Toner manufacturing method
The toner manufacturing method addresses the challenge of achieving fixability and storage stability by using a specific combination of polyester resin A and prepolymer B with controlled acid values, ensuring compatibility and stability through phase inversion emulsification.
Patent Information
- Application Number
- JP2021066336
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-04-09
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2041-04-09
AI Technical Summary
Existing toner manufacturing methods using phase inversion emulsification struggle to achieve both fixability and storage stability, with issues arising from the use of prepolymers that generate coarse particles and affect particle size distribution and stability.
A toner manufacturing method involving the preparation of a solution with polyester resin A and prepolymer B in an organic solvent, followed by phase inversion emulsification and coagulation, where the acid value of polyester resin A and prepolymer B satisfies A>B>5, ensuring the prepolymer does not have isocyanate groups, to enhance fixability and storage stability.
The method achieves both fixability and storage stability in toner manufacturing, improving the degree of coloring and fixing properties at high temperatures.
Smart Images

Figure 0007567635000001 
Figure 0007567635000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a toner. [Background technology]
[0002] In recent years, there has been a demand for toners that have a reduced environmental impact. To meet this demand, for example, reductions in power consumption through improvements in the low-temperature fixing properties of the toner itself, and reductions in the amounts of energy and chemicals used in the toner manufacturing process are being considered.
[0003] As a method for improving the low-temperature fixing property of a toner, a method for lowering the glass transition temperature or softening point of a resin, a method for adding a crystalline resin, etc. are widely known. However, since lowering the thermal properties of a toner deteriorates the fixing property at high temperatures, a method for adding a polymer resin to maintain the fixing property at high temperatures, or a method for adding a prepolymer during production and polymerizing it after forming toner particles, etc., are used. In addition, a pulverization method was used as a manufacturing method for toner, but due to the large amount of energy used in the production and the trend toward smaller toner particles, chemical toners such as suspension polymerization are becoming mainstream. Summary of the Invention [Problem to be solved by the invention]
[0004] As a method for reducing the amount of chemicals used during toner production, there is a phase inversion emulsification method that can reduce the amount of surfactant. As mentioned above, as a method for maintaining the fixing property at high temperatures, there is a method for adding a prepolymer during production and polymerizing it after the toner particles are formed. It is considered that by combining these methods to produce a toner, it is possible to produce a toner with good fixing property while reducing the amount of surfactant used. For example, Patent Documents 1 and 2 have been proposed. However, the toner produced by such a method has a problem in that it is not possible to achieve both fixability and storage stability.
[0005] Therefore, an object of the present invention is to provide a method for producing a toner using a phase inversion emulsification method, which can achieve both good fixability and good storage stability. [Means for solving the problem]
[0006] In order to solve the above problems, the method for producing a toner of the present invention comprises the steps of: a) preparing a solution by dissolving or dispersing a polyester resin A and a prepolymer B in an organic solvent; b) adding water to the solution to effect phase inversion emulsification to prepare an oil-in-water dispersion; c) aggregating the oil-in-water dispersion, The prepolymer B does not have an isocyanate group, The acid value [mgKOH / g] of the polyester resin A and the prepolymer B is A>B>5 The present invention is characterized in that: Effect of the Invention
[0007] According to the present invention, it is possible to provide a method for producing a toner using a phase inversion emulsification method, which can achieve both good fixability and good storage stability. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] The toner manufacturing method according to the present invention will be described below. Note that the present invention is not limited to the following embodiments, and may be modified, added, modified, deleted, or otherwise altered within the scope of what a person skilled in the art can conceive, and any embodiment is within the scope of the present invention as long as it exhibits the functions and effects of the present invention.
[0009] In the conventional technology, when a prepolymer is added to an oil phase and a toner is produced by phase inversion emulsification, there is a problem that fixability and storage stability cannot be achieved at the same time. As a result of examining the reason for this, it is considered that the cause is that when a prepolymer is added to an oil phase and a toner is produced by phase inversion emulsification, coarse particles caused by the prepolymer are generated in the resulting emulsion. It is presumed that such coarse particles affect the particle size distribution of the final toner and affect the coloring degree. In addition, when a metal salt is added as a flocculant in the flocculation process, the prepolymer does not form metal crosslinks, so it is presumed that it affects storage stability and high-temperature fixability, and fixability and storage stability cannot be achieved at the same time. It is presumed that both of these problems are caused by the acid value of the prepolymer being too low.
[0010] Therefore, the present inventors conducted further investigations and arrived at the present invention. The method for producing the toner of the present invention comprises the steps of: a) preparing a solution by dissolving or dispersing a polyester resin A and a prepolymer B in an organic solvent; b) adding water to the solution to effect phase inversion emulsification to prepare an oil-in-water dispersion; c) aggregating the oil-in-water dispersion, The prepolymer B does not have an isocyanate group, The acid value [mgKOH / g] of the polyester resin A and the prepolymer B is A>B>5 The present invention is characterized in that:
[0011] According to the present invention, a method for producing a toner that can achieve both fixability and storage stability can be provided. In addition, when a colorant is used, the degree of coloring can be improved.
[0012] (Step a: Dissolution solution preparation step) In step a (solution preparation step), a solution is prepared by dissolving or dispersing polyester resin A and prepolymer B in an organic solvent. In addition to the above, a colorant or the like may be used in the solution preparation step. The solution may be referred to as an oil phase, and the solution preparation step may be referred to as an oil phase preparation step. In the following description, the solution is mainly referred to as an oil phase.
[0013] The oil phase may be prepared by gradually adding the resin, colorant, etc. to the organic solvent while stirring the organic solvent, and dissolving or dispersing the resin, colorant, etc. In the case of dispersion, a known dispersing machine, for example, a bead mill or a disk mill, may be used.
[0014] In the present invention, the acid value [mgKOH / g] of the polyester resin A and prepolymer B used in the oil phase preparation process satisfies A>B>5. By using such prepolymer B, coarsening of the prepolymer during phase inversion emulsification can be suppressed, and in the aggregation process, for example, the metal salt of the flocculant and prepolymer B crosslink to improve both fixability and storage stability. In addition, by using such polyester resin A and prepolymer B, it is possible to improve the degree of coloration and fixability at high temperatures.
[0015] On the other hand, if the acid value of prepolymer B is 5 mgKOH / g or less, coarse particles due to the prepolymer are generated, and both fixability and storage stability cannot be achieved, and particularly good results cannot be obtained in terms of high-temperature fixability and heat-resistant storage stability. If the acid value of polyester resin A and the acid value of prepolymer B are A≦B, environmental stability may be impaired. If the acid value of polyester resin A is A≦5, it is not emulsified and cannot be made into a toner.
[0016] The acid value [mgKOH / g] of polyester resin A and prepolymer B is A>B>10 In this case, the fixing property and the storage stability can be improved.
[0017] The acid values of the polyester resin A and the prepolymer B are measured in accordance with JIS K0070.
[0018] The glass transition temperature Tg [℃] of polyester resin A and prepolymer B is A>0>B It is preferable that the above condition is satisfied. In this case, the fixing property and the storage property can be improved. The method for measuring Tg and the like will be described later.
[0019] <Polyester resin A> When used as a toner for developing electrostatic latent images in electrophotography, good fixability can be obtained by using a resin having a polyester skeleton. Resins having a polyester skeleton include polyester resins and block polymers of polyester and resins having other skeletons, and the use of a polyester resin can improve the uniformity of the resulting colored resin particles. The polyester resin used in the oil phase preparation process is called polyester resin A.
[0020] Examples of the polyester resin A include ring-opening polymerization products of lactones, condensation polymerization products of hydroxycarboxylic acids, and polycondensation products of polyol (1) and polycarboxylic acid (2). From the viewpoint of freedom in design, polycondensation products of polyol and polycarboxylic acid are preferred.
[0021] The weight average molecular weight of the polyester resin A is preferably from 1000 to 30000, more preferably from 3000 to 15000, and further preferably from 5000 to 12000. If it is less than 1000, the heat resistant storage stability may deteriorate, and if it exceeds 30000, the low temperature fixability as a toner for developing an electrostatic latent image may deteriorate.
[0022] The glass transition temperature Tg of the polyester resin A is preferably 35 to 80° C., more preferably 40 to 70° C., and even more preferably 45 to 65° C. If the temperature is less than 35° C., the resulting colored resin particles may deform when placed in a high-temperature environment such as midsummer, or the colored resin particles may stick to each other and not be able to behave as particles as they should. If the temperature exceeds 80° C., the colored resin particles may not have good fixability when used as a toner for developing electrostatic latent images.
[0023] <<Polyol>> The polyol (1) may be a diol (1-1) or a trihydric or higher polyol (1-2). Preferably, (1-1) is used alone or a mixture of (1-1) and a small amount of (1-2). Examples of the diol (1-1) include alkylene glycols (ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,4-butanediol, 1,6-hexanediol, etc.); alkylene ether glycols (diethylene glycol, triethylene glycol, dipropylene glycol, polyethylene glycol, polypropylene glycol, polytetramethylene ether glycol, etc.); alicyclic diols (1,4-cyclohexanedimethanol, hydrogenated bisphenol A, etc.); bisphenols (bisphenol A, bisphenol F, bisphenol S, etc.); alkylene oxides of the above alicyclic diols (ethylene oxide, propylene oxide, butylene oxide, side, etc.) adducts; 4,4'-dihydroxybiphenyls such as 3,3'-difluoro-4,4'-dihydroxybiphenyl; bis(hydroxyphenyl)alkanes such as bis(3-fluoro-4-hydroxyphenyl)methane, 1-phenyl-1,1-bis(3-fluoro-4-hydroxyphenyl)ethane, 2,2-bis(3-fluoro-4-hydroxyphenyl)propane, 2,2-bis(3,5-difluoro-4-hydroxyphenyl)propane (also known as tetrafluorobisphenol A), and 2,2-bis(3-hydroxyphenyl)-1,1,1,3,3,3-hexafluoropropane; bis(4-hydroxyphenyl)ethers such as bis(3-fluoro-4-hydroxyphenyl)ether; Examples of the bisphenols include alkylene oxide (ethylene oxide, propylene oxide, butylene oxide, etc.) adducts.
