Tube container
A tube container cap composed of a polypropylene and high-density polyethylene blend reduces opening torque, addressing the difficulty of opening caps for vulnerable groups and ensuring ease of use and sealing.
Patent Information
- Application Number
- JP2021063148
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-04-01
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2041-04-01
AI Technical Summary
Existing tube container caps made of polypropylene are difficult to open and require high torque, posing a challenge for socially vulnerable groups such as the elderly and those with disabilities.
The tube container design incorporates a cap made of a blend of polypropylene and high-density polyethylene with a density of 0.915 g/cm³ or higher, in a ratio of 70:30 to 25:75, which reduces the opening torque and enhances ease of use.
The blend polymer cap design significantly reduces the torque required to open the container, making it easier for individuals with limited dexterity to use, while maintaining structural integrity and sealing performance.
Smart Images

Figure 0007567629000002 
Figure 0007567629000003 
Figure 0007567629000004
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a tube container, and more specifically, to a tube container having a tube container body including a head having a spout portion and a body portion connected to the head, and a cap that is attached to the spout portion of the tube container body to close the spout portion. [Background technology]
[0002] A tube container generally has a structure including a cylindrical body portion with one end closed and the other end open, and a head portion having a spout connected to the other open end of the body portion. Such a tube container is provided with a cap that can close the spout so that the contents do not leak out during use. In general, the outer peripheral surface of the spout of the tube container body and the inner peripheral surface of the cap have a structure that allows the spout and the cap to be screwed or fitted together to close the spout (Patent Document 1).
[0003] The head (pouring outlet) and cap of the tube container body as described above are generally formed by compression molding or injection molding using thermoplastic resin such as polyolefin. For example, the head of the tube container body is formed using resin such as polyethylene, and the cap is formed using resin such as polypropylene (Patent Document 2). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Application Publication No. 10-166530 [Patent Document 2] Japanese Patent Application Publication No. 10-1149 Summary of the Invention [Problem to be solved by the invention]
[0005] In recent years, with the trend towards universal design in pharmaceutical and food packaging, emphasis has been placed on methods that are easy for consumers to open, such as easy opening, as a consideration for the socially vulnerable (elderly, young children, people with disabilities, etc.). Among these, easy-to-open caps used for containers, etc., are gaining in importance. Generally, caps made of resins such as polypropylene require a large torque to open, are tightly fastened, and have a surface that is difficult to open.
[0006] Therefore, the present disclosure has been made in consideration of such problems, and aims to provide a tube container that is easy to open and can reduce the torque required to open the cap without changing the cap molding mold from a conventional mold that molds caps from 100% by mass of polypropylene resin. [Means for solving the problem]
[0007] That is, a tube container according to one embodiment includes a tube container body having a head portion having a pouring outlet portion and a body portion connected to the head portion, and a cap that is detachably attached to the pouring outlet portion of the tube container body and closes the pouring outlet portion, wherein the pouring outlet portion of the tube container body contains high density polyethylene as a main component, the cap contains a blend polymer of polypropylene and high density polyethylene, the blend polymer has a compounding ratio of the polypropylene and the high density polyethylene of 70:30 to 25:75 by mass, and the density of the blend polymer is 0.915 g / cm 3 More than 0.930g / cm 3 The following is the result. Effect of the Invention
[0008] According to the present disclosure, it is possible to provide a tube container that is easy to open by keeping the torque required when opening the cap small. [Brief description of the drawings]
[0009] [Figure 1]FIG. 1 is a perspective view showing a simplified configuration of a tube container according to an embodiment of the present invention. [Diagram 2] Cross-sectional view A-A in Figure 1. [Diagram 3] FIG. 2 is a partial cross-sectional view of a laminate sheet constituting a body portion of the tube container according to the present embodiment. [Figure 4] FIG. 2 is a partial cross-sectional view of a laminate sheet constituting a body portion of the tube container according to the present embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] An embodiment will be described below with reference to the drawings. Figures 1 to 3 are diagrams showing an embodiment. Each of the drawings shown below is a schematic diagram. Furthermore, the numerical values such as dimensions of each member and the names of materials described in this specification are examples of an embodiment, and are not limited to these, and can be appropriately selected and used.
[0011] First, a tube container 1 according to the present embodiment will be described with reference to FIG. The tube container according to this embodiment is composed of a tube container body 10 and a cap 20. The tube container body 10 has a head portion 11 and a body portion 12.
[0012] Head 11 is connected to one end of body 12, and has a spout 14. In this embodiment, head 11 has a shoulder 13 connected to one end of body 12, and a spout 14 connected to shoulder 13. In addition, a thread 15 is provided on the outer circumferential surface of spout 14 for attaching a cap.
[0013] The tube container body 10 having such a configuration is obtained through the following manufacturing process. First, using the tube container packaging material (laminate sheet) 30 according to this embodiment, both ends of the tube container packaging material 30 are overlapped as shown in FIG. 2, and the outer and inner surfaces of the overlapped portions are heat-sealed to form a heat-sealed portion 17, thereby manufacturing the cylindrical body portion 12. Next, the cylindrical body portion 12 is placed in a mold, and a shoulder portion 13 and a pouring outlet portion 14 are formed at one opening of the cylindrical body portion 12 by a normal method such as compression molding. In this manner, the tube container body 10 is produced. Also, a cap 20 is attached to the pouring outlet portion 14 of the tube container body 10.
[0014] Thereafter, an appropriate amount of, for example, toothpaste or other contents is filled into the tube container body 10 from the other opening of the cylindrical body of the tube container body 10. The other opening is then welded to form a bottom seal portion 16, thereby obtaining a packaged product including the tube container body 10 filled with the contents.
