxially oriented polyester film of the present invention will be described in detail below. The biaxially oriented polyester film of the present invention is a biaxially oriented polyester film mainly composed of an aromatic dicarboxylic acid component and a diol component, and the diol component includes a diol component (Ev) having an even carbon number in the main chain and a diol component (Od) having an odd carbon number in the main chain, and has a polyester layer A in which the molar ratio (Ev) / (Od) of the diol component (Ev) to the diol component (Od) is 88 / 12 to 50 / 50. This configuration not only suppresses rainbow unevenness when mounted on a flat panel display, but also exhibits excellent flexibility and bending resistance because the main carbon chain of the diol component contains an even component and an odd component. The flexibility referred to here is an index of the Young's modulus obtained by the method described in Evaluation method (11) Young's modulus of biaxially oriented polyester film, and indicates that the Young's modulus in both the longitudinal and transverse directions is low. A film having 3.5 GPa or less in both the longitudinal and transverse directions can be said to have excellent flexibility. The Young's modulus in either the longitudinal or transverse direction is preferably less than 3.3 GPa, and both the longitudinal and transverse directions are preferably less than 3.3 GPa. The mechanism by which rainbow unevenness can be suppressed is that by including a diol component having an odd number of carbon atoms in the main chain and a diol component having an even number of carbon atoms in the main chain, rainbow unevenness can be suppressed when mounted on a flat panel display compared to a case in which the main chain is composed only of diol components having an even number of carbon atoms, and heat resistance is superior to a case in which the main chain is composed only of diol components having an odd number of carbon atoms. In addition, the larger the main chain carbon number of the diol component, the longer the molecular chain, improving flexibility and bending resistance. On the other hand, if the main chain carbon number is too large, heat resistance may be poor.
[0011] When the molar ratio (Ev) / (Od) of the diol component (Ev) having an even number of carbon atoms in the main chain and the diol component (Od) having an odd number of carbon atoms in the main chain constituting the polyester layer A is more than 88 / less than 12, the low retardation property and flexibility are poor, and when it is less than 50 / more than 50, the heat resistance is poor. A molar ratio (Ev) / (Od) of 80 / 20 to 60 / 40 is preferable from the viewpoint of achieving both low retardation property and heat resistance.
[0012] In the present invention, from the viewpoint of heat resistance, the diol component (Od) having an odd number of carbon atoms in the main chain preferably contains at least one of diol components having a carbon number of 3, 5, or 7. If the main chain carbon number of the diol component (Od) having an odd number of carbon atoms in the main chain exceeds 7, the heat resistance may be poor. In addition, when considering all of low retardation, heat resistance, and flexibility, the diol component (Od) is most preferably trimethylene glycol.
[0013] In the present invention, from the viewpoint of heat resistance, the diol component (Ev) having an even number of carbon atoms in the main chain preferably contains at least one of diol components having a main chain carbon number of 2 or 4. From the viewpoint of heat resistance, it is most preferable that it is ethylene glycol having a main chain carbon number of 2. From the viewpoint of heat resistance, it is preferable that the main chain carbon number of the diol component (Ev) having an even number of carbon atoms in the main chain is smaller than that of the diol component (Od) having an odd number of carbon atoms in the main chain.
[0014] In the present invention, the polyester dicarboxylic acid component may be a single component or may be composed of two or more kinds. For example, when the dicarboxylic acid component is composed of two or more kinds, the thermal properties such as the glass transition temperature and the crystallinity can be adjusted compared to the case where the polyester is composed of a single component.
[0015] In the present invention, when the polyester contains two or more types of diol components and / or dicarboxylic acid components, a method in which the polyester resin contains 60 mol % or more of structural units derived from ethylene glycol relative to the structural units derived from the diol, or a method in which the polyester resin contains 60 mol % or more of structural units derived from terephthalic acid relative to the structural units derived from the dicarboxylic acid is preferably used.
[0016] Examples of structural units of the diol component (Ev) having an even number of carbon atoms in the main chain constituting the biaxially oriented polyester of the present invention include ethylene glycol, 1,3-butanediol, 1,4-butanediol, tetramethylene glycol, 1,6-hexanediol, 1,2-cyclohexanedimethanol, 1,3-cyclohexanedimethanol, 1,4-cyclohexanedimethanol, diethylene glycol, triethylene glycol, polyalkylene glycols having an even number of carbon atoms, isosorbate, etc. From the viewpoint of achieving both heat resistance and iridescent unevenness, ethylene glycol, 1,4-butanediol, isosorbide, and 1,4-cyclohexanedimethanol are preferred.
[0017] Examples of the structural unit of the diol component (Od) having an odd number of carbon atoms in the main chain constituting the biaxially oriented polyester of the present invention include 1,2-propanediol, 1,3-propanediol, neopentyl glycol, 1,5-pentanediol, 1,7-heptanediol, 2,2-bis(4-hydroxyethoxyphenyl)propane, spiroglycol, etc. Among them, 1,3-propanediol is preferably used from the viewpoint of achieving both rainbow unevenness and light-emitting diode pattern.
[0018] In addition, as the aromatic dicarboxylic acid component of the present invention, structural units derived from dicarboxylic acids other than structural units derived from terephthalic acid include, for example, structural units derived from aromatic dicarboxylic acids such as isophthalic acid, phthalic acid, 1,4-naphthalenedicarboxylic acid, 1,5-naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, 4,4'-diphenyldicarboxylic acid, 4,4'-diphenyletherdicarboxylic acid, and 4,4'-diphenylsulfonedicarboxylic acid. Among them, isophthalic acid, cyclohexanedicarboxylic acid, and naphthalenedicarboxylic acid are preferably used from the viewpoint of flexibility. These structural units derived from dicarboxylic acids may be used alone or in combination with two or more types other than the structural units derived from terephthalic acid, and may further be partially copolymerized with oxyacids such as hydroxybenzoic acid.
