How the product is manufactured
The method simplifies the manufacturing process by using inorganic powders with varying binder melting points or particle sizes to join parts effectively, addressing the complexity of existing methods and enhancing product bonding strength and size.
Patent Information
- Application Number
- JP2020216427
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-12-25
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2040-12-25
AI Technical Summary
Existing methods for manufacturing products by joining multiple parts require precise control of carbon content and dimensions, making the process complex and difficult to execute.
A manufacturing method involving three-dimensional modeling and injection molding processes, where parts are joined using inorganic powders with different binder melting points or particle sizes, followed by controlled heating and sintering to facilitate bonding without gaps.
Enables the production of complex, large-sized products with improved bonding strength and reduced complexity by ensuring effective joining of parts through controlled melting and sintering processes.
Smart Images

Figure 0007567460000001 
Figure 0007567460000002 
Figure 0007567460000003
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a method for manufacturing an article. [Background technology]
[0002] Regarding technology for manufacturing products, Patent Document 1 discloses a method for joining, in a sintering process, molten steel material having a shaft and a green compact having a hole formed by compression molding a mixed powder containing an iron-based metal powder by controlling the carbon amount in the surface layer of the shaft and the fitting dimensions. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Japanese Patent Application Publication No. 6-330108 Summary of the Invention [Problem to be solved by the invention]
[0004] The above-mentioned methods require control of the carbon content and dimensions, making them relatively difficult to manufacture, and therefore there is a demand for a technology that can manufacture products by joining multiple parts in a simpler manner. [Means for solving the problem]
[0005] According to a first aspect of the present disclosure, there is provided a manufacturing method for manufacturing a product by bonding a first part containing an inorganic powder and a binder to a second part containing an inorganic powder and a binder. The manufacturing method includes a first step of generating the first part by a three-dimensional printing apparatus, a second step of generating the second part, a third step of assembling the first part and the second part to obtain an assembly, a fourth step of heating the assembly at a first temperature, and a fifth step of heating the assembly at a second temperature higher than the first temperature after the fourth step, wherein the first part has a first region in contact with the second part and a second region not in contact with the second part, and the melting point of the binder contained in the first region is lower than the melting point of the binder contained in the second region.
[0006] According to a second aspect of the present disclosure, there is provided a manufacturing method for manufacturing a product by bonding a first part containing an inorganic powder and a binder to a second part containing an inorganic powder and a binder. The manufacturing method includes a first step of generating the first part by a three-dimensional modeling device, a second step of generating the second part, a third step of assembling the first part and the second part to obtain an assembly, a fourth step of heating the assembly at a first temperature, and a fifth step of heating the assembly at a second temperature higher than the first temperature after the fourth step, wherein the first part has a first region in contact with the second part and a second region not in contact with the second part, and the particle size of the inorganic powder contained in the first region is smaller than the particle size of the inorganic powder contained in the second region. [Brief description of the drawings]
[0007] [Figure 1] FIG. 1 is a diagram showing a schematic configuration of a manufacturing system according to a first embodiment. [Diagram 2] FIG. 2 is a diagram showing a schematic configuration of a hopper and a discharge unit. [Diagram 3] FIG. 2 is a schematic perspective view showing a configuration of a screw. [Figure 4] FIG. 2 is a top view showing the configuration of the barrel. [Diagram 5] FIG. 1 is a cross-sectional view showing a schematic configuration of an injection molding machine. [Figure 6]FIG. 2 is a process diagram showing a manufacturing method of a product in the first embodiment. [Figure 7] 3A and 3B are diagrams illustrating an example of a first part and an example of a second part. [Figure 8] FIG. 2 is a diagram showing an assembly in which the first part and the second part are assembled. [Figure 9] FIG. 13 is a diagram showing a schematic configuration of a manufacturing system according to a fourth embodiment. [Figure 10] FIG. 11 is a process diagram showing a manufacturing method of a product in a fourth embodiment. [Figure 11] FIG. 13 is a diagram showing a schematic configuration of a manufacturing system according to a fifth embodiment. [Figure 12] FIG. 13 is a process diagram showing a manufacturing method of a product in the fifth embodiment. [Figure 13] FIG. 13 is an explanatory diagram showing an overview of a manufacturing method for a product in a fifth embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] A. First embodiment: Fig. 1 is a diagram showing a schematic configuration of a manufacturing system 5 in the first embodiment. The manufacturing system 5 includes a three-dimensional modeling apparatus 100, an injection molding machine 200, a degreasing apparatus 300, and a sintering furnace 400. The X, Y, and Z directions shown in Fig. 1 correspond to the X, Y, and Z directions shown in Fig. 2 and subsequent figures.