[0015] Next, the tube container packaging material 30 from which the tube container body 10 is made will be described. The tube container packaging material 30 from which the tube container body 10 is produced is composed of a laminated sheet including an outer layer 31, an intermediate layer 32, and an inner layer 33, which are arranged in this order from the outer surface to the inner surface, as shown in Fig. 3. Moreover, the tube container packaging material 30 from which the tube container body 10 is produced may further include a barrier layer 34 arranged between the intermediate layer 32 and the inner layer 33, as shown in Fig. 4.
[0016] Next, the cap 20 that is attached to the spout portion 14 of the tube container body 10 will be described.
[0017] Cap 20 is detachably attached to the spout 14 of head 11 and has the function of closing spout 14. The cap may be a screw-type cap having a groove on its inner surface so as to screw into thread 15 provided on the outer circumferential surface of spout 14 as shown in FIG.
[0018] The cap 20 can be integrally formed by a molding method such as compression molding or injection molding using a resin composition containing a blend polymer of polypropylene and polyethylene. The blending ratio (mass%) of polypropylene and polyethylene is preferably 70:30 to 25:75, more preferably 70:30 to 50:50. Within the above range, the cap in the state of a blend of polypropylene and polyethylene has excellent moldability, and the cap can be produced without changing from a conventional molding die for polypropylene alone, and has excellent long-term productivity.
[0019] The blend polymer of polypropylene and polyethylene used in the resin composition constituting the cap 20 has a density of 0.915 g / cm 3 More than 0.930g / cm 3 It is preferable that the content is within the following range. The above range is preferable from the viewpoints of compatibility between polypropylene and polyethylene, heat resistance of the cap, and the torque required to open the cap being smaller than that required in the past.
[0020] Examples of polypropylene used in the resin composition constituting the cap 20 include homopolymers and copolymers of propylene. The structure of these polypropylenes may be isotactic or syndiotactic. Examples of polypropylene include copolymers of propylene and other olefins such as ethylene, 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, and 4-methyl-1-pentene, and these copolymers may be random copolymers or block copolymers.
[0021] In the present embodiment, the polypropylene used in the resin composition constituting the cap 20 is preferably a propylene-ethylene block copolymer having an ethylene content of 2% by mass or more and 10% by mass or less. When the ethylene content is within the above range, the polypropylene has excellent compatibility with polyethylene, the cap has excellent formability in the blended state, and the torque required to open the cap can be reduced compared to conventional methods.
[0022] The polypropylene used in the resin composition constituting the cap 20 preferably has a melt flow rate (temperature 230°C, load 21.18N) in the range of 3g / 10min or more and 20g / 10min or less. If it is within the above range, the cap 20 will have excellent moldability, sealing properties, and mechanical strength.
[0023] The polyethylene used in the resin composition constituting the cap 20 may be a resin composition mainly composed of high density polyethylene, medium density polyethylene, low density polyethylene, or linear low density polyethylene, or a combination of one, two, three, or four of high density polyethylene, medium density polyethylene, low density polyethylene, or linear low density polyethylene. The method of blending is not particularly limited, and dry blending or melt blending may be used.
[0024] The polyethylene used in the resin composition constituting the cap 20 has a density of 0.940 g / cm 3 More than 0.970g / cm 3 It is preferable that the content is in the following range. The above range is preferable from the viewpoints of compatibility with polypropylene, heat resistance of the cap, and drop strength in a low-temperature environment. Therefore, it is preferable that the resin composition constituting the cap 20 contains high-density polyethylene. Here, high-density polyethylene is defined as polyethylene having a density of 0.940 g / cm 3 More than 0.970g / cm 3 and refers to the polymerisation of ethylene by low pressure polymerization (gas phase polymerization using a Ziegler-Natta catalyst or liquid phase polymerization using a metallocene catalyst).
[0025] The polyethylene used in the resin composition constituting the cap 20 may be derived from fossil fuels, but may be derived from biomass, which is known as a carbon-neutral material, to reduce the environmental impact. Since the cap occupies a large mass ratio in the tube container, by molding the cap using biomass-derived polyethylene, the amount of fossil fuel used for the entire tube container can be significantly reduced, and the environmental impact can be reduced. Furthermore, biomass-derived polyethylene has a higher haze value than fossil fuel-derived polyethylene, and when light is irradiated onto the cap, the haze is 90% or more, and the cap has a higher reflectance, so that the cap can have a white, opaque appearance without adding a colorant to shield the contents from the outside.
[0026] Here, biomass-derived polyethylene is a monomer polymer containing biomass-derived ethylene. Since biomass-derived ethylene is used as the raw material monomer, the polymerized polyethylene is derived from biomass. The content of biomass-derived ethylene in the raw material monomer is preferably 50% by mass or more, more preferably 80% by mass or more. The raw material monomer may contain ethylene derived from fossil fuels, or may contain α-olefin monomers such as butylene, hexene, and octene. Even in such a case, the obtained polymer is called biomass polyethylene. When biomass-derived polyethylene is used, it may contain two or more polyolefins with different biomass degrees.
[0027] When the fossil fuel-derived polyethylene and the biomass-derived polyethylene are blended, the blending method is not particularly limited and may be dry blending or melt blending. When the two are blended, the blending ratio of the fossil fuel-derived polyethylene to the biomass-derived polyethylene is preferably 1:9 to 9:1, more preferably 2:8 to 8:2, in mass ratio.
[0028] For example, biomass-derived ethylene can be produced using biomass-derived ethanol as a raw material. In particular, it is preferable to use biomass-derived fermented ethanol obtained from a plant raw material. The plant raw material is not particularly limited, and any conventionally known plant can be used. Examples of the plant raw material include corn, sugarcane, beet, and manioc.
