Positive electrode for all-solid-state battery, all-solid-state battery, and method for producing positive electrode for all-solid-state battery

The positive electrode for all-solid-state batteries, featuring a sulfide-based glass and crystalline solid electrolyte matrix with a composite coating, addresses the capacity retention issue by improving ion conduction and reaction interfaces, enhancing battery performance.

JP7567508B2Active Publication Date: 2024-10-16GS YUASA CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2021012454
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-01-28
Publication Date
2024-10-16
Estimated Expiration
2041-01-28

AI Technical Summary

Technical Problem

All-solid-state batteries used in hybrid electric vehicles and hybrid industrial machinery experience a significant decrease in capacity retention rate after charge/discharge cycles, necessitating an improvement in battery performance.

Method used

A positive electrode for all-solid-state batteries is designed with a matrix composed of a sulfide-based glass solid electrolyte and a sulfide-based crystalline solid electrolyte, incorporating a positive electrode active material composite that covers the active material particles, enhancing ion conduction paths and reaction interfaces to improve capacity retention.

Benefits of technology

The proposed electrode structure effectively suppresses the decrease in capacity retention rate after charge/discharge cycles, maintaining battery performance and efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007567508000002
    Figure 0007567508000002
  • Figure 0007567508000003
    Figure 0007567508000003
  • Figure 0007567508000004
    Figure 0007567508000004
Patent Text Reader

Abstract

To provide a positive electrode for an all-solid-state battery capable of suppressing a decrease in capacity retention rate after the charge-discharge cycle of the all-solid-state battery.SOLUTION: A positive electrode for an all-solid-state battery includes a positive electrode base material and a positive electrode mixture layer, and the positive electrode mixture layer includes a matrix mainly composed of a first sulfide-based solid electrolyte, and a positive electrode active material composite dispersed in the matrix, the positive electrode active material composite includes positive electrode active material particles and a second sulfide-based solid electrolyte that directly or indirectly coats at least part of the surfaces the positive electrode active material particles, and the first sulfide-based solid electrolyte includes a sulfide-based glass solid electrolyte and a sulfide-based crystalline solid electrolyte.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a positive electrode for an all-solid-state battery, an all-solid-state battery, and a method for producing a positive electrode for an all-solid-state battery. [Background technology]

[0002] Lithium ion secondary batteries are widely used in electronic devices such as personal computers and communication terminals, automobiles, etc., due to their high energy density. The lithium ion secondary battery generally has a pair of electrodes electrically isolated by a separator and a non-aqueous electrolyte interposed between the electrodes, and is configured to charge and discharge by transferring lithium ions between the electrodes. In addition, capacitors such as lithium ion capacitors are also widely used as all-solid-state batteries other than lithium ion secondary batteries.

[0003] In recent years, with the aim of improving the safety of non-aqueous electrolyte secondary batteries, all-solid-state batteries have been proposed that use a sulfide solid electrolyte or the like as the non-aqueous electrolyte instead of a liquid electrolyte such as an organic solvent (see Patent Document 1). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2000-340257 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, in all-solid-state batteries used in hybrid electric vehicles (hereinafter also referred to as "HEVs") and hybrid industrial machinery (heavy machinery, construction machinery, etc.), there is a demand for an improvement in the effect of suppressing the decrease in capacity retention rate after charge-discharge cycles.

[0006] The present invention has been made in light of the above circumstances, and has an object to provide a positive electrode for an all-solid-state battery that can suppress a decrease in the capacity retention rate after charge-discharge cycles of the all-solid-state battery. [Means for solving the problem]

[0007] A positive electrode for an all-solid-state battery according to one aspect of the present invention includes a positive electrode base material and a positive electrode mixture layer, the positive electrode mixture layer having a matrix mainly composed of a first sulfide-based solid electrolyte and a positive electrode active material composite dispersed in the matrix, the positive electrode active material composite containing positive electrode active material particles and a second sulfide-based solid electrolyte directly or indirectly covering at least a portion of the surface of the positive electrode active material particles, and the first sulfide-based solid electrolyte includes a sulfide-based glass solid electrolyte and a sulfide-based crystalline solid electrolyte.

[0008] A method for producing a positive electrode for an all-solid-state battery according to another aspect of the present invention includes compounding positive electrode active material particles and a sulfide-based solid electrolyte, and producing a positive electrode mixture including the positive electrode active material composite obtained by the compounding, a sulfide-based glass solid electrolyte, and a sulfide-based crystalline solid electrolyte. Effect of the Invention

[0009] According to the positive electrode for an all-solid-state battery according to one aspect of the present invention, it is possible to suppress a decrease in the capacity retention rate after charge-discharge cycles of the all-solid-state battery. [Brief description of the drawings]

[0010] [Figure 1] FIG. 1 is a schematic cross-sectional view of a positive electrode for an all-solid-state battery according to one embodiment of the present invention. [Diagram 2] FIG. 2 is a schematic cross-sectional view of an all-solid-state battery according to one embodiment of the present invention. [Diagram 3] FIG. 3 is a schematic diagram showing an electricity storage device configured by assembling a plurality of all-solid-state batteries according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] First, an outline of the positive electrode for an all-solid-state battery, the all-solid-state battery, and the method for producing the positive electrode for an all-solid-state battery disclosed in this specification will be described.

[0012] A positive electrode for an all-solid-state battery according to one aspect of the present invention includes a positive electrode base material and a positive electrode mixture layer, the positive electrode mixture layer having a matrix mainly composed of a first sulfide-based solid electrolyte and a positive electrode active material composite dispersed in the matrix, the positive electrode active material composite containing positive electrode active material particles and a second sulfide-based solid electrolyte directly or indirectly covering at least a portion of the surface of the positive electrode active material particles, and the first sulfide-based solid electrolyte includes a sulfide-based glass solid electrolyte and a sulfide-based crystalline solid electrolyte.

[0013] The present inventors have found that the increase in resistance of an all-solid-state battery accompanying charge-discharge cycles can be suppressed by using a composite of a cathode active material particle and a sulfide-based solid electrolyte, in which at least a part of the surface of the cathode active material particle is directly or indirectly coated with a specific sulfide-based solid electrolyte. The inventors have come up with the present invention, thinking that the decrease in the capacity retention rate after charge-discharge cycles of an all-solid-state battery can be suppressed by using the above composite in combination with a matrix mainly composed of a specific sulfide-based solid electrolyte as a material for a cathode for an all-solid-state battery. The cathode for an all-solid-state battery can suppress the decrease in the capacity retention rate after charge-discharge cycles of an all-solid-state battery. The reason for this is unclear, but the following reason is presumed. The cathode active material composite is a composite of a cathode active material particle and a second sulfide-based solid electrolyte, and thus a good ion conduction path is formed. Therefore, the ion conductivity at the interface of the cathode active material particles is improved. In addition, since the matrix of the positive electrode mixture layer is mainly composed of a first sulfide-based solid electrolyte that is a combination of a relatively soft sulfide-based glass solid electrolyte and a relatively hard sulfide-based crystalline solid electrolyte, the packing density of the positive electrode mixture can be increased. By increasing the charging density, a good reaction interface is formed, improving the uniformity of the charge / discharge reaction. Therefore, the positive electrode can suppress the decrease in the capacity retention rate after the charge / discharge cycle of the all-solid-state battery.

