Dispersion liquid, ink composition for ink-jet recording, and dispersion resin
A dispersion resin with specific structural units addresses the redispersibility issue in ink compositions, ensuring stable particle size and viscosity, thus enhancing inkjet recording performance.
Patent Information
- Application Number
- JP2020192510
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-11-19
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2040-11-19
AI Technical Summary
Conventional ink compositions using styrene-acrylic resins face difficulties in redispersing coloring materials after they solidify, leading to issues such as clogging and instability in inkjet recording processes, especially when stored at high temperatures.
A dispersion resin with specific structural units A, B, and C, and optionally D, is used to improve redispersibility, comprising a copolymer with monomers like N-methanesulfonic acid maleimide and styrene, which enhances the stability of coloring materials even at high temperatures.
The dispersion resin effectively maintains stable particle size and viscosity, preventing clogging and improving ink ejection stability, allowing easy redispersement of solidified coloring materials.
Smart Images

Figure 0007567391000001 
Figure 0007567391000002 
Figure 0007567391000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a dispersion liquid, an ink composition for ink-jet recording, and a dispersion resin. [Background technology]
[0002] The ink-jet recording method is capable of recording high-definition images using a relatively simple device, and has been rapidly developed in various fields. In the process, various studies have been conducted on the dispersibility of coloring materials in ink.
[0003] One method for improving the dispersibility of a colorant is to use a dispersant. For example, Patent Document 1 discloses an ink that uses a styrene-acrylic acid resin and / or a styrene-maleic acid resin as a dispersant. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2015-048437 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, ink compositions containing conventional dispersants such as the styrene-acrylic resin described in Patent Document 1 have the problem that once the ink dries and the colorant solidifies, it is difficult to redisperse the ink, and problems tend to occur when the ink is re-ejected after drying. [Means for solving the problem]
[0006] The present invention provides a dispersion liquid that includes water, a colorant, and a dispersion resin that disperses the colorant, the dispersion resin having a structural unit A represented by the following formula (1), a structural unit B represented by any one of the following formulas (2-1) to (2-2), and a structural unit C represented by any one of the following formulas (3-1) to (3-4). [ka] (In the formula, R 1 each independently represents a divalent organic group having 1 to 20 carbon atoms; R 2 each independently represents a sulfo group or a salt thereof. [ka] (In the formula, R 3 each independently represents a monovalent organic group having 1 to 20 carbon atoms; R 4 each independently represents a divalent organic group having 1 to 12 carbon atoms; R 5 each independently represents an organic group having 1 to 12 carbon atoms. [ka] (In the formula, R 6 each independently represents a hydrogen atom, an alkyl group having 1 to 12 carbon atoms, or an alkoxy group having 1 to 12 carbon atoms.
[0007] The present invention also provides an ink composition for ink jet recording, comprising the above dispersion, a surfactant, and a water-soluble organic solvent.
[0008] Furthermore, the present invention relates to a dispersion resin having a structural unit A represented by the above formula (1), a structural unit B represented by any one of the above formulas (2-1) to (2-2), and a structural unit C represented by any one of the above formulas (3-1) to (3-4). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Below, we will explain in detail the embodiment of the present invention (hereinafter referred to as the "present embodiment"). However, the present invention is not limited to this embodiment, and various modifications are possible without departing from the gist of the present invention.
[0010] 1.Dispersion liquid The dispersion liquid of the present embodiment contains water, a colorant, and a dispersion resin that disperses the colorant. The dispersion resin has a structural unit A represented by the following formula (1), a structural unit B represented by any one of the following formulas (2-1) to (2-2), and a structural unit C represented by any one of the following formulas (3-1) to (3-4). [ka] (In the formula, R 1 each independently represents a divalent organic group having 1 to 20 carbon atoms; R 2 each independently represents a sulfo group or a salt thereof. [ka] (In the formula, R 3 each independently represents a monovalent organic group having 1 to 20 carbon atoms; R 4 each independently represents a divalent organic group having 1 to 12 carbon atoms; R 5 each independently represents an organic group having 1 to 12 carbon atoms. [ka] (In the formula, R 6 each independently represents a hydrogen atom, an alkyl group having 1 to 12 carbon atoms, or an alkoxy group having 1 to 12 carbon atoms.
[0011] A dispersion liquid or ink composition using a conventional dispersion resin has a problem that once the colorant solidifies, it is difficult to redisperse it. In contrast, in the present embodiment, by using a dispersion resin having the above-mentioned configuration, it is possible to easily redisperse the solidified colorant, and even when stored at high temperatures, there is little change in the particle size of the colorant particles or in the viscosity of the dispersion liquid, which makes it possible to prevent clogging and further improve the ejection stability of the ink composition for inkjet recording using the dispersion liquid. Each component will be described in detail below.
[0012] 1.1.Dispersion resin The dispersion resin has a structural unit A represented by the above formula (1), a structural unit B represented by any one of the above formulas (2-1) to (2-2), and a structural unit C represented by any one of the above formulas (3-1) to (3-4), and may have a structural unit D described below, as necessary. In this embodiment, the term "structural unit" refers to a repeating unit that constitutes a part of the dispersion resin after polymerization, and the term "monomer" refers to a monomer having a polymerizable unsaturated bond before polymerization.
[0013] The dispersion resin may be a random copolymer, a block copolymer, or a graft copolymer. Examples of the block copolymer include a triblock copolymer having a block A composed of a structural unit A, a block B composed of a structural unit B, and a block C composed of a structural unit C, as well as a diblock copolymer having a block A composed of a structural unit A and a random block B / C composed of a structural unit B and a structural unit C. Examples of the graft copolymer include a styrene-maleic acid copolymer in which a structural unit containing maleic acid is modified to a structural unit A. By using such a dispersion resin, the redispersibility after solidification is further improved, and even when stored at high temperatures, the particle size and viscosity change tend to be smaller.
