Fermentation liquid filtration method
The described method for fermentation liquid filtration using cross-flow filtration and chemical cleaning maintains membrane stability and efficiency by addressing fouling issues, thereby reducing cleaning frequency and costs.
Patent Information
- Application Number
- JP2020165357
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-09-30
- Filing Date
- 2020-09-30
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2040-09-30
AI Technical Summary
Fermentation liquids clog separation membranes due to substances like proteins, polysaccharides, and polyphenols, leading to frequent chemical cleaning, increased costs, and reduced water permeability over time.
A method involving cross-flow filtration, followed by rinsing with water and chemical solutions of specific pH and oxidizing agents, to maintain membrane cleanliness and stability.
The method enables stable, long-term repeated filtration by effectively cleaning and preventing membrane fouling, reducing cleaning frequency and costs.
Smart Images

Figure 0007567335000010 
Figure 0007567335000011 
Figure 0007567335000012
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for filtering a fermentation liquid using a membrane module in the fields of fermentation industry, food industry, and the like. [Background technology]
[0002] In particular, in the treatment of fermented liquid in the food industry, diatomaceous earth has traditionally been used to remove yeast, solids, colloids, etc. from beer and wine after fermentation, but there have been problems with the safety of diatomaceous earth itself, the inability to incinerate used diatomaceous earth, and the high disposal costs associated with the large amounts used. Therefore, in recent years, attention has been focused on the treatment of fermented liquid using separation membranes such as ultrafiltration membranes and microfiltration membranes, which are excellent for miniaturizing the equipment.
[0003] When treating fermented liquids such as beer and wine using a separation membrane module, a layer consisting of the removed microorganisms, their crushed materials, colloids, etc. forms on the membrane surface, which can clog the membrane and cause an increase in filtration pressure and a decrease in filtration rate over time.
[0004] As a membrane structure that is less likely to clog the membrane surface and can exhibit filtering properties, a membrane capable of so-called depth filtration has been developed in which the surface pore size on one side of the separation membrane is larger than the substance to be removed, and the other surface or the membrane thickness has a minimum pore size layer, and impurities are captured inside the membrane. Patent documents 1 and 2 propose a membrane with a gradient structure in which the pore size gradually increases from the outer surface of the hollow fiber membrane to the inner surface. The membranes disclosed in these documents either have insufficient water permeability, or have high water permeability but insufficient membrane rupture strength, and thus insufficient suppression of clogging.
[0005] Furthermore, relatively recently, hollow fiber membranes for beer filtration that contain a hydrophilic polymer and have an asymmetric structure have been disclosed, as described in Patent Documents 3 and 4. The filtration performance of the membranes disclosed in these documents is relatively high, but the membranes do not have sufficient washability with general-purpose chemicals such as an aqueous sodium hydroxide solution, and are not economical because expensive chemicals are required to achieve high washability.
[0006] Furthermore, Patent Document 5 proposes a hollow fiber membrane that is excellent in chemical resistance, excellent in mechanical breaking strength, and high pure water permeability by heat-treating a separation membrane made of a polyvinylidene fluoride resin at a constant temperature condition near the membrane melting point. However, in the manufacturing method disclosed therein, the solid parts shrink excessively, and fine gaps between the solid parts are partially blocked, resulting in a membrane with poor branching of the flow path. The above-mentioned membrane has a characteristic that the membrane area of the permeable flow path, i.e., the effective membrane area, is greatly reduced by local clogging, so that when filtering a liquid that is prone to clogging, such as a fermentation liquid, the effective membrane area decreases at an accelerated rate as the filtration proceeds. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] WO2002 / 058828 [Patent Document 2] WO2010 / 035793 [Patent Document 3] WO2016 / 182015 [Patent Document 4] WO2017 / 155034 [Patent Document 5] JP 2008-105016 A Summary of the Invention [Problem to be solved by the invention]
[0008] Fermentation liquid is filtered through a separation membrane for various purposes, such as separating fermentation products and concentrating microorganisms. However, the fermentation liquid contains various organic substances, such as proteins, polysaccharides, and polyphenols, which cause fouling of the separation membrane. Fouled separation membranes can be reused by recovering their water permeability through chemical cleaning, but if the separation membrane is prone to fouling, the frequency of chemical cleaning increases, and cleaning costs become high. Furthermore, repeated filtration of the fermentation liquid and chemical cleaning gradually accumulate fouling substances that cannot be washed away in the membrane, making it difficult to recover water permeability and lengthening the cleaning time.
[0009] The present invention has been made in view of the above, and an object of the present invention is to provide a method for filtering a fermentation liquid using a membrane module, which enables repeated filtration stably over a long period of time. [Means for solving the problem]
[0010] In order to solve the above-mentioned problems, the present invention provides the following techniques [1] to [9]. [1] A method for filtering a fermentation liquid by carrying out the following steps a to d in this order: (a) subjecting a fermentation liquid to cross-flow filtration using a membrane module having a separation membrane; (b) rinsing the separation membrane with water; (c) permeating the chemical solution having a pH of 10 to 14 from the secondary side to the primary side of the separation membrane; (d) rinsing the separation membrane with water; Including, The cross-flow membrane permeate in the step (a) has a total sugar concentration of 1000 mg / L or more and 100000 mg / L or less, a protein concentration of 50 mg / L or more and 10000 mg / L or less, and a polyphenol concentration of 50 mg / L or more and 10000 mg / L or less, The step c is (c-1) A step of passing a chemical solution A having a pH of 10 to 14 and an oxidant concentration of 0.01% or more from the secondary side to the primary side of the membrane module. A method for filtering a fermentation liquid comprising the steps of: [2] The step c is (c-2) A step before the step c-1, in which a chemical solution B having an oxidant concentration of less than 0.01% is permeated from the secondary side to the primary side of the separation membrane. The method for filtering a fermentation liquid according to [1], further comprising: [3] After step d, (e) passing a chemical solution C having a pH of 0 to 4 from the secondary side to the primary side of the separation membrane; (f) after step e, rinsing the membrane module with water; The method for filtering a fermentation liquid according to any one of [1] to [2], further comprising: [4] In the steps c and e, the flux (m 3 / m 2 / d) is 1.5 times or more and 10 times or less the cross-flow flux of the step a. [5] The chemical solution C is an aqueous solution containing at least one compound selected from the group consisting of hydrochloric acid, nitric acid, sulfuric acid, phosphoric acid, formic acid, acetic acid, propionic acid, butyric acid, citric acid, oxalic acid, ascorbic acid, and lactic acid. The method for filtering a fermentation liquid according to any one of [3] to [4]. [6] The chemical solutions A, B and C each contain at least one cleaning auxiliary selected from the group consisting of a surfactant, an enzyme and a chelating agent. A method for filtering a fermentation liquid using the membrane module described in any one of [1] to [5]. [7] A method for filtering a fermentation liquid according to any one of [1] to [6] above, in which the polysaccharide concentration Ct in the raw water is in the range of 1.3 to 15 times the concentration C0 at the start of the filtration when the process is transferred from step a to step b. [8] The method for filtering a fermentation liquid according to any one of [1] to [7] above, wherein the separation membrane is a hollow fiber membrane. [9] The separation membrane contains a hydrophobic polymer resin, The pore volume V2 of the pores having a diameter of less than 100 nm as measured by a gas adsorption method is 0.02 cm3 / g or more and less than 0.1 cm3 / g, The pore volume V1 of pores having a diameter of 100 nm or more as measured by mercury intrusion porosimetry is 0.1 cm3 / g or more, The ratio V1 / V2 of the pore volume V2 to the pore volume V1 is 3 or more and 60 or less. The method for filtering a fermentation liquid according to the above item [8]. V1: Pore volume with a pore diameter of 100 nm or more measured by mercury intrusion porosimetry V2: Pore volume with a pore diameter of less than 100 nm measured by gas adsorption method
[10] The method for filtering a fermentation broth according to the above [9], wherein the separation membrane has a breaking elongation of 38% or more.
[11] The separation membrane according to the above [9] or
[10] , wherein the shrinkage rate of the hollow fiber membrane length when the membrane is heat-treated in a water vapor atmosphere at 125°C for 20 hours is 0.5% or more.
[12] The separation membrane contains a hydrophilic polymer, The hydrophilic polymer contains a copolymer composed of N types of monomer units 1, 2,...i...N, and has a hydration energy density of 40 to 70 cal·mol -1 ·Å -3 is A method for filtering a fermentation liquid according to any one of [1] to
[11] above.
[0011]
number
[0012] [In formula (1), the hydration energy of any monomer unit i is the absolute value of the energy of the monomer unit i in water minus the energy of the monomer unit i in a vacuum, N is the total number of monomer species constituting the copolymer, i is an integer of 1 to N, and N is an integer of 2 or more.]
[13] The hydrophobic polymer resin is a fluorine-based resin or a sulfone-based resin. A method for filtering a fermentation liquid according to any one of [1] to
[12] above.
[14] The filtration in the step a is an external pressure filtration in which filtration is performed from the outer periphery to the inner periphery of the hollow fiber membrane, and in the steps c and e, the flux of the permeating chemical solution is 7.0 m per inner area of the hollow fiber membrane. 3 / m 2 / d or more 10m3 / m 2 The method for filtering a fermentation liquid according to any one of [1] to
[13] above, wherein the filtration rate is 100 / d or less. Effect of the Invention
[0013] The method for filtering a fermentation liquid using a membrane module of the present invention is a filtration method that repeats four steps: (a) cross-flow filtration of the fermentation liquid, (b) water rinsing, (c) alkaline chemical washing, and (d) water rinsing. In this method, the cross-flow membrane permeate composition in step a has a total sugar concentration of 1000 mg / L to 100,000 mg / L, a protein concentration of 50 mg / L to 10,000 mg / L, and a polyphenol concentration of 50 mg / L to 10,000 mg / L. In step c, a chemical washing is performed by passing a chemical solution having a pH of 10 to 14 and containing an oxidizing agent from the secondary side to the primary side. This provides a high cleaning effect in a short cleaning time and enables stable filtration over a long period of time. [Brief description of the drawings]
[0014] [Figure 1] FIG. 1 is a schematic diagram of a filtration device according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a flow chart showing an example of the method for filtering a fermentation broth of the present invention. [Diagram 3] FIG. 3 is a flow chart showing an example of the method for filtering a fermentation broth of the present invention. [Figure 4] FIG. 4 is a perspective view of a hollow fiber membrane used in the present invention. [Diagram 5] FIG. 5 is a perspective view showing an outline of the spherical structure contained in the hollow fiber membrane. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] The filtration method using the membrane module according to the embodiment of the present invention will be described in detail below with reference to the drawings. In the present invention, "upper" and "lower" are based on the state shown in the drawings and are for convenience, with the side into which the raw liquid flows being the "lower" direction and the side into which the filtrate flows being the "upper" direction. Usually, in the position of the membrane module when in use, the upper and lower directions coincide with the upper and lower directions in the drawings.
[0016] The configuration of a filtration device for a fermentation liquid according to an embodiment of the present invention will be described with reference to the drawings. Fig. 1 is a schematic diagram of a filtration device according to an embodiment of the present invention, and Fig. 2 is a flow chart showing an example of a method for filtering a fermentation liquid.
[0017] First, we will provide an overview of the entire process using the flowchart in Figure 2.
[0018] The method for filtering a fermentation liquid using a membrane module according to the present invention includes the following steps a to d. By repeating these steps a to d, it becomes possible to perform repeated filtration stably for a long period of time.
[0019] (a) a step of subjecting a fermentation liquid to cross-flow filtration using a membrane module having a separation membrane (b) After step (a), a step of rinsing the separation membrane with water. (c) after the step (b), injecting a chemical solution having a pH of 10 or more and 14 or less from the secondary side of the membrane of the membrane module to the primary side; (d) after step c, rinsing the separation membrane with water Furthermore, as shown in the flow chart of FIG. 3, by repeating steps a to f, which are steps a to d plus steps e and f, filtration can be stably and repeatedly performed for a longer period of time. (e) after the step d, a step of injecting a chemical solution having a pH of 0 or more and 4 or less from the secondary side of the membrane of the membrane module to the primary side; (f) After step e, rinsing the separation membrane with water. In the first step, step a, the fermentation liquid is cross-flow filtered using a membrane module. In this step a, the fouling state of the separation membrane can be judged from the transmembrane pressure difference, which is the pressure on the raw liquid side of the separation membrane minus the pressure on the filtrate side. When the transmembrane pressure difference value rises to a predetermined value, the process proceeds to step b, and when it is equal to or lower than the predetermined value, the cross-flow filtration of step a is continued. In step b, the membrane module is washed by rinsing with water. When step b is completed, the process proceeds to step c, where the membrane module is washed with a chemical solution. When step c is completed, a water rinse is performed in step d. Here, if the washing recovery is insufficient, after step d is completed, the process proceeds to step e, where additional chemical washing of the membrane module is performed. When step e is completed, a water rinse is performed in step f, and the process returns to step a again. The fermentation liquid is filtered by repeating steps a to d, or a to f.
