Rosin modified phenolic resin, varnish for printing ink and printing ink

A rosin-modified phenolic resin using rosin, vegetable oil fatty acids, and polyols addresses low-temperature dissolution and emulsification issues, enhancing varnish formation and ink properties for energy-efficient printing.

JP7567556B2Active Publication Date: 2024-10-16ARAKAWA CHEM IND LTD
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2021032455
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-03-27
Filing Date
2021-03-02
Publication Date
2024-10-16
Estimated Expiration
2041-03-02

AI Technical Summary

Technical Problem

Existing rosin-modified phenolic resins face challenges in dissolving at low temperatures and exhibit poor emulsification resistance when used in printing ink varnishes, hindering energy-efficient varnishing processes.

Method used

A rosin-modified phenolic resin is formulated using specific components including rosin, vegetable oil fatty acids, and polyols, which allows for low-temperature varnish preparation and enhances emulsion resistance.

Benefits of technology

The resin enables varnish formation at lower temperatures with improved emulsion resistance, resulting in printing inks with excellent misting resistance and gloss, suitable for offset and sheet-fed printing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007567556000001
    Figure 0007567556000001
  • Figure 0007567556000002
    Figure 0007567556000002
  • Figure 0007567556000003
    Figure 0007567556000003
Patent Text Reader

Abstract

To provide a rosin-modified phenolic resin that can be made into varnish at low temperature and has excellent resistance to emulsification, and a print ink containing the rosin-modified phenolic resin.SOLUTION: A rosin-modified phenolic resin contains a rosin (A) with a communic acid content of 0.1-8 wt.%, formaldehyde (B), a phenol (C), vegetable oil fatty acid and / or vegetable oil fatty acid ester (D), and a polyol (E) as reaction components.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a rosin-modified phenolic resin, a varnish for printing ink, and a printing ink. [Background technology]

[0002] Rosin-modified phenolic resin is a high molecular weight polymer made mainly from rosins, phenols, formaldehyde and polyols, which dissolves in various printing ink solvents and exhibits excellent printability (emulsion resistance, misting resistance, gloss, drying properties, etc.), and has been widely used as a printing ink binder. In addition, gum rosin has been widely used as the raw rosin in the production of the resin because of its ease of availability (Patent Documents 1 and 2).

[0003] On the other hand, in the printing ink field, there is an increasing need to lower the temperature in the varnish production process in order to save energy. However, when varnish is produced at low temperatures, the rosin-modified phenolic resin becomes less soluble in printing ink solvents, and the emulsification resistance tends to deteriorate.

[0004] As a means for increasing solubility in printing ink solvents and improving emulsification resistance, a rosin-modified phenolic resin is known in which a monoester formed by partially esterifying a mixture of rosin and animal and vegetable oil fatty acids with a monoalcohol is further reacted with a polyhydric alcohol and a phenol-formaldehyde initial condensate, but it has not yet become possible to form a varnish at low temperatures. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2004-352782 A [Patent Document 2] JP 2004-269752 A Summary of the Invention [Problem to be solved by the invention]

[0006] An object of the present invention is to provide a rosin-modified phenolic resin which can be turned into a varnish at low temperatures and also exhibits excellent emulsification resistance, and a printing ink containing the rosin-modified phenolic resin. [Means for solving the problem]

[0007] The present inventors have conducted extensive research and found that a rosin-modified phenolic resin obtained by using a reaction component containing specific rosins and vegetable oil fatty acids can solve the above problems, leading to the completion of the present invention. That is, the present invention relates to the following rosin-modified phenolic resin, varnish for printing ink, and printing ink.

[0008] 1. A rosin-modified phenolic resin containing as reactive components rosins (A) having a communicable acid content of 0.1 to 8% by weight, formaldehyde (B), phenols (C), vegetable oil fatty acids and / or vegetable oil fatty acid esters (D), and polyol (E).

[0009] 2. A rosin-modified phenolic resin as described in the preceding paragraph 1, in which the component (C) is a p-alkylphenol.

[0010] 3. A rosin-modified phenolic resin according to item 1 or 2 above, wherein component (D) is at least one selected from the group consisting of soybean oil fatty acids, linseed oil fatty acids, soybean oil fatty acid esters and linseed oil fatty acid esters.

