Porous film, separator for secondary battery, and secondary battery

The porous film with a heat-resistant resin layer on a polyolefin base material addresses the issues of dimensional stability and heat rupture resistance, enhancing battery performance and safety through improved electrolyte wettability and shutdown characteristics, leading to high-capacity and long-life batteries.

JP7567477B2Active Publication Date: 2024-10-16TORAY INDUSTRIES INC
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2020536890
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-03-28
Filing Date
2020-03-13
Publication Date
2024-10-16
Estimated Expiration
2040-03-13

AI Technical Summary

Technical Problem

Existing secondary battery separators lack sufficient dimensional stability, heat rupture resistance, and electrolyte wettability, leading to insufficient battery performance and safety issues.

Method used

A porous film with a heat-resistant resin layer having a melting point of 200°C or higher, laminated on a polyolefin porous base material, containing inorganic particles and achieving a porosity of 50-80% and a strength of 0.4N/10mm, with specific permeation rates and temperatures for electrolyte penetration and shutdown characteristics.

Benefits of technology

The porous film provides excellent electrolyte wettability, low-temperature shutdown characteristics, high-temperature dimensional stability, and heat-resistant membrane rupture properties, resulting in high-capacity, high-output, and long-life secondary batteries at a lower cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007567477000001
    Figure 0007567477000001
  • Figure 0007567477000002
    Figure 0007567477000002
  • Figure 0007567477000003
    Figure 0007567477000003
Patent Text Reader

Abstract

[Problem] The purpose of the present invention is to provide, at low cost, a separator for secondary batteries, which sufficiently exhibits the characteristics of a porous layer by having excellent adhesion between the porous layer and a porous base material, and which has excellent battery characteristics. [Solution] A porous film which is obtained by superposing a porous layer that contains a heat-resistant resin having no melting point or a melting point of 200°C or higher on at least one surface of a porous base material that is formed of a polyolefin, and which is configured such that: the porous layer has a porosity of from 50% to 80% (inclusive) and a strength of 0.4 N / 10 mm or more; and the strength of the porous layer is lower than the adhesion strength between the porous layer and the porous base material formed of a polyolefin as determined by a 180 degree peel test in the longitudinal direction.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a porous film, a separator for a secondary battery, and a secondary battery. [Background technology]

[0002] 2. Description of the Related Art Secondary batteries such as lithium-ion batteries are widely used in a variety of applications, including portable digital devices such as smartphones, tablets, mobile phones, laptops, digital cameras, digital video cameras, and portable game consoles; portable devices such as power tools, electric motorcycles, and electrically assisted bicycles; and automotive applications such as electric vehicles, hybrid vehicles, and plug-in hybrid vehicles.

[0003] A lithium-ion battery generally has a configuration in which a positive electrode in which a positive electrode active material is laminated on a positive electrode current collector, a negative electrode in which a negative electrode active material is laminated on a negative electrode current collector, and a secondary battery separator and an electrolyte are interposed between them.

[0004] Polyolefin-based porous substrates are used as separators for secondary batteries. The characteristics required for separators for secondary batteries include a characteristic of containing an electrolyte in the porous structure to enable ion migration, and a shutdown characteristic of stopping power generation by melting the porous structure with heat and stopping ion migration when the lithium-ion battery generates abnormal heat.

[0005] In addition to the above characteristics, secondary battery separators are required to have dimensional stability and heat-resistant film rupture resistance at high temperatures. When a lithium ion battery generates abnormal heat, the above-mentioned shutdown characteristic is activated, and the battery is further heated, which may cause a short circuit due to contraction of the secondary battery separator. In addition, when an impact is applied to a lithium ion battery, heat is generated under localized pressure, and film rupture of the secondary battery separator may occur. When such a film rupture occurs in the secondary battery separator, a short circuit may occur inside the battery.

[0006] Thus, secondary battery separators are required to have heat resistance to film rupture at high temperatures in addition to shutdown characteristics. Furthermore, lithium ion batteries are required to have improved battery characteristics such as higher output, longer life, and higher capacity, as well as to be provided at low cost.

[0007] In response to these demands, Patent Document 1 proposes a battery separator that can reduce the thermal shrinkage rate by having a porous film mainly made of polyolefin and a porous film containing a binder and a plate-like inorganic filler.

[0008] Moreover, Patent Document 2 proposes a laminated porous film having shape stability at high temperatures by laminating a heat-resistant layer containing a resin binder and a filler on a porous substrate mainly composed of polyolefin.

[0009] Patent Document 3 proposes a lithium battery separator having excellent shutdown properties, which is composed of a three-layer microporous membrane characterized in that both surface layers are microporous layers made of a copolymer containing vinylidene fluoride and have a melting point of 145°C or less, and an intermediate layer is a microporous layer made of a polyolefin and has a melting point of 140°C or less.

[0010] Furthermore, Patent Document 4 proposes a secondary battery separator in which a heat-resistant porous layer of a heat-resistant polymer and an inorganic filler is laminated on a microporous film for the purpose of improving shutdown characteristics and heat resistance. [Prior art documents] [Patent documents]

[0011] [Patent Document 1] JP 2010-123465 A [Patent Document 2] JP 2016-130027 A [Patent Document 3] JP 2002-216734 A [Patent Document 4] JP 2009-231281 A Summary of the Invention [Problem to be solved by the invention]

[0012] From the viewpoint of battery safety, battery separators are required to have not only shutdown characteristics but also heat resistance to film rupture, good ion mobility, and good electrolyte wettability to improve productivity.

[0013] However, although Patent Document 1 has good wettability in the thickness direction of the electrolyte, the heat resistance of the binder used in the porous layer increases the heat shrinkage rate when the high temperature range after shutdown is reached, and sufficient dimensional stability and heat resistance to film breakage at high temperatures cannot be obtained. In Patent Document 2, since a heat-resistant nitrogen-containing aromatic polymer is laminated, the heat shrinkage rate is small when the high temperature range after shutdown is reached, but sufficient battery characteristics cannot be obtained because the characteristics of the resin binder do not provide sufficient heat resistance to film breakage and wettability with the electrolyte.

[0014] Patent Document 3 proposes providing a porous layer with a melting point of 145°C or lower. However, such a porous layer has a large thermal shrinkage rate when it reaches the high temperature range after shutdown, and it is not possible to ensure sufficient dimensional stability and heat-resistant film rupture at high temperatures.

[0015] In Patent Document 4, a heat-resistant resin with a relatively low molecular weight is used, which reduces the strength of the heat-resistant porous layer and the adhesion between the heat-resistant porous layer and the microporous membrane. This results in powder falling of inorganic particles during the process of providing the heat-resistant porous layer and / or the battery production process, and the heat resistance to film rupture of the separator cannot be ensured, making it impossible to fully utilize the shutdown properties of the porous material.

