(Meth)acrylate resin having acid group, curable resin composition, cured product, insulating material, and resist member
A (meth)acrylate resin with acid groups, composed of specific epoxy and anhydride components, addresses the dielectric issues in conventional solder resist compositions by enhancing photosensitivity and dielectric properties, suitable for solder resist coatings.
Patent Information
- Application Number
- JP2020175894
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-10-20
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2040-10-20
AI Technical Summary
Conventional curable compositions for solder resists, such as those containing acid group-containing epoxy resins, suffer from insufficient dielectric properties due to the generation of hydroxyl groups, leading to increased dielectric constant and dielectric loss tangent.
A (meth)acrylate resin with acid groups is formulated using an epoxy resin, an unsaturated monobasic acid, and a polybasic acid anhydride, incorporating a compound with a phenolic hydroxyl group and an aromatic compound with at least two ethylenically unsaturated bonds, which are reacted with epihalohydrin to enhance photosensitivity, alkali developability, and dielectric properties.
The resulting resin exhibits high photosensitivity, excellent alkali developability, and forms a cured product with superior elongation and dielectric properties, making it suitable for applications like solder resist coatings.
Smart Images

Figure 0007567351000001 
Figure 0007567351000002 
Figure 0007567351000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a (meth)acrylate resin having an acid group capable of forming a cured product having high photosensitivity and excellent elongation and dielectric properties, a curable resin composition containing the same, a cured product of the curable resin composition, an insulating material, and a resist member. [Background technology]
[0002] In recent years, curable compositions such as active energy ray curable compositions that can be cured by active energy rays such as ultraviolet rays and thermosetting compositions that can be cured by heat have been widely used in the fields of inks, paints, coating agents, adhesives, optical members, etc. In particular, for the above-mentioned coating agent applications, it is generally required that the coating agent can impart design to the surfaces of various substrates, has excellent curability, and can form a coating film that can prevent deterioration of the substrate surface. Furthermore, when used as a curable composition for solder resist for printed wiring boards, it is also required that the composition can be cured with a small amount of exposure.
[0003] As a conventional curable composition for a solder resist, a photosensitive resin composition containing an acid group-containing epoxy acrylate resin obtained by further reacting tetrahydrophthalic anhydride with an intermediate obtained by reacting a cresol novolac epoxy resin with acrylic acid and phthalic anhydride is known (see, for example, Patent Document 1). However, there are problems such as insufficient dielectric properties, for example, an increase in dielectric constant and dielectric loss tangent due to the generation of hydroxyl groups.
[0004] Therefore, there has been a demand for a material that has high photosensitivity, excellent alkaline developability, and excellent elongation and dielectric properties. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Application Publication No. 8-259663 Summary of the Invention [Problem to be solved by the invention]
[0006] The problem to be solved by the present invention is to provide a (meth)acrylate resin having an acid group, which has high photosensitivity and excellent alkaline developability, and is capable of forming a cured product having excellent elongation and dielectric properties; a curable resin composition containing the same; and a cured product of the curable resin composition, an insulating material, and a resist member. [Means for solving the problem]
[0007] Means for Solving the Problems The present inventors have conducted intensive research to solve the above problems, and as a result have found that the above problems can be solved by using an epoxy resin using, as essential raw materials, a compound having a phenolic hydroxyl group, an aromatic compound having at least two ethylenically unsaturated bonds, and epihalohydrin, and a (meth)acrylate resin having an acid group, the essential raw materials of which are an unsaturated monobasic acid and a polybasic acid anhydride, and have thus completed the present invention.
[0008] That is, the present invention relates to a (meth)acrylate resin having an acid group, which is made from an epoxy resin (A), an unsaturated monobasic acid (B), and a polybasic acid anhydride (C) as essential raw materials, wherein the epoxy resin (A) is made from a compound (a1) having a phenolic hydroxyl group, an aromatic compound (a2) having at least two ethylenically unsaturated bonds, and an epihalohydrin (a3) as essential raw materials; a curable resin composition containing the same; and a cured product of the curable resin composition, an insulating material, and a resist member. Effect of the Invention
[0009] The (meth)acrylate resin having an acid group of the present invention has high photosensitivity and excellent alkaline developability, and can form a cured product having excellent elongation and dielectric properties, so that a curable resin composition containing the (meth)acrylate resin having an acid group and a photopolymerization initiator can be used as a coating agent or adhesive, and as the coating agent, it is particularly suitable for use in solder resist applications. Note that the "excellent dielectric properties" in the present invention refer to a low dielectric constant and a low dielectric loss tangent. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The (meth)acrylate resin having an acid group of the present invention is characterized in that it contains, as essential raw materials, an epoxy resin (A), an unsaturated monobasic acid (B), and a polybasic acid anhydride (C).
[0011] In the present invention, "(meth)acrylate" means acrylate and / or methacrylate. "(meth)acryloyl" means acryloyl and / or methacryloyl. "(meth)acrylic" means acrylic and / or methacrylic.
[0012] Examples of the acid group contained in the (meth)acrylate resin having an acid group of the present invention include a carboxyl group, a sulfonic acid group, a phosphoric acid group, etc. Among these, the carboxyl group is preferred.
[0013] The epoxy resin (A) used comprises, as essential raw materials, a compound (a1) having a phenolic hydroxyl group, an aromatic compound (a2) having at least two ethylenically unsaturated bonds, and an epihalohydrin (a3).
[0014] The compound (a1) having a phenolic hydroxyl group refers to a compound having at least one phenolic hydroxyl group in the molecule. Examples of the compound having at least one phenolic hydroxyl group in the molecule include compounds represented by the following structural formulas (1-1) to (1-4).
[0015] [ka]
[0016] In the above structural formulas (1-1) to (1-4), R 1 is any one of an alkyl group having 1 to 20 carbon atoms, an alkoxy group having 1 to 20 carbon atoms, an aryl group, and a halogen atom; R 2 are each independently a hydrogen atom or a methyl group. p is 0 or an integer of 1 or more, preferably 0 or an integer of 1 to 3, more preferably 0 or 1, and even more preferably 0. q is an integer of 1 or more, preferably 2 or 3. The position of the substituent on the aromatic ring in the above structural formula is arbitrary. For example, in the naphthalene ring of structural formula (1-2), the substituent may be on any ring, in structural formula (1-3), the substituent may be on any ring of the benzene ring present in one molecule, and in structural formula (1-4), the substituent may be on any ring of the benzene ring present in one molecule, and the numbers of the substituents in one molecule are p and q.
[0017] The compound (a1) having a phenolic hydroxyl group may be, for example, a reaction product obtained by using as essential reaction raw materials a compound having at least one phenolic hydroxyl group in the molecule and a compound represented by any one of the following structural formulas (x-1) to (x-5). Also, a novolac-type phenolic resin may be obtained by using as reaction raw materials one or more compounds having at least one phenolic hydroxyl group in the molecule.
[0018] [ka]
[0019] [In formula (x-1), h is 0 or 1. In formulas (x-2) to (x-5), R 3is any one of an alkyl group having 1 to 20 carbon atoms, an alkoxy group having 1 to 20 carbon atoms, an aryl group, and a halogen atom, and i is 0 or an integer of 1 to 4. In formulas (x-2), (x-3), and (x-5), Z is each independently any one of a vinyl group, a halomethyl group, a hydroxymethyl group, and an alkyloxymethyl group. In formula (x-5), Y is any one of an alkylene group having 1 to 4 carbon atoms, an oxygen atom, a sulfur atom, and a carbonyl group, and j is an integer of 1 to 4.]
[0020] These compounds (a1) having a phenolic hydroxyl group can be used alone or in combination of two or more kinds.
[0021] The aromatic compound (a2) has at least two ethylenically unsaturated bonds. Examples of the aromatic divinyl compounds include divinylbenzene, alkyl divinylbenzene, diallyl phthalate, and diisopropenylbenzene. These aromatic compounds (a2) can be used alone or in combination of two or more. In addition, aromatic divinyl compounds are preferred, and divinylbenzene and diisopropenylbenzene are particularly preferred, because they provide a (meth)acrylate resin having an acid group capable of forming a cured product having high photosensitivity, excellent alkaline developability, and excellent elongation and dielectric properties.
[0022] Examples of the divinylbenzene include 1,2-divinylbenzene, 1,3-divinylbenzene, 1,4-divinylbenzene, etc. These divinylbenzenes can be used alone or in combination of two or more kinds.
[0023] Examples of the diisopropenylbenzene include 1,2-diisopropenylbenzene, 1,3-diisopropenylbenzene, 1,4-diisopropenylbenzene, etc. These diisopropenylbenzenes can be used alone or in combination of two or more kinds.
[0024] In addition, the aromatic compound (a2) may be used in combination with other reactive third components as necessary. Examples of the reactive third components include aromatic monovinyl compounds such as styrene, methylstyrene, ethylstyrene, and monobromostyrene, and aliphatic monovinyl compounds such as (meth)acrylic acid methyl ester, (meth)acrylic acid stearyl ester, (meth)acrylic acid, N-methylol (meth)acrylamide, and γ-mercaptopropyl trimethoxysilane. These reactive third components may be used alone or in combination of two or more.
[0025] The amount of the aromatic compound (a2) used is preferably in the range of 0.25 to 1 mole per mole of the compound (a1) having a phenolic hydroxyl group, since a (meth)acrylate resin having an acid group capable of forming a cured product having high photosensitivity, excellent alkali developability, and excellent elongation and dielectric properties can be obtained.
[0026] Examples of the epihalohydrin (a3) include epichlorohydrin and epibromohydrin. These epihalohydrins can be used alone or in combination of two or more. Among these, epichlorohydrin is preferred because it is easy to control the reaction.
[0027] Furthermore, the (meth)acrylate resin having an acid group of the present invention is preferably one represented by the following structure, since it has high photosensitivity and excellent alkaline developability, and is capable of forming a cured product having excellent elongation and dielectric properties.
[0028] [ka]
[0029] [In formula (2), each ring A is independently a benzene ring or a naphthalene ring; R 1 are each independently a hydrogen atom, a methyl group, an ethyl group, or a propyl group; R 2are each independently a hydrogen atom, a methyl group, an ethyl group, or a propyl group, and each X is independently represented by the following structural formula (X-1) or (X-2), m is an integer of 1 to 6, and n is an integer of 1 to 20.]
[0030] [ka]
[0031] [In formula (X-1), R 3 is a hydrogen atom or a methyl group, R 4 is a hydrocarbon group having 1 to 10 carbon atoms, a benzene ring and / or a cyclo ring. The cyclo ring includes those having an unsaturated bond.]
[0032] [In formula (X-2), R 5 is a hydrogen atom or a methyl group.
[0033] The method for producing the epoxy resin (A) is not particularly limited, and the epoxy resin (A) may be produced by any known method. For example, the epoxy resin (A) may be produced by reacting all of the reaction raw materials at once, or by reacting the reaction raw materials sequentially.
[0034] Examples of the method of reacting the reaction raw materials sequentially include a method of first reacting the compound (a1) having a phenolic hydroxyl group with the aromatic compound (a2) in the presence of an acid catalyst at a temperature range of 80 to 200°C, then adding 1 to 10 moles of the epihalohydrin (a3) per mole of hydroxyl group contained in the reaction product of the compound (a1) having a phenolic hydroxyl group with the aromatic compound (a2), and further adding 0.5 to 10 moles of a basic catalyst per mole of hydroxyl group of the raw material all at once or gradually while reacting for 0.5 to 10 hours at a temperature of 20 to 120°C to perform an epoxidation reaction. The basic catalyst may be a solid or an aqueous solution thereof. When an aqueous solution is used, it may be added continuously, and water and epihalohydrin may be continuously distilled from the reaction mixture under reduced pressure or normal pressure, and further separated to remove water and return epihalohydrin to the reaction mixture continuously.
[0035] The reaction of the compound (a1) having a phenolic hydroxyl group, the aromatic compound (a2) and the epihalohydrin (a3) can also be carried out in an organic solvent, if necessary.
[0036] In industrial production, all of the epihalohydrin used for charging in the first batch of epoxy resin production is new, but from the next batch onwards, it is preferable to use epihalohydrin recovered from the crude reaction product in combination with fresh epihalohydrin equivalent to the amount consumed and lost in the reaction. In this case, impurities derived from the reaction of epichlorohydrin with water, organic solvents, etc., such as glycidol, may be contained.
[0037] The obtained epoxy resin (A) is washed with water as necessary, and unreacted epihalohydrin and the organic solvent used are removed by distillation under reduced pressure with heating. In order to obtain an epoxy resin with a smaller amount of hydrolyzable halogen, the obtained epoxy resin (A) can be dissolved again in an organic solvent such as toluene, methyl isobutyl ketone, or methyl ethyl ketone, and an aqueous solution of an alkali metal hydroxide such as sodium hydroxide or potassium hydroxide can be added to perform a further reaction. In this case, a phase transfer catalyst such as a quaternary ammonium salt or crown ether may be present in order to improve the reaction rate. When the phase transfer catalyst is used, the amount of the catalyst used is preferably in the range of 0.1 to 3 mass% relative to the epoxy resin used. After the reaction is completed, the salt formed is removed by filtration, washing with water, or the like, and the solvent such as toluene or methyl isobutyl ketone is further removed by distillation under reduced pressure with heating, to obtain a high-purity epoxy resin (A).
[0038] In particular, when the reaction product of the compound (a1) having a phenolic hydroxyl group and the aromatic compound (a2) is reacted with epihalohydrin (a3), the water concentration in the solvent is adjusted to 5 to 25%, whereby the desired epoxy resin can be efficiently obtained.
[0039] Examples of the acid catalyst include inorganic acids such as hydrochloric acid, sulfuric acid, and phosphoric acid, organic acids such as methanesulfonic acid, paratoluenesulfonic acid, and oxalic acid, and Lewis acids such as boron trifluoride, anhydrous aluminum chloride, and zinc chloride. In addition, solid acid catalysts having a strong acid such as a sulfonyl group can also be used. These acid catalysts can be used alone or in combination of two or more.
[0040] Examples of commercially available solid acid catalysts include "Amberlyst 15DRY", "Amberlyst 15JWET", "Amberlyst 16WET", "Amberlyst 35WET", and "Amberlyst 33" manufactured by Organo Corporation, and "Teikacure-6", "Teikacure-10", and "Teikacure-15" manufactured by Teika Corporation.
[0041] Examples of the basic catalyst include amine compounds such as N-methylmorpholine, pyridine, 1,8-diazabicyclo[5.4.0]undecene-7 (DBU), 1,5-diazabicyclo[4.3.0]nonene-5 (DBN), 1,4-diazabicyclo[2.2.2]octane (DABCO), tri-n-butylamine or dimethylbenzylamine, butylamine, octylamine, monoethanolamine, diethanolamine, triethanolamine, imidazole, 1-methylimidazole, 2,4-dimethylimidazole, 1,4-diethylimidazole, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-(N-phenyl)aminopropyltrimethoxysilane, 3-(2-aminoethyl)aminopropyltrimethoxysilane, 3-(2-aminoethyl)aminopropylmethyldimethoxysilane, and tetramethylammonium hydroxide; trioctylmethylammonium chloride, trioctylmethylammonium chloride, and trioctylmethylammonium chloride. Examples of the quaternary ammonium salts include octylmethylammonium acetate; phosphine compounds such as trimethylphosphine, tributylphosphine, and triphenylphosphine; phosphonium salts such as tetramethylphosphonium chloride, tetraethylphosphonium chloride, tetrapropylphosphonium chloride, tetrabutylphosphonium chloride, tetrabutylphosphonium bromide, trimethyl(2-hydroxypropyl)phosphonium chloride, triphenylphosphonium chloride, and benzylphosphonium chloride; organic tin compounds such as dibutyltin dilaurate, octyltin trilaurate, octyltin diacetate, dioctyltin diacetate, dioctyltin dineodecanoate, dibutyltin diacetate, tin octylate, and 1,1,3,3-tetrabutyl-1,3-dodecanoyldistannoxane; organic metal compounds such as zinc octylate and bismuth octylate; inorganic tin compounds such as tin octanoate; and inorganic metal compounds. In addition, alkaline earth metal hydroxides, alkali metal carbonates, and alkali metal hydroxides can also be used. In particular, alkali metal hydroxides are preferred because they have excellent catalytic activity in the epoxy resin synthesis reaction, and for example, sodium hydroxide and potassium hydroxide are more preferred. These basic catalysts can be used alone or in combination of two or more kinds.When the basic catalyst is used, it may be used in the form of an aqueous solution of about 10% by mass to 55% by mass, or in the form of a solid.