[0009] The three-dimensional modeling device 100 generates a first part including inorganic powder such as metal or ceramic and a binder by additive manufacturing. The injection molding machine 200 generates a second part including inorganic powder such as metal or ceramic and a binder by injection molding. The degreasing device 300 heats an assembly obtained by assembling the first part and the second part at a first temperature to perform degreasing. The sintering furnace 400 sinters the assembly by heating it at a second temperature higher than the first temperature to complete a product. In this specification, the term "product" refers to an object manufactured in the manufacturing system 5, and includes an object that becomes a part of another product and an object that is subjected to post-treatment or processing after sintering.
[0010] The three-dimensional modeling apparatus 100 includes a first discharge unit 10a, a second discharge unit 10b, a first hopper 20a, a second hopper 20b, a moving mechanism unit 70, a stage 80, and a control unit 90. In the following, when the first discharge unit 10a and the second discharge unit 10b are described without any particular distinction, they may be simply referred to as the discharge unit 10. Similarly, when the first hopper 20a and the second hopper 20b are described without any particular distinction, they may be simply referred to as the hopper 20.
[0011] The moving mechanism 70 changes the relative position of the discharge unit 10 and the stage 80. In this embodiment, the moving mechanism 70 moves the stage 80 relative to the first discharge unit 10a and the second discharge unit 10b. The moving mechanism 70 in this embodiment is configured by a three-axis positioner that moves the stage 80 in three axial directions, that is, the X, Y, and Z directions, by the driving forces of three motors. Each motor is driven under the control of the control unit 90. Note that in other embodiments, the moving mechanism 70 may not be configured to move the stage 80, but may be configured to move the discharge unit 10 without moving the stage 80, for example. The moving mechanism 70 may also be configured to move both the stage 80 and the discharge unit 10.
[0012] The control unit 90 is configured by a computer having one or more processors, a main storage device, and an input / output interface for inputting and outputting signals from and to the outside. In this embodiment, the control unit 90 performs various functions, such as a function of executing a three-dimensional modeling process for forming a three-dimensional object by the processor executing a program or command loaded onto the main storage device. The control unit 90 can form a three-dimensional object by switching between two different types of materials by selectively using the first discharge unit 10a and the second discharge unit 10b. The control unit 90 may be configured by a combination of multiple circuits instead of a computer.
[0013] FIG. 2 is a diagram showing a schematic configuration of the hopper 20 and the discharge unit 10 provided in the three-dimensional modeling apparatus 100. The discharge unit 10 includes a plasticizing unit 30 and a nozzle 60. The material stored in the hopper 20 is supplied to the discharge unit 10. Under the control of the control unit 90, the discharge unit 10 plasticizes at least a part of the material supplied from the hopper 20 by the plasticizing unit 30 to generate a plasticized material, and discharges the generated plasticized material from the nozzle 60 onto the stage 80 to laminate it. In this embodiment, "plasticization" means that heat is applied to a material having thermoplasticity to melt it. "Melting" means not only that a material having thermoplasticity is heated to a temperature above its melting point to become liquid, but also that a material having thermoplasticity is softened by heating to a temperature above its glass transition point to develop fluidity.
[0014] The hopper 20 contains a pellet-shaped material containing inorganic powder such as metal or ceramic and a binder. The material contained in the hopper 20 is supplied to the plasticizing section 30 through a supply path 22 provided below the hopper 20 so as to connect the hopper 20 and the discharge section 10. In this embodiment, the first material is contained in the first hopper 20a, and the second material is contained in the second hopper 20b. Therefore, the first material contained in the first hopper 20a is supplied to the first discharge section 10a, and the second material contained in the second hopper 20b is supplied to the second discharge section 10b. The first material has a lower melting temperature than the second material. In other words, the second material has a higher melting temperature than the first material.
[0015] The plasticizing section 30 includes a screw case 31, a screw 41 housed in the screw case 31, a drive motor 32 that drives the screw 41, a barrel 50, and a heater 58. The barrel 50 is provided with a communication hole 56. The heater 58 is embedded in the barrel 50. The screw 41 of this embodiment is a so-called flat screw, and is also called a "scroll."
[0016] The screw 41 has a generally cylindrical shape with a height along the central axis RX smaller than its diameter. The screw 41 has a groove forming surface 42 on which a screw groove 45 is formed, on a surface facing the barrel 50. The groove forming surface 42 faces a screw facing surface 52 of the barrel 50.
[0017] The drive motor 32 is connected to the surface of the screw 41 opposite to the groove forming surface 42. The drive motor 32 is driven under the control of a control unit 90. The screw 41 rotates about a central axis RX by torque generated by the rotation of the drive motor 32. Note that the drive motor 32 does not have to be directly connected to the screw 41, and may be connected via a reducer, for example.
[0018] The barrel 50 has a screw-facing surface 52 that faces the groove forming surface 42 of the screw 41. A communication hole 56 provided in the barrel 50 is formed so as to be aligned with the central axis RX of the screw 41.
[0019] The nozzle 60 has a nozzle opening 63 at its tip. The nozzle opening 63 is in communication with the communication hole 56 provided in the barrel 50. The nozzle 60 ejects the material plasticized by the plasticizing unit 30 from the nozzle opening 63 toward the stage 80.
