A thermoplastic resin containing norbornene polymer is used to create a thin stretched film with high tensile elongation and improved handling properties, addressing the mechanical weaknesses of conventional films.
Patent Information
- Application Number
- JP2021516007
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-04-26
- Filing Date
- 2020-04-13
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2040-04-13
AI Technical Summary
Conventional thin stretched films made from thermoplastic resins with excellent birefringence properties have low mechanical strength, particularly low tensile elongation at break, and poor handling properties during production.
Using a thermoplastic resin containing a norbornene polymer selected from specific monomer compositions, the film is stretched to achieve a thickness of 40 μm or less with a high tensile elongation at break and improved handling properties.
The stretched film exhibits a large tensile elongation at break and excellent handling properties, maintaining high retardation despite its thinness, with enhanced mechanical strength and reduced film breakage during production.
Smart Images

Figure 0007567782000001 
Figure 0007567782000002 
Figure 0007567782000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a stretched film and a method for producing the same. [Background technology]
[0002] Conventionally, films formed from thermoplastic resins have been known. For example, Patent Document 1 describes a technique for forming an optical film from a cycloolefin resin. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] International Publication No. 2017 / 002508 Summary of the Invention [Problem to be solved by the invention]
[0004] An optical film provided in an image display device such as a liquid crystal display device may be required to have a predetermined retardation. An optical film having such a retardation is generally produced as a stretched film by stretching a resin film formed of a thermoplastic resin.
[0005] A stretched film may be required to be thin, for example, to have a thickness of 40 μm or less. However, since retardation is generally proportional to thickness, the thinner the film, the smaller the retardation tends to be. Therefore, from the viewpoint of realizing a stretched film having a desired retardation even if it is thin, the present inventors have considered using a resin having excellent birefringence expression as a material for the stretched film.
[0006] However, conventional thin stretched films formed using resins with excellent birefringence tend to have low mechanical strength, particularly low tensile elongation at break. Furthermore, when stretching a film made of a resin with excellent birefringence to produce a stretched film, the film tends to have poor handleability during the production process. Specifically, the film tends to break easily during the production process.
[0007] The present invention has been made in view of the above problems, and an object of the present invention is to provide a stretched film having a large tensile breaking elongation and excellent handleability, and a method for producing the same. [Means for solving the problem]
[0008] The present inventors have conducted extensive research to solve the above problems, and as a result, have found that a stretched film having high tensile elongation at break and excellent handleability can be produced by using a thermoplastic resin containing a norbornene polymer selected from the group consisting of polymers of specific norbornene monomer compositions and hydrogenated products thereof, thereby completing the present invention. That is, the present invention includes the following.
[0009] [1] A stretched film formed of a thermoplastic resin containing a norbornene-based polymer, the norbornene-based polymer is selected from the group consisting of polymers of norbornene-based monomer compositions and hydrogenated products thereof, The norbornene-based monomer composition contains 50% by weight or more of one or more monomers selected from the group consisting of a monomer represented by the following formula (T) and a monomer represented by the following formula (D), and 1% by weight to 15% by weight of a monomer represented by the following formula (N): The stretched film has a thickness of 40 μm or less. [ka] (In formula (T), nt1 and nt2 each independently represent 1 or 2; If nt1 is 1, then R t1 represents a divalent hydrocarbon group, If nt1 is 2, then R t1 each independently represents a hydrogen atom, an alkyl group, or an alkyloxycarbonyl group, If nt2 is 1, then R t2 represents a divalent hydrocarbon group, If nt2 is 2, then R t2 each independently represents a hydrogen atom, an alkyl group, or an alkyloxycarbonyl group; In formula (D), nd1, nd2 and nd3 each independently represent 1 or 2; If nd1 is 1, R d1 represents a hydrogen atom, an alkyl group, an alkyloxycarbonyl group, or a divalent hydrocarbon group, If nd1 is 2, R d1 each independently represents a hydrogen atom, an alkyl group, or an alkyloxycarbonyl group, If nd2 is 1, R d2 represents a hydrogen atom, an alkyl group, an alkyloxycarbonyl group, or a divalent hydrocarbon group, If nd2 is 2, R d2 each independently represents a hydrogen atom, an alkyl group, or an alkyloxycarbonyl group, If nd3 is 1, R d3 represents a divalent hydrocarbon group, If nd3 is 2, R d3 each independently represents a hydrogen atom, an alkyl group, or an alkyloxycarbonyl group; In formula (N), nn1 and nn2 each independently represent 1 or 2; If nn1 is 1, then R n1 represents a divalent hydrocarbon group, If nn1 is 2, then R n1 each independently represents a hydrogen atom, an alkyl group, or an alkyloxycarbonyl group, If nn2 is 1, then R n2 represents a divalent hydrocarbon group, If nn2 is 2, then R n2 each independently represents a hydrogen atom, an alkyl group, or an alkyloxycarbonyl group. [2] The stretched film according to [1], wherein the stretched film is an obliquely stretched film. [3] The stretched film according to [1], wherein the stretched film is a biaxially stretched film. [4] The ratio (Rth / d) of the retardation Rth in the thickness direction of the stretched film to the thickness d of the stretched film is 3×10 -3 The stretched film according to any one of [1] to [3] above. [5] The stretched film according to any one of [1] to [4], wherein the areal stretching ratio of the stretched film is 1.4 times or more. [6] The stress birefringence CR of the thermoplastic resin is 1650×10 -12 Pa -1 The stretched film according to any one of [1] to [5], [7] The stretched film according to any one of [1] to [6], wherein the stretched film has a tensile elongation at break of 85% or more. [8] The stretched film according to any one of [1] to [7], wherein the glass transition temperature Tg of the thermoplastic resin is 105° C. or higher and lower than 170° C. [9] A method for producing the stretched film according to any one of [1] to [8], The method includes the steps of: preparing a resin film formed of a thermoplastic resin containing a norbornene-based polymer; and stretching the resin film; the norbornene-based polymer is selected from the group consisting of polymers of norbornene-based monomer compositions and hydrogenated products thereof, The norbornene-based monomer composition contains 50% by weight or more of one or more monomers selected from the group consisting of a monomer represented by the following formula (T) and a monomer represented by the following formula (D), and 1% by weight to 15% by weight of a monomer represented by the following formula (N). [ka] (In formula (T), nt1 and nt2 each independently represent 1 or 2; If nt1 is 1, then R t1 represents a divalent hydrocarbon group, If nt1 is 2, then R t1 each independently represents a hydrogen atom, an alkyl group, or an alkyloxycarbonyl group, If nt2 is 1, then R t2 represents a divalent hydrocarbon group, If nt2 is 2, then R t2 each independently represents a hydrogen atom, an alkyl group, or an alkyloxycarbonyl group; In formula (D), nd1, nd2 and nd3 each independently represent 1 or 2; If nd1 is 1, R d1 represents a hydrogen atom, an alkyl group, an alkyloxycarbonyl group, or a divalent hydrocarbon group, If nd1 is 2, R d1 each independently represents a hydrogen atom, an alkyl group, or an alkyloxycarbonyl group, If nd2 is 1, R d2 represents a hydrogen atom, an alkyl group, an alkyloxycarbonyl group, or a divalent hydrocarbon group, If nd2 is 2, R d2 each independently represents a hydrogen atom, an alkyl group, or an alkyloxycarbonyl group, If nd3 is 1, R d3 represents a divalent hydrocarbon group, If nd3 is 2, R d3 each independently represents a hydrogen atom, an alkyl group, or an alkyloxycarbonyl group; In formula (N), nn1 and nn2 each independently represent 1 or 2; If nn1 is 1, then R n1 represents a divalent hydrocarbon group, If nn1 is 2, then R n1each independently represents a hydrogen atom, an alkyl group, or an alkyloxycarbonyl group, If nn2 is 1, then R n2 represents a divalent hydrocarbon group, If nn2 is 2, then R n2 each independently represents a hydrogen atom, an alkyl group, or an alkyloxycarbonyl group.
[10] The method for producing a stretched film according to [9], wherein the areal stretching ratio of the stretched film is 1.4 times or more. Effect of the Invention
[0010] According to the present invention, it is possible to provide a stretched film having a large tensile elongation at break and excellent handleability, and a method for producing the same. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] The present invention will be described in detail below with reference to the embodiments and examples. However, the present invention is not limited to the embodiments and examples shown below, and may be modified and implemented as desired without departing from the scope of the claims of the present invention and the scope of equivalents thereto.
[0012] In the following description, the in-plane retardation Re of the film is a value expressed by Re = (nx - ny) x d, unless otherwise specified. The retardation Rth in the thickness direction of the film is a value expressed by Rth = [{(nx + ny) / 2} - nz] x d, unless otherwise specified. Here, nx represents the refractive index in the direction perpendicular to the thickness direction of the film (in-plane direction) and giving the maximum refractive index. ny represents the refractive index in the in-plane direction perpendicular to the direction of nx. nz represents the refractive index in the thickness direction. d represents the thickness of the film. The measurement wavelength is 550 nm, unless otherwise specified.
[0013] In the following description, a "long" film refers to a film having a length of 5 times or more its width, preferably 10 times or more its width, specifically a film having a length long enough to be wound into a roll for storage or transportation. The upper limit of the ratio of the length to the width of the film is not particularly limited, but may be, for example, 100,000 times or less.
[0014] In the structural formulae shown in the following description, the following line segments represented by a combination of parallel solid and dashed lines represent either a single bond or a double bond, unless otherwise specified.
[0015] [ka]
[0016] [1. Overview of oriented film] The stretched film according to one embodiment of the present invention is a stretched film made of a thermoplastic resin and has a thickness equal to or less than a specific value. The thermoplastic resin contained in the stretched film contains one or more norbornene polymers selected from the group consisting of polymers of norbornene monomer compositions and their hydrogenated products. The term "norbornene monomer composition" refers to a general term for monomers used as raw materials for norbornene polymers. Thus, norbornene polymers may generally have a structure formed by polymerization of a norbornene monomer composition, or a structure in which the carbon-carbon unsaturated bonds of the structure are hydrogenated.
[0017] The norbornene-based monomer composition contains one or more monomers selected from the group consisting of a monomer represented by formula (T) and a monomer represented by formula (D), and a monomer represented by formula (N) in a specific ratio.
