Positive plate, preparation method thereof and semi-solid-state battery

By covering the surface of the positive electrode material of the semi-solid lithium-ion battery with solid oxide electrolyte and adding lithium manganese iron phosphate, combining a double-coated separator and lightweight composite foil, the problem of taking into account both the electrochemical performance and safety performance of semi-solid battery is solved. , achieving compatibility effects of high energy density and high safety performance.

CN118899392APending Publication Date: 2024-11-05中汽新能(天津)电池科技有限公司
View PDF 0 Cites 6 Cited by

Patent Information

Application Number
CN202410986424.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

Existing semi-solid lithium-ion batteries are difficult to balance the improvement of electrochemical performance and safety performance, especially the excessive addition of oxide solid electrolytes will lead to a decrease in energy density.

Method used

The surface of the positive electrode material is coated with oxide solid electrolyte, and lithium manganese iron phosphate is added as a safety additive, and a double-coated diaphragm and lightweight high-safe composite foil is used to form a lean and high-safe liquid electrolyte to form a high energy A cathode sheet with density and high safety performance.

Benefits of technology

It achieves compatibility of high energy density and high safety performance of semi-solid state batteries, improves the safety performance of batteries through multiple safety technologies, and reduces the battery weight through lightweight materials and thinner diaphragms and improves energy density.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118899392A_ABST
    Figure CN118899392A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of batteries, and particularly relates to a positive plate, a preparation method thereof and a semi-solid battery. The positive plate comprises a positive current collector and a positive active material layer coated on the surface of the positive current collector; the positive active material layer comprises a positive active material, a positive conductive agent and a positive binder; the positive electrode active substance comprises a positive electrode material and an oxide solid electrolyte coated on the surface of the positive electrode material. According to the technical scheme, the solid electrolyte is modified on the surface of the high-nickel ternary positive electrode material, and the lithium manganese iron phosphate safety additive is added into the high-nickel ternary positive electrode, so that the positive electrode plate with high energy density and high safety performance is obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of batteries, and in particular relates to a positive electrode sheet and a preparation method thereof, and a semi-solid battery. Background Art

[0002] All-solid-state batteries with high energy density and high safety performance are the research and development hotspots of the next generation of lithium-ion batteries. However, problems such as interface compatibility, production line compatibility and material costs have hindered their application in electric vehicles and energy storage for several years. In contrast, the electrode material system of semi-solid batteries has changed little, and diaphragms and traditional electrolytes are still used. The mass or volume of solid electrolytes in semi-solid batteries accounts for half of the total mass or volume of electrolytes in monomers. The solid electrolytes in semi-solid batteries are non-flammable, and the amount of liquid electrolytes is greatly reduced. The presence of a small amount of electrolyte can reduce the risk of thermal runaway while ensuring the excellent electrochemical performance of the battery. Therefore, when damage or puncture occurs, spontaneous combustion or explosion will be effectively avoided. In addition, the supply chain, manufacturing process and equipment of semi-solid batteries have extremely high overlap and compatibility with traditional liquid batteries, and have high safety, long life and good economy. The semi-solid battery system has little replacement for the existing liquid lithium-ion battery system and will become an improved solution for the transition from traditional liquid batteries to all-solid-state batteries.

[0003] At present, traditional semi-solid-state batteries use oxide solid electrolytes to coat the positive electrode particles and the diaphragm coating. The oxide solid electrolyte is resistant to high temperature, non-flammable, non-corrosive, and non-volatile. Although the safety performance is improved compared to liquid lithium-ion batteries, excessive addition of oxide solid electrolytes will cause the energy density of lithium-ion batteries to decrease. Therefore, how to maximize the compatibility of electrochemical performance and safety performance of semi-solid-state batteries is a difficulty faced by the development of semi-solid-state battery systems. Summary of the invention

[0004] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a positive electrode sheet and a preparation method thereof and a semi-solid battery.

[0005] To achieve the above object, the technical solution adopted by the present invention is:

[0006] A positive electrode sheet comprises a positive electrode current collector and a positive electrode active material layer coated on the surface of the positive electrode current collector; the positive electrode active material layer comprises a positive electrode active material, a positive electrode conductive agent, and a positive electrode binder.

[0007] Preferably, it also includes a safety agent, lithium manganese iron phosphate; preferably, the amount of lithium manganese iron phosphate added to the positive electrode active material layer is 5-20%, preferably 10%;

[0008] The positive electrode active material comprises a positive electrode material and an oxide solid electrolyte coated on the surface of the positive electrode material;

[0009] Preferably, the positive electrode material is one of lithium cobalt oxide, lithium manganese oxide, lithium nickel cobalt manganese oxide, and lithium nickel cobalt aluminum oxide, or a mixture of at least two thereof;

[0010] The oxide solid electrolyte is one of lithium aluminum titanium phosphate (LATP), lithium aluminum germanium phosphate (LAGP), lithium lanthanum zirconium oxide (LLZO), lithium lanthanum titanium oxide (LLTO), and lithium lanthanum zirconium tantalum oxide (LLZTO), or a mixture of at least two thereof;

[0011] The positive electrode conductive agent is one of conductive carbon black, conductive graphite, carbon nanotubes, carbon nanofibers, and graphene, or a mixture of at least two of them;

[0012] The positive electrode binder is one of polyvinylidene fluoride (PVDF), styrene-butadiene rubber (SBR), carboxymethyl cellulose (CMC), and polytetrafluoroethylene (PTFE), or a mixture of at least two of them.