[0011] 4. The rosin-modified phenolic resin according to any one of items 1 to 3 above, wherein the amount of component (D) used, in terms of solid content weight, is 1 to 15 parts by weight per 100 parts by weight of component (A).

[0012] 5. The rosin-modified phenolic resin according to any one of items 1 to 4 above, which has a weight average molecular weight of 50,000 to 300,000.

[0013] 6. A varnish for printing ink, comprising the rosin-modified phenolic resin according to any one of items 1 to 4 above, and vegetable oils and / or petroleum-based solvents.

[0014] 7. Printing inks containing the printing ink varnish described in paragraph 6 above. Effect of the Invention

[0015] According to the rosin-modified phenolic resin of the present invention, since the resin itself has a low softening point, a varnish for printing ink can be prepared even at a relatively low temperature, and further, when preparing a gel varnish or printing ink, the varnish exhibits excellent emulsification resistance. The obtained printing ink also has excellent misting resistance and gloss. The printing ink is particularly suitable for offset printing ink and sheet-fed ink. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] The rosin-modified phenolic resin of the present invention contains, as reactive components, rosin (A) having a communicable acid content of 0.1 to 8% by weight (hereinafter referred to as component (A)), formaldehyde (B) (hereinafter referred to as component (B)), phenol (C) (hereinafter referred to as component (C)), vegetable oil fatty acid and / or its ester (D) (hereinafter referred to as component (D)), and polyol (E) (hereinafter referred to as component (E)).

[0017] Component (A) is a rosin containing 0.1-8% by weight of communicable acid. When the communicable acid content is within the above range, the softening point of the rosin-modified phenolic resin is lowered by using it as a reactive component, making it possible to produce a varnish at a low temperature, and the hydrophobicity of the resin is increased, resulting in excellent emulsification resistance of the printing ink. From the same viewpoint, the communicable acid content is preferably 1-6% by weight, more preferably 2-5% by weight.

[0018] The content of communic acid can be measured by various known methods. For example, when the rosin is unmodified rosin, the content of communic acid can be obtained by using gas chromatography (GC) to determine the ratio (%) of the peak area of ​​communic acid to the peak area of ​​all resin acids (100%). When the rosin is modified rosin, the content of communic acid can be obtained by the absolute calibration curve method using gas chromatography (GC), taking into account that this is a high molecular weight substance.

[0019] In this specification, the "communic acid" contained in component (A) refers to isomers such as cis-communic acid, trans-communic acid, and mirceo-communic acid. An example structure is shown below.

[0020] [ka]

[0021] The method for obtaining the component (A) is not particularly limited, and examples thereof include the following methods. [1] Combining rosin that does not contain communicable acid (unmodified rosin or modified rosin) with communicable acid obtained separately. [2] Use rosins that originally contain comunic acid as is. [3] Combining rosins that naturally contain communicable acid with rosins that do not contain communicable acid. [4] Combining rosins that already contain communicable acid with communicable acid obtained separately.

[0022] Communic acid can be isolated from unmodified rosin or its derivatives which originally contain communicic acid by various known methods, such as silica gel column chromatography (J. Am. Chem. Soc., 77, 2823 (1955), etc.).

[0023] Rosins that naturally contain communicable acid include, for example, marsh pine rosin.

[0024] The content of communic acid in rosins that originally contain communic acid is usually about 1 to 8% by weight, and preferably about 1 to 6% by weight.

[0025] Examples of rosins that do not contain communicable acid include unmodified rosins such as gum rosin, tall oil rosin, wood rosin, and Merkus pine rosin; polymerized rosin obtained by polymerizing the unmodified rosins; hydrogenated rosin obtained by hydrogenating the unmodified rosins; and modified rosins such as carboxylic acid-modified rosin obtained by reacting the unmodified rosins with α,β-unsaturated carboxylic acids.

[0026] Examples of the α,β-unsaturated carboxylic acid include α,β-unsaturated dicarboxylic acids such as maleic acid, maleic anhydride, and fumaric acid, and α,β-unsaturated monocarboxylic acids such as acrylic acid and methacrylic acid. The amount of the α,β-unsaturated carboxylic acid used is not particularly limited, but is usually about 1 to 30 parts by weight per 100 parts by weight of unmodified rosin.

[0027] Furthermore, as the component (A), a product obtained by reacting the component (A) with the above-mentioned α,β-unsaturated carboxylic acid may be used.

[0028] The component (B) is not particularly limited, and examples thereof include formalin and paraformaldehyde.

