Optical film and method for producing same
By contacting a crystalline polymer resin film with a solvent below its glass transition temperature, the method addresses the complexity and inefficiency of conventional optical film production, achieving an NZ coefficient of less than 1.0 and low solvent content in optical films.
Patent Information
- Application Number
- JP2020219540
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-12-28
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2040-12-28
AI Technical Summary
Conventional methods for producing optical films with an NZ coefficient of less than 1.0 are complex and often result in high solvent content, requiring precise thickness adjustments and multiple steps, and are inefficient in changing birefringence in the thickness direction.
A method involving a resin film formed of a crystalline polymer contacted with a solvent having a boiling point lower than its glass transition temperature to change birefringence in the thickness direction, with controlled temperature and solvent content to achieve an NZ coefficient of less than 1.0 and low solvent content.
The method allows for the production of optical films with an NZ coefficient of less than 1.0 and low solvent content, enhancing display quality and efficiency by simplifying the manufacturing process and reducing solvent retention.
Smart Images

Figure 0007567473000001
Abstract
Description
[Technical field]
[0001] The present invention relates to an optical film and a method for producing the same. [Background technology]
[0002] 2. Description of the Related Art Conventionally, techniques for producing films using resins have been proposed (Patent Document 1). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] International Publication No. 2017 / 065222 Summary of the Invention [Problem to be solved by the invention]
[0004] Resins may be used to manufacture optical films having anisotropy in refractive index. Such optical films having anisotropy in refractive index may have birefringence. Optical films having birefringence may be provided in display devices as films such as anti-reflection films and viewing angle compensation films.
[0005] When an optical film is provided in a display device, it is required to appropriately adjust the balance between the birefringence in the thickness direction and the birefringence in the in-plane direction perpendicular to the thickness direction. The balance between the birefringence in the thickness direction and the birefringence in the in-plane direction can be expressed by the NZ coefficient of the optical film. For example, if an optical film with an NZ coefficient of less than 1.0 is obtained, the optical film can improve the display quality of the display device, such as the viewing angle, contrast, and image quality.
[0006] A method for manufacturing an optical film having an NZ coefficient of less than 1.0 has been known in the past. However, the conventional manufacturing method could not easily manufacture an optical film having an NZ coefficient of less than 1.0. For example, the method described in Patent Document 1 requires a combination of film stretching and shrinkage, or requires the use of a film having multiple layers with precisely adjusted thickness. Therefore, the manufacturing method tends to be complicated due to the large number of control items and steps.
[0007] In view of the above circumstances, the present inventors have studied a manufacturing method for easily manufacturing an optical film having an NZ coefficient of less than 1.0. As a result, the present inventors have found that when a resin film formed of a resin containing a crystalline polymer is brought into contact with a solvent, the birefringence of the resin film in the thickness direction can be changed. Then, the present inventors have found that by utilizing such contact between a resin film and a solvent, an optical film having an NZ coefficient of less than 1.0 can be manufactured.
[0008] However, optical films produced through contact between a resin film and a solvent tend to contain a large amount of solvent. Although it is difficult to completely eliminate the amount of solvent contained in an optical film, it is desirable to reduce the amount of solvent as much as possible.
[0009] In addition, in a method for producing an optical film by utilizing a change in birefringence in the thickness direction caused by contact of a resin film with a solvent, a long contact time is required to obtain a large change in birefringence in the thickness direction. In order to increase production efficiency, it is desirable to increase the rate of change in birefringence in the thickness direction caused by contact of a resin film with a solvent.
[0010] The present invention has been devised in view of the above problems. Specifically, a first object of the present invention is to provide an optical film having an NZ coefficient of less than 1.0 and a low solvent content, and a method for producing the same. A second object of the present invention is to provide a method for producing an optical film, which includes changing the birefringence in the thickness direction of a resin film by contacting the resin film with a solvent, and which can accelerate the rate of change in the birefringence in the thickness direction due to contacting the resin film with the solvent. [Means for solving the problem]
[0011] The present inventors have conducted intensive research to solve the above-mentioned problems. As a result, the present inventors have found that the first problem can be solved by a method for producing an optical film including a step of contacting a resin film formed of a resin containing a crystalline polymer with a solvent having a boiling point lower than the glass transition temperature of the crystalline polymer to change the birefringence in the thickness direction. The present inventors have also found that the second problem can be solved by a method for producing an optical film including a step of contacting a resin film formed of a resin containing a crystalline polymer with a solvent at a specific temperature to change the birefringence in the thickness direction. The present invention has been completed based on the above-mentioned findings. That is, the present invention includes the following.
[0012] [1] An optical film formed of a resin containing a crystalline polymer, the optical film contains 0.01% by weight to 5% by weight of a solvent having a boiling point lower than the glass transition temperature of the crystalline polymer; The optical film has an NZ coefficient of less than 1.0. [2] The optical film according to [1], wherein the crystalline polymer has positive intrinsic birefringence. [3] The optical film according to [1] or [2], wherein the crystalline polymer contains an alicyclic structure. [4] The optical film according to any one of [1] to [3], wherein the crystallinity of the crystalline polymer measured by X-ray diffraction is 10% or more. [5] A method for producing the optical film according to any one of [1] to [4], A step (i) of preparing a resin film formed of a resin containing a crystalline polymer; and (ii) contacting the resin film with a solvent having a boiling point lower than the glass transition temperature of the crystalline polymer to change the birefringence in the thickness direction. [6] The method for producing an optical film according to [5], wherein the temperature of the solvent in contact with the resin film is 30° C. to 80° C. and lower than the boiling point of the solvent. [7] A step (i) of preparing a resin film formed of a resin containing a crystalline polymer; and (ii) contacting the resin film with a solvent to change the birefringence in the thickness direction, The method for producing an optical film, wherein the temperature of the solvent in contact with the resin film is 30° C. to 80° C. and is lower than the boiling point of the solvent. [8] The method for producing an optical film according to [7], wherein the solvent has a boiling point lower than the glass transition temperature of the crystalline polymer. [9] The method for producing an optical film according to any one of [5] to [8], wherein the step (i) includes melt-extruding the resin.
[10] The method for producing an optical film according to any one of [5] to [9], comprising, after the step (ii), a step (iii) of stretching the resin film.
[11] The method for producing an optical film according to
[10] , wherein the amount of the solvent contained in the produced optical film is 1 wt % or less. Effect of the Invention
[0013] According to the present invention, firstly, it is possible to provide an optical film having an NZ coefficient of less than 1.0 and a small amount of solvent, and a manufacturing method thereof. Alternatively, according to the present invention, secondly, it is possible to provide a manufacturing method of an optical film including changing the birefringence in the thickness direction of a resin film by contacting the resin film with a solvent, which can increase the rate of change in the birefringence in the thickness direction due to contacting the resin film with the solvent. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] The present invention will be described in detail below with reference to embodiments and examples. However, the present invention is not limited to the embodiments and examples shown below, and may be modified and implemented as desired without departing from the scope of the claims of the present invention and their equivalents.
[0015] In the following description, the in-plane retardation Re of the film is a value expressed by Re = (nx - ny) x d unless otherwise specified. The birefringence in the in-plane direction of the film is a value expressed by (nx - ny) unless otherwise specified, and is therefore expressed by Re / d. The retardation Rth in the thickness direction of the film is a value expressed by Rth = [{(nx + ny) / 2} - nz] x d unless otherwise specified. The birefringence in the thickness direction of the film is a value expressed by [{(nx + ny) / 2} - nz] unless otherwise specified, and is therefore expressed by Rth / d. The NZ coefficient of the film is a value expressed by (nx - nz) / (nx - ny) unless otherwise specified. Here, nx represents the refractive index in the direction perpendicular to the thickness direction of the film (in-plane direction) and giving the maximum refractive index. ny represents the refractive index in the in-plane direction of the film and perpendicular to the direction of nx. nz represents the refractive index in the thickness direction of the film. d represents the thickness of the film. The measurement wavelength is 590 nm unless otherwise specified.