[0013] The coating amount of the oxide solid electrolyte is 0.5-3%, preferably 2%.

[0014] The mass ratio of the positive electrode active material, lithium manganese iron phosphate, positive electrode conductor, and positive electrode binder is: (74-96): (1-15): (1-5): (2-6); preferably 85:10:2:3.

[0015] The positive electrode current collector comprises a polymer insulating layer and aluminum foil layers arranged on both sides of the polymer insulating layer;

[0016] Preferably, the thickness of the polymer insulating layer is 2-10 μm, preferably 4 μm; the thickness of the aluminum foil layer is 1-5 μm, preferably 1.5 μm;

[0017] Preferably, the polymer insulation layer is made of polyethylene, polypropylene, polyvinyl chloride, polyimide, polyacrylonitrile or polyethylene terephthalate, or a mixture of at least two of them.

[0018] The present invention also includes a method for preparing the positive electrode sheet, comprising the following steps: mixing a positive electrode active material, lithium manganese iron phosphate, a positive electrode conductive agent, and a positive electrode binder to prepare a positive electrode slurry, coating the positive electrode slurry on both sides of the positive electrode current collector, drying, rolling, and cutting to obtain a positive electrode sheet; preferably, the coating surface density of the positive electrode active material layer is 10-50 mg / cm 2 .

[0019] The present invention also includes a semi-solid battery, comprising the positive electrode sheet, the negative electrode sheet, the separator and the electrolyte.

[0020] The negative electrode sheet comprises a negative electrode current collector and a negative electrode active material layer coated on both sides of the negative electrode current collector;

[0021] The negative electrode active material layer comprises a negative electrode active material, an oxide solid electrolyte, a negative electrode conductive agent, and a negative electrode binder;

[0022] Preferably, the mass ratio of the negative electrode active material, the oxide solid electrolyte, the negative electrode conductive agent, and the negative electrode binder is: (83-97): (1-5): (1-5): (1-7); preferably 93: 2: 2: 3;

[0023] Preferably, the negative electrode active material is one of silicon, silicon dioxide, silicon oxide, artificial graphite, natural graphite, composite graphite, soft carbon, and hard carbon, or a mixture of at least two thereof;

[0024] Preferably, the negative electrode binder is one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), polytetrafluoroethylene (PTFE), or a mixture of at least two thereof;

[0025] Preferably, the negative electrode current collector comprises a polymer insulating layer and copper foil layers arranged on both sides of the polymer insulating layer;

[0026] Preferably, the thickness of the polymer insulation layer is 2-10 μm, preferably 4.5 μm; the thickness of the copper foil layer is 1-5 μm, preferably 1 μm;

[0027] Preferably, the polymer insulating layer is made of one of polyethylene, polypropylene, polyvinyl chloride, polyimide, polyacrylonitrile or polyethylene terephthalate, or a mixture of at least two of them;

[0028] Preferably, the negative electrode sheet is prepared by the following method: negative electrode active material, oxide solid electrolyte, negative electrode conductive agent, and negative electrode binder are mixed to form negative electrode slurry, the negative electrode slurry is coated on both sides of the negative electrode current collector, and after drying, rolling and cutting, a positive electrode sheet is obtained; preferably, the coating surface density of the negative electrode active material layer is 5-30 mg / cm 2 .

[0029] The diaphragm includes a base film and a solid electrolyte coating disposed on both sides of the base film close to the negative electrode sheet and a nanofiber coating close to the positive electrode sheet;

[0030] Preferably, the base film is one of a polyethylene base film, a polyethylene non-woven base film, a polypropylene base film, a polypropylene non-woven base film, a polypropylene / polyethylene / polypropylene composite base film, a polyimide base film, a polyimide non-woven base film, a polytetrafluoroethylene base film, a polytetrafluoroethylene non-woven base film, a polyvinyl chloride base film, and a polyvinyl chloride non-woven base film;

[0031] Preferably, the nanofiber coating comprises ceramic powder and nanofibers;

[0032] The ceramic powder includes one or a mixture of at least two of aluminum oxide, zirconium oxide, boehmite, magnesium hydroxide, barium sulfate, silicon oxide, aluminum nitride, magnesium oxide, titanium dioxide, yttrium oxide and cerium oxide, and has a particle size of 5-200 nm;

[0033] The nanofibers include a mixture of at least two of carbon nanotubes, boron carbide nanowires, nanocellulose, and nanoaramid fibers, and the nanofibers have a diameter of 10-50 nm and a length of 100-1000 μm.

[0034] The mass ratio of nanofiber to ceramic powder is (0.1-1):1; preferably 1:9, and the thickness of the nanofiber coating is 0.1-5 μm; preferably 2 μm;

[0035] The solid electrolyte coating includes a solid electrolyte; the solid electrolyte includes one or a mixture of at least two of lithium aluminum titanium phosphate (LATP), lithium aluminum germanium phosphate (LAGP), lithium lanthanum zirconium oxide (LLZO), lithium lanthanum titanium oxide (LLTO), and lithium lanthanum zirconium tantalum oxide (LLZTO), with a particle size of 100-500nm. The thickness of the solid electrolyte coating is 0.1-3μm; preferably 2μm.