[0029] The amount of component (B) used is not particularly limited, but from the viewpoint of reducing the environmental burden, it is usually 5 to 80 parts by weight, and preferably 10 to 30 parts by weight, per 100 parts by weight of component (A) calculated as solid content.

[0030] The component (C) is a phenol, and examples thereof include carbolic acid (phenol) and alkylphenols. Examples of alkylphenols include methylphenol (cresol), n-butylphenol, isobutylphenol, t-butylphenol, n-pentylcresol (amylphenol), n-octylphenol, n-nonylphenol, n-decylphenol, n-dodecylphenol, n-tetradecylphenol, and n-hexyldecylphenol. These may be used alone or in combination of two or more. The alkylphenol may be any of o-alkylphenol, m-alkylphenol, and p-alkylphenol. Among them, p-alkylphenol is preferred from the viewpoint of obtaining a high molecular weight rosin-modified phenolic resin, and pt-butylphenol and p-octylphenol are more preferred.

[0031] The amount of component (C) used is not particularly limited, but in order to obtain a high molecular weight rosin-modified phenolic resin, it is usually 3 to 100 parts by weight, and preferably 5 to 80 parts by weight, per 100 parts by weight of component (A) in terms of solid content.

[0032] The ratio of the (B) component to the (C) component is not particularly limited, but the molar ratio [(B) / (C)] is usually 1.5 to 3. In addition, in order to reduce the environmental load and obtain a high molecular weight rosin-modified phenolic resin, (B) / (C) is preferably 1.8 to 2.8, more preferably 2 to 2.6. In the following, the (B) / (C) ratio is also referred to as the F / P ratio.

[0033] In the present invention, a condensate of the (B) component and the (C) component (a resol type phenolic resin, a novolac type phenolic resin) may be used. The resol type phenolic resin may be a condensate obtained by addition-condensation reaction in the presence of a basic catalyst. The novolac type phenolic resin may be a condensate obtained by addition-condensation reaction in the presence of an acid catalyst.

[0034] The basic catalyst is not particularly limited, and examples thereof include organic amines such as triethylamine, metal oxides such as magnesium oxide and zinc oxide, metal hydroxides such as sodium hydroxide, magnesium hydroxide and calcium hydroxide, and metal acetates such as calcium acetate, magnesium acetate and zinc acetate. Examples of the acidic catalyst include inorganic acids such as hydrochloric acid and sulfuric acid, and organic acids such as oxalic acid, methanesulfonic acid, paratoluenesulfonic acid and dodecylbenzenesulfonic acid. These may be used alone or in combination of two or more.

[0035] The condensate can be produced in the presence of an organic solvent such as toluene or xylene, or water. The production conditions are not particularly limited, but for example, the components (B) and (C) may be separately charged and reacted at a reaction temperature of about 100 to 300° C. for a reaction time of about 1 to 24 hours.

[0036] The component (D) is a vegetable oil fatty acid and / or a vegetable oil fatty acid ester, and by being incorporated into the skeleton of the rosin-modified phenolic resin, the hydrophobicity of the rosin-modified phenolic resin is increased and the resin exhibits good solubility in petroleum-based solvents. This also enables the resin to be made into a varnish at low temperatures, and also provides the printing ink with excellent emulsification resistance.

[0037] Examples of the (D) component include vegetable oil fatty acids such as soybean oil fatty acid, hydrogenated soybean oil fatty acid, linseed oil fatty acid, tung oil fatty acid, camellia oil fatty acid, corn oil fatty acid, coconut oil fatty acid, palm oil fatty acid, rapeseed oil fatty acid, and tall oil fatty acid; and vegetable oil fatty acid esters such as methyl ester, ethyl ester, n-propyl ester, n-butyl ester, n-pentyl ester, n-hexyl ester, n-heptyl ester, n-octyl ester, and glycerin of these vegetable oil fatty acids. The glycerin ester of vegetable oil fatty acid means vegetable oil such as soybean oil, linseed oil, tung oil, camellia oil, corn oil, coconut oil, palm oil, rapeseed oil, and tall oil. These may be used alone or in combination of two or more. Among them, soybean oil fatty acid, linseed oil fatty acid, soybean oil fatty acid ester, and linseed oil fatty acid ester are preferred from the viewpoint of good solubility of rosin-modified phenolic resin in petroleum-based solvents and excellent emulsification resistance of printing ink.