[0014] The content of the dispersion resin is preferably 2.5 to 12.5% by mass, more preferably 3.5 to 10% by mass, and further preferably 4.5 to 9.0% by mass, based on the total amount of the dispersion liquid. By having the content of the dispersion resin within the above range, redispersibility after solidification is improved, and even when stored at high temperatures, changes in particle size and viscosity tend to be smaller.
[0015] The content of the dispersion resin is preferably 20 to 100 parts by mass, more preferably 30 to 80 parts by mass, and even more preferably 40 to 70 parts by mass, relative to 100 parts by mass of the colorant. By having the content of the dispersion resin within the above range, redispersibility after solidification is improved, and even when stored at high temperatures, there is a tendency for the particle size and viscosity to change less.
[0016] 1.1.1. Building Block A The structural unit A is a structural unit represented by the following formula (1): The monomers constituting the structural unit A may be used alone or in combination of two or more kinds. [ka] (In the formula, R 1 each independently represents a divalent organic group having 1 to 20 carbon atoms; R 2 each independently represents a sulfo group or a salt thereof.
[0017] In the formula, R 1 The divalent organic group having 1 to 20 carbon atoms represented by the formula (I) is not particularly limited, and examples thereof include divalent aliphatic hydrocarbon groups (alkylene groups, cycloalkylene groups, alkylene-cycloalkylene groups, etc.), divalent aromatic hydrocarbon groups (arylene groups, alkylene-arylene groups, etc.), and the like.
[0018] Among these, divalent aliphatic hydrocarbon groups are preferred, and alkylene groups are more preferred. Examples of the alkylene group include, but are not limited to, an ethylene group, a propylene group, an isopropylene group, a butylene group, a 1,2-dimethylethylene group, a pentylene group, a 1-methylbutylene group, a 2-methylbutylene group, a heptylene group, an octylene group, a nonylene group, and a decylene group.
[0019] Also, R 1 The divalent organic group represented by the formula: has 1 to 20 carbon atoms, preferably 1 to 12 carbon atoms, and more preferably 1 to 8 carbon atoms.
[0020] R 2 The salt of the sulfo group represented by the formula (I) is not particularly limited, but examples thereof include sodium salt, lithium salt, potassium salt, and ammonium salt.
[0021] Among these, it is preferable that the monomer constituting the structural unit A contains at least one selected from the group consisting of N-methanesulfonic acid maleimide, N-ethanesulfonic acid maleimide, N-propanesulfonic acid maleimide, N-benzenesulfonic acid maleimide, and salts thereof. By using such a structural unit A, redispersibility after solidification is improved, and even when stored at high temperatures, the particle size and viscosity change tend to be smaller.
[0022] The content of the structural unit A is preferably 5 to 55 mol% or more, more preferably 10 to 50 mol%, and even more preferably 10 to 45 mol% based on the total amount of the dispersion resin. By having the content of the structural unit A within the above range, redispersibility after solidification is improved, and even when stored at high temperatures, changes in particle size and viscosity tend to be smaller.
[0023] 1.1.2. Building block B The structural unit B is a structural unit represented by any one of the following formulas (2-1) to (2-2): The monomer constituting the structural unit B may be used alone or in combination of two or more kinds. [ka] (In the formula, R 3 each independently represents a monovalent organic group having 1 to 20 carbon atoms; R 4 each independently represents a divalent organic group having 1 to 12 carbon atoms; R 5 each independently represents an organic group having 1 to 12 carbon atoms.
[0024] In the formula, R 3 The monovalent organic group having 1 to 20 carbon atoms represented by the formula (I) is not particularly limited, but examples thereof include monovalent aliphatic hydrocarbon groups (alkyl groups, cycloalkyl groups, alkyl-cycloalkyl groups, etc.), monovalent aromatic hydrocarbon groups (aryl groups, alkyl-aryl groups, etc.), etc. Among these, monovalent aromatic hydrocarbon groups are preferred, and alkyl-aryl groups such as a benzyl group are more preferred.
[0025] Also, R3 The monovalent organic group represented by the formula: has 1 to 20 carbon atoms, preferably 1 to 12 carbon atoms, and more preferably 1 to 8 carbon atoms.
[0026] In the formula, R 4 The divalent organic group having 1 to 12 carbon atoms represented by the formula (I) is not particularly limited, and examples thereof include divalent aliphatic hydrocarbon groups (alkylene groups, cycloalkylene groups, alkylene-cycloalkylene groups, etc.), divalent aromatic hydrocarbon groups (arylene groups, alkylene-arylene groups, etc.), and the like.
[0027] Among these, divalent aliphatic hydrocarbon groups are preferred, and alkylene groups are more preferred. Examples of the alkylene group include, but are not limited to, an ethylene group, a propylene group, an isopropylene group, a butylene group, a 1,2-dimethylethylene group, a pentylene group, a 1-methylbutylene group, a 2-methylbutylene group, a heptylene group, and an octylene group.
[0028] Also, R 4 The monovalent organic group represented by the formula: has 1 to 12 carbon atoms, preferably 1 to 8 carbon atoms, and more preferably 1 to 4 carbon atoms.
[0029] In the formula, R 5 The monovalent organic group having 1 to 12 carbon atoms represented by the formula (I) is not particularly limited, but examples thereof include monovalent aliphatic hydrocarbon groups (alkyl groups, cycloalkyl groups, alkyl-cycloalkyl groups, etc.), monovalent aromatic hydrocarbon groups (aryl groups, alkyl-aryl groups, etc.), etc. Among these, monovalent aromatic hydrocarbon groups are preferred, and aryl groups such as a phenyl group are more preferred.
[0030] Also, R 3 The monovalent organic group represented by the formula: has 1 to 20 carbon atoms, preferably 1 to 12 carbon atoms, and more preferably 1 to 8 carbon atoms.