[0016] Therefore, in view of the above problems, the object of the present invention is to provide a porous film at low cost that has excellent battery characteristics and excellent wettability with an electrolyte even when it is provided with shutdown characteristics at low temperatures, dimensional stability at high temperatures, and heat resistance to film rupture. Also, the object of the present invention is to provide a secondary battery that has good low-temperature shutdown characteristics, dimensional stability at high temperatures, and heat resistance to film rupture, and has high capacity, high output, long life, and low cost. [Means for solving the problem]

[0017] Therefore, the present inventors have conducted extensive research to provide a porous film having excellent battery characteristics at low cost by imparting to a separator for a secondary battery shutdown characteristics at low temperatures, a large temperature difference between the shutdown temperature and the temperature at which the separator melts, and dimensional stability and heat-resistant film breakage resistance at high temperatures. In addition, the inventors have found that by setting the permeation rate of the electrolyte, which is an index of the permeability of the electrolyte, and the immersion area per unit time of the electrolyte within a certain range, the cycle characteristics and rate characteristics of the battery can be improved, and have arrived at the present invention.

[0018] In order to solve the above problems, the porous film of the present invention has the following configuration. (1) A porous film comprising a polyolefin porous substrate and a porous layer laminated on at least one side thereof, the porous layer having a porosity of 50% or more and 80% or less and a strength of 0.4 N / 10 mm or more, the strength of the porous layer being lower than the adhesive strength between the polyolefin porous substrate and the porous layer in a 180-degree peel test in the longitudinal direction. (2) The permeation rate of diethyl carbonate into the porous film is 4 μm / min or more, and the permeation area of ​​diethyl carbonate after 10 seconds is 500 mm 2 The porous film is as described above. The permeation rate was calculated from the time it took for 100 μL of diethyl carbonate to reach the back surface after being dropped and the thickness of the porous film. The permeation area was calculated by dropping 100 μL of diethyl carbonate, leaving it for 10 seconds, and then taking an image, and using image analysis software to calculate the permeation area of ​​diethyl carbonate. (3) The porous film according to (1) or (2), wherein the porous layer contains inorganic particles. (4) The porous film according to any one of (1) to (3), wherein the porous film has a falling ball rupture temperature of 250° C. or higher. (5) The porous film according to any one of (1) to (4), wherein the shutdown temperature of the porous film is 135° C. or lower. (6) The porous film according to any one of (1) to (5), wherein the difference between the shutdown temperature and the meltdown temperature of the porous film is 70° C. or more. (7) A separator for a secondary battery, comprising the porous film according to any one of (1) to (6). (8) A secondary battery using the separator for secondary batteries according to (7). Effect of the Invention

[0019] According to the present invention, even if the porous film is provided with low-temperature shutdown characteristics, dimensional stability at high temperatures, and heat-resistant film rupture resistance, it is possible to provide a porous film having excellent wettability with an electrolyte and excellent battery characteristics at low cost. In addition, by using the separator for a secondary battery of the present invention, it is possible to provide a secondary battery having good low-temperature shutdown characteristics, dimensional stability at high temperatures, and heat-resistant film rupture resistance, and having high capacity, high output, long life, and low cost. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0020] The porous film of the present invention is a porous film in which a porous layer containing a heat-resistant resin is laminated on at least one surface of a porous substrate. The present invention will be described in detail below.

[0021] [Porous layer] (Heat-resistant resin) The porous layer provides a large difference between the shutdown temperature and the temperature at which the separator melts, and also provides dimensional stability and heat resistance to film rupture at high temperatures. From this viewpoint, the porous layer contains (A) a heat-resistant resin having a melting point of 200°C or higher or (B) a heat-resistant resin that has no melting point.

[0022] A heat-resistant resin with a melting point of 200°C or higher is a resin that, when measured using a differential scanning calorimeter (DSC) in accordance with JIS K7121 (2012), exhibits an endothermic peak of 200°C or higher during the second heating cycle after the first heating and cooling.

[0023] A heat-resistant resin without a melting point is a resin that does not have an endothermic peak in the temperature range of -20 to 230°C during the second heating cycle after the first heating and cooling cycle, as measured by DSC in accordance with JIS K7121 (2012). Unless a heat-resistant resin having the characteristics of (A) or (B) is used, it is not possible to impart dimensional stability and heat-resistant film rupture resistance at high temperatures to the separator.

[0024] Examples of the heat-resistant resin include polyethylene terephthalate, polysulfone, polyethersulfone, polyphenylene sulfide, polyacrylate, polyetherimide, polyetheretherketone, polyamide, polyimide, polyamideimide, fluororesin, cellulose and derivatives thereof, etc. Also, a plurality of these resins may be used.

[0025] Among these, aromatic polyamide, aromatic polyimide, and aromatic polyamideimide are more preferred, and aromatic polyamide is most preferred.

[0026] Examples of aromatic polyamides include meta-oriented aromatic polyamides and para-oriented aromatic polyamides. Either may be used, but para-oriented aromatic polyamides are preferred because they provide excellent battery characteristics and thermal shrinkage when the porous film is used as a separator for a secondary battery.

[0027] Aromatic polyamides that can be suitably used are those having repeating units represented by the following formula (1) and / or formula (2). (1):

[0028] [ka]

[0029] ification(2):

[0030] [ka]

[0031] In the present invention, the precipitation rate of the heat-resistant resin in the phase separation step described below can be adjusted by adjusting the hydrophilicity of the heat-resistant resin. By precipitating the resin quickly and growing the resin fibrils uniformly, the adhesion between the porous substrate and the porous layer can be improved, the heat resistance and strength of the porous layer can be increased, and the dropout of inorganic particles during battery assembly or coating can be suppressed. The hydrophilicity of the heat-resistant resin can be adjusted by adjusting the copolymerization ratio or logarithmic viscosity of the heat-resistant resin. From this viewpoint, a copolymer consisting of basic units represented by Chemical (1) and Chemical (2) is preferred.

[0032] The copolymerization ratio of the copolymer is preferably 80% or more of the basic unit represented by Chemical formula (1). From the viewpoint of increasing the adhesion between the porous substrate and the porous layer and fully exhibiting the shutdown property of the porous film described later, it is more preferably 85% or more, and even more preferably 90% or more. In addition, the upper limit of the copolymerization ratio of the basic unit represented by Chemical formula (1) is preferably 99% or less.

[0033] Here, examples of Ar1, Ar2 and Ar3 include groups selected from the groups represented by the following formulas (3) to (7). Convert(3)~(7):

[0034] [ka]

[0035] Furthermore, X and Y are selected from -O-, -CO-, -CO2-, -SO2-, -CH2-, -S-, -C(CH3)2- and the like, but are not limited thereto.

[0036] Furthermore, a part of the hydrogen atoms on the aromatic rings in these Ar1 to Ar3 may be substituted with a substituent such as a halogen group such as fluorine, bromine, or chlorine, a nitro group, a cyano group, an alkyl group, or an alkoxy group. In particular, when the compound has an electron-withdrawing substituent such as a halogen group, a nitro group, or a cyano group, it is preferable because it has excellent electrochemical oxidation resistance and can prevent deterioration such as oxidation on the positive electrode side when used as a separator. Among them, a halogen group is more preferable as the substituent, and a chlorine atom is most preferable.