[0018] [ka]
[0019] (In formula (T), nt1 and nt2 each independently represent 1 or 2; If nt1 is 1, then R t1 represents a divalent hydrocarbon group, If nt1 is 2, then R t1 each independently represents a hydrogen atom, an alkyl group, or an alkyloxycarbonyl group, If nt2 is 1, then R t2 represents a divalent hydrocarbon group, If nt2 is 2, then R t2 each independently represents a hydrogen atom, an alkyl group, or an alkyloxycarbonyl group; In formula (D), nd1, nd2 and nd3 each independently represent 1 or 2; If nd1 is 1, R d1 represents a hydrogen atom, an alkyl group, an alkyloxycarbonyl group, or a divalent hydrocarbon group, If nd1 is 2, R d1 each independently represents a hydrogen atom, an alkyl group, or an alkyloxycarbonyl group, If nd2 is 1, R d2 represents a hydrogen atom, an alkyl group, an alkyloxycarbonyl group, or a divalent hydrocarbon group, If nd2 is 2, R d2 each independently represents a hydrogen atom, an alkyl group, or an alkyloxycarbonyl group, If nd3 is 1, R d3 represents a divalent hydrocarbon group, If nd3 is 2, R d3 each independently represents a hydrogen atom, an alkyl group, or an alkyloxycarbonyl group; In formula (N), nn1 and nn2 each independently represent 1 or 2; If nn1 is 1, then R n1 represents a divalent hydrocarbon group, If nn1 is 2, then R n1 each independently represents a hydrogen atom, an alkyl group, or an alkyloxycarbonyl group, If nn2 is 1, then R n2 represents a divalent hydrocarbon group, If nn2 is 2, then R n2 each independently represents a hydrogen atom, an alkyl group, or an alkyloxycarbonyl group.
[0020] The stretched film has a large tensile elongation at break and excellent handleability even though it is thin. In addition, since the thermoplastic resin forming the stretched film usually has excellent birefringence expression, the stretched film can have a large retardation even though it is thin.
[0021] In the following description, the monomer represented by formula (T) may be referred to as a "TCD-based monomer." The monomer represented by formula (D) may be referred to as a "DCP-based monomer." Furthermore, the monomer represented by formula (N) may be referred to as a "NB-based monomer."
[0022] [2. Norbornene-based polymers] The norbornene polymer is selected from the group consisting of polymers of norbornene monomer compositions and their hydrogenated products. The norbornene monomer composition contains at least one monomer selected from the group consisting of TCD monomers and DCP monomers in combination with an NB monomer. Preferred combinations of monomers contained in the norbornene monomer composition include combinations containing TCD monomers, DCP monomers, and NB monomers; and combinations containing TCD monomers and NB monomers but not DCP monomers. When a norbornene monomer composition containing a combination of TCD monomers, DCP monomers, and NB monomers is used, a norbornene polymer is usually obtained as at least a ternary copolymer containing three or more types of repeating units. In addition, when a norbornene-based monomer composition containing a combination of a TCD-based monomer and an NB-based monomer and not containing a DCP-based monomer is used, a norbornene-based polymer is usually obtained as at least a binary copolymer containing two or more kinds of repeating units. If necessary, the norbornene-based monomer composition may contain any monomer other than the TCD-based monomer, the DCP-based monomer, and the NB-based monomer.
[0023] The TCD monomer is represented by formula (T). Under appropriate conditions, this TCD monomer can undergo polymerization reactions such as ring-opening polymerization and addition polymerization. In addition, the polymer obtained by the polymerization reaction can be hydrogenated to convert the carbon-carbon unsaturated bond into a carbon-carbon single bond. For example, when the TCD monomer represented by formula (T-1) described later undergoes ring-opening polymerization and hydrogenation, a polymer containing a repeating unit represented by formula (TA) can be obtained.
[0024] [ka]
[0025] In formula (T), nt1 and nt2 each independently represent 1 or 2. When nt1 is 1, R t1 The bond of may represent a double bond. Also, when nt1 is 2, R t1The bond of may represent a single bond. Furthermore, when nt2 is 1, R t2 The bond of may represent a double bond. Also, when nt2 is 2, R t2 may represent a single bond. Thus, formula (T) includes structures represented by the following formulae (T-1) to (T-4). In detail, a structure in which nt1 is 1 may be represented by formulae (T-2) and (T-4), and a structure in which nt1 is 2 may be represented by formulae (T-1) and (T-3). A structure in which nt2 is 1 may be represented by formulae (T-2) and (T-3), and a structure in which nt2 is 2 may be represented by formulae (T-1) and (T-4).
[0026] [ka]
[0027] If nt1 is 1, then R t1 represents a divalent hydrocarbon group. From the viewpoint of obtaining a stretched film having particularly excellent tensile elongation at break and handleability, the divalent hydrocarbon group is preferably an aliphatic hydrocarbon group, and more preferably a saturated aliphatic hydrocarbon group. The number of carbon atoms in this divalent hydrocarbon group is usually 1 or more and usually 6 or less, preferably 4 or less, more preferably 2 or less. When the number of carbon atoms is within the above range, a stretched film having particularly excellent tensile elongation at break and handleability can be obtained, and moreover, it is usually easy to increase the birefringence of the thermoplastic resin. Examples of the divalent hydrocarbon group include a methylidene group and an ethylidene group.
[0028] If nt1 is 2, then R t1 R each independently represents a hydrogen atom, an alkyl group, or an alkyloxycarbonyl group. t1The number of carbon atoms in the alkyl group as the alkyloxycarbonyl group is usually 1 or more, and usually 6 or less, preferably 4 or less, and more preferably 2 or less. The number of carbon atoms in the alkyl group contained in the alkyloxycarbonyl group is usually 1 or more, and usually 6 or less, preferably 4 or less, and more preferably 2 or less. When the number of carbon atoms is within the above range, a stretched film having particularly excellent tensile elongation at break and handleability can be obtained, and moreover, it is usually easy to increase the birefringence of the thermoplastic resin. Examples of the alkyl group include a methyl group and an ethyl group. Among them, from the viewpoint of effectively improving the tensile elongation at break, R t1 is preferably a hydrogen atom. When nt1 is 2, the TCD monomer has multiple R t1 These R t1 may be the same or different.
[0029] If nt2 is 1, then R t2 R represents a divalent hydrocarbon group. t2 The divalent hydrocarbon group represented by R t1 The divalent hydrocarbon group represented by R may be the same as that represented by R t1 The same advantages as described for
[0030] If nt2 is 2, then R t2 R each independently represents a hydrogen atom, an alkyl group, or an alkyloxycarbonyl group. t2 The alkyl group and alkyloxycarbonyl group represented by R t1 The same range of alkyl groups and alkyloxycarbonyl groups represented by R can be used. t1 In particular, from the viewpoint of effectively improving the tensile elongation at break, t2 is preferably a hydrogen atom. When nt2 is 2, the TCD monomer has multiple R t2 These R t2 may be the same or different.
[0031] Examples of TCD monomers include the following monomers:
[0032] [ka]
[0033] The TCD monomer may be used alone or in combination of two or more kinds in any ratio.
[0034] The amount of the TCD monomer is usually set so that the amount of one or more monomers selected from the group consisting of TCD monomers and DCP monomers relative to the total amount of the norbornene monomer composition (100% by weight) falls within a specific range. Specifically, the amount of one or more monomers selected from the group consisting of TCD monomers and DCP monomers is usually 50% by weight or more, more preferably 60% by weight or more, particularly preferably 70% by weight or more, and usually 99% by weight or less, preferably 98% by weight or less, relative to the total amount of the norbornene monomer composition (100% by weight). When the amount of one or more monomers selected from the group consisting of TCD monomers and DCP monomers is within the above range, a stretched film having excellent tensile elongation at break and handleability can be obtained, and moreover, a thermoplastic resin having excellent birefringence expression can usually be obtained.
[0035] When the norbornene monomer composition contains a combination of a TCD monomer, a DCP monomer, and an NB monomer, the amount of the TCD monomer is preferably 20% by weight or more, more preferably 22% by weight or more, particularly preferably 25% by weight or more, and preferably 35% by weight or less, more preferably 34% by weight or less, particularly preferably 33% by weight or less, based on 100% by weight of the total amount of the norbornene monomer composition. When the amount of the TCD monomer is within the above range, it is easy to increase the expression of birefringence while maintaining the flexibility of the thermoplastic resin.
[0036] In addition, when the norbornene-based monomer composition contains a combination of a TCD-based monomer and an NB-based monomer and does not contain a DCP-based monomer, the amount of the TCD-based monomer is preferably 80% by weight or more, more preferably 93% by weight or more, particularly preferably 94% by weight or more, and preferably 99% by weight or less, more preferably 98% by weight or less, particularly preferably 97% by weight or less, based on 100% by weight of the total amount of the norbornene-based monomer composition. When the amount of the TCD-based monomer is within the above range, it is easy to increase the heat resistance of the thermoplastic resin.
[0037] The DCP monomer is represented by formula (D). Under appropriate conditions, this DCP monomer can undergo polymerization reactions such as ring-opening polymerization and addition polymerization. Furthermore, the polymer obtained by the polymerization reaction can be hydrogenated to convert the carbon-carbon unsaturated bond into a carbon-carbon single bond. For example, when a DCP monomer represented by formula (D-1) described later undergoes ring-opening polymerization and hydrogenation, a polymer containing a repeating unit represented by formula (DA) can be obtained.
[0038] [ka]
[0039] In formula (D), nd1, nd2 and nd3 each independently represent 1 or 2. When nd1 is 1, R d1 The bond of may represent a single bond or a double bond. When nd1 is 2, R d1 The bond of may represent a single bond. Furthermore, when nd2 is 1, R d2 The bond of may represent a single bond or a double bond. When nd2 is 2, R d2 The bond of may represent a single bond. d1 The carbon atom to which R is bonded d2 When the bond between the carbon atom to which is bonded (i.e., the bond represented by a combination of a solid line and a dashed line included in the five-membered ring) is a double bond, nd1 is 1, R d1 The bond of is a single bond, nd2 is 1, R d2 The bond of can represent a single bond. d1The carbon atom to which R is bonded d2 When the bond between the carbon atom to which R is bonded is a single bond, nd1 is 1 or 2, R d1 The bond of is a single bond or a double bond, nd2 is 1 or 2, R d2 The bond of may represent a single bond or a double bond. Furthermore, when nd3 is 1, R d3 The bond of may represent a double bond. Also, when nd3 is 2, R d3 may represent a single bond. Therefore, formula (D) includes structures represented by the following formulas (D-1) to (D-10). In detail, the structure in which nd1 is 1 may be represented by formula (D-1), (D-2), (D-4), (D-7), (D-8) and (D-10), and the structure in which nd1 is 2 may be represented by formula (D-3), (D-5), (D-6) and (D-9). The structure in which nd2 is 1 may be represented by formula (D-1), (D-2), (D-5), (D-7), (D-9) and (D-10), and the structure in which nd2 is 2 may be represented by formula (D-3), (D-4), (D-6) and (D-8). Furthermore, the structure in which nd3 is 1 can be represented by formula (D-2), formula (D-6), formula (D-8), formula (D-9) and formula (D-10), and the structure in which nd3 is 2 can be represented by formula (D-1), formula (D-3), formula (D-4), formula (D-5) and formula (D-7).