[0031] The content of the structural unit B is preferably 1 to 20 mol% or more, more preferably 3 to 15 mol%, and even more preferably 5 to 10 mol% based on the total amount of the dispersion resin. By having the content of the structural unit B within the above range, redispersibility after solidification is improved, and even when stored at high temperatures, changes in particle size and viscosity tend to be smaller.
[0032] 1.1.3. Building Block C The structural unit C is a structural unit represented by any one of the following formulas (3-1) to (3-4): The monomers constituting the structural unit C may be used alone or in combination of two or more kinds. [ka] (In the formula, R 6 each independently represents a hydrogen atom, an alkyl group having 1 to 12 carbon atoms, or an alkoxy group having 1 to 12 carbon atoms.
[0033] R 6 As the alkyl group having 1 to 12 carbon atoms, a straight-chain, branched-chain or cyclic alkyl group can be used. Such an alkyl group is not particularly limited, but examples thereof include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, a t-butyl group, an n-pentyl group, a neopentyl group, an n-hexyl group, a cyclohexyl group, an n-heptyl group, an n-octyl group, an n-ethylhexyl group, an n-nonyl group and an n-decyl group.
[0034] R 6 The alkoxy group having 1 to 12 carbon atoms represented by the formula (I) is not particularly limited, but examples thereof include a methoxy group, an ethoxy group, a propoxy group, a butoxy group, a pentyloxy group, a hexyloxy group, an octyloxy group, a decyloxy group, a dodecyloxy group, a hexadecyloxy group, and an octadecyloxy group.
[0035] R 6 The alkyl group or alkoxy group represented by the following formula has 1 to 12 carbon atoms, preferably 1 to 6 carbon atoms, and more preferably 1 to 3 carbon atoms.
[0036] Among these, it is preferable that the monomer constituting the structural unit C contains at least one selected from the group consisting of styrene, allylbenzene, vinyltoluene, 1-vinylnaphthalene, and 2-vinylnaphthalene. By using such a structural unit C, redispersibility after solidification is improved, and even when stored at high temperatures, the particle size and viscosity tend to change less.
[0037] The content of the structural unit C is preferably 40 to 90 mol%, more preferably 45 to 85 mol%, and even more preferably 50 to 75 mol%, based on the total amount of the dispersion resin. By having the content of the structural unit B within the above range, redispersibility after solidification is improved, and even when stored at high temperatures, the change in particle size and viscosity tends to be smaller.
[0038] 1.1.4. Building Block D The dispersion resin may further include a structural unit D represented by the following formula (4): By including such a structural unit D, redispersibility after solidification is improved, and even when stored at high temperatures, the change in particle size and viscosity tends to be smaller. [ka] (In the formula, R 7 each independently represents a hydrogen atom or a methyl group; R 8 each independently represents a hydrogen atom or an alkyl group having 1 to 12 carbon atoms.
[0039] R 8 As the alkyl group having 1 to 12 carbon atoms, a straight-chain, branched-chain or cyclic alkyl group can be used. Such an alkyl group is not particularly limited, but examples thereof include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, a t-butyl group, an n-pentyl group, a neopentyl group, an n-hexyl group, a cyclohexyl group, an n-heptyl group, an n-octyl group, an n-ethylhexyl group, an n-nonyl group and an n-decyl group.
[0040] R 8 The alkyl group represented by the following formula (1) has 1 to 12 carbon atoms, preferably 1 to 10 carbon atoms, and more preferably 1 to 8 carbon atoms.
[0041] Among these, it is preferable to include at least one selected from the group consisting of methyl acrylate, n-butyl acrylate, isobutyl acrylate, cyclohexyl acrylate, methyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, and cyclohexyl methacrylate. By using such a structural unit D, redispersibility after solidification is improved, and even when stored at high temperatures, the particle size and viscosity tend to change less.
[0042] The content of the structural unit D is preferably 1 to 20 mol%, more preferably 3 to 15 mol%, and even more preferably 5 to 10 mol%, based on the total amount of the dispersion resin. By having the content of the structural unit D within the above range, redispersibility after solidification is improved, and even when stored at high temperatures, changes in particle size and viscosity tend to be smaller.
[0043] 1.1.5. Other building blocks The dispersion resin of the present embodiment may have a structural unit containing maleic acid or a derivative thereof as a structural unit other than the above structural units.
[0044] 1.1.6.Weight average molecular weight The weight average molecular weight of the dispersion resin is 10,000 to 60,000, preferably 12,500 to 45,000, and more preferably 15,000 to 30,000. When the weight average molecular weight of the dispersion resin is within the above range, redispersibility after solidification is improved, and even when stored at high temperatures, changes in particle size and viscosity tend to be smaller.
[0045] The weight average molecular weight can be measured by a known method, such as a chromatography method, and more specifically, by the method described in the Examples.
[0046] 1.1.7. Manufacturing method The dispersion resin of this embodiment can be obtained by copolymerizing the monomers constituting each of the above-mentioned structural units. The polymerization reaction is not particularly limited, but for example, radical polymerization, particularly living radical polymerization, can be used. In addition, the structural unit containing maleic acid of the styrene-maleic acid copolymer may be modified to structural unit A (maleimide unit).
[0047] 1.2.Water The water content is preferably 60 to 95% by mass, more preferably 65 to 95% by mass, and further preferably 75 to 90% by mass, based on the total amount of the dispersion.
[0048] 1.3.Colorants The coloring material is not particularly limited, but may be, for example, a disperse dye or a pigment. Among these, a disperse dye is preferable. By using a disperse dye, the redispersibility after solidification is improved, and even when stored at high temperatures, the particle size and viscosity tend to change less. The coloring material may be used alone or in combination of two or more kinds.