[0019] From the viewpoint of heat resistance, the biaxially oriented polyester film of the present invention preferably has a crystalline melting energy ΔHm of 25 J / g or more and 55 J / g or less. Here, heat resistance refers to a property obtained by evaluation using the method described in Evaluation Method (10) Heat Resistance. Conventionally, when controlling the birefringence of a stretched polyester film to be low, it is known that the birefringence caused by stretching is suppressed by lowering the crystallinity of the resin, but in the present application, as described above, the polyester layer A is provided, so that low birefringence can be maintained even if orientation and crystallization progress by stretching. Therefore, it is possible to maintain high crystallinity while maintaining low birefringence, which makes it possible to maintain heat resistance. Therefore, it is preferable that the crystalline melting energy ΔHm of the film is 25 J / g or more and 55 J / g or less. If the crystalline melting energy ΔHm is less than 25 J / g, it is advantageous for suppressing iridescent unevenness, but heat resistance may be poor. On the other hand, although there is no particular upper limit within the range in which the effects of the present invention are achieved, when polyester is used as the main component, it is difficult to make the crystal melting energy ΔHm exceed 55 J / g. There is no particular limitation on the method for making the crystal melting energy ΔHm 25 J / g or more. In addition, a method of forming a film by mixing only a plurality of homopolyesters is cited as a preferred method. The polyester layer A of the present application is mainly composed of an aromatic dicarboxylic acid component and a diol component, and the diol component includes a diol component (Ev) having an even number of carbon atoms in the main chain and a diol component (Od) having an odd number of carbon atoms in the main chain. The molar ratio (Ev) / (Od) of the diol component (Ev) to the diol component (Od) is 88 / 12 to 50 / 50. However, it is preferable to obtain a biaxially oriented polyester film with the above molar ratio (Ev) / (Od) by mixing a homopolyester having a diol component having an odd number of carbon atoms in the main chain and a homopolyester having a diol component having an even number of carbon atoms in the main chain, from the viewpoint of obtaining a ΔHm of 25 J / g or more and 55 J / g or less. It is presumed that this is because mixing homopolyesters having crystallinity suppresses ester exchange during melt extrusion and suppresses the decrease in ΔHm. In addition, in the case of polyester-based resins, ΔHm is often limited to 55 J / g.In addition, from the viewpoint of controlling the crystal melting energy ΔHm to 25 J / g or more and 55 J / g or less, when a copolymerization component is introduced, it is preferable that both the dicarboxylic acid component and the diol component are 11 mol% or less. If the copolymerization component exceeds 15 mol% and the crystal melting energy is 25 J / g or less, it is advantageous for reducing iridescent unevenness, but heat resistance may be poor. From the viewpoint of heat resistance, it is preferable that the crystal melting energy ΔHm is 35 J / g or more.
[0020] From the viewpoint of global environmental conservation, the biaxially oriented polyester film of the present invention preferably has a bio-based synthetic polymer content of 10 mol% or more. Here, bio-based synthetic polymer refers to a resin whose raw material is derived from living organisms. Representative examples include polylactic acid made from plants such as corn and sugarcane, polyhydroxyalkanoic acid synthesized by microorganisms, and resins made from plant-derived 1,3-propanediol. The bio-based synthetic polymer content can be evaluated by distinguishing between carbon derived from biomass and carbon derived from fossils according to the bio-based concentration test standard ASTM D6866.
[0021] The biaxially oriented polyester film of the present invention has a difference ΔT between the maximum and minimum values of the spectral transmittance at a wavelength of 400 to 800 nm, as measured by the following measuring method, of 0% or more and 30% or less. (Method of measuring spectral transmittance) The film was cut into a length of 4.0 cm and a width of 5.0 cm, and the film was sandwiched between two polarizing plates (Kenis Co., Ltd., polarizing film thin S size, transmittance 0.43, polarization rate 0.9999) so that the absorption axis of the polarizing plate was parallel to the length of the film to prepare a measurement sample. The measurement was performed using a Hitachi High-Technologies Corporation spectrophotometer U-4100 equipped with an attached U-4100 type spectrophotometer angle variable transmission accessory, a light source mask of 8 mm (H) x 5 mm (W), and a mirror-based normal incidence detector to measure the light transmittance of 400 to 800 nm. The measurement conditions were a scanning speed of 600 nm / min, a sampling pitch of 1 nm, and high-resolution measurement mode. During measurement, the angle of the angle-variable transmission accessory is set to 30°, and the sample is placed so that the angle between the film width direction and the horizontal plane is 30°, based on the state where the absorption axis of the polarizing plate coincides with the horizontal plane. For baseline measurement, two polarizing plates alone are stacked so that their absorption axes coincide with each other, and the measurement is performed in the same manner as above. The difference between the maximum and minimum light transmittance at wavelengths of 400 to 800 nm is calculated as ΔT. By setting the spectral transmittance within the above range, rainbow unevenness can be suppressed when the film is mounted as a screen protection film or a polarizer protection film. In order to achieve this range, the polyester layer A is configured to have a resin composition that satisfies the requirements, and at least the ratio FOt / SOt obtained by dividing the total stretching ratio FOt in the longitudinal direction by the total stretching ratio SOt in the width direction, which is the direction perpendicular to the longitudinal direction, under the film forming conditions is set to 0.8 or more, and the total area ratio is set to 10 times or more. In order to suppress rainbow unevenness when the film is mounted as a polarizer protection film in a flat panel display or the like and improve visibility, it is preferable that the difference ΔT between the maximum and minimum values of the spectral transmittance measured by the above measurement method is 0% or more and 20% or less, and preferably 0% or more and 15% or less. It is most preferable that ΔT is 0% from the viewpoint of suppressing rainbow unevenness, but when ΔT is close to 0%, the anisotropy of the in-plane orientation of the film needs to be very strong, and the tear strength in the direction of strong orientation may be poor. For this reason, when considering both rainbow unevenness and tear strength, ΔT is preferably 5% or more. In order to keep ΔT at 5% or more and 15% or less, it is preferable to control FOt / SOt to 1.0 or more, preferably FOt / SOt to 1.5 or more, and the ratio of the final longitudinal stretching ratio to the total area stretching ratio to 0.1 or more. When FOt / SOt is 1.0 or more and the ratio of the final longitudinal stretching ratio to the total area stretching ratio is 0.2 or more, this is a preferable embodiment for keeping ΔT at 5% or less, but the tear strength may be poor.