[0029] In this embodiment, the fermented ethanol derived from biomass refers to ethanol produced by contacting a culture solution containing a carbon source obtained from a plant raw material with an ethanol-producing microorganism or a product derived from its crushed material, and then purifying the ethanol. Conventionally known methods such as distillation, membrane separation, and extraction can be applied to purify ethanol from the culture solution. For example, a method of adding benzene, cyclohexane, etc., and removing water by azeotropy or membrane separation can be used.
[0030] In the present embodiment, a suitable example of biomass-derived polyethylene is SHA7260 (density: 0.955 g / cm) manufactured by Braskem. 3 , MFR: 20g / 10min, biomass content 94%, SHC7260 (density: 0.959g / cm 3 , MFR: 7.2g / 10min, biomass content 94%), SHD7255LSL (density: 0.954g / cm 3 , MFR: 4.5g / 10min, biomass content 94%, SGE7252 (density: 0.953g / cm 3 , MFR: 2.2 g / 10 min, biomass degree: 96%).
[0031] The biomass degree is the value of the C14 content obtained by a radiocarbon (C14) measurement method in accordance with ASTM-D6866. Carbon dioxide in the atmosphere contains a certain proportion of C14 (105.5 pMC), and it is known that the C14 content in plants that grow by absorbing carbon dioxide from the atmosphere, such as corn, is also about 105.5 pMC. It is also known that fossil fuels contain almost no C14. Therefore, the proportion of carbon derived from biomass can be calculated by measuring the proportion of C14 contained in the total carbon atoms in polyethylene. In the present invention, when the content of C14 in polyethylene is PC14, the content of carbon derived from biomass, Pbio, can be calculated as follows. Pbio(%)=PC14 / 105.5×100
[0032] In the blended polymer of polypropylene and polyethylene, the polyethylene is preferably used in an amount of 1 part by mass or more and 99 parts by mass or less, more preferably 10 parts by mass or more and 80 parts by mass or less, per 100 parts by weight of the total of polypropylene and polyethylene. When the blended amount of polyethylene is within the above range, the compatibility with polyethylene is excellent without modifying an existing mold, the formability of the cap 20 in the blended state is excellent, and the torque required to open the cap can be reduced compared to the conventional case. In addition, in the blended polymer of polypropylene and polyethylene, when the mass ratio of polypropylene is larger than the mass ratio of polyethylene, the polyethylene molecules are dispersed in the polypropylene molecules having a larger mass ratio. Therefore, the polyethylene molecules are dispersed in the polypropylene base material, and the appearance can be white and opaque.
[0033] The cap 20 can be manufactured by a conventionally known method using the above-mentioned resin composition, and can be molded integrally by, for example, a compression molding method or an injection molding method.
[0034] As described above, various additives may be added to the resin composition constituting the cap 20 within a range that does not impair the characteristics of the resin composition. Examples of additives that can be added include plasticizers, UV stabilizers, coloring inhibitors, matting agents, deodorants, flame retardants, weather resistance agents, antistatic agents, thread friction reducing agents, slip agents, mold release agents, antioxidants, ion exchange agents, and color pigments. These additives are preferably added in an amount of 0.5% by mass or more and 20% by mass or less, and more preferably 1% by mass or more and 10% by mass or less, based on the entire resin composition.
[0035] Next, the resin composition used in the head portion 11 of the tube container body 10 will be described.
[0036] The resin composition used in the head 11 of the tube container body 10 contains polyethylene as a main component. In this embodiment, the main component means that the head 11 may be formed using only polyethylene, or may contain various resins and additives other than polyethylene as long as the characteristics are not impaired.
[0037] The polyethylene used in the head 11 of the tube container body 10 has a density of 0.940 g / cm 3 or more, preferably 0.940 g / cm 3 More than 0.9670g / cm 3 It is obtained by polymerizing ethylene using a low-pressure polymerization method (gas phase polymerization using a Ziegler-Natta catalyst or liquid phase polymerization using a metallocene catalyst). The density of polyethylene is the value measured according to the method specified in Method A of JIS K7112-1980 after annealing as specified in JIS K6760-1995.
[0038] The melt flow rate (MFR) of the polyethylene is preferably 1 g / 10 min or more and 30 g / 10 min or less, more preferably 2 g / 10 min or more and 20 g / 10 min or less. By using a polyethylene having an MFR within the above range, when the head 11 is molded by injection molding or compression molding, the head 11 obtained can be molded exactly to the mold, and stable moldability can be achieved. The melt flow rate is a value measured by the method A specified in JIS K7210-1995 under the conditions of a temperature of 190° C. and a load of 21.18 N.
[0039] The polyethylene mentioned above may be derived from fossil fuels, but biomass-derived polyethylene, known as a carbon-neutral material, may be used to reduce the environmental burden. Since the head occupies a large mass ratio in the tube container, by molding the head using biomass-derived polyethylene, the amount of fossil fuel used for the entire tube container can be significantly reduced, and the environmental burden can be reduced. Furthermore, biomass-derived polyethylene has a higher haze value than fossil fuel-derived polyethylene, and when light is irradiated from the outside of the tube container, the haze is 90% or more, and it has a higher reflectance, so it can present a white, opaque appearance without adding a coloring agent to shield the contents from the outside. In addition, the head 11 of the tube container body 10 is comparable in physical properties such as mechanical properties to heads manufactured from conventional raw materials obtained from fossil fuels, so it can replace conventional heads.