[0020] Fig. 3 is a schematic perspective view showing the configuration of the groove forming surface 42 side of the screw 41. In Fig. 3, the position of the central axis RX of the screw 41 is indicated by a dashed line. As described above, the groove forming surface 42 is provided with a screw groove 45. A screw central portion 47, which is the central portion of the groove forming surface 42 of the screw 41, is configured as a recess to which one end of the screw groove 45 is connected. The screw central portion 47 faces the communication hole 56 of the barrel 50. The screw central portion 47 intersects with the central axis RX.
[0021] The screw groove 45 of the screw 41 constitutes a so-called scroll groove. The screw groove 45 extends from the screw center 47 toward the outer periphery of the screw 41 in an arc-like spiral shape. The screw groove 45 may be configured to extend in an involute curve shape or a spiral shape. The groove forming surface 42 is provided with a convex rib portion 46 that constitutes the side wall portion of the screw groove 45 and extends along each screw groove 45. The screw groove 45 continues to a material inlet 44 formed on a side surface 43 of the screw 41. This material inlet 44 is a portion that receives the material supplied from the hopper 20 via the supply path 22.
[0022] 3 shows an example of a screw 41 having three screw grooves 45 and three ridge portions 46. The number of screw grooves 45 and ridge portions 46 provided on the screw 41 is not limited to three, and only one screw groove 45 may be provided, or two or more screw grooves 45 may be provided. Also, FIG. 3 shows an example of a screw 41 in which a material introduction port 44 is formed in three places. The number of material introduction ports 44 provided on the screw 41 is not limited to three, and may be only one place, or two or more places.
[0023] FIG. 4 is a top view showing the configuration of the screw-opposing surface 52 side of the barrel 50. As described above, a communication hole 56 is formed in the center of the screw-opposing surface 52. A plurality of guide grooves 54 are formed around the communication hole 56 in the screw-opposing surface 52. One end of each guide groove 54 is connected to the communication hole 56, and extends in a spiral shape from the communication hole 56 toward the outer periphery of the screw-opposing surface 52. Each guide groove 54 has a function of guiding the molding material to the communication hole 56. Note that one end of the guide groove 54 does not have to be connected to the communication hole 56. Also, the guide groove 54 does not have to be formed in the barrel 50.
[0024] Returning to FIG. 1 for explanation, the injection molding machine 200 includes a plasticizing device 210 and a clamping device 230. The plasticizing device 210 and the clamping device 230 are each fixed to a base 205. The base 205 is equipped with a control unit 290. The injection molding machine 200 injects a plasticizing material from the plasticizing device 210 into a molding die 220 attached to the clamping device 230 to mold a molded product. In this embodiment, a metallic molding die 220 is attached to the clamping device 230. The molding die 220 attached to the clamping device 230 is not limited to being made of metal, and may be made of resin or ceramic. The metallic molding die 220 is called a metal mold.
[0025] The plasticizer 210 is connected to a material supply unit 208 into which the material of the molded product is fed. A pellet-shaped material containing inorganic powder such as metal or ceramic and a binder is used as the material of the molded product. The plasticizer 210 plasticizes at least a portion of the material fed from the material supply unit 208 to generate a plasticized material.
[0026] The control unit 290 is configured by a computer equipped with one or more processors, a main memory device, and an input / output interface for inputting and outputting signals from and to the outside. The processor loads and executes a program on the main memory device, whereby the control unit 290 controls the plasticizing unit 210 and the mold clamping unit 230 to manufacture a molded product.
[0027] 5 is a cross-sectional view showing a schematic configuration of the injection molding machine 200. As described above, the injection molding machine 200 is equipped with the plasticizing unit 210, the mold clamping unit 230, and the molding die 220, and also equipped with the injection control mechanism 240.
[0028] The plasticizing device 210 has a screw 211, a barrel 212, a heater 213, and a nozzle 214. The screw 211 is accommodated in a storage section 215 that accommodates the screw 211. The screw 211 of this embodiment is a so-called flat screw, and is also called a "scroll". The screw 211 is driven to rotate around its central axis RX in the storage section 215 by a screw driving section 216 equipped with a driving motor. A communication hole 217 is formed in the center of the barrel 212. An injection cylinder 241, which will be described later, is connected to the communication hole 217. A check valve 218 is provided in the communication hole 217 upstream of the injection cylinder 241. The rotation of the screw 211 by the screw driving section 216 and the heating by the heater 213 are controlled by a control section 290.
[0029] The injection control mechanism 240 includes an injection cylinder 241, a plunger 242, and a plunger drive unit 243 equipped with a drive motor. The injection control mechanism 240 has a function of injecting the plasticized material in the injection cylinder 241 into the cavity 223 described later. The injection control mechanism 240 controls the injection amount of the plasticized material from the nozzle 214 under the control of the control unit 290. The injection cylinder 241 is a substantially cylindrical member connected to the communication hole 217 of the barrel 212, and includes a plunger 242 therein. The plunger 242 slides inside the injection cylinder 241, and pressure-feeds the plasticized material in the injection cylinder 241 to the nozzle 214 provided in the plasticizing device 210. The plunger 242 is driven by the plunger drive unit 243.