[0020] <Undiluted solution> In this embodiment, a fermentation liquid is used as the raw liquid. Examples of the fermentation liquid include beer, wine, sake, vinegar, soy sauce, amino acid fermentation liquid, organic acid fermentation liquid, and fermentation liquid of biopharmaceuticals. The fermentation liquid contains a fermentation product produced by a microorganism, but the type of the microorganism and the type of the fermentation product are not limited to the specific examples.
[0021] It is preferable that the total sugar concentration of the filtrate obtained by permeating the fermentation liquid through the membrane module in the cross-flow filtration of step a is 1,000 mg / L or more and 100,000 mg / L or less, the protein concentration is 50 mg / L or more and 10,000 mg / L or less, and the polyphenol concentration is 50 mg / L or more and 10,000 mg / L or less.
[0022] The total sugar concentration, protein concentration, and polyphenol concentration in the fermentation liquid (i.e., the raw liquid) before passing through the membrane module may be the same as the filtrate that has passed through, or may be different from the filtrate that has passed through, depending on the pore size and structure of the separation membrane contained in the membrane module. When a part of the components is blocked by the separation membrane, the concentration of the components in the filtrate decreases compared to the concentration of the components in the raw liquid. Here, the total sugar concentration, protein concentration, and polyphenol concentration in the raw liquid or the filtrate can be calculated by the following methods. That is, the total sugar concentration is calculated by the phenol-sulfuric acid method or the monosaccharide quantification method by hydrolysis, the protein concentration is calculated by the BCA method, the Bradford method, the Lowry method, and the Pierce 660 nm Protein Assay method, and the polyphenol concentration is calculated by the Folin-Ciocalteu method, the Folin-Denis method, and the ferric tartrate absorptiometry method, but are not limited to these. (Step a) <Cross-flow filtration> Fermentation liquid contains various organic matter such as microorganisms, proteins, polysaccharides, and lipids, and dead-end filtration, which filters all of the liquid supplied to the membrane module, is prone to fouling. Therefore, cross-flow filtration, in which the raw fermentation liquid is flowed parallel to the membrane surface to wash the membrane surface while filtering, is more suitable (step (a-1) of cross-flow filtering the fermentation liquid through the membrane module).
[0023] As shown in Fig. 1, when performing cross-flow filtration, a fermentation liquid (stock liquid) is supplied from a stock liquid tank 1 to a membrane module 2 by a stock liquid pump 3, and a part of the stock liquid is returned to the stock liquid tank 1. In addition, the filtrate filtered through the separation membrane of the membrane module 2 is sent to a filtrate tank 6. Note that in order to improve the filtration operability of the fermentation liquid, a process such as centrifugation may be performed before the membrane filtration.
[0024] As described above, in cross-flow filtration, the raw liquid is circulated between the raw liquid tank 1 and the membrane module 2 because the raw liquid flows parallel to the membrane surface. In this case, it is preferable to adjust the circulation flow rate of the raw liquid to a constant membrane surface linear velocity. The membrane surface linear velocity refers to the circulation flow rate of the raw liquid divided by the cross-sectional area through which the circulation flow in the membrane module flows. The membrane surface linear velocity may be set appropriately according to the properties of the raw liquid, but is preferably 0.1 m / s to 3.0 m / s, and more preferably 0.3 m / s to 2.5 m / s. If the membrane surface linear velocity is less than 0.1 m / s, sufficient cleaning effect may not be obtained. In addition, if the membrane surface linear velocity exceeds 3.0 m / s, it is not preferable because the power cost becomes high. The flow rate of the raw liquid can be controlled by the raw liquid pump 3 and the circulation control valve 4.
[0025] The filtration flux during cross-flow filtration can be set appropriately according to the properties of the raw liquid. 3 / m 2 / d or more 2.5m 3 / m 2 / d or less, and 0.3m 3 / m 2 / d or more 2.0m 3 / m 2 It is more preferable that the filtration flux is 0.1 m 3 / m 2 If the filtration flux is less than 2.5 m / d, the number of membrane modules required will increase, leading to higher costs. 3 / m 2 If the ratio exceeds 1 / d, fouling of the separation membrane may progress rapidly, which is not preferable. The flow rate of the filtrate can be controlled by the raw liquid pump 3, the circulation control valve 4, and the filtrate control valve 5.
[0026] In filtration using a separation membrane, the fouling state of the separation membrane can be judged from the transmembrane pressure, which is the pressure on the raw liquid side of the separation membrane minus the pressure on the filtrate side. In the case of dead-end filtration, the transmembrane pressure can be calculated from the pressure gauge 21 on the raw liquid inlet side of the membrane module 2 and the pressure gauge 23 on the filtrate outlet side of the membrane module 2. At the same filtration flux, the transmembrane pressure increases as fouling of the separation membrane progresses. However, in the case of cross-flow filtration, the pressure loss is large when the raw liquid passes through the raw liquid side flow path of the membrane module 2 and flows back to the raw liquid tank 1, and the above-mentioned calculation method includes the pressure loss of the raw liquid side flow path, making it difficult to calculate the transmembrane pressure appropriately. Therefore, the transmembrane pressure can be calculated from the difference between the average value of the pressure gauge 21 on the raw liquid inlet side of the membrane module 2 and the pressure gauge 22 on the outlet side and the value of the pressure gauge 23 on the filtrate outlet side of the membrane module 2.
[0027] In the cross-flow filtration of step a, as the fouling of the separation membrane progresses, the transmembrane pressure difference increases, so it is preferable to move to step b when the membrane is clogged to a certain extent. The timing of moving to step b is determined based on the concentration C t It is preferable that the concentration C is in the range of 1.3 to 15 times the concentration C0 at the start of filtration. t When the concentration C0 is 1.3 or more, polysaccharides tend to accumulate on the membrane surface, so washing in the opposite direction to the filtration can provide a significant washing effect. t If the concentration C0 is 15 or less, the fouling of the separation membrane has not progressed excessively, and there is a high possibility that the water permeability of the separation membrane can be sufficiently restored by performing chemical cleaning.
[0028] The polysaccharide may be appropriately selected depending on the type of fermentation liquid and the fermentation raw materials, and examples thereof include β-glucan, amylose, amylopectin, pectin, dextran, cellulose, chitin, chitosan, glucomannan, and the like.
[0029] The concentration of polysaccharides in raw water can be measured by extracting a polysaccharide fraction from the raw water by ethanol precipitation or the like, subjecting the polysaccharide fraction to hydrolysis using enzymes or alkali, etc., and analyzing the resulting constituent monosaccharides using high performance liquid chromatography (HPLC), but this is not limited to this method.
[0030] <Backwash> Step a may include step (a-1) of performing cross-flow filtration, and step (a-2) of periodically stopping the cross-flow filtration and backwashing the membrane module. When permeability is restored by backwashing, the filtration time can be extended, and the frequency of chemical cleaning can be reduced, thereby reducing operating costs. Steps (a-1) and (a-2) can be repeated alternately any number of times.
[0031] Backwashing can be performed using filtrate or other liquids such as water. However, if you do not want other liquids such as water to be mixed into the raw liquid, you can backwash with filtrate, or you can switch by operating a valve to perform backwashing so that the backwash liquid does not get mixed into the raw liquid.
[0032] The backwash flux during backwashing may be set appropriately depending on the properties of the raw liquid and the fouling state of the separation membrane. 3 / m 2 / d or more 10.0m 3 / m 2 / d or less, and 1.5m 3 / m 2 / d or more 5.0m 3 / m 2 It is more preferable that the backwash flux is 1.0 m 3 / m 2 If the backwash flux is less than 10.0 m / d, the cleaning effect will be reduced, which is not preferable. 3 / m 2 If the ratio exceeds 1 / d, the power cost will increase and a large amount of liquid will be required for backwashing, which is not preferable.
[0033] If the separation membrane is a hollow fiber membrane, the filtration in step a is preferably external pressure filtration in which filtration is performed from the outer periphery side to the inner periphery side of the hollow fiber membrane, and the backwashing in step a-2 is preferably performed by flowing a liquid from the inner periphery side to the outer periphery side of the hollow fiber membrane. In this case, the backwashing flux, calculated per inner area of the hollow fiber membrane, is preferably 4.0 m 3 / m 2 / d or more 10.0m 3 / m 2 / d or less, and 7.0m 3 / m 2 / d or more 10.0m 3 / m 2 In step a, if the liquid is made to flow from the outside to the inside of the hollow fiber membrane at a high flux rate, the hollow fiber membrane will be compressed and crushed, but by making the liquid flow from the inside to the outside of the hollow fiber membrane, cleaning at a high flux rate can be achieved, and a high cleaning effect can be obtained.
[0034] <Concentrated liquid recovery> If cross-flow filtration is continued in step a, the amount of liquid in the stock solution tank will eventually decrease, making it difficult to circulate the stock solution between the stock solution tank and the membrane module. Here, in order to recover the stock solution remaining in the stock solution tank, piping, and membrane module, dead-end filtration or diafiltration can be performed. In the case of dead-end filtration, for example, water is charged into the stock solution tank 1, the stock solution is supplied to the membrane module 2 by the stock solution pump 3, and dead-end filtration is performed, and the filtration is stopped before the water reaches the membrane module. Dead-end filtration can also be performed by supplying gas to the stock solution tank 1 or piping. In diafiltration, water is charged into the stock solution tank 1 to perform cross-flow filtration, and when the amount of liquid in the stock solution tank 1 decreases, water is charged again and cross-flow filtration is repeated, thereby improving the recovery rate of the stock solution.
[0035] (Step b) <Water rinse> In step b, the membrane module 2 is rinsed with water, with the purpose of reducing organic and other contaminant components before the chemical cleaning in step c. In chemical cleaning, cleaning is performed with a chemical solution with a pH of 10 or more and 14 or less that contains an oxidizing agent, but if a large amount of organic matter remains, the oxidizing agent will be consumed and the separation membrane may not be sufficiently cleaned, so the separation membrane is rinsed with water before chemical cleaning.
[0036] As a method of water rinsing, for example, water is charged into the cleaning liquid tank 10 and cross-flow filtration of the membrane module 2 is performed to clean the entire inside of the membrane module 2, that is, both the primary side and the secondary side. At this time, water is pumped from the backwash liquid tank 7 to perform backwashing with water at the same time, thereby improving the cleaning effect. The membrane surface linear velocity, filtration flux, and backwash flux may be performed under the same conditions as in step a.
[0037] (Step c) <Alkaline chemical cleaning> In step c, the membrane module 2 is washed with a chemical solution to remove fouling components adhering to the separation membrane. Chemical solutions for washing separation membranes include acids, alkalis, oxidizing agents, surfactants, and chelating agents. We found that washing the separation membrane after filtration of the fermentation liquid is effective when using a combination of an oxidizing agent at a pH of 10 or more and 14 or less, and injecting a chemical solution from the secondary side of the membrane to the primary side.
[0038] The pH of the chemical solution is preferably 10 to 14, more preferably 11 to 13. The pH is adjusted with sodium hydroxide, potassium hydroxide, or the like. The fouling substances in the fermentation broth are mainly organic matter, and high pH conditions enhance cleaning power, but conditions above pH 14 may cause deterioration of the membrane, membrane module components, piping, etc. On the other hand, a pH below 10 may result in insufficient cleaning effect.
[0039] Examples of the oxidizing agent include hypochlorites such as sodium hypochlorite, calcium hypochlorite, and potassium hypochlorite, hydrogen persulfates such as sodium hydrogen persulfate and potassium hydrogen persulfate, persulfates such as sodium persulfate and potassium persulfate, percarbonates such as sodium percarbonate and potassium percarbonate, permanganates, ozone, and peroxides such as hydrogen peroxide, and in order to obtain a sufficient cleaning effect, hypochlorites such as sodium hypochlorite, calcium hypochlorite, and potassium hypochlorite are preferred. These oxidizing agents can be used alone or in combination of two or more.