[0040] From the viewpoint of reducing the environmental load, it is preferable to use only biomass-derived polyethylene, but in consideration of the manufacturing cost and the reuse of existing molds for producing caps made of polypropylene only, a blend of fossil fuel-derived polyethylene and the above-mentioned biomass-derived polyethylene may be used. When using biomass-derived polyethylene, it may contain two or more polyolefins with different biomass degrees. When blending fossil fuel-derived polyethylene and biomass-derived polyethylene, the mixing method is not particularly limited, and dry blending or melt blending may be used. When mixing the two, the mixing ratio of fossil fuel-derived polyethylene and biomass-derived polyethylene is preferably 1:9 to 9:1 in mass ratio, more preferably 2:8 to 8:2.
[0041] As long as the resin composition used in the head 11 of the tube container body contains the above-mentioned polyethylene as a main component, various additives may be added to the extent that the characteristics are not impaired. Examples of additives that can be added include plasticizers, UV stabilizers, color inhibitors, matting agents, deodorants, flame retardants, weather resistance agents, antistatic agents, thread friction reducers, slip agents, mold release agents, antioxidants, ion exchange agents, and color pigments. These additives are added in an amount of preferably 0.5% by mass to 20% by mass, more preferably 1% by mass to 10% by mass, based on the entire resin composition.
[0042] The head 11 can be manufactured by a conventionally known method using the above-mentioned resin composition, and can be molded integrally by, for example, a compression molding method or an injection molding method.
[0043] The tube container packaging material 30 constituting the trunk portion 12 of the tube container body 10 will be described below.
[0044] As shown in Fig. 3, the outer layer 31 and the inner layer 33 are provided on both sides of the intermediate layer 32. The outer layer 31 and the inner layer 33 are layers formed of a film of a heat-sealable resin that can be fused to each other by heat. Since the body 12 is manufactured by rolling the laminated sheet 30 and welding the overlapping ends, a film of a resin that can be melted by heating and fused to each other can be used. The material for forming the outer layer 31 and the inner layer 33 is not particularly limited as long as it is a resin that can be fused to each other by heat (heat-sealable resin). Specifically, examples of the resin include, in addition to the low-density polyethylene, linear low-density polyethylene, and high-density polyethylene described above, ethylene-α-olefin copolymer resins polymerized using a metallocene catalyst, ethylene-polypropylene random or block copolymer resins, polypropylene, ethylene-vinyl acetate copolymer (EVA) resin, ethylene-acrylic acid copolymer (EAA) resin, ethylene-ethyl acrylate copolymer (EEA) resin, ethylene-methacrylic acid copolymer (EMAA) resin, ethylene-methyl methacrylate copolymer (EMMA) resin, ionomer resin, heat-sealable ethylene-vinyl alcohol resin, and polyolefin resins such as copolymerized resins methylpentene resins, ethylene-propylene copolymers, methylpentene polymers, polybutene polymers, polyethylene, polypropylene, and cyclic olefin copolymers; acid-modified polyolefin resins obtained by modifying polyolefin resins with unsaturated carboxylic acids such as acrylic acid, methacrylic acid, maleic acid, maleic anhydride, fumaric acid, and itaconic acid; polyvinyl acetate resins, poly(meth)acrylic resins, polyvinyl chloride resins, and other resins. These may be used alone or in combination of two or more.
[0045] When polyethylene is used as the material for forming the outer layer 31 and the inner layer 33, a biomass-derived polyethylene resin may be used instead of a fossil fuel-derived polyethylene resin from the viewpoint of reducing the environmental load. As the biomass-derived polyethylene resin, the above-mentioned materials can be used, but as the polyethylene for film molding, one having a melt flow rate (MFR) of 0.1 g / 10 min or more and 10 g / 10 min or less can be preferably used. Examples of suitable biomass-derived low-density polyethylene include Braskem's SBC818 (density: 0.918 g / cm3, MFR: 8.1 g / 10 min, biomass degree 96%), SBF032HC (density: 0.923 g / cm3, MFR: 0.32 g / 10 min, biomass degree 95%), STN7006 (density: 0.924 g / cm3, MFR: 0.6 g / 10 min, biomass degree 95%), SEB853 (density: 0.923 g / cm3, MFR: 2.7 g / 10 min, biomass degree 95%), and SPB681 (density: 0.922 g / cm3, MFR: 3.8 g / 10 min, biomass degree 95%). A mixture of the above-mentioned biomass-derived polyethylene resin and a fossil fuel-derived polyethylene resin may also be used. By forming the outer layer 31 and the inner layer 33 using a resin material containing biomass-derived polyethylene, the amount of fossil fuel used to form the tube container body 10 can be further reduced, and carbon dioxide emissions can be reduced.
[0046] In this embodiment, the outer layer 31 and the inner layer 33 are each a single layer, but they may each be two or more layers. When the outer layer 31 and the inner layer 33 are each two or more layers, they may each have the same composition or different compositions.
[0047] The thickness of the outer layer 31 and the inner layer 33 is preferably 20 μm or more and 300 μm or less, and more preferably 30 μm or more and 250 μm or less.
[0048] The intermediate layer 32 has a function of supporting the laminated sheet 30 constituting the trunk portion 12, and can be made of any material capable of supporting the laminated sheet 30. For example, various resins such as polyester resins such as polyethylene terephthalate and polyethylene naphthalate, polyvinylidene chloride resins, polyvinyl alcohol resins, saponified ethylene-vinyl acetate copolymers, fluorine resins, polyacrylonitrile resins, polyamide resins, polyolefin resins such as polyethylene and polypropylene, and other resins, and metal foils such as aluminum foil can be used. In addition, the above-mentioned resins may be not only those derived from fossil fuels, but also those derived from biomass. For example, in addition to the above-mentioned polyethylene resin derived from biomass, biomass polyesters using ethylene glycol derived from biomass as a diol component, polylactic acid resins, cellophane, starch, cellulose, and the like can be used. Furthermore, the intermediate layer 32 may be two or more layers. When the intermediate layer 32 is two or more layers, each layer may have the same composition or different compositions.