[0049] The disperse dye is not particularly limited, and known disperse dyes such as CI Disperse Yellow, CI Disperse Orange, CI Disperse Blue, CI Disperse Violet, and CI Disperse Black can be used.
[0050] The inorganic pigment is not particularly limited, but examples thereof include carbon blacks (CI Pigment Black 7) such as furnace black, lamp black, acetylene black, and channel black, iron oxide, and titanium oxide.
[0051] Examples of organic pigments include, but are not limited to, quinacridone pigments, quinacridonequinone pigments, dioxazine pigments, phthalocyanine pigments, anthrapyrimidine pigments, anthanthrone pigments, indanthrone pigments, flavanthrone pigments, perylene pigments, diketopyrrolopyrrole pigments, perinone pigments, quinophthalone pigments, anthraquinone pigments, thioindigo pigments, benzimidazolone pigments, isoindolinone pigments, azomethine pigments, and azo pigments.
[0052] The content of the coloring material is preferably 7.5 to 30% by mass, more preferably 7.5 to 25% by mass, and further preferably 8.5 to 20% by mass, based on the total amount of the dispersion.
[0053] 1.4.pH adjusters The dispersion liquid may further contain a pH adjuster. The pH adjuster is not particularly limited, but examples thereof include inorganic acids (e.g., sulfuric acid, hydrochloric acid, nitric acid, etc.), inorganic bases (e.g., lithium hydroxide, sodium hydroxide, potassium hydroxide, ammonia, etc.), organic bases (triethanolamine, diethanolamine, monoethanolamine, tripropanolamine), organic acids (e.g., adipic acid, citric acid, succinic acid, etc.), etc. The pH adjuster may be used alone or in combination of two or more.
[0054] 2. Ink composition for ink-jet recording The ink composition for inkjet recording of this embodiment (also simply referred to as "ink composition") contains the above-mentioned dispersion liquid, a surfactant, and a water-soluble organic solvent, and may contain other components as necessary. Note that "for inkjet recording" means that the composition is used by an inkjet method in which ink droplets are ejected from the nozzles of an inkjet head.
[0055] 2.1.Dispersion liquid The dispersion liquid is as described above. The content of the dispersion resin added to the ink composition together with the dispersion liquid is preferably 0.1 to 3.5 mass %, more preferably 0.3 to 3.0 mass %, and even more preferably 0.5 to 2.5 mass %, based on the total amount of the ink composition. By having the content of the dispersion resin within the above range, redispersibility after solidification is improved, and even when stored at high temperatures, there is a tendency for the particle size and viscosity changes to be smaller.
[0056] The content of the colorant added to the ink composition together with the dispersion liquid is preferably 0.5 to 7.0% by mass, more preferably 1.0 to 6.0% by mass, and even more preferably 1.5 to 4.5% by mass, based on the total amount of the ink composition. By having the content of the colorant within the above range, redispersibility after solidification is improved, and even when stored at high temperatures, changes in particle size and viscosity tend to be smaller.
[0057] In the ink composition, the content of the dispersion resin is preferably 20 to 100 parts by mass, more preferably 30 to 80 parts by mass, and even more preferably 40 to 70 parts by mass, relative to 100 parts by mass of the colorant. By having the content of the dispersion resin within the above range, redispersibility after solidification is improved, and even when stored at high temperatures, changes in particle size and viscosity tend to be smaller.
[0058] 2.2.Surfactants The surfactant is not particularly limited, but examples thereof include acetylene glycol surfactants, fluorine-based surfactants, and silicone-based surfactants.
[0059] The acetylene glycol surfactant is not particularly limited, but for example, one or more selected from 2,4,7,9-tetramethyl-5-decyne-4,7-diol, alkylene oxide adducts of 2,4,7,9-tetramethyl-5-decyne-4,7-diol, and alkylene oxide adducts of 2,4-dimethyl-5-decyne-4-ol and alkylene oxide adducts of 2,4-dimethyl-5-decyne-4-ol are preferred.
[0060] The fluorine-based surfactant is not particularly limited, but examples thereof include perfluoroalkyl sulfonate, perfluoroalkyl carboxylate, perfluoroalkyl phosphate, perfluoroalkyl ethylene oxide adduct, perfluoroalkyl betaine, and perfluoroalkyl amine oxide compound.
[0061] Examples of silicone surfactants include polysiloxane compounds and polyether-modified organosiloxanes.
[0062] The content of the surfactant is preferably 0.1 to 3.0% by mass, and more preferably 0.1 to 1.0% by mass, relative to the total amount of the ink composition.
[0063] 2.3. Water-soluble organic solvents The water-soluble organic solvent is not particularly limited, and examples thereof include glycerin; glycols such as ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, dipropylene glycol, 1,3-propanediol, 1,2-butanediol, 1,2-pentanediol, 1,2-hexanediol, 1,4-butanediol, 1,5-pentanediol, and 1,6-hexanediol; ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, and propylene glycol monomethyl ether. Examples of the water-soluble organic solvent include glycol monoethers such as ethyl ether, propylene glycol monoethyl ether, dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, and triethylene glycol monomethyl ether; nitrogen-containing solvents such as 2-pyrrolidone, N-methyl-2-pyrrolidone, and N-ethyl-2-pyrrolidone; and alcohols such as methanol, ethanol, n-propyl alcohol, isopropyl alcohol, n-butanol, 2-butanol, tert-butanol, iso-butanol, n-pentanol, 2-pentanol, 3-pentanol, and tert-pentanol. Among these, glycerin, glycols, and glycol monoethers are preferred, and diethylene glycol, propylene glycol, triethylene glycol monomethyl ether, and glycerin are more preferred. The water-soluble organic solvent may be used alone or in combination of two or more.