[0024] Among these, preferred are alkylene glycols having 2 to 12 carbon atoms and alkylene oxide adducts of bisphenols, and particularly preferred are alkylene oxide adducts of bisphenols and their combined use with alkylene glycols having 2 to 12 carbon atoms.
[0025] Examples of the trihydric or higher polyol (1-2) include trihydric to octahydric or higher polyhydric aliphatic alcohols (glycerin, trimethylolethane, trimethylolpropane, pentaerythritol, sorbitol, etc.); trihydric or higher phenols (trisphenol PA, phenol novolac, cresol novolac, etc.); and alkylene oxide adducts of the above trihydric or higher polyphenols.
[0026] <<Polycarboxylic acid>> The polycarboxylic acid (2) may be a dicarboxylic acid (2-1) or a tri- or higher polycarboxylic acid (2-2). Preferably, (2-1) is used alone or a mixture of (2-1) and a small amount of (2-2).
[0027] Examples of the dicarboxylic acid (2-1) include alkylene dicarboxylic acids (succinic acid, adipic acid, sebacic acid, etc.); alkenylene dicarboxylic acids (maleic acid, fumaric acid, etc.); aromatic dicarboxylic acids (phthalic acid, isophthalic acid, terephthalic acid, naphthalene dicarboxylic acid, etc.), 3-fluoroisophthalic acid, 2-fluoroisophthalic acid, 2-fluoroterephthalic acid, 2,4,5,6-tetrafluoroisophthalic acid, 2,3,5,6-tetrafluoroterephthalic acid, 5-trifluoro Examples of such dicarboxylic acids include methylisophthalic acid, 2,2-bis(4-carboxyphenyl)hexafluoropropane, 2,2-bis(3-carboxyphenyl)hexafluoropropane, 2,2'-bis(trifluoromethyl)-4,4'-biphenyldicarboxylic acid, 3,3'-bis(trifluoromethyl)-4,4'-biphenyldicarboxylic acid, 2,2'-bis(trifluoromethyl)-3,3'-biphenyldicarboxylic acid, and hexafluoroisopropylidenediphthalic anhydride. Among these, preferred are alkenylene dicarboxylic acids having 4 to 20 carbon atoms and aromatic dicarboxylic acids having 8 to 20 carbon atoms.
[0028] Examples of the trivalent or higher polycarboxylic acid (2-2) include aromatic polycarboxylic acids having 9 to 20 carbon atoms (trimellitic acid, pyromellitic acid, etc.). The polycarboxylic acid (2) may be an acid anhydride or a lower alkyl ester (methyl ester, ethyl ester, isopropyl ester, etc.) of the above-mentioned compounds, which may be reacted with the polyol (1).
[0029] The ratio of polyol to polycarboxylic acid, expressed as the equivalent ratio [OH] / [COOH] of the hydroxyl group [OH] to the carboxyl group [COOH], is usually 2 / 1 to 1 / 2, preferably 1.5 / 1 to 1 / 1.5, and more preferably 1.3 / 1 to 1 / 1.3.
[0030] <Prepolymer B> The prepolymer B (also called reactive precursor) used in the oil phase preparation process does not have an isocyanate group. If the prepolymer B has an isocyanate group, it will not crosslink with the metal, and therefore the upper limit of fixation and storage stability will not be satisfied.
[0031] To say that prepolymer B does not have an isocyanate group, it can be determined from the material formulation (type, amount added, etc.). In addition, for example, viscoelasticity measurement using a rheometer device or quantification of the gel amount of ethyl acetate or MEK insoluble matter using the Soxhlet extraction method may be performed to determine the absence of an isocyanate group. The G' at the high temperature side of the viscoelasticity measurement and the gel amount by Soxhlet extraction are carboxylic acid-terminated prepolymer that crosslinks with metal > isocyanate-terminated prepolymer that does not crosslink with metal.
[0032] The prepolymer B may be a polyester having a group capable of reacting with an active hydrogen group. Examples of the group capable of reacting with an active hydrogen group include an isocyanate group, an epoxy group, a carboxylic acid, and an acid chloride group. Among these, a carboxylic acid is preferred because it can be crosslinked with the metal salt of the flocculant. The reactive precursor may have a branched structure provided by at least one of a trivalent or higher alcohol and a trivalent or higher carboxylic acid.
[0033] Examples of polyester resins containing a group capable of reacting with an active hydrogen group include a reaction product of a polyester resin having an active hydrogen group and a polyisocyanate. The polyester resin having an active hydrogen group is obtained, for example, by polycondensation of a diol, a dicarboxylic acid, and at least one of a trivalent or higher alcohol and a trivalent or higher carboxylic acid. The trivalent or higher alcohol and the trivalent or higher carboxylic acid impart a branched structure to the polyester resin containing an isocyanate group.
[0034] Examples of the diol include aliphatic diols such as ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,4-butanediol, 2-methyl-1,3-propanediol, 1,5-pentanediol, 3-methyl-1,5-pentanediol, 1,6-hexanediol, 1,8-octanediol, 1,10-decanediol, and 1,12-dodecanediol; diethylene glycol, triethylene glycol, dipropylene glycol, polyethylene glycol, polypropylene glycol, and polytetramethyl ether. Examples of the alkylene oxide adducts include diols having an oxyalkylene group, such as ethylene glycol; alicyclic diols, such as 1,4-cyclohexanedimethanol and hydrogenated bisphenol A; alicyclic diols to which alkylene oxides, such as ethylene oxide, propylene oxide and butylene oxide, have been added; bisphenols, such as bisphenol A, bisphenol F and bisphenol S; and alkylene oxide adducts of bisphenols, such as bisphenols to which alkylene oxides, such as ethylene oxide, propylene oxide and butylene oxide, have been added.
[0035] Among these, from the viewpoint of controlling the glass transition temperature Tg of the prepolymer B to 20° C. or less, it is preferable to use an aliphatic diol having 3 to 10 carbon atoms, such as 1,2-propylene glycol, 1,3-propylene glycol, 1,4-butanediol, 2-methyl-1,3-propanediol, 1,5-pentanediol, or 3-methyl-1,5-pentanediol, and it is more preferable that these account for 50 mol % or more of the alcohol components in the resin. These diols may be used alone or in combination of two or more.
[0036] The prepolymer B is preferably an amorphous resin, and the melt viscosity during fixing is reduced by providing steric hindrance to the resin chain, which makes it easier to achieve low-temperature fixing properties. For this reason, the main chain of the aliphatic diol preferably has a structure represented by the following general formula (1).
[0037] [ka]
[0038] [In the formula, R1 and R2 each independently represent a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, and n represents an odd number from 3 to 9. However, in the n repeating units, R1 and R2 may be the same or different.]
[0039] Here, the main chain of the aliphatic diol in the present invention refers to a carbon chain that connects two hydroxyl groups of the aliphatic diol with the shortest number of carbon atoms. When the carbon number of the main chain is odd, the crystallinity decreases due to the odd-even nature, which is preferable. In addition, when the main chain has at least one alkyl group having 1 to 3 carbon atoms in the side chain, the interaction energy between the main chain molecules decreases due to the steric nature, which is more preferable.
[0040] Examples of the dicarboxylic acid include aliphatic dicarboxylic acids such as succinic acid, adipic acid, sebacic acid, dodecanedioic acid, maleic acid, and fumaric acid; and aromatic dicarboxylic acids such as phthalic acid, isophthalic acid, terephthalic acid, and naphthalenedicarboxylic acid. In addition, anhydrides, lower (1 to 3 carbon atoms) alkyl esters, and halides of these may be used. Among these, from the viewpoint of controlling the Tg of the prepolymer B to 20° C. or less, aliphatic dicarboxylic acids having 4 to 12 carbon atoms are preferred, and it is more preferred to use them in an amount of 50% by mass or more of the carboxylic acid component in the resin. These dicarboxylic acids may be used alone or in combination of two or more.
[0041] Examples of the trihydric or higher alcohol include trihydric or higher aliphatic alcohols such as glycerin, trimethylolethane, trimethylolpropane, pentaerythritol, and sorbitol; trihydric or higher polyphenols such as trisphenol PA, phenol novolac, and cresol novolac; and alkylene oxide adducts of trihydric or higher polyphenols, such as those obtained by adding alkylene oxides such as ethylene oxide, propylene oxide, and butylene oxide to trihydric or higher polyphenols.
[0042] Examples of the trivalent or higher carboxylic acid include trivalent or higher aromatic carboxylic acids, and particularly preferred are trivalent or higher aromatic carboxylic acids having 9 to 20 carbon atoms, such as trimellitic acid and pyromellitic acid. In addition, anhydrides, lower (carbon number 1 to 3) alkyl esters, and halides of these may also be used.