[0040] The oxidizing agent is dissolved in an alkaline aqueous solution having a pH of 10 or more and 14 or less and used as a cleaning solution. The oxidizing agent may be used in a high concentration from the beginning, or in the order of low concentration and high concentration. Specifically, there is a method of performing step (c-1) of injecting a chemical solution A having a pH of 10 or more and 14 or less containing 0.01% or more of an oxidizing agent from the secondary side to the primary side of the membrane alone, or a method of performing step (c-2) of injecting a chemical solution B having a pH of 10 or more and 14 or less containing less than 0.01% of an oxidizing agent from the secondary side to the primary side of the membrane sequentially before c-1. In the present invention, when a chemical solution having a pH of 10 or more and 14 or less containing an oxidizing agent is injected from the secondary side of the membrane of the membrane module to the primary side, a synergistic effect is achieved to obtain a high cleaning effect in a short time. Furthermore, since the initial alkaline chemical solution injected from the secondary side to the primary side of the membrane of the membrane module in each of steps c-1 and c-2 contains a large amount of dirt components, it is possible to prevent reattachment to the membrane and obtain a higher cleaning effect by discarding it without reusing it. The discard time is preferably about 5 to 10 minutes.
[0041] The concentration of the oxidizing agent used in the chemical cleaning is preferably 0.01% to 1%, more preferably 0.1% to 0.5%, when the chemical cleaning is performed in one step. On the other hand, when the chemical cleaning is performed in two or more steps, the concentration of the oxidizing agent in at least the first cleaning step is preferably less than 0.01%, and in at least one cleaning step from the second step onwards, the concentration of the oxidizing agent is preferably 0.01% to 1%, more preferably 0.1% to 0.5%. In step (c-1) where the oxidizing agent is used at a high concentration, a sufficient cleaning effect can be obtained by setting the oxidizing agent concentration to 0.01% or more. In addition, by setting the oxidizing agent concentration to 1% or less, a balance can be achieved between cost and cleaning effect. In addition, when chemical cleaning is performed in two or more steps, by performing cleaning with an oxidizing agent concentration of less than 0.01% in at least one step, the foulant components attached to the membrane can be removed without being denatured by the oxidizing agent, and then by performing further cleaning with an oxidizing agent concentration of 0.01% or more, the cleaning effect of the oxidizing agent can also be obtained. Whether chemical cleaning is performed in one step or two steps can be appropriately changed depending on the properties of the raw solution, the fouling components of the separation membrane, and the fouling state.
[0042] The temperature of the chemical solution is preferably 20° C. to 70° C., and more preferably 40° C. to 60° C. If the temperature of the chemical solution is less than 20° C., it may not be possible to achieve a sufficient cleaning effect. On the other hand, if the temperature exceeds 70° C., it is not preferable because the decomposition of the oxidizing agent is accelerated.
[0043] The injection flux of the chemical solution from the secondary side to the primary side may be set appropriately depending on the properties of the raw liquid and the fouling state of the separation membrane, but is preferably 1.5 times or more and 10 times or less, and more preferably 2.0 times or more and 4.0 times or less, of the filtration flux during cross-flow filtration in step a. If the injection flux of the chemical solution from the secondary side to the primary side is less than 1.5 times, the cleaning effect will be reduced, which is not preferable. Also, if the injection flux of the chemical solution from the secondary side to the primary side is more than 10 times, the power cost will be high and a large amount of chemical solution will be required, which is not preferable.
[0044] If the separation membrane is a hollow fiber membrane, it is preferable that the filtration in step a is an external pressure filtration in which filtration is performed from the outer periphery side of the hollow fiber membrane to the inner periphery side, and that the water rinsing in step b and the chemical washing in step c are performed by flowing water or a chemical solution from the inner periphery side of the hollow fiber membrane to the outer periphery side. In this case, the backwash flux, calculated per inner area of the hollow fiber membrane, is 4.0 m 3 / m 2 / d or more 10.0m 3 / m 2 / d or less, and 7.0m 3 / m 2 / d or more 10.0m 3 / m 2 In steps b and c, if the liquid is made to flow from the outside to the inside of the hollow fiber membrane at a high flux, the hollow fiber membrane will be compressed and crushed, but by making the liquid flow from the inside to the outside of the hollow fiber membrane, cleaning at a high flux can be achieved, and a high cleaning effect can be obtained.
[0045] (Step d) <Water rinse> In step d, the membrane module 2 is rinsed with water, the purpose of which is to wash away the chemical solution remaining after the chemical solution cleaning in step c. The water rinsing method may be the same as that in step b.
[0046] (Step e) <Acid chemical cleaning> In step e, an acidic chemical solution c is injected from the secondary side to the primary side of the membrane of the membrane module 2 to remove fouling components remaining in the separation membrane that could not be washed in step c. The pH of the chemical solution c is preferably 0 or more and 4.0 or less, and more preferably 1.0 or more and 3.0 or less. The pH is adjusted with at least one compound selected from the group consisting of hydrochloric acid, nitric acid, sulfuric acid, phosphoric acid, formic acid, acetic acid, propionic acid, butyric acid, citric acid, oxalic acid, ascorbic acid, and lactic acid. The lower the pH, the higher the cleaning power, but under conditions where the pH is less than 0, the membrane, membrane module components, piping, etc. may deteriorate. On the other hand, under conditions where the pH is more than 4, the acidity is insufficient and the cleaning effect is insufficient.
[0047] The temperature of the chemical solution is preferably 20° C. or higher and 70° C. or lower, and more preferably 40° C. or higher and 60° C. or lower. If the temperature of the chemical solution is lower than 20° C., the cleaning effect may not be sufficient. On the other hand, if the temperature exceeds 70° C., the membrane, the membrane module components, the piping, etc. may deteriorate, which is not preferable.
[0048] The injection flux of the chemical solution from the secondary side to the primary side may be appropriately set according to the properties of the raw liquid and the fouling state of the separation membrane, but is preferably 1.5 times or more and 10 times or less, and more preferably 2.0 times or more and 4.0 times or less, of the filtration flux during cross-flow filtration in step a. If the injection flux of the chemical solution from the secondary side to the primary side is less than 1.5 times, the cleaning effect is reduced, which is not preferable. Furthermore, if the injection flux of the chemical solution from the secondary side to the primary side exceeds 10 times, the power cost increases and a large amount of chemical solution is required, which is not preferable. Furthermore, since the initial acid chemical solution injected from the secondary side to the primary side of the membrane of the membrane module contains a large amount of fouling components, it is discarded without being reused, so that re-adhesion to the membrane can be prevented and a higher cleaning effect can be obtained. The discarding time is preferably about 5 to 10 minutes.
[0049] If the separation membrane is a hollow fiber membrane, it is preferable that the filtration in step a is an external pressure filtration in which filtration is performed from the outer periphery side of the hollow fiber membrane to the inner periphery side, and that the water rinsing in step b and the chemical washing in step c are performed by flowing water or a chemical solution from the inner periphery side of the hollow fiber membrane to the outer periphery side. In this case, the backwash flux, calculated per inner area of the hollow fiber membrane, is 4.0 m 3 / m 2 / d or more 10.0m 3 / m 2 / d or less, and 7.0 m3 / m2 / d to 10.0 m 3 / m 2 In steps b and c, if the liquid is made to flow from the outside to the inside of the hollow fiber membrane at a high flux, the hollow fiber membrane will be compressed and crushed, but by making the liquid flow from the inside to the outside of the hollow fiber membrane, cleaning at a high flux can be achieved, and a high cleaning effect can be obtained.
[0050] (Step f) <Water rinse> In step f, the membrane module 2 is rinsed with water, the purpose of which is to wash away the chemical solution remaining after the chemical solution cleaning in step e. The water rinsing method may be the same as that in step b.
[0051] <Cleaning aid> It is preferable that the above-mentioned chemical solutions A and B contain, in addition to an alkali and an oxidizing agent, a surfactant, an enzyme, a chelating agent, or a polyphosphate as a cleaning auxiliary, and the above-mentioned chemical solution C contains, in addition to an acid, a surfactant such as a nonionic surfactant, an anionic surfactant, or a cationic surfactant, with nonionic surfactants being particularly preferable, EDTA being the chelating agent, and protease, mannanase, or β-glucanase being particularly preferable as the enzyme.
[0052] Examples of nonionic surfactants include polyoxyethylene alkyl ethers, polyoxyethylene alkylphenyl ethers, polysorbates (polyoxyethylene sorbitan fatty acid esters), polyoxyethylene polystyrylphenyl ethers, polyoxyethylene-polyoxypropylene glycols, polyoxyethylene-polyoxypropylene alkyl ethers, polyhydric alcohol fatty acid partial esters, polyoxyethylene polyhydric alcohol fatty acid partial esters, polyoxyethylene fatty acid esters, polyglycerin fatty acid esters, polyoxyethylated castor oil, and the like. The nonionic surfactants can be used alone or in combination of two or more. It is considered that the hydrophobic portion of the molecule of fouling substances such as proteins, polysaccharides, and lipids adheres to the separation membrane. Therefore, the interaction between the hydrophobic portion (lipophilic portion) of the surfactant and the hydrophobic portion of the fouling substance, and the solubility of the surfactant in water affect the cleaning properties. The HLB value, which indicates the hydrophilic-lipophilic balance of the nonionic surfactant, is preferably 12 to 18, more preferably 13 to 17. When the HLB is within this range, the surfactant has an excellent balance between hydrophilicity and lipophilicity, resulting in enhanced cleaning effect.
[0053] The concentration of the cleaning aid used in the chemical cleaning is preferably 0.05% to 3%, more preferably 0.1% to 1%. The critical micelle concentration of the surfactant varies depending on the type, but it is preferable to use a concentration equal to or higher than the critical micelle concentration in order to achieve a sufficient cleaning effect.
[0054] <Membrane module> The type of membrane module used in the present invention is not particularly limited, but a hollow fiber membrane module is preferred because it generally has a large specific surface area, can filter a large amount of liquid per unit time, and can be backwashed.
[0055] <Separation membrane> The structure of the separation membrane is not particularly limited, but examples include a symmetric membrane with a uniform pore size overall, an asymmetric membrane with a pore size that varies in the thickness direction of the membrane, and a composite membrane having a support layer for maintaining strength and a separation functional layer for separating the target substance.
[0056] The separation membrane preferably satisfies one or more of the following (A) to (D), and more preferably satisfies all of them. (A) The separation membrane contains a hydrophobic polymer, and the pore volume V2 of the pores having a diameter of less than 100 nm is 0.02 cm 3 / g or more 0.1cm 3 / g and the pore volume V1 of the pores with a pore diameter of 100 nm or more is 0.1 cm 3 / g or more, and the ratio V1 / V2 of the pore volume V2 to the pore volume V1 is 3 or more and 60 or less. (B) The breaking elongation of the separation membrane is 38% or more. (C) The shrinkage rate of the hollow fiber membrane length when the separation membrane is heat-treated in a water vapor atmosphere at 125°C for 20 hours is 0.5% or more. (D) The separation membrane contains a hydrophilic polymer, the hydrophilic polymer contains a copolymer composed of N types of monomer units 1, 2,...i...N, and the hydration energy density of the hydrophilic polymer calculated based on the following formula (1) is 40 to 70 cal mol -1 ·Å -3 To be.
[0057]
number
[0058] [In formula (1), the hydration energy of any monomer unit i is the absolute value of the energy of the monomer unit i in water minus the energy of the monomer unit i in a vacuum, N is the total number of monomer species constituting the copolymer, i is an integer of 1 to N, and N is an integer of 2 or more.] Details are explained below.
[0059] (1) Hydrophobic polymers In the present invention, the hydrophobic polymer is not limited as long as it dissolves in the hydrophobic organic solvent used in the film formation. Examples of hydrophobic polymers include polyesters such as polytetrafluoroethylene, polyvinylidene fluoride, polylactic acid, polyhydroxyacetic acid, polycaprolactone, and polyethylene adipate, polyurethanes, poly(meth)acrylic acid esters, polyvinyl acetals, polyamides, polystyrenes, polysulfones, cellulose derivatives, polyphenylene ethers, and polycarbonates, and other single components, polymer alloys and blends of two or more selected from these, or copolymers of monomers forming the above polymers, but are not limited to the above examples. Among these, resin components with excellent heat resistance, chemical resistance, etc. include fluorine-based resins such as polytetrafluoroethylene and polyvinylidene fluoride, or sulfone-based resins such as polysulfone and polyethersulfone. Among these, vinylidene fluoride resins are particularly preferred because they have high compatibility with solvents and can easily produce a uniform manufacturing stock solution. The vinylidene fluoride resin means a resin containing at least one of a vinylidene fluoride homopolymer and a vinylidene fluoride copolymer. The vinylidene fluoride resin may contain a plurality of kinds of vinylidene fluoride copolymers.