[0040] [ka]
[0041] If nd1 is 1, R d1 represents a hydrogen atom, an alkyl group, an alkyloxycarbonyl group, or a divalent hydrocarbon group. When nd1 is 2, R d1 R each independently represents a hydrogen atom, an alkyl group, or an alkyloxycarbonyl group. d1The number of carbon atoms of the alkyl group as the alkyl group is usually 1 or more, usually 6 or less, preferably 4 or less, more preferably 2 or less. The number of carbon atoms of the alkyl group contained in the alkyloxycarbonyl group is usually 1 or more, usually 6 or less, preferably 4 or less, more preferably 2 or less. When the number of carbon atoms is within the above range, a stretched film having particularly excellent tensile elongation at break and handleability can be obtained, and more usually, the birefringence of the thermoplastic resin is easily increased. Examples of the alkyl group include a methyl group and an ethyl group. In addition, as the divalent hydrocarbon group, from the viewpoint of obtaining a stretched film having particularly excellent tensile elongation at break and handleability, an aliphatic hydrocarbon group is preferable, and a saturated aliphatic hydrocarbon group is more preferable. The number of carbon atoms of this divalent hydrocarbon group is usually 1 or more, usually 6 or less, preferably 4 or less, more preferably 2 or less. When the number of carbon atoms is within the above range, a stretched film having particularly excellent tensile elongation at break and handleability can be obtained, and more usually, the birefringence of the thermoplastic resin is easily increased. Examples of the divalent hydrocarbon group include a methylidene group and an ethylidene group. Among them, from the viewpoint of effectively improving the tensile elongation at break and the handling property, R d1 is preferably a hydrogen atom. When nd1 is 2, the DCP monomer has a plurality of R d1 These R d1 may be the same or different.
[0042] If nd2 is 1, R d2 represents a hydrogen atom, an alkyl group, an alkyloxycarbonyl group, or a divalent hydrocarbon group. When nd2 is 2, R d2 R each independently represents a hydrogen atom, an alkyl group, or an alkyloxycarbonyl group. d2 The alkyl group, alkyloxycarbonyl group, and divalent hydrocarbon group represented by R d1 The same range of alkyl groups, alkyloxycarbonyl groups, and divalent hydrocarbon groups represented by R can be used. d1In particular, from the viewpoint of effectively improving the tensile elongation at break and the handling property, R d2 is preferably a hydrogen atom. When nd2 is 2, the DCP monomer has a plurality of R d2 These R d2 may be the same or different.
[0043] If nd3 is 1, R d3 R represents a divalent hydrocarbon group. d3 The divalent hydrocarbon group represented by R d1 The divalent hydrocarbon group represented by R may be the same as that represented by R d1 The same advantages as described for
[0044] If nd3 is 2, R d3 R each independently represents a hydrogen atom, an alkyl group, or an alkyloxycarbonyl group. d3 The alkyl group and alkyloxycarbonyl group represented by R d1 The same range of alkyl groups and alkyloxycarbonyl groups represented by R can be used. d1 In particular, from the viewpoint of effectively improving the tensile elongation at break and the handling property, R d3 is preferably a hydrogen atom. When nd3 is 2, the DCP monomer has a plurality of R d3 These R d3 may be the same or different.
[0045] Examples of DCP monomers include the following monomers:
[0046] [ka]
[0047] The DCP monomer may be used alone or in combination of two or more kinds in any ratio.
[0048] When the norbornene-based monomer composition contains a combination of a TCD-based monomer, a DCP-based monomer, and an NB-based monomer, the amount of the DCP-based monomer is preferably 65% by weight or more, more preferably 66% by weight or more, particularly preferably 67% by weight or more, and is preferably 80% by weight or less, more preferably 77% by weight or less, particularly preferably 75% by weight or less, based on 100% by weight of the total amount of the norbornene-based monomer composition. When the amount of the DCP-based monomer is within the above range, it is easy to increase the birefringence of the thermoplastic resin.
[0049] The amount of the DCP monomer is preferably equal to or greater than the amount of the TCD monomer. More specifically, the amount of the DCP monomer relative to 100 parts by weight of the TCD monomer is preferably equal to or greater than 100 parts by weight, more preferably equal to or greater than 150 parts by weight, particularly preferably equal to or greater than 200 parts by weight, and is preferably equal to or less than 500 parts by weight, more preferably equal to or less than 450 parts by weight, particularly preferably equal to or less than 400 parts by weight. When the amount of the DCP monomer is within the above range, the tensile elongation at break of the stretched film can be effectively improved.
[0050] The NB monomer is represented by formula (N). Under appropriate conditions, this NB monomer can undergo polymerization reactions such as ring-opening polymerization and addition polymerization. In addition, the polymer obtained by the polymerization reaction can be hydrogenated to convert the carbon-carbon unsaturated bond into a carbon-carbon single bond. For example, when the NB monomer represented by formula (N-1) described later undergoes ring-opening polymerization and hydrogenation, a polymer containing a repeating unit represented by formula (NA) can be obtained.
[0051] [ka]
[0052] In formula (N), nn1 and nn2 each independently represent 1 or 2. When nn1 is 1, R n1 The bond of may represent a double bond. Also, when nn1 is 2, R n1The bond of may represent a single bond. Furthermore, when nn2 is 1, R n2 The bond of may represent a double bond. Also, when nn2 is 2, R n2 may represent a single bond. Therefore, formula (N) includes structures represented by the following formulae (N-1) to (N-4). In detail, a structure in which nn1 is 1 is represented by formulae (N-2) and (N-4), and a structure in which nn1 is 2 is represented by formulae (N-1) and (N-3). A structure in which nn2 is 1 is represented by formulae (N-2) and (N-3), and a structure in which nn2 is 2 can be represented by formulae (N-1) and (N-4).
[0053] [ka]
[0054] If nn1 is 1, then R n1 represents a divalent hydrocarbon group. From the viewpoint of obtaining a stretched film having particularly excellent tensile elongation at break and handleability, the divalent hydrocarbon group is preferably an aliphatic hydrocarbon group, and more preferably a saturated aliphatic hydrocarbon group. The number of carbon atoms in this divalent hydrocarbon group is usually 1 or more and usually 6 or less, preferably 4 or less, more preferably 2 or less. When the number of carbon atoms is within the above range, a stretched film having particularly excellent tensile elongation at break and handleability can be obtained, and moreover, it is usually easy to increase the birefringence of the thermoplastic resin. Examples of the divalent hydrocarbon group include a methylidene group and an ethylidene group.
[0055] If nn1 is 2, then R n1 R each independently represents a hydrogen atom, an alkyl group, or an alkyloxycarbonyl group. n1The number of carbon atoms in the alkyl group as the alkyloxycarbonyl group is usually 1 or more, and usually 6 or less, preferably 4 or less, and more preferably 2 or less. The number of carbon atoms in the alkyl group contained in the alkyloxycarbonyl group is usually 1 or more, and usually 6 or less, preferably 4 or less, and more preferably 2 or less. When the number of carbon atoms is within the above range, a stretched film having particularly excellent tensile elongation at break and handleability can be obtained, and moreover, it is usually easy to increase the birefringence of the thermoplastic resin. Examples of the alkyl group include a methyl group and an ethyl group. Among them, from the viewpoint of effectively improving the tensile elongation at break, R n1 is preferably a hydrogen atom. When nn1 is 2, the NB monomer has a plurality of R n1 These R n1 may be the same or different.
[0056] If nn2 is 1, then R n2 R represents a divalent hydrocarbon group. n2 The divalent hydrocarbon group represented by R n1 The divalent hydrocarbon group represented by R may be the same as that represented by R n1 The same advantages as described for
[0057] If nn2 is 2, then R n2 R each independently represents a hydrogen atom, an alkyl group, or an alkyloxycarbonyl group. n2 The alkyl group and alkyloxycarbonyl group represented by R n1 The same range of alkyl groups and alkyloxycarbonyl groups represented by R can be used. n1 In particular, from the viewpoint of effectively improving the tensile elongation at break, n2 is preferably a hydrogen atom. When nn2 is 2, the NB monomer has a plurality of R n2 These R n2 may be the same or different.
[0058] Examples of NB-based monomers include the following monomers:
[0059] [ka]
[0060] The NB monomer may be used alone or in combination of two or more kinds in any ratio.
[0061] The amount of the NB monomer is usually 1% by weight or more, and usually 15% by weight or less, preferably 7% by weight or less, and more preferably 4% by weight or less, based on 100% by weight of the total amount of the norbornene monomer composition. When the amount of the NB monomer is within the above range, a stretched film having excellent tensile elongation at break and handleability can be obtained, and moreover, a thermoplastic resin having excellent birefringence expression can usually be obtained.
[0062] The amount of the NB monomer is preferably 0.5 parts by weight or more, more preferably 0.8 parts by weight or more, particularly preferably 1.0 part by weight or more, and is preferably 20 parts by weight or less, more preferably 15 parts by weight or less, particularly preferably 10 parts by weight or less, relative to 100 parts by weight of the amount of one or more monomers selected from the group consisting of TCD monomers and DCP monomers. When the amount of the NB monomer is within the above range, a stretched film having particularly excellent tensile elongation at break and handleability can be obtained.
[0063] The norbornene-based monomer composition may contain, in addition to the TCD-based monomer, the DCP-based monomer, and the NB-based monomer, any monomer polymerizable with the TCD-based monomer, the DCP-based monomer, or the NB-based monomer, within a range that does not significantly impair the effects of the present invention. The any monomer may be used alone or in combination of two or more kinds at any ratio. The amount of the any monomer is preferably 0% by weight to 5.0% by weight, more preferably 0% by weight to 3.0% by weight, and particularly preferably 0% by weight to 1.0% by weight, based on the total amount of the norbornene-based monomer composition (100% by weight). In particular, it is preferable that the norbornene-based monomer composition does not contain any any monomer.