[0043] <Organic solvent> The organic solvent can be appropriately selected, and for example, a volatile organic solvent with a boiling point of less than 100° C. is preferred from the viewpoint of ease of removal in a subsequent step. Examples of such organic solvents include toluene, xylene, benzene, carbon tetrachloride, methylene chloride, 1,2-dichloroethane, 1,1,2-trichloroethane, trichloroethylene, chloroform, monochlorobenzene, dichloroethylidene, methyl acetate, ethyl acetate, methyl ethyl ketone, methyl isobutyl ketone, methanol, ethanol, and isopropyl alcohol, which can be used alone or in combination of two or more kinds.
[0044] When the resin to be dissolved or dispersed in the organic solvent is a resin having a polyester skeleton, it is preferable to use an ester-based solvent such as methyl acetate, ethyl acetate, or butyl acetate, or a ketone-based solvent such as methyl ethyl ketone or methyl isobutyl ketone. In this case, the solubility can be increased. Among these, methyl acetate, ethyl acetate, and methyl ethyl ketone, which have high solvent removability, are particularly preferable.
[0045] <Coloring agent> As the colorant used in the present invention, known dyes and pigments can be used, for example, carbon black, nigrosine dye, iron black, naphthol yellow S, Hansa yellow (10G, 5G, G), cadmium yellow, yellow iron oxide, yellow ochre, yellow lead, titanium yellow, polyazo yellow, oil yellow, Hansa yellow (GR, A, RN, R), pigment yellow L, benzidine yellow (G, GR), permanent yellow (NCG), Balkan fast yellow (5G, R), tartrazine lake, quinoline yellow lake, anthrazan yellow BGL, iridium yellow, etc. Soindolinone Yellow, Bengala, Red Lead, Cinnabar, Cadmium Red, Cadmium Mercury Red, Antimony Vermilion, Permanent Red 4R, Para Red, Phaysee Red, Parachlor Orthonitroaniline Red, Lithol Fast Scarlet G, Brilliant Fast Scarlet, Brilliant Kanmin BS, Permanent Red (F2R, F4R, FRL, FRLL, F4RH), Fast Scarlet VD, Belkan Fast Rubin B, Brilliant Scarlet G, Lithol Rubin GX, Permanent Red F5R, Brilliant Carmine 6B, Pogment Scarlet 3B, Bordeaux 5B, Toluidine Maroon, Permanent Bordeaux F2K, Helio Bordeaux BL, Bordeaux 10B, Bon Maroon Light, Bon Maroon Medium, Eosin Lake, Rhodamine Lake B, Rhodamine Lake Y, Alizarin Lake, Thioindigo Red B, Thioindigo Maroon, Oil Red, Quinacridone Red, Pyrazolone Red, Polyazo Red, Chrome Vermilion, Benzidine Orange, Perinone Orange, Oil Orange, Cobalt Blue, Cerulean Blue, Alkaline Blue Lake, Peacock Blue Lake, Victoria Blue Lake, Metal-free Phthalocyanine Blue, Phthalocyanine Blue, Fast Sky Blue, Indanthrene Blue (RS, BC), Indigo, Ultramarine Blue, Prussian Blue, Anthraquinone Blue, Fast Violet B, Methyl Violet Lake, Cobalt Purple, Manganese Purple, Dioxane Violet, Anthraquinone Violet, Chrome Green, Zinc Green, Chromium Oxide, Pyridian, Emerald Green, Pigment Green B, Naphthol Green B, Green Gold, Acid Green Lake,Malachite green lake, phthalocyanine green, anthraquinone green, titanium oxide, zinc oxide, lithopone and mixtures thereof can be used.
[0046] Regarding the colorant, a master batch may be prepared by kneading the colorant with a resin, and the master batch may be dissolved or dispersed in an organic solvent together with the polyester resin A and the prepolymer B to prepare the oil phase.
[0047] The resin used for preparing the master batch can be appropriately selected, but it is preferable that it is a resin that is soluble in an organic solvent and insoluble or almost insoluble in water. Examples of the resin used include polystyrene, styrene-acrylic copolymer, polyvinyl chloride, polyvinyl acetate, polymethacrylic acid ester, polymethyl acrylate, polyacrylic acid ester, polyacrylonitrile, epoxy resin, polyethylene, polyurethane, polyester, polyethylene terephthalate, polyamide, paraffin wax, etc. These may be used alone or in combination. From the viewpoint of obtaining good fixability, polyester resin is preferable.
[0048] The master batch can be prepared by kneading the above-mentioned colorant and the above-mentioned resin. For example, a general kneader such as a twin-screw extrusion kneader, a three-roll mill, or a lab blast mill can be used for the kneading process. An internal additive may be added during the kneading process. It is preferable to heat the kneading process, and the heating conditions can be appropriately set.
[0049] The ratio of the resin and the colorant in preparing the master batch can be appropriately selected.
[0050] <Charge control agent> In addition to the above, a charge control agent and the like may be added to the oil phase. Any of the known charge control agents can be used, such as nigrosine dyes, triphenylmethane dyes, chromium-containing metal complex dyes, molybdic acid chelate pigments, rhodamine dyes, alkoxy amines, quaternary ammonium salts (including fluorine-modified quaternary ammonium salts), alkylamides, phosphorus simple substance or compounds, tungsten simple substance or compounds, fluorine-based activators, metal salicylic acid salts, and metal salts of salicylic acid derivatives.
[0051] Specifically, for example, the nigrosine dye Bontron 03, the quaternary ammonium salt Bontron P-51, the metal-containing azo dye Bontron S-34, the oxynaphthoic acid metal complex E-82, the salicylic acid metal complex E-84, the phenol condensate E-89 (all manufactured by Orient Chemical Industry Co., Ltd.), the quaternary ammonium salt molybdenum complexes TP-302 and TP-415 (all manufactured by Hodogaya Chemical Co., Ltd.), the quaternary ammonium salt Copy Charge PSY VP2038, the triphenylmethane derivative Copy Blue PR, the quaternary ammonium salt Copy Charge NEG VP2036, and Copy Charge NX. Examples of suitable pigments include VP434 (all manufactured by Hoechst), LRA-901, the boron complex LR-147 (manufactured by Nippon Carlit), copper phthalocyanine, perylene, quinacridone, azo pigments, and other polymeric compounds having functional groups such as sulfonic acid groups, carboxyl groups, and quaternary ammonium salts.
[0052] The charge control agent may be used in an amount that allows the agent to exhibit its performance and does not impair fixability, etc. When contained in the toner, the amount is preferably 0.5 to 5 mass % and more preferably 0.8 to 3 mass % in the toner.
[0053] <Neutralization process> In the oil phase preparation step, the master batch is dissolved in an organic solvent to obtain an oil phase, and the oil phase may then be neutralized with an alkaline aqueous solution, such as an aqueous ammonia solution.
[0054] (Step b: Water phase preparation step) In step b (aqueous phase preparation step), an organic solvent and water are mixed to prepare an aqueous phase. By going through the step of mixing an organic solvent and water to prepare an aqueous phase, it is possible to prevent the conditions at the time of emulsification from changing due to the solvent dissolving into water when the aqueous phase and oil phase are dissolved, and it is possible to prepare sharp nano-sized particles. Furthermore, the particle size distribution of the toner is also sharp, and the reproducibility of fine lines in images can be improved. It is not important to prepare the aqueous phase or the solution first.
[0055] The organic solvent used in preparing the aqueous phase can be appropriately selected, and for example, the organic solvents listed in step a can be used. In particular, it is preferable that the organic solvent in the dissolution preparation step is the same as the organic solvent in the aqueous phase preparation step. By using the same organic solvent, it is possible to minimize the variation caused by the dissolution of the solvent into water during emulsification.
[0056] Furthermore, the organic solvent in step a and step b is preferably ethyl acetate or methyl ethyl ketone. In this case, the advantages of using the same organic solvent in step a and step b are obtained, and the solvent removal is high, and the selectivity of materials when preparing a master batch or a solution is improved, which is more preferable.
[0057] The mixing ratio of the organic solvent and water can be appropriately selected. It is preferable to prepare an aqueous solution in which the amount of the dissolved organic solvent is 80% or more of the saturated solubility amount by using the organic solvent and water. By making the amount of the organic solvent 80% or more of the saturated solubility amount, the amount of the organic solvent eluted from the oil phase to the aqueous phase can be reduced.
[0058] The aqueous phase may contain, in addition to the above, a surfactant, such as sodium dodecyl sulfate.
[0059] (Step c: Phase inversion emulsification step) In step c (phase inversion emulsification step), the aqueous phase is added to the solution to effect phase inversion emulsification to produce an oil-in-water dispersion. By going through the step of adding the aqueous phase to the solution to invert the phase from the water-in-oil dispersion to the oil-in-water dispersion, it becomes possible to perform granulation with a reduced amount of surfactant used.
[0060] <Solvent removal process> In the step c (phase inversion emulsification step) in this embodiment, a solvent removal step may be carried out. The solvent removal step may be included in the emulsion phase inversion step, or may be separate from the emulsion phase inversion step.
[0061] In order to remove the organic solvent from the oil-in-water dispersion (also called the fine particle dispersion or colored fine particle dispersion), for example, a method can be adopted in which the temperature is gradually raised while stirring the entire system, and the organic solvent in the droplets is evaporated and removed. Alternatively, the obtained colored fine particle dispersion can be sprayed into a dry atmosphere while stirring to completely remove the organic solvent in the droplets. Alternatively, the colored fine particle dispersion can be depressurized while stirring to evaporate and remove the organic solvent. The latter two methods can be used in combination with the first method.
[0062] The drying atmosphere in which the colored fine particle dispersion is sprayed generally includes, for example, air, nitrogen, carbon dioxide, a gas obtained by heating combustion gas, etc., and in particular, various air streams heated to a temperature equal to or higher than the boiling point of the highest boiling point solvent used. In such a method, the desired quality can be obtained sufficiently by short-term treatment with a spray dryer, a belt dryer, a rotary kiln, etc.