[0037] The bonds in Ar1 to Ar3 may be ortho-, meta-, or para-oriented, but it is preferable that those having para orientation account for 50 mol % or more of all aromatic rings. More preferably, it is 100 mol %. The para orientation here refers to a state in which divalent bonds constituting the main chain in the aromatic ring are coaxial or parallel to each other.

[0038] The lower limit of the logarithmic viscosity (ηinh) of the heat-resistant resin is preferably 4.0 dl / g or more from the viewpoint of increasing the adhesion between the porous substrate and the porous layer, heat resistance, and strength of the porous layer, and suppressing the falling off of inorganic particles during battery assembly and coating. It is more preferably 4.5 dl / g or more from the viewpoint of increasing the heat resistance and adhesion between the porous substrate and the porous layer, and fully expressing the shutdown characteristics of the porous film described below. The upper limit of the logarithmic viscosity is preferably 7.0 dl / g or less from the viewpoint of dispersibility with inorganic particles in the coating liquid and productivity. The logarithmic viscosity of the resin is an index of molecular weight.

[0039] By using a heat-resistant resin whose copolymerization ratio and / or logarithmic viscosity is appropriately adjusted for the porous layer, it is possible to impart high strength to the porous layer even if the porosity of the porous layer is 50% or more and 80% or less.

[0040] Furthermore, when it is desired to impart a low-temperature shutdown characteristic to the porous layer, it is preferable to incorporate an organic resin other than the heat-resistant resin into the porous layer. Here, the low-temperature shutdown characteristic refers to a characteristic in which the shutdown temperature described below is 135° C. or less. From the viewpoint of further lowering the heat generation start temperature when the secondary battery has a high capacity and high output, 130° C. or less is more preferable.

[0041] The organic resin is preferably an organic resin having a melting point of, for example, 135° C. or less. The organic resin is not particularly limited as long as it has a melting point of 135° C. or less, but when used in a lithium ion battery, which is a non-aqueous electrolyte secondary battery, it is extremely difficult to bring moisture into the system, so polyolefin resin, acrylic resin, fluororesin, polyvinylidene fluoride, etc. can be suitably used. In particular, it is more preferable to use particles made of high-density polyethylene, low-molecular-weight polyethylene, etc.

[0042] (Inorganic particles) In order to impart foreign matter resistance to the porous layer, it is preferable that the porous layer contains inorganic particles. Foreign matter resistance refers to resistance to foreign matter that falls off active materials from the positive electrode and negative electrode or that gets mixed in during the manufacturing process of the battery.

[0043] Examples of inorganic particles include inorganic oxide particles such as aluminum oxide, boehmite, silica, titanium oxide, zirconium oxide, iron oxide, and magnesium oxide, inorganic nitride particles such as aluminum nitride and silicon nitride, and sparingly soluble ion crystal particles such as calcium fluoride, barium fluoride, and barium sulfate. These particles may be used alone or in combination of two or more kinds.

[0044] The content of inorganic particles in the porous layer is preferably 80% by mass or more and less than 97% by mass in terms of the porosity of the porous layer and battery characteristics, and more preferably 85% by mass or more and less than 95% by mass in terms of both thermal shrinkage and battery characteristics. When the content of inorganic particles is within the above-mentioned preferred range, it can be adjusted within the above-mentioned range of copolymerization ratio and logarithmic viscosity of the heat-resistant resin in order to improve the strength of the porous layer and prevent the inorganic particles from falling off from the porous layer.

[0045] The primary average particle diameter of the inorganic particles used is preferably 0.10 μm or more and 5.0 μm or less, more preferably 0.10 μm or more and 2.5 μm or less, from the viewpoint of the strength and porosity of the porous layer. By setting the lower limit of the primary average particle diameter to 0.10 μm or more, the porous layer becomes dense, and the pores of the porous substrate are closed, which increases the air permeability and prevents the battery characteristics from deteriorating. In addition, by setting the upper limit to 5.0 μm or less, the porous layer is prevented from having a non-uniform structure and being unable to obtain a sufficient heat shrinkage rate, and the thickness of the porous layer is prevented from increasing, which prevents the battery characteristics from deteriorating.

[0046] In addition, in order to achieve both the porosity and strength of the porous layer, it is preferable for the porous layer to contain two or more types of particles with different average particle sizes, and it is more preferable for the porous layer to contain inorganic particles with an average particle size of 0.30 μm or more and 2.5 μm or less and inorganic particles with an average particle size of 0.10 μm or more and less than 0.30 μm.

[0047] The shape of the particles used may be any of spherical, plate-like, needle-like, rod-like, elliptical, etc. Among these, spherical shapes are preferred from the viewpoints of surface modification, dispersibility, and coatability.

[0048] (Production of Porous Layer) The porous layer in the present invention refers to a layer having pores therein. The composition and method of forming the porous layer are not particularly limited, but as an example, a porous layer containing an aromatic polyamide resin as a heat-resistant resin will be described below.

[0049] The order of preparing the coating liquid is not particularly limited, but from the viewpoint of uniformly dispersing the inorganic particles and uniformity of the particle size of the inorganic particles in the coating liquid, it is preferable to mix a solution in which an aromatic polyamide resin and an aprotic organic polar solvent are mixed and dissolved with a dispersion in which inorganic particles and an aprotic organic polar solvent are dispersed, and further add other organic resins, additives, etc. as necessary to prepare the coating liquid.

[0050] For example, a coating liquid is prepared from a solution containing an aromatic polyamide resin produced by a known method such as solution polymerization using diamine and acid dichloride as raw materials, and a dispersion in which inorganic particles are dispersed.

[0051] Here, as the solvent for dispersing the inorganic particles, aprotic organic polar solvents such as N-methyl-2-pyrrolidone, N,N-dimethylacetamide, dimethylformamide, dimethylsulfoxide, etc. Among these, N-methyl-2-pyrrolidone is particularly preferable from the viewpoint of forming a porous structure in a later process.

[0052] In addition, a poor solvent for the aromatic polyamide resin may be added as an additive to promote porosity. Among them, the addition of water is preferred, and the amount of water added is preferably 500 parts by mass or less per 100 parts by mass of the aromatic polyamide resin. If the amount of water added is more than 500 parts by mass, the aromatic polyamide resin may solidify in the coating liquid, and the stability of the coating liquid may not be sufficient.

[0053] In addition to the aromatic polyamide resin and inorganic particles, the coating liquid may contain, if necessary, an organic resin, a dispersant, a thickener, a stabilizer, an antifoaming agent, a leveling agent, and the like.