[0022] The biaxially oriented polyester film of the present invention preferably has a spectral transmittance of 60% or more at any wavelength of 400 to 800 nm. By being in this range, the brightness of the liquid crystal becomes clear, and a higher quality image can be displayed. It is preferably 70% or more at any wavelength, and most preferably 80% or more. In order to achieve this range, it can be controlled by setting the total area stretch ratio to 10.5 times or more, FOt / SOt to 1.0 or more, and the final longitudinal stretch ratio to the total area stretch ratio to 0.1 or more. This is a preferred embodiment because the higher the longitudinal stretch ratio / transverse stretch ratio FOt / SOt and the final stretch ratio are, the higher the spectral transmittance can be, within a range that does not impair the effects of the present invention.
[0023] The biaxially oriented polyester film of the present invention preferably has a bending stiffness of 0.1 mN or more and 1.0 mN or less, as measured by a loop stiffness tester. By being in this range, damage or functional deterioration due to repeated bending can be suppressed, and the film has excellent bending resistance. In order to control the bending stiffness low, the most effective method is to make the film thickness 50 μm or less, and then, it is a preferable method to reduce the Young's modulus of the film. In order to reduce the Young's modulus, the number of main chain carbon atoms of the diol component (Ev) having an even number of main chain carbon atoms and the diol component (Od) having an odd number of main chain carbon atoms can be increased, the value of the Ev / Od molar ratio can be reduced, and the total stretch ratio can be reduced. In addition, the Young's modulus can be reduced by adding a plasticizer or an elastomer within a range that does not impair the effects of the present invention. Examples of elastomers include Hytrel manufactured by DuPont. In addition, when the thickness of the film exceeds 50 μm, it is difficult to reduce the bending stiffness to 1.0 mN or less regardless of the Young's modulus of the biaxially oriented polyester film.
[0024] The biaxially oriented polyester film of the present invention preferably has a tear strength of 3.0 mN / mm or more in both the longitudinal and transverse directions. There is no particular upper limit, but if the biaxially oriented polyester film exceeds 100 mN / mm, the phase difference becomes too large, and rainbow unevenness may occur. By having tear strengths of 3.0 mN / mm or more in both the longitudinal and transverse directions, breakage during the winding process during film production can be suppressed, resulting in excellent mass productivity. The above range can be achieved by setting the areal stretch ratio to 10 times or more, FOt / SOt to 1.0 or more, and setting the ratio of the final longitudinal stretch ratio to the total areal stretch ratio to 0.2 or less.
[0025] The biaxially oriented polyester film of the present invention may be a single layer film consisting of only the polyester layer A, or may be a laminated biaxially oriented polyester film having a polyester layer other than the polyester layer A. In the case of a laminated biaxially oriented polyester film having a polyester layer other than the polyester layer A, it is preferable that the proportion of the polyester layer A in the entire laminated biaxially oriented polyester film is 80% or more. For example, by providing a slippery layer to which particles are added on both surface layers of the polyester layer A for the purpose of imparting the film with handleability and scratch resistance, the amount of particles added that cause a decrease in total light transmittance can be reduced throughout the entire film, and the decrease in total light transmittance can be suppressed while imparting slipperiness.
[0026] Furthermore, the biaxially oriented polyester film of the present invention may be laminated with various functional layers. For example, a laminate sheet having a layer containing a curable resin on at least one side of the biaxially oriented polyester film of the present invention may be mentioned. By forming a laminate sheet having a layer containing a curable resin on at least one side of the biaxially oriented polyester film of the present invention, it is possible to enhance the effect of suppressing scratches against impact from the curable resin layer side, and therefore it can be suitably used for flexible devices such as organic electroluminescence display devices. In addition, an easy-adhesion layer may be provided on the surface of the polyester layer A. By providing an easy-adhesion layer, the adhesion of the curable resin and the like is improved.
[0027] In addition, the biaxially oriented polyester film of the present invention may contain various additives, such as antioxidants, heat stabilizers, weather stabilizers, ultraviolet absorbers, organic lubricants, pigments, dyes, organic or inorganic fine particles, fillers, antistatic agents, nucleating agents, etc., to the extent that they do not deteriorate the properties of the film.
[0028] In order to stabilize the manufacturing process and impart durability in the usage environment, the biaxially oriented polyester film of the present invention preferably has a surface layer on at least one surface thereof exhibiting one or more functions selected from the group consisting of hard coat properties, self-repair properties, antiglare properties, antireflection properties, low reflectivity, ultraviolet shielding properties, and antistatic properties.