[0064] The norbornene polymer is selected from the group consisting of the polymer of the norbornene monomer composition and its hydrogenated product. Examples of the polymer of the norbornene monomer composition include a ring-opened polymer of the norbornene monomer composition and an addition polymer of the norbornene monomer composition. The hydrogenated product may be a polymer in which the non-aromatic carbon-carbon unsaturated bond in the polymer is hydrogenated, a polymer in which the aromatic carbon-carbon unsaturated bond in the polymer is hydrogenated, or a polymer in which both the non-aromatic carbon-carbon unsaturated bond and the aromatic carbon-carbon unsaturated bond in the polymer are hydrogenated. In particular, a hydrogenated product of a ring-opened polymer of a norbornene monomer composition is preferred, and a hydrogenated product in which both the non-aromatic carbon-carbon unsaturated bond and the aromatic carbon-carbon unsaturated bond in the ring-opened polymer of a norbornene monomer composition are hydrogenated is more preferred. The use of such norbornene-based polymers makes it possible to obtain stretched films having particularly excellent tensile elongation at break and handling properties, and generally makes it easy to increase the birefringence of the thermoplastic resin, and generally improves the mechanical strength, moisture resistance, heat resistance, and other properties of the stretched films.
[0065] The hydrogenation rate of the hydrogenated product may be any value within a range that does not significantly impair the effects of the present invention. From the viewpoint of improving the transparency and heat resistance of the stretched film, the hydrogenation rate of the non-aromatic carbon-carbon unsaturated bonds is preferably 90% to 100%, more preferably 97% to 100%, and particularly preferably 99% to 100%. From the viewpoint of improving the transparency and heat resistance of the stretched film, the hydrogenation rate of the aromatic carbon-carbon unsaturated bonds is preferably 90% to 100%, more preferably 93% to 100%, and particularly preferably 95% to 100%. The hydrogenation rate is 1 It can be measured by H-NMR.
[0066] The weight average molecular weight Mw of the norbornene polymer is preferably 10,000 to 100,000, more preferably 15,000 to 80,000, and particularly preferably 20,000 to 70,000. When the weight average molecular weight is within the above range, the mechanical strength and formability of the stretched film are highly balanced.
[0067] The molecular weight distribution (weight average molecular weight (Mw) / number average molecular weight (Mn)) of the norbornene polymer is preferably 3 or less, more preferably 2.8 or less, and preferably 1.0 or more, more preferably 1.2 or more. When the molecular weight distribution Mw / Mn is within the above range, the heat resistance of the stretched film can be improved.
[0068] The weight average molecular weight Mw and number average molecular weight Mn of the polymer can be measured in terms of polyisoprene by gel permeation chromatography using cyclohexane as the eluent. If the polymer is not soluble in cyclohexane, gel permeation chromatography can be performed using tetrahydrofuran (THF) as the eluent. When the eluent is THF, the weight average molecular weight Mw and number average molecular weight Mn of the polymer can be measured in terms of polystyrene.
[0069] The norbornene polymer can be produced, for example, by a production method including polymerizing a norbornene monomer composition in the presence of a suitable catalyst. When a hydrogenated product is produced as the norbornene polymer, the production method of the norbornene polymer may include, after the polymerization, contacting the resulting polymer with hydrogen in the presence of a hydrogenation catalyst including a transition metal such as nickel, palladium, or ruthenium to hydrogenate the carbon-carbon unsaturated bonds.
[0070] The norbornene-based polymer contained in the thermoplastic resin may be of one type or of two or more types.
[0071] The amount of the norbornene-based polymer contained in the thermoplastic resin is arbitrary within a range that allows a stretched film having excellent tensile elongation at break and handleability to be obtained. Specifically, the amount of the norbornene-based polymer contained in the thermoplastic resin is preferably 80% by weight to 100% by weight, more preferably 90% by weight to 100% by weight, and particularly preferably 95% by weight to 100% by weight, based on 100% by weight of the thermoplastic resin.
[0072] [3. Thermoplastic resin] The thermoplastic resin contained in the stretched film according to the present embodiment includes the above-mentioned norbornene-based polymer. By being made of the thermoplastic resin containing the above-mentioned norbornene-based polymer, the stretched film according to the present embodiment has a large tensile elongation at break and excellent handleability even if it is thin. In addition, this stretched film can usually have a large retardation even if it is thin.
[0073] The thermoplastic resin may contain optional components other than the norbornene polymer. Examples of the optional components include light absorbers such as ultraviolet absorbers and infrared absorbers, antioxidants, heat stabilizers, light stabilizers, antistatic agents, dispersants, chlorine scavengers, flame retardants, crystallization nucleating agents, reinforcing agents, antiblocking agents, antifogging agents, mold release agents, pigments, organic or inorganic fillers, neutralizing agents, lubricants, decomposers, metal deactivators, antifouling agents, and antibacterial agents. The optional components may be used alone or in combination of two or more at any ratio.
[0074] The stress birefringence CR of the thermoplastic resin is preferably 1650×10 -12 Pa -1 Larger, preferably 1700 x 10 -12 Pa -1 Larger, preferably 2800 x 10 -12 Pa -1 Less than 2700×10 -12 Pa -1 It is less than. When the stress birefringence CR of the thermoplastic resin is larger than the lower limit of the above range, the film containing the thermoplastic resin tends to exhibit a large birefringence due to stretching, and therefore, the retardation of the stretched film is easily increased. When the stress birefringence CR of the thermoplastic resin is less than the upper limit of the above range, the retardation of the stretched film is easily controlled, and the in-plane variation of the retardation can be suppressed.
[0075] The stress birefringence CR of a thermoplastic resin can be measured by the following method. A thermoplastic resin is molded into a sheet to obtain a sheet. Both ends of the sheet are fixed with clips, and then a weight of a predetermined weight (for example, 55 g) is fixed to one of the clips. Next, the sheet is hung in an oven set to a predetermined temperature (for example, a temperature 15° C. higher than the glass transition temperature Tg of the thermoplastic resin) from the clip to which the weight is not fixed for a predetermined time (for example, 1 hour) to perform a stretching process. The sheet that has been stretched is slowly cooled to room temperature. The in-plane retardation Re(b) of the sheet at the center is measured at a measurement wavelength of 650 nm, and the in-plane retardation Re(b) is divided by the thickness T(b) of the sheet center to calculate the Δn value. Then, the stress birefringence CR can be obtained by dividing the Δn value by the stress applied to the sheet (in the above case, the stress applied when the predetermined weight is fixed).
[0076] The stress birefringence CR of a thermoplastic resin can be adjusted by the types and quantitative ratios of monomers contained in a norbornene-based monomer composition as a raw material for a norbornene-based polymer, and the content of the norbornene-based polymer in the thermoplastic resin.
[0077] The glass transition temperature Tg of the thermoplastic resin is preferably 105°C or higher, more preferably 108°C or higher, particularly preferably 110°C or higher, and is preferably less than 170°C, more preferably less than 160°C, particularly preferably less than 150°C. When the glass transition temperature Tg of the thermoplastic resin is equal to or higher than the lower limit of the above range, relaxation of the orientation of the norbornene-based polymer in a high-temperature environment can be suppressed. Therefore, the change in retardation of the stretched film in a high-temperature environment can be suppressed. In addition, since the expression of birefringence by stretching can usually be increased, the retardation of the stretched film can be easily increased. On the other hand, when the glass transition temperature Tg of the thermoplastic resin is lower than the upper limit of the above range, it is easy to perform stretch processing.
[0078] The glass transition temperature Tg of a thermoplastic resin can be measured using a differential scanning calorimeter in accordance with JIS K 6911 at a temperature rise rate of 10° C. / min.
[0079] The glass transition temperature Tg of the thermoplastic resin can be adjusted, for example, by the types and quantitative ratios of monomers contained in the norbornene-based monomer composition as a raw material for the norbornene-based polymer, and the content of the norbornene-based polymer in the thermoplastic resin.
[0080] [4. Characteristics of oriented film] The stretched film according to the present embodiment is formed of a thermoplastic resin containing the norbornene-based polymer described above, and has a thickness within a specific range. The specific thickness of the stretched film is usually 40 μm or less, preferably 35 μm or less, and more preferably 30 μm or less. Although the stretched film according to the present embodiment is a thin film, it has a large tensile elongation at break and excellent handling properties. In addition, since the thermoplastic resin is usually excellent in expressing birefringence, the stretched film can have a large retardation even if it is as thin as described above. There is no particular limit to the lower limit of the thickness of the stretched film, but from the viewpoint of effectively increasing the tensile elongation at break, it may be preferably 10 μm or more, more preferably 15 μm or more, and particularly preferably 20 μm or more.
[0081] A stretched film is unlikely to break when pulled. Therefore, the stretched film can have a large tensile breaking elongation E. The specific tensile breaking elongation E of the stretched film is preferably 85% or more, more preferably 90% or more. There is no particular upper limit to the tensile breaking elongation E of the stretched film, and it can be, for example, 150% or less.
[0082] The tensile elongation at break E of the stretched film can be measured by the following method in accordance with JIS K7127. Ten dumbbell-shaped test pieces of Type 1B are punched out from the stretched film to be measured. When punching out the test pieces, the longitudinal direction of five test pieces and the longitudinal direction of the other five test pieces are set perpendicular to each other. For example, in a long stretched film, the longitudinal direction of five test pieces may be set parallel to the longitudinal direction of the stretched film, and the longitudinal direction of the other five test pieces may be set parallel to the width direction of the stretched film. Then, the tensile breaking elongation of these test pieces is measured. The tensile breaking elongation is measured using a tensile tester equipped with a thermo-hygrostat (for example, "5564" manufactured by Instron) at a pulling speed of 20 mm / min in an environment of normal temperature and normal pressure. The average value of the measured tensile breaking elongation of the test pieces may be the tensile breaking elongation E of the stretched film.
[0083] The stretched film has excellent handleability, specifically, it is unlikely to break even when it is subjected to a stretching process and a trimming process during production of the stretched film.
[0084] A stretched film is a film produced by a production method including stretching, and therefore the molecules of the norbornene-based polymer contained in the stretched film are usually oriented. Therefore, the stretched film can be an optically anisotropic film having birefringence according to the orientation of the molecules. Therefore, the stretched film can have retardation.
[0085] The thermoplastic resin contained in the stretched film can exhibit high birefringence. Therefore, by utilizing this high exhibitability, the stretched film preferably has a large retardation. Specifically, it is preferable that the ratio Rth / d of the retardation Rth in the thickness direction of the stretched film to the thickness d is in a specific range. The specific range of the ratio Rth / d is preferably 3.0×10 -3 More than 3.1×10 -3 More preferably, 3.2×10 -3 The upper limit of the ratio Rth / d is not particularly limited, but from the viewpoint of effectively increasing the tensile breaking elongation of the stretched film, it is preferably 9.5×10 -3 Less than or equal to 9.0×10-3 Less than 8.5×10, particularly preferably -3 Generally, a stretched film having a larger areal stretch ratio tends to have a larger ratio Rth / d.