[0054] The method for dispersing the coating liquid is not particularly limited, but from the viewpoints of heat resistance and wettability with the electrolyte, it is important that the particles are uniformly dispersed and that the particle diameter of the inorganic particles in the coating liquid is uniform. It is preferable to disperse the particles in a solvent by milling using a ball mill, a bead mill, a sand mill, a roll mill, or the like, and then disperse the organic resin in the solvent in which the particles have been dispersed by milling using a ball mill, a bead mill, a sand mill, a roll mill, or the like.

[0055] In particular, when a heat-resistant resin is added and dispersed, from the viewpoint of uniformity of the particle size of the inorganic particles in the coating liquid, it is preferable to disperse the resin using a bead mill. The diameter of the beads used in the bead mill is preferably 0.1 to 1 mm, and the material of the beads used is preferably aluminum oxide, zirconium oxide, zirconia-reinforced alumina, or the like.

[0056] In addition, it is preferable to add and disperse the heat-resistant resin multiple times, and further, it is preferable that the peripheral speed is faster than the speed at which the inorganic particles are dispersed in the solvent and is increased stepwise from the viewpoint of uniformity of the particle size of the inorganic particles in the coating liquid.

[0057] From the viewpoint of heat resistance, the viscosity of the coating liquid is preferably 1,000 to 2,000 mPa·s, and more preferably 1,000 to 1,800 mPa·s. The viscosity of the coating liquid can be controlled by the solids concentration of the coating liquid, the mixing ratio of the organic resin and the inorganic particles, and the molecular weight of the organic resin.

[0058] Next, the obtained coating liquid is coated on a porous substrate, passed through an air gap, immersed in a water tank, and dried to laminate a porous layer. When passing through the air gap, it is preferable to set the atmosphere under the conditions of a temperature of 40 to 80°C and a humidity of 60 to 80 RH% or more in order to improve the wettability of the electrolyte and to open uniform fine pores in the surface structure of the porous layer without having coarse pores in order to improve heat resistance.

[0059] The coating method may be a known method. For example, dip coating, gravure coating, slit die coating, knife coating, comma coating, kiss coating, roll coating, bar coating, spray coating, immersion coating, spin coating, screen printing, inkjet printing, pad printing, other types of printing, etc. may be used. The coating method is not limited to these, and may be selected according to the preferred conditions of the heat-resistant resin, aprotic organic polar solvent, inorganic particles, organic resin, dispersant, leveling agent, solvent to be used, substrate, etc. In addition, in order to improve the coatability, for example, the porous substrate may be subjected to a surface treatment of the coating surface, such as a corona treatment or a plasma treatment. (Characteristics of the porous layer) The porosity of the porous layer is 50% or more and 80% or less. The porosity is preferably 55% or more and 80% or less, more preferably 55% or more and 75% or less. When the porosity of the porous layer is 50% or more, deterioration of the battery characteristics can be prevented. When the porosity of the porous layer is 80% or less, for example, heat resistance can be sufficiently expressed. In addition, when the porosity of the porous layer is less than 50%, the ion permeability is reduced, and the battery characteristics may deteriorate, and when the porosity is higher than 80%, the heat resistance may decrease or powder fall of inorganic particles may occur. The porosity of the porous layer can be adjusted by adjusting the content and average particle size of the inorganic particles in the porous layer. In addition, the porosity of the porous layer can be calculated by binarization processing of the cross-sectional image or the affinity, thickness, and basis weight of the porous layer. Specifically, it can be obtained by the measurement method described in the examples.

[0060] The total thickness of the porous layers is preferably 1 μm or more and 6 μm or less. More preferably, it is 1.5 μm or more and 5 μm or less. Even more preferably, it is 2 μm or more and 4 μm or less. Here, the "total thickness of the porous layers" refers to the thickness of the porous layers when the porous substrate has a porous layer on one side, and refers to the total thickness of both porous layers when the porous substrate has a porous layer on both sides. When the total thickness of the porous layers is 1 μm or more, sufficient heat resistance to film breakage is obtained. Also, when it is 6 μm or less, a sufficient porous structure is obtained and the deterioration of the battery characteristics can be prevented. It is also advantageous in terms of cost.

[0061] [Porous polyolefin substrate] In the present invention, the polyolefin porous substrate may be a porous membrane, nonwoven fabric, or fibrous material containing polyolefin and having pores therein. The use of polyolefin can provide a shutdown function. The shutdown function here refers to a function that, when the lithium ion battery generates abnormal heat, closes the porous structure by melting with heat, stops ion movement, and stops power generation.

[0062] The polyolefin porous substrate is more preferably a porous substrate containing a polyolefin having a melting point of 200° C. or less. Specific examples of polyolefin include polyethylene, polypropylene, copolymers thereof, and mixtures of these, such as a single-layer porous substrate containing 90% by mass or more of polyethylene, and a multi-layer porous substrate made of polyethylene and polypropylene.

[0063] Examples of methods for producing a polyolefin porous substrate include a method in which a polyolefin resin is formed into a sheet and then stretched to make it porous, and a method in which a polyolefin resin is dissolved in a solvent such as liquid paraffin, formed into a sheet, and then the solvent is extracted to make it porous.

[0064] From the viewpoint of adhesion with the porous layer, the polyolefin porous substrate obtained by the above method may be subjected to surface treatment. Among them, it is preferable to perform corona treatment in air, nitrogen, or carbon dioxide gas atmosphere from the viewpoint of increasing the adhesion strength of the porous layer. However, corona treatment may cause holes in the polyolefin porous substrate if the treatment strength is too high.

[0065] The maximum height difference of the surface of the polyolefin porous substrate obtained by the above method is preferably 150 nm or more in terms of adhesion with the porous layer. The maximum height difference of the surface can be measured by an atomic force microscope. The measurement area is 4 × 4 μm. The maximum height difference of the surface of the porous substrate can be controlled by changing the stretching conditions of the porous substrate, specifically, the stretching ratio and the stretching temperature.

[0066] The thickness of the polyolefin porous substrate is preferably 3 μm or more and 50 μm or less, more preferably 5 μm or more and 30 μm or less. When the thickness of the polyolefin porous substrate is 50 μm or less, the internal resistance of the polyolefin porous substrate can be suppressed. Also, when the thickness of the polyolefin porous substrate is 3 μm or more, the mechanical properties required for transportation and coating can be obtained.

[0067] The air permeability of the polyolefin porous substrate is preferably 50 sec / 100 cc or more and 1,000 sec / 100 cc or less. More preferably, it is 50 sec / 100 cc or more and 500 sec / 100 cc or less. If the air permeability is 1,000 sec / 100 cc or less, sufficient ion mobility is obtained, and the battery can fully exhibit its characteristics. Also, if the air permeability is 50 sec / 100 cc or more, the mechanical properties required for transportation and coating can be obtained.

[0068] [Porous film] In the porous film of the present invention, the strength of the porous layer is 0.4 N / 10 mm or more, and the strength of the porous layer is lower than the adhesive strength between the polyolefin porous substrate and the porous layer in a 180-degree peel test in the longitudinal direction.