[0014] The term "composite" refers to a state in which the positive electrode active material particles and the second sulfide-based solid electrolyte are mechanically combined. The above-mentioned composite refers to a state in which the positive electrode active material particles and the second sulfide-based solid electrolyte are present in one particle, and means that the positive electrode active material particles and the second sulfide-based solid electrolyte form an aggregated state, or that at least a part of the surface of the positive electrode active material particles is directly or indirectly covered with the second sulfide-based solid electrolyte. The term "main component" refers to a component that is contained in the largest amount, for example, a component that is contained in an amount of 50 mass% or more relative to the total mass.

[0015] The second sulfide-based solid electrolyte is preferably a sulfide-based crystalline solid electrolyte. By using the second sulfide-based solid electrolyte as a sulfide-based crystalline solid electrolyte, the effect of suppressing the decrease in the capacity retention rate after charge-discharge cycles of the all-solid-state battery can be improved.

[0016] It is preferable that the sulfide-based glass solid electrolyte is yLi2S·(1-y)P2S5 (where 0.75≦y≦0.77) and the sulfide-based crystalline solid electrolyte has a crystal structure that is cubic, orthorhombic, triclinic, or a combination thereof. By the sulfide-based glass solid electrolyte being yLi2S·(1-y)P2S5 (where 0.75≦y≦0.77) and the sulfide-based crystalline solid electrolyte having a crystal structure that is cubic, orthorhombic, or a combination thereof, the effect of suppressing the decrease in the capacity retention rate after charge-discharge cycles of the all-solid-state battery can be improved.

[0017] An all-solid-state battery according to one aspect of the present invention is an all-solid-state battery including the positive electrode. Since the all-solid-state battery includes the positive electrode, a decrease in capacity retention rate after charge-discharge cycles can be suppressed.

[0018] A method for producing a positive electrode for an all-solid-state battery according to another aspect of the present invention includes compounding positive electrode active material particles and a sulfide-based solid electrolyte, and producing a positive electrode mixture including the positive electrode active material composite obtained by the compounding, a sulfide-based glass solid electrolyte, and a sulfide-based crystalline solid electrolyte.

[0019] The manufacturing method for an all-solid-state battery positive electrode includes the above steps, and thereby can reliably manufacture a positive electrode for an all-solid-state battery that can suppress a decrease in the capacity retention rate after charge-discharge cycles of the all-solid-state battery.

[0020] Here, "composite" means that mechanical energy such as impact, compression, shear, etc. is applied to a mixture of core positive electrode active material particles and sulfide-based solid electrolyte particles that are a different material from the positive electrode active material particles and are smaller than the positive electrode active material particles, thereby directly or indirectly covering at least a portion of the surface of the positive electrode active material particles with a large number of sulfide-based solid electrolyte particles without using a binder, thereby generating a composite.

[0021] The configuration of the positive electrode for an all-solid-state battery according to one embodiment of the present invention, the configuration of the all-solid-state battery, the manufacturing method of the positive electrode for an all-solid-state battery, and other embodiments will be described in detail. Note that the names of the components (each component) used in each embodiment may differ from the names of the components (each component) used in the background art.

[0022] <Cathode for all-solid-state batteries> The positive electrode for an all-solid-state battery according to one embodiment of the present invention includes a positive electrode substrate and a positive electrode mixture layer. In the positive electrode of this embodiment, the positive electrode mixture layer is disposed on the positive electrode substrate directly or via an intermediate layer.

[0023] [Positive electrode substrate] The positive electrode substrate has electrical conductivity. Whether or not it has "electrical conductivity" is judged by using a volume resistivity of 107 Ω·cm measured in accordance with JIS-H-0505 (1975) as a threshold value. Metals such as aluminum, titanium, tantalum, stainless steel, etc., or alloys thereof are used as the material of the positive electrode substrate. Among these, aluminum or aluminum alloys are preferred from the viewpoints of potential resistance, high electrical conductivity, and cost. Examples of the positive electrode substrate include foil, vapor deposition film, mesh, and porous material, and foil is preferred from the viewpoint of cost. Therefore, aluminum foil or aluminum alloy foil is preferred as the positive electrode substrate. Examples of aluminum or aluminum alloys include A1085, A3003, A1N30, etc., as specified in JIS-H-4000 (2014) or JIS-H4160 (2006).

[0024] The average thickness of the positive electrode substrate is preferably 3 μm to 50 μm, more preferably 5 μm to 40 μm, even more preferably 8 μm to 30 μm, and particularly preferably 10 μm to 25 μm. By setting the average thickness of the positive electrode substrate within the above range, it is possible to increase the strength of the positive electrode substrate and to increase the energy density per volume of the secondary battery.

[0025] The intermediate layer is a layer disposed between the positive electrode substrate and the positive electrode mixture layer. The intermediate layer contains a conductive agent such as carbon particles to reduce the contact resistance between the positive electrode substrate and the positive electrode mixture layer. The configuration of the intermediate layer is not particularly limited, and may contain, for example, a binder and a conductive agent.

[0026] [Positive electrode mixture layer] The positive electrode mixture layer has a matrix mainly composed of a first sulfide-based solid electrolyte and a positive electrode active material composite dispersed in the matrix. The positive electrode mixture layer contains optional components such as a conductive agent, a binder, a thickener, and a filler as necessary. FIG. 1 is a schematic cross-sectional view of a positive electrode for an all-solid-state battery according to one embodiment of the present invention. As shown in FIG. 1, the positive electrode for an all-solid-state battery 1 includes a positive electrode substrate 4 and a positive electrode mixture layer 5. The positive electrode mixture layer 5 includes a matrix 12 mainly composed of a first sulfide-based solid electrolyte and a positive electrode active material composite 14 dispersed in the matrix 12. The positive electrode active material composite 14 contains a positive electrode active material particle 11 and a second sulfide-based solid electrolyte 13 that directly or indirectly covers at least a part of the surface of the positive electrode active material particle 11.

[0027] (matrix) The matrix 12 is mainly composed of a first sulfide-based solid electrolyte. The first sulfide-based solid electrolyte includes a sulfide-based glass solid electrolyte and a sulfide-based crystalline solid electrolyte. The matrix 12 of the positive electrode mixture layer is mainly composed of the first sulfide-based solid electrolyte, which is a combination of a relatively soft sulfide-based glass solid electrolyte and a relatively hard sulfide-based crystalline solid electrolyte, and therefore the packing density of the positive electrode mixture can be increased.