[0063] (Step d: agglomeration step) In step d (aggregation step), the oil-in-water dispersion is aggregated. By going through a step of aggregating fine particles in the oil-in-water dispersion to form particles smaller than toner particles once, even if particles of only prepolymer B are generated, these fine particles can be aggregated.
[0064] In the aggregation step, for example, the oil-in-water dispersion is agitated to aggregate, thereby adjusting the particle size to any desired size. In the aggregation step, existing methods such as adding an aggregating agent and adjusting the pH can be used. When adding an aggregating agent, it may be added as is, but it is preferable to add the aggregating agent in an aqueous solution, since this can avoid localized high concentration. In addition, it is preferable to gradually add the aggregating salt while observing the particle size of the colored particles.
[0065] The temperature of the dispersion during aggregation is preferably near the glass transition temperature Tg of the resin used. If the liquid temperature is too low, aggregation does not proceed well, which may result in poor efficiency, whereas if the liquid temperature is too high, the aggregation rate increases, which may result in the generation of coarse particles and a poor particle size distribution.
[0066] In the aggregation process, aggregation is stopped when the target particle size is reached. Methods for stopping aggregation include adding a salt or a chelating agent with a low ionic valence, adjusting the pH, lowering the temperature of the dispersion, and adding a large amount of an aqueous medium to dilute the concentration. By the above methods, a dispersion of colored aggregated particles can be obtained. The dispersion obtained by the aggregation process may be called an aggregated particle dispersion, a colored aggregated particle dispersion, or the like. The particles in these dispersions may be called aggregated particles, or the like.
[0067] In the aggregation step, wax may be added as a release agent, or a crystalline resin may be added for low-temperature fixability. In that case, it is preferable to prepare a dispersion liquid in which wax is dispersed in an aqueous medium, or a dispersion liquid of a crystalline resin in the same manner, and mix it with the colored particle dispersion liquid before aggregation. In this case, aggregated particles in which the wax or crystalline resin is uniformly dispersed can be obtained.
[0068] <Flocculant> As the flocculant, a known one can be used. For example, metal salts of monovalent metals such as sodium and potassium, metal salts of divalent metals such as calcium and magnesium, and metal salts of trivalent metals such as iron and aluminum can be used. The amount of flocculant to be added is not particularly limited and can be selected appropriately.
[0069] <Release agent> Wax can be used as a release agent. The wax is not particularly limited and can be appropriately selected depending on the purpose, but a release agent with a low melting point of 50°C to 120°C is preferable. The release agent with a low melting point is dispersed in the resin, and effectively acts as a release agent between the fixing roller and the toner interface, thereby improving hot offset properties even in an oil-less case (no release agent such as oil is applied to the fixing roller).
[0070] Suitable examples of the release agent include waxes. Examples of the waxes include natural waxes such as vegetable waxes such as carnauba wax, cotton wax, wood wax, and rice wax; animal waxes such as beeswax and lanolin; mineral waxes such as ozokerite and cerusine; and petroleum waxes such as paraffin, microcrystalline, and petrolatum. In addition to these natural waxes, synthetic hydrocarbon waxes such as Fischer-Tropsch wax and polyethylene wax; synthetic waxes such as esters, ketones, and ethers; and the like. Furthermore, fatty acid amides such as 12-hydroxystearic acid amide, stearic acid amide, phthalic anhydride, and chlorinated hydrocarbons; homopolymers or copolymers of polyacrylates such as poly-n-stearyl methacrylate and poly-n-lauryl methacrylate, which are low molecular weight crystalline polymer resins (for example, copolymers of n-stearyl acrylate and ethyl methacrylate); and crystalline polymers having long alkyl groups on the side chains may be used. These may be used alone or in combination of two or more.
[0071] The melting point of the wax is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 50° C. to 120° C., and more preferably 60° C. to 90° C. If the melting point is 50° C. or higher, the wax can be prevented from adversely affecting the heat resistance storage stability, and if the melting point is 120° C. or lower, the problem of cold offset occurring during fixing at low temperatures can be effectively prevented.
[0072] The melt viscosity of the wax is preferably 5 cps to 1,000 cps, more preferably 10 cps to 100 cps, as measured at a temperature 20° C. higher than the melting point of the wax. If the melt viscosity is 5 cps or more, the release property can be prevented from decreasing, and if it is 1,000 cps or less, the effects of hot offset resistance and low-temperature fixability can be sufficiently exhibited.
[0073] The wax content in the toner is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 0% by mass to 40% by mass, and more preferably 3% by mass to 30% by mass. If the wax content is 40% by mass or less, the fluidity of the toner can be prevented from deteriorating.
[0074] <Crystalline polyester resin> In the aggregation step, it is preferable to use a crystalline polyester resin. The crystalline polyester resin can be added and used at the same time as the flocculant in the aggregation step. By using the crystalline polyester resin, it is possible to improve the fixability and storage stability, and when a colorant is used, it is possible to improve the coloring degree. The crystalline polyester resin is obtained from a polyhydric alcohol and a polycarboxylic acid or a derivative thereof, such as a polycarboxylic acid, a polycarboxylic anhydride, or a polycarboxylic ester.
[0075] In the present invention, the crystalline polyester resin refers to a resin obtained by using a polyhydric alcohol and a polycarboxylic acid or a derivative thereof, such as a polycarboxylic acid, a polycarboxylic anhydride, or a polycarboxylic ester, as described above. Modified polyester resins, such as prepolymers and resins obtained by subjecting the prepolymers to a crosslinking and / or elongation reaction, do not belong to the crystalline polyester resin.
[0076] <<Polyhydric alcohol>> The polyhydric alcohol is not particularly limited and can be appropriately selected depending on the purpose. Examples of the polyhydric alcohol include diols and trihydric or higher alcohols.
[0077] Examples of the diol include saturated aliphatic diols. Examples of the saturated aliphatic diol include linear saturated aliphatic diols and branched saturated aliphatic diols. Among these, linear saturated aliphatic diols are preferred, and linear saturated aliphatic diols having 2 to 12 carbon atoms are more preferred. If the saturated aliphatic diol is a branched type, the crystallinity of the crystalline polyester resin may decrease, resulting in a decrease in melting point. In addition, if the carbon number of the saturated aliphatic diol exceeds 12, it becomes difficult to obtain a practical material.
[0078] Examples of the saturated aliphatic diol include ethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,11-undecanediol, 1,12-dodecanediol, 1,13-tridecanediol, 1,14-tetradecanediol, 1,18-octadecanediol, 1,14-eicosanedecanediol, etc. Among these, ethylene glycol, 1,4-butanediol, 1,6-hexanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, and 1,12-dodecanediol are preferred in terms of the high crystallinity of the crystalline polyester resin and excellent sharp melt properties.
[0079] Examples of the trihydric or higher alcohol include glycerin, trimethylolethane, trimethylolpropane, pentaerythritol, etc. These may be used alone or in combination of two or more.
[0080] <<Polycarboxylic acids>> The polyvalent carboxylic acid is not particularly limited and can be appropriately selected depending on the purpose. Examples thereof include divalent carboxylic acids and trivalent or higher carboxylic acids.
[0081] Examples of the divalent carboxylic acid include saturated aliphatic dicarboxylic acids such as oxalic acid, succinic acid, glutaric acid, adipic acid, suberic acid, azelaic acid, sebacic acid, 1,9-nonanedicarboxylic acid, 1,10-decanedicarboxylic acid, 1,12-dodecanedicarboxylic acid, 1,14-tetradecanedicarboxylic acid, and 1,18-octadecanedicarboxylic acid; aromatic dicarboxylic acids such as phthalic acid, isophthalic acid, terephthalic acid, naphthalene-2,6-dicarboxylic acid, malonic acid, and mesaconic acid; and the like. Further examples include anhydrides of these acids and lower (carbon number 1 to 3) alkyl esters of these acids.
[0082] Examples of the trivalent or higher carboxylic acid include 1,2,4-benzenetricarboxylic acid, 1,2,5-benzenetricarboxylic acid, 1,2,4-naphthalenetricarboxylic acid, and the like, as well as anhydrides and lower (carbon number 1 to 3) alkyl esters thereof. These may be used alone or in combination of two or more.
[0083] The crystalline polyester resin is preferably composed of a linear saturated aliphatic dicarboxylic acid having 4 to 12 carbon atoms and a linear saturated aliphatic diol having 2 to 12 carbon atoms, which provides high crystallinity and excellent sharp melting properties, thereby enabling the toner to exhibit excellent low-temperature fixing properties.
[0084] In addition, as a method for controlling the crystallinity and softening point of a crystalline polyester resin, there can be mentioned a method of designing and using a non-linear polyester obtained by adding a trivalent or higher polyhydric alcohol such as glycerin to the alcohol component during polyester synthesis, or a trivalent or higher polycarboxylic acid such as trimellitic anhydride to the acid component and carrying out condensation polymerization.
[0085] The molecular structure of the crystalline polyester resin in this embodiment can be confirmed by NMR measurement of a solution or solid, as well as X-ray diffraction, GC / MS, LC / MS, IR measurement, etc. -1 Or 990±10cm -1 to the δ of olefinCH One example is one that has absorption based on (out-of-plane bending vibration).