[0064] The content of the water-soluble organic solvent is preferably 5.0 to 30% by mass, and more preferably 10 to 20% by mass, based on the total amount of the ink composition. When the content of the water-soluble organic solvent is within the above range, redispersibility after solidification is improved, and even when stored at high temperatures, changes in particle size and viscosity tend to be smaller.
[0065] 2.4.Water The water content is preferably 60 to 90% by mass, and more preferably 70 to 85% by mass, based on the total amount of the ink composition. When the water content is within the above range, redispersibility after solidification is improved, and changes in particle size and viscosity tend to be smaller even when stored at high temperatures.
[0066] 2.5. pH Adjusters The ink composition may further contain a pH adjuster. The pH adjuster is not particularly limited, but may be any of those exemplified in the dispersion liquid. The pH adjuster in the ink composition may be one that is mixed originating from the dispersion liquid, or may be one that is added separately when preparing the ink composition.
[0067] The content of the pH adjuster is preferably 0.1 to 2.0% by mass, and more preferably 0.5 to 1.5% by mass, relative to the total amount of the ink composition.
[0068] 2.6.Other resins The ink composition may further contain other resins other than the dispersion resin. The other resins are not particularly limited, but may include, for example, anionic resins, cationic resins, or nonionic resins. By including such resins, the colorant can be fixed to the recording medium.
[0069] The cationic resin is not particularly limited, but examples thereof include starch derivatives such as cationic starch, cationic urethane resins, cationic olefin resins, and cationic allylamine resins.
[0070] Examples of anionic resins include carboxymethyl cellulose salts, cellulose derivatives such as viscose, alginates, gum arabic, gum tragacanth, and lignin sulfonates. Examples of natural resins include:
[0071] The nonionic resin is not particularly limited, but examples thereof include acrylic resins, styrene-acrylic resins, urethane resins, ester resins, olefin resins, and vinyl acetate resins.
[0072] The content of the other resin is preferably 0.1 to 2.0 mass %, and more preferably 0.5 to 1.5 mass %, relative to the total amount of the ink composition. EXAMPLES
[0073] The present invention will be described in more detail below using examples and comparative examples, but the present invention is not limited to the following examples.
[0074] 1. Synthesis example 1.1. Monomer synthesis 1.1.1. Synthesis Example 1 In a three-neck flask equipped with a reflux condenser and a thermometer, 8.8 g of aminomethanesulfonic acid (Tokyo Chemical Industry Co., Ltd., 80 mmol), 7.84 g of maleic anhydride (Fujifilm Wako Pure Chemical Industries, Ltd., 80 mmol), and 300 mL of acetic acid (Fujifilm Wako Pure Chemical Industries, Ltd.) were placed, and the mixture was stirred for 15 hours at room temperature under atmospheric pressure using a magnetic stirrer, and then heated and refluxed for 8 hours. After distilling off the acetic acid under reduced pressure, impurities were separated by silica gel column chromatography, and recrystallization was performed to obtain N-methanesulfonic acid maleimide (a-1) (8.5 g, yield 55.6%) represented by the following formula. The compound was identified by proton nuclear magnetic resonance spectroscopy. 1H-NMR(400MHz,DMSO-d6)δ(ppm)=7.64(1H,s,SO3H), 6.75(2H,s,2×CH),3.58(2H,s,CH2) [ka]
[0075] 1.1.2. Synthesis Example 2 N-propanesulfonic acid maleimide (a-2) was obtained in the same manner as in Synthesis Example 1, except that 3-aminopropanesulfonic acid was used instead of aminomethanesulfonic acid.
[0076] 1.1.3. Synthesis Example 3 N-Ethanesulfonic acid maleimide (a-3) was obtained in the same manner as in Synthesis Example 1, except that 2-aminoethanesulfonic acid sodium salt was used instead of aminomethanesulfonic acid.
[0077] 1.1.4. Synthesis Example 4 N-Benzenesulfonic acid maleimide (a-4) was obtained in the same manner as in Synthesis Example 1, except that p-aminobenzenesulfonic acid sodium salt was used instead of aminomethanesulfonic acid.
[0078] The following Table 1 shows the R in formula (1) of the monomer constituting the structural unit A obtained in the above Synthesis Examples 1 to 4. 1 and R 2 Shows. [Table 1]
[0079] 1.1.5. Synthesis Example 5 The same procedure as in Synthesis Example 1 was carried out except that benzylamine (manufactured by Tokyo Chemical Industry Co., Ltd.) was used instead of aminomethanesulfonic acid, to obtain N-maleimide monomer (b-1).
[0080] 1.1.6. Synthesis Example 6 The same procedure as in Synthesis Example 1 was carried out except that 3-butoxypropylamine (manufactured by Tokyo Chemical Industry Co., Ltd.) was used instead of aminomethanesulfonic acid, to obtain N-maleimide monomer (b-2).
[0081] 1.1.7. Synthesis Example 7 The same procedure as in Synthesis Example 1 was carried out except that 2-phenoxyethylamine (manufactured by Tokyo Chemical Industry Co., Ltd.) was used instead of aminomethanesulfonic acid, to obtain N-maleimide monomer (b-3).
[0082] The following Table 2 shows the R in formula (2-1) or (2-2) of the monomer constituting the structural unit B obtained in the above Synthesis Examples 5 to 7. 3 , R 4, and R 5 Shows. [Table 2]
[0083] 1.2.Copolymer synthesis 1.2.1. Synthesis Example 8 In a three-neck flask equipped with a reflux condenser and a thermometer, 5.74 g (30 mmol) of N-methanesulfonic acid maleimide (a-1) that gives structural unit A, 11.0 g (10 mmol) of N-maleimide monomer (b-1) that gives structural unit B, 10.4 g of styrene (manufactured by Tokyo Chemical Industry Co., Ltd., 100 mmol) as a monomer that gives structural unit C, and 60 g of dimethyl sulfoxide (DMSO) (manufactured by Tokyo Chemical Industry Co., Ltd.) were placed and dissolved using a magnetic stirrer. In addition, 0.46 g of azobisisobutyronitrile (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., 2.8 mmol) was placed in another glass bottle and dissolved in 20 g of DMSO to obtain an initiator solution. After replacing the inside of the reactor with nitrogen, the initiator solution was dropped into the flask. Then, the mixture was reacted at 75° C. for 5 hours. After the reaction was completed, the reactant was dropped into water to precipitate a white solid. The white solid was filtered by suction, washed repeatedly with water, and dried in vacuum at 50° C. for 10 hours to obtain 13.2 g of copolymer A-1.