[0049] The intermediate layer 32 may be a film made of the above-mentioned resin, but it is preferable to use a film stretched in a uniaxial or biaxial direction from the viewpoint of strength, etc. Hereinafter, the film made of the resin is also referred to as a base film.
[0050] The laminate sheet may have at least one other layer in addition to the outer layer 31, the intermediate layer 32, and the inner layer 33. Examples of the other layers include a gas barrier layer, a light-shielding layer, and a printed layer. When the laminate sheet has two or more other layers, the other layers may have the same composition or different compositions. Examples of the resin constituting the gas barrier layer include polyvinylidene chloride resins, polyvinyl alcohol resins, saponified ethylene-vinyl acetate copolymers, fluorine-based resins, polyacrylonitrile resins, and other resins. Examples of the resin having water vapor barrier properties include olefin resins such as polyethylene and polypropylene.
[0051] As the gas barrier layer, a metal foil such as aluminum foil may be provided, or a vapor-deposited layer of a metal such as aluminum, or a vapor-deposited layer of an inorganic oxide such as aluminum oxide or silicon oxide may be provided. A barrier coating film formed by coating a substrate film with a barrier coating agent such as polyvinylidene chloride or an acrylic acid resin may be used as an intermediate layer. When a metal foil or a vapor-deposited layer is provided on the surface of the substrate film, the surface of the substrate film may be previously subjected to a plasma treatment using an inert gas. Such a surface treatment improves the adhesion between the substrate film and the metal foil or vapor-deposited layer, and prevents delamination.
[0052] Examples of metals that can be used to form the deposition layer include deposited films of metals such as aluminum (Al), magnesium (Mg), tin (Sn), sodium (Na), titanium (Ti), lead (Pb), zirconium (Zr), yttrium (Y), gold (Au), and chromium (Cr).
[0053] Examples of inorganic oxides that can be used to form the vapor-deposited layer include silicon oxide, tin oxide, zinc oxide, indium oxide, titanium oxide, and aluminum oxide.
[0054] Examples of the method for forming the metal or inorganic oxide vapor deposition layer on one side of the resin film include physical vapor deposition methods (PVD method) such as vacuum deposition method, sputtering method, and ion plating method, and chemical vapor deposition methods (CVD method) such as plasma chemical vapor deposition method, thermal chemical vapor deposition method, and photochemical vapor deposition method. The thickness of the metal or inorganic oxide vapor deposition layer varies depending on the type of material used, but is preferably 5 nm to 200 nm, and more preferably is selected and formed within the range of 10 nm to 100 nm. More specifically, when an aluminum vapor deposition film is provided, the thickness is preferably 5 nm to 60 nm, and more preferably 10 nm to 45 nm.
[0055] In order to improve the gas barrier property, a vapor deposition layer of a metal or metal oxide as described above may be provided on a substrate film, and then a gas barrier coating film may be provided on the vapor deposition layer. 1n M(OR2) m (wherein, R1 and R2 represent an organic group having 1 to 8 carbon atoms, M represents a metal atom, n represents an integer of 0 or more, m represents an integer of 1 or more, and n+m represents the atomic valence of M), and either or both of a polyvinyl alcohol resin and an ethylene-vinyl alcohol copolymer, and further comprising a step of preparing a gas barrier composition by polycondensation through a sol-gel process in the presence of a sol-gel process catalyst, an acid, water, and an organic solvent; The film can be produced by a production process including, if necessary, a step of coating the gas barrier composition polycondensed by the sol-gel method via a surface that has been plasma-treated with oxygen gas to provide a coating film, and a step of heat-treating the base film provided with the coating film at 20°C to 180°C and at a temperature not higher than the melting point of the base film for 10 seconds to 10 minutes to form a gas barrier coating film of the gas barrier composition on the deposition layer provided on one side of the base film, if necessary, via a surface that has been plasma-treated with oxygen gas.
[0056] The general formula R for forming a gas barrier coating film 1n M(OR2) m As the alkoxide represented by the formula (I), at least one of a partial hydrolyzate of an alkoxide and a hydrolysis condensate of an alkoxide can be used. In addition, as the partial hydrolyzate of an alkoxide, it is not necessary that all of the alkoxy groups are hydrolyzed, and one in which one or more are hydrolyzed, or a mixture thereof may be used. Furthermore, as the hydrolysis condensate, a dimer or more of a partially hydrolyzed alkoxide, specifically a dimer to hexamer, is used.
[0057] The above general formula R 1n M(OR2)m In the alkoxide represented by the formula (I), silicon, zirconium, titanium, aluminum, and the like can be used as the metal atom represented by M. In the present invention, preferred metals include, for example, silicon and titanium. In the present invention, the alkoxide can be used alone or in the form of a mixture of two or more different metal atoms in the same solution.
[0058] In addition, the above general formula R 1n M(OR2) m In the alkoxide represented by the above general formula R, specific examples of the organic group represented by R1 include alkyl groups such as methyl, ethyl, n-propyl, i-propyl, n-butyl, i-butyl, sec-butyl, t-butyl, n-hexyl, n-octyl, and the like. 1n M(OR2) m In the alkoxide represented by the formula (I), specific examples of the organic group represented by R2 include a methyl group, an ethyl group, an n-propyl group, an i-propyl group, an n-butyl group, a sec-butyl group, etc. In the present invention, these alkyl groups may be the same or different in the same molecule.