[0042] Examples of the organic solvent include ketone solvents such as methyl ethyl ketone, acetone, dimethylformamide, and methyl isobutyl ketone; cyclic ether solvents such as tetrahydrofuran and dioxolane; ester solvents such as methyl acetate, ethyl acetate, and butyl acetate; aromatic solvents such as toluene, xylene, and solvent naphtha; alicyclic solvents such as cyclohexane and methylcyclohexane; alcohol solvents such as carbitol, cellosolve, methanol, isopropanol, butanol, and propylene glycol monomethyl ether; glycol ether solvents such as alkylene glycol monoalkyl ether, dialkylene glycol monoalkyl ether, and dialkylene glycol monoalkyl ether acetate; methoxypropanol, cyclohexanone, methyl cellosolve, diethylene glycol monoethyl ether acetate, and propylene glycol monomethyl ether acetate. These organic solvents can be used alone or in combination of two or more. The amount of the organic solvent used is preferably in the range of about 0.1 to 5 times the total mass of the reaction raw materials, since this improves the reaction efficiency.
[0043] In the production of the epoxy resin (A), a compound having a phenolic hydroxyl group other than the compound (a1) having a phenolic hydroxyl group can be used in combination, provided that the effects of the present invention are not impaired.
[0044] Examples of the unsaturated monobasic acid (B) include acrylic acid, methacrylic acid, crotonic acid, cinnamic acid, α-cyanocinnamic acid, β-styrylacrylic acid, β-furfurylacrylic acid, etc. In addition, esters, acid halides, acid anhydrides, etc. of the unsaturated monobasic acids can also be used. Furthermore, compounds represented by the following structural formula (3) can also be used.
[0045] [ka] [In formula (3), X represents an alkylene chain having 1 to 10 carbon atoms, a polyoxyalkylene chain, a (poly)ester chain, an aromatic hydrocarbon chain, or a (poly)carbonate chain, and may have a halogen atom, an alkoxy group, or the like in the structure. Y represents a hydrogen atom or a methyl group.]
[0046] Examples of the polyoxyalkylene chain include a polyoxyethylene chain and a polyoxypropylene chain.
[0047] An example of the (poly)ester chain is a (poly)ester chain represented by the following structural formula (4).
[0048] [ka] [In formula (4), R 1 is an alkylene group having 1 to 10 carbon atoms, and n is an integer of 1 to 5.
[0049] Examples of the aromatic hydrocarbon chain include a phenylene chain, a naphthylene chain, a biphenylene chain, a phenylnaphthylene chain, a binaphthylene chain, etc. In addition, a hydrocarbon chain having an aromatic ring such as a benzene ring, a naphthalene ring, an anthracene ring, or a phenanthrene ring as a partial structure can also be used.
[0050] These unsaturated monobasic acids (B) can be used alone or in combination of two or more kinds.
[0051] The amount of the unsaturated monobasic acid (B) used is preferably in the range of 0.9 to 1.1, and more preferably 0.95 to 1.05, in terms of the number of moles of the acid groups of the unsaturated monobasic acid (B) per mole of the epoxy groups of the epoxy resin (A), since a (meth)acrylate resin having high photosensitivity and excellent alkali developability and capable of forming a cured product excellent in elongation and dielectric properties can be obtained.
[0052] Examples of the polybasic acid anhydride (C) include aliphatic polybasic acid anhydrides, alicyclic polybasic acid anhydrides, and aromatic polybasic acid anhydrides.
[0053] Examples of the aliphatic polybasic acid anhydride include anhydrides of oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, maleic acid, fumaric acid, citraconic acid, itaconic acid, glutaconic acid, 1,2,3,4-butanetetracarboxylic acid, etc. In addition, the aliphatic polybasic acid anhydride may have an aliphatic hydrocarbon group of either a straight-chain type or a branched type, and may have an unsaturated bond in the structure.
[0054] In the present invention, the alicyclic polybasic acid anhydride is one in which an acid anhydride group is bonded to an alicyclic structure, and the presence or absence of aromatic rings in other structural parts is not important. Examples of the alicyclic polybasic acid anhydride include tetrahydrophthalic acid, hexahydrophthalic acid, methylhexahydrophthalic acid, cyclohexanetricarboxylic acid, cyclohexanetetracarboxylic acid, bicyclo[2.2.1]heptane-2,3-dicarboxylic acid, methylbicyclo[2.2.1]heptane-2,3-dicarboxylic acid, and 4-(2,5-dioxotetrahydrofuran-3-yl)-1,2,3,4-tetrahydronaphthalene-1,2-dicarboxylic acid anhydrides.
[0055] Examples of the aromatic polybasic acid anhydride include anhydrides of phthalic acid, trimellitic acid, pyromellitic acid, naphthalene dicarboxylic acid, naphthalene tricarboxylic acid, naphthalene tetracarboxylic acid, biphenyl dicarboxylic acid, biphenyl tricarboxylic acid, biphenyl tetracarboxylic acid, and benzophenone tetracarboxylic acid.
[0056] These polybasic acid anhydrides (C) can be used alone or in combination of two or more kinds.
[0057] The amount of the polybasic acid anhydride (C) used is preferably in the range of 0.45 to 1 mole, more preferably 0.45 to 0.95 moles, per mole of the epoxy group in the epoxy resin (A), since a (meth)acrylate resin having an acid group capable of forming a cured product having high photosensitivity, excellent alkali developability, and excellent elongation and dielectric properties can be obtained.
[0058] The method for producing the acid group (meth)acrylate resin of the present invention is not particularly limited, and it can be produced by a known method as appropriate. For example, it may be produced by a method in which all of the reaction raw materials are reacted at once, or by a method in which the reaction raw materials are reacted sequentially.
[0059] As a method for reacting the reaction raw materials in sequence, a method is preferred in which the epoxy resin (A) and the unsaturated monobasic acid (B) are first reacted in the presence of an acidic catalyst or a basic catalyst at a temperature range of 80 to 140°C, and then the polybasic acid anhydride (C) is added and reacted at a temperature range of 80 to 140°C.
[0060] Furthermore, the reaction between the epoxy resin (A), the unsaturated monobasic acid (B) and the polybasic acid anhydride (C) can also be carried out in an organic solvent, if necessary.
[0061] As the acid catalyst, the same as those exemplified above as the acid catalyst can be used, and the acid catalyst can be used alone or in combination of two or more kinds.
[0062] The basic catalyst may be the same as the basic catalyst exemplified above, and the basic catalyst may be used alone or in combination of two or more. Among these, phosphine compounds are preferred because they can provide a (meth)acrylate resin having high photosensitivity and excellent alkaline developability, and capable of forming a cured product having excellent elongation and dielectric properties, and thus have an acid group.
[0063] As the organic solvent, the same organic solvents as those exemplified above can be used, and the organic solvents can be used alone or in combination of two or more kinds.
[0064] In the production of the acid group-containing (meth)acrylate resin of the present invention, a polymerization inhibitor, an antioxidant, etc. may also be used, if necessary.
[0065] Examples of the polymerization inhibitor include p-methoxyphenol, p-methoxycresol, 4-methoxy-1-naphthol, 4,4'-dialkoxy-2,2'-bi-1-naphthol, 3-(N-salicyloyl)amino-1,2,4-triazole, N'1,N'12-bis(2-hydroxybenzoyl)dodecane dihydrazide, styrenated phenol, N-isopropyl-N'-phenylbenzene-1,4-diamine, 6-ethoxy-2,2,4-trimethyl- Phenol compounds such as 1,2-dihydroquinoline, quinone compounds such as hydroquinone, methylhydroquinone, p-benzoquinone, methyl-p-benzoquinone, 2,5-diphenylbenzoquinone, 2-hydroxy-1,4-naphthoquinone, anthraquinone, and diphenoquinone, melamine, p-phenylenediamine, 4-aminodiphenylamine, N.N'-diphenyl-p-phenylenediamine, Ni-propyl-N'-phenyl-p-phenylenediamine, N-(1.amine compounds such as 3-dimethylbutyl)-N'-phenyl-p-phenylenediamine, diphenylamine, 4,4'-dicumyl-diphenylamine, 4,4'-dioctyl-diphenylamine, poly(2,2,4-trimethyl-1,2-dihydroquinoline), styrenated diphenylamine, reaction products of styrenated diphenylamine and 2,4,4-trimethylpentene, reaction products of diphenylamine and 2,4,4-trimethylpentene, phenothiazine, distearyl thiodipropionate, 2,2-bis({[3-(dodecyl) thioether compounds such as N-nitrosodiphenylamine, N-nitrosophenylnaphthylamine, p-nitrosophenol, nitrosobenzene, p-nitrosodiphenylamine, α-nitroso-β-naphthol, N,N-dimethyl p-nitrosoaniline, p-nitrosodiphenylamine, p-nitrosodimethylamine, p-nitroso ... -N,N-diethylamine, N-nitrosoethanolamine, N-nitrosodi-n-butylamine, N-nitroso-Nn-butyl-4-butanolamine, N-nitroso-diisopropanolamine, N-nitroso-N-ethyl-4-butanolamine, 5-nitroso-8-hydroxyquinoline, N-nitrosomorpholine, N-nitroso-N-phenylhydroxylamine ammonium salt, nitrosobenzene, N-nitroso-N-methyl-p-toluenesulfonamide, N-nitroso-N-ethylurethane, N-nitroso-Nn -Propyl urethane, 1-nitroso-2-naphthol, 2-nitroso-1-naphthol, sodium 1-nitroso-2-naphthol-3,6-sulfonate, sodium 2-nitroso-1-naphthol-4-sulfonate, 2-nitroso-5-methylaminophenol hydrochloride, 2-nitroso-5-methylaminophenol hydrochloride and other nitroso compounds, esters of phosphoric acid and octadecane-1-ol, triphenyl phosphite, 3,9-dioctadecan-1-yl-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]Undecane, trisnonylphenyl phosphite, phosphorous acid-(1-methylethylidene)-di-4,1-phenylenetetra-C12-15-alkyl ester, 2-ethylhexyl diphenyl phosphite, diphenyl isodecyl phosphite, triisodecyl phosphite, tris(2,4-di-tert-butylphenyl) phosphite and other phosphite compounds, bis(dimethyldithiocarbamato-κ(2)S,S')zinc, diethyldithiocarbamate , zinc compounds such as zinc dibutyl dithiocarbamate, nickel compounds such as bis(N,N-dibutylcarbamodithioato-S,S')nickel, sulfur compounds such as 1,3-dihydro-2H-benzimidazole-2-thione, 4,6-bis(octylthiomethyl)-o-cresol, 2-methyl-4,6-bis[(octan-1-ylsulfanyl)methyl]phenol, dilauryl thiodipropionate, and distearyl 3,3'-thiodipropionate. These polymerization inhibitors can be used alone or in combination of two or more.
[0066] As the antioxidant, the same compounds as those exemplified as the polymerization inhibitor can be used, and the antioxidants can be used alone or in combination of two or more kinds.
[0067] In addition, examples of commercially available products of the polymerization inhibitor and the antioxidant include "Q-1300" and "Q-1301" manufactured by Wako Pure Chemical Industries, Ltd., and "Sumilizer BBM-S" and "Sumilizer GA-80" manufactured by Sumitomo Chemical Co., Ltd.
[0068] The (meth)acrylate resin having an acid group of the present invention can be used as a curable resin composition by adding a photopolymerization initiator.
[0069] Examples of the photopolymerization initiator include photoradical polymerization initiators such as 1-hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenylpropan-1-one, 1-[4-(2-hydroxyethoxy)phenyl]-2-hydroxy-2-methyl-1-propan-1-one, thioxanthone and thioxanthone derivatives, 2,2'-dimethoxy-1,2-diphenylethan-1-one, diphenyl(2,4,6-trimethoxybenzoyl)phosphine oxide, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide, 2-methyl-1-(4-methylthiophenyl)-2-morpholinopropan-1-one, and 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-1-butanone.
[0070] Examples of commercially available photopolymerization initiators include "Omnirad 1173", "Omnirad 184", "Omnirad 127", "Omnirad 2959", "Omnirad 369", "Omnirad 379", "Omnirad 907", "Omnirad 4265", "Omnirad 1000", "Omnirad 651", "Omnirad TPO", "Omnirad 819", "Omnirad 2022", "Omnirad 2100", "Omnirad 754", "Omnirad 784", "Omnirad 500", and "Omnirad 81" (manufactured by IGM Resins); "KAYACURE DETX", "KAYACURE MBP", "KAYACURE DMBI", "KAYACURE EPA", and "KAYACURE OA" (manufactured by Nippon Kayaku Co., Ltd.); and "Vicure 10" and "Vicure 55" (manufactured by Stoffa Examples of photopolymerization initiators include "Trigonal P1" (manufactured by Akzo Nobel), "SANDORAY 1000" (manufactured by SANDOZ), "DEAP" (manufactured by Upjohn Chemical), "Quantacure PDO", "Quantacure ITX", "Quantacure EPD" (manufactured by Ward Blenkinsop), and "Runtecure 1104" (manufactured by Runtec). These photopolymerization initiators can be used alone or in combination of two or more kinds.
[0071] The amount of the photopolymerization initiator added is preferably within a range of, for example, 0.5 to 20% by mass in the curable resin composition.
[0072] The curable resin composition of the present invention may contain a resin component other than the (meth)acrylate resin having an acid group (hereinafter, sometimes referred to as "other resin components"). Examples of the other resin components include a resin having an acid group and a polymerizable unsaturated group, various (meth)acrylate monomers, etc.
[0073] The resin having an acid group and a polymerizable unsaturated group may be any resin having an acid group and a polymerizable unsaturated group in the resin, and examples thereof include an epoxy resin having an acid group and a polymerizable unsaturated group, a urethane resin having an acid group and a polymerizable unsaturated group, an acrylic resin having an acid group and a polymerizable unsaturated group, an amide-imide resin having an acid group and a polymerizable unsaturated group, an acrylamide resin having an acid group and a polymerizable unsaturated group, and an ester resin having an acid group and a polymerizable unsaturated group.
[0074] Examples of the acid group include a carboxyl group, a sulfonic acid group, and a phosphoric acid group.
[0075] Examples of the epoxy resin having an acid group and a polymerizable unsaturated group include epoxy (meth)acrylate resins having an acid group, which have as essential raw materials an epoxy resin, an unsaturated monobasic acid, and a polybasic acid anhydride; and epoxy (meth)acrylate resins having an acid group and a urethane group, which have as reaction raw materials an epoxy resin, an unsaturated monobasic acid, a polybasic acid anhydride, a polyisocyanate compound, and a (meth)acrylate compound having a hydroxyl group.