[0016] In the following description, unless otherwise specified, a material having positive inherent birefringence means a material whose refractive index in the stretching direction is greater than that in the direction perpendicular thereto. Therefore, a polymer having positive inherent birefringence means a polymer whose refractive index in the stretching direction is greater than that in the direction perpendicular thereto, unless otherwise specified. Furthermore, a material having negative inherent birefringence means a material whose refractive index in the stretching direction is smaller than that in the direction perpendicular thereto, unless otherwise specified. Therefore, a polymer having negative inherent birefringence means a polymer whose refractive index in the stretching direction is smaller than that in the direction perpendicular thereto, unless otherwise specified.
[0017] In the following description, a "long" shape refers to a shape having a length 5 times or more than the width, preferably 10 times or more, specifically a film shape having a length that can be wound into a roll for storage or transportation. There is no particular upper limit on the length, but it is usually 100,000 times or less than the width.
[0018] In the following description, unless otherwise specified, the directions of elements as "parallel," "vertical," and "orthogonal" may include an error within a range that does not impair the effect of the present invention, for example, within a range of ±5°.
[0019] Unless otherwise specified, the terms "polarizing plate," "circularly polarizing plate," and "wave plate" include not only rigid members but also flexible members such as resin films.
[0020] [1. Overview of the Optical Film According to the First Embodiment] The optical film according to the first embodiment of the present invention satisfies the following requirements (A) to (C) in combination. Requirement (A): The optical film is formed of a resin containing a crystalline polymer. Requirement (B): The optical film contains 0.01% by weight to 5% by weight of a solvent having a boiling point lower than the glass transition temperature of the crystalline polymer. Requirement (C): The NZ coefficient of the optical film is less than 1.0.
[0021] Although the above optical film has been difficult to produce in the past, it can be easily produced by using a specific production method described later.
[0022] [2. Resins containing crystalline polymers] The optical film according to the first embodiment is formed of a resin containing a crystalline polymer. The crystalline polymer refers to a polymer having crystallinity. The crystalline polymer refers to a polymer having a melting point Tm (i.e., the melting point Tm can be observed by a differential scanning calorimeter (DSC)). In the following description, a resin containing a crystalline polymer may be referred to as a "crystalline resin". This crystalline resin is preferably a thermoplastic resin. Therefore, the optical film preferably contains a crystalline resin, and more preferably consists of only a crystalline resin.
[0023] The crystalline polymer may have a negative intrinsic birefringence, but preferably has a positive intrinsic birefringence. When a crystalline polymer having a positive intrinsic birefringence is used, an optical film having an NZ coefficient of less than 1.0 can be easily produced.
[0024] The crystalline polymer may be, for example, polyester such as polyethylene terephthalate (PET) or polyethylene naphthalate (PEN); polyolefin such as polyethylene (PE) or polypropylene (PP); and the like, but is not particularly limited, and preferably contains an alicyclic structure. When a crystalline polymer containing an alicyclic structure is used, the mechanical properties, heat resistance, transparency, low moisture absorption, dimensional stability, and light weight of the optical film can be improved. The polymer containing an alicyclic structure refers to a polymer having an alicyclic structure in the molecule. Such a polymer containing an alicyclic structure may be, for example, a polymer obtained by a polymerization reaction using a cyclic olefin as a monomer, or a hydrogenated product thereof.
[0025] Examples of the alicyclic structure include a cycloalkane structure and a cycloalkene structure. Among these, the cycloalkane structure is preferred because it is easy to obtain an optical film having excellent properties such as thermal stability. The number of carbon atoms contained in one alicyclic structure is preferably 4 or more, more preferably 5 or more, and preferably 30 or less, more preferably 20 or less, and particularly preferably 15 or less. When the number of carbon atoms contained in one alicyclic structure is within the above range, mechanical strength, heat resistance, and moldability are highly balanced.
[0026] In the crystalline polymer containing an alicyclic structure, the ratio of the structural unit having an alicyclic structure to all structural units is preferably 30% by weight or more, more preferably 50% by weight or more, and particularly preferably 70% by weight or more. When the ratio of the structural unit having an alicyclic structure is high as described above, heat resistance can be improved. The ratio of the structural unit having an alicyclic structure to all structural units can be 100% by weight or less. In addition, in the crystalline polymer containing an alicyclic structure, the remainder other than the structural unit having an alicyclic structure is not particularly limited and can be appropriately selected according to the purpose of use.
[0027] Examples of the crystalline polymer containing an alicyclic structure include the following polymers (α) to (δ). Among these, polymer (β) is preferred because it is easy to obtain an optical film having excellent heat resistance. Polymer (α): A ring-opening polymer of a cyclic olefin monomer, which has crystallinity. Polymer (β): A hydrogenated product of polymer (α) and has crystallinity. Polymer (γ): An addition polymer of a cyclic olefin monomer, which has crystallinity. Polymer (δ): A hydrogenated polymer (γ) having crystallinity.
[0028] Specifically, the crystalline polymer containing an alicyclic structure is preferably a dicyclopentadiene ring-opening polymer having crystallinity, and a dicyclopentadiene ring-opening polymer hydrogenation product having crystallinity. Among them, a dicyclopentadiene ring-opening polymer hydrogenation product having crystallinity is particularly preferred. Here, the dicyclopentadiene ring-opening polymer refers to a polymer in which the ratio of dicyclopentadiene-derived structural units to all structural units is usually 50% by weight or more, preferably 70% by weight or more, more preferably 90% by weight or more, and even more preferably 100% by weight.
[0029] The hydrogenated ring-opening polymer of dicyclopentadiene preferably has a high ratio of racemo dyads. Specifically, the ratio of racemo dyads in the repeating units of the hydrogenated ring-opening polymer of dicyclopentadiene is preferably 51% or more, more preferably 70% or more, and particularly preferably 85% or more. A high ratio of racemo dyads indicates high syndiotactic stereoregularity. Therefore, the higher the ratio of racemo dyads, the higher the melting point of the hydrogenated ring-opening polymer of dicyclopentadiene tends to be. The ratio of racemo-dyads is described in the Examples below. 13 It can be determined based on C-NMR spectrum analysis.
[0030] As the polymer (α) to polymer (δ), polymers obtained by the production method disclosed in WO 2018 / 062067 can be used.
[0031] The melting point Tm of the crystalline polymer is preferably 200° C. or higher, more preferably 230° C. or higher, and preferably 290° C. or lower. When a crystalline polymer having such a melting point Tm is used, an optical film having an even better balance between formability and heat resistance can be obtained.
[0032] Generally, a crystalline polymer has a glass transition temperature Tg. The specific glass transition temperature Tg of a crystalline polymer is not particularly limited, but is generally 85°C or higher and generally 170°C or lower.
[0033] The glass transition temperature Tg and melting point Tm of a polymer can be measured by the following method. First, the polymer is melted by heating, and the melted polymer is quenched with dry ice. Then, using this polymer as a test specimen, the glass transition temperature Tg and melting point Tm of the polymer can be measured using a differential scanning calorimeter (DSC) at a heating rate of 10° C. / min (heating mode).
[0034] The weight average molecular weight (Mw) of the crystalline polymer is preferably 1,000 or more, more preferably 2,000 or more, and is preferably 1,000,000 or less, more preferably 500,000 or less. A crystalline polymer having such a weight average molecular weight has an excellent balance between moldability and heat resistance.
[0035] The molecular weight distribution (Mw / Mn) of the crystalline polymer is preferably 1.0 or more, more preferably 1.5 or more, and is preferably 4.0 or less, more preferably 3.5 or less. Here, Mn represents the number average molecular weight. A crystalline polymer having such a molecular weight distribution has excellent moldability.
[0036] The weight average molecular weight (Mw) and molecular weight distribution (Mw / Mn) of the polymer can be measured in terms of polystyrene by gel permeation chromatography (GPC) using tetrahydrofuran as a developing solvent.