[0060] The vinylidene fluoride copolymer is a polymer having a vinylidene fluoride residue structure, and is typically a copolymer of vinylidene fluoride monomer and other fluorine-based monomers, etc. Examples of such copolymers include copolymers of vinylidene fluoride and one or more monomers selected from vinyl fluoride, tetrafluoroethylene, hexafluoropropylene, and trifluorochloroethylene.
[0061] The weight-average molecular weight of the vinylidene fluoride resin may be appropriately selected depending on the required strength and water permeability of the separation membrane, but as the weight-average molecular weight increases, the water permeability decreases, and as the weight-average molecular weight decreases, the strength decreases. For this reason, the weight-average molecular weight is preferably 50,000 to 1,000,000. In the case of water treatment applications in which the separation membrane is exposed to chemical washing, the weight-average molecular weight is preferably 100,000 to 700,000, and more preferably 150,000 to 600,000.
[0062] The separation membrane preferably contains vinylidene fluoride resin as a main component, and the proportion of vinylidene fluoride resin in the hollow fiber membrane is preferably 80% by weight or more, more preferably 90% by weight or more, and even more preferably 95% by weight or more.
[0063] (2) Average pore diameter The separation membrane of the present invention preferably has pores with an average pore size in the range of 10 to 10,000 nm. The average pore size of the pores is more preferably in the range of 50 to 5,000 nm, and even more preferably in the range of 100 to 3,000 nm. When the average pore size is 100 nm or more, the permeation resistance is unlikely to increase, and the pressure required for filtration can be prevented from increasing. For example, when a liquid containing microbial particles is filtered, the destruction of microbial particles, clogging of the membrane surface due to deformation, and a decrease in filtration efficiency can be prevented. Furthermore, when the average pore size is 3,000 nm or less, sufficient fractionation can be obtained.
[0064] The pore size can be measured by mercury intrusion porosimetry, in which pressure p is applied to mercury so that it is forced into the pores of the separation membrane, and the volume change dV of the mercury in the cell is measured relative to the pressure increment dp, and the pore distribution function F(r) is calculated from the following equation (A).
[0065]
number
[0066] (Here, r is the pore radius, σ is the surface tension of mercury (0.480 N / m), and θ is the contact angle (140°).) The average pore size can be calculated by the following formula (B).
[0067]
number
[0068] (3) Pore volume Pores with a diameter of less than 100 nm are mainly voids within the solid parts that make up the separation membrane, and also include minute voids between the solid parts.Pores with a diameter of 100 nm or more are large voids between the solid parts that make up the separation membrane. The fact that the voids within the solid portion are small means that the polymer molecules that make up the solid portion are more densely arranged, and a separation membrane formed from such a solid portion has high breaking strength and breaking elongation. In addition, pores with a diameter of less than 100 nm can become the starting point for the adhesion of contaminants such as proteins in the fermentation liquid, resulting in clogging. Therefore, the small voids in the solid part provide high filtering properties for the fermentation liquid. In addition, the adhesion of flavor components is reduced, meaning that there is less odor when switching between types of fermentation liquid to be filtered.
[0069] On the other hand, if the pore volume of pores with diameters of less than 100 nm is extremely small, the flow paths in the separation membrane will be poorly branched. If the fine voids between solids are partially blocked and disappear, the pore volume of pores with diameters of less than 100 nm will often become too small.
[0070] In the filtration of liquids that are prone to clogging, such as fermentation liquid, separation membranes have a characteristic in that the membrane area of the permeable flow path, i.e., the effective membrane area, is significantly reduced due to localized clogging, and the effective membrane area decreases at an accelerated rate as filtration progresses. Therefore, high filtration performance is imparted by leaving a certain amount of fine voids.
[0071] Furthermore, when the volume of the voids between the solid parts, i.e., the volume of pores with a pore size of 100 nm or more, is large, the voids between the solid parts forming the separation membrane are large, and the membrane exhibits high pure water permeability. In addition, since there is little inclusion of chemicals on the surface that comes into contact with chemicals during cleaning, the effect of chemical surface modification on the inside of the membrane structure is minimal, and the membrane has excellent chemical resistance.
[0072] On the other hand, good mechanical strength can be obtained by keeping the pore volume of pores with diameters of 100 nm or more below a certain value. 3 / g or more 1.0cm 3 It is preferable that the molecular weight is less than 1 / g.
[0073] That is, in the separation membrane, the pore volume V1 of the pores with a diameter of less than 100 nm is 0.02 cm 3 / g or more 0.1cm 3 / g and the pore volume V2 of the pores with a pore diameter of 100 nm or more is 0.1 cm 3 / g or more, and the ratio V1 / V2 of the pore volume V2 to the pore volume V1 is 3 or more and 60 or less, the separation membrane has excellent mechanical strength and durability against chemical cleaning, and is less likely to clog during filtration of the fermentation broth and less likely to adhere to flavor components during filtration.
[0074] The pore volume V1 of pores with a diameter of 100 nm or more is 0.3 cm 3 / g or more, and 0.35 cm 3 / g or more. The pore volume V1 of pores with diameters of 100 nm or more is preferably 0.5 cm 3 / g or less, and 0.45 cm 3 It is more preferable that the molecular weight is not more than 1 / g.
[0075] The pore volume V2 of pores with a diameter of less than 100 nm is 0.020 cm 3 / g or more, and 3 / g or more is more preferable, and 0.030 cm 3 / g or more. The pore volume V2 of pores with a pore diameter of less than 100 nm is preferably 0.1 cm 3 / g or less, and 3 / g or less is more preferable, and 0.050 cm 3 It is more preferable that the molecular weight is not more than 1 / g.
[0076] The ratio V1 / V2 of the pore volume V2 to the pore volume V1 is preferably at least 3. In addition, V1 / V2 is preferably at most 60, more preferably at most 20, and even more preferably at most 15.
[0077] The pore volume of pores with a pore size of 100 nm or more may be measured by the above-mentioned mercury intrusion method, and that of pores with a pore size of less than 100 nm may be measured by a gas adsorption method. In the gas adsorption method, for example, after removing water and the like adsorbed to the separation membrane, nitrogen gas adsorption measurement is performed at liquid nitrogen temperature, and the pore volume V (cm) of the separation membrane is calculated from the amount of nitrogen gas adsorption (liquid equivalent) at a relative pressure (adsorption equilibrium pressure / saturated vapor pressure at liquid nitrogen temperature) of 0.99. 3 / g) can be measured.
[0078] Within the above range, a separation membrane in which the pore volume of pores with pore sizes smaller than the average pore size accounts for 60% or more of the total pore volume, as measured by mercury intrusion porosimetry, has many branched flow paths and distributes the load caused by localized clogging to other flow paths, making it suitable for filtering liquids that are prone to clogging, such as fermentation liquids.
[0079] (4) Spherical structure In the separation membrane according to the embodiment of the present invention, the solid portion preferably has a spherical structure. The spherical structure is a structure in which spheres are connected. When the inside of the separation membrane has such a structure, the voids between the solid portions (spheres) are less likely to shrink, and high pure water permeability can be maintained. In addition, the spherical structure can achieve higher strength and higher water permeability than conventional mesh-like structures. Moreover, the spherical structure preferably contains vinylidene fluoride resin, and the separation membrane preferably has a spherical structure and is a hollow fiber membrane. A part of a hollow fiber membrane is illustrated in Fig. 4. When the separation membrane is a hollow fiber membrane 30 shown in Fig. 4, the inside of the separation membrane refers to the part excluding the outer surface 31, that is, the substantial inside and / or inner surface 32 of the hollow fiber membrane.
[0080] A portion of the spherical structure is shown diagrammatically in Fig. 5. In the spherical structure 40 of Fig. 5, a plurality of spherical bodies 41 are connected. The spherical bodies 41 are approximately spherical or approximately ellipsoidal. As shown in Fig. 5, the spherical body 241 is connected to other spherical bodies 41, so that the entire spherical or ellipsoidal surface cannot be observed. However, the diameter, major axis, and minor axis can be estimated from the shape shown in the external shape.
[0081] The connections between the spheres may be formed by direct bonding between the spheres, or may be formed by non-spherical portions (also called constrictions) 42 between the spheres. The gaps 43 between the spheres are the gaps between the solid parts described above. As described above for the solid parts, minute gaps also exist within the spheres.
[0082] The average diameter of the spheres is in the range of 0.5 to 15 μm, preferably in the range of 0.6 to 10 μm, and more preferably in the range of 0.8 to 8 μm. The diameter of the spheres is determined by taking a photograph of the cross section and / or inner surface of the hollow fiber membrane using a scanning electron microscope or the like at a magnification at which the spherical structure can be clearly observed, measuring the diameters of 10 or more, preferably 20 or more, arbitrary spheres, and averaging them. It is also preferable to analyze the photograph with an image processing device and determine the average of the equivalent circle diameter. The density of the spheres is 10 3 ~108 pieces / mm 2 The range is preferably 10 4 ~10 6 pieces / mm 2 The density of the sphere is in the range of 10 3 pieces / mm 2 This provides the high strength required for fermentation liquid processing, and 8 pieces / mm 2 High pure water permeability can be obtained by satisfying the following:
[0083] The density of the spheres is measured by taking a photograph in the same manner as in the measurement of the diameter, and counting the number of spheres per unit area. The circularity ratio (minor diameter / major diameter) is preferably 0.5 or more, more preferably 0.6 or more, and even more preferably 0.7 or more.
[0084] (5) Hydrophilic polymer The hollow fiber membrane contains a copolymer composed of N types of monomer units, and the hydration energy density of the hydrophilic polymer calculated based on the above formula (1) is 40 to 70 cal mol -1 ·Å -3 It is preferable that the hydrophilic polymer contains a hydrophilic polymer represented by the formula:
[0085] In addition, the volume fraction of the monomer unit with the highest hydration energy density is 35-90%, and the difference in hydration energy density is 10-100 cal mol -1 ·Å -3 It is.
[0086] The term "monomer unit" refers to a repeating unit in a homopolymer or copolymer obtained by polymerizing a monomer. For example, a hydrophobic monomer unit refers to a repeating unit in a homopolymer or copolymer obtained by polymerizing a hydrophobic monomer.
[0087] "Containing N types of monomer units" means that the copolymer contains N types of repeating units (i.e., monomer units). N is an integer of 2 or more, and a monomer unit i refers to any one of the N types of monomer units. For example, a vinylpyrrolidone / vinyl decanoate random copolymer contains two types of monomer units, vinylpyrrolidone and vinyl decanoate.
[0088] By "copolymer" is meant a polymer composed of two or more types of monomer units.
[0089] "Hydration energy" refers to the energy change that a system undergoes when a solute is placed in an aqueous solution.
[0090] "Hydration energy of a monomer unit" means the absolute value of the energy of a monomer unit in water minus the energy of the monomer unit in a vacuum.
[0091] "Hydration energy density" means the hydration energy per unit volume. For example, in the case of a monomer, it is a numerical value defined by the following formula (2).
[0092] Hydration energy density (cal mol -1 ·Å -3 ) = (hydration energy of monomer unit i) / (volume of monomer unit i) Equation (2) The "difference in hydration energy density" refers to the numerical value defined by the following formula (3).
[0093] Hydration energy density difference (cal mol -1 ·Å -3 ) = (hydration energy density of the monomer unit with the largest hydration energy density) - (hydration energy density of the monomer unit with the smallest hydration energy density) Equation (3) "Monomer unit j having the highest hydration energy density" means a monomer unit having the highest hydration energy density defined by the formula (2) among monomer units constituting a hydrophilic polymer.
[0094] "Monomer unit k having the smallest hydration energy density" means a monomer unit having the smallest hydration energy density defined by the formula (2) among monomer units constituting a hydrophilic polymer.
[0095] Regarding the molecular model of the monomer unit, for example, when the monomer unit has a structure represented by the chemical formula (I) below, the structure represented by the chemical formula (II) below is used as the calculation target. That is, a structure is used in which the carbon terminal on the side to which the side chain R is bonded is terminated with a methyl group ((a) in the following formula (II)), and the carbon terminal on the side to which the side chain R is not bonded is terminated with a hydrogen atom ((b) in the following formula (II)).
[0096] [ka]
[0097] [ka]
[0098] The energy of the monomer unit in the above formula (1) in a vacuum and in water can be calculated by the following method.