[0029] Next, a preferred method for producing the film of the present invention will be described below, but the present invention should not be construed as being limited to such an example.
[0030] 30% by mass of polytrimethylene terephthalate as a resin constituting the polyester layer A and 70% by mass of polyethylene terephthalate copolymerized with 10 mol% isophthalic acid as another resin are fed to a vented twin-screw extruder and melt-extruded. At this time, it is preferable to control the oxygen concentration in the extruder to 0.7% by volume or less under a flowing nitrogen atmosphere and the resin temperature to 240°C to 280°C. Next, the mixture is passed through a filter or a gear pump to remove foreign matter and to equalize the extrusion amount, and then discharged in a sheet form onto a cooling drum from a T-die. At this time, the sheet-shaped polymer is adhered to the casting drum by a static electricity application method using an electrode to which a high voltage is applied to bring the cooling drum and the resin into contact with each other by static electricity, a casting method in which a water film is provided between the casting drum and the extruded polymer sheet, a method in which the casting drum temperature is made lower than the glass transition point of the polyester resin to make the extruded polymer adhere, or a method in which a combination of these methods is used, and the sheet-shaped polymer is then adhered to the casting drum, cooled and solidified, to obtain an unstretched film. Among these casting methods, when polyester is used, the static electricity application method is preferably used from the viewpoints of productivity and flatness.
[0031] The biaxially oriented polyester film of the present invention is preferably biaxially oriented from the viewpoints of heat resistance, dimensional stability, mechanical strength, flatness, and thickness unevenness. Biaxial orientation can be obtained by stretching an unstretched film in the longitudinal direction and then in the width direction, or by a sequential biaxial stretching method in which the film is stretched in the width direction and then in the longitudinal direction, or by a simultaneous biaxial stretching method in which the film is stretched in the longitudinal direction and the width direction almost simultaneously. In addition, the film may be further stretched in the longitudinal direction or the width direction after biaxial orientation.
[0032] In the stretching method, the stretching ratio in the first axis is preferably 1.05 to 2.0 times, or 2.6 to 4.0 times. If the stretching ratio in the first axis is more than 2.0 times and less than 2.6 times, the thickness unevenness becomes large and the phase difference may vary. The stretching speed is preferably 1,000% / min to 200,000% / min. The preheating temperature is preferably the glass transition temperature of the resin -30°C or more and the glass transition temperature of the resin +10°C or less, and the stretching temperature is preferably the glass transition temperature of the resin or more and the glass transition temperature of the resin +40°C or less.
[0033] The biaxial stretching ratio is preferably 2.8 to 4.0 times, and more preferably 3 to 3.8 times. The biaxial stretching speed is desirably 1,000% / min to 200,000% / min. The preheating temperature is preferably at least 20°C below the glass transition temperature of the resin and at most 20°C above the glass transition temperature of the resin, and the stretching temperature is preferably at least the glass transition temperature of the resin and at most 60°C above the glass transition temperature of the resin.
[0034] In the present invention, the film may be further stretched in the longitudinal direction and the width direction after the biaxial stretching. When the film is further stretched after the biaxial stretching, the orientation is biased to the final stretching direction, the orientation angle is uniformed, and in-plane unevenness can be suppressed.
[0035] In the present invention, the total area stretching ratio is preferably 10 times or more from the viewpoint of thickness unevenness. In addition, in order to control the difference ΔT between the maximum and minimum values of the spectral transmittance to 0% or more and 30% or less, it can be controlled by setting the ratio FOt / SOt, which is the total stretching ratio in the longitudinal direction FOt divided by the total stretching ratio in the width direction perpendicular to the longitudinal direction, to 0.8 or more, the total area ratio to 10 times or more, and the ratio of the final longitudinal stretching ratio to the total area stretching ratio to 0.08 or more. A preferable control method is to set FOt / SOt to 1.0 or more, preferably FOt / SOt to 1.5 or more, and the ratio of the final longitudinal stretching ratio to the total area stretching ratio to 0.1 or more.
[0036] In the present invention, the film may be heat-treated after each stretching step. The heat treatment may be performed by any conventional method such as in an oven or on a heated roll. The heat treatment temperature is preferably 100°C or higher and lower than the crystal melting peak temperature Tm of the resin constituting the polyester layer A. When heat treatment is performed after each step, the highest heat treatment is preferably performed after the final stretching in terms of stretchability. In addition, when considering dimensional stability, the highest heat treatment temperature is preferably controlled to 160°C or higher and lower than the melting point of the resin constituting the polyester layer A -10°C. In addition, the heat treatment time can be any time within a range that does not deteriorate the properties, and is preferably 5 seconds to 60 seconds, more preferably 10 seconds to 40 seconds, and most preferably 15 seconds to 30 seconds.
[0037] Furthermore, in order to improve the adhesive strength with the polarizer, at least one side may be subjected to corona treatment or coated with an easy-adhesion layer. As a method for providing the coating layer in-line in the film manufacturing process, a method is preferred in which a coating layer composition dispersed in water is uniformly applied to a film that has been at least uniaxially stretched using a metaling wire bar or a gravure roll, and the coating agent is dried while being stretched, and in this case, the thickness of the easy-adhesion layer is preferably 0.01 μm or more and 1 μm or less. In addition, various additives such as antioxidants, heat stabilizers, ultraviolet absorbers, infrared absorbers, pigments, dyes, organic or inorganic particles, antistatic agents, nucleating agents, etc. may be added to the easy-adhesion layer. As a resin preferably used for the easy-adhesion layer, at least one resin selected from acrylic resins, polyester resins, and urethane resins is preferable in terms of adhesiveness and handling. Furthermore, off-annealing under conditions of 90 to 200° C. is also preferably used.