[0076] Examples of the epoxy resin include bisphenol type epoxy resin, phenylene ether type epoxy resin, naphthylene ether type epoxy resin, biphenyl type epoxy resin, triphenylmethane type epoxy resin, phenol novolac type epoxy resin, cresol novolac type epoxy resin, bisphenol novolac type epoxy resin, naphthol novolac type epoxy resin, naphthol-phenol co-condensed novolac type epoxy resin, naphthol-cresol co-condensed novolac type epoxy resin, phenol aralkyl type epoxy resin, naphthol aralkyl type epoxy resin, dicyclopentadiene-phenol addition reaction type epoxy resin, biphenyl aralkyl type epoxy resin, fluorene type epoxy resin, xanthene type epoxy resin, dihydroxybenzene type epoxy resin, trihydroxybenzene type epoxy resin, oxazolidone type epoxy resin, etc. These epoxy resins can be used alone or in combination of two or more.
[0077] Examples of the bisphenol type epoxy resin include bisphenol A type epoxy resin, bisphenol AP type epoxy resin, bisphenol B type epoxy resin, bisphenol BP type epoxy resin, bisphenol E type epoxy resin, bisphenol F type epoxy resin, and bisphenol S type epoxy resin.
[0078] Examples of the hydrogenated bisphenol type epoxy resin include hydrogenated bisphenol A type epoxy resin, hydrogenated bisphenol B type epoxy resin, hydrogenated bisphenol E type epoxy resin, hydrogenated bisphenol F type epoxy resin, and hydrogenated bisphenol S type epoxy resin.
[0079] Examples of the biphenol type epoxy resin include 4,4'-biphenol type epoxy resin, 2,2'-biphenol type epoxy resin, tetramethyl-4,4'-biphenol type epoxy resin, and tetramethyl-2,2'-biphenol type epoxy resin.
[0080] Examples of the hydrogenated biphenol type epoxy resin include hydrogenated 4,4'-biphenol type epoxy resin, hydrogenated 2,2'-biphenol type epoxy resin, hydrogenated tetramethyl-4,4'-biphenol type epoxy resin, and hydrogenated tetramethyl-2,2'-biphenol type epoxy resin.
[0081] As the unsaturated monobasic acid, the same as those exemplified as the above-mentioned unsaturated monobasic acid (B) can be used, and the unsaturated monobasic acids can be used alone or in combination of two or more kinds.
[0082] As the polybasic acid anhydride, the same as those exemplified as the polybasic acid anhydride (C) described above can be used, and the polybasic acid anhydrides can be used alone or in combination of two or more kinds.
[0083] Examples of the polyisocyanate compound include aliphatic diisocyanate compounds such as butane diisocyanate, hexamethylene diisocyanate, 2,2,4-trimethylhexamethylene diisocyanate, and 2,4,4-trimethylhexamethylene diisocyanate; alicyclic diisocyanate compounds such as norbornane diisocyanate, isophorone diisocyanate, hydrogenated xylylene diisocyanate, and hydrogenated diphenylmethane diisocyanate; tolylene diisocyanate, cyclohexane diisocyanate, and cyclohexane diisocyanate; Examples of the polyisocyanate include aromatic diisocyanate compounds such as silylene diisocyanate, tetramethylxylylene diisocyanate, diphenylmethane diisocyanate, 1,5-naphthalene diisocyanate, 4,4'-diisocyanato-3,3'-dimethylbiphenyl, and o-tolidine diisocyanate; polymethylene polyphenyl polyisocyanate having a repeating structure represented by the following structural formula (5); and isocyanurate-modified, biuret-modified, and allophanate-modified products thereof. These polyisocyanate compounds can be used alone or in combination of two or more.
[0084] [ka] [In the formula, R 1 R are each independently a hydrogen atom or a hydrocarbon group having 1 to 6 carbon atoms. 2 are each independently either an alkyl group having 1 to 4 carbon atoms or a bonding point connecting the structural portion represented by structural formula (5) via a methylene group marked with an *. l is 0 or an integer of 1 to 3, and m is an integer of 1 to 15.]
[0085] As the (meth)acrylate compound having a hydroxyl group, the same compounds as those exemplified as the (meth)acrylate compound having a hydroxyl group described above can be used, and the (meth)acrylate compound having a hydroxyl group can be used alone or in combination of two or more kinds.
[0086] The method for producing the epoxy resin having an acid group and a polymerizable unsaturated group is not particularly limited, and any method may be used. The production of the epoxy resin having an acid group and a polymerizable unsaturated group may be carried out in an organic solvent as necessary, and may also use a basic catalyst as necessary.
[0087] As the organic solvent, the same organic solvents as those exemplified above can be used, and the organic solvents can be used alone or in combination of two or more kinds.
[0088] As the basic catalyst, the same ones as those exemplified above as the basic catalyst can be used, and the basic catalysts can be used alone or in combination of two or more kinds.
[0089] Examples of the urethane resin having an acid group and a polymerizable unsaturated group include those obtained by reacting a polyisocyanate compound, a (meth)acrylate compound having a hydroxyl group, a polyol compound having a carboxyl group, and, if necessary, a polybasic acid anhydride, and a polyol compound other than the polyol compound having a carboxyl group; and those obtained by reacting a polyisocyanate compound, a (meth)acrylate compound having a hydroxyl group, a polybasic acid anhydride, and a polyol compound other than the polyol compound having a carboxyl group.
[0090] As the polyisocyanate compound, the same compounds as those exemplified above as the polyisocyanate compounds can be used, and the polyisocyanate compounds can be used alone or in combination of two or more kinds.
[0091] As the (meth)acrylate compound having a hydroxyl group, the same compounds as those exemplified as the (meth)acrylate compound having a hydroxyl group described above can be used, and the (meth)acrylate compound having a hydroxyl group can be used alone or in combination of two or more kinds.
[0092] Examples of the polyol compound having a carboxyl group include 2,2-dimethylolpropionic acid, 2,2-dimethylolbutanoic acid, 2,2-dimethylolvaleric acid, etc. The polyol compound having a carboxyl group can be used alone or in combination of two or more kinds.
[0093] As the polybasic acid anhydride, the same as those exemplified as the polybasic acid anhydride (C) described above can be used, and the polybasic acid anhydrides can be used alone or in combination of two or more kinds.
[0094] Examples of polyol compounds other than the polyol compounds having a carboxyl group include aliphatic polyol compounds such as ethylene glycol, propylene glycol, butanediol, hexanediol, glycerin, trimethylolpropane, ditrimethylolpropane, pentaerythritol, and dipentaerythritol; aromatic polyol compounds such as biphenol and bisphenol; (poly)oxyalkylene modified products in which (poly)oxyalkylene chains such as (poly)oxyethylene chains, (poly)oxypropylene chains, and (poly)oxytetramethylene chains are introduced into the molecular structure of the various polyol compounds; lactone modified products in which (poly)lactone structures are introduced into the molecular structure of the various polyol compounds. The polyol compounds other than the polyol compounds having a carboxyl group can be used alone or in combination of two or more kinds.
[0095] The method for producing the urethane resin having an acid group and a polymerizable unsaturated group is not particularly limited, and any method may be used. The production of the urethane resin having an acid group and a polymerizable unsaturated group may be carried out in an organic solvent as necessary, and may also use a basic catalyst as necessary.
[0096] As the organic solvent, the same organic solvents as those exemplified above can be used, and the organic solvents can be used alone or in combination of two or more kinds.
[0097] As the basic catalyst, the same ones as those exemplified above as the basic catalyst can be used, and the basic catalysts can be used alone or in combination of two or more kinds.
[0098] Examples of the acrylic resin having an acid group and a polymerizable unsaturated group include a reaction product obtained by polymerizing an acrylic resin intermediate obtained by polymerizing, as an essential component, a (meth)acrylate compound (α) having a reactive functional group such as a hydroxyl group, a carboxyl group, an isocyanate group, or a glycidyl group, and then reacting the resulting acrylic resin intermediate with a (meth)acrylate compound (β) having a reactive functional group capable of reacting with the functional group, thereby introducing a (meth)acryloyl group, and a reaction product obtained by reacting a polybasic acid anhydride with a hydroxyl group in the reaction product.
[0099] The acrylic resin intermediate may be a copolymer of the (meth)acrylate compound (α) and other compounds having a polymerizable unsaturated group as necessary. Examples of the compounds having a polymerizable unsaturated group include (meth)acrylic acid alkyl esters such as methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate; alicyclic structure-containing (meth)acrylates such as cyclohexyl (meth)acrylate, isobornyl (meth)acrylate, and dicyclopentanyl (meth)acrylate; aromatic ring-containing (meth)acrylates such as phenyl (meth)acrylate, benzyl (meth)acrylate, and phenoxyethyl acrylate; silyl group-containing (meth)acrylates such as 3-methacryloxypropyltrimethoxysilane; and styrene derivatives such as styrene, α-methylstyrene, and chlorostyrene. These compounds may be used alone or in combination of two or more.
[0100] The (meth)acrylate compound (β) is not particularly limited as long as it can react with the reactive functional group of the (meth)acrylate compound (α), but the following combinations are preferable from the viewpoint of reactivity. That is, when a (meth)acrylate having a hydroxyl group is used as the (meth)acrylate compound (α), it is preferable to use a (meth)acrylate having an isocyanate group as the (meth)acrylate compound (β). When a (meth)acrylate having a carboxyl group is used as the (meth)acrylate compound (α), it is preferable to use a (meth)acrylate having a glycidyl group as the (meth)acrylate compound (β). When a (meth)acrylate having an isocyanate group is used as the (meth)acrylate compound (α), it is preferable to use a (meth)acrylate having a hydroxyl group as the (meth)acrylate compound (β). When a (meth)acrylate having a glycidyl group is used as the (meth)acrylate compound (α), it is preferable to use a (meth)acrylate having a carboxyl group as the (meth)acrylate compound (β). The (meth)acrylate compound (β) can be used alone or in combination of two or more kinds.
[0101] The polybasic acid anhydride may be the same as those exemplified as the polybasic acid anhydride (C) described above. The polybasic acid anhydrides may be used alone or in combination of two or more kinds.
[0102] The method for producing the acrylic resin having an acid group and a polymerizable unsaturated group is not particularly limited, and any method may be used. The production of the acrylic resin having an acid group and a polymerizable unsaturated group may be carried out in an organic solvent as necessary, and may also use a basic catalyst as necessary.
[0103] As the organic solvent, the same organic solvents as those exemplified above can be used, and the organic solvents can be used alone or in combination of two or more kinds.
[0104] As the basic catalyst, the same ones as those exemplified above as the basic catalyst can be used, and the basic catalysts can be used alone or in combination of two or more kinds.
[0105] The amide-imide resin having an acid group and a polymerizable unsaturated group may be, for example, a product obtained by reacting an amide-imide resin having an acid group and / or an acid anhydride group with a (meth)acrylate compound having a hydroxyl group and / or a (meth)acrylate compound having an epoxy group, and, if necessary, a compound having one or more reactive functional groups selected from the group consisting of a hydroxyl group, a carboxyl group, an isocyanate group, a glycidyl group, and an acid anhydride group. The compound having a reactive functional group may or may not have a (meth)acryloyl group.
[0106] The amide-imide resin may have either an acid group or an acid anhydride group, or may have both. From the viewpoint of reactivity and reaction control with a (meth)acrylate compound having a hydroxyl group or an epoxy compound having a (meth)acryloyl group, it is preferable that the resin has an acid anhydride group, and it is more preferable that the resin has both an acid group and an acid anhydride group. The solid content acid value of the amide-imide resin is preferably in the range of 60 to 350 mgKOH / g under neutral conditions, i.e., conditions in which the acid anhydride group is not ring-opened. On the other hand, it is preferably in the range of 61 to 360 mgKOH / g under conditions in which the acid anhydride group is ring-opened, such as in the presence of water.
[0107] The amide-imide resin may be, for example, one obtained by reacting a polyisocyanate compound with a polybasic acid anhydride as raw materials.
[0108] As the polyisocyanate compound, the same compounds as those exemplified above as the polyisocyanate compounds can be used, and the polyisocyanate compounds can be used alone or in combination of two or more kinds.
[0109] As the polybasic acid anhydride, the same as those exemplified as the polybasic acid anhydride (C) described above can be used, and the polybasic acid anhydrides can be used alone or in combination of two or more kinds.
[0110] Furthermore, the amide-imide resin may contain, as necessary, a polybasic acid as a reaction raw material in addition to the polyisocyanate compound and the polybasic acid anhydride.
[0111] The polybasic acid may be any compound having two or more carboxyl groups in one molecule. For example, oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, maleic acid, fumaric acid, phthalic acid, isophthalic acid, terephthalic acid, tetrahydrophthalic acid, hexahydrophthalic acid, methylhexahydrophthalic acid, citraconic acid, itaconic acid, glutaconic acid, 1,2,3,4-butanetetracarboxylic acid, cyclohexanetricarboxylic acid, cyclohexanetetracarboxylic acid, bicyclo[2.2.1]heptane-2,3 -dicarboxylic acid, methylbicyclo[2.2.1]heptane-2,3-dicarboxylic acid, 4-(2,5-dioxotetrahydrofuran-3-yl)-1,2,3,4-tetrahydronaphthalene-1,2-dicarboxylic acid, trimellitic acid, pyromellitic acid, naphthalene dicarboxylic acid, naphthalene tricarboxylic acid, naphthalene tetracarboxylic acid, biphenyl dicarboxylic acid, biphenyl tricarboxylic acid, biphenyl tetracarboxylic acid, benzophenone tetracarboxylic acid, etc. In addition, as the polybasic acid, for example, a copolymer of a conjugated diene vinyl monomer and acrylonitrile, which has a carboxyl group in the molecule, can also be used. These polybasic acids can be used alone or in combination of two or more kinds.
[0112] As the (meth)acrylate compound having a hydroxyl group, the same compounds as those exemplified as the (meth)acrylate compound having a hydroxyl group described above can be used, and the (meth)acrylate compound having a hydroxyl group can be used alone or in combination of two or more kinds.
[0113] As the (meth)acrylate compound having an epoxy group, the same compounds as those exemplified as the (meth)acrylate compound having an epoxy group described above can be used, and the (meth)acrylate compound having an epoxy group can be used alone or in combination of two or more kinds.
[0114] The method for producing the amide-imide resin having an acid group and a polymerizable unsaturated group is not particularly limited, and any method may be used. The production of the amide-imide resin having an acid group and a polymerizable unsaturated group may be carried out in an organic solvent as necessary, and may also use a basic catalyst as necessary.
[0115] As the organic solvent, the same organic solvents as those exemplified above can be used, and the organic solvents can be used alone or in combination of two or more kinds.
[0116] As the basic catalyst, the same ones as those exemplified above as the basic catalyst can be used, and the basic catalysts can be used alone or in combination of two or more kinds.
[0117] Examples of the acrylamide resin having an acid group and a polymerizable unsaturated group include those obtained by reacting a compound having a phenolic hydroxyl group, an alkylene oxide or alkylene carbonate, an N-alkoxyalkyl (meth)acrylamide compound, a polybasic acid anhydride, and, if necessary, an unsaturated monobasic acid.
[0118] As the compound having a phenolic hydroxyl group, the same compounds as those exemplified as the compound (a1) having a phenolic hydroxyl group described above can be used, and the compound having a phenolic hydroxyl group can be used alone or in combination of two or more kinds.
[0119] Examples of the alkylene oxide include ethylene oxide, propylene oxide, butylene oxide, and pentylene oxide. Among these, ethylene oxide or propylene oxide is preferred because it provides a curable resin composition that has high photosensitivity and excellent alkaline developability and can form a cured product with excellent elongation and dielectric properties. The alkylene oxides can be used alone or in combination of two or more.