[0099] First, the molecular model of the monomer unit is structurally optimized. Density functional theory is used for structural optimization. B3LYP is used as the functional, and 6-31G(d,p) is used as the basis function. In addition, opt is set as a keyword to be written in the input file.
[0100] Next, the energy in vacuum and the energy in water are calculated for the optimized structure. The energy in vacuum is calculated using density functional theory. B3LYP is used as the functional and 6-31G(d,p) is used as the basis function. The energy in water is calculated using density functional theory. B3LYP is used as the functional and 6-31G(d,p) is used as the basis function. Furthermore, to calculate the energy in water, a continuous dielectric model is used, and the following keywords are used: SCRF=(PCM, G03Defaults, Read, Solvent=Water) Radii=UAHF Alpha=1.20 The hydration energy of the monomer unit is determined by calculating the SCF energy in vacuum and in water, where the SCF energy is the value of E written on the line labeled "SCF Done:".
[0101] The energy calculation is carried out using quantum chemical calculation software Gaussian09 (registered trademark) manufactured by Gaussian Corporation.
[0102] In the hydrophilic polymer, the hydration energy density of the hydrophilic polymer is defined based on the above formula (1).
[0103] The volume of the monomer unit in the formula (1) is the volume of the structure optimized. The volume of the monomer unit can be calculated, for example, by using the Connolly surface method of MaterialsStudio (registered trademark) manufactured by BIOVIA. In this case, the parameters to be set are as follows. Gridresolution=Coarse Grid interval=0.75Å vdWfactor=1.0 Connolly radius=1.0Å The hydration energy density of the hydrophilic polymer is 40 to 70 cal·mol -1 ·Å -3 and preferably 43 to 60 cal·mol-1 ·Å -3 and more preferably, 45 to 55 cal·mol -1 ·Å -3 Any preferred lower limit may be combined with any preferred upper limit.
[0104] The total number N of monomer species constituting the hydrophilic polymer is not particularly limited as an upper limit, but is preferably 2 to 5, more preferably 2 to 3, and most preferably 2.
[0105] The hydration energy density of the entire hydrophilic polymer is 40 cal mol -1 ·Å -3 More than 70 cal·mol -1 ·Å -3 It is considered that the structures of the hydrophilic polymer, the adsorbed water of the hydrophilic polymer, and the impurities in the fermentation liquid, and the adsorbed water of the impurities in the fermentation liquid are stabilized by satisfying the following conditions: As a result, electrostatic interaction or hydrophobic interaction between the hydrophilic polymer present on the surface of the hollow fiber membrane and the impurities in the fermentation liquid is reduced, and adhesion of the impurities in the fermentation liquid to the hollow fiber membrane is suppressed.
[0106] The molar fractions of the monomer units of the above formula (1) and the following formula (4) are the ratios of the number of each type of monomer unit to the total number of monomer units constituting the hydrophilic polymer. As described below, they are measured with a nuclear magnetic resonance (NMR) device and calculated from the peak area. When the molar fractions cannot be calculated by NMR measurement due to overlapping peaks, etc., the molar fractions may be calculated by elemental analysis.
[0107]
number
[0108] [In the formula (4), N and i are defined as above.] As described below, the hollow fiber membrane is formed by phase separation of a hydrophobic polymer and the subsequent introduction of a hydrophilic polymer, and has an aggregate of spherical structures composed of hydrophobic polymers and hydrophilic polymers attached to the surfaces of the spherical structures.
[0109] The number average molecular weight of the hydrophilic polymer is preferably 2,000 or more, more preferably 3,000 or more, in order to suppress adhesion of impurities in the fermentation liquid, and is preferably 1,000,000 or less, more preferably 200,000 or less, and even more preferably 100,000 or less, in order to achieve high incorporation efficiency into the membrane.
[0110] In the hydrophilic polymer, the volume fraction of the monomer unit having the highest hydration energy density calculated based on the formula (2) (for convenience of explanation, referred to as monomer unit j) is 35% to 90%, preferably 40% to 80%, more preferably 40% to 75%, and even more preferably 40% to 70%. Any of the preferable lower limits can be combined with any of the preferable upper limits.
[0111] When the volume fraction is within the above range, it is believed that due to the effects of both the hydrophilic monomer units and the hydrophobic monomer units, the interaction between the hydrophilic polymer present on the surface of the hollow fiber membrane and the adsorbed water of the hydrophilic polymer, on the impurities in the fermentation liquor and the adsorbed water of the impurities in the fermentation liquor, is of an appropriate magnitude, and as a result, adhesion of impurities in the fermentation liquor is suppressed.
[0112] In addition, in the hydrophilic polymer, the difference in hydration energy density is calculated by the following formula (5). (difference in hydration energy density) cal mol -1 ·Å -3 = (Hydration energy density of monomer unit j with the highest hydration energy density) - (Hydration energy density of monomer unit k with the lowest hydration energy density) Equation (5) The difference in hydration energy density is 10 to 100 cal mol -1 ·Å -3 and 10 to 80 cal mol -1 ·Å -3 It is preferable that the range is 10 to 60 cal·mol -1 ·Å -3It is more preferable that:
[0113] When the difference in hydration energy density is within the above range, it is considered that the hydrophilic monomer units of the hydrophilic polymer present on the surface of the hollow fiber membrane play a role in retaining the adsorbed water, and the hydrophobic monomer units play a role in controlling the mobility of the adsorbed water. As a result, it is considered that the interaction between the hydrophilic polymer present on the surface of the material and the adsorbed water of the hydrophilic polymer on the impurities in the fermentation liquid and the adsorbed water of the impurities in the fermentation liquid is of an appropriate magnitude, and as a result, the adhesion of the impurities in the fermentation liquid is suppressed.
[0114] The two or more types of monomer units are preferably a hydrophobic monomer unit and a hydrophilic monomer unit.
[0115] The term "hydrophobic monomer unit" refers to a monomer unit having a smaller hydration energy density than a hydrophilic monomer unit, and is preferably a repeating unit in a homopolymer or copolymer obtained by polymerizing a monomer selected from the group consisting of vinyl carboxylate, methacrylic acid ester, acrylic acid ester, and styrene derivative. Among these, a repeating unit in a homopolymer obtained by polymerizing vinyl carboxylate or a copolymer obtained by copolymerizing vinyl carboxylate is more preferred, and a repeating unit in a homopolymer obtained by polymerizing vinyl carboxylate is even more preferred, because it is easy to balance with the hydrophilic monomer unit and easy to control the mobility of adsorbed water present on the material surface.
[0116] The term "hydrophilic monomer unit" refers to a monomer unit having a larger hydration energy density than a hydrophobic monomer unit, and for example, a repeating unit in a homopolymer or copolymer obtained by polymerizing a monomer selected from the group consisting of allylamine, vinylamine, N-vinylamide, N-vinyllactam, and N-acryloylmorpholine is preferably used. Among these, a repeating unit in a homopolymer obtained by polymerizing N-vinyllactam or a copolymer obtained by copolymerizing N-vinyllactam is preferred, since it does not have too strong an interaction with the adsorbed water present on the material surface and is easy to balance with the hydrophobic monomer unit, and a repeating unit in a homopolymer obtained by polymerizing N-vinyllactam is more preferred. Among these, a repeating unit in a homopolymer obtained by polymerizing vinylpyrrolidone or a copolymer obtained by copolymerizing vinylpyrrolidone is more preferred, and a homopolymer obtained by polymerizing vinylpyrrolidone is most preferred.
[0117] In addition, other monomers, for example, monomers containing a reactive group such as a glycidyl group, may be copolymerized to the extent that the action and function of the hydrophilic polymer is not impaired, i.e., within the range satisfying the above [8].
[0118] Examples of the arrangement of the hydrophilic monomer units and the hydrophobic monomer units in the hydrophilic polymer include graft copolymers, block copolymers, alternating copolymers, and random copolymers. Among these, block copolymers, alternating copolymers, and random copolymers are preferred in terms of their high adhesion suppression function against impurities in the fermentation liquid, and random copolymers or alternating copolymers are more preferred in terms of their moderate balance of hydrophilicity and hydrophobicity in one molecule. The reason why block copolymers, alternating copolymers, and random copolymers have a higher adhesion suppression function against impurities in the fermentation liquid than graft copolymers, such as graft copolymers consisting of hydrophilic monomer units in the main chain and hydrophobic monomer units in the side chain, is thought to be because in the graft copolymer, the monomer unit portion grafted to the main chain has many opportunities to come into contact with proteins, etc., and therefore the characteristics of the graft chain portion have a greater influence than the characteristics of the copolymer. In addition, the reason why alternating copolymers and random copolymers are more preferred than block copolymers in terms of the moderate balance of hydrophilicity and hydrophobicity is thought to be because the characteristics of each monomer unit are clearly separated in the block copolymer.
[0119] The hydrophilic polymer can be synthesized, for example, by a chain polymerization method typified by a radical polymerization method using an azo-based initiator, but the synthesis method is not limited to this.
[0120] The hydrophilic polymer is produced, for example, by the following production method, but is not limited to this method.
[0121] A predetermined amount of hydrophilic monomer and hydrophobic monomer are mixed with a polymerization solvent and a polymerization initiator, and the mixture is stirred under a nitrogen atmosphere at a predetermined temperature for a predetermined time to cause a polymerization reaction. The ratio of the amount of the hydrophilic monomer to the amount of the hydrophobic monomer can be determined according to the molar fraction of the hydrophilic monomer unit in the copolymer. The reaction liquid is cooled to room temperature to stop the polymerization reaction, and is then poured into a solvent such as hexane. The precipitate is collected and dried under reduced pressure to obtain a hydrophilic polymer.
[0122] The reaction temperature of the above polymerization reaction is preferably from 30 to 150°C, more preferably from 50 to 100°C, and further preferably from 70 to 80°C.
[0123] The pressure for the polymerization reaction is preferably normal pressure.
[0124] The reaction time of the polymerization reaction is appropriately selected depending on the conditions such as the reaction temperature, but is preferably 1 hour or more, more preferably 3 hours or more, and even more preferably 5 hours or more. If the reaction time is short, a large amount of unreacted monomer may easily remain in the copolymer. On the other hand, the reaction time is preferably 24 hours or less, more preferably 12 hours or less. If the reaction time is long, side reactions such as the formation of dimers may easily occur, and it may be difficult to control the molecular weight.
[0125] The polymerization solvent used in the polymerization reaction is not particularly limited as long as it is a solvent that is compatible with the monomer. For example, an ether solvent such as dioxane or tetrahydrofuran, an amide solvent such as N,N-dimethylformamide, a sulfoxide solvent such as dimethyl sulfoxide, an aromatic hydrocarbon solvent such as benzene or toluene, an alcohol solvent such as methanol, ethanol, isopropyl alcohol, amyl alcohol, or hexanol, or water may be used. From the viewpoint of toxicity, however, it is preferable to use an alcohol solvent or water.
[0126] As the polymerization initiator for the polymerization reaction, for example, a photopolymerization initiator or a thermal polymerization initiator is used. Although a polymerization initiator that generates any of radicals, cations, or anions may be used, a radical polymerization initiator is preferably used since it does not cause decomposition of the monomer. As the radical polymerization initiator, for example, an azo-based initiator such as azobisisobutyronitrile, azobisdimethylvaleronitrile, or azobis(isobutyric acid) dimethyl, or a peroxide initiator such as hydrogen peroxide, benzoyl peroxide, di-tert-butyl peroxide, or dicumyl peroxide is used.
[0127] After the polymerization reaction has been stopped, the solvent into which the polymerization reaction solution is poured is not particularly limited as long as it is a solvent in which the copolymer precipitates. For example, a hydrocarbon solvent such as pentane, hexane, heptane, octane, nonane, or decane, or an ether solvent such as dimethyl ether, ethyl methyl ether, diethyl ether, or diphenyl ether may be used.
[0128] (6)Other When the separation membrane of the present invention is in the form of a hollow fiber membrane, the outer diameter and membrane thickness of the hollow fiber may be determined so that the water permeation rate of the membrane module is a target value, taking into consideration the pressure loss in the longitudinal direction inside the hollow fiber membrane, within a range that does not impair the strength of the membrane. That is, a larger outer diameter is advantageous in terms of pressure loss, but the number of fibers packed is reduced, which is disadvantageous in terms of membrane area. On the other hand, a smaller outer diameter is advantageous in terms of membrane area, since the number of fibers packed can be increased, but is disadvantageous in terms of pressure loss. In addition, the membrane thickness is preferably thin within a range that does not impair the strength. Therefore, as a rough guide, the outer diameter of the hollow fiber membrane is preferably 0.3 to 3 mm, more preferably 0.4 to 2.5 mm, and even more preferably 0.5 to 2.0 mm. In addition, the membrane thickness is preferably 0.08 to 0.4 times the outer diameter, more preferably 0.1 to 0.35 times, and even more preferably 0.12 to 0.3 times.