[0059] As the polyvinyl alcohol resin and / or ethylene-vinyl alcohol copolymer forming the gas barrier coating film, the polyvinyl alcohol resin or the ethylene-vinyl alcohol copolymer can be used alone, or the polyvinyl alcohol resin and the ethylene-vinyl alcohol copolymer can be used in combination. In the present invention, by using either one or both of the polyvinyl alcohol resin and the ethylene-vinyl alcohol copolymer, the gas barrier coating film can be significantly improved in physical properties such as gas barrier properties, water resistance, weather resistance, etc. In particular, in the present invention, by using the polyvinyl alcohol resin and the ethylene-vinyl alcohol copolymer in combination, a laminate film can be formed that is significantly excellent in hot water resistance and gas barrier properties after hot water treatment in addition to the above gas barrier properties.
[0060] The outer layer 31, the intermediate layer 32, the inner layer 33, and other layers can be laminated to one another via an adhesive layer by dry lamination, or via an adhesive resin layer by melt extrusion lamination.
[0061] When two layers are bonded by dry lamination, the adhesive layer can be formed by applying an adhesive to the surface of the layer to be laminated and drying it. As the adhesive, for example, one-component or two-component curing or non-curing type vinyl, (meth)acrylic, polyamide, polyester, polyether, polyurethane, epoxy, rubber, and other solvent-based, water-based, or emulsion-type adhesives can be used. As a two-component curing type adhesive, a cured product of polyol and an isocyanate compound can be used. As a coating method of the above-mentioned adhesive for lamination, for example, it can be applied to the coating surface of the layer constituting the laminate by a direct gravure roll coating method, a gravure roll coating method, a kiss coating method, a reverse roll coating method, a Fountain method, a transfer roll coating method, or other methods.
[0062] The adhesive layer may be an adhesive resin layer used when bonding two layers together by a sand lamination method or a melt extrusion lamination method. Thermoplastic resins that can be used for the adhesive resin layer include polyethylene resins, polypropylene resins, cyclic polyolefin resins, copolymer resins, modified resins, or mixtures (including alloys) that contain these resins as the main components. Examples of polyolefin resins include the above-mentioned polyethylene, polypropylene, ethylene-α-olefin copolymers polymerized using a metallocene catalyst, random or block copolymers of ethylene and polypropylene, ethylene-vinyl acetate copolymer (EVA), ethylene-acrylic acid copolymer (EAA), ethylene-ethyl acrylate copolymer (EEA), ethylene-methacrylic acid copolymer (EMAA), ethylene-methyl methacrylate copolymer (EMMA), ethylene-maleic acid copolymer, and ionomer resins. In addition, in order to improve the adhesion between layers, acid-modified polyolefin resins obtained by modifying the above-mentioned polyolefin resins with unsaturated carboxylic acids such as acrylic acid, methacrylic acid, maleic acid, maleic anhydride, fumaric acid, and itaconic acid can be used. In addition, resins obtained by graft-polymerizing or copolymerizing unsaturated carboxylic acids, unsaturated carboxylic anhydrides, and ester monomers with polyolefin resins can be used. These materials can be used alone or in combination of two or more. Examples of the cyclic polyolefin resin include cyclic polyolefins such as ethylene-propylene copolymers, polymethylpentene, polybutene, and polynorbornene. These resins can be used alone or in combination. The above-mentioned polyethylene resin can be made using the above-mentioned biomass-derived ethylene as a monomer unit to further improve the biomass content.
[0063] When the adhesive resin layer is laminated by the melt extrusion lamination method, an anchor coat layer may be provided on the surface of the layer to be laminated by applying and drying an anchor coat agent. The anchor coat agent may be any resin having a heat resistance of 135°C or higher, such as a vinyl modified resin, an epoxy resin, a urethane resin, a polyester resin, or a polyethyleneimine. In particular, an anchor coat agent that is a cured product of a polyacrylic or polymethacrylic resin (polyol) having two or more hydroxyl groups in the structure and an isocyanate compound as a curing agent is preferably used. In addition, a silane coupling agent may be used in combination with this as an additive, and nitrocellulose may be used in combination to increase heat resistance.
[0064] The thickness of the anchor coat layer after drying is preferably 0.1 μm to 1 μm, more preferably 0.3 μm to 0.5 μm. The thickness of the adhesive layer after drying is preferably 1 μm to 10 μm, more preferably 2 μm to 5 μm. The thickness of the adhesive resin layer is preferably 5 μm to 50 μm, more preferably 10 μm to 30 μm.
[0065] The intermediate layer 32 may have various layer configurations depending on the type of contents to be filled in the tube container, the purpose of packaging, the packaging form, the distribution form, the sales form, and other conditions.
[0066] The body 12 is produced by rolling the laminated sheet into a cylindrical shape, overlapping the outer layer 31 and the inner layer 33 at both ends of the body 12 as shown in Fig. 2, and heat-sealing the overlapped portion to form a heat-sealed portion 17. The head 11 is connected to the upper part of one opening of the body 12. Note that the method of overlapping the outer layer 31 and the inner layer 33 at both ends of the body 12 is not limited to overlapping the outer layer 31 and the inner layer 33, and the inner layers 33 may be overlapped. Also, as described above, the body may be formed into a cylindrical body by inflation molding, and then the cylindrical body may be cut to a predetermined length to form a cylindrical body.
[0067] Heat sealing can be performed by a conventional method such as bar sealing, rotary roll sealing, belt sealing, impulse sealing, high frequency sealing, ultrasonic sealing, or flame sealing.
[0068] The method for connecting the body 12 to the head 11 having the above-mentioned pouring outlet 14 is not particularly limited. As an example, when the head is molded using a compression molding method or an injection molding method, one end of the cylindrical body is inserted into a mold used for molding the head 11, and a polyethylene resin composition is pressed into the mold, thereby molding the head 11 and joining it to one opening of the body 12, thereby forming the tube container body 10.