[0028] Examples of the sulfide-based glass solid electrolyte include Li2S-P2S5, Li2S-P2S5-LiI, Li2S-P2S5-LiCl, Li2S-P2S5-LiBr, etc. Among them, from the viewpoint of improving the effect of suppressing the decrease in the capacity retention rate after charge-discharge cycles of the all-solid-state battery, yLi2S·(1-y)P2S5 (where 0.75≦y≦0.77) is preferred, and 0.75Li2S·0.25P2S5 is more preferred.

[0029] The sulfide-based crystalline solid electrolyte preferably has a crystal structure that is a cubic system, an orthorhombic system, a triclinic system, or a combination thereof, from the viewpoint of improving the effect of suppressing the decrease in the capacity retention rate after charge / discharge cycles of the all-solid-state battery.

[0030] Examples of the sulfide-based crystalline solid electrolyte having a cubic crystal structure include Li6PS5Cl and Li7PS6.

[0031] As an example of the sulfide-based crystalline solid electrolyte having the above-mentioned orthorhombic crystal structure, there is β-Li3S 11 , Li 9.6 P3S 12 , Li 10 GeP2S 12 , Li 9.54 S 1.74 P 1.44 S 11.7 Cl 0.3 etc.

[0032] As an example of the sulfide-based crystalline solid electrolyte having the above-mentioned triclinic crystal structure, Li7P3S 11 etc.

[0033] Of these, the sulfide-based crystalline solid electrolyte is preferably a cubic crystal, an orthorhombic crystal, or a combination thereof, from the viewpoint of the effect of suppressing the decrease in the capacity retention rate after charge-discharge cycles.

[0034] The shape of the sulfide-based glass solid electrolyte and the sulfide-based crystalline solid electrolyte is not particularly limited, and is usually granular, blocky, or the like.

[0035] The ratio of the contents of the sulfide-based glass solid electrolyte and the sulfide-based crystalline solid electrolyte in the first sulfide-based solid electrolyte (sulfide-based crystalline solid electrolyte / sulfide-based glass solid electrolyte) is preferably 30 / 70 or more and 70 / 30 or less, more preferably 50 / 50, by mass ratio. By having the ratio of the contents of the sulfide-based glass solid electrolyte and the sulfide-based crystalline solid electrolyte within the above range, the effect of suppressing the decrease in the capacity retention rate after charge / discharge cycles of the all-solid-state battery can be improved.

[0036] (Cathode active material composite) The positive electrode active material composite 14 contains positive electrode active material particles 11 and a second sulfide-based solid electrolyte 13 that directly or indirectly covers at least a part of the surface of the positive electrode active material particles. Since the positive electrode active material composite 14 is a composite of the positive electrode active material particles 11 and the sulfide-based solid electrolyte 13, a good ion conduction path is formed, and therefore the ion conductivity at the interface between the positive electrode active material particles is improved.

[0037] The ratio of the contents of the cathode active material particles 11 and the second sulfide solid electrolyte 13 in the cathode active material composite 14 (second sulfide solid electrolyte 13 / cathode active material particles 11) is preferably 5 / 95 to 10 / 90 in mass ratio, and more preferably 5 / 95 to 7 / 93 in mass ratio. By having the ratio of the contents of the cathode active material particles 11 and the second sulfide solid electrolyte 13 within the above range, it is possible to improve ion conductivity while suppressing a decrease in charge / discharge performance due to an increase in resistance of the all-solid-state battery.

[0038] The total surface area [m 2 The content [g] of the second sulfide-based solid electrolyte 13 relative to the total mass of the electrolyte is 0.75 g / 28.5 m. 2 More than 1.5g / 5.4m 2 Less than 0.75g / 14.25m is preferred. 2 More than 0.75g / 8.55m 2 The following is more preferable. When the content of the second sulfide-based solid electrolyte 13 relative to the total surface area of ​​the positive electrode active material particles 11 is within the above range, it is possible to improve ion conductivity while suppressing a decrease in charge / discharge performance due to an increase in resistance of the all-solid-state battery.

[0039] (Cathode active material particles) A material capable of absorbing and releasing lithium ions is usually used as the positive electrode active material particles 11. Examples of the positive electrode active material particles 11 include lithium transition metal composite oxides having an α-NaFeO2 crystal structure, lithium transition metal composite oxides having a spinel crystal structure, polyanion compounds, chalcogen compounds, and sulfur. Examples of the lithium transition metal composite oxides having an α-NaFeO2 crystal structure include Li[Lix Ni (1-x) ]O2(0≦x<0.5), Li[Li x Ni γ Co (1-x-γ) ]O2(0≦x<0.5, 0<γ<1), Li[Li x Co (1-x) ]O2(0≦x<0.5), Li[Li x Ni γ Mn (1-x-γ) ]O2(0≦x<0.5, 0<γ<1), Li[Li x Ni γ Mn β Co (1-x-γ-β) ]O2(0≦x<0.5, 0<γ, 0<β, 0.5<γ+β<1), Li[Li x Ni γ Co β Al (1-x-γ-β) ]O2 (0≦x<0.5, 0<γ, 0<β, 0.5<γ+β<1), etc. Lithium transition metal composite oxides with spinel crystal structure include Li x Mn2O4, Li x Ni γ Mn (2-γ) O4, etc. Examples of polyanion compounds include LiFePO4, LiMnPO4, LiNiPO4, LiCoPO4, Li3V2(PO4)3, Li2MnSiO4, Li2CoPO4F, etc. Examples of chalcogen compounds include titanium disulfide, molybdenum disulfide, molybdenum dioxide, etc. Atoms or polyanions in these materials may be partially substituted with atoms or anion species of other elements. The surfaces of these materials may be coated with other materials. In the positive electrode active material particles 11, one of these materials may be used alone, or two or more of them may be mixed and used.

[0040] The average particle size of the positive electrode active material particles 11 is preferably, for example, 0.1 μm or more and 20 μm or less. By setting the average particle size of the positive electrode active material particles 11 to the above lower limit or more, the positive electrode active material particles 11 can be easily manufactured or handled. By setting the average particle size of the positive electrode active material particles 11 to the above upper limit or less, the electronic conductivity of the positive electrode mixture layer 5 is improved. The "average particle size" refers to a value at which the volume-based cumulative distribution calculated in accordance with JIS-Z-8819-2 (2001) is 50% based on the particle size distribution measured by a laser diffraction / scattering method for a diluted solution obtained by diluting particles with a solvent in accordance with JIS-Z-8825 (2013).