[0086] The retardation Rth in the thickness direction of the stretched film is arbitrary depending on the application of the stretched film. To show a specific range, the retardation Rth in the thickness direction of the stretched film is preferably 40 nm or more, more preferably 50 nm or more, particularly preferably 60 nm or more, and is preferably 450 nm or less, more preferably 400 nm or less, particularly preferably 350 nm or less.
[0087] The in-plane retardation Re of the stretched film is arbitrary depending on the application of the stretched film. Specifically, the in-plane retardation Re of the stretched film is preferably 0 nm or more, more preferably 10 nm or more, particularly preferably 20 nm or more, and is preferably 300 nm or less, more preferably 250 nm or less, particularly preferably 200 nm or less.
[0088] The stretched film preferably has a high total light transmittance. The specific total light transmittance of the stretched film is preferably 85% to 100%, more preferably 87% to 100%, and particularly preferably 90% to 100%. The total light transmittance can be measured in the wavelength range of 400 nm to 700 nm using a commercially available spectrophotometer.
[0089] The stretched film preferably has a small haze in order to improve the image clarity of the image display device to which the stretched film is applied. The haze of the stretched film is preferably 1% or less, more preferably 0.8% or less, and particularly preferably 0.5% or less. The haze can be measured using a turbidimeter in accordance with JIS K7361-1997.
[0090] [5. Manufacturing method of stretched film] The stretched film described above can be produced, for example, by a production method including the steps of preparing a resin film formed of a thermoplastic resin containing a norbornene-based polymer and stretching the resin film. In order to distinguish the resin film before stretching from the stretched film obtained after stretching, the resin film before stretching may be referred to as the "film before stretching" as appropriate hereinafter.
[0091] In the step of preparing the pre-stretched film, a thermoplastic resin is usually molded to obtain the pre-stretched film. There is no limitation on the molding method. Examples of the molding method include extrusion molding, solution casting, and inflation molding. Among them, extrusion molding and solution casting are preferred, and extrusion molding is particularly preferred.
[0092] After preparing the pre-stretch film, a step of stretching the pre-stretch film is carried out. This stretching orients the molecules of the norbornene-based polymer in the film, so that a stretched film having desired optical properties can be obtained. In addition, since the film is formed of a thermoplastic resin containing the above-mentioned norbornene-based polymer, film breakage due to this stretching can be suppressed. The stretching conditions in the step of stretching the pre-stretch film can be set arbitrarily within a range in which a desired stretched film can be obtained.
[0093] The stretching mode of the pre-stretched film may be, for example, uniaxial stretching in which stretching is performed in one direction, or biaxial stretching in which stretching is performed in two non-parallel directions. The biaxial stretching may be simultaneous biaxial stretching in which stretching is performed simultaneously in two directions, or sequential biaxial stretching in which stretching is performed in one direction and then in the other direction. Among them, biaxial stretching is preferred, and sequential biaxial stretching is more preferred. A stretched film produced by a production method including biaxial stretching may be called a "biaxially stretched film". Biaxial stretching can easily increase the retardation Rth in the thickness direction.
[0094] The stretching direction of the pre-stretching film can be set arbitrarily. For example, when the pre-stretching film is a long film, the stretching direction may be the longitudinal direction, the transverse direction, or the oblique direction. The longitudinal direction refers to the length direction of the long film, the transverse direction refers to the width direction of the long film, and the oblique direction refers to a direction that is neither parallel nor perpendicular to the length direction of the long film. Among them, the oblique direction is preferable. A stretched film produced by a manufacturing method including stretching in an oblique direction is sometimes called an "obliquely stretched film". The obliquely stretched film may have a slow axis in an oblique direction. Therefore, the obliquely stretched film can easily perform axis alignment when bonding with a general polarizing film having an absorption axis in the longitudinal or width direction, and preferably enables roll-to-roll bonding.
[0095] The areal stretching ratio of the stretching is preferably 1.4 or more, more preferably 1.42 or more, particularly preferably 1.45 or more, and preferably 2.5 or less, more preferably 2.45 or less, particularly preferably 2.4 or less. The areal stretching ratio represents the product of the stretching ratios in each stretching direction. Thus, for example, in uniaxial stretching, the stretching ratio of the uniaxial stretching represents the areal stretching ratio. Also, for example, in biaxial stretching, the product of the stretching ratios in two directions represents the areal stretching ratio. When the areal stretching ratio is equal to or greater than the lower limit of the range, a stretched film having a large retardation Rth in the thickness direction can be obtained. In addition, conventional films stretched at such a large areal stretching ratio tend to have poor tensile elongation at break and handleability. In contrast, the stretched film according to the present embodiment is excellent in tensile elongation at break and handleability while being stretched at a large areal stretching ratio as described above. From the viewpoint of utilizing the advantages of excellent tensile elongation at break and handleability, the areal stretching ratio is preferably equal to or greater than the lower limit of the above range, whereas if the areal stretching ratio is equal to or less than the upper limit of the above range, a stretched film having particularly excellent tensile elongation at break and handleability can be obtained.
[0096] The stretching temperature is preferably Tg° C. or higher, more preferably Tg+5° C. or higher, and preferably Tg+40° C. or lower, more preferably Tg+30° C. or lower. Here, Tg represents the glass transition temperature of the thermoplastic resin. When the stretching temperature is within the above range, it is easy to make the thickness of the stretched film uniform.
[0097] In the above-mentioned manufacturing method, as described above, a stretched film can be obtained by stretching a pre-stretched film, but the above-mentioned manufacturing method may further include any step. For example, the above-mentioned manufacturing method may include a step of trimming the stretched film. In this step, a long stretched film is usually continuously trimmed at appropriate positions to continuously remove the ends in the width direction of the stretched film. In a conventional film with poor handling properties, this trimming tends to cause breakage in the stretched film or the ends removed from the stretched film. In contrast, the stretched film according to the present embodiment has excellent handling properties, and therefore breakage of the stretched film and the ends due to the trimming can be suppressed.
[0098] According to the above-mentioned manufacturing method, a long stretched film can be obtained. Such a long stretched film can be continuously manufactured, and is excellent in productivity. In addition, lamination with other films can be performed by roll-to-roll, and in this respect, too, the productivity is excellent. Usually, a long stretched film is wound up and stored and transported in a roll state.
[0099] [6. Uses of oriented films] The above-mentioned stretched film can be provided as an optical film in an image display device such as a liquid crystal display device. In this case, the stretched film may be provided alone in the image display device, or may be attached to any film to form a multilayer film in the image display device. As a specific example, a multilayer film may be obtained by attaching a stretched film to a polarizing film, and the multilayer film may be provided in the image display device. EXAMPLES
[0100] The present invention will be described in detail below with reference to examples. However, the present invention is not limited to the following examples, and can be modified and carried out as desired without departing from the scope of the claims of the present invention and the scope of equivalents thereto. In the following description, the units "%" and "parts" that represent amounts are by weight unless otherwise specified. The following operations were carried out in air at room temperature and normal pressure unless otherwise specified.
[0101] [I. Methods for measuring and calculating physical properties of polymers and resins] (Method of measuring weight average molecular weight Mw of polymer) The weight-average molecular weight Mw of the polymer was measured by gel permeation chromatography (GPC) using cyclohexane as an eluent, and was calculated as a value converted into standard polyisoprene. When the polymer was not soluble in cyclohexane, THF was used as an eluent. When THF was used as an eluent, the weight-average molecular weight Mw was measured in terms of polystyrene. As the standard polyisoprene, standard polyisoprene manufactured by Tosoh Corporation (Mw=602, 1390, 3920, 8050, 13800, 22700, 58800, 71300, 109000, 280000) was used. The measurements were performed using three Tosoh columns (TSKgel G5000HXL, TSKgel G4000HXL, and TSKgel G2000HXL) connected in series under conditions of a flow rate of 1.0 mL / min, a sample injection amount of 100 μL, and a column temperature of 40°C.
[0102] (Method of measuring glass transition temperature Tg) The glass transition temperature Tg was measured using a differential scanning calorimeter ("DSC6220SII" manufactured by Nano Technology Corporation) in accordance with JIS K 6911 at a temperature rise rate of 10°C / min.
[0103] (Method of measuring stress birefringence CR) The resin was molded into a sheet of 35 mm length x 10 mm width x 1 mm thickness to obtain a sample sheet. Both ends of the sample sheet were fixed with clips, and then a weight of 55 g was fixed to one of the clips. Next, the sample sheet was hung for 1 hour in an oven set to the glass transition temperature Tg+15°C of the resin, starting from the clip to which the weight was not fixed, and stretched. The sample sheet was then slowly cooled to room temperature to obtain a measurement sample.
[0104] The in-plane retardation Re(b) [nm] of the center of the sample was measured at a wavelength of 650 nm using a birefringence meter (Photonic Lattice's "WPA-100"). The thickness T(b) [mm] of the center of the sample was also measured. Using these measured values Re(b) and T(b), the Δn value was calculated according to the following formula (X1). δn=Re(b)×(1 / T(b))×10 -6 (X1) Using the Δn value and the stress F applied to the sample, the stress birefringence CR was calculated according to the following formula (X2). CR=δn / F(X2)
[0105] [II. Film Evaluation Method] (Method of measuring film thickness) The thickness of the film was measured with a snap gauge ("ID-C112BS" manufactured by Mitutoyo Corporation) at the center in the width direction of the film.
[0106] (Method of measuring thickness direction retardation Rth and ratio Rth / d) The retardation Rth [nm] in the thickness direction of the stretched film was measured using a phase difference meter (AXOMETRICS "AXOSCAN") at a measurement wavelength of 550 nm. The ratio Rth / d was calculated using the measured value Rth [nm] and the thickness d [mm] of the stretched film according to the following formula (X3). Rth / d=Rth×(1 / d)×10 -6 (X3)
[0107] (Calculation method for areal stretch ratio S) The areal stretch ratio, which represents the total stretch ratio, was calculated as follows. In the examples and comparative examples in which longitudinal stretching and transverse stretching were performed, the areal stretching ratio was calculated by multiplying the longitudinal stretching ratio by the transverse stretching ratio. In the examples and comparative examples in which oblique stretching was performed, the stretching ratio in the oblique direction itself was adopted as the areal stretching ratio.