[0069] After the tube container body 10 is molded, the contents are filled from the other open end connected to the head 11 of the body 12, and the opening is welded to form the bottom seal 16. This makes it possible to obtain the tube container body 10 filled and packaged with the contents. The cap to be attached to the spout 14 is detachably attached by various methods, such as by screwing, according to the shape of the spout 14. EXAMPLES
[0070] The present invention will be described below based on examples, but the present invention is not limited to these.
[0071] (1) Preparation of packaging material 30 for tube containers The substrate film used was a biaxially oriented polyethylene terephthalate film (manufactured by Toyobo Co., Ltd., product name "EB512") having a thickness of 12 μm and having one side subjected to corona discharge treatment. Printing ink was applied to the corona discharge treated side by gravure printing so that the thickness when dried was 3 μm. Next, the printed surface was coated with a dry coating weight of 3 g / m 2A two-component curing urethane adhesive (manufactured by Rock Paint Co., Ltd., product name "RU-80 / H-5") was applied so that the thickness was 12 μm, and an aluminum-deposited biaxially oriented polyethylene terephthalate film (manufactured by Oike Materials Co., Ltd., product name "Tetlite EXC-B") with a thickness of 12 μm was laminated as a barrier layer. Furthermore, a 12 μm thick aluminum-deposited biaxially oriented polyethylene terephthalate film with a coating amount of 3 g / m2 when dried was laminated on the back side of the aluminum-deposited biaxially oriented polyethylene terephthalate film. 2 Apply a two-component curing urethane adhesive (manufactured by Rock Paint Co., Ltd., product name "RU-80 / H-5") so that the surface is A 150 μm-thick low-density polyethylene film (trade name "BCO-LZ27N" manufactured by Dai Nippon Printing Co., Ltd.) was laminated as a heat-sealable film to obtain a laminated sheet. Next, a coating amount of 3 g / m2 was applied on the biaxially stretched polyethylene terephthalate film on the front side of the laminate. 2 A two-component curing urethane adhesive (manufactured by Rock Paint Co., Ltd., product name "RU-80 / H-5") was applied so that the surface was covered with the adhesive, and then a 110 μm-thick low-density polyethylene film containing an antistatic agent (manufactured by Dai Nippon Printing Co., Ltd., product name "BCO-LZ27NAS") was laminated on top of the adhesive. The layer structure of the obtained tube container packaging material 30, from the outermost layer to the innermost layer, is low-density polyethylene film 110 μm / two-component curing urethane adhesive layer / biaxially oriented polyethylene terephthalate film 12 μm / two-component curing urethane adhesive layer / aluminum-vapor-deposited biaxially oriented polyethylene terephthalate 12 μm / two-component curing urethane adhesive layer / low-density polyethylene film 150 μm.
[0072] (2) Preparation of the cylindrical body The tube container packaging material 30 obtained as described above was processed into a slit with a width of 126.8 mm using a bobbin cutter, and both ends in the width direction were overlapped so that the overlap width was about 1.5 mm, and then the overlapped ends were heat-sealed at a heat seal temperature of 60° C. to 120° C. to obtain a cylindrical raw roll with a tube pasted on it. The obtained raw roll was cut in the length direction to a length of 160 mm to produce a cylindrical body portion that would become the body portion 12 of the tube container body 10.
[0073] (3) Head The cylindrical body 12 is attached to a mandrel for forming a tube container, and then a head 11 consisting of a truncated cone-shaped shoulder 13 and a cylindrical pouring outlet 14 connected to the shoulder 13 is attached to one end of the cylindrical body using high-density polyethylene (density 0.953 g / cm 3 A tubular container body 10 as shown in FIG. 1 was produced by injection molding at a temperature of 270° C. using a fluororesin (MFR 2.2 g / 10 min, manufactured by Braskem Corporation, product name "SGE7252"). The resulting tubular container body had a head outlet part with an outer diameter of φ11.4 mm, an inner diameter of φ8.9 mm, and a height of 16.5 mm, and a threaded part 15 was provided on the side of the outlet part 14. The threaded part 15 was provided with three turns (double thread) at intervals of 0.6 mm on the side of the outlet part, and the height of the threaded part was 1.0 mm. The outer diameter of the shoulder part was a major axis: 46.57 mm, and a minor axis: 31.65 mm.
[0074] (4) Cap A resin having the composition shown in Table 1 below was used in a mold capable of molding a cap 20 having a groove on the inner surface so as to screw into the spout 14 of the head 11, and the resin was injection molded at a temperature of 220°C to produce the cap 20. The density is a value determined by the gas displacement method (dry density meter: Accupyc H1340, manufactured by Shimadzu Corporation-Micromeritics) in accordance with JIS R1620 (1995). 3 The sample was cut to a size that could fit into a cell, and the entire amount was collected in the cell, and measurements were repeated five times to determine the average value. The values in Table 1 represent parts by mass. The outer diameter of the cap 20 was 46.2 mm long and 22.7 mm short.
[0075] [Capping test] 300 tube containers 1 were prepared, and the caps 20 were attached to the threaded portions provided on the spout portions 14 of the tube container bodies 10 using a capping machine. It was confirmed that there were no problems with the attachment of the caps 20.
[0076] As a result, in all of the caps 20, there was no problem in closing the caps 20.
[0077] [Opening torque] The cap 20 was spirally wound onto the spout 14 of the tube container body 10 obtained as described above, and then 50 g of hand cream was filled as the content from the other opening of the cylindrical body, and the opening of the cylindrical body was heat-sealed to produce a tube container 1 as shown in Figure 1. The cap 20 was closed with a set tightening torque of 14.7 N·cm. The torque required to open the cap 20 of the tube container 1 was then measured using a torque meter (manufactured by Nidec-Shimpo Corporation, model TNJ-5). The average value of the 10 measurement results was taken as the opening torque value. The results are shown in Table 1 below.