[0084] 1.2.2. Synthesis Examples 9-14 Copolymers A-2 to A-7 were obtained in the same manner as in Synthesis Example 8, except that the monomers shown in Table 3 were used and the amounts of each monomer and initiator used were adjusted.
[0085] 1.2.3. Synthesis Example 15 In a three-neck flask equipped with a reflux condenser and a thermometer, 8.32 g of styrene (Tokyo Chemical Industry Co., Ltd., 80 mmol) as a monomer that gives the structural unit C, 2-{[(carboxymethyl)sulfanylthiocarbonyl]sulfanyl}propanoic acid (CSPA) (Tokyo Chemical Industry Co., Ltd., 9.6 mmol), 0.52 g of azobisisobutyronitrile (Fujifilm Wako Pure Chemical Industries, Ltd., 3.2 mmol), and 80 g of dimethylformamide (DMF) (Tokyo Chemical Industry Co., Ltd.) were placed and dissolved using a magnetic stirrer. After degassing by nitrogen bubbling, the mixture was heated at 75 ° C for 6 hours. After the reaction was completed, the reactant was dropped into water to precipitate a pale yellow solid. The obtained solid was filtered, washed with a small amount of methanol, and vacuum dried at 50 ° C for 10 hours to obtain a polystyrene Raft agent adduct (mb-1).
[0086] Next, in a three-neck flask equipped with a reflux condenser and a thermometer, the polystyrene Raft agent adduct (mb-1), 5.74 g (30 mmol) of N-methanesulfonic acid maleimide (a-1) that gives structural unit A, 1.87 g (10 mmol) of N-maleimide monomer (b-1) that gives structural unit B, 10.4 g of styrene (Tokyo Chemical Industry Co., Ltd., 100 mmol) as a monomer that gives structural unit C, 0.52 g of azobisisobutyronitrile (Fujifilm Wako Pure Chemical Industries, Ltd., 3.2 mmol), and 60 g of DMF (Tokyo Chemical Industry Co., Ltd.) were placed and dissolved using a magnetic stirrer. After degassing by nitrogen bubbling, the mixture was heated at 75 ° C for 6 hours. After the reaction was completed, the reaction solution was diluted with methanol and added to methyl ethyl ketone to precipitate a pale yellow solid. The resulting solid was recovered by centrifugation and vacuum dried at 50° C. for 10 hours to obtain 19.5 g of Copolymer B-1.
[0087] The resulting copolymer B-1 was a block copolymer having a block of the structural unit C and a random block of the structural units A, B and C.
[0088] 1.2.4. Synthesis Example 16 Copolymer B-2 was obtained in the same manner as in Synthesis Example 15, except that the monomers shown in Table 3 were used as monomers that provide structural unit A, and the amounts of the monomers used were adjusted.
[0089] 1.2.5. Synthesis Example 17 In a three-neck flask equipped with a reflux condenser and a thermometer, 7.5 g of styrene-maleic anhydride copolymer containing structural unit C (SMA EF60, styrene / maleic anhydride ratio: 6 / 1, Kawahara Oil Chemical Co., Ltd.) was added to a methyl ethyl ketone (25 mL) solution of 1.35 g of 2-aminoethanesulfonic acid (Tokyo Chemical Industry Co., Ltd.) that gives structural unit A, and 0.54 g of benzylamine that gives structural unit B were added, and the mixture was heated and stirred at 100 ° C for 1 hour under a nitrogen stream. Once cooled, a distillation apparatus was attached, and methyl ethyl ketone and water were distilled off to obtain a pale yellow solid. 6.0 g of N-methylpyrrolidone (Tokyo Chemical Industry Co., Ltd.) was added to this pale yellow solid, and the mixture was heated and stirred at 180 ° C for 2.5 hours under a N2 stream. After cooling, the yellow liquid was added to isopropyl alcohol (500 ml), and the precipitated solid was filtered off, washed with a small amount of isopropyl alcohol, and vacuum dried at 50° C. for 10 hours to obtain 8.2 g of copolymer C-1.
[0090] 1.2.6. Synthesis Examples 18-19 In Synthesis Example 18, styrene-maleic anhydride copolymer (SMA EF40, styrene / maleic anhydride ratio: 4 / 1) was used instead of styrene-maleic anhydride copolymer (SMA EF60), and in Synthesis Example 19, 4-aminobenzenesulfonic acid was used instead of 2-aminoethanesulfonic acid that gives structural unit A, and styrene-maleic anhydride copolymer (SMA 3000, styrene / maleic anhydride ratio: 3 / 1) was used instead of styrene-maleic anhydride copolymer (SMA EF60). Except for this, copolymers C-2 to C-3 were obtained in the same manner as in Synthesis Example 17.
[0091] 1.2.7. Synthesis Examples 20-21 Copolymers D-1 to D-2 were obtained in the same manner as in Synthesis Example 8, except that the monomers shown in Table 3 were further used as monomers providing structural unit D and the amounts of the monomers and initiator used were adjusted.