[0038] The amount of component (D) used is not particularly limited, but from the viewpoints of good solubility of the rosin-modified phenolic resin in petroleum-based solvents and excellent emulsification resistance of the printing ink, it is preferably 1 to 15 parts by weight, and more preferably 2 to 10 parts by weight, per 100 parts by weight of component (A) in terms of solid content.

[0039] The component (E) is not particularly limited as long as it has two or more hydroxyl groups in one molecule, and various known ones can be used. For example, diols such as ethylene glycol, diethylene glycol, triethylene glycol, 1,3-propylene glycol, 1,4-butanediol, neopentyl glycol, 3-methyl-1,5-pentanediol, 1,6-hexanediol, etc.; triols such as glycerin, trimethylolethane, trimethylolpropane, etc.; tetraols such as pentaerythritol, diglycerin, ditrimethylolethane, ditrimethylolpropane, etc.; and polyols with 5 or more valences such as dipentaerythritol. These may be used alone or in combination of two or more. Among these, triols and / or tetraols are preferred because it is easy to control the physical properties such as the softening point and weight average molecular weight of the rosin-modified phenolic resin.

[0040] The proportion of component (E) used is not particularly limited, but from the viewpoint of emulsification resistance of the offset printing ink, it is preferable that the ratio (OH / COOH) of the total hydroxyl group equivalent number (OH) of component (E) to the total carboxyl group equivalent number (COOH) of component (A) is about 0.5 to 1.5.

[0041] The rosin-modified phenolic resin of the present invention is obtained by reacting components (A) to (E) in the presence of a catalyst. There is no particular limitation on the production method, but examples thereof include methods (1) to (7). In the following methods, the order of addition of each component is not particularly limited. (1) A method in which components (A) to (E) are charged all at once and reacted in the presence of a catalyst (2) A method in which components (A) to (D) are charged all at once and reacted in the presence of a catalyst, and then component (E) is added and reacted. (3) A method in which component (A) is reacted with a condensate of components (B) and (C) in the presence of a catalyst, and then components (D) and (E) are added and reacted. (4) A method in which component (A) is reacted with a condensate of components (B) and (C) in the presence of a catalyst, component (D) is added and reacted, and then component (E) is added and reacted. (5) A method in which components (A) and (D) are reacted together, and then a condensate of components (B) and (C), and component (E), which will be described later, are added and reacted. (6) A method in which components (A), (B), and (C) are reacted in the presence of a catalyst, and then components (D) and (E) are added and reacted. (7) A method in which components (A), (B), and (C) are reacted in the presence of a catalyst, component (D) is added and reacted, and then component (E) is added and reacted.

[0042] The catalyst is not particularly limited, and examples thereof include the above-mentioned basic catalysts, acid catalysts, etc. The amount of the catalyst used is also not particularly limited, and is preferably 0.05 to 5 parts by weight, and more preferably 0.05 to 3 parts by weight, per 100 parts by weight of the component (A).

[0043] The production conditions are not particularly limited and are usually a reaction temperature of about 100 to 300°C and a reaction time of about 1 to 24 hours. However, in the method for producing the rosin-modified phenolic resin of the present invention, from the standpoint of reactivity, it is preferable to carry out the reaction at a temperature of about 100 to 260°C and for a reaction time of about 8 to 24 hours.

[0044] The weight average molecular weight (referred to as a polystyrene equivalent value in gel permeation chromatography; the same applies hereinafter) of the rosin-modified phenolic resin obtained by the above-mentioned production method is not particularly limited, but from the viewpoints of good solubility of the rosin-modified phenolic resin in petroleum-based solvents and excellent misting resistance of printing inks, it is preferably about 50,000 to 300,000, and more preferably 100,000 to 300,000.

[0045] Other physical properties are not particularly limited either. For example, the softening point (JIS K5601) is usually 120 to 200° C., and the acid value (JIS K5601) is usually about 5 to 30 mgKOH / g.

[0046] The varnish for printing ink of the present invention contains the rosin-modified phenolic resin of the present invention and vegetable oils and / or petroleum-based solvents.