[0069] If the strength of the porous layer is less than 0.4 N / 10 mm, the strength of the porous layer is low, the function of the porous layer cannot be fully exhibited, and inorganic particles may be detached from the porous layer during battery assembly or coating, thereby contaminating the process. The strength of the porous layer is not particularly limited to an upper limit, but is preferably 5 N / 10 mm or less.

[0070] If the strength of the porous layer is greater than the adhesion strength between the polyolefin porous substrate and the porous layer in a 180-degree peel test in the longitudinal direction, the adhesion between the polyolefin porous substrate and the porous layer may be weak, and the functions of the porous substrate and the porous layer may not be fully expressed.

[0071] The balance between the strength of the porous layer and the adhesion strength between the polyolefin porous substrate and the porous layer in a 180-degree peel test in the longitudinal direction can be adjusted by adjusting the copolymerization ratio and / or logarithmic viscosity of the heat-resistant resin.

[0072] In addition, the strength of the porous layer and the adhesive strength between the polyolefin porous substrate and the porous layer in a 180-degree peel test in the longitudinal direction are determined by tape peeling measurement. The tape peeling measurement can be performed according to 10.3 Test Method-Method 1 described in JIS Z0237 (2009), by a 180-degree peel test in the longitudinal direction of the porous film. Specifically, it can be determined by the measurement method described in the examples.

[0073] The permeation rate of diethyl carbonate in the porous film of the present invention is preferably 4 μm / min or more. The upper limit of the permeation rate of diethyl carbonate is not particularly limited, but is preferably 200 μm / min or less. The permeation rate of diethyl carbonate is an index of the wettability of the electrolyte in the thickness direction. If the permeation rate of diethyl carbonate is less than 4 μm / min, the wettability of the electrolyte becomes insufficient, the electrolyte injection time in the battery assembly process becomes long, the process passability becomes poor, and the impregnation of the electrolyte in the thickness direction may become non-uniform.

[0074] The permeation rate of diethyl carbonate into a porous film can be calculated from the time it takes for 100 μL of diethyl carbonate to reach the back surface of a porous film when dropped onto the front surface of the film, and the thickness of the porous film.

[0075] The permeation area of ​​the porous film after 10 seconds of diethyl carbonate is 500 mm 2 The diethyl carbonate permeation area after 10 seconds is an index of the wettability of the electrolyte in the surface direction. 2 If the thickness is less than this, the wettability of the electrolyte may be insufficient, and the impregnation of the electrolyte in the surface direction may become non-uniform, which may result in deterioration of the battery characteristics.

[0076] The area of ​​diethyl carbonate permeated into the porous film after 10 seconds was calculated using image analysis software from an image of the surface of the porous film after 100 μL of diethyl carbonate was dropped and left for 10 seconds.

[0077] The permeation rate of diethyl carbonate into the porous film and the permeation area of ​​diethyl carbonate after 10 seconds can be adjusted by adjusting the copolymerization ratio and / or logarithmic viscosity of the heat-resistant resin and the content of inorganic particles in the porous layer.

[0078] The falling ball rupture temperature of the porous film is preferably 250°C or higher. The falling ball rupture temperature means the temperature at which a short circuit occurs under a constant load, and is an index for evaluating heat resistance. By setting the temperature at 250°C or higher, when the battery abnormally heats up, further heat generation due to short circuit of the battery and expansion of the short circuit area can be prevented. From the viewpoint of imparting heat resistance to the secondary battery, the falling ball rupture temperature is more preferably 280°C or higher, even more preferably 300°C or higher, and most preferably 350°C or higher.

[0079] The shutdown temperature of the porous film is preferably 135° C. or lower. When the shutdown temperature is 135° C. or lower, the shutdown function can be operated sufficiently even if the heat generation start temperature is lowered when the secondary battery has a high capacity and high output. From the viewpoint of further lowering the heat generation start temperature when the secondary battery has a high capacity and high output, the shutdown temperature is more preferably 130° C. or lower.

[0080] The difference between the shutdown temperature and the meltdown temperature of the porous film (meltdown temperature-shutdown temperature) is preferably 75°C or more. The above temperature difference can be achieved by either lowering the shutdown temperature or raising the meltdown temperature. When the difference between the shutdown temperature and the meltdown temperature is 75°C or more, the temperature difference until complete melting after the porous structure is closed by melting with heat due to heat generation becomes large, and the battery is short-circuited and heat generation can be suppressed. From the viewpoint of preventing short-circuiting, the difference between the shutdown temperature and the meltdown temperature is more preferably 100°C or more. The shutdown temperature refers to the temperature at which the porous structure is closed by melting with heat when the lithium ion battery generates abnormal heat, ion migration is stopped, and power generation is stopped, and the meltdown temperature refers to the temperature at which the porous film melts and the battery is short-circuited when heat is generated at or above the shutdown temperature. The shutdown temperature and meltdown temperature in the present invention can be evaluated by measuring the air permeability while increasing the temperature by the method described in the Examples section, and the change in air permeability.

[0081] The air permeability of the porous film is preferably 50 sec / 100 cc or more and 1,000 sec / 100 cc or less. More preferably, it is 50 sec / 100 cc or more and 500 sec / 100 cc or less. When the air permeability is 50 sec / 100 cc or more and 1,000 sec / 100 cc or less, sufficient ion mobility is obtained, and sufficient battery characteristics and sufficient mechanical characteristics are obtained.

[0082] [Secondary battery] The porous film of the present invention can be suitably used as a separator for secondary batteries such as lithium ion batteries. A lithium ion battery has a configuration in which a secondary battery separator and an electrolyte are interposed between a positive electrode in which a positive electrode active material is laminated on a positive electrode current collector and a negative electrode in which a negative electrode active material is laminated on a negative electrode current collector.

[0083] The positive electrode is a positive electrode material consisting of an active material, a binder resin, and a conductive assistant layered on a current collector. Examples of the active material include layered lithium-containing transition metal oxides such as LiCoO2, LiNiO2, and Li(NiCoMn)O2, spinel-type manganese oxides such as LiMn2O4, and iron-based compounds such as LiFePO4. As the binder resin, a resin with high oxidation resistance may be used. Specific examples include fluororesin, acrylic resin, and styrene-butadiene resin. Carbon materials such as carbon black and graphite are used as the conductive assistant. Metal foil is suitable as the current collector, and aluminum is often used in particular.

[0084] The negative electrode is a current collector on which negative electrode materials consisting of active materials and binder resins are laminated. The active materials include carbon materials such as artificial graphite, natural graphite, hard carbon, and soft carbon, lithium alloy materials such as tin and silicon, metal materials such as Li, and lithium titanate (Li4Ti5O 12 ) and the like. As the binder resin, fluororesin, acrylic resin, styrene-butadiene resin, and the like are used. As the current collector, a metal foil is suitable, and in particular, copper foil is often used.