[0037] The crystallinity of the crystalline polymer contained in the optical film is preferably 10% or more, more preferably 13% or more, and particularly preferably 15% or more. There is no particular upper limit, and it can be, for example, 70% or less. The crystallinity of the crystalline polymer can be measured by X-ray diffraction. In general, when X-ray diffraction measurement is performed on a crystallized crystalline polymer, a peak occurs in the diffracted X-ray intensity at a specific diffraction angle 2θ. When X-ray diffraction measurement is performed on a crystalline polymer contained in an optical film, a peak can be measured at a specific diffraction angle 2θ, and the crystallinity of the crystalline polymer contained in the optical film can be measured by this peak. When X-ray diffraction measurement is performed on a crystalline polymer contained in an optical film, a broad peak can be measured at the specific diffraction angle 2θ. Therefore, the present inventor believes that the value of the crystallinity of the crystalline polymer contained in the optical film may include the influence of diffraction due to factors other than the crystallization of the crystalline polymer. However, the high crystallinity of the crystalline polymer contained in the optical film indicates that the molecules of the crystalline polymer contained in the optical film have an orientation state with regularity that can at least cause X-ray diffraction. Therefore, the crystallinity is a parameter that represents the orientation state of the molecules of the crystalline polymer contained in the optical film, and is therefore considered to be related to the optical properties of the optical film according to this embodiment.
[0038] The crystalline polymer may be used alone or in combination of two or more kinds in any ratio.
[0039] The proportion of the crystalline polymer in the crystalline resin is preferably 50% by weight or more, more preferably 70% by weight or more, and particularly preferably 90% by weight or more. When the proportion of the crystalline polymer is equal to or more than the lower limit of the above range, the birefringence expression and heat resistance of the optical film can be improved. The upper limit of the proportion of the crystalline polymer can be 100% by weight or less.
[0040] The crystalline resin may contain optional components in addition to the crystalline polymer. Examples of the optional components include antioxidants such as phenol-based antioxidants, phosphorus-based antioxidants, and sulfur-based antioxidants; light stabilizers such as hindered amine-based light stabilizers; waxes such as petroleum wax, Fischer-Tropsch wax, and polyalkylene wax; nucleating agents such as sorbitol-based compounds, metal salts of organic phosphoric acids, metal salts of organic carboxylic acids, kaolin, and talc; diaminostilbene derivatives, coumarin derivatives, and azole-based derivatives (e.g., benzoxazole derivatives, benzotriazole derivatives, and benzimide derivatives). Examples of the optional components include fluorescent brighteners such as benzothiazole derivatives, carbazole derivatives, pyridine derivatives, naphthalic acid derivatives, and imidazolone derivatives; ultraviolet absorbers such as benzophenone-based ultraviolet absorbers, salicylic acid-based ultraviolet absorbers, and benzotriazole-based ultraviolet absorbers; inorganic fillers such as talc, silica, calcium carbonate, and glass fibers; colorants; flame retardants; flame retardant assistants; antistatic agents; plasticizers; near-infrared absorbers; lubricants; fillers; and any polymer other than a crystalline polymer, such as a soft polymer. The optional components may be used alone or in combination of two or more types in any ratio. The amount of the optional components may be appropriately determined within a range that does not significantly impair the effects of the present invention. The amount of the optional components may be, for example, within a range that can maintain the total light transmittance of the optical film at 85% or more.
[0041] [3. Solvents contained in optical films] The optical film according to the first embodiment contains a solvent. This solvent is usually incorporated into the film in step (ii) of the method for producing an optical film described below. In detail, all or a part of the solvent incorporated into the film in step (ii) may penetrate into the inside of the polymer. Therefore, even if drying is performed, it is difficult to easily remove the solvent completely. Therefore, the optical film according to the first embodiment contains a solvent.
[0042] The solvent contained in the optical film has a boiling point Bp lower than the glass transition temperature Tg of the crystalline polymer. The difference Tg-Bp between the glass transition temperature Tg of the crystalline polymer and the boiling point Bp of the solvent is preferably 5°C or more, more preferably 10°C or more, even more preferably 20°C or more, and particularly preferably 30°C or more. When the temperature difference Tg-Bp is equal to or higher than the lower limit, the solvent can be effectively dried at a temperature lower than the glass transition temperature Tg of the crystalline polymer. Therefore, the amount of the solvent contained in the optical film can be effectively reduced while suppressing the change in the optical properties of the optical film due to the orientation relaxation. The upper limit of the temperature difference Tg-Bp is not particularly limited, but can be, for example, 80°C or less.
[0043] The boiling point of the solvent can be measured as the equilibrium reflux boiling point by distillation of the solvent at 1 atmosphere according to JIS K 2233.
[0044] The solvent may be one that does not dissolve the crystalline polymer. This solvent is usually an organic solvent. Preferred solvents include, for example, hydrocarbon solvents such as cyclohexane, toluene, limonene, and decalin; and carbon disulfide. The type of solvent may be one type or two or more types.
[0045] The solvent content as a ratio of the solvent contained in the optical film (i.e., a solvent having a boiling point lower than the glass transition temperature of the crystalline polymer) to 100% by weight of the optical film according to the first embodiment is in a specific small range. The specific solvent content is usually 0.01% by weight or more, and usually 5% by weight or less, more preferably 2% by weight or less, even more preferably 1% by weight or less, even more preferably 0.1% by weight or less, and particularly preferably 0.05% by weight or less. An optical film having such a small solvent content can suppress the release of the solvent from the optical film, and therefore can suppress the change in optical properties over time.
[0046] The solvent content of the optical film can be measured by the measurement method described in the Examples.
[0047] [4. NZ coefficient of optical film] The NZ coefficient of the optical film according to the first embodiment is usually less than 1.0. When an optical film having an NZ coefficient of less than 1.0 is provided in a display device, it is possible to improve the display quality of the display device, such as the viewing angle, contrast, and image quality.
[0048] The specific value of the NZ coefficient of the optical film can be appropriately set depending on the application of the optical film. In one example, the range of the NZ coefficient is preferably less than 0.0, more preferably -5.0 or less, even more preferably -10 or less, even more preferably -20 or less, even more preferably -40 or less, even more preferably -70 or less, and particularly preferably -110 or less. In this case, the lower limit is preferably -500 or more, more preferably -300 or more, and particularly preferably -200 or more. Such an optical film having an NZ coefficient of less than 0.0 can be produced, for example, as an optical film before stretching in the optical film production method described later.
[0049] In another example, the range of the NZ coefficient is preferably 0.0 or more, more preferably greater than 0.0, even more preferably 0.1 or more, even more preferably 0.15 or more, particularly preferably 0.2 or more, and may be usually less than 1.0, preferably 0.9 or less, even more preferably 0.85 or less, particularly preferably 0.8 or less. Such an optical film having an NZ coefficient of 0 or more can be produced as a stretched optical film, for example, in the optical film production method described later. In the following description, the stretched optical film may be referred to as an "optically stretched film".
[0050] The NZ coefficient of a film can be calculated from the in-plane retardation Re and the retardation in the thickness direction Rth of the film.
[0051] [5. Layer structure of optical film] The optical film according to the first embodiment may have a multi-layer structure including a plurality of layers, but preferably has a single-layer structure. The single-layer structure refers to a structure having only a single layer having the same composition, and not having a layer having a different composition from the composition. Therefore, it is preferable that the optical film has a single layer formed of the crystalline resin.
[0052] [6. Characteristics of optical films] The optical film according to the first embodiment preferably has an in-plane retardation in an appropriate range depending on its application. For example, the specific in-plane retardation Re of the optical film may be preferably 10 nm or less, more preferably 5 nm or less, and particularly preferably 3 nm or less. In this case, the optical film can function as a negative C plate. The optical film having the in-plane retardation Re in such a range may be manufactured as an optical film before stretching in the manufacturing method of the optical film described later, for example.
[0053] For example, the specific in-plane retardation Re of the optical film can be preferably 100 nm or more, more preferably 110 nm or more, particularly preferably 120 nm or more, and can be preferably 180 nm or less, more preferably 170 nm or less, particularly preferably 160 nm or less. In this case, the optical film can function as a quarter-wave plate. The optical film having the in-plane retardation Re in such a range can be manufactured as an optical stretched film, for example, in the manufacturing method of the optical film described later.
[0054] For example, the specific in-plane retardation Re of the optical film can be preferably 245 nm or more, more preferably 265 nm or more, particularly preferably 270 nm or more, and can be preferably 320 nm or less, more preferably 300 nm or less, particularly preferably 295 nm or less. In this case, the optical film can function as a 1 / 2 wavelength plate. The optical film having the in-plane retardation Re in such a range can be manufactured as an optical stretched film, for example, in the manufacturing method of the optical film described later.