[0038] The biaxially oriented polyester film of the present invention has a small difference between the maximum and minimum values of spectral transmittance under specific conditions and is flexible, so that it does not exhibit interference colors when mounted on a display that is repeatedly folded or an image display device that has a curved surface, and is used as a polarizing plate by being laminated to a PVA sheet (polarizer) prepared by incorporating iodine into PVA and orienting it.
[0039] In the biaxially oriented polyester film of the present invention, when a surface layer is laminated on the outermost surface in order to impart functions such as hard coat properties, self-repair properties, antiglare properties, antireflection properties, low reflectivity, and antistatic properties, it is preferable to use a manufacturing method in which the above-mentioned coating composition is applied, dried, and cured to form the surface layer.
[0040] The method for producing the surface layer by coating is not particularly limited, but it is preferable to form the surface layer by coating the coating composition on a supporting substrate or the like by a dip coating method, a roller coating method, a wire bar coating method, a gravure coating method, a die coating method (U.S. Pat. No. 2,681,294), etc. Furthermore, among these coating methods, the gravure coating method or the die coating method is more preferable as the coating method.
[0041] Next, the applied liquid film is dried to completely remove the solvent, so the drying process preferably involves heating the liquid film. Drying methods include heat transfer drying (contact with a hot object), convection heat transfer (hot air), radiation heat transfer (infrared rays), and others (microwaves, induction heating). Among these, methods using convection heat transfer or radiation heat transfer are preferred because of the need to precisely uniform the drying speed even in the width direction.
[0042] Furthermore, a further curing operation (curing step) may be performed by irradiating heat or energy rays. In the curing step, when curing is performed by heat, the temperature is preferably from room temperature to 200° C., and from the viewpoint of activation energy of the curing reaction, the temperature is more preferably from 100° C. to 200° C., and even more preferably from 130° C. to 200° C.
[0043] When curing with active energy rays, electron beams (EB rays) and / or ultraviolet rays (UV rays) are preferred from the viewpoint of versatility. When curing with ultraviolet rays, it is preferred that the oxygen concentration is as low as possible in order to prevent oxygen inhibition, and it is more preferred to cure in a nitrogen atmosphere (nitrogen purging). When the oxygen concentration is high, the curing of the outermost surface is inhibited, and the surface curing may be insufficient. Examples of the type of ultraviolet lamp used for irradiating ultraviolet rays include discharge lamp type, flash type, laser type, and electrodeless lamp type. When curing with ultraviolet rays using a high-pressure mercury lamp that is a discharge lamp type, the illuminance of the ultraviolet rays is 100 to 3,000 mW / cm. 2 , preferably 200 to 2,000 mW / cm 2 , and more preferably 300 to 1,500 mW / cm2 It is preferable to perform ultraviolet irradiation under the conditions where the integrated amount of ultraviolet light is 100 to 3,000 mJ / cm 2 , preferably 200 to 2,000 mJ / cm 2 , and more preferably 300 to 1,500 mJ / cm 2 It is more preferable to perform ultraviolet irradiation under the condition that: 1. The illuminance of ultraviolet light is the irradiation intensity per unit area, and varies depending on the lamp output, emission spectrum efficiency, diameter of the light-emitting bulb, design of the reflector, and the distance between the irradiated object and the light source. However, the illuminance does not vary depending on the conveying speed. The integrated amount of ultraviolet light is the irradiation energy per unit area, and is the total amount of photons that reach the surface. The integrated amount of light is inversely proportional to the irradiation speed passing under the light source, and proportional to the number of irradiations and the number of lamps.
[0044] The biaxially oriented polyester film of the present invention has excellent bending resistance and can be particularly suitably used as a flexible device for use in flat panel displays and the like. For example, by applying it as a cover film for an organic electroluminescence display device, it is possible to prevent the display device surface from being scratched without impairing the flexibility of the display device. In addition to optical films, it is also preferred to use it as various cover films utilizing the characteristics of the present invention and as construction films for packaging applications.
[0045] (Methods for measuring characteristics and evaluating effects) The methods for measuring the characteristics and evaluating the effects of the present invention are as follows.
[0046] (1) Polyester composition The film was hydrolyzed with an alkali, and each component was analyzed by gas chromatography or high performance liquid chromatography, and the composition ratio was determined from the peak area of each component. An example is shown below. Dicarboxylic acid components and other components were measured by high performance liquid chromatography. Analysis can be performed using known measurement conditions, and an example of the measurement conditions is shown below. Note that the measurement was performed after filtering and separating inorganic particles. Equipment: Shimadzu LC-10A Column: YMC-Pack ODS-A 150×4.6mm S-5μm 120A Column temperature: 40℃ Flow rate: 1.2ml / min Detector: UV 240nm The diol components and other components were quantitatively determined by gas chromatography using known methods. The following is an example of the measurement conditions. Equipment: Shimadzu 9A (manufactured by Shimadzu Corporation) Column: SUPELCOWAX-10 capillary column 30m Column temperature: 140℃~250℃ (heating rate 5℃ / min) Flow rate: Nitrogen 25ml / min Detector: FID (2) Intrinsic viscosity of polyester The intrinsic viscosity of polyester resin and film was measured by dissolving polyester in orthochlorophenol and using an Ostwald viscometer at 25° C. In the case of a laminated film, the intrinsic viscosity of each layer alone can be evaluated by scraping off each layer of the film according to the laminate thickness.
[0047] (3) Film thickness, layer thickness The film was embedded in epoxy resin, and the cross section of the film was cut out with a microtome. The cross section was observed with a transmission electron microscope (TEM H7100 manufactured by Hitachi) at a magnification (any magnification between 100 and 5000) sufficient to grasp the overall image of the film cross section, and the film thickness and, in the case of a laminated structure, the thickness of each layer were determined.