[0120] Examples of the alkylene carbonate include ethylene carbonate, propylene carbonate, butylene carbonate, and pentylene carbonate. Among these, ethylene carbonate or propylene carbonate is preferred because it can provide a curable resin composition that has high photosensitivity and excellent alkaline developability and can form a cured product with excellent elongation and dielectric properties. The alkylene carbonates can be used alone or in combination of two or more.
[0121] Examples of the N-alkoxyalkyl(meth)acrylamide compound include N-methoxymethyl(meth)acrylamide, N-ethoxymethyl(meth)acrylamide, N-butoxymethyl(meth)acrylamide, N-methoxyethyl(meth)acrylamide, N-ethoxyethyl(meth)acrylamide, N-butoxyethyl(meth)acrylamide, etc. The N-alkoxyalkyl(meth)acrylamide compound can be used alone or in combination of two or more kinds.
[0122] As the polybasic acid anhydride, the same as those exemplified as the polybasic acid anhydride (C) described above can be used, and the polybasic acid anhydrides can be used alone or in combination of two or more kinds.
[0123] As the unsaturated monobasic acid, the same as those exemplified above as the unsaturated monobasic acid (B) can be used, and the unsaturated monobasic acids can be used alone or in combination of two or more kinds.
[0124] The method for producing the acrylamide resin having an acid group and a polymerizable unsaturated group is not particularly limited, and any method may be used. The production of the acrylamide resin having an acid group and a polymerizable unsaturated group may be carried out in an organic solvent as necessary, and a basic catalyst and an acid catalyst may be used as necessary.
[0125] As the organic solvent, the same organic solvents as those exemplified above can be used, and the organic solvents can be used alone or in combination of two or more kinds.
[0126] As the basic catalyst, the same ones as those exemplified above as the basic catalyst can be used, and the basic catalysts can be used alone or in combination of two or more kinds.
[0127] As the acid catalyst, the same as those exemplified above as the acid catalyst can be used, and the acid catalyst can be used alone or in combination of two or more kinds.
[0128] Examples of the ester resin having an acid group and a polymerizable unsaturated group include those obtained by reacting a compound having a phenolic hydroxyl group with an alkylene oxide or alkylene carbonate, an unsaturated monobasic acid, and a polybasic acid anhydride.
[0129] As the compound having a phenolic hydroxyl group, the same compounds as those exemplified above as the compound having a phenolic hydroxyl group can be used, and the compound having a phenolic hydroxyl group can be used alone or in combination of two or more kinds.
[0130] The alkylene oxide may be the same as those exemplified above. Among these, ethylene oxide or propylene oxide is preferred because it can provide a curable resin composition having high photosensitivity and excellent alkaline developability, and capable of forming a cured product having excellent elongation and dielectric properties. The alkylene oxide may be used alone or in combination of two or more kinds.
[0131] The alkylene carbonate may be the same as the alkylene carbonate exemplified above. Among these, ethylene carbonate or propylene carbonate is preferred because it can obtain a curable resin composition having high photosensitivity and excellent alkaline developability, and capable of forming a cured product having excellent elongation and dielectric properties. The alkylene carbonate may be used alone or in combination of two or more kinds.
[0132] As the unsaturated monobasic acid, the same as those exemplified above as the unsaturated monobasic acid (B) can be used, and the unsaturated monobasic acids can be used alone or in combination of two or more kinds.
[0133] As the polybasic acid anhydride, the same as those exemplified as the polybasic acid anhydride (C) described above can be used, and the polybasic acid anhydrides can be used alone or in combination of two or more kinds.
[0134] The method for producing the ester resin having an acid group and a polymerizable unsaturated group is not particularly limited, and any method may be used. The production of the ester resin having an acid group and a polymerizable unsaturated group may be carried out in an organic solvent as necessary, and a basic catalyst and an acid catalyst may be used as necessary.
[0135] As the organic solvent, the same organic solvents as those exemplified above can be used, and the organic solvents can be used alone or in combination of two or more kinds.
[0136] As the basic catalyst, the same ones as those exemplified above as the basic catalyst can be used, and the basic catalysts can be used alone or in combination of two or more kinds.
[0137] As the acid catalyst, the same as those exemplified above as the acid catalyst can be used, and the acid catalyst can be used alone or in combination of two or more kinds.
[0138] The amount of the resin having an acid group and a polymerizable unsaturated group used is preferably within a range of 10 to 900 parts by mass per 100 parts by mass of the (meth)acrylate resin having an acid group of the present invention.
[0139] Examples of the various (meth)acrylate monomers include aliphatic mono(meth)acrylate compounds such as methyl(meth)acrylate, ethyl(meth)acrylate, propyl(meth)acrylate, butyl(meth)acrylate, pentyl(meth)acrylate, hexyl(meth)acrylate, 2-ethylhexyl(meth)acrylate, and octyl(meth)acrylate; and alicyclic mono(meth)acrylates such as cyclohexyl(meth)acrylate, isobornyl(meth)acrylate, and adamantyl mono(meth)acrylate. heterocyclic mono(meth)acrylate compounds such as glycidyl (meth)acrylate and tetrahydrofurfuryl acrylate; benzyl (meth)acrylate, phenyl (meth)acrylate, phenylbenzyl (meth)acrylate, phenoxy (meth)acrylate, phenoxyethyl (meth)acrylate, phenoxyethoxyethyl (meth)acrylate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, phenoxybenzyl (meth)acrylate, phenylphenoxyethyl (meth)acrylate, etc. Mono(meth)acrylate compounds such as the aromatic mono(meth)acrylate compounds of the above: (poly)oxyalkylene-modified mono(meth)acrylate compounds in which a polyoxyalkylene chain such as a (poly)oxyethylene chain, a (poly)oxypropylene chain, or a (poly)oxytetramethylene chain has been introduced into the molecular structure of the above-mentioned various mono(meth)acrylate monomers; lactone-modified mono(meth)acrylate compounds in which a (poly)lactone structure has been introduced into the molecular structure of the above-mentioned various mono(meth)acrylate compounds; ethylene glycol di(meth)acrylate, Aliphatic di(meth)acrylate compounds such as propylene glycol di(meth)acrylate, butanediol di(meth)acrylate, hexanediol di(meth)acrylate, and neopentyl glycol di(meth)acrylate; alicyclic di(meth)acrylate compounds such as 1,4-cyclohexanedimethanol di(meth)acrylate, norbornane di(meth)acrylate, norbornane dimethanol di(meth)acrylate, dicyclopentanyl di(meth)acrylate, and tricyclodecane dimethanol di(meth)acrylate;Aromatic di(meth)acrylate compounds such as biphenol di(meth)acrylate and bisphenol di(meth)acrylate; polyoxyalkylene-modified di(meth)acrylate compounds in which a (poly)oxyalkylene chain such as a (poly)oxyethylene chain, a (poly)oxypropylene chain, or a (poly)oxytetramethylene chain has been introduced into the molecular structure of the various di(meth)acrylate compounds; lactone-modified di(meth)acrylate compounds in which a (poly)lactone structure has been introduced into the molecular structure of the various di(meth)acrylate compounds; aliphatic tri(meth)acrylate compounds such as trimethylolpropane tri(meth)acrylate and glycerin tri(meth)acrylate; (poly)oxyalkylene chains in which a (poly)oxyethylene chain, a (poly)oxypropylene chain, or a (poly)oxytetramethylene chain has been introduced into the molecular structure of the aliphatic tri(meth)acrylate compounds Examples of the alkylene-modified tri(meth)acrylate compound include: a lactone-modified tri(meth)acrylate compound obtained by introducing a (poly)lactone structure into the molecular structure of the aliphatic tri(meth)acrylate compound; aliphatic poly(meth)acrylate compounds having 4 or more functional groups, such as pentaerythritol tetra(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, and dipentaerythritol hexa(meth)acrylate; aliphatic poly(meth)acrylate compounds having 4 or more functional groups, such as (poly)oxyalkylene chains, such as (poly)oxyethylene chains, (poly)oxypropylene chains, and (poly)oxytetramethylene chains, obtained by introducing a (poly)oxyalkylene chain into the molecular structure of the aliphatic poly(meth)acrylate compound; and a lactone-modified poly(meth)acrylate compound having 4 or more functional groups, such as (poly)lactone structure into the molecular structure of the aliphatic poly(meth)acrylate compound.
[0140] In addition to the above, the other (meth)acrylate monomers that can be used include (meth)acrylate monomers having a phenol compound, a cyclic carbonate compound or a cyclic ether compound, and an unsaturated monocarboxylic acid as essential reaction raw materials.
[0141] Examples of the phenol compound include cresol, xylenol, catechol, resorcinol, hydroquinone, 3-methylcatechol, 4-methylcatechol, 4-allylpyrocatechol, 1,2,3-trihydroxybenzene, 1,2,4-trihydroxybenzene, 1-naphthol, 2-naphthol, 1,3-naphthalenediol, 1,5-naphthalenediol, 2,6-naphthalenediol, 2,7-naphthalenediol, hydrogenated bisphenol, hydrogenated biphenol, polyphenylene ether type diol, polynaphthylene ether type diol, phenol novolac resin, cresol novolac resin, bisphenol novolac type resin, naphthol novolac type resin, phenol aralkyl type resin, naphthol aralkyl type resin, and cyclo ring structure-containing phenol resin.
[0142] Examples of the cyclic carbonate compound include ethylene carbonate, propylene carbonate, butylene carbonate, pentylene carbonate, etc. These cyclic carbonate compounds can be used alone or in combination of two or more kinds.
[0143] Examples of the cyclic ether compound include ethylene oxide, propylene oxide, tetrahydrofuran, etc. These cyclic ether compounds can be used alone or in combination of two or more kinds.
[0144] As the unsaturated monocarboxylic acid, the same as those exemplified above as the unsaturated monobasic acid (B) can be used.
[0145] The content of the other (meth)acrylate monomers in the curable resin composition of the present invention is preferably 90% by mass or less.
[0146] Furthermore, the curable resin composition of the present invention may contain various additives, such as a curing agent, a curing accelerator, an ultraviolet absorber, an organic solvent, an inorganic filler, polymer fine particles, a pigment, an antifoaming agent, a viscosity adjuster, a leveling agent, a flame retardant, and a storage stabilizer, as necessary.
[0147] Examples of the curing agent include epoxy resins, polybasic acids, unsaturated monobasic acids, amine compounds, amide compounds, azo compounds, organic peroxides, polyol compounds, and epoxy resins.
[0148] As the epoxy resin, the same ones as those exemplified above as the epoxy resin can be used, and the epoxy resins can be used alone or in combination of two or more kinds.
[0149] Examples of the polybasic acid include oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, maleic acid, fumaric acid, phthalic acid, isophthalic acid, terephthalic acid, tetrahydrophthalic acid, hexahydrophthalic acid, methylhexahydrophthalic acid, citraconic acid, itaconic acid, glutaconic acid, 1,2,3,4-butanetetracarboxylic acid, cyclohexanetricarboxylic acid, cyclohexanetetracarboxylic acid, and bicyclo[2.2.1]heptacarboxylic acid. Examples of the polybasic acid include 2,3-dicarboxylic acid, methylbicyclo[2.2.1]heptane-2,3-dicarboxylic acid, 4-(2,5-dioxotetrahydrofuran-3-yl)-1,2,3,4-tetrahydronaphthalene-1,2-dicarboxylic acid, trimellitic acid, pyromellitic acid, naphthalene dicarboxylic acid, naphthalene tricarboxylic acid, naphthalene tetracarboxylic acid, biphenyl dicarboxylic acid, biphenyl tricarboxylic acid, biphenyl tetracarboxylic acid, and benzophenone tetracarboxylic acid. In addition, examples of the polybasic acid include a copolymer of a conjugated diene vinyl monomer and acrylonitrile, which has a carboxyl group in the molecule. These polybasic acids can be used alone or in combination of two or more.
[0150] As the unsaturated monobasic acid, the same as those exemplified as the above-mentioned unsaturated monobasic acid (B) can be used, and the unsaturated monobasic acids can be used alone or in combination of two or more kinds.
[0151] Examples of the amine compound include diaminodiphenylmethane, diethylenetriamine, triethylenetetramine, diaminodiphenylsulfone, isophoronediamine, imidazole, BF3-amine complex, guanidine derivatives, etc. These amine compounds can be used alone or in combination of two or more kinds.
[0152] Examples of the amide-based compound include dicyandiamide, a polyamide resin synthesized from a dimer of linoleic acid and ethylenediamine, etc. These amide compounds can be used alone or in combination of two or more kinds.
[0153] Examples of the azo compound include azobisisobutyronitrile.
[0154] Examples of the organic peroxide include ketone peroxides, peroxyketals, hydroperoxides, dialkyl peroxides, diacyl peroxides, peroxy esters, peroxydicarbonates, alkyl peroxycarbonates, etc. These organic peroxides can be used alone or in combination of two or more kinds.
[0155] Examples of the polyol compound include polyol monomers such as ethylene glycol, diethylene glycol, propylene glycol, 1,3-propanediol, 1,4-butanediol, 1,3-butanediol, 3-methyl-1,3-butanediol, 1,5-pentanediol, neopentyl glycol, 1,6-hexanediol, glycerin, glycerin mono(meth)acrylate, trimethylolethane, trimethylolmethane mono(meth)acrylate, trimethylolpropane, trimethylolpropane mono(meth)acrylate, pentaerythritol mono(meth)acrylate, and pentaerythritol di(meth)acrylate; mixtures of the above polyol monomers with succinic acid, adipic acid, azelaic acid, sebacic acid, and the like. polyester polyols obtained by co-condensation of the polyol monomers with dicarboxylic acids such as terephthalic acid, isophthalic acid, orthophthalic acid, tetrahydrophthalic acid, hexahydrophthalic acid, maleic acid, fumaric acid, citraconic acid, itaconic acid, glutaconic acid, and 1,4-cyclohexanedicarboxylic acid; lactone-type polyester polyols obtained by polycondensation of the polyol monomers with various lactones such as ε-caprolactone, δ-valerolactone, and 3-methyl-δ-valerolactone; and polyether polyols obtained by ring-opening polymerization of the polyol monomers with cyclic ether compounds such as ethylene oxide, propylene oxide, tetrahydrofuran, ethyl glycidyl ether, and propyl glycidyl ether. These polyol compounds can be used alone or in combination of two or more.
[0156] As the epoxy resin, the same ones as those exemplified above as the epoxy resin can be used, and the epoxy resins can be used alone or in combination of two or more kinds.
[0157] The curing accelerator is one that accelerates the curing reaction, and examples thereof include phosphorus compounds, amine compounds, imidazole, organic acid metal salts, Lewis acids, and amine complex salts. These curing accelerators can be used alone or in combination of two or more. The amount of the curing accelerator added is preferably within a range of 0.01 to 10 mass % based on the solid content of the curable resin composition.
[0158] Examples of the ultraviolet absorbent include triazine derivatives such as 2-[4-{(2-hydroxy-3-dodecyloxypropyl)oxy}-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine and 2-[4-{(2-hydroxy-3-tridecyloxypropyl)oxy}-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine, 2-(2'-xanthenecarboxy-5'-methylphenyl)benzotriazole, 2-(2'-o-nitrobenzyloxy-5'-methylphenyl)benzotriazole, 2-xanthenecarboxy-4-dodecyloxybenzophenone, and 2-o-nitrobenzyloxy-4-dodecyloxybenzophenone. These ultraviolet absorbents can be used alone or in combination of two or more.
[0159] As the organic solvent, the same organic solvents as those exemplified above can be used, and the organic solvents can be used alone or in combination of two or more kinds.
[0160] Examples of the inorganic filler include fused silica, crystalline silica, alumina, silicon nitride, and aluminum hydroxide.
[0161] As the pigment, known and commonly used inorganic pigments and organic pigments can be used.