[0129] The separation membrane of the present invention preferably has substantially no macrovoids. Here, the term "macrovoids" refers to voids having a major axis of 50 μm or more observed in the membrane substance portion in the cross section of the separation membrane. "Substantially no macrovoids" refers to voids having a major axis of 10 / mm in the cross section. 2 Less than 5 / mm 2 and most preferably none at all.
[0130] The separation membrane of the present invention has a water permeability of 0.1 to 10 m at 10 kPa and 25°C. 3 / m 2 h, preferably 0.2 to 5 m 3 / m 2 h, more preferably 0.4 to 2 m 3 / m 2When the separation membrane of the present invention is in the form of a hollow fiber membrane, the breaking strength of the hollow fiber is preferably in the range of 0.3 to 3 kg / fiber, preferably 0.4 to 2.5 kg / fiber, more preferably 0.5 to 2 kg / fiber, and the breaking elongation is preferably in the range of 20 to 1000%, preferably 40 to 800%, more preferably 60 to 500%. By being in these ranges, sufficient water permeability is exhibited under normal use conditions, and the hollow fiber membrane does not break.
[0131] <Membrane manufacturing method> Next, a method for obtaining a hollow fiber membrane from a polyvinylidene fluoride resin as a hydrophobic polymer among the separation membranes of the present invention will be described, but the present invention is not limited to these manufacturing methods. An example of the manufacturing method for the hollow fiber membrane described above will be described below. The manufacturing method described below includes the following steps: (a) forming hollow fibers by phase separation of a solution containing a hydrophobic polymer, and then post-treating the hollow fibers by immersion in a solvent; (b) introducing a hydrophilic polymer into the hollow fiber has.
[0132] (a) Forming hollow fibers and post-treating them by solvent immersion Methods for producing hollow fiber membranes from polyvinylidene fluoride resins include thermally induced phase separation, non-solvent induced phase separation, melt extraction, and stretching and opening methods. Of these, it is preferable to use the thermally induced phase separation or non-solvent induced phase separation method.
[0133] Thermally induced phase separation is a phase separation in which a resin solution dissolved at high temperature is solidified by cooling, while non-solvent induced phase separation is a phase separation in which a resin solution is solidified by contacting it with a non-solvent.
[0134] When a hollow fiber membrane is produced by utilizing a thermally induced phase separation method, the solvent for the polyvinylidene fluoride resin solution is preferably a poor solvent for the resin, and particularly preferably used are poor solvents in which the resin has a relatively high solubility, such as alkyl ketones such as cyclohexanone, isophorone, γ-butyrolactone, and dimethyl sulfoxide, and esters.
[0135] In addition, when a hollow fiber membrane is produced using a non-solvent induced phase separation method, the solvent of the polyvinylidene fluoride resin solution is preferably a good solvent for the resin, and examples of the good solvent include lower alkyl ketones such as N-methyl-2-pyrrolidone, dimethylacetamide, dimethylformamide, methyl ethyl ketone, acetone, and tetrahydrofuran, esters, amides, and mixtures thereof. On the other hand, the non-solvent is a non-solvent for the resin, and examples of the non-solvent include aliphatic hydrocarbons such as water, hexane, pentane, benzene, toluene, methanol, ethanol, carbon tetrachloride, o-dichlorobenzene, trichloroethylene, ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, butylene glycol, pentanediol, hexanediol, and low molecular weight polyethylene glycol, aromatic hydrocarbons, aliphatic polyhydric alcohols, aromatic polyhydric alcohols, chlorinated hydrocarbons, or other chlorinated organic liquids and mixtures thereof.
[0136] In the thermally induced phase separation method and the non-solvent induced phase separation method, a good solvent or a poor solvent in which the resin has high solubility is used, so that the resin and the solvent can be mixed at the molecular level, and when solidified, the solvent molecules are interposed between the resin molecules. Therefore, many inter-molecular gaps are formed. Therefore, in order to control the pore volume to a range that provides excellent filterability for the fermentation liquid, it is preferable to perform a post-treatment to reduce the inter-molecular gaps on the separation membrane obtained by the phase separation method.
[0137] As a post-treatment for reducing the voids between molecules, a solvent immersion treatment is preferred in which the solid part is immersed in a poor solvent with a relatively high solubility of vinylidene fluoride resin at a constant temperature for a short time to dissolve only the outer surface structure of the solid part and then replaced with a non-solvent of vinylidene fluoride resin. In the solvent immersion treatment, while the voids inside the solid part are blocked, it is considered that the voids between the solid parts are hardly affected, resulting in a pore structure suitable for filtering liquids such as fermentation broth that are prone to clogging.
[0138] On the other hand, when the separation membrane obtained by the thermally induced phase separation method or the non-solvent induced phase separation method is heat-treated at a high temperature near the melting point Tm of the separation membrane, after the polymer's micro-Brownian motion is activated in the amorphous part inside the solid part forming the separation membrane, a part crystallizes, or the crystal part that melts at a temperature lower than the melting point of the separation membrane inside the solid part recrystallizes into a crystal part that melts at a higher temperature after once melting, causing the solid part to shrink. Since there are minute voids in such crystal parts and amorphous parts, it is expected that the voids will be filled by the shrinkage, thereby reducing the adhesion starting points of dirt components such as proteins in the fermentation broth.
[0139] However, it is considered that the shrinkage of the entire membrane during heat treatment blocks the minute voids between the solid parts, resulting in an effect of reducing the branching of the flow path, so it is not suitable for filtering liquids such as fermentation broth that are prone to clogging. As a method for quantifying the minute voids between the solid parts, it is possible to measure the shrinkage rate of the hollow fiber membrane when heat-treated at a temperature T that satisfies Tm - 60°C ≤ T < Tm - 40°C, where Tm is the melting point of the separation membrane.
[0140] The melting point Tm of the separation membrane is the peak top temperature when a dry separation membrane is heated at a rate of 10°C / min using a differential scanning calorimetry (DSC) device, and is around 175°C in the case of a hollow fiber membrane made of polyvinylidene fluoride. In the case of a hollow fiber membrane made of vinylidene fluoride resin, if the shrinkage rate of the hollow fiber membrane length when heat-treated for 20 hours in a water vapor atmosphere at 125°C is 0.5% or more, it has sufficient microvoids between solid parts. A more preferable shrinkage rate is 1.0% or more, and even more preferable is 2.0% or more. On the other hand, excessive heat shrinkage induces thread breakage and deformation inside the module, so it is preferably 25% or less.
[0141] There are two main types of phase separation mechanisms in thermally induced phase separation: one is liquid-liquid phase separation, in which a resin solution that is uniformly dissolved at high temperatures separates into a resin-rich phase and a resin-dilute phase as the temperature decreases due to a decrease in the dissolving ability of the solution, and the other is solid-liquid phase separation, in which a resin solution that is uniformly dissolved at high temperatures separates into a polymer solid phase and a polymer-dilute solution phase as the temperature decreases due to crystallization of the resin. In the former method, a three-dimensional network structure is mainly formed, and in the latter method, a spherical structure is formed. In the present invention, for the reasons described above, it is more preferable to form a spherical structure by the latter phase separation mechanism. According to this phase separation mechanism, a spherical structure having spherulites (spherical bodies) containing a lamellar structure and polymer chains connecting one lamellar structure to another lamellar structure is formed. In the case of a spherical structure, since the solid part is bulky, the voids between the solid parts are less likely to shrink, and it is also preferable that high pure water permeability can be maintained. For this reason, it is preferable to select a resin concentration and a solvent that induce solid-liquid phase separation. In addition, it is preferable to use a cooling bath when cooling, and it is preferable to contain the same solvent as the resin solution or a low concentration of a non-solvent for the resin to speed up solidification, etc.
[0142] For the above reasons, the method for producing the separation membrane of the embodiment of the present invention preferably employs a solid-liquid phase separation method that uses thermally induced phase separation to form a spherical structure, and the obtained separation membrane is preferably subjected to a solvent immersion treatment.
[0143] When the separation membrane of the present invention is in the form of a hollow fiber membrane, the hollow fiber membrane produced by the non-solvent induced phase separation method or the heat induced phase separation method is preferably stretched to expand the pores and improve the pure water permeability. The stretching conditions are preferably a temperature range of 50 to 120°C, more preferably 60 to 100°C, and a stretching ratio of preferably 1.1 to 4 times.
[0144] At temperatures below 50°C, it is difficult to achieve stable and uniform stretching, and at temperatures above 120°C, the hollow fiber membrane may soften and the hollow portion may collapse. Stretching is preferably performed in a liquid because temperature control is easy, but it may also be performed in a gas such as steam. Water is the preferred liquid because it is simple, but when stretching at temperatures above about 90°C, it is also preferred to use low molecular weight polyethylene glycol or the like.
[0145] Heat treatment of separation membranes is generally known, but in the conventional technology, it is used for dimensional stability below the heat treatment temperature, and therefore the heat treatment temperature is lower than that of the present invention, and does not impart excellent filtration performance for fermentation liquid to the separation membrane.
[0146] (b) Hydrophilic polymer introduction process The types of hydrophilic polymers are as explained in the section on hollow fiber membranes. Methods for introducing hydrophilic polymers include a method in which an aqueous solution in which a hydrophilic polymer is dissolved is passed through or immersed in the hollow fiber membrane, followed by irradiation or heat treatment to insolubilize the hydrophilic polymer, or a method in which a covalent bond is formed by a chemical reaction with a reactive group present in the hollow fiber membrane.
[0147] If the concentration of the hydrophilic polymer aqueous solution is too low, a sufficient amount of the hydrophilic polymer will not be introduced to the surface. Therefore, the copolymer concentration in the aqueous solution is preferably 10 ppm or more, more preferably 100 ppm or more, and most preferably 500 ppm or more. However, if the concentration of the hydrophilic polymer in the aqueous solution is too high, there is a concern that the amount of elution from the module will increase, so the copolymer concentration in the aqueous solution is preferably 100,000 ppm or less, and more preferably 10,000 ppm or less. The number average molecular weight of the hydrophilic polymer is measured by gel permeation chromatography (GPC) as described below.
[0148] In addition, when the hydrophilic polymer is poorly soluble or insoluble in water, the hydrophilic polymer may be dissolved in an organic solvent that does not dissolve the hollow fiber or a mixed solvent of water and an organic solvent that is compatible with water and does not dissolve the hollow fiber. Specific examples of the organic solvent that can be used for the organic solvent or the mixed solvent include alcohol solvents such as methanol, ethanol, and propanol, but are not limited to these.
[0149] Furthermore, if the ratio of the organic solvent in the mixed solvent is high, the hollow fibers may swell, which may result in changes in the pore size of the hollow fiber membrane, etc. Therefore, the weight fraction of the organic solvent in the mixed solvent is preferably 60% or less, more preferably 10% or less, and most preferably 1% or less.
[0150] The radiation irradiation may be α-rays, β-rays, γ-rays, X-rays, ultraviolet rays, or electron beams. From the viewpoints of safety and simplicity, radiation methods using γ-rays or electron beams are preferred. The radiation exposure dose is preferably 15 kGy or more, more preferably 25 kGy or more. By applying a dose of 15 kGy or more, the hydrophilic polymer can be effectively introduced. The radiation exposure dose is preferably 100 kGy or less. If the radiation exposure dose exceeds 100 kGy, the copolymer may be prone to three-dimensional crosslinking or decomposition of the ester group portion of the vinyl carboxylate monomer unit.
[0151] In order to suppress the crosslinking reaction during irradiation with radiation, an antioxidant may be used. The antioxidant refers to a substance that has the property of easily donating electrons to other molecules, and examples thereof include water-soluble vitamins such as vitamin C, polyphenols, and alcohol solvents such as methanol, ethanol, and propanol, but are not limited thereto. These antioxidants may be used alone or in combination of two or more kinds. When using an antioxidant, safety must be taken into consideration, so that antioxidants with low toxicity such as ethanol and propanol are preferably used.
[0152] In addition, a method for forming a covalent bond by a chemical reaction with a reactive group can be specifically achieved by reacting a reactive group such as an amino group, a sulfonic acid group, or a halogenated alkyl group on the surface of the substrate of the material with a reactive group introduced into the end of the main chain or into the side chain of the copolymer.