[0048] (4) Longitudinal and transverse directions In the present invention, the flow direction during film production is defined as the longitudinal direction, and the direction perpendicular to the longitudinal direction is defined as the width direction. When the longitudinal direction and the width direction are unknown, an arbitrary direction is set as 0° as the reference, and the refractive index is measured from 0 to 360° at 15° intervals from there, and the direction with the highest refractive index is defined as the longitudinal direction, and the direction perpendicular to that is defined as the width direction. The refractive index is measured using an Abbe refractometer with sodium D line (wavelength 589 nm) as a light source.
[0049] (5) Refractive index Using sodium D line (wavelength 589 nm) as a light source, an Abbe refractometer was used to measure the refractive index (n MD ), the refractive index in the width direction (n TD ), the refractive index in the thickness direction (n ZD The plane orientation coefficient (fn) can be calculated from the following formula. fn=(n MD +n TD ) / 2-n ZD (6) Crystal melting energy ΔHm In accordance with JIS K7121 (1999), a differential scanning calorimeter robot DSC-RDC6220 manufactured by Seiko Denshi Kogyo Co., Ltd. was used for data analysis, and the crystal melting energy ΔHm [J / g] was measured and analyzed in accordance with JIS K-7122 (1987 edition). 5 mg of the biaxially oriented polyester film of the present invention was used as a sample, and the temperature of the apex of the endothermic peak obtained from the DSC curve when the temperature was raised from 25°C to 300°C at 20°C / min was taken as the melting point. In addition, the amount of heat per unit mass obtained from the endothermic peak area was taken as the crystal melting energy ΔHm [J / g]. When the DSC curve was straight, the points that left the baseline and the points that returned to the baseline before and after the peak were connected by a straight line, and when the DSC curve was curved, the analysis was performed by connecting the two points by the curved curve. When there are multiple endothermic peaks, the temperature at the apex of the highest endothermic peak was taken as the melting point, and the heat per unit mass obtained from the endothermic peak area was taken as the crystal melting energy ΔHm. Note that endothermic peaks with extremely small peak areas (0.5 J / g or less in terms of crystal melting energy) seen on the baseline were removed as noise.
[0050] (7) Spectral transmittance The film was cut into a length of 4.0 cm and a width of 5.0 cm, and the film was sandwiched between two polarizing plates (Kenis Co., Ltd., polarizing film thin S size, transmittance 0.43, polarization rate 0.9999) so that the absorption axis of the polarizing plate was parallel to the length of the film to prepare a measurement sample. The measurement was performed using a Hitachi High-Technologies Corporation spectrophotometer U-4100 equipped with an attached U-4100 type spectrophotometer angle variable transmission accessory, a light source mask of 8 mm (H) x 5 mm (W), and a mirror-based normal incidence detector to measure the light transmittance of 400 to 800 nm. The measurement conditions were a scanning speed of 600 nm / min, a sampling pitch of 1 nm, and high-resolution measurement mode. During measurement, the angle of the angle-variable transmission accessory is set to 30°, and the sample is placed so that the angle between the film width direction and the horizontal plane is 30°, based on the state where the absorption axis of the polarizing plate coincides with the horizontal plane. For baseline measurement, two polarizing plates alone are stacked so that their absorption axes coincide with each other, and the measurement is performed in the same manner as above. The difference between the maximum and minimum light transmittance at wavelengths of 400 to 800 nm is calculated as ΔT.
[0051] (8) Visibility test (rainbow unevenness) A sample cut to a size of 300 mm in the longitudinal direction and 210 mm in the transverse direction was sandwiched between two polarizing plates (Kenis Corporation, thin polarizing film S size, transmittance 0.43, polarization rate 0.9999) so that the longitudinal direction of the film and the absorption axis of the polarizing plate were parallel to each other to prepare a test piece. When the test piece was placed on an LED light source (Trytec A3-101), the visibility was confirmed from an angle of 60° to the normal direction of the test piece plane.
[0052] ◎: Almost no interference color is observed.
[0053] ◯: A slight interference color is observed, but this does not affect practical use.
[0054] △: A slight interference color is observed, but this does not cause any problems in practical use.
[0055] ×: interference colors are clearly observed, and the display is not suitable for use as a display.
[0056] (9) Haze value Measurements were made according to JIS K-7105 using a direct-reading haze computer manufactured by Suga Test Instruments Co., Ltd. Each measurement was made three times, and the average value was used.
[0057] (10) Heat resistance □Samples cut into 100 mm squares were hung in a tree shape in a 120°C hot air oven so as not to come into contact with the top, bottom, left, or right walls of the oven. They were then stored for 4 hours and heat-treated, after which the haze of the film was measured and the increase in haze compared to before heat treatment was judged according to the following criteria.
[0058] ◎: Haze increase is less than 1% ○: Haze increase is 1% or more and less than 3% △: Haze increase is 3% or more but less than 5% ×: Haze increase exceeds 5% (11) Young’s modulus of biaxially oriented polyester film A rectangular sample of 150 mm in length and 10 mm in width was cut out in the longitudinal and transverse directions of the film. Young's modulus was measured using an Instron-type tensile tester according to the method specified in JIS Z1702. The measurement was carried out under the following conditions, with 10 samples, and the average value was calculated. Measuring device: Orientec Co., Ltd.'s automatic film strength and elongation measuring device "Tensilon AMF / RTA-100" Sample size: width 10mm x length 50mm Pulling speed: 300mm / min Measurement environment: temperature 23℃, humidity 65%RH.