[0036] The electrolyte includes lithium salt, solvent, and additives;

[0037] The lithium salt is one of lithium hexafluorophosphate (Li PF6), lithium bis(fluorosulfonyl)imide (Li FSI), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium tetrafluoroborate (LiBF4), lithium bis(oxalatoborate) (LiBOB), lithium difluorophosphate (LiPO2F2), lithium difluorooxalatoborate (LiDFOB), etc., or a mixture of at least two thereof;

[0038] The molar concentration of the lithium salt is 0.5-2 mol / L;

[0039] The solvent includes propylene carbonate (PC), ethylene carbonate (EC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), phthalate (DMP), dimethyl maleate (DMM), ethylene glycol dimethyl ether (DME), tetrahydrofuran (TH) F, etc., or a mixture of at least two thereof;

[0040] The additive is one or a mixture of at least two of vinylene carbonate (VC), vinyl ethylene carbonate (VEC), fluoroethylene carbonate (FEC), propane sultone (PS), propene sultone (PST), diethylene sulfate (DTD), difluoroethylene carbonate (DFEC), ethoxy pentafluorocyclophosphazene (PFPN), etc.;

[0041] Preferably, the electrolyte comprises LiPF6 / EC+PC+DMC+VC+FEC+DTD, and the proportion of each component is 15%:20%:20%:30%:2.1%:10%:2.9%, wt%;

[0042] Preferably, the electrolyte comprises LiPF6 / EC+PC+DMC+VC+FEC+DTD+PFPN, and the proportion of each component is 15%:20%:18.5%:27%:2%:10%:2.5%:5%, wt%;

[0043] The electrolyte injection amount of each battery is 0.5-1.0g / Ah.

[0044] Compared with the prior art, the present invention has the following beneficial effects:

[0045] The technical solution of the present application obtains a positive electrode sheet with both high energy density and high safety performance by modifying the solid electrolyte on the surface of a high-nickel ternary positive electrode material and adding a lithium iron manganese phosphate safety additive to the high-nickel ternary positive electrode; as a preferred form thereof, with the use of a double-coated diaphragm, a lightweight high-safety composite foil, and a lean high-safety liquid electrolyte, the battery has better safety performance under the joint action of multiple safety technologies. At the same time, the use of lightweight foils, thin diaphragms, and lean high-safety liquid electrolytes can reduce the weight of the battery, increase the energy density of the battery, and achieve the advantages of the compatibility of high energy density and high safety performance of semi-solid batteries. BRIEF DESCRIPTION OF THE DRAWINGS

[0046] Figure 1 Schematic diagram of the structure of a semi-solid-state battery according to an embodiment of the present invention. DETAILED DESCRIPTION

[0047] In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention is further described in detail below in conjunction with embodiments.

[0048] Figure 1 A semi-solid battery is shown, comprising a positive electrode sheet 1, a negative electrode sheet 2, a separator 3 and an electrolyte;

[0049] The positive electrode sheet includes a positive electrode current collector 101 and a positive electrode active material layer 102 coated on the surface of the positive electrode current collector;

[0050] The negative electrode sheet includes a negative electrode current collector 201 and a negative electrode active material layer 202 coated on the surface of the negative electrode current collector;

[0051] The separator includes a base film 301 and a solid electrolyte coating 303 disposed on both sides of the base film 301 close to the negative electrode sheet and a nanofiber coating 302 close to the positive electrode sheet;

[0052] Example 1

[0053] A method for preparing a semi-solid battery comprises the following steps:

[0054] 1) Preparation of positive electrode sheet: 95% positive electrode active material (ternary nickel cobalt manganese oxide NCM coated on the surface of LATP, Ni% = 90%, coating amount 2%), 2% positive electrode conductive agent Super P and 3% positive electrode binder PVDF were mixed to prepare positive electrode slurry, and the positive electrode slurry was coated on both sides of the positive electrode current collector, and the positive electrode coating surface density was 45 mg / cm 2 After drying, rolling and cutting are performed to obtain the positive electrode sheet; the positive electrode current collector is aluminum foil with a thickness of 6 μm.

[0055] 2) Preparation of negative electrode sheet: 93% negative electrode active material (a mixture of graphite and silicon oxide, the ratio of the two is 80%:20%), 2% solid electrolyte (LLZTO), 2% conductive agent Super P and 3% binder PAA are mixed to make negative electrode slurry, and the negative electrode slurry is coated on both sides of the negative electrode current collector. The surface density of the negative electrode coating is 20mg / cm 2 After drying, rolling and cutting, negative electrode sheets are obtained. The negative electrode current collector is copper foil with a thickness of 4.5 μm;

[0056] 3) stacking the negative electrode sheet, the separator and the positive electrode sheet in sequence through a lamination process to prepare a soft-pack semi-solid battery, wherein the separator includes a base film and a ceramic coating arranged on both sides of the base film, the thickness of the separator is 13 μm, the base film is a PE base film with a thickness of 9 μm, and the thickness of the ceramic coating on both sides is 2 μm;

[0057] Through the aluminum-plastic film package, 1 mol / L of electrolyte is injected at an injection coefficient of 1.5g / Ah;

[0058] (LiPF6 / EC+PC+DMC+VC+FEC+DTD, 15%: 20%: 20%: 30%: 2.1%: 10%: 2.9%, wt%), high temperature static, fixture pre-charge, degas, formation, aging, capacity division and other processes to complete the battery preparation and basic electrical performance testing. Pre-charge, formation and capacity division are carried out under 1000kgf pressure, 25℃ ambient temperature and 0.2C rate.