[0086] Regarding the molecular weight, from the viewpoint that a low molecular weight with a sharp molecular weight distribution is excellent in low temperature fixability, and a large amount of low molecular weight components deteriorates heat resistance storage stability, the following has been found to be preferable, for example. In the molecular weight distribution by GPC of the soluble portion in o-dichlorobenzene, the molecular weight distribution diagram with the horizontal axis being log(M) and the vertical axis being weight % has a peak position in the range of 3.5 to 4.0, the half width of the peak is 1.5 or less, and the weight average molecular weight (Mw) is preferably 3,000 to 30,000, the number average molecular weight (Mn) is 1,000 to 10,000, and Mw / Mn is 1 to 10. Furthermore, the weight average molecular weight (Mw) is preferably 5,000 to 15,000, the number average molecular weight (Mn) is preferably 2,000 to 10,000, and Mw / Mn is preferably 1 to 5.
[0087] From the viewpoint of the affinity between paper and resin, the acid value of the crystalline polyester resin is preferably 5 mgKOH / g or more in order to achieve the desired low-temperature fixability. In addition, for the preparation of fine particles by phase inversion emulsification, the acid value is more preferably 7 mgKOH / g or more. On the other hand, in order to improve hot offset properties, the acid value is preferably 45 mgKOH / g or less. In addition, the hydroxyl value of the crystalline polymer is preferably 0 to 50 mgKOH / g, more preferably 5 to 50 mgKOH / g, in order to achieve a predetermined low-temperature fixability and good charging properties.
[0088] (Process e: Fusion process) In this embodiment, a step e (fusion step) may be performed. In the fusion step, the aggregated particles obtained in the aggregation step are fused by heat treatment, so that unevenness can be reduced. Fusion can be performed by heating a dispersion of colored aggregated particles while stirring. The temperature of the liquid is preferably near a temperature exceeding the glass transition temperature Tg of the resin used.
[0089] (Step f: washing or drying step) In this embodiment, step f (cleaning and drying steps) may be performed. Since the toner particle dispersion obtained by the above method may contain sub-materials such as coagulating salts in addition to the toner particles, it is preferable to perform cleaning in order to extract only the toner particles from the dispersion.
[0090] The washing method of the toner particles includes, for example, a centrifugation method, a vacuum filtration method, a filter press method, and the like, but is not particularly limited in the present invention. Any of the methods can obtain a cake of toner particles, but if the toner particles cannot be washed sufficiently in one operation, the obtained cake may be dispersed again in an aqueous solvent to form a slurry, and the process of extracting the toner particles by any of the above methods may be repeated. In addition, if washing is performed by the vacuum filtration method or the filter press method, a method may be adopted in which the aqueous solvent is penetrated into the cake to wash away the secondary material embraced by the colored resin particles. The aqueous solvent used for this washing can be water or a mixed solvent obtained by mixing water with an alcohol such as methanol or ethanol. Considering the cost and the environmental load due to wastewater treatment, it is preferable to use water.
[0091] Since the washed toner particles contain a large amount of the aqueous medium, the toner particles can be obtained by drying and removing the aqueous medium. For the drying method, a dryer such as a spray dryer, a vacuum freeze dryer, a reduced pressure dryer, a stationary shelf dryer, a movable shelf dryer, a fluidized bed dryer, a rotary dryer, or an agitator dryer can be used.
[0092] The dried toner particles are preferably dried until the moisture content is finally reduced to less than 1%. In addition, the colored resin particles after drying may be in the form of soft aggregates, and if this causes inconvenience during use, the particles may be disintegrated using a device such as a jet mill, a Henschel mixer, a super mixer, a coffee mill, an Oster blender, or a food processor to break up the soft aggregates.
[0093] (Step g: Annealing step) In this embodiment, step g (annealing step) may be performed. When a crystalline resin is added, the non-crystalline resin and the crystalline resin are phase-separated by performing an annealing treatment after drying, and the fixing property is improved. Specifically, the toner may be stored for 10 hours or more at a temperature near the glass transition temperature Tg of the resin.
[0094] (Process h: External addition process) In this embodiment, a step h (external addition step) may be performed. In order to impart fluidity, chargeability, cleaning properties, etc. to the toner particles obtained in this embodiment, inorganic fine particles, polymeric fine particles, cleaning aids, etc. may be added and mixed. Specific mixing means include a method of applying an impact force to the mixture by a blade rotating at high speed, a method of introducing the mixture into a high-speed air stream, accelerating it, and causing the particles to collide with each other or the composite particles with an appropriate collision plate, etc.
[0095] Examples of equipment include an Angmill (manufactured by Hosokawa Micron Corporation), a modified I-type mill (manufactured by Japan Pneumatic Co., Ltd.) with reduced grinding air pressure, a hybridization system (manufactured by Nara Machinery Works, Ltd.), a Cryptron system (manufactured by Kawasaki Heavy Industries, Ltd.), and an automatic mortar.
[0096] <External additives> The primary particle diameter of the inorganic fine particles is preferably 5 nm to 2 μm, and more preferably 5 nm to 500 nm. The specific surface area as measured by the BET method is preferably 20 to 500 m. 2 The content of the inorganic fine particles is preferably 0.01 to 5% by mass of the toner.
[0097] Specific examples of inorganic fine particles include silica, alumina, titanium oxide, barium titanate, magnesium titanate, calcium titanate, strontium titanate, zinc oxide, tin oxide, silica sand, clay, mica, wollastonite, diatomaceous earth, chromium oxide, cerium oxide, pengallo, antimony trioxide, magnesium oxide, zirconium oxide, barium sulfate, barium carbonate, calcium carbonate, silicon carbide, and silicon nitride.
[0098] Examples of polymeric fine particles include polystyrene obtained by soap-free emulsion polymerization, suspension polymerization, or dispersion polymerization, methacrylic acid ester or acrylic acid ester copolymers, polycondensation systems such as silicone, benzoguanamine, and nylon, and polymer particles made of thermosetting resins.
[0099] Such external additives can be surface-treated to increase hydrophobicity and prevent deterioration of flow properties and charging properties even under high humidity. For example, silane coupling agents, silylating agents, silane coupling agents having a fluorinated alkyl group, organic titanate coupling agents, aluminum coupling agents, silicone oils, modified silicone oils, etc. are preferred surface treatment agents.
[0100] In addition to the above, a cleaning property improver may be used as an external additive. Examples of cleaning property improvers for removing the developer remaining on the photoconductor or primary transfer medium after transfer include fatty acid metal salts such as zinc stearate, calcium stearate, and stearic acid, and polymer fine particles produced by soap-free emulsion polymerization such as polymethyl methacrylate fine particles and polystyrene fine particles. The polymer fine particles preferably have a relatively narrow particle size distribution and a volume average particle size of 0.01 μm to 1 μm.
[0101] (Method of measuring toner physical properties) <Particle size measurement of dispersion liquid> The particle size of the resin dispersion in the present invention can be measured, for example, using a Nanotrack particle size distribution analyzer UPA-EX150 (Nikkiso Co., Ltd., dynamic light scattering method / laser Doppler method). As a specific measurement method, the dispersion in which the resin fine particles are dispersed is adjusted to a measurement concentration range and measured. At that time, a background measurement is performed in advance using only the dispersion solvent of the dispersion. With this measurement method, it is possible to measure the volume average particle size range of the resin fine particles used in the present invention, from several tens of nm to several μm. In the present invention, the particle size refers to the volume average particle size (volume average diameter).
[0102] <<Melting point and glass transition temperature (Tg) measurement method>> The glass transition temperature Tg in the present invention can be measured, for example, by using a DSC system (differential scanning calorimeter) ("Q-200", manufactured by TA Instruments). Specifically, the melting point and glass transition temperature of a sample can be measured by the following procedure. First, about 5.0 mg of the target sample is placed in an aluminum sample container, the sample container is placed on a holder unit, and set in an electric furnace. Next, in a nitrogen atmosphere, the sample is heated from -80°C to 150°C at a heating rate of 10°C / min (first heating). After that, the sample is cooled from 150°C to -80°C at a temperature drop rate of 10°C / min, and further heated to 150°C at a heating rate of 10°C / min (second heating). During each of the first and second heating, a DSC curve is measured using a differential scanning calorimeter ("Q-200", manufactured by TA Instruments). From the obtained DSC curves, the DSC curve during the first heating is selected using an analysis program in the Q-200 system, and the glass transition temperature during the first heating of the target sample can be obtained. Similarly, the DSC curve during the second heating is selected, and the glass transition temperature during the second heating of the target sample can be obtained. In the present invention, Tg refers to the glass transition temperature at the second heating step.
[0103] <Molecular weight> The molecular weight of the polyester resin, vinyl copolymer resin, etc. used is measured by GPC (gel permeation chromatography) under the following conditions, unless otherwise specified. Equipment: HLC-8220GPC (Tosoh Corporation) Column: TSKgel SuperHZM-Mx3 ·Temperature: 40℃ Solvent: THF (tetrahydrofuran) ·Flow rate: 0.35mL / min Sample: 0.01mL of sample with a concentration of 0.05 to 0.6% From the molecular weight distribution of the toner resin measured under the above conditions, the weight average molecular weight Mw is calculated using a molecular weight calibration curve prepared from a monodisperse polystyrene standard sample. The monodisperse polystyrene standard sample is 5.8×10 2 , 1.085×10 4 , 5.95×10 4 , 3.2×10 5 , 2.56×10 6 , 2.93×10 3 , 2.85×10 4 , 1.48×10 5 , 8.417×10 5 , 7.5×10 6 Ten items from the above were used.
[0104] <Acid value> As mentioned above, the acid value is measured in accordance with JIS K0070. EXAMPLES
[0105] The present invention will be described in more detail below by way of examples, but the present invention is not limited to these examples.