[0059] (12) Bending rigidity Using a loop stiffness tester manufactured by Toyo Seiki Seisakusho Co., Ltd., the sample was cut into a length of 120 mm and a width of 5 mm in the measurement direction, and measurements were taken with a loop circumference of 100 mm and a crushing distance of 5 mm, and the peak value was taken as the bending stiffness (mN). Next, measurements were taken five times in both the longitudinal and transverse directions, and the average value for each measurement direction was taken as the bending stiffness.
[0060] (13) Bending resistance Using a U-shaped stretch tester (Yuasa System Devices, DLDMLH-FS), a sample was cut to a length of 112 mm and a width of 108 mm, with the long side being the direction in which the bending hysteresis 2HB in the film plane was the smallest. The sample was attached to the end of the tilt clamp so that the tilt clamp was in a horizontal position and the stroke direction was the length direction of the sample. The sample was bent 10,000 times at a test speed of 60 r / min, a test stroke of 60 mm, and a face-to-face distance of 3 mm. After the test, the sample was judged as follows based on the reflected light from the fluorescent light on the side and its appearance. A: No change in appearance was observed, and no distortion of reflected light was observed. B: No change in appearance, but distortion of reflected light was observed. C: Faint fold lines were visible, but no practical problems were observed. D: Fold lines were clearly observed on the exterior.
[0061] (14) Tear strength (tear propagation resistance) Measurements were made in accordance with JIS-K-7128-2 (1998 model) using a light-load tear tester manufactured by Toyo Seiki Co., Ltd. The film was cut into a 50 mm wide x 64 mm long sample in the longitudinal and transverse directions. A 13 mm cut was made in the longitudinal direction from the end of the widthwise center of this sample, and the resistance value was read when the remaining 51 mm in the longitudinal direction was torn off, and the average value of 10 measurements was taken as the tear strength [mN / mm].
[0062] (15) Bio-based synthetic polymer content According to the biobased content test standard ASTM D6866, the biobased synthetic polymer content (mol%) was calculated by distinguishing between carbon derived from biomass and carbon derived from fossil fuels. EXAMPLES
[0063] (Production of polyester) The polyester resin used for film formation was prepared as follows.
[0064] (Polyester A) A polyethylene terephthalate resin (intrinsic viscosity 0.7) having 100 mol % terephthalic acid as the dicarboxylic acid component and 100 mol % ethylene glycol as the glycol component.
[0065] (Polyester B) An isophthalic acid copolymerized polyethylene terephthalate resin (intrinsic viscosity 0.8) having a dicarboxylic acid component of 90 mol % terephthalic acid component, 10 mol % isophthalic acid component, and a glycol component of 100 mol % ethylene glycol component.
[0066] (Polyester C) An isophthalic acid copolymerized polyethylene terephthalate resin (intrinsic viscosity 0.8) having, as the dicarboxylic acid component, 78 mol % of a terephthalic acid component, 22 mol % of an isophthalic acid component, and as the glycol component, 100 mol % of an ethylene glycol component.
[0067] (Polyester D) A naphthalenedicarboxylic acid copolymerized polyethylene terephthalate resin (intrinsic viscosity 0.8) having, as a dicarboxylic acid component, 86.5 mol % of a terephthalic acid component, 13.5 mol % of a naphthalenedicarboxylic acid component, and as a glycol component, 100 mol % of an ethylene glycol component.
[0068] (Polyester E) A spiroglycol copolymerized polyethylene terephthalate resin (intrinsic viscosity 0.8) having 100 mol % of terephthalic acid as a dicarboxylic acid component, 86.5 mol % of ethylene glycol as a glycol component, and 13.5 mol % of spiroglycol as a glycol component.
[0069] (Polyester F) A cyclohexanedimethanol copolymerized polyethylene terephthalate resin (intrinsic viscosity 0.8) having 100 mol % of terephthalic acid as a dicarboxylic acid component, 80 mol % of ethylene glycol as a glycol component, and 20 mol % of cyclohexanedimethanol as a glycol component.
[0070] (Polyester G) Polyheptylene terephthalate resin (intrinsic viscosity 1.4) containing 100 mol % terephthalic acid as the dicarboxylic acid component and 100 mol % 1,7-heptanediol as the glycol component.
[0071] (Polyester H) Polypentylene terephthalate resin (intrinsic viscosity 1.4) containing 100 mol % terephthalic acid as the dicarboxylic acid component and 100 mol % 1,5-pentanediol as the glycol component.
[0072] (Polyester I) Polypropylene terephthalate resin (intrinsic viscosity 1.4) containing 100 mol% terephthalic acid as the dicarboxylic acid component and 100 mol% 1,3-propanediol as the glycol component. Bio-resource-derived component content: 37% by weight.
[0073] (Polyester J) Polybutylene terephthalate (intrinsic viscosity 1.2) having 100 mol % terephthalic acid as the dicarboxylic acid component and 100 mol % 1,4-butanediol as the glycol component.
[0074] (Polyester K) The dicarboxylic acid component is 100 mol % terephthalic acid, and the glycol component is ethyl. R Polyester resin (intrinsic viscosity 0.8) containing 75.5 mol% ethylene glycol and 24.5 mol% 1,3-propanediol. (Particle Master A) Polyethylene terephthalate particle master (intrinsic viscosity 0.65) containing aggregated silica particles with a number average particle diameter of 2.2 μm at a particle concentration of 2.0 mass % in polyester A.