[0041] In order to obtain powder with a predetermined particle size, a pulverizer, a classifier, etc. are used. Examples of the pulverization method include a method using a mortar, a ball mill, a sand mill, a vibration ball mill, a planetary ball mill, a jet mill, a counter jet mill, a swirling airflow type jet mill, or a sieve. During pulverization, wet pulverization in the presence of water or an organic solvent such as hexane can also be used. As a classification method, a sieve, an air classifier, etc. are used as necessary for both the dry and wet methods.

[0042] The positive electrode active material particles 11 preferably have a coating layer. By having the coating layer, the positive electrode active material particles 11 can suppress a side reaction with the sulfide solid electrolyte. The side reaction is a reaction in which a high resistance layer is formed on the surface of the positive electrode active material particles 11 due to a reaction between the positive electrode active material particles 11 and the sulfide solid electrolyte. The formation of the high resistance layer reduces the charge and discharge performance of the all-solid-state battery. The coating material that is the material for the coating layer is not particularly limited, and examples thereof include LiNbO3, LiTaO3, Li2ZrO3, Li 4 / 3 Ti 5 / 3 O4, Li2TiO3.

[0043] (Second sulfide solid electrolyte) The second sulfide-based solid electrolyte 13 is preferably a sulfide-based crystalline solid electrolyte. When the second sulfide-based solid electrolyte 13 is a sulfide-based crystalline solid electrolyte, the effect of suppressing the decrease in the capacity retention rate after charge-discharge cycles of the all-solid-state battery can be improved.

[0044] The sulfide-based crystalline solid electrolyte used in the second sulfide-based solid electrolyte 13 may be the same as the sulfide-based crystalline solid electrolyte used in the first sulfide-based solid electrolyte. The sulfide-based crystalline solid electrolyte used in the second sulfide-based solid electrolyte 13 may be the same as or different from the sulfide-based crystalline solid electrolyte used in the first sulfide-based solid electrolyte.

[0045] The average particle size of the positive electrode active material composite 14 is, for example, preferably 0.1 μm to 20 μm, more preferably 3 μm to 10 μm. By setting the average particle size of the positive electrode active material composite 14 to the above lower limit or more, the positive electrode active material composite 14 becomes easy to manufacture or handle. By setting the average particle size of the positive electrode active material composite 14 to the above upper limit or less, the contact area between the positive electrode active material composite 14 and the matrix 12 increases, and the charge / discharge characteristics of the all-solid-state battery are improved.

[0046] The content of the positive electrode active material composite 14 in the positive electrode mixture layer 5 is preferably 70 mass % or more and 90 mass % or less, and more preferably 70 mass % or more and 80 mass % or less. By setting the content of the positive electrode active material composite 14 within the above range, the electric capacity of the all-solid-state battery can be increased.

[0047] (Conductive agent) The conductive agent is not particularly limited as long as it is a material having electrical conductivity. Examples of such conductive agents include carbonaceous materials, metals, conductive ceramics, and the like. Examples of carbonaceous materials include graphite, non-graphitic carbon, graphene-based carbon, and the like. Examples of non-graphitic carbon include carbon nanofibers, pitch-based carbon fibers, carbon black, and the like. Examples of carbon black include furnace black, acetylene black, ketjen black, and the like. Examples of graphene-based carbon include graphene, carbon nanotubes (CNT), fullerene, and the like. Examples of the conductive agent include powder and fiber. As the conductive agent, one of these materials may be used alone, or two or more of them may be mixed and used. These materials may also be used in combination. For example, a material in which carbon black and CNT are combined may be used. Among these, carbon black is preferable from the viewpoint of electronic conductivity and coatability, and acetylene black is preferable among them.

[0048] The content of the conductive agent in the positive electrode 1 is preferably 1% by mass or more and 10% by mass or less, and more preferably 3% by mass or more and 9% by mass or less. By setting the content of the conductive agent in the above range, the electric capacity of the all-solid-state battery 10 can be increased.

[0049] (Binder) Examples of binders include thermoplastic resins such as fluororesins (polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), etc.), polyethylene, polypropylene, polyacrylic, polyimide, etc.; elastomers such as ethylene-propylene-diene rubber (EPDM), sulfonated EPDM, styrene butadiene rubber (SBR), fluororubber, etc.; polysaccharide polymers, etc.

[0050] The content of the binder in the positive electrode 1 is preferably from 1% by mass to 10% by mass, and more preferably from 3% by mass to 9% by mass. By setting the content of the binder in the above range, the active material can be stably held.

[0051] (Thickener) Examples of the thickener include polysaccharide polymers such as carboxymethyl cellulose (CMC), methyl cellulose, etc. When the thickener has a functional group that reacts with lithium or the like, this functional group may be deactivated in advance by methylation or the like.

[0052] (Filler) The filler is not particularly limited. Examples of the filler include polyolefins such as polypropylene and polyethylene, inorganic oxides such as silicon dioxide, alumina, titanium dioxide, calcium oxide, strontium oxide, barium oxide, magnesium oxide, and aluminosilicates, hydroxides such as magnesium hydroxide, calcium hydroxide, and aluminum hydroxide, carbonates such as calcium carbonate, poorly soluble ion crystals such as calcium fluoride, barium fluoride, and barium sulfate, nitrides such as aluminum nitride and silicon nitride, and mineral resource-derived substances such as talc, montmorillonite, boehmite, zeolite, apatite, kaolin, mullite, spinel, olivine, sericite, bentonite, and mica, or artificial products thereof.

[0053] The positive electrode mixture layer 5 may contain typical nonmetallic elements such as B, N, P, F, Cl, Br, and I, typical metallic elements such as Li, Na, Mg, Al, K, Ca, Zn, Ga, Ge, Sn, Sr, and Ba, and transition metallic elements such as Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Mo, Zr, Nb, and W as components other than the positive electrode active material, conductive agent, binder, thickener, and filler.

[0054] The average thickness of the positive electrode mixture layer 5 is preferably 30 μm or more and 1,000 μm or less, more preferably 60 μm or more and 500 μm or less. By setting the average thickness of the positive electrode mixture layer 5 to the above lower limit or more, an all-solid-state battery having a high energy density can be obtained. By setting the average thickness of the positive electrode mixture layer to the above upper limit or less, it is possible to miniaturize the all-solid-state battery. The average thickness of the positive electrode mixture layer 5 is the average value of thicknesses measured at any five points. The same applies to the average thicknesses of the negative electrode mixture layer and the separator layer described later.