[0030] The molding die 220 includes a movable die 221 and a fixed die 222. The movable die 221 and the fixed die 222 are disposed facing each other, and have a cavity 223 therebetween, which is a space corresponding to the shape of the molded product. The plasticized material flowing out from the communication hole 217 of the barrel 212 is pressure-fed by the injection control mechanism 240 and injected from the nozzle 214 into the cavity 223.
[0031] The mold clamping device 230 includes a mold drive unit 231 equipped with a drive motor, and has the function of opening and closing the movable mold 221 and the fixed mold 222. Under the control of the control unit 290, the mold clamping device 230 drives the mold drive unit 231 configured by a motor to rotate the ball screw 232, and moves the movable mold 221 coupled to the ball screw 232 relative to the fixed mold 222, thereby opening and closing the mold 220.
[0032] As described above, in this embodiment, both the three-dimensional modeling apparatus 100 and the injection molding machine 200 are provided with a flat screw for plasticizing the material. Alternatively, the three-dimensional modeling apparatus 100 and the injection molding machine 200 may be provided with an in-line screw for plasticizing the material.
[0033] 6 is a process diagram showing a method for manufacturing a product in the first embodiment. In a first step S10, a first part is modeled by the three-dimensional modeling apparatus 100. In a second step S20, a second part is molded by the injection molding machine 200. The first step S10 and the second step S20 may be performed in any order, and may be performed simultaneously. The first part modeled by the three-dimensional modeling apparatus 100 and the second part molded by the injection molding machine 200 are each called a green body.
[0034] Fig. 7 is a diagram showing an example of a first part P1 and an example of a second part P2. Fig. 7 shows a first part P1 having a rectangular parallelepiped shape and a second part P2 having a shape in which two cylinders are connected so that their central axes intersect. The shapes of the first part P1 and the second part P2 are not limited to the shapes shown in Fig. 7, and various shapes are possible.
[0035] The first part P1 includes a first area A1 and a second area A2. The first area A1 is an area that comes into contact with the second part P2, and is formed as a circular area on the top surface of the first part P1. The first area A1 is also called a "joining area." The second area A2 is an area that does not come into contact with the second part P2.
[0036] In the first step S10, the three-dimensional modeling apparatus 100 plasticizes and discharges a first material containing SUS and a first binder from the first discharge unit 10a to form a first region A1. The three-dimensional modeling apparatus 100 plasticizes and discharges a second material containing SUS and a second binder from the second discharge unit 10b to form a second region A2 other than the first region A1. In this embodiment, the inorganic powder used in the first region A1 and the inorganic powder used in the second region A2 are the same SUS and contain the same element as a main component. The main component means the main element of the inorganic powder, and refers to the element that occupies the largest content in the inorganic powder.
[0037] In this embodiment, the first binder and the second binder each contain a resin and a wax. However, by using different types of resin for the first binder and the second binder, the melting point of the first binder contained in the first region A1 is lower than the melting point of the second binder contained in the second region A2. More specifically, the melting point of the first binder is lower than the temperature at which the wax component is removed in the degreasing process described later, and the melting point of the second binder is higher than the temperature at which the wax component is removed in the degreasing process described later. The first binder can also be called a low melting point binder, and the second binder can also be called a high melting point binder.
[0038] The resin used for the first binder and the resin used for the second binder can be selected from general-purpose engineering plastics such as polystyrene resin (PS), polyethylene resin (PE), polypropylene resin (PP), polyacetal resin (POM), polyvinyl chloride resin (PVC), polyamide resin (PA), acrylonitrile-butadiene-styrene resin (ABS), polylactic acid resin (PLA), polyphenylene sulfide resin (PPS), polycarbonate (PC), modified polyphenylene ether, polybutylene terephthalate, and polyethylene terephthalate, and thermoplastic resins such as polysulfone, polyethersulfone, polyphenylene sulfide, polyarylate, polyimide, polyamideimide, polyetherimide, and polyetheretherketone (PEEK), so long as they satisfy the melting points described above.
[0039] In this embodiment, since the first part P1 is formed by the three-dimensional printing apparatus 100, it is difficult to form the first part P1 into a small, complex shape, but it is possible to form the first part P1 into a relatively large shape.
[0040] In this embodiment, the first material and the second material contain SUS as inorganic powder, but it is not limited to SUS, and may be a single metal such as magnesium (Mg), iron (Fe), cobalt (Co), chromium (Cr), aluminum (Al), titanium (Ti), copper (Cu), or nickel (Ni), or an alloy containing one or more of these metals, or an alloy such as maraging steel, cobalt chromium molybdenum, titanium alloy, nickel alloy, aluminum alloy, cobalt alloy, or cobalt chromium alloy. In addition, the inorganic powder is not limited to metal, and may be oxide ceramics such as silicon dioxide, titanium dioxide, aluminum oxide, or zirconium oxide, or non-oxide ceramics such as aluminum nitride.