[0055] The optical film according to the first embodiment preferably has a retardation Rth in the thickness direction within an appropriate range depending on the application. For example, the specific retardation Rth of the optical film in the thickness direction is preferably 300 nm or less, more preferably 100 nm or less, even more preferably 30 nm or less, even more preferably less than 0 nm, and is preferably -10,000 nm or more, more preferably -1000 nm or more, and particularly preferably -500 nm or more.
[0056] The retardation of the film can be measured by a phase difference meter ("AxoScan OPMF-1" manufactured by AXOMETRICS).
[0057] The optical film according to the first embodiment preferably has an in-plane birefringence Re / d in an appropriate range depending on the application. For example, the birefringence Re / d in the specific in-plane direction of an optical film is usually 0.00×10 -3 More than 0.01×10 -3 More preferably, 0.05×10 -3 or more, preferably 1.00×10 -3 Less than or equal to 0.80×10 -3 Less than 0.50×10, particularly preferably -3 The following is an example of an optical film having an in-plane birefringence Re / d in such a range.
[0058] For example, the specific in-plane birefringence Re / d of the optical film is preferably 2.0×10 -3 More preferably, 4.0×10 -3 More preferably, 5.0×10 -3 or more, preferably 30.0×10 -3 Less than or equal to 20.0×10 -3 The following is particularly preferably 15.0×10 -3The following is an example of an optical film having an in-plane birefringence Re / d in this range.
[0059] The optical film according to the first embodiment preferably has a birefringence Rth / d in the thickness direction within an appropriate range depending on the application. For example, the specific birefringence Rth / d of the optical film in the thickness direction is preferably −30.0×10 -3 More preferably, -20.0×10 -3 More preferably, −10.0×10 -3 or more, preferably -1.0×10 -3 Less than or equal to -2.0×10 -3 Less than or equal to -4.0×10 is particularly preferable. -3 The following is an example of an optical film having a birefringence Rth / d in the thickness direction within such a range.
[0060] For example, the specific birefringence Rth / d of the optical film in the thickness direction is preferably −1.0×10 -3 or more, preferably -0.5×10 -3 More preferably, -0.1×10 -3 or more, preferably 30.0×10 -3 Less than or equal to 10.0×10 -3 Less than 5.0×10 -3 The following is an example of an optical film having a birefringence Rth / d in the thickness direction within such a range.
[0061] The optical film preferably has high transparency. The specific total light transmittance of the optical film is preferably 80% or more, more preferably 85% or more, and particularly preferably 88% or more. The total light transmittance of the film can be measured in the wavelength range of 400 nm to 700 nm using an ultraviolet-visible spectrometer.
[0062] The optical film preferably has a small haze. The haze of the optical film is preferably less than 1.0%, more preferably less than 0.8%, particularly preferably less than 0.5%, and ideally 0.0%. When an optical film having such a small haze is provided in a display device, the clarity of the image displayed on the display device can be increased. The haze of the film can be measured using a haze meter (for example, "NDH5000" manufactured by Nippon Denshoku Industries Co., Ltd.).
[0063] The optical film may be a film that has not been subjected to a stretching process, or may be an optically stretched film that has been subjected to a stretching process. When the optical film is an optically stretched film, the optically stretched film is preferably a uniaxially stretched film. A uniaxially stretched film refers to a film that is actively stretched in only one direction and is not actively stretched in any other direction. Since a uniaxially stretched film can be produced by stretching in only one direction, the production process can be simplified, and therefore easy production can be realized.
[0064] The optical film may be a sheet of film or a long film having a long shape. When the optical film has a long shape, the optical film and a long polarizing film are bonded together to continuously produce a polarizing plate.
[0065] The thickness of the optical film can be appropriately set depending on the application of the optical film. The specific thickness of the optical film is preferably 5 μm or more, more preferably 10 μm or more, particularly preferably 30 μm or more, and is preferably 400 μm or less, more preferably 300 μm or less, particularly preferably 200 μm or less.
[0066] [7. Method for producing optical film according to the first embodiment] The optical film according to the first embodiment is (i) preparing a resin film formed of a crystalline resin; (ii) contacting the resin film with a solvent having a boiling point lower than the glass transition temperature Tg of the crystalline polymer to change the birefringence in the thickness direction; It can be produced by a production method including the steps of:
[0067] The present inventors speculate that the mechanism by which an optical film is obtained by the above-mentioned manufacturing method is as follows, although the technical scope of the present invention is not limited to the mechanism described below.
[0068] When a resin film formed of a crystalline resin containing a crystalline polymer is brought into contact with a solvent, the solvent penetrates into the resin film. The action of the penetrating solvent causes micro-Brownian motion in the molecules of the crystalline polymer in the film, and the molecular chains are oriented. According to the study by the present inventors, it is believed that the solvent-induced crystallization phenomenon of the crystalline polymer may progress during this orientation of the molecular chains.
[0069] Incidentally, the surface area of the resin film is large on the front surface and the back surface, which are the main surfaces. Therefore, the penetration speed of the solvent is high in the thickness direction through the front surface or the back surface. Then, the orientation of the molecules of the crystalline polymer can proceed so that the molecules of the polymer are oriented in the thickness direction. By orienting the molecules of the crystalline polymer in the thickness direction, the birefringence in the thickness direction changes, so that the NZ coefficient of the resin film can be adjusted. Therefore, the resin film after contact with the solvent can be obtained as an optical film having an NZ coefficient of less than 1.0.
[0070] In addition, the solvent has a boiling point lower than the glass transition temperature Tg of the crystalline polymer. Therefore, the drying of the solvent can be effectively promoted at a temperature lower than the glass transition temperature Tg of the crystalline polymer. In this way, the solvent can be removed while suppressing the change in the orientation state of the crystalline polymer due to high temperature, so that the amount of solvent in the film can be effectively reduced while suppressing the change in optical properties such as the NZ coefficient. Therefore, an optical film having desired optical properties and a low solvent content can be obtained.
[0071] The above-mentioned method for producing an optical film may further include any step in combination with step (i) and step (ii). For example, the method for producing an optical film may include step (iii) of stretching a resin film after step (ii). When step (iii) is performed, an optical film (i.e., an optically stretched film) can be obtained as a resin film whose properties are adjusted by the stretching in step (iii). In addition, for example, the method for producing an optical film may include step (iv) of drying the resin film after step (ii).
[0072] [8. Step (i) of preparing a resin film] The method for producing an optical film according to the first embodiment includes a step (i) of preparing a resin film made of a crystalline resin containing a crystalline polymer. The crystalline resin used as the material of the resin film prepared in the step (i) may be the same as the crystalline resin contained in the optical film.
[0073] However, the crystallinity of the crystalline polymer contained in the resin film is preferably small. The specific crystallinity is preferably less than 10%, more preferably less than 5%, and particularly preferably less than 3%. If the crystallinity of the crystalline polymer contained in the resin film before contact with the solvent is low, many molecules of the crystalline polymer can be oriented in the thickness direction by contact with the solvent, so that the NZ coefficient can be adjusted in a wide range.
[0074] The resin film preferably has a small solvent content, and more preferably does not contain a solvent. The ratio of the solvent contained in the resin film to 100% by weight of the resin film (solvent content) is preferably 1% or less, more preferably 0.5% or less, particularly preferably 0.1% or less, and ideally 0.0%. Since the amount of solvent contained in the resin film before contact with the solvent is small, many crystalline polymer molecules can be oriented in the thickness direction by contact with the solvent, making it possible to adjust the NZ coefficient in a wide range. The solvent content of the resin film can be measured by its density.
[0075] The resin film preferably has optical isotropy. Therefore, the resin film preferably has a small birefringence Re / d in the in-plane direction, and preferably has a small absolute value |Rth / d| of birefringence in the thickness direction. Specifically, the birefringence Re / d in the in-plane direction of the resin film is preferably 1.0×10 -3 less than 0.5×10 -3 less than 0.3×10 -3 The absolute value of birefringence in the thickness direction of the resin film |Rth / d| is preferably less than 1.0×10 -3 less than 0.5×10 -3 less than 0.3×10 -3 The optical isotropy indicates that the orientation of the crystalline polymer molecules contained in the resin film is low and substantially non-oriented. When such an optically isotropic resin film is used, precise control of the optical properties of the resin film is not required, and therefore precise control of the orientation of the crystalline polymer molecules is not required, so that the manufacturing method of the optical film can be simplified. Furthermore, when an optically isotropic resin film is used, an optical film with small haze can usually be obtained.