[0162] Examples of the inorganic pigment include white pigments, antimony red, red iron oxide, cadmium red, cadmium yellow, cobalt blue, Prussian blue, ultramarine blue, carbon black, graphite, etc. These inorganic pigments can be used alone or in combination of two or more kinds.
[0163] Examples of the white pigment include titanium oxide, zinc oxide, magnesium oxide, zirconium oxide, aluminum oxide, barium sulfate, silica, talc, mica, aluminum hydroxide, calcium silicate, aluminum silicate, hollow resin particles, and zinc sulfide.
[0164] Examples of the organic pigment include quinacridone pigments, quinacridonequinone pigments, dioxazine pigments, phthalocyanine pigments, anthrapyrimidine pigments, anthanthrone pigments, indanthrone pigments, flavanthrone pigments, perylene pigments, diketopyrrolopyrrole pigments, perinone pigments, quinophthalone pigments, anthraquinone pigments, thioindigo pigments, benzimidazolone pigments, azo pigments, etc. These organic pigments can be used alone or in combination of two or more kinds.
[0165] Examples of the flame retardant include inorganic phosphorus compounds such as red phosphorus, ammonium phosphates such as monoammonium phosphate, diammonium phosphate, triammonium phosphate, and ammonium polyphosphate, and phosphoric acid amides; phosphoric acid ester compounds, phosphonic acid compounds, phosphinic acid compounds, phosphine oxide compounds, phosphorane compounds, organic nitrogen-containing phosphorus compounds, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, 10-(2,5-dihydroxyphenyl)-10H-9-oxa-10-phosphaphenanthrene-10-oxy, and the like. Examples of suitable flame retardants include organic phosphorus compounds such as cyclic organic phosphorus compounds such as 10-(2,7-dihydroxynaphthyl)-10H-9-oxa-10-phosphaphenanthrene-10-oxide and derivatives thereof reacted with compounds such as epoxy resins and phenolic resins; nitrogen-based flame retardants such as triazine compounds, cyanuric acid compounds, isocyanuric acid compounds, and phenothiazine; silicone-based flame retardants such as silicone oils, silicone rubbers, and silicone resins; and inorganic flame retardants such as metal hydroxides, metal oxides, metal carbonate compounds, metal powders, boron compounds, and low-melting glass. These flame retardants can be used alone or in combination of two or more. When these flame retardants are used, the amount is preferably in the range of 0.1 to 20 mass% in the total resin composition.
[0166] The cured product of the present invention can be obtained by irradiating the curable resin composition with active energy rays. Examples of the active energy rays include ionizing radiation such as ultraviolet rays, electron beams, α rays, β rays, and γ rays. When ultraviolet rays are used as the active energy rays, irradiation may be performed under an inert gas atmosphere such as nitrogen gas, or under an air atmosphere in order to efficiently carry out a curing reaction by ultraviolet rays.
[0167] As a source of ultraviolet light, ultraviolet lamps are generally used from the viewpoints of practicality and economy, and specific examples include low-pressure mercury lamps, high-pressure mercury lamps, ultra-high-pressure mercury lamps, xenon lamps, gallium lamps, metal halide lamps, sunlight, LEDs, etc.
[0168] The cumulative amount of the active energy rays is not particularly limited, but is preferably 0.1 to 50 kJ / m 2 is preferably 0.5 to 10 kJ / m 2 It is more preferable that the integrated light amount is within the above range, since it is possible to prevent or suppress the occurrence of uncured portions.
[0169] The irradiation of the active energy rays may be carried out in one step or in two or more steps.
[0170] In addition, the cured product of the present invention has high photosensitivity, excellent alkaline developability, and excellent elongation and dielectric properties, and therefore can be suitably used, for example, in semiconductor device applications as solder resist, interlayer insulating material, packaging material, underfill material, package adhesive layer for circuit elements, and adhesive layer between integrated circuit elements and circuit boards. In addition, in thin display applications such as LCD and OELD, it can be suitably used as thin film transistor protective film, liquid crystal color filter protective film, pigment resist for color filter, resist for black matrix, spacer, and the like. Among these, it can be particularly suitably used for solder resist applications.
[0171] The resin material for a solder resist of the present invention comprises the above-mentioned curable resin composition.
[0172] The resist member of the present invention can be obtained, for example, by applying the solder resist resin material onto a substrate, evaporating and drying the organic solvent at a temperature range of about 60 to 100°C, exposing the substrate to active energy rays through a photomask having a desired pattern formed thereon, developing the unexposed areas with an alkaline aqueous solution, and further heating and curing the substrate at a temperature range of about 140 to 200°C.
[0173] Examples of the substrate include a metal-clad laminate of copper, aluminum, or the like. EXAMPLES
[0174] The present invention will be specifically described below with reference to examples and comparative examples, but the present invention is not limited to the examples given below.
[0175] (Synthesis Example 1: Production of Epoxy Resin (1)) 285 parts by mass of toluene, 220 parts by mass of resorcinol, and 2.2 parts by mass of paratoluenesulfonic acid were added to a flask equipped with a thermometer, a stirrer, and a reflux condenser, and the temperature was raised to 115°C under a nitrogen atmosphere. 208 parts by mass of 1,4-divinylbenzene were added dropwise over 2 hours, and the mixture was held at 115°C for 5 hours. 2.3 parts by mass of a 20% by mass aqueous sodium hydroxide solution were added, and the toluene was removed at 170°C to obtain a phenolic resin (1). The hydroxyl group equivalent of this phenolic resin (1) was 108 g / equivalent. The number of moles of 1,4-divinylbenzene corresponding to the aromatic compound (a2) defined in the present invention was 0.8 relative to 1 mole of resorcinol corresponding to the compound (a1) having a phenolic hydroxyl group defined in the present invention.
[0176] Next, 108 parts by mass of the phenolic resin (1) was dissolved in 462.5 parts by mass of epichlorohydrin in a flask equipped with a thermometer, a stirrer, a dropping funnel and a reflux condenser, and then 1,000 parts by mass of a 20% by mass aqueous sodium hydroxide solution was dropped at 80°C over 5 hours while stirring, and the reaction was continued for another hour. Next, the aqueous layer was discarded by a separation operation, and the excess epichlorohydrin present in the organic layer was recovered by distillation to obtain a reaction crude product. 250 parts by mass of methyl isobutyl ketone was added to the organic layer to dissolve the contents uniformly, and then the organic layer was washed with water. Next, water was removed from the organic layer by azeotropic distillation, and the precipitated insoluble matter was removed by filtration, and then the methyl isobutyl ketone was distilled off to obtain the desired epoxy resin (1). The epoxy equivalent of this epoxy resin (1) was 195 g / equivalent.
[0177] (Synthesis Example 2: Production of Epoxy Resin (2)) 233 parts by mass of toluene, 220 parts by mass of resorcinol, and 2.2 parts by mass of paratoluenesulfonic acid were added to a flask equipped with a thermometer, a stirrer, and a reflux condenser, and the temperature was raised to 115°C under a nitrogen atmosphere. 130 parts by mass of 1,4-divinylbenzene was added dropwise over 2 hours, and the mixture was held at 115°C for 3 hours. 2.3 parts by mass of a 20% by mass aqueous sodium hydroxide solution was added, and the toluene was removed at 170°C to obtain a phenolic resin (2). The hydroxyl group equivalent of this phenolic resin (2) was 90 g / equivalent. The number of moles of 1,4-divinylbenzene corresponding to the aromatic compound (a2) specified in the present invention was 0.5 relative to 1 mole of resorcinol corresponding to the compound (a1) having a phenolic hydroxyl group specified in the present invention.
[0178] Next, 90 parts by mass of the phenolic resin (2) was dissolved in 462.5 parts by mass of epichlorohydrin in a flask equipped with a thermometer, a stirrer, a dropping funnel and a reflux condenser, and then 1,000 parts by mass of a 20% by mass aqueous sodium hydroxide solution was dropped at 80°C over 5 hours while stirring, and the reaction was continued for another hour. Next, the aqueous layer was discarded by a separation operation, and the excess epichlorohydrin present in the organic layer was recovered by distillation to obtain a reaction crude product. 250 parts by mass of methyl isobutyl ketone was added to the organic layer to dissolve the contents uniformly, and then the organic layer was washed with water. Next, water was removed from the organic layer by azeotropic distillation, and the precipitated insoluble matter was removed by filtration, and then the methyl isobutyl ketone was distilled off to obtain the desired epoxy resin (2). The epoxy equivalent of this epoxy resin (2) was 178 g / equivalent.
[0179] (Synthesis Example 3: Production of Epoxy Resin (3)) In a flask equipped with a thermometer, a stirrer, and a reflux condenser, 199 parts by mass of toluene, 220 parts by mass of resorcinol, and 2.2 parts by mass of paratoluenesulfonic acid were added, and the mixture was heated to 115°C under a nitrogen atmosphere. 78 parts by mass of 1,4-divinylbenzene were added dropwise over 2 hours, and the mixture was held at 115°C for 3 hours. 2.3 parts by mass of a 20% by mass aqueous sodium hydroxide solution were added, and the toluene was removed at 170°C to obtain a phenolic resin (3). The hydroxyl group equivalent of this phenolic resin (3) was 79 g / equivalent. The number of moles of 1,4-divinylbenzene corresponding to the aromatic compound (a2) defined in the present invention was 0.3 relative to 1 mole of resorcinol corresponding to the compound (a1) having a phenolic hydroxyl group defined in the present invention.
[0180] Next, 79 parts by mass of the phenolic resin (3) was dissolved in 462.5 parts by mass of epichlorohydrin in a flask equipped with a thermometer, a stirrer, a dropping funnel and a reflux condenser, and then 1,000 parts by mass of a 20% by mass aqueous sodium hydroxide solution was dropped at 80°C over 5 hours while stirring, and the reaction was continued for another hour. Next, the aqueous layer was discarded by a separation operation, and the excess epichlorohydrin present in the organic layer was recovered by distillation to obtain a reaction crude product. 250 parts by mass of methyl isobutyl ketone was added to the organic layer to dissolve the contents uniformly, and then the organic layer was washed with water. Next, water was removed from the organic layer by azeotropic distillation, and the precipitated insoluble matter was removed by filtration, and then the methyl isobutyl ketone was distilled off to obtain the desired epoxy resin (3). The epoxy equivalent of this epoxy resin (3) was 164 g / equivalent.
[0181] (Synthesis Example 4: Production of Epoxy Resin (4)) In a flask equipped with a thermometer, a stirrer, and a reflux condenser, 181 parts by mass of toluene, 220 parts by mass of resorcinol, and 2.2 parts by mass of paratoluenesulfonic acid were added, and the mixture was heated to 115°C under a nitrogen atmosphere. 52 parts by mass of 1,4-divinylbenzene were added dropwise over 2 hours, and the mixture was held at 115°C for 3 hours. 2.3 parts by mass of a 20% by mass aqueous sodium hydroxide solution were added, and the toluene was removed at 170°C to obtain a phenolic resin (4). The hydroxyl group equivalent of this phenolic resin (4) was 72 g / equivalent. The number of moles of 1,4-divinylbenzene corresponding to the aromatic compound (a2) defined in the present invention was 0.2 relative to 1 mole of resorcinol corresponding to the compound (a1) having a phenolic hydroxyl group defined in the present invention.
[0182] Next, 72 parts by mass of the phenolic resin (4) was dissolved in 462.5 parts by mass of epichlorohydrin in a flask equipped with a thermometer, a stirrer, a dropping funnel and a reflux condenser, and then 1,000 parts by mass of a 20% by mass aqueous sodium hydroxide solution was dropped at 80°C over 5 hours while stirring, and the reaction was continued for another hour. Next, the aqueous layer was discarded by a separation operation, and the excess epichlorohydrin present in the organic layer was recovered by distillation to obtain a reaction crude product. 250 parts by mass of methyl isobutyl ketone was added to the organic layer to dissolve the contents uniformly, and then the organic layer was washed with water. Next, water was removed from the organic layer by azeotropic distillation, and the precipitated insoluble matter was removed by filtration, and then the methyl isobutyl ketone was distilled off to obtain the desired epoxy resin (4). The epoxy equivalent of this epoxy resin (4) was 158 g / equivalent.
[0183] (Synthesis Example 5: Production of Epoxy Resin (5)) A flask equipped with a thermometer, a stirrer, and a reflux condenser was charged with 320 parts by mass of toluene, 220 parts by mass of resorcinol, and 4.4 parts by mass of paratoluenesulfonic acid, and the temperature was raised to 115°C under a nitrogen atmosphere. 260 parts by mass of 1,4-divinylbenzene was added dropwise over 3 hours, and the mixture was held at 115°C for 7 hours. 4.6 parts by mass of a 20% by mass aqueous sodium hydroxide solution was added, and the toluene was removed at 170°C to obtain a phenolic resin (5). The hydroxyl group equivalent of this phenolic resin (5) was 131 g / equivalent. The number of moles of 1,4-divinylbenzene corresponding to the aromatic compound (a2) defined in the present invention was 1.0 relative to 1 mole of resorcinol corresponding to the compound (a1) having a phenolic hydroxyl group defined in the present invention.
[0184] Next, 131 parts by mass of the phenolic resin (5) was dissolved in 462.5 parts by mass of epichlorohydrin in a flask equipped with a thermometer, a stirrer, a dropping funnel and a reflux condenser, and then 1,000 parts by mass of a 20% by mass aqueous sodium hydroxide solution was dropped at 80°C over 5 hours while stirring, and the reaction was continued for another hour. Next, the aqueous layer was discarded by a separation operation, and the excess epichlorohydrin present in the organic layer was recovered by distillation to obtain a reaction crude product. 250 parts by mass of methyl isobutyl ketone was added to the organic layer to dissolve the contents uniformly, and then the organic layer was washed with water. Next, water was removed from the organic layer by azeotropic distillation, and the precipitated insoluble matter was removed by filtration, and then the methyl isobutyl ketone was distilled off to obtain the desired epoxy resin (5). The epoxy equivalent of this epoxy resin (5) was 219 g / equivalent.
[0185] (Synthesis Example 6: Production of epoxy resin (6)) 329 parts by mass of toluene, 220 parts by mass of resorcinol, and 4.4 parts by mass of paratoluenesulfonic acid were added to a flask equipped with a thermometer, a stirrer, and a reflux condenser, and the temperature was raised to 115°C under a nitrogen atmosphere. 273 parts by mass of 1,4-divinylbenzene were added dropwise over 3 hours, and the mixture was held at 115°C for 7 hours. 4.6 parts by mass of a 20% by mass aqueous sodium hydroxide solution were added, and the toluene was removed at 170°C to obtain a phenolic resin (6). The hydroxyl group equivalent of this phenolic resin (6) was 135 g / equivalent. The number of moles of 1,4-divinylbenzene corresponding to the aromatic compound (a2) defined in the present invention was 1.05 relative to 1 mole of resorcinol corresponding to the compound (a1) having a phenolic hydroxyl group defined in the present invention.
[0186] Next, 135 parts by mass of the phenolic resin (6) was dissolved in 462.5 parts by mass of epichlorohydrin in a flask equipped with a thermometer, a stirrer, a dropping funnel and a reflux condenser, and then 1,000 parts by mass of a 20% by mass aqueous sodium hydroxide solution was dropped at 80°C over 5 hours while stirring, and the reaction was continued for another hour. Next, the aqueous layer was discarded by a separation operation, and the excess epichlorohydrin present in the organic layer was recovered by distillation to obtain a reaction crude product. 250 parts by mass of methyl isobutyl ketone was added to the organic layer to dissolve the contents uniformly, and then the organic layer was washed with water. Next, water was removed from the organic layer by azeotropic distillation, and the precipitated insoluble matter was removed by filtration, and then the methyl isobutyl ketone was distilled off to obtain the desired epoxy resin (6). The epoxy equivalent of this epoxy resin (6) was 223 g / equivalent.