[0055] <All-solid-state battery> An all-solid-state battery according to one embodiment of the present invention will be described. The all-solid-state battery 10 shown in FIG. 2 is a secondary battery in which a positive electrode 1 and a negative electrode 2 are arranged with an isolation layer 3 interposed therebetween. In the all-solid-state battery of this embodiment, the positive electrode 1 has a positive electrode substrate 4 and a positive electrode mixture layer 5, and the positive electrode substrate 4 is the outermost layer of the positive electrode 1. The negative electrode 2 has a negative electrode substrate 7 and a negative electrode mixture layer 6, and the negative electrode substrate 7 is the outermost layer of the negative electrode 2. In the all-solid-state battery 10 shown in FIG. 1, the negative electrode mixture layer 6, the isolation layer 3, the positive electrode 1, and the positive electrode substrate 4 are laminated in this order on the negative electrode substrate 7.

[0056] The all-solid-state battery 10 may use a known general solid electrolyte in addition to the first sulfide-based solid electrolyte and the second sulfide-based solid electrolyte. Examples of such solid electrolytes include sulfide solid electrolytes, oxide-based solid electrolytes, dry polymer electrolytes, gel polymer electrolytes, and pseudo-solid electrolytes, and sulfide solid electrolytes are preferred. In addition, a single layer in the all-solid-state battery 10 may contain multiple different types of solid electrolytes, or each layer may contain a different solid electrolyte.

[0057] Examples of sulfide solid electrolytes include Li2S-P2S5, Li2S-P2S5-LiI, Li2S-P2S5-LiCl, Li2S-P2S5-LiBr, Li2S-P2S5-Li2O, Li2S-P2S5-Li2O-LiI, Li2S-P2S5-Li3N, Li2S-SiS2, Li2S-SiS2-LiI, Li2S-SiS2-LiBr, Li2S-SiS2-LiCl, Li2S-SiS2-B2S3-LiI, Li2S-SiS2-P2S5-LiI, Li2S-B2S3, and Li2S-P2S5-Z. m S 2n (where m and n are positive numbers, and Z is Ge, Zn, or Ga.), Li2S-GeS2, Li2S-SiS2-Li3PO4, Li2S-SiS2-Li x MO y (where x and y are positive numbers, and M is P, Si, Ge, B, Al, Ga, or In.) Li 10 GeP2S 12 etc. can be mentioned.

[0058] [Positive electrode] The positive electrode 1 of the all-solid-state battery is the positive electrode for an all-solid-state battery according to one embodiment of the present invention. Since the all-solid-state battery includes the positive electrode for an all-solid-state battery, the decrease in the capacity retention rate after charge-discharge cycles can be suppressed.

[0059] [Negative electrode] The negative electrode 2 has a negative electrode substrate 7 and a negative electrode mixture layer 6 disposed directly or via an intermediate layer on the negative electrode substrate 7. The configuration of the intermediate layer is not particularly limited and can be selected from the configurations exemplified for the positive electrode for an all-solid-state battery, for example.

[0060] (Negative electrode substrate) The negative electrode substrate 7 is conductive. Metals such as copper, nickel, stainless steel, nickel-plated steel, and aluminum, or alloys thereof, carbonaceous materials, and the like are used as the material of the negative electrode substrate 7. Among these, copper or copper alloys are preferred. Examples of the negative electrode substrate include foils, vapor deposition films, meshes, and porous materials, and foils are preferred from the viewpoint of cost. Therefore, copper foil or copper alloy foil is preferred as the negative electrode substrate. Examples of copper foil include rolled copper foil and electrolytic copper foil.

[0061] The average thickness of the negative electrode substrate is preferably 2 μm to 35 μm, more preferably 3 μm to 30 μm, further preferably 4 μm to 25 μm, and particularly preferably 5 μm to 20 μm. By setting the average thickness of the negative electrode substrate within the above range, it is possible to increase the strength of the negative electrode substrate and to increase the energy density per volume of the all-solid-state battery.

[0062] The negative electrode mixture layer contains a negative electrode active material. The negative electrode mixture layer contains optional components such as a conductive agent, a binder, a thickener, and a filler, as necessary. The optional components such as a conductive agent, a binder, a thickener, and a filler can be selected from the materials exemplified for the positive electrode for the all-solid-state battery.

[0063] The negative electrode mixture layer may contain typical nonmetallic elements such as B, N, P, F, Cl, Br, and I, typical metallic elements such as Li, Na, Mg, Al, K, Ca, Zn, Ga, Ge, Sn, Sr, and Ba, and transition metallic elements such as Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Mo, Zr, Ta, Hf, Nb, and W as components other than the negative electrode active material, conductive agent, binder, thickener, and filler.

[0064] The negative electrode active material can be appropriately selected from known negative electrode active materials. As the negative electrode active material, a material capable of absorbing and releasing lithium ions is usually used. Examples of the negative electrode active material include metal Li; metals or semimetals such as Si and Sn; metal oxides or semimetal oxides such as Si oxide, Ti oxide, and Sn oxide; and Li4Ti5O 12 , LiTiO 2、 Examples of the material include titanium-containing oxides such as TiNb2O7, polyphosphate compounds, silicon carbide, and carbon materials such as graphite and non-graphitic carbon (easily graphitized carbon or non-graphitizable carbon). Among these materials, graphite and non-graphitic carbon are preferred. In the negative electrode mixture layer, one of these materials may be used alone, or two or more of them may be used in combination.

[0065] "Graphite" refers to a material that has an average lattice spacing (d 002 ) is 0.33 nm or more and less than 0.34 nm. Examples of graphite include natural graphite and artificial graphite. Artificial graphite is preferred from the viewpoint of availability of materials with stable physical properties.

[0066] "Non-graphitic carbon" refers to carbon that has an average lattice spacing (d 002 ) is 0.34 nm or more and 0.42 nm or less. Examples of non-graphitizable carbon include non-graphitizable carbon and graphitizable carbon. Examples of non-graphitizable carbon include resin-derived materials, petroleum pitch or petroleum pitch-derived materials, petroleum coke or petroleum coke-derived materials, plant-derived materials, and alcohol-derived materials.

[0067] Here, the "discharged state" refers to a state in which the negative electrode active material carbon material is discharged so that lithium ions that can be absorbed and released during charging and discharging are sufficiently released. For example, in a single-electrode battery using a negative electrode containing a carbon material as a negative electrode active material as a working electrode and metallic Li as a counter electrode, the state is one in which the open circuit voltage is 0.7 V or more.

[0068] "Non-graphitizable carbon" means the above d 002 This refers to carbon materials with a particle size of 0.36 nm or more and 0.42 nm or less.

[0069] "Graphitizable carbon" means the above d 002 This refers to carbon materials with a particle size of 0.34 nm or more and less than 0.36 nm.