[0047] Examples of vegetable oils include vegetable oils such as linseed oil, tung oil, safflower oil, dehydrated castor oil, and soybean oil; vegetable oil monoesters such as linseed oil fatty acid methyl, soybean oil fatty acid methyl, linseed oil fatty acid ethyl, soybean oil fatty acid ethyl, linseed oil fatty acid n-propyl, soybean oil fatty acid n-propyl, linseed oil fatty acid n-butyl, and soybean oil fatty acid n-butyl. These may be used alone or in combination of two or more. The use of vegetable oils is preferred because the rosin-modified phenolic resin exhibits good solubility in petroleum-based solvents and a printing ink with excellent emulsification resistance can be obtained.

[0048] The petroleum-based solvent is not particularly limited, and examples thereof include petroleum-based solvents from JXTG Nippon Oil & Energy Corporation such as No. 0 Solvent, No. 4 Solvent, No. 5 Solvent, No. 6 Solvent, No. 7 Solvent, AF Solvent No. 4, AF Solvent No. 5, AF Solvent No. 6, and AF Solvent No. 7, which may be used alone or in combination of two or more.

[0049] The printing ink varnish of the present invention may also contain a gelling agent.

[0050] The gelling agent is not particularly limited, and examples thereof include aluminum-based gelling agents such as aluminum octylate, aluminum stearate, aluminum triisopropoxide, aluminum tributoxide, aluminum dipropoxide monoacetylacetate, aluminum dibutoxide monoacetylacetate, and aluminum triacetylacetate, which may be used alone or in combination of two or more kinds.

[0051] The printing ink varnish of the present invention is not particularly limited, and can be obtained, for example, by mixing a rosin-modified phenolic resin, a vegetable oil and / or a petroleum-based solvent, and, if necessary, a gelling agent with stirring, and reacting the mixture at a reaction temperature of usually about 100 to 240° C. During the reaction, additives such as an antioxidant may be added.

[0052] The printing ink of the present invention includes the printing ink varnish of the present invention. Specifically, the printing ink varnish, pigments (yellow, red, indigo, black, etc.), and, if necessary, the above-mentioned vegetable oils, petroleum-based solvents, and additives such as surfactants and waxes are milled using an ink manufacturing device such as a roll mill, ball mill, attritor, sand mill, etc., to prepare appropriate ink constants. EXAMPLES

[0053] The present invention will be described in more detail below with reference to examples, but is not limited thereto. Unless otherwise specified, all "parts" and "%" are by weight.

[0054] (Communic acid content) The value was determined using a commercially available gas chromatograph (GC-14A, manufactured by Shimadzu Corporation).

[0055] (Weight average molecular weight) The values ​​are polystyrene-equivalent values ​​measured using a commercially available gel permeation chromatography apparatus (HLC-8320GPC, manufactured by Tosoh Corporation), a commercially available column (TSK-GEL column, manufactured by Tosoh Corporation), and tetrahydrofuran as the developing solvent.

[0056] (Viscosity of printing ink varnish) The value (Pa·s) was measured using an E-type viscometer (manufactured by Toki Sangyo) with printing ink varnish adjusted to 25°C.

[0057] Preparation Example 1 (Isolation of communicable acid) Absorbent cotton and sea sand were spread in a glass funnel equipped with a cock, and silica gel 60 (manufactured by Wako Pure Chemical Industries, Ltd.) moistened with isooctane was filled. Isooctane was used as the developing solvent. Next, 1,000 parts of gum rosin (manufactured by Wuyihuaqi Chemical Co., Guangxi Province) containing comunic acid was dissolved in 2,768 parts of isooctane to prepare a gum rosin solution, and the solution was poured onto the silica gel. Next, the eluate was separated into test tubes, and only the fraction containing comunic acid was collected to make one solution, and the solution was concentrated with an evaporator, then diluted again with isooctane, and 3 mol / L aqueous sodium hydroxide solution was dropped while stirring. Next, the precipitated sodium salt was filtered and dried, and the dried product was dissolved in diethyl ether to make a solution, and 1 mol / L aqueous phosphoric acid solution was dropped while stirring until the solution became neutral. Next, the obtained solution was concentrated with an evaporator to obtain liquid comunic acid. In the following examples, the required amounts were prepared as required.

[0058] Preparation Example 2 974 parts of gum rosin containing 3% communicable acid was charged into a reaction vessel equipped with a stirrer, a reflux condenser with a water divider, and a thermometer, and the mixture was heated to 180°C under a nitrogen atmosphere while stirring to melt. Next, 26 parts of communicable acid obtained by the method of Preparation Example 1 was charged and stirred for 1 hour to prepare rosin (A-1). The communicable acid content in component (A-1) was approximately 5.5% by weight.