[0106] (Preparation of polyester resin A) In a reaction vessel equipped with a cooling tube, a stirrer, and a nitrogen inlet tube, 2 mol ethylene oxide adduct of bisphenol A / 3 mol propylene oxide adduct of bisphenol A (molar ratio 40 / 60) as a diol component, terephthalic acid / adipic acid (molar ratio 85 / 15) as a dicarboxylic acid component, and 3.5 mol% trimethylolpropane based on the total monomer amount were added so that the molar ratio of hydroxyl group to carboxylic acid (OH / COOH) was 1.2. Furthermore, 1,000 ppm of tetrabutyl orthotitanate based on the total monomer amount was added as a condensation catalyst, and the temperature was raised to 230°C over 2 hours under a nitrogen stream, and the reaction was carried out for 5 hours while distilling off the generated water. Then, the mixture was reacted for 4 hours under reduced pressure of 5mmHg to 15mmHg, and cooled to 180°C. Then, 1.0 mol% of trimellitic anhydride based on the total monomer amount and 200 ppm of tetrabutyl orthotitanate based on the total monomer amount were added, and the mixture was reacted at normal pressure and 180°C for 1 hour. Then, the mixture was further reacted for 3 hours under reduced pressure of 5mmHg to 20mmHg to obtain [Polyester Resin A]. [Polyester Resin A] had a glass transition temperature Tg of 58°C, a weight average molecular weight of 10,500, and an acid value of 20 mgKOH / g, as determined from the DSC curve of the second heating cycle by DSC.
[0107] (Preparation of prepolymer B-1) In a reaction vessel equipped with a cooling tube, a stirrer, and a nitrogen inlet tube, 3-methyl-1,5-pentanediol, isophthalic acid, adipic acid, and trimellitic anhydride were added together with titanium tetraisopropoxide (1,000 ppm relative to the resin component) so that the OH / COOH molar ratio of hydroxyl groups to carboxyl groups was 1.1, the composition of the diol component was 110 mol% of 3-methyl-1,5-pentanediol, the composition of the dicarboxylic acid component was 40 mol% of isophthalic acid and 60 mol% of adipic acid, and the amount of trimellitic anhydride in the total monomers was 1 mol%. After that, the temperature was raised to 200°C in about 4 hours, and then raised to 230°C in 2 hours, and the reaction was carried out until no water was discharged. After that, the reaction was further carried out for 5 hours under a reduced pressure of 10 mmHg to 15 mmHg to obtain [Intermediate Polyester B-1]. Next, in a reaction vessel equipped with a cooling tube, a stirrer, and a nitrogen inlet tube, [intermediate polyester B-1] and hexamethylene diisocyanate derivative (HDI isocyanate) were added in an amount such that the molar ratio (NCO / OH) of the isocyanate group of HDI isocyanate to the hydroxyl group of [intermediate polyester B-1] was 2.0, and ethyl acetate was added to dissolve so as to obtain a 50% ethyl acetate solution. Then, the temperature was raised to 80°C under a nitrogen stream and the reaction was carried out for 5 hours to obtain an ethyl acetate solution of [prepolymer B-1(OH)], which is a prepolymer with a hydroxyl group terminal. Then, the pressure was reduced until the amount of remaining ethyl acetate in the ethyl acetate solution of [prepolymer B-1(OH)] was 100 ppm or less. Next, in a reaction vessel equipped with a cooling tube, a stirrer, and a nitrogen inlet tube, [Prepolymer B-1(OH)] and monomethyl ester succinic acid were added in such an amount that the molar ratio (CH3 / OH) of the hydroxyl groups of [Prepolymer B-1(OH)] to the methyl groups of monomethyl ester succinic acid was 2.0, and the mixture was reacted at 150°C for 6 hours to obtain [Prepolymer B-1], a prepolymer with a carboxylic acid terminal. [Prepolymer B-1] has a glass transition temperature Tg of -37°C and an acid value of 7 mgKOH / g.
[0108] (Preparation of prepolymer B-2) In a reaction vessel equipped with a cooling tube, a stirrer, and a nitrogen inlet tube, 1,6-hexanediol, isophthalic acid, adipic acid, and trimellitic anhydride were added together with titanium tetraisopropoxide (1,000 ppm relative to the resin component) so that the molar ratio of hydroxyl groups to carboxyl groups, OH / COOH, was 1.1, the composition of the diol component was 1,6-hexanediol 110 mol%, the composition of the dicarboxylic acid component was 40 mol% isophthalic acid and 60 mol% adipic acid, and the amount of trimellitic anhydride in the total monomers was 1 mol%. After that, the temperature was raised to 200°C in about 4 hours, and then raised to 230°C in 2 hours, and the reaction was carried out until no water was discharged. After that, the reaction was further carried out for 5 hours under a reduced pressure of 10 mmHg to 15 mmHg to obtain [Intermediate Polyester B-2]. Next, in a reaction vessel equipped with a cooling tube, a stirrer, and a nitrogen inlet tube, [intermediate polyester B-2] and hexamethylene diisocyanate derivative (HDI isocyanate) were added in an amount such that the molar ratio (NCO / OH) of the isocyanate group of HDI isocyanate to the hydroxyl group of [intermediate polyester B-2] was 2.0, and ethyl acetate was added to dissolve so as to obtain a 50% ethyl acetate solution. Then, the temperature was raised to 80°C under a nitrogen stream and reacted for 5 hours to obtain an ethyl acetate solution of [prepolymer B-2(OH)], which is a prepolymer with a hydroxyl group terminal. Then, the pressure was reduced until the amount of remaining ethyl acetate in the ethyl acetate solution of [prepolymer B-2(OH)] was 100 ppm or less. Next, in a reaction vessel equipped with a cooling tube, a stirrer, and a nitrogen inlet tube, [Prepolymer B-2(OH)] and monomethyl ester succinic acid were added in such an amount that the molar ratio (CH3 / OH) of the hydroxyl groups of [Prepolymer B-2(OH)] to the methyl groups of monomethyl ester succinic acid was 2.0, and the reaction was carried out at 150°C for 6 hours to obtain [Prepolymer B-2], a prepolymer with a carboxylic acid terminal. [Prepolymer B-2] has a glass transition temperature Tg of -5°C and an acid value of 7 mgKOH / g.
[0109] (Preparation of prepolymer B-3) In a reaction vessel equipped with a cooling tube, a stirrer, and a nitrogen inlet tube, 3-methyl-1,5-pentanediol, isophthalic acid, adipic acid, and trimellitic anhydride were added together with titanium tetraisopropoxide (1,000 ppm relative to the resin component) so that the OH / COOH molar ratio of hydroxyl groups to carboxyl groups was 1.1, the composition of the diol component was 110 mol% of 3-methyl-1,5-pentanediol, the composition of the dicarboxylic acid component was 50 mol% of isophthalic acid and 50 mol% of adipic acid, and the amount of trimellitic anhydride in the total monomers was 1 mol%. After that, the temperature was raised to 200°C in about 4 hours, and then raised to 230°C in 2 hours, and the reaction was carried out until no water was discharged. After that, the reaction was further carried out for 5 hours under a reduced pressure of 10 mmHg to 15 mmHg to obtain [Intermediate Polyester B-3]. Next, in a reaction vessel equipped with a cooling tube, a stirrer, and a nitrogen inlet tube, [intermediate polyester B-3] and hexamethylene diisocyanate derivative (HDI isocyanate) were added in an amount such that the molar ratio (NCO / OH) of the isocyanate group of HDI isocyanate to the hydroxyl group of [intermediate polyester B-3] was 2.0, and ethyl acetate was added to dissolve so as to obtain a 50% ethyl acetate solution. Then, the temperature was raised to 80°C under a nitrogen stream and the reaction was carried out for 5 hours to obtain an ethyl acetate solution of a prepolymer ([prepolymer B-3(OH)]) with a hydroxyl group terminal. Then, the pressure was reduced until the amount of remaining ethyl acetate in the ethyl acetate solution of [prepolymer B-3(OH)] was 100 ppm or less. Next, in a reaction vessel equipped with a cooling tube, a stirrer, and a nitrogen inlet tube, [Prepolymer B-3(OH)] and monomethyl ester succinic acid were added in amounts such that the molar ratio (CH3 / OH) of the hydroxyl groups of [Prepolymer B-3(OH)] to the methyl groups of monomethyl ester succinic acid was 2.0, and the mixture was reacted at 150°C for 6 hours to obtain a carboxylic acid-terminated prepolymer [Prepolymer B-3]. [Prepolymer B-3] has a glass transition temperature Tg of -37°C and an acid value of 12 mgKOH / g.