[0070] The negative electrode active material is usually a particle (powder). The average particle size of the negative electrode active material can be, for example, 1 nm or more and 100 μm or less. When the negative electrode active material is a carbon material, a titanium-containing oxide, or a polyphosphate compound, the average particle size may be 1 μm or more and 100 μm or less. When the negative electrode active material is Si, Sn, Si oxide, Sn oxide, or the like, the average particle size may be 1 nm or more and 1 μm or less. By setting the average particle size of the negative electrode active material to the above lower limit or more, the negative electrode active material can be easily manufactured or handled. By setting the average particle size of the negative electrode active material to the above upper limit or less, the electronic conductivity of the negative electrode mixture layer is improved. In order to obtain powder with a predetermined particle size, a pulverizer, a classifier, or the like is used. The pulverization method and the powder classification method can be selected from, for example, the methods exemplified for the positive electrode. When the negative electrode active material is a metal such as metallic Li, the negative electrode active material may be in the form of a foil.

[0071] The content of the negative electrode active material in the negative electrode mixture layer 6 is preferably 60% by mass or more and 99% by mass or less, and more preferably 90% by mass or more and 98% by mass or less. By setting the content of the negative electrode active material within the above range, it is possible to achieve both a high energy density and manufacturability of the negative electrode mixture layer 6.

[0072] When the negative electrode mixture layer 6 contains a solid electrolyte, the content of the solid electrolyte is preferably 1% by mass or more and 40% by mass or less, and more preferably 2% by mass or more and 10% by mass or less. By setting the content of the solid electrolyte in the above range, the electric capacity of the all-solid-state battery 10 can be increased.

[0073] When the negative electrode mixture layer 6 contains a solid electrolyte, it may be a mixture or composite of the above-mentioned negative electrode active material and the solid electrolyte.

[0074] The average thickness of the negative electrode mixture layer 6 is preferably 30 μm or more and 1,000 μm or less, and more preferably 60 μm or more and 500 μm or less. By setting the average thickness of the negative electrode mixture layer 6 to be equal to or more than the above lower limit, an all-solid-state battery 10 having a high energy density can be obtained. By setting the average thickness of the negative electrode mixture layer 6 to be equal to or less than the above upper limit, the all-solid-state battery 10 can be made smaller.

[0075] [Isolation layer] The isolating layer 3 contains a solid electrolyte. The solid electrolyte contained in the isolating layer 3 is not particularly limited, and the above-mentioned various general solid electrolytes can be used, among which it is preferable to use a sulfide solid electrolyte. The content of the solid electrolyte in the isolating layer 3 is preferably 70% by mass or more, more preferably 90% by mass or more, even more preferably 99% by mass or more, and even more preferably substantially 100% by mass.

[0076] The isolating layer 3 may contain optional components such as a binder, a thickener, a filler, etc. The optional components such as the binder, the thickener, the filler, etc. can be selected from the materials exemplified for the positive electrode for the all-solid-state battery.

[0077] The average thickness of the isolating layer 3 is preferably 1 μm or more and 50 μm or less, and more preferably 3 μm or more and 20 μm or less. By setting the average thickness of the isolating layer 3 to be equal to or more than the above lower limit, it is possible to insulate the positive electrode 1 and the negative electrode 2 with high reliability. By setting the average thickness of the isolating layer 3 to be equal to or less than the above upper limit, it is possible to increase the energy density of the all-solid-state battery 10.

[0078] [Configuration of the power storage device] The all-solid-state battery of this embodiment can be mounted as a power storage device formed by assembling a plurality of all-solid-state batteries in a power source for an automobile such as an electric vehicle (EV), a hybrid vehicle (HEV), or a plug-in hybrid vehicle (PHEV), a power source for electronic devices such as a personal computer or a communication terminal, or a power storage power source, etc. In this case, the technology of the present invention may be applied to at least one all-solid-state battery included in the power storage device. 3 shows an example of a power storage device 30 in which power storage units 20, each of which is an assembly of two or more electrically connected all-solid-state batteries 1, are further assembled. The power storage device 30 may include a bus bar (not shown) that electrically connects the two or more all-solid-state batteries 1, a bus bar (not shown) that electrically connects the two or more power storage units 20, and the like. The power storage unit 20 or the power storage device 30 may include a status monitoring device (not shown) that monitors the status of the one or more all-solid-state batteries.

[0079] <Method of manufacturing positive electrodes for all-solid-state batteries> A method for producing a positive electrode for an all-solid-state battery according to one embodiment of the present invention includes compounding positive electrode active material particles with a sulfide-based solid electrolyte (compounding step), and preparing a positive electrode mixture including the positive electrode active material composite obtained by the compounding, a sulfide-based glass solid electrolyte, and a sulfide-based crystalline solid electrolyte (positive electrode mixture preparation step). The method for producing a positive electrode for an all-solid-state battery may also include a positive electrode substrate preparation step.

[0080] (1) Composite process In this step, the positive electrode active material particles and the sulfide-based solid electrolyte are composited. As a composite method, for example, the sulfide-based solid electrolyte is composited on the surface of the positive electrode active material particles by dry composite. By composited with the sulfide-based solid electrolyte on the surface of the positive electrode active material particles, at least a part of the surface of the positive electrode active material particles is directly or indirectly covered with the sulfide-based solid electrolyte.

[0081] The dry compounding is carried out, for example, by the following steps. That is, the positive electrode active material particles and the sulfide-based solid electrolyte are put into a dry particle compounding device (such as Nobiltamini manufactured by Hosokawa Micron Corporation) in a predetermined mass ratio. Next, the dry particle compounding device is driven at a peripheral speed of 5000 rpm to 9000 rpm and a driving time of 1 minute to 5 minutes. This allows the sulfide-based solid electrolyte to be compounded on the surface of the positive electrode active material particles. (2) Positive electrode mixture production process In this step, a positive electrode mixture for forming a positive electrode mixture layer is prepared. Specifically, in this step, a positive electrode mixture containing the positive electrode active material composite obtained by the above-mentioned compounding, a sulfide-based glass solid electrolyte, and a sulfide-based crystalline solid electrolyte is prepared. The method for preparing the positive electrode mixture is not particularly limited and can be appropriately selected according to the purpose. For example, a stirring and mixing process using a kneader of a positive electrode active material composite, a sulfide-based glass solid electrolyte, a sulfide-based crystalline solid electrolyte, an arbitrary material such as a conductive agent, a binder, and a solvent, a mixture or composite preparation using a mechanical milling method or the like of the material of the positive electrode mixture, compression molding of the material of the positive electrode mixture, and the like can be mentioned.

[0082] According to the method for producing a positive electrode for an all-solid-state battery, by including the above steps, it is possible to reliably produce a positive electrode for an all-solid-state battery that can suppress a decrease in the capacity retention rate after charge-discharge cycles of the all-solid-state battery.