[0059] Comparative Example 1

[0060] A method for preparing a semi-solid battery comprises the following steps:

[0061] 1) Preparation of positive electrode sheet: 95% positive electrode active material (ternary nickel cobalt manganese oxide NCM, Ni% = 90%), 2% positive electrode conductive agent Super P and 3% positive electrode binder PVDF were mixed to prepare positive electrode slurry, and the positive electrode slurry was coated on both sides of the positive electrode current collector. The surface density of the positive electrode coating was 45 mg / cm 2 After drying, rolling and cutting are performed to obtain the positive electrode sheet; the positive electrode current collector is aluminum foil with a thickness of 6 μm.

[0062] 2) Preparation of negative electrode sheet: 93% negative electrode active material (a mixture of graphite and silicon oxide, the ratio of the two is 80%:20%), 2% solid electrolyte (LLZTO), 2% conductive agent Super P and 3% binder PAA are mixed to make negative electrode slurry, and the negative electrode slurry is coated on both sides of the negative electrode current collector. The surface density of the negative electrode coating is 20mg / cm 2 After drying, rolling and cutting, negative electrode sheets are obtained. The negative electrode current collector is copper foil with a thickness of 4.5 μm;

[0063] 3) stacking the negative electrode sheet, the separator and the positive electrode sheet in sequence through a lamination process to prepare a soft-pack semi-solid battery, wherein the separator includes a base film and a ceramic coating arranged on both sides of the base film, the thickness of the separator is 13 μm, the base film is a PE base film with a thickness of 9 μm, and the thickness of the ceramic coating on both sides is 2 μm;

[0064] Through aluminum plastic film packaging, inject 1 mol / L of electrolyte at an injection coefficient of 1.5g / Ah

[0065] (LiPF6 / EC+PC+DMC+VC+FEC+DTD, 15%: 20%: 20%: 30%: 2.1%: 10%: 2.9%, wt%), high temperature static, fixture pre-charge, degas, formation, aging, capacity division and other processes to complete the battery preparation and basic electrical performance testing. Pre-charge, formation and capacity division are carried out under 1000kgf pressure, 25℃ ambient temperature and 0.2C rate.

[0066] Example 2

[0067] A method for preparing a semi-solid battery comprises the following steps:

[0068] 1) Preparation of positive electrode sheet: 85% positive electrode active material (ternary nickel cobalt manganese oxide NCM coated on the surface of LATP, Ni% = 90%, coating amount is 2%), 10% lithium manganese iron phosphate safety additive LMFP, 2% positive electrode conductive agent Super P and 3% positive electrode binder PVDF are mixed to make positive electrode slurry, and the positive electrode slurry is coated on both sides of the positive electrode current collector, and the positive electrode coating surface density is 45mg / cm 2 After drying, rolling and cutting are performed to obtain the positive electrode sheet; the positive electrode current collector is aluminum foil with a thickness of 6 μm.

[0069] 2) Preparation of negative electrode sheet: 93% negative electrode active material (a mixture of graphite and silicon oxide, the ratio of the two is 80%:20%), 2% solid electrolyte (LLZTO), 2% conductive agent Super P and 3% binder PAA are mixed to make negative electrode slurry, and the negative electrode slurry is coated on both sides of the negative electrode current collector. The surface density of the negative electrode coating is 20mg / cm 2 After drying, rolling and cutting, negative electrode sheets are obtained. The negative electrode current collector is copper foil with a thickness of 4.5 μm;

[0070] 3) stacking the negative electrode sheet, the separator and the positive electrode sheet in sequence through a lamination process to prepare a soft-pack semi-solid battery, wherein the separator includes a base film and a ceramic coating arranged on both sides of the base film, the thickness of the separator is 13 μm, the base film is a PE base film with a thickness of 9 μm, and the thickness of the ceramic coating on both sides is 2 μm;

[0071] Through aluminum plastic film packaging, inject 1 mol / L of electrolyte at an injection coefficient of 1.5g / Ah

[0072] (LiPF6 / EC+PC+DMC+VC+FEC+DTD, 15%: 20%: 20%: 30%: 2.1%: 10%: 2.9%, wt%), high temperature static, fixture pre-charge, degas, formation, aging, capacity division and other processes to complete the battery preparation and basic electrical performance testing. Pre-charge, formation and capacity division are carried out under 1000kgf pressure, 25℃ ambient temperature and 0.2C rate.

[0073] Example 3

[0074] A method for preparing a semi-solid battery comprises the following steps:

[0075] 1) Preparation of positive electrode sheet: 95% positive electrode active material (ternary nickel cobalt manganese oxide NCM coated on the surface of LATP, Ni% = 90%, coating amount 2%), 2% positive electrode conductive agent Super P and 3% positive electrode binder PVDF were mixed to prepare positive electrode slurry, and the positive electrode slurry was coated on both sides of the positive electrode current collector, and the positive electrode coating surface density was 45 mg / cm 2After drying, rolling and cutting are performed to obtain the positive electrode sheet; the positive electrode current collector is aluminum foil with a thickness of 6 μm.