[0153] Examples of methods for introducing reactive groups onto the surface of a material include a method in which a monomer having a reactive group is polymerized to obtain a substrate having a reactive group on its surface, and a method in which the reactive group is introduced by ozone treatment or plasma treatment after polymerization.
[0154] Examples of a method for introducing a reactive group into the end of the main chain of the copolymer include a method using an initiator having a reactive group, such as 2,2'-azobis[2-methyl-N-(2-hydroxyethyl)propionamide] or 4,4'-azobis(4-cyanovaleric acid).
[0155] Examples of a method for introducing a reactive group into the side chain of the copolymer include a method of copolymerizing a monomer having a reactive group, such as glycidyl methacrylate, to an extent that does not impair the action and function of the copolymer.
[0156] The amount of the hydrophilic polymer introduced into the hollow fiber membrane can be quantified by attenuated total reflection infrared spectroscopy (ATR-IR) as described above. If necessary, it can also be quantified by X-ray photoelectron spectroscopy (XPS) or the like.
[0157] Furthermore, the hollow fiber membrane produced by the above-mentioned production method can be used as a hollow fiber membrane module. The module is a module in which a plurality of hollow fiber membranes are bundled together and placed in a cylindrical container, and both ends or one end are fixed with polyurethane, epoxy resin, etc. to enable collection of permeate water, or both ends of the hollow fiber membrane are fixed to a flat plate shape to enable collection of permeate water. By providing a pressurizing means such as a pump or a water level difference on the raw liquid side of this hollow fiber membrane module, or by providing a suction means such as a pump or a siphon on the permeate side, it can be used as a separation device for performing membrane filtration of the raw liquid, which is the fermentation liquid. By using this separation device, a purified permeate can be produced from the fermentation liquid.
[0158] <Use of hollow fiber membrane> The hollow fiber membrane described above is preferably used in the process of filtering the fermentation liquid of the present invention using the hollow fiber membrane. The fermentation liquid is not particularly limited by the type of microorganism or fermentation product, but examples thereof include beer, wine, sake, vinegar, soy sauce, amino acid fermentation liquid, organic acid fermentation liquid, and fermentation liquid of biopharmaceuticals. By filtering, unnecessary components for the product, such as microbial particles and turbidity in the fermentation liquid, can be removed. The hollow fiber membrane described above is suitable for these applications because it is less likely to clog during filtration and its performance recovery by chemical cleaning after clogging is maintained for a long period of time.
[0159] The present invention is not limited to the above-described embodiment, and can be freely modified as appropriate. In addition, the material, shape, size, value, form, number, location, etc. of each component in the above-described embodiment are arbitrary as long as they can achieve the present invention, and are not limited. EXAMPLES
[0160] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples in any way.
[0161] In the following examples, the separation membrane of the present invention will be described in the form of a hollow fiber membrane.
[0162] <Measuring pore size distribution of hollow fiber membranes using mercury intrusion method> The hollow fiber membranes were bone-dried by the following method. The hollow fiber membranes wet with water were freeze-dried at -20°C for about 50 hours, and then vacuum-dried at room temperature for about 8 hours. The hollow fiber membranes not wet with water were vacuum-dried at room temperature for about 8 hours. The bone-dried hollow fiber membranes were cut to a length of about 5 mm, and the sample weight was measured using an electronic balance (AW220, manufactured by Shimadzu Corporation). The pore size distribution was measured using a Poresizer 9320 manufactured by Micromeritics. The test pieces were cut into pieces of about 5 cm 3 The sample was sealed in a glass cell and mercury was injected under reduced pressure, then the pressure was increased to a range of approximately 4 kPa to 207 MPa (corresponding to pore diameters of approximately 7 nm to 350 μm) through oil in a pressure-resistant container attached to the device. The surface tension of mercury was calculated as 484 dyn / cm and the contact angle of mercury was calculated as 141.3°. The volume of pores with a pore diameter of 100 nm or more was defined as V1.
[0163] <Measurement of pore volume of hollow fiber membrane by gas adsorption method> The hollow fiber membrane dried under reduced pressure was cut to a length of approximately 10 cm, and the sample weight was weighed using an electronic balance (AW220, manufactured by Shimadzu Corporation). The amount of nitrogen gas adsorption was measured using an automatic specific surface area / pore size distribution measuring device (BELSORP-mini II, manufactured by Microtrack-Bell). The BET specific surface area was calculated using the attached analysis program. The pore volume of pores with a diameter of less than 100 nm was defined as V2.
[0164] <Preparation of membrane module> A plurality of hollow fiber membranes were cut to a length of about 30 cm and wrapped in a polyethylene film to form a hollow fiber membrane bundle. This hollow fiber membrane bundle was inserted into a cylindrical polycarbonate module case, and both ends were fixed with an epoxy potting agent. The ends were cut to obtain a module with both ends open. The number of hollow fiber membranes was 100 to 200 cm in Examples 1 to 7, 10, and 11 and Comparative Examples 1 to 3, with the membrane area based on the inner diameter of the hollow fiber membrane being 100 to 200 cm. 2 In Examples 8 and 9 and Comparative Examples 4 to 9, the average particle diameter is 1000 to 2000 cm 2The cylindrical module case was provided with ports at two locations near both ends to allow fluid to perfuse the outer surface of the hollow fiber membrane, and end caps having liquid inlets and outlets were attached to both ends to allow fluid to perfuse the hollow part of the hollow fiber membrane.
[0165] <Measurement of total sugar concentration> The total sugar in the sample solution was quantified by the phenol-sulfuric acid method. That is, the sample and 5% phenol solution were mixed in equal amounts, and then 1.5 times the amount of concentrated sulfuric acid was quickly added and stirred. The temperature was kept constant (20-30°C) for 20-30 minutes. Then, the absorbance of the mixed solution at a wavelength of 480 nm was measured using a UV-Visible Spectrophotometer (Shimadzu Corporation, UV2450). Meanwhile, a calibration curve was created using a glucose standard solution, and the total sugar concentration (glucose equivalent value) in the sample solution was calculated using the obtained calibration curve.
[0166] <Measurement of protein concentration> 150 μL of the sample solution was mixed with 1350 μL of Coomassie (Bradford) Protein Assay Reagent (Thermo Fisher Scientific), which is a Bradford reagent, and allowed to stand at room temperature for 10 minutes to react. After the reaction, the absorbance of the mixed solution at a wavelength of 470 nm was measured using an ultraviolet-visible spectrophotometer (Shimadzu Corporation, UV2450). Meanwhile, a bovine serum albumin standard sample was reacted with the Bradford reagent in the same manner as above to create a calibration curve, and the protein concentration in the sample solution was calculated using the obtained calibration curve.
[0167] <Measurement of polyphenol concentration> 500μL of the sample solution was mixed with 2500μL of 1% phenol reagent solution, stirred, and left to stand at room temperature for 5 minutes. Then, 2mL of 7.5% sodium carbonate solution was mixed, stirred, and left to stand at room temperature for 60 minutes. The absorbance of the mixed solution at a wavelength of 765nm was measured using a UV-Vis spectrophotometer (U-2001, manufactured by Hitachi, Ltd.).
[0168] <Shrinkage rate during sterilization> The hollow fiber membrane was sterilized by the following method: The hollow fiber membrane was cut to a length of 40 cm, and sterilized for 20 hours using an autoclave (Tomy Seiko Co., Ltd., LSX-300) at a set temperature of 125° C. The length of the hollow fiber membrane was measured, and the shrinkage rate was calculated by dividing the shrinkage length by the length of the hollow fiber membrane before sterilization.
[0169] <Measurement of maximum stress and breaking elongation> The strength was measured at a full-scale load of 5 kg and a crosshead speed of 50 mm / min using a tensile tester (TENSILON / RTM100 manufactured by Toyo Baldwin Co., Ltd.) A test piece with a test length of 50 mm was used for the measurement in a wet state.
[0170] <Measurement of β-glucan> The measurement of β-glucan was carried out using a β-glucan measurement kit (Mixed-linkage β-glucan) manufactured by Megazyme, Inc. The measurement was carried out according to the attached protocol.
[0171] (Reference example 1) 28% by weight of vinylidene fluoride homopolymer with a weight average molecular weight of 417,000 and 72% by weight of dimethyl sulfoxide were dissolved at 120°C. This vinylidene fluoride homopolymer solution was discharged from the outer tube of a double-tube type spinneret, and at the same time, a 90% by weight aqueous solution of dimethyl sulfoxide was discharged from the inner tube of the double-tube type spinneret. The solution was solidified in a bath of 85% by weight aqueous solution of dimethyl sulfoxide at a temperature of 10°C, and then washed with water and stretched to 1.4 times in water at 90°C. The pore size of the obtained hollow fiber membrane was 100 nm. End The pore volume (V1) of 3 / g), pore size 100nm less than The pore volume (V2) of 3 / g).
[0172] (Reference example 2) The hollow fiber membrane obtained in Reference Example 1 was immersed in dimethyl sulfoxide at 10° C. for 15 minutes to replace the poor solvent with water. The pore size of the obtained hollow fiber membrane was 100 nm. End The pore volume (V1) of3 / g), pore size 100nm less than The pore volume (V2) of 3 The shrinkage rate at 125°C sterilization was 5.1%, and the elongation at break was 35%. (Reference example 3) Vinylpyrrolidone / vinyl acetate random copolymer (Kollidon VA64; manufactured by BASF) The hollow fiber membrane prepared in Reference Example 2 was immersed for 2 hours in a 0.1 wt% aqueous ethanol solution in which 1000 ppm of a hydrophilic polymer consisting of the above was dissolved, and then irradiated with 25 kGy of gamma rays to introduce a vinylpyrrolidone / vinyl acetate random copolymer into the hollow fiber membrane. The ratio of monomer units in the vinylpyrrolidone / vinyl acetate random copolymer was 6 / 4, and the hydration energy density of the hydrophilic polymer / volume fraction of the monomer unit with the highest hydration energy density (vinylpyrrolidone) / difference in hydration energy density between vinylpyrrolidone and vinyl acetate was 45.2 / 60 / 14.
[0173] Example 1 Using the hollow fiber membrane module prepared using the hollow fiber membrane of Reference Example 1, cross-flow filtration of beer was carried out with the filtration device of FIG. 1 (step a). The beer used was "Ginga Kogen Beer", a commercially available unfiltered beer containing brewer's yeast (hereinafter referred to as evaluation beer). After filling the module with RO water and leaving it for more than one hour, the RO water outside the hollow fiber membrane was discharged, and the water present in the hollow portion was replaced with the evaluation beer. 2 L of evaluation beer maintained at 0°C was prepared in a container, and a circuit was constructed so that the evaluation beer was perfused from this container through the outer surface of the hollow fiber membrane via a pump and returned to the container, and at the same time, the filtrate filtered by the hollow fiber membrane was collected in a container different from the container containing the evaluation beer. At that time, the inlet pressure and outlet pressure of the evaluation beer to the module and the pressure on the filtration side could be measured. The evaluation beer was introduced into the module inlet so that the evaluation beer would flow at a membrane surface linear velocity of 1.5 m / sec. The filtration flux was 100 [L / m 2 / h]. In this state, the beer for evaluation was perfused on the outer surface of the hollow fiber membrane at 5±3°C, and cross-flow filtration was continued in which a portion of it was filtered. The inlet pressure, outlet pressure, and pressure on the filtration side were measured at specified time intervals, and filtration was continued until the transmembrane pressure difference (TMP) rose to 150 kPa, and the amount of beer processed was calculated. Additional beer for evaluation was added as necessary so that 2 L was maintained in the container. TMP = (Pi + Po) / 2 - Pf. where Pi is the inlet pressure, Po is the outlet pressure and Pf is the pressure on the filtration side. Beer throughput [L / m 2 ]=filtration flux 100 [L / m 2 / h] × time for pressure to rise to 150 kPa [h]. After the TMP reached 150 kPa, the filtration was stopped, the liquid was drained, and the filtrate was rinsed with pure water (step b). The rinsing with pure water was performed at a membrane surface linear velocity of 1.5 m / s and a filtration flux of 100 [L / m 2 / h] for 5 minutes, then 100[L / m 2 Backwashing was performed at [rpm] for 3 minutes. Next, chemical cleaning (step c) was performed. The chemical cleaning was performed with a 0.3% aqueous solution of sodium hypochlorite (pH 12) at 50°C, with 140 [L / m 2 / h], and the membrane was washed until the second beer filtration yielded 90% or more of the first beer throughput before the TMP rose to 150 kPa. Finally, the chemicals were drained, followed by rinsing with pure water (step d). The rinsing with pure water was performed at a membrane surface linear velocity of 1.5 m / s and a filtration flux of 100 [L / m 2 / h] for 5 minutes, after which the water was drained and rinsed again with pure water, and the same procedure was repeated a total of three times. The recovery rate of the beer throughput was calculated from the amount of beer throughput after repeating the above steps a to d 20 times. Note that the time for the first chemical cleaning was used for the time for the second and subsequent chemical cleanings. Beer processing volume recovery rate (%) = Beer processing volume (20th time) / Beer processing volume (1st time) × 100 The results of each filtration (beer throughput in the first filtration, the first cleaning time, the beer throughput in the 20th filtration, and the beer throughput recovery rate) are shown in Table 1.