[0076] The haze of the resin film is preferably less than 1.0%, preferably less than 0.8%, more preferably less than 0.5%, and ideally 0.0%. The smaller the haze of the resin film, the easier it is to reduce the haze of the resulting optical film.
[0077] The thickness of the resin film is preferably set according to the thickness of the optical film to be produced. Usually, the thickness is increased by contacting with a solvent in step (ii). On the other hand, when stretching is performed in step (iii), the thickness is decreased by the stretching. Therefore, the thickness of the resin film may be set in consideration of the change in thickness in the steps after step (ii) as described above.
[0078] The resin film may be a sheet-like film, but is preferably a long film. By using a long resin film, the optical film can be continuously produced by a roll-to-roll method, and the productivity of the optical film can be effectively improved.
[0079] As a method for producing the resin film, a resin molding method such as an injection molding method, an extrusion molding method, a press molding method, an inflation molding method, a blow molding method, a calendar molding method, a cast molding method, a compression molding method, etc. is preferable because a resin film containing no solvent can be obtained. Among these, an extrusion molding method including melt extrusion of a crystalline resin is preferable because the thickness can be easily controlled.
[0080] The manufacturing conditions in the extrusion molding method are preferably as follows. The cylinder temperature (molten resin temperature) is preferably Tm or higher, more preferably "Tm+20°C" or higher, and preferably "Tm+100°C" or lower, more preferably "Tm+50°C" or lower. The cooling body that the molten resin extruded into a film first comes into contact with is not particularly limited, but a cast roll is usually used. The cast roll temperature is preferably "Tg-50°C" or higher, preferably "Tg+70°C" or lower, more preferably "Tg+40°C" or lower. When a resin film is manufactured under such conditions, a resin film having a thickness of 1 μm to 1 mm can be easily manufactured. Here, "Tm" represents the melting point of the crystalline polymer, and "Tg" represents the glass transition temperature of the crystalline polymer.
[0081] [9. Step (ii) of contacting the resin film with a solvent] The method for producing an optical film according to the first embodiment includes a step (ii) of contacting a resin film with a solvent after the step (i). The step (ii) changes the birefringence in the thickness direction of the resin film, so that an optical film having a birefringence in the thickness direction different from that before the contact with the solvent can be obtained.
[0082] The solvent to be used is within the above-mentioned range as the solvent contained in the optical film. Therefore, in the step (ii), the solvent having a boiling point Bp lower than the glass transition temperature Tg of the crystalline polymer contained in the resin film comes into contact with the resin film.
[0083] The method of contacting the resin film with the solvent is not limited. Examples of the contact method include a spray method in which the resin film is sprayed with the solvent, a coating method in which the resin film is coated with the solvent, and a dipping method in which the resin film is dipped in the solvent. Among these, the dipping method is preferred because it is easy to perform continuous contact.
[0084] The temperature of the solvent contacted with the resin film is arbitrary within the range in which the solvent can maintain a liquid state, and can therefore be set in the range higher than the melting point and lower than the boiling point of the solvent. In particular, from the viewpoint of accelerating the rate of change in birefringence in the thickness direction due to contact between the resin film and the solvent, the temperature of the solvent is preferably in a specific temperature range higher than room temperature. The specific temperature range is preferably 30°C or higher, more preferably 35°C or higher, particularly preferably 40°C or higher, and preferably 80°C or lower, more preferably 70°C or lower, particularly preferably 60°C or lower.
[0085] The contact time between the resin film and the solvent can be appropriately set within a range in which an optical film having desired optical properties can be obtained. The specific contact time is preferably 0.5 seconds or more, more preferably 1.0 seconds or more, particularly preferably 5.0 seconds or more, and preferably 120 seconds or less, more preferably 80 seconds or less, particularly preferably 60 seconds or less. When the contact time is equal to or greater than the lower limit of the range, the birefringence in the thickness direction can be effectively changed by contact with the solvent. On the other hand, even if the immersion time is extended, the amount of change in birefringence tends not to change significantly. Therefore, when the contact time is equal to or less than the upper limit of the range, the productivity can be increased without impairing the quality of the optical film.
[0086] The birefringence Rth / d in the thickness direction of the resin film changes when the resin film is contacted with the solvent. The change in the birefringence Rth / d in the thickness direction of the resin film caused by the contact with the solvent is preferably 1.0×10 -3 More preferably, 2.0×10 -3 More preferably, 4.0×10 -3 or more, preferably 50.0×10 -3 Less than or equal to 30.0×10 -3 The following is particularly preferably 20.0×10 -3 The change in the birefringence Rth / d in the thickness direction represents the absolute value of the change in the birefringence Rth / d in the thickness direction. A specific change in the birefringence Rth / d in the thickness direction is calculated by subtracting the birefringence Rth / d in the thickness direction of the resin film before contact with the solvent from the birefringence Rth / d in the thickness direction of the resin film after contact with the solvent, and then calculating the absolute value. Preferably, the birefringence Rth / d in the thickness direction is reduced (i.e., changes in the negative direction) by contacting the resin film with the solvent.
[0087] The in-plane birefringence Re / d of the resin film may or may not change upon contact with the solvent. From the viewpoint of easily controlling the in-plane retardation Re of the optical film, it is preferable that the change in the in-plane birefringence Re / d of the resin film caused by contact with the solvent is small, and it is more preferable that no change occurs. The change in the in-plane birefringence Re / d of the resin film caused by contact with the solvent is preferably 0.0×10 -3 ~1.0×10 -3 , more preferably 0.0×10 -3 ~0.5×10 -3 , particularly preferably 0.0×10 -3 ~0.3×10 -3 The change in the in-plane birefringence Re / d refers to the absolute value of the change in the in-plane birefringence Re / d. A specific change in the in-plane birefringence Re / d is calculated as the absolute value by subtracting the in-plane birefringence Re / d of the resin film before contact with the solvent from the in-plane birefringence Re / d of the resin film after contact with the solvent.
[0088] In step (ii), the thickness of the resin film is usually increased by the penetration of the solvent contacted with the resin film into the resin film. The lower limit of the change rate of the thickness of the resin film at this time may be, for example, 1% or more, 10% or more, or 20% or more. The upper limit of the change rate of the thickness may be, for example, 80% or less, 50% or less, or 40% or less. The change rate of the thickness of the resin film is a ratio obtained by dividing the difference in thickness between the resin film before contact with the solvent and the resin film after contact with the solvent by the thickness of the resin film before contact with the solvent.
[0089] As described above, the birefringence Rth / d in the thickness direction of the resin film is changed by the step (ii). When a resin film having desired optical properties can be obtained by changing the birefringence Rth / d in the thickness direction, the resin film can be obtained as an optical film.
[0090] [10. Step (iii) of stretching the resin film] The method for producing an optical film according to the first embodiment may include a step (iii) of stretching the resin film after the step (ii). The stretching can orient the molecules of the crystalline polymer contained in the resin film in a direction corresponding to the stretching direction. Thus, this stretching can adjust the optical properties of the resin film, such as the in-plane birefringence Re / d, in-plane retardation Re, thickness birefringence Rth / d, thickness retardation Rth, and NZ coefficient; as well as the thickness d.
[0091] For example, when a crystalline polymer having negative intrinsic birefringence is used, if the molecules of the crystalline polymer in the resin film are oriented in the thickness direction by contact with the solvent in step (ii), a resin film having an NZ coefficient of more than 1.0 can be obtained. In this case, by performing stretching in step (iii), the NZ coefficient can be adjusted to less than 1.0 by the stretching, and an optical film can be obtained as an optically stretched film produced through the stretching process.
[0092] In addition, for example, a resin film may be obtained as an optical film having an NZ coefficient of less than 1.0 by contacting with a solvent in step (ii). In this case, the resin film may be stretched to obtain an optical film as an optically stretched film having appropriate optical properties according to the application.