[0059] Preparation Example 3 Gum rosin containing 3% comunic acid was used as it was as rosin (A-2).

[0060] Preparation Example 4 In a reaction vessel equipped with a stirrer, a reflux condenser with a water divider, and a thermometer, 800 parts of rosin containing 3% communicable acid and 200 parts of Chinese gum rosin (communic acid: 0%) were charged, and the mixture was heated to 180°C while stirring under a nitrogen atmosphere until melted, after which it was stirred for 1 hour to prepare rosin (A-3). The communicable acid content in component (A-3) was approximately 2.4% by weight.

[0061] Preparation Example 5 In a reaction vessel equipped with a stirrer, a reflux condenser with a water divider, and a thermometer, 600 parts of rosin containing 3% communicable acid and 400 parts of Chinese gum rosin (communic acid: 0%) were charged, and the mixture was heated to 180°C while stirring under a nitrogen atmosphere until melted, after which it was stirred for 1 hour to prepare rosin (A-4). The communicable acid content in component (A-4) was approximately 1.8% by weight.

[0062] Example 1 In a reaction vessel equipped with a stirrer, a reflux condenser with a water divider and a thermometer, 1000 parts of rosin (A-1), 500 parts of p-octylphenol (POP), 198 parts of 92% paraformaldehyde (solid content: 182.2 parts) (F / P ratio = 2.5), and 25 parts of soybean oil fatty acid were charged, and the temperature was raised to 100 ° C while stirring, 5 parts of zinc oxide were added, and the temperature was kept for 4 hours. After that, the temperature was raised to 230 ° C, 65 parts of glycerin and 25 parts of pentaerythritol were added, and the mixture was reacted at 245 to 270 ° C for 12 hours to obtain a rosin-modified phenolic resin. The weight average molecular weight, acid value and softening point of the obtained resin are shown in Table 1 (same below).

[0063] Examples 2 to 4, Comparative Example 1 The synthesis was carried out in the same manner as in Example 1, except that the type of rosin was changed, to obtain each of the rosin-modified phenolic resins.

[0064] Example 5 A rosin-modified phenolic resin was obtained by the same synthesis method as in Example 1, except that 350 parts of POP and 110 parts of pt-butylphenol (PTBP) were charged as the alkylphenol.

[0065] Examples 6 to 9 The synthesis was carried out in the same manner as in Example 1 except that the amount of formaldehyde added was changed, to obtain each of the rosin-modified phenolic resins.

[0066] Example 10 A rosin-modified phenolic resin was obtained in the same manner as in Example 1, except that the soybean oil fatty acid was changed to linseed oil fatty acid.

[0067] Examples 11 to 13 The synthesis was carried out in the same manner as in Example 1, except that the amount of soybean oil fatty acid added was changed, to obtain each rosin-modified phenolic resin.

[0068] Comparative Example 2 A rosin-modified phenolic resin was obtained by synthesis in the same manner as in Example 1, without using soybean oil fatty acid.

[0069] Comparative Example 3 A rosin-modified phenolic resin was obtained by synthesis in the same manner as in Example 1, except that 65 parts of glycerin and 25 parts of pentaerythritol were added to the raw material composition of Comparative Example 1 and then reacted at 245 to 270° C. for 18 hours.

[0070] [Table 1]

[0071] <Varnishing at low temperatures (preparation of varnish for printing ink)> Evaluation examples 1-1 to 1-13, Comparative evaluation examples 1-1 to 1-3 In a reaction vessel equipped with a stirrer, reflux condenser, and thermometer, 40 parts of each rosin-modified phenolic resin listed in Table 2, 30 parts of soybean oil, and 29 parts of petroleum-based solvent (AF Solvent No. 6) were charged and mixed at 180°C for 30 minutes to obtain printing ink varnish (V). The rosin-modified phenols of Comparative Examples 1 and 2 were mixed at 180°C for 60 minutes, but insoluble matter was generated and they were not used for the subsequent evaluation. For reference, the same composition was charged and then mixed at 200°C for 30 minutes to obtain printing ink varnish (V'). The viscosity (Pa·s) of the printing ink varnish was measured. The results are shown in Table 2.