[0108] (Method of measuring tensile elongation at break E) In accordance with JIS K7127, the tensile elongation at break of the film to be measured was measured by the following method. Ten dumbbell-shaped test pieces of Type 1B were punched out from the film to be measured. Five of the test pieces were punched out so that the MD direction (flow direction, equivalent to the longitudinal direction) of the film was parallel to the longitudinal direction of the dumbbell-shaped test pieces. The remaining five test pieces were punched out so that the TD direction (direction perpendicular to the flow direction, equivalent to the width direction) of the film was parallel to the longitudinal direction of the dumbbell-shaped test pieces. The tensile elongation at break of the test pieces thus obtained was measured using a tensile tester (Instron "5564" model) equipped with a thermo-hygrostat. The tensile speed was 20 mm / min. The average value of the measured values of the five test pieces having a longitudinal direction parallel to the MD direction of the film and the measured values of the five test pieces having a longitudinal direction parallel to the TD direction of the film was calculated, and this average value was taken as the tensile elongation at break E of the film.
[0109] (Method of evaluating handling) The handleability of the film in the production process of the stretched film was evaluated according to the following evaluation criteria. A: From the time the pre-stretched film is supplied to the longitudinal stretching machine or oblique stretching machine until the stretched film is taken up by the winding machine, there are no tears in the pre-stretched film, the intermediate film, the stretched film, or the widthwise ends cut from the stretched film. B: No breaks in the pre-stretched film, intermediate film, or stretched film in the oven of the longitudinal stretching machine, transverse stretching machine, or oblique stretching machine. However, during the trimming process in which the ends in the width direction are cut off from the stretched film, breaks occur in the stretched film or in the ends cut off from the stretched film. C: In the oven of the longitudinal stretching machine, the transverse stretching machine, or the oblique stretching machine, breakage occurs in the pre-stretched film, the intermediate film, or the stretched film. Furthermore, during a trimming process in which the end portions in the width direction are cut off from the stretched film, breakage occurs in the stretched film or in the end portions cut off from the stretched film.
[0110] [Example 1] (1-1) Preparation of norbornene ring-opening polymer: In a glass reactor with the inside replaced with nitrogen, 200 parts of dehydrated cyclohexane, 0.73 mol% of 1-hexene, 0.15 mol% of diisopropyl ether, and 0.44 mol% of triisobutylaluminum were placed at room temperature and mixed relative to a total of 100 parts by weight of the monomers described below. Thereafter, while maintaining the polymerization temperature at 45°C, 70 parts by weight of dicyclopentadiene (abbreviated as "DCPD"), 29 parts by weight of tetracyclododecene (abbreviated as "TCD"), and 1 part by weight of norbornene (abbreviated as "NB"), as monomers, and 0.02 mol% of tungsten hexachloride (0.65 wt% toluene solution) were continuously added in parallel to the reactor over a period of 2 hours to polymerize. Next, 0.2 mol% of isopropyl alcohol was added to the polymerization solution to inactivate the polymerization catalyst and terminate the polymerization reaction. In the above explanation, the amount indicated by the unit "mol%" is a value based on the total amount of the monomers being 100 mol%. As a result, a reaction solution containing a norbornene-based ring-opening polymer as a polymer of the monomer was obtained. The conversion rate of the monomer to the polymer was 100%.
[0111] (1-2) Production of norbornene-based hydrides by hydrogenation: Next, 67 parts by weight of cyclohexane was added to 183 parts by weight of the reaction solution containing the norbornene-based ring-opening polymer obtained in the above step (1-1), and 0.8% by weight of a diatomaceous earth supported nickel catalyst ("T8400RL" manufactured by JGC Chemical Co., Ltd., nickel loading rate 57%) was further added as a hydrogenation catalyst. The amount of hydrogenation catalyst is expressed as a value relative to 100% by weight of the norbornene-based ring-opening polymer contained in the reaction solution. Thereafter, the reaction solution was pressurized to 4.5 MPa with hydrogen and heated to a temperature of 190°C while stirring, and the hydrogenation reaction was carried out for 8 hours. As a result, a reaction solution containing a norbornene-based hydrogenated product as a hydrogenated product of the norbornene-based ring-opening polymer was obtained. The hydrogenation rate of this norbornene-based hydrogenated product was calculated as follows: 1 The hydrogenation rate of the non-aromatic carbon-carbon unsaturated bonds was determined to be 99.9% by 1 H-NMR.
[0112] The obtained reaction solution was filtered under pressure at a pressure of 0.25 MPa using Radiolite #500 as a filter bed (Ishikawajima-Harima Heavy Industries Co., Ltd.'s "Fundaback Filter") to remove the hydrogenation catalyst and obtain a colorless, transparent solution. The obtained solution was poured into a large amount of isopropanol to precipitate a norbornene-based hydrogenated product. The precipitated norbornene-based hydrogenated product was filtered off. Then, 2.0 parts of a xylene solution in which 0.1 parts of an antioxidant [pentaerythritol-tetrakis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate] (Ciba Specialty Chemicals Co., Ltd.'s "Irganox (registered trademark) 1010)] was dissolved was added to 100 parts of the norbornene-based hydrogenated product. Next, the mixture was dried in a vacuum dryer (200°C, 1 Torr) for 6 hours to obtain a thermoplastic norbornene-based resin. The weight average molecular weight Mw of the norbornene-based hydrogenated product was 4.2 × 10 4 It was.
[0113] The glass transition temperature Tg and stress birefringence CR of the thermoplastic norbornene resin were measured by the above-mentioned method. The glass transition temperature Tg of the thermoplastic norbornene resin was 111° C., and the stress birefringence CR was 2450×10 -12 Pa -1 It was.
[0114] (1-3) Preparation of pre-stretched film: The thermoplastic norbornene resin obtained in the above step was fed into a twin-screw extruder and molded into a strand-shaped molded body by hot melt extrusion molding. The molded body was chopped with a strand cutter to obtain pellets of the thermoplastic norbornene resin.
[0115] The pellets were dried at 80° C. for 5 hours. Thereafter, the pellets were fed to an extruder by a conventional method and melted at 250° C. The molten thermoplastic norbornene-based resin was extruded from a die onto a cooling drum to produce a long resin film having a thickness of 47 μm, and a pre-stretched film was continuously produced.
[0116] (1-4) Production of stretched film: A longitudinal stretching machine equipped with rolls and an oven and using a float method between rolls was prepared. Using this longitudinal stretching machine, the pre-stretched film was stretched in the longitudinal direction by 1.1 times to obtain an intermediate film. The stretching temperature in the longitudinal stretching machine was 116°C. The intermediate film was then fed to a transverse stretching machine equipped with an oven and using a tenter method. Using this transverse stretching machine, the intermediate film was stretched 1.5 times in the transverse direction while adjusting the take-up tension and the tenter chain tension, to obtain a long stretched film as a biaxially stretched film. The stretching temperature in the transverse stretching machine was 116°C. The areal stretch ratio for these stretches was 1.65 times.
[0117] The obtained stretched film was subjected to a trimming process in which the stretched film was cut at a position 350 mm away from the edge in the width direction using a trimming device equipped with a cutter while being conveyed in the longitudinal direction. As a result, the end in the width direction was removed from the stretched film. Thereafter, the stretched film from which the end was removed was wound into a roll using a winding machine.
[0118] The stretched film thus obtained was evaluated by the above-mentioned method. The stretched film thus obtained had a retardation in the thickness direction Rth of 130 nm, a thickness d of 30 μm, and an Rth / d of 4.33×10 -3 The tensile elongation at break E was 105%. The handleability was rated A according to the above-mentioned evaluation criteria.
[0119] [Example 2] In the above step (1-3), the thickness of the film before stretching was changed to 43 μm by adjusting the resin take-up speed by the cooling drum. In addition, in the above step (1-4), the stretching ratio and stretching temperature of the film before stretching by the longitudinal stretching machine were changed to 1.25 times and 120° C. In addition, in the above step (1-4), the stretching ratio and stretching temperature of the intermediate film by the transverse stretching machine were changed to 1.55 times and 120° C. Except for the above, the stretched film was produced and evaluated in the same manner as in Example 1.
[0120] [Example 3] In the above step (1-3), the thickness of the film before stretching was changed to 72 μm by adjusting the resin take-up speed by the cooling drum. In addition, in the above step (1-4), the stretching ratio and stretching temperature of the film before stretching by the longitudinal stretching machine were changed to 1.4 times and 111° C. In addition, in the above step (1-4), the stretching ratio and stretching temperature of the intermediate film by the transverse stretching machine were changed to 1.7 times and 111° C. Except for the above, the stretched film was produced and evaluated in the same manner as in Example 1.
[0121] [Example 4] (4-1) Preparation of pre-stretched film: A long pre-stretched film was produced in the same manner as steps (1-1) to (1-3) of Example 1, except that the thickness of the pre-stretched film produced was changed to 32 μm by adjusting the resin take-up speed by the cooling drum.
[0122] (4-2) Production of stretched film: The pre-stretched film was fed to an oblique stretching machine equipped with an oven and using a tenter method. Using this oblique stretching machine, the pre-stretched film was stretched in an oblique direction by 1.5 times while adjusting the take-up tension, the tenter chain tension, and the tenter chain speed, to obtain a stretched film as an obliquely stretched film. In this example, the oblique direction as the stretching direction was a method in which an angle of 45° was formed with respect to the longitudinal direction of the pre-stretched film. The stretching temperature of the oblique stretching machine was 119°C.
[0123] The obtained stretched film was conveyed in the longitudinal direction and subjected to the same trimming treatment as in Example 1. The stretched film from which the end was removed was then wound into a roll using a winding machine. The stretched film thus obtained was evaluated by the method described above.
[0124] [Example 5] (5-1) Preparation of thermoplastic norbornene-based resin containing norbornene-based hydride: The combination of monomers used was changed to 28 parts by weight of tetracyclododecene (TCD), 70 parts by weight of dicyclopentadiene (DCPD), and 2 parts by weight of norbornene (NB). The amount of 1-hexene was changed to 0.78 mol%. Except for the above, a thermoplastic norbornene resin containing a norbornene-based hydride and an antioxidant was obtained by the same method as in step (1-1) and step (1-2) of Example 1. The weight average molecular weight Mw of the norbornene-based hydride was 3.9×10 4 The glass transition temperature Tg of the thermoplastic norbornene resin was 108°C, and the stress birefringence CR was 2550×10 -12 Pa -1 It was.
[0125] (5-2) Preparation of pre-stretched film: The thermoplastic norbornene resin produced in the above step (5-1) was used instead of the thermoplastic norbornene resin produced in Example 1. The thickness of the pre-stretched film produced was changed to 33 μm by adjusting the resin take-up speed by the cooling drum. A long pre-stretched film was produced in the same manner as in step (1-3) of Example 1, except for the above.