[0093] There is no limitation on the stretching direction, and examples thereof include the longitudinal direction, the width direction, and the oblique direction. Here, the oblique direction refers to a direction perpendicular to the thickness direction, and is neither parallel nor perpendicular to the width direction. The stretching direction may be one direction or two or more directions. Thus, examples of the stretching method include uniaxial stretching methods such as a method of uniaxially stretching a resin film in the longitudinal direction (longitudinal uniaxial stretching method) and a method of uniaxially stretching a resin film in the width direction (transverse uniaxial stretching method); biaxial stretching methods such as a simultaneous biaxial stretching method in which a resin film is stretched in the longitudinal direction and simultaneously stretched in the width direction, and a sequential biaxial stretching method in which a resin film is stretched in one of the longitudinal direction and the width direction and then stretched in the other direction; and a method of stretching a resin film in an oblique direction (oblique stretching method). Among these, a uniaxial stretching method in which stretching is performed only in one direction is preferred, and a free uniaxial stretching method in which no restraining force is applied in a direction other than the stretching direction is more preferred.
[0094] The stretching ratio is preferably 1.1 times or more, more preferably 1.2 times or more, and preferably 20.0 times or less, more preferably 10.0 times or less, even more preferably 5.0 times or less, and particularly preferably 2.0 times or less. It is desirable to appropriately set the specific stretching ratio according to factors such as the optical properties, thickness, and mechanical strength of the optical film to be produced. When the stretching ratio is equal to or greater than the lower limit of the above range, the birefringence can be significantly changed by stretching. Also, when the stretching ratio is equal to or less than the upper limit of the above range, the direction of the slow axis can be easily controlled and the breakage of the film can be effectively suppressed.
[0095] The stretching temperature is preferably "Tg+5°C" or higher, more preferably "Tg+10°C" or higher, and preferably "Tg+100°C" or lower, more preferably "Tg+90°C" or lower. Here, "Tg" represents the glass transition temperature of the crystalline polymer. When the stretching temperature is equal to or higher than the lower limit of the above range, the resin film can be sufficiently softened to perform uniform stretching. When the stretching temperature is equal to or lower than the upper limit of the above range, the hardening of the resin film due to the progress of crystallization of the crystalline polymer can be suppressed, so that the stretching can be performed smoothly, and large birefringence can be expressed by stretching. Furthermore, the haze of the obtained resin film can usually be reduced to increase transparency.
[0096] By carrying out the stretching process, an optically stretched film can be obtained as a stretched resin film. Usually, the heat applied during stretching evaporates and removes the solvent contained in the resin film, so that it is possible to obtain an optically stretched film with a low solvent content. Therefore, the amount of solvent contained in the obtained optically stretched film can be particularly reduced. Specifically, the ratio of the solvent contained in the optically stretched film (solvent content) is preferably 1% by weight or less, more preferably 0.1% by weight or less, particularly preferably 0.05% by weight or less, and is usually 0.01% by weight or more. The solvent content of the optically stretched film can be measured by a measurement method described in the examples.
[0097] [11. Step (iv) of drying the resin film] The method for producing an optical film according to the first embodiment may include a step (iv) of drying the resin film after the step (ii). By drying, the solvent content of the resin film can be reduced, and an optical film having a low solvent content can be obtained as described above. The step (iv) of drying the resin film may be performed before or after the step (iii).
[0098] Drying is usually carried out at a drying temperature lower than the glass transition temperature Tg of the crystalline polymer in order to suppress the change in the orientation state of the crystalline polymer due to heat during drying. Even at such a drying temperature, if the boiling point Bp of the solvent is lower than the glass transition temperature Tg of the crystalline polymer, the solvent can be effectively removed. The specific drying temperature is preferably 50°C or higher, more preferably 60°C or higher, and even more preferably 70°C or higher, and is preferably lower than Tg, more preferably Tg-5°C or lower, and even more preferably Tg-10°C or lower.
[0099] The drying time is preferably 30 seconds or more, more preferably 1 minute or more, particularly preferably 5 minutes or more, and is preferably 6 hours or less, more preferably 3 hours or less, particularly preferably 1 hour or less.
[0100] [12. Optional process] The method for producing an optical film according to the first embodiment may further include any step in combination with the steps described above, such as a step of preheating the resin film before step (iii), a step of subjecting the optical film to a heat treatment to promote crystallization of the crystalline polymer, a step of thermally shrinking the optical film to remove residual stress in the film, etc.
[0101] According to the above-mentioned manufacturing method, a long optical film can be manufactured using a long resin film. The manufacturing method of the optical film may include a step of winding the long optical film thus manufactured into a roll. Furthermore, the manufacturing method of the optical film may include a step of cutting the long optical film into a desired shape.
[0102] [13. Method for producing optical film according to second embodiment] As described in the above-mentioned method for producing an optical film according to the first embodiment, in the method for producing an optical film by contacting a resin film made of a crystalline resin with a solvent to change the birefringence in the thickness direction, when the temperature of the solvent is set to a specific temperature range higher than room temperature, the rate of change in the birefringence in the thickness direction due to the contact of the resin film with the solvent can be increased. The above-mentioned advantage obtained by setting the temperature of the solvent to a specific temperature range can be obtained not only when a solvent having a boiling point lower than the glass transition temperature of the crystalline polymer is used, but also when a solvent having a boiling point equal to or higher than the glass transition temperature of the crystalline polymer is used. In addition, the above-mentioned advantage can be obtained not only when an optical film having an NZ coefficient of less than 1.0 is produced, but also when an optical film having an NZ coefficient of 1.0 or more is produced. Using this advantage, the method for producing an optical film according to the second embodiment described below may be carried out.
[0103] A method for producing an optical film according to a second embodiment of the present invention includes the steps of: (i) preparing a resin film formed of a crystalline resin; (ii) contacting the resin film with a solvent to change the birefringence in the thickness direction; The temperature of the solvent in contact with the resin film is set to the specific temperature range higher than room temperature.
[0104] According to this manufacturing method, the rate of change of the birefringence in the thickness direction due to the contact of the resin film with the solvent can be increased. Therefore, the time required to manufacture an optical film having desired optical properties can be shortened, and the manufacturing efficiency of the optical film can be improved. In addition, since the birefringence in the thickness direction of the resin film can be significantly changed in a short time, the optical properties of the optical film can be adjusted with a high degree of freedom even when the contact time between the resin film and the solvent is limited.
[0105] The method for producing the optical film according to the second embodiment may be the same as the method for producing the optical film according to the first embodiment, except that a solvent having a boiling point equal to or higher than the glass transition temperature of the crystalline polymer may be used. In particular, in the method for producing the optical film according to the second embodiment, it is preferable that the solvent has a boiling point lower than the glass transition temperature Tg of the crystalline polymer.
[0106] The optical film produced by the production method according to the second embodiment may be the same as the optical film according to the first embodiment, except that the requirements (B) and (C) described in the first embodiment may not necessarily be satisfied. In particular, the optical film produced by the production method according to the second embodiment preferably contains a solvent having a boiling point lower than the glass transition temperature Tg of the crystalline polymer at the solvent content described in the requirement (B). In addition, the optical film produced by the production method according to the second embodiment preferably has an NZ coefficient in the range described in the requirement (C). In particular, when the production method for the optical film according to the second embodiment includes the step (iii) of stretching the resin film, the optically stretched film as the optical film produced can achieve the low solvent content (preferably 1 wt % or less) described in the first embodiment.
[0107] [14. Applications of optical films] There is no limitation in the applications of the optical film according to the first embodiment and the optical film manufactured by the manufacturing method according to the second embodiment. These optical films can be used alone or in combination with other members for a wide range of applications in the optical field. Examples of applications of the optical film include a substrate film for forming an arbitrary layer on the substrate film; a polarizing plate protective film; a viewing angle compensation film for a liquid crystal display device, and a retardation film such as a quarter-wave plate provided on a circular polarizing plate; and the like. EXAMPLES
[0108] The present invention will be described in detail below with reference to examples. However, the present invention is not limited to the examples shown below, and can be modified and carried out as desired without departing from the scope of the claims of the present invention and the scope of equivalents thereto. In the following description, the units "%" and "parts" are by weight unless otherwise specified. Furthermore, the operations described below were carried out in air at room temperature and normal pressure (23°C and 1 atm) unless otherwise specified.