[0187] (Synthesis Example 7: Production of epoxy resin (7)) 283 parts by mass of toluene, 216 parts by mass of orthocresol, and 2.2 parts by mass of paratoluenesulfonic acid were added to a flask equipped with a thermometer, a stirrer, and a reflux condenser, and the temperature was raised to 115°C under a nitrogen atmosphere. 208 parts by mass of 1,4-divinylbenzene were added dropwise over 2 hours, and the mixture was held at 115°C for 5 hours. 2.3 parts by mass of a 20% by mass aqueous sodium hydroxide solution were added, and the toluene was removed at 170°C to obtain a phenolic resin (7). The hydroxyl group equivalent of this phenolic resin (7) was 219 g / equivalent. The number of moles of 1,4-divinylbenzene corresponding to the aromatic compound (a2) defined in the present invention was 0.8 relative to 1 mole of orthocresol corresponding to the compound (a1) having a phenolic hydroxyl group defined in the present invention.
[0188] Next, 219 parts by mass of the phenolic resin (7) was dissolved in 462.5 parts by mass of epichlorohydrin in a flask equipped with a thermometer, a stirrer, a dropping funnel and a reflux condenser, and then 1,000 parts by mass of a 20% by mass aqueous sodium hydroxide solution was dropped at 80°C over 5 hours while stirring, and the reaction was continued for another hour. Next, the aqueous layer was discarded by a separation operation, and the excess epichlorohydrin present in the organic layer was recovered by distillation to obtain a reaction crude product. 250 parts by mass of methyl isobutyl ketone was added to the organic layer to dissolve the contents uniformly, and then the organic layer was washed with water. Next, water was removed from the organic layer by azeotropic distillation, and the precipitated insoluble matter was removed by filtration, and then the methyl isobutyl ketone was distilled off to obtain the desired epoxy resin (7). The epoxy equivalent of this epoxy resin (7) was 300 g / equivalent.
[0189] (Synthesis Example 8: Production of epoxy resin (8)) In a flask equipped with a thermometer, a stirrer, and a reflux condenser, 300 parts by mass of toluene, 320 parts by mass of 1,6-dihydroxynaphthalene, and 3.2 parts by mass of paratoluenesulfonic acid were added, and the mixture was heated to 115°C under a nitrogen atmosphere. 130 parts by mass of 1,4-divinylbenzene was added dropwise over 2 hours, and the mixture was held at 115°C for 5 hours. 3.4 parts by mass of a 20% by mass aqueous sodium hydroxide solution was added, and the toluene was removed at 170°C to obtain a phenolic resin (8). The hydroxyl group equivalent of this phenolic resin (8) was 119 g / equivalent. The number of moles of 1,4-divinylbenzene corresponding to the aromatic compound (a2) defined in the present invention was 0.5 relative to 1 mole of 1,6-dihydroxynaphthalene corresponding to the compound (a1) having a phenolic hydroxyl group defined in the present invention.
[0190] Next, 119 parts by mass of the phenol resin (8) was dissolved in 462.5 parts by mass of epichlorohydrin in a flask equipped with a thermometer, a stirrer, a dropping funnel, and a reflux condenser, and then 1,000 parts by mass of a 20% by mass aqueous sodium hydroxide solution was dropped at 80°C over 5 hours while stirring, and the reaction was continued for another hour. Next, the aqueous layer was discarded by a separation operation, and the excess epichlorohydrin present in the organic layer was recovered by distillation to obtain a reaction crude product. 250 parts by mass of methyl isobutyl ketone was added to the organic layer to dissolve the contents uniformly, and then the organic layer was washed with water. Next, water was removed from the organic layer by azeotropic distillation, and the precipitated insoluble matter was removed by filtration, and then the methyl isobutyl ketone was distilled off to obtain the desired epoxy resin (8). The epoxy equivalent of this epoxy resin (8) was 206 g / equivalent.
[0191] (Synthesis Example 9: Production of epoxy resin (9)) 285 parts by mass of toluene, 220 parts by mass of catechol, and 2.2 parts by mass of paratoluenesulfonic acid were added to a flask equipped with a thermometer, a stirrer, and a reflux condenser, and the temperature was raised to 115°C under a nitrogen atmosphere. 208 parts by mass of 1,4-divinylbenzene were added dropwise over 2 hours, and the mixture was held at 115°C for 5 hours. 2.3 parts by mass of a 20% by mass aqueous sodium hydroxide solution were added, and the toluene was removed at 170°C to obtain a phenolic resin (9). The hydroxyl group equivalent of this phenolic resin (9) was 110 g / equivalent. The number of moles of 1,4-divinylbenzene corresponding to the aromatic compound (a2) defined in the present invention was 0.8 relative to 1 mole of catechol corresponding to the compound (a1) having a phenolic hydroxyl group defined in the present invention.
[0192] Next, 110 parts by mass of the phenol resin (9) was dissolved in 462.5 parts by mass of epichlorohydrin in a flask equipped with a thermometer, a stirrer, a dropping funnel, and a reflux condenser, and then 1,000 parts by mass of a 20% by mass aqueous sodium hydroxide solution was dropped at 80°C over 5 hours while stirring, and the reaction was continued for another hour. Next, the aqueous layer was discarded by a separation operation, and the excess epichlorohydrin present in the organic layer was recovered by distillation to obtain a reaction crude product. 250 parts by mass of methyl isobutyl ketone was added to the organic layer to dissolve the contents uniformly, and then the organic layer was washed with water. Next, water was removed from the organic layer by azeotropic distillation, and the precipitated insoluble matter was removed by filtration, and then the methyl isobutyl ketone was distilled off to obtain the desired epoxy resin (9). The epoxy equivalent of this epoxy resin (9) was 199 g / equivalent.
[0193] (Synthesis Example 10: Production of epoxy resin (10)) To a flask equipped with a thermometer, a stirrer, and a reflux condenser, 409 parts by mass of toluene, 220 parts by mass of resorcinol, and 4.4 parts by mass of paratoluenesulfonic acid were added, and the mixture was heated to 115°C under a nitrogen atmosphere. 394 parts by mass of diallyl phthalate were added dropwise over 3 hours, and the mixture was held at 115°C for 8 hours. 2.3 parts by mass of a 20% by mass aqueous sodium hydroxide solution were added, and the toluene was removed at 170°C to obtain a phenolic resin (10). The hydroxyl group equivalent of this phenolic resin (10) was 161 g / equivalent. The number of moles of diallyl phthalate corresponding to the aromatic compound (a2) defined in the present invention was 0.8 relative to 1 mole of resorcinol corresponding to the compound (a1) having a phenolic hydroxyl group defined in the present invention.
[0194] Next, 161 parts by mass of the phenol resin (10) was dissolved in 462.5 parts by mass of epichlorohydrin in a flask equipped with a thermometer, a stirrer, a dropping funnel, and a reflux condenser, and then 1,000 parts by mass of a 20% by mass aqueous sodium hydroxide solution was dropped at 80° C. over 5 hours while stirring, and the reaction was continued for another hour. Next, the aqueous layer was discarded by a separation operation, and the excess epichlorohydrin present in the organic layer was recovered by distillation to obtain a reaction crude product. 250 parts by mass of methyl isobutyl ketone was added to the organic layer to dissolve the contents uniformly, and then the organic layer was washed with water. Next, water was removed from the organic layer by azeotropic distillation, and the precipitated insoluble matter was removed by filtration, and then the methyl isobutyl ketone was distilled off to obtain the desired epoxy resin (10). The epoxy equivalent of this epoxy resin (10) was 249 g / equivalent.
[0195] (Synthesis Example 11: Production of epoxy resin (11)) A flask equipped with a thermometer, a stirrer, and a reflux condenser was charged with 315 parts by mass of toluene, 220 parts by mass of resorcinol, and 2.2 parts by mass of paratoluenesulfonic acid, and the temperature was raised to 115°C under a nitrogen atmosphere. 253 parts by mass of 1,4-diisopropenylbenzene was added dropwise over 2 hours, and the mixture was held at 115°C for 5 hours. 2.3 parts by mass of a 20% by mass aqueous sodium hydroxide solution was added, and the toluene was removed at 170°C to obtain a phenolic resin (11). The hydroxyl group equivalent of this phenolic resin (11) was 123 g / equivalent. The number of moles of 1,4-diisopropenylbenzene corresponding to the aromatic compound (a2) defined in the present invention was 0.8 relative to 1 mole of resorcinol corresponding to the compound (a1) having a phenolic hydroxyl group defined in the present invention.
[0196] Next, 123 parts by mass of the phenol resin (11) was dissolved in 462.5 parts by mass of epichlorohydrin in a flask equipped with a thermometer, a stirrer, a dropping funnel, and a reflux condenser, and then 1,000 parts by mass of a 20% by mass aqueous sodium hydroxide solution was dropped at 80° C. over 5 hours while stirring, and the reaction was continued for another hour. Next, the aqueous layer was discarded by a separation operation, and the excess epichlorohydrin present in the organic layer was recovered by distillation to obtain a reaction crude product. 250 parts by mass of methyl isobutyl ketone was added to the organic layer to dissolve the contents uniformly, and then the organic layer was washed with water. Next, water was removed from the organic layer by azeotropic distillation, and the precipitated insoluble matter was removed by filtration, and then the methyl isobutyl ketone was distilled off to obtain the desired epoxy resin (11). The epoxy equivalent of this epoxy resin (11) was 211 g / equivalent.
[0197] (Example 1: Preparation of acrylate resin (1) having acid groups) In a flask equipped with a thermometer, a stirrer, and a reflux condenser, 67 parts by mass of diethylene glycol monomethyl ether acetate was placed, 195 parts by mass of epoxy resin (1) was dissolved, 0.5 parts by mass of dibutylhydroxytoluene and 0.1 parts by mass of methoquinone were added, and then 72 parts by mass of acrylic acid and 1.4 parts by mass of triphenylphosphine were added, and an esterification reaction was carried out at 120°C for 8 hours while blowing in air. Then, 116 parts by mass of diethylene glycol monomethyl ether acetate and 71.4 parts by mass of tetrahydrophthalic anhydride were added and reacted at 110°C for 3 hours to obtain an acrylate resin (1) having an acid group. The non-volatile content of this acrylate resin (1) having an acid group was 65%, and the solid acid value was 80 mgKOH / g. The acid value was measured based on the neutralization titration method of JIS K 0070 (1992). Furthermore, the number of moles of acrylic acid per mole of epoxy groups in the epoxy resin (1) was 1, and the number of moles of tetrahydrophthalic anhydride per mole of epoxy groups in the epoxy resin (1) was 0.47.
[0198] (Example 2: Preparation of acrylate resin (2) having acid groups) In a flask equipped with a thermometer, a stirrer, and a reflux condenser, 63 parts by mass of diethylene glycol monomethyl ether acetate was placed, 178 parts by mass of epoxy resin (2) was dissolved, 0.5 parts by mass of dibutylhydroxytoluene and 0.1 parts by mass of methoquinone were added, and then 72 parts by mass of acrylic acid and 1.3 parts by mass of triphenylphosphine were added, and an esterification reaction was carried out for 8 hours at 120°C while blowing in air. Then, 108 parts by mass of diethylene glycol monomethyl ether acetate and 66.9 parts by mass of tetrahydrophthalic anhydride were added, and the reaction was carried out for 3 hours at 110°C, to obtain an acrylate resin (2) having an acid group. The non-volatile content of this acrylate resin (2) having an acid group was 65%, and the solid acid value was 80 mgKOH / g. Furthermore, the number of moles of acrylic acid per mole of epoxy groups in the epoxy resin (2) was 1, and the number of moles of tetrahydrophthalic anhydride per mole of epoxy groups in the epoxy resin (2) was 0.44.
[0199] (Example 3: Preparation of acrylate resin (3) having acid groups) In a flask equipped with a thermometer, a stirrer, and a reflux condenser, 59 parts by mass of diethylene glycol monomethyl ether acetate was placed, 164 parts by mass of epoxy resin (3) was dissolved, 0.5 parts by mass of dibutylhydroxytoluene and 0.1 parts by mass of methoquinone were added, and then 72 parts by mass of acrylic acid and 1.2 parts by mass of triphenylphosphine were added, and an esterification reaction was carried out at 120°C for 9 hours while blowing in air. Then, 103 parts by mass of diethylene glycol monomethyl ether acetate and 63.8 parts by mass of tetrahydrophthalic anhydride were added and reacted at 110°C for 3 hours to obtain an acrylate resin (3) having an acid group. The non-volatile content of this acrylate resin (3) having an acid group was 65%, and the solid acid value was 81 mgKOH / g. Furthermore, the number of moles of acrylic acid per mole of epoxy groups in the epoxy resin (3) was 1, and the number of moles of tetrahydrophthalic anhydride per mole of epoxy groups in the epoxy resin (3) was 0.42.
[0200] (Example 4: Preparation of acrylate resin (4) having acid groups) In a flask equipped with a thermometer, a stirrer, and a reflux condenser, 58 parts by mass of diethylene glycol monomethyl ether acetate was placed, 158 parts by mass of epoxy resin (4) was dissolved, 0.5 parts by mass of dibutylhydroxytoluene and 0.1 parts by mass of methoquinone were added, and then 72 parts by mass of acrylic acid and 1.2 parts by mass of triphenylphosphine were added, and an esterification reaction was carried out at 120°C for 10 hours while blowing in air. Then, 100 parts by mass of diethylene glycol monomethyl ether acetate and 62.3 parts by mass of tetrahydrophthalic anhydride were added, and the reaction was carried out at 110°C for 3 hours to obtain an acrylate resin (4) having an acid group. The non-volatile content of this acrylate resin (4) having an acid group was 65%, and the solid acid value was 81 mgKOH / g. Furthermore, the number of moles of acrylic acid per mole of epoxy groups in the epoxy resin (4) was 1, and the number of moles of tetrahydrophthalic anhydride per mole of epoxy groups in the epoxy resin (4) was 0.41.
[0201] (Example 5: Preparation of acrylate resin (5) having acid groups) In a flask equipped with a thermometer, a stirrer, and a reflux condenser, 73 parts by mass of diethylene glycol monomethyl ether acetate was placed, 219 parts by mass of epoxy resin (5) was dissolved, 0.6 parts by mass of dibutylhydroxytoluene and 0.1 parts by mass of methoquinone were added, and then 72 parts by mass of acrylic acid and 1.5 parts by mass of triphenylphosphine were added, and an esterification reaction was carried out at 120°C for 7 hours while blowing in air. Then, 126 parts by mass of diethylene glycol monomethyl ether acetate and 77.5 parts by mass of tetrahydrophthalic anhydride were added, and the reaction was carried out at 110°C for 3 hours to obtain an acrylate resin (5) having an acid group. The non-volatile content of this acrylate resin (5) having an acid group was 65%, and the solid acid value was 80 mgKOH / g. Furthermore, the number of moles of acrylic acid per mole of epoxy groups in the epoxy resin (5) was 1, and the number of moles of tetrahydrophthalic anhydride per mole of epoxy groups in the epoxy resin (5) was 0.51.