[0110] (Preparation of prepolymer B-4) In a reaction vessel equipped with a cooling tube, a stirrer and a nitrogen inlet tube, 3-methyl-1,5-pentanediol as a diol component, terephthalic acid / adipic acid (molar ratio 55 / 45) as a dicarboxylic acid component, 1.0 mol% trimethylolpropane with respect to the total monomer amount, and 0.5 mol% trimellitic anhydride with respect to the total monomer amount were added so that the molar ratio of hydroxyl group to carboxylic acid (OH / COOH) was 1.5. Furthermore, 1,000 ppm of tetrabutyl orthotitanate with respect to the total monomer amount was added as a condensation catalyst, and the temperature was raised to 200°C over 2 hours under a nitrogen stream, and the temperature was further raised to 230°C over 2 hours, and the reaction was carried out for 3 hours while distilling off the generated water. After that, the reaction was carried out for 5 hours under a reduced pressure of 5 mmHg to 15 mmHg to obtain [Intermediate polyester B-4] having a weight average molecular weight of 18,000. Next, in a reaction vessel equipped with a cooling tube, a stirrer, and a nitrogen inlet tube, [Intermediate polyester B-4] and isophorone diisocyanate (IPDI) were added in amounts such that the molar ratio (NCO / OH) of the isocyanate group of IPDI to the hydroxyl group of [Intermediate polyester B-4] was 2.0, and ethyl acetate was added to dissolve so as to make a 50% ethyl acetate solution. After that, the temperature was raised to 80°C under a nitrogen stream and the reaction was carried out for 5 hours, to obtain an ethyl acetate solution of [Prepolymer B-4], which is a reactive precursor of polyester resin (A). Next, an amine-extended product of [Prepolymer B-4] was obtained as follows. First, ethyl acetate was added to [Prepolymer B-4] to prepare a 20% ethyl acetate solution. Next, while stirring, a 20% ethyl acetate solution of isophorone diamine (IPDA) was dropped in an amount such that the molar ratio (NH2 / NCO) of the isocyanate group of [Prepolymer B-4] to the amino group of IPDA was 1.1, and the mixture was thoroughly stirred. This resulted in an ethyl acetate solution of the amine extension product. Next, the obtained ethyl acetate solution of the amine extension product was cast on a Teflon petri dish and dried for 10 hours in an environment of 80°C. Furthermore, the mixture was dried under reduced pressure in an environment of 120°C and 10 kPa or less to thoroughly remove the solvent. This resulted in an amine extension product of [Prepolymer B-4]. The amine-extended product of [Prepolymer B-4] has a glass transition temperature Tg of −37° C. and an acid value of 1 mgKOH / g, as determined from the DSC curve of the first heating run by DSC.
[0111] (Preparation of prepolymer B-5) In a reaction vessel equipped with a cooling tube, a stirrer, and a nitrogen inlet tube, 1,6-hexanediol, isophthalic acid, adipic acid, and trimellitic anhydride were added together with titanium tetraisopropoxide (1,000 ppm relative to the resin component) so that the molar ratio of hydroxyl groups to carboxyl groups, OH / COOH, was 1.1, the composition of the diol component was 1,6-hexanediol 110 mol%, the composition of the dicarboxylic acid component was 60 mol% isophthalic acid and 40 mol% adipic acid, and the amount of trimellitic anhydride in the total monomers was 1 mol%. After that, the temperature was raised to 200°C in about 4 hours, and then raised to 230°C in 2 hours, and the reaction was carried out until no water was discharged. After that, the reaction was further carried out for 5 hours under a reduced pressure of 10 mmHg to 15 mmHg to obtain [Intermediate Polyester B-5]. Next, in a reaction vessel equipped with a cooling tube, a stirrer, and a nitrogen inlet tube, [intermediate polyester B-5] and hexamethylene diisocyanate derivative (HDI isocyanate) were added in an amount such that the molar ratio (NCO / OH) of the isocyanate group of HDI isocyanate to the hydroxyl group of [intermediate polyester B-5] was 2.0, and ethyl acetate was added to dissolve so as to obtain a 50% ethyl acetate solution. Then, the temperature was raised to 80°C under a nitrogen stream and reacted for 5 hours to obtain an ethyl acetate solution of [prepolymer B-5(OH)], which is a prepolymer with a hydroxyl group terminal. Then, the pressure was reduced until the amount of remaining ethyl acetate in the ethyl acetate solution of [prepolymer B-5(OH)] was 100 ppm or less. Next, in a reaction vessel equipped with a cooling tube, a stirrer, and a nitrogen inlet tube, [Prepolymer B-5(OH)] and monomethyl ester succinic acid were added in such an amount that the molar ratio (CH3 / OH) of the hydroxyl group of [Prepolymer B-5(OH)] to the methyl group of monomethyl ester succinic acid was 2.0, and the mixture was reacted at 150°C for 6 hours to obtain [Prepolymer B-5], a prepolymer with a carboxylic acid terminal. [Prepolymer B-5] has a glass transition temperature Tg of 5°C and an acid value of 7 mgKOH / g.
[0112] (Preparation of prepolymer B-6) In a reaction vessel equipped with a cooling tube, a stirrer, and a nitrogen inlet tube, 3-methyl-1,5-pentanediol, isophthalic acid, adipic acid, and trimellitic anhydride were added together with titanium tetraisopropoxide (1,000 ppm relative to the resin component) so that the OH / COOH molar ratio of hydroxyl groups to carboxyl groups was 1.1, the composition of the diol component was 110 mol% of 3-methyl-1,5-pentanediol, the composition of the dicarboxylic acid component was 40 mol% of isophthalic acid and 60 mol% of adipic acid, and the amount of trimellitic anhydride in the total monomers was 1 mol%. After that, the temperature was raised to 200°C in about 4 hours, and then raised to 230°C in 2 hours, and the reaction was carried out until no water was discharged. After that, the reaction was further carried out for 5 hours under a reduced pressure of 10 mmHg to 15 mmHg to obtain [Intermediate Polyester B-6]. Next, in a reaction vessel equipped with a cooling tube, a stirrer, and a nitrogen inlet tube, [intermediate polyester B-6] and hexamethylene diisocyanate derivative (HDI isocyanate) were added in an amount such that the molar ratio (NCO / OH) of the isocyanate group of HDI isocyanate to the hydroxyl group of [intermediate polyester B-6] was 2.0, and ethyl acetate was added to dissolve so as to obtain a 50% ethyl acetate solution. Then, the temperature was raised to 80°C under a nitrogen stream and the reaction was carried out for 5 hours, to obtain an ethyl acetate solution of [prepolymer B-6(OH)], which is a prepolymer with a hydroxyl group terminal. Then, the pressure was reduced until the amount of remaining ethyl acetate in the ethyl acetate solution of [prepolymer B-6(OH)] was 100 ppm or less. Next, in a reaction vessel equipped with a cooling tube, a stirrer, and a nitrogen inlet tube, [Prepolymer B-6(OH)] and monomethyl ester succinic acid were added in such an amount that the molar ratio (CH3 / OH) of the hydroxyl group of [Prepolymer B-6(OH)] to the methyl group of monomethyl ester succinic acid was 2.0, and the reaction was carried out at 150°C for 6 hours to obtain [Prepolymer B-6], a prepolymer with a carboxylic acid terminal. [Prepolymer B-6] has a glass transition temperature Tg of -37°C and an acid value of 17 mgKOH / g.
[0113] (Preparation of Crystalline Polyester Resin 1) 1,6-hexanediol and sebacic acid were charged into a 5L four-neck flask equipped with a nitrogen inlet tube, a dehydration tube, a stirrer, and a thermocouple so that the ratio of OH groups to COOH groups (OH / COOH) was 1.1. The mixture was reacted while draining water along with 500 ppm titanium tetraisopropoxide relative to the mass of the charged raw materials, and finally heated to 235°C and reacted for 1 hour. Then, the mixture was reacted for 6 hours under a reduced pressure of 10 mmHg or less. The temperature was then set to 185°C, and trimellitic anhydride was added so that the molar ratio with COOH groups was 0.053, and the mixture was reacted for 2 hours with stirring to obtain [Crystalline polyester resin 1]. Next, 55 parts by weight of [crystalline polyester resin 1], 35 parts by weight of methyl ethyl ketone, and 10 parts by weight of 2-propyl alcohol were added to a four-neck flask. Then, the mixture was heated and stirred at the melting point temperature of [crystalline polyester resin 1] to dissolve the crystalline polyester resin. Then, 28% by weight of aqueous ammonia was added so that the neutralization rate was 200%. The neutralization rate was calculated from the acid value of the crystalline polyester resin. Furthermore, 130 parts by weight of ion-exchanged water was gradually added to perform phase inversion emulsification, and then the solvent was removed. Then, ion-exchanged water was added to adjust the solid concentration (concentration of the crystalline polyester resin) to 25% by mass, and [crystalline polyester resin dispersion 1], which is a binder resin dispersion for toner, was obtained. When the particle size of [crystalline polyester resin dispersion 1] was measured, the particle size was 250 nm. In addition, the solid concentration was 27%.
[0114] (Preparation of wax emulsion 1) To 100 parts by weight of ion-exchanged water, 28 parts by weight of HNP-9 (manufactured by Nippon Seiro) as a wax and Sanisol B50 as a surfactant were added. This was dispersed using a homogenizer while being heated to 90°C, to obtain [Wax Emulsion 1]. The solid content was 30%.
[0115] (Preparation of Masterbatch 1) 1,200 parts of water, 500 parts of carbon black (Printex 35 manufactured by Dexa) [DBP oil absorption = 42 mL / 100 mg, pH = 9.5], and 500 parts of polyester resin A were added and mixed in a Henschel mixer (manufactured by Mitsui Mining Co., Ltd.), and the mixture was kneaded using two rolls at 150 ° C. for 30 minutes. Then, it was rolled and cooled, and pulverized with a pulverizer to obtain [Master batch 1].
[0116] Example 1 <Oil phase preparation process, aqueous phase preparation process, and phase inversion emulsification process> In a four-neck flask, 100 parts by weight of [polyester resin A], 30 parts by weight of [prepolymer B-1], and 30 parts by weight of [master batch 1] were added to 160 parts by weight of ethyl acetate, and the mixture was stirred to dissolve or disperse. Then, 5 parts by weight of 28% by mass aqueous ammonia was added while stirring to obtain a neutralization rate of 500%, to prepare a solution (oil phase). Ethyl acetate was added to 370 parts by weight of ion-exchanged water so that the amount was 100% relative to the saturated dissolution amount, and a surfactant (sodium dodecyl sulfate) was added so that the amount was 2% relative to the total amount of ion-exchanged water and ethyl acetate, to prepare an aqueous phase. Next, the water phase was gradually added to the oil phase to perform phase inversion emulsification. After that, the solvent was removed to obtain [Slurry 1]. The particle size of [Slurry 1] was measured to be 0.60 μm. The solid content was also measured to be 25.0%.