[0109] [Evaluation method] (Method of measuring weight average molecular weight Mw and number average molecular weight Mn of polymer) The weight average molecular weight Mw and number average molecular weight Mn of the polymer were measured as polystyrene equivalent values using a gel permeation chromatography (GPC) system (Tosoh Corporation, "HLC-8320"). In the measurement, an H-type column (Tosoh Corporation) was used as the column, and tetrahydrofuran was used as the solvent. The temperature during the measurement was 40°C.
[0110] (Method for measuring hydrogenation rate of polymer) The hydrogenation rate of the polymer is 4 as a solvent at 145°C, 1 Measured by H-NMR measurement.
[0111] (Method of measuring glass transition temperature Tg and melting point Tm) The glass transition temperature Tg and melting point Tm of the polymer were measured as follows. First, the polymer was melted by heating, and the melted polymer was quenched with dry ice. Then, the glass transition temperature Tg and melting point Tm of the polymer were measured using a differential scanning calorimeter (DSC) at a heating rate of 10°C / min (heating mode) using the polymer as a test specimen.
[0112] (Method for measuring the ratio of racemo-dyads in polymers) The ratio of racemo-dyads in the polymer was determined as follows. 4The inverse-gated decoupling method was applied to the polymer at 200°C using 13 C-NMR measurements were performed. 13 The results of C-NMR measurement showed that o-dichlorobenzene-d 4 Using the peak at 127.5 ppm as the reference shift, the signal at 43.35 ppm from the meso-dyad and the signal at 43.43 ppm from the racemo-dyad were identified. The ratio of the racemo-dyads in the polymer was calculated based on the intensity ratio of these signals.
[0113] (Method of measuring film retardation, NZ coefficient and slow axis direction) The in-plane retardation Re, thickness retardation Rth, NZ coefficient and slow axis direction of the film were measured by a phase difference meter ("AxoScan OPMF-1" manufactured by AXOMETRICS) at a wavelength of 590 nm.
[0114] (Method for measuring the crystallinity of crystalline polymers) The crystallinity of the crystalline polymer contained in the film was confirmed by X-ray diffraction in accordance with JIS K 0131. Specifically, the diffracted X-ray intensity from the crystallized portion was determined using a wide-angle X-ray diffractometer (Rigaku Corporation, "RINT 2000"), and the crystallinity was calculated from the ratio to the total diffracted X-ray intensity according to the following formula (I). Xc=K·Ic / It (I) In the above formula (I), Xc represents the crystallinity of the test sample, Ic represents the diffracted X-ray intensity from the crystallized portion, It represents the total diffracted X-ray intensity, and K represents a correction term.
[0115] (Method for measuring the solvent content of film) In the examples and comparative examples described later, the solvent content of the sample film as the measurement object (optical film in Examples 1 to 3 and 5 and Comparative Example 1; optical stretched film in Example 4) was measured by the following method. A film piece was cut from the optical film to be measured, and the film piece was weighed at 0.5 mg. However, in the case of a sample where the peak was saturated, it was weighed at 0.2 mg. The weight of the film piece weighed here was designated as W0. For the weighed film sample, outgas measurement by GC / MS (gas chromatography-mass spectrometry) was carried out under the following conditions to determine the weight of the solvent St contained in the optical film of weight W0. The weight of the solvent St used the value converted with n-decane as the standard sample. The solvent content was determined by St / W0×100 (%).
[0116] <GC / MS Measurement Conditions> Purge flow rate: 180 °C × 30 min (40 °C / min) 30 mL / min Trap: -130 °C INJ: 300 °C × 5 min Init 2 min Column: HP-5ms 0.25 mm × 30 m df = 0.25 μm Oven: 40 °C × 3 min, then heated to 120 °C at 10 °C / min, and then heated to 280 °C at 40 °C / min Interface: 280 °C He flow rate: 1.0 mL / min TDS: splitless CIS: split 1 / 50 Measured ions: 29 - 550
[0117] [Production Example 1. Production of Crystalline Resin] After thoroughly drying a metal pressure reactor, it was purged with nitrogen. To this metal pressure reactor, 154.5 parts of cyclohexane, 42.8 parts of a 70% cyclohexane solution of dicyclopentadiene (end isomer content 99% or more) (30 parts as the amount of dicyclopentadiene), and 1.9 parts of 1-hexene were added and heated to 53 °C.
[0118] 0.014 parts of tetrachlorotungsten phenylimide (tetrahydrofuran) complex was dissolved in 0.70 parts of toluene to prepare a solution. 0.061 parts of a 19% diethylaluminum ethoxide / n-hexane solution was added to this solution and stirred for 10 minutes to prepare a catalyst solution. This catalyst solution was added to a pressure-resistant reactor to start a ring-opening polymerization reaction. The reaction was then continued for 4 hours while maintaining the temperature at 53°C to obtain a solution of a ring-opened polymer of dicyclopentadiene. The number-average molecular weight (Mn) and weight-average molecular weight (Mw) of the obtained ring-opened polymer of dicyclopentadiene were 8,750 and 28,100, respectively, and the molecular weight distribution (Mw / Mn) calculated from these was 3.21.
[0119] To 200 parts of the obtained solution of the ring-opening polymer of dicyclopentadiene, 0.037 parts of 1,2-ethanediol was added as a terminator, heated to 60°C, and stirred for 1 hour to terminate the polymerization reaction. One part of a hydrotalcite-like compound (Kyowa Chemical Industry Co., Ltd.'s "Kyoward (registered trademark) 2000") was added, heated to 60°C, and stirred for 1 hour. Thereafter, 0.4 parts of a filter aid (Showa Chemical Industry Co., Ltd.'s "Radiolight (registered trademark) #1500") was added, and the adsorbent and the solution were filtered using a PP pleated cartridge filter (ADVANTEC Toyo Co., Ltd.'s "TCP-HX").
[0120] 100 parts of cyclohexane was added to 200 parts of the filtered ring-opening polymer solution (polymer amount 30 parts), and 0.0043 parts of chlorohydridocarbonyltris(triphenylphosphine)ruthenium was added, and hydrogenation reaction was carried out at 180°C and hydrogen pressure of 6 MPa for 4 hours. As a result, a reaction liquid containing a hydrogenated product of the ring-opening polymer of dicyclopentadiene was obtained. The reaction liquid was a slurry solution in which the hydrogenated product was precipitated.
[0121] The hydrogenated product and the solution contained in the reaction solution were separated using a centrifuge and dried under reduced pressure at 60°C for 24 hours to obtain 28.5 parts of a hydrogenated ring-opening polymer of dicyclopentadiene as a crystalline polymer having positive intrinsic birefringence. The hydrogenation rate of this hydrogenated product was 99% or more, the glass transition temperature (Tg) was 93°C, the melting point (Tm) was 262°C, and the ratio of racemo-dyads was 89%.
[0122] 100 parts of the obtained hydrogenated ring-opening polymer of dicyclopentadiene was mixed with 1.1 parts of an antioxidant (tetrakis [methylene-3-(3',5'-di-t-butyl-4'-hydroxyphenyl) propionate] methane; "Irganox (registered trademark) 1010" manufactured by BASF Japan Ltd.), and then the mixture was put into a twin-screw extruder (product name "TEM-37B", manufactured by Toshiba Machine Co., Ltd.) equipped with four die holes having an inner diameter of 3 mm. The mixture of the hydrogenated ring-opening polymer of dicyclopentadiene and the antioxidant was molded into a strand shape by hot melt extrusion molding, and then chopped with a strand cutter to obtain pellets of a crystalline resin. The operating conditions of the twin-screw extruder were as follows. Barrel temperature setting: 270~280℃ Die temperature setting = 250℃ Screw speed: 145 rpm
[0123] [Example 1] (1-1. Extrusion film formation) The crystalline resin pellets were melt-extruded using a hot melt extrusion film molding machine equipped with a T-die (Optical Control Systems' "Measuring Extruder Type Me-20 / 2800V3") and wound on a roll at a speed of 1.5 m / min to obtain a long resin film approximately 120 mm wide. The operating conditions of the film molding machine are listed below. Barrel temperature setting: 280℃~300℃ Die temperature = 300℃ Screw speed = 30 rpm Cast roll temperature = 80℃
[0124] The thickness of the obtained resin film was 50 μm. When the retardation of the resin film was measured at a wavelength of 590 nm, the in-plane retardation Re was 4 nm, and the retardation in the thickness direction Rth was 8 nm.