[0085] The electrolyte is a place where ions move between the positive and negative electrodes in the secondary battery, and is composed of an electrolyte dissolved in an organic solvent. Examples of the electrolyte include LiPF6, LiBF4, and LiClO4, and LiPF6 is preferably used from the viewpoint of solubility in organic solvents and ionic conductivity. Examples of the organic solvent include diethyl carbonate, propylene carbonate, fluorodiethyl carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, gamma butyrolactone, and sulfolane, and two or more of these organic solvents may be mixed and used.

[0086] In the method of producing a secondary battery, first, an active material and a conductive assistant are dispersed in a binder solution to prepare an electrode coating solution, and the coating solution is applied onto a current collector, and the solvent is dried to obtain a positive electrode and a negative electrode. The thickness of the coating film after drying is preferably 50 μm to 500 μm. A separator for a secondary battery is placed between the obtained positive electrode and negative electrode so as to contact the active material layer of each electrode, and the separator is enclosed in an exterior material such as an aluminum laminate film. After injecting an electrolyte, a negative electrode lead and a safety valve are installed, and the exterior material is sealed. The secondary battery obtained in this way has high heat resistance to film breakage, has excellent battery characteristics, and can be manufactured at low cost. EXAMPLES

[0087] The present invention will be described in more detail below with reference to examples, but the present invention is not limited thereto. Measurement methods used in the examples are as follows.

[0088] [Measurement method] (1) Melting point of heat-resistant resin Using a differential scanning calorimeter (DSC) measuring in accordance with JIS K7121 (2012), the presence or absence of an endothermic peak during the second heating cycle after the first heating and cooling was measured, and the temperature of that peak was also measured.

[0089] (2) Strength of the porous layer and adhesion strength at the interface between the porous substrate and the porous layer According to 10.3 Test Method-Method 1 described in JIS Z0237 (2009), a 180-degree peel test was carried out using a RHEO METER CR-3000EX-S (manufactured by Sun Science Co., Ltd.) at a pulling speed of 5.0 mm per second in the longitudinal direction of the sample. A sample cut to a size of 10 mm x 150 mm from the porous film obtained in the embodiment was attached to a test plate with double-sided tape. Cellophane tape (manufactured by Nichiban) of the same size was attached to the surface of the sample using a roll press machine under conditions of 0.5 MPa and 0.2 m / min, and the end of the tape was held and folded 180° so that the back of the cellophane tape overlapped, and the cellophane tape was peeled off. When the cellophane tape was peeled off from the sample by 50% of the length, if even one polyolefin porous substrate was confirmed at the peeled portion, it was determined that the adhesion strength between the polyolefin porous substrate and the porous layer was lower than the strength of the porous layer, and peeling occurred at the interface between the polyolefin porous substrate and the porous layer (Table 1 "Interface"). In other words, it indicates that the strength of the porous layer is higher than the adhesive strength between the polyolefin porous substrate and the porous layer. When the polyolefin porous substrate could not be confirmed (when the surface of the polyolefin porous substrate of the peeled sample was covered with the resin or particles that constitute the porous layer), it was determined that the adhesive strength between the polyolefin porous substrate and the porous layer was higher than the strength of the porous layer, and cohesive failure occurred at the porous layer (Table 1 "Porous Layer"). In other words, it indicates that the strength of the porous layer is lower than the adhesive strength between the polyolefin porous substrate and the porous layer. The strength of the porous layer was the average value of the measured values ​​of 50% of the length peeled off from the test plate when cohesive failure occurred (excluding the measured values ​​of the first 25% of the length after the start of measurement). Measurements were performed five times for each sample. The unit was expressed in N / 10 mm. The peeled part was the part with the lowest strength.

[0090] (3) Porosity of the porous layer The porosity of the porous layer was measured by freezing the porous film with liquid nitrogen, irradiating it with an argon beam from above, preparing a cross section (Cryo-BIB method), and ion-coating the cross section with an ion coater to prepare a measurement sample. The obtained sample was observed with a Hitachi High-Technologies Corporation field emission scanning electron microscope (FE-SEM) S4800 at an accelerating voltage of 1.5 kV, with a magnification of 20,000 times for the surface and 40,000 times for the cross section, to obtain image data (images of only the observed part without any indication of scale bars, etc.). The image was cut out from the obtained image data so that only the porous layer remained, and image analysis was performed using MVTec's HALCON Ver.10.0 to calculate the porosity of the porous layer. As an image analysis method, first, an 11-pixel average image A and a 3-pixel average image B were generated from the 256-tone monochrome image, and the area (Area_all) of the entire image B was calculated. Next, image A was removed as the difference from image B to generate image C, and area D with a brightness of ≥ 10 was extracted. The extracted region D was divided into chunks, and a region E with an area of ​​≧100 was extracted. A region F was generated by closing the region E with a circular element of radius 2.5 pixels, and a region G was generated by opening the region E with a rectangular element of 1 horizontal x 5 vertical pixels, thereby removing pixels with a vertical size <5. Then, the fibril region was extracted by dividing the region G into chunks and extracting a region H with an area of ​​≧500. Furthermore, a region I with an image size ≧5 was extracted in the image C, and the region I was divided into chunks to extract a region J with an area ≧300. After opening the region J with a circular element of radius 1.5 pixels, a region K with a closing process with a circular element of radius 8.5 pixels was generated, and a region L with an area ≧200 was extracted from the region K. In the region L, a region M in which a dark part with an area ≧4,000 pixels was filled with a light part was generated to extract the unopened part other than the fibril. Finally, the area of ​​the unopened portion was obtained by generating a sum area N of the areas H and M and calculating the area (Area_closed) of the sum area N. The calculation was performed using the following formula. Porosity of porous layer (%) = (Area_all - Area_closed) / Area_all × 100 (4) Diethyl carbonate permeation rate and permeation area A sample of 100 mm x 100 mm was cut out and used as a sample. The sample was attached to a metal frame (outer diameter 100 mm x 100 mm, inner diameter 90 mm x 90 mm), and then 100 μL of diethyl carbonate was dropped onto the sample. The permeation rate of diethyl carbonate was calculated from the time it took for diethyl carbonate to reach the back side of the sample and the thickness of the sample.

[0091] In addition, diethyl carbonate was dropped and left for 10 seconds, after which an image was taken. The image was analyzed using image analysis software (Toyo Corporation, SPIP) as follows. After emphasizing the boundary between diethyl carbonate and the film using a general-purpose plug-in (PrugIn_BoundaryDropper (Particle7x7)) for the HeightSensor image, the area of ​​diethyl carbonate included in the field of view, excluding the edge of the image, was calculated using an automatic threshold calculation, and the value was taken as the penetration area.

[0092] (5) Falling ball rupture temperature A sample of 50 mm x 50 mm was cut out and used as a sample. The cut out sample was fixed in a metal frame with a φ12 mm hole in the center. A φ10 mm tungsten ball was placed in the φ12 mm hole and set in a hot air oven. The temperature was raised at 5°C / min, and the temperature at which the tungsten ball fell was measured. The temperature was averaged over five tests for each sample and used as the falling ball film rupture temperature.