[0078] [Drop test] The tube container 1 was dropped vertically from a height of 1 m in a room temperature environment without acceleration so that the cap was facing down, and the container was visually checked for the presence or absence of the cap coming off or cracking. This evaluation was carried out 10 times, and an overall evaluation was made according to the following evaluation criteria. ◯: Cap removal or cap cracking was not observed even once. ×: Cap coming off or cap cracking was observed at least once. Furthermore, the tube container 1 was left in an environment of 3° C. for 12 hours, and then dropped vertically from a height of 1 m without acceleration so that the cap 20 was facing downward, and visually checked for the cap coming off or cracking. This evaluation was performed 10 times, and an overall evaluation was performed according to the following evaluation criteria. In addition, the tube container 1 was left in an environment at 3°C for one month, and then further left in an environment at room temperature, and then dropped vertically from a height of 1 m without acceleration so that the cap 20 was facing downward, and then a drop test evaluation similar to that described above was performed. This evaluation was performed three times. In addition, the tube container 1 was left in an environment at 3° C. for 2 months, and then left in an environment at room temperature, after which a drop test was performed in the same manner as above. This evaluation was performed three times, and evaluation was performed in the same manner as above. Furthermore, the tube container 1 was left in an environment at 3°C for 3 months, and then left in an environment at room temperature, and then the drop test was performed in the same manner as above. This evaluation was performed three times and evaluated in the same manner as above. The evaluation results are shown in Table 1 below.
[0079] [Leakage] The cap 20 was spirally screwed onto the outlet 14 of the tube container body 10, and then 100 ml of a 1:1 water:ethanol solution colored with methylene blue was poured into the other opening of the cylindrical body, and the opening of the cylindrical body was then heat-sealed to produce a tube container 1 as shown in Figure 1. The set tightening torque (positive torque) when closing the cap 20 was 60.0 N·cm. The set torque (negative torque) when opening the cap 20 was 35.0 N·cm. Next, the tube container 1 was left in a room temperature environment for 24 weeks, and the contents were visually checked every day for leakage. The evaluation criteria for leakage were as follows. ○: No leakage of contents from the cap was observed even after 2 weeks. ×: Leakage of contents from the cap was observed within 2 weeks. The evaluation results are shown in Table 1 below.
[0080] [Haze value] The haze value was measured for the caps of Example 1 and Comparative Example. Specifically, it was measured by the following method using a haze meter "HM-150" manufactured by Murakami Color Research Laboratory Co., Ltd. That is, the ratio of diffuse transmitted light to the total transmitted light when the cap was irradiated with visible light was measured by applying the light perpendicularly to the mat-forming layer 1 on the outermost surface of the laminate. The haze is expressed as scattered light / total light transmitted light×100(%). The evaluation results are shown in Table 1 below.
[0081] [Table 1]
[0082] The resin abbreviations in Table 1 represent the following resins. Petrochemical PP is polypropylene, PM921M (density 0.900 (g / cm) manufactured by Sunallomer Co., Ltd. 3 ), MFR25 (g / 10 min). Bio-HDPE is Braskem's high-density polyethylene, SHA7260 (density 0.955 (g / cm 3 ), MFR20 (g / 10 min).
[0083] From the above evaluation results, it was found that the opening torque value of the caps 20 of the tube containers 1 in Examples 1 to 3 could be kept lower than that of the polypropylene cap in Comparative Example 1. Moreover, it was found that the caps 20 of Examples 1 to 3 had no problems with plugging properties and were excellent in sealing properties. Furthermore, since the cap 20 of Example 1 has a higher bio content than Comparative Example 1 and a higher haze value than the cap of Comparative Example 1, when light is irradiated from the outside of the cap, the haze is 90% or more and has a higher reflectance, and it is found that the cap has a white, opaque appearance without adding a colorant to shield the contents from the outside. [Explanation of symbols]
[0084] 1 tube container 10 Tube container body 11 Head 12 Torso 13 Shoulder 14 Spout part 15 Screw part 16 Bottom seal 17 Heat seal section 20 Cap 30 Packaging material for tube containers (laminated sheet) 31 Outer layer 32 Middle Class 33 Inner layer 34 Barrier Layer
Claims
1. A tube container comprising a tube container body having a head portion having a pouring outlet and a body portion connected to the head portion, and a cap that is detachably attached to the pouring outlet of the tube container body to close the pouring outlet, The spout portion of the tube container body contains high-density polyethylene as a main component, The cap comprises a blend polymer of polypropylene and high density polyethylene; The blend polymer has a blending ratio of the polypropylene and the high-density polyethylene of 70:30 to 25:75 by mass ratio, The density of the blend polymer is 0.915 g / cm 3 0.930g / cm or more 3 A tube container characterized in that:
2. 2. The tube container according to claim 1, wherein the polyethylene constituting the cap contains biomass-derived polyethylene obtained by polymerizing a monomer containing biomass-derived ethylene.
3. 3. The tube container according to claim 1, wherein the polyethylene constituting the head portion of the tube container body comprises biomass-derived polyethylene obtained by polymerizing a monomer containing ethylene derived from biomass.
Citation Information
Patent Citations
Pull-open cap with hinge
JP1990045362A
Multi-layer tubular container
JP1998001149A
Laminate material for forming laminated tube container and laminated tube container using it
JP1998166530A
Cap made of resin which can be heat-sterilized
JP2002068282A
Container-sealed assembly
JP2017218213A