[0125] (1-2. Solvent Contact) The resin film was cut into a rectangle of 120 mm x 120 mm. This rectangular resin film was immersed in carbon disulfide (boiling point 46.3°C) as a solvent stored in a tray for 1 minute to obtain an optical film. At this time, the temperature of the solvent was room temperature. The optical film was removed from the solvent, and the solvent on the film surface was wiped with a Kimtowel. When the retardation of this optical film was measured, the in-plane retardation Re was 19 nm, and the retardation in the thickness direction Rth was -481 nm. The thickness of the optical film was 61 μm.
[0126] (1-3. Drying) The optical film was placed in a dryer at 80°C and dried for 30 minutes. After drying, the optical film was removed from the dryer. The degree of crystallinity of the crystalline polymer contained in the optical film and the solvent content of the optical film were measured for the optical film after drying. In addition, the retardation of the optical film after drying was measured, and the in-plane retardation Re was 18 nm and the retardation in the thickness direction Rth was -499 nm.
[0127] [Example 2] The line speed in step (1-1) was changed to change the thickness of the long resin film to 39 μm. In step (1-2), the type of solvent was changed to cyclohexane (boiling point 80.75° C.), and the temperature of the solvent was changed to 40° C. Except for the above, the optical film was produced and evaluated in the same manner as in Example 1.
[0128] [Example 3] The line speed in step (1-1) was changed to change the thickness of the long resin film to 39 μm. In step (1-2), the type of solvent was changed to cyclohexane (boiling point 80.75° C.), and the temperature of the solvent was changed to 50° C. Except for the above, the optical film was produced and evaluated in the same manner as in Example 1.
[0129] [Example 4] The line speed in step (1-1) was changed to change the thickness of the long resin film to 25 μm. In step (1-2), the type of solvent was changed to cyclohexane (boiling point 80.75° C.), and the temperature of the solvent was changed to 50° C. Except for the above, the optical film was produced and evaluated in the same manner as in Example 1.
[0130] A batch-type biaxial stretching device (manufactured by Etoh Co., Ltd.) was prepared. This stretching device was equipped with an oven unit and a clip for stretching capable of fixing a film. By using this stretching device, it is possible to stretch the film by pulling the film with the clip in the oven.
[0131] The optical film was cut into a rectangle of 100 mm x 100 mm. Both ends of this rectangular optical film were held by five clips of the stretching device. The optical film was pulled by the clips and freely uniaxially stretched in the longitudinal direction of the long resin film obtained in the extrusion film formation process. The stretching temperature was 170°C and the stretching ratio was 1.2 times. By this free uniaxial stretching, an optically stretched film was obtained as the optical film after stretching. When the retardation of the optically stretched film was measured at a measurement wavelength of 590 nm, the in-plane retardation Re was 280 nm and the retardation in the thickness direction Rth was 3 nm. In addition, the thickness of the optically stretched film was 27 μm. For this optically stretched film, the crystallinity of the crystalline polymer contained in the optical film and the solvent content of the optically stretched film were measured.
[0132] [Example 5] The line speed in step (1-1) was changed to change the thickness of the long resin film to 39 μm. In addition, in step (1-2), the type of solvent was changed to cyclohexane (boiling point 80.75° C.). Except for the above, the optical film was produced and evaluated in the same manner as in Example 1.
[0133] In this Example 5, a long resin film was produced by melt extrusion under the same conditions as in Examples 2 and 3. The retardation and NZ coefficient of the resin film obtained in Example 5 are different from those in Examples 2 and 3. However, the degree of this difference is sufficiently small and within the range of normal error.
[0134] [Comparative Example 1] In step (1-2), the type of solvent was changed to toluene (boiling point 110.6° C.), and the temperature of the solvent was changed to 110.6° C. Except for the above, the same method as in Example 1 was used to produce and evaluate an optical film.
[0135] [result] The results of the above-mentioned Examples and Comparative Examples are shown in the following table. In the table, the meanings of the abbreviations are as follows. CS2: Carbon disulfide. Cy: Cyclohexane. Tl: toluene.
[0136] [Table 1]
[0137] [Consider] In Examples 1 to 5, the birefringence Rth / d in the thickness direction of the resin film is changed by contact with a solvent, and an optical film having an NZ coefficient of less than 1.0 is obtained. In addition, in Examples 1 to 5, a solvent having a boiling point lower than the glass transition temperature Tg of the crystalline polymer is used, and thus the solvent is effectively dried to achieve a small solvent content. Therefore, it was confirmed that an optical film having an NZ coefficient of less than 1.0 and a small solvent content can be realized in Examples 1 to 5.
[0138] In addition, comparing Examples 2 to 5 using the same solvent, in Examples 2 to 4 in which the resin film was contacted with a solvent in a specific temperature range higher than room temperature, the birefringence in the thickness direction could be changed significantly by contact with the solvent, compared to Example 5 in which the resin film was contacted with a solvent at room temperature. Since the contact time between the resin film and the solvent was the same in Examples 2 to 5, the large amount of change in birefringence in Examples 2 to 4 indicates that the rate of change in birefringence in the thickness direction due to contact between the resin film and the solvent in those Examples 2 to 4 was faster than that in Example 5. Therefore, it was confirmed that the rate of change in birefringence in the thickness direction due to contact between the resin film and the solvent can be increased in Examples 2 to 4.
Claims
1. An optical film formed of a resin containing a crystalline polymer, the optical film containing 0.01% by weight to 5% by weight of a solvent having a boiling point lower than the glass transition temperature of the crystalline polymer, the optical film having an in-plane retardation Re of 10 nm or less, and an NZ coefficient of less than 1.
0.
2. The optical film of claim 1 , wherein the crystalline polymer has positive intrinsic birefringence.
3. The optical film according to claim 1 , wherein the crystalline polymer contains an alicyclic structure.
4. 4. The optical film according to claim 1, wherein the crystallinity of the crystalline polymer measured by X-ray diffraction is 10% or more.
5. A method for producing an optical film, comprising the steps of: The optical film is formed of a resin containing a crystalline polymer, an optical film comprising 0.01% by weight to 5% by weight of a solvent having a boiling point lower than the glass transition temperature of the crystalline polymer, and an NZ coefficient of the optical film being less than 1.0; The manufacturing method includes: A step (i) of preparing a resin film formed of a resin containing a crystalline polymer and having optical isotropy; and (ii) a step of contacting the resin film with a solvent having a boiling point lower than the glass transition temperature of the crystalline polymer to change the birefringence Rth / d in the thickness direction, The method for producing an optical film, wherein in the step (ii), a change in the birefringence in the thickness direction, Rth / d, caused by contact with the solvent is 1.0×10 −3 or more.
6. 6. The method for producing an optical film according to claim 5, wherein the temperature of the solvent in contact with the resin film is 30° C. to 80° C. and lower than the boiling point of the solvent.
7. A step (i) of preparing a resin film formed of a resin containing a crystalline polymer and having optical isotropy; (ii) contacting the resin film with a solvent to change the birefringence Rth / d in the thickness direction; In the step (ii), a change in the birefringence Rth / d in the thickness direction caused by contact with the solvent is 1.0×10 −3 or more; The method for producing an optical film, wherein the temperature of the solvent in contact with the resin film is 30° C. to 80° C. and is lower than the boiling point of the solvent.
8. The method for producing an optical film according to claim 7 , wherein the solvent has a boiling point lower than the glass transition temperature of the crystalline polymer.
9. The method for producing an optical film according to any one of claims 5 to 8, wherein step (i) comprises melt-extruding the resin.
10. The method for producing an optical film according to any one of claims 5 to 9, further comprising, after the step (ii), a step (iii) of stretching the resin film.
11. The method for producing an optical film according to claim 10 , wherein the amount of the solvent contained in the produced optical film is 1% by weight or less.
Citation Information
Patent Citations
Method for producing birefringent film and liquid crystal display device using the same
JP1993346507A
Method of manufacturing multilayer optical film, multilayer optical film and use thereof
JP2009251011A
Method for producing resin film, resin film, and optical film
JP2016026909A
Multilayer film and method for producing the same
JP2019028109A
Phase difference film and production method for same
WO2017065222A1