[0092] 1.2.8. Synthesis Examples 22-23 Copolymers E-1 to E-2 were obtained in the same manner as in Synthesis Examples 15 to 16, except that the monomers shown in Table 3 were further used as monomers that provide structural unit D in addition to structural units A, B, and C to the polystyrene Raft agent adduct (mb-1), and the amounts of the monomers and initiator used were adjusted. The obtained copolymers E-1 to E-2 were block copolymers having a block of structural unit B and random blocks of structural units A, B, C, and D.
[0093] 1.2.9. Synthesis Example 24 In a three-neck flask equipped with a reflux condenser and a thermometer, 6.77 g of styrene (manufactured by Tokyo Chemical Industry Co., Ltd., 65 mmol) as a monomer that gives structural unit C, 1.50 g of methyl methacrylate (manufactured by Tokyo Chemical Industry Co., Ltd., 15 mmol) as a monomer that gives structural unit D, and DMSO (manufactured by Tokyo Chemical Industry Co., Ltd., 80 g) were placed and dissolved using a magnetic stirrer. In addition, 1.96 g of maleic anhydride (manufactured by Tokyo Chemical Industry Co., Ltd., 20 mmol) and 0.52 g of azobisisobutyronitrile (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., 3.2 mmol) were placed in another glass bottle and dissolved in 25 g of DMSO to obtain an initiator mixture solution. After replacing the inside of the reactor with nitrogen, the initiator mixture solution was dropped into it. Then, the reaction was carried out at 75 ° C for 6 hours. After the reaction was completed, the reactant was dropped into water to precipitate a white solid. The white solid was filtered by suction, washed repeatedly with water, and dried in vacuum at 50° C. for 10 hours to obtain 8.7 g of copolymer (f-1).
[0094] Next, in a three-neck flask equipped with a reflux condenser and a thermometer, 8.0 g of the obtained copolymer (f-1, styrene / maleic anhydride / methyl methacrylate ratio: 13 / 4 / 3) was dissolved in methyl ethyl ketone (25 mL) and an aqueous solution of 2.5 g of 2-aminoethanesulfonic acid (Tokyo Chemical Industry Co., Ltd., 20 mmol) that gives the structural unit A was dissolved in 10 wt% aqueous sodium hydroxide solution (8.0 g) and added to the solution, and the mixture was heated and stirred at 100 ° C. for 1 hour under a nitrogen stream. Once cooled, a distillation apparatus was attached, and methyl ethyl ketone and water were distilled off to obtain a pale yellow solid. 1.1 g of benzylamine (Tokyo Chemical Industry Co., Ltd.) that gives the structural unit B and 6.0 g of N-methylpyrrolidone (Tokyo Chemical Industry Co., Ltd.) were added to the pale yellow solid, and the mixture was heated and stirred at 180 ° C. for 2.5 hours under a nitrogen stream. After cooling, the yellow liquid was added to isopropyl alcohol (500 ml), and the precipitated solid was filtered off, washed with a small amount of isopropyl alcohol, and vacuum dried at 50° C. for 10 hours to obtain 7.5 g of copolymer F-1.
[0095] 1.2.10. Synthesis Examples 25-27 In Synthesis Examples 25 and 26, the monomers shown in Table 3 were used as monomers that provide structural unit C, and the amounts of the monomers and initiator used were adjusted, but the procedure was the same as in Synthesis Example 24 to obtain copolymers F-2 to F-3. In Synthesis Example 27, 4-aminobenzenesulfonic acid was used instead of 2-aminoethanesulfonic acid that provides structural unit A, and the procedure was the same as in Synthesis Example 24 to obtain copolymer F-4, but the procedure was the same as in Synthesis Example 24 to obtain copolymer F-4.
[0096] Table 3 shows the weight average molecular weight Mw of each copolymer obtained in the above synthesis examples and the composition ratio of each structural unit.
[0097] [Table 3]
[0098] 1.3.NMR analysis The composition ratio of each structural unit was confirmed by 1H-NMR analysis and 13C-NMR analysis. In the NMR analysis, a nuclear magnetic resonance apparatus (JNM-ECX400, manufactured by JEOL Ltd.) was used.
[0099] 1.4.Weight average molecular weight The weight average molecular weight Mw of each dispersion resin was measured by a chromatography method under the following conditions. (Measurement conditions) Device name: HLC8320GPC (Tosoh) Guard column: TSKgel guarcolumn SuperAWM-H Column: TSKgel SuperAWM-H Column temperature: 25℃ Eluent: 10mmol / L lithium bromide in dimethylacetamide Flow rate: 0.6 mL / mIn Detector: RI
[0100] 2. Preparation of Dispersion Liquid (Examples 1 to 20 and Comparative Examples 1 to 2) A 1 L eggplant-shaped flask (stirring bar, Dimroth condenser) was set, and 15 parts by mass of the copolymer shown in Table 4 and 70 parts by mass of pure water were added, and the mixture was heated and stirred at 80° C. Triethanolamine was added thereto until the pH became 8.0, and the pure water was added to make up to 100 parts by mass. After cooling to 25° C., the dissolved aqueous solution was used as a varnish liquid.
[0101] Next, zirconia beads, 13 parts by mass of the varnish liquid, 4 parts by mass of DISPERSE RED 364 (hereinafter also referred to as "DR364") or DISPERSE BLUE 359 (hereinafter also referred to as "DB359") as a water-insoluble colorant, and 17 parts by mass of pure water were added and ground in a bead mill for 1 hour to prepare a dispersion containing 5.7% by mass of the copolymer and 11.7% by mass of the colorant.