[0041] In this embodiment, the second part P2 is molded in the second step S20 by injecting the same material as that of the second region A2 of the first part P1 into the molding die 220 by the injection molding machine 200. The inorganic powder used in the second part P2 may be different from the inorganic powder used in the first part P1. The binder resin used in the second part P2 may be a different type of resin from that used in the second region A2 of the first part P1, as long as the resin has a melting point higher than the temperature at which the wax component is removed in the degreasing process described below.
[0042] In this embodiment, since the second part P2 is molded by the injection molding machine 200, it is difficult to make the second part P2 large in shape, but it can be made small and have a complex shape without using support materials, etc.
[0043] In the third step S30, the first part P1 and the second part P2 are assembled to obtain an assembly. The assembly of the first part P1 and the second part P2 can be performed, for example, by a robot. In this embodiment, as shown in Fig. 7, the assembly is performed by placing the second part P2 on the first area A1 of the first part P1. Fig. 8 shows an assembly AB in which the first part P1 and the second part P2 are assembled.
[0044] In the fourth step S40, a degreasing process is performed by the degreasing device 300, in which the assembly AB is heated at a first temperature to perform degreasing. The first temperature is a temperature for removing wax components contained in the first part P1 and the second part P2, and is, for example, 110°C. The melting point of the resin contained in the first region A1 of the first part P1 is a temperature lower than the first temperature. Therefore, the first region A1 is softened by the degreasing process, and the first part P1 and the second part P2 are in good contact with each other in the first region A1. In the fourth step S40, after the wax components are removed by the first temperature, the first temperature is increased to 400 to 500°C to remove the resin components in the binder contained in the assembly AB.
[0045] In a fifth step S50, the degreased assembly AB is heated and sintered at a second temperature higher than the first temperature in a sintering furnace 400. The second temperature is, for example, 1200° C. Through the series of steps described above, a product made up of the first part P1 and the second part P2 is manufactured.
[0046] According to the manufacturing method of the product in the first embodiment described above, by switching between multiple materials using the three-dimensional modeling apparatus 100 equipped with multiple discharge units 10, a material having a binder with a low melting point can be selectively placed in the first area A1, which is the joining area of the first part P1 and the second part P2. Therefore, when the first part P1 and the second part P2 are heated and degreased, it is possible to prevent the binder component of the first part P1 from melting in the joining area and the generation of a gap between the first part P1 and the second part P2. As a result, a product can be manufactured by joining multiple parts well using a simple method.
[0047] In this embodiment, since the second part P2 is molded by the injection molding machine 200, the second part P2 can be generated in a short time, and the second part P2 having a complex shape can be manufactured without using support materials. In this embodiment, since the first part P1 is molded by the three-dimensional printing device 100, a hollow structure or a lightening structure can be easily formed, and a large first part P1 can be molded. Therefore, by joining the first part P1 and the second part P2, a large product having a complex shape and not dependent on the size of the mold of the injection molding machine 200 can be manufactured.
[0048] In this embodiment, the inorganic powder contained in the first region A1 of the first component P1 contains the same elements as the inorganic powder contained in the second region A2 as main components, so that the first component P1 and the second component P2 can be joined without using wax or the like in the joining regions, thereby preventing a decrease in the strength of the product in the joining regions.
[0049] B. Second embodiment: In the second embodiment, the configuration of the manufacturing system 5 and the series of steps of the product manufacturing method are the same as those in the first embodiment. In the first embodiment, binders having different melting points are used for the first material used to form the first region A1 of the first part P1 and the second material used to form the second region A2. In contrast, in the second embodiment, the particle size of the inorganic powder of the first material used to form the first region A1 of the first part P1 is made smaller than the particle size of the inorganic powder of the second material used to form the second region A2. In this embodiment, the particle size means the median particle size.
[0050] More specifically, in the second embodiment, SUS with a median particle size of 5 μm is used as the inorganic powder contained in the first material. SUS with a median particle size of 10 μm is used as the inorganic powder contained in the second material. In this way, by using a powder with a small particle size in the first region A1, which is the joining region where the first part P1 and the second part P2 are joined, diffusion bonding in the joining region during sintering is promoted, and the sintering start temperature in the joining region can be lowered. For example, when SUS with a median particle size of 5 μm is used as the inorganic powder contained in the first material and SUS with a median particle size of 10 μm is used as the inorganic powder contained in the second material, the sintering start temperature in the joining region can be lowered from 1200° C. to 1150° C. As a result, the first part P1 and the second part P2 can be joined well starting from the first region A1 of the first part P1.