[0072] [Table 2]

[0073] <Preparation of printing ink> Evaluation examples 2-1 to 2-14, Comparative evaluation examples 2-1 to 2-4 99 parts of each printing ink varnish shown in Table 3 and 0.5 parts of AF Solvent No. 6 were charged and mixed and dissolved at 160° C. for 30 minutes. After cooling to 80° C., 0.5 parts of aluminum dipropoxide monoacetyl acetate (trade name: “Kerope EP-2”, Hope Pharmaceutical Co., Ltd.) (hereinafter referred to as “gelling agent”) was added as a gelling agent, and the mixture was heated to 200° C. and subjected to a gelling reaction for 1 hour to obtain a printing ink gel varnish. Next, the above-mentioned gel varnish for printing ink was used and milled in a three-roll mill in the following mixing ratio, and appropriately adjusted so that the tack value was 9.0±0.5 and the spread meter flow value (diameter value) was 38.0±1.0 to obtain the printing ink of the present invention. Phthalocyanine blue (indigo pigment) 18 parts by weight Gel varnish for printing ink 66-71 parts by weight AF Solvent No. 6 11 to 16 parts by weight Based on the above formulation, the viscosity was adjusted appropriately to 35 to 45 Pa·s as measured by an E-type viscometer (manufactured by Toki Sangyo Co., Ltd.).

[0074] (Emulsification resistance) 15.0 g of each printing ink was emulsified using an emulsification tester (NOVOMATICS) (rotation speed: 1200 rpm, temperature: 40°C, pure water supply rate: 1.2 ml / min), and after removing excess water, the emulsification rate (%) was measured using a Karl Fischer moisture meter (Kyoto Electronics Manufacturing Co., Ltd.). The smaller the value, the better the emulsification resistance. The results are shown in Table 3 (same below).

[0075] (Misting resistance) 2.6 ml of each printing ink was spread on an Incometer (manufactured by Toyo Seiki Seisakusho Co., Ltd.), and the roll was rotated at 400 rpm for 1 minute at a roll temperature of 30°C, and then at 1800 rpm for 2 minutes. The degree of ink scattering on a white paper placed directly under the roll was observed and rated on a scale of 1 to 5. The higher the value, the better the misting resistance. (Evaluation Criteria) 5: Less ink scattering on white paper 4: The degree of ink scattering on white paper is somewhat low. 3: There is a little bit of ink scattering on the white paper. 2: High ink splash on white paper 1: Very high ink splash rate on white paper

[0076] (Glossy) 0.4 ml of each printing ink was applied to art paper using an RI tester (manufactured by Ishikawajima Industrial Machinery Co., Ltd.), and then the paper was conditioned at 23°C and 50% RH for 24 hours, after which the reflectance at 60°-60° was measured using a gloss meter. The higher the value, the better the gloss.

[0077] [Table 3]

Claims

1. The reaction components include rosins (A) having a communicable acid content of 0.1 to 8% by weight, formaldehyde (B), phenols (C), vegetable oil fatty acids and / or vegetable oil fatty acid esters (D), and polyols (E), The component (D) is at least one selected from the group consisting of soybean oil fatty acids, linseed oil fatty acids, soybean oil fatty acid esters, and linseed oil fatty acid esters, A rosin-modified phenolic resin in which the amount of component (D) used is 1 to 15 parts by weight, in terms of solid content, per 100 parts by weight of component (A).

2. 2. The rosin-modified phenolic resin according to claim 1, wherein the component (C) is a p-alkylphenol.

3. 3. The rosin-modified phenolic resin according to claim 1, having a weight average molecular weight of 50,000 to 300,000.

4. A varnish for printing ink comprising the rosin-modified phenolic resin according to claim 3 and vegetable oils and / or petroleum-based solvents.

5. A printing ink comprising the printing ink varnish of claim 4.

Citation Information

Patent Citations

  • Preparation of rosin phenolic resin for printing ink modified with oil

    JP1982002319A

  • Production of oil-modified resin phenol resin for printing ink

    JP1982061017A

  • Rosin-modified phenol resin, gel varnish, printing ink and printing method each using the same resin and method for producing rosin-modified phenol resin

    JP2004269752A

  • Rosin-modified phenol resin, gel varnish, printing ink and method for producing rosin-modified phenol resin

    JP2004352782A

  • Rosin-modified phenolic resin, printing ink varnish, and printing ink

    JP2012001714A