[0117] <Aggregation process and fusion process> 200 parts by weight of [Slurry 1], 11.0 parts by weight of [Crystalline polyester resin dispersion 1], 10.5 parts by weight of [Wax emulsion 1], and 50 parts by weight of ion-exchanged water were placed in a container and stirred for 5 minutes. Next, 30 parts by weight of 10% magnesium chloride solution was added dropwise and stirred for another 5 minutes, after which the temperature was raised to 60° C. When the particle size reached 5.0 μm, 6 parts by weight of sodium chloride was added to terminate the aggregation process, and [Aggregated Slurry 1] was obtained. [Aggregated Slurry 1] was heated to 70° C. while stirring, and when the desired circularity of 0.960 was reached, it was cooled, and [Toner Dispersion 1] was obtained.
[0118] <Annealing step and cleaning or drying step> [Toner dispersion liquid 1] was stored at 45° C. for 10 hours, filtered under reduced pressure, and washed and dried as follows. (1) 100 parts of ion-exchanged water was added to the filter cake, mixed with a TK homomixer (at 12,000 rpm for 10 minutes), and then filtered. (2): 900 parts of ion-exchanged water was added to the filter cake of (1), and ultrasonic vibration was applied and mixed with a TK homomixer (rotation speed 12,000 rpm for 30 minutes), and then the mixture was filtered under reduced pressure. This operation was repeated until the electrical conductivity of the reslurry liquid became 10 μC / cm or less, and then the mixture was filtered to obtain [Filter cake 1]. The [filter cake 1] was dried in a circulating air dryer at 45° C. for 48 hours and sieved through a 75 μm mesh to obtain [colored resin particles 1].
[0119] <External attachment> To 100 parts by weight of [Colored Resin Particles 1], 2.5 parts by weight of inorganic fine particles TS530 manufactured by Cabosil Corporation was added, and mixed for 10 minutes at 40 m / s in a Henschel mixer to obtain the toner of Example 1.
[0120] Example 2 A toner of Example 2 was obtained in the same manner as in Example 1, except that [Prepolymer B-1] in Example 1 was changed to [Prepolymer B-3].
[0121] Example 3 <Oil phase preparation, phase inversion emulsification> In a four-neck flask, 100 parts by weight of [Polyester Resin A], 30 parts by weight of [Prepolymer B-3], and 30 parts by weight of [Masterbatch 1] were added to 160 parts by weight of MEK, and the mixture was stirred to dissolve and disperse. Then, 5 parts by weight of 28% by mass aqueous ammonia was added while stirring to achieve a neutralization rate of 500%, to prepare an oil phase. MEK (methyl ethyl ketone) was added to 400 parts by weight of ion-exchanged water so that the amount of MEK was 100% relative to the saturated solubility, to prepare an aqueous phase. Next, the water phase was gradually added to the oil phase to perform phase inversion emulsification. After that, the solvent was removed to obtain [Slurry 3]. The particle size of [Slurry 3] was measured to be 0.30 μm. The solid content was also measured to be 25.0%.
[0122] <Aggregation process and fusion process> 220 parts by weight of [Slurry 3], 12.0 parts by weight of [Crystalline polyester resin dispersion 1], 11.5 parts by weight of [Wax emulsion 1], and 50 parts by weight of ion-exchanged water were placed in a container and stirred for 5 minutes. Next, 0.75 parts by weight of a 10% magnesium chloride solution was added dropwise and stirred for an additional 5 minutes, after which the temperature was raised to 60° C. Thereafter, when the particle size reached 5.0 μm, the pH was adjusted to 8.5 with sodium hydroxide, and 100 parts by weight of ion-exchanged water was added to terminate the aggregation process, yielding [Aggregated Slurry 3]. [Aggregated Slurry 3] was heated to 70° C. while stirring, and cooled when the desired circularity of 0.960 was reached, yielding [Toner Dispersion 3]. The subsequent steps were the same as in Example 1, and a toner of Example 3 was obtained.
[0123] Example 4 A toner of Example 4 was obtained in the same manner as in Example 1, except that [Prepolymer B-1] in Example 1 was changed to [Prepolymer B-5].
[0124] Example 5 A toner of Example 5 was obtained in the same manner as in Example 1, except that [Prepolymer B-1] in Example 1 was changed to [Prepolymer B-2].
[0125] Example 6 The toner of Example 6 was obtained in the same manner as in Example 1, except that in the oil phase preparation process of Example 1, [Prepolymer B-1] was changed to [Prepolymer B-6], and further, in the aggregation process, [Crystalline polyester resin 1] was added together with the aggregating agent.
[0126] Example 7 The toner of Example 7 was obtained in the same manner as in Example 1, except that in the aqueous phase preparation step of Example 1, ethyl acetate was changed to MEK.
[0127] Comparative Example 1 A toner of Comparative Example 1 was obtained in the same manner as in Example 1, except that the prepolymer was not added.
[0128] Comparative Example 2 A toner of Comparative Example 2 was obtained in the same manner as in Example 1, except that [Prepolymer B-1] in Example 1 was changed to an amine-extended product of [Prepolymer B-4].
[0129] Comparative Example 3 A toner of Comparative Example 3 was obtained in the same manner as in Example 3, except that [Prepolymer B-3] in Example 3 was changed to an amine-extended product of [Prepolymer B-4].
[0130] (evaluation) <Low temperature fixability> Using the fixing unit of a color multifunction printer (imagio MP C4500, manufactured by Ricoh Co., Ltd.), a 0.6 mg / cm2 ink was applied to plain paper. 2 The temperature at which cold offset occurs was measured and rated on a four-point scale.
[0131] [Evaluation Criteria] ◎: Less than 120℃ ○: 120℃ or higher and lower than 125℃ △: 125℃ or higher but less than 130℃ ×: 130℃ or higher
[0132] <High temperature fixability> Using the fixing unit of a color multifunction printer (imagio MP C4500, manufactured by Ricoh Co., Ltd.), a 0.6 mg / cm2 ink was applied to plain paper. 2 The temperature at which hot offset occurred was measured and rated on a four-point scale.
[0133] [Evaluation Criteria] ◎: 190℃ or higher ○: 180℃ or higher and lower than 190℃ △: 170℃ or higher but less than 180℃ ×: Less than 170℃
[0134] <Heat-resistant storage stability> The heat resistance storage stability was evaluated by placing 10 g of the toner in a 100 ml glass bottle, leaving it in an environment of 50° C. for 24 hours, and evaluating the stability based on the following criteria.
[0135] [Evaluation Criteria] ◎: Shake 10 times and everything will turn back into powder 〇: Shake 10 times and half of it will turn back into powder △: Shake 10 times and it turns back into powder ×: Does not turn back into powder even after shaking 10 times
[0136] <Coloring degree> Using the fixing unit of a color multifunction printer (imagio Mp C4500, manufactured by Ricoh Co., Ltd.), a 0.4 mg / cm2 ink was applied to plain paper. 2 A solid fixed image was formed and fixed at a fixing temperature of 130° C. The coloring degree of the image was measured using an X-Rite exact at an average of 5 points and evaluated on a 4-point scale.
[0137] [Evaluation Criteria] ◎: Coloring degree is 2.00 or more ○: Coloring degree is 1.50 or more and less than 2.00 △: Coloring degree is 1.25 or more and less than 1.50 ×: Coloring degree is less than 1.25
[0138] The evaluation results of the toners of the examples and comparative examples are shown in Table 1. Note that MEK stands for methyl ethyl ketone.
[0139] [Table 1] [Prior art documents] [Patent documents]
[0140] [Patent Document 1] Patent No. 4239267 [Patent Document 2] JP 2018-159057 A
Claims
1. a) preparing a solution by dissolving or dispersing a polyester resin A and a prepolymer B in an organic solvent; b) mixing an organic solvent and water to form an aqueous phase; c) adding the aqueous phase to the solution to effect phase inversion emulsification to prepare an oil-in-water dispersion; d) aggregating the oil-in-water dispersion, The prepolymer B does not have an isocyanate group, The acid value [mgKOH / g] of the polyester resin A and the prepolymer B is A>B>5 A toner manufacturing method comprising the steps of:
2. The acid value [mgKOH / g] of the polyester resin A and the prepolymer B is A>B>10 2. The method for producing a toner according to claim 1, wherein the above formula (1) is satisfied.
3. 3. The method for producing a toner according to claim 1, wherein the organic solvent in the step a and the step b is ethyl acetate or methyl ethyl ketone.
4. The glass transition temperature Tg [°C] of the polyester resin A and the prepolymer B is A>0>B 4. The method for producing a toner according to claim 1, wherein the above-mentioned condition is satisfied.
5. 5. The method for producing a toner according to claim 1, wherein the step (d) uses a crystalline polyester resin.
Citation Information
Patent Citations
Toner and developer
JP2006293304A
Toner for electrostatic latent image development, method for manufacturing the same, electrostatic latent image developer using the toner, toner container, image forming apparatus and process cartridge
JP2008070829A
Electrophotographic toner, developer using the toner, image forming apparatus, and process cartridge
JP2013068795A
Phase inversion emulsification process for controlling latex particle size
JP2018159057A
Toner, developer, and image forming apparatus
JP2021039284A