[0075] (Examples 1 to 3 7 , Comparative Examples 1 to 9) The composition was as shown in Tables 1 and 6, and the raw materials were fed to a vented co-rotating twin-screw extruder with an oxygen concentration of 0.2% by volume, melted at the extruder cylinder temperature (extrusion temperature), short tube temperature, and die temperature shown in Table 1, and discharged from a T-die into a sheet onto a cooling drum controlled at the temperatures shown in Tables 2 and 7. At that time, electrostatic was applied using a wire-shaped electrode with a diameter of 0.1 mm, and an unstretched sheet was obtained by adhering it to the cooling drum. Next, a biaxially oriented polyester film was obtained under the film-forming conditions shown in Tables 2 and 7. All of the films obtained in the examples were excellent in heat resistance, bending resistance, and visibility. On the other hand, the comparative examples were inferior in heat resistance, bending resistance, and visibility.
[0076] [Table 1]
[0077] [Table 2]
[0078] [Table 3]
[0079] [Table 4]
[0080] [Table 5]
[0081] [Table 6]
[0082] [Table 7]
[0083] [Table 8]
[0084] [Table 9]
[0085] [Table 10] [Industrial Applicability]
[0086] The present invention uses a polyester resin of a specific composition and has a spectral transmittance in a specific range under specific conditions, and therefore can be used for optical films for flat panel displays and the like that are resistant to bending, have little visible rainbow unevenness, and have excellent heat resistance. [Explanation of symbols]
[0087] 1:Light source 2: Measurement sample 3: Normal incidence detector 4: Angle of the variable angle transmission device 5: Angle between the film length and the horizontal plane 6: Longitudinal direction of film 7: Horizontal plane a: Orthogonal direction to the surface direction of measurement sample 2
Claims
1. The biaxially oriented polyester film is a biaxially oriented polyester film mainly composed of an aromatic dicarboxylic acid component and a diol component, the diol component includes a diol component (Ev) having an even number of carbon atoms in its main chain and a diol component (Od) having an odd number of carbon atoms in its main chain, and the biaxially oriented polyester film has a polyester layer A having a molar ratio (Ev) / (Od) of the diol component (Ev) to the diol component (Od) of 88 / 12 to 50 / 50, The structural unit of the diol component (Ev) having an even carbon number in the main chain is one or more of ethylene glycol, cyclohexanedimethanol, and 1,4-butanediol, The structural unit of the diol component (Od) having an odd number of carbon atoms in the main chain is one or more of spiroglycol, 1,7-heptanediol, 1,5-pentanediol, and 1,3-propanediol, and the difference ΔT between the maximum and minimum values of the spectral transmittance at a wavelength of 400 to 800 nm measured by the following measurement method is 0% or more and 30% or less. (Method of measuring spectral transmittance) The film was cut into a length of 4.0 cm and a width of 5.0 cm, and the film was sandwiched between two polarizing plates (Kenis Co., Ltd., thin polarizing film S size, transmittance 0.43, polarization rate 0.9999) so that the absorption axis of the polarizing plate was parallel to the length of the film to obtain a measurement sample. The measurement was performed using a Hitachi High-Technologies Corporation U-4100 spectrophotometer equipped with an attached U-4100 type spectrophotometer angle variable transmission accessory, a light source mask of 8 mm (H) x 5 mm (W), and a mirror-based normal incidence detector to measure the light transmittance of wavelengths of 400 to 800 nm. The measurement conditions were set to a scanning speed of 600 nm / min, a sampling pitch of 1 nm, and a high-resolution measurement mode. During measurement, the angle of the angle-variable transmission accessory is set to 30°, and the sample is placed so that the angle between the film width direction and the horizontal plane is 30°, based on the state in which the absorption axis of the polarizing plate coincides with the horizontal plane. For baseline measurement, two polarizing plates alone are stacked together so that their absorption axes coincide, and the measurement is performed in the same manner as above. The difference between the maximum and minimum light transmittance values at wavelengths of 400 to 800 nm is calculated as ΔT. In the above evaluation, when the longitudinal direction and the width direction are unknown, an arbitrary direction is set as 0° as a reference, and the refractive index is measured from 0° to 360° in 15° increments from there, and the direction with the highest refractive index is set as the longitudinal direction and the direction perpendicular to that is the width direction. The refractive index is measured using an Abbe refractometer with sodium D line (wavelength 589 nm) as a light source.
2. 2. The biaxially oriented polyester film according to claim 1, wherein the spectral transmittance is 60% or more at any wavelength from 400 to 800 nm.
3. 3. The biaxially oriented polyester film according to claim 1, wherein the diol component (Od) comprises at least one diol component having a main chain carbon number of 3, 5, or 7.
4. The biaxially oriented polyester film according to any one of claims 1 to 3, wherein the bio-based synthetic polymer content is 10 mol % or more.
5. 5. The biaxially oriented polyester film according to claim 1, wherein the bending stiffness in both the longitudinal and transverse directions measured by a loop stiffness tester is 0.1 mN or more and 1.0 mN or less.
6. The biaxially oriented polyester film according to any one of claims 1 to 5, wherein the tear strength in both the longitudinal direction and the transverse direction is 3.0 mN / mm or more.
7. 7. The biaxially oriented polyester film according to claim 1, wherein the crystalline melting energy ΔHm of the film is 25 J / g or more and 55 J / g or less.
8. The biaxially oriented polyester film according to any one of claims 1 to 7, which is mounted on a flexible display.
Citation Information
Patent Citations
Polyester film for forming
JP2005290354A
Polyester film for polarizing plate-protection
JP2013200435A
Hard coat film and image display unit
JP2015061750A
Optical polyester film and polarizing plate using the same, and transparent conductive film
JP2016001305A
Polarizer protective film, polarizing plate, and liquid crystal display device using the same
JP2016021000A