[0102] 3. Preparation of Ink Composition The dispersion liquid obtained as described above was mixed with other components so as to obtain each of the ink compositions shown below. Dispersion liquid 15.0% by mass Organic solvent: Diethylene glycol 10.0% by mass 1,2-Hexanediol 3.0% by mass Other resins Carboxymethylcellulose sodium salt 1.0% by mass Surfactant BYK-348 0.3% by weight pH adjuster: Triethanolamine 1.0% by mass Water remaining
[0103] 4. Evaluation 4.1. Changes in particle size distribution The ink composition prepared as above was placed in a sample bottle and left at 60°C for 5 days. The volume-based cumulative 50% particle size (D50) of the ink composition before and after leaving it was measured by dynamic light scattering to confirm the change in cumulative 50% particle size before and after leaving it. A Microtrac UPA150 (trade name, manufactured by Microtrac Inc.) was used as the measuring device. The change in particle size distribution was determined based on the obtained measurement results. (Evaluation Criteria) A: The cumulative 50% increase in particle size was less than 10%. B: The cumulative 50% increase in particle size was 10% or more and less than 30%. C: The cumulative 50% increase in particle size was 30% or more.
[0104] 4.2. Redispersibility The ink composition prepared as above was dropped onto a glass slide and dried in a dryer at 40° C. for 16 hours to solidify. The glass slide was then immersed in a sample bottle containing ink water, and the behavior of redispersion of the solid matter was visually confirmed. Note that the operation was performed with care not to stir the ink water. Note that the ink water refers to the ink composition that does not contain the dispersion liquid. The evaluation criteria for redispersibility are shown below. (Evaluation Criteria) A: The solid matter disappeared and redispersed. B: Some solid matter remained, but redispersion was observed. C: Solid matter remained and no redispersion was observed.
[0105] [Table 4] *JONCRYL 61J (BASF Japan water-soluble styrene acrylic resin) *SMA1440F (Styrene maleic anhydride ester resin manufactured by Kawahara Oil Chemical Co., Ltd.)
Claims
1. The ink contains water, a colorant, and a dispersion resin that disperses the colorant, The dispersion resin has a structural unit A represented by the following formula (1), a structural unit B represented by any one of the following formulas (2-1) to (2-2), and a structural unit C represented by any one of the following formulas (3-1) to (3-4): dispersion liquid. [Formula 1] (In the formula, R 1 each independently represents a divalent organic group having 1 to 20 carbon atoms; R 2 each independently represents a sulfo group or a salt thereof. [chemical 2] (In the formula, R 3 each independently represents a monovalent organic group having 1 to 20 carbon atoms; R 4 each independently represents a divalent organic group having 1 to 12 carbon atoms; R 5 each independently represents an organic group having 1 to 12 carbon atoms. [C3] (In the formula, R 6 each independently represents a hydrogen atom, an alkyl group having 1 to 12 carbon atoms, or an alkoxy group having 1 to 12 carbon atoms.
2. The content of the structural unit A is 5 to 55 mol% based on the total amount of the dispersion resin. The dispersion of claim 1.
3. The content of the structural unit B is 1 to 20 mol% based on the total amount of the dispersion resin.
3. The dispersion according to claim 1 or 2.
4. The content of the structural unit C is 40 to 90 mol% based on the total amount of the dispersion resin. The dispersion according to any one of claims 1 to 3.
5. The content of the structural unit C is 50 to 75 mol% based on the total amount of the dispersion resin. The dispersion of claim 4.
6. The dispersion resin further has a structural unit D represented by the following formula (4): The dispersion according to any one of claims 1 to 5. [C4] (In the formula, R 7 each independently represents a hydrogen atom or a methyl group; R 8 each independently represents a hydrogen atom or an alkyl group having 1 to 12 carbon atoms.
7. The content of the structural unit D is 1 to 20 mol% based on the total amount of the dispersion resin. The dispersion of claim 6.
8. The structural unit A includes at least one selected from the group consisting of N-methanesulfonic acid maleimide, N-ethanesulfonic acid maleimide, N-propanesulfonic acid maleimide, N-benzenesulfonic acid maleimide, and salts thereof. The dispersion according to any one of claims 1 to 7.
9. The structural unit B includes at least one selected from the group consisting of N-benzylmaleimide and 3-butoxypropylmaleimide. The dispersion according to any one of claims 1 to 8.
10. The structural unit C includes at least one selected from the group consisting of styrene, allylbenzene, vinyltoluene, 1-vinylnaphthalene, and 2-vinylnaphthalene. The dispersion according to any one of claims 1 to 9.
11. The weight average molecular weight of the dispersion resin is 10,000 to 60,000. The dispersion according to any one of claims 1 to 10.
12. The colorant is a disperse dye. The dispersion according to any one of claims 1 to 11.
13. The dispersion liquid according to any one of claims 1 to 12, a surfactant, and a water-soluble organic solvent. An ink composition for ink-jet recording.
14. The present invention has a structural unit A represented by the following formula (1), a structural unit B represented by any one of the following formulas (2-1) to (2-2), and a structural unit C represented by any one of the following formulas (3-1) to (3-4), Dispersion resin. [C5] (In the formula, R 1 each independently represents a divalent organic group having 1 to 20 carbon atoms; R 2 each independently represents a sulfo group or a salt thereof. [C6] (In the formula, R 3 each independently represents a monovalent organic group having 1 to 20 carbon atoms; R 4 each independently represents a divalent organic group having 1 to 12 carbon atoms; R 5 each independently represents an organic group having 1 to 12 carbon atoms. [C7] (In the formula, R 6 each independently represents a hydrogen atom, an alkyl group having 1 to 12 carbon atoms, or an alkoxy group having 1 to 12 carbon atoms.
Citation Information
Patent Citations
Dispersant for drilling fluid
JP1985106875A
Microcapsule, preparation thereof and method for releasing substance under control
JP1995144126A
Composition for forming organic conductive film and the organic conductive film
JP2013036013A
Inkjet ink composition, inkjet recording method, ink set, decorative sheet, decorative sheet molded product, method for producing in-mold molded product and in-mold molded product
JP2014173039A
Watercolor pigment ink composition
JP2015048437A