[0174] Example 2 The chemical cleaning (step c) was carried out in the same manner as in Example 1, except that the first step was carried out using a 0.04% NaOH aqueous solution at 50° C., and the second step was carried out using a 0.3% sodium hypochlorite aqueous solution (pH 12) at 50° C. The results in Table 1 were obtained. The first and second cleaning steps were carried out for the same time.
[0175] Example 3 In Example 2, after step d, an additional chemical cleaning was performed for 15 minutes using a 3.0% citric acid aqueous solution at 50° C. in the same manner as in step b (step e). Furthermore, the chemical solution was drained, followed by rinsing with pure water (step f). The rinsing with pure water was performed at a membrane surface linear velocity of 1.5 m / s and a filtration flux of 100 [L / m 2 / h] for 5 minutes. Thereafter, the water was drained and rinsed again with pure water, and the same operation was repeated a total of three times. The same method as in Example 2 was carried out except that the above-mentioned steps a to f were repeated, and the results in Table 1 were obtained.
[0176] Example 4 In step c of Example 2, the flux of back-filtration from the inside (secondary side) of the hollow fiber membrane to the outside (primary side) during chemical cleaning was 250 [L / m 2 / h], the same method as in Example 2 was repeated to obtain the results shown in Table 1.
[0177] Example 5 The same procedure as in Example 2 was repeated except that in step c of Example 2, 0.2% Tween 20 (polyoxyethylene sorbitan monolaurate, manufactured by Wako Pure Chemical Industries, Ltd.) was added as a nonionic surfactant to the chemical solution in the first stage, and the results in Table 1 were obtained.
[0178] Example 6 The same procedure was carried out as in Example 2, except that the hollow fiber membrane of Reference Example 2 was used, and the results in Table 1 were obtained. In addition, a sample of the membrane used was cut out and subjected to stress measurement, and the maximum stress was 1800 gf / mm 2 It was.
[0179] Example 7 The same procedure was carried out as in Example 2, except that the hollow fiber membrane of Reference Example 3 was used, and the results in Table 1 were obtained.
[0180] Comparative Example 1 The same procedure was carried out as in Example 2, except that in step c, the sample was immersed in a chemical solution, and the results in Table 1 were obtained.
[0181] Comparative Example 2 The same procedure was carried out as in Example 2, step c, except that the chemical solution was caused to flow from the outside (primary side) to the inside (secondary side), and the results in Table 1 were obtained.
[0182] Comparative Example 3 The same procedure was carried out as in Example 7, except that in step c, the chemical solution was caused to flow from the outside (primary side) to the inside (secondary side), and the results in Table 1 were obtained.
[0183] Example 8 In Example 2, the filtration in step a was performed in the same manner, except that the amount of evaluation beer held in the container was 500 mL, and the filtration was performed until the β-glucan concentration in the raw water reached 1.3 times the initial concentration, obtaining the results in Table 1. Note that the density of the beer was calculated by arranging an electromagnetic flowmeter and a Coriolis flowmeter in series in the circulation section of the evaluation beer, and when the beer density reached a value corresponding to the previously measured β-glucan concentration, it was determined that the β-glucan concentration had reached 1.3 times, and washing was performed.
[0184] Comparative Example 4 The same method was carried out as in Example 8, except that the chemical solution in step c was flowed from the outside (primary side) to the inside (secondary side), and the results in Table 1 were obtained.
[0185] Comparative Example 5 The same method was used as in Example 8, except that the filtration in step a was carried out until the β-glucan concentration in the raw water reached 1.2 times the initial concentration, and the results shown in Table 1 were obtained.
[0186] Comparative Example 6 In Example 8, the filtration in step a was carried out until the β-glucan concentration in the raw water reached 1.2 times the initial concentration, and the chemical solution in step c was flowed from the outside (primary side) to the inside (secondary side). Except for this, the same method was used, and the results in Table 1 were obtained.
[0187] Example 9 In Example 6, the filtration in step a was carried out in the same manner except that the amount of evaluation beer held in the container was 50 mL and the filtration was carried out until the β-glucan concentration in the raw water reached 15 times the initial concentration, and the results in Table 1 were obtained.
[0188] Comparative Example 7 The same method was carried out as in Example 9, except that the chemical solution in step c was flowed from the outside (primary side) to the inside (secondary side), and the results in Table 1 were obtained.
[0189] Comparative Example 8 In Example 6, the amount of evaluation beer held in the container was 20 mL, and the filtration of step a was carried out until the β-glucan concentration in the raw water reached 20 times the initial concentration, but the same method was used, and the results in Table 1 were obtained.
[0190] Comparative Example 9 In Comparative Example 8, the same procedure was carried out except that the chemical solution in step c was flowed from the outside (primary side) to the inside (secondary side), and the results in Table 1 were obtained.
[0191] Example 10 The same procedure was carried out as in Example 6, except that the first step of step c was carried out using a 0.4% NaOH aqueous solution at 50° C., and the results in Table 1 were obtained. The membrane used was cut out and subjected to stress measurement, and the maximum point stress was 1800 gf / mm 2 As compared with Example 6, no decrease in strength was observed.
[0192] Example 11 The same procedure was carried out as in Example 6, except that the second stage of step c was carried out using a 1.0% aqueous solution of sodium hypochlorite (pH 12) at 50° C., and the results in Table 1 were obtained. The membrane used was cut out and subjected to stress measurement, and the maximum point stress was 1800 gf / mm 2 As compared with Example 6, no decrease in strength was observed.
[0193] Comparative Example 10 The same procedure was carried out as in Example 2, except that the first step of step c was carried out using a 0.4% NaOH aqueous solution at 50° C., and the results in Table 1 were obtained. The membrane used was cut out and subjected to stress measurement, and the maximum point stress was 1600 gf / mm 2 The recovery rate was the same as in Example 10, but the maximum point stress was reduced.
[0194] [Table 1]
[0195] Examples 1 to 7 were all superior to Comparative Examples 1 to 3 in terms of beer processing volume, chemical cleaning time, and beer processing volume recovery rate. These results demonstrate that the filtration method of the present invention enables fermentation broth to be filtrated stably over a long period of time. [Industrial Applicability]
[0196] The method for filtering a fermentation broth of the present invention can be used for filtering a fermentation broth in the fields of fermentation industry, food industry, and the like. [Explanation of symbols]
[0197] 1. Concentrate tank 2. Membrane module 3. Stock solution pump 4 Circulation Control Valve 5 Filtration Control Valve 6 Filtrate tank 7 Backwash tank 8 Backwash Pump 9 Backwash Control Valve 10 Cleaning solution tank 11~20 valves 21~23 Pressure gauge 24~26 Flowmeter 30 Hollow fiber membrane 31 External surface 32 Inner surface 40 Spherical structure 41 Spherical body 42 Non-spherical part (also called constriction) 43 void
Claims
1. A method for filtering a fermentation liquid by carrying out the following steps a to f in this order: (a) subjecting a fermentation liquid to cross-flow filtration using a membrane module having a separation membrane; (b) rinsing the separation membrane with water; (c) permeating a chemical solution having a pH of 10 to 14 from the secondary side to the primary side of the separation membrane; (d) rinsing the separation membrane with water; After step d, (e) passing a chemical solution C having a pH of 0 to 4 from the secondary side to the primary side of the separation membrane; (f) after step e, rinsing the membrane module with water; Including, The cross-flow membrane permeate in the step (a) has a total sugar concentration of 1,000 mg / L or more and 100,000 mg / L or less, a protein concentration of 50 mg / L or more and 10,000 mg / L or less, and a polyphenol concentration of 50 mg / L or more and 10,000 mg / L or less, The step c is (c-1) A method for filtering a fermentation liquid, comprising a step of passing a chemical solution A having a pH of 10 or more and 14 or less and an oxidant concentration of 0.01% or more from the secondary side to the primary side of a membrane module.
2. The step c is (c-2) Before the step c-1, a step of permeating a chemical solution B having an oxidant concentration of less than 0.01% and a pH of 10 to 14 from the secondary side of the separation membrane to the primary side is further provided. The filtration method for the fermentation liquid according to claim 1.
3. In the steps c and e, the flux (m 3 / m 2 3. The method for filtering a fermentation broth according to claim 1 or 2, wherein the cross-flow flux in step a) is 1.5 to 10 times that in step a).
4. The fermentation liquor filtration method according to any one of claims 1 to 3, wherein the chemical solution C is an aqueous solution containing at least one compound selected from the group consisting of hydrochloric acid, nitric acid, sulfuric acid, phosphoric acid, formic acid, acetic acid, propionic acid, butyric acid, citric acid, oxalic acid, ascorbic acid and lactic acid.
5. 3. The method for filtering a fermentation liquid using a membrane module according to claim 2, wherein the chemical solutions A, B and C contain at least one cleaning auxiliary selected from the group consisting of a surfactant, an enzyme and a chelating agent.
6. Polysaccharide concentration in raw water C t is the concentration at the start of filtration C 0 The method for filtering a fermentation broth according to any one of claims 1 to 5, wherein the step (a) is carried out at a concentration in the range of 1.3 to 15 times the concentration of the fermentation broth.
7. The method for filtering a fermentation liquid according to any one of claims 1 to 6, wherein the separation membrane is a hollow fiber membrane.
8. The separation membrane contains a hydrophobic polymer resin, The pore volume V2 of pores with a pore diameter of less than 100 nm measured by gas adsorption method is 0.02 cm 3 / g or more 0.1cm 3 / g or less, and The pore volume V1 of pores with a diameter of 100 nm or more measured by mercury intrusion porosimetry is 0.1 cm 3 / g or more, 8. The method for filtering a fermentation broth according to claim 7, wherein the ratio V1 / V2 of the pore volume V2 to the pore volume V1 is 3 or more and 60 or less. V1: pore volume of pores having a pore diameter of 100 nm or more measured by mercury intrusion porosimetry V2: pore volume of pores with a pore diameter of less than 100 nm measured by gas adsorption method
9. 9. The method for filtering a fermentation broth according to claim 8, wherein the separation membrane has a breaking elongation of 38% or more.
10. 10. The separation membrane according to claim 8, wherein the shrinkage rate of the hollow fiber membrane length when the membrane is heat-treated in a water vapor atmosphere at 125°C for 20 hours is 0.5% or more.
11. The separation membrane contains a hydrophilic polymer, The hydrophilic polymer contains a copolymer composed of N types of monomer units 1, 2, ... i ... N, and the hydration energy density of the hydrophilic polymer calculated based on the following formula (1) is 40 to 70 cal mol -1 ・Å -3 The method for filtering a fermentation liquid according to any one of claims 1 to 10. [0010] [In formula (1), the hydration energy of any monomer unit i is the absolute value of the energy of the monomer unit i in water minus the energy of the monomer unit i in a vacuum, N is the total number of monomer species constituting the copolymer, i is an integer of 1 to N, and N is an integer of 2 or more.]
12. The method for filtering a fermentation broth according to any one of claims 8 to 10, wherein the hydrophobic polymer resin is a fluorine-based resin or a sulfone-based resin.
13. The filtration in step a is an external pressure filtration in which filtration is performed from the outer periphery side of the hollow fiber membrane to the inner periphery side, and in steps c and e, the flux of the chemical solution to be permeated is 7.0 m per inner area of the hollow fiber membrane. 3 / m 2 / d or more 10m 3 / m 2 The method for filtering a fermentation liquid according to any one of claims 1 to 12, wherein the filtration rate is 1 / d or less.
Citation Information
Patent Citations
Method for washing permeable membrane
JP2005224671A
Hollow fiber membrane made of polyvinylidene fluoride resin, and its manufacturing method
JP2008105016A
Operation method of filtration apparatus
JP2017056371A
Hollow fiber membrane, manufacturing method of hollow fiber membrane, and production method of beer, wine or japanese sake using hollow fiber membrane
JP2019130522A
Asymmetric hollow fiber membranes
WO2002058828A1