[0093] (6) Thickness of the porous layer A cross section of the sample was cut out with a microtome, and the cross section was observed with a field emission scanning electron microscope. Within the observed area, the apex of the part that penetrated the porous layer the most was selected, and the distance from the bottom surface (porous substrate side) of the porous layer to the highest point on the surface was measured as the thickness of the porous layer. The average value of the observation, selection, and measurement of five arbitrary points on a 100 mm x 100 mm sample was taken as the thickness of the porous layer.

[0094] (7) Shutdown temperature, meltdown temperature The shutdown temperature and meltdown were measured by the method disclosed in WO 2007 / 052663. According to this method, the porous film was exposed to an atmosphere of 30°C and heated at a rate of 5°C / min, during which the air permeability of the membrane was measured. The air permeability of the porous film (Oken) was initially 100,000 sec / 100 cm 3 The temperature at which the air permeability exceeds 100,000 sec / 100 cm is defined as the shutdown temperature of the porous film. 3 Then, first 10 seconds / 100cm 3 The temperature at which the temperature reached or below this value was defined as the meltdown temperature of the porous film. The upper limit of the meltdown temperature measurement is 250° C. The air resistance of the porous film was measured according to JIS P8117 (2009) using an Oken type air resistance meter (EGO-1T, manufactured by Asahi Seiko Co., Ltd.).

[0095] (8) Air permeability Measurements were performed using an Oken air resistance meter (EGO-1T, manufactured by Asahi Seiko Co., Ltd.) in accordance with JIS P8117 (1998).

[0096] (9) Battery construction The positive electrode sheet contains Li(Ni 5 / 10 Mn 2 / 10 Co 3 / 10 A positive electrode slurry was prepared by dispersing 92 parts by mass of 10 ... 2). This positive electrode sheet was cut to 40 mm x 40 mm. At this time, the current collecting tab adhesive portion without the active material layer was cut out to a size of 5 mm x 5 mm on the outside of the active material surface. An aluminum tab with a width of 5 mm and a thickness of 0.1 mm was ultrasonically welded to the tab adhesive portion. The negative electrode sheet was prepared by dispersing 98 parts by mass of natural graphite as the negative electrode active material, 1 part by mass of carboxymethyl cellulose as a thickener, and 1 part by mass of styrene-butadiene copolymer as a negative electrode binder in water using a planetary mixer, coating the negative electrode slurry on copper foil, drying, and rolling (coating basis weight: 5.5 mg / cm). 2 ). This negative electrode sheet was cut to 45 mm x 45 mm. At this time, the tab adhesive part for current collection without the active material layer was cut out to a size of 5 mm x 5 mm on the outside of the active material surface. A copper tab of the same size as the positive electrode tab was ultrasonically welded to the tab adhesive part. Next, a porous film was cut to 55 mm x 55 mm, and the positive electrode and negative electrode were stacked on both sides of the porous film so that the active material layer separated the porous film, and the positive electrode coating part was arranged so that all the positive electrode coating parts faced the negative electrode coating parts to obtain an electrode group. The positive electrode, negative electrode, and porous film were sandwiched between one 90 mm x 200 mm aluminum laminate film, the long side of the aluminum laminate film was folded, and the two long sides of the aluminum laminate film were heat-sealed to form a bag shape. The electrolyte was prepared by dissolving LiPF6 as a solute in a mixed solvent of diethyl carbonate:diethyl carbonate = 1:1 (volume ratio) to a concentration of 1 mol / L. 1.5 g of the electrolyte was poured into a bag-shaped aluminum laminate film, and the short sides of the aluminum laminate film were heat-sealed while being impregnated under reduced pressure to form a laminated battery.

[0097] (10) Discharge rate characteristics The discharge rate characteristics of the laminated battery were tested according to the following procedure, and evaluated by the discharge capacity retention rate. The charging conditions were constant current charging at 0.5C and 4.25V, and the discharging conditions were constant current discharging at 0.5C and 7C and 2.7V. <Calculation of Discharge Capacity Retention Rate> The discharge capacity retention rate was calculated by (discharge capacity at 7C) / (discharge capacity at 0.5C) x 100. Five laminated batteries were produced, and the average was taken as the discharge capacity retention rate. The ratings were as follows: ◯: 80% or more, △: 75% or more but less than 80%, ×: less than 75%.

[0098] (11) Cycle characteristics The cycle characteristics of the laminated battery were tested according to the following procedure, and evaluated based on the discharge capacity retention rate after 500 cycles. The charging conditions were constant current charging at 2C and 4.25V, and the discharging conditions were constant current discharging at 2C and 2.7V. <Calculation of Discharge Capacity Retention Rate> The discharge capacity retention rate was calculated by (discharge capacity at 500 cycles) / (discharge capacity at 1 cycle) x 100. Five laminated batteries were produced, and the average was taken as the discharge capacity retention rate. The ratings were as follows: Good (○): 80% or more, Average (△): 75% to less than 80%, and Poor (×): less than 75%.

[0099] (12) Hot box test The laminated battery thus produced was subjected to a hot box test according to the following procedure, and was evaluated based on the discharge capacity retention rate. The battery was charged at a constant current of 0.5C and 4.25V, and the temperature was raised to 150°C at 5°C / min to check for smoke and fire. Five laminated batteries were produced, and the results were judged as follows: ○: no smoke or fire, ×: smoke or fire.

[0100] Example 1 2-chloro-1,4-phenylenediamine equivalent to 85 mol % and 4,4'-diaminodiphenyl ether equivalent to 15 mol % were dissolved in dehydrated N-methyl-2-pyrrolidone. 2-chloroterephthaloyl chloride equivalent to 99 mol % of the total amount of diamine was added thereto as an acid dichloride and stirred to polymerize an aromatic polyamide resin. The obtained polymerization solution was neutralized with lithium carbonate of 97 mol % of the total amount of acid dichloride, and further neutralized with diethanolamine of 15 mol % and triethanolamine of 25 mol % to obtain an aromatic polyamide resin solution with an aromatic polyamide resin concentration of 10 mass %. The obtained aromatic polyamide resin does not have the above-mentioned peak top in the measurement temperature range of -20 to 230 ° C., and can be said to be a heat-resistant resin without a melting point. In addition, the logarithmic viscosity ηinh of the obtained aromatic polyamide was 4.5 dl / g. N-methyl-2-pyrrolidone was added to the obtained aromatic polyamide resin solution, and the solution was primarily dispersed with a stirrer. In addition, N-methyl-2-pyrrolidone was added to alumina particles A (average particle size 0.4 μm) and alumina particles B (average particle size 0.05 μm), and the solution was primarily dispersed with a stirrer. The dispersions obtained by the primary dispersion were combined and mixed so that the aromatic polyamide resin was 10 parts by mass, the alumina particles A was 85 parts by mass, and the alumina particles B was 5 parts by mass, relative to a total of 100 parts by mass of the aromatic polyamide resin and the alumina particles, and N-methyl-2-pyrrolidone was additionally added so that the solid content concentration was 20% by mass. The mixed solution was further primarily dispersed with a stirrer. The prepared primary dispersion was dispersed using a bead mill. Zirconia-reinforced alumina beads with a diameter of 0.5 mm were used, and the beads were dispersed once at a peripheral speed of 5 m / s, once at a peripheral speed of 7 m / s, and twice at a peripheral speed of 10 m / s to obtain a secondary dispersion. The viscosity of the obtained secondary dispersion was 1200 mPa·s. The obtained secondary dispersion was applied by dip coating to both sides of a polyethylene porous substrate (thickness 5 μm, air permeability 120 sec / 100 cc, maximum surface height difference 160 nm) that had been corona-treated in an air atmosphere, and then immersed in a water tank and dried until the solvent contained therein volatilized to form a porous layer, thereby obtaining a porous film of the present invention. The measurement results of the properties of the obtained porous film are shown in Table 1.