[0126] (5-3) Production of stretched film: The pre-stretched film was fed to an oblique stretching machine equipped with an oven and using a tenter method. Using this oblique stretching machine, the pre-stretched film was stretched in an oblique direction by 1.45 times while adjusting the take-up tension, the tenter chain tension, and the tenter chain speed, to obtain a stretched film as an obliquely stretched film. In this example, the oblique direction as the stretching direction was a method in which an angle of 45° was formed with respect to the longitudinal direction of the pre-stretched film. The stretching temperature of the oblique stretching machine was 120°C.
[0127] The obtained stretched film was conveyed in the longitudinal direction and subjected to the same trimming treatment as in Example 1. The stretched film from which the end was removed was then wound into a roll using a winding machine. The stretched film thus obtained was evaluated by the method described above.
[0128] [Example 6] (6-1) 8-Methyl-8-methoxycarbonyltetracyclo[4.4.0.1 2,5 .1 7,10 Preparation of ]-3-dodecene (abbreviated as "DNM"): Methyl 2-methylbicyclo[2,2,1]-5-heptene-2-carboxylate (Cas. 7398-76-7; manufactured by Angene International Limited) and dicyclopentadiene (DCPD) were charged in a high pressure vessel at a molar ratio of 88:12. The air in the vessel was then replaced with nitrogen, and the vessel was heated to 165°C at a stirring speed of 600 rpm and held for 1 minute. The vessel was then heated to 200°C and reacted for 3 hours to produce 8-methyl-8-methoxycarbonyltetracyclo[4.4.0.1 2,5 .17,10 ]-3-dodecene (DNM) was obtained.
[0129] (6-2) Preparation of norbornene ring-opening polymer: In a glass reactor with the inside replaced with nitrogen, 200 parts of dehydrated toluene and 7 parts of 1-hexene were placed at room temperature, based on 100 parts by weight of the monomers described below, and mixed. Then, while keeping the temperature at 100°C, 8-methyl-8-methoxycarbonyltetracyclo[4.4.0.1 2,5 .1 7,10 87 parts of ]-3-dodecene (DNM) were added, then 0.005 parts of triethylaluminum and 0.005 parts of methanol-modified tungsten hexachloride were added, and 13 parts of norbornene (NB) as a monomer was added over 20 minutes. Then, the reaction was continued for another 45 minutes. Next, 0.2 mol% of isopropyl alcohol was added to the polymerization solution to inactivate the polymerization catalyst and terminate the polymerization reaction. In the above explanation, the amount indicated by the unit "mol%" is a value assuming that the total amount of monomers is 100 mol%. As a result, a reaction solution containing a norbornene-based ring-opening polymer as a polymer of the monomer was obtained. The conversion rate of the monomer to the polymer was 100%.
[0130] (6-3) Production of norbornene-based hydrides by hydrogenation: Next, 67 parts of toluene was added to 183 parts of the reaction solution containing the norbornene-based ring-opening polymer obtained in the above step (6-2), and 0.0043 parts of chlorohydridocarbonyltris(triphenylphosphine)ruthenium (hereinafter, sometimes abbreviated as "ruthenium catalyst") was further added as a hydrogenation catalyst. Thereafter, the hydrogenation reaction was carried out at a hydrogen pressure of 4.5 MPa and 160°C for 4 hours. As a result, a reaction solution containing a norbornene-based hydride as a hydrogenated product of the norbornene-based ring-opening polymer was obtained.
[0131] The obtained solution was poured into a large amount of isopropanol to precipitate a norbornene-based hydride. The precipitated norbornene-based hydride was collected by filtration. Then, 2.0 parts of a xylene solution in which 0.1 parts of an antioxidant [pentaerythritol-tetrakis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate] (manufactured by Ciba Specialty Chemicals, Inc., "Irganox (registered trademark) 1010)] was dissolved was added to 100 parts of the norbornene-based hydride. Then, the mixture was dried in a vacuum dryer (200°C, 1 Torr) for 6 hours to obtain a thermoplastic norbornene-based resin. The weight average molecular weight Mw of the norbornene-based hydride was 9.5×10 4 It was.
[0132] The glass transition temperature Tg and stress birefringence CR of the thermoplastic norbornene resin were measured by the above-mentioned method. The glass transition temperature Tg of the thermoplastic norbornene resin was 123° C., and the stress birefringence CR was 1900×10 -12 Pa -1 It was.
[0133] (6-4) Preparation of pre-stretched film: The thermoplastic norbornene resin produced in the above step (6-3) was used instead of the thermoplastic norbornene resin produced in Example 1. The thickness of the pre-stretched film produced was changed to 33 μm by adjusting the resin take-up speed by the cooling drum. A long pre-stretched film was produced in the same manner as in step (1-3) of Example 1, except for the above.
[0134] (6-5) Production of stretched film: The pre-stretched film was fed to an oblique stretching machine equipped with an oven and using a tenter method. Using this oblique stretching machine, the pre-stretched film was stretched in an oblique direction by 1.45 times while adjusting the take-up tension, the tenter chain tension, and the tenter chain speed, to obtain a stretched film as an obliquely stretched film. In this example, the oblique direction as the stretching direction was a method in which an angle of 45° was formed with respect to the longitudinal direction of the pre-stretched film. The stretching temperature of the oblique stretching machine was 130°C.
[0135] The obtained stretched film was conveyed in the longitudinal direction and subjected to the same trimming treatment as in Example 1. The stretched film from which the end was removed was then wound into a roll using a winding machine. The stretched film thus obtained was evaluated by the method described above.
[0136] [Example 7] (7-1) Preparation of thermoplastic norbornene-based resin containing norbornene-based hydride: 8-Methyl-8-methoxycarbonyltetracyclo[4.4.0.1 2,5 .1 7,10 The amount of 1-hexene (10 parts by weight) was changed to 10 parts by weight, the amount of 1-hexene (10 parts by weight) was changed to 10 parts by weight, and the amount of 1-hexene (10 parts by weight) was changed to 92 parts by weight. Except for the above, a thermoplastic norbornene-based resin containing a norbornene-based hydride and an antioxidant was obtained in the same manner as in steps (6-1) to (6-3) of Example 6. The weight average molecular weight Mw of the norbornene-based hydride was 5.0×10 4 The glass transition temperature Tg of the thermoplastic norbornene resin was 136°C, and the stress birefringence CR was 1800×10 -12 Pa -1 It was.
[0137] (7-2) Preparation of pre-stretched film: The thermoplastic norbornene resin produced in the above step (7-1) was used instead of the thermoplastic norbornene resin produced in Example 1. The thickness of the pre-stretched film produced was changed to 39 μm by adjusting the resin take-up speed by the cooling drum. Except for the above, the pre-stretched film was produced in the same manner as in step (1-3) of Example 1.
[0138] (7-3) Production of stretched film: Instead of the pre-stretched film produced in Example 1, the pre-stretched film produced in the above step (7-2) was used. In addition, the stretching temperature of the pre-stretched film in the longitudinal stretching machine was changed to 141° C. In addition, the stretching temperature of the intermediate film in the transverse stretching machine was changed to 141° C. Except for the above, the stretched film was produced and evaluated in the same manner as in step (1-4) of Example 1.
[0139] [Example 8] (8-1) Preparation of thermoplastic norbornene-based resin containing norbornene-based hydride: 8-Methyl-8-methoxycarbonyltetracyclo[4.4.0.1 2,5 .1 7,10 The amount of 1-hexene (1-hexene) was changed to 6 parts by weight, the amount of 1-hexene (1-hexene) was changed to 6 parts by weight, and the amount of 1-hexene (1-hexene) was changed to 6 parts by weight. Except for the above, a thermoplastic norbornene-based resin containing a norbornene-based hydride and an antioxidant was obtained in the same manner as in steps (6-1) to (6-3) of Example 6. The weight average molecular weight Mw of the norbornene-based hydride was 6.5×10 4 The glass transition temperature Tg of the thermoplastic norbornene resin was 150°C, and the stress birefringence CR was 1700×10 -12 Pa -1 It was.
[0140] (8-2) Preparation of pre-stretched film: The thermoplastic norbornene resin produced in the above step (8-1) was used instead of the thermoplastic norbornene resin produced in Example 1. The thickness of the pre-stretched film produced was changed to 39 μm by adjusting the resin take-up speed by the cooling drum. Except for the above, the pre-stretched film was produced in the same manner as in step (1-3) of Example 1.
[0141] (8-3) Production of stretched film: Instead of the pre-stretched film produced in Example 1, the pre-stretched film produced in the above step (8-2) was used. In addition, the stretching temperature of the pre-stretched film by the longitudinal stretching machine was changed to 155° C. In addition, the stretching temperature of the intermediate film by the transverse stretching machine was changed to 155° C. Except for the above, the stretched film was produced and evaluated in the same manner as in step (1-4) of Example 1.
[0142] [Comparative Example 1] (C1-1) Preparation of thermoplastic norbornene-based resin containing norbornene-based hydride: The combination of monomers used was changed to 60 parts by weight of methanotetrahydrofluorene (MTF) and 40 parts by weight of tetracyclododecene (TCD). The amount of 1-hexene was changed to 0.8 mol%. The polymerization temperature of the monomers was changed to 55°C. Except for the above, a thermoplastic norbornene-based resin containing a norbornene-based hydride and an antioxidant was obtained in the same manner as in step (1-1) and step (1-2) of Example 1. The weight average molecular weight Mw of the norbornene-based hydride was 3.1 x 10 4 The glass transition temperature Tg of the thermoplastic norbornene resin was 161°C, and the stress birefringence CR was 1600×10 -12 Pa -1 It was.
[0143] (C1-2) Production of pre-stretched film: The thermoplastic norbornene resin produced in the above step (C1-1) was used instead of the thermoplastic norbornene resin produced in Example 1. The thickness of the pre-stretched film produced was changed to 63 μm by adjusting the resin take-up speed by the cooling drum. Except for the above, the pre-stretched film was produced in the same manner as in step (1-3) of Example 1.
[0144] (C1-3) Production of stretched film: Instead of the pre-stretched film produced in Example 1, the pre-stretched film produced in the above step (C1-2) was used. In addition, the stretching temperature of the pre-stretched film by the longitudinal stretching machine was changed to 168° C. In addition, the stretching temperature of the intermediate film by the transverse stretching machine was changed to 168° C. Except for the above, the stretched film was produced and evaluated in the same manner as in step (1-4) of Example 1.