[0202] (Example 6: Preparation of acrylate resin (6) having acid groups) In a flask equipped with a thermometer, a stirrer, and a reflux condenser, 74 parts by mass of diethylene glycol monomethyl ether acetate was placed, 223 parts by mass of epoxy resin (6) was dissolved, 0.6 parts by mass of dibutylhydroxytoluene and 0.1 parts by mass of methoquinone were added, and then 72 parts by mass of acrylic acid and 1.5 parts by mass of triphenylphosphine were added, and an esterification reaction was carried out at 120°C for 7 hours while blowing in air. Then, 128 parts by mass of diethylene glycol monomethyl ether acetate and 79 parts by mass of tetrahydrophthalic anhydride were added and reacted at 110°C for 3 hours to obtain an acrylate resin (6) having an acid group. The non-volatile content of this acrylate resin (6) having an acid group was 65%, and the solid acid value was 81 mgKOH / g. In addition, the number of moles of acrylic acid per mole of epoxy groups in epoxy resin (6) was 1, and the number of moles of tetrahydrophthalic anhydride per mole of epoxy groups in epoxy resin (6) was 0.52.
[0203] (Example 7: Preparation of acrylate resin (7) having acid groups) In a flask equipped with a thermometer, a stirrer, and a reflux condenser, 93 parts by mass of diethylene glycol monomethyl ether acetate was placed, 300 parts by mass of epoxy resin (7) was dissolved, 0.7 parts by mass of dibutylhydroxytoluene and 0.2 parts by mass of methoquinone were added, and then 72 parts by mass of acrylic acid and 1.9 parts by mass of triphenylphosphine were added, and an esterification reaction was carried out at 120°C for 7 hours while blowing in air. Then, 161 parts by mass of diethylene glycol monomethyl ether acetate and 99 parts by mass of tetrahydrophthalic anhydride were added and reacted at 110°C for 3 hours to obtain an acrylate resin (7) having an acid group. The non-volatile content of this acrylate resin (7) having an acid group was 65%, and the solid acid value was 80 mgKOH / g. In addition, the number of moles of acrylic acid per mole of epoxy groups in the epoxy resin (7) was 1, and the number of moles of tetrahydrophthalic anhydride per mole of epoxy groups in the epoxy resin (7) was 0.65.
[0204] (Example 8: Preparation of acrylate resin (8) having acid groups) In a flask equipped with a thermometer, a stirrer, and a reflux condenser, 70 parts by mass of diethylene glycol monomethyl ether acetate was placed, 206 parts by mass of epoxy resin (8) was dissolved, 0.6 parts by mass of dibutylhydroxytoluene and 0.1 parts by mass of methoquinone were added, and then 72 parts by mass of acrylic acid and 1.4 parts by mass of triphenylphosphine were added, and an esterification reaction was carried out at 120°C for 7 hours while blowing in air. Then, 120 parts by mass of diethylene glycol monomethyl ether acetate and 74.5 parts by mass of tetrahydrophthalic anhydride were added and reacted at 110°C for 3 hours to obtain an acrylate resin (8) having an acid group. The non-volatile content of this acrylate resin (8) having an acid group was 65%, and the solid acid value was 80 mgKOH / g. Furthermore, the number of moles of acrylic acid per mole of epoxy groups in the epoxy resin (8) was 1, and the number of moles of tetrahydrophthalic anhydride per mole of epoxy groups in the epoxy resin (8) was 0.49.
[0205] (Example 9: Preparation of acrylate resin (9) having acid groups) In a flask equipped with a thermometer, a stirrer, and a reflux condenser, 68 parts by mass of diethylene glycol monomethyl ether acetate was placed, 199 parts by mass of epoxy resin (9) was dissolved, 0.5 parts by mass of dibutylhydroxytoluene and 0.1 parts by mass of methoquinone were added, and then 72 parts by mass of acrylic acid and 1.4 parts by mass of triphenylphosphine were added, and an esterification reaction was carried out at 120°C for 8 hours while blowing in air. Then, 118 parts by mass of diethylene glycol monomethyl ether acetate and 73 parts by mass of tetrahydrophthalic anhydride were added and reacted at 110°C for 3 hours to obtain an acrylate resin (9) having an acid group. The non-volatile content of this acrylate resin (9) having an acid group was 65%, and the solid acid value was 81 mgKOH / g. In addition, the number of moles of acrylic acid per mole of epoxy groups in epoxy resin (9) was 1, and the number of moles of tetrahydrophthalic anhydride per mole of epoxy groups in epoxy resin (9) was 0.48.
[0206] (Example 10: Preparation of acrylate resin (10) having acid groups) In a flask equipped with a thermometer, a stirrer, and a reflux condenser, 80 parts by mass of diethylene glycol monomethyl ether acetate was placed, 249 parts by mass of epoxy resin (10) was dissolved, 0.6 parts by mass of dibutylhydroxytoluene and 0.2 parts by mass of methoquinone were added, and then 72 parts by mass of acrylic acid and 1.6 parts by mass of triphenylphosphine were added, and an esterification reaction was carried out at 120°C for 7 hours while blowing in air. Then, 139 parts by mass of diethylene glycol monomethyl ether acetate and 86.6 parts by mass of tetrahydrophthalic anhydride were added, and the reaction was carried out at 110°C for 3 hours to obtain an acrylate resin (10) having an acid group. The non-volatile content of this acrylate resin (10) having an acid group was 65%, and the solid acid value was 81 mgKOH / g. Furthermore, the number of moles of acrylic acid per mole of epoxy groups in the epoxy resin (10) was 1, and the number of moles of tetrahydrophthalic anhydride per mole of epoxy groups in the epoxy resin (10) was 0.57.
[0207] (Example 11: Preparation of acrylate resin (11) having acid groups) In a flask equipped with a thermometer, a stirrer, and a reflux condenser, 71 parts by mass of diethylene glycol monomethyl ether acetate was placed, 211 parts by mass of epoxy resin (11) was dissolved, 0.6 parts by mass of dibutylhydroxytoluene and 0.1 parts by mass of methoquinone were added, and then 72 parts by mass of acrylic acid and 1.4 parts by mass of triphenylphosphine were added, and an esterification reaction was carried out for 8 hours at 120°C while blowing in air. Then, 123 parts by mass of diethylene glycol monomethyl ether acetate and 76 parts by mass of tetrahydrophthalic anhydride were added, and the reaction was carried out for 3 hours at 110°C, to obtain an acrylate resin (11) having an acid group. The non-volatile content of this acrylate resin (11) having an acid group was 65%, and the solid acid value was 80 mgKOH / g. Furthermore, the number of moles of acrylic acid per mole of epoxy groups in the epoxy resin (11) was 1, and the number of moles of tetrahydrophthalic anhydride per mole of epoxy groups in the epoxy resin (11) was 0.5.
[0208] (Example 12: Preparation of acrylate resin (12) having acid groups) In a flask equipped with a thermometer, a stirrer, and a reflux condenser, 65 parts by mass of diethylene glycol monomethyl ether acetate was placed, 195 parts by mass of epoxy resin (1) was dissolved, 0.5 parts by mass of dibutylhydroxytoluene and 0.1 parts by mass of methoquinone were added, and then 63.4 parts by mass of acrylic acid and 1.3 parts by mass of triphenylphosphine were added, and an esterification reaction was carried out at 100°C for 10 hours while blowing in air. Then, 119 parts by mass of diethylene glycol monomethyl ether acetate and 82 parts by mass of tetrahydrophthalic anhydride were added, and the reaction was carried out at 100°C for 3 hours to obtain an acrylate resin (12) having an acid group. The non-volatile content of this acrylate resin (12) having an acid group was 65%, and the solid acid value was 78 mgKOH / g. Furthermore, the number of moles of acrylic acid per mole of epoxy groups in the epoxy resin (1) was 0.89, and the number of moles of tetrahydrophthalic anhydride per mole of epoxy groups in the epoxy resin (1) was 0.54.
[0209] (Example 13: Preparation of acrylate resin (13) having acid groups) In a flask equipped with a thermometer, a stirrer, and a reflux condenser, 66 parts by mass of diethylene glycol monomethyl ether acetate was placed, 195 parts by mass of epoxy resin (1) was dissolved, 0.5 parts by mass of dibutylhydroxytoluene and 0.1 parts by mass of methoquinone were added, and then 68.4 parts by mass of acrylic acid and 1.3 parts by mass of triphenylphosphine were added, and an esterification reaction was carried out for 8 hours at 110°C while blowing in air. Then, 119 parts by mass of diethylene glycol monomethyl ether acetate and 79 parts by mass of tetrahydrophthalic anhydride were added, and the reaction was carried out for 3 hours at 100°C, to obtain an acrylate resin (13) having an acid group. The non-volatile content of this acrylate resin (13) having an acid group was 65%, and the solid acid value was 80 mgKOH / g. Furthermore, the number of moles of acrylic acid per mole of epoxy groups in the epoxy resin (1) was 0.95, and the number of moles of tetrahydrophthalic anhydride per mole of epoxy groups in the epoxy resin (1) was 0.52.
[0210] (Example 14: Preparation of acrylate resin (14) having acid groups) In a flask equipped with a thermometer, a stirrer, and a reflux condenser, 68 parts by mass of diethylene glycol monomethyl ether acetate was placed, 195 parts by mass of epoxy resin (1) was dissolved, 0.5 parts by mass of dibutylhydroxytoluene and 0.1 parts by mass of methoquinone were added, and then 75.6 parts by mass of acrylic acid and 1.4 parts by mass of triphenylphosphine were added, and an esterification reaction was carried out for 8 hours at 120°C while blowing in air. Then, 113 parts by mass of diethylene glycol monomethyl ether acetate and 65 parts by mass of tetrahydrophthalic anhydride were added, and the reaction was carried out for 3 hours at 110°C, to obtain an acrylate resin (14) having an acid group. The non-volatile content of this acrylate resin (14) having an acid group was 65%, and the solid acid value was 79 mgKOH / g. Furthermore, the number of moles of acrylic acid relative to 1 mole of epoxy groups in the epoxy resin (1) was 1.05, and the number of moles of tetrahydrophthalic anhydride relative to 1 mole of epoxy groups in the epoxy resin (1) was 0.43.
[0211] (Example 15: Preparation of acrylate resin (15) having acid groups) In a flask equipped with a thermometer, a stirrer, and a reflux condenser, 69 parts by mass of diethylene glycol monomethyl ether acetate was placed, 195 parts by mass of epoxy resin (1) was dissolved, 0.6 parts by mass of dibutylhydroxytoluene and 0.1 parts by mass of methoquinone were added, and then 79.9 parts by mass of acrylic acid and 1.4 parts by mass of triphenylphosphine were added, and an esterification reaction was carried out for 8 hours at 120°C while blowing in air. Then, 112 parts by mass of diethylene glycol monomethyl ether acetate and 61 parts by mass of tetrahydrophthalic anhydride were added, and the reaction was carried out for 3 hours at 110°C, to obtain an acrylate resin (15) having an acid group. The non-volatile content of this acrylate resin (15) having an acid group was 65%, and the solid acid value was 78 mgKOH / g. Furthermore, the number of moles of acrylic acid relative to 1 mole of epoxy groups in the epoxy resin (1) was 1.11, and the number of moles of tetrahydrophthalic anhydride relative to 1 mole of epoxy groups in the epoxy resin (1) was 0.4.
[0212] (Example 16: Preparation of acrylate resin (16) having acid groups) In a flask equipped with a thermometer, a stirrer, and a reflux condenser, 67 parts by mass of diethylene glycol monomethyl ether acetate was placed, 195 parts by mass of epoxy resin (1) was dissolved, 0.5 parts by mass of dibutylhydroxytoluene and 0.1 parts by mass of methoquinone were added, and then 72 parts by mass of acrylic acid and 1.3 parts by mass of triphenylphosphine were added, and an esterification reaction was carried out at 120°C for 8 hours while blowing in air. Then, 98 parts by mass of diethylene glycol monomethyl ether acetate and 39.5 parts by mass of tetrahydrophthalic anhydride were added, and the reaction was carried out at 110°C for 3 hours to obtain an acrylate resin (16) having an acid group. The non-volatile content of this acrylate resin (16) having an acid group was 65%, and the solid acid value was 50 mgKOH / g. Furthermore, the number of moles of acrylic acid per mole of epoxy groups in the epoxy resin (1) was 1, and the number of moles of tetrahydrophthalic anhydride per mole of epoxy groups in the epoxy resin (1) was 0.26.
[0213] (Example 17: Preparation of acrylate resin (17) having acid groups) In a flask equipped with a thermometer, a stirrer, and a reflux condenser, 67 parts by mass of diethylene glycol monomethyl ether acetate was placed, 195 parts by mass of epoxy resin (1) was dissolved, 0.5 parts by mass of dibutylhydroxytoluene and 0.1 parts by mass of methoquinone were added, and then 72 parts by mass of acrylic acid and 1.3 parts by mass of triphenylphosphine were added, and an esterification reaction was carried out at 120°C for 8 hours while blowing in air. Then, 96 parts by mass of diethylene glycol monomethyl ether acetate and 35 parts by mass of tetrahydrophthalic anhydride were added and reacted at 110°C for 3 hours to obtain an acrylate resin (17) having an acid group. The non-volatile content of this acrylate resin (17) having an acid group was 65%, and the solid acid value was 44 mgKOH / g. In addition, the number of moles of acrylic acid per mole of epoxy groups in epoxy resin (1) was 1, and the number of moles of tetrahydrophthalic anhydride per mole of epoxy groups in epoxy resin (1) was 0.23.
[0214] (Example 18: Preparation of acrylate resin (18) having acid groups) In a flask equipped with a thermometer, a stirrer, and a reflux condenser, 67 parts by mass of diethylene glycol monomethyl ether acetate was placed, 195 parts by mass of epoxy resin (1) was dissolved, 0.5 parts by mass of dibutylhydroxytoluene and 0.1 parts by mass of methoquinone were added, and then 72 parts by mass of acrylic acid and 1.3 parts by mass of triphenylphosphine were added, and an esterification reaction was carried out for 8 hours at 120°C while blowing in air. Then, 159 parts by mass of diethylene glycol monomethyl ether acetate and 152 parts by mass of tetrahydrophthalic anhydride were added, and the reaction was carried out for 5 hours at 110°C to obtain an acrylate resin (18) having an acid group. The non-volatile content of this acrylate resin (18) having an acid group was 65%, and the solid acid value was 137 mgKOH / g. Furthermore, the number of moles of acrylic acid was 1 relative to 1 mole of epoxy groups in the epoxy resin (1), and the number of moles of tetrahydrophthalic anhydride was 1 relative to 1 mole of epoxy groups in the epoxy resin (1).
[0215] (Example 19: Preparation of acrylate resin (19) having acid groups) In a flask equipped with a thermometer, a stirrer, and a reflux condenser, 67 parts by mass of diethylene glycol monomethyl ether acetate was placed, 195 parts by mass of epoxy resin (1) was dissolved, 0.5 parts by mass of dibutylhydroxytoluene and 0.1 parts by mass of methoquinone were added, and then 72 parts by mass of acrylic acid and 1.3 parts by mass of triphenylphosphine were added, and an esterification reaction was carried out for 8 hours at 120°C while blowing in air. Then, 161 parts by mass of diethylene glycol monomethyl ether acetate and 156.6 parts by mass of tetrahydrophthalic anhydride were added, and the reaction was carried out for 6 hours at 110°C, to obtain an acrylate resin (19) having an acid group. The non-volatile content of this acrylate resin (19) having an acid group was 65%, and the solid acid value was 141 mgKOH / g. Furthermore, the number of moles of acrylic acid per mole of epoxy groups in the epoxy resin (1) was 1, and the number of moles of tetrahydrophthalic anhydride per mole of epoxy groups in the epoxy resin (1) was 1.03.