[0083] <Manufacturing method for all-solid-state batteries> The method for producing an all-solid-state battery according to one embodiment of the present invention can be carried out by a generally known method, except that the method for producing a positive electrode for an all-solid-state battery described above is used as the method for producing a positive electrode. Specifically, the method for producing the all-solid-state battery includes, for example, (1) preparing a positive electrode, (2) preparing an isolation layer, (3) preparing a negative electrode, and (4) stacking the positive electrode, the isolation layer, and the negative electrode. Each step will be described in detail below.

[0084] (1) Positive electrode preparation process In this step, the steps of the method for producing the positive electrode for an all-solid-state battery described above are carried out.

[0085] (2) Preparation of materials for the isolation layer In this process, an isolation layer material for forming an isolation layer is usually prepared. When the all-solid-state battery is a lithium-ion all-solid-state battery, the isolation layer material can be a solid electrolyte. The solid electrolyte as the isolation layer material can be prepared by a conventionally known method. For example, it can be obtained by processing a predetermined material by a mechanical milling method. The isolation layer material may be prepared by heating a predetermined material to a melting temperature or higher by a melt quenching method, melting and mixing the two at a predetermined ratio, and quenching. Other methods for synthesizing the isolation layer material include, for example, a solid phase method in which the material is sealed under reduced pressure and fired, a liquid phase method such as dissolution deposition, a gas phase method (PLD), and firing under an argon atmosphere after mechanical milling.

[0086] (3) Negative electrode preparation process In this step, a negative electrode mixture for forming a negative electrode mixture layer is usually prepared. The specific method for preparing the negative electrode mixture is the same as that for the positive electrode mixture. When the negative electrode mixture contains a mixture or composite containing a negative electrode active material and a solid electrolyte, this step may include, for example, mixing the negative electrode active material and the solid electrolyte using a mechanical milling method or the like to prepare a mixture or composite of the negative electrode active material and the solid electrolyte. In addition, this step may include a negative electrode substrate preparation step.

[0087] (Lamination process) In this step, for example, a positive electrode having a positive electrode substrate and a positive electrode mixture layer, an isolation layer, and a negative electrode having a negative electrode substrate and a negative electrode mixture layer are laminated. In this step, the positive electrode, the isolation layer, and the negative electrode may be formed in this order, or vice versa, and the order of formation of each layer is not particularly important. The positive electrode is formed, for example, by pressure molding the positive electrode substrate and the positive electrode mixture, the isolation layer is formed by pressure molding the isolation layer material, and the negative electrode is formed by pressure molding the negative electrode substrate and the negative electrode mixture. The positive electrode, the isolation layer, and the negative electrode may be laminated by pressure molding the positive electrode substrate, the positive electrode mixture, the isolation layer material, the negative electrode mixture, and the negative electrode substrate at once. The positive electrode and the negative electrode may be molded in advance, respectively, and then pressure molded and laminated with the isolation layer.

[0088] [Other embodiments] The present invention is not limited to the above-mentioned embodiment, and can be embodied in various modified and improved forms in addition to the above-mentioned forms. For example, the all-solid-state battery according to the present invention may have layers other than the positive electrode, the separator layer, and the negative electrode, such as an intermediate layer or an adhesive layer. In addition, the all-solid-state battery according to the present invention may contain a liquid in one or more of the layers.

[0089] In the above embodiment, the positive electrode mixture layer of the positive electrode is disposed directly or via an intermediate layer on the positive electrode substrate, but is not limited thereto. For example, the positive electrode mixture layer may be filled into the voids of a sponge-like positive electrode substrate. EXAMPLES

[0090] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples.

[0091] [Examples 1 to 3, Comparative Examples 1 and 2] The all-solid-state batteries of Examples 1 to 3 and Comparative Examples 1 and 2 were produced as follows.

[0092] (Preparation of Positive Electrode Active Material Particles) NCM523 (LiNi 0.5 Co 0.2 Mn 0.3Particles of LiNbO2 were prepared. Next, LiNbO3 was coated as a coating layer for the positive electrode active material particles in the following procedure. First, metal Li was dissolved in ultra-dehydrated ethanol, and then niobium ethoxide (Nb(OC2H5)5) was dissolved to prepare a LiNbO3 precursor solution. Using a rolling fluidized coating device (FD-MP-01F) manufactured by Powrex Corporation, the LiNbO3 precursor was coated on the particle surface of NCM523. The LiNbO3-coated NCM523 was produced by heat-treating the NCM523 coated with the LiNbO3 precursor at 400°C for 30 minutes. This LiNbO3-coated NCM523 was used as the positive electrode active material particles. The coating amount of LiNbO3 with respect to NCM523 was 0.75 mass%.

[0093] (Composite processing process) A composite process was carried out using the above-mentioned positive electrode active material particles and Li6PS5Cl (cubic argyrodite crystal structure) as the second sulfide-based solid electrolyte to produce a positive electrode active material composite. The mass ratio in the positive electrode active material composite was positive electrode active material particles:second sulfide-based solid electrolyte=95% by mass:5% by mass. The composite was then carried out by the following process. That is, the positive electrode active material particles and the second sulfide-based solid electrolyte were put into a Nobiltamini manufactured by Hosokawa Micron Corporation and driven. As a result, a coating of the second sulfide-based solid electrolyte was formed on the surface of the positive electrode active material particles.

[0094] (Production of all-solid-state batteries) The above positive electrode active material composite, 75Li2S·25P2S5 and Li6PS5Cl listed in Table 1 as the first sulfide-based solid electrolyte, acetylene black as the conductive agent, and SBR as the binder were weighed out to a mass ratio of 80:16:2:2. First, the above positive electrode active material composite, the first sulfide-based solid electrolyte, and the conductive agent were mixed in an agate mortar. Next, butyl acetate as the binder and solvent was added to this mixture, and the mixture was kneaded in a hybrid mixer to obtain a positive electrode mixture slurry. The obtained positive electrode mixture slurry was applied to an aluminum foil (average thickness 20 μm) as the positive electrode substrate using a YBA type Baker applicator so that the coating amount after drying was 15 mg / cm. 2More than 25mg / cm 2 The coating was performed as follows: Next, the positive electrode mixture layer was formed on the positive electrode substrate by drying for 10 minutes under normal pressure in a dryer in an argon atmosphere at 100°C and then drying for 10 minutes under reduced pressure, and the positive electrode mixture layer was punched out into a circle with a diameter of 10 mm to prepare a positive electrode for evaluation. Next, 60 mg of Li6PS5Cl, a sulfide-based solid electrolyte, was put into a powder molding machine with an inner diameter of 10 mm as an isolation layer material, and then pressure molding was performed using a hydraulic press to prepare an isolation layer. After releasing the pressure, a positive electrode was placed on one side of the isolation layer so that the positive electrode mixture layer faced the other side, and pressure molding was performed at 360 MPa for 5 minutes. After releasing the pressure, a negative electrode, in which a metal Li foil and a metal In foil, which are negative electrode mixture layers, were previously attached to a stainless steel plate, which is a negative electrode substrate, was placed on the other side of the isolation layer so that the negative electrode mixture layer faced the other side, and pressure molding was performed at 120 MPa for 3 minutes. As a result, a laminate having a diameter of 10 mm was obtained, which had a positive electrode substrate, a positive electrode mixture layer, an isolation layer, a negative electrode mixture layer, and a negative electrode substrate. A rectangular PTFE plate with a diameter of about 30 mm square and a through hole with a diameter of about 10 mm was prepared in the center, and the obtained laminate was placed in the through hole, and the PTFE plate was sandwiched between two sheets of stainless steel foil so as to cover the center of the PTFE plate. This was housed in an exterior body made of an aluminum metal resin composite film, and the opening was reduced in pressure by heat welding. At this time, each end of the lead terminal made of nickel foil previously attached to each stainless steel foil was led out from the sealing part of the exterior body. Both sides of this exterior body were sandwiched between two PTFE sheets of about 40 mm square, and further sandwiched between two stainless steel plates of about 60 mm square, and the stainless steel plates were screwed together under the condition that a pressure of 25 MPa was applied to the laminate. In this way, the all-solid-state batteries of Example 1 to Example 3, Comparative Example 1 and Comparative Example 2 were obtained.