[0145] [Comparative Example 2] (C2-1) Preparation of thermoplastic norbornene-based resin containing norbornene-based hydride: The combination of monomers used was changed to 10 parts by weight of methanotetrahydrofluorene (MTF), 40 parts by weight of tetracyclododecene (TCD), and 50 parts by weight of dicyclopentadiene (DCPD). The amount of 1-hexene was changed to 0.76 mol%. The polymerization temperature of the monomers was changed to 55°C. Except for the above, a thermoplastic norbornene-based resin containing a norbornene-based hydride and an antioxidant was obtained by the same method as in step (1-1) and step (1-2) of Example 1. The weight average molecular weight Mw of the norbornene-based hydride was 3.6 x 10 4 The glass transition temperature Tg of the thermoplastic norbornene resin was 128°C, and the stress birefringence CR was 2020×10 -12 Pa -1 It was.
[0146] (C2-2) Production of pre-stretched film: The thermoplastic norbornene resin produced in the above step (C2-1) was used instead of the thermoplastic norbornene resin produced in Example 1. The thickness of the pre-stretched film produced was changed to 33 μm by adjusting the resin take-up speed by the cooling drum. Except for the above, the pre-stretched film was produced in the same manner as in step (1-3) of Example 1.
[0147] (C2-3) Production of stretched film: Instead of the pre-stretched film produced in Example 1, the pre-stretched film produced in the above step (C2-2) was used. In addition, the stretching ratio and stretching temperature of the pre-stretched film in the longitudinal stretching machine were changed to 1.2 times and 130° C., respectively. In addition, the stretching temperature of the intermediate film in the transverse stretching machine was changed to 130° C. Except for the above, the stretched film was produced and evaluated in the same manner as in step (1-4) of Example 1.
[0148] [Comparative Example 3] (C3-1) Preparation of thermoplastic norbornene-based resin containing norbornene-based hydride: 8-Methyl-8-methoxycarbonyltetracyclo[4.4.0.1 2,5 .1 7,10 The amount of 1-hexene (DNM) was changed to 100 parts. The amount of 1-hexene was changed to 10 parts. Furthermore, norbornene (NB) was not used. Except for the above, a thermoplastic norbornene resin containing a norbornene-based hydride and an antioxidant was obtained in the same manner as in step (6-2) and step (6-3) of Example 6. The weight average molecular weight Mw of the norbornene-based hydride was 13.0×10 4 The glass transition temperature Tg of the thermoplastic norbornene resin was 165°C, and the stress birefringence CR was 2100×10 -12 Pa -1 It was.
[0149] (C3-2) Production of pre-stretched film: The thermoplastic norbornene resin produced in the above step (C3-1) was used instead of the thermoplastic norbornene resin produced in Example 1. The thickness of the pre-stretched film produced was changed to 63 μm by adjusting the resin take-up speed by the cooling drum. Except for the above, the pre-stretched film was produced in the same manner as in step (1-3) of Example 1.
[0150] (C3-3) Production of stretched film: Instead of the pre-stretched film produced in Example 1, the pre-stretched film produced in the above-mentioned step (C3-2) was used. In addition, the stretching temperature of the pre-stretched film by the longitudinal stretching machine was changed to 177° C. In addition, the stretching temperature of the intermediate film by the transverse stretching machine was changed to 177° C. Except for the above, the stretched film was produced and evaluated in the same manner as in step (1-4) of Example 1.
[0151] [result] The results of the above-mentioned Examples and Comparative Examples are shown in the following table. In the following table, the meanings of the abbreviations are as follows. TCD: tetracyclododecene. DNM: 8-methyl-8-methoxycarbonyltetracyclo[4.4.0.1 2,5 .1 7,10 ]-3-Dodecene. DCPD: dicyclopentadiene. NB: Norbornene. MTF: methanotetrahydrofluorene. Mw: Weight average molecular weight of norbornene hydride. Tg: Glass transition temperature of thermoplastic norbornene resin. CR value: Stress birefringence of thermoplastic norbornene resin. Rth: Retardation in the thickness direction of the stretched film. Rth / d: Ratio of retardation Rth in the thickness direction to the thickness d of the stretched film.
[0152] [Table 1]
[0153] [Table 2]
[0154] [Table 3]
Claims
1. A stretched film formed of a thermoplastic resin containing a norbornene-based polymer, the norbornene-based polymer is selected from the group consisting of polymers of norbornene-based monomer compositions and hydrogenated products thereof, The norbornene-based monomer composition contains a monomer represented by the following formula (T) and a monomer represented by the following formula (D) in an amount of 50% by weight or more, and a monomer represented by the following formula (N) in an amount of 1% by weight to 15% by weight, The amount of the monomer represented by the following formula (T) is 35% by weight or less with respect to 100% by weight of the total amount of the norbornene-based monomer composition, The amount of the monomer represented by the following formula (D) is 65% by weight or more based on 100% by weight of the total amount of the norbornene-based monomer composition, The stretched film has a thickness of 40 μm or less. [Formula 1] (In formula (T), Each of nt1 and nt2 independently represents 1 or 2; When nt1 is 1, R t1 represents a divalent hydrocarbon group, When nt1 is 2, R t1 each independently represents a hydrogen atom, an alkyl group, or an alkyloxycarbonyl group, When nt2 is 1, R t2 represents a divalent hydrocarbon group, When nt2 is 2, R t2 each independently represents a hydrogen atom, an alkyl group, or an alkyloxycarbonyl group; In formula (D), nd1, nd2 and nd3 each independently represent 1 or 2; When nd1 is 1, R d1 represents a hydrogen atom, an alkyl group, an alkyloxycarbonyl group, or a divalent hydrocarbon group, When nd1 is 2, R d1 each independently represents a hydrogen atom, an alkyl group, or an alkyloxycarbonyl group, When nd2 is 1, R d2 represents a hydrogen atom, an alkyl group, an alkyloxycarbonyl group, or a divalent hydrocarbon group, When nd2 is 2, R d2 each independently represents a hydrogen atom, an alkyl group, or an alkyloxycarbonyl group, When nd3 is 1, R d3 represents a divalent hydrocarbon group, When nd3 is 2, R d3 each independently represents a hydrogen atom, an alkyl group, or an alkyloxycarbonyl group; In formula (N), nn1 and nn2 each independently represent 1 or 2; When nn1 is 1, R n1 represents a divalent hydrocarbon group, When nn1 is 2, R n1 each independently represents a hydrogen atom, an alkyl group, or an alkyloxycarbonyl group, If nn2 is 1, then R n2 represents a divalent hydrocarbon group, When nn2 is 2, R n2 each independently represents a hydrogen atom, an alkyl group, or an alkyloxycarbonyl group.
2. The stretched film according to claim 1 , wherein the stretched film is an obliquely stretched film.
3. 10. The stretched film of claim 1, wherein the stretched film is a biaxially stretched film.
4. The ratio (Rth / d) of the retardation Rth in the thickness direction of the stretched film to the thickness d of the stretched film is 3×10 -3 The stretched film according to any one of claims 1 to 3.
5. The stretched film according to any one of claims 1 to 4, wherein the areal stretching ratio of the stretched film is 1.4 times or more.
6. The stress birefringence CR of the thermoplastic resin is 1650×10 -12 P -1 The stretched film according to any one of claims 1 to 5,
7. The stretched film according to any one of claims 1 to 6, wherein the stretched film has a tensile elongation at break of 85% or more.
8. The stretched film according to any one of claims 1 to 7, wherein the glass transition temperature Tg of the thermoplastic resin is 105°C or higher and lower than 170°C.
9. A method for producing the stretched film according to any one of claims 1 to 8, The method includes the steps of: preparing a resin film formed of a thermoplastic resin containing a norbornene-based polymer; and stretching the resin film; the norbornene-based polymer is selected from the group consisting of polymers of norbornene-based monomer compositions and hydrogenated products thereof, The norbornene-based monomer composition contains a monomer represented by the following formula (T) and a monomer represented by the following formula (D) in an amount of 50% by weight or more, and a monomer represented by the following formula (N) in an amount of 1% by weight to 15% by weight, The amount of the monomer represented by the following formula (T) is 35% by weight or less with respect to 100% by weight of the total amount of the norbornene-based monomer composition, A method for producing a stretched film, wherein the amount of the monomer represented by the following formula (D) is 65% by weight or more relative to 100% by weight of a total amount of the norbornene-based monomer composition: [chemical 2] (In formula (T), Each of nt1 and nt2 independently represents 1 or 2; When nt1 is 1, R t1 represents a divalent hydrocarbon group, When nt1 is 2, R t1 each independently represents a hydrogen atom, an alkyl group, or an alkyloxycarbonyl group, When nt2 is 1, R t2represents a divalent hydrocarbon group, When nt2 is 2, R t2 each independently represents a hydrogen atom, an alkyl group, or an alkyloxycarbonyl group; In formula (D), nd1, nd2 and nd3 each independently represent 1 or 2; When nd1 is 1, R d1 represents a hydrogen atom, an alkyl group, an alkyloxycarbonyl group, or a divalent hydrocarbon group, When nd1 is 2, R d1 each independently represents a hydrogen atom, an alkyl group, or an alkyloxycarbonyl group, When nd2 is 1, R d2 represents a hydrogen atom, an alkyl group, an alkyloxycarbonyl group, or a divalent hydrocarbon group, When nd2 is 2, R d2 each independently represents a hydrogen atom, an alkyl group, or an alkyloxycarbonyl group, When nd3 is 1, R d3 represents a divalent hydrocarbon group, When nd3 is 2, R d3 each independently represents a hydrogen atom, an alkyl group, or an alkyloxycarbonyl group; In formula (N), nn1 and nn2 each independently represent 1 or 2; When nn1 is 1, R n1 represents a divalent hydrocarbon group, When nn1 is 2, R n1 each independently represents a hydrogen atom, an alkyl group, or an alkyloxycarbonyl group, If nn2 is 1, then R n2 represents a divalent hydrocarbon group, When nn2 is 2, R n2 each independently represents a hydrogen atom, an alkyl group, or an alkyloxycarbonyl group.
10. The method for producing a stretched film according to claim 9, wherein the areal stretching ratio of the stretched film is 1.4 times or more.
Citation Information
Patent Citations
Optical film and its manufacturing method
JP2008030243A
Method of manufacturing stretched film
JP2010221719A
Cyclic olefin resin composition, optical film and retardation plate using the composition, and their production methods
WO2008015919A1
Long optical film, method for producing same, polarizing plate and display device
WO2017002508A1