[0051] According to the second embodiment described above, the three-dimensional modeling apparatus 100 can place a material having an inorganic powder with a small particle size in the joining region of the first part P1 and the second part P2. Therefore, when sintering the first part P1 and the second part P2, sintering starts early in the joining region, and they can be joined well. As a result, a product can be manufactured by joining multiple parts by a simple method. In this embodiment, the types of binders contained in the first material and the second material may be the same or different. However, as in the first embodiment, it is preferable that the melting point of the first binder contained in the first material is lower than the melting point of the second binder contained in the second material.
[0052] C. Third embodiment: In the third embodiment, the configuration of the manufacturing system 5 and the series of steps in the product manufacturing method are the same as those in the first embodiment.
[0053] In the third embodiment, the particle density of the inorganic powder in the first material used in the three-dimensional modeling apparatus 100 is made higher than the particle density of the inorganic powder in the second material, so that the particle density of the first region A1 of the first part P1 is made higher than the particle density of the second region A2 of the first part P1 before the fourth step S40 shown in FIG. 6, i.e., before the degreasing process. Specifically, the particle density of the first material is increased by making the number of binder parts of the first material used in the first region A1 smaller than the number of binder parts of the second material used in the second region A2. For example, in this embodiment, the composition of the first material used in the first region A1 is 7.0g of binder with respect to 100g of SUS, so that the number of binder parts is 7.0, and the composition of the second material used in the second region A2 is 8.5g of binder with respect to 100g of SUS, so that the number of binder parts is 8.5.
[0054] According to the third embodiment described above, by reducing the particle density of the first region A1 included in the first part P1, the interval between the inorganic particles included in the first part P1 and the inorganic particles included in the second part P2 in the assembly AB can be narrowed. Therefore, it is possible to prevent the joint between the first part P1 and the second part P2 from becoming weak after sintering. The types of resin and binder included in the first material and the second material are the same as those in the first embodiment. Also, the particle size of the inorganic particles may be the same in the first material and the second material, or may be different in the first material and the second material as in the second embodiment.
[0055] D. Fourth embodiment: FIG. 9 is a diagram showing a schematic configuration of a manufacturing system 5d in the fourth embodiment. The manufacturing system 5d includes a first three-dimensional modeling device 101, a second three-dimensional modeling device 102, a degreasing device 300, and a sintering furnace 400. That is, in the fourth embodiment, the manufacturing system 5d includes the second three-dimensional modeling device 102 instead of the injection molding machine 200. The configurations of the first three-dimensional modeling device 101 and the second three-dimensional modeling device 102 are the same as the configuration of the three-dimensional modeling device 100 in the first embodiment. The first three-dimensional modeling device 101 and the second three-dimensional modeling device 102 include a hopper 20, a plasticizing unit 30, and a nozzle 60, respectively. In the fourth embodiment, any of the materials described in the first to third embodiments can be used as the material used to manufacture the product.
[0056] FIG. 10 is a process diagram showing a method for manufacturing a product in the fourth embodiment. In this embodiment, in the first step S10, a first part P1 is formed by the first three-dimensional modeling device 101. In the second step S20d, a second part is formed by the second three-dimensional modeling device 102, not by the injection molding machine 200. The order of the first step S10 and the second step S20d is arbitrary, and they may be performed simultaneously. The processing contents of the third step S30 to the fifth step S50 are the same as those of the first embodiment. Through the series of steps described above, in this embodiment, a product is manufactured by joining the first part and the second part formed by the three-dimensional modeling device.
[0057] According to the fourth embodiment described above, the first part P1 and the second part P2 are formed and joined by the 3D printing apparatuses 101, 102, so that it is possible to manufacture products larger than the size that can be formed at one time by the 3D printing apparatuses 101, 102. This increases the degree of freedom in product design.
[0058] In this embodiment, both the first 3D modeling device 101 and the second 3D modeling device 102 are equipped with the hopper 20, so the first part P1 and the second part P2 can be modeled using the same type of pellets in the first 3D modeling device 101 and the second 3D modeling device 102. This makes it possible to suppress changes in physical properties between the first part P1 and the second part P2, thereby improving product quality.
[0059] E. Fifth embodiment: 11 is a diagram showing a schematic configuration of a manufacturing system 5e in the fifth embodiment. The manufacturing system 5e includes a three-dimensional modeling apparatus 100, a degreasing apparatus 300, and a sintering furnace 400. That is, the manufacturing system 5e in the fifth embodiment includes only one three-dimensional modeling apparatus 100, and does not include an injection molding machine 200.
[0060] Fig. 12 is a process diagram showing a method for manufacturing a product in the fifth embodiment. Fig. 13 is an explanatory diagram showing an overview of the method for manufacturing a product in the fifth embodiment. In this embodiment, in the first step S10e, the first part P1 and the second part P2 are formed in parallel on the same stage 80 by the three-dimensional printing apparatus 100. The left side of Fig. 13 shows the state in which the elongated first part P1 and second part P2 are formed along the vertical direction. In the first step S10e of this embodiment, it can be said that the first step for forming the first part P1 and the second step for forming the second part P2 are performed simultaneously.