[0076] 2) Preparation of negative electrode sheet: 93% negative electrode active material (a mixture of graphite and silicon oxide, the ratio of the two is 80%:20%), 2% solid electrolyte (LLZTO), 2% conductive agent Super P and 3% binder PAA are mixed to make negative electrode slurry, and the negative electrode slurry is coated on both sides of the negative electrode current collector. The surface density of the negative electrode coating is 20mg / cm 2 After drying, rolling and cutting, negative electrode sheets are obtained. The negative electrode current collector is copper foil with a thickness of 4.5 μm;

[0077] 3) stacking the negative electrode sheet, the separator and the positive electrode sheet in sequence through a lamination process to prepare a soft-pack semi-solid battery, wherein the separator comprises a base film and a solid electrolyte coating disposed on both sides of the base film close to the negative electrode sheet and a nanofiber coating close to the positive electrode sheet; the thickness of the separator is 13 μm, the base film is a PE base film with a thickness of 9 μm, the nanofiber coating close to the positive electrode side comprises nanocellulose and alumina in a mass ratio of (1:9), and the coating thickness is 2 μm; the solid electrolyte coating comprises a LATP solid electrolyte with a coating thickness of 2 μm;

[0078] Through aluminum plastic film packaging, inject 1 mol / L of electrolyte at an injection coefficient of 1.5g / Ah

[0079] (LiPF6 / EC+PC+DMC+VC+FEC+DTD, 15%: 20%: 20%: 30%: 2.1%: 10%: 2.9%, wt%), high temperature static, fixture pre-charge, degas, formation, aging, capacity division and other processes to complete the battery preparation and basic electrical performance testing. Pre-charge, formation and capacity division are carried out under 1000kgf pressure, 25℃ ambient temperature and 0.2C rate.

[0080] Example 4

[0081] A method for preparing a semi-solid battery comprises the following steps:

[0082] 1) Preparation of positive electrode sheet: 95% positive electrode active material (ternary nickel cobalt manganese oxide NCM coated on the surface of LATP, Ni% = 90%, coating amount 2%), 2% positive electrode conductive agent Super P and 3% positive electrode binder PVDF were mixed to prepare positive electrode slurry, and the positive electrode slurry was coated on both sides of the positive electrode current collector, and the positive electrode coating surface density was 45 mg / cm 2 , after drying, rolling and cutting to obtain the positive electrode sheet; the positive electrode current collector includes a PET polymer insulating layer and aluminum foil layers arranged on both sides of the polymer insulating layer; the thickness of the polymer insulating layer is 4μm; the thickness of the aluminum foil layer is 1.5μm.

[0083] 2) Preparation of negative electrode sheet: 93% negative electrode active material (a mixture of graphite and silicon oxide, the ratio of the two is 80%:20%), 2% solid electrolyte (LLZTO), 2% conductive agent Super P and 3% binder PAA are mixed to make negative electrode slurry, and the negative electrode slurry is coated on both sides of the negative electrode current collector. The surface density of the negative electrode coating is 20mg / cm 2 After drying, rolling and cutting, the negative electrode sheet is obtained. The negative electrode current collector includes a PET polymer insulating layer and copper foil layers arranged on both sides of the PET polymer insulating layer; the thickness of the polymer insulating layer is 4.5 μm; the thickness of the copper foil layer is 1 μm;

[0084] 3) stacking the negative electrode sheet, the separator and the positive electrode sheet in sequence through a lamination process to prepare a soft-pack semi-solid battery, wherein the separator includes a base film and a ceramic coating arranged on both sides of the base film, the thickness of the separator is 13 μm, the base film is a PE base film with a thickness of 9 μm, and the thickness of the ceramic coating on both sides is 2 μm;

[0085] The battery preparation and basic electrical performance testing were completed through aluminum-plastic film packaging, injection of electrolyte (1 mol / L (LiPF6 / EC+PC+DMC+VC+FEC+DTD, 15%:20%:20%:30%:2.1%:10%:2.9%, wt%) at an injection coefficient of 1.5g / Ah), high-temperature standing, fixture pre-charging, degas, formation, aging, and capacity division. The pre-charging, formation, and capacity division were carried out under 1000kgf pressure, 25°C ambient temperature, and 0.2C rate.

[0086] Example 5

[0087] A method for preparing a semi-solid battery comprises the following steps:

[0088] 1) Preparation of positive electrode sheet: 95% positive electrode active material (ternary nickel cobalt manganese oxide NCM coated on the surface of LATP, Ni% = 90%, coating amount 2%), 2% positive electrode conductive agent Super P and 3% positive electrode binder PVDF were mixed to prepare positive electrode slurry, and the positive electrode slurry was coated on both sides of the positive electrode current collector, and the positive electrode coating surface density was 45 mg / cm 2 After drying, rolling and cutting are performed to obtain the positive electrode sheet; the positive electrode current collector is aluminum foil with a thickness of 6 μm.