[0101] Example 2 In dehydrated N-methyl-2-pyrrolidone, 2-chloro-1,4-phenylenediamine equivalent to 90 mol % and 4,4'-diaminodiphenyl ether equivalent to 10 mol % were dissolved relative to the total amount of diamines. The resulting aromatic polyamide does not have the above-mentioned peak top in the measurement temperature range of -20 to 230°C, and can be said to be a heat-resistant resin that does not have a melting point. In addition, the inherent viscosity ηinh was 4.7 dl / g. In the same manner as in Example 1, a porous film of the present invention was obtained.

[0102] Example 3 2-chloro-1,4-phenylenediamine equivalent to 95 mol % and 4,4'-diaminodiphenyl ether equivalent to 5 mol % based on the total amount of diamines were dissolved in dehydrated N-methyl-2-pyrrolidone, and the resulting aromatic polyamide did not have the above-mentioned peak top in the measurement temperature range of -20 to 230 ° C., and it can be said to be a heat-resistant resin that does not have a melting point. In addition, the inherent viscosity ηinh was 4.9 dl / g. In the same manner as in Example 1, a porous film of the present invention was obtained.

[0103] Example 4 A porous film of the present invention was obtained in the same manner as in Example 1, except that the maximum height difference of the polyethylene porous substrate was set to 200 nm.

[0104] Example 5 The secondary dispersion obtained in Example 3 was applied by dip coating to both sides of a polyethylene porous substrate (thickness 5 μm, air permeability 120 sec / 100 cc) that had been subjected to corona treatment under an air atmosphere, and the porous film of the present invention was obtained in the same manner as in Example 3, except that the substrate was passed through an air gap at a temperature of 60°C and a humidity of 70 RH%.

[0105] Example 6 The secondary dispersion obtained in Example 3 was applied by dip coating to both sides of a polyethylene porous substrate (thickness 5 μm, air permeability 120 sec / 100 cc) that had been subjected to corona treatment under an air atmosphere, and the porous film of the present invention was obtained in the same manner as in Example 3, except that the substrate was passed through an air gap at a temperature of 65°C and a humidity of 75 RH%.

[0106] Comparative Example 1 In dehydrated N-methyl-2-pyrrolidone, 2-chloro-1,4-phenylenediamine equivalent to 75 mol% and 4,4'-diaminodiphenyl ether equivalent to 25 mol% were dissolved relative to the total amount of diamines, and the resulting aromatic polyamide had no peak top in the measurement temperature range of -20 to 230 ° C., and could be said to be a heat-resistant resin without a melting point, and had a logarithmic viscosity ηinh of 2.5 dl / g. A porous film was obtained in the same manner as in Example 1, except that the aromatic polyamide resin was 10 parts by mass and the alumina particles A were 90 parts by mass relative to a total of 100 parts by mass of the aromatic polyamide resin and the alumina particles A, and the polyethylene porous substrate with a maximum height difference of 130 nm was not corona-treated.

[0107] Comparative Example 2 In dehydrated N-methyl-2-pyrrolidone, 2-chloro-1,4-phenylenediamine equivalent to 75 mol% and 4,4'-diaminodiphenyl ether equivalent to 25 mol% were dissolved relative to the total amount of diamines, and the resulting aromatic polyamide had no peak top in the measurement temperature range of -20 to 230 ° C., and could be said to be a heat-resistant resin without a melting point, and had a logarithmic viscosity ηinh of 2.2 dl / g. A porous film was obtained in the same manner as in Example 1, except that the aromatic polyamide resin was 30 parts by mass and the alumina particles A were 70 parts by mass relative to a total of 100 parts by mass of the aromatic polyamide resin and the alumina particles A, and the polyethylene porous substrate with a maximum height difference of 130 nm was not corona-treated.

[0108] [Table 1]

[0109] As can be seen from Table 1, in all of the Examples, the properties of the porous layer are fully exhibited, and good battery properties are obtained.

[0110] On the other hand, in the comparative examples, the strength of the porous layer was low, or the adhesion strength at the interface between the porous layer and the porous substrate was low, so that the characteristics of the porous layer were not expressed, or the battery characteristics were insufficient.

Claims

1. A porous film in which a porous layer containing a heat-resistant resin having a melting point of 200° C. or more or having no melting point is laminated on at least one surface of a polyolefin porous substrate, the porous layer has a porosity of 50% or more and 80% or less, and has a strength of 0.4 N / 10 mm or more as measured according to 10.3 Test Method-Method 1 described in JIS Z0237 (2009), and the strength of the porous layer is lower than the adhesion strength between the polyolefin porous substrate and the porous layer in a 180-degree peel test in the longitudinal direction; The permeation rate of diethyl carbonate through the porous film is 4 μm / min or more, and the permeation area of ​​diethyl carbonate after 10 seconds is 500 mm 2 or more, The difference between the shutdown temperature and the meltdown temperature of the porous film is 70° C. or more; Porous film. The permeation rate was calculated from the time taken for 100 μL of diethyl carbonate to reach the rear surface after being dropped and the thickness of the porous film. The permeation area of ​​diethyl carbonate is calculated using image analysis software from an image taken after dropping 100 μL of diethyl carbonate and leaving it for 10 seconds.

2. The porous film according to claim 1 , wherein the porous layer contains inorganic particles.

3. The porous film according to claim 1 or 2, wherein the porous film has a falling ball rupture temperature of 250°C or higher.

4. A separator for a secondary battery, comprising the porous film according to any one of claims 1 to 3.

5. A secondary battery using the separator for secondary batteries according to claim 4.

Citation Information

Patent Citations

  • Non-aqueous electrolyte battery separator and lithium secondary battery

    JP2000030686A

  • Separator for lithium battery

    JP2002216734A

  • Nonaqueous electrolyte battery separator and nonaqueous electrolyte secondary battery

    JP2009231281A

  • Separator for battery and lithium secondary battery

    JP2010123465A

  • Porous polypropylene film, and separator for electricity storing device

    JP2012117047A