[0216] (Example 20: Preparation of acrylate resin (20) having acid groups) In a flask equipped with a thermometer, a stirrer, and a reflux condenser, 67 parts by mass of diethylene glycol monomethyl ether acetate was placed, 195 parts by mass of epoxy resin (1) was dissolved, 0.5 parts by mass of dibutylhydroxytoluene and 0.1 parts by mass of methoquinone were added, and then 72 parts by mass of acrylic acid and 1.3 parts by mass of triphenylphosphine were added, and an esterification reaction was carried out at 120°C for 8 hours while blowing in air. Then, 100 parts by mass of diethylene glycol monomethyl ether acetate and 43 parts by mass of succinic anhydride were added and reacted at 110°C for 3 hours to obtain an acrylate resin (20) having an acid group. The non-volatile content of this acrylate resin (20) having an acid group was 65%, and the solid acid value was 80 mgKOH / g. In addition, the number of moles of acrylic acid per mole of epoxy groups in epoxy resin (1) was 1, and the number of moles of succinic anhydride per mole of epoxy groups in epoxy resin (1) was 0.43.
[0217] (Example 21: Preparation of acrylate resin (21) having acid groups) In a flask equipped with a thermometer, a stirrer, and a reflux condenser, 70 parts by mass of diethylene glycol monomethyl ether acetate was placed, 195 parts by mass of epoxy resin (1) was dissolved, 0.6 parts by mass of dibutylhydroxytoluene and 0.1 parts by mass of methoquinone were added, and then 86 parts by mass of methacrylic acid and 1.4 parts by mass of triphenylphosphine were added, and an esterification reaction was carried out at 120°C for 7 hours while blowing in air. Then, 122 parts by mass of diethylene glycol monomethyl ether acetate and 76 parts by mass of tetrahydrophthalic anhydride were added, and the reaction was carried out at 110°C for 3 hours to obtain an acrylate resin (21) having an acid group. The non-volatile content of this acrylate resin (21) having an acid group was 65%, and the solid acid value was 81 mgKOH / g. Furthermore, the number of moles of methacrylic acid per mole of epoxy groups in the epoxy resin (1) was 1, and the number of moles of tetrahydrophthalic anhydride per mole of epoxy groups in the epoxy resin (1) was 0.5.
[0218] (Comparative Example 1: Preparation of Acrylate Resin (R1) Having Acid Groups) In a flask equipped with a thermometer, a stirrer, and a reflux condenser, 101 parts by mass of diethylene glycol monomethyl ether acetate was placed, and 428 parts by mass of orthocresol novolac epoxy resin (DIC Corporation's "EPICLON N-680", epoxy equivalent: 214g / eq) was dissolved. After adding 4 parts by mass of dibutylhydroxytoluene and 0.4 parts by mass of methoquinone, 144 parts by mass of acrylic acid and 1.6 parts by mass of triphenylphosphine were added, and an esterification reaction was carried out at 120°C for 10 hours while blowing in air. Thereafter, 311 parts by mass of diethylene glycol monomethyl ether acetate and 160 parts by mass of tetrahydrophthalic anhydride were added and reacted at 110°C for 2.5 hours to obtain an acrylate resin (R1) having an acid group. The solid acid value of this acrylate resin (R1) having an acid group was 85mgKOH / g.
[0219] (Example 22: Preparation of curable resin composition (1)) 100 parts by mass of the acrylate resin (1) having an acid group and a non-volatile content of 65% by mass obtained in Example 1, 26.2 parts by mass of an orthocresol novolac type epoxy resin (EPICLON N-680 manufactured by DIC Corporation, epoxy equivalent: 214) as a curing agent, 14.1 parts by mass of diethylene glycol monoethyl ether acetate, 3.5 parts by mass of a photopolymerization initiator (Omnirad 907 manufactured by IGM Resins), 7.0 parts by mass of dipentaerythritol hexaacrylate, 0.5 parts by mass of 2-ethyl-4-methyl-imidazole, and 0.7 parts by mass of phthalocyanine green were mixed to obtain a curable resin composition (1).
[0220] (Examples 23 to 43: Preparation of curable resin compositions (2) to (22)) Curable resin compositions (2) to (22) were obtained in the same manner as in Example 22, except that the acrylate resins (2) to (21) having an acid group and a non-volatile content of 65 mass% obtained in Examples 2 to 21 were used in place of the acrylate resin (1) having an acid group used in Example 22 in the blending amounts shown in Tables 1 and 2.
[0221] (Comparative Example 2: Preparation of curable resin composition (R1)) 100 parts by mass of the acrylate resin (R1) having an acid group and a non-volatile content of 65% by mass obtained in Comparative Example 1, 24.9 parts by mass of an orthocresol novolac epoxy resin (EPICLON N-680 manufactured by DIC Corporation, epoxy equivalent: 214) as a curing agent, 13.4 parts by mass of diethylene glycol monoethyl ether acetate, 3.2 parts by mass of a photopolymerization initiator (Omnirad 907 manufactured by IGM Resins), 6.4 parts by mass of dipentaerythritol hexaacrylate, 0.5 parts by mass of 2-ethyl-4-methyl-imidazole, and 0.7 parts by mass of phthalocyanine green were mixed to obtain a curable resin composition (R1).
[0222] The curable resin compositions (1) to (22) and (R1) obtained in the above Examples and Comparative Examples were used to carry out the following evaluations.
[0223] [Method of evaluating light sensitivity] The curable resin composition obtained in each of the Examples and Comparative Examples was applied to a glass substrate using an applicator to a film thickness of 50 μm, and then dried at 80° C. for 30 minutes. Then, the composition was exposed to 10 kJ / m 2 of a metal halide lamp through a Kodak Step Tablet No. 2. 2 This was developed for 180 seconds with a 1% by weight aqueous solution of sodium carbonate, and the number of remaining steps was evaluated according to the following criteria. Note that the greater the number of remaining steps, the higher the photosensitivity.
[0224] A: The number of remaining steps was 11 or more. B: The number of remaining steps was 9 or more but less than 11 steps. C: The number of remaining steps was 7 or more but less than 9 steps. D: The number of remaining steps was 6 or more but less than 7 steps. E: Fewer than 6 steps remained.
[0225] [Method for evaluating alkaline developability] The curable resin composition obtained in each Example and Comparative Example was applied to a glass substrate using an applicator to a film thickness of 50 μm, and then dried at 80° C. for 40 minutes, 50 minutes, 60 minutes, 70 minutes, 80 minutes, 90 minutes, 100 minutes, and 110 minutes, respectively, to prepare samples with different drying times. These were developed with a 1% aqueous sodium carbonate solution at 30° C. for 180 seconds, and the drying time at 80° C. of the samples that did not leave any residue on the substrate was evaluated according to the following criteria as the drying control width. Note that a longer drying control width indicates better alkaline developability.
[0226] A: The drying control range was 90 minutes or more. B: The drying control range was between 70 minutes and 90 minutes. C: The drying control range was 50 minutes or more and less than 70 minutes. D: The drying control range was 40 minutes or more and less than 50 minutes. E: The drying control window was less than 40 minutes.
[0227] The compositions and evaluation results of the curable resin compositions (1) to (22) prepared in Examples 22 to 43 and the curable resin composition (R1) prepared in Comparative Example 2 are shown in Tables 1 and 2.
[0228] [Table 1]
[0229] [Table 2]
[0230] (Example 44: Preparation of curable resin composition (23)) 100 parts by mass of the acrylate resin (1) having an acid group obtained in Example 1, 26.2 parts by mass of an orthocresol novolac epoxy resin (EPICLON N-680 manufactured by DIC Corporation, epoxy equivalent: 214) as a curing agent, 14.1 parts by mass of diethylene glycol monoethyl ether acetate, and 3.5 parts by mass of a photopolymerization initiator (Omnirad 907 manufactured by IGM Resins) were mixed to obtain a curable resin composition (23).
[0231] (Examples 45 to 65: Preparation of curable resin compositions (24) to (44)) Curable resin compositions (24) to (44) were obtained in the same manner as in Example 44, except that the acrylate resins (2) to (21) having an acid group obtained in Examples 2 to 21 were used in place of the acrylate resin (1) having an acid group used in Example 44 in the blending amounts shown in Tables 3 and 4.
[0232] (Comparative Example 3: Preparation of curable resin composition (R2)) 100 parts by mass of the acrylate resin (R1) having an acid group obtained in Comparative Example 1, 24.9 parts by mass of an orthocresol novolac epoxy resin (EPICLON N-680 manufactured by DIC Corporation, epoxy equivalent: 214) as a curing agent, 13.4 parts by mass of diethylene glycol monoethyl ether acetate, and 3.2 parts by mass of a photopolymerization initiator (Omnirad 907 manufactured by IGM Resins) were mixed to obtain a curable resin composition (R2).
[0233] The following evaluations were carried out using the curable resin compositions (23) to (44), and (R2) obtained in the above Examples and Comparative Examples.
[0234] [Method of measuring elongation] The elongation was measured based on a tensile test. <Preparation of test piece 1> The curable resin compositions obtained in the Examples and Comparative Examples were applied onto a copper foil (electrolytic copper foil "F2-WS" 18 μm, manufactured by Furukawa Sangyo Co., Ltd.) using a 50 μm applicator, and then heated at 10 kJ / m using a metal halide lamp. 2 After being irradiated with ultraviolet light, the cured product was heated for 1 hour at 160° C. The cured product was peeled off from the copper foil to obtain a test piece 1 (cured product).
[0235] <Tensile test> The test piece 1 was cut into a size of 10 mm x 80 mm, and a tensile test was performed on the test piece 1 under the following measurement conditions using a precision universal testing machine "Autograph AG-IS" manufactured by Shimadzu Corporation. The elongation (%) until the test piece broke was measured and evaluated according to the following criteria.
[0236] Measurement conditions: temperature 23℃, humidity 50%, distance between gauge lines 20mm, distance between supports 20mm, tensile speed 10mm / min
[0237] A: The elongation was 3.9% or more. B: The elongation was 3.6% or more and less than 3.9%. C: The elongation was 3.3% or more and less than 3.6%. D: The elongation was 3.0% or more and less than 3.3%. E: The elongation was less than 3.0%.
[0238] [Method of measuring dielectric constant] The curable resin composition obtained in each of the Examples and Comparative Examples was applied to a glass substrate using an applicator to a thickness of 50 μm, and dried at 80° C. for 30 minutes. Then, a metal halide lamp was used to apply a 10 kJ / m 2 After irradiating the sample with ultraviolet rays, the sample was heated at 160°C for 1 hour to obtain a cured coating film. The cured coating film was then peeled off from the glass substrate to obtain a cured product. The sample was then stored for 24 hours in a room at a temperature of 23°C and a humidity of 50% to obtain a test piece. The dielectric constant of the test piece at 1GHz was measured by the cavity resonance method using a Network Analyzer E8362C manufactured by Agilent Technologies, Inc., and evaluated according to the following criteria.
[0239] A: The dielectric constant was 2.3% or less. B: The dielectric constant was more than 2.3% and was 2.44 or less. C: The dielectric constant was more than 2.44% and not more than 2.58%. D: The dielectric constant was more than 2.58% and 2.72% or less. E: The dielectric constant was greater than 2.72%.
[0240] [Method of measuring dielectric tangent] The curable resin composition obtained in each of the Examples and Comparative Examples was applied to a glass substrate using an applicator to a thickness of 50 μm, and dried at 80° C. for 30 minutes. Then, a metal halide lamp was used to apply a 10 kJ / m 2 After irradiating the sample with ultraviolet rays, the sample was heated at 160°C for 1 hour to obtain a cured coating film. The cured coating film was then peeled off from the glass substrate to obtain a cured product. The sample was then stored for 24 hours in a room at a temperature of 23°C and a humidity of 50% to obtain a test piece. The dielectric loss tangent of the test piece at 1GHz was measured by the cavity resonance method using a Network Analyzer E8362C manufactured by Agilent Technologies, Inc., and evaluated according to the following criteria.
[0241] A: The dielectric tangent was 0.02 or less. B: The dielectric tangent was greater than 0.02 and not more than 0.022. C: The dielectric tangent was greater than 0.022 and not greater than 0.024. D: The dielectric tangent was greater than 0.024 and not more than 0.026. E: The dielectric tangent was more than 0.026.
[0242] Table 2 shows the compositions and evaluation results of the curable resin compositions (3) and (4) prepared in Examples 5 and 6, and the curable resin composition (R2) prepared in Comparative Example 3.
[0243] [Table 3]
[0244] [Table 4]
[0245] In addition, the parts by mass of the acrylate resin having an acid group in Tables 1 to 4 are solid content values.
[0246] "Curing agent" in Tables 1 and 2 refers to an orthocresol novolac type epoxy resin ("EPICLON N-680" manufactured by DIC Corporation).
[0247] "Organic solvent" in Tables 1 and 2 refers to diethylene glycol monomethyl ether acetate.
[0248] "Photopolymerization initiator" in Tables 1 and 2 refers to "Omnirad 907" manufactured by IGM Resins.
[0249] Examples 22 to 43 shown in Tables 1 and 2 are examples of curable resin compositions using the acrylate resin having an acid group of the present invention. It was confirmed that the cured products of these curable resin compositions had high sensitivity and excellent alkaline developability.
[0250] Examples 44 to 65 shown in Tables 3 and 4 are examples of curable resin compositions using the acrylate resin having an acid group of the present invention. It was confirmed that the cured products of these curable resin compositions had excellent elongation and dielectric properties.
[0251] On the other hand, Comparative Example 2 is an example of a curable resin composition containing a (meth)acrylate resin having an acid group, which uses an epoxy resin that does not use an aromatic compound (a2) having at least two ethylenically unsaturated bonds as a raw material. It was confirmed that this curable resin composition was insufficient in both photosensitivity and alkaline developability.
[0252] Comparative Example 3 is an example of a curable resin composition containing a (meth)acrylate resin having an acid group, which uses an epoxy resin that does not use an aromatic compound (a2) having at least two ethylenically unsaturated bonds as a raw material, similar to Comparative Example 2. It was confirmed that this curable resin composition has insufficient elongation, a high dielectric constant, and insufficient dielectric properties.
Claims
1. An epoxy resin (A), An unsaturated monobasic acid (B); A (meth)acrylate resin having an acid group, the (meth)acrylate resin being made of a polybasic acid anhydride (C) as an essential raw material. hand, The epoxy resin (A) is produced using, as essential raw materials, a compound (a1) having a phenolic hydroxyl group, an aromatic compound (a2) having at least two ethylenically unsaturated bonds, and an epihalohydrin (a3), the aromatic compound (a2) is divinylbenzene and / or diisopropenylbenzene, The (meth)acrylate resin having an acid group, wherein the number of moles of the aromatic compound (a2) is within a range of 0.25 to 1 mole per mole of the compound (a1) having a phenolic hydroxyl group.
2. The (meth)acrylate resin having an acid group according to claim 1, wherein the amount of the unsaturated monobasic acid (B) used is in the range of 0.9 to 1.1 mol based on the acid group of the unsaturated monobasic acid (B) per 1 mol of the epoxy group of the epoxy resin (A).
3. 3. The (meth)acrylate resin having an acid group according to claim 1, wherein the amount of the polybasic acid anhydride (C) used is in the range of 0.45 to 1 mol per 1 mol of the epoxy group contained in the epoxy resin (A).
4. A curable resin composition comprising the (meth)acrylate resin having an acid group according to any one of claims 1 to 3 and a photopolymerization initiator.
5. The curable resin composition according to claim 4, further comprising a resin having an acid group and a polymerizable unsaturated group other than the (meth)acrylate resin having an acid group.
6. A cured product of the curable resin composition according to claim 4 or 5.
7. An insulating material comprising the cured product according to claim 6.
8. A resist member comprising the cured product according to claim 6.
Citation Information
Patent Citations
Active energy ray-curable epoxy acrylate resin composition
JP1996259663A
Epoxy resin, resin composition containing the same and photosensitive resin composition containing the resin composition
JP2004359879A