[0089] 2) Preparation of negative electrode sheet: 93% negative electrode active material (a mixture of graphite and silicon oxide, the ratio of the two is 80%:20%), 2% solid electrolyte (LLZTO), 2% conductive agent Super P and 3% binder PAA are mixed to make negative electrode slurry, and the negative electrode slurry is coated on both sides of the negative electrode current collector. The surface density of the negative electrode coating is 20mg / cm 2 After drying, rolling and cutting, negative electrode sheets are obtained. The negative electrode current collector is copper foil with a thickness of 4.5 μm;

[0090] 3) stacking the negative electrode sheet, the separator and the positive electrode sheet in sequence through a lamination process to prepare a soft-pack semi-solid battery, wherein the separator includes a base film and a ceramic coating arranged on both sides of the base film, the thickness of the separator is 13 μm, the base film is a PE base film with a thickness of 9 μm, and the thickness of the ceramic coating on both sides is 2 μm;

[0091] Through aluminum plastic film packaging, inject 1 mol / L of electrolyte at an injection coefficient of 1.5g / Ah

[0092] (LiPF6 / EC+PC+DMC+VC+FEC+DTD+PFPN, 15%: 20%: 18.5%: 27%: 2%: 10%: 2.5%: 5%, wt%), high temperature static, fixture pre-charge, degas, formation, aging, capacity division and other processes to complete the battery preparation and basic electrical performance testing. Pre-charge, formation and capacity division are carried out under 1000kgf pressure, 25℃ ambient temperature and 0.2C rate.

[0093] Example 6

[0094] A method for preparing a semi-solid battery comprises the following steps:

[0095] 1) Preparation of positive electrode sheet: 95% positive electrode active material (ternary nickel cobalt manganese oxide NCM coated on the surface of LATP, Ni% = 90%, coating amount 2%), 2% positive electrode conductive agent Super P and 3% positive electrode binder PVDF were mixed to prepare positive electrode slurry, and the positive electrode slurry was coated on both sides of the positive electrode current collector, and the positive electrode coating surface density was 45 mg / cm 2 After drying, rolling and cutting are performed to obtain the positive electrode sheet; the positive electrode current collector is aluminum foil with a thickness of 6 μm.

[0096] 2) Preparation of negative electrode sheet: 93% negative electrode active material (a mixture of graphite and silicon oxide, the ratio of the two is 80%:20%), 2% solid electrolyte (LLZTO), 2% conductive agent Super P and 3% binder PAA are mixed to make negative electrode slurry, and the negative electrode slurry is coated on both sides of the negative electrode current collector. The surface density of the negative electrode coating is 20mg / cm 2After drying, rolling and cutting, negative electrode sheets are obtained. The negative electrode current collector is copper foil with a thickness of 4.5 μm;

[0097] 3) stacking the negative electrode sheet, the separator and the positive electrode sheet in sequence through a lamination process to prepare a soft-pack semi-solid battery, wherein the separator includes a base film and a ceramic coating arranged on both sides of the base film, the thickness of the separator is 13 μm, the base film is a PE base film with a thickness of 9 μm, and the thickness of the ceramic coating on both sides is 2 μm;

[0098] Through the aluminum plastic film package, inject 1 mol / L of electrolyte at a liquid injection coefficient of 1.0g / Ah

[0099] (LiPF6 / EC+PC+DMC+VC+FEC+DTD+PFPN, 15%: 20%: 18.5%: 27%: 2%: 10%: 2.5%: 5%, wt%), high temperature static, fixture pre-charge, degas, formation, aging, capacity division and other processes to complete the battery preparation and basic electrical performance testing. Pre-charge, formation and capacity division are carried out under 1000kgf pressure, 25℃ ambient temperature and 0.2C rate.

[0100] Example 7

[0101] A method for preparing a semi-solid battery comprises the following steps:

[0102] 1) Preparation of positive electrode sheet: 85% positive electrode active material (ternary nickel cobalt manganese oxide NCM coated on the surface of LATP, Ni% = 90%, coating amount 2%), 10% lithium manganese iron phosphate safety additive LMFP, 2% positive electrode conductor Super P and 3% positive electrode binder PVDF are mixed to make positive electrode slurry, and the positive electrode slurry is coated on both sides of the positive electrode current collector, and the positive electrode coating surface density is 45mg / cm 2 , after drying, rolling and cutting to obtain the positive electrode sheet; the positive electrode current collector includes a PET polymer insulating layer and aluminum foil layers arranged on both sides of the polymer insulating layer; the thickness of the polymer insulating layer is 4μm; the thickness of the aluminum foil layer is 1.5μm.

[0103] 2) Preparation of negative electrode sheet: 93% negative electrode active material (a mixture of graphite and silicon oxide, the ratio of the two is 80%:20%), 2% solid electrolyte (LLZTO), 2% conductive agent Super P and 3% binder PAA are mixed to make negative electrode slurry, and the negative electrode slurry is coated on both sides of the negative electrode current collector. The surface density of the negative electrode coating is 20mg / cm 2 After drying, rolling and cutting, the negative electrode sheet is obtained. The negative electrode current collector includes a PET polymer insulating layer and copper foil layers arranged on both sides of the polymer insulating layer; the thickness of the polymer insulating layer is 4.5 μm; the thickness of the copper foil layer is 1 μm;