[0095] [Comparative Example 3 and Comparative Example 4] All-solid-state batteries of Comparative Example 3 and Comparative Example 4 were obtained in the same manner as in Example 1, except that the composite treatment step was not performed, the above-mentioned NCM523 particles were used as the positive electrode active material particles, and the first sulfide-based solid electrolyte was as shown in Table 1.

[0096] [evaluation] (1) Discharge capacity confirmation test A discharge capacity confirmation test was performed on each of the obtained all-solid-state batteries under the following conditions. In a thermostatic chamber at 50°C, the battery was charged at a constant current of 0.05C up to 3.75V, and then charged at a constant voltage of 3.75V. The charge termination condition was that the charge current during constant voltage charging was 0.025C. After a 10-minute pause after charging, the battery was discharged at a constant current of 0.20C up to 2.25V. A 10-minute pause was provided after discharging. This charge and discharge cycle was performed. Next, one cycle of charge and discharge was performed under the same conditions except that the discharge current was 0.10C. Furthermore, one cycle of charge and discharge was performed under the same conditions except that the discharge current was 0.05C. Then, the discharge capacity [mAh] under each condition was measured. The discharge capacity [mAh] under each condition at this time was divided by the mass of the positive electrode active material contained in the positive electrode, and the discharge capacity [mAh / g] under each condition is shown in Table 1. (2) Charge / discharge cycle test Next, a charge / discharge cycle test was performed under the following conditions. At 50°C, charging was performed at a constant current and constant voltage of 0.20C and 3.75V, and the charge termination condition was that the charging current was 0.05C. Discharging was performed at a constant current of 0.20C and a termination voltage of 2.25V. This charge / discharge cycle was performed for 30 cycles. A 10-minute rest period was provided after each charging and discharging. Next, one cycle of charging and discharging was performed under the same conditions as in the above discharge capacity confirmation test, with a discharge current of 0.20 C. The discharge capacity [mAh] at this time was divided by the mass of the positive electrode active material contained in the positive electrode and recorded as the discharge capacity [mAh / g] after the charge-discharge cycle test. The percentage of the discharge capacity after the charge-discharge cycle test relative to the discharge capacity at a discharge current of 0.2 C in the above discharge capacity confirmation test discharge is shown in Table 1 as the capacity retention rate [%].

[0097] [Table 1]

[0098] As shown in Table 1, the all-solid-state batteries of Examples 1 to 3 suppressed the decrease in capacity retention rate after charge-discharge cycles at high temperature (50° C.). In contrast, the all-solid-state batteries of Comparative Examples 1 and 2 in which the first sulfide-based solid electrolyte was either a sulfide-based glass solid electrolyte or a sulfide-based crystalline solid electrolyte, and the all-solid-state batteries of Comparative Examples 3 and 4 in which no positive electrode active material composite was used, showed a large decrease in capacity retention rate after charge-discharge cycles compared to Examples 1 to 3.

[0099] The above results show that the positive electrode for an all-solid-state battery can suppress a decrease in the capacity retention rate after charge-discharge cycles of the all-solid-state battery. The positive electrode can be suitably used as a positive electrode for an all-solid-state battery. [Explanation of symbols]

[0100] 1 positive electrode 2 negative electrode 3 isolation layer 4. Positive electrode substrate 5 Positive electrode mixture layer 6 Negative electrode mixture layer 7. Negative electrode substrate 10 All-solid-state battery 11 Positive electrode active material particles 12. Matrix mainly composed of sulfide-based solid electrolyte 13 Secondary sulfide solid electrolyte 14 Cathode active material composite 20 Energy Storage Unit 30 Energy storage device

Claims

1. A positive electrode substrate; Positive electrode mixture layer Equipped with the positive electrode mixture layer has a matrix mainly composed of a first sulfide-based solid electrolyte and a positive electrode active material composite dispersed in the matrix, the positive electrode active material composite contains positive electrode active material particles and a second sulfide-based solid electrolyte that directly or indirectly covers at least a portion of a surface of the positive electrode active material particles, The positive electrode for an all-solid-state battery, wherein the first sulfide-based solid electrolyte includes a sulfide-based glass solid electrolyte and a sulfide-based crystalline solid electrolyte.

2. 2. The positive electrode for an all-solid-state battery according to claim 1, wherein the second sulfide-based solid electrolyte is a sulfide-based crystalline solid electrolyte.

3. The sulfide-based glass solid electrolyte is yLi 2 S (1-y) P 2 S 5 (where 0.75≦y≦0.77), 3. The positive electrode for an all-solid-state battery according to claim 1, wherein the sulfide-based crystalline solid electrolyte has a crystal structure that is a cubic system, an orthorhombic system, a triclinic system, or a combination thereof.

4. An all-solid-state battery comprising the positive electrode according to claim 1 , 2 or 3 .

5. Composite positive electrode active material particles and a sulfide-based solid electrolyte; A positive electrode mixture is prepared, the positive electrode mixture including the positive electrode active material composite obtained by the above-mentioned compounding, a sulfide-based glass solid electrolyte, and a sulfide-based crystalline solid electrolyte. A method for producing a positive electrode for an all-solid-state battery comprising the steps of:

Citation Information

Patent Citations

  • Lithium secondary battery

    JP2000340257A

  • Electrode material, and solid secondary battery using it

    JP2008103282A

  • All-solid lithium secondary battery

    JP2011187253A

  • Positive electrode for all-solid lithium ion battery

    JP2015005398A

  • Electrode mixture

    JP2016207418A