[0061] In the third step S30, the first part P1 and the second part P2 are assembled. The right side of FIG. 13 shows an assembly AB in which the first part P1 and the second part P2 are assembled, arranged in the degreasing device 300. In this embodiment, the first region A1 is shaped to have a step at the end of the first part P1, and when the first part P1 and the second part P2 are assembled, the step formed at the end of the second part P2 is arranged to overlap with the step. The assembly AB assembled in this manner is degreased in the fourth step S40 and sintered in the fifth step S50. Note that the shape of the joint portion of the first part P1 and the second part P2 is not limited to the shape shown in FIG. 13, and for example, it is also possible to make one of the joint portions convex and the other joint portion concave.
[0062] According to the fifth embodiment described above, the first part P1 and the second part P2 can be simultaneously formed in parallel by one 3D printing apparatus 100, so that products can be manufactured efficiently. In addition, the space efficiency when forming the first part P1 and the second part P2 can be improved. Furthermore, since the first part P1 and the second part P2 can be produced under the same environmental conditions such as humidity and temperature, it is possible to prevent the quality of the products from becoming uneven for each part. In addition, it is possible to manufacture products of sizes that exceed the maximum size that can be formed by the 3D printing apparatus 100.
[0063] The present disclosure is not limited to the above-described embodiment, and the first part P1 may be formed by a three-dimensional printing apparatus of a different type, such as a binder jet type or a material jet type.
[0064] F. Other forms: The present disclosure is not limited to the above-mentioned embodiment, and can be realized in various configurations without departing from the spirit of the present disclosure. For example, the technical features of the embodiments corresponding to the technical features in each form described below can be appropriately replaced or combined in order to solve some or all of the above-mentioned problems or to achieve some or all of the above-mentioned effects. Furthermore, if a technical feature is not described as essential in this specification, it can be appropriately deleted.
[0065] (1) According to a first aspect of the present disclosure, there is provided a manufacturing method for manufacturing a product by bonding a first part containing an inorganic powder and a binder to a second part containing an inorganic powder and a binder. The manufacturing method includes a first step of generating the first part by a three-dimensional printing apparatus, a second step of generating the second part, a third step of assembling the first part and the second part to obtain an assembly, a fourth step of heating the assembly at a first temperature, and a fifth step of heating the assembly at a second temperature higher than the first temperature after the fourth step, wherein the first part has a first region in contact with the second part and a second region not in contact with the second part, and the melting point of the binder contained in the first region is lower than the melting point of the binder contained in the second region. In this embodiment, the three-dimensional printing apparatus can place a material having a binder with a low melting point in the joining region of the first part with the second part. Therefore, when the first part and the second part are heated and degreased in the fourth step, the binder component of the first part melts in the joining region, preventing a gap from being generated between the first part and the second part. As a result, a product can be manufactured by joining multiple parts well using a simple method.
[0066] (2) According to a second aspect of the present disclosure, there is provided a manufacturing method for manufacturing a product by bonding a first part containing an inorganic powder and a binder to a second part containing an inorganic powder and a binder, the manufacturing method including a first step of generating the first part by a three-dimensional printing apparatus, a second step of generating the second part, a third step of assembling the first part and the second part to obtain an assembly, a fourth step of heating the assembly at a first temperature, and a fifth step of heating the assembly at a second temperature higher than the first temperature after the fourth step, the first part has a first region in contact with the second part and a second region not in contact with the second part, and the particle size of the inorganic powder contained in the first region is smaller than the particle size of the inorganic powder contained in the second region. In this embodiment, the three-dimensional modeling device can place a material containing inorganic powder with a small particle size in the joining region of the first part with the second part. Therefore, when the first part and the second part are sintered in the fifth step, sintering starts early in the joining region, and they can be joined well. As a result, a product can be manufactured by joining multiple parts well using a simple method.
[0067] (3) In the above embodiment, in the second step, the second part may be produced by an injection molding machine. In this embodiment, since the second part is produced by the injection molding machine, a second part having a complex shape can be manufactured without using a support material. Also, since the first part is modeled by a three-dimensional modeling device, a large first part can be modeled. Therefore, by joining the first part and the second part, a large product having a complex shape can be manufactured.
[0068] (4) In the above embodiment, the second part may be generated by a three-dimensional printing device in the second step. In this embodiment, the first part and the second part are printed by the three-dimensional printing device and then joined together, so that a product larger than the size that can be printed at one time by the three-dimensional printing device can be manufactured.
[0069] (5) In the above embodiment, the 3D modeling device used in the first step and the 3D modeling device used in the second step may each include a hopper into which a pellet-shaped material is fed, a plasticizing unit that plasticizes the material, and a nozzle that discharges the plasticized material. In this embodiment, the first and second 3D modeling devices can generate the first and second parts using the same type of pellets, thereby suppressing changes in physical properties between the first and second parts.