[0104] 3) stacking the negative electrode sheet, the separator and the positive electrode sheet in sequence through a lamination process to prepare a soft-pack semi-solid battery, wherein the separator comprises a base film and a solid electrolyte coating disposed on both sides of the base film close to the negative electrode sheet and a nanofiber coating close to the positive electrode sheet; the thickness of the separator is 13 μm, the base film is a PE base film with a thickness of 9 μm, the nanofiber coating close to the positive electrode side comprises nanocellulose and alumina in a mass ratio of (1:9), and the coating thickness is 2 μm; the solid electrolyte coating comprises a LATP solid electrolyte with a coating thickness of 2 μm;

[0105] Through the aluminum plastic film package, inject 1 mol / L of electrolyte at a liquid injection coefficient of 1.0g / Ah

[0106] (LiPF6 / EC+PC+DMC+VC+FEC+DTD+PFPN, 15%: 20%: 18.5%: 27%: 2%: 10%: 2.5%: 5%, wt%), high temperature static, fixture pre-charge, degas, formation, aging, capacity division and other processes to complete the battery preparation and basic electrical performance testing. Pre-charge, formation and capacity division are carried out under 1000kgf pressure, 25℃ ambient temperature and 0.2C rate.

[0107] The performance of the batteries prepared in Examples 1-7 and Comparative Example 1 was tested, and the results are shown in Table 1 below.

[0108] Table 1

[0109]

[0110]

[0111] To summarize, the technical solution of the present application obtains a positive electrode sheet with both high energy density and high safety performance by modifying the solid electrolyte on the surface of the high-nickel ternary positive electrode material and adding lithium iron manganese phosphate safety additives to the high-nickel ternary positive electrode; as a preferred form thereof, with the application of double-coated diaphragms, lightweight high-safety composite foils, and lean high-safety liquid electrolytes, the battery has better safety performance under the joint action of multiple safety technologies. At the same time, the use of lightweight foils, thin diaphragms, and lean high-safety liquid electrolytes can reduce the weight of the battery, increase the energy density of the battery, and achieve the advantages of high energy density and high safety performance of semi-solid batteries.

[0112] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A positive electrode sheet, characterized in that: It includes a positive electrode current collector and a positive electrode active material layer coated on the surface of the positive electrode current collector; the positive electrode active material layer includes a positive electrode active material, a positive electrode conductor, and a positive electrode binder; the positive electrode active material includes a positive electrode material and an oxide solid electrolyte coated on the surface of the positive electrode material.

2. The positive electrode sheet according to claim 1, characterized in that: It also includes a safety agent, lithium manganese iron phosphate; preferably, the amount of lithium manganese iron phosphate added to the positive electrode active material layer is 5-20%, preferably 10%; Preferably, the positive electrode material is one of lithium cobalt oxide, lithium manganese oxide, lithium nickel cobalt manganese oxide, and lithium nickel cobalt aluminum oxide, or a mixture of at least two thereof; The oxide solid electrolyte is one of lithium aluminum titanium phosphate, lithium aluminum germanium phosphate, lithium lanthanum zirconium oxide, lithium lanthanum titanium oxide, and lithium lanthanum zirconium tantalum oxide, or a mixture of at least two of them; The positive electrode conductive agent is one of conductive carbon black, conductive graphite, carbon nanotubes, carbon nanofibers, and graphene, or a mixture of at least two of them; The positive electrode binder is one of polyvinylidene fluoride, styrene-butadiene rubber, carboxymethyl cellulose and polytetrafluoroethylene, or a mixture of at least two of them.

3. The positive electrode sheet according to claim 1, characterized in that: The coating amount of the oxide solid electrolyte is 0.5-3%, preferably 2%.

4. The positive electrode sheet according to claim 2, characterized in that: The mass ratio of the positive electrode active material, lithium manganese iron phosphate, positive electrode conductor, and positive electrode binder is: (74-96): (1-15): (1-5): (2-6); preferably 85:10:2:

3.

5. The positive electrode sheet according to any one of claims 1 to 4, characterized in that: The positive electrode current collector comprises a polymer insulating layer and aluminum foil layers arranged on both sides of the polymer insulating layer; Preferably, the thickness of the polymer insulating layer is 2-10 μm, preferably 4 μm; the thickness of the aluminum foil layer is 1-5 μm, preferably 1.5 μm; Preferably, the polymer insulation layer is made of polyethylene, polypropylene, polyvinyl chloride, polyimide, polyacrylonitrile or polyethylene terephthalate, or a mixture of at least two of them.

6. A method for preparing a positive electrode sheet according to any one of claims 1 to 5, characterized in that: The method comprises the following steps: mixing a positive electrode active material, lithium manganese iron phosphate, a positive electrode conductive agent, and a positive electrode binder to prepare a positive electrode slurry, coating the positive electrode slurry on both sides of a positive electrode current collector, drying, rolling, and cutting to obtain a positive electrode sheet; preferably, the coating surface density of the positive electrode active material layer is 10-50 mg / cm 2 .

7. A semi-solid battery, characterized in that: It comprises the positive electrode sheet, negative electrode sheet, separator and electrolyte as described in any one of claims 1 to 5.

8. The semi-solid-state battery according to claim 7, characterized in that: The negative electrode sheet comprises a negative electrode current collector and a negative electrode active material layer coated on both sides of the negative electrode current collector; The negative electrode active material layer comprises a negative electrode active material, an oxide solid electrolyte, a negative electrode conductive agent, and a negative electrode binder; Preferably, the mass ratio of the negative electrode active material, the oxide solid electrolyte, the negative electrode conductive agent, and the negative electrode binder is: (83-97): (1-5): (1-5): (1-7); preferably 93:2:2:3; Preferably, the negative electrode active material is one of silicon, silicon dioxide, silicon oxide, artificial graphite, natural graphite, composite graphite, soft carbon, and hard carbon, or a mixture of at least two thereof; Preferably, the negative electrode binder is one of styrene-butadiene rubber, polyacrylic acid, and polytetrafluoroethylene, or a mixture of at least two of them; Preferably, the negative electrode current collector comprises a polymer insulating layer and copper foil layers arranged on both sides of the polymer insulating layer; Preferably, the thickness of the polymer insulation layer is 2-10 μm, preferably 4.5 μm; the thickness of the copper foil layer is 1-5 μm, preferably 1 μm; Preferably, the polymer insulating layer is made of one of polyethylene, polypropylene, polyvinyl chloride, polyimide, polyacrylonitrile or polyethylene terephthalate, or a mixture of at least two of them; Preferably, the negative electrode sheet is prepared by the following method: negative electrode active material, oxide solid electrolyte, negative electrode conductive agent, and negative electrode binder are mixed to form negative electrode slurry, the negative electrode slurry is coated on both sides of the negative electrode current collector, and after drying, rolling and cutting, a positive electrode sheet is obtained; preferably, the coating surface density of the negative electrode active material layer is 5-30 mg / cm 2 .

9. The semi-solid-state battery according to claim 7, characterized in that: The diaphragm includes a base film and a solid electrolyte coating disposed on both sides of the base film close to the negative electrode sheet and a nanofiber coating close to the positive electrode sheet; Preferably, the base film is one of a polyethylene base film, a polyethylene non-woven base film, a polypropylene base film, a polypropylene non-woven base film, a polypropylene / polyethylene / polypropylene composite base film, a polyimide base film, a polyimide non-woven base film, a polytetrafluoroethylene base film, a polytetrafluoroethylene non-woven base film, a polyvinyl chloride base film, and a polyvinyl chloride non-woven base film; Preferably, the nanofiber coating comprises ceramic powder and nanofibers; The ceramic powder includes one or a mixture of at least two of aluminum oxide, zirconium oxide, boehmite, magnesium hydroxide, barium sulfate, silicon oxide, aluminum nitride, magnesium oxide, titanium dioxide, yttrium oxide and cerium oxide, and has a particle size of 5-200 nm; The nanofibers include a mixture of at least two of carbon nanotubes, boron carbide nanowires, nanocellulose, and nanoaramid fibers, and the nanofibers have a diameter of 10-50 nm and a length of 100-1000 μm. The mass ratio of nanofiber to ceramic powder is (0.1-1):1; preferably 1:9, and the thickness of the nanofiber coating is 0.1-5 μm; preferably 2 μm; The solid electrolyte coating includes a solid electrolyte; the solid electrolyte includes one or a mixture of at least two of lithium aluminum titanium phosphate, lithium aluminum germanium phosphate, lithium lanthanum zirconium oxide, lithium lanthanum titanium oxide, and lithium lanthanum zirconium tantalum oxide, with a particle size of 100-500nm; the thickness of the solid electrolyte coating is 0.1-3μm; preferably 2μm.

10. The semi-solid-state battery according to claim 7, characterized in that: The electrolyte includes lithium salt, solvent, and additives; The lithium salt is one of lithium hexafluorophosphate, lithium bis(fluorosulfonyl imide), lithium bis(trifluoromethanesulfonyl imide), lithium tetrafluoroborate, lithium bis(oxalatoborate), lithium difluorophosphate, and lithium difluorooxalatoborate, or a mixture of at least two of them; The molar concentration of the lithium salt is 0.5-2 mol / L; preferably 1 mol / L; The solvent includes propylene carbonate, ethylene carbonate, dimethyl carbonate, ethyl methyl carbonate, diethyl carbonate, phthalate, dimethyl maleate, ethylene glycol dimethyl ether, tetrahydrofuran, or a mixture of at least two thereof; The additive is one or a mixture of at least two of vinylene carbonate, vinyl ethylene carbonate, fluoroethylene carbonate, propane sultone, propene sultone, vinyl sulfate, bisfluoroethylene carbonate, and ethoxy pentafluorocyclophosphazene; Preferably, the electrolyte comprises LiPF6 / EC+PC+DMC+VC+FEC+DTD, and the proportion of each component is 15%:20%:20%:30%:2.1%:10%:2.9%, wt%; Preferably, the electrolyte comprises LiPF6 / EC+PC+DMC+VC+FEC+DTD+PFPN, and the proportion of each component is 15%:20%:18.5%:27%:2%:10%:2.5%:5%, wt%; The electrolyte injection amount of each battery is 0.5-1.0g / Ah.

Citation Information

Cited By

  • Battery monomer, battery device, power utilization device and energy storage device

    CN120600796A

  • Battery cell, battery device, power consuming device, and energy storage device

    CN120600796B

  • Positive plate, manufacturing method thereof and secondary battery

    CN120933376A

  • Efficient pre-lithiation / sodium treatment method of energy storage device and application of efficient pre-lithiation / sodium treatment method

    CN121416638A

  • Lithium-ion secondary battery

    US20260188723A1