[0070] (6) In the above embodiment, the 3D printing device used in the first step and the 3D printing device used in the second step may be the same 3D printing device, and the first part and the second part may be generated in parallel on the same stage provided in the 3D printing device. In this embodiment, it is possible to improve space efficiency when generating the first part and the second part, and also to suppress unevenness in product quality between parts, since the first part and the second part can be generated under the same environmental conditions such as humidity and temperature.
[0071] (7) In the above embodiment, a particle density of the inorganic powder in the first region may be higher than a particle density of the inorganic powder in the second region before the fourth step. With this embodiment, it is possible to prevent a bonded portion between the first component and the second component from becoming brittle after sintering.
[0072] (8) In the above embodiment, the inorganic powder contained in the first region may contain the same element as the inorganic powder contained in the second region as a main component. In this embodiment, the first component and the second component can be joined without using wax or the like in the joining region. Therefore, a decrease in the strength of the product in the joining region can be suppressed. [Explanation of symbols]
[0073] 5... manufacturing system, 10... discharge section, 20... hopper, 22... supply path, 30... plasticizing section, 31... screw case, 32... drive motor, 41... screw, 42... groove forming surface, 43... side, 44... material inlet, 45... screw groove, 46... convex rib section, 47... screw center, 50... barrel, 52... screw facing surface, 54... guide groove, 56... communication hole, 58... heater, 60... nozzle, 63... nozzle opening, 70... movement mechanism section, 80... stage, 90... control section, 100... three-dimensional modeling device, 101... first three-dimensional modeling device, 102... second three-dimensional modeling device, 200... injection molding machine, 205... base, 208... material supply section, 210... plasticizing device, 211... screw, 212... barrel, 213... heater, 214... nozzle, 215... storage section, 216... screw drive section, 217... communication hole, 218... check valve, 220... mold, 221... movable mold, 222... fixed mold, 223... cavity, 230... mold clamping device, 231... mold drive section, 232... ball screw, 240... injection control mechanism, 241... injection cylinder, 242... plunger, 243... plunger drive section, 290... control section, 300... degreasing device, 400... sintering furnace
Claims
1. A first part including an inorganic powder and a binder; and a second part including an inorganic powder and a binder. A manufacturing method for manufacturing a product by joining a first step of generating the first part by a three-dimensional modeling device; a second step of generating the second part; a third step of assembling the first part and the second part to obtain an assembly; a fourth step of heating the assembly at a first temperature; After the fourth step, the assembly is sintered by heating it at a second temperature higher than the first temperature. A fifth step, Equipped with The first part has a first region that contacts the second part and a second region that does not contact the second part. and The melting point of the binder contained in the first region is greater than the melting point of the binder contained in the second region. A manufacturing method that is lower than the standard.
2. A first part including an inorganic powder and a binder; and a second part including an inorganic powder and a binder. A manufacturing method for manufacturing a product by joining a first step of generating the first part by a three-dimensional modeling device; a second step of generating the second part; a third step of assembling the first part and the second part to obtain an assembly; a fourth step of heating the assembly at a first temperature; After the fourth step, the assembly is sintered by heating it at a second temperature higher than the first temperature. A fifth step, Equipped with The first part has a first region that contacts the second part and a second region that does not contact the second part. Having an area, The particle size of the inorganic powder contained in the first region is larger than the particle size of the inorganic powder contained in the second region. Smaller in comparison, manufacturing method.
3. The method according to claim 1 or 2, In the second step, the second part is produced by an injection molding machine.
4. The method according to any one of claims 1 to 3, In the second step, the second part is generated by a three-dimensional modeling apparatus.
5. The method according to claim 4, further comprising the steps of: The three-dimensional modeling apparatus used in the first step and the three-dimensional modeling apparatus used in the second step The three-dimensional modeling apparatus used has a hopper into which pellet-shaped material is fed, A plasticizing unit that plasticizes the material, and a nozzle that discharges the plasticized material. A manufacturing method.
6. The method according to claim 5, The three-dimensional modeling apparatus used in the first step and the three-dimensional modeling apparatus used in the second step The 3D modeling device used is the same 3D modeling device, The first part and the second part are placed on the same stage of the three-dimensional modeling apparatus. Parallel production,methods.
7. The method according to any one of claims 1 to 6, Prior to the fourth step, the particle density of the inorganic powder in the first region is The particle density of the inorganic powder in the second region is higher than that in the first region.
8. The method according to any one of claims 1 to 7, The inorganic powder contained in the first region is the same as the inorganic powder contained in the second region. A manufacturing method that includes the element as a main component.
Citation Information
Patent Citations
Ceramic composition, product thereof and preparation method thereof
CN112010641A
Production of sintered composite mechanical parts
JP1994330108A
Method for manufacturing three dimensional molding, component, and manufacturing program
JP2018094817A
3-D printed materials, structures and processes
US10751951B1
Method for improved manufacturing of a dual microstructure part
US20200180083A1